betaFeedback

WorksPhysics and Astronomy

Combinatorial synthesis of cation-disordered manganese tin nitride MnSnN2_2 thin films with magnetic and semiconducting properties

Abstract

Magnetic semiconductors may soon improve the energy efficiency of computers, but materials exhibiting these dual properties remain underexplored. Here, we report the computational prediction and realization of a new magnetic and semiconducting material, MnSnN2_2, via combinatorial sputtering of thin films. Grazing incidence wide angle X-ray scattering and laboratory X-ray diffraction studies show a wide composition tolerance for this wurtzite-like MnSnN2_2, ranging from 20%<20\% < Mn/(Mn+Sn) <65< 65% with cation disorder across this composition space. Magnetic susceptibility measurements reveal a low-temperature transition (T∗≈10T^{\mathrm{*}} \approx 10 K) for MnSnN2_2 and strong antiferromagnetic correlations, although the ordering below this transition may be complex. This finding contrasts with bulk MnSiN2_2 and MnGeN2_2, which exhibited antiferromagnetic ordering above 400 K in previous studies. Spectroscopic ellipsometry identifies an optical absorption onset of 1 eV for the experimentally-synthesized phase exhibiting cation disorder, consistent with the computationally-predicted 1.2 eV bandgap for the cation-ordered structure. Electronic conductivity measurements confirm the semiconducting nature of this new phase by showing increasing conductivity with increasing temperature. This work adds to the set of known semiconductors that are paramagnetic at room temperature and will help guide future work targeted at controlling the structure and properties of semiconducting materials that exhibit magnetic behavior.

Introduction

Ternary nitrides are an emerging class of semiconducting materials. 1 In particular, II-IV-N2\mathrm{N_2} compounds offer a highly tunable platform that are structurally compatible with well-developed III-N technologies (e.g., GaN). 2,3 In the past few years, many new compounds were discovered in this phase space as thin films (e.g., MgTiN2\mathrm{MgTiN_2}, ZnMoN2\mathrm{ZnMoN_2}, ZnZrN2\mathrm{ZnZrN_2}), 4–6 bulk solids (e.g., CaSnN2\mathrm{CaSnN_2}, CaTiN2\mathrm{CaTiN_2}), 7,8 or both (e.g., MgSnN2\mathrm{MgSnN_2}, MgZrN2\mathrm{MgZrN_2}). 9–12 These particular compounds—with Mg2+\mathrm{Mg^{2+}}, Ca2+\mathrm{Ca^{2+}}, and Zn2+\mathrm{Zn^{2+}} as the divalent cation—have been investigated for their semiconducting properties. However, using transition metals with unpaired electrons—like Mn2+\mathrm{Mn^{2+}}—as the divalent cation may add technologically useful magnetic properties.

For example, magnetic semiconductors are of interest for applications in spintronic devices. 13 By using both charge and spin, spintronics may enable more energy efficient computing than traditional electronics, which rely on charge alone. While these devices have largely relied on ferromagnetic materials to record information in spins, ferromagnetic devices face the drawback of memory erasure if accidentally exposed to strong magnetic fields. 14 A breakthrough came in 2016, when Wadley, et al. reported the use of an antiferromagnetic material (CuMnAs\mathrm{CuMnAs}) to read and write information based on the direction of the anti-aligned spins. 15 Basing spintronic devices on antiferromagnetic materials comes with the benefit of rapid switching and robust storage, and is a promising direction for increasing the efficiency of computer processing. 16

II-IV-N2\mathrm{N_2} semiconductors with Mn2+\mathrm{Mn^{2+}} offer an underexplored platform for these antiferromagnetic spintronics. Bulk methods have been used to synthesize MnSiN2\mathrm{MnSiN_2} and MnGeN2\mathrm{MnGeN_2}, and these phases are known to be antiferromagnetic (AFM) semiconductors with Néel temperatures of TN=490T_N = 490 K and 448 K, respectively. 17,18 These materials take on a wurtzite-derived structure, with cations and anions in tetrahedral coordination environments. They are structurally analogous to GaN, suggesting the possibility of AFM spintronic integration into III-N based device stacks. In this vein, Liu, et al. reported epitaxial growth of MnGeN2\mathrm{MnGeN_2} films by molecular-beam epitaxy and identified magnetic properties that varied with composition and substrate. 19 However, much remains to be learned about the fundamental chemistry and physics of these materials.

We note that the tin-containing analogue, MnSnN2\mathrm{MnSnN_2}, has not yet been reported. Thus, the discovery of MnSnN2\mathrm{MnSnN_2} presents an opportunity to deepen our understanding of ternary II-IV-N2\mathrm{N_2} nitrides in general as well as the physics underlying this MnMN2\mathrm{MnMN_2} (M=SiM = \mathrm{Si}, Ge, Sn) wurtzite family in particular. With the powerful tool of combinatorial sputtering, we can answer questions like: How much off-stoichiometry can MnSnN2\mathrm{MnSnN_2} accommodate? How does the cation ratio affect the unit cell? How does cation disorder affect magnetism? To begin answering these questions, we report on our prediction, synthesis, and characterization of thin films of MnSnN2\mathrm{MnSnN_2}, a new paramagnetic semiconductor.

Methods

Computational methods

First-principles density functional theory (DFT) calculations were performed using the Vienna Ab initio Simulation Package (VASP). 20,21 Electronic structure and band gap calculations were performed using the GW approximation22 as described previously.23 Calculations were spin polarized to account for the expected magnetic moment of Mn. Computational results and details are available in the NREL Materials Database (https://materials.nrel.gov/), with ID 287033 (GW) and 287034 (DFT).

Synthesis

The Mn-Sn-N phase space was explored using combinatorial radiofrequency (RF) cosputtering methods. Libraries were deposited using an AJA International ATC 2200-V sputtering chamber. The chamber base pressure was between 2 and 5×10−85 \times10^{-8} Torr prior to depositions. During depositions, the pressure was maintained at 12±112 \pm1 mTorr with 15 sccm N2_2 and 5 sccm Ar. The N2_2 was activated by passing the gas through an electron-cyclotron resonance plasma source set at 150 W.

To create compositional gradients within each 2" × 2" sample library, metals were cosputtered from 3" diameter Mn and Sn targets aimed towards the substrate (Kurt J. Lesker; 99.95% and 99.998%, respectively). The substrate was held stationary during deposition, and the relative position of the sputtering targets (180° relative to one another in the plane of the substrate) resulted in 1-dimensional gradients in composition across the substrate. Prior to each deposition, the targets were presputtered for 30 min with the shutters closed. Subsequently, the shutters were opened and deposition was conducted for 120 min. The sample platens were heated with lamp heaters during the depositions, with substrate temperature denoted here as TdepT_{\mathrm{dep}}. This temperature was calibrated without sputtering, and therefore provides a lower bound for the sample temperature, as the impact of sputtered elements raises the substrate temperature. Depositions were conducted between Tdep=25T_{\mathrm{dep}} = 25 °C nominally (ambient conditions) and 275 °C. Cation composition was tuned by varying magnetron power, with Mn held at 108 W and Sn at either 36 W or 48 W. Most substrates were pp-type Si wafers with native surface oxide, although select samples were grown on Eagle Corning XG glass (EXG, optically transparent and electronically insulating) and pp-type Si with 100 nm of thermal oxide (electronically insulating) for certain property measurements as denoted in the text.

Characterization

Each 2" × 2" sample library was mapped as a 4×114 \times11 grid following the standard combinatorial mapping workflow at the National Renewable Energy Laboratory (NREL).24 Experimental data used by this study have been analyzed using the COMBIgor software package24 and are publicly available in the high-throughput experimental materials database at https://htem.nrel.gov.25

High-throughput X-ray diffraction (XRD) mapping was conducted using a Bruker D8 Discover (Cu Kα radiation) equipped with an area detector. High resolution synchrotron grazing incidence wide angle X-ray scattering (GIWAXS) measurements were conducted on select samples at beamline 11-3 of the Stanford Synchrotron Radiation Lightsource, SLAC National Accelerator Laboratory with λ=0.9744\lambda= 0.9744 Å, a 3° incident angle, and spot size of 50 microns vertical × 150 microns horizontal. GIWAXS images were integrated with GSAS-II.26 LeBail refinements were used to extract lattice parameters for MnSnN2_2 in the P63mcP6_3mc space group, performed with TOPAS Academic v6.27 Peak broadening was modeled via the Thompson-Cox-Hastings pseudo-Voigt “TCHZ” peak type as implemented in TOPAS. Reference patterns were generated using VESTA for visual comparisons.28 As the MnSnN2_2 phase has not been previously reported, we modeled the structure as follows: starting from the wurtzite AlN structure,[29] we replaced Al3+^{3+} with a 1:1 mixture of Mn2+^{2+} and Sn4+^{4+} and shifted the unit cell parameters to match the LeBail refinement for the near-stoichiometric MnSnN2_2 pattern (51% Mn/(Mn+Sn)). Those refined cell parameters are a=3.441a = 3.441 Å and c=5.562c = 5.562 Å (Table S1).

%  Mn/(Mn+Sn)\,\mathrm{Mn}/(\mathrm{Mn}+\mathrm{Sn})Molar Mass (g/mol\mathrm{g/mol})Thickness (μm\mu\mathrm{m})aa (A˚\mathrm{\AA})cc (A˚\mathrm{\AA})T∗T^* (K)
422120.3053.4495.6676
512010.3043.4415.56210
561940.3023.4385.53612

Table S1. Summary of composition, thickness, hexagonal lattice parameters, and magnetic transition temperatures (T∗T^*) for the samples selected for magnetic measurements.

Compositional analysis was performed with X-ray fluorescence (XRF) and Rutherford Back-Scattering (RBS) methods. Metal ratios were mapped using a Fischer XDV-SDD XRF with a Rh source and a 3 mm diameter spot size. The measurements were performed at ambient pressure with an exposure time of 60 s for each measurement. Nitrogen and oxygen ratios for select samples were quantified with RBS. RBS was run in a 168° backscattering configuration using a model 3S-150 RBS system from National Electrostatics Corporation with a 2 MeV He+^{+} beam energy. Samples were measured for a total integrated charge of 160 uC. RBS spectra were modeled with the RUMP software package.[30] Agreement on metal ratios between XRF and RBS are shown in Figure S8. A representative RBS spectrum and fit are shown in Figure S9.

XRF and RBS measurements

Figure S8. A) XRF measurements of % Mn/(Mn+Sn) agree well with measurements by RBS. The grey trace represents perfect agreement between the techniques. Blue squares are the data. B) RBS measurements of % O/(N+O) show that the proportion of oxygen content increases slightly with increasing Mn content.

Representative RBS data and fits

Figure S9. Representative RBS data (black traces) of one sample and fits (red traces) following different fitting procedures. A) Fit by freely varying a fuzz parameter, film thickness, and relative amounts of Mn, N, O, normalized to Sn = 1. The minimization overfits the anion content, leading to an unreasonable ratio of (N+O)/(Mn+Sn) = 1.6 (expecting 1 for the wurtzite structure). B) Fitting the same data by refining thickness and Mn content and constraining N content to N = Mn+Sn (i.e., Sn = 1, Mn = 0.8, N = 1.8). While the lack of a fuzz parameter leads to poor fitting of curvature, the constrained anion content still produces a reasonable fit to the intensity in the 0.5 MeV region. Quantitative assessment of low-atomic number anion content is therefore tricky given the low signal and high background. However, these data show a non-zero oxygen content with a substantially larger proportion of nitrogen content.

Film thicknesses were measured using a Dektak profilometer and were approximately 200 to 300 nm following 2 h growth times. Cross-sectional scanning electron microscopy (SEM) was conducted for select samples on a Hitachi S-4800 SEM operating at 3 keV accelerating voltage and 8 mm working distance to corroborate film thickness measurements and identify film morphology.

DC magnetic susceptibility was measured in a Quantum Design Magnetic Properties Measurement System (MPMS3) via vibrating sample magnetometry. The films were measured from 2 K to 300 K under applied fields from -7 to +7 T, with the applied field parallel to the plane of the film. The measured samples were 5 mm × 5 mm squares from a sample library deposited at Tdep=225T_{\mathrm{dep}} = 225 °C on a substrate of 100 nm of SiO2_2 on pSi(100). Each square was characterized by XRF and synchrotron GIWAXS to ensure magnetic properties were accurately correlated with composition and structure. To isolate the signal of the films, a bare substrate (100 nm of SiO2_2 on pSi(100)) was also measured and subtracted (Figure S11 and S12). Additional analysis details are in the Electronic Supplementary Information.

Background subtraction example for zero-field cooled temperature sweeps

Figure S11. Background subtraction example for zero-field cooled temperature sweeps measured at μ0H=5\mu_0 H = 5 T. The raw moments of the sample and a blank substrate are shown, along with the background-subtracted data showing magnetism from the film alone (sample − blank).

Room temperature conductivity was measured using a custom built collinear four-point probe instrument by sweeping current between the outer two pins while measuring voltage between the inner pins (1 mm between each pin). Conventional geometric corrections were applied to convert the measured resistance into sheet resistance and then conductivity.[31] Error bars are propagated from sheet resistance error (from I-V curve fits) and an estimated 5% relative error in profilometry thickness measurements.

Temperature-dependent electrical conductivity was measured using a Lake Shore Cryotronics Model 8425. A 5 mm × 5 mm square was scribed out of a library deposited on EXG at approximately 200 °C. Although the deposition temperature on EXG was not calibrated, XRD patterns appeared similar to those deposited on at a calibrated Tdep=225T_{\mathrm{dep}} = 225 °C on silicon (i.e., XRD showed only MnSnN2_2 with no signs of Sn or Mn3_3N2_2 decomposition products). Indium contacts were pressed into the square near the corners of the film, and temperature-dependent sheet resistance was measured from 104 K to 298 K. Conductivity was calculated using the profilometry-measured thickness of 260 nm.

Spectroscopic ellipsometry was performed on a single row of a select sample library (11 points per row) using a J.A. Woollam Co. M-2000 variable angle ellipsometer. CompleteEASE software (version 6.56) was used to do the modeling. The data were modeled by fitting the imaginary part of the dielectric function with a combination of one Tauc-Lorentz, one Gaussian, and one Drude oscillator.

Results and Discussion

Computational findings

To investigate the stability of a possible MnSnN2_2 phase, we performed density functional theory (DFT) calculations. We hypothesized that this phase would form in the wurtzite-derived structure and therefore constructed a cation-ordered MnSnN2_2 structure in the orthorhombic space group Pna21Pna2_1. DFT calculations suggest that this cation-ordered orthorhombic MnSnN2_2 is slightly metastable (+0.038 eV/atom above the hull, Figure 1A). Therefore, a traditional bulk synthetic approach of reacting Mn and Sn under 1 atm of N2_2 would likely fail. However, sputtering

Phase diagram and density of states for MnSnN2

Figure 1. A) A pseudobinary phase diagram of the space from Sn3_3N4_4 to Mn3_3N2_2 at T=0T = 0 K. The solid blue trace shows the hull under activated nitrogen conditions (μN=+1\mu_{\mathrm{N}} = +1 eV/atom), as occurs in plasma synthesis. [32, 33] Cation-ordered MnSnN2_2 is more stable than a linear combination of these two binary nitrides. B) Total density of states calculated for cation-ordered MnSnN2_2 in the Pna21Pna2_1 space group. The calculated band gap (EgE_{\mathrm{g}}) is 1.22 eV, shown in grey. N-p and Mn-d states comprise the valence band, while the conduction band consists of Sn-s and N-p states.

in an activated nitrogen atmosphere (i.e., a N2_2 plasma) stabilizes metastable phases (e.g., Cu3_3N and Sn3_3N4_4) by increasing the chemical potential of nitrogen up to +1 eV/atom. [32, 34] Figure 1A shows that while MnSnN2_2 is metastable with respect to Sn+N2_2 and Mn3_3N2_2, the phase is stable with respect to Sn3_3N4_4 and Mn3_3N2_2. Therefore, the nitrogen plasma environment that rendered Sn3_3N4_4 synthetically accessible should also stabilize MnSnN2_2.

Our calculations also suggest that MnSnN2_2 should exhibit semi-conducting properties and antiferromagnetic behavior. The calculated bandgap is 1.22 eV (Figure 1B), with a density of states (DOS) effective hole mass of mh∗=5.9m0m_{\mathrm{h}}^* = 5.9m_0. The band effective mass is me∗=0.22m0m_{\mathrm{e}}^* = 0.22m_0. The low electron mass is remarkable for a transition metal compound (Mott insulator), but not uncommon for Mn2+^{2+}. [35, 36] The local magnetic moment is calculated as μeff=4.3 μB\mu_{\mathrm{eff}} = 4.3\,\mu_{\mathrm{B}} per Mn. This μeff\mu_{\mathrm{eff}} is less than the spin-only value expected for high-spin Mn2+^{2+} (S=52S = \frac{5}{2}; μeff=5.9 μB\mu_{\mathrm{eff}} = 5.9\,\mu_{\mathrm{B}}), indicating that some spin density resides on the nitrogen sites. The four Mn atoms per cell exhibit antiferromagnetic order in the ground state, resulting in a net moment of 0 μB\mu_{\mathrm{B}} per cell.

Synthesis and structure of MnSnN2 thin films

Stability and cation disorder

We synthesized MnSnN2_2 films using combinatorial sputtering and assessed the crystallinity using X-ray diffraction techniques (synchrotron GIWAXS and laboratory XRD). Synchrotron GIWAXS of stoichiometric films shows that MnSnN2_2 crystallizes in a phase-pure cation-disordered wurtzite structure at Tdep=225T_{\mathrm{dep}} = 225 °C (Figure 2A,C). The absence of supercell reflections (peaks near Q=1.5Q = 1.5 Å−1^{-1}) of the Pna21Pna2_1 space group indicate that long-range ordering of cations in MnSnN2_2 does not occur in these samples (Figure 2B,C). Above Tdep=225T_{\mathrm{dep}} = 225 °C, Sn and Mn3_3N2_2 are also observed in the diffraction patterns, while below 225 °C, the material is poorly crystalline. These trends are true across the compositional gradient (Figure S4). This relatively low decomposition temperature (Tdep∼250T_{\mathrm{dep}} \sim250 °C) suggests that MnSnN2_2 is less stable than related ternary nitrides like MgSnN2_2 (stable up to 500 °C in the same deposition chamber) 9 and ZnSnN2_2 (stable up to 340 °C). [37] Annealing experiments under flowing N2_2 suggest that, once deposited, MnSnN2_2 films are stable up to Tanneal=300T_{\mathrm{anneal}} = 300 °C, but decomposition is still observed by Tanneal=400T_{\mathrm{anneal}} = 400 °C (Figure S6).

Unit cells and GIWAXS data for MnSnN2

Figure 2. A) The unit cell of MnSnN2_2 in the experimentally observed cation-disordered hexagonal structure (P63mcP6_3mc), and the B) computationally predicted ordered orthorhombic structure (Pna21Pna2_1). C) Synchrotron GIWAXS data of samples with Mn/(Mn+Sn) = 50% deposited at various temperatures (TdepT_{\mathrm{dep}}) are shown in the bottom box, with reference patterns shown in the top box. The optimal deposition temperature for single phase crystalline MnSnN2_2 (P63mcP6_3mc) is Tdep=225T_{\mathrm{dep}} = 225 °C. The ordered MnSnN2_2 (Pna21Pna2_1) phase is not observed.

GIWAXS phase-presence patterns for MnSnN₂, Sn, and Mn₃N₂

Figure S4. GIWAXS patterns were collected on select points from a variety of libraries. Manual inspection revealed the predominance of a single phase, MnSnN2\mathrm{MnSnN}_{2} up to 225 °C. However, at higher temperatures, the MnSnN2\mathrm{MnSnN}_{2} phase begins decomposing into Mn3N2\mathrm{Mn}_{3}\mathrm{N}_{2} and Sn. The coexistence of all three suggests non-equilibrium conditions.

Rapid thermal annealing experiments

Figure S6. Rapid thermal annealing experiments show that a library row synthesized at Tdep=225T_{\mathrm{dep}} = 225 °C is stable up to an annealing temperature of 300 °C. Annealing experiments were conducted on individual rows from a library, first heated to 100 °C to drive off adsorbed water, then heated to the TannealT_{\mathrm{anneal}} temperature for a 30 min anneal. Heating ramps for each step were conducted in 1 minute, and cooling occurred by turning the power to the furnace off. The sample was enclosed in flowing N2\mathrm{N}_2 for the duration of the experiment.

We conducted these annealing experiments in an attempt to induce cation ordering, [38] but saw no evidence of cation order below the decomposition temperature of Tanneal=400T_{\mathrm{anneal}} = 400 °C (Figure S6). By the methods applied here, long-range cation ordering of MnSnN2_2 appears inaccessible. In contrast, the bulk synthesis methods employed for MnSiN2_2 and MnGeN2_2 yielded cation-ordered phases (space group Pna21Pna2_1). 17,18 The prior report on thin films of MnGeN2_2 did not assess cation ordering via diffraction. 19

The lack of long-range cation ordering exhibited by MnSnN2_2 is common in sputtered films. MgSnN2_2 and ZnSnN2_2 thin films are both cation disordered, [37] [9] and ZnGeN2_2 forms as a cation-disordered thin film but crystallizes in the ordered Pna21Pna2_1 structure when synthesized by bulk ammonolysis. [39, 40] The high effective temperature of the sputtering synthesis technique, along with the entropic benefit of disorder, can stabilize a disordered structure by approximately 0.1 eV/atom relative to the DFT-predicted ordered structures. 6 II-Sn-N2_2 phases in particular have a tendency for disorder because Sn4+^{4+} is closer in ionic radius (0.55 Å) to the divalent cations—Mn2+^{2+} (0.66 Å), Mg (0.57 Å), and Zn (0.60 Å)—than the other main group elements—Ge4+^{4+} (0.39 Å) and Si4+^{4+} (0.26 Å). [41, 42] [9] This size similarity leads to cation disorder even in bulk MgSnN2_2. 10 While short-range ordering is possible even with the absence of a supercell reflection and may impact properties, [38, 43, 44] such analysis is beyond the scope of this study.

Compositional and structural trends

Despite this low thermal stability, the wurtzite structure of MnSnN2_2 accommodates a wide range of cation off-stoichiometry (18% < Mn/(Mn+Sn) < 65%) when deposited at the optimal temperature of Tdep=225T_{\mathrm{dep}} = 225 °C. Within the composition range of Mn/(Mn+Sn) = 38% to 65%, all reflections in the GIWAXS patterns can be indexed to P63mcP6_3mc symmetry (Figure 3). In laboratory XRD, we observe MnSnN2_2 down to Mn/(Mn+Sn) = 18% (the Mn-poor limit of the library, Figure S7). However, this may not be the true lower compositional limit of this phase. In contrast, we have determined that the upper limit of Mn content in MnSnN2_2 by diffraction is Mn/(Mn+Sn) ≈ 65%. At high Mn content (> 65%), the lattice parameters of MnSnN2_2 plateau and the uncertainty in the refinement grows (Figure 3C and Figure S3). Broad peaks that index to Mn3_3N2_2 also appear, indicative of a two-phase region. The only other known Mn-Sn-N ternary compound is the antiperovskite Mn3_3SnN (Mn/(Mn+Sn) = 75%), [45, 46] which is more Mn-rich than our depositions and does not appear in our diffraction patterns.

Synchrotron GIWAXS data and lattice-parameter analysis

Figure 3. A) Synchrotron GIWAXS data of select samples from a combinatorial library row deposited at Tdep=225T_{\mathrm{dep}} = 225 °C shows that reflections can be indexed to the P63mcP6_{3}mc space group, indicative of a cation-disordered wurtzite structure. B) Magnified QQ range of the diffraction patterns, showing the shift in the (002) reflection with changing Mn/(Mn+Sn). C) The cc axis contracts relative to the aa axis with increasing Mn content, which causes the c/ac/a ratio to decrease. The vertical dotted line indicates the composition of stoichiometric MnSnN2_2 and the horizontal dashed line indicates the ideal c/ac/a ratio of the wurtzite structure (8/3\sqrt{8}/3). Fits to the data are shown in Figure S2.

Extracted lattice parameters and residuals from LeBail refinements

Figure S3. A) Extracted lattice parameters aa (green circles) and cc (gold squares) from LeBail refinements used to calculate the c/ac/a ratio in Figure 3C. Error bars are within the size of the markers. B) Residuals from the LeBail refinements presented in Figure S2. The modeled P63mcP6_{3}mc phase fits best with the slightly Mn-rich composition. Anisotropic peak broadening worsens the fit in the Mn-poor region. A poorly crystalline Mn3_3N2_2 secondary phase, which was not included in the model, worsens the fit in the Mn-rich region.

Diffraction patterns of a library deposited under Mn-poor conditions

Figure S7. A library deposited under Mn-poor conditions at Tdep=225T_{\mathrm{dep}} = 225 °C show the continued presence of wurtzite peaks. A structural change to the spinel Sn3N4\mathrm{Sn}_3\mathrm{N}_4 is not observed, although prior sputtering syntheses of this binary phase revealed poor crystallinity of binary Sn-N nitrides.[33]

This wide range of off-stoichiometry can make naming ternary nitrides difficult, as noted by Wood-Robinson, et al. 6 A precise formula would be Mnx_xSn1−x_{1-x}N1−y_{1-y}Oy_y, where xx is the cation fraction of Mn/(Mn+Sn) and yy is the amount of oxygen substitution for nitrogen (estimated to be y≈0.2y \approx0.2 by RBS, Figure S8B). The oxygen likely originates from oxide contamination of the Mn sputter target, and either charge balances with Mn2+^{2+} via (MnSnN2_2)1−x_{1-x}(MnO)x_x or with Mn3+^{3+} via Mn1+x_{1+x}Sn1−x_{1-x}N2−x_{2-x}Ox_x. For simplicity, we use “MnSnN2_2” to refer to the cation-disordered wurtzite-like phase across the whole composition range and specify a cation fraction as a percentage of Mn/(Mn+Sn) where relevant (i.e., stoichiometric MnSnN2_2 has Mn/(Mn+Sn) = 50%).

The c/ac/a ratio of MnSnN2_2 varies with composition, but deviates only slightly from the ideal wurtzite value of 1.633 (Figure 3C). For stoichiometric MnSnN2_2, c/a=5.562c/a = 5.562 Å / 3.441 Å = 1.616, which—although smaller than the ideal wurtzite—is larger than MgSnN2_2 (1.598). 9 The change in c/ac/a is driven primarily by a change in the cc lattice parameter while the aa lattice parameter remains largely unchanged (Figure S3A), suggesting that the tetrahedra may be distorting along the cc axis. That shift may be caused by metal vacancies, a change in electron count of the metals, oxygen incorporation (observed by RBS, Figure S8B), or some combination thereof as the system shifts to maintain charge neutrality across this compositional range. However, since atomic positions cannot be resolved from the synchrotron GIWAXS data sets, we cannot more precisely identify the cause of this distortion.

To probe the microstructure of the film, we turn to electron microscopy and diffraction analysis. SEM shows columnar grain morphology that is typical for sputtered films (Figure 4). Diffraction images display some signs of texturing (Figure S1). The (002) reflection appears towards the edges of the integration window, suggesting the {002} planes are oriented normal to the plane of the substrate. In contrast, the (100) reflection appears strongly in the center axis of the frame, 90° relative to the (002) reflection, and diminishes in intensity towards the edge of the integration window, suggesting preferential growth along the [100] direction (Figure 3B). This finding stands in contrast to typical wurtzite films, which tend to grow with (002) preferential orientation. [37, 47]

Cross-sectional SEM micrograph of columnar grains

Figure 4. Cross-sectional SEM micrograph showing columnar grains typical of sputtered films. This representative image shows a 50% Mn/(Mn+Sn) film deposited on a silicon substrate with 100 nm of SiO2_2. The scale bar is 300 nm.

A representative 2-D diffraction image from a GIWAXS measurement at SSRL beamline 11-3

Figure S1. A representative 2-D diffraction image from a GIWAXS measurement at SSRL beamline 11-3. Hot pixels are masked in red to avoid background contribution to the integrated diffraction pattern. The first six reflections of MnSnN2_2 are also labeled. Strong spots from the Si substrate (331) planes are visible near the edge of the frame.

Magnetic properties

Given the presence of tetrahedrally coordinated Mn2+^{2+} (expected: S=52S = \frac{5}{2} and μeff=5.9 μB\mu_{\mathrm{eff}} = 5.9\,\mu_{\mathrm{B}}) cations in stoichiometric MnSnN2_2, as well as the possible presence of Mn3+^{3+} (expected: S=2S = 2 and μeff=4.9 μB\mu_{\mathrm{eff}} = 4.9\,\mu_{\mathrm{B}}) in Mn-rich compositions, DC magnetic susceptibility was employed to investigate the magnetic response of several thin films with a range of compositions 42% ≤ Mn/(Mn+Sn) ≤ 56%. We cannot independently determine the film mass, so susceptibility (χ\chi) was calculated from the raw moment data using the same estimated mass (0.04 mg) for each sample. Uncertainty in film thickness, composition, and porosity may introduce substantial error in the calculated mass of the films, and by extension, the absolute value of χ\chi. In addition, each measured sample contains a compositional gradient of approximately 4% Mn/(Mn+Sn). Despite these caveats, errors from sample to sample are likely systematic, allowing us to identify trends in magnetism related to composition. Additional details and discussion are in the Electronic Supplementary Information (Section 3).

As shown in Figure 5A, zero-field-cooled (ZFC) temperature-dependent susceptibility measurements performed at high applied field exhibit peaks near 10 K, indicating a magnetic transition (T∗T^*). The T∗T^*, extracted as the temperature where χ\chi reaches a maximum, increases slightly with increasing Mn content, from T∗≈6T^* \approx6 K at 42% Mn to T∗≈12T^* \approx12 K at 56% Mn (Figure 5B). Curie-Weiss fits in the paramagnetic region 150–300 K (see inset of Figure 5A and Figure S13) show large, negative Weiss temperatures (ΘCW\Theta_{\mathrm{CW}}, Figure 5B), consistent with overall antiferromagnetic (AFM) correlations. However, the uncertainties in background subtraction and in the calculation of χ\chi inhibit meaningful extraction of Curie constants and effective moments from these fits (see Electronic Supplementary Information Section 3). The magnitude of χ\chi decreases with increasing Mn fraction, which would be consistent with Mn3+^{3+} replacing Mn2+^{2+}. However, we are not able to detect a significant amount of Mn3+^{3+} in XANES measurements (Figure S10). This apparent shift in χ\chi may therefore be an artifact of the uncertainty in film mass. Measurements in lower applied field (μ0H=0.1\mu_{0}H = 0.1 T; Figure 5C) show clear bifurcation in ZFC and field-cooled (FC) susceptibility below the transition temperature, which is consistent with either long-range AFM order or a spin-glass ground state.

Zero-field-cooled and field-cooled magnetic susceptibility measurements

Figure 5. A) Zero-field-cooled (ZFC) DC magnetic susceptibility (χ\chi) as a function of temperature measured in an applied field of μ0H=5\mu_0H = 5 T, show a peak in χ\chi at T∗≈10T^* \approx10 K across a range of Mn contents. The inset shows χ−1\chi^{-1} as a function of temperature with a diamagnetic correction χ0=−5.5×10−3\chi_0 = -5.5 \times10^{-3} emu Oe−1^{-1} mol−1^{-1} for 51% Mn/(Mn+Sn). The dashed trace shows the Curie-Weiss fit from 150 K to 300 K. B) Extracted transition temperatures (T∗T^*, left axis) and Weiss temperatures (ΘCW\Theta_{\mathrm{CW}}, right axis) as a function of increasing Mn content. C) ZFC and field-cooled (FC) DC magnetic susceptibility measurements at lower applied field of μ0H=0.1\mu_0H = 0.1 T show bifurcation below the transition temperature.

XANES total electron yield and partial fluorescence yield spectra

Figure S10. The XANES total electron yield (A) and partial fluorescence yield (B) of the Mn-LL edge shows that all three samples used for the magnetism measurements have similar spectral profiles. This profile matches Mn2+^{2+} compounds in literature. [56, 57] Subtle differences can be seen on the peak shoulders of the L3 edge, but these shifts are near the noise level of the measurement.

Inverse susceptibility data and Curie-Weiss fits

Figure S13. A) Inverse susceptibility plotted without a diamagnetic correction factor shows significant non-linearity. Inverse susceptibility data and Curie-Weiss fits performed with a diamagnetic correction (χ0\chi_0) between B) 150–300 K C) 50–150K. The fits are shown as solid bars. Parameters ΘCW\Theta_{\mathrm{CW}} and χ0\chi_0 are shown in Table S2.

The magnetic moment measured as a function of applied field at T=2T = 2 K (below the transition at T∗≈10T^* \approx10 K) is consistent with AFM correlations, shown for Mn/(Mn+Sn) = 51% in Figure 6 and for the remaining samples in Figure S14. In the T=2T = 2 K data of all samples measured, there is small but observable hysteresis with a minute net moment at zero field (inset of Figure 6). This net moment may originate from spin canting, uncompensated moments from defects, the Dzyaloshinsky-Moriya interaction, or slow magnetic relaxation of a spin glass state. Similar net moments were observed in thin films of MnGeN2_2 and were attributed to cation site disorder.19 Above T∗T^*, (e.g., at T=40T = 40 K), the linear behavior is consistent with paramagnetism. The traces do not plateau at high fields, indicating that the magnetic moment is not saturated at μ0H=±7\mu_{0}H = \pm7 T.

Background-subtracted isothermal magnetization measurements

Figure 6. Background-subtracted isothermal magnetization measurements of near-stoichiometric MnSnN2_2 at T=2T = 2 K (solid circles) and T=40T = 40 K (open circles). The inset details the small net ferromagnetic moment at T=2T = 2 K and the absence of such net moment at T=40T = 40 K.

Isothermal magnetic moment measurements at 2 K of MnSnN₂ samples

Figure S14. Isothermal magnetic moment measurements at 2 K of MnSnN2_2 samples show decreasing moment with increasing Mn content. Traces are offset horizontally by μ0H=3\mu_0 H = 3 T for clarity (grey lines guide the eye to each origin). The substrate contribution has been subtracted.

Overall, the susceptibility measurements and Curie-Weiss fit results point to clear, strong AFM correlations in MnSnN2_2 with a transition at approximately T∗≈10T^* \approx10 K. This transition shifts as a function of Mn/(Mn+Sn). We are unable to determine whether the ground state below this transition temperature is long-range AFM order or spin glass. [48] If the ground state is an ordered AFM, it would likely be complex, especially given the cation disorder and compositional gradients in these samples. The small net moment observed at T<T∗T < T^* may imply the presence of spin canting, Dzyaloshinsky-Moriya interactions, or uncompensated residual spins, as mentioned above, and the ZFC-FC splitting suggests a relaxation process. However, the Mn content in these samples (41–56%) is well above the percolation threshold (20% for this hexagonal close packed metal sublattice), [49] so the AFM correlations likely extend throughout the crystalline domains. To probe the possibility of spin glass behavior, we performed AC susceptibility measurements, but the signal was below the instrumental sensitivity limit.

The low-temperature magnetic transition (T∗≈10T^* \approx10 K) of the cation-disordered MnSnN2_2 thin films examined here contrasts starkly with the high-temperature AFM ordering of cation-ordered MnGeN2_2 (TN=448T_{\mathrm{N}} = 448 K) and MnSiN2_2 (TN=490T_{\mathrm{N}} = 490 K) synthesized as bulk single crystals. 17,18 To explain these differences, we posit that cation ordering is an important factor in determining the energy scale of magnetic order in this family of wurtzite ternary nitrides. That influence may be exerted via magnetic frustration, if the ground state is AFM order: the tetrahedrally-based lattice of Mn2+^{2+}, together with the large ratio of the Weiss temperatures (ΘCW≈−200\Theta_{\mathrm{CW}} \approx-200 K) and the low transition temperatures (T∗≈10T^* \approx10 K) of these films, suggest the presence of a high degree of magnetic frustration. [48, 50] This is not unexpected, as triangular-based lattices are one of the most common hosts of geometric frustration, and frustration also often arises from cation disorder. [51, 52] In addition, frustration was observed even in the cation-ordered MnSiN2_2. 17 Should bulk powders or single crystals of MnSnN2_2 be synthesized, comparing their magnetic properties and defect chemistry with the thin film behavior observed here would be illuminating.

Optoelectronic properties

Room temperature conductivity measurements show that the MnSnN2_2 films exhibit conductivity on the order of 20 S/cm (Figure 7A). Conductivity decreases slightly as Mn content increases from 38% to 60% Mn/(Mn+Sn) but then increases as a metallic secondary phase (Mn3_3N2_2) grows in. This increase in conductivity for Mn/(Mn+Sn) ≥60%\ge60\% suggests that the true single-phase region may have a lower Mn limit (∼60%\sim60\% maximum) than detected by GIWAXS (∼65%\sim65\% maximum). For the Mn/(Mn+Sn) <60%< 60\% region, conductivity is likely tuned by carrier concentration. Prior work on ZnSnN2_2 demonstrated that a similar trend (decreasing conductivity with increasing Zn) was correlated with a decrease in carrier concentration (while mobility was unaffected). [37] In both cases (MnSnN2_2 and ZnSnN2_2), the conductivity reaches a minimum in the Sn-poor region (i.e., Zn or Mn ≈60%\approx60\%), as the excess Zn or Mn compensate for oxygen substitution on nitrogen sites. At Mn/(Mn+Sn) = 60%, the charge-balanced chemical formula is Mn0.6_{0.6}Sn0.4_{0.4}N0.8_{0.8}O0.2_{0.2} (assuming Mn2+^{2+} and Sn4+^{4+}), consistent with the oxygen content identified by RBS (Figure S8B).

Conductivity and optical absorption measurements

Figure 7. A) Room temperature conductivity measurements performed in a collinear four-point probe configuration show that conductivity initially decreases slightly with increasing Mn content, then increases rapidly above 60% Mn/(Mn+Sn). B) Conductivity increases as a function of temperature, confirming the semiconducting nature of MnSn2_2 films. The anomaly in slope near 250 K is an instrumental artifact. C) Optical ellipsometry measurements indicate a gradual absorption onset, with minima in the absorption coefficients near 1 eV.

Temperature-dependent conductivity measurements performed in Van der Pauw geometry on films grown on insulating EXG glass show that the conductivity increases with increasing temperature, confirming semiconducting behavior in MnSnN2_2 (Figure 7B). Increasing conductivity with increasing temperature suggests that mobile carriers are thermally activated (i.e., a bandgap is present in the material). However, the conductivity is only weakly dependent on temperature, with the conductivity at 298 K only 30% greater than the conductivity at 104 K.

Ellipsometry measurements and modeling show that MnSnN2_2 has a gradual absorption onset near 1 eV (Figure 7C). Overall, the absorptivity increases slightly with increasing Mn content, although the absorption onset stays relatively constant. This absorption onset may be attributable to a bandgap, as the bandgap for this material is expected to be lower than the experimentally reported bandgaps in cation-ordered MnSiN2_2 (3.5 eV) and MnGeN2_2 (2.5 eV). [53] The DFT-calculated bandgap for cation-ordered MnSnN2_2 is 1.22 eV (Figure 1B), and the cation-disorder of the material synthesized here leads to lower the bandgap relative to cation-ordered analogues. [38] However, Mn2+^{2+} dd-dd transitions are also known to occur in this energy region, 17 and unfortunately, this technique cannot distinguish between single-ion electronic transitions and bandgap excitations. We also attempted UV-vis measurements of films deposited on transparent substrates to verify the optical absorption onset, but the onset was below the limit of the instrument (Figure S15). Regardless, the optoelectronic and magnetic behavior of this new compound present opportunities for further study.

Photo of a library and reflectance, transmittance, and absorbance spectra

Figure S15. A) Photo of a library deposited on a 2×22 \times2" Eagle XG glass substrate. The library was deposited at a set point of 250 °C, which corresponds to a substrate temperature of < 225 °C as evidenced by the lack of decomposition of the MnSnN2_2 phase (confirmed by XRD). The film is dark brown in color. B) Reflectance RR and C) Reflection-corrected transmittance TT were used to calculate the absorbance via Absorbance A=ln⁡T1−RA = \ln\frac{T}{1-R}, as implemented in Combigor. 24 D) The absorbance is high across measurable range. The colorbar shown in panel B is used for panels C and D as well.

Conclusions

We have synthesized thin films of a new ternary nitride material, MnSnN2_2, using combinatorial co-sputtering. The material crystallizes in a cation-disordered wurtzite-like structure common for II-IV-N2_2 semiconductors with lattice parameters a=3.441a = 3.441 Å and c=5.562c = 5.562 Å for the stoichiometric material. MnSnN2_2 exhibits semiconducting properties, including a bandgap near 1 eV—the lowest bandgap yet observed in the MnMN2_2 wurtzite family. [53] We observe a magnetic transition in cation-disordered MnSnN2_2 at low temperature (T∗≈10T^* \approx10 K) consistent with AFM correlations, which contrasts dramatically with the high AFM ordering temperatures of cation-ordered MnGeN2_2 and MnSiN2_2 (TN=448T_N = 448 K and 490 K, respectively). 17,18 These discoveries suggest that future work could use composition and cation disorder in the Mn-MM-N2_2 (MM = Si, Ge, Sn) system to tune both semiconducting and magnetic properties.

Author Contributions

J.S.A. and A.C.T. conceived of the project. J.S.A. and C.L.R. conducted depositions, XRF, and XRD measurements. C.L.R. and R.W.S conducted magnetism and electronic conductivity measurements. R.R.S. and C.L.M. conducted ellipsometry measurements. L.T.S. and C.L.R. conducted synchrotron GIWAXS measurements. K.N.H. conducted RBS analysis. J.S.M. conducted microscopy. S.J.-L. conducted XAS measurements. S.L. conducted DFT calculations. C.L.M. and A.L.G. aided in synthesis and maintenance of the deposition chamber. C.L.R. and R.W.S. wrote the majority of the manuscript with guidance from S.R.B., J.R.N., A.C.T., and J.S.A as well as feedback from all other authors.

Conflicts of interest

There are no conflicts of interest to declare

Acknowledgements

This work was authored in part by the National Renewable Energy Laboratory (NREL), operated by Alliance for Sustainable Energy, LLC, for the U.S. Department of Energy (DOE) under Contract No. DE-AC36-08GO28308. Primary funding was provided by the U.S. Department of Energy, Office of Science, Basic Energy Sciences, Materials Sciences and Engineering Division. C.L.R. acknowledges support from the DOE Science Graduate Research Program (SCGSR). R.W.S. acknowledges support from the Director’s Fellowship within NREL’s Laboratory Directed Research and Development program. Use of the Stanford Synchrotron Radiation Lightsource, SLAC National Accelerator Laboratory, is supported by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences under Contract No. DE-AC02-76SF00515. We thank the Analytical Resources Core at Colorado State University for instrument access and training. We thank Charles Titus and Andriy Zakutayev for helpful conversations. The views expressed in the article do not necessarily represent the views of the DOE or the U.S. Government.

Structural characterization

Synchrotron grazing incidence wide angle X-ray scattering (GIWAXS) reveals the polycrystalline nature of the films deposited on silicon with a 100 nm surface layer of SiO2\mathrm{SiO}_{2} (Figure S1). Hot pixels were manually masked when identified to avoid spurious peaks in the integrated patterns. Broad and weak reflection spots are visible and attributable to silicon, but these spots were not masked owing to significant overlap with the powder rings. These spots contribute to elevated background scattering in the integrated diffraction patterns. Full LeBail fits for the patterns shown in Figure 3 are shown in Figure S2. Figure S3A shows the extracted hexagonal lattice parameters and Figure S3B show the fit residuals.

GIWAXS patterns and focused Q-range fits

Figure S2. A) Full patterns of the GIWAXS data presented in Figure 3 of the main text. VESTA-generated reference patterns are shown at the top. The main reflections match the P63mcP6_{3}mc space group of the cation-disordered wurtzite structure type MnSnN2_2. Evidence of cation ordering is not observed in diffraction. At Mn-rich compositions (≥69\geq69%), broad peaks corresponding to Mn3_3N2_2 appear. LeBail refinements were conducted on these patterns to extract lattice parameters of the wurtzite phase MnSnN2_2. Black points are data, orange traces are fits, and blue traces are difference curves. B) Focused QQ-range of fits to the first three wurtzite reflections, corresponding to Figure 3B of the main text. Although the peak broadness is poorly captured owing to anisotropic broadening, the peak positions are relatively well described by the fit.

Fitting residuals were minimized for the patterns with slight excess Mn, with worsening fits in the Mn-poor and Mn-rich regions (Figure S3B). Fit residuals also increase in the Mn-rich region, here owing to the growth of a secondary Mn3N2\mathrm{Mn}_{3}\mathrm{N}_{2} phase that is visible as broad peaks but was not modeled. Some of this broadening may also be due to scattering from the silicon substrate, which may vary from sample to sample depending on the exact orientation of the substrate. Lastly, some degree of texturing is observed (Figure S1), which affects the relative heights of integrated peaks.

A major finding in the thin film synthesis of MgSnN2\mathrm{MgSnN}_{2} by Greenaway et al. was a wurtzite-to-rocksalt structural transition, and we find a small amount of evidence that a similar phenomenon occurs in the MnSnN2\mathrm{MnSnN}_{2} system (Figure S5). In our studies of MnSnN2\mathrm{MnSnN}_{2}, a single synchrotron GIWAXS pattern revealed a rocksalt type structure at Mn/(Mn+Sn) = 68%. The rocksalt appears under similar conditions needed for rocksalt MgSnN2\mathrm{MgSnN}_{2} (Sn poor, low TdepT_{\mathrm{dep}}). However, the refined lattice parameter for our MnSnN2\mathrm{MnSnN}_{2} rocksalt (a=4.378a = 4.378 Å) is very similar to the rocksalt lattice parameter for MnO (a=4.446a = 4.446 Å); the ternary is 1.5% smaller than the binary. In contrast, rocksalt MgSnN2\mathrm{MgSnN}_{2} (a=4.483a = 4.483 Å) is 6.3% larger than MgO (a=4.217a = 4.217 Å). The presence of a rocksalt polymorph in the Mn-Sn-N system may merit further study.

GIWAXS pattern and fit for a rocksalt MnSnN₂ sample

Figure S5. GIWAXS pattern for a sample at 68% Mn/(Mn+Sn) and Tdep=100T_{\mathrm{dep}} = 100 °C showing a rocksalt (Fm3ˉmFm\bar{3}m) crystal structure (a=4.378 A˚a = 4.378\ \AA).

Rapid thermal annealing experiments revealed that the MnSnN2\mathrm{MnSnN}_{2} phase is stable against decomposition up to at least Tanneal=300T_{\mathrm{anneal}} = 300 °C for 30 minutes (Figure S6). At Tanneal=400T_{\mathrm{anneal}} = 400 °C, the ternary phase begins decomposing to Sn, Mn4N\mathrm{Mn}_{4}\mathrm{N}, and N2\mathrm{N}_{2}. This stability up to 300 °C suggests either i) that cation-disordered MnSnN2\mathrm{MnSnN}_{2} is more thermodynamically stable than that predicted for the cation-ordered phase (+0.038 eV/atom above the hull) or ii) that decomposition up to 300 °C is kinetically slow.

To assess the limits of off stoichiometry in the hexagonal MnSnN2\mathrm{MnSnN}_{2} phase, one library was deposited with a lower power on the Mn target (54 W as opposed to the typical 108 W), leading to a Mn-poor film (Figure S7). This Mn-poor film still exhibited wurtzite-like reflections down to approximately 18% Mn/(Mn+Sn)\mathrm{Mn}/(\mathrm{Mn}+\mathrm{Sn}), limited by the edge of the library rather than by a structural change. This composition nominally corresponds to Mn0.36Sn1.64N2\mathrm{Mn}_{0.36}\mathrm{Sn}_{1.64}\mathrm{N}_2 (assuming a fixed anion content). For compositions with Mn/(Mn+Sn)<50%\mathrm{Mn}/(\mathrm{Mn}+\mathrm{Sn}) < 50\%, charge balancing must occur through either Sn2+\mathrm{Sn}^{2+} substitution for Mn2+\mathrm{Mn}^{2+} or metal vacancies. Although we did not explore this Mn-poor region further, this finding suggests that Mn-poor MnSnN2\mathrm{MnSnN}_2 could be of interest for dilute magnetic semiconductor studies.

Compositional characterization

RBS

RBS measurements for select samples corroborate the high-throughput XRF measurements done for each combinatorial film (Figure S8A). Furthermore, RBS measurements identify the presence of oxygen in the MnSnN2_2 films (Figure S8B). The convolution of the N and O signals in RBS with the signal from the substrate inhibit the quantitative relation of anion content (N+O) with cation content (Mn+Sn) (Figure S9), but the qualitative comparison of the trends in O/(N+O) as a function of cation content are still valid. Oxygen content increases with increasing Mn content, consistent with the lower electronegativity of Mn (1.55 on the Pauling scale) compared to Sn (1.96). The width of the oxygen region of the RBS spectra is similar to the width of the other elemental regions, suggesting that oxygen is distributed throughout the film thickness rather than being isolated to the surface. Oxygen substitution might help charge balance excess Mn via Mn1+y_{1+y}Sn1−y_{1-y}N2−y_{2-y}Oy_y, where yy is both the number of oxides substituting for nitrides and the number of Mn3+^{3+} ions substituting for Sn4+^{4+}. Alternatively, oxygen substitution could occur with exclusively Mn2+^{2+}, following a formula of (MnO)x_x(MnSnN2_2)(1−x)_{(1-x)}, similar to the oxygen balancing seen in MgZrN2_2 thin films. [54]

XANES

In an attempt to identify the presence of Mn3+^{3+} and assess Mn2+^{2+}:Mn3+^{3+} ratios, high-resolution Mn L3L_3-edge X-ray absorption near-edge spectroscopy (XANES) measurements were conducted. Measurements were carried out on thin films at room temperature at the Stanford Synchrotron Radiation Lightsource (SSRL), SLAC National Accelerator Laboratory, beamline 10-1. Samples were measured under high vacuum conditions of ∼2.7×10−6\sim2.7 \times10^{-6} Pa (∼2×10−8\sim2 \times10^{-8} Torr) with a ring current of 500 mA. The synchrotron radiation was monochromatized using the beamline’s 600 line/mm monochromator with entrance and exit slits of 35 μ\mum. A transition edge sensor (TES) spectrometer [55] was used to collect resonant inelastic x-ray scattering (RIXS) planes with a resolution of 2 eV. The energy measured by the TES was calibrated by periodically measuring a reference sample of graphite, BN, Fe2_2O3_3, NiO, and CuO, which provide a stable set of emission lines. From the RIXS planes, we extracted the LαL_\alpha and LβL_\beta lines, leading to partial fluorescence yield XAS.

XANES measurements (Figure S10) show consistent spectra across the measured composition range, so we are not able to identify a change in oxidation state. There are subtle differences between the spectra, as highlighted in the insets, but these differences are hard to distinguish from noise. We observe no consistent trend with composition and no distinct features indicative of Mn3+^{3+}. Instead, each the spectral profile is consistent with Mn2+^{2+} spectra seen in literature. [56, 57]

Magnetic properties

Background subtraction and data analysis

As noted in the main text, for each magnetic measurement performed, an analogous blank substrate was measured with identical scan parameters, allowing for direct, point by point background subtraction. These blanks were 5 mm × 5 mm squares of the substrate alone (100 nm SiO2_2 on pSi), taken from the same wafer batch used for the deposition. Figure S11–Figure S12 show examples of the background subtraction for temperature- and applied field-dependent measurements, respectively.

Background subtraction example for applied field sweeps

Figure S12. Background subtraction example for applied field sweeps measured at T=2T = 2 K. The raw moments of the sample and a blank substrate are shown, along with the background-subtracted data showing magnetism from the film alone (sample - blank)

Following background subtraction, the susceptibility (χ\chi) was calculated using the background-subtracted raw moment value described above, along with a film mass of 0.00004 g and the molar mass calculated as Mn2x_{2x}Sn2−2x_{2-2x}N2_2 (Table S1) where xx is the Mn fraction of cation content (Mn/[Mn+Sn]). The % Mn/(Mn+Sn) values were determined by XRF on the individual squares. We note that the small mass of Mn2x_{2x}Sn2−2x_{2-2x}N2_2 present during the measurements and the several possible sources of error in the film mass calculation and background subtraction make direct, quantitative comparisons of the magnitude of χ\chi between samples difficult. The value of 0.00004 g for a film mass is a reasonable approximation given the film surface area (25 mm2^2), thickness, and composition.

Additional data

Inverse susceptibility data as a function of temperature show an approximately linear region above the T∗∼10T^* \sim10 K transition temperatures for each composition, provided a diamagnetic correction (χ0\chi_0) is applied (Figure S13). Inverse χ\chi without a diamagnetic correction exhibits significant non-linearity (Figure S13A). Therefore, Curie-Weiss fits were performed on (χ−χ0)−1(\chi-\chi_0)^{-1} from 150–300 K, as shown in Figure S13B. As the inverse χ\chi plots exhibited a second linear region (50–150 K), we also applied Curie-Weiss analysis to this lower temperature region (Figure S13C), which resulted in a smaller magnitude ΘCW\Theta_{\mathrm{CW}} and a smaller magnitude χ0\chi_0 than the high temperature fits (Table S2). Weiss temperatures from both fit ranges indicate antiferromagnetic (AFM) correlations. The change in slope may indicate a change in the energy scale of the dominant interactions in different temperature regions, or the emergence of competing interactions, although further investigation will be required to elucidate these subtle differences. We note that the uncertainty in background subtraction and film mass discussed above and in the main text inhibits quantitative extraction of Curie constants (CC) or effective moments (μeff\mu_{\mathrm{eff}}) from the Curie-Weiss fits.

% Mn/(Mn+Sn)50–150 K ΘCW\Theta_{\mathrm{CW}} (K)50–150 K χ0\chi_0 (emu/Oe mol)150–300 K ΘCW\Theta_{\mathrm{CW}} (K)150–300 K χ0\chi_0 (emu/Oe mol)
42-47-0.0025-324-0.0083
51-63-0.0030-243-0.0055
56-79-0.0038-356-0.0057

Table S2. Weiss temperatures (ΘCW\Theta_{\mathrm{CW}}) extracted from Curie-Weiss fits performed from 50–150K and 150–300 K with the diamagnetic corrections (χ0\chi_0) listed.

Figure S14 shows the background-subtracted moment as a function of applied field measured at T=2T = 2 K for all samples. This low-temperature behavior (below the transition temperature) is consistent with an AFM ground state across the composition series. The small hysteresis and net ferromagnetic moment noted in the Mn/(Mn+Sn) = 51% sample (Figure 6 in the main text) are also present across the measured composition range, supporting our assignment of this moment arising from canting or defects. The samples do not exhibit a plateau in moment, suggesting that the magnetism is not saturated at the limit of the instrument (μ0H=7\mu_0H = 7 T). The moment at μ0H=7\mu_0H = 7 T decreases with increasing Mn/(Mn+Sn) content, attributable to either the substitution of Mn3+^{3+} for Mn2+^{2+} or uncertainty in the mass used for normalization. Also, the low-field slope changes with increasing Mn/(Mn+Sn): at Mn/(Mn+Sn) = 56%, it appears to have two components, while at Mn/(Mn+Sn) = 42% there is only one component. This behavior may be related to uncompensated moments from Mn3+^{3+}.

Optoelectronic measurements

In addition to the ellipsometry measurements and modeling reported in the main text (Figure 7C), we conducted transmission and reflection UV-vis measurements on select substrates deposited on EXG, a transparent substrate (Figure S15). Transmission (TT) and reflectance (RR) spectra were collected in the UV-Vis-NIR spectral ranges (300–1100 nm) using a home-built thin film optical spectroscopy system equipped with deuterium and tungsten/halogen light sources and a Si detector array. The collected spectra were then used to calculate absorbance using the relation Absorbance, A=ln⁡[T/(1−R)]A = \ln[T/(1-R)]. Unfortunately, the UV-vis spectrometer did not reach a sufficiently low energy to observe the absorption onset (1 eV, 1200 nm). However, these data support a low energy absorption onset without the need for modeling of the spectra (as needed for ellipsometry).

In addition to measuring electrical conductivity of a film on EXG (Figure 7), we also conducted temperature dependent electrical measurements on select samples deposited on an insulating 100 nm of SiO2_2 on Si (Figure S16). These measurements were consistent with our observations for the sample on EXG (Figure 7B), showing increasing conductivity with increasing temperature. However, these blanket films on 100 nm of SiO2_2 have a tendency to short across such a narrow insulating layer if cleaved (as for these samples). To ensure we were exclusively measuring conductivity of the film, rather than the Si substrate, we repeated the measurement on EXG and report that in the main body of the text.

Conductivity measurements as a function of temperature

Figure S16. Conductivity measurements on 5 mm × 5 mm squares scribed from a library deposited at Tdep=225T_{\mathrm{dep}} = 225 °C on Si with 100 nm SiO2_2.

References

  1. [29]1977, 23, 815–819.
  2. [30]N. Barradas, K. Arstila, G. Battistig, M. Bianconi, N. Dytlewski, C. Jeynes, E. Kótai, G. Lulli, M. Mayer, E. Rauhala et al., Nuclear Instruments and Methods in Physics Research Section B: Beam Interactions with Materials and Atoms, 2008, 266, 1338–1342.
  3. [31]F. Smits, Bell System Technical Journal, 1958, 37, 711–718.
  4. [32]C. M. Caskey, R. M. Richards, D. S. Ginley and A. Zakutayev, Materials Horizons, 2014, 1, 424–430.
  5. [33]C. M. Caskey, A. Holder, S. Shulda, S. T. Christensen, D. Diercks, C. P. Schwartz, D. Biagioni, D. Nordlund, A. Kukliansky, A. Natan et al., The Journal of chemical physics, 2016, 144, 144201.
  6. [34]C. M. Caskey, J. A. Seabold, V. Stevanović, M. Ma, W. A. Smith, D. S. Ginley, N. R. Neale, R. M. Richards, S. Lany and A. Zakutayev, Journal of Materials Chemistry C, 2015, 3, 1389–1396.
  7. [35]H. Peng, P. F. Ndione, D. S. Ginley, A. Zakutayev and S. Lany, Physical Review X, 2015, 5, 021016.
  8. [36]G. Hautier, A. Miglio, D. Waroquiers, G.-M. Rignanese and X. Gonze, Chemistry of Materials, 2014, 26, 5447–5458.
  9. [37]A. N. Fioretti, A. Zakutayev, H. Moutinho, C. Melamed, J. D. Perkins, A. G. Norman, M. Al-Jassim, E. S. Toberer and A. C. Tamboli, Journal of Materials Chemistry C, 2015, 3, 11017–11028.
  10. [38]R. R. Schnepf, J. J. Cordell, M. B. Tellekamp, C. L. Melamed, A. L. Greenaway, A. Mis, G. L. Brennecka, S. Christensen, G. J. Tucker, E. S. Toberer et al., ACS Energy Letters, 2020, 5, 2027–2041.
  11. [39]C. L. Melamed, J. Pan, A. Mis, K. Hein selman, R. R. Schnepf, R. Woods-Robinson, J. J. Cordell, S. Lany, E. S. Toberer and A. C. Tamboli, Journal of Materials Chemistry C, 2020, 8, 8736–8746.
  12. [40]E. W. Blanton, K. He, J. Shan and K. Kash, Journal of Crystal Growth, 2017, 461, 38–45.
  13. [41]I. S. Khan, K. N. Heinselman and A. Zakutayev, Journal of Physics: Energy, 2020, 2, 032007.
  14. [42]R. T. Shannon and C. T. Prewitt, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 1969, 25, 925–946.
  15. [43]P. C. Quayle, E. W. Blanton, A. Punya, G. T. Junno, K. He, L. Han, H. Zhao, J. Shan, W. R. Lambrecht and K. Kash, Physical Review B, 2015, 91, 205207.
  16. [44]C. L. Melamed, M. K. Miller, J. Cordell, L. Pucurimay, A. Livingood, R. R. Schnepf, J. Pan, K. N. Heinselman, F. D. Vila, A. Mis et al., Chemistry of Materials, 2022, 34, 3910–3919.
  17. [45]M. Nardin, G. Lorthioir, M. Barberon, R. Madar, E. Fruchart and R. Fruchart, Comptes Rendus Hebdomadaires des Seances des Sciences, Serie C, Sciences Chimiques, 1972, 274, 2168–2171.
  18. [46]M. Mekata, Journal of the Physical Society of Japan, 1962, 17, 796–803.
  19. [47]S. Fay, U. Kroll, C. Bucher, E. Vallat-Sauvain and A. Shah, Solar Energy Materials and Solar Cells, 2005, 86, 385–397.
  20. [48]S. Mugiraneza and A. M. Hallas, Communications Physics, 2022, 5, 1–12.
  21. [49]S. C. van der Marck, Physical Review E, 1997, 55, 6593.
  22. [50]A. P. Ramirez, Annu. Rev. Mater. Sci., 1994, 24, 453–480.
  23. [51]V. Ney, B. Henne, J. Lumetzberger, F. Wilhelm, K. Ollefs, A. Rogalev, A. Kovacs, M. Kieschnick and A. Ney, Phys. Rev. B, 2016, 94, 224405.
  24. [52]A. Simonov and A. Goodwin, Nat. Rev. Chem., 2020, 4, 657–673.
  25. [53]J. Häusler, R. Niklaus, J. Minár and W. Schnick, Chemistry–A European Journal, 2018, 24, 1686–1693.
  26. [54]S. R. Bauers, D. M. Hamann, A. Patterson, J. D. Perkins, K. R. Talley and A. Zakutayev, Japanese Journal of Applied Physics, 2019, 58, SC1015.
  27. [55]S.-J. Lee, C. J. Titus, R. Alonso Mori, M. L. Baker, D. A. Bennett, H.-M. Cho, W. B. Doriese, J. W. Fowler, K. J. Gaffney, A. Gallo, J. D. Gard, G. C. Hilton, H. Jang, Y. I. Joe, C. J. Kenney, J. Knight, T. Kroll, J.-S. Lee, D. Li, D. Lu, R. Marks, M. P. Minit­ti, K. M. Morgan, H. Ogasa wara, G. C. O’Neil, C. D. Reintsema, D. R. Schmidt, D. Sokaras, J. N. Ullom, T.-C. Weng, C. Williams, B. A. Young, D. S. Swetz, K. D. Irwin and D. Nordlund, Review of Scientific Instruments, 2019, 90, 113101.
  28. [56]R. Niewa, Z. Hu, C. Grazioli, U. Rösler, M. Golden, M. Knupfer, J. Fink, H. Giefers, G. Wortmann, F. De Groot et al., Journal of alloys and compounds, 2002, 346, 129–133.
  29. [57]S. Cramer, F. DeGroot, Y. Ma, C. Chen, F. Sette, C. Kipke, D. Eichhorn, M. Chan, W. Armstrong, E. Libby et al., Journal of the American Chemical Society, 2002, 113, 7937–7940.

Paper details

vlnc:W_3a2yvmga
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents