betaFeedback

WorksPhysics and Astronomy

Epitaxial integration of GaN μμ-platelets and thin films on metallic TiN using a hybrid approach

Abstract

We demonstrate the synthesis of epitaxial, self-organized GaN μμ-platelets on metallic TiN thin films. To this end, we first nucleate self-assembled GaN nanowires with number densities between 0.01 to 300 μm−2μm^{-2} by molecular beam epitaxy. Subsequent overgrowth of these seed nanowires by metal-organic vapor phase epitaxy yields GaN μμ-platelets with corresponding number densities. The platelets exhibit N-polarity and form an ohmic contact to the metallic TiN substrate. By adjusting the growth conditions during the metal-organic vapor phase epitaxy, particularly the carrier gas and precursor ratio, the morphology of the GaN can be controlled across a broad range. Growth under N2_{2} carrier gas and with a 1:1 NH3_{3}/trimethylgallium precursor flow ratio results in platelet ensembles with broad diameter and height distributions. In contrast, employing an N2_{2}/H2_{2} carrier gas mixture promotes the formation of more homogeneous ensembles with narrower size distributions around a diameter of ≈\approx2 μmμm. Finally, N-rich growth conditions under H2_{2} carrier gas enhance lateral growth, leading to the formation of coalesced GaN layers. GaN grown under these latter conditions exhibits strong near-band-edge emission, accompanied by only weak deep-level luminescence at room temperature.

Introduction

Group-III nitrides, particularly GaN, are the dominant semiconductor materials in solid-state lighting[1, 2] and are becoming increasingly important for power electronics.[3, 4] Currently, common III-nitride devices such as light-emitting diodes (LEDs) and high electron-mobility transistors (HEMTs) are typically based on quasi-vertical and lateral architectures, respectively. A fully vertical architecture, in contrast, uses a conductive substrate as the bottom electrode, thus enabling direct vertical current conduction through the active region of a device. This design offers several advantages over conventional lateral architectures, including superior current spreading, improved heat dissipation, reduced series resistance, and potentially higher integration density.[5, 6, 7, 8] Despite these benefits, vertical III-nitride-based devices remain relatively scarce.

The limited vertical integration of III-nitrides likely stems from two main challenges. First, bulk GaN substrates are still mainly available on a small scale and at high cost. Second, while heteroepitaxy of GaN on large and cost-effective substrates such as sapphire and Si is nowadays widely established, neither substrate offers a straightforward pathway towards vertical GaN-based devices. Due to its electrically insulating nature, sapphire prevents any vertical current transport through the substrate. Growth on Si, on the other hand, generally requires an insulating buffer layer such as AlN to suppress the reaction between Ga and Si known as meltback etching. Consequently, fabricating vertical devices from heterostructures grown on Si demands additional and complex processing steps, such as layer transfer or etching through both the Si substrate and the insulating buffer layer to establish an electrical backside contact.[6]

An interesting alternative to classical semiconducting substrates are metallic thin films, exhibiting orders of magnitude higher electrical conductivity, as displayed in Figure 1. Furthermore, they can be deposited on low-cost substrates of any size, thus presenting a cost-efficient, scalable approach. In optoelectronic applications, a metallic substrate can additionally serve as a back reflector, potentially enhancing light extraction by reflecting photons emitted towards the metal layer back to the top surface.

Figure 1. Electrical conductivity of possible substrate materials for III-nitride growth, plotted against their thermal stability limit TstabT_{\mathrm{stab}}, i. e., their melting point (filled symbols) or sublimation temperature (open symbols). Materials include bulk semiconductors (▲) and insulators (■), as well as thin films of noble metals (●), transition metals (◆) and transition metal nitrides (▼). Electrical conductivity data are taken from Refs. 9–15, values for TstabT_{\mathrm{stab}} are taken from Refs. 15–20.

Yet, classical conductors such as Ag, Cu, Al and Au exhibit relatively low melting points, not suitable for the growth of epitaxial III-nitrides taking place at elevated temperatures (cf. Figure 1). In contrast, transition metals and, especially, their nitrides exhibit an outstanding thermal stability and, at the same time, a high electrical conductivity.

Various refractory metals and transition metal nitrides have been explored as substrates for GaN growth, predominantly by molecular beam epitaxy (MBE). Examples include Ti, Ta and Mo thin films[21, 22] and foils,[23, 24, 25] as well as, more recently, ZnN thin films.[26, 27] However, these studies have focused on the growth of self-assembled GaN nanowires, generally leading to nanowire ensembles with high number densities and, when grown on polycrystalline substrates, often broad distributions of in-plane orientations. Although vertical electrical conduction and even nanowire-based LEDs have been demonstrated using such ensembles,[22, 23, 24, 27] the limited control over nanowire density, morphology and orientation remains a challenge for their integration into other devices.

In our previous works, we have demonstrated the growth of III-nitride nanowires on epitaxial TiN yielding self-assembled GaN[21, 28] and AlN[29, 30] nanowire ensembles with well-defined in-plane orientations. Furthermore, we recently demonstrated precise control over the GaN nucleation process by depositing SiNx_x islands that serve as preferential nucleation sites, allowing the nanowire density to be tuned over several orders of magnitude.[28] Although the integration of bottom-up nanostructures into electronic devices is generally challenging, our TiN-supported III-nitride nanowire ensembles have recently been incorporated into vertical piezoelectric nanogenerators.[31, 32] This demonstration highlights the potential of TiN as an integrated bottom electrode for other III-nitride-based devices.

In contrast to the self-assembled nanowire growth typically obtained by MBE, metal-organic vapor-phase epitaxy (MOVPE) of GaN on TiN has been reported to result in the nucleation of large, μ\mum-sized 3D crystallites, as found in several studies by the group of Murakami.[33, 34, 35, 36] The formation of such islands has been attributed to the poor wetting of GaN on TiN, potentially associated with a high GaN/TiN interfacial energy. Although these 3D crystallites can subsequently be coalesced into GaN layers by lateral overgrowth, the resulting layers exhibit root-mean-square (RMS) surface roughnesses of several hundred nanometers. The deposition of an AlN buffer layer has been recently demonstrated to yield smoother GaN layers on TiN.[37] However, the introduction of such an insulating buffer layer again compromises vertical electrical conduction.

In this work, we combine the advantages of MBE and MOVPE in a hybrid approach that decouples GaN nucleation from subsequent lateral growth. We first employ MBE to nucleate self-assembled nanowires on 200 nm-thick TiN layers, similar to our previous work.[28] These seed nanowires are subsequently overgrown by MOVPE to form both μ\mum-sized GaN platelets and coalesced layers, thereby shifting the growth front from the GaN/TiN interface towards the established GaN surfaces. Such an MBE/MOVPE hybrid approach has been recently introduced by Henriques et al.,[38, 39] but on insulating 300 nm SiO2_2/Si substrates and with patterned graphene patches serving as nucleation sites. Our GaN/TiN heterostructures exhibit an ohmic contact to the metallic TiN layer even after the high-temperature overgrowth, demonstrating that the electrical functionality of the TiN substrate is retained. The μ\mu-platelets are thus promising building blocks for future vertical μ\mu-LED architectures, while coalesced GaN layers could enable novel vertical GaN power devices.

Experimental details

GaN nanowires are grown by MBE at ≈840 ∘C\approx840\,^{\circ}\mathrm{C} on 200 nm-thick sputtered TiN(111)/Al2_2O3_3(0001) templates, as described in our previous works.[28, 30, 40] The nanowire nucleation does not occurr directly on the TiN thin film, but exclusively on SiNx_x islands deposited in the MBE chamber prior to GaN growth. Consequently, the nanowire number density is directly proportional to the density of the SiNx_x islands, which can be precisely controlled through the amount of deposited SiNx_x.[28]

Self-assembled nanowire ensembles of different densities (0.01 μ\mum−2^{-2}, 0.2 μ\mum−2^{-2}, 5 μ\mum−2^{-2} and 300 μ\mum−2^{-2}) are simultaneously overgrown by MOVPE for 10 min, using trimethylgallium (TMGa) and NH3_3 as precursors. A total carrier gas flow of 8 slm of either N2_2, H2_2 or an N2_2/H2_2 mixture is used. The growth temperature is kept between 925 and 1020 ∘C^{\circ}\mathrm{C} and the pressure between 75 and 100 Torr. In some growth experiments, 0.01 sccm of SiH4_4 is added, in order to achieve nn-type doping.

The morphology of the grown GaN structures is analyzed with scanning electron microscopy (SEM) and atomic force microscopy (AFM). Their polarity is assessed by wet etching experiments, using a 20% KOH solution for 3 min at 70 ∘C^{\circ}\mathrm{C}.

To investigate the microstructure of selected samples, scanning transmission electron microscopy (STEM) was performed in a Titan SPECTRA 200 (ThermoFisher), equipped with a cold field emission gun and a Cs aberration probe corrector. Cross-section lamellae were prepared by focused ion beam sectioning inside a Thermo Fisher Helios 5 UX SEM.

The electrical contact between the grown GaN and the TiN layer was investigated by current–voltage measurements through several GaN platelets and the TiN substrate using a conventional two-point measurement probe station, with one probe needle placed on a μ\mum-sized GaN platelet and the other on the TiN layer.

Optical characterization was performed by cathodoluminescence (CL) spectroscopy at room temperature, using a Delmic Sparc Spectral CL system particularly designed for the detection of UV emission. Excitation was performed inside a Thermo Fisher Verios 5 UC field emission SEM, using an acceleration voltage and beam current of 3 kV and 0.4 nA, respectively. The emitted light was collected by a parabolic mirror and focused on the 10 μ\mum wide entrance slit of the spectrometer. Signal recording takes place by a UV-enhanced CCD camera at the output of the spectrometer. At least five different platelets were analyzed and representative spectra are shown.

Results and Discussion

Figure 2 displays a typical overgrowth of MBE-grown GaN nanowires by MOVPE. In particular, a nanowire ensemble with a number density of 0.01 μ\mum−2^{-2} [Figure 2(a)] self-assembled on TiN is overgrown at 985 °C under pure N2_2 carrier gas, using 40 sccm TMGa and 40 sccm NH3_3. The MOVPE overgrowth leads to both a lateral and axial expansion of the seed nanowire, forming a μ\mum-sized hexagonal GaN platelet [Figure 2(b)]. Notably, the TiN(111) surface remains intact after MOVPE growth, exhibiting flat grains arranged in long, parallel domains with an average diameter of ≈75 nm and a root mean square (RMS) roughness of 1.4 nm, as revealed by the atomic force topograph in Figure 2(c). This morphology contrasts the initial TiN surface that is characterized by small circular grains with inclined {100} facets, and a grain diameter of ≈25 nm, as investigated in our previous works.[28, 30] The high temperature during the MOVPE thus leads to a structural reshaping of the TiN with significant grain growth and the formation of flat {111} facets. Note that this process may already commence during the initial heating phase and may be further promoted by the presence of NH3_3, which has been reported to enhance recrystallization in TiN.[41] The parallel domain orientation found here may be kinetically governed by the atomic step morphology of the Al2_2O3_3(0001) substrate. Note that a similar morphology has

Figure 2. MBE-grown GaN nanowire on sputtered TiN thin film (a) before and (b) after lateral overgrowth by MOVPE, yielding an μ\mum-sized hexagonal platelet. (c) and (d) show atomic force topographs of the TiN surface and the GaN μ\mu-platelet after the MOVPE growth, respectively. The height scale is identical for both topographs and shown in (d).

been observed by Wright et al. 42 after the MBE growth of δ\delta-NbN(111) on SiC(0001), where alternating domains have been identified as the two in-plane rotational domains of the NbN. Such domains inevitably form during the epitaxy of cubic rock-salt materials with (111) orientation on hexagonal wurtzite (0001) surfaces due to the symmetry mismatch between the two surfaces, exhibiting 3m3m and 6mm6mm symmetry, respectively.[43]

Figure 2(d) illustrates the morphology of a selected area of an hexagonal GaN μ\mu-platelet. The atomic force topograph of this platelet reveals a relatively smooth surface (RMS = 1.0 nm) with a growth mode characterized by step-bunching. Note that the surface morphology of the GaN μ\mu-platelets is generally found to be dependent on the MOVPE growth conditions and can vary even within one sample, as further revealed below.

Next, we investigate the impact of the GaN seed nanowire number density on the resulting platelet morphology. Figure 3(a) displays secondary electron micrographs of three GaN nanowire ensembles with densities of 0.01 (left panel), 0.2 (center panel) and 5 μm−2\mu\mathrm{m}^{-2} (right panel) grown by MBE. These samples are overgrown by MOVPE in the same growth run, using similar conditions to the ones used in Figure 2. In addition, SiH4_4 is introduced during growth to achieve nn-type doping, thereby enabling the electrical measurements presented later.

Figure 3. GaN nanowire seeds with number densities of 0.01 (left) 0.2 (center) and 5 μm−2\mu\mathrm{m}^{-2} (right) before (a) and after (b) MOVPE overgrowth at 985 °C under N2N_2 carrier gas and the presence of SiH4_4. (c) Number density of MOVPE-grown GaN μ\mu-platelets as a function of MBE seed nanowire density. Note that for the highest seed density (5 μm−2\mu\mathrm{m}^{-2}), both large platelets and residual thin nanowires are included in the count. (d) GaN μ\mu-platelets with a number density of 5 μm−2\mu\mathrm{m}^{-2} after KOH etching. White arrows in (b) indicate Ga-polar inversion domains.

The result of the MOVPE overgrowth is displayed in Figure 3(b). The secondary electron micrographs evidence the formation of GaN platelets for all overgrown nanowire ensembles, yet, with distinct morphologies. The overgrowth of the low-density nanowire ensemble (0.01 μm−2\mu\mathrm{m}^{-2}) yields few and very large GaN platelets (left panel). An increase in nanowire number density to 0.2 μm−2\mu\mathrm{m}^{-2} leads also to an increased platelet density, but with a smaller average diameter and height (center panel) and broad diameter and height distributions. This trend is continued for a seed nanowire density of 5 μm−2\mu\mathrm{m}^{-2} (right panel). The quantitative diameter and height distributions of all GaN μ\mu-platelet ensembles are displayed in Figure S1 of the supporting information.

Figure S1. Diameter (a)–(c) and height (d)–(f) statistics of MOVPE-grown GaN μ\mu-platelets. Each pair of vertically stacked panels corresponds to the same GaN nanowire seed number density, as indicated above.

Figure 3(c) displays the number density of MOVPE platelets resulting from the overgrowth, as a function of initial MBE-grown GaN seed nanowire density. Note that for the highest seed density (5 μm−2\mu\mathrm{m}^{-2}, cf. Figure 3(b), right panel) the reported platelet density includes both large μ\mu-platelets and residual thinner nanowires that did not form full platelets during overgrowth. The dependence is close to a 1:1 ratio (dotted line), with negligible parasitic growth found on the bare TiN substrate in absence of any seed nanowires. This result confirms that the TiN layer acts as a mask for GaN nucleation during the MOVPE process, the growth thus only taking place in the presence of MBE seed nanowires, leading to their axial and radial enlargement.

The decrease of platelet diameter and height as a function of seed nanowire density may be explained by the precursor diffusion processes characterizing selective-area MOVPE, as described in previous studies.[44, 45, 46] In particular, when the distance between initial seed nanowires becomes smaller than the effective diffusion length of the precursor molecules, a decrease of the local precursor concentration adjacent to the growing structures is expected, thus lowering the overall platelet growth rate. Consequently, the local precursor concentration close to a nanowire or platelet becomes highly dependent on the neighboring mask area, possibly explaining the large variation of growth rate also within each self-assembled nanowire ensemble, since each nanowire exhibits a characteristic nearest-neighbor distance.

In order to investigate the polarity of our GaN μ\mu-platelets, we performed KOH etching experiments. As displayed in Figure 3(d), the KOH solution leads to an etching of the top facets in the MOVPE ensemble with an initial GaN seed nanowire density of 5 μm−2\mu\mathrm{m}^{-2} (cf. Figure 3(b), right panel). This result evidences the N-polarity of our μ\mu-platelets,[47] consistent with the polarity of the GaN seed nanowires assessed independently by piezoelectric force microscopy.[48] The occasional formation of small, 3D islands on the (0001) top facets (indicated by the white arrows in Figure 3(b), center panel) likely indicates the formation of Ga-polar inversion domains within the N-polar matrix, as found previously by Henriques et al. 39 for their MBE-MOVPE grown GaN μ\mu-platelets.

Consistently, these areas are not etched by the KOH solution (not shown). To improve the homogeneity of our self-assembled GaN μ\mu-platelets, we next investigate the impact of MOVPE growth conditions on the overgrowth of the GaN nanowire ensemble with the number density of 0.2 μm−2\mu\mathrm{m}^{-2}. Figure 4(a) displays again the overgrowth ensemble obtained in Figure 3, center panel, i.e., grown under pure N2N_2 carrier gas at 985 °C and 0.01 sccm SiH4_4, exhibiting a large diameter and height distribution.

Scanning electron microscopy and high-resolution HAADF micrographs of GaN nanowires and overgrown GaN μ-platelets

Figure 4. (a)–(c) GaN nanowires with a number density of 0.2 μm−2\mu\mathrm{m}^{-2} and overgrown by MOVPE with different growth conditions, as indicated above. (d) MOVPE overgrowth of GaN nanowires with a number density of 300 μm−2\mu\mathrm{m}^{-2}, with the growth conditions used in (c). (e) High-resolution HAADF micrograph of the GaN/TiN interface from the sample shown in (d).

In contrast, Figure 4(b) displays an overgrowth of the same GaN seed nanowires, but with a 1:1 mixture of N2N_2 and H2H_2 carrier gases, carried out at a substrate temperature of 925 °C and in presence of 0.01 sccm SiH4_4. The resulting GaN μ\mu-platelets have a larger average diameter compared to those grown under pure N2N_2 carrier gas [cf. Figure 4(a)], indicating that these conditions favor besides axial also lateral overgrowth. The platelet’s diameter distribution is narrow (1.9 ± 0.4) μ\mum, the narrowest among all grown ensembles.

Finally, Figure 4(c) displays an MOVPE overgrowth carried out under pure H2H_2 carrier gas and conditions typical for GaN layer growth, i.e., a growth temperature of 1020 °C, a TMGa flow of 60 sccm and an NH3\mathrm{NH_3} flow of 8 slm, under a pure H2\mathrm{H_2} carrier gas atmosphere and in absence of SiH4\mathrm{SiH_4}. As a result, strong lateral growth is found, leading to the formation of an almost entirely coalesced GaN layer. The RMS roughness of the GaN thin film is with ≈110\approx110 nm very high, likely due to a large seed nanowire length distribution, which is related to subsequent nucleation of nanowires during the long incubation times occurring in our GaN nanowires.[28]

To further enhance coalescence and decrease surface roughness, we attempted an overgrowth on short, highly dense nanowires (ensemble with an average length of (47±15)(47 \pm15) nm and a number density of 300 μm−2\mathrm{\mu m^{-2}}), the morphology being displayed in Figure S2 of the supporting information. Although this approach resulted in the formation of a fully coalesced thin film, [see Figure 4(d)] the obtained GaN layer still exhibits a high RMS roughness of approximately ≈50\approx50 nm. Hence, growth on nanowire ensembles with narrower length distributions and/or an increase of overgrowth thickness is necessary to further reduce the surface roughness of such coalesced GaN layers on TiN.

Figure S2. XRD ω\omega-scans of (a) MBE-grown, self-assembled GaN nanowire seeds with a number density of 300 μm−2\mu\mathrm{m}^{-2} and (b) the same nanowire ensemble after MOVPE overgrowth, yielding a coalesced GaN layer. The MOVPE was performed under H2_2 carrier gas using 40 sccm TMGa and 8000 sccm NH3_3 at 1020 °C. The rocking curves were measured with a Panalytical X’Pert diffractometer equipped with a two-bounce Ge(220) hybrid monochromator, providing CuKα1\alpha_1 radiation. The measurements were performed in double-crystal geometry, with a 1 mm receiving slit placed in front of the x-ray detector.

We performed STEM measurements to investigate the interface between the overgrown GaN and the TiN template. A sharp interface with no evident inter-diffusion is revealed in the high-resolution high-angle annular dark field (HAADF) micrograph in Figure 4(e). The GaN layer exhibits an ABAB stacking sequence along the [11ˉ20]GaN[1\bar{1}20]_{\mathrm{GaN}} zone axis, characteristic for the hexagonal wurtzite structure. In contrast, the TiN layer exhibits an ABCABC stacking sequence along the [11ˉ0]TiN[1\bar{1}0]_{\mathrm{TiN}} zone axis, consistent with its cubic rock-salt structure. The complete epitaxial relationship is thus GaN(0001ˉ)[112ˉ0]∥TiN(111)[11ˉ0]\mathrm{GaN}(000\bar{1})[11\bar{2}0] \parallel\mathrm{TiN}(111)[1\bar{1}0], as commonly observed for group-III nitrides grown on TiN.[21, 35] Note that the interface of the heterostructure locally exhibits an increased roughness (not shown), which can be attributed to the surface roughness of the TiN layer [cf. Figure 2(c)].

X-ray diffraction measurements reveal relatively narrow rocking curves. A full-width at

half maximum (FWHM) of 0.57∘0.57^\circ is found for an ω\omega-scan across the (0002) reflection, much narrower than the corresponding FWHM of the initial seed nanowire sample of 2.1∘2.1^\circ, as typically found due to a strong nanowire-to-nanowire tilt (see Figure S2 of the supporting information). This phenomenon has been observed previously during the MOVPE coalescence of GaN nanostructures and is attributed to a reorientation of the initially misoriented, individual GaN nanowires upon the early stage of their coalescence, thus forming a coalesced layer with comparatively higher crystalline quality.[49]

We have demonstrated that the MOVPE growth conditions, particularly the carrier gas mixture and precursor ratio, can be utilized to form either GaN μ\mathrm{\mu}-platelets or coalesced thin films on metallic TiN templates when overgrowing GaN seed nanowires. Yet, for a potential use of our epitaxial GaN-on-TiN platform in functional devices, the evaluation of the electrical contact characteristics between the TiN layer and GaN is essential. For this purpose, we measured two-point probe current-voltage curves. First, we evaluated the conductivity of the TiN substrate after the MOVPE overgrowth by placing both probe needles on the exposed TiN substrate between large GaN platelets. The dotted line in Figure 5 shows a strong, linear increase in current as a function of voltage, confirming the metallic behavior of the TiN layer after the MOVPE overgrowth. Next, we repeated the same measurement, but with one probe needle placed on a large, Si-doped GaN μ\mu-platelet (cf. Figure 3(b), left panel) and the second one remaining on the TiN layer. These measurements were performed without depositing electrical contacts on the GaN platelets, as schematically displayed in the inset of Figure 5. The solid lines display the resulting current-voltage curves through several single GaN μ\mu-platelets. A quasi-linear relationship is found with a maximum current of ≈20\approx20 mA at 1.0 V, indicating an ohmic contact between the GaN and the TiN layer. This ohmic behavior is consistent with previous experimental studies[50, 51] and can be explained by the low work function of TiN.[52] Note that the measured current, limited by the platelet’s lateral dimension (diameter ≤10 μm\leq10\,\mu\mathrm{m}), is sufficient to power GaN-based μ\mu-LEDs[53, 54] or vertical GaN diodes,[55] as such devices typically have comparable or larger contact areas.

Figure 5. Current-voltage curves measured through several Si-doped GaN platelets and the TiN substrate. The measurements were performed using probe needles, with one needle placed on a large GaN platelet and the other one on the TiN layer, as indicated in the top left corner. The dashed line corresponds to a reference measurement with both needles placed on the TiN surface. Different solid lines correspond to measurements on different GaN platelets.

Finally, we evaluated the optical properties of our GaN platelets and thin films using CL spectroscopy. Figure 6(a) displays room-temperature CL spectra of the nanowire ensembles overgrown at different conditions, with an initial number density of 0.2 μm−2\mu\mathrm{m}^{-2}. The quasi-coalesced GaN layer grown under H2_2 carrier gas at 1020 ∘C1020\,^\circ\mathrm{C} [cf. Figure 4(c)] is characterized by a dominant near-band edge emission centered around 3.395 eV, and comparatively weak emission from deep levels between 2.0 and 2.5 eV (gray curve, bottom spectrum), indicating a relatively low density of point defects. The near-band edge region of this sample is shown in Figure 6(b), together with a reference photoluminescence (PL) spectrum of a free-standing GaN crystal (orange curve), featuring a narrow free exciton transition (FXA_A) at 3.401 eV (364.4 nm) and well-defined longitudinal optical (LO) phonon replica. Compared to the narrow peak of the free-standing GaN with an FWHM of 67 meV, the emission band of our GaN/TiN is broader (FWHM of 100 meV). This broadening is likely caused by a higher excitation density in CL compared to PL,[56] the presence inhomogeneous strain in the GaN/TiN layer,[57] and, potentially, a higher background doping density.[58]

Figure 6. (a) CL spectra of GaN nanowires with a number density of 0.2 μm−2\mu\mathrm{m}^{-2}, overgrown by MOVPE under different conditions, as indicated below each spectrum. (b) Normalized near-band edge region of the bottom spectrum shown in (a), together with a photoluminescence spectrum of free-standing (FS) GaN for reference.

Changing the growth conditions to favor the formation of GaN μ\mu-platelets drastically alters the emission characteristics. Remarkably, the μ\mu-platelets with the narrowest height and diameter distributions [cf. Figure 4(b)], grown under an H2_2/N2_2 mixture with a 1:1 NH3_3/TMGa precursor flow ratio at 925 ∘C925\,^\circ\mathrm{C} exhibit no near-band luminescence (Figure 6(a), red curve). Instead, a pronounced defect band with two broad peaks centered around 2.0 eV (620 nm) and 2.35 eV (525 nm) is found. In undoped GaN, deep-level luminescence is commonly associated with the presence of C impurities substituting N (CN_N), nitrogen vacancies (VN_N) or oxygen-containing defect complexes.[59] The formation of CN_N and VN_N defects is generally favored under Ga-rich conditions and at relatively low growth temperatures,[60, 61] in agreement with the conditions used for the overgrowth, and may therefore also contribute to the observed emission. In addition, the presence of SiH4_4 during the growth of this μ\mu-platelet ensemble suggests that Si-related defect complexes likely contribute to the near-band edge quenching and to the observed deep-level luminescence.[58, 62, 63]

Similar deep-level luminescence features, this time centered around 2.2 eV (560 nm), are found for the GaN μ\mu-platelets exhibiting large diameter and height distributions [grown at 985 ∘C985\,^\circ\mathrm{C} with a 1:1 NH3_3/TMGa precursor flow ratio under N2_2 carrier gas, cf. Figure 4(a)], as displayed in the third-lowest spectrum (blue curve). In addition, a weak, broad near-band edge emission feature is found centered at 3.35 eV, which may be explained by the slightly higher growth temperature used for this ensemble. The peak position and large FWHM still suggest a very high point defect density.

To investigate the impact of Si doping on the luminescence properties of our GaN μ\mu-platelets, we grew one ensemble under identical conditions as that of Figure 4(a) [blue curve, third-lowest spectrum in Figure 6(a)], but without the addition of SiH4_4. The CL spectrum of this undoped ensemble [green curve, top spectrum in Figure 6(a)] exhibits spectral features similar the Si-doped one, i. e. a pronounced defect band around 2.2 eV and a broad near-band edge emission band around 3.35 eV. Yet, the near-band edge luminescence in the undoped sample shows a narrower FWHM, indicating that Si incorporation indeed contributes to the broadening of the near-band edge luminescence.

Conclusion

We have demonstrated the integration of epitaxial GaN on metallic TiN thin films through a two-step growth approach, involving the initial nucleation of self-assembled GaN nanowires by MBE, followed by their overgrowth by MOVPE. By tuning the seed nanowire density and the MOVPE overgrowth conditions, the morphology of the resulting GaN/TiN heterostructures can be controlled from relatively homogeneous, micrometer-sized platelets to fully coalesced thin films. The ohmic contact formed between GaN and TiN makes these heterostructures promising templates for the development of vertical III-nitride devices. In particular, the nn-type GaN platelets, with diameters of approximately 2 μm\mu\mathrm{m}, offer a potential platform for the fabrication of vertical Inx_xGa1−x_{1-x}N based μ\mu-LEDs. On the other hand, fully coalesced GaN layers on metallic TiN may provide a suitable platform for future vertical power devices and bulk acoustic wave resonators.

Acknowledgement The authors thank their PDI colleagues C. Matzcek for TEM sample preparation and C. Stemmler for dedicated MBE maintenance. They further acknowledge A. Courville from CRHEA for assistance in MOVPE growth. We are grateful to J. Kang for critically reading the manuscript. This work was funded by Deutsche Forschungsgemeinschaft (568879259) and Agence Nationale de la Recherche (ANR-25-CE24-0472) through the project MINT and supported by COST Action OPERA from the European Network for Innovative and Advanced Epitaxy, CA20116 (www.cost.eu). We further acknowledge co-funding by the European Regional Development Fund (ERDF) through the Berlin Senate for the application laboratory time-resolved cathodoluminescence spectroscopy (ZALKAL).

Supporting information

References

  1. [1]Pust, P.; Schmidt, P. J.; Schnick, W. A Revolution in Lighting. Nat. Mater. 2015, 14, 454–458, DOI: 10.1038/nmat4270.DOI
  2. [2]Weinold, M. P.; Kolesnikov, S.; Anadón, L. D. Rapid Technological Progress in White Light-Emitting Diodes and Its Source in Innovation and Technology Spillovers. Nat. Energy 2025, 10, 616–629, DOI: 10.1038/s41560-025-01757-1.DOI
  3. [3]Amano, H. et al. The 2018 GaN Power Electronics Roadmap. J. Phys. Appl. Phys. 2018, 51, 163001, DOI: 10.1088/1361-6463/aaaf9d.DOI
  4. [4]Tu, C.-C. et al. Industry Perspective on Power Electronics for Electric Vehicles. Nat. Rev. Electr. Eng. 2024, 1, 435–452, DOI: 10.1038/s44287-024-00055-4.DOI
  5. [5]Li, C.-K.; Wu, Y.-R. Study on the Current Spreading Effect and Light Extraction Enhancement of Vertical GaN/InGaN LEDs. IEEE Trans. Electron Devices 2012, 59, 400–407, DOI: 10.1109/TED.2011.2176132.
  6. [6]Zhang, Y.; Dadgar, A.; Palacios, T. Gallium Nitride Vertical Power Devices on Foreign Substrates: A Review and Outlook. J. Phys. Appl. Phys. 2018, 51, 273001, DOI: 10.1088/1361-6463/aac8aa.DOI
  7. [7]You, S. et al. Vertical GaN Devices: Process and Reliability. Microelectron. Reliab. 2021, 126, 114218, DOI: 10.1016/j.micror el.2021.114218.DOI
  8. [8]Shankari, R.; Supraja, G.; Krushnasamy, V.; Haripriya, D.; Elangovan, K. Vertical Gallium Nitride MOSFETs: Advanced Architectures, Fabrication Technologies, and Performance Breakthroughs for High-Power Applications. Microelectron. Eng. 2026, 302, 112418, DOI: 10.1016/j.mee.2025.112418.DOI
  9. [21]Wölz, M.; Hauswald, C.; Flissikowski, T.; Gotschke, T.; Fernández-Garrido, S.; Brandt, O.; Grahn, H. T.; Geelhaar, L.; Riechert, H. Epitaxial Growth of GaN Nanowires with High Structural Perfection on a Metallic TiN Film. Nano Lett. 2015, 15, 3743–3747, DOI: 10.1021/acs.nanolett.5b000251.DOI
  10. [22]Sarwar, A. G.; Carnevale, S. D.; Yang, F.; Kent, T. F.; Jamison, J. J.; McComb, D. W.; Myers, R. C. Semiconductor Nanowire Light-Emitting Diodes Grown on Metal: A Direction Toward Large-Scale Fabrication of Nanowire Devices. Small 2015, 11, 5402–5408, DOI: 10.1002/smll.201501909.DOI
  11. [23]Zhao, C.; Ng, T. K.; Wei, N.; Prabaswara, A.; Alias, M. S.; Janjua, B.; Shen, C.; Ooi, B. S. Facile Formation of High-Quality InGaN/GaN Quantum-Disks-in-Nanowires on Bulk-Metal Substrates for High-Power Light-Emitters. Nano Lett. 2016, 16, 1056–1063, DOI: 10.1021/acs.nanolett.5b04190.DOI
  12. [24]May, B. J.; Sarwar, A. T. M. G.; Myers, R. C. Nanowire LEDs Grown Directly on Flexible Metal Foil. Appl. Phys. Lett. 2016, 108, 141103, DOI: 10.1063/1.4945419.DOI
  13. [25]Calabrese, G.; Corfdır, P.; Gao, G.; Pfüller, C.; Trampert, A.; Brandt, O.; Geelhaar, L.; Fernández-Garrido, S. Molecular Beam Epitaxy of Single Crystalline GaN Nanowires on a Flexible Ti Foil. Appl. Phys. Lett. 2016, 108, 202101, DOI: 10.1063/1.4950707.DOI
  14. [26]Olszewski, K.; Sobanska, M.; Dubrovskii, V. G.; Leshchenko, E. D.; Wierzbicka, A.; Zytkiewicz, Z. R. Geometrical Selection of GaN Nanowires Grown by Plasma-Assisted MBE on Polycrystalline ZrN Layers. Nanomaterials 2023, 13, 2587, DOI: 10.3390/nano13182587.DOI
  15. [27]Tiagulskyi, S.; Yatskiv, R.; Sobanska, M.; Olszewski, K.; Zytkiewicz, Z. R.; Grym, J. ZrN Nucleation Layer Provides Back-side Ohmic Contact to MBE-Grown GaN Nanowires. Nanoscale 2025, 17, 8111–8117, DOI: 10.1039/D5NR00321K.DOI
  16. [28]Auzelle, T.; Oliva, M.; John, P.; Ramsteiner, M.; Trampert, A.; Geelhaar, L.; Brandt, O. Density Control of GaN Nanowires at the Wafer Scale Using Self-Assembled SiNx Patches on Sputtered TiN(111). Nanotechnology 2023, 34, 375602, DOI: 10.1088/1361-6528/acdde8.DOI
  17. [29]Azadmand, M.; Auzelle, T.; Lähnemann, J.; Gao, G.; Nicolai, L.; Ramsteiner, M.; Trampert, A.; Sanguinetti, S.; Brandt, O.; Geelhaar, L. Self-Assembly of Well-Separated AlN Nanowires Directly on Sputtered Metallic TiN Films. Phys. Status Solidi RRL – Rapid Res. Lett. 2020, 14, 1900615, DOI: 10.1002/pssr.201900615.DOI
  18. [30]John, P.; Gómez Ruiz, M.; Van Deurzen, L.; Lähnemann, J.; Trampert, A.; Geelhaar, L.; Brandt, O.; Auzelle, T. Growth Kinetics and Substrate Stability during High-Temperature Molecular Beam Epitaxy of AlN Nanowires. Nanotechnology 2023, 34, 465605, DOI: 10.1088/1361-6528/acefd8.DOI
  19. [31]Buatip, N.; Auzelle, T.; John, P.; Rauwerdink, S.; Sodhi, M.; Salaün, M.; Fernandez, B.; Monroy, E.; Mornex, D.; Bowen, C. R.; Songmuang, R. AlN Nanowire-Based Vertically Integrated Piezoelectric Nanogenerators. ACS Appl. Nano Mater. 2024, 7, 15798–15807.arxiv.org/abs/2402.09771
  20. [32]Notarangelo, A.; Songmuang, R.; Saleh, M.; Buatip, N.; Florea, I.; Vennégùes, P.; Campbell, A. F.; Tornatzky, H.; Lähnemann, J.; Auzelle, T.; Geelhaar, L.; Brandt, O.; John, P. M. Molecular Beam Epitaxy of Al₁−ₓScₓN Nanowires: Towards Group-III Nitride Piezoelectric Nanogenerators with Enhanced Response. 2026.
  21. [33]Watanabe, T.; Ito, K.; Tsukimoto, S.; Ushida, Y.; Moriyama, M.; Shibata, N.; Murakami, M. Growth of GaN on Nitriding TiN Buffer Layers. Mater. Trans. 2005, 46, 1975–1978, DOI: 10.2320/matertrans.46.1975.DOI
  22. [34]Ito, K.; Uchida, Y.; Lee, S.-j.; Tsukimoto, S.; Ikemoto, Y.; Hirata, K.; Shibata, N.; Murakami, M. Epitaxial GaN Layer Growth Using Nitrogen Enriched TiN Buffer Layers. MRS Proc. 2006, 916, 0916–DD04–06, DOI: 10.1557/PROC-0916-DD04–06.DOI
  23. [35]Uchida, Y.; Ito, K.; Tsukimoto, S.; Ikemoto, Y.; Hirata, K.; Shibata, N.; Murakami, M. Epitaxial Growth of GaN Layers on Metallic TiN Buffer Layers. J. Electron. Mater. 2006, 35, 1806–1811, DOI: 10.1007/s11664-006-0161-6.
  24. [36]Ito, K.; Uchida, Y.; Lee, S.; Tsukimoto, S.; Ikemoto, Y.; Hirata, K.; Murakami, M. Effects of TiN Buffer Layer Thickness on GaN Growth. J. Electron. Mater. 2009, 38, 511–517, DOI: 10.1007/s11664-008-0597-y.DOI
  25. [37]Hörich, F.; Lüttich, C.; Grümbel, J.; Bläsing, J.; Feneberg, M.; Dadgar, A.; Goldhahn, R.; Strittmatter, A. Epitaxial Growth of Transition Metal Nitrides by Reactive Sputtering. Front. Mater. 2025, 12, 1507123, DOI: 10.3389/fmats.2025.1507123.DOI
  26. [38]Henriques, J.; Tamsaout, D.; Largeau, L.; Cambril, E.; Valera, L.; Jacopin, G.; Tchernycheva, M.; Harmand, J.-C.; Eymery, J.; Durand, C. Selective Area Growth of GaN μ-Platelets on Graphene. Cryst. Growth Des. 2024, acs.cgd.4c00708, DOI: 10.1021/acs.cgd.4c00708.
  27. [39]Henriques, J.; Tamsaout, D.; Largeau, L.; Cambril, E.; Jacopin, G.; Tchernycheva, M.; Harmand, J.-C.; Eymery, J.; Durand, C. InGaN/GaN Multiple Quantum Wells on N-Polar μ-Platelets Grown on Graphene. Cryst. Growth Des. 2025, acs.cgd.5c01095, DOI: 10.1021/acs.cgd.5c01095.
  28. [40]John, P.; Trampert, A.; Van Dinh, D.; Spallek, D.; Lähnemann, J.; Kaganer, V. M.; Geelhaar, L.; Brandt, O.; Auzelle, T. ScN/GaN(1̄100): A New Platform for the Epitaxy of Twin-Free Metal–Semiconductor Heterostructures. Nano Lett. 2024, 24, 6233–6239, DOI: 10.1021/acs.nanolett.4c00659.DOI
  29. [41]Sun, S. C.; Tsai, M. H. Effect of Rapid Thermal Annealing on the Electrical and Physical Properties of Metalorganic Chemical-Vapor-Deposited TiN. Appl. Phys. Lett. 1996, 68, 670–672, DOI: 10.1063/1.116586.DOI
  30. [43]Grundmann, M. Formation of Epitaxial Domains: Unified Theory and Survey of Experimental Results. Phys. Status Solidi B 2011, 248, 805–824, DOI: 10.1002/pssb.201046530.DOI
  31. [44]Olsson, F.; Zhu, T.; Mion, G.; Lourdudoss, S. Large Mask Area Effects in Selective Area Growth. J. Cryst. Growth 2006, 289, 24–30, DOI: 10.1016/j.jcrysgro.2005.10.130.
  32. [45]Dubrovskij, V. G. Theory of MOCVD Growth of III-V Nanowires on Patterned Substrates. Nanomaterials 2022, 12, 2632, DOI: 10.3390/nano12152632.
  33. [46]Stępniak, M.; Wośko, M.; Kijaszek, W.; Prażmowska-Czajka, J.; Stafiniak, A.; Paszkiewicz, R. Mask Interference Effect in GaN SA-MOVPE: Predicting the Growth of Isolated Structures. Mater. Sci. Eng. B 2026, 323, 118730, DOI: 10.1016/j.mseb.2025.118730.DOI
  34. [47]Zúñiga-Pérez, I. et al. Polarity in GaN and ZnO: Theory, Measurement, Growth, and Devices. Appl. Phys. Rev. 2016, 3, 041303, DOI: 10.1063/1.4963919.
  35. [48]Jaloustre, L.; Le Denmat, S.; Auzelle, T.; Azadmand, M.; Geelhaar, L.; Dahlem, F.; Songmuang, R. Toward Quantitative Measurements of Piezoelectricity in III-N Semiconductor Nanowires. ACS Appl. Nano Mater. 2021, 4, 43–52, DOI: 10.1021/acsanm.0c02078.DOI
  36. [49]Wehbe, M.; Charles, M.; Pino Muñoz, D.; Baril, K.; Labchir, N.; Labau, S.; Gourgon, C.; Alloing, B.; Coulon, P.-M.; Zuniga-Perez, J.; Zatterin, E.; Gergaud, P. Demonstration of Grain Reorientation during GaN Early Stage Coalescence Grown by Novel Pendeo-Epitaxy Approach. J. Appl. Phys. 2024, 136, 224302, DOI: 10.1063/5.0235955.DOI
  37. [50]Jeon, J.-W.; Seong, T.-Y.; Kim, H.; Kim, K.-K. TiN/Al Ohmic Contacts to N-Face n-Type GaN for High-Performance Vertical Light-Emitting Diodes. Appl. Phys. Lett. 2009, 94, 042102, DOI: 10.1063/1.3073887.DOI
  38. [51]Zhu, Y.; Huang, R.; Li, Z.; Hao, H.; An, Y.; Liu, T.; Zhao, Y.; Shen, Y.; Guo, Y.; Li, F.; Ding, S. Interface Analysis of TiN/n-GaN Ohmic Contacts with High Thermal Stability. Appl. Surf. Sci. 2019, 481, 1148–1153, DOI: 10.1016/j.apsusc.2019.03.212.DOI
  39. [52]Zhu, Y.; Li, F.; Huang, R.; Liu, T.; Zhao, Y.; Shen, Y.; Zhang, J.; Dingsun, A.; Guo, Y. Remote Plasma-Enhanced Atomic Layer Deposition of Metallic TiN Films with Low Work Function and High Uniformity. J. Vac. Sci. Technol. Vac. Surf. Films 2018, 36, 041501, DOI: 10.1116/1.5025557.DOI
  40. [53]Li, C. C.; Zhan, J. L.; Chen, Z. Z.; Jiao, F.; Chen, Y. F.; Chen, Y. Y.; Nie, J. X.; Kang, X. N.; Li, S. F.; Wang, Q.; Zhang, G. Y.; Shen, B. Operating Behavior of Micro-LEDs on a GaN Substrate at Ultrahigh Injection Current Densities. Opt. Express 2019, 27, A1146, DOI: 10.1364/OE.27.0A1146.DOI
  41. [54]Zhang, Z.; Jin, Z.; Ruan, Y.; Lin, R.; Ren, T.; Gu, E.; Cui, X.; Tian, P. High-Performance Green Micro-LED Array with Isolated n-GaN Layers for 6.58 Gbps High-Speed Visible Light Communication. J. Appl. Phys. 2025, 138, 145706, DOI: 10.1063/5.0272905.DOI
  42. [55]Zhang, Y.; Sun, M.; Piedra, D.; Hennig, J.; Dadgar, A.; Palacios, T. Reduction of On-Resistance and Current Crowding in Quasi-Vertical GaN Power Diodes. Appl. Phys. Lett. 2017, 111, 163506, DOI: 10.1063/1.4989599.DOI
  43. [56]Damilano, B.; Aristégui, R.; Teisseyre, H.; Vézian, S.; Guigoz, V.; Courville, A.; Florea, I.; Vennègues, P.; Boćkowski, M.; Guillet, T.; Vladimirova, M. Molecular Beam Epitaxy of GaN/AlGaN Quantum Wells on Bulk GaN Substrate in the Step-Flow or Step Meandering Regime: Influence on Indirect Exciton Diffusion. J. Appl. Phys. 2024, 135, 095702, DOI: 10.1063/5.0182659.DOI
  44. [57]Kaganer, V. M.; Jenichen, B.; Ramsteiner, M.; Jahn, U.; Hauswald, C.; Grosse, F.; Fernández-Garrido, S.; Brandt, O. Quantitative Evaluation of the Broadening of X-Ray Diffraction, Raman, and Photoluminescence Lines by Dislocation-Induced Strain in Heteroepitaxial GaN Films. J. Phys. Appl. Phys. 2015, 48, 385105, DOI: 10.1088/0022–3727/48/38/385105.DOI
  45. [58]Schubert, E. F.; Goepfert, I. D.; Grieshaber, W.; Redwing, J. M. Optical Properties of Si-Doped GaN. Appl. Phys. Lett. 1997, 71, 921–923, DOI: 10.1063/1.119689.DOI
  46. [59]Reshchikov, M. A. On the Origin of the Yellow Luminescence Band in GaN. Phys. Status Solidi B 2023, 260, 2200488, DOI: 10.1002/pssb.202200488.DOI
  47. [60]Ciarkowski, T.; Allen, N.; Carlson, E.; McCarthy, R.; Youtsey, C.; Wang, J.; Fay, P.; Xie, J.; Guido, L. Connection between Carbon Incorporation and Growth Rate for GaN Epitaxial Layers Prepared by OMVPE. Materials 2019, 12, 2455, DOI: 10.3390/ma12152455.DOI
  48. [61]Li, C.; Zhang, K.; Qiaoyu Zeng; Yin, X.; Ge, X.; Wang, J.; Wang, Q.; He, C.; Zhao, W.; Chen, Z. High Quality N-Polar GaN Films Grown with Varied V/III Ratios by Metal–Organic Vapor Phase Epitaxy. RSC Adv. 2020, 10, 43187–43192, DOI: 10.1039/D0RA07856E.DOI
  49. [62]Kaufmann, U.; Kunzer, M.; Obloh, H.; Maier, M.; Manz, Ch.; Ramakrishnan, A.; Santic, B. Origin of Defect-Related Photoluminescence Bands in Doped and Nominally Undoped GaN. Phys. Rev. B 1999, 59, 5561–5567, DOI: 10.1103/PhysRevB.59.5561.DOI
  50. [63]Díaz-Guerra, C.; Piqueras, J.; Castaldini, A.; Cavallini, A.; Polenta, L. Time-Resolved Cathodoluminescence and Photocurrent Study of the Yellow Band in Si-Doped GaN. J. Appl. Phys. 2003, 94, 2341–2346, DOI: 10.1063/1.1592296.

Paper details

vlnc:W_52pw6df3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents