betaFeedback

WorksPhysics and Astronomy

Broadband photoresponse enhancement by band engineering in Sb-doped MnBi2Te4

Abstract

Topological materials have attracted considerable attention for their potential in broadband and fast photoresponse, particularly in the infrared regime. However, the high carrier concentration in these systems often leads to rapid recombination of photogenerated carriers, limiting the photoresponsivity. Here, we demonstrate that Sb doping in MnBi2Te4 effectively reduces carrier concentration and suppresses electron-hole recombination, thereby significantly improving the optoelectronic performance across the visible to mid-infrared spectra. The optimally doped Mn(Bi0.82Sb0.18)2Te4 photodetector achieves a responsivity of 3.02 mA W-1 with a response time of 18.5 μs at 1550 nm, and 0.795 mA W-1 with a response time of 9.0 μs at 4 μm. These values represent nearly two orders of magnitude improvement compared to undoped MnBi2Te4. Our results highlight band engineering as an effective strategy to enhance the infrared performance of topological material-based photodetectors, opening new avenues for high-sensitivity infrared detection.

Introduction

Infrared photodetectors have attracted great research interest due to their wide-ranging applications in video imaging, medical diagnostics, environmental monitoring, and optical communications.[1, 2, 3, 4, 5] These device applications require an efficient conversion of low-energy infrared photons into electrical signals, which is particularly challenging in the mid- and far-infrared regions. Narrow-bandgap semiconductors, such as HgCdTe\mathrm{HgCdTe},[6, 7, 8] have been successfully utilized in infrared detection owing to their exceptionally high responsivity. However, the practical application of these traditional infrared detectors is often hampered by challenges such as high growth costs, cryogenic cooling requirements, and the presence of environmentally toxic materials.[9] While microbolometers offer room-temperature operation, their slow response limits their use in high-speed applications.[10, 11, 12] Thus, there is a growing demand for fast, highly sensitive infrared photodetectors that operate at room temperature without significant trade-offs in performance.

Recently, considerable progress has been made in the development of photodetectors based on semimetallic topological materials, such as Cd3As2\mathrm{Cd}_{3}\mathrm{As}_{2}, TaIrTe4\mathrm{TaIrTe}_{4}, SnSb2Te4\mathrm{SnSb}_{2}\mathrm{Te}_{4}, among others.[13, 14, 15, 16, 17, 18, 19, 20, 21] These materials exhibit unique electronic properties derived from their nontrivial topological band structures and possess high carrier mobility, enabling efficient and ultrafast photoresponse across a broad spectral range, including the infrared region. Unlike semiconductors, which rely on band gaps to generate photo-excited carriers, topological materials exhibit gapless or nearly gapless states, facilitating broadband absorption and rapid carrier dynamics.[22, 23, 24] This makes them ideal for high-speed photodetection without the need for cryogenic cooling. However, the excessively high carrier concentration inherent in semimetal systems can lead to increased recombination of photoexcited carriers, thereby limiting photocurrent response and sensitivity. The intrinsic band structure of semimetals also poses challenges for improving photoresponse through conventional techniques like gate tuning.[25, 26] While innovative approaches such as semimetal-semiconductor heterojunctions and artificial metasurfaces have been proposed to enhance photoresponse, these designs significantly increase fabrication complexity.[27, 28, 29, 30] Therefore, before implementing these more complex device configurations, it is essential to optimize the semimetal materials themselves to improve optoelectronic properties. Atomic doping engineering has been demonstrated as an effective strategy to enhance optoelectronic performance in various devices, including traditional semiconductors, 2D semiconductors, and topological insulators.[31, 32, 33] These improvements are primarily attributed to the suppression of carrier recombination, the modulation of energy bands, or the increase of absorption coefficients, etc.

In this work, we investigate the optoelectronic performance of devices based on the Sb-doped MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4} family, focusing on their potential for infrared photodetection. While MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4} is well-known for its quantum anomalous Hall and axion insulator states,[34, 35, 36] its paramagnetic phase above the Néel temperature (∼\sim25 K) remains underexplored. Room-temperature angle-resolved photoemission spectroscopy has revealed a bulk band gap of approximately 150 meV with a gapless surface state,[37] highlighting its suitability for infrared detection. By introducing Sb doping, Sb-induced electron acceptors progressively replaced Bi-induced electron donors,[38] allowing for successful tuning of the Fermi level within the bulk band gap and effective reduction of carrier concentration with an optimal doping ratio of x=0.18x = 0.18. We demonstrate that the Mn(Bi0.82Sb0.18)2Te4\mathrm{Mn(Bi}_{0.82}\mathrm{Sb}_{0.18}\mathrm{)}_{2}\mathrm{Te}_{4} device achieve a zero-bias photoresponsivity of 3.08 mA W−1^{-1} at 633 nm and 0.795 mA W−1^{-1} at 4 μ\mum, representing nearly two orders of magnitude improvement compared to undoped ones. Furthermore, the detector demonstrated a rapid response time ranging from 9 to 19 μ\mus in the infrared range. These results highlight the promise of band engineering in topological materials for optimizing the photoresponse of infrared photodetectors based on topological materials.

Results and Discussion

MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4} crystallizes in the rhombohedral space group Rˉ3m\bar{R}3m,[39] featuring a layered structure of Te-Bi-Te-Mn-Te-Bi-Te sequences stacking along the cc axis (Figure 1a). These layers are held together by van der Waals interaction along the stacking direction. When doped with Sb, part of Bi atoms are replaced by Sb atoms, forming Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4, which retains the same crystal structure as MnBi2_2Te4_4.[40] This doping approach provides a promising avenue for band engineering to optimize the material's physical properties. In this work, a series of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 single crystals were synthesized by chemical vapor transport (Methods), and the Sb doping levels were determined by the energy-dispersive X-ray spectra (EDS) measurement (Figure S1). X-ray diffraction (XRD) patterns for Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 crystals with the substituting ratio xx from 0 to 0.22 are displayed in Figure 1b, where the diffraction peak positions remain consistent with those of the undoped crystal, confirming structural consistency.

Structural and transport characterization of Mn(Bi1-xSbx)2Te4 samples

Figure 1. Structural and transport characterization of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 samples. (a) Crystal structure of MnBi2_2Te4_4. (b) XRD patterns for Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 crystals with different Sb substituting ratios. The inset shows a Mn(Bi0.78_{0.78}Sb0.22_{0.22})2_2Te4_4 single crystal. Scale bar: 1 mm. (c-d) Measurements of Hall resistivity ρyx\rho_{yx} as a function of magnetic field BB in nanodevices with different Sb substitution ratios at 295K and 30K, respectively. The inset in (c) shows a typical Hall bar device (channel length: 22.2μ\mum, channel width: 11.1μ\mum). Scale bar: 20 μ\mum. (e) Absolute values of calculated carrier density with different Sb substituting ratios at 30 K. The inset illustrates the evolution of Fermi levels with respect to energy bands. (f) Temperature dependence of the Hall coefficient and carrier concentration for Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4.

The carrier density of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 was investigated by measuring the Hall resistivity ρyx\rho_{yx} as a function of magnetic field BB at different temperatures on nanoflakes exfoliated from bulk crystals. Devices were fabricated using standard electron beam lithography techniques (Methods), and a typical Hall device configuration is shown in the inset of Figure 1c. Figure 1c and Figure 1d compare ρyx\rho_{yx} at 295 K and 30 K for different doping levels. As the Sb content increases, the slope of ρyx\rho_{yx} switches from negative to positive, corresponding to the transition from electron to hole carriers. Figure 1e shows the calculated carrier density at 30 K, with the x=0.18x=0.18 samples exhibiting the lowest carrier concentration, suggesting that the Fermi level is closest to the charge neutral point (CNP) within the bulk band gap. The distinct thermal activation behavior of carrier density from 30 K to 295 K (Figure S2) further corroborates that this doping level optimally positions the Fermi level near the CNP. In contrast, Hall resistivity of other samples shows a weak temperature dependence due to the intrinsic high carrier density. Figure 1f presents the temperature-dependent Hall coefficient and carrier density for one of the x=0.18x=0.18 samples. These results confirm that Sb doping effectively reduces carrier concentration, particularly when the Fermi level lies within the band gap.

Next, we investigate the performance of photodetector devices based on the Sb-doped MnBi2Te4\mathrm{MnBi_{2}Te_{4}} family. A representative device with two metal electrodes is shown in the optical image in Figure 2a. The flake thickness is about 55 nm (Figure 2b) as determined by atomic force microscopy (AFM). Figure 2c illustrates the schematic of photocurrent measurement setup, where a laser was focused on the sample through an objective lens, and the photocurrent was measured by a lock-in amplifier under zero bias conditions (Methods). A scanning galvanometer was used to direct a light spot to different locations on the device. The scanning photocurrent microscopy images at wavelengths of 633 nm (1.96 eV), 1550 nm (0.8 eV) and 4 μ\mum (0.31 eV) (Figure 2d-Figure 2f) show consistent spatial photocurrent distribution at both the MnBi2Te4\mathrm{MnBi_{2}Te_{4}}-metal junctions and regions relatively away from the electrodes. While the mid-infrared results are affected by the laser spot size, similar trends are observed, suggesting that the photocurrent generation mechanisms are wavelength-independent.

Figure 2. Spatially resolved and power-dependent photocurrent measurements of the MnBi2Te4\mathrm{MnBi_{2}Te_{4}} device. (a) Optical image of a MnBi2Te4\mathrm{MnBi_{2}Te_{4}} device (channel length: 16.1 μ\mum, channel width: 10.3 μ\mum). Scale bar: 5 μ\mum. (b) AFM image of the MnBi2Te4\mathrm{MnBi_{2}Te_{4}} device. The inset shows the height profile along the red dashed line in (b). Scale bar: 2 μ\mum. (c) Schematic of scanning photocurrent measurement setup. (d-f) Scanning photocurrent microscopy images of the MnBi2Te4\mathrm{MnBi_{2}Te_{4}} device under 633 nm (169 μ\muW), 1550 nm (295 μ\muW), and 4 μ\mum (1395 μ\muW) excitation,

respectively. Scale bar: 5 μm\mu\mathrm{m}. (g) Photocurrent response of the MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4} device along the line cut marked by the red dashed line in (a), under 633 nm laser powers ranging from 8 μW\mu\mathrm{W} to 585 μW\mu\mathrm{W}. The black dashed lines indicate the contact edges. The inset shows the linear photocurrent response as a function of laser power. (h) Photocurrent responsivity of the MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4} device under different excitation wavelengths.

To elucidate the photocurrent generation mechanism, we performed power-dependent photocurrent measurements by scanning a line cut across the electrode-flake-electrode region (Figure 2a, red dashed line). The shape of the photocurrent response remains consistent at different excitation powers with its magnitude increasing linearly (Figure 2g). The peak near the electrode results from a dominant photovoltaic effect, wherein photoexcited electron-hole pairs are separated by the built-in electric field at the MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4}-metal interface. Simultaneously, the negative photocurrent response away from the electrodes indicates a contribution from the photothermoelectric effect, driven by a temperature gradient rather than a contact potential. Compared to the photovoltaic effect closely restricted to contact regions, the photo-thermoelectric effect manifests as dispersive patterns in the photocurrent mapping with a sign reversal in the middle of two electrodes. These dual photogeneration mechanisms, common in topological semimetal-based zero-bias photodetectors, have been discussed extensively in previous studies.[15, 41] Figure 2h shows the zero-bias photoresponse at the maximum photocurrent position for three wavelengths. The responsivity values for 633 nm, 1550 nm and 4 μm\mu\mathrm{m} are 1.18×10−11.18 \times10^{-1} mA W−1^{-1}, 4.31×10−24.31 \times10^{-2} mA W−1^{-1} and 9.12×10−39.12 \times10^{-3} mA W−1^{-1}, respectively.

Having established the photocurrent generation mechanism, we now turn to improve the photoresponse through Sb doping in MnBi2Te4\mathrm{MnBi}_{2}\mathrm{Te}_{4}. Figure 3a compares the device performance based on Mn(Bi1−xSbx)2Te4\mathrm{Mn}(\mathrm{Bi}_{1-x}\mathrm{Sb}_{x})_{2}\mathrm{Te}_{4} with four doping levels (x=0x=0, 0.14, 0.18 and 0.22). Results for each doping level are confirmed by three devices to minimize sample variation. A peak responsivity is achieved at x=0.18x=0.18, exhibiting an improvement of nearly two orders of magnitude, particularly in the long-wavelength region. The non-monotonic relationship between responsivity and doping levels suggests that the enhanced photoresponse is not primarily driven by changes in the contact barrier due to Fermi level shifts. Instead, as collaborated by the Hall effect measurements in Figure 1e, the improvement is closely tied to the reduction in carrier concentration. This can be explained by the increased electron-hole recombination when the Fermi level is positioned outside the band gap, as the recombination rate is directly proportional to the majority carrier concentration (Figure 3b, top panel). Conversely, when the Fermi level lies within the bulk band gap, the reduced carrier concentration effectively suppresses recombination, leading to enhanced photoresponse (Figure 3b, bottom panel).

Comparison of the photoresponse and power-dependent photocurrent measurements

Figure 3. Comparison of the photoresponse of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 devices and power-dependent photocurrent measurements of the Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 device. (a) Comparison of the photoresponse of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 devices with varying Sb substituting ratios under different excitation wavelengths. Data from three devices is shown for each doping ratio. (b) Schematic plot of the generation and recombination of photoexcited electron-hole pairs. Red arrows, yellow arrows, solid circles and hollow circles refer to generation process, recombination process, electrons and holes, respectively. The top panel shows high recombination probability when the Fermi level is above the conduction band, while the bottom panel shows reduced recombination probability when the Fermi level is within the band gap. (c-e) Photocurrent response of Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 device as a function of excitation power at the wavelengths of 633 nm, 1550 nm and 4 μm, respectively. The solid lines represent power law fits.

The responsivity of the best-performing Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 devices (Figure S3) was determined as 3.08 mA W−1^{-1}, 3.02 mA W−1^{-1} and 0.795 mA W−1^{-1} for 633 nm, 1550 nm and 4 μm, respectively. The corresponding specific detectivity was calculated to be 1.23 × 105^{5} jones, 2.12 × 105^{5} jones and 9.59 × 104^{4} jones. Compared to some previous reports,[14, 42] the specific detectivity here was extracted based on experimental noise measurements rather than calculated values (Part IV of Supporting Information). The latter may significantly underestimate the noise level by overlooking essential components, potentially leading to over-optimistic detectivity estimates.[43, 44] Currently, the specific detectivity is limited by the dependence of the photoelectric response on the interface barrier near the electrode, which plays a key role in the separation of photogenerated carriers. Improving the detectivity could be achieved by utilizing a metal with a greater work function difference from Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 as an electrode, or by integrating the material with an n-type two-dimensional semiconductor to create a vertical heterojunction.[29, 45] This improvement facilitates the separation of photogenerated electron-hole pairs, thereby increasing both responsivity and specific detectivity. It is also important to note that the response wavelength range is limited by the light sources available in the laboratory. The Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 devices, in principle, can be used to detect photons with lower energy down to terahertz range,[46, 47] due to the small band gap that can be further tuned by doping.

Figure 3c-e illustrates the power dependence of the photocurrent at these three wavelengths, showing a monotonic increase in current with increasing power. The photocurrent follows a power law relationship, Iph∝PβI_{\mathrm{ph}} \propto P^{\beta}, where IphI_{\mathrm{ph}} is the photocurrent, PP is the laser power and β\beta is an index that reflects the photodetector sensitivity. The fitting β\beta values are all slightly less than 1, suggesting minimal impact from defects or trap states on the recombination probability of photoexcited carriers.[48, 49] Figure 4a-b presents the chopping frequency-dependent photocurrent measurement at infrared wavelengths (Methods). The fitting response times are 18.5 μs and 9.0 μs for 1550 nm and 4 μm, respectively. It highlights a markedly higher response speed compared to conventional two-dimensional semiconductor detectors, which typically exhibit millisecond response times in the infrared region. Given the high infrared responsivity and rapid response speed of the Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 devices, as well as their two-dimensional van der Waals characteristic and room-temperature self-powered operation, their potential applications in wearable and portable infrared detection appear highly attractive.

Figure 4c provides a comparison of the responsivity among different topological materials and graphene functioning as self-powered photodetectors in the visible-to-mid-infrared range (633 nm to 4 μm) at room temperature.[13, 14, 15, 16, 41, 42, 50, 51] [52] The Sb-doped MnBi2_2Te4_4 photodetectors demonstrated in this work generally exhibit superior responsivity compared to other topological-material-based photodetectors, particularly in the infrared region. Furthermore, the photocurrent response time of the device based on Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 is notably fast compared to other similar topological materials except Dirac semimetal Cd3_3As2_2 (Table 1). However, it is important to acknowledge that their responsivity remains lower than that of state-of-the-art narrow-bandgap semiconductor detectors, such as bb-AsP.[32] Despite this limitation, Sb-doped MnBi2_2Te4_4 photodetectors offer a significant advantage in terms of broader wavelength response, thanks to their narrower bulk bandgap and gapless surface states.[37] Previous studies have demonstrated the terahertz photocurrent response of MnBi2_2Te4_4,[46, 47] indicating potential for further exploration. Thus, while there is room for improvement in responsivity, particularly compared to narrow-bandgap semiconductors, the broader spectral response of Sb-doped MnBi2_2Te4_4 makes it a promising candidate for wide-spectrum detection applications. Given the good infrared photocurrent response of Sb-doped MnBi2_2Te4_4 and its ability to exhibit antiferromagnetic states at low temperatures and tunable ferromagnetic states under external magnetic fields,[53] it presents an ideal platform for investigating the magnetic photogalvanic effect.[54, 55] This capability holds promise for utilizing magnetic fields to modulate the light-matter interaction, facilitating the development of switchable devices that integrate magnetic, electronic, and optical functionalities in the future.

Response time of Mn(Bi₀.₈₂Sb₀.₁₈)₂Te₄ photodetector and comparison of broadband zero-bias photodetectors

Figure 4. Response time of Mn(Bi₀.₈₂Sb₀.₁₈)₂Te₄ photodetector and comparison of broadband zero-bias photodetectors. (a-b) Photocurrent of the Mn(Bi₀.₈₂Sb₀.₁₈)₂Te₄ device as a function of chopping frequency under 1550 nm and 4 μm excitation. Solid lines represent the fits to the data. (c) Photocurrent responsivity across the visible to mid-infrared range (633 nm to 4 μm) for various self-powered photodetectors based on topological materials and graphene at room temperature.[13, 14, 15, 16, 41, 42, 50, 51] [52]

MaterialResponse timeRef
Mn(Bi₀.₈₂Sb₀.₁₈)₂Te₄9.0 μsOur work
Cd₃As₂6.9 psWang et al.[13]
TaAs200 msChi et al.[14]

Table 4.

Td_{\mathrm{d}}-MoTe2_231.7 μ\musLai et al.[15]
TaIrTe4_425.7 μ\musLai et al.[16]
PtTe2_233.7 μ\musLai et al.[41]
Bi2_2SeTe2_240 msSahu et al.[51]

caption: Table 1 | Photoresponse time for various self-powered photodetectors based on topological materials at room temperature.

Conclusion

In summary, we demonstrate a significant enhancement in the broadband photoresponse of Sb-doped MnBi2_2Te4_4 compared to intrinsic MnBi2_2Te4_4. The optimally doped device exhibits a room-temperature self-powered responsivity of 3.08 mA W−1^{-1} with a detectivity of 1.23 ×\times 105^{5} jones at 633 nm, and 0.795 mA W−1^{-1} with a detectivity of 9.59 ×\times 104^{4} jones at 4 μ\mum. These results highlight the superior responsivity of Sb-doped MnBi2_2Te4_4 across the visible to mid-infrared spectra, outperforming other topological materials in similar regimes. This work demonstrates that band engineering is an effective approach to enhance the infrared performance of topological material-based photodetectors, paving the way for high-sensitivity infrared detection.

Methods

Material growth

High-quality single crystals were synthesized using the chemical vapor transport (CVT) method. Mn pieces (99.98%), Bi granules (99.999%), Sb granules (99.99%) and Te ingots (99.99%) were mixed in the molar ratio of Mn:(Bi+Sb):Te=3:2:6 and heated at 630 °C for 3 days to obtain the precursors. For Sb-doped samples, Sb was added at a ratio of (xx+0.04) to achieve the desired substitution level. The precursors were then recrystallized using the CVT method with I2_2 as the transporting agent (Figure S4). A temperature gradient of approximately 20 °C between the source and low-temperature zones was maintained for 14 days, followed by natural cooling to room temperature to yield the target crystals. The reaction temperature for different doping levels were slightly adjusted (Table S1), with specific details available in the referenced literature.[56] All reactions were conducted in high-vacuum quartz tubes.

Structural and Spectrum Characterization

The elemental composition of the single crystals was determined using energy-dispersive X-ray spectroscopy (EDS, Oxford X-Max) with an electron beam energy of 10 keV. X-ray diffraction patterns were recorded using a diffractometer (Bruker, D8 Discover) equipped with Cu Kα_{\alpha} (λ\lambda=1.5418 Å) radiation from the (001) surface of the crystals.

Device fabrication

Thin Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 flakes were mechanically exfoliated from bulk crystals onto Si/SiO2_2(285 nm) substrates. Polymethyl Methacrylate (PMMA) was spin coated onto the substrates. Standard electron beam lithography technique was used to define the electrode patterns, and Ti (5 nm)/ Au (120 nm) was deposited as electrodes via electron beam evaporation. The flake thickness was measured by atomic force microscopy (AFM) after transport or photocurrent measurements.

Electrical measurements

The Hall resistivity was measured in a probe station system (East Changing, PS4-9K-1T). An a.c. current (Stanford Research System, CS580) with a frequency of 17.7 Hz was applied to the devices, while the Hall voltage was measured using a lock-in amplifier (Stanford Research System, SR865).

Photoresponse measurements

Scanning photocurrent measurements were performed using a scanning galvanometer to direct the laser beam onto the device in ambient conditions. The light sources included lasers with wavelengths of 633 nm, 1550 nm and 4 μ\mum. The 633 nm light source is a continuous-wave (CW) He-Ne laser, while the 1550 nm and 4 μ\mum sources were CW quantum cascade lasers. For visible light, a 40×\times transmissive objective lens was used to focus the beam, and for infrared light, a 40×\times reflective objective was employed. The full width at half maximum (FWHM) of the laser spots was approximately 1.8 μ\mum, 3.9 μ\mum and 11 μ\mum for 633 nm, 1550 nm and 4 μ\mum excitation, respectively (Figure S5). The laser was modulated at 389 Hz, and the zero-bias photocurrent was measured using a lock-in amplifier (Stanford Research System, SR865). The responsivity (RλR_\lambda) was calculated using Rλ=Iph/PR_\lambda= I_{ph}/P, with IphI_{ph} the photocurrent magnitude and PP the total incident power on the device. The specific detectivity D∗D^* was calculated by D∗=RλAdΔf/inD^* = R_\lambda\sqrt{A_d\Delta f}/i_n, where AdA_d, Δf\Delta f and ini_n represent the device effective area, the operating bandwidth and the noise current. [44] Response time was obtained by the modulated frequency dependence of photocurrent through the laser controller (Thorlabs, ITC4002QCL). The photocurrent (IfI_f) as a function of the frequency (ff) was fitted with If=I0/1+(2πfτ)2I_f = I_0/\sqrt{1+(2\pi f\tau)^2} to obtain the response time (τ\tau).

Supporting Information

EDS characterization of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 crystals; transport data of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 devices; optoelectronic measurement of the Mn(Bi0.82_{0.82}Sb0.18_{0.18})2_2Te4_4 device; calculation of specific detectivity; chemical vapor transport growth of Mn(Bi1−x_{1-x}Sbx_x)2_2Te4_4 crystals; measurement of focused laser spot size.

Funding Sources

This work was supported by the National Key R&D Program of China (Grant No. 2022YFA1405700), the National Natural Science Foundation of China (Grant No. 92365104 and 12174069), and Shuguang Program from the Shanghai Education Development Foundation.

Acknowledgements

Part of the sample fabrication was performed at Fudan Nano-fabrication Laboratory.

References

  1. [1]Long, M.; Wang, P.; Fang, H.; Hu, W. Progress, challenges, and opportunities for 2D material based photodetectors. Advanced Functional Materials 2019, 29 (19), 1803807.DOI
  2. [2]Lahiri, B. B.; Bagavathiappan, S.; Jayakumar, T.; Philip, J. Medical applications of infrared thermography: a review. Infrared physics & technology 2012, 55 (4), 221-235.DOI
  3. [3]Xu, H.; Liu, J.; Zhang, J.; Zhou, G.; Luo, N.; Zhao, N. Flexible organic/inorganic hybrid near-infrared photoplethysmogram sensor for cardiovascular monitoring. Advanced Materials 2017, 29 (31), 1700975.DOI
  4. [4]Ottonello-Briano, F.; Errando-Herranz, C.; Rödjegård, H.; Martin, H.; Sohlström, H.; Gylfason, K. B. Carbon dioxide absorption spectroscopy with a mid-infrared silicon photonic waveguide. Optics Letters 2019, 45 (1), 109-112.DOI
  5. [5]Mueller, T.; Xia, F.; Avouris, P. Graphene photodetectors for high-speed optical communications. Nature photonics 2010, 4 (5), 297-301.DOI
  6. [6]Rogalski, A. Toward third generation HgCdTe infrared detectors. Journal of alloys and compounds 2004, 371 (1-2), 53-57.DOI
  7. [7]Bhan, R.; Dhar, V. Recent infrared detector technologies, applications, trends and development of HgCdTe based cooled infrared focal plane arrays and their characterization. Opto-Electronics Review 2019, 27 (2), 174-193.DOI
  8. [8]Wang, Y.; Gu, Y.; Cui, A.; Li, Q.; He, T.; Zhang, K.; Wang, Z.; Li, Z.; Zhang, Z.; Wu, P.; et al. Fast uncooled mid-wavelength infrared photodetectors with heterostructures of van der Waals on epitaxial HgCdTe. Advanced Materials 2022, 34 (6), 2107772.DOI
  9. [9]Lei, W.; Antoszewski, J.; Faraone, L. Progress, challenges, and opportunities for HgCdTe infrared materials and detectors. Applied Physics Reviews 2015, 2 (4).DOI
  10. [10]Rogalski, A.; Martyniuk, P.; Kopytko, M. Challenges of small-pixel infrared detectors: a review. Reports on Progress in Physics 2016, 79 (4), 046501.DOI
  11. [11]Kimata, M. Uncooled infrared focal plane arrays. IEEJ Transactions on Electrical and Electronic Engineering 2018, 13 (1), 4-12.
  12. [12]Chen, C.; Li, C.; Min, S.; Guo, Q.; Xia, Z.; Liu, D.; Ma, Z.; Xia, F. Ultrafast silicon nanomembrane microbolometer for long-wavelength infrared light detection. Nano Letters 2021, 21 (19), 8385-8392.DOI
  13. [13]Wang, Q.; Li, C.-Z.; Ge, S.; Li, J.-G.; Lu, W.; Lai, J.; Liu, X.; Ma, J.; Yu, D.-P.; Liao, Z.-M.; et al. Ultrafast broadband photodetectors based on three-dimensional Dirac semimetal Cd₃As₂. Nano letters 2017, 17 (2), 834-841.
  14. [14]Chi, S.; Li, Z.; Xie, Y.; Zhao, Y.; Wang, Z.; Li, L.; Yu, H.; Wang, G.; Weng, H.; Zhang, H.; et al. A Wide-Range Photosensitive Weyl Semimetal Single Crystal—TaAs. Advanced Materials 2018, 30 (43), 1801372.DOI
  15. [15]Lai, J.; Liu, X.; Ma, J.; Wang, Q.; Zhang, K.; Ren, X.; Liu, Y.; Gu, Q.; Zhuo, X.; Lu, W.; et al. Anisotropic broadband photoresponse of layered type-II weyl semimetal MoTe₂. Advanced materials 2018, 30 (22), 1707152.DOI
  16. [16]Lai, J.; Liu, Y.; Ma, J.; Zhuo, X.; Peng, Y.; Lu, W.; Liu, Z.; Chen, J.; Sun, D. Broadband anisotropic photoresponse of the “hydrogen atom” version type-II Weyl semimetal candidate TaIrTe₄. ACS nano 2018, 12 (4), 4055-4061.DOI
  17. [17]Li, J.; Li, Q.; Mi, J.; Xu, Z.; Xie, Y.; Tang, W.; Zhu, H.; Li, L.; Tong, L. Ultrabroadband High Photoresponsivity at Room Temperature Based on Quasi-1D Pseudogap System (TaSe₄)₂I. Advanced Science 2024, 11 (7), 2302886.DOI
  18. [18]Ma, J.; Gu, Q.; Liu, Y.; Lai, J.; Yu, P.; Zhuo, X.; Liu, Z.; Chen, J.-H.; Feng, J.; Sun, D. Nonlinear photoresponse of type-II Weyl semimetals. Nature materials 2019, 18 (5), 476-481.DOI
  19. [19]Ji, Z.; Liu, G.; Addison, Z.; Liu, W.; Yu, P.; Gao, H.; Liu, Z.; Rappe, A. M.; Kane, C. L.; Mele, E. J.; et al. Spatially dispersive circular photogalvanic effect in a Weyl semimetal. Nature materials 2019, 18 (9), 955-962.
  20. [20]Osterhoudt, G. B.; Diebel, L. K.; Gray, M. J.; Yang, X.; Stanco, J.; Huang, X.; Shen, B.; Ni, N.; Moll, P. J.; Ran, Y.; et al. Colossal mid-infrared bulk photovoltaic effect in a type-I Weyl semimetal. Nature materials 2019, 18 (5), 471-475.DOI
  21. [21]Li, Y.; Li, D.; Wazir, N.; Zhu, Y.; Wang, Y.; Wang, Q.; Zhou, W.; Zhou, J.; Li, S.; Li, S. Chemical Vapor Deposition Growth of Atomically Thin SnSb2Te4 Single Crystals Toward Fast Photodetection. Advanced Functional Materials 2024, 2316849.DOI
  22. [22]Liu, J.; Xia, F.; Xiao, D.; Garcia de Abajo, F. J.; Sun, D. Semimetals for high-performance photodetection. Nature materials 2020, 19 (8), 830-837.DOI
  23. [23]Wang, A.-Q.; Ye, X.-G.; Yu, D.-P.; Liao, Z.-M. Topological semimetal nanostructures: From properties to topotronics. ACS nano 2020, 14 (4), 3755-3778.DOI
  24. [24]Wu, K.; Liao, X.; Iqbal, M. A.; Zeng, Y.-J. Research progress on topological material-based photodetectors. Materials Advances 2023, 4, 5018-5032.DOI
  25. [25]Lopez-Sanchez, O.; Lembke, D.; Kayci, M.; Radenovic, A.; Kis, A. Ultrasensitive photodetectors based on monolayer MoS₂. Nature nanotechnology 2013, 8 (7), 497-501.
  26. [26]Fang, H.; Hu, W. Photogating in low dimensional photodetectors. Advanced science 2017, 4 (12), 1700323.DOI
  27. [27]Zhang, X.; Pan, R.; Yang, Y.; Han, Q.; Liu, X.; Zhang, C.; Zhou, H.; Han, J.; Gou, J.; Wang, J. High-performance photodetector based on a 3D Dirac semimetal Cd₃As₂/tungsten disulfide (WS2) van der Waals heterojunction. Advanced Photonics Research 2021, 2 (6), 2000194.DOI
  28. [28]Zhang, L.; Han, X.; Wen, P.; Zhang, S.; Zheng, Z.; Li, J.; Gao, W. Weyl-semimetal TaIrTe₄/Si nanostructures for self-powered Schottky photodetectors. ACS Applied Nano Materials 2022, 5 (5), 6523-6531.DOI
  29. [29]Wang, G.; Sun, Y.; Yang, Z.; Lu, W.; Chen, S.; Zhang, X.; Ma, H.; Sun, T.; Huo, P.; Cui, X.; et al. Near-ideal Schottky junction photodetectors based on semimetal-semiconductor van der Waals heterostructures. Advanced Functional Materials 2024, 2316267.DOI
  30. [30]Xue, Z.; Fan, Z.; Liao, X.; Li, Y.; Qin, Y.; Zhang, G.; Song, X.; Liao, Z.-M.; Sun, D.; Lu, G.; et al. Metasurface Enabled Photothermoelectric Photoresponse of Semimetal Cd₃As₂ for Broadband Photodetection. Nano Letters 2022, 22 (21), 8728-8734.DOI
  31. [31]Ning, C.-Z.; Dou, L.; Yang, P. Bandgap engineering in semiconductor alloy nanomaterials with widely tunable compositions. Nature Reviews Materials 2017, 2 (12), 1-14.DOI
  32. [32]Long, M.; Gao, A.; Wang, P.; Xia, H.; Ott, C.; Pan, C.; Fu, Y.; Liu, E.; Chen, X.; Lu, W.; et al. Room temperature high-detectivity mid-infrared photodetectors based on black arsenic phosphorus. Science advances 2017, 3 (6), e1700589.DOI
  33. [33]Paul, S.; Hossain, M. T.; Mia, A. K.; Giri, P. Ultrabroadband Absorption and High-Performance Photodetection in Europium-Doped 2D Topological Insulator Bi₂Se₃ Nanosheets. ACS Applied Nano Materials 2021, 4 (11), 12527-12540.DOI
  34. [34]Deng, Y.; Yu, Y.; Shi, M. Z.; Guo, Z.; Xu, Z.; Wang, J.; Chen, X. H.; Zhang, Y. Quantum anomalous Hall effect in intrinsic magnetic topological insulator MnBi₂Te₄. Science 2020, 367 (6480), 895-900.DOI
  35. [35]Zhang, D.; Shi, M.; Zhu, T.; Xing, D.; Zhang, H.; Wang, J. Topological axion states in the magnetic insulator MnBi₂Te₄ with the quantized magnetoelectric effect. Physical review letters 2019, 122 (20), 206401.DOI
  36. [36]Liu, C.; Wang, Y.; Li, H.; Wu, Y.; Li, Y.; Li, J.; He, K.; Xu, Y.; Zhang, J.; Wang, Y. Robust axion insulator and Chern insulator phases in a two-dimensional antiferromagnetic topological insulator. Nature materials 2020, 19 (5), 522-527.
  37. [37]Hao, Y.-J.; Liu, P.; Feng, Y.; Ma, X.-M.; Schwier, E. F.; Arita, M.; Kumar, S.; Hu, C.; Lu, R. e.; Zeng, M.; et al. Gapless surface Dirac cone in antiferromagnetic topological insulator MnBi₂Te₄. Physical Review X 2019, 9 (4), 041038.DOI
  38. [38]Du, M. H.; Yan, J.; Cooper, V. R.; Eisenbach, M. Tuning Fermi levels in intrinsic antiferromagnetic topological insulators MnBi₂Te₄ and MnBi₄Te₇ by defect engineering and chemical doping. Advanced Functional Materials 2021, 31 (3), 2006516.arxiv.org/abs/2006.15475
  39. [39]Lee, D. S.; Kim, T.-H.; Park, C.-H.; Chung, C.-Y.; Lim, Y. S.; Seo, W.-S.; Park, H.-H. Crystal structure, properties and nanostructuring of a new layered chalcogenide semiconductor, Bi₂MnTe₄. CrystEngComm 2013, 15 (27), 5532-5538.DOI
  40. [40]Chen, B.; Fei, F.; Zhang, D.; Zhang, B.; Liu, W.; Zhang, S.; Wang, P.; Wei, B.; Zhang, Y.; Zuo, Z.; et al. Intrinsic magnetic topological insulator phases in the Sb doped MnBi₂Te₄ bulks and thin flakes. Nature communications 2019, 10 (1), 4469.DOI
  41. [41]Lai, J.; Ma, J.; Liu, Y.; Zhang, K.; Zhuo, X.; Chen, J.; Zhou, S.; Sun, D. Photocurrent response of type-II Dirac semimetal PtTe₂. 2D Materials 2020, 7 (3), 034003.DOI
  42. [42]Xia, C.; Yu, T.; Liu, J.; Li, X.; Wang, J.; Ma, S.; Yang, G.; Qiu, H.; Hu, Z.; Ye, N.; et al. Effective Self-Powered Semimetal TaTe₂ Photodetector with the Thermal Localization Photothermoelectric Effect from Ultraviolet to Mid-Infrared Range. Advanced Optical Materials 2024, 12 (22), 2400314.
  43. [43]Wang, J.; Fang, H.; Wang, X.; Chen, X.; Lu, W.; Hu, W. Recent progress on localized field enhanced two-dimensional material photodetectors from ultraviolet—visible to infrared. Small 2017, 13 (35), 1700894.DOI
  44. [44]Wang, F.; Zhang, T.; Xie, R.; Wang, Z.; Hu, W. How to characterize figures of merit of two-dimensional photodetectors. Nature Communications 2023, 14 (1), 2224.DOI
  45. [45]Zhang, K.; Zhang, T.; Cheng, G.; Li, T.; Wang, S.; Wei, W.; Zhou, X.; Yu, W.; Sun, Y.; Wang, P.; et al. Interlayer transition and infrared photodetection in atomically thin type-II MoTe₂/MoS₂ van der Waals heterostructures. ACS nano 2016, 10 (3), 3852-3858.DOI
  46. [46]Guo, S.; He, Y.; Lv, X.; Jiang, M.; Wei, Y.; Deng, Y.; Pan, X.; Lan, S.; Wang, D.; Liu, A.; et al. Topological insulator MnBi₂Te₄ and its van der Waals heterostructure for sensitive room-temperature terahertz photodetection. 2D Materials 2024, 11 (3), 035008.DOI
  47. [47]Guo, C.; Chen, Z.; Yu, X.; Zhang, L.; Wang, X.; Chen, X.; Wang, L. Ultrasensitive anisotropic room-temperature terahertz photodetector based on an intrinsic magnetic topological insulator MnBi₂Te₄. Nano Letters 2022, 22 (18), 7492-7498.DOI
  48. [48]Li, J.; Wang, Z.; Wen, Y.; Chu, J.; Yin, L.; Cheng, R.; Lei, L.; He, P.; Jiang, C.; Feng, L.; et al. High-performance near-infrared photodetector based on ultrathin Bi₂O₂Se nanosheets. Advanced Functional Materials 2018, 28 (10), 1706437.DOI
  49. [49]Wang, F.; Li, L.; Huang, W.; Li, L.; Jin, B.; Li, H.; Zhai, T. Submillimeter 2D Bi₂Se₃ flakes toward high-performance infrared photodetection at optical communication wavelength. Advanced Functional Materials 2018, 28 (33), 1802707.DOI
  50. [50]Zhang, X.; Zheng, J.; Ma, J.; Song, Y.; Zhang, X.; Liu, Q.; Wang, L.; Xiao, P.; Li, Y.; Wang, Z.; et al. Anisotropic photocurrent response at MnBi₂Te₄-metal interface. 2D Materials 2023, 10 (4), 045011.DOI
  51. [51]Sahu, S.; Panda, J.; Haider, G.; Frank, O.; Kalbáč, M.; Velický, M. j. Self-Biased High-Responsivity Photodetector Based on a Bi₂SeTe₂ Topological Insulator. ACS Applied Electronic Materials 2023, 5 (12), 6697- (52) Xia, F.; Mueller, T.; Golizadeh-Mojarad, R.; Freitag, M.; Lin, Y.-m.; Tsang, J.; Perebeinos, V.; Avouris, P. Photocurrent imaging and efficient photon detection in a graphene transistor. Nano letters 2009, 9 (3), 1039-1044.
  52. [53]Li, S.; Liu, T.; Liu, C.; Wang, Y.; Lu, H.-Z.; Xie, X. Progress on the antiferromagnetic topological insulator MnBi₂Te₄. National Science Review 2024, 11 (2), nwac296.DOI
  53. [54]Zhang, Y.; Holder, T.; Ishizuka, H.; de Juan, F.; Nagaosa, N.; Felser, C.; Yan, B. Switchable magnetic bulk photovoltaic effect in the two-dimensional magnet CrI₃. Nature communications 2019, 10 (1), 3783.DOI
  54. [55]Takagi, T.; Watanabe, R.; Yoshimi, R.; Tsukazaki, A.; Takahashi, K. S.; Kawasaki, M.; Tokura, Y.; Ogawa, N. Photogalvanic spectroscopy on MnBi₂Te₄ topological insulator thin films. Applied Physics Letters 2024, 124 (16).
  55. [56]Chen, H.; Jiayu, W.; Huayao, L.; Lin, M.; Zhang, C. Towards stoichiometric MnBi₂₋ₓSbₓTe₄ with tunable Fermi level and high mobility by optimized chemical vapor transport. In preparation.

Paper details

vlnc:W_3u4njxu3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents