as a 2 eV Single-Photon Emitter Candidate in Hexagonal Boron Nitride
Abstract
The generation of single-photon emitters in hexagonal boron nitride around 2 eV emission is experimentally well-recognized; however the atomic nature of these emitters is unknown. In this paper, we use first-principles calculations to demonstrate that is a possible source of 2 eV single-photon emitter. We showcase the calculations of a complete set of static and dynamical properties related to defects, including exciton-defect couplings and electron-phonon interactions. In particular, we show it is critical to consider nonradiative processes when comparing with experimental lifetime for known 2 eV emitters. We find that has several key physical properties matching the ones of experimentally observed single-photon emitters. These include the zero-phonon line (2.13eV), Huang-Rhys factor (1.35), photoluminescence lifetime (2.19 ns), phonon-sideband energy (180meV), and photoluminescence spectrum. The identification of defect candidates for 2 eV emission paves the way for controllable single-photon emission generation.
Introduction
A single-photon emitter is a crucial component in building quantum information technologies, such as linear-optic quantum information processing [1], quantum simulation [2] and quantum communication [3]. Hexagonal boron nitride (hBN) is a two-dimensional (2D) material with a wide bandgap ( eV) [4, 5], and can host stable and bright color centers which possess single-photon emission [6]. Meanwhile, the manipulation of the optoelectronic properties of singe-photon emitters has garnered special interest [7, 8]. These properties imply a great potential of hBN in developing quantum applications. Being able to select and purify single-photon emitters is critical for generating controllable and narrow line width single-photon emission. Hence, the identification of the atomic origin of the single-photon emitters is crucial to the development of this field.
Since 2016 [9], numerous experimental results have been reported on the photoluminescent properties of the single-photon emitters at eV in hBN [27] [7, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26]. In TABLE I, we summarize the range and averaged values of photoluminescence properties observed in experiments, including the zero-phonon line (ZPL), phonon-sideband energy (PSE), Huang-Rhys factor (HR factor), and the photoluminescence lifetime (). Typically, a eV single-photon emitter in hBN exhibits a photoluminescence (PL) spectrum comprised of a sharp ZPL and one or two moderate phonon-sidebands (PSB) at room temperature. The PSE is the energy separation between
the ZPL and the first PSB peak. The electron-phonon coupling is estimated by either HR factor () or Debye-Waller (DW factor ) [28]. The HR factor is typically , which indicates weak electron-phonon coupling. Furthermore, the PL lifetime is on the order of a few ns, and quantum yield (QY, ) is reported to be 6–12% [8]. PL lifetime () reflects the lifetime of an excited state, determined by radiative () and nonradiative recombination together (, ). On the other hand, QY () reflects the proportion of radiative recombination rates with respect to the total recombination rates, and is related to PL lifetime through . PL lifetime and QY underscore the importance of studying both radiative and nonradiative recombination lifetimes. Finally, many of the reported single-photon emitters eV possess linearly polarized excitation and emission [29, 31, 32] [9, 13, 15, 16, 17, 18, 19, 23], indicating the anisotropic structural symmetry of the corresponding defects [33, 34], i.e. possibly belonging to , or groups.
In terms of the atomic origin of these single-photon emitters, annular dark-field images have shown that carbon substitutions are abundant in hBN [35]. Recently, Mendelson et al. [13] has identified that various techniques of incorporating carbon into hBN yield eV single-photon emitters. Moreover, X-ray photoelectron spectroscopy measurements show that more C-B bonds exist than that of C-N bonds [13]. This is an evidence that carbon substitution of nitrogen is more likely than carbon substitution of boron.
Theoretically, several defects have been proposed to be possibly responsible for single-photon emission, such as CV [36] [6], boron dangling bonds [37], NV [38], and carbon trimers [39]. Based on experimental obser-
| ZPL (eV) | PSE (meV) | HR factor | (ns) | |
| Range(exp.) | 1.56–2.24 | 30–200 | 0.63–1.93 | 0.38–19.7 |
| Mean(exp.) | 2.00 ± 0.19 | 156 ± 33 | 1.19 ± 0.43 | 2.6 ± 1.5 |
| CC(cal.) | 2.13 | 180 | 1.35 | 2.19 |
| CC(cal.) | 1.42 | 175 | 1.25 | 3.83 × 10 |
Table 1. Summary of the zero-phonon line (ZPL), phonon-sideband (PSE), Huang-Rhys (HR) factor and photoluminescence (PL) lifetime () for ∼2 eV single-photon emitters in -BN from experimental measurements and our calculated two carbon defects.
vations [13], we focus on carbon defects in this work. Among the carbon defects, CV has high formation energy, 3∼6 eV higher than other carbon defects such as carbon dimer and trimers [40]. Carbon trimers including CC and CC, theoretically proposed by Jara et al. [39], were found energetically favorable and in good agreement with experimental PSE and PL [39]. However, some important information is still missing to confirm carbon trimers as a SPE candidate in Ref. 39. For example, only the ZPL for the lowest transition was calculated, about 0.4 eV smaller than the mean of ZPL in TABLE I. And other important properties such as HR factor, PL lifetime and QY, as the experimental characteristics of ∼2 eV single-photon emitters, were not calculated. Therefore, further study on these properties is desired to unveil the role of carbon trimers as experimentally observed SPEs.
In this paper, electronic and optical properties of the carbon trimers CC and CC are calculated from both first-principles many-body perturbation theory and DFT levels. We evaluate both static and dynamical properties of radiative and phonon-assisted nonradiative recombination, including exciton-defect and electron-phonon interactions. Our results demonstrate that CC has remarkable agreement with experimental observations of 2 eV single photon emitters, including ZPL, PL lifetime, PSE, HR factor, and PL spectrum. We emphasize the importance of comparing all key signatures between theory and experiments for defect identification and validations.
Computational Methods
We employ open source plane-wave code Quantum ESPRESSO [41] for structural relaxation and phonon calculations of carbon defects in monolayer hBN. We use the optimized norm-conserving Vanderbilt (ONCV) pseudopotentials [42] and a 55 Ry wavefunction energy cutoff. We choose a supercell size of 6 × 6 which shows good convergence as tested in Ref. 38, 43, 44. Charged defect correction is included to eliminate the spurious electrostatic interaction by using the techniques developed in Refs. 45, 46 and implemented in the JDFTx code [47]. Total energy, defect formation energy and geometry are obtained with the Perdew-Burke-Ernzerhof (PBE) exchange correlation functional [48]. The charged defect formation energy with the charge state is calculated by
where is the total energy of the charged defect, is the total energy of the pristine system, is the number of atoms of atomic species that is added () or removed (), is the chemical potential of the atomic species , is the electron chemical potential, and is the charged defect correction. The chemical potentials of B, N and C are obtained as follows. In the N-rich condition, where is the total energy of N molecule. In the N-poor condition, where is one atom’s total energy in a boron crystal. and are calculated according to the constraint , where is the total energy of BN with one unit cell. , on the other hand, is one atom’s total energy in graphene.
We evaluate electronic structures under GW approximation with the PBE eigenvalues and wavefunctions as the starting point by using the Yambo code [49]. The starting wavefunctions at PBE are sufficient for accurate descriptions of current defect wavefunctions by comparing with the ones at hybrid functionals (see SI FIG. S1 for wavefunction comparison [44, 50, 51]). In single-shot GW () calculations in this work, the Godby-Needs plasmon-pole approximation (PPA) [52, 53] is used to calculate the dielectric matrices with the plasmon frequency eV. Then Bethe-Salpeter Equation (BSE) is further solved on top of the GW approximation to include the electron-hole interaction in absorption spectra. Coulomb truncation for 2D systems [54] is applied to the out-of-plane direction, and k-point sampling is set to 3 × 3 × 1 for 6 × 6 × 1 supercells in all of the and BSE calculations. More details on convergence tests can be found in SI Section II.
The method in Ref. 39 based on Fermi’s golden rule and solving BSE is applied for calculating radiative lifetime of intra-defect transitions that include exciton-defect coupling. Nonradiative recombination lifetime is also calculated with electron-phonon matrix elements in the static coupling approximation. The details of the nonradiative recombination can be found in Ref. 38, 55. The generating function approach, which is detailed in Ref. 56, is applied to the calculation of PL lineshape. More benchmark and convergence tests on PL calculations can be found in SI Section V.
Results and Discussions
Our results and discussions are organized as follows. First, we discuss the defect stability and their stable charge states through defect formation energies and charge transition levels. Then, we present the electronic structure, optical spectra, and radiative lifetime of the defects. Next, we show ZPL and nonradiative recombination processes of the intra-defect transitions (transition between two states localized on one isolated defect). We then discuss competition between radiative and nonradiative recombination processes and the resulting PL lifetime. Moreover, the PL lineshape and spectral function with the dominant phonon mode are discussed. Finally, we show a full picture comprised of ZPL, PL lifetimes, PSE, HR factor, and PL spectrum of CCN in comparison with experiments.
Charged Defect Formation Energy
When nitrogen and boron atoms are unevenly substituted by atomic impurities, the formation energy of the defects depends on the elemental chemical potentials, i.e. different at the N-rich (B-poor) and N-poor (B-rich) conditions. In the N-rich condition, CCB is more likely to form than CCN because of the smaller formation energy of CCB, as shown in Figure 1(b). On the other hand, CCN is more likely to form in the N-poor condition. It is also found that both defects can be stable in charge states of at a range of electron chemical potentials within the electronic band gap. Without losing generality, we investigate both CCN and CCB in all possible charge states of , and we find that the charge states have ZPL either too large or too small, away from the experimental range (details found in SI TABLE S1). Thus, we focus on the neutral state of the defects. In particular, we find that the neutral CCN have good agreement with experiments on all properties of eV single-photon emitter, so we mainly discuss the neutral CCN in the following. The results of CCB can be found in SI Section III and summarized in Table I. We find the major discrepancy of CCB to experiments is in ZPL and PL lifetime.

Figure 1. Charged defect formation energy of defects CCN and CCB as a function of Fermi level at (a) N-poor and (b) N-rich conditions.
Electronic Structure and Optical Properties
The single-particle diagram in Figure 2(a) shows the defect-related electronic energy levels with their wavefunctions, and the host monolayer hBN band edges at the GW approximation, referenced to the vacuum level. One unoccupied defect state () and three occupied defect states (, , ) in the spin-down channel can lead to intra-defect transitions via radiative recombination or nonradiative recombination. To obtain optical transitions (or two-particle excitations), we calculate the absorption spectra by solving the BSE, which uses GW quasiparticle energies as inputs and includes excitonic effect. Details of numerical convergence tests can be found in SI Section II. Here only spin-conserved transitions are considered. We then calculate the radiative lifetimes of the intra-defect recombination via Fermi’s golden rule by the Eq. (2) (with dielectric constant equal to unity for monolayer 2D systems),

Figure 2. (a) Single-particle diagram of the ground state at the level of GW@PBE, and (b) GW/BSE@PBE of CC. VBM and CBM are -7.431 eV and -0.400 eV, respectively [60]. The defect states in the band gap are denoted by the irreducible representations of C symmetry group based on corresponding wavefunction symmetry. The isosurface of the wavefunctions (PBE) is 3% of the maximum. In the GW/BSE@PBE spectra, the absorption peaks are labeled by the corresponding intra-defect transitions. x and y are the in-plane directions that are perpendicular and parallel to the C axis, respectively, and z is the out-of-plane direction. The spectral broadening is 0.02 eV.
where is the excitation energy, and is modulus square of exciton dipole moment in atomic units. The derivation detail of this equation can be found in Ref. 33, 57. We find two strong absorption peaks due to the optically allowed intra-defect transitions in Figure 2(b) and summarize the optical properties in TABLE II. In particular, only the transition shows a relatively short radiative lifetime that possibly falls into the range of experimental values. The other transition has an order of magnitude longer radiative lifetime. Therefore, we mainly focus on the former transition. Its shorter lifetime (i.e. 51.9 ns) is because of stronger oscillator strength and higher excitation energy (shown in Table II). Note that the excitonic effect at the defect is comparable or stronger than its host materials [58, 59], e.g. over one eV exciton binding energy for both transitions in Table II. The exciton wavefunction in SI FIG. S3 shows that the exciton is localized and bound to the carbon defect CCN and a few neighboring BN atoms, consistent with its large exciton binding energy. In order to compare with the experimental PL lifetimes in TABLE I, we also need to compute nonradiative lifetime as follows.
| Transition | (eV) | (a.u.) | (ns) | (eV) |
| 1.34 | 2.21 | |||
| 2.33 | 1.43 | 1.76 |
Table 2. Radiative recombination of CC. Excitation energy (), square modulus of dipole moment (), radiative lifetime (), and exciton binding energy () of the CC defect for the two transitions that are prominent in the optical excitations below the optical gap.
Nonradiative Recombination
Nonradiative lifetime () is a measure of how fast the nonradiative recombination happens between the final state and initial state . The phonon-assisted nonradiative recombination is influenced by several factors and also evaluated via Fermi’s golden rule as below,
where is the electron-phonon coupling Hamiltonian, is the degeneracy factor of the final state that depends on the number of equivalent atomic configurations, and is the occupation number of the vibronic state following Boltzmann distribution.
Under the static coupling approximation with one-dimensional (1D) phonon approximation [38, 55], we can rewrite Eq. (3) as
Eq. 4 is separated into the electronic term () that depends on the electronic wavefunction () overlap, and the phonon term () that describes the strength of phonon contribution. The phonon term includes the energy conservation between initial and final vibronic states with vibrational frequencies of and , and is the phonon wavefunction. The detailed derivation can be found in Ref. 38, 55.
We summarize the nonradiative recombination lifetime of the intra-defect transitions, along with ZPL, HR factor of the final state ((1D)) in TABLE III. Note that the HR factor from the nonradiative recombination calculation is with 1D effective phonon approximation. Its comparison with the full-phonon HR factor (, including all phonon eigenmodes) can be found in SI Section V. The calculated 1D HR factor is close to the full-phonon HR factor as can be seen by comparing Table III (1D) with Figure 3 (full phonon). ZPL is evaluated by two methods: one is using the vertical neutral excitation energy obtained from BSE with subtracting the Frank-Condon shift in the excited state (ZPL(BSE)), and another is from constrained DFT (CDFT) at the PBE level with geometry optimization (ZPL(CDFT)). The ZPL from two methods has 0.1 and 0.4 eV energy difference for the first two transitions, respectively. We used the CDFT in the nonradiative lifetime calculation to be consistent with other quantities in the equation. The nonradiative recombination of is fast due to the following reason. The electronic term of is large because it is symmetry-allowed, about four orders of magnitude larger than the other two transitions. Since is inversely proportional to the square of according to Eq. (4), difference of dominates over phonon contribution in . The nonradiative lifetime of (2.29 ns) is several orders shorter than other two transitions.

Figure 3. Multiplet structure and important physical parameters of CCN in hBN. is the ground state, and and are the excited states. The red solid lines denote radiative recombination and the blue dashed lines denote nonradiative recombination. is the HR factor with full phonon calculations. and are the radiative lifetime and nonradiative lifetime, respectively. and are the QY and PL lifetime, respectively.
| Transition | (eV) | ZPL(BSE) (eV) | ZPL(CDFT) (eV) | (amuÅ) | (meV) | (eV/(amuÅ)) | (amu·Å/eV) | ||
| 0.13 | 1.21 | 1.16 | 0.26 | 122 | 0.95 | ms | |||
| 0.20 | 2.13 | 1.70 | 0.27 | 145 | 1.26 | 2.29 ns | |||
| 0.01 | – | 0.55 | 0.19 | 128 | 0.67 | 3.20 s |
Table III. Properties of nonradiative recombination of the intra-defect transitions. The transitions are denoted using the multielectron wavefunction notations. The ZPL(BSE) are evaluated by subtracting the Franck-Condon shift () from the excitation energies from /BSE calculations. The ZPL(CDFT) are obtained by constrained DFT calculations at PBE level, which are used as the energy input for the nonradiative lifetime. is the nuclear coordinate change between the initial and final states. is the phonon energy of the final state. is the HR factor with 1D effective phonon approximation. and are the electronic and phonon terms, respectively. The nonradiative lifetimes are calculated with supercell at 300 K at PBE level. Here, is related to the transition in the single particle picture; transition is related to the transition ; transition is related to the transition .
PL Lifetime and Quantum Yield
Next we will compute PL lifetime and quantum yield [37] using radiative and nonradiative recombination lifetime from TABLE II and Table III, respectively. We list them along with the full-phonon HR factors calculated with the method in Ref. 56, and quantum yield () computed by Eq. (7) [61] in the multiplet diagram Figure 3.
where denotes the nonradiative pathway for the transition from the initial state. In addition, we calculate the PL lifetime which is the inverse of the total recombination rate by Eq. (8)
For transition , the nonradiative lifetime is nearly ten times shorter than the radiative lifetime. By including the nonradiative recombination , the overall recombination leads to the quantum yield of 4.23%, about 2% lower than the experimental quantum yield range 6∼12% [8]. More importantly, the PL lifetime of transition from Eq. (8) is calculated to be 2.19 ns, exactly within the experimental range of PL lifetimes (TABLE I and Figure 5(a)). In addition, the calculated full-phonon HR factor of this transition is 1.35, indicating weak electron-phonon interaction and good agreement with the experimental HR factor in TABLE I and Figure 5(b).
Figure 5. The calculated properties of CC along with the experimental values which are summarized in TABLE. I. (a) PL lifetime vs ZPL; (b) HR factor vs ZPL; (c) PSE vs ZPL; (d) comparison between the theoretical PL spectrum (this work) and the experimental PL spectrum (Exp) [13]. In (a), (b) and (c), the blue dots are for the experimental values of 2 eV single-photon emitters, the green dot is for the experimental PL lifetime of 20 ns, and the red dots are for the calculated values. The calculated ZPL here is from GW/BSE@PBE calculation. The comparison shows that ZPL, PL lifetime, HR factor and PSE are all in the experimental range. The calculated PL spectrum also matches well with the experimental PL of the 2 eV single-photon emission [13].
Phonon Modes of C2CN in hBN
To get more insights into electron-phonon coupling of CCN in hBN, we calculate the spectral function () of with the partial HR factor () of phonon mode as shown in Figure 4. The phonon modes spread over the range 0∼190 meV, and the phonon modes around 180 meV have the largest contribution to the spectral function. In particular, the 187 meV phonon mode has the largest partial HR factor among these modes. By visualizing this phonon mode shown by the inset in Figure 4, we find it to be an out-of-phase phonon mode. The atoms involved in this phonon mode include not only defect-related atoms but also many B and N atoms around and away from the defect. Hence, the 187 meV phonon mode is quasi-local. To quantitatively characterize the localization of dominant phonon modes, we estimate the number of atoms involved in the vibration of a phonon mode, by projection of inverse participation ratio (IPR) on this phonon mode [56],
Figure 4. Spectral function that shows the distribution of phonon modes and the contribution of phonon modes to the electron-phonon interaction of CC defect in hBN. The left vertical axis and black solid line are for the spectral function, and the right vertical axis and red dots are for the partial HR factor as a function of phonon energy. The inset figures are the low energy phonon mode (60 meV) and dominant phonon mode (187 meV) of CC for transition . The red arrows show the atom displacement of the corresponding phonon modes.
where is a normalized vector that describes the displacement of the atom along the direction in the phonon mode between the initial and final states. We then estimate the localization of the phonon mode by the localization ratio ,
where NAT stands for the total number of atoms in the supercell. The larger the localization ratio is, the more localized the phonon mode is. We find that the IPR of the 187 meV phonon mode is 46 for the 6x6 supercell calculation, and the localization ratio is 2. The IPR of this mode increases as a function of supercell sizes, but the localization ratio keeps constant, as can be seen in the SI TABLE S4. This again reflects the nature of this mode being a mixture of defect and bulk phonons or a “quasi-local” mode. Besides the 187 meV phonon, the 60 meV phonon is pronounced in the low-energy range of the spectral function, as an in-phase phonon mode (see the inset in Figure 4). It also has a large IPR of 48 and of 2. Comparing the calculated phonon mode energies with the experimental ones for 2eV single-photon emitters [62] [7], the 187 meV phonon mode is in good agreement with the 180 meV longitudinal optical phonon that leads to the pronounced PSB.
Comparison between C2CN defect and Experiments
To further validate that CC is a possible candidate of experimentally observed single-photon emitters, we calculate the PL of CC for transition and compare it with the PL spectra of 2 eV SPEs [13] in Figure 5. The details of the PL calculation can be found in SI Section V. The calculated PL shows similar PSB peaks to the experimental PL [13], as can be seen in Figure 5(d). A weak PSB peak next to the first PSB peak can be seen in both calculated and experimental PL spectra. This peak has been found to be more visible when the brightness is enhanced in an as-prepared array [62]. In addition, phonon-sideband energy can be a measure of the averaged phonon energy, found to be 180 meV, within the experimental range in TABLE I and Figure 5(c). The excellent agreement between the calculated and experimental physical parameters including ZPL, PL lifetime, HR factor, PSE and PL spectrum strongly suggest that the CC defect is one possible source of 2 eV single-photon emission. Finally, we note that the variation in experimental results shown in TABLE I can be from several sources of single-photon emitters and possible internal strains due to material preparation. Further defect identification including spin related properties can be through calculations of optically detected magnetic resonance (ODMR), which measures the spin-dependent optical contrast and is directly related to the information readout of spin qubits [63].
Conclusions
In conclusion, we investigated the possibilities of carbon defects for 2 eV single photon emission in hBN, by comparing key physical properties from first-principles calculations with experiments, including ZPL, PL lifetime and lineshape, as well as HR factor. We showcase the importance of considering multiple key signatures including both static and dynamical properties when identifying defects through theory and experimental comparison. We found CC has the best agreement with experiments on all concerned properties. In particular, we show the radiative lifetime can be an order longer than the experimentally observed PL lifetime; but after including nonradiative processes, the agreement with experimental PL lifetime is excellent. We show the electron-phonon coupling in CC is moderate with small HR factor and the dominant phonon mode at 180 meV is quasi-local with significant participation of bulk atoms. Our work provides insight into the 2 eV single-photon emission from the theoretical perspective, which is important for unraveling the unknown chemical nature of defects in hBN, manipulating defects and developing quantum applications.
Acknowledgments
We acknowledge the support by the National Science Foundation under grant no. DMR-1760260. This research used resources of the Scientific Data and Computing center, a component of the Computational Science Initiative, at Brookhaven National Laboratory under Contract No. DE-SC0012704, the lux supercomputer at UC Santa Cruz, funded by NSF MRI grant AST 1828315, the National Energy Research Scientific Computing Center (NERSC) a U.S. Department of Energy Office of Science User Facility operated under Contract No. DE-AC02-05CH11231, the Extreme Science and Engineering Discovery Environment (XSede) which is supported by National Science Foundation Grant No. ACI-
References
- [27]G. Grosso, H. Moon, C. J. Ciccarino, J. Flick, N. Mendelson, L. Mennel, M. Toth, I. Aharonovich, P. Narang, and D. R. Englund, Low-temperature electron–phonon interaction of quantum emitters in hexagonal boron nitride, ACS Photonics 7, 1410 (2020).arxiv.org/abs/1910.02053
- [28]E. Neu, D. Steinmetz, J. Riedrich-Möller, S. Gsell, M. Fischer, M. Schreck, and C. Becher, Single photon emission from silicon-vacancy colour centres in chemical vapour deposition nano-diamonds on iridium, New J. Phys. 13, 025012 (2011).
- [29]K. Konthasinghe, C. Chakraborty, N. Mathur, L. Qiu, A. Mukherjee, G. D. Fuchs, and A. N. Vamivakas, Rabi oscillations and resonance fluorescence from a single hexagonal boron nitride quantum emitter, Optica 6, 542 (2019).
- [31]A. W. Schell, H. Takashima, T. T. Tran, I. Aharonovich, and S. Takeuchi, Coupling quantum emitters in 2d materials with tapered fibers, ACS Photonics 4, 761 (2017).
- [32]A. L. Exarhos, D. A. Hopper, R. N. Patel, M. W. Doherty, and C. L. Bassett, Magnetic-field-dependent quantum emission in hexagonal boron nitride at room temperature, Nat. Commun. 10, 1 (2019).
- [33]F. Wu, D. Rocca, and Y. Ping, Dimensionality and anisotropy dependence of radiative recombination in nanostructured phosphorene, J. Mater. Chem. C 7, 12891 (2019).
- [34]D. Yim, M. Yu, G. Noh, J. Lee, and H. Seo, Polarization and localization of single-photon emitters in hexagonal boron nitride wrinkles, ACS Appl. Mater. Interfaces 12, 36362 (2020).
- [35]O. L. Krivanek, M. F. Chisholm, V. Nicolosi, T. J. Pennycook, G. J. Corbin, N. Dellby, M. F. Murfitt, C. S. Own, Z. S. Szilagyi, M. P. Oxley, et al., Atom-by-atom structural and chemical analysis by annular dark-field electron microscopy, Nature 464, 571 (2010).
- [36]A. Sajid and K. S. Thygesen, VncB defect as source of single photon emission from hexagonal boron nitride, 2D Mater. 7, 031007 (2020).
- [37]M. E. Turiansky and C. G. Van de Walle, Impact of dangling bonds on properties of h-bn, 2D Mater. 8, 024002 (2021).
- [38]F. Wu, T. J. Smart, J. Xu, and Y. Ping, Carrier recombination mechanism at defects in wide band gap two-dimensional materials from first principles, Phys. Rev. B 100, 081407 (2019).
- [39]C. Jara, T. Rausch, S. Botti, M. A. Marques, A. Norambuena, R. Coto, J. Castellanos-Aguila, J. R. Maze, and F. Munoz, First-principles identification of single photon emitters based on carbon clusters in hexagonal boron nitride, J. Phys. Chem. A 125, 1325 (2021).
- [40]G. Cheng, Y. Zhang, L. Yan, H. Huang, Q. Huang, Y. Song, Y. Chen, and Z. Tang, A paramagnetic neutral cbvn center in hexagonal boron nitride monolayer for spin qubit application, Comput. Mater. Sci. 129, 247 (2017).
- [41]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, I. Dabo, A. Dal Corso, S. de Gironcoli, S. Fabris, G. Fratesi, R. Gebauer, U. Gerstmann, C. Gougoussis, A. Kokalj, M. Lazzeri, L. Martin-Samos, N. Marzari, F. Mauri, R. Mazzarello, S. Paolini, A. Pasquarello, L. Paulatto, C. Sbraccia, S. Scandolo, G. Sclauzero, A. P. Seitsonen, A. Smogunov, P. Umari, and R. M. Wentzcovitch, QUANTUM ESPRESSO: A Modular and Open-Source Project for Quantum Simulations of Materials., J. Phys.: Condens. Matter 21, 395502 (2009).DOI
- [42]D. R. Hamann, Optimized Norm-Conserving Vanderbilt Pseudopotentials, Phys. Rev. B 88, 085117 (2013).DOI
- [44]T. J. Smart, K. Li, J. Xu, and Y. Ping, Intersystem Crossing and Exciton–Defect Coupling of Spin Defects in Hexagonal Boron Nitride, npj Comput. Mater. 7, 59 (2021).arxiv.org/abs/2009.02830
- [47]R. Sundararaman, K. Letchworth-Weaver, K. A. Schwarz, D. Gunceler, Y. Ozhabes, and T. Arias, JDFTx: software for joint density-functional theory, SoftwareX 6, 278 (2017).DOI
- [48]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
- [49]A. Marini, C. Hogan, M. Grüning, and D. Varsano, Yambo: An ab initio tool for excited state calculations, Comput. Phys. Commun. 180, 1392 (2009).DOI
- [50]F. Fuchs, J. Furthmüller, F. Bechstedt, M. Shishkin, and G. Kresse, Quasiparticle band structure based on a generalized kohn-sham scheme, Phys. Rev. B 76, 115109 (2007).DOI
- [51]F. Bechstedt, Many-Body Approach to Electronic Excitations (Springer-Verlag: Berlin, 2016).DOI
- [52]R. W. Godby and R. Needs, Metal-insulator transition in kohn-sham theory and quasiparticle theory, Phys. Rev. Lett. 22, 1169 (1989).pubmed.ncbi.nlm.nih.gov/10039594
- [53]A. Oschlies, R. Godby, and R. Needs, Gw self-energy calculations of carrier-induced band-gap narrowing in n-type silicon, Phys. Rev. B 51, 1527 (1995).pubmed.ncbi.nlm.nih.gov/9978867
- [54]C. A. Rozzi, D. Varsano, A. Marini, E. K. Gross, and A. Rubio, Exact coulomb cutoff technique for supercell calculations, Phys. Rev. B 73, 205119 (2006).DOI
- [55]A. Alkauskas, Q. Yan, and C. G. Van de Walle, First-principles theory of nonradiative carrier capture via multiphonon emission, Phys. Rev. B 90, 075202 (2014).DOI
- [56]A. Alkauskas, B. B. Buckley, D. D. Awschalom, and C. G. Van de Walle, First-principles theory of the luminescence lineshape for the triplet transition in diamond nv centres, New J. Phys. 16, 073026 (2014).DOI
- [58]C. Guo, J. Xu, and Y. Ping, Substrate effect on excitonic shift and radiative lifetime of two-dimensional materials, J. Phys. Condens. Matter 33, 234001 (2021).DOI
- [59]C. Attaccalite, M. Bockstedte, A. Marini, A. Rubio, and L. Wirtz, Coupling of excitons and defect states in boron- nitride nanostructures. Phys. Rev. B 83, 144115 (2011).
- [60]T. J. Smart, F. Wu, M. Govoni, and Y. Ping, Fundamental principles for calculating charged defect ionization energies in ultrathin two-dimensional materials, Phys. Rev. Mater. 2, 124002 (2018).DOI
- [61]L. Novotny and B. Hecht, Principles of Nano-Optics (Cambridge university press, 2012).
- [62]J. A. Preuß, E. Rudi, J. Kern, R. Schmidt, R. Bratschitsch, and S. M. de Vasconcellos, Assembly of large hbn nanocrystal arrays for quantum light emission, 2D Mater. 8, 035005 (2021).DOI
- [63]P. Auburger and A. Gali, Towards ab initio identification of paramagnetic substitutional carbon defects in hexagonal boron nitride acting as quantum bits, Phys. Rev. B 104, 075410 (2021).DOI