Emergent Topological Superconductor by Charge Density Wave Transition

Abstract

Many-body instabilities and topological physics are two attractive topics in condensed matter physics. It is intriguing to explore the interplay between these phenomena in a single quantum material. Here, using the prototypical charge density wave (CDW) material monolayer 1H-NbSe2_2 as an example, we show how momentum-dependent electron-phonon coupling drives the CDW transition from 3×33\times3 to 2×22\times2 phase under electron doping. More interestingly, we find the coexistence of superconductivity and nontrivial topology in one of the two 2×22\times2 CDW phases, the latter of which is identified by the nonzero Z2_2 invariant with ideal Dirac cone edge states near the Fermi level. A similar CDW transition-induced topological superconductor has also been confirmed in monolayer 1H-TaSe2_2. Our findings not only reveal a unique and general method to introduce nontrivial topology by CDW transition, but also provide an ideal platform to modulate different quantum orders by electron doping, thus stimulating experimental interest.

  • Corresponding authors:

Jun Zhou ([email protected])

Kian Ping Loh ([email protected])

Yuan Ping Feng ([email protected])

Introduction

Two-dimensional (2D) materials are among the most exciting research topics for their novel properties and promising applications in advanced electronic devices{sup}1,2`.

Specifically, transition metal dichalcogenides (TMDs) are an important member of the 2D material family, which offer an ideal platform to study quantum materials with topological physics and many-body instabilities including magnetism, superconductivity, and charge density wave (CDW){sup}3–6. CDW is of particular interest as it can coexist or compete with other quantum phenomena. For example, CDW order and superconductivity usually compete with each other because the CDW gap opening decreases the density of states (DOS) at the Fermi level, which suppresses the formation of Cooper pairs below the superconducting transition temperature ($T_C$){sup}7,8. Therefore, it is intriguing to modify electronic states at the Fermi level by external stimulus and study the interaction between CDW and superconductivity.

2H2\mathrm{H}-NbSe2\mathrm{NbSe}_{2} is a typical TMD that draws a great deal of attention due to the many-body instabilities{sup}9–16. The bulk $2\mathrm{H}$-$\mathrm{NbSe}_{2}$ is a hole metal at room temperature, and it undergoes a CDW transition with in-plane $3 \times 3$ periodic distortion at $T_{CDW} \sim 33$ K as well as a superconducting transition at $T_C \sim 7$ K{sup}9. Both CDW and superconductivity have retained to the monolayer thickness{sup}14–16. With the decrease of the layer thickness, the suppression of the $T_C$ has been consistently demonstrated by many experiments{sup}15–17. However, the TCDWT_{CDW} in the monolayer limit is under debate. The monolayer 1H1\mathrm{H}-NbSe2\mathrm{NbSe}_{2} obtained by molecular-beam epitaxy (MBE) has a low TCDW∼25T_{CDW} \sim25 K{sup}15`, while the samples obtained by the mechanical exfoliation exhibit a high TCDW∼145T_{CDW} \sim145 K[14, 18].

The discrepancy is believed to be due to the charge transfer from the substrates to the monolayer NbSe2_2 samples[18, 19, 20].

In order to gain deeper insight into the relation between charge doping and the many-body instabilities of NbSe2_2, a variety of doping methods have been used experimentally, including the electric double-layer transistor[17], ionic liquid gate[21], polymer electrolyte gating[22], Cu intercalation[23], and sandwiched NbSe2_2 with an electron donor[24]. Interestingly, in contrast to the other CDW materials[25, 26], both CDW and superconductivity in NbSe2_2 are suppressed simultaneously under electron doping. Remarkably, NbSe2_2 becomes a 2×22 \times2 CDW under high electron doping[24]. However, the basic understanding of this CDW transition and the physical properties of the 2×22 \times2 CDW structure are still absent.

In this work, based on first-principles calculations and mean-field theory, we perform a systematic investigation of the properties of monolayer NbSe2_2 under electron doping. Momentum-dependent electron-phonon coupling (qq-EPC) is found to account for both the 3×33 \times3 CDW formation and the phase transition from 3×33 \times3 to 2×22 \times2 CDW. Then we determine two possible 2×22 \times2 CDW structures for monolayer NbSe2_2, which may exist when the doping concentration reaches 0.2 electrons per formula unit (e−e^{-}/f.u.). Besides, compared to the CDW gaps predicated by the mean-field model, the coupled electrons, which contribute mainly to the phonon softening, are found to be responsible for the CDW gap opening. In addition, the superconductivity of monolayer NbSe2_2 is suppressed in the 2×22 \times2 CDW phases due to the reduced total electron-phonon coupling (EPC) strength under electron doping. More interestingly, we find one of the two 2×22 \times2 CDW phases topological nontrivial with a nonzero Z2Z_{2} invariant, corresponding to the Dirac cone edge states near the Fermi level. Thus, monolayer NbSe2_2 can be an EPC-driven topological superconductor. Similar behavior is also observed in other TMDs, confirming its generality.

A CDW Transition under Electron Doping

doping (0.1–0.3 e−e^{-}/f.u.). (e) The formation energies for the 3 × 3 filled, 3 × 3 hollow, 2 × 2 filled, and 2 × 2 hollow CDW structures as a function of electron doping concentration. The high-symmetry points are indicated in Figure S1.

The structure of normal monolayer NbSe2_2 is shown in Figure 1a, which has a P6ˉm2P\bar{6}m2 space group. Nb atoms are sandwiched between two Se layers with the trigonal prismatic cells. The optimized lattice constant of NbSe2_2 is 3.474 Å, which is very close to the experimental value[15, 19]. The phonon dispersion of normal NbSe2_2 displays imaginary frequencies around 2/3ΓM2/3\Gamma M (Figure 1d), corresponding to a 3 × 3 CDW. And it has been argued that there are two possible NbSe2_2 3 × 3 CDW structures (Figures S2e and S2f), which are known as 3 × 3 hollow and 3 × 3 filled CDW structures with Nb clusters centered on the hollow sites and Se atoms of the honeycomb lattice, respectively[8, 27, 28]. With the increase of electron doping concentration, the position of imaginary phonons gradually evolves from 2/3ΓM2/3\Gamma M to the MM point (Figure 1d), which implies a transition from 3 × 3 to 2 × 2 CDW. Similarly, we found two possible 2 × 2 CDW structures when doping concentration is above 0.2 e−e^{-}/f.u., and we denote them as 2 × 2 filled (Figure 1b) and 2 × 2 hollow (Figure 1c) CDW structures according to the location of the centers of the Nb clusters.

Schematic diagram of normal NbSe2 monolayer and CDW structures, phonon spectra, and energy differences under electron doping

Figure 1. (a) Schematic diagram of normal NbSe2_2 monolayer in the top and side views. (b) 2×22 \times2 filled and (c) 2×22 \times2 hollow NbSe2_2 CDW structures. (d) The phonon spectra of NbSe2_2 under different electron doping concentrations. Since the optical phonon modes hardly change, we only show acoustic phonon modes for systems under electron

To further verify CDW transition under electron doping in NbSe2_2, the energetic hierarchy of these CDW structures is calculated at various doping concentrations. The CDW formation energies ΔE\Delta E are calculated by ECDW/x−E0E_{\mathrm{CDW}}/x-E_0, where ECDWE_{\mathrm{CDW}} and E0E_0 are the total energies of the CDW and the 1×11 \times1 normal phases, respectively, xx is the number of formula units in the CDW phase. For the doping concentrations studied in this work, Figure 1f clearly shows a transition from 3×33 \times3 hollow CDW to 2×22 \times2 filled CDW at a critical doping concentration of around 0.2 e-/f.u., in agreement with phonon calculations (Figure 1d).

Next, we discuss the underlying physics of this CDW transition. It is known that the softened phonon frequency ωq\omega_{\mathbf{q}} can be obtained by[29]:

ωq2=Ωq2−2ΩqΠq,(1)\omega_{\mathbf{q}}^{2} = \Omega_{\mathbf{q}}^{2} - 2\Omega_{\mathbf{q}}\Pi_{\mathbf{q}}, \tag*{(1)}

where Ωq\Omega_{\mathbf{q}} is the bare phonon frequency, and Πq\Pi_{\mathbf{q}} is the real part of the phonon self-energy, the latter of which carries the information from both EPC and Fermi surface nesting (FSN). In the static limit, Πq\Pi_{\mathbf{q}} has the form:

Πq=∑k∣gk,k+q∣2f(εk)−f(εk+q)εk+q−εk.(2)\Pi_{\mathbf{q}} = \sum_{\mathbf{k}} \lvert g_{\mathbf{k},\mathbf{k}+\mathbf{q}}\rvert^{2} \frac{f(\varepsilon_{\mathbf{k}})-f(\varepsilon_{\mathbf{k}+\mathbf{q}})}{\varepsilon_{\mathbf{k}+\mathbf{q}}-\varepsilon_{\mathbf{k}}}. \tag*{(2)}

Here, f(εk)f(\varepsilon_{\mathbf{k}}) is the Fermi-Dirac function with energy ε\varepsilon at k\mathbf{k} point, and gk,k+qg_{\mathbf{k},\mathbf{k}+\mathbf{q}} is the EPC matrix element which can be calculated via[30]:

gk,k+q=(ℏ2Mωq)1/2⟨φk+q∣∂qV∣φk⟩,(3)g_{\mathbf{k},\mathbf{k}+\mathbf{q}} = \left(\frac{\hbar}{2M\omega_{\mathbf{q}}}\right)^{1/2} \langle\varphi_{\mathbf{k}+\mathbf{q}} \lvert\partial_{\mathbf{q}} V \rvert\varphi_{\mathbf{k}} \rangle, \tag*{(3)}

where φk\varphi_{\mathbf{k}} is the electronic wavefunction with wavevector k\mathbf{k}, VV is the Kohn-Sham potential. The imaginary phonon frequency, suggesting CDW formation, appears when Πq\Pi_{\mathbf{q}} is larger than (1/2)Ωq(1/2)\Omega_{\mathbf{q}}. The peak location of Πq\Pi_{\mathbf{q}} corresponds to the dip position of ωq\omega_{\mathbf{q}}, which can be converted to the CDW vector in the reciprocal space, and the CDW lattice in the real space[31]. Due to the low energy physics studied in this work, the coupling is considered between the softened phonon branch and the single electronic band which crosses the Fermi level (Figure 2a and Figure 2c). Taking ∣gk,k+q∣2∼∣gq∣2|g_{\mathbf{k},\mathbf{k}+\mathbf{q}}|^2 \sim|g_{\mathbf{q}}|^2, which is known as q-EPC and can be extracted from Πq\Pi_{\mathbf{q}} to represent the EPC contribution[12], the remaining part is:

Distribution of the softened phonon frequency, phonon self-energy, q-EPC, and bare electronic susceptibility in pristine and doped NbSe2

Figure 2. (a) The softened phonon frequency ωq\omega_{\mathbf{q}}, (b) the real part of the phonon self-energy Πq\Pi_{\mathbf{q}}, (c) q-EPC ∣gq∣2|g_{\mathbf{q}}|^2 and (d) the real part of the bare electronic susceptibility χq\chi_{\mathbf{q}} in the first BZ of pristine NbSe2_2. (e-h) Same as panels (a-d) but for NbSe2_2 under 0.3 e−^{-}/f.u. doping concentration.

χq=∑kf(εk)−f(εk+q)εk+q−εk,(4)\chi_{\mathbf{q}} = \sum_{\mathbf{k}} \frac{f(\varepsilon_{\mathbf{k}})-f(\varepsilon_{\mathbf{k}+\mathbf{q}})}{\varepsilon_{\mathbf{k}+\mathbf{q}}-\varepsilon_{\mathbf{k}}}, \tag*{(4)}

where χq\chi_{\mathbf{q}} is the real part of the bare electronic susceptibility, which captures the Fermi surface topology as the FSN effect[32]. These quantities (Πq\Pi_{\mathbf{q}}, ∣gq∣2|g_{\mathbf{q}}|^2 and χq\chi_{\mathbf{q}}) are further quantitatively analyzed to reveal the underlying mechanism for the NbSe2_2 CDW formation and the phase transition from 3×33 \times3 to 2×22 \times2 CDW.

Figures 2a and 2e display the distribution of the softened phonon frequency ωq\omega_{\mathbf{q}} in the first Brillouin zone (BZ) of NbSe2\mathrm{NbSe}_{2} without doping and under 0.3 e−/f.u.0.3\ \mathrm{e}^{-}/\mathrm{f.u.} doping concentration, respectively. The distribution of imaginary phonon frequencies (see the dark blue areas in Figures. Figure 2a and Figure 2e) clearly changes from the egg shape centered at 2/3ΓM2/3\Gamma M to the valley shape centered at MM point. Meanwhile, a similar transition can be found for the peak of the real part of the phonon self-energy Πq\Pi_{\mathbf{q}} (see the yellow areas in Figures. Figure 2b and Figure 2f). Furthermore, we decompose the contribution of the real part of the phonon self-energy Πq\Pi_{\mathbf{q}} into pure effect of EPC and FSN by calculating ∣gq∣2\lvert g_{\mathbf{q}}\rvert^{2} and χq\chi_{\mathbf{q}} separately. For pristine NbSe2\mathrm{NbSe}_{2}, it is interesting to note that ∣gq∣2\lvert g_{\mathbf{q}}\rvert^{2} and Πq\Pi_{\mathbf{q}} have very similar patterns in the first BZ, which both have maxima at 2/3ΓM2/3\Gamma M (Figures. Figure 2b and Figure 2c). However, the χq\chi_{\mathbf{q}} displays the highland in a fan-shaped region around 2/5ΓM2/5\Gamma M (see the yellow region in Figure 2d), which deviates from the dip of ωq\omega_{\mathbf{q}} in Figure 2a and the peak of Πq\Pi_{\mathbf{q}} in Figure 2b. When the system is under 0.3 e−/f.u.0.3\ \mathrm{e}^{-}/\mathrm{f.u.} doping concentration, the distribution of ∣gq∣2\lvert g_{\mathbf{q}}\rvert^{2} is again very close to Πq\Pi_{\mathbf{q}} with a ridge-like feature centered at MM point (Figures. Figure 2f and Figure 2g), corresponding to the valley in ωq\omega_{\mathbf{q}} (Figure 2e). The calculated χq\chi_{\mathbf{q}} under 0.3 e−/f.u.0.3\ \mathrm{e}^{-}/\mathrm{f.u.} is shown in Figure 2h, and its peak at 1/2ΓM1/2\Gamma M corresponds to a 4×44 \times4 CDW, in stark contrast with the experimental observation[24]. Thus, we can conclude that ∣gq∣2\lvert g_{\mathbf{q}}\rvert^{2} provides the main contribution to Πq\Pi_{\mathbf{q}} and determines the phonon softening, confirming q-EPC as the driving force for the NbSe2\mathrm{NbSe}_{2} CDW formation as well as the CDW transition from 3×33 \times3 to 2×22 \times2 CDW under electron doping.

To elucidate the k\mathbf{k}-resolved contributions to Πq\Pi_{\mathbf{q}}, it is instructive to change the sum over k\mathbf{k} to the sum over q\mathbf{q}, which leads to:

Πk=∑q∣gk,k+q∣2f(εk)−f(εk+q)εk+q−εk.(5)\Pi_{\mathbf{k}} = \sum_{\mathbf{q}} \left|g_{\mathbf{k},\mathbf{k}+\mathbf{q}}\right|^2 \frac{f(\varepsilon_{\mathbf{k}})-f(\varepsilon_{\mathbf{k}+\mathbf{q}})}{\varepsilon_{\mathbf{k}+\mathbf{q}}-\varepsilon_{\mathbf{k}}}. \tag*{(5)}

Here, Πk\Pi_{\mathbf{k}} diagnostically indicates the distribution of the coupled electrons in the reciprocal space. For pristine NbSe2_2, the coupled electrons are concentrated on the KK pocket, and they display the maximum intensity at the ΓK\Gamma K path (see the red arc in Figure 3a). Interestingly, the high-intensity sector of Πk\Pi_{\mathbf{k}} is consistent with the full CDW gap position (see the white arrow in Figure 3b), as revealed by the calculated spectral function (see Supplementary information I for details). It is expected as these electrons are strongly disturbed by phonons. When NbSe2_2 is under electron doping, the intraband screening processes are suppressed, which decreases the coupling between electrons and phonons. Thus, the peak of Πk\Pi_{\mathbf{k}} decreases and its position moves towards the KK point due to the shrink of the K pocket under the electron doping (see the yellow arc in Figure 3c). And the band-gapped sector in the KK pocket also decreases with a full to partial gap transition (see the orange arrow in Figure 3d).

Calculated $\Pi_{\mathbf{k}}$ and simulated Fermi surfaces of NbSe2

Figure 3. (a) The calculated Πk\Pi_{\mathbf{k}} in the first BZ of pristine NbSe2_2. (b) The simulated Fermi surface of pristine NbSe2_2 in ground-state 3×33 \times3 CDW phase. (c) The calculated Πk\Pi_{\mathbf{k}} in the first BZ of NbSe2_2 under 0.3 e−^{-}/f.u. doping concentration. (d) The simulated Fermi surface of NbSe2_2 in ground-state 2×22 \times2 CDW phase under 0.3 e−^{-}/f.u. doping concentration. The white arrow in (b) denotes the full CDW gap. The orange arrow in (d) denotes the partial CDW gap. The Fermi surfaces of normal phases of NbSe2_2 are shown in Supplementary Figs. 2b and 2d.

A 2D Topological Superconductor

After studying the CDW properties of NbSe2_2, we now explore its superconducting properties. According to the Allen-Dynes modified McMillan theory[30], the Eliashberg spectral function is obtained by:

α2F(ω)=12Nq∑qνλqνωqνδ(ω−ωqν),(6)\alpha^2 F(\omega) = \frac{1}{2N_{\mathbf{q}}} \sum_{\mathbf{q}\nu} \lambda_{\mathbf{q}\nu}\omega_{\mathbf{q}\nu}\delta\left(\omega-\omega_{\mathbf{q}\nu}\right), \tag*{(6)}

where λqν\lambda_{\mathbf{q}\nu} is the electron-phonon coupling strength of phonon mode ν\nu with momentum q\mathbf{q}, ωqν\omega_{\mathbf{q}\nu} is the phonon frequency. The total EPC strength is given by:

λ=2∫0∞α2F(ω)ω dω.(7)\lambda= 2 \int_{0}^{\infty} \frac{\alpha^2 F(\omega)}{\omega}\,d\omega. \tag*{(7)}

The superconducting transition temperature TCT_C can be calculated by:

TC=ωlog⁡1.2exp⁡[−1.04(1+λ)λ−μ∗(1+0.62λ)].(8)T_C = \frac{\omega_{\log}}{1.2} \exp\left[\frac{-1.04(1+\lambda)}{\lambda-\mu^*(1+0.62\lambda)}\right]. \tag*{(8)}

Here, ωlog⁡\omega_{\log} is the logarithmically averaged phonon frequency, μ∗\mu^* is the effective screened Coulomb parameter which is estimated from the DOS at the Fermi energy:

μ∗≈0.26NF/(1+NF)\mu^* \approx0.26N_F/(1+N_F)[7, 21].

Figure 4a and S3a show the calculated phonon spectra for 2×22 \times2 hollow CDW and 2×22 \times2 filled CDW structures, respectively, under 0.3 e−0.3\ \mathrm{e}^{-}/f.u. doping concentration. The absence of imaginary phonon frequency indicates the stability of these two structures. And the small energy difference (∼0.8\sim0.8 meV/f.u., see Figure 1f) between these two structures suggests that both may exist in experiments. As shown in Figure 4a and Supplementary Figure 3a, the vibration of Se atoms is concentrated in the middle-frequency region (i.e., 17meV to 22meV), while Nb and Se atoms have similar contributions to the phonon DOS (PHDOS) outside this region. However, the high PHDOS of Se atoms in the middle-frequency region has small contributions to α2F(ω)\alpha^{2}F(\omega) as well as λ\lambda. The total EPC strength λ\lambda is calculated to be 0.57 (0.54) for the 2×22 \times2 hollow (2×22 \times2 filled) CDW phase. Considering the effective screened Coulomb parameter μ∗\mu^{*} of 0.15, the TCT_{\mathrm{C}} is estimated to be 1.7 K and 1.3 K for 2×22 \times2 hollow CDW and filled CDW, respectively, both of which are smaller than the TC∼3T_{\mathrm{C}} \sim3 K for the 3×33 \times3 CDW[14, 16]. Thus, the superconductivity of NbSe2_2 is suppressed under 0.3 e−^{-}/f.u. doping concentration, which is consistent with the previous experimental results of the electron-doped 2D NbSe2_2[17, 21, 22, 23]. The main reason for this suppression is due to the reduced λ\lambda of the 2×22 \times2 CDW systems under electron doping[8].

Phonon spectrum, PHDOS, Eliashberg spectral function, integrated EPC, band structure, and edge states

Figure 4. (a) The phonon spectrum, PHDOS, Eliashberg spectral function α2F(ω)\alpha^{2}F(\omega) and frequency-dependent integrated EPC λ(ω)\lambda(\omega) of 2×22 \times2 hollow CDW under 0.3 e−0.3\ \mathrm{e}^{-}/f.u. doping concentration. (b) The band structure of 2×22 \times2 hollow CDW under 0.3 e−0.3\ \mathrm{e}^{-}/f.u. doping concentration with (blue solid lines) and without (black dashed lines) SOC. (c) The edge states of 2×22 \times2 hollow CDW are projected on the (100) edge. Red colors indicate higher local DOS and blue colors represent the bulk band gap. The high-symmetry points are indicated in Figure S1.

Figure 4b shows the electronic band structure of 2×22 \times2 hollow CDW of NbSe2_2 with and without spin-orbital coupling (SOC). Without SOC, there is a Weyl node protected by the mirror symmetry on the ΓM∗\Gamma M^{*} path. The SOC opens a band gap of about 15 meV (see the red circle in Figure 4b), resulting in the nontrivial topological phase characterized by a nonzero topological invariant Z2=1Z_{2}=1. According to the bulk-edge correspondence, the nonzero Z2Z_{2} invariant is closely related to the nontrivial helical edge states that emerge inside the gap between two energy bands in a semi-infinite system. As presented in Figure 4c, there are Dirac cone edge states connecting the valence and conduction bands. Therefore, the 2×22 \times2 hollow CDW phase is a 2D superconductor with clearly visible topological edge states near the Fermi level, which is rarely reported in 2D systems and may have promising applications in fault-tolerant quantum computation[33, 34, 35].

Conclusion

In summary, using first-principles calculations and mean-field theory, we construct a theoretical framework to study the mechanism of CDW formation and CDW transition in NbSe2NbSe_{2} from both phononic and electronic perspectives. We demonstrate that qq-EPC makes the dominant contribution to the 3×33 \times3 CDW formation of NbSe2NbSe_{2} as well as the transition to 2×22 \times2 CDW under electron doping. In addition, we find that electron doping suppresses both the qq-EPC ∣gq∣2\lvert g_{\mathbf{q}}\rvert^{2} and the total EPC strength λ\lambda, leading to the simultaneous suppression of CDW and superconducting orders. All these results agree with previous works. More importantly, to the best of our knowledge, the 2×22 \times2 hollow CDW phase of monolayer NbSe2NbSe_{2} under 0.3 e-/f.u. doping is the first reported topological superconductor driven by CDW transition. Such phenomenon is also found in monolayer TaSe2TaSe_{2}. Our seminal work not only deepens the understanding of CDW theory, but also presents a new strategy for developing topological superconductor.

Acknowledgments

C.C. thanks for the support from Shuimu Tsinghua Scholar Program. This research project was funded by the Ministry of Education, Singapore, under its MOE AcRF Tier 3 Award MOE2018-T3-1-002, and MOE AcRF Tier 2 Award MOE2019-T2-2-030. Computations were supported by the Center of Advanced 2D Materials (CA2DM) HPC infrastructure.

Competing Interests

The authors declare no competing financial or non-financial interests.

References

  1. [7]Zheng, F.; Feng, J. Electron-Phonon Coupling and the Coexistence of Superconductivity and Charge-Density Wave in Monolayer NbSe₂. Phys. Rev. B 2019, 99 (16), 161119(R). https://doi.org/10.1103/PhysRevB.99.161119.
  2. [8]Lian, C. S.; Si, C.; Duan, W. Unveiling Charge-Density Wave, Superconductivity, and Their Competitive Nature in Two-Dimensional NbSe₂. Nano Lett. 2018, 18 (5), 2924–2929. https://doi.org/10.1021/acs.nanolett.8b00237.
  3. [12]Zhu, X.; Cao, Y.; Zhang, J.; Plummer, E. W.; Guo, J. Classification of Charge Density Waves Based on Their Nature. Proc. Natl. Acad. Sci. U. S. A. 2015, 112 (8), 2367. https://doi.org/10.1073/pnas.1424791112.
  4. [14]Xi, X.; Zhao, L.; Wang, Z.; Berger, H.; Forró, L.; Shan, J.; Mak, K. F. Strongly Enhanced Charge-Density-Wave Order in Monolayer NbSe₂. Nat. Nanotechnol. 2015, 10 (9), 765–769. https://doi.org/10.1038/nnano.2015.143.
  5. [15]Ugeda, M. M.; Bradley, A. J.; Zhang, Y.; Onishi, S.; Chen, Y.; Ruan, W.; Ojeda-Aristizabal, C.; Ryu, H.; Edmonds, M. T.; Tsai, H. Z.; Riss, A.; Mo, S. K.; Lee, D.; Zettl, A.; Hussain, Z.; Shen, Z. X.; Crommie, M. F. Characterization of Collective Ground States in Single-Layer NbSe₂. Nat. Phys. 2016, 12 (1), 92. https://doi.org/10.1038/nphys3527.
  6. [16]Xi, X.; Wang, Z.; Zhao, W.; Park, J. H.; Law, K. T.; Berger, H.; Forró, L.; Shan, J.; Mak, K. F. Ising Pairing in Superconducting NbSe₂ Atomic Layers. Nat. Phys. 2016, 12 (2), 139–143. https://doi.org/10.1038/nphys3538.
  7. [17]Yoshida, M.; Ye, J.; Nishizaki, T.; Kobayashi, N.; Iwasa, Y. Electrostatic and Electrochemical Tuning of Superconductivity in Two-Dimensional NbSe₂ Crystals. Appl. Phys. Lett. 2016, 108 (20), 202602. https://doi.org/10.1063/1.4950804.
  8. [18]Lin, D.; Li, S.; Wen, J.; Berger, H.; Forró, L.; Zhou, H.; Jia, S.; Taniguchi, T.; Watanabe, K.; Xi, X.; Bahramy, M. S. Patterns and Driving Forces of Dimensionality-Dependent Charge Density Waves in 2H-Type Transition Metal Dichalcogenides. Nat. Commun. 2020, 11 (1), 2406. https://doi.org/10.1038/s41467-020-15715-w.
  9. [19]Chen, Y.; Wu, L.; Xu, H.; Cong, C.; Li, S.; Feng, S.; Zhang, H.; Zou, C.; Shang, J.; Yang, S. A.; Loh, K. P.; Huang, W.; Yu, T. Visualizing the Anomalous Charge Density Wave States in Graphene/NbSe₂ Heterostructures. Adv. Mater. 2020, 32 (45), 2003746. https://doi.org/10.1002/adma.202003746.
  10. [20]José Ángel Silva-Guillén; Pablo Ordejón; Francisco Guinea; Canadell, E. Electronic Structure of 2H-NbSe₂ Single-Layers in the CDW State. 2D Mater. 2016, 3, 035028. https://doi.org/10.1088/2053-1583/3/3/035028.
  11. [21]Xi, X.; Berger, H.; Forró, L.; Shan, J.; Mak, K. F. Gate Tuning of Electronic Phase Transitions in Two-Dimensional NbSe₂. Phys. Rev. Lett. 2016, 117 (10), 106801. https://doi.org/10.1103/PhysRevLett.117.106801.
  12. [22]Li, Z. J.; Gao, B. F.; Zhao, J. L.; Xie, X. M.; Jiang, M. H. Effect of Electrolyte Gating on the Superconducting Properties of Thin 2H-NbSe₂ Platelets. Supercond. Sci. Technol. 2014, 27 (1), 015004. https://doi.org/10.1088/0953-2048/27/1/015004.
  13. [23]Luo, H.; Strychalska-Nowak, J.; Li, J.; Tao, J.; Klimczuk, T.; Cava, R. J. Shaped Suppression of the Superconducting Transition Temperature in Cu-Intercalated NbSe₂. Chem. Mater. 2017, 29 (8), 3704–3712. https://doi.org/10.1021/acs.chemmater.7b00655.
  14. [24]Leriche, R. T.; Palacio-morales, A.; Campetella, M.; Tresca, C.; Sasaki, S.; Brun, C.; Debontrider, F.; David, P.; Arfaoui, I.; Šofranko, O.; Samuely, T.; Kremer, G.; Monney, C.; Jaouen, T.; Cario, L.; Calandra, M.; Cren, T. Misfit Layer Compounds : A Platform for Heavily Doped 2D Transition Metal Dichalcogenides. Adv. Funct. Mater. 2021, 2007706, 1–10. https://doi.org/10.1002/adfm.202007706.
  15. [25]Kusmartseva, A. F.; Sipos, B.; Berger, H.; Forró, L.; Tutiš, E. Pressure Induced Superconductivity in Pristine 1T-TiSe₂. Phys. Rev. Lett. 2009, 103 (23), 236401. https://doi.org/10.1103/PhysRevLett.103.236401.
  16. [26]Sipos, B.; Kusmartseva, A. F.; Akrap, A.; Berger, H.; Forró, L.; Tuti, E. From Mott State to Superconductivity in 1T-TaS₂. Nat. Mater. 2008, 7 (12), 960–965. https://doi.org/10.1038/nmat2318.
  17. [27]Gye, G.; Oh, E.; Yeom, H. W. Topological Landscape of Competing Charge Density Waves in 2H-NbSe₂. Phys. Rev. Lett. 2019, 122 (1), 016403. https://doi.org/10.1103/PhysRevLett.122.016403.
  18. [28]Oh, E.; Gye, G.; Yeom, H. W. Defect-Selective Charge-Density-Wave Condensation in 2H-NbSe₂. Phys. Rev. Lett. 2020, 125 (3). https://doi.org/10.1103/PhysRevLett.125.036804.
  19. [29]Flicker, F.; Van Wezel, J. Charge Order in NbSe₂. Phys. Rev. B 2016, 94 (23), 235135. https://doi.org/10.1103/PhysRevB.94.235135.
  20. [30]Giustino, F. Electron-Phonon Interactions from First Principles. Rev. Mod. Phys. 2017, 89 (1), 015003. https://doi.org/10.1103/RevModPhys.89.015003.
  21. [31]Wang, Z.; Zhou, J.; Loh, K. P.; Feng, Y. P. Controllable Phase Transitions between Multiple Charge Density Waves in Monolayer 1T-VSe₂ via Charge Doping. Appl. Phys. Lett. 2021, 119 (16), 163101. https://doi.org/10.1063/5.0068241.
  22. [32]Johannes, M. D.; Mazin, I. I. Fermi Surface Nesting and the Origin of Charge Density Waves in Metals. Phys. Rev. B 2008, 77 (16), 165135. https://doi.org/10.1103/PhysRevB.77.165135.
  23. [33]Pan, X. C.; Chen, X.; Liu, H.; Feng, Y.; Wei, Z.; Zhou, Y.; Chi, Z.; Pi, L.; Yen, F.; Song, F.; Wan, X.; Yang, Z.; Wang, B.; Wang, G.; Zhang, Y. Pressure-Driven Dome-Shaped Superconductivity and Electronic Structural Evolution in Tungsten Ditelluride. Nat. Commun. 2015, 6, 7805. https://doi.org/10.1038/ncomms8805.
  24. [34]Liu, Y.; Zhao, J. Z.; Yu, L.; Lin, C. T.; Liang, A. J.; Hu, C.; Ding, Y.; Xu, Y.; He, S. L.; Zhao, L.; Liu, G. D.; Dong, X. L.; Zhang, J.; Chen, C. T.; Xu, Z. Y.; Weng, H. M.; Dai, X.; Fang, Z.; Zhou, X. J. Identification of Topological Surface State in PdTe2 Superconductor by Angle-Resolved Photoemission Spectroscopy. Chinese Phys. Lett. 2015, 32 (6), 067303. https://doi.org/10.1088/0256-307X/32/6/067303.
  25. [35]Qi, Y.; Naumov, P. G.; Ali, M. N.; Rajamathi, C. R.; Schnelle, W.; Barkalov, O.; Hanfland, M.; Wu, S. C.; Shekhar, C.; Sun, Y.; Süß, V.; Schmidt, M.; Schwarz, U.; Pippel, E.; Werner, P.; Hillebrand, R.; Förster, T.; Kampert, E.; Parkin, S.; Cava, R. J.; Felser, C.; Yan, B.; Medvedev, S. A. Superconductivity in Weyl Semimetal Candidate MoTe2. Nat. Commun. 2016, 7, 11038. https://doi.org/10.1038/ncomms11038.

Paper details

vlnc:W_5gzm958e
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents