Transition-Metal-Oxygen Covalency Controls Ligand-Hole Stability in Li-Rich Cathode

Abstract

Lithium-rich cathodes boast a large specific capacity due to the presence of excess lithium per transition metal. However, making use of that excess Li drives the cathodes to unusually high formal oxidation states, often triggering unwanted side reactions, typically signaled by gas release and commonly associated with oxygen oxidation. By varying the transition metal (TM) chemistry in Li-rich materials, cyclability can vary drastically, with some materials suffering rapid capacity fade while others are able to maintain large and stable voltage windows. Such observations indicate a crucial role for both TM and O activities, but the details remain elusive. Here, we model core-level spectroscopy to understand differences in the charge compensation mechanism between different Li2MO3 (M = Mn, Ru, Ir) cathode materials. We find that ligand holes are important throughout the series, but their stability depends strongly on the transition-metal-oxygen electronic structure. In Li2MnO3, the ground state is already strongly negative-charge-transfer-like, so further delithiation rapidly increases ligand-hole character and promotes instability. Moving from Mn to Ru and Ir increases TM-O hybridization while reducing the tendency toward an extreme negative-charge-transfer state, allowing additional holes to remain delocalized over the covalent TM-O network over a wider range of charge. These results identify TM-O covalency, rather than the absence of oxygen-hole character, as a key factor controlling reversible high-valent redox and suggest a route for stabilizing high-energy-density cathodes without invoking reversible molecular oxygen formation.

Introduction

Electrochemical processes feature reduction and oxidation (redox) reactions of a variety of species across a multitude of relevant energy and industrial technologies. Transition metal (TM) oxides hold a unique place as workhorses for current and future renewable energy applications, ranging from their role as electrodes in Li-ion batteries to catalysts for hydrogen and oxygen evolution reactions. Electrochemical energy applications often trigger the formation of unconventional oxide states through a wide range of redox voltage. These states define the properties of energy materials and more importantly, their practical performance. Thus, fundamental understanding of the electronic structure and the evolution of redox active materials is paramount for the development of next generation devices.

Most challenges in developing high-performance energy storage stem from the inherent trade-off between high energy density and cycling stability in cathode materials, especially at high voltages. A representative family is lithium-rich layered oxide cathodes. Relative to conventional stoichiometric layered oxides, e.g. LiMO2_2 (M = Co, Ni), lithium-rich cathodes feature more lithium than TM per formula unit, and therefore higher theoretical specific capacity. [3] [1, 2] However, accessing this additional capacity can lead to instabilities, which often trigger voltage hysteresis and gas release [4, 5, 6, 7, 8, 9, 10]. These instabilities have been attributed to the involvement of oxygen atoms in the redox reaction.

Extensive efforts have focused on stabilizing oxygen redox reactions with direct oxygen bonding to access capacity beyond the cationic redox limit at high voltage, referred to as “anionic/oxygen redox” [11, 12, 13, 14]. These efforts have faced challenges to stability and kinetics [6, 15, 16, 17, 18], with highly oxidized oxygen anions often forming chemically defined species, especially peroxo- and O2_2. Nevertheless, some studies have reported signatures of stabilized oxygen holes in 3d TM oxide cathodes with low hysteresis and voltage fade, even at high voltages [14, 19, 20, 21, 22, 23], although the mechanism that enables stable cycling performance remains unclear.

While achieving stable high-valent redox with 3d TMs is challenging, layered oxides containing heavier TMs have demonstrated the capability to undergo relatively more reversible high-valent redox processes [24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36]. This is often attributed to charge compensation mediated by the heavy TMs. However, spectroscopic measurements on oxygen atoms reveal clear signatures of oxygen participation in the redox process with non-negligible ligand hole density [30, 31, 32, 33, 34, 35, 36], suggesting that oxygen plays a significant role in the redox activities. In practice, the strong hybridization between the heavy TMs and oxygen makes it difficult to disentangle their individual contributions to the redox activity, resulting in a lack of consensus on the underlying mechanism that stabilizes high voltage, high-valent cycling in heavy TM oxides. Nonetheless, experimental measurements point to the same trend: heavier TM oxide cathodes can accommodate higher levels of delithiation with reversible capacity at high voltages. Thus, clarifying the TM effects on Li-rich cathode properties through a comparative study becomes crucial for understanding the fundamental mechanism that enables reversible high-voltage redox.

A natural framework for addressing this question is provided by the competition between charge-transfer energetics and TM–O hybridization. In a negative charge-transfer (NCT) regime, oxidation can be accommodated predominantly through ligand-hole configurations dn+1Ld^{n+1}\mathrm{L}, rather than by further oxidation of the nominal TM ion [37]. However, substantial ligand-hole character does not by itself imply a strongly negative charge-transfer energy: ligand holes can also arise from strong covalent mixing between TM dd and O 2p2p states. This distinction becomes increasingly important in moving from 3d3d to 4d4d and 5d5d transition metals, whose more spatially extended dd orbitals enhance TM–O hybridization. The stability of high-valent redox may therefore depend not simply on the number of oxygen holes, but on the electronic environment in which those holes are accommodated.

Here, we test this picture through a systematic comparison of Li2MO3\mathrm{Li_2MO_3} (M = Mn, Ru, Ir), combining charge-transfer multiplet and first-principles calculations with experimental X-ray absorption spectroscopy (XAS) and resonant inelastic X-ray scattering (RIXS). By examining both the O KK-edge and TM L3L_3-edge, we track the evolution of metal and ligand configurations during delithiation and distinguish ligand-hole formation associated with strong covalency from the evolution toward a strongly NCT state. The Mn-Ru-Ir series provides a particularly useful comparison because the progressively more extended TM dd orbitals increase TM–O hybridization while the materials exhibit markedly different ranges of reversible delithiation.

We find that ligand holes are important throughout the Mn-Ru-Ir series, but their presence alone does not determine stability. Li2MnO3\mathrm{Li_2MnO_3} begins in a strongly NCT regime, such that further delithiation rapidly increases ligand-hole character and drives the system toward oxygen instability. In the Ru- and Ir-based compounds, stronger TM–O hybridization produces substantial ligand-hole character even when the charge-transfer energy is less negative. The resulting holes are distributed over a more strongly covalent TM–O network, allowing progressively deeper oxidation before the system reaches the regime associated with O–O dimerization and irreversible oxygen chemistry. We therefore identify the interplay between charge-transfer energy and TM–O hybridization, rather than a simple division between “cationic” and “anionic” redox, as a key control parameter for reversible high-valent redox in Li-rich cathodes.

Methods and Results

We now examine how the balance between charge-transfer energetics and TM–O hybridization evolves across Li2MO3\mathrm{Li_2MO_3} (M = Mn, Ru, Ir). We begin with Li2MnO3\mathrm{Li_2MnO_3}, where the localized nature of the Mn 3d3d orbitals provides the strongly NCT limit of this series, before considering the progressively more covalent Ru 4d4d and Ir 5d5d compounds.

Manganates

Li2MnO3\mathrm{Li_2MnO_3} provides the natural starting point for this comparison. Formally, Mn is already Mn4+\mathrm{Mn^{4+}} in the pristine compound, leaving little capacity for further conventional Mn-centered oxidation during delithiation. Experimentally, Li2MnO3\mathrm{Li_2MnO_3} exhibits pronounced voltage hysteresis, structural degradation, and oxygen loss during the first charge [7, 8, 9, 10]. Its additional capacity has consequently been associated with oxygen-derived charge compensation, including the formation of oxygen-hole, O–O dimer, and ultimately molecular oxygen species. The key question for the present work is therefore how this oxygen activity emerges from the electronic structure of the pristine material and evolves upon further oxidation.

Here, we model pristine Li2MnO3\mathrm{Li_2MnO_3} using a charge transfer multiplet formalism [38], which allows for simulations of both the TM L3L_3- and O KK-edge spectra in the same cluster (see supplementary section ??). Theoretical calculations of XAS and RIXS for both O KK-edge and Mn L3L_3-edge show remarkable agreement with the experimental measurements (Figure 1) [8, 10]. The calculation points to an NCT ground state with an even distribution of d4L‾d^{4}\underline{L} and d5L‾2d^{5}\underline{L}^{2} (where L‾\underline{L} denotes a ligand hole) with a significant number of holes on the oxygen orbitals. Signatures of the NCT ground state can be observed in the elastic scattering feature at the O KK-edge with an incident energy around 529 eV (Figure 1(b)). Excess hole formation within the oxygen 2p2p orbitals allows for a large coherence between the ground and intermediate states. This near elastic scattering feature at low absorption energy can also be seen in other NCT active cathode materials [19, 39], and stands in stark contrast to the O2_2 RIXS feature seen around an absorption energy of 531 eV [6]. Additionally, fluorescent like features that can be seen around 643 eV to 645 eV in incident energy at the Mn L3L_{3}-edge (Figure 1(e) and (Figure 1f)) signify the transition from a charge transfer picture with clear, localized dd-dd excitations to a more strongly hybridized ground state with enhanced NCT and more itinerant electrons. First-principles calculations also show oxygen hole density present in the pristine material (Figs. ?? and ??). On the other hand, clear signatures of dd-dd excitations at the Mn L3L_{3}-edge (≈3\approx3 eV energy loss) point to still well localized Mn dd orbital states (Figure 1(e)), which contributes to the stability of stoichiometric Li2_2MnO3_3. Delithiation of Li2_2MnO3_3 leads to a further increase in the NCT character of the ground state and an overpopulation of ligand holes, triggering structural instability and cycling irreversibility as previously reported. [7, 8, 9, 10]

Simulated and experimental XAS and RIXS of pristine Li2MnO3

Figure 1. Simulated and Experimental XAS and RIXS of pristine Li2_2MnO3_3. (a) Comparison between experimental (total electron yield mode TEY; black) and multiplet-simulated (red) O KK-edge XAS of Li2_2MnO3_3. (b) Simulated and (c) experimental O KK-edge RIXS (reproduced from ref. [30]) of Li2_2MnO3_3, plotted using incident and emission energy axes. (d) Comparison between experimental and multiplet-simulated Mn L3L_3-edge XAS of Li2_2MnO3_3. (e) Simulated and (f) experimental Mn L3L_3-edge RIXS (reproduced from ref. [10]) of Li2_2MnO3_3, plotted as energy loss axis to highlight different dd-dd and charge transfer excitations.

The prevalence of a NCT ground state with significant ligand hole density in pristine Li2_2MnO3_3, as seen in our calculations, is quite similar to its charged counterparts Li1−x_{1-x}NiO2_2 and Li1−x_{1-x}CoO2_2, with a formal valence of TM4+^{4+} on the transition metal, except here it manifests as the starting point of the lithiated material. Delithiation leads to an increase of this NCT character. This interpretation differs from previous theoretical work, such as the proposed Mn4+^{4+}/Mn7+^{7+} [40] redox couple or “non-bonding” oxygen pp-orbitals [41] as the main contributors to the first-charge capacity. Experimentally, oxygen outgassing and dimer formation make it challenging to model the spectroscopy and elucidate the charge compensating mechanism, leading to reports of either a lack of change in both Mn and O valence states [7, 8] or bulk reduction due to structural degradation [10]. Here, the increase of the NCT character of the ground state upon delithiation serves as a precursor for the structural instabilities and oxygen dimerization seen experimentally, in contrast to the more stable positive to negative charge transfer transition, as seen in LiCoO2_2 and LiNiO2_2 [39], or the purely positive charge transfer redox mechanism seen in LiFePO4_4.

We note that this evolution of the NCT ground state in Mn cathodes can be stabilized, as seen in Na2_2Mn3_3O7_7, which cycles reversibly beyond a formal valence of Mn4+^{4+} [19, 20]. For the pristine material, multiplet calculations for this system show good agreement with experimental O KK-edge RIXS and XAS (Figs. ??(a) and (b)), where the peak emerging at ≈527.5\approx527.5 eV can be associated with an increase in oxygen hole density [19]. Meanwhile, both calculated and experimental Mn L3L_{3}-edge XAS show little change in the spectral line-shape (Fig. ??(d)) [19], while the calculated RIXS map shows an increase in the intensity of charge transfer excitations (Fig. ??(e)). For the charged nominal Mn5+^{5+} state, the calculated ground-state wavefunction is dominated by d4L‾2d^{4}\underline{L}^{2} and d5L‾3d^{5}\underline{L}^{3} configurations (Table ??). This suggests that charge compensation occurs exclusively on ligand orbitals that is driven by the increase of NCT energy. This result is consistent with previous literature, where the stability of added oxygen hole density in the material upon charging was attributed to polaronic effects [19].

Our calculations draw a consistent conclusion with our previous studies of conventional cathode systems [39]: at high formal valence, 3d3d transition metal tends to favor an NCT ground state, in which strong TM-ligand hybridization stabilizes excess ligand holes. A ground state with large NCT energy often triggers structural disorder, but can be stabilized kinetically, as in Na2_2Mn3_3O7_7 [19, 23]. In both Li2_2MnO3_3 and Na2_2Mn3_3O7_7, the pristine discharged cathode has the same formal valence: Mn4+^{4+}. Upon charging, the voltage of Li2_2MnO3_3 quickly increases above 4.5 V [7, 8, 9], with observed instability and dimerization. On the other hand, Na2_2Mn3_3O7_7 operates below 4.5 V while maintaining a stable NCT ground state with significant ligand hole density [19]. This contrast demonstrates that a ground state with large NCT energy can be accommodated without severe degradation.

Li2_2MnO3_3 therefore represents one limit of the Li2_2MO3_3 series: substantial ligand-hole character is already present before charging, and further delithiation rapidly drives the system deeper into the NCT regime. We next ask how this evolution changes when Mn 3d3d orbitals are replaced by the more spatially extended 4d4d orbitals of Ru, thereby increasing TM–O hybridization.

Ruthenates

Replacing Mn by the more spatially extended 4d4d orbitals of Ru provides a direct test of the role of TM–O hybridization in stabilizing ligand-hole character. Li2_2RuO3_3 is structurally similar to Li2_2MnO3_3, but exhibits substantially greater electrochemical reversibility, with low hysteresis and reversible extraction of approximately one Li per formula unit [24, 25, 26, 35, 36]. Further delithiation beyond the nominal Ru5+^{5+} state becomes increasingly irreversible [29, 30, 36]. Li2_2RuO3_3 therefore provides an intermediate case between the rapidly destabilized Mn compound and the still more covalent Ir system considered later.

The more extended Ru 4d4d orbitals are expected to produce stronger Ru–O hybridization than in the Mn 3d3d compound. Consequently, substantial ligand-hole character does not imply that pristine Li2_2RuO3_3 is already in a strongly NCT regime. Instead, ligand-hole configurations can acquire appreciable weight through covalent mixing between Ru 4d4d and O 2p2p states. This distinction between covalency-induced ligand-hole weight and ligand-hole self-doping associated with negative charge-transfer energy is central to understanding the different responses of Li2_2MnO3_3 and Li2_2RuO3_3 to delithiation.

The nature of the strong TM-ligand hybridization can be examined by core-level spectroscopy at both the O KK-edge and the Ru L3L_{3}-edge, which show clear changes in spectral features upon charging [29, 30, 31, 35]. Here, we model XAS and RIXS spectra of Lix_xRuO₃ using both charge-transfer multiplet and the Bethe-Salpeter equation (BSE) based OCEAN code [42, 43, 44]. Due to the weaker electron-electron interactions in 4d4d orbitals [45], the Ru L3L_3-edge spectra can be modeled well by both multiplet cluster and ab-initio calculations, not having the dominant multiplet splittings seen in 3d3d systems. Figure 2(a) shows two absorption features around 529 eV and 531.5 eV at the OO KK-edge, and broad features around 2841 eV and 2843 eV at the Ru L3L_3-edge (Figure 2(e))). These features are associated with TM–O $\pi$ and $\sigma$ bonds (or $t_{2g}$ and $e_g$ orbitals), respectively [30], and agree well with previous experimental measurements {citep}[30, 31]. Theoretical $O$ $K$-edge RIXS ({xref}Figs. 2(b,c)) shows good agreement compared to previous experimental results as well ({xref}Fig. 2(d)) {citep}[30], with a distinct two peak structure in the XAS. Additionally, calculated Ru $L_3$-edge RIXS spectra ({xref}Figs. 2(f,g)) for Li₂RuO₃ reproduces the reference Ca₂RuO₄ spectra {citep}[46]`, which carries the same nominal Ru valence.

Simulated and experimental XAS and RIXS of Li₂RuO₃

Figure 2. Simulated and Experimental XAS and RIXS of Li₂RuO₃. (a) Comparison between experimental (partial fluorescence yield mode PFY; black), BSE-based OCEAN code simulated (blue-green), and multiplet-simulated (red) OO KK-edge XAS of Li₂RuO₃. (b) OCEAN simulated, (c) multiplet simulated and (d) experimental OO KK-edge RIXS of Li₂RuO₃, plotted using incident and emission energy axes. (e) Comparison between experimental, OCEAN, and multiplet-simulated Ru L3L_3-edge XAS of Li₂RuO₃. (f) Simulated and (g) experimental Ru L3L_3-edge RIXS of Li₂RuO₃, plotted using energy loss. (h-k) Experimental and Simulated OO KK-edge XAS and RIXS for charged LiRuO₃, in the same order as panels (a-d). (l-n) Experimental and simulated Ru L3L_3-edge XAS and RIXS for charged LiRuO₃, in the same order as panels (e-g). All experimental data in this figure are reproduced from Ref. [30]. No experimental measurements of Ru L3L_3-edge RIXS are currently available for comparison due to its tender X-ray range. LiRuO₃ was experimentally reached by cycling the electrode to 4.1 V.

Multiplet calculations for pristine Li₂RuO₃ reveal a ground-state configuration that differs qualitatively from that of Li₂MnO₃, with significant weight across d4d^4, d5L‾d^5\underline{L}, and d6L‾2d^6\underline{L}^2 states (Table. ??). Importantly, however, this ligand-hole weight occurs even though the system is not yet strongly NCT. Instead, it arises predominantly from the large Ru 4d4d-O 2p2p hybridization. First-principles calculations support this interpretation, showing substantial overlap of Ru 4d4d and O 2p2p states near the Fermi level (Fig. ??). Evidence of strong hybridization in pristine Li₂RuO₃ can also be seen in experimental L3L_3-edge RIXS measurements of the reference compound Ca₂RuO₄ [46], displaying strong fluorescent emission signals that mirror the Li₂MnO₃ L3L_3-edge measurements in Figure 1(f). Thus, large ligand-hole density and a strongly negative charge-transfer energy are not equivalent: strong covalency alone can generate substantial ligand-hole character.

Upon charging to LiRuO₃ (one lithium extracted per formula unit), both the OO KK-edge and the Ru L3L_3-edge XAS exhibit similar changes in the spectra (Figure 2(h) and (Figure 2l)). The separation between the two absorption features becomes larger, with the lower-energy t2gt_{2g} feature increasing in intensity. While some discrepancies between the experimental and simulated spectra have been attributed to oxygen deficiency in stoichiometric Lix_xRuO₃ [31], the observed spectral changes still point to electron removal from the TM–O π\pi-bonded orbitals, which contributes to the initial charge capacity. This is further reflected by changes in the RIXS spectra: features associated with excitation to the TM–O σ\sigma-bonded orbitals, namely at an incident energy ∼528\sim528 eV at the OO KK-edge (Figure 2(i-Figure 2k)), and energy loss features above 5 eV at the Ru L3L_3-edge (Figure 2(m,Figure 2n)), become more pronounced with additional delithiation. We note that there are slight differences in the charge transfer excitations from the theoretical Ru L3L_3-edge RIXS calculations, due to the localized nature of the multiplet Hamiltonian, whereas the BSE calculated RIXS shows a continuum of charge transfer excitations. The increase in ligand hole density is reflected by a ground state reconfiguration of LiRuO₃, where our multiplet calculations show a more even distribution across the d4L‾d^4\underline{L}, d5L‾2d^5\underline{L}^2, and d6L‾3d^6\underline{L}^3 components, with slightly larger hybridization strength compared to pristine Li₂RuO₃ (Table. ??). Similarly, figure ??(b) shows states with strong Ru and O character, with additional oxygen 2p2p density above the Fermi energy. A similar trend can be seen in the Ru M3M_3-edge (Figs. ??(a-f)), which shows softer X-ray transitions to the 4d4d orbitals of Ru (see supplementary section ??).

The comparison with Li₂MnO₃ reveals why substantial oxygen participation need not immediately produce instability. Pristine Li2_2RuO3_3 contains appreciable ligand-hole weight, but begins from a less NCT electronic structure in which those holes are distributed over strongly hybridized Ru–O states. Delithiation can therefore be accommodated by a continuous redistribution of charge across this covalent network, involving both Ru and O character, before the system reaches the strongly NCT regime associated with oxygen instability. This behavior differs from a purely cationic-redox picture, but also from Li2_2MnO3_3, which begins from an already strongly NCT state.

It is important to emphasize that there is still significant ligand hole density at the onset of charging, which leads to large pre-edge features in O K-edge XAS (Figure 2(a)). However, this is distinctly different from the cationic redox mechanism that has been suggested by previous studies [28]. Instead, the mechanism closely resembles the NCT ground state of Li1−x_{1-x}CoO2_2 and Li1−x_{1-x}NiO2_2 [39]. Here, the delocalization of the added charge allows LiRuO3_3 to offset the increased NCT energy, instead of resulting in the irreversibilities associated with Li2_2MnO3_3. This stabilization has a finite range. Upon delithiation beyond approximately one Li per Ru, the electronic structure becomes increasingly NCT and the additional ligand-hole density is eventually accompanied by O–O dimer formation and oxygen vacancies [20, 28, 29, 30, 31, 36]. Ru therefore does not eliminate oxygen instability; rather, stronger Ru–O covalency extends the range of oxidation over which ligand holes can be accommodated without irreversible oxygen chemistry. This observation suggests a natural progression to the 5d limit: if increasing TM–O hybridization expands this stable window, Li2_2IrO3_3 should tolerate still deeper delithiation before reaching the corresponding instability.

Iridates

Extending this comparison to the 5d series provides a further test of the role of TM–O covalency. Among the compounds considered here, Li2_2IrO3_3 supports the deepest reversible delithiation, with extraction of approximately 1.5 Li per Ir [27]. Despite reaching a formal Ir valence as high as Ir5.5+^{5.5+}, the material exhibits comparatively little structural degradation and clear oxygen participation in charge compensation without formation of short O–O dimers [32, 33, 34, 35]. Evidence for peroxide formation emerges only upon still deeper oxidation [34, 35]. Li2_2IrO3_3 therefore provides an important limiting case: substantial ligand-hole character and very high formal oxidation can coexist with reversible redox over a wider range than in the Mn- or Ru-based compounds.

To evaluate this extended stability, we investigate whether the increased TM–O covalency in Li2_2IrO3_3 allows ligand holes to be accommodated further before entering the strongly NCT regime associated with O–O bond formation. Here, we focus on the non-hysteretic region of the Lix_xIrO3_3 (x≥0.5x \ge0.5) electrochemical cycle to test whether the trend seen in the Mn and Ru Li-rich systems holds as discussed earlier. We model O K-edge and Ir L3L_3-edge core-level spectroscopy using both the multiplet formalism and ab-initio calculations along with experimental measurements at the O K-edge (see supplementary section ??).

For pristine Li2_2IrO3_3, XAS spectra for both experimental and simulated O K-edge displays the same characteristics as Li2_2RuO3_3, where two major features can be seen around ≈529\approx529 eV and 533 eV (Figure 3(a)) that are associated with the TM–O π\pi and σ\sigma bonds, respectively. On the other hand, the Ir L3L_3-edge (and M3M_3-edge [32]) only shows one broad feature (see Figure 3(e)) [34], due to the short core-hole lifetime of the intermediate state; however, finer resolution may be achieved by high energy X-ray techniques such as HERFD.

Simulated and experimental XAS and RIXS of Li2IrO3

Figure 3. Simulated and Experimental XAS and RIXS of Li2_2IrO3_3. (a) Comparison between experimental (PFY; black), BSE-based OCEAN code simulated (blue-green), and multiplet-simulated (red) O K-edge XAS of Li2_2IrO3_3. (b) OCEAN simulated, (c) multiplet simulated and (d) experimental O K-edge RIXS of Li2_2IrO3_3, plotted using incident and emission energy axes. (e) Comparison between experimental, OCEAN, and multiplet-simulated Ir L3_3-edge XAS of Li2_2IrO3_3. (f) Simulated and (g) experimental Ir L3_3-edge RIXS of Li2_2IrO3_3, plotted as energy loss. (h-k) Experimental and simulated O K-edge XAS and RIXS for charged LiIrO3_3, in the same order as panels (a-d). (l-n) Experimental and simulated Ir L3_3-edge XAS and RIXS for charged LiIrO3_3, in the same order as panels (e-g). (o-s) Experimental and simulated O K-edge XAS and RIXS for charged Li0.5_{0.5}IrO3_3, in the same order as panels (a-d). (t-v) Experimental and simulated Ir L3_3-edge XAS and RIXS for charged Li0.5_{0.5}IrO3_3, in the same order as panels (e-g). Details of experimental measurements of Lix_xIrO3_3 at the O K-edge are provided in supplementary section ??, whereas Ir L3_3-edge experimental data in this figure are reproduced from Ref. [34]. No experimental measurements are currently available for comparison with Ir L3_3-edge RIXS.

Simulated O K-edge RIXS (Figure 3(b) and (Figure 3c)) shows similar features, with excitations across the emission energy axis due to the strong hybridization (see also Fig. ??). Multiplet calculations point to a ground state with small positive charge transfer energy, but large hybridization that contributes to the large ligand hole density with a broad distribution across the d5d^5, d6L‾d^6\underline{\mathrm{L}} and d7L‾2d^7\underline{\mathrm{L}}^2 ground state (Table. ??). Indications of strong TM–O hybridization are observed in the OCEAN-calculated RIXS centered at 525 eV emission energy [32, 34, 47] (Figure 3(b)), with good agreement to experimental measurement [34] (Figure 3(d)). Ir L3L_3-edge RIXS (Figure 3(f) and (Figure 3g)) shows broad t2gt_{2g} to ege_g excitations around 3 eV to 4 eV energy loss in both simulated spectra, while the multiplet calculations (Figure 3(g)) also capture dd-dd excitations under 1 eV energy loss within the t2gt_{2g} manifold, which qualitatively agree with prior experimental measurements [48]. Combining O K-edge and Ir L3L_3-edge calculations, pristine Li2_2IrO3_3 is therefore best viewed as a highly covalent positive-charge-transfer system rather than a strongly NCT material.

In charged LiIrO3_3, the O K-edge low-energy peak associated with Ir t2gt_{2g} orbitals grows (Figure 3(h)), while the Ir L3L_3-edge centroid shifts to a higher incident energy (Figure 3(l)). This trend continues until charged to the formal Ir5.5+^{5.5+} state (Figure 3(o–Figure 3v)). The subtle spectral changes make it challenging to categorize the redox mechanism in Lix_xIrO3_3 cathodes, with lattice oxygen redox [33], TM–O hybridized redox [34], and redox on non-bonded oxygen orbitals [32] all proposed as possible mechanisms. Here, theoretical O K-edge XAS and RIXS spectra show good agreement with experimental measurements (Figure 3(h–Figure 3k), (Figure 3o–Figure 3s)). The ground state configuration of LiIrO3_3 shows a highly covalent, slightly NCT ground state with even distribution of d5d^5L, d6d^6L2^2 and d7d^7L3^3 (Table. ??). This reflects the decreased Coulomb interaction in heavy TMs when compared to a typical 3d TM, resulting in less negative charge transfer energy. First-principles calculations point to the same result, where the bands below the Fermi level are mostly highly covalent Ir–O states (Fig. ??), in which oxygen contributes the majority of charge compensation [33].

While Ir L3L_3-edge XAS shows small changes upon charging, RIXS calculations show a distinctly different loss energy profile for different Lix_xIrO3_3. Upon charging, the RIXS intensity shifts from t2gt_{2g} to ege_g dd-dd excitation to a more charge transfer type excitation (i.e. d6L‾2→d5L‾d^6\underline{\mathrm{L}}^2 \rightarrow d^5\underline{\mathrm{L}}), highlighting a change to the NCT ground state (Figure 3(l–Figure 3n)). Further delithiation continues this trend (Figure 3(t–Figure 3v)). Compared to the multiplet calculation (Figure 3(g,Figure 3n,Figure 3v)), OCEAN simulated RIXS maps (Figure 3(f,Figure 3m,Figure 3u)) show a more diffusive charge transfer type excitation with loss energy from approximately 5 eV to 10 eV due to the itinerant nature of the exciton, while retaining the same trend as the multiplet calculations. Theoretical Ir M3_3-edge RIXS shows similar changes in loss profile (Figs. ??(g-o)), and requires X-ray photon energy closer to the soft X-ray range (≈2.5\approx2.5 keV), making it an ideal experiment to examine the change of ground state character in the Lix_xIrO3_3 cathode.

Multiplet and DFT calculations for Lix_xIrO3_3 point to a majority of charge compensation from oxygen atoms, where strong TM–O covalency and a smaller NCT energy enable stable multivalent redox up to formal Ir5.5+^{5.5+}. However, as in the Ru compound, this stabilization is not unlimited. Upon oxidation beyond the formal Ir5.5+^{5.5+} state, peroxide-like species have been observed [34, 35], indicating that sufficiently deep delithiation ultimately drives even the highly covalent Ir-O network toward localized oxygen chemistry. Conversely, the observation that a structurally stabilized Li2_2IrO3_3 polymorph can undergo still deeper delithiation with reduced hysteresis [49] emphasizes that the onset of instability is controlled jointly by electronic and structural energetics. Strong TM–O covalency expands the range over which ligand holes can be accommodated, while the lattice ultimately determines whether those holes remain distributed or condense into O–O species.

Discussion

The comparison of Li2_2MnO3_3 (M = Mn, Ru, Ir) reveals that ligand-hole character is a common feature of high-valent redox across the series, but that its presence alone does not determine electrochemical stability. Instead, the three compounds differ in how ligand holes are generated and accommodated within the hybridized TM–O electronic structure. This distinction can be understood through the interplay between the charge-transfer energy, ΔCT\Delta_{\mathrm{CT}}, and TM–O hybridization, tpdt_{pd}. Together, these parameters determine both the ligand-hole content of the ground state and how rapidly the system evolves toward strongly negative charge-transfer character upon delithiation.

Li2_2MnO3_3 and Li2_2IrO3_3 illustrate the two limiting cases. In Li2_2MnO3_3, the ground state is already strongly NCT before delithiation, with substantial dn+1L‾d^{n+1}\underline{L} and higher ligand-hole character. Further oxidation therefore drives a rapid increase in ligand-hole density from an already NCT starting point. In Li2_2IrO3_3, by contrast, strong Ir–O hybridization produces substantial ligand-hole character even while ΔCT\Delta_{\mathrm{CT}} remains slightly positive. Delithiation can consequently proceed through a broad range of strongly covalent states before the system becomes deeply NCT. Li2_2RuO3_3 lies between these limits, combining stronger TM–O hybridization than the Mn compound with a less NCT pristine electronic structure. The progression from Mn to Ru to Ir therefore separates two quantities that are often conflated: ligand-hole density and negative charge-transfer character.

This distinction places the NCT ground state at the center of the redox mechanism across high-energy Li2_2MO3_3 cathodes. From this perspective, different types of “oxygen redox”, such as long peroxo bonds [25, 28, 33], unbonded oxygen redox [14, 19, 41] or π\pi-redox networks [22, 50] can all be categorized as rearrangement of ligand hole density governed by the NCT ground state. However, the NCT ground state can enable stable, non-hysteretic electrochemical cycling below 4.5 V, avoiding oxygen evolution reactions while expanding the specific energy density of a cathode material via engineered structural stability (see section ?? and refs. [19, 20, 21]). On the other hand, oxygen dimerization and out-gassing are known phenomena when the battery voltage rises above 4.5 V [7, 8, 9, 35, 36, 39]. While this process can be somewhat reversible [25, 30], it will eventually lead to poor kinetics and capacity loss. Thus, we must prioritize stabilizing NCT ground states at high states of charge, as the large ligand hole density can easily lead to oxygen dimer formation.

Ultimately, these observations highlight the importance of the TM, as it plays a central role in dictating the stability of a high energy density cathode. At high voltages, the cathode likely exhibits an NCT ground state, where redox reactions occur on the highly hybridized TM–O. The overall stability of the cathode is dictated by the redox active TM–O framework. Cathodes that are doped with non-redox active TMs, such as Sn [25, 26, 34, 35], will have a lower energy density compared to its non-doped counterpart. On the other hand, doping heavy metals into 3d TM based cathodes can stabilize the excess ligand hole and the NCT ground states, allowing more lithium extraction per formula unit [24, 51]. Careful selection of the TM element is therefore key to designing cathode materials that combine high energy density with structural stability.

In conclusion, by using theoretical core-level spectroscopy calculations, we reveal the underlying mechanism responsible for the different electrochemical behaviors of Li-rich parent compounds with different TMs. We found the critical stabilization effect of heavy TMs is achieved through increased covalency, while NCT evolution remains the core universal redox mechanism among all materials. Here, extended dd-orbitals lead to a less NCT ground state and stronger covalency with the ligand orbitals. This leads to greater stability at high voltages without the formation of irreversible oxidized oxygen species. This new theoretical insight provides an alternative method and opens up new design rules for stabilizing NCT states for high energy density cathodes that avoid dimerizing “oxygen redox” and poor electrochemical reversibility [16].

Acknowledgements

This paper was supported in part by the U.S. Department of Energy, Office of Basic Energy Sciences, Materials Sciences and Engineering Division. Calculations were performed on the Sherlock cluster at Stanford University and on resources of the National Energy Research Scientific Computing Center (NERSC), a Department of Energy Office of Science User Facility, using NERSC award BES-ERCAP0027203. Experimental work was supported by Korea Institute for Advancement of Technology (KIAT) grant funded by the Korea Government (MOTIE) (RS-2024-00419413, HRD Program for Industrial Innovation) and the National Research Foundation of Korea (NRF) grant funded by the Korea government (MSIT) (RS-2025-00517846). Spectroscopic experiments are performed at Beamline 8.0.1.1 (iRIXS) and 6.0.2 (QERLIN) of the Advanced Light Source, a U.S. DOE Office of Science User Facility under contract no. DE-AC02-05CH11231.

Certain software is identified in this paper in order to specify the experimental procedure adequately. Such identification is not intended to imply recommendation or endorsement of any product or service by NIST, nor is it intended to imply that the materials or equipment identified are necessarily the best available for the purpose.

We thank William Chueh, Will Gent and Edward Mu for helpful discussions.

Author Contributions

T.P.D and W.Y. conceived the study. K.H.H and E.G.L. performed the DFT calculations and data analysis under the supervision of B.M., and T.P.D.. K.H.H and E.G.L. performed the spectroscopic XAS and RIXS simulations under the supervision of J.V., J.J.K., B.M., and T.P.D.. J.K, G. L., J. H. and W.Y. conducted synchrotron experiments and sample preparation. A.Z. and W.-S.L. conducted data analysis and revisions for the manuscript. K.H.H and E.G.L. wrote the first draft of the manuscript and all authors reviewed and approved the final version.

Competing Interests

The authors declare no competing interests.

Data Availability

Data is available from the authors upon reasonable request.

References

  1. [3]H. Kobayashi, M. Tabuchi, M. Shikano, H. Kageyama, and R. Kanno, Structure, and magnetic and electrochemical properties of layered oxides, Li₂IrO₃, Journal of Materials Chemistry 13, 957 (2003), https://pubs.rsc.org/jm/article-pdf/13/4/957/1047506/b207282c.pdf.
  2. [4]R. A. House, G. J. Rees, M. A. Pérez-Osorio, J.-J. Marie, E. Boivin, A. W. Robertson, A. Nag, M. Garcia-Fernandez, K.-J. Zhou, and P. G. Bruce, First-cycle voltage hysteresis in Li-rich 3d cathodes associated with molecular O₂ trapped in the bulk, Nature Energy 5, 777 (2020).DOI
  3. [5]R. A. House, J.-J. Marie, M. A. Pérez-Osorio, G. J. Rees, E. Boivin, and P. G. Bruce, The role of O₂ in O-redox cathodes for Li-ion batteries, Nature Energy 6, 781 (2021).DOI
  4. [6]J.-J. Marie, R. A. House, G. J. Rees, A. W. Robertson, M. Jenkins, J. Chen, S. Agrestini, M. Garcia-Fernandez, K.-J. Zhou, and P. G. Bruce, Trapped O₂ and the origin of voltage fade in layered Li-rich cathodes, Nature Materials 23, 818 (2024).DOI
  5. [7]J. Rana, J. K. Papp, Z. Lebens-Higgins, M. Zuba, L. A. Kaufman, A. Goel, R. Schmuck, M. Winter, M. S. Whittingham, W. Yang, B. D. McCloskey, and L. F. J. Piper, Quantifying the Capacity Contributions during Activation of Li₂MnO₃, ACS Energy Letters 5, 634 (2020).
  6. [8]Z. Zhuo, K. Dai, R. Qiao, R. Wang, J. Wu, Y. Liu, J. Peng, L. Chen, Y.-d. Chuang, F. Pan, Z.-x. Shen, G. Liu, H. Li, T. P. Devereaux, and W. Yang, Cycling mechanism of Li₂MnO₃: Li–CO₂ batteries and commonality on oxygen redox in cathode materials, Joule 5, 975 (2021).DOI
  7. [9]E. Cho, K. Kim, C. Jung, S.-W. Seo, K. Min, H. S. Lee, G.-S. Park, and J. Shin, Overview of the Oxygen Behavior in the Degradation of Li₂MnO₃ Cathode Material, The Journal of Physical Chemistry C 121, 21118 (2017).DOI
  8. [10]F. Massel, K. Hikima, H. Rensmo, K. Suzuki, M. Hirayama, C. Xu, R. Younesi, Y.-S. Liu, J. Guo, R. Kanno, M. Hahlin, and L.-C. Duda, Excess Lithium in Transition Metal Layers of Epitaxially Grown Thin Film Cathodes of Li₂MnO₃ Leads to Rapid Loss of Covalency during First Battery Cycle, The Journal of Physical Chemistry C 123, 28519 (2019).
  9. [11]G. Assat and J.-M. Tarascon, Fundamental understanding and practical challenges of anionic redox activity in Li-ion batteries, Nature Energy 3, 373 (2018).DOI
  10. [12]A. Grimaud, W. T. Hong, Y. Shao-Horn, and J.-M. Tarascon, Anionic redox processes for electrochemical devices, Nature Materials 15, 121 (2016).DOI
  11. [13]M. Ben Yahia, J. Vergnet, M. Saubanere, and M. L. Doublet, Unified picture of anionic redox in Li/Na-ion batteries, Nature Materials 18, 496 (2019).DOI
  12. [14]K. Luo, M. R. Roberts, R. Hao, N. Guerrini, D. M. Pickup, Y.-S. Liu, K. Edström, J. Guo, A. V. Chadwick, L. C. Duda, and P. G. Bruce, Charge-compensation in 3d-transition-metal-oxide intercalation cathodes through the generation of localized electron holes on oxygen, Nature Chemistry 8, 684 (2016).DOI
  13. [15]W. E. Gent, K. Lim, Y. Liang, Q. Li, T. Barnes, S.-J. Ahn, K. H. Stone, M. McIntire, J. Hong, J. H. Song, Y. Li, A. Mehta, S. Ermon, T. Tyliszczak, D. Kilcoyne, D. Vine, J.-H. Park, S.-K. Doo, M. F. Toney, W. Yang, D. Prendergast, and W. C. Chueh, Coupling between oxygen redox and cation migration explains unusual electrochemistry in lithium-rich layered oxides, Nature Communications 8, 2091 (2017).DOI
  14. [16]W. E. Gent, I. I. Abate, W. Yang, L. F. Nazar, and W. C. Chueh, Design Rules for High-Valent Redox in Intercalation Electrodes, Joule 4, 1369 (2020).DOI
  15. [17]B. Kim, J.-H. Song, D. Eum, S. Yu, K. Oh, M. H. Lee, H.-Y. Jang, and K. Kang, A theoretical framework for oxygen redox chemistry for sustainable batteries, Nature Sustainability 5, 708 (2022).DOI
  16. [18]B. Qiu, Y. Zhou, H. Liang, M. Zhang, K. Gu, T. Zeng, Z. Zhou, W. Wen, P. Miao, L. He, Y. Xiao, S. Burke, Z. Liu, and Y. S. Meng, Negative thermal expansion and oxygen-redox electrochemistry, Nature 640, 941 (2025).DOI
  17. [19]I. I. Abate, C. D. Pemmaraju, S. Y. Kim, K. H. Hsu, S. Sainio, B. Moritz, J. Vinson, M. F. Toney, W. Yang, W. E. Gent, T. P. Devereaux, L. F. Nazar, and W. C. Chueh, Coulombically-stabilized oxygen hole polarons enable fully reversible oxygen redox, Energy Environ. Sci. 14, 4858 (2021).DOI
  18. [20]R. A. House, U. Maitra, M. A. Pérez-Osorio, J. G. Lozano, L. Jin, J. W. Somerville, L. C. Duda, A. Nag, A. Walters, K.-J. Zhou, M. R. Roberts, and P. G. Bruce, Superstructure control of first-cycle voltage hysteresis in oxygen-redox cathodes, Nature 577, 502 (2020).DOI
  19. [21]H. Ramachandran, E. W. Mu, E. G. Lomeli, A. Braun, M. Goto, K. H. Hsu, J. Liu, Z. Jiang, K. Lim, G. M. Busse, B. Moritz, J. J. Kas, J. Vinson, J. J. Rehr, J. I. Abate, Y. Shimakawa, E. I. Solomon, W. Yang, W. E. Gent, T. P. Devereaux, and W. C. Chueh, A formal FeIII/IV redox couple in an intercalation electrode, Nature Materials 10.1038/s41563-025-02356-x (2025).
  20. [22]R. A. House, G. J. Rees, K. McColl, J.-J. Marie, M. Garcia-Fernandez, A. Nag, K.-J. Zhou, S. Cassidy, B. J. Morgan, M. Saiful Islam, and P. G. Bruce, Delocalized electron holes on oxygen in a battery cathode, Nature Energy 8, 351 (2023).DOI
  21. [23]Y. Li, X. Wang, Y. Gao, Q. Zhang, G. Tan, Q. Kong, S. Bak, G. Lu, X.-Q. Yang, L. Gu, J. Lu, K. Amine, Z. Wang, and L. Chen, Native Vacancy Enhanced Oxygen Redox Reversibility and Structural Robustness, Advanced Energy Materials 9, 1803087 (2019).DOI
  22. [24]M. Sathiya, K. Ramesha, G. Rousse, D. Foix, D. Gonbeau, A. S. Prakash, M. L. Doublet, K. Hemalatha, and J.-M. Tarascon, High Performance Li₂Ru1−yMnyO₃ (0.2 ≤ y ≤ 0.8) Cathode Materials for Rechargeable Lithium-Ion Batteries: Their Understanding, Chemistry of Materials 25, 1121 (2013).DOI
  23. [25]M. Sathiya, G. Rousse, K. Ramesha, C. P. Laisa, H. Vezin, M. T. Sougrati, M.-L. Doublet, D. Foix, D. Gonbeau, W. Walker, A. S. Prakash, M. Ben Hassine, L. Dupont, and J.-M. Tarascon, Reversible anionic redox chemistry in high-capacity layered-oxide electrodes, Nature Materials 12, 827 (2013).DOI
  24. [26]M. Sathiya, A. M. Abakumov, D. Foix, G. Rousse, K. Ramesha, M. Saubanère, M. L. Doublet, H. Vezin, C. P. Laisa, A. S. Prakash, D. Gonbeau, G. Van Tendeloo, and J.-M. Tarascon, Origin of voltage decay in high-capacity layered oxide electrodes, Nature Materials 14, 230 (2015).DOI
  25. [27]H. Kobayashi, R. Kanno, M. Tabuchi, H. Kageyama, O. Nakamura, and M. Takano, Structure and charge/discharge characteristics of new layered oxides: Li₁.₈Ru₀.₆Fe₀.₆O₃ and Li₂IrO₃, Journal of Power Sources 68, 686 (1997), proceedings of the Eighth International Meeting on Lithium Batteries.DOI
  26. [28]M. Saubanère, E. McCalla, J.-M. Tarascon, and M.-L. Doublet, The intriguing question of anionic redox in high-energy density cathodes for Li-ion batteries, Energy Environ. Sci. 9, 984 (2016).
  27. [29]Y. Wu, K. Zhou, F. Ren, Y. Ha, Z. Liang, X. Zheng, Z. Wang, W. Yang, M. Zhang, M. Luo, C. Battaglia, W. Yang, L. Zhu, Z. Gong, and Y. Yang, Highly reversible Li₂RuO₃ cathodes in sulfide-based all solid-state lithium batteries, Energy Environ. Sci. 15, 3470 (2022).DOI
  28. [30]Z. Zhuo, K. Dai, J. Wu, L. Zhang, N. Tamura, Y.-d. Chuang, J. Feng, J. Guo, Z.-x. Shen, G. Liu, F. Pan, and W. Yang, Distinct Oxygen Redox activities in Li₂MO₃ (M = Mn, Ru, Ir), ACS Energy Letters 6, 3417 (2021).DOI
  29. [31]Y. Yu, P. Karayevlayali, S. H. Nowak, L. Giordano, M. Gauthier, W. Hong, R. Kou, Q. Li, J. Vinson, T. Kroll, D. Sokaras, C.-J. Sun, N. Charles, F. Maglia, R. Jung, and Y. Shao-Horn, Revealing Electronic Signatures of Lattice Oxygen Redox in Lithium Ruthenates and Implications for High-Energy Li-Ion Battery Material Designs, Chemistry of Materials 31, 7864 (2019).DOI
  30. [32]L. Li, F. C. Castro, J. S. Park, H. Li, E. Lee, T. D. Boyko, J. W. Freeland, Z. Yao, T. T. Fister, J. Vinson, E. L. Shirley, C. Wolverton, J. Cabana, V. P. Dravid, M. M. Thackeray, and M. K. Y. Chan, Probing Electrochemically Induced Structural Evolution and Oxygen Redox Reactions in Layered Lithium Iridate, Chemistry of Materials 31, 4341 (2019).DOI
  31. [33]E. McCalla, A. M. Abakumov, M. Saubanère, D. Foix, E. J. Berg, G. Rouse, M.-L. Doublet, D. Gonbeau, P. Novák, G. V. Tendeloo, R. Dominko, and J.-M. Tarascon, Visualization of O-O peroxide-like dimers in high-capacity layered oxides for Li-ion batteries, Science 350, 1516 (2015).DOI
  32. [34]J. Hong, W. E. Gent, P. Xiao, K. Lim, D.-H. Seo, J. Wu, P. M. Csernica, C. J. Takacs, D. Nordlund, C.-J. Sun, K. H. Stone, D. Passarello, W. Yang, D. Prendergast, G. Ceder, M. F. Toney, and W. C. Chueh, Metal–oxygen decoordination stabilizes anion redox in Li-rich oxides, Nature Materials 18, 256 (2019).DOI
  33. [35]R. A. House, J.-J. Marie, J. Park, G. J. Rees, S. Agrestini, A. Nag, M. Garcia-Fernandez, K.-J. Zhou, and P. G. Bruce, Covalency does not suppress O2 formation in 4d and 5d Li-rich O-redox cathodes, Nature Communications 12, 2975 (2021).DOI
  34. [36]H. Li, B. Song, Y. Chen, X. Rui, R. F. Klie, T. D. Boyko, J. W. Freeland, M. K. Y. Chan, J. Liu, and J. Cabana, Structural and electronic changes in Li2RuO3 induced by lithium intercalation, Phys. Rev. Mater. 9, 125402 (2025).
  35. [37]J. Zaanen, G. A. Sawatzky, and J. W. Allen, Band gaps and electronic structure of transition-metal compounds, Phys. Rev. Lett. 55, 418 (1985).pubmed.ncbi.nlm.nih.gov/10032345
  36. [38]K. H. Hsu, khhsu0724/CTFAMultiplet: v1.0.0 (2025).DOI
  37. [39]E. G. Lomeli, Q. Li, K. H. Hsu, G.-H. Lee, Z. Zhuo, B.-J. Polzin, J. Gim, B. Shi, E. Lee, Y. Wang, H. Li, P. Yu, J. Wu, Z.-X. Shen, S. Yan, L. Lla, J. J. Kas, J. J. Rehr, J. Vinson, B. Moritz, Y.-S. Liu, J. Guo, Y. de Chuang, W. Yang, and T. P. Devereaux, Negative Charge Transfer: Ground State Precursor towards High Energy Batteries (2025), arXiv:2509.20622 [cond-mat.mtrl-sci].arxiv.org/abs/2509.20622
  38. [40]M. D. Radin, J. Vinckeviciute, R. Seshadri, and A. Van der Ven, Manganese oxidation as the origin of the anomalous capacity of Mn-containing Li-excess cathode materials, Nature Energy 4, 639 (2019).DOI
  39. [41]D.-H. Seo, J. Lee, A. Urban, R. Malik, S. Kang, and G. Ceder, The structural and chemical origin of the oxygen redox activity in layered and cation-disordered Li-excess cathode materials, Nature Chemistry 8, 692 (2016).DOI
  40. [42]D. R. Hamann, Optimized norm-conserving Vanderbilt pseudopotentials, Phys. Rev. B 88, 085117 (2013).DOI
  41. [43]J. Vinson, J. J. Rehr, J. J. Kas, and E. L. Shirley, Bethe-Salpeter equation calculations of core excitation spectra, Phys. Rev. B 83, 115106 (2011).DOI
  42. [44]J. Vinson, Advances in the ocean-3 spectroscopy package, Phys. Chem. Chem. Phys. 24, 12887 (2022).DOI
  43. [45]Z. Hu, H. von Lips, M. S. Golden, J. Fink, G. Kaindl, F. M. F. de Groot, S. Ebbinghaus, and A. Reller, Multiplet effects in the Ru L2,3 x-ray-absorption spectra of Ru(IV) and Ru(V) compounds, Phys. Rev. B 61, 5262 (2000).
  44. [46]H. Gretarsson, H. Suzuki, H. Kim, K. Ueda, M. Krautloher, B. J. Kim, H. Yavaş, G. Khaliullin, and B. Keimer, Observation of spin-orbit excitations and Hund’s multiplets in Ca2RuO4, Phys. Rev. B 100, 045123 (2019).DOI
  45. [47]W. Yang and T. P. Devereaux, Anionic and cationic redox and interfaces in batteries: Advances from soft X-ray absorption spectroscopy to resonant inelastic scattering, Journal of Power Sources 389, 188 (2018).DOI
  46. [48]H. Gretarsson, J. P. Clancy, X. Liu, J. P. Hill, E. Bozin, Y. Singh, S. Manni, P. Gegenwart, J. Kim, A. H. Said, D. Casa, T. Gog, M. H. Upton, H.-S. Kim, J. Yu, V. M. Katukuri, L. Hozoi, J. van den Brink, and Y.-J. Kim, Crystal-Field Splitting and Correlation Effect on the Electronic Structure of A2IrO3, Phys. Rev. Lett. 110, 076402 (2013).DOI
  47. [49]P. E. Pearce, A. J. Perez, G. Rouse, M. Saubanère, D. Batuk, D. Foix, E. McCalla, A. M. Abakumov, G. Van Tendeloo, M.-L. Doublet, and J.-M. Tarascon, Evidence for anionic redox activity in a tridimensional-ordered Li-rich positive electrode β-Li2IrO3, Nature Materials 16, 580 (2017).DOI
  48. [50]D. A. Kitchaeve, J. Vinckeviciute, and A. Van der Ven, Delocalized Metal–Oxygen π-Redox Is the Origin of Anomalous Non-hysteretic Capacity in Li-Ion and Na-Ion Cathode Materials, Journal of the American Chemical Society 143, 1908 (2021).
  49. [51]J. Xu, M. Sun, R. Qiao, S. E. Renfrew, L. Ma, T. Wu, S. Hwang, D. Nordlund, D. Su, K. Amine, J. Lu, B. D. McCloskey, W. Yang, and W. Tong, Elucidating anionic oxygen activity in lithium-rich layered oxides, Nature Communications 9, 947 (2018).DOI

Paper details

vlnc:W_3n3nnftm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents