Interfacial origin of unconventional spin-orbit torque in Py/γ−γ-IrMn3_{3}

Abstract

Angle-resolved spin-torque ferromagnetic resonance measurements are carried out in heterostructures consisting of Py (Ni81_{81}Fe19_{19}) and a noncollinear antiferromagnetic quantum material γ−γ-IrMn3_{3}. The structural characterization reveals that γ−γ-IrMn3_{3} is polycrystalline in nature. A large exchange bias of 158~Oe is found in Py/γ−γ-IrMn3_{3} at room temperature, while γ−γ-IrMn3_{3}/Py and Py/Cu/γ−γ-IrMn3_{3} exhibited no exchange bias. Regardless of the exchange bias and stacking sequence, we observe a substantial unconventional out-of-plane anti-damping torque when γ−γ-IrMn3_{3} is in direct contact with Py. The magnitude of the out-of-plane spin-orbit torque efficiency is found to be twice as large as the in-plane spin-orbit torque efficiency. The unconventional spin-orbit torque vanishes when a Cu spacer is introduced between Py and γ−γ-IrMn3_{3}, indicating that the unconventional spin-orbit torque in this system originates at the interface. These findings are important for realizing efficient antiferromagnet-based spintronic devices via interfacial engineering.

Spin-orbit torques (SOTs) in ferromagnetic/heavy metal (FM/HM) heterostructures have emerged as a powerful tool for a wide range of spintronic applications.1–6 Large anti-damping SOTs are of utmost interest and play a pivotal role in ultrafast magnetization switching3,7, spintronic oscillators4,6,8–10 as well as the emerging area of spintronic-based neuromorphic computing.11–15 In the FM/HM system, the SOT is generated either via the spin Hall effect[19] [16, 17, 18] from the HM layer and/or the Rashba-Edelstein effect[20, 21] from the interface between the FM and HM layers. In both cases, when a charge current flows in the xx−direction, it generates a spin current in the zz−direction with the spin polarization along the yy−direction, which can apply an in-plane anti-damping torque on the adjacent FM layer.[19] [2] This is often referred to as “conventional SOT.” Due to the symmetry of the conventional SOT, it is difficult to achieve deterministic switching of a perpendicularly magnetized system used in high-density magnetic recording. Recently, an out-of-plane damping-like torque was reported in WTe2_2/Py by using the low crystalline symmetry of WTe2_2.[22] Field-free switching in perpendicularly magnetized FMs using the unconventional spin-orbit torques (USOTs) in WTe2_2 was also demonstrated recently.[23] Since then, USOTs have been reported in non-collinear antiferromagnets such as Mn3_3GaN,[24] Mn3_3Sn,[25] Mn3_3Sn[26] and IrMn3_3[27] by using their low magnetic symmetry, which gives rise to an out-of-plane spin polarization for in-plane charge currents. The non-collinear antiferromagnetic also exhibits a large anomalous Hall effect due to the non-zero Berry curvature caused by the spin texture in the Kagome plane.[28, 29, 30, 31, 32, 33] In addition, the ferromagnetic/antiferromagnetic (FM/AFM) bilayer systems are also extensively explored for the presence of exchange bias[34] and large SOTs, which lead to field-free switching of ferromagnets.[35, 36, 37] Particularly, for the non-collinear antiferromagnet IrMn3_3, an unconventional torque is reported for epitaxial L10_0−IrMn and L12_2−IrMn3_3.[27]

In this work, we investigate SOT in Py(=Ni81_{81}Fe19_{19})/γ\gamma−IrMn3_3, γ\gamma−IrMn3_3/Py and Py/Cu/γ\gamma−IrMn3_3 using the spin-torque ferromagnetic resonance (STFMR) technique and determine ξDLx\xi_{\mathrm{DL}}^x, ξDLy\xi_{\mathrm{DL}}^y and ξDLz\xi_{\mathrm{DL}}^z which represents damping-like spin torque efficiency in xx−, yy− and zz− direction, respectively. All the three components ξDLx\xi_{\mathrm{DL}}^x, ξDLy\xi_{\mathrm{DL}}^y, and ξDLz\xi_{\mathrm{DL}}^z are found to be present in Py/γ\gamma−IrMn3_3, γ\gamma−IrMn3_3/Py system, while only ξDLy\xi_{\mathrm{DL}}^y is found to be present in Py/Cu/γ\gamma−IrMn3_3. This means that while USOT exists in both Py/γ\gamma−IrMn3_3 and γ\gamma−IrMn3_3/Py systems, the Py/Cu/γ\gamma−IrMn3_3 system has only conventional SOT. Thus, the USOT in our case arises from the interface between Py and polycrystalline γ\gamma−IrMn3_3, which is in stark contrast with previous findings where the USOT was observed only due to the presence of low magnetic symmetry in the bulk of IrMn3_3.[27] Our results show that USOT can be obtained using a CMOS-compatible naturally oxidized high resistive Si substrate, unlike previous studies of Zhou et al.,[27] for which the authors used specialized substrates, which is not compatible with CMOS-technology.

The thin film heterostructures are grown using an AJA Orion 8 UHV magnetron sputtering system at room temperature. The base pressure of the sputtering system is better than 2×10−82 \times10^{-8} Torr. Samples were grown at a working pressure of 1×10−31 \times10^{-3} Torr. First, we optimized the growth of IrMn3_3. We used a target with the composition of 20 at% Ir and 80 at% Mn. Subsequently, we deposited multilayer samples with Py and γ\gamma−IrMn3_3 on Si substrates at room temperature. The structural characterization was performed using X-ray diffraction (XRD) using a PANalytical x-ray diffractometer equipped with Cu Kα_\alpha (λ=1.5406\lambda= 1.5406 Å) source. We use in-plane grazing incidence X-ray diffraction at an incidence angle of 1∘1^\circ to determine the crystalline phase of IrMn3_3, as shown in Figure 1(a). The Bragg peaks are observed at 2θ=41.6∘2\theta= 41.6^\circ, 48.3∘48.3^\circ, 70.7∘70.7^\circ, and 85.4∘85.4^\circ, which correspond to the IrMn3_3 (111), (200), and (220) and (311)-planes, respectively. The superlattice reflection of L12_2-IrMn3_3, namely peaks corresponding to (110) and (211), are absent in our sample, indicating polycrystalline growth of only γ\gamma-IrMn3_3 phase.[38, 39] The thickness, density, and roughness of the films were analyzed using X-ray reflectivity (XRR) technique and fitted using recursive Parratt’s formalism[40] as shown in Figure 1(b). The thickness and roughness of γ\gamma-IrMn3_3 in this thin film were found to be ≈62\approx62 nm and <0.3< 0.3 nm, respectively. The optimal growth rate of γ\gamma-IrMn3_3 was ≈0.9\approx0.9 Å/s. The zoomed XRR spectrum and respective fit are shown in the inset of Figure 1(b). From the XRR measurements, the interface roughness of multilayer structures was found to be <0.3< 0.3 nm (not shown). To induce exchange bias, these structures were grown in the presence of a 300 Oe in-situ in-plane magnetic field. To avoid oxidation, samples were capped with 2 nm Ta or Pt thin films. Microstrip devices of dimension (4 μ\mum ×\times 12 μ\mum) were fabricated for the STFMR measurements using optical lithography followed by Ar-ion etching. Ground-signal-ground electrodes with 150 μ\mum pitch are fabricated for contact pads. In the present manuscript, we discuss the results for three samples, denoted by Py/γ\gamma-IrMn3_3: Py (8.7 nm)/γ\gamma-IrMn3_3(13 nm), γ\gamma-IrMn3_3/Py: γ\gamma-IrMn3_3(15 nm)/Py(20 nm), and Py/Cu/γ\gamma-IrMn3_3: Py(10 nm)/Cu(1.5 nm)/γ\gamma-IrMn3_3(13 nm).

Figure 1. (a) Grazing-incidence X-ray diffraction spectrum measured in θ−2θ\theta- 2\theta mode, and (b) X-ray reflectivity spectra (black line) as well as the fit (red line) for a 62 nm thick IrMn3_3 thin film. The inset in (b) shows a zoomed portion of XRR spectra with the fit (red line).

Figure 2 shows the magneto-optic Kerr effect (MOKE) measurements performed in the longitudinal configuration with an intensity stabilized He-Ne laser (5 mW and wavelength of 632.8 nm). The incident laser light was p-polarized, and the reflected light is passed through a photoelastic modulator (PEM) followed by an analyzer kept at 45° with respect to the first polarizer. A photodiode was then used to measure the MOKE signal using the lock-in technique. The lock-in amplifier was locked to the second harmonic of PEM frequency. More details of the MOKE setup can be found elsewhere.[41] Figure 2(a), (b), and (c) shows the hysteresis loops measured using the magneto-optic Kerr effect at room temperature for Py/γ\gamma-IrMn3_3, γ\gamma-IrMn3_3/Py and Py/Cu/γ\gamma-IrMn3_3 samples, respectively. The sample Py/γ\gamma-IrMn3_3 in which γ\gamma-IrMn3_3 is deposited on top of Py shows large exchange bias, HexH_{\rm ex} of about 158 Oe. However, we do not observe any exchange bias in samples with reversed stack sequence[42], i.e., γ\gamma-IrMn3_3/Py as well as in the sample with Cu spacer i.e., Py/Cu/γ\gamma-IrMn3_3. We use 1.5 nm thick Cu spacer to break any interfacial coupling between Py and γ\gamma-IrMn3_3, as shown in Supplementary Figure S1. Microstrip devices of dimension (4 μ\mum ×\times 12 μ\mum) were fabricated for the STFMR measurements. For the STFMR measurements, a bias tee is utilized to separate the DC (rectified voltage) and RF port (high-frequency RF current) connected to the microstrip via a Ground-signal-Ground probe.[43] The high-frequency RF current was supplied by R&S signal generator (SMB 100A) at a constant RF power of +3 dBm. The RF signal was amplitude modulated with an 86 Hz signal. The rectified voltage VDCV_{\rm DC} was detected using a lock-in amplifier. The magnetic field was applied in the sample plane at an angle φ\varphi with respect to the current direction (xx-direction) along the long axis of the microstrip. The angle, φ\varphi, was varied from (0–360°) with the help of a vector field magnet. Figure 2(c), (d) and (e) show examples of STFMR spectra measured at 8 GHz with φ=60∘\varphi= 60^\circ for Py/γ\gamma-IrMn3_3, γ\gamma-IrMn3_3/Py and Py/Cu/γ\gamma-IrMn3_3, respectively. Due to the presence of exchange bias, the resonance field (HRH_{\rm R}) for the positive and negative fields was found to be different only for Py/γ\gamma-IrMn3_3. We determine the exchange bias as Hex=∣HR(H>0)−HR(H<0)∣/2H_{\rm ex} = \lvert H_{\rm R}(H > 0) - H_{\rm R}(H < 0) \rvert/2 and found it to be 80 Oe (at φ=60∘\varphi= 60^\circ), which agrees with the magneto-optic Kerr effect measurements after taking into account of the angular dependence of exchange bias. The lineshape of measured STFMR spectra for the three devices shows dramatically different behavior. For both Py/γ\gamma-IrMn3_3 and γ\gamma-IrMn3_3/Py, the lineshape is found to change upon reversal of the field polarity. However, no such change of lineshape with field polarity is observed for Py/Cu/γ\gamma-IrMn3_3, which is similar to the case of the FM/HM system.[22, 44] The measured STFMR signal (VDCV_{\rm DC}) can be fitted using a combination of symmetric and anti-symmetric Lorentzian function[43, 44]:

Magnetic hysteresis loops and STFMR measurements for Py/γ−IrMn3, γ−IrMn3/Py, and Py/Cu/γ−IrMn3

Figure 2. Magnetic hysteresis loops measured using magneto-optic Kerr effect magnetometer for (a) Py/γ\gamma−IrMn3, (b) γ\gamma−IrMn3/Py, and (c) Py/Cu/γ\gamma−IrMn3, respectively. A positive exchange bias of 158 Oe was observed for the sample with γ\gamma−IrMn3 grown directly on top of Py. STFMR measurement for (d) Py/γ\gamma−IrMn3, (e) γ\gamma−IrMn3/Py, and (f) Py/Cu/γ\gamma−IrMn3, respectively. The solid line is the Lorentzian fit using Eq. (1). The symmetric (VSV_\mathrm{S}) and anti-symmetric (VAV_\mathrm{A}) components of the fitted curve are depicted in black and red, respectively. The STFMR measurements reveal that Py/γ\gamma−IrMn3 and γ\gamma−IrMn3/Py systems show a dramatic change of lineshape with field reversal, which is absent in the Py/Cu/γ\gamma−IrMn3 system.

FMR measurements and exchange bias variation

Figure S1. (a) FMR measurements for Py/γ\gamma−IrMn3_3 (black) and Py/Cu (1.5 nm)/γ\gamma−IrMn3_3 (red) sample measured at 8 GHz with sweeping magnetic field parallel to exchange bias. The field reversal spectra show that exchange bias generates a shift in the resonance field in Py/γ\gamma−IrMn3_3. (b) Variation of exchange bias as a function of Cu spacer thickness.

VDC=VSΔH2ΔH2+(H−HR)2+VAΔH(H−HR)ΔH2+(H−HR)2,(1)V_{\rm DC}=V_{\rm S}\frac{\Delta H^{2}}{\Delta H^{2}+(H-H_{\rm R})^{2}}+V_{\rm A}\frac{\Delta H(H-H_{\rm R})}{\Delta H^{2}+(H-H_{\rm R})^{2}}, \tag*{(1)}

Where VSV_{\rm S} and VAV_{\rm A} are symmetric and anti-symmetric voltage components of the rectified voltage. ΔH\Delta H represents the linewidth. The measured STFMR data are fitted with the above equation, as shown by solid lines. We also separately show the symmetric (black) and antisymmetric (red) components.

The magnitude and/or sign of VSV_{\rm S} and VAV_{\rm A} are found to change with the reversal of field polarity for Py/γ\gamma-IrMn3_3 and γ\gamma-IrMn3_3/Py. For a conventional SOT, only sign of VSV_{\rm S} and VAV_{\rm A} should change with the reversal of field polarity. Hence, the SOT for Py/γ\gamma-IrMn3_3 and γ\gamma-IrMn3_3/Py can be considered unconventional. However, when the 1.5 nm thick Cu spacer is present between Py and γ\gamma-IrMn3_3, only sign of VSV_{\rm S} and VAV_{\rm A} changes with the reversal of field polarity- indicating the absence of USOT. Thus, these results indicate that the USOT in our system does not arise from the bulk γ\gamma-IrMn3_3 but from the interface of Py and γ\gamma-IrMn3_3. This is in stark contrast to the recent results of USOT in L12_2–IrMn3_3/Py by Zhou et al. [27], where the USOT was present even with the insertion of Cu layer. Moreover, Zhou et al. used epitaxial L12_2–IrMn3_3, whereas we have γ\gamma-IrMn3_3 phase, for which no

USOT is expected from the broken magnetic mirror symmetry.[27] Additionally, any USOT due to bulk crystal structure is expected to be averaged out for polycrystalline films. Furthermore, USOTs is present even without the exchange bias for γ\gamma−IrMn3/Py indicating that USOT, which we observe, is not linked to the exchange bias.

To systematically examine the presence of USOT and quantify the damping-like torque efficiencies, we have performed complete angular dependent STFMR measurements as shown in Figure 3. First, second and third column corresponds to Py/γ\gamma−IrMn3, γ\gamma−IrMn3/Py and Py/Cu/γ\gamma−IrMn3, respectively. Figure 3(a), (b), and (c) show the extracted symmetric voltage components, and Fig. 3(d), (e), and (f) show the extracted anti-symmetric voltage components. Conventional SOTs (spin polarization along the yy-direction) lead to sin⁡(2φ)cos⁡(φ)\sin(2\varphi)\cos(\varphi)-dependence for both symmetric and anti-symmetric voltage components.[22, 45] However, the data for Py/γ\gamma−IrMn3 and γ\gamma−IrMn3/Py do not follow the sin⁡(2φ)cos⁡(φ)\sin(2\varphi)\cos(\varphi)-dependence indicating that the spin polarization is not restricted to the yy-direction only but also have xx- and zz- components. Considering the spin polarization in an arbitrary direction, the angular dependence of VSV_\mathrm{S} and VAV_\mathrm{A} components can be generalized as[22, 24, 45]:

Image not extracted

Figure 3. Angular dependence of VSV_S and VAV_A components for (a), and (d) Py/γ\gamma–IrMn3_3, (b), and (e) γ\gamma–IrMn3_3/Py (c), and (f) Py/Cu/γ\gamma–IrMn3_3 sample with Cu spacer to avoid exchange coupling between Py and γ\gamma–IrMn3_3. The fitting (solid lines) is performed using Eq. (2) and Eq. (3). The other solid lines (brown, blue, and green) show the extracted angular dependence of voltage contributions from xx–, yy–, and zz–direction spin polarization.

VS=SDLxsin⁡(2φ)sin⁡(φ)+SDLysin⁡(2φ)cos⁡(φ)+SFLzsin⁡(2φ)(2)V_\mathrm{S}=S_\mathrm{DL}^{x}\sin(2\varphi)\sin(\varphi)+S_\mathrm{DL}^{y}\sin(2\varphi)\cos(\varphi)+S_\mathrm{FL}^{z}\sin(2\varphi) \tag*{(2)}
VA=AFLxsin⁡(2φ)sin⁡(φ)+AFLysin⁡(2φ)cos⁡(φ)+ADLzsin⁡(2φ).(3)V_\mathrm{A}=A_\mathrm{FL}^{x}\sin(2\varphi)\sin(\varphi)+A_\mathrm{FL}^{y}\sin(2\varphi)\cos(\varphi)+A_\mathrm{DL}^{z}\sin(2\varphi). \tag*{(3)}

Here, SDLxS_\mathrm{DL}^{x}, SDLyS_\mathrm{DL}^{y} and ADLzA_\mathrm{DL}^{z} are the coefficients for the damping-like torque generated by the different components of spin Hall conductivity tensor, σzxx\sigma_{zx}^{x}, σzyy\sigma_{zy}^{y}, and σzxz\sigma_{zx}^{z} respectively. Similarly, AFLxA_\mathrm{FL}^{x}, AFLyA_\mathrm{FL}^{y}, and SFLzS_\mathrm{FL}^{z} represent the coefficients corresponding to a field-like component of the spin Hall conductivity tensor. Thus by fitting the angular dependence of VSV_\mathrm{S} and VAV_\mathrm{A} using Eq. (2) and Eq. (3), various contributions can be separated. Assuming that AFLyA_\mathrm{FL}^{y} is due to the Oersted field alone, we can quantify the amplitude of three components of damping-like torque efficiencies.[27, 45]

ξDLx=SDLxAFLyeμ0MStFMdNMℏ[1+4πMeffHR]1/2(4)\xi_\mathrm{DL}^{x}=\frac{S_\mathrm{DL}^{x}}{A_\mathrm{FL}^{y}}\frac{e\mu_{0}M_\mathrm{S}t_\mathrm{FM}d_\mathrm{NM}}{\hbar}\left[1+\frac{4\pi M_\mathrm{eff}}{H_\mathrm{R}}\right]^{1/2} \tag*{(4)}
ξDLy=SDLyAFLyeμ0MStFMdNMℏ[1+4πMeffHR]1/2(5)\xi_\mathrm{DL}^{y}=\frac{S_\mathrm{DL}^{y}}{A_\mathrm{FL}^{y}}\frac{e\mu_{0}M_\mathrm{S}t_\mathrm{FM}d_\mathrm{NM}}{\hbar}\left[1+\frac{4\pi M_\mathrm{eff}}{H_\mathrm{R}}\right]^{1/2} \tag*{(5)}
ξDLz=ADLzAFLyeμ0MStFMdNMℏ(6)\xi_\mathrm{DL}^{z}=\frac{A_\mathrm{DL}^{z}}{A_\mathrm{FL}^{y}}\frac{e\mu_{0}M_\mathrm{S}t_\mathrm{FM}d_\mathrm{NM}}{\hbar} \tag*{(6)}

Here, dNMd_{\mathrm{NM}} and tFMt_{\mathrm{FM}} are the non-magnetic and ferromagnetic layer thicknesses, respectively. The parameters ee, ℏ\hbar, and MSM_{\mathrm{S}} represent the electric charge, reduced Planck’s constant, and saturation magnetization, respectively. The effective magnetization, MeffM_{\mathrm{eff}}, is determined from the fitting of ff versus HRH_{\mathrm{R}} [obtained from Eq. (1)] data using the Kittel equation.[46]

Table S1 summarizes the results of fitting of angular dependence of VSV_{\mathrm{S}} and VAV_{\mathrm{A}} for Py/γ\gamma–IrMn3_3, γ\gamma–IrMn3_3/Py and Py/Cu/γ\gamma–IrMn3_3 structure. In the table, ξDLy\xi_{\mathrm{DL}}^{y} denotes the effective conventional damping-like efficiency in the yy–direction, while ξDLx\xi_{\mathrm{DL}}^{x} and ξDLz\xi_{\mathrm{DL}}^{z} represent the unconventional damping-like efficiencies in the xx– and zz–direction, respectively. All the three components ξDLy\xi_{\mathrm{DL}}^{y}, ξDLx\xi_{\mathrm{DL}}^{x}, and ξDLz\xi_{\mathrm{DL}}^{z} are found to be present in Py/γ\gamma–IrMn3_3, γ\gamma–IrMn3_3/Py system, while only ξDLy\xi_{\mathrm{DL}}^{y} is found to be present in Py/Cu/γ\gamma–IrMn3_3. The conventional damping-like efficiency ξDLy\xi_{\mathrm{DL}}^{y} is found to be (0.08±0.03)(0.08 \pm0.03), (−0.25±0.02)(-0.25 \pm0.02) and (0.16±0.02)(0.16 \pm0.02) for Py/γ\gamma–IrMn3_3, γ\gamma–IrMn3_3/Py and Py/Cu/γ\gamma–IrMn3_3, respectively. Here, the sign change in amplitude for ξDLy\xi_{\mathrm{DL}}^{y} for Py/γ\gamma–IrMn3_3, γ\gamma–IrMn3_3/Py is observed because of the stack sequence. The uncertainty in damping-like efficiency values denotes device-to-device variability and fitting errors in VSV_{\mathrm{S}} and VAV_{\mathrm{A}}. The magnitude of ξDLy\xi_{\mathrm{DL}}^{y} for Py/Cu/γ\gamma–IrMn3_3 is found to be greater than that of Py/γ\gamma–IrMn3_3 and lower than that of γ\gamma–IrMn3_3/Py system. This implies that the unconventional contributions in Py/γ\gamma–IrMn3_3 and γ\gamma–IrMn3_3/Py directly increase or decrease the bulk ξDLy\xi_{\mathrm{DL}}^{y} resulting in higher or lower effective ξDLy\xi_{\mathrm{DL}}^{y}. In an earlier report by Tshitoyan, et al.⁴⁷ ξDLy\xi_{\mathrm{DL}}^{y} was reported to be higher for Py/IrMn compared to Py/Cu/IrMn, which was correlated to the exchange bias.

In contrast, our study shows a higher value of the ξDLy\xi_{\mathrm{DL}}^{y} for Py/Cu/γ\gamma–IrMn3_3 due to the exchange bi-ased sample Py/γ\gamma–IrMn3_3 indicating a different mechanism of damping-like spin-orbit torque in our system. We believe this is due to a combination of bulk and interfacial effects. The bulk effect from γ\gamma–IrMn3_3 can be considered as the value of ξDLy\xi_{\mathrm{DL}}^{y} we measure for Py/Cu/γ\gamma–IrMn3_3. The interfacial contributions for Py/γ\gamma–IrMn3_3 and γ\gamma–IrMn3_3/Py have opposite signs, which explains the observed values of ξDLy\xi_{\mathrm{DL}}^{y}.

The unconventional efficiencies in our system are of pure interfacial origin, as stated earlier. The xx– component of USOT (ξDLx\xi_{\mathrm{DL}}^{x}) is found to be 0.28±0.040.28 \pm0.04 and 0.55±0.070.55 \pm0.07 for Py/γ\gamma–IrMn3_3 and γ\gamma–IrMn3_3/Py, respectively. Similarly, the zz– component of USOT (ξDLz\xi_{\mathrm{DL}}^{z}) is found to be −0.12±0.02-0.12 \pm0.02 and −0.40±0.11-0.40 \pm0.11 for Py/γ\gamma–IrMn3_3 and γ\gamma–IrMn3_3/Py, respectively. Interestingly, unconventional torque efficiencies are larger than conventional ξDLy\xi_{\mathrm{DL}}^{y}, which has never been reported before to our knowledge. We also investigated the dependency of USOT on the thickness of Py layer. We do not observe any systematic variation of USOT with Py thickness, as shown in the Supplementary Fig. S2. However, we consistently find that the unconventional torque efficiencies are larger than the conventional ξDLy\xi_{\mathrm{DL}}^{y} for a different devices and with varying Py thicknesses.

We believe the generation of USOTs at the interface of Py and γ\gamma–IrMn3_3 could be due to the spin swapping effect49. The Py/γ\gamma–IrMn3_3 interface works as a magnetic scattering center causing spin swapping (exchange of spin polarization and flow) of bulk spin currents generated by the interior of γ\gamma–IrMn3_3. The interfacial scattering can deflect the spin current flow, resulting in the generation of spin currents polarized in x−x- and z−z- directions, which are non-trivial in nature for normal heavy metals exhibiting the bulk spin Hall effect.19 A similar effect was recently observed in another collinear antiferromagnet, Mn3_3Sn.50 Hence, we believe the interfacial USOT that we observe is unique to γ\gamma–IrMn3_3, since such USOT has not been reported in IrMn previously.47,51,52

SampleExchange Bias (Oe)Direction of polarizationξDLx\xi_{\mathrm{DL}}^{x}ξDLy\xi_{\mathrm{DL}}^{y}ξDLz\xi_{\mathrm{DL}}^{z}
Py/γ\gamma–IrMn3_3158 Oex−x-, y−y-, and z−z- direction0.28±0.040.28\pm0.040.08±0.030.08\pm0.03−0.12±0.02-0.12\pm0.02
γ\gamma–IrMn3_3/Py0 Oex−x-, y−y-, and z−z- direction0.55±0.070.55\pm0.07−0.25±0.03-0.25\pm0.03−0.40±0.11-0.40\pm0.11
Py/Cu/γ\gamma–IrMn3_30 Oey−y- direction only000.16±0.020.16\pm0.0200

Table I. Exchange bias, damping-like efficiency, and spin polarization for Py/γ\gamma–IrMn3_3, γ\gamma–IrMn3_3/Py and Py/Cu/γ\gamma–IrMn3_3.

We observed unconventional spin-orbit torques in heterostructures consisting of Py and polycrystalline γ\gamma–IrMn3_3. The systematic investigation of the angular dependence of symmetric and anti-symmetric components of STFMR measurements suggests the presence of unconventional spin-orbit torques in Py/γ\gamma–IrMn3_3 and γ\gamma–IrMn3_3/Py. The interface between Py and γ\gamma–IrMn3_3 gives rise to substantial out-of-plane damping-like spin-orbit torques in addition to the conventional spin-orbit torques. These unconventional spin-orbit torques can be eliminated by inserting a Cu spacer between Py and γ\gamma–IrMn3_3—indicating an interfacial origin of the unconventional spin-orbit torques in contrast to the previously reported studies that demonstrated a bulk origin arising from the magnetic mirror asymmetry in IrMn3_3. A large in-plane damping-like efficiency of 0.16 is also observed for the Py/Cu/γ\gamma–IrMn3_3 system, indicating that γ\gamma–IrMn3_3 is an efficient source of spin current. These findings emphasize the importance of investigating the interfacial origin of these torques to comprehend the physics of collinear antiferromagnets. The large out-of-plane damping-like efficiency that we observed in our system can be utilized to effectively switch a perpendicularly magnetized system used in high-density magnetic recording.3,36 Therefore, it has high technological relevance for energy-efficient spintronic devices.

Acknowledgments

We acknowledge the Department of Science and Technology for supporting this collaborative work under the Indo-Japan project (grant no: DST /INT/JSPS/P – 266/2018). The partial support from the Science & Engineering Research Board (SERB File no. CRG/2018/001012), the Ministry of Human Resource Development under the IMPRINT program (Grant no: 7519 and 7058), the Department of Science and Technology under the Nanomission program (grant no: SR/NM/NT – 1041/2016(G)), the Department of Electronics and Information Technology (DeitY), Joint Advanced Technology Centre at IIT Delhi, and the Grand Challenge project supported by IIT Delhi are gratefully acknowledged. A. K. acknowledges support from the Council of Scientific and Industrial Research (CSIR), India.

I AUTHOR DECLARATIONS

Conflict of Interest

The authors have no conflicts to disclose.

II DATA AVAILABILITY

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Supplemental Materials: Interfacial origin of unconventional spin-orbit torque in Py/γ\gamma–IrMn3_3

Effect of Cu thickness on interface between Py and γ\gamma–IrMn3_3

A Cu spacer can control the exchange coupling in the Py/γ\gamma–IrMn3_3 thin films. We use the ferromagnetic resonance (FMR) method to determine the effect of Cu thickness at the Py/γ\gamma–IrMn3_3 interface. From FMR measurements, we determine the exchange bias of Py/γ\gamma–IrMn3_3 from the resonance fields (HRH_\mathrm{R}) for the positive and negative fields. Figure S1 shows measured FMR spectra for Py/γ\gamma–IrMn3_3 and Py/Cu/γ\gamma–IrMn3_3 samples. The resonance field in Py/γ\gamma–IrMn3_3 is changed by reversing the field direction. This is caused by the exchange bias, which can be determined as Hex=∣HR(H>0)−HR(H<0)∣/2H_\mathrm{ex}=\lvert H_\mathrm{R}(H>0)-H_\mathrm{R}(H<0)\rvert/2. Figure S1 shows the behavior of HexH_\mathrm{ex} with the thickness of the Cu spacer. The exchange bias shows a steep decrease with the thickness of the Cu layer. The exchange bias completely disappears after a thickness of 1 nm of Cu. Hence, we chose Py/Cu/IrMn3_3 samples with 1.5 nm Cu in the main text to eliminate the exchange coupling between Py and γ\gamma–IrMn3_3.

Thickness dependence of the SOT efficiencies

SOT efficiency was measured for different thicknesses of Py in contact with γ\gamma–IrMn3_3. Figure S2, (Figure S2) shows the ST-FMR spectra for Py(5 nm)/γ\gamma–IrMn3_3 and Py(13 nm)/γ\gamma–IrMn3_3. The angular-dependent of VSV_\mathrm{S} and VAV_\mathrm{A} is shown in Figure S2, (Figure S2), (Figure S2), and (Figure S2) show the presence of unconventional torque in both systems. We summarize the extracted torques in Table S1. Though all samples with Py/γ\gamma–IrMn3_3 show the presence of USOT, no systematic thickness dependence is observed by varying Py thickness from 5 nm→8.7 nm→13 nm. We also found larger ξDLz>ξDLy\xi_\mathrm{DL}^{z}>\xi_\mathrm{DL}^{y} for all the samples.

Figure S2. STFMR measurements on (a) Py(5 nm)/γ\gamma−IrMn3_3, and (d) Py(13 nm)/γ\gamma−IrMn3_3, Angular dependence of VSV_{\mathrm{S}} and VAV_{\mathrm{A}} components for (b), and (c) Py(5 nm)/γ\gamma−IrMn3_3, and (e), and (f) Py(13 nm)/γ\gamma−IrMn3_3. The solid lines in (a) and (d) represent Lorentzian fit using Eq (1) of the main text. The symmetric (VSV_{\mathrm{S}}) and anti-symmetric (VAV_{\mathrm{A}}) components of the fitted curve are depicted in black and red, respectively. The fitting (solid lines) in (b), (c), (e), and (f) are performed using Eq. (2) and Eq. (3) of the main text. The solid lines (brown, blue, and green) in these figures show the extracted angular dependence of voltage contributions from xx−, yy−, and zz−direction spin polarization.

SampleDirection of polarizationξDLx\xi_{\mathrm{DL}}^{x}ξDLy\xi_{\mathrm{DL}}^{y}ξDLz\xi_{\mathrm{DL}}^{z}
Py (5 nm)/γ\gamma−IrMn3_3xx−, yy−, and zz− direction−0.58±0.19-0.58\pm0.190.02±0.100.02\pm0.10−0.06±0.04-0.06\pm0.04
Py (13 nm)/γ\gamma−IrMn3_3xx−, yy−, and zz− direction0.53±0.060.53\pm0.060.04±0.080.04\pm0.08−0.15±0.02-0.15\pm0.02

Table S1. Spin polarization direction and damping-like efficiency for different Py thickness:

References

  1. [19]A. Manchon, I. Železný, I. M. Miron, T. Jungwirth, J. Sinova, A. Thiaville, K. Garello, and P. Gambardella, Rev. Mod. Phys. 91, 035004 (2019).
  2. [20]Y. A. Bychkov and É. I. Rashba, JETP Lett. 39, 78 (1984).
  3. [21]Y. M. Edelstein, Solid State Commun. 73, 233 (1990).
  4. [22]D. MacNeill, G. M. Stiehl, M. H. D. Guimaraes, R. A. Buhrman, J. Park, and D. C. Ralph, Nat. Phys. 13, 300 (2017).
  5. [23]Q. Xie, W. Lin, S. Sarkar, X. Shu, S. Chen, L. Liu, T. Zhao, C. Zhou, H. Wang, J. Zhou, S. Gradečak, and J. Chen, APL Mater. 9, 051114 (2021).
  6. [24]T. Nan, C. X. Quintela, J. Irwin, G. Gurung, D. F. Shao, J. Gibbons, N. Campbell, K. Song, S. Y. Choi, L. Guo, R. D. Johnson, P. Manuel, R. V. Chopdekar, I. Hallsteinsen, T. Tybell, P. J. Ryan, J. W. Kim, Y. Choi, P. G. Radaelli, D. C. Ralph, E. Y. Tsymbal, M. S. Rzchowski, and C. B. Eom, Nat. Commun. 11, 1 (2020).
  7. [25]Y. You, H. Bai, X. Feng, X. Fan, L. Han, X. Zhou, Y. Zhou, R. Zhang, T. Chen, F. Pan, and C. Song, Nat. Commun. 12, 1 (2021).
  8. [26]K. Kondou, H. Chen, T. Tomita, M. Ikhlas, T. Higo, A. H. MacDonald, S. Nakatsuji, and Y. Otani, Nat. Commun. 12, 1 (2021).
  9. [27]J. Zhou, X. Shu, Y. Liu, X. Wang, W. Lin, S. Chen, L. Liu, Q. Xie, T. Hong, P. Yang, B. Yan, X. Han, and J. Chen, Phys. Rev. B 101, 184403 (2020).
  10. [28]R. Shindou and N. Nagaosa, Phys. Rev. Lett. 87, 116801 (2001).
  11. [29]J. Kübler and C. Felser, EPL 108, 67001 (2014).
  12. [30]H. Chen, Q. Niu, and A. H. MacDonald, Phys. Rev. Lett. 112, 017205 (2014).
  13. [31]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Rev. Mod. Phys. 82, 1539 (2010).
  14. [32]T. Higo, D. Qu, Y. Li, C. Chien, Y. Otani, and S. Nakatsuji, Appl. Phys. Lett. 113, 202402 (2018).
  15. [33]W. Han, Y. Otani, and S. Maekawa, npj Quantum Mater. 3, 1 (2018).
  16. [34]J. Nogués and I. K. Schuller, J. Magn. Magn. Mater. 192, 203 (1999).
  17. [35]Y.-W. Oh, S.-H. Chris Baek, Y.-M. Kim, H. Y. Lee, K.-D. Lee, C.-G. Yang, E.-S. Park, K.-S. Lee, K.-W. Kim, G. Go, J.-R. Jeong, B.-C. Min, H.-W. Lee, K.-J. Lee, and B.-G. Park, Nat. Nano. 11, 878 (2016).
  18. [36]S. Fukami, C. Zhang, S. Duttagupta, A. Kurkov, and H. Ohno, Nat. Mater. 15, 535 (2016).
  19. [37]A. van den Brink, G. Vermijs, A. Solignac, J. Koo, J. T. Kohlhepp, H. J. Swagten, and B. Koopmans, Nat. Commun. 7, 1 (2016).
  20. [38]A. Migliorini, B. Kuerbanjiang, T. Huminic, D. Kepaptsoglou, M. Muñoz, J. Cuñado, J. Camarero, C. Aroca, G. Vallejo-Fernández, V. Lazarov, and J. Prieto, Nat. Mater. 17, 28 (2018).
  21. [39]M. Tsunoda, K.-i. Imakita, M. Naka, and M. Takahashi, J. Magn. Magn. Mater. 304, 55 (2006).
  22. [40]L. G. Parratt, Phys. Rev. 95, 359 (1954).
  23. [41]R. Bansal, N. Behera, A. Kumar, and P. Muduli, Appl. Phys. Lett. 110, 202402 (2017).
  24. [42]E. V. Khomenko, N. G. Chechenin, A. Y. Goikhman, and A. V. Zenkevich, JETP Lett. 88, 602 (2008).
  25. [43]A. Kumar, R. Sharma, K. I. Ali Khan, C. Murapaka, G. J. Lim, W. S. Lew, S. Chaudhary, and P. K. Muduli, ACS Appl. Electron. Mater. 3, 3139 (2021).
  26. [44]L. Liu, T. Moriyama, D. C. Ralph, and R. A. Buhrman, Phys. Rev. Lett. 106, 036601 (2011).
  27. [45]A. Bose, N. J. Schreiber, R. Jain, D.-F. Shao, H. P. Nair, J. Sun, X. S. Zhang, D. A. Muller, E. Y. Tsymbal, D. G. Schlom, and D. C. Ralph, Nat. Electron. 5, 267 (2022).
  28. [46]C. Kittel, Phys. Rev. 73, 155 (1948).

Paper details

vlnc:W_2ujb2mpx
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents