Forbidden p-d Orbital Coupling Accelerates High-Power-Factor Materials Discovery

Abstract

The intrinsic entanglement between electrical conductivity (σσ) and the Seebeck coefficient (SS) significantly constrains power factor (PF) enhancement in thermoelectric (TE) materials. While high valley degeneracy (NvkN_{\mathrm{vk}}) effectively balances σσ and SS to improve PF, identifying compounds with high NvkN_{\mathrm{vk}} remains challenging. In this study, we develop an effective approach to rapid discover pp-type semiconductors with high NvkN_{\mathrm{vk}} through manipulating anion-pp and cation-dd orbital coupling. By prohibiting pp-dd orbital coupling at the ΓΓ point, the valence band maximum shifts away from the ΓΓ point (where NvkN_{\mathrm{vk}}=1), thereby increasing NvkN_{\mathrm{vk}}. Through the examination of the common irreducible representations of anion-pp and cation-dd orbitals at the ΓΓ point, we identify 7 compounds with NvkN_{\mathrm{vk}} ≥\ge 6 from 921 binary and ternary semiconductors. First-principles calculations with electron-phonon coupling demonstrate that PtP2_2, PtAs2_2, and PtS2_2 exhibit exceptionally high PFs of 130, 127, and 82 μμWcm−1^{-1}K−2^{-2} at 300K, respectively, which are three to five times higher than those of the well-studied TE materials. This work not only elucidates the underlying mechanism of high NvkN_{\mathrm{vk}} formation through group theory, but also establishes an efficient high-PF material discovery paradigm, extended to more complex systems.

TE materials facilitate the direct conversion between electrical and thermal energy, presenting promising applications in the transforming of (waste) heat into electrical energy and the provision of solid-state cooling [1, 2, 3, 4, 5, 6]. The efficiency of energy-to-electricity conversion is intricately linked to the dimensionless figure of merit (ZTZT), which is defined as ZT=S2σT/(κL+κe)ZT = S^2\sigma T/(\kappa_\mathrm{L} + \kappa_\mathrm{e}), where SS, σ\sigma, κL\kappa_\mathrm{L}, κe\kappa_\mathrm{e}, and TT are Seebeck coefficient, electrical conductivity, lattice thermal conductivity, electron thermal conductivity, and absolute temperature, respectively. The deep entanglement among these parameters prevents simultaneous optimization, thereby limiting the energy conversion efficiency of TE materials [7, 8, 9]. Enhancing ZTZT necessitates either an increase in the power factor (PF, S2σS^2\sigma) or a reduction in both κL\kappa_\mathrm{L} and κe\kappa_\mathrm{e}. Given that κe\kappa_\mathrm{e} is proportional to σ\sigma, according to the Wiedemann-Franz law [10], the primary strategy for improving ZTZT involves reducing κL\kappa_\mathrm{L} while simultaneously increasing the PF. In the framework of kinetic theory [11], κL\kappa_\mathrm{L} can be expressed as 13Cvvg2τ\frac{1}{3}C_\mathrm{v}v_\mathrm{g}^2\tau, where CvC_\mathrm{v}, vgv_\mathrm{g}, and τ\tau are heat capacity, phonon group velocity, and phonon relaxation time, respectively. Since vgv_\mathrm{g} is proportional to k/M\sqrt{k/M}, where kk denotes chemical bond strength and MM represents atomic mass, materials with short τ\tau, low CvC_\mathrm{v}, weak kk, and relatively large MM typically exhibit low κL\kappa_\mathrm{L}. To date, numerous strategies have been employed to suppress κL\kappa_\mathrm{L}, including defect engineering [12, 13, 14], nano-structure precipitate [15, 16, 17, 18], lone-pair electrons [19, 20], rattling phonon modes [21, 22, 23], and weak chemical [24, 25, 26].

Another crucial factor for enhancing ZTZT is the increase of the PF. Furthermore, the output power density of a device is directly correlated with PF, and thus high PF is essential for achieving high power density output [27]. However, σ\sigma and SS are heavily entangled—specifically, σ\sigma is directly proportional to the carrier concentration (nn), whereas SS exhibits an inverse relationship with nn [28]. Band alignment is an effective strategy for enhancing PF of TE materials [29, 30, 31, 32, 33]. This is attributed to the fact that SS is proportional to the effective mass of the density of states (md∗m_\mathrm{d}^*), which in turn is proportional to both the band effective mass (mb∗m_\mathrm{b}^*) and band degeneracy NvN_\mathrm{v} (Nv=Nvk×NvoN_\mathrm{v}=N_\mathrm{vk}\times N_\mathrm{vo}, where NvoN_\mathrm{vo} is the orbital degeneracy) within a single parabolic band [34]. Consequently, a high NvkN_\mathrm{vk} can significantly alleviate the competition between SS and σ\sigma, thereby enhancing the PF [35, 36, 37, 38, 39, 40]. For instance, the convergence of the second maximum of the valence band (located at the midpoint of the Σ\Sigma line, exhibiting a NvkN_\mathrm{vk} of 12) with the valence band maximum (VBM) at the L point (Nvk=4N_\mathrm{vk}=4) in PbTe, through appropriate alloying with PbSe, can result in a substantial increase in ZTZT from 0.8 to 1.8 [41]. Similarly, the solid solution Mg2_2Si0.3_{0.3}Sn0.7_{0.7} enhances the PF to 48 μ\muW cm−1^{-1}K−2^{-2} at 550 K, which is more than double that of traditional n-type materials [42]. However, materials with intrinsically high NvN_\mathrm{v} are relatively rare, and many TE materials require heavy doping or alloying, complicating material fabrication and potentially reduce stabilities. Therefore, explore semiconductors with intrinsically high NvkN_\mathrm{vk} in both VBM and conduction band minimum (CBM) is highly advantageous. The value of NvkN_\mathrm{vk} is determined by the positions of VBM or CBM within the first Brillouin zone (BZ). The Γ\Gamma point possesses the lowest NvkN_\mathrm{vk}, equal to 1, while the zone boundaries, particularly at the midpoint of the lines connecting two high symmetry points, exhibit a high NvkN_\mathrm{vk} if the compound has a high symmetry.

For most ionic semiconductors lacking transition metals, the valence and conduction bands predominantly arise from the anion-pp and cation-ss orbitals, respectively. Consequently, the VBM and CBM of these compounds are typically located at the Γ\Gamma point, as observed in NaCl and CaS, since the pp orbitals are aligned ‘downhill’ and ss orbitals ‘uphill’ [43, 44]. However, in compounds containing cations with lone-pair electrons, the VBM may shift away from the Γ\Gamma point, resulting in a higher NvkN_{\mathrm{vk}}. This shift occurs because ss orbitals are positioned ‘uphill’, with notable examples including PbTe [45], Bi2_2Te3_3 [46], and Li2_2TlBi [26]. This strategy has been widely employed in the design of high-performance TE materials [24, 44]. Is there other strategy of designing semiconductors with high NvkN_{\mathrm{vk}}?

In this work, we proposed a strategy for identifying pp-type TE materials with high NvkN_{\mathrm{vk}} based on pp-dd orbital coupling and group theory. The anti-bonding states formed through pp-dd coupling located below the Fermi level can mitigate the ‘downhill’ behavior of the anion-pp orbitals. If the pp-dd coupling is prohibited at the Γ\Gamma point, the energy bands will ‘uphill’ from the non-bonding states (low energy) at the Γ\Gamma point to the anti-bonding states (high energy) near the zone boundary, leading to an increased NvkN_{\mathrm{vk}}. We then analyze the conditions necessary for the formation of forbidden pp-dd coupling at the Γ\Gamma point by utilizing symmetry-adapted band-representation analysis. With this approach, we screen 921 binary and ternary compounds stored in the Materials Project (www.materialproject.org) [47] and identify 41 compounds with high NvkN_{\mathrm{vk}}. Electron transport calculations based on electron-phonon coupling demonstrate that PtP2_2, PtAs2_2, and PtS2_2 exhibit maximum PF of 130, 127, and 82 μ\muWcm−1^{-1}K−2^{-2} at 300K, which are 3-5 times greater than those of the well-studied TE compounds. Our results not only elucidate the underlying mechanism for the formation of high NvkN_{\mathrm{vk}} in compounds exhibiting pp-dd coupling, but also facilitate the discovery of new compounds with high PF. Furthermore, this novel strategy is universal and can be extended to more complicated systems.

Results and discussion

Electronic structures of rock-salt and zinc blende AgBr

As illustrated in Figure 1(a), AgBr crystallizes in a rock-salt structure (space group Fm3ˉmFm\bar{3}m, No. 225), in which the Ag+^+ cation is octahedrally coordinated by six Br−^- anions. The band structure, depicted in Figure 1(b), reveals that the VBM is situated at the L point of the BZ, which has NvkN_{\mathrm{vk}} of 4, while the second highest valence band is located midway between the Γ\Gamma and K points (Σ\Sigma line), which possesses NvkN_{\mathrm{vk}} of 12. In contrast, the electronic structure of zinc blende AgBr (F4ˉ3mF\bar{4}3m, No. 216), illustrated in Figure 1(c), differs significantly from that of rock-salt structure. In this structure, the VBM is located at the Γ\Gamma point (Nvk=1N_{\mathrm{vk}}=1), and the highest-energy valence band exhibits a ‘downhill’ dispersion. The high NvkN_{\mathrm{vk}} can be directly visualized by the Fermi surface; there are 8 hole pockets at the L point for rock-salt AgBr, each shared with another BZ. Conversely, in the zinc blende structure, only one pocket exists at the zone center of the first BZ, as shown in the insets of Figure 1(b) and Figure 1(d). This phenomenon can be attributed to the prohibition of pp-dd orbital coupling at the Γ\Gamma point within the rock-salt structure, arising from the inverse symmetry of the octahedral crystal field, while the tetrahedral crystal field in zinc blende structure, which lacks inverse symmetry, permits pp-dd coupling at the Γ\Gamma point [24, 48]. However, this explanation is incomplete; other symmetry operations within the space group must also be considered.

Figure 1. (a-b) The crystal structures, orbital-electronic structures with irreps., -COHP, and MO diagrams at the Γ\Gamma point of rock-salt AgBr, respectively. (c-d) The crystal structures, orbital-projected electronic structures with irreps., -COHP, and MO diagrams at the Γ\Gamma point of zinc blende AgBr, respectively. Insets in the electronic structures are the Fermi surfaces 50 meV below the Fermi level. The color indicates the contributions from Br-pp and Ag-dd orbitals. Positive -COHP values indicate bonding interactions, while negative -COHP values indicate antibonding interactions.

As shown in the orbital-projected band structures of Figure 1(b) and Figure 1(d), the valence bands of both rock-salt and zinc blende AgBr display a strong pp-dd coupling, due to the high energy of the Ag-dd orbitals and their favorable energy match with Br-pp orbitals [24, 48]. These valence bands are the anti-bonding states formed by the coupling of Ag-dd and Br-pp orbitals because the dd-orbitals of Ag+^+ is fully occupied. This is supported by the COHP analysis, which indicates negative -COHP value within the energy range of -2.5 eV to the Fermi level. It is important to note that the pp-dd orbital coupling exhibits strongly variation along the high-symmetry points in kk-space for both structures. In rock-salt AgBr, Ag-dd and Br-pp orbitals can’t hybridize at the Γ\Gamma point, whereas strong coupling occurs at the L point, leading to an approximate 2 eV energy increase from the Γ\Gamma to the L point. In contrast, for zinc blende AgBr, pp-dd orbital coupling is allowed at all kk points of the first BZ. Consequently, the energy of the highest valence band at the Γ\Gamma point surpasses that at the L point, indicating stronger coupling at the Γ\Gamma point. The pp-dd coupling can be further confirmed by the band-decomposed charge density. As depicted in Figure S1(b) and (c), both Ag and Br exhibit substantial charge density at the L point for rock-salt AgBr, while charge density at the Γ\Gamma point is only associated with Ag. In the zinc blende AgBr, although Br contributes similarly to both the Γ\Gamma and L points, Ag displays a slightly larger contribution to the Γ\Gamma point, as illustrated in Figure S1(e) and (f).

Under the octahedral crystal field of rock-salt AgBr, the dd orbitals of Ag+^+ undergo splitting into higher-energy EgE_g (dz2d_{z^2} and dx2−y2d_{x^2-y^2}) and lower-energy T2gT_{2g} orbitals (dxyd_{xy}, dxzd_{xz}, and dyzd_{yz}). The Ag+^+ cation has 10 dd electrons, and 6 of them occupy the T2gT_{2g} orbitals and the remaining 4 electrons fill the EgE_g orbitals, hence all these antibonding states are fully occupied. Consequently, the band structure at the Γ\Gamma point is formed, as illustrated in Figure 1(b). The irreps. calculated using IRVSP code [49] at the Γ\Gamma and L points are also labeled in Figure 1 (b) and (d). At the Γ\Gamma point of rock-salt AgBr, the top three valence bands originate solely from Br-pp orbitals, forming the Γ4−\Gamma_4^- band representations, while the lower five valence bands originate solely from Ag-dd orbitals, contributing to the formation of the Γ3+\Gamma_3^+ and Γ5+\Gamma_5^+ band representations. Therefore, there is no pp-dd orbital hybridization present at the Γ\Gamma point. At the L point, however, the highest two valence bands correspond to the L3+L_3^+ irrep, and both Br-pp and Ag-dd orbitals have large contribution, as shown in

OrbitalsWKS (qq)BasisIrreps. (pp)ABRs (p@qp@q)EBRs (Γ\Gamma)EBRs (L)
Rock-salt AgBrAg dd4a4adz2,dx2−y2d_{z^2},d_{x^2-y^2}EgE_gEg@4aE_g@4aΓ3+(2)\Gamma_3^+(2)L3+(2)L_3^+(2)
dxy,dxz,dyzd_{xy},d_{xz},d_{yz}T2gT_{2g}T2g@4aT_{2g}@4aΓ5+(3)\Gamma_5^+(3)L1+(1)⊕L3+(2)L_1^+(1)\oplus L_3^+(2)
Br pp4b4bpx,py,pzp_x,p_y,p_zT1uT_{1u}T1u@4bT_{1u}@4bΓ4−(3)\Gamma_4^-(3)L1+(1)⊕L3+(2)L_1^+(1)\oplus L_3^+(2)
Zinc blende AgBrAg dd4d4ddz2,dx2−y2d_{z^2},d_{x^2-y^2}EEE@4dE@4dΓ3(2)\Gamma_3(2)L3(2)L_3(2)
dxy,dxz,dyzd_{xy},d_{xz},d_{yz}T2T_2T2@4dT_2@4dΓ4(3)\Gamma_4(3)L1(1)⊕L3(2)L_1(1)\oplus L_3(2)
Br pp4a4apx,py,pzp_x,p_y,p_zT2T_2T2@4aT_2@4aΓ4(3)\Gamma_4(3)L1(1)⊕L3(2)L_1(1)\oplus L_3(2)

Table 1. The atomic valence-electron band representations (ABRs) of rock-salt AgBr (Fm3ˉmFm\bar{3}m) and zinc blende AgBr (F4ˉ3mF\bar{4}3m), along with the elementary band representations (EBRs) induced by them at the high-symmetry points Γ\Gamma and L. The number in parentheses denotes the dimensionality of the representation.

fig:S2.

Symmetry principles of pp-dd orbital coupling. The molecular orbital (MO) theory states that for atomic orbitals to combine and form MOs, they must adhere to the principles of symmetry matching, energy proximity, and maximum overlap [50, 51, 52, 53, 54]. Among these principles, symmetry matching serves as a prerequisite, which determines whether a MO can be generated, while the other two principles influence the strength of the MOs. The principle of symmetry matching stipulates that in a crystal structure, the band representations induced by different atomic valence-electron band representations (ABRs) must coincide. Only those orbitals that possess matching band

Symmetry principles of p-d orbital coupling

representations are eligible to hybridize and form MOs. The band representations at the Γ\Gamma and L points induced by Br-pp orbitals and Ag-dd orbitals in rock-salt AgBr and zinc blende AgBr are tabulated in Table I. The EBRs induced by Eg@4aE_g@4a, T2g@4aT_{2g}@4a, and T1u@4bT_{1u}@4b ABR at the Γ\Gamma point in rock-salt AgBr are Γ3+\Gamma_3^{+}, Γ5+\Gamma_5^{+} and Γ4−\Gamma_4^{-}, respectively. Due to the absence of common irreps. between Ag-related and Br-related EBRs, the coupling between corresponding Br-pp and Ag-dd orbitals is forbidden by symmetry. This is illustrated in the MO diagram at the Γ\Gamma point, where no bonding interaction occurs between the Br-pp and Ag-dd orbitals, as shown in Figure 1. However, at the L point, the EBRs induced by Eg@4aE_g@4a, T2g@4aT_{2g}@4a, and T1u@4bT_{1u}@4b are L3+L_3^{+}, L1+⊕L3+L_1^{+} \oplus L_3^{+} and L1+⊕L3+L_1^{+} \oplus L_3^{+}, respectively. The Ag-related and Br-related EBRs share the irreps. L1+L_1^{+} and L3+L_3^{+}, indicating that the coupling between Br-pp and Ag-dd orbitals is symmetry-allowed, as observed in the band structure depicted in Figure 1. In summary, at the Γ\Gamma point, the pp and dd orbitals are symmetry-incompatible, preventing pp-dd orbital coupling. In contrast, at the L point, symmetry compatibility between the pp and dd orbitals allows the formation of MOs.

The band structure of zinc blende AgBr can also be elucidated using EBRs. As summarized in Table I, the EBRs induced by E@4dE@4d, T2@4dT_2@4d, and T2@4aT_2@4a at the Γ\Gamma point are Γ3\Gamma_3, Γ4\Gamma_4, and Γ4\Gamma_4, respectively. Therefore, the T2T_2 orbitals of Ag and pp-orbitals of Br exhibit strong coupling at the Γ\Gamma point, while the EgE_g orbitals of Ag do not couple with Br-pp orbitals at this point, as illustrated in Figure S3. At the L point, the EBRs induced by E@4dE@4d, T2@4dT_2@4d, and T2@4aT_2@4a are L3L_3, L1⊕L3L_1 \oplus L_3, and L1⊕L3L_1 \oplus L_3, respectively. The common irrep. L1L_1 and L3L_3 allow the coupling between Ag-dd and Br-pp orbitals, despite the pp-dd coupling at the L point is relatively weak, as shown in Figure S3. Note that in addition to symmetry compatibility, other factors—such as energy alignment—plays important roles in orbital hybridization. The MO diagram at the Γ\Gamma point demonstrates that the Br-pp and Ag-dd orbitals transforming as the T2T_2 representation yield bonding and anti-bonding states, respectively, whereas the Ag-dd orbitals in the EE representation remain non-bonding.

The presence of the inversion center in the octahedron of rock-salt AgBr results in the ABRs of Ag-dd orbitals exhibiting even parity (“g”) and those of Br-pp orbitals displaying odd parity (“u”) at the Γ\Gamma point. This parity opposition leads to the EBRs induced at the Γ\Gamma point being labeled with positive (“+”) and negative (“−”) signs, rendering them incompatible and thereby prohibiting pp-dd coupling at the Γ\Gamma point. Therefore, the determination of pp-dd coupling can be made without the need for irrep. calculations, which facilitates the search for new materials. Note the parity criterion for ABRs discussed here differs from the previous work focusing on the mixing of even and odd angular moment [48]. In contrast, since zinc blende AgBr lacks an inversion center, the potential for pp-dd orbital coupling cannot be assessed solely based on ABRs, thereby necessitating irrep. calculations.

Electronic transport properties of rock-salt and zinc blende AgBr

In order to verify the role played by high NvkN_{\mathrm{vk}} in enhancing PF, we calculate σ\sigma and SS of the rock-salt and zinc blende AgBr, explicitly including electron-phonon coupling, as detailed in the computational method section. As shown in Figure 2(a) and (b), the σ\sigma of both rock-salt and zinc blende AgBr increases with rising hole concentration (nhn_{\mathrm{h}}), which is expected from the Drude model. Conversely, SS declines linearly as nhn_{\mathrm{h}} increasing for both structures. For a given nhn_{\mathrm{h}}, rock-salt AgBr demonstrates higher σ\sigma and SS values at the same time, leading to a higher PF, see Figure 2(c). Notably, the superior PF of rock-salt AgBr is particularly pronounced at elevated nhn_{\mathrm{h}}. The high σ\sigma of rock-salt AgBr is attributed to its high μ\mu, which is associated with a smaller m∗m^{*}, as depicted in Figure 2(c) and (d). The electron-phonon scattering rates near the Fermi level are very similar for both rock-salt and zinc blende AgBr, as shown in Figure 2(e), despite rock-salt AgBr has a higher NvkN_{\mathrm{vk}}. Evidently, the low m∗m^{*} and high SS observed in rock-salt AgBr is due to its high NvkN_{\mathrm{vk}} (Nvk=4N_{\mathrm{vk}}=4), which contributes to a larger md∗m_{\mathrm{d}}^{*}. Overall, these factors make the PF of rock-salt AgBr 2∼32 \sim3 times higher than that of zinc blende AgBr, underscoring the significance of a high NvkN_{\mathrm{vk}}.

Figure 2. (a)–(e) respectively show the variation trends of the conductivity (σ\sigma), Seebeck coefficient (SS), power factor (PF), mobility (μ\mu), and transport effective mass (m∗m^{*}) of rock-salt and zinc blende AgBr with nhn_h, at 300K. (f) shows the variation trend of the electron-phonon scattering rate (1/τ1/\tau) of these two phases with energy, at 300K.

Since AgCl exhibits similar band structures as AgBr, we applied the same approach to compute electron transport properties of the rock-salt and zinc blende AgCl. The results presented in Figures S7 and S8 indicate that rock-salt AgCl has a significantly larger PF than its zinc blende counterpart, further confirming the importance of high NvkN_{\mathrm{vk}} in enhancing PF. In conclusion, when comparing the zinc blende structures of AgCl and AgBr to their rock-salt counterparts, the smaller m∗m^{*} of the rock-salt structures results in higher σ\sigma, while the high NvkN_{\mathrm{vk}} enlarges md∗m_{\mathrm{d}}^{*}, ultimately leading to high PF. Consequently, rock-salt AgCl and AgBr exhibit higher PFs.

High NvkN_{\mathrm{vk}} materials screening. With the ingredients of achieving high PF in mind, we design a screening process based on our analysis to identify new materials with high PF from the Materials Project (www.materialproject.org) [47], as shown in Figure 3. Firstly, we restrict our search to the compounds that have anti-bonding states as their valence bands. Therefore, we focus on the cations likely to form anti-bonding states in the valence band due to pp-dd coupling. These include Ni4+^{4+}, Pd4+^{4+}, Pt4+^{4+}, Cu+^{+}, Ag+^{+}, Au+^{+}, Zn2+^{2+}, Cd2+^{2+}, and Hg2+^{2+}. Notably, Ni4+^{4+}, Pd4+^{4+}, and Pt4+^{4+} possess 6 dd-electrons that fully occupy the T2gT_{2g} orbitals within an octahedral crystal field, while Cu+^{+}, Ag+^{+}, Au+^{+}, Zn2+^{2+}, Cd2+^{2+}, and Hg2+^{2+} have 10 dd-electrons, which completely occupy all the dd orbitals. The effective EBR at the Γ\Gamma point are then determined by combining the POS2ABR program with our homemade CEEBR (Common Elements of EBR) code. For compounds displaying forbidden pp-dd coupling at the Γ\Gamma point, band structure calculations are conducted to identify the value of NvkN_{\mathrm{vk}}. Transport properties of all compounds with NvkN_{\mathrm{vk}} (within 50 meV below the Fermi level) greater than 6 are calculated using the BolzTraP2 code [55], without including the electron relaxation time (τ\tau). Subsequently, the PF of the compounds exhibiting high S2/m∗S^{2}/m^{*} (>3000 μVm−1K−2> 3000\ \mu\mathrm{V}\mathrm{m}^{-1}\mathrm{K}^{-2}) are computed using the electron-phonon coupling approach. To streamline our search, we focus exclusively on compounds that contain no more than 3 elements and fewer than 12 atoms per primitive unit cell. Given that the low symmetry space group tend to exhibit low NvkN_{\mathrm{vk}}, even when the VBM is located at the boundary of the BZ, we concentrate our study on space group above the tetragonal system (space group number >142> 142).

Figure 3. Screening flow chart of materials.

Our results are summarized in Table II and Table III. For the compounds listed in Table II, the EBRs induced by cation-dd orbitals carry a “+” sign, indicating spatial inversion symmetry, while those induced by anion-pp orbitals carry a “−” sign, reflecting spatial inversion anti-symmetry. Since even and odd parity cannot mix, it follows that pp-dd coupling is forbidden at the Γ\Gamma point for all energy bands of these compounds. The values of NvkN_{\mathrm{vk}} obtained from the search are listed in Table II, and the orbital-projected electronic structures are illustrated in Figures S9-S12. Additionally, all compounds exhibit high NvkN_{\mathrm{vk}} values for their VBM. For example, the NvkN_{\mathrm{vk}} of Ag3SI, NbAgO3, and AgTaO3 with space group 221 is as high as 6, and the NvkN_{\mathrm{vk}} value for CdS (with space group 225) is even as high as 12. The NvkN_{\mathrm{vk}} values of other compounds are 3 or 4.

Comp.Space groupEBRs(dd orbitals)EBRs(pp orbitals)NvkN_{\mathrm{vk}}(VBM)NvkN_{\mathrm{vk}}(50meV)NvN_{\mathrm{v}}(50meV)
AgCl221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}336
AgBr221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}336
Cu3_3N221Γ1+⊕Γ3+,Γ2+⊕Γ3+,Γ5+,Γ4+⊕Γ5+\Gamma_{1}^{+}\oplus\Gamma_{3}^{+},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+},\Gamma_{5}^{+},\Gamma_{4}^{+}\oplus\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}4412
Ag3_3SI221Γ1+⊕Γ3+,Γ2+⊕Γ3+,Γ5+,Γ4+⊕Γ5+\Gamma_{1}^{+}\oplus\Gamma_{3}^{+},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+},\Gamma_{5}^{+},\Gamma_{4}^{+}\oplus\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}6612
KZnF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
KCdF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
RbCdF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
RbHgF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
CsCdF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
CsCdCl3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
CsCdBr3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
CsHgF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
ZnAgF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
MgAgF3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}6918
Mg3_3ZnO4_4221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
Mg3_3CdO4_4221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}41014
NbAgO3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}666
TaAgO3_3221Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−,Γ4−⊕Γ5−\Gamma_{4}^{-},\Gamma_{4}^{-}\oplus\Gamma_{5}^{-}666
CuCl225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
CuBr225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
AgCl225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
AgBr225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
AgI225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
ZnO225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}448
CdS225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−\Gamma_{4}^{-}121620

Table II. Compounds with absolutely forbidden pp-dd orbital coupling at the Γ\Gamma point, together with the EBRs at the Γ\Gamma point induced by their dd and pp orbitals, the NvkN_{\mathrm{vk}} of the VBM, and both the NvkN_{\mathrm{vk}} and NvN_{\mathrm{v}} within 50 meV below the Fermi level.

Comp.Space groupEBRs(dd orbitals)EBRs/BRs(pp orbitals)Irrep.NvkN_{\mathrm{vk}}(VBM)NvkN_{\mathrm{vk}}(50meV)NvN_{\mathrm{v}}(50meV)
NiO2_2164Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}61212
PtS2_2164Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}61818
PtSe2_2164Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}61212
NiO2_2166Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}61212
ScAgO2_2166Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ3−\Gamma_{3}^{-}333
ErAgS2_2166Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ2−,Γ3−,Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{2}^{-},\Gamma_{3}^{-},\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}678
TmAgS2_2166Γ1+,Γ3+\Gamma_{1}^{+},\Gamma_{3}^{+}Γ2−,Γ3−,Γ1+⊕Γ2−,Γ3+⊕Γ3−\Gamma_{2}^{-},\Gamma_{3}^{-},\Gamma_{1}^{+}\oplus\Gamma_{2}^{-},\Gamma_{3}^{+}\oplus\Gamma_{3}^{-}Γ2−\Gamma_{2}^{-}678
PtP2_2205Γ1+⊕Γ4+,Γ2+⊕Γ3+⊕Γ4+\Gamma_{1}^{+}\oplus\Gamma_{4}^{+},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+}\oplus\Gamma_{4}^{+}Γ1+⊕Γ1−⊕Γ4+⊕Γ4−,Γ2+⊕Γ3+⊕Γ2−⊕Γ3−⊕2Γ4+⊕2Γ4−\Gamma_{1}^{+}\oplus\Gamma_{1}^{-}\oplus\Gamma_{4}^{+}\oplus\Gamma_{4}^{-},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+}\oplus\Gamma_{2}^{-}\oplus\Gamma_{3}^{-}\oplus2\Gamma_{4}^{+}\oplus2\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}121212
PtAs2_2205Γ1+⊕Γ4+,Γ2+⊕Γ3+⊕Γ4+\Gamma_{1}^{+}\oplus\Gamma_{4}^{+},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+}\oplus\Gamma_{4}^{+}Γ1+⊕Γ1−⊕Γ4+⊕Γ4−,Γ2+⊕Γ3+⊕Γ2−⊕Γ3−⊕2Γ4+⊕2Γ4−\Gamma_{1}^{+}\oplus\Gamma_{1}^{-}\oplus\Gamma_{4}^{+}\oplus\Gamma_{4}^{-},\Gamma_{2}^{+}\oplus\Gamma_{3}^{+}\oplus\Gamma_{2}^{-}\oplus\Gamma_{3}^{-}\oplus2\Gamma_{4}^{+}\oplus2\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}121212
Ca2_2AuAs225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Ca2_2AuSb225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Sr2_2AuAs225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Sr2_2AuSb225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Sr2_2AuBi225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Yb2_2AuAs225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444
Yb2_2AuSb225Γ3+,Γ5+\Gamma_{3}^{+},\Gamma_{5}^{+}Γ4−⊕Γ5+,Γ4−\Gamma_{4}^{-}\oplus\Gamma_{5}^{+},\Gamma_{4}^{-}Γ4−\Gamma_{4}^{-}444

Table III. Compounds with forbidden pp-dd orbital coupling at the Γ\Gamma point for the highest valence band, together with the EBRs at the Γ\Gamma point induced by their dd orbitals, the BRs at the Γ\Gamma point induced by their pp orbitals, the irrep. of the highest valence band calculated by the Irvsp, the NvkN_{\mathrm{vk}} of the VBM, and both the NvkN_{\mathrm{vk}} and NvN_{\mathrm{v}} within 50 meV below the Fermi level.

The compounds listed in Table III belong to a different category, wherein pp-dd orbital coupling is not completely forbidden for all energy bands at the Γ\Gamma point but is specifically prohibited at the Γ\Gamma point of the highest valence band. Take PtP₂ with space group 205 as an example. At the Γ\Gamma point, the EBRs induced by Pt-dd orbitals is Γ1+⊕Γ4+\Gamma_{1}^{+} \oplus\Gamma_{4}^{+}, Γ2+Γ3+⊕Γ4+\Gamma_{2}^{+}\Gamma_{3}^{+} \oplus\Gamma_{4}^{+}, while the BRs induced by P-pp orbitals are Γ1+⊕Γ1−⊕Γ4+⊕Γ4−\Gamma_{1}^{+} \oplus\Gamma_{1}^{-} \oplus\Gamma_{4}^{+} \oplus\Gamma_{4}^{-} and Γ2+Γ3+⊕Γ2−Γ3−⊕2Γ4+⊕2Γ4−\Gamma_{2}^{+}\Gamma_{3}^{+} \oplus\Gamma_{2}^{-}\Gamma_{3}^{-} \oplus2\Gamma_{4}^{+} \oplus2\Gamma_{4}^{-}. Due to the overlap of these two sets of EBRs or BRs in certain irreps., an analysis based solely on EBRs or BRs cannot unambiguously establish whether pp-dd orbital coupling occurs. Our IRVSP calculations show that the irrep. at the Γ\Gamma point of the highest valence band is Γ4−\Gamma_{4}^{-}, indicating that this point can only be attributed from As-pp orbitals, and thus pp-dd orbital coupling is symmetrically prohibited. The EBRs or BRs at the Γ\Gamma point, along with valley degeneracy and corresponding orbital-projected electronic structures of these materials, are summarized in Table III and illustrated in Figures S13 and S14. Among them, for PtS₂ and PtSe₂ with space group P3ˉm1P\bar{3}m1 (No. 164), as well as TmAgS₂ and ErAgS₂ with space group R3ˉmR\bar{3}m (No. 166), the NvkN_{\mathrm{vk}} reaches a value of 6. In contrast, PtP₂ and PtAs₂, which also belong to space group 205, exhibit an even higher NvkN_{\mathrm{vk}} of 12.

Subsequently, we calculated S2/m∗S^{2}/m^{*} at nh=1×1019 cm−3n_{\mathrm{h}} = 1 \times10^{19}\ \mathrm{cm}^{-3} for the compounds listed in Table II and Table III with Nvk≥6N_{\mathrm{vk}} \ge6 within 50 meV below the Fermi level. The optimal values of S2/m∗S^{2}/m^{*}, along with the corresponding SS, m∗m^{*}, and TT, are presented in Table S1. Compounds exhibiting S2/m∗≥3000 μV2m−1K−2S^{2}/m^{*} \ge3000\ \mu\mathrm{V}^{2}\mathrm{m}^{-1}\mathrm{K}^{-2} include PtP₂, CdS, ErAgS₂, TmAgS₂, Ag₃SI, and PtS₂. Due to the presence of imaginary frequencies in CdS, ErAgS₂, TmAgS₂, and Ag₃SI at 0 K, electron-phonon coupling calculations are not feasible for these compounds. Therefore, we next calculated the PF of PtP₂, PtAs₂, and PtS₂ using the electron-phonon coupling method.

Electronic transport properties of PtP₂ and PtS₂. The crystal structures, orbital-projected electronic structures, and Fermi surfaces of PtP₂ (space group Pa3ˉPa\bar{3}, No. 205) and PtS₂ (space group P3ˉm1P\bar{3}m1, No. 164) are shown in Figure 4. PtP₂ and PtS₂ belong to the cubic and trigonal crystal systems, respectively, with the Pt⁴⁺ cation coordinated in an octahedral geometry by six P²⁻ or six S²⁻ anions. The presence of P-P bond in PtP₂ leads to (P₂)⁴⁻ or effectively P²⁻ anion. Notably, the P-Pt-P (or S-Pt-S) bond angles of both octahedra are distorted away from 180°. As illustrated in Figure 4(b) and (Figure 4e), both PtP₂ and PtS₂ are indirect bandgap semiconductors.

Crystal structures, orbital-projected electronic structures, and Fermi surfaces of PtP₂ and PtS₂

Figure 4. (a–c) Crystal structure, orbital-projected electronic structure, and Fermi surface 10 meV below the Fermi level of PtP₂ with space group No. 205, respectively. (d–f) Crystal structure, orbital-projected electronic structure, and Fermi surface 10 meV below the Fermi level of PtS₂ with space group No. 164, respectively.

The VBM of PtP2_2 is located between the Γ\Gamma and M points (the Σ\Sigma line), while that of PtS2_2 lies between the Γ\Gamma and K points (Λ\Lambda line). At the VBM, PtP2_2 exhibits 12 hole pockets, whereas PtS2_2 has 6, as shown in Figure 4(c) and (f), corresponding to a NvkN_{\mathrm{vk}} of 12 and 6, respectively. It is noteworthy that the Γ\Gamma-K direction where the VBM of PtS2_2 is located is an in-plane direction, which typically leads to superior properties in the in-plane orientation.

The electronic transport properties and the electron-phonon scattering rate (1/τ1/\tau) of PtP2_2 are shown in Figure 5. The σ\sigma of PtP2_2 increases with rising nhn_h and decreases with increasing TT, while the SS exhibits the opposite tend, decreasing with increasing nhn_h and increasing with increasing TT. These trends in σ\sigma and SS are consistent with those observed in rock-salt and zinc blende AgBr, as discussed earlier. Notably, at 300 K and an nhn_h of 1×10191 \times10^{19} cm−3^{-3}, the σ\sigma of PtP2_2 is two orders of magnitude greater than that of rock-salt AgBr. This disparity can be attributed to the facts that the m∗m^* of PtP2_2 is approximately 3 times smaller than that of rock-salt AgBr, and 1/τ1/\tau is more than one order of magnitude lower, see Figure 2(f) and Figure 5(f). The SS of PtP2_2 is approximately half that of rock-salt AgBr, as its extremely small m∗m^* limits the SS, despite the higher NvkN_{\mathrm{vk}} value of PtP2_2 relative to rock-salt AgBr. Due to the opposite dependence of σ\sigma and SS on carrier concentration, the PFPF exhibits an inverted parabolic shape with respect to carrier concentration, initially increasing before decreasing, as illustrated in Figure 5(c). At 300 K, the PFPF of PtP2_2 reaches a maximum value (PFmax⁡PF_{\max}) of 130 μ\muW cm−1^{-1} K−2^{-2} at an nhn_h of 4×10194 \times10^{19} cm−3^{-3}, while at 800 K, the PFmax⁡PF_{\max} of 82 μ\muW cm−1^{-1} K−2^{-2} is achieved at nhn_h of 2×10202 \times10^{20} cm−3^{-3}. The outstanding PFPF of PtP2_2 stems from its small m∗m^* and high μ\mu (see Figure 5(d) and (e)), which lead to high σ\sigma, and its high NvkN_{\mathrm{vk}}, which ensures a relatively high SS.

Figure 5. The electronic transport properties, transport effective mass, and electron-phonon scattering rate of the Ia3ˉ\bar{3} phase of PtP2_2. (a)-(e) The variation trends of σ\sigma, SS, PFPF, μ\mu, and m∗m^* of the Ia3ˉ\bar{3} phase of PtP2_2 with nhn_h at different TT, respectively. (f) The variation trend of the 1/τ1/\tau of the Ia3ˉ\bar{3} phase of the PtP2_2 with energy at different TT.

For the isoelectrical compound PtAs2_2, the PFmax⁡PF_{\max} value at 300 K and 800 K are 127 μ\muW cm−1^{-1} K−2^{-2} and 73 μ\muW cm−1^{-1} K−2^{-2}, respectively (see Figure S15). In the case of trigonal PtS2_2, the in-place PFmax⁡PF_{\max} is 82 μ\muW cm−1^{-1} K−2^{-2} at 300 K and 64 μ\muW cm−1^{-1} K−2^{-2} at 800K (see Figure S16). These PFPF values are approximately 3 ∼ 5 times higher than those of high-ZT materials, such as SnSe [56], and even exceed that of NbFeSb (106 μ\muW cm−1^{-1} K−2^{-2} at room temperature) [57], which is known to exhibit the highest PFPF among experimentally measured semiconductors. To validate our calculations, we also compute the electrical transport properties of pp-type half-Heusler NbFeSb using the same methodology. Our calculations indicate that NbFeSb exhibits an optimal PFPF of approximately 90 μ\muW cm−1^{-1} K−2^{-2} at 300 K, as illustrated in Figure S17. The good agreement between our calculated value, experimental date [57], and a previous theoretical value [58] supports the reliability of our computational approach.

In summary, we propose a novel strategy of designing pp-type semiconductors with high valley degeneracy and high power factor, based on molecular orbital theory and group theory. For compounds exhibiting strong pp-dd or bital coupling, the absence of certain common symmetry elements in the elementary band representations—arising from anion-pp and cation-dd orbitals at the Brillouin zone center—gives rise to low-energy non-bonding states. Conversely, symmetry-allowed pp-dd anti-bonding interactions at other kk-points raise the energy of the valence band maximum, shifting it from the Γ\Gamma to kk-points near the zone boundaries. This shift effectively increases NvkN_{\mathrm{vk}}, leading to a significant enhancement in PF. Combining first-principles calculations with symmetry analysis based on group theory, we systematically explored 921 binary and ternary semiconductors from the Materials Project, and identified 41 compounds with Nvk≥3N_{\mathrm{vk}} \geq3 and 7 compounds with Nvk≥6N_{\mathrm{vk}} \geq6 that exhibit high S2/m∗S^2/m^*. High-accuracy DFT calculations, which fully account for electron-phonon coupling, demonstrate that PtP2_2 (Nvk=12N_{\mathrm{vk}} = 12), PtAs2_2 (Nvk=12N_{\mathrm{vk}} = 12), and PtS2_2 (Nvk=18N_{\mathrm{vk}} = 18) exhibit maximum PF of 130, 127, and 82 μ\muWcm−1^{-1}K−2^{-2} at 300K, respectively. These values are three to five times higher than those of well-studied TE materials and even exceed that of NbFeSb, which possesses the highest PF among known semiconductors. Our results not only elucidate the fundamental mechanisms governing orbital coupling in solids with pp-dd coupling but also establish a universal framework for efficiently screening pp-type semiconductors with high NvkN_{\mathrm{vk}} through symmetry analysis. By integrating group theory with computational materials screening, this work provides a clear pathway for the rational design of next-generation high-performance thermoelectric materials.

Computational methods

The transport effective mass [59] is defined as m∗(T,ϵ)=e2τσ(T,ϵ)n(T,ϵ)m^*(T,\epsilon) = \frac{e^2\tau}{\sigma(T,\epsilon)}n(T,\epsilon), where ee, τ\tau, and ϵ\epsilon denote the electron charge, relaxation time, and electron chemical potential, respectively. The values of SS and σ/τ\sigma/\tau were calculated using BoltzTraP2 [55], based on density functional theory (DFT) calculations performed with the Vienna ab initio simulation package (VASP) [60, 61]. The PBE functional and a plane-wave basis set with a cut-off energy of 520 eV were adopted. For all self-consistent calculations, a convergence criterion of 10−810^{-8} eV was applied. The Γ\Gamma-centered kk-point grid was designed to be sufficiently dense to ensure accurate sampling of the BZ. The crystal orbital Hamilton population (COHP) and irreducible representations (irreps.) were computed using the LOBSTER [62] and IRVSP codes [49], respectively, both of which rely on the output of self-consistent calculations. The crystal structure and Fermi surface were visualized using VESTA [63] and Fermi surfer [64], respectively.

Electron structures, phonon dispersions, and electron-phonon matrix elements were calculated using the Perdew-Burke-Ernzerhof (PBE) exchange-correlation functional and Rabe-Rappe-Kaxiras-Joannopoulos (RRKJ) ultrasoft pseudopotential [66], as implemented in the Quantum Espresso (QE) package [67, 68, 69]. The plane-wave kinetic energy cutoff, BZ kk-points grid, and the qq-points grid are summarized in Table S2. The Wannier90 [70] code was employed to obtain maximally localized Wannier functions. The electron transport properties, including σ\sigma, SS, mobility (μ\mu), and electron-phonon scattering rate (1/τ1/\tau) were calculated by solving the Boltzmann transport equation (BTE) within the framework of the iterative approach (ITA), as implemented in the PERTURBO [71] code. Detailed information regarding the fine BZ grids utilized for both kk-points and qq-points is also provided in Table S2.

Data availability

The data generated in this study is provided in the Source Data file. Source data are provided with this paper.

Code availability

The in-house code CEEBR is available for download at https://github.com/.

Acknowledgement

We would like to acknowledge Zhijun Wang for insightful discussions. We acknowledge the support received from the Fundamental Research Funds for the Central Universities of China (USTB) and the National Natural Science Foundation of China (Grant No. 12304115). We also appreciate the computing resources provided by the USTB MatCom at the Beijing Advanced Innovation Center for Materials Genome Engineering.

Author contribution

J.H. conceived and supervised the project. W.X., assisted by Z.H. and Z.X., performed materials screening and electronic transport calculations. W.X. and Z.Y. conducted symmetry analysis, and all authors participated in data interpretation. The manuscript was collaboratively written and reviewed by all authors.

Competing interests

The authors declare no competing interests.

Additional information

Supplementary information is available in the online version of the paper. Competing interests: The authors declare no competing financial interests.

References

  1. [1]H. J. Goldsmid et al., Introduction to thermoelectricity, Vol. 121 (Springer, 2010).
  2. [2]C. Uher, Materials aspect of thermoelectricity (CRC press, 2016).
  3. [3]J. P. Heremans, V. Jovovic, E. S. Toberer, A. Saramat, K. Kurosaki, A. Charoenphakdee, S. Yamanaka, and G. J. Snyder, Science 321, 554 (2008).
  4. [4]T. Jia, J. Carrete, G. K. H. Madsen, Y. Zhang, and S.-H. Wei, Phys. Rev. B 105, 245203 (2022).
  5. [5]Y. Qin, B. Qin, D. Wang, C. Chang, and L.-D. Zhao, Energy Environ. Sci. 15, 4527 (2022).
  6. [6]Z. Han, J. Wang, C. Zhang, Z. Xia, and J. He, Inorganic Chemistry 64, 8040 (2025).
  7. [7]S. Shittu, G. Li, X. Zhao, and X. Ma, Applied Energy 268, 115075 (2020).
  8. [8]W. G. Zeier, Current Opinion in Green and Sustainable Chemistry 4, 23 (2017).
  9. [9]Q. Zhang, Y. Sun, W. Xu, and D. Zhu, Advanced Materials 26, 6829 (2014).
  10. [10]N. W. Ashcroft and N. D. Mermin, Solid State Physics (Philadelphia: Saunders College, 1979).
  11. [11]T. M. Tritt, Thermal Conductivity: Theory, Properties, and Applications (Springer New York, 2004).
  12. [12]J. Mao, Z. Liu, J. Zhou, H. Zhu, Q. Zhang, G. Chen, and Z. R. S. J. Mao, Advances in physics 67, 69 (2018).
  13. [13]Z. Liu, J. Mao, T. H. Liu, G. Chen, and Z. Ren, Mrs Bulletin 43, 181 (2018).
  14. [14]B. Poudel, Q. Hao, Y. Ma, Y. Lan, A. Minnich, B. Yu, X. Yan, D. Wang, A. Muto, and D. Vashaee, Science 320, 634 (2008).
  15. [15]K. F. Hsu, S. Loo, F. Guo, W. Chen, J. S. Dyck, C. Uher, T. Hogan, E. K. Polychroniadis, and M. G. Kanatzidis, Science 303, 818 (2004).
  16. [16]K. Biswas, J. He, I. D. Blum, C. I. Wu, T. P. Hogan, D. N. Seidman, V. P. Dravid, and M. G. Kanatzidis, Nature 489, 414 (2012).
  17. [17]B. Poudel, Q. Hao, Y. Ma, Y. Lan, A. Minnich, B. Yu, X. Yan, D. Wang, A. Muto, D. Vashaee, X. Chen, J. Liu, M. S. Dresselhaus, G. Chen, and Z. Ren, Science 320, 634 (2008).
  18. [18]A. I. Hochbaum, R. Chen, R. D. Delgado, W. Liang, E. C. G. Naret, M. Najarian, A. Majumdar, and P. Yang, Nature 39, 163 (2008).
  19. [19]E. J. Skoug and D. T. Morelli, Phys. Rev. Lett. 107, 235901 (2011).
  20. [20]M. D. Nielsen, V. Ozolins, and J. P. Heremans, Energy Environmental ence 6, 570 (2013).
  21. [21]T. Tadano, Y. Gohda, and S. Tsuneyuki, Physical Review Letters 114, 095501.1 (2015).
  22. [22]J. He, M. Amsler, Y. Xia, S. S. Naghavi, V. I. Hegde, S. Hao, S. Goedecker, V. Ozolins, and C. Wolverton, Phys. Rev. Lett. 117, 046602 (2016).
  23. [23]Y. Zhu, B. Wei, J. Liu, N. Z. Koocher, and J. Hong, Materials Today Physics 19, 100428 (2021).
  24. [24]J. He, Y. Xia, W. Lin, K. Pal, Y. Zhu, M. G. Kanatzidis, and C. Wolverton, Advanced Functional Materials 32, 2108532 (2022).
  25. [25]Z. Xia, X. Shen, J. Zhou, Y. Huang, Y. Yang, J. He, and Y. Xia, Advanced Science 12, 2417292 (2025).
  26. [26]J. He, Y. Xia, S. S. Naghavi, V. Ozoliņš, and C. Wolverton, Nature communications 10, 719 (2019).
  27. [27]D. Narducci, Applied Physics Letters 99, 102104 (2011).
  28. [28]G. J. Snyder and E. S. Toberer, Nature Materials 7, 105 (2008).
  29. [29]R. Moshwan, W.-D. Liu, X.-L. Shi, Y.-P. Wang, J. Zou, and Z.-G. Chen, Nano Energy 65, 104056 (2019).
  30. [30]X. Tan, L. Wang, H. Shao, S. Yue, J. Xu, G. Liu, H. Jiang, and J. Jiang, Advanced Energy Materials 7, 1700076 (2017).
  31. [31]Z. Long, Y. Wang, X. Sun, Y. Li, Z. Zeng, L. Zhang, and H. Chen, Advanced Materials 35, 2210345 (2023).
  32. [32]Y. Pei, H. Wang, and G. J. Snyder, Advanced Materials 24, 6124 (2012).
  33. [33]H.-S. Kim, N. A. Heinz, Z. M. Gibbs, Y. Tang, S. D. Kang, and G. J. Snyder, Materials Today 20, 452 (2017).
  34. [34]A. Zevalkink, D. M. Smiadak, J. L. Blackburn, A. J. Ferguson, M. L. Chabinyc, O. Delaire, J. Wang, K. Kovnir, J. Martin, L. T. Schelhas, T. D. Sparks, S. D. Kang, M. T. Dylla, G. J. Snyder, B. R. Ortiz, and E. S. Toberer, Applied Physics Reviews 5, 021303 (2018).
  35. [35]K. Kōmoto and T. Mori, Thermoelectric Nanomaterials: Materials Design and Applications (Springer, 2013).
  36. [36]X.-J. Wang, M.-B. Tang, H.-H. Chen, X.-X. Yang, J.-T. Zhao, U. Burkhardt, and Y. Grin, Applied Physics Letters 94, 092106 (2009).
  37. [37]Z.-Z. Luo, S. Cai, S. Hao, T. P. Bailey, I. Spanopoulos, Y. Luo, J. Xu, C. Uher, C. Wolverton, V. P. David, Q. Yan, and M. G. Kanatzidis, Angewandte Chemie International Edition 60, 268 (2021).
  38. [38]K. H. Lee, S.-i. Kim, H.-S. Kim, and S. W. Kim, ACS Applied Energy Materials 3, 2214 (2020).
  39. [39]C. Fu, T. Zhu, Y. Pei, H. Xie, H. Wang, G. J. Snyder, Y. Liu, Y. Liu, and X. Zhao, Advanced Energy Materials 4, 1400600 (2014).
  40. [40]Y. Feng, J. Li, Y. Li, T. Ding, C. Zhang, L. Hu, F. Liu, W. Ao, and C. Zhang, J. Mater. Chem. A 8, 11370 (2020).
  41. [41]Y. Pei, X. Shi, LaLonde, Aaron, H. Wang, L. Chen, Snyder, and G. Jeffrey, Nature (2011), 10.1038/nature09996.
  42. [42]W. Liu, X. Tan, K. Yin, H. Liu, X. Tang, J. Shi, Q. Zhang, and C. Uher, Phys. Rev. Lett. 108, 166601 (2012).
  43. [43]R. Hoffmann, Angewandte Chemie International Edition in English 26, 846 (1987).
  44. [44]W. G. Zeier, A. Zevalkink, Z. M. Gibbs, G. Hautier, M. G. Kanatzidis, and G. J. Snyder, Angewandte Chemie International Edition 55, 6826 (2016).
  45. [45]S.-H. Wei and A. Zunger, Phys. Rev. B 55, 13605 (1997).
  46. [46]T. Fang, X. Li, C. Hu, Q. Zhang, J. Yang, W. Zhang, X. Zhao, D. J. Singh, and T. Zhu, Advanced Functional Materials 29, 1900677 (2019).
  47. [47]A. Jain, S. P. Ong, G. Hautier, W. Chen, W. D. Richards, S. Dacek, S. Cholia, D. Gunter, M. Skinner, G. Ceder, and K. A. Persson, APL Materials 1, 011002 (2013).
  48. [48]S.-H. Wei and A. Zunger, Phys. Rev. B 37, 8958 (1988).
  49. [49]J. Gao, Q. Wu, C. Persson, and Z. Wang, Computer Physics Communications 261, 107760 (2021).
  50. [50]R. S. Mulliken, Phys. Rev. 32, 186 (1928).
  51. [51]F. Hund, Zeitschrift für Physik 40, 742 (1927).
  52. [52]E. Hückel, Zeitschrift für Physik 76, 628 (1932).
  53. [53]J. E. Lennard-Jones, Transactions of the Faraday Society 25, 668 (1929).
  54. [54]Q. B. Zum Bezolproblem and Q. B. zum Problem, Zeitschrift Fuer Physikalische Chemie 70, 204 (1931).
  55. [55]G. K. H. Madsen, J. Carrete, and M. J. Verstraete, Computer Physics Communications, S0010465518301632 (2017).
  56. [56]L.-D. Zhao, G. Tan, S. Hao, J. He, Y. Pei, H. Chi, H. Wang, S. Gong, H. Xu, V. P. Dravid, C. Uher, G. J. Snyder, C. Wolverton, and M. G. Kanatzidis, Science 351, 141 (2016).
  57. [57]R. He, D. Kraemer, J. Mao, L. Zeng, Q. Jie, Y. Lan, C. Li, J. Shuai, H. S. Kim, Y. Liu, D. Broido, C.-W. Chu, G. Chen, and Z. Ren, Proceedings of the National Academy of Sciences 113, 13576 (2016).
  58. [58]J. Zhou, H. Zhu, T.-H. Liu, Q. Song, R. He, J. Mao, Z. Liu, W. Ren, B. Liao, D. J. Singh, et al., Nature communications 9, 1721 (2018).
  59. [59]Z. M. Gibbs, F. Ricci, G. Li, H. Zhu, K. Persson, G. Ceder, G. Hautier, A. Jain, and G. J. Snyder, npj Computational Materials 3, 8 (2017).
  60. [60]G. Kresse and J. Furthmüller, Phys. Rev. B 54, 11169 (1996).
  61. [61]G. Kresse and J. Furthmüller, Comput. Mater. Sci. 6, 15 (1996).
  62. [62]S. Maintz, V. L. Deringer, A. L. Tchougréeff, and R. Dronskowski, Journal of Computational Chemistry 37 (2016), 10.1002/jcc.24300.
  63. [63]K. Momma and F. Izumi, Journal of Applied Crystallography 44, 1272 (2011).
  64. [64]M. Kawamura, Computer Physics Communications 239, 197 (2019).
  65. [66]A. M. Rappe, K. M. Rabe, E. Kaxiras, and J. D. Joannopoulos, Phys. Rev. B 41, 1227 (1990).
  66. [67]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, and I. Dabo, J Phys Condens Matter 21, 395502 (2009).
  67. [68]P. Giannozzi, O. Basseggio, P. Bonfà, D. Brunato, R. Car, I. Carnimeo, C. Cavazzoni, S. de Gironcoli, P. Delugas, F. Ferrari Ruffino, A. Ferretti, N. Marzari, I. Timrov, A. Urru, and S. Baroni, The Journal of Chemical Physics 152, 154105 (2020).
  68. [69]P. Giannozzi, O. Andreussi, T. Brumme, O. Bunau, M. B. Nardelli, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, M. Cococcioni, et al., Journal of physics: Condensed matter 29, 465901 (2017).
  69. [70]A. A. Mostofi, J. R. Yates, Y.-S. Lee, I. Souza, D. Vanderbilt, and N. Marzari, Computer Physics Communications 178, 685 (2008).
  70. [71]J.-J. Zhou, J. Park, I.-T. Lu, I. Maliyo, X. Tong, and M. Bernardi, Computer Physics Communications 264, 107970 (2021)

Paper details

vlnc:W_4dat5j37
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents