betaFeedback

WorksPhysics and Astronomy

Ferroelectric and dielectric properties of Hf0.5Zr0.5O2 thin film near morphotropic phase boundary

Abstract

Recently, based on the phase-field modeling, it was predicted that Hf1-xZrxO2 (HZO) exhibits the morphotropic phase boundary (MPB) in its compositional phase diagram. Here, we investigate the effect of structural changes between tetragonal (t) and orthorhombic (o) phases on the ferroelectric and dielectric properties of HZO films to probe the existence of MPB region. The structural analysis show that by adjusting the ozone dosage during the atomic layer deposition process and annealing conditions, different ratios of t- to o-phases (f_(t/o) ) were achieved which consequently affect the ferroelectric and dielectric properties of the samples. Polarization versus electric field measurements show a remarkable increase in ferroelectric characteristics (Pr and Ec) of the sample that contains the minimum t-phase fraction (f_(t/o)~ 0.04). This sample shows the lowest dielectric constant compared to the other samples which is due to the formation of ferroelectric o-phase. The sample that contains the maximum f_(t/o)~ 0.41 demonstrates the highest dielectric response. By adjusting the f_(t/o), a large dielectric constant of ~ 55 is achieved. Our study reveals a direct relation between f_(t/o) and dielectric constant of HZO thin films which can be understood by considering the density of MPB region.

Dielectric constant as a function of the tetragonal/orthorhombic phase fraction, with ferroelectric polarization–electric field hysteresis loops for orthorhombic and tetragonal phases

Figure 1.

Introduction

Since the discovery of ferroelectric properties in HfO2\mathrm{HfO_2}-based materials [1], numerous advantages such as simple structures, strong binding energy between oxygen and transition metal ions, large bandgap (∼\sim5.3–5.7 eV), and compatibility with current complementary metal–oxide semiconductor technologies led to extensive research that focused on potential diverse applications such as ferroelectric memory, ferroelectric field effect transistors (Fe-FETs), pyroelectric sensors, and energy harvesters. Meanwhile, from the material survey of ferroelectrics, it is conventional that the structural phase transition induced by a compositional change plays a special role in obtaining excellent piezoelectric and dielectric properties [2, 3, 4, 5, 6, 7, 8, 9]. The phase boundary known as morphotropic phase boundary (MPB) separates regions of different symmetry by varying their composition in ferroelectrics [2, 3, 4, 5, 6, 7, 8, 9]. In fact, when different structural phases are almost degenerate near the MPB, rotations of polarization occur in response to external electric fields instead of a change in the magnitude of polarization [5]. Consequently, materials exhibit maximum piezoelectric and dielectric responses near the MPB as several phases co-exist and there is nearly no energy barrier separating them. The MPB has garnered significant practical interest because the variable that drives the transition (i.e., compositions) is inherent. Therefore, it provides an alternative approach to boost the dielectric constant ϵr\epsilon_r without degrading the bandgap. MPB ceramics are the basis of a wide range of piezoelectric and dielectric technologies, such as high-kk materials, sensors, actuators, smart systems, ultrasound generation and sensing and underwater acoustics. These applications motivated researchers to investigate the existence of MPB in the novel promising ceramic compounds e.g., PbHfO3\mathrm{PbHfO_3}–PbTiO3\mathrm{PbTiO_3}–Pb(Mg1/3Nb2/3)O3\mathrm{Pb(Mg_{1/3}Nb_{2/3})O_3} [10, 11], lead free BiFeO3\mathrm{BiFeO_3}-BaTiO3\mathrm{BaTiO_3} [12, 13], Pb(In1/2Nb1/2)O3\mathrm{Pb(In_{1/2}Nb_{1/2})O_3}–Pb(Mg1/3Nb2/3)O3\mathrm{Pb(Mg_{1/3}Nb_{2/3})O_3}–PbTiO3\mathrm{PbTiO_3} [14], PbSnO3\mathrm{PbSnO_3}–Pb(Mg1/3Nb2/3)O3\mathrm{Pb(Mg_{1/3}Nb_{2/3})O_3}–PbTiO3\mathrm{PbTiO_3} [15], BiScO3\mathrm{BiScO_3}-PbTiO3\mathrm{PbTiO_3}-Pb(Cd1/3Nb2/3)O3\mathrm{Pb(Cd_{1/3}Nb_{2/3})O_3} [16], and even present new methods to induce MPB into the ordinary ferroelectric ceramics e.g., BaTiO3\mathrm{BaTiO_3} [17].

Recently, Park et al. [18] and Hyun et al. [19] investigated the dielectric properties of the Zr-doped HfO2\mathrm{HfO_2} (Hf1−xZrxO2\mathrm{Hf_{1-x}Zr_xO_2} (HZO)) thin films. Their study proposed the existence of MPB phenomenon in Hf0.5Zr0.5O2\mathrm{Hf_{0.5}Zr_{0.5}O_2} composition. On one end (x=0x = 0), it is monoclinic (m-phase) and thus paraelectric, whereas on the other end (x=1x = 1), it is tetragonal (t-phase) and purely anti-ferroelectric (AFE). In between, by adjusting the fabrication conditions, it exhibits a non-centrosymmetric orthorhombic ferroelectric (FE) phase (o-phase) [20]. The multiphase in HZO is located between the boundary of the FE and AFE phases [18, 19, 20]. The existence of MPB in HZO system opened a new challenge to increase the dielectric properties of a silicon-compatible compound because the use of ZrO2\mathrm{ZrO_2} and HfO2\mathrm{HfO_2} in the semiconductor fabrication process is in the mature stage.

The phase evolution in HZO is largely affected by its composition, film thickness, and other thin film processing parameters, and therefore, the region of multiphase formation is influenced by the fabrication conditions [21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33]. In contrast to other high-ϵr\epsilon_r dielectrics, where the ϵr\epsilon_r value decreases with decreasing film thickness, these films show increasing ϵr\epsilon_r values with decreasing film thicknesses in the ∼5\sim5–2020 nm range by adjusting the MPB region [18], which is highly promising for future dynamic random access memories. Therefore, this approach emerges as an alternative method for engineering an extremely thin equivalent oxide thickness (EOT).

Despite the numerous advantages of the existence of the MPB region in HZO films, very few studies have been conducted to date, and there has not been any direct evidence that supports the presence of the MPB phenomenon in HZO materials [18, 19, 20]. In this study, we fabricate the HZO-based Metal-Insulator-Metal (MIM) capacitors with different t-phaseo-phase\frac{t\text{-phase}}{o\text{-phase}} ratios (ftfo\frac{f_t}{f_o}) to investigate the possible existence of the MPB region by evaluating the effect of ftfo\frac{f_t}{f_o} on ϵr\epsilon_r. This study provides evidence of the existence of the MPB region in HZO films.

The thermal expansion coefficient (TEC) of capping electrodes appeared to be a crucial parameter in facilitating or impeding the formation of o-phase in HfO2\mathrm{HfO_2}-based thin films, thus affecting ftfo\frac{f_t}{f_o}. It was established that metals with relatively low TEC compared to HZO provided additional driving force for t- to o-phase transition during rapid thermal annealing (RTA) [34]. Moreover, suppression of twin deformation through the formation of m-phase can be substantially prevented [35]. Another parameter that can affect ftfo\frac{f_t}{f_o} is the ozone dosage during the atomic layer deposition (ALD) of HfO2\mathrm{HfO_2}-based thin film. The primary role of the ozone O3\mathrm{O_3} pulses is to infuse oxygen into Hf and Zr layers, leading to the formation of HfO2\mathrm{HfO_2} and ZrO2\mathrm{ZrO_2} compounds, respectively. Moreover, the removal of C–O bonds from the sample by applying O3\mathrm{O_3} pulses can remarkably change the subsequent annealing behavior of the as-grown film. The C–O bonds can remain between pure HfO2\mathrm{HfO_2} domains owing to the incomplete chemical reaction of the precursors that subsequently prevent the agglomeration of the nanoscale domains, resulting in the stabilization of the tetragonal phase and thus change of the ftfo\frac{f_t}{f_o} [35, 36, 37, 38]. It has been proven that the ratio of tetragonal to orthorhombic phases ft/fof_t/f_o can be adjusted by applying different ozone dosages during deposition [35]. Therefore, fabrication of HZO films at different ozone pulses and adjusting annealing conditions enabled us to obtain MIM stacks with different ft/fof_t/f_o. The evaluation of ϵr\epsilon_r of the MIM stacks with different ft/fof_t/f_o is a promising approach to investigate the possible existence of the MPB region in HZO-based devices.

Experiments

The ∼\sim10-nm HZO films were deposited on 50-nm thick W bottom electrodes sputtered on SiO2_2/Si substrate using the ALD technique. Different ozone pulse durations from 2 to 30 s were applied during each deposition. The substrate temperature was maintained at 250 °C. The Hf [N–(C2_2H5_5) CH3_3]4_4 and Zr [N–(C2_2H5_5) CH3_3]4_4 precursors (EG Chem CO.) were used as the Hf and Zr metal sources, respectively. The growth rate of HfO2_2 and ZrO2_2 were almost the same (∼\sim1 Å/cycle). After deposition, all films were capped with a 50-nm W electrode using rf-sputtering technique to fabricate MIM capacitors. Finally, W/HZO/W capacitors with different electrode areas were passed through an annealing process in ambient N2_2 under two different conditions, i.e. 500 °C for 30 s (A1) and 700 °C for 5 s (A2), to achieve different t-/o-phase ratios ft/fof_t/f_o according to these references [35, 39].

The elemental composition was evaluated through X-ray photoelectron spectroscopy (XPS). A high-resolution transmission electron microscopy (HRTEM) and an X-ray reflectometer (XRR) were used to measure the film thickness. We have considered the oscillations in the XRR pattern and using equation (1) the film thickness was obtained.

t∼λ21θm+1−θm(1)t \sim\frac{\lambda}{2}\frac{1}{\theta_{m+1}-\theta_m} \tag*{(1)}

Where λ\lambda is wavelength of X-ray, θm+1\theta_{m+1} and θm\theta_m are the position of (m+1)(m+1)-th and mm-th interference maximums, respectively.

The crystalline structures of the films were investigated using an X-ray diffractometer (XRD) within a grazing incidence. The ft/fof_t/f_o was evaluated through a double-peak fitting of the o/t-phase characteristic Bragg peak. The ferroelectric properties of MIM capacitors were measured using a LCII ferroelectric precision tester (Radiant Technologies), and the dielectric permittivity was extracted from the small signal (50 mV) measurement of capacitance versus electric field at 10 kHz using the Keysight B1500A semiconductor device parameter analyzer. All measurements were performed at room temperature.

Results and discussion

Figure 1 shows the XPS data of the as-deposited sample that revealed the Zr/Hf ratio to be approximately 1, indicating the Zr0.5Hf0.5Ox\mathrm{Zr}_{0.5}\mathrm{Hf}_{0.5}\mathrm{O}_{x} composition which is a promising system to demonstrate the MPB phenomenon, as investigated by Park et al. [18]. The composition of deposited films was estimated by XPS intensities of the main peaks of Hf 4f, Zr 3d and O 1s.

X-ray Photoelectron Spectroscopy survey spectrum and O 1s, Hf 4f, and Zr 3d spectra

Figure 1 (PDF p. 6). (a) X-ray Photoelectron Spectroscopy (XPS) survey spectrum of the as – deposited Hf0.5Zr0.5O2\mathrm{Hf}_{0.5}\mathrm{Zr}_{0.5}\mathrm{O}_{2} sample. (b) O 1s, (c) Hf 4f and (d) Zr 3d XPS spectra.

The atomic ratio of Zr, Hf and O acquired from the calculation of the ratio of respective area under the Zr 3d, Hf 4f and O 1s peaks considering atomic sensitivity factors. Our investigation showsratyn that the ozone dosage or annealing conditions do not affect the Zr/Hf ratio and it is almost the same for all four samples.

The pristine polarization versus electric field (P–E) curves for the MIM devices fabricated under varying conditions are presented in Figure 2. The increase in ozone dosage during the film deposition resulted in a more open loop that might be due to the suppression of the mechanisms that cause the wake-up effect [35]. Our recent study presented in reference [35] showed that the carbon contaminants, which stabilize the tt-phase, can be removed through ozone treatment. Meanwhile, a higher ozone dosage can provide sufficient oxygen to form stoichiometric HZO films. Therefore, a de-pinched P–E loop was expected as the ozone dosage increased during the deposition. The sample annealed at 700 °C for 5 s (A2), resulting in a very high 2Pr2P_{\mathrm r} value of ~ 63 µC/cm². This huge increase in 2Pr2P_{\mathrm r} value compared to the samples annealed at 500 °C (A1) was attributed to the high mechanical stress applied to the HZO film during the cooling step of RTA, according to equation (2).

Figure 2. P–E curves of HZO devices fabricated under different conditions. A1 presents annealing at 500 °C for 30 min, whereas A2 presents annealing at 700 °C for 5 sec.

ϵT(TA)=∫TRTTA(αfilm−αCap) dT(2)\epsilon_{\mathrm T}(T_{\mathrm A}) = \int_{T_{\mathrm{RT}}}^{T_{\mathrm A}}(\alpha_{\mathrm{film}}-\alpha_{\mathrm{Cap}})\,dT \tag*{(2)}

where αfilm\alpha_{\mathrm{film}} and αCap\alpha_{\mathrm{Cap}} are the TEC of the film and capping materials, respectively, and TAT_A is the post-annealing temperature. The TEC of W is lower than HZO film, which causes a tensile strain on HZO film during the cooling step of RTA. The tensile strain on HZO can facilitate the formation of o-phase by suppression of the twin deformation, which causes m-phase formation.

Figure 3a presents HRTEM image of the sample annealed at 700 °C for 5 sec. From the XRR scan (Figure 3b) the thickness was calculated using equation (1). An almost 10 nm film was deposited on W bottom electrode during the ALD process, which was confirmed by the cross-sectional HRTEM image. XRD results presented in figures 3c and 3d, indicate the two important features of different devices. In all MIM stacks, the formation of the m-phase was suppressed, and only t- and o-phase characteristic Bragg peaks were observed at approximately 2θ=30.5∘2\theta= 30.5^\circ. The increase in ozone dosage is accompanied by a left-shift of the t/o characteristic Bragg peaks (Figure 3d). This left-shift revealed an important structural feature of different HZO films. The fraction of the non-centrosymmetric o-phase in HZO films increases as ozone dosage increases. Therefore, the 2Pr2P_{\mathrm{r}} value increased as illustrated in figure 2. Consequently, the ozone dosage during the film deposition can adjust ft/fof_{\mathrm{t}}/f_{\mathrm{o}}. Annealing at higher temperatures (700 ºC) further shifted the t/o characteristic Bragg peak to the left side and almost suppressed the formation of the t-phase (therefore, ft/fo∼0f_{\mathrm{t}}/f_{\mathrm{o}} \sim0) after the cooling process to room temperature. This caused a huge increase in the 2Pr2P_{\mathrm{r}} value as was already presented in figure 2.

Cross-sectional HRTEM, X-ray reflectivity, XRD patterns, and magnified XRD region

Figure 3. (a) A cross-sectional HRTEM of W/HZO/W device. (b) X-ray reflectivity of the ∼\sim10-nm films grown at 5 sec ozone dosage. (b) XRD patterns for HZO films deposited under different conditions. (d) The magnified region of XRD patterns showing the evolution of o/t Bragg peak versus fabrication conditions.

To evaluate the structural changes of HZO film fabricated at different conditions, the characteristic o/t peaks that were detected around 2θ∼30.5∘2\theta\sim30.5^\circ was precisely investigated. Figure 4 and Table 1 revealed that the fto\frac{f_t}{o} substantially changes depends on the fabrication condition. The fto\frac{f_t}{o} values were directly calculated by considering the relative area below each characteristic peak. Therefore, different fabrication procedures cause the deposition of HZO films with different fto\frac{f_t}{o} (Table 1).

X-ray diffraction patterns of HZO films fabricated at different ozone dosages and annealing conditions

Figure 4. X-ray diffraction patterns of the HZO films fabricated at (a) 5 s ozone dosage A1, (b) 15 s ozone dosage A1, (c) 30 s ozone dosage A1, and (d) 15 s ozone dosage A2. The red area presents o (111) peak and the pink area presents t (011) peak.

Fabrication condition5 s O3_3, A115 s O3_3, A130 s O3_3, A115 s O3_3, A2
ftfo\frac{f_t}{f_o}0.410.190.080.04

Table 1. The calculated ftfo\frac{f_t}{f_o} in HZO films deposited at different ozone dosages and annealing conditions. The ftfo\frac{f_t}{f_o} was directly evaluated using the relative area below characteristic Bragg peaks from figure 4.

Recently, Park et al. [18, 19] investigated the existence of MPB in HZO thin films. According to their study, the Hf0.5_{0.5}Zr0.5_{0.5}O2_2 film is the promising candidate to show the MPB region. However, different studies showed that the compositional region (xx) in which the Hf1−x_{1-x}Zrx_xO2_2 thin films show MPB-like behavior is greatly affected by the fabrication process, as the coexistence of the t/o-phase can be substantially altered during the fabrication process.

It has been shown that materials exhibit maximum piezoelectric and dielectric responses near the MPB [5]. The response to external stimuli is significant near the MPB, as several phases (different phases have different charge responses, such as dielectric, ferroelectric, and anti-ferroelectric) co-exist and there is nearly no energy barrier separating them. Consequently, a slight mechanical or electrical perturbation could induce a significant charge response. Therefore, we measured the ϵr\epsilon_r values as a function of applied bias electric field for different HZO films (Figure 5a) and established that the sample containing higher ft/fof_t/f_o shows higher ϵr\epsilon_r in different ranges of applied bias voltage. The butterfly-like capacitance versus bias voltage is due to the increase in motion of domain walls under the application of a strong DC electric field. It has been shown that the application of strong electric field on HZO film can induce the phase transition from t- to o-phase affecting the MPB region [40]. Therefore, apart from the domain wall permittivity, the capacitance of the HZO-based MIM stack can be further increased by the application of a strong electric field that causes the phase transition between t- and o-phases.

The sample with the minimum ft/fof_t/f_o, which showed strong ferroelectric polarization (Figure 2), demonstrates the lowest electric field-induced permittivity compared to the other samples. Conversely, the sample with the maximum ft/fof_t/f_o (confirmed through XRD measurement) shows the highest electric field-induced permittivity. Therefore, the ft/fof_t/f_o in the HZO film determines its dielectric permittivity under a bias electric field. A higher fraction of the t-phase results in a higher response from the film under external stimuli (electric field). According to the MPB-based point of view, the highest ratio of o/t-phase (ft/fof_t/f_o) provides the highest density of the MPB region in the deposited materials. Therefore, an external stimulus such as a strong electric field receives strong feedback from the material. Figure 5b shows ϵrmax\epsilon_r^{max} (Maximum dielectric constant) and ϵrE=0\epsilon_r^{E=0} (Dielectric constant at zero-biased field) versus ft/fof_t/f_o for different samples. Two important features can be observed in this figure. First, as ft/fof_t/f_o increases, both dielectric constants (ϵrmax\epsilon_r^{max} and ϵrE=0\epsilon_r^{E=0}) increased and the sample with the maximum ft/fof_t/f_o attained the maximum ϵr\epsilon_r. The second feature that is a meaningful trend, is the difference between two dielectric constants i.e., Δϵr=ϵrmax−ϵrE=0\Delta\epsilon_r = \epsilon_r^{max} - \epsilon_r^{E=0} for each sample (Inset of Figure 5b). This difference indicates the extent to which the biased electric field can increase the ϵr\epsilon_r in each sample. The sample with the highest ft/fof_t/f_o has the highest electric field-induced increase in dielectric constant (Δϵr\Delta\epsilon_r), whereas the sample with the lowest ft/fof_t/f_o has the minimum increase in dielectric constant under the application of a biased field. The difference between ϵrmax\epsilon_r^{max} and ϵrE=0\epsilon_r^{E=0} (Δϵr\Delta\epsilon_r) increases as ft/fof_t/f_o increases.

Dielectric constant versus bias electric field

(a)

Dielectric constant versus $f_t/f_o$

(b)

Capacitance versus electric field

(c)

Figure 5. (a) Dielectric constant vs. bias electric field for the samples grown under different conditions measured at 10 kHz. (b) The ϵrmax\epsilon_r^{max} and ϵrE=0\epsilon_r^{E=0} versus ft/fof_t/f_o. The inset shows the difference between ϵrmax\epsilon_r^{max} and ϵrE=0\epsilon_r^{E=0} (Δϵr\Delta\epsilon_r) as a function of ft/fof_t/f_o. (c) Capacitance vs. electric field for different samples as a function of applied frequency. The Red branch corresponds to the samples grown at 5 s ozone dosage, Blue branch at 15 s, and Green branch at 30 s. All samples were annealed under the A1 conditions.

To further investigate the C–E behavior of MIM devices fabricated under different conditions, the capacitance was measured at higher frequencies, i.e., 100 kHz and 1 MHz. The results for different capacitors show a decrease in dielectric capacitance as the frequency increases (Figure 5c). This behavior was expected as some polarization mechanisms can be suppressed at higher frequencies, in particular, space-charge polarization that occurs owing to the structural defects [41, 42]. Therefore, by increasing the frequency, we attempted to separate the contribution of space-charge polarization from the intrinsic polarization mechanisms (i.e., electronic, ionic, dipole, and domain wall polarizations). Figure 5c shows that even at 1 MHz, the sample with the maximum ft/fof_{t}/f_{o} (Red branch) exhibits the highest capacitance compared to the other samples. These results provide evidence of the existence of the MPB region due to the coexistence of t- and o-phases in HZO films.

Conclusion

The existence of the MPB region in HZO thin films was investigated through XPS, XRD, and dielectric measurements. The HZO thin films with different ft/fof_{t}/f_{o} were deposited through adjusting fabrication conditions. The sample with the lowest ft/fof_{t}/f_{o} showed the smallest ϵr\epsilon_{r}, whereas that with the maximum ft/fof_{t}/f_{o} showed a large ϵr\epsilon_{r} of ~55. There has been a direct relation between ft/fof_{t}/f_{o} and ϵr\epsilon_{r}. Moreover, the ft/fof_{t}/f_{o} determined the electric field-induced increase of ϵr\epsilon_{r} in each sample. These observations provide strong evidence supporting the existence of the MPB region in HZO films.

Acknowledgements

This work was supported by the National Research Foundation of Korea funded by the Korea government (MSIT), Grant No. NRF-2018R1A3B1052693. The authors thank Dr. Stanislav Kamba, Dr. Writam Banerjee and Dr. Nikam for helpful discussions.

References

  1. [1]Böсke, T.; Müller, S.; Bräuhaus, J. D.; Schröder, U.; Böttger, U. Ferroelectricity in hafnium oxide thin films. Appl. Phys. Lett. 2011, 99, 102903.DOI
  2. [2]Dinh Tung Luan N, Vuong LD, Van Chuong T, Truong Tho N. Structure and physical properties of PZT-PMnN-PSN ceramics near the morphological phase boundary. Adv Mater Sci Eng 2014;2014.DOI
  3. [3]Liu H, Chen J, Huang H, Fan L, Ren Y, Pan Z, et al. Role of Reversible Phase Transformation for Strong Piezoelectric Performance at the Morphotropic Phase Boundary. Phys Rev Lett 2018; 120:55501.DOI
  4. [4]Tomita Y, Kato T. Relaxor behavior and morphotropic phase boundary in a simple model. J Phys Soc Japan 2013; 82:1–5.DOI
  5. [5]Guo R, Cross LE, Park SE, Noheda B, Cox DE, Shirane G. Origin of the high piezoelectric response in PbZr₁-xTiₓO₃. Phys Rev Lett 2000; 84:5423–6.pubmed.ncbi.nlm.nih.gov/10990959
  6. [6]Ahart M, Somayazulu M, Cohen RE, Ganesh P, Dera P, Mao HK, et al. Origin of morphotropic phase boundaries in ferroelectrics. Nature 2008; 451:545–8.DOI
  7. [7]Iwata M, Ishibashi Y. Theory of morphotropic phase boundary in solid solution systems of perovskite-type oxide ferroelectrics. Japanese J Appl Physics, Part 1 Regul Pap Short Notes Rev Pap 1999; 38:5670–3.
  8. [8]Cross, E.; Lead-Free at Last, Nature 432, 24, (2004).pubmed.ncbi.nlm.nih.gov/15516920
  9. [9]Damjanovic D. A morphotropic phase boundary system based on polarization rotation and polarization extension. Appl Phys Lett 2010; 97:24–7.DOI
  10. [10]Wang, D., Cao, M., & Zhang, S. (2012). Investigation of ternary system PbHfO₃–PbTiO₃–Pb (Mg₁/₃Nb₂/₃)O₃ with morphotropic phase boundary compositions. Journal of the American Ceramic Society, 95(10), 3220-3228.DOI
  11. [11]Wang, D., Cao, M., & Zhang, S. (2012). Piezoelectric properties of PbHfO₃–PbTiO₃–Pb (Mg₁/₃Nb₂/₃)O₃ ternary ceramics. physica status solidi (RRL)–Rapid Research Letters, 6(3), 135-137.DOI
  12. [12]Murakami, S., Ahmed, N. T. A. F., Wang, D., Feteira, A., Sinclair, D. C., & Reaney, I. M. (2018). Optimising dopants and properties in BiMeO₃ (Me= Al, Ga, Sc, Y, Mg₂/₃Nb₁/₃, Zn₂/₃Nb₁/₃, Zn₁/₂Ti₁/₂) lead-free BaTiO₃-BiFeO₃ based ceramics for actuator applications. Journal of the European Ceramic Society, 38(12), 4220-4231.DOI
  13. [13]Wang, G., Fan, Z., Murakami, S., Lu, Z., Hall, D.A., Sinclair, D.C., Feteira, A., Tan, X., Jones, J.L., Kleppe, A.K. and Wang, D., 2019. Origin of the large electrostrain in BiFeO₃-BaTiO₃ based lead-free ceramics. Journal of Materials Chemistry A, 7(37), pp.21254-21263.DOI
  14. [14]Wang, D., Cao, M., & Zhang, S. (2012). Phase diagram and properties of Pb(In₁/₂Nb₁/₂)O₃–Pb (Mg₁/₃Nb₂/₃)O₃–PbTiO₃ polycrystalline ceramics. Journal of the European Ceramic Society, 32(2), 433-439.DOI
  15. [15]Wang, D., Cao, M., & Zhang, S. (2011). Piezoelectric ceramics in the PbSnO₃–Pb(Mg₁/₃Nb₂/₃)O₃–PbTiO₃ ternary system. Journal of the American Ceramic Society, 94(11), 3690-3693.
  16. [16]Lan, Z., Chen, K., He, X., Zhou, S., Zheng, X., Liu, J., Fang, L., Lei, X., Wang, D., Peng, B. and Liu, L., 2019. Phase evolution and thermal stability of high Curie temperature BiScO₃-PbTiO₃-Pb (Cd₁/₃Nb₂/₃)O₃ ceramics near MPB. Journal of Applied Physics, 126(23), p.234103.DOI
  17. [17]Wang, D., Fan, Z., Rao, G., Wang, G., Liu, Y., Yuan, C., Ma, T., Li, D., Tan, X., Lu, Z. and Feteira, A., 2020. Ultrahigh piezoelectricity in lead-free piezoceramics by synergistic design. Nano Energy, 76, p.104944.DOI
  18. [18]Park MH, Lee YH, Kim HJ, Kim YJ, Moon T, Kim K Do, et al. Morphotropic Phase Boundary of Hf₁₋ₓZrₓO₂ Thin Films for Dynamic Random Access Memories. ACS Appl Mater Interfaces 2018;10: 42666–73.DOI
  19. [19]Hyun, S.D., Park, H.W., Park, M.H., Lee, Y.H., Lee, Y.B., Kim, B.Y., Kim, H.H., Kim, B.S. and Hwang, C.S., Field-Induced Ferroelectric Hf₁₋ₓZrₓO₂ Thin Films for High-k Dynamic Random Access Memory. Advanced Electronic Materials, 2020; p.2000631.DOI
  20. [20]Ni K, Saha A, Chakraborty W, Ye H, Grisafe B, Smith J, et al. Equivalent Oxide Thickness (EOT) Scaling with Hafnium Zirconium Oxide High-k Dielectric Near Morphotropic Phase Boundary. Tech Dig - Int Electron Devices Meet IEDM 2019; 2019-December:7–10.DOI
  21. [21]Park, M. H.; Lee, Y. H.; Kim, H. J.; Kim, Y. J.; Moon, T.; Kim, K. D.; Müller, J.; Kersch, A.; Schroeder, U.; Mikolajick, T.; Hwang, C. S. Ferroelectricity and Antiferroelectricity of Doped Thin HfO₂-Based Films. Adv. Mater. 2015, 27, 1811.DOI
  22. [22]Parija, A.; Waetzig, G. R.; Andrews, J. L.; Banerjee, S. Traversing Energy Landscapes Away from Equilibrium: Strategies for Accessing and Utilizing Metastable Phase Space. J. Phys. Chem. C 2018, 122, 25709.DOI
  23. [23]Batra, R.; Huan, T. D.; Jones J. L.; Rossetti, G.; Ramprasad, R. Factors Favoring Ferroelectricity in Hafnia: A First-Principles Computational Study. J. Phys. Chem. C 2017, 121, 4139.DOI
  24. [24]Park, M. H.; Lee, Y. H.; Mikolajick, T.; Schroeder, U.; Hwang, C. S. Thermodynamic and Kinetic Origins of Ferroelectricity in Fluorite Structure Oxides. Adv. Electron. Mater. 2019, 5, 1800522.DOI
  25. [25]Shandalov, M.; McIntyre, P. C. Size-dependent polymorphism in HfO₂ nanotubes and nanoscale thin films. J. Appl. Phys. 2009, 106, 084322.DOI
  26. [26]Dogan, M.; Gong, N.; Ma, T. P.; Ismail-Beigi, S. Causes of ferroelectricity in HfO₂-based thin films: an ab initio perspective. Phys. Chem. Chem. Phys. 2019, 21, 12150.DOI
  27. [27]Batra, R.; Tran, H. D.; Ramprasad, R. Stabilization of metastable phases in hafnia owing to surface energy effects. Appl. Phys. Lett. 2016, 108, 172902.DOI
  28. [28]Park, M. H.; Lee, Y. H.; Kim, H. J.; Kim, Y. J.; Moon, T.; Kim, K. D.; Hyun, S. D.; Mikolajick, T.; Schroeder, U.; Hwang, C. S. Understanding the formation of the metastable ferroelectric phase in hafnia–zirconia solid solution thin films. Nanoscale 2018, 10, 716.DOI
  29. [29]Materlik, R.; Kunneth, C.; Kersch, A. The origin of ferroelectricity in Hf₁−ₓZrₓO₂: A computational investigation and a surface energy model. J. Appl. Phys. 2015, 117, 134109.DOI
  30. [30]Navrotsky, A. Thermochemical insights into refractory ceramic materials based on oxides with large tetravalent cations. J. Mater. Chem. 2005, 15, 1883.DOI
  31. [31]Fan, P.; Zhang, Y. K.; Yang, Q.; Jiang, J.; Jiang, L. M.; Liao, M.; Zhou, Y. C. Origin of the Intrinsic Ferroelectricity of HfO2 from ab Initio Molecular Dynamics. J. Phys. Chem. C 2019, 123, 21743.DOI
  32. [32]Sharma, G.; Ushakov, S. V.; Navrotsky, A. Size driven thermodynamic crossovers in phase stability in zirconia and hafnia. J. Am. Ceram. Soc. 2018, 101, 31.DOI
  33. [33]Sang, X.; Grimley, E. D.; Schenk, T.; Schroeder, U.; Lebeau, J. M. On the structural origins of ferroelectricity in HfO₂ thin films. Appl. Phys. Lett. 2015, 106, 162905.DOI
  34. [34]Cao, R.; Wang, Y.; Zhao, S.; Yang, Y.; Zhao, X.; Wang, W.; Zhang, X.; Lv, H.; Liu, Q.; Liu, M. Effects of Capping Electrode on Ferroelectric Properties of Hf₀.₅Zr₀.₅O₂ Thin Films. IEEE Electron Device Lett. 2018, 39, 8, 1207.
  35. [35]Kashir, A.; Oh, S. Y.; Hwang, H. S. Defect Engineering to Achieve Wake-up Free HfO2-Based Ferroelectrics, Adv. Eng. Mat., 2020, 2000791. DOI: 10.1002/adem.202000791DOI
  36. [36]Cho, D. Y.; Jung, H. S.; Yu, I. H.; Yoon, J. H.; Kim, H. K.; Lee, S. Y.; Jeon, S. H.; Han, S.; Kim, J. H.; Park, T. J.; Park, B. G.; Hwang, C. S. Stabilization of Tetragonal HfO₂ under Low Active Oxygen Source Environment in Atomic Layer Deposition. Chem. Mater. 2012, 24, 3534.
  37. [37]Kim, B. S.; Hyun, S. D.; Moon, T.; Kim, K. D.; Lee, Y. H.; Park, H. W.; Lee, Y. B.; Roh, J.; Kim, B. Y.; Kim, H. H.; Park, M. H.; Hwang, C. S. A Comparative Study on the Ferroelectric Performances in Atomic Layer Deposited Hf₀.₅Zr₀.₅O₂ Thin Films Using Tetrakis (ethylmethylamino) and Tetrakis (dimethylamino) Precursors. Nanoscale Res. Lett. 2020, 15, 72.DOI
  38. [38]Jung, H. S.; Jeon, S. H.; Kim, H. K.; Yu, I. H.; Lee, S. Y.; Lee, J.; Chung, Y. J.; Cho, D. Y.; Lee, N. I.; Park, T. J.; Choi, J. H.; Han, S.; Hwang, C. S. The Impact of Carbon Concentration on the Crystalline Phase and Dielectric Constant of Atomic Layer Deposited HfO₂ Films on Ge Substrate. ECS J. Solid State Sci. Technol. 2012, 1, N33.DOI
  39. [39]Kashir, A.; Kim, H. W.; Oh, S. Y.; Hwang, H. S., Large remnant polarization in a wake-up free Hf₀.₅Zr₀.₅O₂ ferroelectric film through bulk and interface engineering, ACS Appl. Electron. Matter. DOI: 10.1021/acsаelm.0c00671
  40. [40]Chouprik, A., Zakharchenko, S., Spiridonov, M., Zarubin, S., Chernikova, A., Kirtaev, R., Buragohain, P., Gruverman, A., Zenkevich, A. and Negrov, D., 2018. Ferroelectricity in Hf0. 5Zr0. 5O2 thin films: a microscopic study of the polarization-switching phenomenon and field-induced phase transformations. ACS applied materials & interfaces, 10 (10), 8818-8826.DOI
  41. [41]Kashir, A., Jeong, H.W., Jung, W., Jeong, Y.H. and Lee, G.H., 2019. Strain-induced increase of dielectric constant in EuO thin film. Materials Research Express, 6 (10), 106321.DOI
  42. [42]Kashir, A., Jeong, H.W., Lee, G.H., Mikheenko, P. and Jeong, Y.H., 2019. Dielectric properties of strained nickel oxide thin films. Journal of the Korean Physical Society, 74(10), 984-988.DOI

Paper details

vlnc:W_3ys3j4ve
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy