betaFeedback

WorksPhysics and Astronomy

Origin of Flat Bands and Role of Electron Correlation in Lutetium Hydrides

Abstract

Lutetium hydrides (LuHx_x, 1.75≤x≤31.75 \leq x \leq 3) form a diverse series of phases, several of which superconduct under pressure. Characterizing their electronic properties has remained challenging owing to a high propensity for hydrogen defect formation, and recent angle-resolved photoemission (ARPES) measurements reveal puzzling flat-band regions that position these materials as candidates where superconductivity and flat-band physics may intersect. Here, by combining density functional theory, dynamical mean-field theory, and the constrained random-phase approximation, we uncover the microscopic origin and correlation nature of these flat bands. Across all compositions, the screened on-site Coulomb interaction is larger for H-s states than for Lu-dd states due to compact hydrogen orbitals. Nevertheless, these systems remain weakly correlated metals: the nearly filled H-ss shell admits little charge fluctuation, so its large interaction acts as a static level shift rather than a source of correlation. Although hydrogen primarily occupies tetrahedral sites at x=2x=2, we discover that anti-site defects–where hydrogens occupy slightly unfavorable octahedral sites–generate both the ARPES flat-band features and the low-energy optical absorption peak, attesting to the usual defective nature of such materials in experimental samples. We further find that correlation strength is governed primarily by hydrogen orbital filling at these sites rather than the interaction magnitude itself. Consequently, we identify hydrogen orbital filling as the fundamental organizing principle dictating correlation and low-energy flat-band physics in lutetium hydrides.

Introduction

Many metal hydrides are well described within conventional band theory, as the metal-derived electrons are mostly itinerant and they effectively screen the hydrogen states. The coupled electronic, structural and phonon properties of stoichiometric and non-stoichiometric lanthanide hydrides have been a puzzling topic of study for over half century. Motivated by the argument of Matthias [1], Merriam and Schreiber [2] searched for superconductivity in lanthanum hydrides to below 1 K. Two decades later, a sub-kelvin TcT_c for LaH2\mathrm{LaH}_2 was estimated based on Bardeen–Cooper–Schrieffer (BCS) theory [3]. This superconductivity was ultimately confirmed [4] in slightly supersoichiometric LaH2+x\mathrm{LaH}_{2+x}. A growing body of later work suggested that certain rare-earth hydrides exhibit behavior beyond the standard band-theory description, including electron–electron correlation effects and correlation-driven metal–insulator transitions.[5, 6, 7, 8] This beyond-band-theory behavior originates in hydrogen lattice itself: a periodic array of such correlation-stabilized ions is a genuine many-body problem exhibiting metallic, intermediate, and Mott-insulating regimes [9], and correlation-based treatments have accordingly cast LaH3/YH3\mathrm{LaH}_3/\mathrm{YH}_3 as correlation-driven insulators [10, 11], with hydrogen ordering proposed as an additional contributing factor [12, 13].

Lutetium hydride is a particularly clean system in which to test these ideas. Its filled 4f4f shell removes the ff-electron correlation that complicates the lighter rare earths, isolating the hydrogen and Lu\mathrm{Lu}-5d5d states as the only candidates for correlated behavior; and its accessible dihydride–trihydride range spans hydrogen fillings from the tetrahedral-only dihydride to the octahedrally-filled trihydride, allowing the hydrogen occupation to be tuned systematically. Weaver et al. [14] measured optical reflectance spectra that established the dominance of Drude absorption and yielded the carrier plasma frequency, while synchrotron photoemission resolved the Lu-dd conduction states near the Fermi level and a H-ss band several eV below it, providing evidence for charge transfer from the lutetium conduction (5d/6s5d/6s) manifold to the hydrogen site [15]. The same measurements locate the filled Lu 4f4f levels as sharp features near −8-8 eV; being a closed, chemically inert shell, the 4f4f states do not participate in the bonding with hydrogen but distinguish lutetium from lanthanum, whose empty 4f4f shell underlies the larger lanthanum lattice constant. The electronic structure of the lutetium dihydride has been characterized experimentally: angle-resolved photoemission on Lu–H–N have been interpreted as indicating a flat band ∼0.2\sim0.2 eV below the Fermi level [?], which has been suggested to reflect strong correlation; whether the near-EFE_F flat band is genuinely correlation-driven, however, remains an open question.

Further, theoretical studies of Sufyan and Larson [?] report that pristine LuH3\mathrm{LuH}_3, in its trigonal structure, hosts nontrivial topological features and van Hove singularities near the Fermi level, and Denchfield et al. [?] show that specific substitutions of nitrogen in the hydrogen sublattice generates flat bands and sharply peaked densities of states.

We show that electronic correlation in the rare-earth hydrides is governed by hydrogen occupation rather than interaction strength — the central result of this work, and one that inverts the usual expectation. Throughout, we use correlation strength to mean the magnitude of many-body renormalization of the one-particle properties, quantified by the mass enhancement m∗/m=1/Zm^{*}/m = 1/Z and by the local spin susceptibility χS\chi_{S} and instantaneous moment ⟨m2⟩\langle m^{2}\rangle; we reserve interaction strength for the magnitude of the screened on-site UU and JJ obtained from cRPA. The two need not track one another, and in these materials they do not: hydrogen carries large cRPA interaction yet remains the weakly renormalized site. Moreover, two hydrogen sublattices are electronically inequivalent, with octahedral hydrogen the more strongly hybridizing of the two, and we find that specific arrangements of tetrahedral vacancies and octahedral occupancies give rise to narrow bands and van Hove singularities near EFE_{F}.

The remainder of this paper is organized as follows. Section II presents the results: the electronic inequivalence of the tetrahedral and octahedral hydrogen sublattices, the mass enhancements and local moments obtained from DMFT, the DFT and DMFT densities of states, the effects of octahedral occupancy and hydrogen vacancies, and comparison with experiment. Section III discusses the origin of the hydrogen filling and its relation to the observed renormalization, and compares our results with spectroscopic measurements on lutetium and other lanthanide hydrides. The paper concludes with a summary of how hydrogen occupation controls the strength of correlation effects in rare-earth hydrides.

Results

Inequivalent Tetrahedral and Octahedral Hydrogen Sublattices

All LnHx_{x} structures considered here (Ln = Lu, La) are built on the cubic fluorite (CaF2_{2}-type) framework, space group Fm3ˉmFm\bar{3}m. The metal atoms form a face-centered cubic (FCC) sublattice on the 4a4a sites, and hydrogen occupies the tetrahedral 8c8c sites, each coordinated by four metal atoms. This accounts for two hydrogen per formula unit, giving the dihydride LnH2_{2}. The remaining octahedral interstitial, the 4b4b site and coordinated by six metal atoms, is vacant in the ideal fluorite structure; progressive filling of this site carries the composition from x=2x = 2 toward the trihydride LnH3_{3}, in which both hydrogen sublattices are fully occupied. We begin by asking whether the two hydrogen sublattices in LnH3_{3} are electronically equivalent. Figure 1 shows the model structure for LuH3_{3}, with tetrahedral hydrogen (Htet_{\mathrm{tet}}) in pink and octahedral

Idealized fluorite structure of LuH3

Figure 1. Idealized fluorite structure of LuH3_{3}. Tetrahedral hydrogens (Htet_{\mathrm{tet}}) are represented by pink atoms, octahedral hydrogens (Hoct_{\mathrm{oct}}) are represented by blue atoms and Lutetium atoms are represented by turquoise atoms.

hydrogen (Hoct_{\mathrm{oct}}) in blue.

To characterize the two hydrogen sites electronically, we extracted their on-site energies, for LnH3_{3}, from the diagonal elements of the Wannier Hamiltonian (Table 1). The tetrahedral and octahedral hydrogen sublattices are found to be electronically inequivalent, differing substantially in their on-site energies (Table 1). For LuH3_{3}, the tetrahedral H-ss level lies 0.97 eV below the octahedral H-ss level, with both situated well below the Fermi level. The Lu-dd on-site energies, by contrast, lie above EFE_{F}, split by the crystal field into two sets at ϵ−EF≈+2.1\epsilon- E_{F} \approx+2.1 and +3.8+3.8 eV, well separated from the hydrogen manifold. The tetrahedral hydrogen, fully coordinated and filled already in the dihydride, is the more strongly bound and more deeply lying species; the octahedral hydrogen—the “extra” hydrogen added on going from the di- to the trihydride—is more weakly bound and sits closer to EFE_{F}.

The ordering is reversed in LaH3_{3}, where the octahedral level lies 0.38 eV below the tetrahedral one. The two compounds differ substantially in lattice constant (5.01 versus 5.65 Å), and the octahedral interstitial, being the larger and less tightly confined site, is expected to be the more sensitive of the two to this difference; the reversal is consistent with the site-resolved occupations, which show the octahedral hydrogen to be the more filled species in LaH3_{3} and the less filled one in LuH3_{3}. We do not attempt to separate the geometric effect from possible chemical differences between the two rare earths.

Cubic trihydrides: interactions do not open the gap

LaH3_{3} and YH3_{3} are semiconductors [5], whereas standard band theory predict these trihydrides to be metallic; hydrogen ordering [12, 13] and electronic correlation [10, 11] have both been proposed as the missing ingredient to open the band gap. Figure 2 tests the correlation scenario directly.

Orbital-resolved density of states of LuH3 and LaH3 for three interaction strengths

Figure 2. Hubbard interactions alone do not gap the cubic trihydrides. Orbital-resolved DOS of LuH3_3 (left) and LaH3_3 (right) at the Wannier level (U=0U = 0, top), from DMFT at the cRPA couplings (middle), and from DMFT with Ud=8U_d = 8 eV at fixed hydrogen interactions (bottom).

At the Wannier level (U=0U = 0, top row) LuH3_3 and LaH3_3 are low-density-of-states metals: EFE_F lies in a shallow minimum with N(EF)=0.02N(E_F) = 0.02 and 0.0020.002 states/eV respectively, produced by residual overlap between the H-derived valence weight and the RE-dd conduction manifold, and part of the H-ss weight remains unoccupied.

Applying correlation at the cRPA couplings (middle row) rearranges the spectrum substantially. The static, orbital-dependent shift of Re⁡Σ(0)−Vdc\operatorname{Re}\Sigma(0) - V^{\mathrm{dc}} drives the occupied H-derived weight below −4-4 eV and removes the unoccupied H-ss admixture, leaving a wide region of negligible spectral weight beneath EFE_F. Both compounds nonetheless remain metallic: the EFE_F is just above the dd conduction manifold with the total density of states N(EF)=0.13N(E_F) = 0.13 and 0.270.27 states/eV and a finite dd occupation nd=0.68n_d = 0.68 per rare earth atom. Raising UdU_d to 8 eV, nearly twice the cRPA value (bottom row), leaves this unchanged, only shifting the d−d- states below EFE_F by a little amount due to the remaining unoccupied H orbitals.

The occupations identify this orbital dependent correlation effect. Hydrogen is a nearly filled shell (nH=1.8n_H = 1.8–1.91.9) and the dd manifold is nearly empty (nd=0.5n_d = 0.5–0.70.7 of ten spin-orbitals); the insulating state these compounds are expected to reach is therefore the ionic RE3+^{3+}(H−^-)3_3 band insulator, requiring nH→2n_H \to2 and nd→0n_d \to0. The two dd sets are themselves well separated: in LuH3_3 the ege_g doublet lies at ϵ−EF=+2.08\epsilon- E_F = +2.08 eV and the t2gt_{2g} triplet at +3.81+3.81 eV, and in LaH3_3 at +1.75+1.75 and +2.75+2.75 eV respectively. The ege_g set therefore lies below t2gt_{2g} in both compounds—the inverse of the familiar octahedral ordering, and the expected result for the eight-fold cubic coordination of the metal by tetrahedral hydrogen in the fluorite structure.

Hubbard interactions push the system toward the insulator limit but cannot complete the charge transfer, because the residual dd occupation is sustained by the strong ss–dd hybridization. Doubling UdU_d accordingly changes nothing. It however is possible to open the gap through distorting the hydrogen sublattice, consistent with DFT+UU and quantum Monte Carlo results in which hydrogen distortions open a small gap that interactions subsequently enlarge [?]—which motivates the vacancy-

and occupancy-resolved analysis of the following sections.

Correlation and Vacancy Effects

We now consider the electronic structure of LuHx_x at five compositions, x=1.75x = 1.75, 2, 2.25, 2.875, and 3. The compositions studied here therefore span partial vacancy of the tetrahedral sublattice below x=2x = 2 and partial filling of the octahedral sublattice above it. Figure 3 shows the DFT-relaxed structures for the compositions considered, together with their band structures and densities of states; the sub-stoichiometric compounds, in which tetrahedral sites are partially vacant, develop flat bands immediately below the Fermi level. The DFT-optimized lattice parameters and the cRPA interaction parameters for all compositions are given in Sections S2.1 and S2.2, respectively.

Lu-H structures with different hydrogen occupation and their associated DFT-calculated electronic properties

Figure 3. Lu-H structures with different hydrogen occupation of HoctH_{\mathrm{oct}} and HtetH_{\mathrm{tet}} studied and their associated DFT calculated electronic properties. For 4 Lu atoms: a) LuH1.75_{1.75} has 7 HtetH_{\mathrm{tet}}. b) LuH2_2 has 8 HtetH_{\mathrm{tet}}. c) LuH2.25_{2.25} has 8 HtetH_{\mathrm{tet}} and 1 HoctH_{\mathrm{oct}}. d) LuH2.875_{2.875} has 8 HtetH_{\mathrm{tet}} and 3 HoctH_{\mathrm{oct}}. e) LuH3_3 has 8 HtetH_{\mathrm{tet}} and 4 HoctH_{\mathrm{oct}}.

Across the LuHx_x series the hydrogen ss shell is close to being fully filled at both sites (n=1.72n = 1.72–1.851.85), consistent with an H−^--like anion, but it is not a closed shell: the deficit from n=2n = 2 is recovered almost exactly as excess dd occupation (Table 18, r=0.99r = 0.99), establishing that the two sublattices are hybridized rather than ionically decoupled. The hydrogen sublattices are themselves re-

ChannelQuantity−1e-1eundoped+1e+1e
Lu-ddnn1.1581.4171.670
Lu-ddχS\chi_S0.15130.21080.2346
Lu-ddχD\chi_D0.03750.03890.0391
Lu-ddχS/χD\chi_S/\chi_D4.045.426.01
Htet_{\mathrm{tet}}nn1.8491.8481.847
Htet_{\mathrm{tet}}χS\chi_S0.00450.00450.0046
Htet_{\mathrm{tet}}χD\chi_D0.00400.00400.0041
Htet_{\mathrm{tet}}χS/χD\chi_S/\chi_D1.121.131.13
Hoct_{\mathrm{oct}}nn1.7251.7201.720
Hoct_{\mathrm{oct}}χS\chi_S0.01250.01290.0130
Hoct_{\mathrm{oct}}χD\chi_D0.00960.00980.0099
Hoct_{\mathrm{oct}}χS/χD\chi_S/\chi_D1.301.311.31

Table 18. Response of the correlated subspace to rigid-band doping in LuH2_2 (7 tet + 1 oct). One electron is added to (+1e) or removed from (−1e) the total electron count in the DMFT step at fixed structure, corresponding to ±5%\pm5\% doping. Occupations nn and local spin and charge susceptibilities χS\chi_S, χD\chi_D from the CTQMC solver at β=50 eV−1\beta=50\ \mathrm{eV}^{-1}. χS\chi_S is a total-shell quantity and is therefore not directly comparable between the five-orbital dd manifold and the single-orbital hydrogen sites.

solvably inequivalent. At every composition containing octahedral hydrogen, noct=1.72n_{\mathrm{oct}} = 1.72–1.761.76 and ntet=1.80n_{\mathrm{tet}} = 1.80–1.851.85, which follows directly from the on-site energies of Sec. II A: the shallower octahedral level is less completely occupied than the deeper tetrahedral one.

Despite the predominantly closed-shell character, residual charge fluctuations are substantial: Pdouble=0.73P_{\mathrm{double}} = 0.73–0.850.85, which corresponds to non-closed-shell configuration 15–27% of the time. The associated instantaneous moment reaches ⟨m2⟩=0.26\langle m^2 \rangle= 0.26 for the octahedral sites, versus 0.145–0.19 on tetrahedral ones. For a single orbital these are not independent diagnostics: ⟨m2⟩=2−n−2Pempty\langle m^2 \rangle= 2 - n - 2P_{\mathrm{empty}} identically, and with Pempty<0.012P_{\mathrm{empty}} < 0.012 throughout, the moment is a direct readout of the charge deviation from the ionic limit. Local charge and spin fluctuations therefore measure the hybridization strength site by site, and are largest where the on-site level lies closest to EFE_F.

The hydrogen mass enhancement increases systematically with octahedral occupation. At the tetrahedral site it rises monotonically from m∗/m=1.20m^*/m = 1.20 in LuH1.75_{1.75} through 1.22 in LuH2_2 and 1.29 in LuH2.875_{2.875} to 1.34 in LuH3_3, and the octahedral site reaches 1.36 in LuH3_3. These values of mass enhancement are comparable to the kagome metal ScV6_6Sn6_6 (m∗/m≈1.3m^*/m \approx1.3) [?] and well below the value for moderately correlated oxides such as SrVO3_3 (m∗/m≈2m^*/m \approx2) [?].

The Lu-dd manifold is similarly weakly correlated but follows a different trend. Its occupation decreases monotonically with hydrogen content, from nd=1.59n_d = 1.59 in LuH1.75_{1.75} to 0.68 in LuH3_3, as hydrogen withdraws charge from the dd band. The dd mass enhancement, however, is non-monotonic: it peaks near the dihydride (m∗/m≈1.28m^*/m \approx1.28–1.321.32 for LuH2_2) and decreases toward the trihydride (1.16–1.18 in LuH3_3). The two crystal-field-split dd-sets track each other closely at all compositions.

The local susceptibilities distinguish the two channels more sharply than the static moments alone. The instantaneous moment measures the magnitude of the local moment at a given instant; the local spin susceptibility χS\chi_S additionally weights its persistence in imaginary time, and their ratio therefore measures how long-lived the moment is relative to its size. For hydrogen this ratio is χS/⟨m2⟩≈0.032\chi_S/\langle m^2 \rangle\approx0.032 at tetrahedral sites but 0.046–0.050 at octahedral sites: the octahedral moment is not merely larger but also longer-lived per unit moment. As we show below, this distinction is not incidental: octahedral and tetrahedral H sites occupy geometrically distinct positions relative to the Lu dd orbitals, and this governs which dd channel each couples to.

The spin and charge susceptibilities are moreover nearly equal on hydrogen (χS/χD=1.1\chi_S/\chi_D = 1.1–1.31.3 at every site and composition), the signature of a site whose fluctuations are hybridization-driven rather than moment-forming, since local-moment behavior requires charge fluctuations to be suppressed relative to spin fluctuations. The dd shell behaves differently: χS/χD\chi_S/\chi_D falls from 4.6–5.4 near the dihydride to 1.7–1.9 at the trihydride, and χS\chi_S itself collapses by a factor of four across the same range, tracking the emptying of the dd band. The dd manifold is thus moment-like — behaving as a localized, correlation-susceptible orbital — where it is close to half-filled, and becomes progressively itinerant or band-like as hydrogen withdraws its charge and the shell empties. Hydrogen, by contrast, remains itinerant and does not develop local-moment character at any composition, consistent with its H-ss band being governed by filling rather than by interaction strength. We note that χS\chi_S is reported here at a single temperature (β=50\beta= 50 eV−1^{-1}); distinguishing Curie from Pauli behavior would require its temperature dependence.

In the ideal fluorite structure the Lu site has OhO_h symmetry, and each hydrogen sublattice hybridizes with only one dd channel: tetrahedral H lies along ⟨111⟩\langle111\rangle, where the ss–ege_g two-center integrals vanish, and octahedral H along ⟨100⟩\langle100\rangle, where the ss–t2gt_{2g} integrals vanish [?]. Since the H-1s1s level lies well below EFE_F, the coupled dd set is pushed upward by antibonding repulsion while the uncoupled set is left unshifted. In the tetrahedral-only dihydride this raises t2gt_{2g} and leaves ege_g essentially nonbonding, so charge accumulates preferentially in ege_g: neg=0.49n_{e_g} = 0.49 against nt2g=0.12n_{t_{2g}} = 0.12. (At intermediate compositions the octahedral sublattice is partially occupied and the site symmetry is reduced, so the separation is only approximate; it is exact in stoichiometric LuH2_2 and LuH3_3.) Because the tetrahedral sublattice is occupied at every composition, the t2gt_{2g} environment is fixed across the series; only the octahedral sublattice varies, and it couples to ege_g alone. Adding additional hydrogen to the octahedral site therefore acts almost exclusively on the ege_g channel, which acquires a hybridization partner of its own and is pushed up in turn. The occupations bear this out: from LuH2_2 to LuH3_3, negn_{e_g} falls by a factor of four (0.49 →\to 0.12; 0.11 in LaH3_3) while nt2gn_{t_{2g}} is nearly unchanged (0.12 →\to 0.11), closing the imbalance from neg/nt2g≈4n_{e_g}/n_{t_{2g}} \approx4 to ≈1.1\approx1.1. Both sets remain far from the half-filled configuration norb=1n_{\mathrm{orb}} = 1 throughout. The composition dependence of the dd-shell occupations thus follows from hybridization geometry and filling rather than from any change in interaction strength.

The local spin susceptibility tracks the ege_g occupation across the series: the compositions with neg≳0.36n_{e_g} \gtrsim0.36 have χS=0.16\chi_S = 0.16–0.220.22, while those with neg≲0.19n_{e_g} \lesssim0.19 have χS=0.05\chi_S = 0.05–0.080.08. The dd-shell spin fluctuations therefore follow the filling of the ege_g channel that hydrogen depopulates, independently of any change in the interaction parameters. The trends above follow from changing the hydrogen content, which alters the filling and the hybridization geometry together. To separate the two we consider rigid-band doping at fixed structure, which changes the carrier count without touching either hydrogen sublattice (Table S10).

The correlated-subspace occupations show where the doped charge is accommodated (Table S10). Across the full ±5%\pm5\% range the Lu-dd occupation shifts by 0.51 electrons, while both hydrogen sites change by less than 0.005—below the resolution at which we quote them. The local susceptibilities behave the same way: χS\chi_S on the dd shell rises by 55% from hole- to electron-doping and its ratio to the charge susceptibility climbs from 4.0 to 6.0, whereas the hydrogen susceptibilities and their ratios are unchanged to within 3% at both sites. Doping therefore acts exclusively on the dd manifold; the hydrogen sublattices, including the more strongly hybridized octahedral site, are spectators. The two perturbations agree: whether the dd filling is changed chemically, by octahedral hydrogen, or rigidly, by doping, χS\chi_S on the dd shell follows the filling while the hydrogen sites do not respond.

The picture that emerges—a nearly filled but hybridized hydrogen shell, weak renormalization in both channels, and an octahedral environment (both the H site and the ege_g orbitals it couples to by symmetry) that is systematically the more strongly hybridized of the two coordination geometries—is one in which every site-resolved distinction traces back to occupation and orbital geometry rather than to interaction strength. This is the central claim of the present work in microscopic form, and it makes a direct prediction for the spectral function: features appearing near EFE_F should be one-body in origin and controlled by octahedral occupancy rather than by interaction strength. We test this against photoemission in the following section.

Electronic Structure, Correlated Spectral Function, and Optical Response

To trace the band-structure origin of the configurational dependence observed in the photoemission and optical response (Figure 5, 6,), we computed the electronic band structures of four representative LuHx_x configurations: (a) pure LuH2_2 with full tetrahedral occupancy, (b) LuH1.75_{1.75} with one tetrahedral H removed, (c) LuH2.25_{2.25} with one additional octahedral H, and (d) nominally LuH2_2 with one tetrahedral vacancy compensated by one octahedral occupant (see Figure 4).

Comparison of band structures and density of states for various LuHₓ structures

Figure 4. Comparision of band structures of various LuHx_x structures showing that flat-bands and van Hove singularity can be tuned near EFE_F. The band structures are for the following structures: (a) LuH2_2 with only tetrahedral-H occupancy (b) LuH1.75_{1.75} with one tetrahedral-H vacancy (c) LuH2.25_{2.25} with one octahedral-H occupancy (d) LuH2_2 with one tetrahedral-H vacancy and one octahedral-H occupancy.

Correlated electronic structure of LuH₂ with Hₒct: theory–experiment comparison

Figure 5. Correlated electronic structure of LuH₂ with Hₒct: theory–experiment comparison. Top: Wannier bands and DMFT spectral function A(k,ω)A(k,\omega) along Γ\Gamma–XX–MM, undoped and at ±5%\pm5\% carrier doping. Relative to the Wannier bands, DMFT produces a narrow band pinned near EFE_F with a saddle at MM, and damped flat features near −0.6-0.6 eV; doping shifts both rigidly in energy (electron doping downward, hole doping upward) without displacing them in momentum. Bottom: ARPES cuts adapted from [?], licensed under CC by 4.0, showing the near-EFE_F flat band with its emerging light band (left), compared with the undoped DMFT spectral function along MM–Γ\Gamma (middle) and the model structure of LuH₂ with Hₒct – teal atoms represent Lu, pink atoms represent Hₜₑₜ and blue atom represents Hₒct (right).

The pure LuH2_2 band structure (panel a) is the canonical fluorite-dihydride result: dispersive Lu-5d bands crossing EFE_F along Γ−X−M−Γ−R\Gamma-X-M-\Gamma-R, with H-derived weight confined well below the Fermi level. The two H-sublattice modifications produce distinct changes near EFE_F. Removing a tetrahedral H (panel d, LuH1.75_{1.75}) introduces a substantially narrow band approximately 0.2 eV below EFE_F along M−ΓM-\Gamma. Adding an octahedral H without removing a tetrahedral one (panel c, LuH2.25_{2.25}) shifts the band crossing at MM downward onto EFE_F, bringing a saddle-point-like feature into coincidence with the Fermi level. The combined configuration (panel b) exhibits both effects simultaneously: a weakly dispersive band near EFE_F inherited from the tetrahedral vacancy, and a van Hove-like feature at MM shifted onto EFE_F by the octahedral occupant.

The two effects therefore appear to act through different mechanisms. Tetrahedral vacancies introduce a localised defect-derived state whose narrow bandwidth reflects the loss of metal-hydrogen hybridization in the immediate vacancy environment. Octahedral occupants shift the Fermi level through electron donation while simultaneously perturbing the Lu-5d states they hybridize with, moving pre-existing dispersion features into coincidence with EFE_F. The combination yields enhanced density of states at the Fermi level relative to the pure dihydride.

The states introduced by tetrahedral vacancies and octahedral occupants are narrow, and it is for narrow bands that correlation can least safely be assumed away, U/WU/W being largest for precisely the weakly dispersing features these modifications place near EFE_F — and the ARPES flat band has itself been interpreted as a correlation feature [?]. Whether such a band is correlated in the many-body sense cannot be decided from the band structure alone, nor from a static Hubbard correction, which shifts levels but cannot distinguish a band reconstructed by a static self-energy from one narrowed by a small quasiparticle residue. We therefore turn to DMFT, which treats the frequency dependence of the self-energy explicitly.

Correlation neither removes nor shifts these features. The flat band at EFE_F and the feature ≈0.5\approx0.5 eV below it survive the inclusion of dynamical correlations essentially unchanged, so that both remain in agreement with the ARPES measurements, complementing the agreement already obtained for the optical conductivity. The self-energies underlying this conclusion, and their decomposition into static shift, mass renormalization and damping, are given in Section S4.

Figure 5 compares the Wannier bands of LuH2_2 containing octahedral hydrogen with the DMFT spectral function A(k,ω)A(k,\omega) along X−Γ−MX-\Gamma-M. Because both are built from the same Wannier Hamiltonian, every difference between them is attributable to the self-energy. Three effects are visible, and we keep them separate throughout.

The first and largest is static. The orbital-dependent Re⁡Σα(0)−Vd−α\operatorname{Re}\Sigma_\alpha(0)-V^{d-\alpha} repositions the hydrogen-derived states relative to the Lu-dd manifold, and where the resulting weakly dispersing level intersects bands of predominantly Lu-dd character, hybridization quenches their dispersion. The clearest consequence is along Γ−X−M\Gamma-X-M: a band that disperses appreciably in the Wannier spectrum becomes a narrow, nearly flat feature pinned close to the Fermi level. At MM this narrow band forms a saddle, hole-like along one in-plane direction and electron-like along the other, lying within a few tens of meV of EFE_F.

The second effect, dynamical mass renormalization, is comparatively weak. The Matsubara self-energies give m∗/m≲1.36m^*/m \lesssim1.36 for either of dd or ss orbitals, bounding the correlation-induced bandwidth reduction to at most ∼36%\sim36\%. The observed flattening of the near-EFE_F band substantially exceeds this bound, identifying it as a reconstruction of the band structure by the static, orbital-dependent part of the self-energy rather than as a mass-enhancement effect.

The third effect is damping. A second set of flat features appears near −0.6-0.6 eV, but with markedly lower intensity and larger energy width than the near-EFE_F band. These features are flat in the dispersive sense; what distinguishes them is lifetime, since ∣Im⁡Σ(ω)∣|\operatorname{Im}\Sigma(\omega)| grows away from the Fermi level and broadens them into low-intensity ridges. The narrow band near EFE_F remains sharp and intense by contrast, protected by the vanishing of Im⁡Σ\operatorname{Im}\Sigma at low frequency.

The ±5%\pm5\% doped spectra differ from the stoichiometric one by an essentially rigid displacement in energy. With each spectrum referenced to its own Fermi level, electron doping raises the chemical potential and the narrow band and its saddle appear at lower energy, moving further below EFE_F; hole doping shifts them upward toward and through EFE_F. No displacement in momentum accompanies these shifts, as required for a momentum-independent self-energy, and the dispersions, intensities and linewidths are unchanged within our resolution. Linear extrapolation of the saddle energy places it at the Fermi level for a hole doping of 5%5\%.

For the LuH2_2 with Hoct_{\mathrm{oct}} structure we also calculate the in-plane and out of plane energy distribution curves (EDC) and compare with EDC curves obtained from ARPES experiment (Figure S3). [?] The construction of such curves, which introduces no adjustable parameters beyond the experimental temperature, energy resolution, and escape-depth momentum broadening, is described in Section S4.3.

In-plane and out-of-plane energy-distribution curves comparing ARPES and DMFT

Figure S3. Correlated electronic structure of LuH2_2 with octahedral hydrogen: theory–experiment comparison. In-plane and out-of-plane energy-distribution curves, adapted from [6], licensed under CC by 4.0, and calculated. Both show a sharp, momentum-independent peak near EFE_F; deeper structure is dispersive in-plane and comparatively flat out-of-plane. Momenta are not registered between calculation and experiment throughout; the comparison is made on energies and band shapes only (see text).

In plane, a sharp maximum sits immediately below EFE_F at fixed energy across the cut, with deeper structure that shifts markedly from curve to curve—the distinction drawn in the measured curves between a flat band and the light band emerging from it, with the calculated near-EFE_F maximum at −50-50 meV against a measured flat-band binding energy of 00–0.20.2 eV. Out of plane, both show a stationary maximum just below EFE_F, persisting across photon energies spanning more than one Brillouin zone along kzk_z; in the calculation this peak is stationary to within 1010 meV over the full range. The calculation additionally resolves a second out-of-plane maximum near −0.6-0.6 eV, dispersing by 0.150.15 eV, which appears in the measurement not as a distinct peak but within the broad enhancement between −0.5-0.5 and −0.9-0.9 eV; we attribute this to momentum integration over the escape-depth window and to the ordered octahedral sublattice of our supercell, which produces coherent minibands where a disordered sample would show an incoherent resonance at the same energy (Sec. S4.3). The comparison is therefore one of feature count, approximate energy, and dispersive character; peak intensities are not compared, since the measured curves carry photoemission matrix elements and an inelastic background absent from A(k,ω)A(k,\omega). Likewise, the calculated DMFT DOS N(ω)N(\omega) for LuH2_2 with Hoct_{\mathrm{oct}} exhibits a pronounced peak at the Fermi level and a broad structure centred near −0.6-0.6 eV, separated by a shallow minimum (Figure S4). The Fermi-level peak is the density-of-states signature of the narrow band identified above: a band of width WW concentrates its spectral weight over that width, so a band of ∼0.2\sim0.2 eV width at EFE_F necessarily produces a peak of this kind. Its orbital decomposition is dominated by Lu-dd states, with the ege_g set carrying the larger share and hydrogen ss weight negligible in this window, the latter having been displaced to higher binding energy by the static shift.

!Photon energy dependent DOS adapted from [6] and calculated DMFT DOS bbox=0.17,0.09,0.84,0.42

Figure S4. Photon energy dependent DOS adapted from [6] licensed under CC by 4.0 (left), and calculated DMFT DOS (right)

Taken together, these results show that the correlated orbital creates a flat band it does not itself occupy. Correlation on the hydrogen ss states is substantial but almost entirely static: Re⁡ΣH−s(0)\operatorname{Re}\Sigma_{\mathrm{H-s}}(0) displaces the H-derived weight to higher binding energy, while m∗/m≲1.3m^*/m \lesssim1.3 leaves the quasiparticle residue close to unity. The narrow band remaining at EFE_F is therefore Lu-dd in character, flattened where the displaced H-ss level crosses it—a hybridization effect driven by a correlation-induced shift, not a heavy quasiparticle. The same self-energy accounts for both photoemission features, the sharp Lu-dd peak at EFE_F protected by the vanishing of Im⁡Σ\operatorname{Im}\Sigma and the broad, damped H-ss structure near −0.6-0.6 eV. Agreement with the measured flat-band binding energy improves under electron doping. Because the mechanism is a level alignment rather than a mass enhancement, its strength is set by where the hydrogen sits and how much of it is present—which is what the comparisons that follow address.

These single-particle differences appear directly in the optical response. Figure 6 shows the absorptivity A(ω)=1−R(ω)A(\omega)=1-R(\omega), computed from the independent-particle dielectric function (Figure S4), for the tetrahedral-only series [panel (b)] and for the octahedrally compensated LuH₂ [panel (a)], together with the measured spectra of Weaver et al. [14]. Configurations (a) and (d) share the same stoichiometry, so any difference between their spectra is structural rather than compositional.

Calculated optical absorption spectra of LuHₓ structures compared with experiment

Figure 6. Calculated optical absorption spectra of LuHₓ structures compared with experiment. (a) Calculated absorptivity for a LuH₂ structure in which one hydrogen occupies an octahedral site, compared with experimental data for LuH₁.₉₈, which also shows weak octahedral occupation. Arrows mark the low-energy feature associated with transitions involving octahedral hydrogen: orange for the calculated LuH₂ curve and green for the experimental LuH₁.₉₈ curve. This feature is absent in the tetrahedral-only structures of panel (b). (b) Calculated absorptivity for LuH₂, LuH₁.₈₇₅, and LuH₁.₇₅, which contain only tetrahedral hydrogen, compared with experimental data for LuH₁.₈₃, which is likewise tetrahedral-only.

In pure LuH2_2, ε2\varepsilon_2 falls below unity between 1.0 and 2.2 eV (Figure S4): the tetrahedral-only band structure supports no direct transitions in this window, hydrogen weight lying several eV below EFE_F. Within the window ε1\varepsilon_1 crosses zero at 1.05 eV with ε2\varepsilon_2 of order unity, so the loss function −Im⁡ε−1-\operatorname{Im}\varepsilon^{-1} reaches order unity and the absorptivity shows the corresponding sharp plasma edge—a single maximum of 0.96 at 1.05 eV over an essentially flat sub-edge background, the canonical Drude-plus-interband response of a clean CaF2_2-structure dihydride. Tetrahedral vacancies (LuH1.875_{1.875}, LuH1.75_{1.75}) progressively broaden this edge, raise the low-energy background, and shift the maximum toward 1.7–2.0 eV, but introduce no new structure below it.

Octahedral occupancy does. The compensated structure develops an occupied H-derived peak near −0.65-0.65 eV in the projected density of states (Figure S2), with no counterpart in any tetrahedral-only configuration. Transitions from this state into the unoccupied Lu-5d manifold set in near 0.65 eV and produce an ε2\varepsilon_2 oscillator peaking at 1.05 eV, consistent with the unoccupied DOS maximum at ≈+0.4\approx+0.4 eV. The zero of ε1\varepsilon_1 moves down to 0.57 eV, where now ε2≈15\varepsilon_2 \approx15 and the loss function is reduced to ≈0.07\approx0.07; the single sharp maximum is replaced by two damped ones, at 0.7 and 1.75 eV, separated by a minimum near 1.15 eV, and the integrated spectral weight below 1 eV substantially exceeds that of any tetrahedral-only spectrum. Both maxima fall at minima of ε2\varepsilon_2 rather than at its peaks: for ∣ε∣≫1|\varepsilon| \gg1 the reflectivity tracks ∣ε∣|\varepsilon|, so AA is largest where ∣ε∣|\varepsilon| is smallest, and neither maximum marks a transition energy.

Discussion

We now examine the physical origin of the trends established above. We first consider how the hydrogen on-site energies fix the sublattice occupations, and how the resulting filling — together with the screening environment set by the Lu-d manifold — determines the correlation strength on hydrogen. We then compare our results with optical and photoemission measurements on lutetium and related lanthanide hydrides, and assess what they imply for the electronic character of the flat bands near the Fermi level.

Origin of Filling and Correlation

The on-site energies provide a direct, one-body explanation for the hydrogen filling that underlies our central result. An orbital’s occupation is set by its energy relative to the Fermi level, and in LuH3_3 both H-ss sublattices lie 3–4 eV below EFE_F: the hydrogen shells are therefore filled and anionic (H−^--like), consistent with the near-full DMFT occupation (nH−s≈1.75n_{\mathrm{H-s}} \approx1.75) and with photoemission evidence for charge transfer to hydrogen [15, ?].

The Wannier analysis further reveals the electronic inequivalence of the two hydrogen sublattices: the octahedral H-ss level lies ∼1\sim1 eV above the tetrahedral one, identifying the octahedral hydrogen as the more weakly bound, shallower species. This is significant because the octahedral hydrogen is the common actor across the phenomenology of these materials: it controls the carrier density probed optically [14], it is the Kondo-like impurity of the breathing-hydrogen picture [10, 11], and it is the sublattice whose distortion opens the gap in cubic LuH3_3 [?]. Our calculation shows directly that, for lutetium hydrides, it is the hydrogen level closest to EFE_F—the least deeply bound and hence the most likely to be electronically and structurally active—while the tetrahedral hydrogen, filled already in the dihydride, lies deeper and is correspondingly inert.

The susceptibilities sharpen this picture and provide the most robust site-resolved discriminant in our data. In every Lu composition the octahedral hydrogen carries 1.8–2.8 times the local spin susceptibility of the tetrahedral hydrogen, without exception—including LuH2.875_{2.875}, where the mass enhancements of the two sites are inverted relative to the other compositions. Because χs\chi_s is a static thermodynamic average rather than a low-frequency derivative of a stochastic quantity, it is the less noise-sensitive diagnostic, and we take the susceptibility ordering as the more reliable statement of site inequivalence. Its ordering follows the on-site energies directly: the shallower octahedral level supports larger and longer-lived local fluctuations than the deeper tetrahedral one. The reversal in LaH3_3, where the octahedral level lies below the tetrahedral one, is reproduced in the susceptibilities as well—octahedral χs\chi_s falls below tetrahedral—so that the level ordering, the occupations, the local moments, and the susceptibilities all identify the same sublattice as the electronically active one in each compound. That four independent diagnostics agree indicates the site hierarchy is a robust feature of the electronic structure rather than an artifact of any single observable.

The level alignment directly rationalizes the weak hydrogen correlation. A shell buried well below EFE_F is filled and far from the half-filled configuration where the interaction could localize it; the large H-ss interaction therefore acts only as a static level shift rather than a mass renormalization, exactly as found in our DMFT self-energies. Level position, filling, and correlation thus form a single causal chain: the host sets the hydrogen level, the level sets the filling, and the filling—not the magnitude of UU—controls the correlation. This is the filling-control principle familiar from Hund’s metals and orbital-selective correlation in dd-electron systems [?, ?], operating here in its simplest setting: a single ss orbital with negligible Hund’s coupling. The same principle couples the two manifolds—the hydrogen acts as the electron reservoir that sets the dd-band filling and thereby its (weak) correlation—as detailed in Section 3C.

The rigid-band doping calculations make the reservoir behavior explicit. Adding or removing one electron per formula unit shifts the Lu-dd occupation by the full doped charge while the hydrogen occupations, moments, and local susceptibilities are unchanged—at the octahedral site as well as the tetrahedral one, even though the octahedral hydrogen is the more electronically active of the two. The hydrogen shell is thus closed not only in its static occupation but in its response: charge introduced at the Fermi level is absorbed entirely by the dd manifold. This is the dynamical counterpart of the deep, filled anionic level identified in the on-site energies, and it is the condition under which the rigid-band comparison with photoemission (Secion II D) is justified—the hydrogen-derived states near EFE_F shift with the chemical potential but do not themselves reconstruct. The dd susceptibility, by contrast, grows steadily with filling and becomes increasingly spin-dominated (χS/χD\chi_S/\chi_D rising from 4.0 to 6.0), the same trend seen across the stoichiometric series as hydrogen content is reduced. The two routes—varying hydrogen content at fixed electron count, and varying electron count at fixed hydrogen content—thus give a consistent account of which manifold is compressible.

The dd-channel behavior follows from the crystal-field structure of the fluorite lattice. The metal is coordinated by eight tetrahedral hydrogen at the cube corners rather than by six ligands octahedrally, and the cubic field inverts the familiar ordering: ege_g, whose lobes point between the ligands, lies below t2gt_{2g}. The ege_g set consequently fills first and sits closer to half filling, carrying the larger per-orbital moment. Adding octahedral hydrogen introduces a competing field of the opposite sign—the 4b site is octahedrally disposed with respect to the metal—which partially cancels the cubic splitting; this accounts for the narrowing of the eg/t2ge_g/t_{2g} occupation contrast from the dihydride to the trihydride.

Because both sets lie below half filling throughout, the spin susceptibility is on the rising side of its filling dependence, and the dd shell moves away from the moment-forming regime as hydrogen content increases. The rigid-band doping calculations confirm this directly: adding electrons raises ndn_d and χS\chi_S monotonically with no turnover (Table 18), as expected when approaching half filling from below. The stoichiometric series and the doping series therefore describe the same dependence traversed in opposite directions, and identify the ege_g occupation—set by hydrogen content—as the variable controlling the dd-shell spin response.

Comparision with Experiment

Angle-resolved photoemission on (nominally nitrogen-doped) lutetium hydride reports a flat band 0–200 meV below EFE_F and a nearby van Hove singularity, interpreted as a signature of strong correlation [?]. Our results bear directly on the origin of this feature. The DMFT Lu-5dd mass enhancement is modest (m∗/m≈1.1m^*/m \approx1.1–1.3), whereas a correlation-driven flat band would require a heavy quasiparticle mass, Z≪1Z \ll1. We therefore find that the near-EFE_F flat band is unlikely to be primarily a correlation-renormalization effect, pointing instead toward a disorder-related (hydrogen-vacancy) or filling/Van Hove origin, consistent with the absence of such a band in pure-LuH2_2 DFT [?]. We note that the precise hydrogen and nitrogen content of the ARPES sample is not firmly established; if the sample is closer to LuH2−x_{2-x} than to a nitrogen-doped composition, this conclusion is unaffected, since the argument rests on the magnitude of the computed renormalization rather than on the dopant.

Figure 6 compares the calculated optical absorptivity A(ω)A(\omega) of LuHx_x in four configurations against the experimental spectra of Weaver et al. [14] at x=1.83x = 1.83 and x=1.98x = 1.98. The dielectric functions (Fig. S[E]) show why octahedral occupation, and only octahedral occupation, restructures the spectrum. The oscillator introduced by the octahedral H falls inside the transparency window of pure LuH2_2—the same window that hosts its plasma edge. Filling the window has two consequences: the added interband screening shifts the zero of ε1\varepsilon_1 from 1.05 down to 0.57 eV, and ε2\varepsilon_2 at the crossing rises by an order of magnitude, collapsing the loss function. The sharp plasma edge of the dihydride is thereby eliminated, leaving a damped feature at 0.7 eV and a residual maximum at 1.75 eV in the part of the window that survives above the oscillator. Tetrahedral vacancies, by contrast, redistribute oscillator strength within the existing bands; they broaden the edge, but the window—and with it the single-maximum line shape—remains.

The measured spectra display the same dichotomy. LuH1.83_{1.83} shows a sharp edge and no sub-eV structure, consistent with predominantly tetrahedral occupation near the dihydride phase boundary; its maximum at 2.05 eV is bracketed by the calculated LuH2_2 (1.05 eV) and LuH1.875_{1.875} (1.85 eV). Near-stoichiometric LuH1.98_{1.98} shows an additional shoulder at 0.3–0.5 eV absent from LuH1.83_{1.83}, in the region where the octahedral calculation peaks, though at somewhat lower energy and with far smaller amplitude: ΔA≈0.02\Delta A \approx0.02 against the calculated ≈0.12\approx0.12, so any octahedral occupancy in the measured sample must be small. Two caveats attend the assignment. A Drude term with a finite scattering rate produces an inflection of similar shape with no interband contribution at all, and a firm identification would require the calculated absorptivity followed as a continuous function of octahedral filling, together with an independent structural determination of the site occupancies. A systematic offset of the calculated edge relative to experiment is also apparent—1.05 eV for the all-tet reference against the measured ∼1.7\sim1.7 eV; we discuss its possible origins in Sec. ??, and the interpretation here rests on the relative behavior across configurations, which is reproduced unambiguously.

The configurational comparison in Figure 6 provides a direct band-structure-level confirmation of the inference first made by Weaver et al. [14] that the sub-eV opti<lemma cal feature observed at near-stoichiometric compositions arises from octahedral H occupation rather than from tetrahedral disorder. The crucial control is the comparison between LuH₁.₇₅ and LuH₁.₈₇₅ (both tetrahedral-only) and LuH₂ with a single octahedral occupant. Tetrahedral vacancies smear the plasmon edge but do not introduce a new oscillator anywhere below 1.5 eV; octahedral occupation does. This separates site type from H content as the controlling variable—a separation that the original optical study could only approach indirectly through the quench-versus-slow-cool experiment on YH₁.₈₉ and through the systematic lattice-constant trend across Sc, Lu, Y.

It is worth recalling how the octahedral assignment was established historically, since the present calculation completes a chain of reasoning begun nearly half a century ago. Weaver et al.’s 1979 optical inference [14] was supported on the theoretical side by the companion self-consistent band calculation of Peterman et al. [?], which showed that tetrahedral-only CaF₂-structure YH₂ has no interband transitions in the 0.5–1.5 eV window, establishing that the sub-eV optical features required states outside the tetrahedral picture. Direct structural confirmation came shortly afterwards: proton NMR rigid-lattice second moments found 10–15% octahedral occupation in YH₁.₉₂ and YH₁.₉₈ [?], and neutron diffraction and inelastic scattering subsequently tracked the temperature dependence of the octahedral occupancy in YH₂.₀ and identified its optic-mode signature [?]. For LuHₓ specifically the direct structural evidence is sparser, and the present supercell calculation occupies a role analogous to Peterman’s but in the affirmative: where the tetrahedral-only band structure could only exclude certain transitions, we include an octahedral occupant and show spectroscopically that it produces the observed feature.

The dichotomy between tetrahedral and octahedral hydrogen is rooted in local coordination. In the fluorite structure, tetrahedrally coordinated H sits in a four-fold metal environment with comparatively short metal–hydrogen distances and strong dd–ss hybridization, which pulls the tetrahedral bonding band well below EFE_F. Octahedrally coordinated H has six metal neighbors at longer distance and weaker hybridization, placing its bonding combination closer to EFE_F. This ordering—tetrahedral deep, octahedral shallow—is the one we obtain for LuH₃, and it is the ordering established in the early rare-earth trihydride band-structure literature [?, ?, ?]. Both sites lie well below the Fermi level, consistent with the universal H⁻ level-alignment framework of Van de Walle and Neugebauer [?].

Coordination is not, however, the only variable. The octahedral interstitial is the larger and less tightly confined of the two sites, and its level is correspondingly more sensitive to the cell volume. In LaH₃, whose lattice constant exceeds that of LuH₃ by more than 10%, this sensitivity is sufficient to reverse the ordering, placing the octahedral level below the tetrahedral one (Table I). The tet/oct hierarchy therefore reflects a competition between coordination-driven hybridization, which favors a deeper tetrahedral level, and the volume dependence of the octahedral site; it is not a fixed property of the fluorite structure.

This level alignment is precisely the hierarchy revealed by our on-site Wannier energies in LuH₃, where the tetrahedral H 1s level sits at ε−EF=−3.8\varepsilon-E_F=-3.8 eV and the octahedral H 1s level at −2.9-2.9 eV with a 0.9 eV splitting in the expected direction (Sec. II A). The on-site energies set the hierarchy, not the transition energies: hybridization with the Lu-5d manifold carries octahedral-derived weight up to the occupied peak at −0.65-0.65 eV seen in the supercell density of states (Fig. S2), and it is transitions from this hybridized manifold into the unoccupied Lu-5d states that produce the oscillator at 1.05 eV. Tetrahedral-derived weight remains several eV below EFE_F even after hybridization, so its transitions lie far outside the Weaver window. The sub-eV structure in our supercell is therefore a direct spectroscopic signature of the shallow octahedral manifold, not a generic stoichiometry effect.

The systematic dependence on the host metal across the trivalent dihydrides reinforces this picture. The octahedral hole grows with the lattice constant in the sequence ScHx_x (a0≈4.78a_0 \approx4.78 Å), LuHx_x (5.03 Å), YHx_x (5.20 Å), and the spectroscopic signature of octahedral occupation follows in lockstep: absent in ScHx_x, weak near 0.4 eV in LuHx_x, and strong with two distinct features at 0.35 and 1.25 eV in YHx_x [14]. This is consistent both with the steric argument (larger octahedral holes are easier to occupy) and with the bonding argument (the octahedral H bonding level rises further toward EFE_F as the metal-hydrogen octahedral distance lengthens, increasing oscillator strength for transitions into the conduction manifold).

This optical interpretation closes the loop on the picture assembled from our cRPA, on-site-alignment, and mass-enhancement analyses, which together identify the octahedral hydrogen sublattice as the electronically active component of LuHx_x in the near-stoichiometric regime. The screened interaction UoctH−sU_{\mathrm{oct}}^{\mathrm{H-s}} is systematically lower than UH−stetU_{\mathrm{H-s}}^{\mathrm{tet}} in the H-s-only subspace and inverts upon enlargement of the active space to include Lu-dd screening, identifying the octahedral H as the more strongly coupled to the metallic conduction electrons; the on-site Wannier energy places it within hybridization range of the Fermi level; and the optical response now supplies an independent, experimentally anchored confirmation that the spectroscopic fingerprint of stoichiometry-driven changes in LuHx_x near x=2x = 2 resides in transitions involving this shallow octahedral manifold.

Conclusions

We investigate electronic correlation in the rare-earth hydrides LuHx_x (x=1.75x = 1.75–3) together with other LnHx_x compound using dynamical mean-field theory (DMFT) with the Hubbard UU values obtained from constrained random-phase approximation (cRPA). Our studies reveal that hydrogen-derived ss orbitals has much larger screened on-site Coulomb interactions than the Lu dd states. A joint analysis of Wannier spread functions and interaction parameters (see discussion in Section S2.2) demonstrates that these trends originate from the interplay of orbital localization and screening efficiency as evidenced by the pronounced dependence of UU on the choice of correlated subspace. The screened hydrogen interaction rises with hydrogen content at nearly fixed lattice constant, driven by the progressive anionic conversion of the octahedral hydrogen, which depletes the conduction-electron screening; this is the same carrier-density reduction observed experimentally as the decreasing Drude plasma frequency across the series [14], here manifested in the interaction parameters.

Despite carrying the largest interaction in the system, the hydrogen is weakly correlated. In hydrides LuHx_x (x=1.75x = 1.75–3) and LaH3_3, DMFT calculations indicates that these materials are weakly correlated metals; within this weakly correlated regime, however, the correlation is strongly filling-controlled. The LuHx_x hydrogen is a nearly filled, closed-shell anion with a deep on-site level consistent with the photoemission evidence for charge transfer to hydrogen [15], whose large interaction is inert because the filled shell admits no charge fluctuations. The Lu-dd band correlation in LuHx_x decreases as octahedral hydrogen dilutes the dd filling. The hydrogen content thus emerges as the principal tuning parameter for correlation in these materials—it is the electron reservoir that sets the filling of every manifold.

These results bear directly on the experimental phenomenology. Our calculations indicate that the flat bands reported near EFE_F by photoemission [?] arise from the presence of Hoct_{\mathrm{oct}} and Htet_{\mathrm{tet}} vacancies. At the same time, tetrahedral vacancies and octahedral occupancy can be tuned to place narrow bands and van Hove singularities near EFE_F, so that hydrogen stoichiometry offers a structural route to engineering the low-energy density of states. The 0.9 eV splitting we compute between the tetrahedral and octahedral hydrogen levels, and the correlation contrast we predict between the lutetium and lanthanum trihydrides, are in principle accessible to photoemission and optical spectroscopy.

The broader lesson is a simple organizing principle for correlation in hydrogen-rich materials: the host band structure sets the hydrogen level, the level sets the filling, and the filling—not the magnitude of UU—controls the correlation. A site-resolved treatment distinguishing the two hydrogen sublattices in LaH3_3, where the hydrogen is correlation-active, is the natural next step and would test the site-selective correlation this principle predicts.

Acknowledgments

This research was supported by the National Science Foundation (NSF) (DMR-2104881, A.L., R.J.H.), the Department of Energy (DOE) National Nuclear Security Administration (NNSA) through the Chicago/DOE Alliance Center (DE-NA0004153; R.J.H.), the DOE Office of Science (SC) (DE-CO0020340, R.J.H.), and NSF SI2-SSE Grant 2513657 (H.P.). P. G. (mentorship, analysis, writing) and H. S. (mentorship, analysis, writing) were supported by the DOE SC, Basic Energy Sciences (BES), Materials Sciences and Engineering Division, as part of the Computational Materials Sciences Program and Center for Predictive Simulation of Functional Materials. The authors gratefully acknowledge the Advanced Cyberinfrastructure for Education and Research (ACER) group at the University of Illinois Chicago for providing computational resources and services needed to deliver the research results presented in this paper. Similarly, this research used resources of the National Energy Research Scientific Computing Center (NERSC), a DOE SC User Facility located at Lawrence Berkeley National Laboratory, operated under Contract No. DE-AC02-05CH11231 using NERSC award BES-ERCAP0023615. This research used resources of the Argonne Leadership Computing Facility, which is a DOE SC User Facility supported under contract DE-AC02-06CH11357. This manuscript has been authored by UT-Battelle, LLC under Contract No. DE-AC05-00OR22725 with the DOE. Part of the DFT-based research was conducted as part of a user project at the Center for Nanophase Materials Sciences (CNMS), a DOE SC User Facility at Oak Ridge National Laboratory. Contributions to the manuscript were also sponsored by UT-Battelle, LLC under the same contract. The U.S. Government (USG) retains, and the publisher, by accepting the article for publication, acknowledges that the USG retains, a non-exclusive, paid-up, irrevocable, worldwide license to publish or reproduce the published form of this manuscript, or allow others to do so, for USG purposes. The DOE will provide public access to the results of federally sponsored research in accordance with the DOE Public Access Plan (http://energy.gov/downloads/doe-public-access-plan).

References

Computational details

First-principles calculations were performed within the framework of density functional theory (DFT) using the Vienna Ab initio Simulation Package (VASP) [4]. The projector augmented-wave (PAW) method [2] was employed to describe the interaction between valence electrons and ionic cores, and the exchange–correlation effects were treated within the generalized gradient approximation (GGA) in the Perdew–Burke–Ernzerhof (PBE) parametrization [9].

The plane-wave basis set was truncated at an energy cutoff of Ecut=650E_{\mathrm{cut}} = 650 eV. Brillouin-zone integrations were performed using a Γ\Gamma-centered Monkhorst–Pack kk-point mesh of 12×12×1212 \times12 \times12. Structural relaxations were carried out until the residual forces on each atom were smaller than 10−210^{-2} eV/Å. Electronic self-consistency was achieved with an energy convergence criterion of 10−610^{-6} eV.

Wannier basis construction

To construct the localized basis used for the effective low-energy model, maximally localized Wannier functions (MLWFs) were generated using the Wannier90 code [8]. The Wannier functions were constructed from a set of Bloch states obtained from VASP through the VASP2Wannier interface. Initial projections were chosen according to the relevant atomic orbitals of the correlated subspace (e.g., Lu dd orbitals and hydrogen ss orbitals). The disentanglement procedure was performed within an energy window extending from −10-10 eV to 10 eV relative to the Fermi level. The resulting Wannier functions reproduce the DFT band structure in the selected energy range with high fidelity.

Constrained Random Phase Approximation

The effective screened Coulomb interaction parameters were calculated within the constrained random phase approximation (cRPA) as implemented in VASP. In this framework, the fully screened interaction is obtained from the bare Coulomb interaction vv and the polarization function PP within the random phase approximation (RPA):

W(ω)=v1−vP(ω).(1)W(\omega) = \frac{v}{1-vP(\omega)}. \tag*{(1)}

In order to construct a low-energy Hamiltonian for the chosen correlated subspace, screening processes arising from electronic transitions within that subspace must be excluded. The total polarization is therefore decomposed as

P(ω)=Pd(ω)+Pr(ω),(2)P(\omega) = P_d(\omega) + P_r(\omega), \tag*{(2)}

where PdP_d corresponds to transitions within the correlated subspace and PrP_r represents the remaining screening channels. The partially screened interaction defining the effective Hubbard interaction is then

Wr(ω)=v1−vPr(ω).(3)W_r(\omega) = \frac{v}{1-vP_r(\omega)}. \tag*{(3)}

The static limit of this interaction (ω→0\omega\to0) provides the effective Hubbard interaction parameters used in model Hamiltonians:

Uijkl=⟨wiwj∣Wr(ω=0)∣wkwl⟩,(4)U_{ijkl} = \langle w_i w_j | W_r(\omega= 0) | w_k w_l \rangle, \tag*{(4)}

where wiw_i are the Wannier orbitals spanning the correlated subspace.

The matrix elements of the screened interaction were evaluated in the Wannier basis constructed from the DFT Bloch states. The calculated interaction matrix was subsequently used to extract the intra-orbital Hubbard interaction UU, the inter-orbital interaction U′U', and the Hund’s coupling JJ.

Density Functional Theory + Dynamical Mean Field Theory methodology

To capture the effects of strong electronic correlations beyond conventional density functional theory (DFT), we employed dynamical mean-field theory (DMFT) in combination with a Wannier-based low-energy Hamiltonian. The DFT+DMFT calculations were performed using the DMFTwDFT framework [11], which interfaces DFT codes with many-body solvers via Wannier90.

In this approach, a correlated subspace is constructed from a set of localized Wannier orbitals, which provide an effective low-energy Hamiltonian,

H=HDFT+Hint−HDC,(5)H = H_{\mathrm{DFT}} + H_{\mathrm{int}} - H_{\mathrm{DC}}, \tag*{(5)}

where HDFTH_{\mathrm{DFT}} is the Wannier-projected non-interacting Hamiltonian, HintH_{\mathrm{int}} describes the local Coulomb interactions within the correlated subspace, and HDCH_{\mathrm{DC}} is the double-counting correction accounting for interactions already included at the DFT level.

Within DMFT, the lattice problem is mapped onto a self-consistent quantum impurity problem, in which the local Green’s function is given by

Gloc(iωn)=∑k[(iωn+μ)I−HDFT(k)−Σ(iωn)]−1,(6)G_{\mathrm{loc}}(i\omega_n) = \sum_{\mathbf{k}} \left[(i\omega_n + \mu)\mathbb{I} - H_{\mathrm{DFT}}(\mathbf{k}) - \Sigma(i\omega_n)\right]^{-1}, \tag*{(6)}

where Σ(iωn)\Sigma(i\omega_n) is the local self-energy and μ\mu is the chemical potential. The impurity problem is solved iteratively to obtain Σ(iωn)\Sigma(i\omega_n), which is then used to update the lattice Green’s function until convergence is achieved.

The interacting Hamiltonian HintH_{\mathrm{int}} is expressed in terms of effective Hubbard interactions (UU, U′U^{\prime}, JJ), obtained from constrained random phase approximation (cRPA) calculations. The DMFT impurity problem was solved using the continuous-time quantum Monte Carlo (CTQMC) method in the hybridization expansion, as implemented in the DMFTwDFT package.

Charge self-consistency between DFT and DMFT was achieved by computing the DMFT density matrix and feeding it back into the DFT calculation, ensuring a consistent treatment of electronic correlations at both the one-particle and many-body levels [11]. This iterative loop continues until convergence in both the charge density and self-energy is reached.

Finally, the momentum-resolved spectral function was obtained from the analytically continued Green’s function,

A(k,ω)=−1πIm⁡Tr⁡[(ω+μ)I−HDFT(k)−Σ(ω)]−1.(7)A(\mathbf{k},\omega) = -\frac{1}{\pi}\operatorname{Im}\operatorname{Tr}\left[(\omega+\mu)\mathbb{I}-H_{\mathrm{DFT}}(\mathbf{k})-\Sigma(\omega)\right]^{-1}. \tag*{(7)}

Correlation diagnostics: self-energy, quasiparticle weight, and local moments

We characterize the strength of electronic correlation using three complementary quantities extracted from the converged DMFT solution: the quasiparticle mass enhancement obtained from the Matsubara self-energy, the per-atom occupation, and the instantaneous local moment obtained from the CTQMC impurity solver’s atomic-state probabilities.

Quasiparticle weight and mass enhancement. Near the Fermi level, the real part of the self-energy can be linearized as Re⁡Σ(ω)≈Re⁡Σ(0)+ω∂ωRe⁡Σ(ω)∣ω=0\operatorname{Re}\Sigma(\omega) \approx\operatorname{Re}\Sigma(0) + \omega\partial_{\omega}\operatorname{Re}\Sigma(\omega)|_{\omega=0}, which defines the quasiparticle weight

Z=(1−∂Re⁡Σ(ω)∂ω∣ω=0)−1.(8)Z = \left(1 - \left.\frac{\partial\operatorname{Re}\Sigma(\omega)}{\partial\omega}\right|_{\omega=0}\right)^{-1}. \tag*{(8)}

For local/momentum-independent self-energy, ZZ is exactly the inverse mass enhancement, m∗/m=1/Zm^*/m = 1/Z. We have:

m∗m=1−∂Im⁡Σ(iωn)∂ωn∣ωn→0,(9)\frac{m^*}{m} = 1 - \left.\frac{\partial\operatorname{Im}\Sigma(i\omega_n)}{\partial\omega_n}\right|_{\omega_n\to0}, \tag*{(9)}

Occupation and local moment. The per-atom occupation nn of each correlated orbital is obtained from the impurity solver and cross-checked against the trace of the local Green’s function. For a single-orbital impurity we have the probabilities of the empty, singly-occupied (spin-up and spin-down), and doubly-occupied configurations, PemptyP_{\mathrm{empty}}, P↑P_{\uparrow}, P↓P_{\downarrow}, and PdoubleP_{\mathrm{double}}, from which the occupation and the instantaneous local moment follow directly,

n=P↑+P↓+2Pdouble,⟨m2⟩=P↑+P↓.(10)n = P_{\uparrow} + P_{\downarrow} + 2P_{\mathrm{double}}, \qquad\langle m^2\rangle= P_{\uparrow} + P_{\downarrow}. \tag*{(10)}

Double counting. The double-counting correction HDCH_{\mathrm{DC}} removes the portion of the local Coulomb interaction already present, in a mean-field sense, in the DFT exchange-correlation functional, and must be subtracted to avoid counting the same interaction twice. We employ the fully localized limit (around-mean-field) form,

HDC=U(n0−12)−12J(n0−1),(11)H_{\mathrm{DC}} = U\left(n_0 - \frac{1}{2}\right) - \frac{1}{2}J(n_0 - 1), \tag*{(11)}

evaluated self-consistently using the DMFT-derived occupation n0n_0 of the correlated orbital at each charge-self-consistency iteration, so that the double-counting potential tracks the converged correlated occupation rather than a fixed nominal value.

Supplementary Results

Figure 1 shows the Lu–H structures considered in this work. The stoichiometric end members LuH3_3 and LuH2_2 adopt the Fm3‾mFm\overline{3}m structure. Hydrogen-deficient structures were generated by removing H from octahedral sites for LuH3−x_{3-x} and from tetrahedral sites for LuH2−x_{2-x}, and all structures were relaxed within DFT; the optimized lattice parameters are summarized in tbl:S1 3.

All compositions relax to cubic or near-cubic cells, with a=b=ca=b=c and α=β=γ\alpha=\beta=\gamma to within 0.02°. The lattice constant varies by less than 0.4% across the entire series and does so non-monotonically, with a shallow minimum near LuH2.875_{2.875}. This near-invariance of the cell geometry is important for interpreting the interaction parameters that follow: because the lattice constant changes so little—and non-monotonically—across the series, any systematic, monotonic trend in the screened interactions with hydrogen content (Sec. 2.2.2) cannot be attributed to cell geometry and must instead be electronic in origin. We return to this point in the cRPA analysis.

Interaction Parameters

Dependence of interaction parameters on orbital character

We performed constrained random-phase approximation (cRPA) calculations of the effective Coulomb interaction parameters for three correlated subspaces: (i) RE-dd only, (ii) H-ss only, and (iii) the combined RE-dd + H-ss manifold. From the interaction matrices we extracted the intra-orbital Hubbard UU, inter-orbital uu, and Hund’s coupling JJ (Table 5,Table 13 and following).

xx in LuHx_xIn Lu-d subspaceIn H-s subspaceIn H-s + Lu-d subspace
ULu−dU_{Lu-d}uLu−du_{Lu-d}JLu−dJ_{Lu-d}UH−sU_{H-s}uH−su_{H-s}JH−sJ_{H-s}UUuuJJ
LuH3_34.45––8.89––9.1––
LuH2.875_{2.875}2.8754.64621.41910.05187.75761.20050.00057.70571.42040.0236
LuH2.25_{2.25}2.253.40470.63620.09155.72960.12330.00365.71090.66280.0541
LuH2_224.30080.82100.09526.52190.36240.00145.16660.50720.0564
LuH1.75_{1.75}1.753.74320.66250.09516.24990.12540.00134.59740.45350.0600

Table 5. cRPA parameters in Lu-d, H-s, and combined subspaces for LuHx_x.

SystemSubspaceSiteUUuuJJ
LuH1.75_{1.75}H-s onlytet (all)6.250.130.001
RE-dd only–3.74–0.09
LuH2_2H-s onlytet (all)6.520.360.001
RE-dd only–4.300.820.095
combined–5.170.510.056
LuH2.875_{2.875}H-s onlytet7.95––
oct7.25––
(avg)7.761.200.001
RE-dd only–4.65––
LuH3_3H-s onlytet9.21––
oct8.25––
(avg)8.892.230.001
RE-dd only–4.461.670.102
combinedtet12.20––
oct12.5––
(avg)9.192.760.045
LaH3_3H-s onlytet8.76––
oct8.01––
(avg)8.512.110.001
RE-dd only–4.69––
combined–7.45––

Table 13. Summary of cRPA screened interaction parameters across LuHx_x stoichiometries and LaH3_3, for the three correlated subspaces (RE-dd only, H-s only, and combined RE-dd+H-s). UU, uu, and JJ are the averaged intra-orbital Hubbard, inter-orbital, and Hund’s coupling parameters. For the H-s channel in the trihydrides, site-resolved values are given for tetrahedral (tet) and octahedral (oct) hydrogen where both are occupied. All values in eV.

Across all stoichiometries the screened intra-orbital interaction on the H-ss orbitals is substantially larger than on the RE-dd orbitals. This is the opposite of the naive expectation that the more spatially compact orbital, or the rare-earth dd manifold often presumed more strongly correlated, should carry the larger UU. We find that two distinct factors must be separated to explain the hierarchy: orbital localization and screening.

The bare local Coulomb matrix element scales inversely with orbital extent, U∼∬dr dr′∣w(r)∣2∣w(r′)∣2∣r−r′∣U \sim\iint\mathrm{d}r\,\mathrm{d}r' \frac{\lvert w(\mathbf{r})\rvert^2\lvert w(\mathbf{r}')\rvert^2}{\lvert\mathbf{r}-\mathbf{r}'\rvert}, so a more localized Wannier function yields a larger bare interaction. The H-ss Wannier functions are indeed more compact (spread ∼0.63\sim0.63 Å2^2) than the RE-dd functions (∼1.40\sim1.40–1.551.55 Å2^2), which is consistent with UH>UdU_H > U_d at the level of the bare interaction. However, localization alone does not control the screened interaction. The decisive test is the change of correlated subspace: enlarging the subspace from H-ss only to the combined RE-dd + H-ss manifold increases the H-ss Wannier spreads (from ∼0.63\sim0.63 to ∼0.72\sim0.72 Å2^2), which on the geometric argument alone would reduce UHU_H. The cRPA result is the opposite: UHU_H increases (from ∼6.1\sim6.1–6.36.3 to ∼6.9\sim6.9–7.67.6 eV). This demonstrates that the screened H-ss interaction is governed primarily by the available screening channels rather than by orbital extent. In cRPA the screened interaction is Wr=[1−vPr]−1vW_r = [1 - vP_r]^{-1}v, where the polarization PrP_r excludes processes within the correlated subspace; enlarging the subspace to include RE-dd transfers the RE-dd polarization out of PrP_r, reducing the screening of UHU_H and raising it. Because the H-ss spread increases while UHU_H also increases, the effect cannot be geometric and must be the loss of RE-dd screening.

The RE-dd sector behaves oppositely, and this asymmetry is itself informative. Enlarging the subspace removes the H-ss screening of RE-dd, yet UdU_d barely changes (and slightly decreases, from 3.643.64–3.903.90 to ≈3.63\approx3.63 eV). The H-ss manifold—filled, deep below EFE_F, and weakly polarizable—is a poor screener of RE-dd, so removing it has little effect; the small residual decrease tracks a slight increase in the RE-dd Wannier spreads upon rehybridization. Thus RE-dd screens H-ss strongly, but H-ss screens RE-dd weakly: the screening is markedly asymmetric, consistent with RE-dd being the itinerant, polarizable manifold near EFE_F and H-ss the localized, filled one well below it. Notably, in the combined subspace the RE-dd onsite UU becomes nearly uniform (≈3.63\approx3.63 eV) even though the Wannier spreads retain their 2+32+3 (eg+t2ge_g+t_{2g}) structure—a further indication that UU is set by screening rather than orbital extent.

Taken together, the H-ss states are compact and weakly screened, giving large local interactions, while the RE-dd states are more extended and more effectively screened despite their multi-orbital character. The hierarchy UH>UdU_H > U_d is therefore driven primarily by differences in screening rather than by localization alone.

Table 5 compares the interaction parameters for the Lu and La hydrides. In the dihydrides, LuH2_2 shows larger UU, uu, and JJ than LaH2_2 in both the RE-dd and H-ss sectors. Both crystallize in Fm3ˉmFm\bar{3}m but with very different lattice constants (5.011 Å for LuH2\mathrm{LuH}_{2}, 5.655 Å for LaH2\mathrm{LaH}_{2}); the smaller LuH2\mathrm{LuH}_{2} cell yields more compact Wannier functions and correspondingly larger interactions, so the dihydride comparison is governed by the lattice constant. This geometric ordering does not, however, carry over cleanly to the trihydrides: while UHU_{\mathrm{H}} remains slightly larger for LuH3\mathrm{LuH}_{3} than LaH3\mathrm{LaH}_{3} (8.89 vs 8.40 eV), the RE-dd interaction reverses, with LaH3\mathrm{LaH}_{3} now larger (4.69 vs 4.45 eV) despite its much larger cell. The RE-dd channel in the trihydride is therefore no longer controlled by geometry alone, reflecting the change in dd-band filling and screening octahedral occupation (Sec. S2.2).

Evolution of the screened interaction with stoichiometry

Table 1 collects the cRPA H-s interaction, the DMFT hydrogen occupation, and the lattice constant across the LuHx\mathrm{LuH}_{x} series. The screened H-s Hubbard UU rises substantially with hydrogen content, from 6.25 eV in LuH1.75\mathrm{LuH}_{1.75} to 8.89 eV in LuH3\mathrm{LuH}_{3}—an increase of roughly 42%. Over the same range the lattice constant is nearly invariant, varying by less than 0.4% (5.027 to 5.014 Å) and non-monotonically. The enhancement of the hydrogen interaction is therefore not a geometric (lattice-volume) effect: at essentially fixed cell size, the screened interaction nonetheless grows by several eV.

Orbitalϵ−EF\epsilon- E_F (eV)
LuH3_3LaH3_3
Htet_{\mathrm{tet}}-s−3.841-3.841−2.751-2.751
Hoct_{\mathrm{oct}}-s−2.868-2.868−3.129-3.129

Table 1. On-site (R=0R = 0 diagonal) Wannier energies of the tetrahedral and octahedral hydrogen ss states relative to the Fermi level, from the MLWF Hamiltonian, for LuH3_3 (EF=4.845E_F = 4.845 eV) and LaH3_3 (EF=7.828E_F = 7.828 eV).

Systemaa (Å)UH−sU_{\mathrm{H-s}} (eV)URE−dU_{\mathrm{RE-d}} (eV)nH−sn_{\mathrm{H-s}}
LuH1.75\mathrm{LuH}_{1.75}5.0276.253.741.91
LuH2\mathrm{LuH}_{2}5.0116.524.301.91
LuH2.875\mathrm{LuH}_{2.875}5.0087.764.651.88
LuH3\mathrm{LuH}_{3}5.0148.894.451.75

Table 1. Evolution across the LuHx\mathrm{LuH}_{x} series: lattice constant aa, averaged cRPA H-s and RE-dd Hubbard UU, and DMFT per-atom H-s occupation. Octahedral occupation begins above LuH2\mathrm{LuH}_{2}. The lattice constant is nearly invariant while UH−sU_{\mathrm{H-s}} rises by ∼40%\sim40\%.

The rise sets in specifically as octahedral sites become occupied. In LuH1.75\mathrm{LuH}_{1.75} and LuH2\mathrm{LuH}_{2}, where only tetrahedral sites are filled, the H-s interaction is comparatively small (6.25 and 6.52 eV) and the matrix is uniform across sites. Once octahedral hydrogen appears (LuH2.875\mathrm{LuH}_{2.875}, LuH3\mathrm{LuH}_{3}), the average UU jumps to 7.76 and 8.89 eV, and the H-s interactions split by site type (Sec. 2.2.3). The RE-dd interaction, by contrast, varies only weakly and non-monotonically across the series (Ud=3.74U_d = 3.74–4.65 eV) and shows no comparable systematic trend, indicating that the strong stoichiometry dependence is specific to the hydrogen sublattice.

The screened H-s Hubbard UU rises monotonically and substantially with hydrogen content, from 6.25 eV in LuH1.75\mathrm{LuH}_{1.75} to 8.89 eV in LuH3\mathrm{LuH}_{3} (Table 1), an increase of ∼40%\sim40\%. The lattice constant, by contrast, varies by less than 0.4% across these compositions and does so non-monotonically, with a minimum near LuH2.875\mathrm{LuH}_{2.875} and the trihydride larger than LuH2.875\mathrm{LuH}_{2.875} (Table 3). The interaction and the lattice constant thus differ in both magnitude and trend: UH−sU_{\mathrm{H-s}} grows steadily while aa wanders within a half-percent window. The enhancement of the hydrogen interaction is therefore decoupled from the cell geometry and is electronic in origin.

Compositionaa (Å)α\alpha (°)Volume (ų)
LuH1.75\mathrm{LuH}_{1.75}5.027290.000127.055
LuH1.78125\mathrm{LuH}_{1.78125}5.027989.987127.104
LuH1.8125\mathrm{LuH}_{1.8125}5.027390.015127.059
LuH1.875\mathrm{LuH}_{1.875}5.028890.018127.179
LuH1.96875\mathrm{LuH}_{1.96875}5.024490.000126.838
LuH2\mathrm{LuH}_25.011290.000125.844
LuH2.25\mathrm{LuH}_{2.25}5.016590.000126.238
LuH2.875\mathrm{LuH}_{2.875}5.007790.000125.576
LuH3\mathrm{LuH}_35.020190.000126.511

Table 3. Lattice parameters of the relaxed LuHx\mathrm{LuH}_x structures.

Site-resolved hydrogen interactions: tetrahedral versus octahedral

In the trihydride, where both interstitial sublattices are occupied, the screened H-s interaction resolves into two site-distinct values. Identifying the sites from the Wannier-function centers, the four octahedral H-s orbitals carry Uoct≈8.25U_{\mathrm{oct}} \approx8.25 eV and the eight tetrahedral Utet≈9.21U_{\mathrm{tet}} \approx9.21 eV in LuH3_3, a difference of ΔU≈1.0\Delta U \approx1.0 eV (∼11%\sim11\%). The same ordering holds in LaH3_3 (Uoct≈8.0U_{\mathrm{oct}} \approx8.0, Utet≈8.8U_{\mathrm{tet}} \approx8.8 eV) and LuH2.875_{2.875} (ΔU≈0.7\Delta U \approx0.7 eV), and is absent in LuH2_2 and LuH1.75_{1.75}, where only tetrahedral sites are occupied and the H-s interactions are uniform.

This difference is not a consequence of orbital extent. The tetrahedral and octahedral H-s Wannier functions have nearly equal spreads, Ωtet≈0.51\Omega_{\mathrm{tet}} \approx0.51 Å2^2 and Ωoct≈0.54\Omega_{\mathrm{oct}} \approx0.54 Å2^2, differing by only ∼5%\sim5\% (Table 2). For a localized ss-like Wannier function the bare onsite Coulomb integral scales inversely with the orbital radius, Ubare∼⟨r2⟩−1/2∼Ω−1/2U_{\mathrm{bare}} \sim\langle r^2\rangle^{-1/2} \sim\Omega^{-1/2}, so the spread difference predicts a bare-interaction ratio of only

SiteH-s only Ω\Omega (Å2^2)H-s only UU (eV)combined Ω\Omega (Å2^2)combined UU (eV)
Octahedral0.5378.250.54212.5
Tetrahedral0.5139.210.53512.20

Table 2. Site-resolved H-s Wannier spreads and screened onsite UU in LuH3_3, in the H-s-only and combined RE-dd+H-s subspaces. The spreads are nearly equal between sublattices, yet UU differs by ∼1\sim1 eV; the tet/oct ordering inverts on enlarging the subspace.

UbaretetUbareoct∼(ΩoctΩtet)1/2=(0.540.51)1/2≈1.02,(12)\frac{U_{\mathrm{bare}}^{\mathrm{tet}}}{U_{\mathrm{bare}}^{\mathrm{oct}}} \sim\left(\frac{\Omega_{\mathrm{oct}}}{\Omega_{\mathrm{tet}}}\right)^{1/2} = \left(\frac{0.54}{0.51}\right)^{1/2} \approx1.02, \tag*{(12)}

i.e. a ∼2%\sim2\% geometric effect. The observed ratio of the screened interactions is

UtetUoct=9.218.25≈1.12,(13)\frac{U_{\mathrm{tet}}}{U_{\mathrm{oct}}} = \frac{9.21}{8.25} \approx1.12, \tag*{(13)}

a ∼12%\sim12\% effect. The geometry therefore accounts for only about one-sixth of the observed difference; the remainder must arise from screening. The two hydrogen sublattices carry essentially the same bare interaction but are screened to differing degrees, the octahedral hydrogen being the more strongly screened.

The screening origin is confirmed directly by enlarging the correlated subspace from H-s only to combined RE-dd+H-s, which removes the RE-dd states from the cRPA screening. Both H-s interactions rise by ∼3\sim3–44 eV, but the octahedral interaction rises more steeply (8.25→12.58.25 \to12.5 eV) than the tetrahedral (9.21→12.209.21 \to12.20 eV), inverting the ordering so that the octahedral interaction becomes the larger (Table 2). Throughout this change the Wannier spreads remain nearly constant (Ωoct:0.537→0.542\Omega_{\mathrm{oct}} : 0.537 \to0.542, Ωtet:0.513→0.535\Omega_{\mathrm{tet}} : 0.513 \to0.535 Å2^2), so the several-eV shifts in UU cannot be geometric. Because the octahedral interaction gains more when the RE-dd screening channels are removed, the octahedral hydrogen is the sublattice more strongly screened by the rare-earth conduction electrons.

Hydrogen filling

To probe the origin of the hydrogen filling directly, we examine the on-site (R = 0, diagonal) elements of the Wannier Hamiltonian, ϵi=⟨wi(0)∣H^∣wi(0)⟩\epsilon_i = \langle w_i(0)|\hat{H}|w_i(0)\rangle, which give the bare one-body energy of each correlated orbital before hybridization. Referencing these to the Fermi level isolates where the hydrogen states sit relative to the conduction manifold, providing a more direct measure of the hydrogen charge state than the occupation alone.

The maximally-localized Wannier functions for LuH3\mathrm{LuH}_3 are well converged, with small, positive spreads (0.69 Å2^2 for octahedral and 0.86 Å2^2 for tetrahedral H-s, and ∼1.0\sim1.0 Å2^2 for Lu-dd), and centers located precisely on the crystallographic sites. The H-s Wannier functions resolve into two symmetry-distinct groups: eight tetrahedral and four octahedral, as expected for the fluorite trihydride.

Correlation effect calculations

Self-energy

We plot the imaginary part of the Matsubara self-energy, −Im⁡Σ(iωn)-\operatorname{Im}\Sigma(i\omega_n) fig:S1b and the analytically continued real-axis self-energy −Im⁡Σ(ω)-\operatorname{Im}\Sigma(\omega) fig:S1a. For every orbital and every stoichiometry, −Im⁡Σ(iωn)-\operatorname{Im}\Sigma(i\omega_n) extrapolates toward zero as ωn→0\omega_n \to0 and rises approximately linearly at low frequency. Also, −Im⁡Σ(iωn)-\operatorname{Im}\Sigma(i\omega_n) shows no upturn or divergence. This is a Fermi-liquid behavior of coherent, finite-lifetime quasiparticles. This shows that LuHx\mathrm{LuH}_x are correlated metals rather than Mott insulators at the temperature considered here.

The low-frequency slope, which sets the mass enhancement m∗/m=Z−1≃1−Im⁡Σ(iω0)/ω0m^*/m = Z^{-1} \simeq1-\operatorname{Im}\Sigma(i\omega_0)/\omega_0, orders the Lu-dd correlation strength as LuH1.75>LuH2.875>LuH3\mathrm{LuH}_{1.75} > \mathrm{LuH}_{2.875} > \mathrm{LuH}_3, i.e. the Lu-dd correlations decrease with increasing hydrogen content. The overall magnitude of −Im⁡Σ-\operatorname{Im}\Sigma is moderate (peaking at ≲0.25\lesssim0.25 eV), consistent with moderately—rather than strongly—renormalized quasiparticles. On the real axis, the Lu-dd incoherent scattering peaks lie just below EFE_F; they are broadest, with a weak above-EFE_F shoulder, for LuH1.75\mathrm{LuH}_{1.75} and collapse to a single sharp sub-EFE_F peak for LuH2.875\mathrm{LuH}_{2.875}, mirroring the Matsubara-axis ordering.

The H-s self-energy is roughly an order of magnitude smaller than that of Lu-dd for all stoichiometries, confirming weak H-s correlation despite the large H-s Hubbard UU (discussed below). Its frequency dependence is noisier at low ωn\omega_n, reflecting the small signal, so the H-s extrapolation is the least certain. Notably, the H-s scattering grows with hydrogen content (LuH3>LuH2.875>LuH1.75\mathrm{LuH}_3 > \mathrm{LuH}_{2.875} > \mathrm{LuH}_{1.75}) — the opposite trend to Lu-dd — and on the real axis its scattering is a narrow peak located essentially at EFE_F.

DFT and DMFT Densities of States

We compare the orbital-projected density of states (DOS) obtained from DFT (top row) and DMFT (bottom row) for the three stoichiometries in Figure S2. Within DFT, all three compositions are metallic, with substantial Lu-dd (blue) spectral weight at and around the Fermi level EFE_F and H-s (orange) bonding states found several eV below EFE_F. This DFT result is expected from mean-field itinerant-band description, with the Lu-dd manifold crossing EFE_F. Now, as we include dynamical correlation through DMFT, the spectral weight is redistributed in all three cases. Occupied Lu-dd weight is pushed to lower energy and becomes incoherent. Next, the DOS near EFE_F is diminished, and a broad high-energy feature emerges in the range ∼1.5\sim1.5–44 eV, reminiscent of an upper Hubbard band. The strength of the near-EFE_F suppression varies across the series: LuH2.875_{2.875} and LuH3_3 show DOS minimum at EFE_F, LuH1.75_{1.75} shows a strong but metallic (bad-metal-like) suppression. The H-s states are mostly situated near the occupied region and are not show much weight transfer.

Comparison of DFT and DMFT densities of states of Lu-H structures

Figure S2. Comparision of DFT and DMFT densities of states of Lu-H structures calculated using cRPA calculated UU values for various stoichiometries. Panels (a,d), (b,e), and (c,f) correspond to LuH1.75_{1.75}, LuH2.875_{2.875}, and LuH3_3, respectively.

Imaginary part of the self-energy as calculated for various stoichiometries

Figure S1. Imaginary part of the self-energy as calculated for various stoichiometries. Left side is analytically continued and right side is averaged over last few converged DMFT iterations

In every LuHx_x stoichiometry the H-1s shell is near-full (nH−s=1.75n_{\mathrm{H-s}} = 1.75–1.911.91, i.e. 88–95% occupied) and shows weaker renormalized (m∗/m≤1.07m^*/m \le1.07, Z≥0.99Z \ge0.99), despite carrying the largest cRPA interaction (up to UH−s=8.89U_{\mathrm{H-s}} = 8.89 eV). The large H-1s interaction manifests instead as a sizable static shift of the real part of the self-energy, Re⁡ΣH−s∼6\operatorname{Re}\Sigma_{\mathrm{H-s}} \sim6–88 eV, which grows with UH−sU_{\mathrm{H-s}} across the series and displaces the H-derived spectral weight from ∼−5\sim-5 eV (DFT) to ∼−8\sim-8 eV (DMFT).

The substoichiometric compounds exhibit multiple sharp features within a narrow energy window of ±0.5\pm0.5 eV around the Fermi level, in contrast to LuH2_2, which shows a comparatively smooth DOS in this region. The DMFT spectral functions over a wider energy range (−6-6 to 44 eV) are shown in Figure 2. The sharp features identified in the DFT DOS can be traced to flat bands located above EFE_F in the non-interacting description. A closer view of the low-energy electronic structure is provided in Figure 4. LuH1.75_{1.75} exhibits a pronounced quasiparticle peak near −0.3-0.3 eV. In addition, the DMFT spectra clearly resolve the crystal-field splitting between the ege_g and t2gt_{2g} manifolds. DFT DOS shows LuH3_3 as semi metallic whereas DMFT shows LuH3_3 as H-dominated metal.

To isolate the variable controlling the H-1s1s correlation, we repeated the LuH3_3 and LaH3_3 calculations with the H-1s1s interaction raised to UH−s=14U_{\mathrm{H-s}} = 14 eV, well above the cRPA values, holding all else fixed. In LuH3_3, where H-1s1s is near-full, this 58% increase in UU changes the H-1s1s quasiparticle weight (Z=0.99→0.83Z = 0.99 \to0.83). H-1s1s correlation is controlled by the orbital filling, not by the magnitude of UU: on-site interaction can renormalize a half-filled H-1s1s shell but is inactive on a near-full one, regardless of its strength. Even at UH−s=14U_{\mathrm{H-s}} = 14 eV, however, LuH3_3 and LaH3_3 remains a correlated metal, not an insulator.

Quasiparticle renormalization and local moments

We quantify the local electronic correlation in each manifold using three complementary diagnostics extracted from the DFT+DMFT solution: the quasiparticle mass enhancement m∗/m=1/Zm^*/m = 1/Z, obtained from the low-frequency slope of the Matsubara self-energy m∗/m=1−∂Im⁡Σ(iωn)/∂ωn∣ωn→0m^*/m = 1 - \left.\partial\operatorname{Im}\Sigma(i\omega_n)/\partial\omega_n\right|_{\omega_n\to0}; the per-atom occupation nn; and the instantaneous local moment ⟨m2⟩\langle m^2\rangle, obtained directly from the CTQMC atomic-state probabilities. The mass enhancement is a low-energy Fermi-liquid quantity and is the most sensitive to statistical noise; the occupation and local moment are static expectation values and are correspondingly robust. We therefore treat the local moment and occupation as the primary correlation diagnostics and report m∗/mm^*/m only where the self-energy slope is resolvable above the statistical noise (verified by a Fermi-liquid check on the low-frequency self-energy and a fit-window sensitivity analysis). Tables 15 and 16 collect the results for the H-ss and RE-dd manifolds, respectively.

Screening versus localization in the cRPA literature. That screening, rather than orbital extent, controls interaction trends is established for the transition-metal oxides. Across the SrMO3_3 series the t2gt_{2g} interaction decreases with atomic number, contrary to the atomic localization trend, because increasing screening overcompensates the increasing orbital localization [14]. The decisive separation of the two effects—bare interaction (orbital extent) versus screening—was demonstrated for metal surfaces, where the variation of UU was shown not to arise from changes in the Wannier-function spread (the bare interaction being essentially unchanged) but from changes in screening, such that UU can even decrease where a simple coordination argument predicts an increase [10]. Our finding that UHU_H rises even as the H-ss Wannier functions become more extended is an instance of the same screening-over-localization principle, and we use the same logic to attribute the H-ss interaction differences to screening.

Dihydride Lu/La comparison. The LuH2_2/LaH2_2 comparison, by contrast, is governed primarily by structure. The much smaller LuH2_2 lattice constant yields more localized Wannier functions for both RE-dd (∼1.40\sim1.40 vs ∼2.17\sim2.17 Å2^2) and H-ss (∼0.63\sim0.63 vs ∼0.78\sim0.78 Å2^2), accounting for the larger interactions in LuH2_2. This geometric ordering is specific to the dihydride: in the trihydride the RE-dd interaction is larger for LaH3_3 despite its larger cell, indicating that octahedral occupation introduces screening and filling changes that override the geometric trend in the dd channel. The rare-earth species also differ in ff-shell occupation (filled for Lu, empty for La), which may further modify the local potential and screening; our calculations do not isolate this from the lattice-constant effect, and we do not assign it a definite role.

Relation to the experimental lattice contraction. The interpretation of the stoichiometry trend aligns with the long-standing anionic picture of hydrogen in the rare-earth hydrides [12, 3] and with the experimental observation that heavy rare-earth β\beta-RH2+x_{2+x} contracts with increasing hydrogen content, attributed to increasing ionic character of the octahedral hydrogen [13]. Our fixed-composition calculations are not designed to reproduce this small structural contraction directly—the lattice constants across our series vary by less than half a percent and non-monotonically—and we therefore treat the structural trend as experimental context. What our calculations establish is the electronic side of the same picture: at fixed geometry, the screened hydrogen interaction tracks the anionic conversion of the octahedral sublattice. The site-resolved interactions reinforce this reading: the octahedral hydrogen, which carries the additional anionic charge, is the sublattice whose interaction is most sensitive to conduction-electron screening, as shown by the inversion of the tetrahedral/octahedral UU ordering when the RE-dd screening channels are removed.

Filling control of the dd manifold; scope of the analogy. The hydrogen reservoir sets the dd-band filling: adding octahedral hydrogen withdraws charge from the dd band, reducing ndn_d from ≈0.83\approx0.83 in the dihydrides to ≈0.56\approx0.56 in LuH3_3, and the dd correlation tracks this dilution, weakening from m∗/m≈1.09m^*/m \approx1.09 to 1.04, with the lowest dd filling (LuH2.875_{2.875}, nd≈0.27n_d \approx0.27) showing no resolvable enhancement. We stress that the filling-control principle at work here is not an orbital-selective Mott transition—there is only a single hydrogen ss orbital per site, with no intra-shell bandwidth disparity to drive orbital-selective localization—but a demonstration that the underlying principle extends to, and is most transparently seen in, a single-orbital host.

Construction of energy-distribution curves

Calculated energy-distribution curves are vertical cuts of the converged spectral function A(k,ω)=−Im⁡G(k,ω)/πA(\mathbf{k},\omega)=-\operatorname{Im}G(\mathbf{k},\omega)/\pi at fixed momentum, evaluated on the same Wannier Hamiltonian and self-energy used for Figure S3. Because the self-energy is momentum independent, these require no additional DMFT iterations: the Green’s function is re-evaluated on the desired k\mathbf{k} list at fixed Σ(ω)\Sigma(\omega) and chemical potential.

Three operations convert A(k,ω)A(\mathbf{k},\omega) into a measured-like intensity, applied in the order

I(k,ω)=[A~(k,ω)f(ω,Texp)]⊗R(ω),(14)I(\mathbf{k},\omega)=\left[\widetilde{A}(\mathbf{k},\omega)f(\omega,T_{\mathrm{exp}})\right]\otimes R(\omega), \tag*{(14)}

where ff is the Fermi function at the measurement temperature Texp=20T_{\mathrm{exp}}=20 K, RR is a Gaussian of 30 meV full width at half maximum representing the analyzer resolution, and A~\widetilde{A} denotes AA after momentum broadening. For out-of-plane cuts the momentum broadening is a Lorentzian of half width 0.15 A˚−1\mathrm{\mathring{A}}^{-1}, corresponding to the momentum uncertainty Δkz≃1/λ\Delta k_z \simeq1/\lambda associated with a photoelectron escape depth λ≈5\lambda\approx5 A˚\mathrm{\mathring{A}}; it is applied by convolution along the cut, with the spectral function mirror-extended about each endpoint so that the kernel is not truncated at the segment edges. In-plane cuts are shown without momentum broadening. All three parameters are fixed by the experimental conditions and none is adjusted to improve agreement. Peak positions quoted in the main text are obtained by parabolic refinement of the maximum of the raw A(k,ω)A(\mathbf{k},\omega) within an energy window bracketing a single band, before the Fermi cutoff and resolution are applied, since both displace the apparent maximum.

Out-of-plane curves are computed along the pure kzk_z line at fixed in-plane momentum k∥=(12,12)\mathbf{k}_{\parallel}=\left(\frac{1}{2},\frac{1}{2}\right), i.e. the MM–RR segment of the simple-cubic zone. The dispersion of the −0.6-0.6 eV feature is quoted over the full segment rather than at a single point: since E(kz)=E(−kz)E(k_z)=E(-k_z), the derivative ∂E/∂kz\partial E/\partial k_z vanishes at both the zone centre and the zone boundary, so curves selected from the immediate vicinity of either endpoint appear flat by symmetry irrespective of the dispersion in between.

Limitations of the comparison of EDC

The measured and calculated curves differ in three respects that bear on the comparison. Energetically, the measurement was performed at 15–30 K with ∼30\sim30 meV analyzer resolution, whereas the impurity problem is solved at T=0.02T=0.02 eV; the calculated linewidths are therefore upper bounds, and analytic continuation of Σ(iωn)\Sigma(i\omega_n) limits the precision of feature positions near EFE_F to a few tens of meV. In momentum, the calculation is evaluated at definite k\mathbf{k}, whereas photoemission integrates over an intrinsic kzk_z uncertainty set by the escape depth and, in these samples, over an additional in-plane spread arising from their multi-domain character, for which high-symmetry directions could not be established. Neither the in-plane origin nor the kzk_z of the measured curves is therefore known, and no momentum-resolved agreement is claimed. In intensity, the measured curves include photoemission matrix elements, which are orbital-, geometry-, and photon-energy-dependent, together with an inelastic background that grows with binding energy; neither is contained in A(k,ω)A(k,\omega), which is why the calculated curves return to zero at high binding energy while the measured ones do not.

A further caveat concerns the ordered arrangement of octahedral hydrogen in our supercell. The energy of the octahedral-derived states is robust, but their residual dispersion and fine structure are artifacts of that ordering: in a disordered sample the same states would appear as an incoherent resonance at similar energy rather than as coherent minibands. Any residual excess sharpness of the calculated features relative to experiment is expected on these grounds alone.

cRPA Interactions

The screened on-site interaction on H-s substantially exceeds that on RE-dd across all compositions, and this hierarchy is a screening effect rather than a localization effect. The decisive evidence is the subspace test: enlarging the correlated subspace from H-s-only to the combined RE-dd+H-s manifold increases both the H-s Wannier spread and the screened UHU_H—a combination the bare-interaction (geometric) picture cannot produce, and which can only arise from the removal of RE-dd screening channels. This is the rare-earth-hydride analogue of the well-known result for SrVO3_3, where including the oxygen 2p2p states in the correlated subspace nearly doubles the static UU by excluding the O-p→t2gp \to t_{2g} screening channel [1]; here the RE-dd manifold plays the role of the oxygen pp states. Likewise, cRPA results also show that screening can override orbital localization in setting interaction trends [14, 10]. We have a further discussion in Sec. SX.

The screening is noticibly asymmetric. The itinerant RE-dd manifold, straddling EFE_F, screens the H-s interaction strongly, whereas the filled, deep-lying H-s manifold screens RE-dd only weakly: removing H-s from the screening channels leaves UdU_d essentially unchanged. In the combined manifold the RE-dd interaction becomes nearly uniform even though the Wannier spreads retain their crystal-field 2 + 3 structure—a further sign that the interaction is set by screening rather than orbital extent.

The screened hydrogen interaction also rises strongly with stoichiometry at nearly fixed lattice constant, identifying the trend as electronic rather than geometric. The mechanism is the progressive anionic conversion of the octahedral hydrogen above x=2x = 2: each octahedral hydrogen that converts toward H−^{-} withdraws an electron from the conduction band, depleting the carriers that screen the local interactions—the same carrier-density reduction observed optically as a decreasing Drude plasma frequency [15]—so that UH−sU_{\mathrm{H-s}} rises as octahedral sites fill. The effect is specific to hydrogen; the RE-dd interaction shows no comparable trend. The dihydride Lu2_2/La comparison, the role of the ff-shell difference, and the relation to the experimental lattice contraction are discussed in Sec. SX.

Details on Absorptivity calculation

We finally remark on the systematic plasmon-position offset between calculation and experiment (∼0.6\sim0.6 eV). Several conventional sources may contribute: the equilibrium DFT lattice constant of LuH2_2 may differ from the experimental composition LuH1.83_{1.83} by a few percent with corresponding effect on the Drude carrier density; convergence of the intraband contribution within epsilon.x requires very dense k-mesh sampling; and the intraband broadening parameter is treated phenomenologically rather than from first principles. We do not attribute the offset to mass renormalization, since our DMFT analysis gives Z5d≈0.95Z_{5d} \approx0.95 for the LuH2_2 end member (Sec. 4.1.1), too close to unity to account for a factor of (1.7/1.1)2≈2.4(1.7/1.1)^2 \approx2.4 in the squared plasma frequency. The relative ordering and qualitative shape of the configurational dependence are robust regardless of the precise plasmon position, and these are what carry the interpretive weight of the present comparison.

Flat Bands, van Hove Singularity, and Comparison with Photoemission

We compare the band structures of the following cubic fluorite based structures: LuH1.75_{1.75} (one Htet_{tet} vacancy), LuH2_2, LuH2.25_{2.25} (one Hoct_{oct} occupancy), oct-LuH2_2 (one Htet_{tet} vacancy and one Hoct_{oct} occupancy) to identify the ingredients for flat bands and van Hove singularity near EFE_F. Tetrahedral vacancies provide flat bands below the Fermi level whereas octahedral occupancy pulls the van Hove singularity above M point down to the Fermi level. The structure with both Htet_{tet} vacancy and Hoct_{oct} occupancy has van Hove singularity situated right at the Fermi level and flat bands below the Fermi level Figure 4. The octahedral-H manifold, which the on-site Wannier alignment places at ε−EF=−4.21\varepsilon- E_F = -4.21 eV in LuH3_3, hybridizes with the Lu-5d states crossing EFE_F in the dihydride and drives a van Hove-like feature at MM toward the Fermi level, while tetrahedral vacancies contribute a localized, weakly dispersing defect band. Where both coexist—the minimal model for the observed LuH1.98_{1.98} optical feature—N(EF)N(E_F) is enhanced relative to the clean dihydride. At the Wannier level these ingredients are present but incomplete: the narrow band is not yet pinned at EFE_F and the saddle is not yet degenerate.

Interactions complete the construction. Since the Wannier and DMFT panels of Figure 5 share a Hamiltonian, and since the mass enhancements extracted from the Matsubara self-energies are bounded by 1.33, the near-EFE_F flattening is too large to be quasiparticle mass enhancement. It originates instead in the static, orbital-dependent shift Re⁡Σ(0)−Vdc\operatorname{Re}\Sigma(0) - V^{\mathrm{dc}}, which relocates the hydrogen level so that its hybridization with the Lu-dd manifold flattens the composite band and brings the saddle into coincidence with EFE_F. This is an interaction effect—it is absent at U=0U = 0—but it is a band reconstruction rather than a correlation-induced narrowing, and its magnitude is sensitive to the double-counting prescription in the hydrogen channel, the dominant systematic uncertainty here.

Carrier doping then tunes the result. The features shift rigidly in energy at 30 meV per percent doping without displacing in momentum, electron doping moving them below EFE_F and hole doping toward and through it. This quantifies, within a correlated framework, the proposal of [6] that aligning the flat band and saddle with EFE_F would enhance a superconducting instability. The compositional series realizes the same tuning self-consistently, since each additional octahedral hydrogen removes ∼0.7\sim0.7–0.80.8 conduction electrons per formula unit while introducing new octahedral levels.

The photoemission comparison supports a two-component reading of both data sets. Experimentally, a sharp flat band lies immediately below EFE_F with a light band emerging from it; in the calculation, the weakly dispersing hybridized band near EFE_F is pro tected against lifetime broadening by the smallness of ∣Im⁡Σ∣\lvert\operatorname{Im}\Sigma\rvert at low frequency, and the deeper structure near −0.6-0.6 eV is dispersive and resolves into individual bands. The energy-distribution curves of Figure S3 reproduce this correspondence: both show a sharp, momentum-independent maximum just below EFE_F, and deeper structure that disperses in plane and is comparatively flat out of plane. That the calculated deep feature appears as separate peaks rather than the single measured hump follows from momentum integration along kzk_z over the escape-depth window and from the ordered octahedral sublattice of our supercell, which produces coherent minibands where a disordered sample would show an incoherent resonance at the same energy. Our calculations contain neither nitrogen nor oxygen, both present in the measured samples of Ref. [6]; occupation of the octahedral site by hydrogen alone therefore suffices to generate the observed phenomenology, and the all-tetrahedral LuH2\mathrm{LuH}_2 calculation, in which neither feature appears, identifies octahedral occupation rather than stoichiometry as the controlling variable. Consistent with this, similar photoemission results have been obtained on nitrogen-free Lu–H crystals [7], indicating that nitrogen is not required for the flat band and saddle to appear.

The comparison is restricted to energies and qualitative band shapes. The measured crystals are multi-domain with no established high-symmetry directions, the flat-band and saddle data were taken at different and undetermined kzk_z, and our momenta refer to a supercell zone; no momentum-resolved agreement is claimed. On the theory side the impurity problem is solved at T=0.02T = 0.02 eV, so linewidths are upper bounds, and analytic continuation limits feature positions near EFE_F to a few tens of meV. Within these limits the picture is consistent and, notably, weakly correlated: mass enhancements nowhere exceed [1.33, local moments are fully screened, and the low-frequency self-energies are Fermi-liquid-like. The flat band and saddle are consequences of octahedral-site chemistry sharpened by an interaction-induced level shift—not manifestations of strong correlation, as has been suggested. What this leaves open is whether such features, once tuned to EFE_F, matter for pairing.

Tables

Below are the tables.

Table 3: Lattice parameters of the relaxed LuHx\mathrm{LuH}_x structures. All cells are (near-)cubic with a=b=ca = b = c and α=β=γ\alpha= \beta= \gamma; deviations of α\alpha from 90∘90^\circ are ≤0.02∘\leq0.02^\circ. The lattice constant varies by less than 0.6%0.6\% across the full composition range.

CompositionULu−d,UH−sU_{Lu-d}, U_{H-s} (eV)a (Å)b (Å)c (Å)α,β,γ\alpha, \beta, \gamma (°)Volume (Å3^3)
LuH1.75_{1.75}0.000, 0.0005.02725.02725.027290.000, 90.000, 90.000127.055
LuH1.75_{1.75}2.000, 6.0005.10325.10325.103290.000, 90.000, 90.000132.897
LuH2_20.000, 0.0005.01125.01125.011290.000, 90.000, 90.000125.841
LuH2_24.300, 6.5225.17715.17715.177190.000, 90.000, 90.000138.759
LuH2_2 [5]–5.0335.0335.03390.000, 90.000, 90.000127.491

Table 4. Lattice parameters and volume comparision between lattice parameters optimized using DFT or DFT+UU. The last row is experimentally measured lattice parameter from [5]

Uijij(H−s)U_{ijij}^{(H-s)}(6.06950.00010.00290.00010.00290.00010.00290.00016.24290.00070.00010.00260.00010.00260.00290.00076.31700.00260.00010.00260.00010.00010.00010.00266.24290.00070.00010.00260.00290.00260.00010.00076.31700.00260.00010.00010.00010.00260.00010.00266.24290.00070.00290.00260.00010.00260.00010.00076.3170)\begin{pmatrix} 6.0695 & 0.0001 & 0.0029 & 0.0001 & 0.0029 & 0.0001 & 0.0029 \\ 0.0001 & 6.2429 & 0.0007 & 0.0001 & 0.0026 & 0.0001 & 0.0026 \\ 0.0029 & 0.0007 & 6.3170 & 0.0026 & 0.0001 & 0.0026 & 0.0001 \\ 0.0001 & 0.0001 & 0.0026 & 6.2429 & 0.0007 & 0.0001 & 0.0026 \\ 0.0029 & 0.0026 & 0.0001 & 0.0007 & 6.3170 & 0.0026 & 0.0001 \\ 0.0001 & 0.0001 & 0.0026 & 0.0001 & 0.0026 & 6.2429 & 0.0007 \\ 0.0029 & 0.0026 & 0.0001 & 0.0026 & 0.0001 & 0.0007 & 6.3170 \end{pmatrix}

Table 6. Screened Coulomb interaction matrix Uijij(H−s)U_{ijij}^{(H-s)} for the H-s subspace.

H siteSpread (Å2^2)UU (eV)
10.62786.0695
20.62596.2429
30.62936.3170
40.62596.2429
50.62936.3170
60.62596.2429
70.62936.3170

Table 7. Wannier spreads and onsite Hubbard UU for the H-s subspace.

Uijij(Lu−d)U_{ijij}^{(Lu-d)}(3.89590.36190.36220.55310.54580.36193.64190.46030.48510.46070.36220.46033.64170.48490.46060.55310.48510.48493.89640.30100.54580.46070.46060.30103.6416)\begin{pmatrix} 3.8959 & 0.3619 & 0.3622 & 0.5531 & 0.5458 \\ 0.3619 & 3.6419 & 0.4603 & 0.4851 & 0.4607 \\ 0.3622 & 0.4603 & 3.6417 & 0.4849 & 0.4606 \\ 0.5531 & 0.4851 & 0.4849 & 3.8964 & 0.3010 \\ 0.5458 & 0.4607 & 0.4606 & 0.3010 & 3.6416 \end{pmatrix}

Table 8. Screened Coulomb interaction matrix Uijij(Lu−d)U_{ijij}^{(Lu-d)} for the Lu-d subspace.

OrbitalSpread (Å2^2)UU (eV)
11.38013.8959
21.44093.6419
31.44083.6417
41.38003.8964
51.44103.6416

Table 9. Wannier spreads and onsite Hubbard UU for the Lu-dd subspace. Lu-dd sites show the 2 + 3 orbital grouping in spreads and onsite UU.

Calculated dielectric function of LuH₂ without and with octahedral hydrogen

Figure S5. Calculated dielectric function of LuH2_2 without (left) and with (right) octahedral hydrogen. (a) Re ε(ω)\varepsilon(\omega); (b) Im ε(ω)\varepsilon(\omega). In the tetrahedral-only structure, ε2\varepsilon_2 falls below unity between 1.0 and 2.2 eV and ε1\varepsilon_1 crosses zero within this window at 1.05 eV, giving a sharp, weakly damped plasma edge. Octahedral occupancy introduces an interband oscillator peaking at 1.05 eV inside this window, moving the zero crossing of ε1\varepsilon_1 down to 0.57 eV and raising ε2\varepsilon_2 at the crossing from ≈1\approx1 to ≈15\approx15, which damps the edge and splits the single absorptivity maximum of Figure 6 into the two observed features.

H siteSpread (Ų)UU (eV)
210.69536.9423
220.71997.2335
230.73197.6308
240.71997.2335
250.73197.6308
260.71987.2335
270.73197.6309

Table 10. Wannier spreads and onsite Hubbard UU for H-s orbitals in the combined Lu-d + H-s correlated subspace.

Lu atomOrbital indexSpread (Ų)Onsite UU (eV)
111.424370753.6296
121.546590423.6299
131.546622023.6299
141.424432763.6301
151.546622413.6292
261.424370673.6296
271.546555583.6298
281.546605483.6298
291.424432953.6301
2101.546596333.6291
3111.424371903.6296
3121.546552563.6297
3131.546530233.6297
3141.424432153.6301
3151.546575193.6290
4161.424373233.6296
4171.546529253.6297
4181.546525193.6297
4191.424431133.6301
4201.546579763.6290

Table 11. Wannier spreads and onsite Hubbard UU for Lu-d orbitals in the combined Lu-d + H-s correlated subspace.

RE-d subspaceH-s subspaceRE-d + H-s subspace
SystemUdU_d (eV)udu_d (eV)JdJ_d (eV)UHU_H (eV)uHu_H (eV)JHJ_H (eV)UU (eV)uu (eV)JJ (eV)
LuH₂4.30080.82100.09526.52190.36240.00145.16660.50720.0564
LaH₂3.32650.81400.07385.80310.24660.00094.81540.77860.0451
LuH₃4.45––8.89––9.1––
LaH₃4.69––8.40––7.45––

Table 12. Screened interaction parameters obtained from cRPA for LuHₓ and LaHₓ for x=2,3x = 2, 3. The table compares intra-orbital Hubbard UU, inter-orbital interaction uu, and Hund’s coupling JJ in the RE-d, H-s, and combined RE-d + H-s correlated subspaces.

SubspaceUtetU_{\mathrm{tet}}UoctU_{\mathrm{oct}}Utet−UoctU_{\mathrm{tet}} - U_{\mathrm{oct}}
H-s only9.218.25+0.96
Lu-dd + H-s12.2012.5−0.3

Table 14. Site-resolved H-s screened UU (eV) in LuH3_3, showing the inversion of the tetrahedral/octahedral ordering upon removal of RE-dd screening (H-s-only → combined subspace).

Table 15: H-ss correlation diagnostics. Occupation nn, atomic-state probabilities, instantaneous local moment ⟨m2⟩\langle m^2\rangle, and quasiparticle mass enhancement m∗/mm^*/m; local spin and charge susceptibilities χS\chi_S and χD\chi_D from the CTQMC solver at β=50 eV−1\beta= 50\ \mathrm{eV}^{-1}. Tetrahedral and octahedral H sites are treated as inequivalent impurities.

SystemSitennPdoubleP_{\mathrm{double}}⟨m2⟩\langle m^2\ranglem∗/mm^*/mχS\chi_SχD\chi_DχS/χD\chi_S/\chi_D
LuH1.75_{1.75}tet1.8330.8380.1571.1990.00520.00471.11
LuH2_2tet1.8070.8140.1791.2210.00580.00521.12
LuH2_2 (7tet+1oct)tet1.8480.8520.1451.2780.00460.00401.13
oct1.7200.7320.2571.3180.01290.00981.31
LuH2.25_{2.25}tet1.789–––0.00650.00581.13
oct1.645–––0.01690.01321.28
LuH2.875_{2.875}tet1.7990.8060.1871.2920.00630.00541.16
oct1.7310.7420.2461.2550.01210.00951.26
LuH3_3tet1.8120.8180.1761.3350.00570.00491.16
oct1.7580.7670.2241.3610.01040.00831.25
LaH3_3tet1.8300.8350.1611.3010.00610.00531.15
oct1.8870.8890.1101.1970.00550.00491.12

Table 15.

Table 16: RE-dd correlation diagnostics. Total dd-shell occupation nn and per-orbital occupations nt2gn_{t_{2g}}, negn_{e_g} from the converged density matrix; instantaneous local moment ⟨m2⟩\langle m^2\rangle (group total) and mass enhancement m∗/mm^*/m resolved by crystal-field set; local spin and charge susceptibilities χS\chi_S, χD\chi_D at β=50 eV−1\beta= 50\ \mathrm{eV}^{-1}. In the cubic field of the fluorite structure the ege_g set lies below t2gt_{2g} and is correspondingly the more occupied of the two at every composition.

Systemnnnorbn_{\mathrm{orb}} t2gt_{2g}norbn_{\mathrm{orb}} ege_g⟨m2⟩\langle m^2\rangle t2gt_{2g}⟨m2⟩\langle m^2\rangle ege_gm∗/mm^*/m t2gt_{2g}m∗/mm^*/m ege_gχS\chi_SχD\chi_DχS/χD\chi_S/\chi_D
LuH1.75_{1.75}1.5880.1880.4620.6420.9461.2111.2470.1990.0513.90
LuH2_21.4280.1230.4890.4271.0011.2781.2950.2170.0474.63
LuH2_2 (7tet+1oct)1.4170.2040.3600.6650.7531.2831.3200.2110.0395.42
LuH2.25_{2.25}1.2960.1370.405––––0.1610.0533.04
LuH2.875_{2.875}0.8300.1220.1860.4870.3431.2041.1990.0600.0311.93
LuH3_30.6790.1110.1220.4000.2791.1781.1610.0490.0301.67
LaH3_30.5310.0700.1050.3550.1751.2131.2030.0750.0411.84

Table 16.

Systemxx∑nH\sum n_{\mathrm{H}}ΔH\Delta_{\mathrm{H}}ndn_dΔd\Delta_dΔd−ΔH\Delta_d-\Delta_{\mathrm{H}}
LuH1.75_{1.75}1.7503.2080.2921.5880.3380.046
LuH2_22.0003.6140.3861.4280.4280.042
LuH2_2 (7tet+1oct)2.0003.6640.3361.4170.4170.081
LuH2.875_{2.875}2.8755.1130.6370.8300.7050.068
LuH3_33.0005.3820.6180.6790.6790.061
LaH3_33.0005.5470.4530.5310.5310.078

Table 17. Charge sharing between the hydrogen and RR-dd sublattices. For RHxRH_x the closed-shell ionic reference has every hydrogen as H−\mathrm{H}^{-}, giving ∑nHionic=2x\sum n_{\mathrm{H}}^{\mathrm{ionic}}=2x and ndionic=3−xn_d^{\mathrm{ionic}}=3-x per formula unit. The hydrogen deficit ΔH=2x−∑nH\Delta_{\mathrm{H}}=2x-\sum n_{\mathrm{H}} and the dd excess Δd=nd−(3−x)\Delta_d=n_d-(3-x) are obtained from Tables 15 and 16. The two track one another across the series with a correlation coefficient of 0.99; the residual Δd−ΔH=0.063±0.015\Delta_d-\Delta_{\mathrm{H}}=0.063\pm0.015 is constant to within its spread and equals the deviation of the total correlated-subspace occupation from the nominal valence count 3+x3+x, i.e. the weight lying outside the Wannier subspace. Charge missing from the hydrogen shell is thus recovered on the dd shell, establishing that the two sublattices are hybridized rather than ionically decoupled.

References

  1. [1]F. Aryasetiawan, T. Miyake, and R. Sakuma. The constrained RPA method for calculating the Hubbard U from first-principles. In Eva Pavarini, Erik Koch, Dieter Vollhardt, and Alexander Lichtenstein, editors, The LDA+DMFT approach to strongly correlated materials, volume 1 of Modeling and Simulation, chapter 7. Forschungszentrum Jülich, Jülich, 2011. ISBN 978-3-89336-734-4. URL https://www.cond-mat.de/events/correll11/manuscript/Aryasetiawan.pdf. Lecture Notes of the Autumn School 2011.
  2. [2]P. E. Blöchl. Projector augmented-wave method. Physical Review B, 50 (24):17953–17979, December 1994. doi: 10.1103/PhysRevB.50.17953. URL https://link.aps.org/doi/10.1103/PhysRevB.50.17953.DOI
  3. [3]M. Gupta and J. P. Burger. Electronic structure of the rare-earth hydrides LaH₂ and LaH₃. Phys. Rev. B, 22(12):6074–6084, 1980. doi: 10.1103/PhysRevB.22.6074.
  4. [4]G. Kresse and J. Furthmüller. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Physical Review B, 54 (16):11169–11186, October 1996. doi: 10.1103/PhysRevB.54.11169. URL https://link.aps.org/doi/10.1103/PhysRevB.54.11169.DOI
  5. [5]Xin Li, Ying Wang, Yuhao Fu, Simon A. T. Redfern, Shuqing Jiang, Pinwen Zhu, and Tian Cui. Stabilization of High-Pressure Phase of Face-Centered Cubic Lutetium Trihydride at Ambient Conditions. Advanced Science, 11 (29):2401642, 2024. ISSN 2198-3844. doi: 10.1002/advs.202401642. URL https://onlinelibrary.wiley.com/doi/abs/10.1002/advs.202401642. eprint: https://advanced.onlinelibrary.wiley.com/doi/pdf/10.1002/advs.202401642.DOI
  6. [6]Xin Liang, Zihan Lin, Jun Zhang, Jianfa Zhao, Shiyu Feng, Wenlong Lu, Guodong Wang, Luchuan Shi, Ningning Wang, Pengfei Shan, Zhao Zhang, Muntaser Naameh, Runzhe Liu, Bastien Michon, Jinguang Cheng, Changqing Jin, Yang Ren, and Junzhang Ma. Observation of flat band and van hove singularity in non-superconducting nitrogen-doped lutetium hydride, 2023. URL https://arxiv.org/abs/2308.16420.
  7. [7]J. Ma. private communication.
  8. [8]Arash A. Mostofi, Jonathan R. Yates, Young-Su Lee, Ivo Souza, David Vanderbilt, and Nicola Marzari. wannier90: A tool for obtaining maximally-localised Wannier functions. Computer Physics Communications, 178(9):685–699, May 2008. ISSN 0010-4655. doi: 10.1016/j.cpc.2007.11.016. URL https://www.sciencedirect.com/science/article/pii/S0010465507004936.DOI
  9. [9]John P. Perdew, Kieron Burke, and Matthias Ernzerhof. Generalized Gradient Approximation Made Simple. Physical Review Letters, 77(18):3865–3868, October 1996. doi: 10.1103/PhysRevLett.77.3865. URL https://link.aps.org/doi/10.1103/PhysRevLett.77.3865.DOI
  10. [10]E. Şaşıoğlu, C. Friedrich, and S. Blügel. Strength of the effective Coulomb interaction at metal and insulator surfaces. Phys. Rev. Lett., 109(16):166405, 2012. doi: 10.1103/PhysRevLett.109.166405.
  11. [11]Vijay Singh, Uthpala Herath, Benny Wah, Xingyu Liao, Aldo H. Romero, and Hyowon Park. DMFTwDFT: An open-source code combining Dynamical Mean Field Theory with various density functional theory packages. Computer Physics Communications, 261:107778, April 2021. ISSN 0010-4655. doi: 10.1016/j.cpc.2020.107778. URL https://www.sciencedirect.com/science/article/pii/S001046552030388X.DOI
  12. [12]A. C. Switendick. The change in electronic properties on hydrogen alloying and hydride formation. In G. Alefeld and J. Völkl, editors, Hydrogen in Metals I: Basic Properties, volume 28 of Topics in Applied Physics, pages 101–129. Springer, Berlin, 1978.DOI
  13. [13]P. Vajda. Hydrogen in rare-earth metals, including RH₂+x phases. In K. A. Gschneidner and L. Eyring, editors, Handbook on the Physics and Chemistry of Rare Earths, volume 20, chapter 137, pages 207–291. Elsevier, Amsterdam, 1995. doi: 10.1016/S0168-1273(05)80071-6.
  14. [14]Loïc Vaugier, Hong Jiang, and Silke Biermann. Hubbard U and Hund’s exchange J in transition metal oxides: Screening versus localization trends from constrained random phase approximation. Phys. Rev. B, 86(16):165105, 2012. doi: 10.1103/PhysRevB.86.165105.DOI
  15. [15]J. H. Weaver, R. Rosei, and D. T. Peterson. Electronic structure of metal hydrides. I. Optical studies of Sc H₂, Y H₂, and Lu H₂. Phys. Rev. B, 19(10):4855–4866, May 1979. ISSN 0163-1829. doi: 10.1103/PhysRevB.19.4855. URL https://link.aps.org/doi/10.1103/PhysRevB.19.4855.DOI

Paper details

vlnc:W_2zpdv6ag
Version
v1 · latest
Published
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents