betaFeedback

WorksPhysics and Astronomy

Crystal growth, magnetic, and transport properties of the candidate altermagnet Cr1/4_{1/4}NbS2_{2}

Abstract

Altermagnetism is a rapidly emerging paradigm in condensed matter magnetism, yet the number of experimentally confirmed altermagnetic candidates remains remarkably limited. Cr1/4_{1/4}NbS2_2 has long been theoretically proposed as a promising altermagnet, but there are no reports on experimental investigation of single crystals. Here, we report the successful growth of high-quality single crystals of Cr1/4_{1/4}NbS2_2 and present its structural, thermal, magnetic, and transport properties. Single-crystal X-ray diffraction provides detailed crystallographic information and confirms the hexagonal crystal symmetry (P63/mmcP6_3/mmc), one of the criteria for altermagnetic behavior. Resistivity and heat capacity measurements unambiguously identify an antiferromagnetic Néel temperature of TN∼141T_N \sim 141 K. Magnetotransport measurements reveal non-trivial features in the magnetoresistance and Hall response, indicative of quantum diffusive transport phenomena. Cr1/4_{1/4}NbS2_2, synthesized here for the first time in single-crystalline form, therefore serves as an experimental platform for probing the rich spectrum of phenomena predicted for altermagnetic materials.

Introduction

Magnetism has long been classified under two canonical paradigms: ferromagnetism (FM), characterized by net spontaneous magnetization, and antiferromagnetism (AFM), defined by compensated magnetic sublattices and zero net magnetization [1]. However, a third class of magnetic order, termed altermagnetism (AM), has recently emerged as a transformative concept that challenges this binary classification [2, 3]. Altermagnets are collinear, spin-compensated magnets that nevertheless exhibit momentum-dependent spin splitting in their electronic band structure, a property previously thought exclusive to ferromagnets and non-collinear antiferromagnets. This spin splitting arises not from spin-orbit coupling but from the real-space crystal symmetry connecting opposite-spin sublattices via rotational operations (proper or improper and symmorphic or non-symmorphic), rather than the inversion or translation symmetries characteristic of conventional antiferromagnets [4, 5, 6, 7, 8, 9, 10]. As a consequence, altermagnets combine the high stability and zero stray fields of antiferromagnets with the spin-polarized transport properties of ferromagnets, positioning them as promising candidates for next-generation spintronics [11].

Although the experimental studies of altermagnetism is still in its early stages, recent advances in experimental observations and theoretical calculations have revealed several exotic physical phenomena, including nonrelativistic lifted Kramers degeneracy [7, 12], anomalous spin transport [13, 14], magneto-optical effects [15, 16], and chiral magnons [17, 18]. The theoretical framework for altermagnetism has rapidly matured, with first-principles calculations predicting huge number of candidate materials spanning insulators, semiconductors, and metals [19, 20, 21, 22, 23, 24, 25]. Among the most widely studied candidates are RuO2_2 [26], α\alpha-MnTe [27], CrSb [28], MnF2_2 [29], Mn5_5Si3_3 [30] and La2_2CuO4_4 [31] which collectively span a broad range of Néel temperatures (TN=69T_{\mathrm{N}} = 69–400 K) and spin-splitting magnitudes (10–1400 meV) [4]. RuO2_2 has attracted the most intense scrutiny as the archetypal altermagnet, due to its rutile crystal structure and predictions of giant spin splitting [32]. However, the magnetic ground state of RuO2_2 remains vigorously debated: whereas neutron diffraction and transport studies report signatures of altermagnetism [33, 34], muon spin rotation (μ\muSR) measurements find no evidence of broken time-reversal symmetry, leaving the question unresolved if RuO2_2 even possesses any magnetic order [35]. α\alpha-MnTe has been shown to exhibit anisotropic band splitting of 0.8 eV arising from time-reversal symmetry breaking, as observed using angle-resolved photoemission spectroscopy (ARPES) in combination with first-principles calculations, providing the first direct experimental evidence of altermagnetic band splitting [36]. CrSb on the other hand shows a significant spin splitting of 0.6 eV detected using soft X-ray ARPES with position of the electronic bands just below the Fermi energy making it an ideal candidate for spintronics devices [37]. Despite these advances, the number of experimentally confirmed altermagnetic candidates remains remarkably small compared to the large pool of theoretically proposed systems. This is perhaps surprising, given that recent symmetry analyses suggest altermagnetism to be the default behavior in antiferromagnets, with spin splitting being ubiquitous rather than exceptional [38]. The scarcity of confirmed candidates thus reflects not a true rarity in nature, but rather the demanding experimental requirements needed to unambiguously identify altermagnetic signatures, and hence pressing need for new, well-characterized candidate materials.

Cr1/4_{1/4}NbS2_2 is a member of the family of transition metal-intercalated transition metal dichalcogenides (TMDs) and has recently been predicted to be a potential altermagnet [19, 20, 22]. Band structure calculations by Guo et al. [22] reveal significant spin splitting in the electronic bands even in the absence of spin–orbit coupling, a key hallmark of altermagnetic behavior. Notably, Cr1/4_{1/4}NbS2_2 is among the few proposed altermagnetic candidates that exhibit metallic conductivity, making it particularly attractive for magnetotransport studies [22]. Further motivation comes from a recent experimental study on Co1/4_{1/4}NbSe2_2, another member of the same TM1/4NbX2TM_{1/4}NbX_2 (TMTM = transition metal, XX = S, Se, Te) family, in which clear evidence of altermagnetic band splitting was demonstrated through combined DFT calculations and ARPES measurements [39]. Cr1/4_{1/4}Nb2_2S2_2 has thus emerged as a theoretically compelling altermagnetic candidate warranting detailed experimental investigation. However, experimental studies on this material remain scarce, and all prior investigations have been conducted exclusively on polycrystalline specimens [40, 41]. The orientation dependent magnetic and magnetotransport studies are essential for probing the anisotropic electronic and magnetic properties predicted for altermagnets. In this work, we report the successful growth of high-quality single crystals of Cr1/4_{1/4}NbS2_2 by the chemical vapor transport technique and present a comprehensive investigation of their structural, chemical, magnetic, and transport properties. Using single-crystal X-ray diffraction we obtain the detailed crystallographic information and further confirm the hexagonal crystal symmetry required to observe the altermagnetic behavior. Electrical resistivity and heat capacity measurements unambiguously establish an antiferromagnetic Néel temperature of TN∼141T_N \sim141 K, while magnetotransport measurement shows unusual features indicative of diffusive quantum transport phenomenon. The successful synthesis of Cr1/4_{1/4}NbS2_2 single crystals and the systematic experimental investigation of their transport and magnetic properties presented here pave the way for future exploration of altermagnetic behaviour in this compound.

Experimental Methods

Single crystals of Cr1/4_{1/4}NbS2_2 were grown by the chemical vapor transport (CVT) method, the details of which are described in Sec. III A. The quality and orientation of the as-grown single crystals were determined by X-ray Laue diffraction using a Photonic Science Laue camera system operating in back-scattering geometry. Single-crystal X-ray diffraction (SCXRD) measurements were performed using a Rigaku Oxford Diffraction Synergy S diffractometer, employing mirror monochromated Mo-Kα_\alpha radiation (λ=0.70173\lambda= 0.70173 Å) generated by a microfocus sealed tube Photon-Jet X-ray source, with diffracted intensities recorded on a HyPix hybrid photon-counting detector. A platelet-shaped single-crystal specimen of dimensions approximately 0.2×0.2×0.20.2 \times0.2 \times0.2 mm3^3, cut from a larger crystal, was measured at 100 K. The intensities were integrated using the CrysAlisPro [42] and the structure solution and refinement were carried out using OLEX2 [43]. The chemical homogeneity and average elemental composition of the single crystals were confirmed by scanning electron microscopy (SEM) coupled with energy-dispersive X-ray spectroscopy (EDX), carried out using a ZEISS GeminiSEM 500 field-emission SEM (FESEM) equipped with an Oxford Instruments EDX detector. EDX spectra were collected at 15–20 different points across a crystal specimens to obtain an average elemental composition. This was further repeated for 4-5 crystal specimens in order to confirm the homogeneity of the crystals grown in this batch. Heat capacity measurements were performed in a Quantum Design Physical Property Measurement System (PPMS) using the 2τ2\tau thermal relaxation method at temperatures from 2 to 270 K in zero applied field. Since the individual single crystals were too small for reliable standalone measurement, several crystals were stacked together using Apiezon N grease to achieve a total sample mass of approximately 12–13 mg. A small error in the absolute heat capacity values may arise due to an uncertainty in the mass of the N grease used to stack the crystals together. DC magnetization measurements were performed as a function of temperature (1.8–300 K) and applied magnetic field (0–7 T) using a Quantum Design Magnetic Property Measurement System (MPMS) magnetometer. Electrical resistivity and Hall measurements were carried out as a function of temperature (1.8–300 K) and magnetic field (0–9 T) using the AC transport option of a Quantum Design PPMS, with excitation currents in the range 1–10 mA at a frequency of 113 Hz for all the transport measurements.

Results and Discussion

Crystal growth of Cr1/4_{1/4}NbS2_2

Single crystals of Cr1/4_{1/4}NbS2_2 were grown by the chemical vapor transport method using a polycrystalline precursor of Cr1/4_{1/4}NbS2_2. The polycrystalline precursor was prepared via solid-state synthesis. Stoichiometric quantities of chromium (powder, 99%, Thermo Scientific), niobium (powder, 99.99%, Thermo Scientific), and sulfur (powder, 99.99%, Thermo Scientific) were thoroughly ground together inside an argon-filled glovebox and sealed in an evacuated quartz ampoule. To avoid a buildup of pressure from sulfur vapor, the sealed ampoule was initially heated slowly to 450 °C at a rate of 15 °C/hr in several steps. The ampoule was subsequently heated to 950 °C, held at this temperature for 100 hr, and finally cooled slowly to room temperature at a rate of 5 °C/hr. The resulting ingot was thoroughly ground to obtain a fine powder. For the crystal growth, the powder was sealed in a quartz ampoule together with iodine (I2_2, ACS reagent, ≥99.8%, Sigma-Aldrich) as the transporting agent. The ampoule was then placed in a two-zone furnace with the source zone maintained at 950 °C and the sink zone at 800 °C (temperature gradient ΔT≈150\Delta T \approx150 °C) for a duration of 20 days. The process is similar to that used for Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_{2} [44, 45]. Shiny, platelet-like single crystals of approximate dimensions 2×2×0.5 mm32 \times2 \times0.5\ \mathrm{mm}^{3} were obtained at the sink end of the ampoule after the transport reaction, as shown in Figure 1(a). The Laue back-scattering image of a representative crystal is shown in Figure 1(b). The sharp, well-defined Laue spots, corresponding to (hk0)(hk0) reflections and obtained with the c-axis oriented perpendicular to the crystal surface, exhibit the six-fold symmetry characteristic of the hexagonal system, confirming the high crystalline quality of the grown single crystals. Figure 1(c) shows the X-ray diffraction pattern in the plane of the single crystal collected in a Bragg–Brentano geometry, showing only (00l)(00l) reflections, confirming the abab-plane orientation of the crystal. The homogeneity and chemical composition of the grown single crystals are presented in the Supplemental Material Sec. A [46]. The average composition obtained from EDX analysis is Cr0.261(6)NbS1.95(2)\mathrm{Cr}_{0.261(6)}\mathrm{NbS}_{1.95(2)}, in good agreement with the nominal stoichiometry of Cr0.25NbS2\mathrm{Cr}_{0.25}\mathrm{NbS}_{2} within the experimental uncertainty of the EDX measurements.

Figure 1. (a) Image of an as-grown single crystal of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2; each grid square corresponds to 1 mm ×\times 1 mm. (b) Back-scattering Laue diffraction pattern collected from the crystal shown in (a) confirms the crystallographic abab-plane lies in the plane of the crystal. (c) X-ray diffraction pattern recorded in Bragg–Brentano geometry, showing dominant (00l)(00l) reflections, confirming that the plane of the crystal shown in (a) corresponds to the abab-plane. Crystal structure of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 visualized using VESTA [47]: (d) projection in the abab-plane showing the triangular arrangement of Cr3+\mathrm{Cr}^{3+} ions (orange dashed lines), and (e) projection along the cc-axis illustrating the alternating 2H–NbS2\mathrm{NbS}_2 and Cr3+\mathrm{Cr}^{3+} intercalation layers, with Cr3+\mathrm{Cr}^{3+} occupying the 2a Wyckoff site (purple dashed lines).

Crystal Structure

Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_{2} belongs to the family of transition metal-intercalated transition metal dichalcogenides with the general formula CrxNbS2\mathrm{Cr}_{x}\mathrm{NbS}_{2}, which crystallizes in two distinct symmetries depending on the concentration xx of the intercalant [41, 48]. For x=1/3x = 1/3, the system adopts the noncentrosymmetric chiral space group P6322P6_{3}22, where the Cr atoms occupy the 2c Wyckoff position and order into a (3×3)R30∘(\sqrt{3} \times\sqrt{3})\mathrm{R}30^{\circ} superstructure [49, 50]. The resulting broken inversion symmetry gives rise to a Dzyaloshinskii–Moriya interaction, driving a chiral helimagnetic ground state and, under applied field, a chiral soliton lattice, both of which have been extensively investigated in the literature [44, 51, 52, 53, 54]. For x=1/4x = 1/4, the system instead crystallizes in the centrosymmetric space group P63/mmcP6_{3}/mmc, where the Cr atoms occupy the octahedral 2a Wyckoff sites and form a 2×22 \times2 in-plane superstructure [40, 41]. Here, the inversion symmetry is preserved and Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_{2} is expected to exhibit conventional magnetic ordering. Single-crystal X-ray diffraction measurements on a crystal specimen grown in this work confirms the P63/mmcP6_{3}/mmc symmetry, in agreement with the early work of Van Laar et al. [40]. The data collection strategy, crystallographic information, and refinement parameters are summarized in Table I. The atomic positions, refined occupancy and corresponding isotropic atomic displacement parameters are listed in Table II. The refined occupancy of Cr3+\mathrm{Cr}^{3+} at the 2a Wyckoff site is marginally below full occupancy, however, it remains 1 to within the experimental error bars. The crystal structure of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_{2}, visualized using VESTA, is shown in Figure 1 (d, Figure 1e). The Cr3+\mathrm{Cr}^{3+} ions form a triangular network in the abab-plane, as shown in Figure 1(d), while Figure 1(e) illustrates the stacking of 2H–NbS2\mathrm{NbS}_2 layers along the cc-axis with the Cr ions occupying the octahedral (2a - Wyckoff site) interlayer sites. The centrosymmetric space group of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 suppresses the Dzyaloshinskii–Moriya interaction that drives helimagnetic order in non-centrosymmetric Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2, and provides a crystallographic framework which is consistent with the symmetry requirements favorable for altermagnetism.

AtomsWyckxxyyzzOcc.UisoeqU_{\mathrm{iso}}^{\mathrm{eq}} (Å2^2)
Cr2a1.00001.00000.50000.97(4)0.0297(13)
Nb12b1.00001.00000.250010.0281(10)
Nb26h0.4942(12)0.9884(2)0.250010.0285(10)
S112k0.8328(15)1.1671(15)0.3811(3)10.0289(12)
S24f0.33330.66670.1152(3)10.0289(13)

Table II. Atomic coordinates xx, yy, zz and the equivalent atomic displacement parameter of single crystal Cr1/4_{1/4}NbS2_2 at 100 K. Unique reflections (obs/all) = 293 / 301, criterion of observability: I>2σ(I)I > 2\sigma(I), RF=0.0911R_{\mathrm{F}} = 0.0911, No. of refined parameters = 19, Refinement method used: least-squares on F, Space group: P63/mmcP6_3/mmc. The anisotropic atomic displacement parameters are shown in the Supplemental Material Sec. B Table S2 [46].

Crystallographic data and refinement parameters for SCXRD of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_{2} single crystal.
Temperature (K)100
Crystal systemHexagonal
Space groupP63/mmcP6_{3}/mmc
No.194
aa (Å)6.62280(10)
cc (Å)11.9573(3)
Volume (Å3^{3})454.200(18)
ZZ2
Density (g/cm3^{3})4.96
Wavelength (Å)0.71073
Rotation per image (deg)0.2
Exposure time (sec)10
θ\theta (°)3.41 to 30.45
Index ranges−9≤h≤9-9 \le h \le9
−9≤k≤9-9 \le k \le9
−17≤l≤17-17 \le l \le17
Absorption, μ\mu (mm−1^{-1})7.78
Tmin⁡T_{\min}, Tmax⁡T_{\max}0.001, 0.009
Criterion of observabilityI>2σ(I)I > 2\sigma(I)
No. of reflections measured12285
Unique reflections (obs/all)293/301
RintR_{\mathrm{int}}0.0622
No. of parameters19
RFR_{\mathrm{F}} (obs)0.0911
wRFwR_{\mathrm{F}} (all)0.2617
GoF1.360
Δρmin⁡\Delta\rho_{\min}, Δρmax⁡\Delta\rho_{\max} (e Å−3^{-3})-1.423, 5.523

Table 1. Crystallographic data and refinement parameters for SCXRD of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_{2} single crystal.

Heat Capacity

The temperature dependence of the heat capacity for single crystal Cr1/4_{1/4}NbS2_2 is shown in Figure 2. The heat capacity exhibits a small λ\lambda-like anomaly characteristic of a second-order phase transition. A view of the CpC_{\mathrm{p}} vs TT data around this anomaly is shown in the top-left inset of Figure 2. This feature signals an antiferromagnetic transition, with the Néel temperature, TNT_{\mathrm{N}}, determined to be 141(1) K, in good agreement with the value obtained from resistivity measurements (see Sec. III E). At high temperatures, the heat capacity approaches the classical Dulong–Petit limit, given by 3NR3NR, where NN is the number of atoms per formula unit and RR is the universal gas constant. For Cr1/4_{1/4}NbS2_2 (N=13N = 13), this corresponds to ∼324\sim324 J mol−1^{-1} K−1^{-1}. At low temperatures the data were fit using the relation Cp(T)/T=γ+βT2C_{\mathrm{p}}(T)/T = \gamma+ \beta T^2, as shown in the bottom-right inset of Figure 2, where γ\gamma is the Sommerfeld coefficient (electronic contribution) and βT3\beta T^3 is made up of lattice (phonon) and a spin-wave (magnon) contributions. The fit yields γ=11.3(2)\gamma= 11.3(2) mJ mol−1^{-1} K−2^{-2} and β=0.336(4)\beta= 0.336(4) mJ mol−1^{-1} K−4^{-4}. The value of γ\gamma is consistent with reports for other members of the family of transition metal intercalated transition metal dichalcogenide [55]. The Cp(T)C_{\mathrm{p}}(T) data were fit between 145 and 270 K using a Debye model including an electronic (γT\gamma T) term, in order to estimate the non-magnetic contribution to the heat capacity, with the fit then extrapolated to 0 K (see Figure 2). The fit gave a Debye temperature θD\theta_{\mathrm{D}} of 502(3) K. Subtracting this non-magnetic component gave the magnetic contribution to the heat capacity Cmag(T)C_{\mathrm{mag}}(T). See Supplemental Material for more details on estimating Cmag(T)C_{\mathrm{mag}}(T) [46].

Temperature dependence of the heat capacity of Cr1/4NbS2

Figure 2. Temperature dependence of the heat capacity of Cr1/4_{1/4}NbS2_2. The solid orange line is a fit to the non-magnetic contribution to the heat capacity, as described in the text. The top-left inset shows a magnified view of the data near the transition temperature TNT_{\mathrm{N}} of 141(1) K. The inset bottom right shows the Cp/TC_p/T vs T2T^2 behavior at low temperature; the red solid is a linear fit to the data (details of which are described in the text).

Having obtained Cmag(T)C_{\mathrm{mag}}(T), the magnetic entropy associated with the ordering of the Cr moments was then estimated to be 9.7 J mol−1^{-1} K−1^{-1}, a little below the expected value of Rln⁡(2S+1)=11.53R \ln(2S+1) = 11.53 J mol−1^{-1} K−1^{-1} for a Cr3+^{3+} ion with S=32S = \frac{3}{2} (see Supplemental Material [46]). This analysis reveals that a large fraction of the magnetic entropy associated with the magnetic ordering is released well below TNT_{\mathrm{N}}, leading to the small anomaly in Cp(T)C_p(T) at the transition. Notably, both the absolute value of the heat capacity and the magnitude of the anomaly at the transition, closely match those reported for the related compound Cr1/3_{1/3}TaS2_2 [56], suggesting a similar strength of magnetic exchange interactions and comparable phonon spectra between the two systems, consistent with their closely related crystal and possibly magnetic structures.

Magnetization

The magnetic susceptibility as a function of temperature for a single crystal of Cr1/4_{1/4}NbS2_2 for two crystallographic orientations, H⊥cH \perp c and H∥cH \parallel c, are shown in Figure 3(a). At lower temperatures the data are dominated by a ferromagnetic component with an ordering temperature, TCT_{\mathrm{C}}, of approximately 75 K. Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 is expected to exhibit an antiferromagnetic transition close to 141 K, as evident from the heat capacity (see Sec. III C) and electrical resistivity (see Sec. III E) measurements. It is therefore worth pausing here to explain the origin of this ferromagnetic signal.

Figure 3. (a) Zero-field-cooled (ZFC) and field-cooled (FC) χ(T)\chi(T) measured under an applied field of μ0H=10\mu_0H = 10 mT for H⊥cH \perp c and H∥cH \parallel c. Inverse magnetic susceptibility, χ−1\chi^{-1}, as a function of temperature for a Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 single crystal with (b) H⊥cH \perp c and (c) H∥cH \parallel c. The open circles represent the experimental data and the black solid lines denote the Curie-Weiss fits performed in the temperature range 200–300 K. The grey dashed line denotes the region of change of slope in χ−1(T)\chi^{-1}(T) near 141 K.

In intercalated CrxNbS2\mathrm{Cr}_x\mathrm{NbS}_2 compounds, the Cr atoms occupy the van der Waals gap between the 2H-NbS2\mathrm{NbS}_2 layers. The magnetic ordering temperatures and the nature of the magnetic ground state are strongly dependent on the Cr occupancy xx. For the x=1/3x = 1/3 compound, the exchange interactions between the Cr moments stabilize long-range ferromagnetic order in the temperature range of 111–127 K [54], below which a rich variety of magnetic phases have been reported, including chiral helimagnetic order, a field-induced chiral soliton lattice, and forced ferromagnetism [44]. The TCT_\mathrm{C} in these compounds is highly sensitive to disorder effects, which have been shown to suppress TCT_\mathrm{C} [57, 58]. The ferromagnetic signal observed in the magnetic susceptibility [Fig. 3(a)] originates from Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 intergrowths. The onset of this ferromagnetic signal occurs at ∼75\sim75 K, which is much lower than the intrinsic TCT_\mathrm{C} of bulk Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2. This suppression of TCT_\mathrm{C} is attributed to the high degree of structural disorder inherent to these intergrowths, which are spatially confined within small domains embedded in the majority Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 matrix. The fact that χ(T)\chi(T) below 75 K is an order of magnitude lower than that expected for bulk Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 [44] (see Supplemental Material for a direct comparison between the χ(T)\chi(T) for Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 and Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 [46]), corroborates the view that the Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 phase is present only as a minority intergrowth within a Cr1/4_{1/4}NbS2_2 matrix. The presence of intergrowths appears to be an intrinsic and unavoidable feature of these systems in general e.g., Cr1/4_{1/4}XS2_2 crystals, with similar observations reported for the related compound Cr1/4_{1/4}TaS2_2, where minority Cr1/3_{1/3}TaS2_2 domains also dominate the magnetization measurements [56].

The χ−1(T)\chi^{-1}(T) curves reveal a clear change of slope near 141 K, as shown in Figure 3(b, Figure 3c), reflecting the intrinsic antiferromagnetic behavior of the Cr1/4_{1/4}NbS2_2 phase. Curie-Weiss fits to the modified Curie-Weiss equation, χ(T)=CT−θCW+χ0\chi(T) = \frac{C}{T-\theta_{\rm CW}} + \chi_0 are also shown in Figure 3(b, Figure 3c). The parameters extracted from the fitting are given in Table III. At high-temperature χ−1(T)\chi^{-1}(T) for HH applied parallel and perpendicular to the cc-axis yields an effective magnetic moment μeff\mu_{\rm eff} of ∼3.8 μB\sim3.8\,\mu_{\rm B}, consistent with the expected value for Cr3+^{3+} in the S=3/2S = 3/2 state (μeffcalc=3.87 μB\mu_{\rm eff}^{\rm calc} = 3.87\,\mu_{\rm B}). The Curie-Weiss temperatures obtained for H⊥cH \perp c and H∥cH \parallel c are θCW⊥∼+32\theta_{\rm CW}^{\perp} \sim+32 K and θCW∥∼+15\theta_{\rm CW}^{\parallel} \sim+15 K, respectively.

Orientationχ0\chi_0 (m3^3 molCr−1_{\rm Cr}^{-1})μeff\mu_{\rm eff} (μB\mu_{\rm B}/f.u.)θCW\theta_{\rm CW} (K)
H⊥cH \perp c−3.51×10−8-3.51 \times10^{-8}3.80(2)32(2)
H∥cH \parallel c−2.60×10−8-2.60 \times10^{-8}3.79(2)15(2)

Table III. Curie-Weiss parameters for Cr1/4_{1/4}NbS2_2 from fits made to χ−1(T)\chi^{-1}(T) in the temperature range 200–300 K for two crystallographic orientations, H⊥cH \perp c and H∥cH \parallel c.

The positive values of θCW\theta_{\rm CW} in both orientations are notable given that bulk Cr1/4_{1/4}NbS2_2 is an antiferromagnet with TN=141T_{\rm N} = 141 K. A similar behavior is observed in many magnetic systems, for example, in A-type antiferromagnets with in-plane ferromagnetic order and antiferromagnet coupling between planes [59, 60]. More specifically, in the family of two-dimensional magnetic van der Waals materials, for example, single crystal CrCl3_3 orders antiferromagnetically below 17 K, yet the Curie-Weiss temperatures are positive for fields applied both in- and out-of-plane due to ferromagnetic interactions that dominate in the paramagnetic state [61, 62]. Competing ferromagnetic and antiferromagnetic interactions yielding a positive θCW\theta_{\rm CW} have also been reported in other members of the transition-metal-intercalated transition metal dichalcogenide family, including V1/4_{1/4}NbSe2_2 [63], Co0.26_{0.26}TaS2_2 [64], and Cr1/4_{1/4}TaS2_2 [56]. We also note that the small volume of ferromagnetic Cr1/3_{1/3}NbS2_2 intergrowths, could contribute, in part, to the positive θCW\theta_{\rm CW} values.

Figures 4(a, b) show the magnetization as a function of applied field for a single crystal of Cr1/4_{1/4}NbS2_2 for two different crystallographic orientations. For H⊥cH \perp c, as shown in Figure 4(a), the magnetization does not saturate in fields up to 5 T and instead increases linearly with field. The maximum moment achieved at 5 T is 0.31 μB\mu_{\mathrm{B}}/f.u., which is an order of magnitude lower than the saturation moment expected for Cr3+^{3+} (3 μB\mu_{\mathrm{B}}/f.u.), consistent with the compensated antiferromagnetic ordering of the sample. The linear behavior persists down to 80 K, below which a slight SS-shaped feature emerges with negligible hysteresis. At 2 K, the magnetization shows signs of saturation around 0.2 μB\mu_{\mathrm{B}}/f.u., accompanied by a hysteresis loop with a coercivity of 23 mT, before continuing to increase linearly with field. The hysteresis behavior, highlighted in the inset of Figure 4(a), arises from the ferromagnetic Cr1/3_{1/3}NbS2_2 intergrowths in the sample. Assuming that the signal of 0.2 μB\mu_{\mathrm{B}}/f.u. arises solely from these intergrowths, an upper bound for the impurity fraction can be estimated from MsampleMsat\frac{M_{\mathrm{sample}}}{M_{\mathrm{sat}}}, normalized by the respective molecular weights, of approximately 5–6%. This is strictly an upper bound, as the magnetization in fact has several contributions including the antiferromagnetic response from the main Cr1/4_{1/4}NbS2_2 phase which increases linearly with the applied field and possibly an intrinsic weak ferromagnetic component, analogous to that reported in α\alpha-MnTe [65].

Figure 4. Magnetization as a function of applied field measured at various temperatures for (a) H⊥cH \perp c and (b) H∥cH \parallel c. The inset shows an enlarged view of the MM vs HH data at 2 K.

A similar behavior is observed for H∥cH \parallel c. The MM vs HH response is linear above 80 K, and below 80 K the curve evolves into an SS-shaped profile, eventually developing a clear hysteresis at 2 K, as shown in the inset of Figure 4(b). The anisotropy observed in the hysteresis loops between the H⊥cH \perp c and H∥cH \parallel c orientations is likely a consequence of the intrinsic magnetic anisotropy of the Cr1/3_{1/3}NbS2_2 intergrowths. An analogous behavior has been reported for Cr1/4_{1/4}TaS2_2 [56].

Magnetotransport

Magnetotransport measurements were conducted using a five-point wire configuration to simultaneously measure the longitudinal resistivity ρxx\rho_{xx} and transverse Hall resistivity ρxy\rho_{xy}, with H∥cH \parallel c and I⊥cI \perp c. Both ρxx\rho_{xx} and ρxy\rho_{xy} are symmetrized and antisymmetrized, respectively, before analysis; the process is summarized in Supplementary Material [46]. Figure 5(a) shows the temperature dependence of the zero-field longitudinal resistivity. The curve exhibits metallic behavior with a sharp drop at ∼141\sim141 K (the inset in Figure 5(a) shows a pronounced dip in d2ρxx(T)/dT2\mathrm{d}^{2}\rho_{xx}(T)/\mathrm{d}T^{2} versus temperature around this temperature), attributed to the suppression of spin disorder scattering as the system undergoes a paramagnetic to antiferromagnetic phase transition [66], establishing the Néel temperature of Cr1/4_{1/4}NbS2_2 at TN∼141(1)T_{\mathrm{N}} \sim141(1) K. The residual resistivity ratio, RRR =ρ(400 K)/ρ(2 K)∼10= \rho(400\ \mathrm{K})/\rho(2\ \mathrm{K}) \sim10, is comparable to that reported for the related compound Cr1/4_{1/4}TaS2_2 [56]. This value is reasonably high for the broader family of transition-metal-intercalated dichalcogenides, where single crystals typically exhibit RRR values below 10 [67, 68], and in several cases as low as 2–3 [39, 69, 70]. This, therefore, confirms the high quality of the Cr1/4_{1/4}NbS2_2 single crystals investigated in this work. Figure 5(b-Figure 5e) present the magnetoresistance (MR) of the sample as a function of applied magnetic field, defined as MR =ρ(H)−ρ(0)ρ(0)×100%= \frac{\rho(H)-\rho(0)}{\rho(0)} \times100\%, where ρ(H)\rho(H) is the longitudinal resistivity at an applied magnetic field HH and ρ(0)\rho(0) is the zero-field resistivity. The MR behavior evolves significantly with temperature and can be categorized into distinct regimes as described below. At low temperatures (T≤30T \le30 K), the MR exhibits a nearly parabolic field dependence (MR ∝H2\propto H^2) over the entire field range as shown in Figure 5(b),

Magnetotransport measurements on Cr$_{1/4}$NbS$_2$

Figure 5. Magnetotransport measurements on Cr1/4_{1/4}NbS2_2. (a) Temperature dependence of ρxx(T)\rho_{xx}(T) measured under H∥cH \parallel c-axis. The inset shows the second derivative d2ρxx(T)/dT2\mathrm{d}^{2}\rho_{xx}(T)/\mathrm{d}T^{2} as a function of temperature, displaying a sharp dip at the Néel temperature TN=141T_{\mathrm{N}} = 141 K. (b) Magnetoresistance (MR) as a function of μ0H\mu_{0}H for temperatures ranging from 2 to 35 K. The gray arrow indicates the kink around 3 T. The inset highlights the linear field dependence of MR below 3 T at 2 K. (c) MR as a function of μ0H\mu_{0}H for temperatures in the range 50 to 210 K. (d) MR as a function of μ0H\mu_{0}H at selected temperatures of 50, 70, 110, and 130 K, with grey arrows marking the anomalous features. (e) Temperature dependence of MR evaluated at μ0H=9\mu_{0}H = 9 T. The dashed line indicates the MR = 0. The inset shows the same data on a square root scale to highlight the behavior close to TNT_{\mathrm{N}}. (f) Hall resistivity ρxy\rho_{xy} as a function of μ0H\mu_{0}H for temperatures in the range 50 to 210 K. The inset shows the corresponding low-temperature data for 2 to 35 K. (g) Anomalous Hall resistivity as a function of μ0H\mu_{0}H at different temperatures. (h) Variation of AHE at 9 T as a function of temperature. (i) Carrier concentration nHn_{\mathrm{H}} (left axis) and carrier mobility μH\mu_{\mathrm{H}} (right axis) as a function of temperature.

with a slight deviation towards linear behavior at low fields below 2.5 T [see inset of Figure 5(b)]. This quadratic field dependence is characteristic of multi-carrier transport within the semiclassical Boltzmann transport theory [71]. A deviation from parabolic behavior occurs above 30 K. At 35 K, altough the parabolic behavior of the MR persists, the curve develops two kink-like features near ±3.3\pm3.3 T [gray arrows in Figure 5(b)]. The higher temperature data (above 35 K) is shown in Figure 5(c), and at 50 K, these kinks evolve into two prominent positive cusps centered at ∼±3.3\sim\pm3.3 T; the MR becomes negative (∼−0.3%\sim-0.3\%) at low fields, rises through the cusps, and eventually recovers to a positive value of ∼0.6%\sim0.6\% at 9 T. At 70 K, the MR becomes entirely negative, following a linear field dependence and reaching ∼−0.6%\sim-0.6\%, before appearing to saturate above 7 T. The curve at 70 K displays an inverted curvature compared to the 50 K isotherm, with a positive cusp appearing at the same field near 3.3 T. Upon further warming to 110 K, the MR continues to remain negative (∼−0.05%\sim-0.05\%) rises through the cusp with increasing field, eventually reaching a positive value of ∼0.03%\sim0.03\%. At 130 K, the MR exhibits a feature that is the mirror image of that observed at 70 K. The field dependence of the curvature of MR at 50, 70, 110 and 130 K temperatures is magnified in Figure 5(d). Further details of the evolution of MR(HH) at different temperatures are provided in the Supplemental Material [46]. Above 130 K, the MR reverts back to a parabolic behavior, however the MR inverted as compared to that at 2 K. The temperature evolution of the magnetoresistance at 9 T is summarized in Figure 5(e). The MR reaches a maximum value of ∼12.7%\sim12.7\% at 2 K, and decreases monotonically with increasing temperature up to 50 K, beyond which it changes sign and becomes negative. The magnitude of the negative MR grows upon further warming, reaching a pronounced dip near 70 K, before recovering toward zero. A further suppression is observed at the Néel temperature TN=141T_{\mathrm{N}} = 141 K, above which the MR saturates and remains nearly temperature independent above 150 K. The non-monotonic evolution of MR with both field and temperature, including the sign changes and cusp-like features, is indicative of quantum diffusive transport phenomena commonly observed in disordered metals [72], dilute magnetic semiconductors [73], or topological insulators [74] arising from constructive and destructive interference between electron trajectories scattered by disorder or spin textures leading to weak localization and weak anti-localization effects [75].

The Hall resistivity at several temperatures ranging from 2 to 210 K is shown in Figure 5(f). The total Hall resistivity ρxy\rho_{xy} in magnetic materials is conventionally decomposed as ρxy=R0μ0H+ρxyAHE\rho_{xy} = R_0\mu_0H + \rho_{xy}^{\mathrm{AHE}}, where the first term is the ordinary Hall effect (OHE) arising from the Lorentz force on the conduction electrons [76], and the second term is the contribution from the anomalous Hall effect (AHE) arising due to intrinsic (Berry curvature) and extrinsic (skew-scattering and side-jump) mechanisms [77]. In magnetic conductors with a large resistivity, the AHE is dominated by the intrinsic and side-jump contributions [78, 79]. To extract the individual Hall contributions, R0R_0 is first obtained by fitting the high-field region (8–9 T) of ρxy\rho_{xy}, where the response is dominated by the linear OHE. The carrier concentration n=1/R0en = 1/R_0 e and carrier mobility μ=1/neρxx\mu= 1/ne\rho_{xx} extracted at each temperature using R0R_0 are presented in Figure 5(i). The carrier concentration is 1.46×1021 cm−31.46 \times10^{21}\ \mathrm{cm}^{-3} at 2 K, drops monotonically to 1.1×1021 cm−31.1 \times10^{21}\ \mathrm{cm}^{-3} around 50 K, and recovers to 1.6×1021 cm−31.6 \times10^{21}\ \mathrm{cm}^{-3} at 210 K, tracing a well-defined dip centered at 50 K. The carrier mobility obtained at 2 K is μ=129 cm2V−1s−1\mu= 129\ \mathrm{cm}^{2}\mathrm{V}^{-1}\mathrm{s}^{-1}. The obtained R0R_0 is then used to compute and subtract the OHE contribution R0μ0HR_0\mu_0H from the total Hall resistivity, yielding the anomalous Hall contributions ρxyAHE\rho_{xy}^{\mathrm{AHE}}. As a consistency check, we assume ρxyAHE=SHρxx2M\rho_{xy}^{\mathrm{AHE}} = S_{\mathrm{H}}\rho_{xx}^{2}M and plot ρxy(H)/μ0H\rho_{xy}(H)/\mu_0H as a function of ρxx(H)2M(H)/μ0H\rho_{xx}(H)^2M(H)/\mu_0H, where the intercept yields R0R_0 and the slope yields the AHE scaling factor SHS_{\mathrm{H}}. The AHE estimated using R0R_0 from this linear fit is in good agreement with that obtained from the high-field fitting. The first method is then applied systematically across all measured temperatures and the resulting AHE contribution as a function of temperature is shown in Figure 5(g). The field dependence of ρxyAHE\rho_{xy}^{\mathrm{AHE}} closely mirrors the magnetization for fields applied along the same direction [see Figure 4(b)]. The evolution of ρxyAHE\rho_{xy}^{\mathrm{AHE}} at 9 T as a function of temperature is shown in Figure 5(h). The ρxyAHE\rho_{xy}^{\mathrm{AHE}} is a maximum (∼0.59 μΩ cm\sim0.59\ \mu\Omega\ \mathrm{cm}) at the lowest measured temperature (2 K) and monotonically reduces with increasing temperature, becomes negative above 70 K with a minimum around 125 K, before becoming zero above 150 K (T>TNT > T_{\mathrm{N}}). The change in sign of ρxyAHE\rho_{xy}^{\mathrm{AHE}} above 50 K, and disappearance of the AHE above 150 K coincide with the unusual features observed in MR including the flattening of the MR response above 50 K, the emergence of weak antilocalization at 50 K, and the anomaly in the carrier concentration at 50 K, strongly suggesting that a common underlying mechanism governs the transport anomalies in this temperature regime.

The temperature and field dependence of ρxyAHE\rho_{xy}^{\mathrm{AHE}} observed in Cr1/4_{1/4}NbS2_2 differ in some respects from those reported for the related compound Cr1/4_{1/4}TaS2_2 [56]. While the AHE in the Ta material is also positive at low temperatures and changes sign close the ordering temperature of what may be a Cr1/3_{1/3}TaS2_2 intergrowth, the signal in the Ta compound is an order of magnitude lower in the positive sector. The reported field dependence of the AHE is also different in Cr1/4_{1/4}TaS2_2. It is unclear if the AHE and magnetization in Cr1/4_{1/4}TaS2_2 exhibit the same field dependence, as M(H)M(H) data for a field applied along the requisite direction are not shown [56].

Although the microscopic origins of the features in the MR and AHE of Cr1/4_{1/4}NbS2_2 remain an open question, several plausible mechanisms may account for the observed behaviour. One possibility is the scattering of charge carriers from domain walls of Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 intergrowths embedded in the host matrix. This could give rise to weak antilocalization effects in MR as discussed earlier [72]; scattering from such defects could also produce the unusual dip in the carrier concentration as observed in systems with defects and local breaking of time-reversal symmetry, could induce a transverse voltage [78] thereby showing a finite AHE. The AHE may also be intrinsic to the Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 phase, which is known to host a giant topological and planar Hall effect [45]. Disentangling these competing scenarios calls for further studies using local experimental probes capable of investigating the sample at microscopic level, in order to fully understand the complex interplay between magnetoresistance, Hall response, composition and morphology that governs the low-temperature transport in this system.

Summary & Conclusions

We report the growth of high-quality single crystals of Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 for the first time, a phase known since 1970, with the motivation of providing a platform for exploring altermagnetism in this material experimentally. The crystals are thoroughly characterized using Laue diffraction and single-crystal X-ray diffraction to assess their quality and establish detailed crystallographic information. EDX analysis confirms the stoichiometry of the crystals as Cr0.25NbS2\mathrm{Cr}_{0.25}\mathrm{NbS}_2. Zero-field longitudinal resistivity and heat capacity measurements unambiguously capture an antiferromagnetic transition at TN∼141T_{\mathrm{N}} \sim141 K. Magnetic measurements also reveal the presence of the unavoidable minority intergrowths of the Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 phase embedded within the majority Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 matrix. Magnetotransport measurements reveal a series of complex features in the magnetoresistance and Hall response. The magnetoresistance as a function of field exhibits a crossover from weak antilocalization at 50 K to weak localization at 130 K. The magnetoresistance at 9 T, as a function of temperature, displays intricate behavior: it decreases monotonically up to 50 K, turns negative upon further warming, and becomes positive again at higher temperatures, before eventually saturating above the Néel temperature. The transverse resistivity likewise shows non-trivial behavior. The carrier concentration extracted from the ordinary Hall component exhibits a pronounced dip near 50 K, and an anomalous Hall signal is observed at low temperatures which tends to saturate above 50 K. These coincident anomalies near 50 K point toward the occurrence of quantum diffusive transport, a phenomenon commonly observed in disordered systems; here, the underlying disorder is attributed to the minority Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_2 intergrowths embedded within the dominant Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 matrix. The successful crystal growth of the potential altermagnetic candidate Cr1/4NbS2\mathrm{Cr}_{1/4}\mathrm{NbS}_2 thus raises several questions regarding the origin of the unusual features observed in its magnetotransport response and warrants further investigation.

Acknowledgments

We acknowledge Ewan Jewkes and Patrick Ruddy for their technical support. This work was financially supported by Engineering and Physical Sciences Research Council grant EP/Z535874/1: ”Single Crystal Growth at Warwick” and UK Research and Innovation grant UKRI648: ”Advanced materials for next-generation spintronics: The deterministic control of altermagnets”.

Equipment used in this work was provided by the University of Warwick’s X-ray Diffraction and Electron Microscopy Research Technology Platforms.

References

  1. [1]L. Néel, Magnetism and local molecular field, Science 174, 985 (1971).pubmed.ncbi.nlm.nih.gov/17757022
  2. [2]L. Šmejkal, J. Sinova, and T. Jungwirth, Beyond conventional ferromagnetism and antiferromagnetism: A phase with nonrelativistic spin and crystal rotation symmetry, Phys. Rev. X 12, 031042 (2022).DOI
  3. [3]I. Mazin (The PRX Editors), Editorial: Altermagnetism—a new punch line of fundamental magnetism, Phys. Rev. X 12, 040002 (2022).DOI
  4. [4]L. Šmejkal, J. Sinova, and T. Jungwirth, Emerging research landscape of altermagnetism, Phys. Rev. X 12, 040501 (2022).arxiv.org/abs/2204.10844
  5. [5]L. Šmejkal, A. B. Hellenes, R. González-Hernández, J. Sinova, and T. Jungwirth, Giant and tunneling magnetoresistance in unconventional collinear antiferromagnets with nonrelativistic spin-momentum coupling, Phys. Rev. X 12, 011028 (2022).DOI
  6. [6]L.-D. Yuan and A. Zunger, Degeneracy removal of spin bands in collinear antiferromagnets with non-interconvertible spin-structure motif pair, Adv. Mater. 35, 2211966 (2023).DOI
  7. [7]J. Krempaský, L. Šmejkal, S. D’Souza, M. Hajlaoui, G. Springholz, K. Uhlířová, F. Alarab, P. C. Constantínou, V. Strocov, D. Usanov, W. R. Pudelko, R. A. González-Hernández, B. Hellenes, Z. Jansa, H. Reichlová, R. D. Šobáň, Z. Gonzalez Betancourt, P. Wadley, J. Sinova, D. Kriegner, J. Minár, J. H. Dil, and T. Jungwirth, Altermagnetic lifting of Kramers spin degeneracy, Nature 626, 517 (2024).DOI
  8. [8]P. A. McClarty and J. G. Rau, Landau theory of altermagnetism, Phys. Rev. Lett. 132, 176702 (2024).DOI
  9. [9]B. Brekke, P. Sukhachov, H. G. Giil, A. Brataas, and J. Linder, Minimal models and transport properties of unconventional p-wave magnets, Phys. Rev. Lett. 133, 236703 (2024).DOI
  10. [10]H. Yan, X. Zhou, P. Qin, and Z. Liu, Review on spin-split antiferromagnetic spintronics, Appl. Phys. Lett. 124, 030503 (2024).DOI
  11. [11]T. Jungwirth, J. Sinova, P. Wadley, D. Kriegner, H. Reichlova, F. Krizek, H. Ohno, and L. Smejkal, Altermagnetic spintronics, arXiv 2508.09748, 10.48550/arXiv.2508.09748 (2025), preprint, cond-mat.mtrl-sci.arxiv.org/abs/2508.09748
  12. [12]M. Hajlaoui, S. Wilfred D’Souza, L. Šmejkal, D. Kriegner, G. Krizman, T. Zakusylo, N. Olszowska, O. Caha, J. Michalička, J. Sánchez-Barriga, A. Marmodoro, K. Výborný, A. Ernst, M. Cinchetti, J. Minar, T. Jungwirth, and G. Springholz, Temperature dependence of relativistic valence band splitting induced by an altermagnetic phase transition, Adv. Mater. 36, 2314076 (2024).DOI
  13. [13]R. D. Gonzalez Betancourt, J. Zubáč, R. Gonzalez-Hernandez, K. Geishendorf, Z. Šobáň, G. Springholz, K. Olejník, L. Šmejkal, J. Sinova, T. Jungwirth, S. T. B. Goennenwein, A. Thomas, H. Reichlová, J. Železný, and D. Kriegner, Spontaneous anomalous Hall effect arising from an unconventional compensated magnetic phase in a semiconductor, Phys. Rev. Lett. 130, 036702 (2023).DOI
  14. [14]L. Han, X. Fu, R. Peng, X. Cheng, J. Dai, L. Liu, Y. Li, Y. Zhang, W. Zhu, H. Bai, Y. Zhou, S. Liang, C. Chen, Q. Wang, X. Chen, L. Yang, Y. Zhang, C. Song, J. Liu, and F. Pan, Electrical 180° switching of Néel vector in spin-splitting antiferromagnet, Sci. Adv. 10, eadn0479 (2024).DOI
  15. [15]N. Wang, J. Chen, N. Ding, H. Zhang, S. Dong, and S.-S. Wang, Magneto-optical Kerr effect and magnetoelasticity in a weakly ferromagnetic RuF₄ monolayer, Phys. Rev. B 106, 064435 (2022).DOI
  16. [16]A. Hariki, A. Dal Din, O. J. Amin, T. Yamaguchi, A. Badura, D. Kriegner, K. W. Edmonds, R. P. Campion, P. Wadley, D. Backes, L. S. I. Veiga, S. S. Dhesi, G. Springholz, L. Šmejkal, K. Výborný, T. Jungwirth, and J. Kuneš, X-ray magnetic circular dichroism in altermagnetic α-MnTe, Phys. Rev. Lett. 132, 176701 (2024).DOI
  17. [17]L. Šmejkal, A. Marmodoro, K.-H. Ahn, R. González-Hernández, I. Turek, S. Mankovsky, H. Ebert, S. W. D’Souza, O. Šipr, J. Sinova, and T. Jungwirth, Chiral magnons in altermagnetic RuO₂, Phys. Rev. Lett. 131, 256703 (2023).arxiv.org/abs/2211.13806
  18. [18]Z. Liu, M. Ozeki, S. Asai, S. Itoh, and T. Masuda, Chiral split magnon in altermagnetic MnTe, Phys. Rev. Lett. 133, 156702 (2024).DOI
  19. [19]L. Bai, W. Feng, S. Liu, L. Šmejkal, Y. Mokrousov, and Y. Yao, Altermagnetism: Exploring new frontiers in magnetism and spintronics, Adv. Funct. Mater. 34, 2409327 (2024).
  20. [20]X. Chen, Y. Liu, P. Liu, et al., Unconventional magnons in collinear magnets dictated by spin space groups, Nature 640, 349 (2025).DOI
  21. [21]R. Bhattarai, P. Minch, and T. D. Rhone, High-throughput screening of altermagnetic materials, Phys. Rev. Mater. 9, 064403 (2025).DOI
  22. [22]Y. Guo, H. Liu, O. Janson, I. C. Fulga, J. van den Brink, and J. I. Facio, Spin-split collinear antiferromagnets: A large-scale ab-initio study, Materials Today Physics 32, 100991 (2023).
  23. [23]Z.-F. Gao, S. Q. B, B. Zeng, Y. Liu, J.-R. Wen, H. Sun, P.-J. Guo, and Z.-Y. Lu, Al-accelerated discovery of altermagnetic materials, Nat. Sci. Rev. 12, nwaf066 (2025).DOI
  24. [24]C. Song, H. Bai, Z. Zhou, L. Han, H. Reichlova, J. H. Dil, J. Liu, X. Chen, and F. Pan, Altermagnets as a new class of functional materials, Nature Reviews Materials 10, 473 (2025).DOI
  25. [25]C.-C. Wei, E. Lawrence, A. Tran, and H. Ji, Crystal chemistry and design principles of altermagnets, ACS Organic & Inorganic Au 4, 604 (2024).DOI
  26. [26]Y. Guo, J. Zhang, Z. Zhu, Y.-y. Jiang, L. Jiang, C. Wu, J. Dong, X. Xu, W. He, B. He, Z. Huang, L. Du, G. Zhang, K. Wu, X. Han, D.-f. Shao, G. Yu, and H. Wu, Direct and inverse spin splitting effects in altermagnetic RuO₂, Adv. Sci. 11, 2400967 (2024).DOI
  27. [27]K. D. Belashchenko, Giant strain-induced spin splitting effect in MnTe, a g-wave altermagnetic semiconductor, Phys. Rev. Lett. 134, 086701 (2025).DOI
  28. [28]G. Yang, Z. Li, S. Yang, J. Li, H. Zheng, W. Zhu, Z. Pan, Y. Xu, S. Cao, W. Zhao, A. Jana, J. Zhang, M. Ye, Y. Song, L.-H. Hu, L. Yang, J. Fujii, I. Vobornik, M. Shi, H. Yuan, Y. Zhang, Y. Xu, and Y. Liu, Three-dimensional mapping of the altermagnetic spin splitting in CrSb, Nat. Commun. 16, 1442 (2025).DOI
  29. [29]S. Lovesey, Altermagnetism and chiral order in a collinear antiferromagnet (MnF₂), Sci. Rep. 16, 14058 (2026).DOI
  30. [30]A. Badura, W. Campos, V. Bharadwaj, et al., Observation of the anomalous nernst effect in altermagnetic candidate Mn₅Si₃, Nat. Commun. 16, 7111 (2025).
  31. [31]T. Saunderson, J. Annett, and S. Lounis, Oxygen-driven altermagnetic symmetry inducing d-wave superconductivity in the cuprates and nickelates, arXiv 2509.06814, 10.48550/arXiv.2509.06814 (2025), preprint, cond-mat.supr-con.arxiv.org/abs/2509.06814
  32. [32]X. Zhou, W. Feng, R.-W. Zhang, L. Šmejkal, J. Sinova, Y. Mokrousov, and Y. Yao, Crystal thermal transport in altermagnetic RuO₂, Phys. Rev. Lett. 132, 056701 (2024).DOI
  33. [33]T. Berlijn, P. C. Snijders, O. Delaire, H.-D. Zhou, T. A. Maier, H.-B. Cao, S.-X. Chi, M. Matsuda, Y. Wang, M. R. Koehler, P. R. C. Kent, and H. H. Weitering, Itinerant antiferromagnetism in RuO₂, Phys. Rev. Lett. 118, 077201 (2017).
  34. [34]Z. H. Zhu, J. Strempfer, R. R. Rao, C. A. Occhialini, J. Pelliciari, Y. Choi, T. Kawaguchi, H. You, J. F. Mitchell, Y. Shao-Horn, and R. Comin, Anomalous antiferromagnetism in metallic RuO₂ determined by resonant x-ray scattering, Phys. Rev. Lett. 122, 017202 (2019).
  35. [35]P. Keßler, L. Garcia-Gassull, A. Suter, T. Prokscha, Z. Salman, D. Khalyavin, P. Manuel, F. Orlandi, I. I. Mazin, R. Valentí, and S. Moser, Absence of magnetic order in RuO₂: Insights from μSR spectroscopy and neutron diffraction, npj Spintronics 2, 50 (2024).
  36. [36]T. Osumi, S. Souma, T. Aoyama, K. Yamauchi, A. Honma, K. Nakayama, T. Takahashi, K. Ohgushi, and T. Sato, Observation of a giant band splitting in altermagnetic MnTe, Phys. Rev. B 109, 115102 (2024).DOI
  37. [37]S. Reimers, L. Odenbreit, L. Šmejkal, V. N. Strocoв, P. Constantinou, A. B. Hellenes, R. Jaeschke Ubiergo, W. H. Campos, V. K. Bharadwaj, A. Chakraborty, T. Denneulin, W. Shi, R. E. Dunin-Borkowski, S. Das, M. Kläui, J. Sinova, and M. Jourdan, Direct observation of altermagnetic band splitting in CrSb thin films, Nat. Commun. 15, 2116 (2024).
  38. [38]N. Spaldin, S. W. Cheong, and S. Griffin, Why are there so few non-altermagnetic antiferromagnets?, arXiv:2602.17181 (2026).arxiv.org/abs/2602.17181
  39. [39]R. B. Regmi, H. Bhandari, B. Thapa, Y. Hao, N. Sharma, J. McKenzie, X. Chen, A. Nayak, M. El Gaz-zah, B. G. Márkus, L. Forró, X. Liu, H. Cao, J. F. Mitchell, I. I. Mazin, and N. J. Ghimire, Altermagnetism in the layered intercalated transition metal dichalcogenide CoNb₄Se₈, Nat. Commun. 16, 4399 (2025).DOI
  40. [40]B. Van Laar, H. Rietveld, and D. Jido, Magnetic and crystallographic structures of MexNbS₂ and MexTaS₂, J. Solid State Chem. 3, 154 (1971).DOI
  41. [41]E. A. Marseglia, Transition metal dichalcogenides and their intercalates, Int. Rev. Phys. Chem. 3, 177 (1983).
  42. [42]Agilent Technologies UK, CrysAlisPRO Software (Yarnton, England, 2014).
  43. [43]O. V. Dolomanov, L. J. Bourhis, R. J. Gildea, J. A. K. Howard, and H. Puschmann, OLEX2: a complete structure solution, refinement and analysis program, J. Appl. Cryst. 42, 339 (2009).DOI
  44. [44]A. E. Hall, J. C. Loudon, P. A. Midgley, A. C. Twitchett-Harrison, S. J. R. Holt, D. A. Mayoh, J. P. Tidey, Y. Han, M. R. Lees, and G. Balakrishnan, Comparative study of the structural and magnetic properties of Mn₁/₃NbS₂ and Cr₁/₃NbS₂, Phys. Rev. Mater. 6, 024407 (2022).DOI
  45. [45]D. A. Mayoh, J. Bouaziz, A. E. Hall, J. B. Staunton, M. R. Lees, and G. Balakrishnan, Giant topological and planar Hall effect in Cr₁/₃NbS₂, Phys. Rev. Res. 4, 013134 (2022).DOI
  46. [46]See Supplemental Material at [URL will be inserted by publisher] for more details of the SEM - EDX analysis, anisotropic displacement parameters, magnetic susceptibility of CrₓNbS₂ (x = 1/4 and 1/3), and magnetotransport measurements.
  47. [47]K. Momma and F. Izumi, VESTA 3 for three-dimensional visualization of crystal, volumetric and morphology data, J. Appl. Crystallogr. 44, 1272 (2011).DOI
  48. [48]F. A. Lévy, Intercalated Layered Materials, Physics and Chemistry of Materials with Layered Structures, Vol. 6 (D. Reidel Publishing Company, Dordrecht, Holland, 1979).DOI
  49. [49]S. S. P. Parkin and R. H. Friend, 3d transition-metal intercalates of the niobium and tantalum dichalcogenides. I. Magnetic properties, Philos. Mag. B 41, 65 (1980).DOI
  50. [50]S. S. P. Parkin and R. H. Friend, 3d transition-metal intercalates of the niobium and tantalum dichalcogenides. II. Transport properties, Philos. Mag. B 41, 95 (1980).DOI
  51. [51]Y. Togawa, T. Koyama, K. Takayanagi, S. Mori, Y. Kousaka, J. Akimitsu, S. Nishihara, K. Inoue, A. S. Ovchinnikov, and J. Kishine, Chiral magnetic soliton lattice on a chiral helimagnet, Phys. Rev. Lett. 108, 107202 (2012).pubmed.ncbi.nlm.nih.gov/22463448
  52. [52]Y. Togawa, T. Koyama, Y. Nishimori, Y. Matsumoto, S. McVitie, D. McGrouther, R. L. Stamps, Y. Kousaka, J. Akimitsu, S. Nishihara, K. Inoue, I. G. Bostrem, V. E. Sinitsyn, A. S. Ovchinnikov, and J. Kishine, Magnetic soliton confinement and discretization effects arising from macroscopic coherence in a chiral spin soliton lattice, Phys. Rev. B 92, 220412(R) (2015).DOI
  53. [53]J.-i. Yonemura, Y. Shimamoto, T. Kida, D. Yoshizawa, Y. Kousaka, S. Nishihara, F. J. T. Goncalves, J. Akimitsu, K. Inoue, M. Hagiwara, and Y. Togawa, Magnetic solitons and magnetic phase diagram of the hexagonal chiral crystal CrNb₃S₆ in oblique magnetic fields, Phys. Rev. B 96, 184423 (2017).DOI
  54. [54]Y. Cao, Z. Huang, Y. Yin, H. Xie, B. Liu, W. Wang, C. Zhu, D. Mandrus, L. Wang, and W. Huang, Overview and advances in a layered chiral helimagnet Cr₁/₃NbS₂, Mater. Today Adv. 7, 100080 (2020).DOI
  55. [55]Y. An, P. Park, C. Kim, K. Zhang, H. Kim, M. Avdeev, J. Kim, M.-J. Han, H.-J. Noh, S. Seong, J.-S. Kang, H.-D. Kim, and J.-G. Park, Bulk properties of the chiral metallic triangular antiferromagnets Ni₁/₃NbS₂ and Ni₁/₃TaS₂, Phys. Rev. B 108, 054418 (2023).DOI
  56. [56]L. S. Xie, S. S. Fender, C. Mollazadeh, W. Fang, M. D. Frontzek, S. Husremović, K. Li, I. M. Craig, B. H. Goodge, M. P. Erodici, O. Gonzalez, J. D. Denlinger, Y. Ping, and D. K. Bediako, Anomalous Hall effect from inter-superlattice scattering in a noncollinear antiferromagnet, Nat. Commun. 16, 5711 (2025).DOI
  57. [57]V. Dyadkin, F. Mushenok, A. Bosak, D. Menzel, S. Grigoriev, P. Pattison, and D. Chernyshov, Structural disorder versus chiral magnetism in Cr₁/₃NbS₂, Phys. Rev. B 91, 184205 (2015).DOI
  58. [58]Y. Kousaka, T. Ogura, J. Jiang, K. Mizutani, S. Iwasaki, J. Akimitsu, and Y. Togawa, An emergence of chiral helimagnetism or ferromagnetism governed by Cr intercalation in a dichalcogenide CrNb₃S₆, APL Materials 10, 090704 (2022).DOI
  59. [59]J.-S. Zhou and J. B. Goodenough, Paramagnetic phase in single-crystal LaMnO₃, Phys. Rev. B 60, R15002(R) (1999).DOI
  60. [60]E. O. Wollan and W. C. Koehler, Neutron diffraction study of the magnetic properties of the series of perovskite-type compounds [(1 − x)La, xCa]MnO₃, Phys. Rev. 100, 545 (1955).
  61. [61]M. A. McGuire, G. Clark, S. KC, W. M. Chance, G. E. Jellison, V. R. Cooper, X. Xu, and B. C. Sales, Magnetic behavior and spin-lattice coupling in cleavable van der Waals layered CrCl₃ crystals, Phys. Rev. Mater. 1, 014001 (2017).arxiv.org/abs/1706.01796
  62. [62]Y. Liu and C. Petrovic, Anisotropic magnetocaloric effect and critical behavior in CrCl₃, Phys. Rev. B 102, 014424 (2020).DOI
  63. [63]K. Han, X.-P. Ma, H. Wang, J.-F. Lin, Y.-T. Wang, X. Dong, Y. Zhang, H.-X. Yang, and T.-L. Xia, Anomalous Hall effect and topological Hall effect in the centrosymmetric antiferromagnet V₁/₄NbSe₂, Phys. Rev. B 113, 094455 (2026).
  64. [64]Y. Liu, Z. Hu, X. Tong, E. D. Bauer, and C. Petrovic, Electrical and thermal transport in van der Waals magnets 2H−MₓTaS₂ (M = Mn, Co), Phys. Rev. Res. 4, 013048 (2022).DOI
  65. [65]S. Wu, Y. Huang, H. Song, and B. Wang, Bulk single crystal growth and magneto-transport properties of α-MnTe, J. Magn. Magn. Mater. 627, 173106 (2025).DOI
  66. [66]V. U. S. Rao and W. E. Wallace, Calculation of the influence of the crystalline electric field on the spin-disorder resistivity of rare-earth alloys and comparison with results on CeAl₂, Phys. Rev. B 2, 4613 (1970).DOI
  67. [67]X. Xu, B. Jiang, R. Wang, Z. Qiu, S. Guo, B. Lv, and R. Zhong, Stoichiometry-controlled structural order and tunable antiferromagnetism in FeₓNbSe₂ (0.05 ≤ x ≤ 0.38), Phys. Rev. B 113, 134420 (2026).DOI
  68. [68]H. Liao, W. Li, Z. Zhou, Q. Jiang, H. Cheng, T. Zuo, H. Cheng, X. Liu, and Y. Zheng, Observation of fluctuation driven topological Hall effect in the chiral magnet Mn₁/₃NbS₂ with weak Dzyaloshinskii–Moriya interactions, Phys. Rev. B 113, 214409 (2026).DOI
  69. [69]M. K. Ray, M. Fu, Y. Chen, T. Chen, T. Nomoto, S. Sakai, M. Kitanani, M. Hirayama, S. Imajo, T. Tomita, A. Sakai, D. Nishio-Hamane, G. T. McCandless, M.-T. Suzuki, Z. Xu, Y. Zhao, T. Fennell, Y. Kohama, J. Y. Chan, R. Arita, C. Broholm, and S. Nakatsuji, Zero-field Hall effect emerging from a non-Fermi liquid in a collinear antiferromagnet V₁/₃NbS₂, Nature Commun. 16, 3532 (2025).DOI
  70. [70]N. Barišić, I. Smiljanić, P. Popčević, A. Bilušić, E. Tutiš, A. Smontara, H. Berger, J. Jaćimović, O. Yuli, and L. Forró, High-pressure study of transport properties in Co₀.₃₃NbS₂, Phys. Rev. B 84, 075157 (2011).
  71. [71]A. B. Pippard, Magnetoresistance in Metals (Cambridge University Press, 1989).
  72. [72]S. Mitra, J. G. S. Kang, J. Shin, J. Q. Ng, S. S. Sunku, T. Kong, P. C. Canfield, B. S. Shastry, P. Sengupta, and C. Panagopoulos, Quadratic to linear magnetoresistance tuning in TmB₄, Phys. Rev. B 99, 045119 (2019).DOI
  73. [73]D. Neumaier, K. Wagner, S. Geißler, U. Wurstbauer, J. Sadowski, W. Wegscheider, and D. Weiss, Weak localization in ferromagnetic (Ga,Mn)As nanostructures, Phys. Rev. Lett. 99, 116803 (2007).
  74. [74]M. Liu, J. Zhang, C.-Z. Chang, Z. Zhang, X. Feng, K. Li, K. He, L.-I. Wang, X. Chen, X. Dai, Z. Fang, Q.-K. Xue, X. Ma, and Y. Wang, Crossover between weak antilocalization and weak localization in a magnetically doped topological insulator, Phys. Rev. Lett. 108, 036805 (2012).pubmed.ncbi.nlm.nih.gov/22400773
  75. [75]B. L. Altshuler, Electron-electron interactions in disordered conductors, in Electron-Electron Interactions in Disordered Systems (Elsevier, New York, 1985) 1st ed., pp. 1–159.DOI
  76. [76]E. H. Hall, On a new action of the magnet on electric currents, American Journal of Mathematics 2, 287 (1879).
  77. [77]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Anomalous hall effect, Rev. Mod. Phys. 82, 1539 (2010).DOI
  78. [78]S. Nakatsuji, N. Kiyohara, and T. Higo, Large anomalous Hall effect in a non-collinear antiferromagnet at room temperature, Nature 527, 212 (2015).
  79. [79]R. Karplus and J. M. Luttinger, Hall effect in ferromagnetics, Phys. Rev. 95, 1154 (1954).DOI

Paper details

vlnc:W_3qbk36n2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents