betaFeedback

WorksPhysics and Astronomy

Complete Raman Tensor Determination in Birefringent ββ-Ga2_2O3_3 by Single-Stage Hyperspectral Analysis of Polarization Angle-Resolved Raman Spectra

Abstract

The low symmetry of the monoclinic phase of Ga2_2O3_3 leads to pronounced optical anisotropy and, consequently, to birefringence, which strongly affects the Raman response. Because Raman scattering is fundamentally sensitive to the polarizability of a material, this anisotropy must be carefully accounted for in order to extract quantitative information - an effort that has only recently been shown to be feasible in such media. Here, we report Raman measurements from all three principal crystal planes (100)(100), (010)(010), and (001)(001), as well as from the (2‾01)(\overline{2}01)-plane of a ββ-Ga2_2O3_3 single crystal. By combining polarization angle-resolved Raman spectroscopy (PARRS) with a newly developed fitting procedure and explicitly accounting for birefringence, we achieve full spectral separation and quantitatively determine the energies and relative Raman tensor elements of all 15 Raman-active modes.

Introduction

The ultra-wide-band-gap semiconductor β\beta-Ga2_2O3_3 has attracted significant attention as a promising material for next-generation power electronics, owing to its widely tunable electrical conductivity, high breakdown field, and the availability of large, scalable substrates for homoepitaxial growth [1, 2, 3, 4, 5, 6, 7, 8].

β\beta-Ga2_2O3_3 crystallizes in a low-symmetry monoclinic structure, with mutually unequal lattice parameters aa, bb, and cc, and a monoclinic angle of 103.8∘103.8^\circ between the aa and cc axes (Figure 1a). This structural anisotropy gives rise to pronounced direction-dependent optical properties [9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29], including a strongly anisotropic Raman response [25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43]. Owing to its biaxial optical symmetry [44], the dielectric tensor of β\beta-Ga2_2O3_3 exhibits three distinct diagonal elements, εx~x~\varepsilon_{\tilde{x}\tilde{x}}, εy~y~\varepsilon_{\tilde{y}\tilde{y}}, and εz~z~\varepsilon_{\tilde{z}\tilde{z}}, when expressed in its eigensystem (x~\tilde{x}, y~\tilde{y}, z~\tilde{z}) [45]. As a consequence, birefringence arises for most light-propagation directions, posing a challenge for the quantitative analysis of Raman scattering — an effort long regarded as “pointless” in optically anisotropic media [46]. For this reason, most Raman studies in the literature have neglected birefringence and instead focused on properties that remain unaffected in polarised [39, 40, 47, 48, 49, 50, 51] or temperature-dependent measurements [41, 52, 53]. Only few studies have explicitly accounted for birefringence: either by introducing a complex Raman tensor [31], or by incorporating the birefringence-dependent physical processes that accompany Raman scattering directly into the analytical model [42].

Image not extracted

Figure 1. a) Unit cell of β\beta-Ga2_2O3_3. The (100), (010), (001) and (201) planes are indicated in different colors. The crystallographic plot was created using VESTA [63]. b) Relation between the crystallographic, principal, and sample surface coordinate systems in β\beta-Ga2_2O3_3.

In this work, we use polarized, angle-resolved Raman scattering (PARRS) adapting the model proposed by Kranert et al. [30, 42], to calculate the PARRS profiles, i. e. the polarization angle dependent intensity, in birefringent media. We develop a new fitting procedure for the hyperspectral data which improves accuracy and enables reliable differentiation of strongly overlapping phonon modes of different symmetries. Applied to β\beta-Ga2_2O3_3, this procedure enables the reliable separation of all Raman active modes and, hence, to determine their energies and relative Raman tensor elements, including the previously unresolved mode pairs Ag(5)/Bg(3)\mathrm{A}_{g}^{(5)}/\mathrm{B}_{g}^{(3)}, Ag(7)/Bg(4)\mathrm{A}_{g}^{(7)}/\mathrm{B}_{g}^{(4)} and Bg(5)/Ag(9)\mathrm{B}_{g}^{(5)}/\mathrm{A}_{g}^{(9)}.

Experimental Methods

Raman scattering measurements were performed at room temperature using the 633 nm line of a HeNe laser and a custom-modified LabRAM HR 800 spectrometer (Horiba Jobin-Yvon). The laser was focused onto the sample through a 50× Olympus microscope objective (NA = 0.55), and scattered light was collected in backscattering geometry. Samples were positioned with their surface normal along the light propagation direction. Inelastically scattered light was dispersed by the 800 mm monochromator equipped with a 1800 lines/mm grating and detected by a CCD. A half-wave plate (λ/2\lambda/2) in the excitation path was set at 0° or 45° to align the incident linear polarization parallel or perpendicular to the detected scattered light, which was selected with a fixed polarizer. Raman spectra were calibrated using multiple neon emission lines. Polarization angle-resolved Raman measurements (PARRS) were performed by introducing an additional half-wave plate between notch filter and the objective, which rotates the polarization of both the incident (e^i\hat{e}_i) and scattered (e^s\hat{e}_s) light by an angle ϕ\phi relative to the fixed sample orientation, effectively simulating a sample rotation. The wave plate is mounted in a motorized, computer-controlled holder, enabling automated recording of polarization-angle-dependent intensity profiles to determine relative Raman tensor elements [42, 54, 55] or the thickness of thin films [56].

Raman spectra were acquired for (100)-, (010)-, (001)- and (201)-oriented β\beta-Ga2_2O3_3 single crystals. The samples were cut from the same undoped, two-inch-diameter crystals grown by the Czochralski method at Leibniz-Institut für Kristallzüchtung using an Ir crucible and an oxidizing growth atmosphere [57, 58], and chemically–mechanically polished. Hall-effect measurements indicate a free-electron concentration of 3.4×1017 cm−33.4 \times10^{17}\ \mathrm{cm}^{-3} and an electron mobility of 118 cm2V−1s−1118\ \mathrm{cm}^{2}\mathrm{V}^{-1}\mathrm{s}^{-1} [59]. The crystals exhibit high structural quality, with no twins, low-angle grain boundaries, or nanopipes, and a dislocation density below ∼103 cm−3\sim10^3\ \mathrm{cm}^{-3} [60].

A newly developed hyperspectral fitting procedure was used for the analysis and is described below. Spectroscopic analysis was performed in part using a non-public alpha version of peak-o-mat2; the stable version is publicly available on GitHub [61, 62].

Results and discussion

The monoclinic unit cell of β\beta-Ga2_2O3_3 contains 10 atoms, giving rise to 30 phonon branches. At the Γ\Gamma point they decompose into the irreducible representations of the C2hC_{2h} point group [64]

Γ=5Au+10Bu+10Ag+5Bg,\Gamma= 5A_u + 10B_u + 10A_g + 5B_g,

where Γaco=Au+2Bu\Gamma_{\mathrm{aco}} = A_u + 2B_u are the acoustic phonons. The optical modes of even parity (index g) are Raman-active with Raman tensors of the form

R:Ag=(ad0db000c),Bg=(00e00fef0),(1)\mathcal{R}: A_g = \begin{pmatrix} a & d & 0 \\ d & b & 0 \\ 0 & 0 & c \end{pmatrix}, \quad B_g = \begin{pmatrix} 0 & 0 & e \\ 0 & 0 & f \\ e & f & 0 \end{pmatrix}, \tag*{(1)}

whereas the modes of odd parity (index u) are IR-active.

We introduce three different coordinate systems, as depicted in Figure 1b, to facilitate the discussion of the crystal’s properties and the analysis: (1) The crystallographic coordinate system (black) where aa, bb, and cc are aligned with the crystallographic directions [100], [10], and [1], respectively. aa and cc enclose the monoclinic angle β=103.8∘\beta= 103.8^\circ. (2) The orthonormal principal axis coordinate system (red), where x~\tilde{x}, y~\tilde{y}, and z~\tilde{z} are defined by the eigenvectors of the dielectric tensor, where z~∥\tilde{z} \parallel [10] due to their natural coincidence. We note that the x~\tilde{x} and y~\tilde{y} vectors’ orientation within the (010)-plane and absolute magnitude are wavelength dependent. For an excitation wavelength of 632.8 nm, y~\tilde{y} and [100] enclose an angle of α=2.33∘\alpha= 2.33^\circ and the dielectric tensor reads in its eigensystem [13, 65]

ε=(3.7270003.6240003.768).(2)\varepsilon= \begin{pmatrix} 3.727 & 0 & 0 \\ 0 & 3.624 & 0 \\ 0 & 0 & 3.768 \end{pmatrix}. \tag*{(2)}

This is the coordinate system in which the Raman tensors in equation 1 are defined. (3) The orthonormal sample coordinate systems (xp′x'_p, yp′y'_p, zp′z'_p) for each of the investigated crystal planes pp. zp′z'_p is chosen to align to the surface normal, i. e. to coincide with the microscope’s optical axis. Consequently, xp′x'_p lies within the pp-plane and is chosen to be aligned with a principal axis; on the bb-plane xb′∥x~x'_b \parallel\tilde{x}, whereas xp′∥z~∥x'_p \parallel\tilde{z} \parallel [10] on the other investigated planes. We note that another commonly used system is the orthonormal quasi-crystallographic coordinate system where two out of (x,y,z)(x, y, z) are chosen to be parallel to the aa and bb lattice vectors. Different definitions are common to different fields, so care should be taken when comparing anisotropic properties [45]. However, this system is not required to understand the arguments in this study. A detailed description of the above systems and their respective transformations is given in the supplemental material [66].

To calculate the Raman selection rules for a given surface geometry, one typically uses the well-established expression

I∝∣e^sRe^i∣2(3)I \propto\left|\hat{e}_{s}R\hat{e}_{i}\right|^{2} \tag*{(3)}

where RR is the Raman tensor and e^i\hat{e}_{i} and e^s\hat{e}_{s} are the incident and scattered polarization vectors, respectively, commonly transformed from the dielectric tensor system (x~,y~,z~)(\tilde{x},\tilde{y},\tilde{z}) (cf. Eq. (1)) into the respective surface system (xp′,yp′,zp′)(x'_{p},y'_{p},z'_{p}). For parallel scattering configuration, they are given by e^i∥=e^s∥=(cos⁡(φ),sin⁡(φ),0)\hat{e}_{i}^{\parallel}=\hat{e}_{s}^{\parallel}=(\cos(\varphi),\sin(\varphi),0), whereas for crossed configuration they read e^i⊥=(cos⁡(φ),sin⁡(φ),0)\hat{e}_{i}^{\perp}=(\cos(\varphi),\sin(\varphi),0) and e^s⊥=(−sin⁡(φ),cos⁡(φ),0)\hat{e}_{s}^{\perp}=(-\sin(\varphi),\cos(\varphi),0). Here, φ\varphi denotes the surface system polarization angle, which is related to the measurement polarization angle ϕ\phi through ϕ=φ−φ0\phi=\varphi-\varphi_{0}. Hence, φ0\varphi_{0} denotes the offset between the crystal orientation with respect to the setup-defined origin of the polarization, so that φ=0∘\varphi=0^{\circ} corresponds to e^i∥xp′\hat{e}_{i}\parallel x'_{p} and φ=90∘\varphi=90^{\circ} to e^i∥yp′\hat{e}_{i}\parallel y'_{p}.

Here, for β\beta-Ga2_{2}O3_{3}, the influence of birefringence must be taken into account when calculating the angle-dependent selection rules. To this end, we follow the approach proposed by Kranert et al. [30, 42], which is briefly summarized in the following.

The most fundamental consequence is that the polarization vectors of the incident and scattered radiation cannot be regarded as fixed during propagation through the birefringent crystal because their relative phase is constantly retarded. However, for excitations within the transparency regime, i.e. large penetration depths, as well as pronounced birefringence, this effect can be accounted for by employing

I∝∣e^sR0e^i∣2+∣e^sR1e^i∣2+∣e^sR2e^i∣2,(4)I \propto\left|\hat{e}_{s}R_{0}\hat{e}_{i}\right|^{2}+\left|\hat{e}_{s}R_{1}\hat{e}_{i}\right|^{2}+\left|\hat{e}_{s}R_{2}\hat{e}_{i}\right|^{2}, \tag*{(4)}

where

R0=(r0000),R1=(0r1r10),R2=(000r2)(5)R_{0}=\begin{pmatrix}r_{0}&0\\0&0\end{pmatrix},\qquad R_{1}=\begin{pmatrix}0&r_{1}\\r_{1}&0\end{pmatrix},\qquad R_{2}=\begin{pmatrix}0&0\\0&r_{2}\end{pmatrix} \tag*{(5)}

are summands of the Raman tensor represented in the corresponding two-dimensional surface system (xp′,yp′)(x'_{p},y'_{p}), such that R=R0+R1+R2R=R_{0}+R_{1}+R_{2}. Another consequence of optical anisotropy is that the eigenpolarizations inside the crystal may exhibit an out-of-plane component when the propagation direction does not coincide with one of the principal axes. Consequently, the external polarization vectors are transformed into the allowed internal polarizations of the crystal by using the transformation matrix

T=(1000εz′z′(εy′z′2+εz′z′2)−1/200εy′z′(εy′z′2+εz′z′2)−1/2).(6)T=\begin{pmatrix} 1&0&0\\ 0&\varepsilon_{z'z'}\left(\varepsilon_{y'z'}^{2}+\varepsilon_{z'z'}^{2}\right)^{-1/2}&0\\ 0&\varepsilon_{y'z'}\left(\varepsilon_{y'z'}^{2}+\varepsilon_{z'z'}^{2}\right)^{-1/2}& \end{pmatrix}. \tag*{(6)}

Here, εy′z′\varepsilon_{y'z'} and εz′z′\varepsilon_{z'z'} denote the corresponding components of the dielectric tensor transformed into the surface system in the same way as the Raman tensor. In addition, a transmission correction is introduced which takes into account the different Fresnel transmission coefficients of s- and p-polarized light at the crystal surface. This correction is implemented by applying the diagonal matrix ρ=diag⁡(tx′x′,ty′y′,1)\rho=\operatorname{diag}(t_{x'x'},t_{y'y'},1) to both the incident and scattered polarization vectors. Here, tx′x′=2/(εx′x′+1)t_{x'x'}=2/(\sqrt{\varepsilon_{x'x'}}+1) denotes the Fresnel transmission coefficient for normal incidence along x^p′\hat{x}'_{p} with polarization parallel to xp′x'_{p}, while ty′y′t_{y'y'} is defined analogously for polarization along yp′y'_{p}. Similarly, birefringence affects the effective solid angle from which scattered light is collected by the microscope objective by changing the refraction of the collection cone inside the crystal. To account for this effect, the solid angle Ω=4πsin⁡2(arcsin⁡(NA/ε)/2)\Omega=4\pi\sin^{2}(\arcsin(NA/\sqrt{\varepsilon})/2) is evaluated for different refractive indices and the correction matrix Z=diag⁡(Ωx′x′,Ωy′y′,1)Z=\operatorname{diag}(\sqrt{\Omega_{x'x'}},\sqrt{\Omega_{y'y'}},1) is applied to the transformed Raman tensor.

In conclusion, the Raman selection rules are obtained by first constructing the effective transformed Raman tensor

Reff=ρTTZRTρ(7)R_{\mathrm{eff}}=\rho T^{T}ZRT\rho \tag*{(7)}

and subsequently inserting it into equation 4, using the decomposition of the Raman tensor defined in equation 5.

Finally, to derive the numerical values of the tensor elements, one has to account for a wavelength dependent prefactor that originates in the nature of dipole scattering [67]:

C(ωp)=ωi(ωi−ωp)3ωp[1−exp⁡(−ℏωpkBT)].(8)C(\omega_{p})=\frac{\omega_{i}(\omega_{i}-\omega_{p})^{3}}{\omega_{p}\left[1-\exp\left(-\frac{\hbar\omega_{p}}{k_{\mathrm{B}}T}\right)\right]}. \tag*{(8)}

Figure 2 displays Raman spectra resolving all 15 Raman-active phonons (10Ag+5Bg10A_{g}+5B_{g}) via a set of dedicated polarization geometries. Scattering geometries are indicated using the Porto notation k^i(e^ie^s)k^s\hat{k}_{i}( \hat{e}_{i}\hat{e}_{s})\hat{k}_{s}, where k^i\hat{k}_{i} and k^s\hat{k}_{s} denote the propagation directions of the incident and scattering light, respectively. The combination of polarization-dependent measurements and Raman selection rules allows the selected detection and differentiation of all AgA_{g} and BgB_{g} modes. This enables the determination of the phonon frequencies for the closely-spaced Ag(5)/Bg(3)A_{g}^{(5)}/B_{g}^{(3)}, Ag(7)/Bg(4)A_{g}^{(7)}/B_{g}^{(4)} and Bg(5)/Ag(9)B_{g}^{(5)}/A_{g}^{(9)} mode pairs despite their spectral overlap from the respective other mode.

As predicted by Raman selection rules, the AgA_{g} modes experience (local) maximum intensity in parallel-polarization scattering geometries with e^i\hat{e}_{i} and e^s\hat{e}_{s} parallel to one of the principal directions (i.e. x~\tilde{x}, y~\tilde{y} or z~\tilde{z}), while modes of BgB_{g} symmetries are absent in these scattering conditions. To acquire spectra only allowing BgB_g modes, (100), (001) and (201) planes are measured with crossed polarization, while e^i\hat{e}_i and e^s\hat{e}_s are parallel to different principal directions. When exciting along the [10] direction, BgB_g modes are always prohibited according to Raman selection rules, regardless of the selected polarization configuration. By fitting Lorentzian line shape functions to the spectra depicted in Figure 2, we determine the peak positions of all 15 Raman-active phonon modes (listed in Tab. I). The obtained results show good agreement with previous experimental [39, 40, 41, 42, 47, 48] and theoretical [40, 41, 42, 43, 47] studies.

Image not extracted

Figure 2. Polarized Raman spectra as measured on the four investigated crystal planes in parallel and crossed polarization scattering geometries. Due to the two-fold rotational symmetry in the parallel polarized spectra, both spectra, with the polarization aligned along one of the sample surface axes (xp′x'_p, yp′y'_p) are plotted. The Raman spectra are depicted with the square root of the intensity for better visualization of small peaks.

We extend this investigation by removing the constraint that the light polarization must be parallel to the principal axes and instead measure Raman spectra in parallel and crossed configuration rotating the light polarization around the crystal surface normal. Figure 3 depicts a representative contour plot of these PARRS spectra on the a-plane in parallel (top) and crossed polarization (bottom) for a sequence of rotational polarization angles ϕ\phi with respect to the fixed sample. ϕ=0\phi= 0 marks the onset of the measurement. Angles coincident with the

Image not extracted

Figure 3. Contour plot of the polarization dependent Raman spectra on the a-plane for parallel (middle) and crossed scattering geometries (bottom). Angles, where xa′∥[010]x'_a \parallel[010] and ya′∥[001]y'_a \parallel[001] are labeled. In the top panel Raman spectra with a polarization angle of ϕ=150∘\phi= 150^\circ are depicted, while the panels on the right show the integrated intensity in the range of the Ag(7)/Bg(4)A_g^{(7)}/B_g^{(4)} pair and the corresponding slice of the fit. The Raman spectra and contour plots are depicted with the square root of the intensity for better visualization of small peaks.

principal axes xa′∥[010]x'_a \parallel[010] and ya′∥[001]y'_a \parallel[001] are labeled and correspond to the spectra plotted in Figure 2. For quantitative analysis, PARRS profiles, i. e. the Raman intensity of each mode expressed as a function of the rotational angle ϕ\phi, are conventionally obtained by individually fitting the Raman spectra and plotting the peak’s intensities over the polarization angle ϕ\phi to fit the relative Raman tensor elements in a consecutive step. Here, we present a new approach where the hyperspectral data is fitted in a single step to obtain the phonon energies, full width at half maximum, and the relative tensor elements. The fit function mainly comprises a two-dimensional function for each of the scattering geometries (sg), i. e. for all combinations of surface plane and polarization configuration:

Fsg(ω,ϕ)=ssg∑iLi(ω)Ai,sg(ϕ)+Bsg(ω,ϕ),F_{\mathrm{sg}}(\omega,\phi)=s_{\mathrm{sg}}\sum_i L_i(\omega)A_{i,\mathrm{sg}}(\phi)+B_{\mathrm{sg}}(\omega,\phi),

where ssg≈1s_{\mathrm{sg}}\approx1 is a scaling factor to account for slight differences in focus and surface roughness induced reflectances, and LiL_i, AiA_i and BsgB_{\mathrm{sg}} denote the Lorentzian line-shape and the PARRS profile of the i-th Raman-active mode, and the background function, respectively. The $L_i】【。 further include the phonon energy and line broadening, while the AiA_i contain parameters of the crystal’s symmetry and scattering properties, i. e. the relative Raman tensor elements. Additional parameters are included to account for experimental artifacts such as a background, slight differences in focus, etc.

Although the presented fitting procedure shows negligible benefits for materials yielding Raman spectra with well isolated peaks, the opposite is true when peaks strongly overlap. By including the modes’ predicted angle responses, it becomes possible to reliably fit spectra with peaks overlapping beyond the spectral resolution, where fits of a single spectrum yield peak intensities with extensive errors. Therefore, in β-Ga2_2O3_3, the newly presented procedure yields a significantly better fit to the hyperspectral data set.

Slices of the fit result are presented alongside the exemplary Raman spectrum and angle dependence of the Ag(8)A_g^{(8)} mode in the top and right panels in Figure 3 as a solid black line. The low deviation from the experimental data provides evidence of an excellent fit. The complete set of data including all PARRS contour plots and plots of the fitted model and residuals is provided in the supplemental material [66].

It is worth mentioning that the determined Raman tensor elements are relative quantities and are therefore typically scaled in such a way that the largest tensor element has a value of 1000; here, this is the case for the aa parameter of the Ag(10)A_g^{(10)} mode. The normalized relative Raman tensor elements are listed in Table I. Our determined tensor elements agree well with most of the experimental values reported in Ref. [42]. Some deviations are likely related to systematic differences, including variations in the experimental setup and the fitting procedure. However, the individual contribution of the systematic errors cannot be distinguished based on the present comparison. Yet, we consider the major contribution to originate from an improved accuracy obtained by the hyperspectral fitting, as this approach enables the determination of the Raman tensor elements for the Bg(3)B_g^{(3)} and Bg(4)B_g^{(4)} modes, which could previously not be determined experimentally and which are in good agreement with the values predicted by theory [42].

ωp\omega_p (cm−1^{-1})aabb∣c∣\lvert c\rvertddeeffC(ωp)C(\omega_p)
Ag(1)A_g^{(1)}111.418−5518−21.000
Ag(2)A_g^{(2)}170.4102140122−70.479
Ag(3)A_g^{(3)}200.9186429321110.364
Ag(4)A_g^{(4)}320.9961471431250.176
Ag(5)A_g^{(5)}347.2428123324−130.157
Ag(6)A_g^{(6)}417.03703013461470.121
Ag(7)A_g^{(7)}475.664−300306−350.101
Ag(8)A_g^{(8)}630.456383232−1540.070
Ag(9)A_g^{(9)}658.5433971343170.066
Ag(10)A_g^{(10)}766.9100038296−3230.055
Bg(1)B_g^{(1)}114.834340.946
Bg(2)B_g^{(2)}145.5119710.626
Bg(3)B_g^{(3)}353.5169−370.153
Bg(4)B_g^{(4)}476.635−2360.101
Bg(5)B_g^{(5)}652.61483590.067

Table I. Phonon mode irreducible representations, determined frequencies ωp\omega_p, Raman tensor elements aa, bb, cc, dd, ee, ff, and scattering strength prefactors C(ωp)C(\omega_p) of the Raman active phonons as obtained by polarization angle-resolved Raman measurements. The tensor elements and C(ωp)C(\omega_p) prefactors are normalized to a value of a=1000a=1000 for the Ag(10)A_g^{(10)} mode and to C(Ag(1))=1C(A_g^{(1)})=1. The error of the phonon energies can be considered well below the spectral resolution of 0.5 cm−1^{-1}.

Since Raman spectra are measured intensities, i. e. formally a quadratic function of the tensor elements, it is often considered that the tensor elements’ signs cannot be determined. This, however, is not necessarily true when scattering information from multiple planes is available: the functions describing the PARRS profiles on planes where the surface normal is not a principal axis of the dielectric tensor will include linear combinations of the tensor elements. These combinations can reveal from the experimental data whether their signs are equal or opposite. Here, due to the set of investigated planes, the tensor elements group as (a,b,d)(a,b,d) and (e,f)(e,f). Hence, fixing the sign of aa and ee to be positive yields the relative sign of bb, dd and ff, respectively. Solely the element cc enters quadratically into all fit formulae (cf. Tab. S2 in the SI). Crystal planes excluding those that contain zz within the surface and the (010) plane, such as the (110)-plane, link the AgA_g-modes’ cc element to the (a,b,d)(a,b,d) group, thereby enabling the determination of the sign of cc relative to aa.

Conclusions

We have applied polarization angle-resolved Raman spectroscopy (PARRS) to determine the Raman tensor elements of the Raman-active phonons of β-Ga2_2O3_3 within an extended tensor formalism that accounts for optical anisotropy and birefringence. By combining measurements on multiple crystal planes with a hyperspectral single-stage fitting procedure, we obtain the phonon energies and relative Raman tensor elements of all 15 Raman-active modes in a self-consistent manner.

This approach enables reliable analysis of strongly overlapping Raman features and yields tensor elements for modes that could not be determined in earlier studies, including the Bg(3)B_g^{(3)} and Bg(4)B_g^{(4)} modes. These results show that a procedure to model the hyperspectral data in a single step is essential for a quantitative analysis of polarized Raman scattering in monoclinic β-Ga2_2O3_3 and provide a complete experimental benchmark for comparison with theory and for future studies of optically anisotropic materials.

Acknowledgments

Chris Sturm (Universität Leipzig) and Christian Kranert (Fraunhofer Technology Centre Semiconductor Materials THM) are gratefully acknowledged for helpful discussions and providing the dielectric tensor elements of β\beta-Ga2_{2}O3_{3} for 632.8 nm. We thank Christian Kristukat for support with the software analysis of the polarization angle-resolved Raman spectra. Andreas Fiedler (Leibniz-Institut für Kristallzüchtung) is acknowledged for critical reading of the paper. Funding by the BMFTR, Berlin Senate and Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) under project number 446185170, by the Bundesministerium für Bildung und Forschung (BMBF) project under Grant No. 16ES1084K, by the MCIN/AEI/10.13039/501100011033 under grant PID2024-162811NB-I00 and the Severo Ochoa Centres of Excellence Program under grant CEX2023-001263-S are acknowledged.

Supplemental material to the article:

Complete Raman Tensor Determination in Birefringent β\beta-Ga2_2O3_3 by Single-Stage Hyperspectral Analysis of Polarization Angle-Resolved Raman Spectra

Conventional coordinate systems in β\beta-Ga2_2O3_3

To understand the theoretical modeling of the selection rules, several coordinate systems are introduced:

  1. The crystallographic coordinate system (a,b,c)(a, b, c) is defined by [100]≡a[100] \equiv a, [010]≡b[010] \equiv b, and [001]≡c[001] \equiv c with a monoclinic angle of β=∠(a,c)=103.8∘\beta= \angle(a,c) = 103.8^\circ between the aa- and cc-axes. The lattice parameters are a0=12.21a_0 = 12.21 Å, b0=3.04b_0 = 3.04 Å and c=5.80c = 5.80 Å [58].

  1. Several equivalent orthonormal quasi-crystal coordinate systems (x,y,z)(x, y, z) are commonly found in the literature. For one definition xx, yy and zz are chosen such that x∥[100]x \parallel[100] and y∥[010]y \parallel[010], while zz is defined perpendicular to both axes. Consequently, the angle between zz and the crystallographic cc-axis is ∠(z,c)=13.8∘\angle(z,c) = 13.8^\circ. All subsequent coordinate systems are expressed with respect to this basis, which is given by

x=(100),y=(010),z=(001).(9)x = \begin{pmatrix} 1 \\ 0 \\ 0 \end{pmatrix}, \qquad y = \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}, \qquad z = \begin{pmatrix} 0 \\ 0 \\ 1 \end{pmatrix}. \tag*{(9)}

Similarly, permutations of the above definition are equivalently valid, and can be found as the common standard description, depending on the field. Hence, it is worth to note that anisotropic properties may not be readily comparable, such as thermal and elastic properties in β\beta-Ga2_2O3_3 [45].

  1. In the orthonormal principal axis coordinate system (x~,y~,z~)(\tilde{x}, \tilde{y}, \tilde{z}) are defined by the eigenvectors of the dielectric tensor. For a wavelength of λ=633\lambda= 633 nm it is obtained by a rotation of α=2.33∘\alpha= 2.33^\circ in the xyxy-plane followed by an anticyclic permutation of xx, yy and zz. Expressed in the above defined quasi-crystal basis, the unit vectors read

x~=(sin⁡(α)0cos⁡(α)),y~=(cos⁡(α)0−sin⁡(α)),z~=(010).(10)\tilde{x} = \begin{pmatrix} \sin(\alpha) \\ 0 \\ \cos(\alpha) \end{pmatrix}, \qquad\tilde{y} = \begin{pmatrix} \cos(\alpha) \\ 0 \\ -\sin(\alpha) \end{pmatrix}, \qquad\tilde{z} = \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}. \tag*{(10)}
  1. Finally, four sample coordinate systems (xp′,yp′,zp′)(x'_p, y'_p, z'_p) with p∈{a,b,c,201‾}p \in\{\mathrm{a}, \mathrm{b}, \mathrm{c}, \overline{2 0 1}\} are introduced. Each system is defined such that zp′z'_p is perpendicular to their respective plane, e. g. z~a⊥(100)\tilde{z}_{\mathrm{a}} \perp(100), which coincides with the direction of light propagation. The axis x~p′\tilde{x}'_p is chosen parallel to a crystallographic direction: for the b-plane, x~b∥[100]\tilde{x}_{\mathrm{b}} \parallel[100], whereas for the other planes xp′∥[010]x'_p \parallel[010]. The remaining axis is then obtained by the cross product yp′=zp′×xp′y'_p = z'_p \times x'_p. The resulting bases, expressed in the quasi-crystal coordinate system, are:

x~a=(010),y~a=(cos⁡(β)0sin⁡(β)),z~a=(sin⁡(β)0−cos⁡(β)),x~b=(sin⁡(α)0cos⁡(α)),y~b=(cos⁡(α)0−sin⁡(α)),z~b=(010),x~c=(010),y~c=(100),z~c=(00−1),x~201‾=(010),y~201‾=(−cos⁡(γ)0−sin⁡(γ)),z~201‾=(−sin⁡(γ)0cos⁡(γ)),γ=50.79∘.(11)\begin{aligned} \tilde{x}_{\mathrm{a}} &= \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}, \qquad \tilde{y}_{\mathrm{a}} = \begin{pmatrix} \cos(\beta) \\ 0 \\ \sin(\beta) \end{pmatrix}, \qquad \tilde{z}_{\mathrm{a}} = \begin{pmatrix} \sin(\beta) \\ 0 \\ -\cos(\beta) \end{pmatrix}, \\ \tilde{x}_{\mathrm{b}} &= \begin{pmatrix} \sin(\alpha) \\ 0 \\ \cos(\alpha) \end{pmatrix}, \qquad \tilde{y}_{\mathrm{b}} = \begin{pmatrix} \cos(\alpha) \\ 0 \\ -\sin(\alpha) \end{pmatrix}, \qquad \tilde{z}_{\mathrm{b}} = \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}, \\ \tilde{x}_{\mathrm{c}} &= \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}, \qquad \tilde{y}_{\mathrm{c}} = \begin{pmatrix} 1 \\ 0 \\ 0 \end{pmatrix}, \qquad \tilde{z}_{\mathrm{c}} = \begin{pmatrix} 0 \\ 0 \\ -1 \end{pmatrix}, \\ \tilde{x}_{\overline{2 0 1}} &= \begin{pmatrix} 0 \\ 1 \\ 0 \end{pmatrix}, \qquad \tilde{y}_{\overline{2 0 1}} = \begin{pmatrix} -\cos(\gamma) \\ 0 \\ -\sin(\gamma) \end{pmatrix}, \qquad \tilde{z}_{\overline{2 0 1}} = \begin{pmatrix} -\sin(\gamma) \\ 0 \\ \cos(\gamma) \end{pmatrix}, \qquad\gamma= 50.79^\circ. \tag*{(11)} \end{aligned}

Base transformations

The Raman tensors defined in equation (1) and the dielectric tensor in equation (2) are both expressed in the eigenbasis of the dielectric tensor. To obtain their representations in the corresponding measurement geometry, they are transformed using the orthogonal matrix QQ, whose elements are given by

Qij=vi′⋅v~j(12)Q_{ij}=v_i' \cdot\tilde{v}_j \tag*{(12)}

where v~j\tilde{v}_j denote the basis vectors of the dielectric tensor (x~\tilde{x}, y~\tilde{y} and z~\tilde{z}), and vi′v_i' denote the basis vectors of the sample system (xp′x_p', yp′y_p' and zp′z_p'). The Raman and dielectric tensors in the measurement geometry are then obtained by the basis transformation

R=QRQT,ε=QεQT,(13)R=QRQ^{\mathsf{T}}, \qquad\varepsilon=Q\varepsilon Q^{\mathsf{T}}, \tag*{(13)}

where QQ and ε\varepsilon are shown exemplarily in Table S1. Using these representations of the dielectric tensor and calculating

a-planeb-planec-plane(2‾01)(\overline{2}01)-plane
QQ(0010.961−0.27800.2780.9610)\begin{pmatrix} 0 & 0 & 1 \\ 0.961 & -0.278 & 0 \\ 0.278 & 0.961 & 0 \end{pmatrix}(100010001)\begin{pmatrix} 1 & 0 & 0 \\ 0 & 1 & 0 \\ 0 & 0 & 1 \end{pmatrix}(0010.0410.9990−0.9990.0410)\begin{pmatrix} 0 & 0 & 1 \\ 0.041 & 0.999 & 0 \\ -0.999 & 0.041 & 0 \end{pmatrix}(001−0.800−0.60000.600−0.8000)\begin{pmatrix} 0 & 0 & 1 \\ -0.800 & -0.600 & 0 \\ 0.600 & -0.800 & 0 \end{pmatrix}
ε\varepsilon(3.8090003.7650.03100.0313.678)\begin{pmatrix} 3.809 & 0 & 0 \\ 0 & 3.765 & 0.031 \\ 0 & 0.031 & 3.678 \end{pmatrix}(3.7270003.6240003.768)\begin{pmatrix} 3.727 & 0 & 0 \\ 0 & 3.624 & 0 \\ 0 & 0 & 3.768 \end{pmatrix}(3.7680003.624−0.0040−0.0043.727)\begin{pmatrix} 3.768 & 0 & 0 \\ 0 & 3.624 & -0.004 \\ 0 & -0.004 & 3.727 \end{pmatrix}(3.7680003.690−0.0490−0.0493.661)\begin{pmatrix} 3.768 & 0 & 0 \\ 0 & 3.690 & -0.049 \\ 0 & -0.049 & 3.661 \end{pmatrix}

Table S1. Compilation of transformation matrices QQ and dielectric tensors ε\varepsilon representations in the surface systems of the investigated crystal planes.

the correction factors ρ\rho, TT and ZZ introduced in equation (7), the explicit selection rules for AgA_g and BgB_g modes can be obtained for each measurement geometry and are summarized in Table S2.

geometryAgA_g (ad0db000c)\begin{pmatrix} a & d & 0 \\ d & b & 0 \\ 0 & 0 & c \end{pmatrix}BgB_g (00e00fef0)\begin{pmatrix} 0 & 0 & e \\ 0 & 0 & f \\ e & f & 0 \end{pmatrix}
a-plane0.970c2cos⁡4(φ)+(0.927a+0.073b−0.521d)2sin⁡4(φ)0.970c^2\cos^4(\varphi)+(0.927a+0.073b-0.521d)^2\sin^4(\varphi)<br>14(0.970c2+(0.927a+0.073b−0.521d)2)sin⁡2(2φ)\frac{1}{4}\left(0.970c^2+(0.927a+0.073b-0.521d)^2\right)\sin^2(2\varphi)(0.952e−0.268f)2sin⁡2(2φ)(0.952e-0.268f)^2\sin^2(2\varphi)<br>(0.952e−0.268f)2cos⁡2(2φ)(0.952e-0.268f)^2\cos^2(2\varphi)
b-plane0.937a2cos⁡4(φ)+b2sin⁡4(φ)+0.954d2sin⁡2(2φ)0.937a^2\cos^4(\varphi)+b^2\sin^4(\varphi)+0.954d^2\sin^2(2\varphi)<br>(0.234a2+0.25b2)sin⁡2(2φ)+0.954d2cos⁡2(2φ)(0.234a^2+0.25b^2)\sin^2(2\varphi)+0.954d^2\cos^2(2\varphi)00<br>00
c-plane0.913c2cos⁡4(φ)+(0.002a+0.998b+0.084d)2sin⁡4(φ)0.913c^2\cos^4(\varphi)+(0.002a+0.998b+0.084d)^2\sin^4(\varphi)<br>14(0.913c2+(0.002a+0.998b+0.084d)2)sin⁡2(2φ)\frac{1}{4}\left(0.913c^2+(0.002a+0.998b+0.084d)^2\right)\sin^2(2\varphi)(0.040e+0.967f)2sin⁡2(2φ)(0.040e+0.967f)^2\sin^2(2\varphi)<br>(0.040e+0.967f)2cos⁡2(2φ)(0.040e+0.967f)^2\cos^2(2\varphi)
(2‾01)(\overline{2}01)-plane0.952c2cos⁡4(φ)+(0.653a+0.347b+0.952d)2sin⁡4(φ)0.952c^2\cos^4(\varphi)+(0.653a+0.347b+0.952d)^2\sin^4(\varphi)<br>14(0.952c2+(0.653a+0.347b+0.952d)2)sin⁡2(2φ)\frac{1}{4}\left(0.952c^2+(0.653a+0.347b+0.952d)^2\right)\sin^2(2\varphi)(0.794e+0.579f)2sin⁡2(2φ)(0.794e+0.579f)^2\sin^2(2\varphi)<br>(0.794e+0.579f)2cos⁡2(2φ)(0.794e+0.579f)^2\cos^2(2\varphi)

Table S2. Polarization angle dependent selection rules A(φ,r)A(\varphi,r), i. e. PARRS profiles for the investigated scattering geometries. Influences of the dielectric tensor described in the extended model for Raman scattering in birefringent media are included in the numerical prefactors.

Contour plots of the (010), (001) and (201) planes

Image not extracted

Figure S1. Contour plot of the polarization dependent Raman spectra on the b-plane for parallel (middle) and crossed scattering geometries (bottom). Angles, where yb′∥[100]y'_b \parallel[100] are labeled. In the top panel Raman spectra with a polarization angle of ϕ=150∘\phi= 150^\circ are depicted, while the panels on the right show the integrated intensity in the range of the Ag(5)A_g^{(5)} mode and the corresponding slice of the fit. The Raman spectra are depicted with the square root of the intensity for better visualization of small peaks.

Contour plot of the polarization dependent Raman spectra on the c-plane

Figure S2. Contour plot of the polarization dependent Raman spectra on the c-plane for parallel (middle) and crossed scattering geometries (bottom). Angles, where xc′∥[010]x'_c \parallel[010] and yc′∥[100]y'_c \parallel[100] are labeled. In the top panel Raman spectra with a polarization angle of ϕ=150∘\phi= 150^\circ are depicted, while the panels on the right show the integrated intensity in the range of the Ag(5)/Bg(3)A_g^{(5)}/B_g^{(3)} pair and the corresponding slice of the fit. The Raman spectra are depicted with the square root of the intensity for better visualization of small peaks.

Contour plot of the polarization dependent Raman spectra on the $\bar{2}01$-plane

Figure S3. Contour plot of the polarization dependent Raman spectra on the 2ˉ01\bar{2}01-plane for parallel (middle) and crossed scattering geometries (bottom). Angles, where x2ˉ01′∥[010]x'_{\bar{2}01} \parallel[010] are labeled. In the top panel Raman spectra with a polarization angle of ϕ=150∘\phi= 150^\circ are depicted, while the panels on the right show the integrated intensity in the range of the Bg(5)/Ag(9)B_g^{(5)} / A_g^{(9)} pair and the corresponding slice of the fit. The Raman spectra are depicted with the square root of the intensity for better visualization of small peaks.

Differences between model fit and Raman spectra for the a-plane

Image not extracted

Figure S4. Contour plot of the experimental polarization dependent Raman spectra (top), model fit (middle) and their difference (bottom) for the a-plane for parallel scattering geometry. The color bar for the Raman spectra and model fit is scaled by the square root for better visualization of small peaks.

Figure S5. Contour plot of the experimental polarization dependent Raman spectra (top), model fit (middle) and their difference (bottom) for the a-plane for crossed scattering geometry.The color bar for the Raman spectra and model fit is scaled by the square root for better visualization of small peaks.

References

  1. [1]S. J. Pearton, J. Yang, P. H. Cary, F. Ren, J. Kim, M. J. Tadjer, and M. A. Mastro, Appl. Phys. Rev. 5, 011301 (2018).
  2. [2]S. J. Pearton, F. Ren, M. Tadjer, and J. Kim, J. Appl. Phys. 124, 220901 (2018).
  3. [3]M. Higashiwaki, K. Sasaki, A. Kuramata, T. Masui, and S. Yamakoshi, Phys. Status Solidi A 211, 21 (2014).
  4. [4]M. Higashiwaki, K. Sasaki, A. Kuramata, T. Masui, and S. Yamakoshi, Appl. Phys. Lett. 100, 013504 (2012).
  5. [5]M. Higashiwaki, A. Kuramata, H. Murakami, and Y. Kumagai, J. Phys. D. Appl. Phys. 50, 333002 (2017).
  6. [6]Y. Kokubun, K. Miura, F. Endo, and S. Nakagomi, Appl. Phys. Lett. 90, 031912 (2007).
  7. [7]T. Oshima, T. Okuno, N. Arai, N. Suzuki, S. Ohira, and S. Fujita, Appl. Phys. Express 1, 011202 (2008).
  8. [8]A. J. Green, J. Speck, G. Xing, P. Moens, F. Aller­stam, K. Gumaelius, T. Neyer, A. Arias-Purdue, V. Mehro­tra, A. Kuramata, K. Sasaki, S. Watanabe, K. Koshi, J. Blevins, O. Bierwagen, S. Krishnamoorthy, K. Leedy, A. R. Arehart, A. T. Neal, S. Mou, S. A. Ringel, A. Kumar, A. Sharma, K. Ghosh, U. Singisetti, W. Li, K. Chabak, K. Liddy, A. Islam, S. Rajan, S. Graham, S. Choi, Z. Cheng, and M. Higashiwaki, APL Mater. 10, 029201 (2022).
  9. [9]T. Matsumoto, M. Aoki, A. Kinoshita, and T. Aono, Jpn. J. Appl. Phys. 13, 1578 (1974).
  10. [10]N. Ueda, H. Hosono, R. Waseda, and H. Kawazoe, Appl. Phys. Lett. 71, 933 (1997).
  11. [11]K. Yamaguchi, Solid State Commun. 131, 739 (2004).
  12. [12]T. Onuma, S. Saito, K. Sasaki, T. Masui, T. Yamaguchi, T. Honda, and M. Higashiwaki, Jpn. J. Appl. Phys. 54, 112601 (2015).
  13. [13]C. Sturm, J. Furthmüller, F. Bechstedt, R. Schmidt-Grund, and M. Grundmann, APL Materials 3, 0 (2015).
  14. [14]J. B. Varley and A. Schleife, Semicond. Sci. Technol. 30, 024010 (2015).
  15. [15]J. Furthmüller and F. Bechstedt, Phys. Rev. B 93, 115204 (2016).
  16. [16]T. Onuma, S. Saito, K. Sasaki, T. Masui, T. Yamaguchi, T. Honda, A. Kuramata, and M. Higashiwaki, Jpn. J. Appl. Phys. 55 (2016).
  17. [17]F. Ricci, F. Boschi, A. Baraldi, A. Filippetti, M. Higashiwaki, A. Kuramata, V. Fiorentini, and R. Fornari, J. Phys. Condens. Matter 28, 224005 (2016).
  18. [18]C. Sturm and M. Grundmann, Phys. Rev. A 93, 053839 (2016).
  19. [19]A. Mock, R. Korlacki, C. Briley, V. Darakchieva, B. Monemar, Y. Kumagai, K. Goto, M. Higashiwaki, and M. Schubert, Phys. Rev. B 96, 245205 (2017).
  20. [20]A. Ratnaparkhe and W. R. L. Lambrecht, Appl. Phys. Lett. 110, 132103 (2017).
  21. [21]P. Gopalan, S. Knight, A. Chanana, M. Stokey, P. Ranga, M. A. Scarpulla, S. Krishnamoorthy, V. Darakchieva, Z. Galazka, K. Irmscher, A. Fiedler, S. Blair, M. Schubert, and B. Sensale-Rodriguez, Appl. Phys. Lett. 117 (2020).
  22. [22]J. B. Cho, G. Jung, K. Kim, J. Kim, S. K. Hong, J. H. Song, and J. I. Jang, J. Phys. Chem. C 125, 1432 (2021).
  23. [23]N. Zhang, I. M. Kisylyakov, C. Xia, H. Qi, J. Wang, and H. F. Mohamed, Opt. Express 29, 18587 (2021).
  24. [24]M. Meißner, N. Bernhardt, F. Nippert, B. M. Janzen, Z. Galazka, and M. R. Wagner, Appl. Phys. Lett. 124, 152102 (2024).
  25. [25]M. Grundmann, C. Sturm, C. Kranert, S. Richter, R. Schmidt-Grund, C. Deparis, and J. Zúñiga-Pérez, Phys. status solidi - Rapid Res. Lett. 11, 1600295 (2016).
  26. [26]T. Onuma, S. Saito, K. Sasaki, K. Goto, T. Masui, T. Yamaguchi, T. Honda, A. Kuramata, and M. Higashiwaki, Appl. Phys. Lett. 108, 101904 (2016).
  27. [27]M. Schubert, R. Korlacki, S. Knight, T. Hofmann, S. Schöche, V. Darakchieva, E. Janzén, B. Monemar, D. Gogova, Q.-T. Thieu, R. Togashi, H. Murakami, Y. Kumagai, K. Goto, A. Kuramata, S. Yamakoshi, and M. Higashiwaki, Phys. Rev. B 93, 125209 (2016).
  28. [28]C. Sturm, R. Schmidt-Grund, C. Kranert, J. Furthmüller, F. Bechstedt, and M. Grundmann, Phys. Rev. B 94, 035148 (2016).
  29. [29]J. A. Spencer, A. L. Mock, A. G. Jacobs, M. Schubert, Y. Zhang, and M. J. Tadjer, Appl. Phys. Rev. 9 (2022).
  30. [30]C. Kranert, C. Sturm, R. Schmidt-Grund, and M. Grundmann, Phys. Rev. Lett. 116, 127401 (2016).
  31. [31]K. Zhang, Z. Xu, J. Zhao, H. Wang, J. Hao, S. Zhang, H. Cheng, and B. Dong, Appl. Surf. Sci. 581, 152426 (2022).
  32. [32]H. von Wenckstern, Adv. Electron. Mater. 3, 1600350 (2017).
  33. [33]A. Parisini, K. Ghosh, U. Singisetti, and R. Fornari, Semicond. Sci. Technol. 33, 105008 (2018).
  34. [34]K. Ghosh and U. Singisetti, Appl. Phys. Lett. 109 (2016).
  35. [35]E. Villora, Y. Morioka, T. Atou, T. Sugawara, M. Kikuchi, and T. Fukuda, Phys. Status Solidi A 193, 187 (2002).
  36. [36]D. C. Look and K. D. Leedy, Sci. Rep. 9, 1290 (2019).
  37. [37]J. R. Ritter, K. G. Lynn, and M. D. McCluskey, J. Appl. Phys. 126, 225705 (2019).
  38. [38]K. A. Mengle and E. Kioupakis, AIP Adv. 9, 015313 (2019).
  39. [39]B. M. Janzen, R. Gillen, Z. Galazka, J. Maultzsch, and M. R. Wagner, Phys. Rev. Mater. 6, 054601 (2022).
  40. [40]B. M. Janzen, P. Mazzolini, R. Gillen, A. Falkenstein, M. Martin, H. Tornatzky, J. Maultzsch, O. Bierwagen, and M. R. Wagner, J. Mater. Chem. C 9, 2311 (2021).
  41. [41]D. Dohy, G. Lucazeau, and A. Revcolevschi, J. Solid State Chem. 45, 180 (1982).
  42. [42]C. Kranert, C. Sturm, R. Schmidt-Grund, and M. Grundmann, Sci. Rep. 6, 35964 (2016).
  43. [43]B. Liu, M. Gu, and X. Liu, Appl. Phys. Lett. 91, 172102 (2007).
  44. [44]M. Grundmann, C. Sturm, C. Kranert, S. Richter, R. Schmidt-Grund, C. Deparis, and J. Zúñiga-Pérez, Phys. Status Solidi Rapid Res. Lett. 11, 1600295 (2017).
  45. [45]K. Xu, S. Zhao, L. S.-M. Choi, N. Bernhardt, P. Emtenani, M. Meißner, H. Tornatzky, O. Bierwagen, P. Mazzolini, R. Mincigrucci, L. Foglia, D. Fainozzi, F. Bencivenga, Z. Galazka, G. Fytas, B. Graczykowski, R. Rurali, M. Scheffler, C. Carbogno, J. S. Reparaz, and M. R. Wagner, Nanoscale origin of thermal anisotropy in monoclinic β-Ga2O3, in preparation.
  46. [46]I. R. Beattie and T. R. Gilson, Proc. R. Soc. Lond. A Math. Phys. Sci. 307, 407 (1968).
  47. [47]D. Machon, P. F. McMillan, B. Xu, and J. Dong, Phys. Rev. B 73, 094125 (2006).
  48. [48]T. Onuma, S. Fujioka, T. Yamaguchi, Y. Itoh, M. Higashiwaki, K. Sasaki, T. Masui, and T. Honda, J. Cryst. Growth 401, 330 (2014).
  49. [49]Y. Yao, Y. Ishikawa, and Y. Sugawara, J. Appl. Phys. 126, 205106 (2019).
  50. [50]K. Zhang, Z. Xu, S. Zhang, H. Wang, H. Cheng, J. Hao, J. Wu, and F. Fang, Physica B Condens. Matter 600, 412624 (2021).
  51. [51]P. Seyidov, M. Ramsteiner, Z. Galazka, and K. Irmscher, J. Appl. Phys. 131, 035707 (2022).
  52. [52]A. Fiedler, M. Ramsteiner, Z. Galazka, and K. Irmscher, Appl. Phys. Lett. 117, 152107 (2020).
  53. [53]K. Zhang, Z. Xu, J. J. Zhao, H. Wang, J. Hao, S. Zhang, H. Cheng, and B. Dong, J. Alloys Compd. 881, 160665 (2021).
  54. [54]T. Z. Kosc, H. Huang, T. J. Kessler, R. A. Negres, and S. G. Demos, Sci. Rep. 10, 16283 (2020).
  55. [55]T. Sander, S. Eisermann, B. K. Meyer, and P. J. Klar, Phys. Rev. B 85, 165208 (2012).
  56. [56]R. Hildebrandt, C. Sturm, M. Wieneke, A. Dadgar, and M. Grundmann, Appl. Phys. Lett. 119, 121109 (2021).
  57. [57]Z. Galazka, R. Uecker, D. Klimm, K. Irmscher, M. Naumann, M. Pietsch, A. Kwasniewski, R. Bertram, S. Ganschow, and M. Bickermann, ECS J. Solid State Sci. Technol. 6, Q3007 (2017).
  58. [58]Z. Galazka, S. Ganschow, K. Irmscher, D. Klimm, M. Albrecht, R. Schewski, M. Pietsch, T. Schulz, A. Dittmar, A. Kwasniewski, R. Grueneberg, S. B. Anooz, A. Popp, U. Juda, I. M. Hanke, T. Schroeder, and M. Bickermann, Prog. Cryst. Growth Charact. Mater. 67, 100511 (2021).
  59. [59]Z. Galazka, S. Ganschow, P. Seyidov, K. Irmscher, M. Pietsch, T.-S. Chou, S. Bin Anooz, R. Grueneberg, A. Popp, A. Dittmar, A. Kwasniewski, M. Suendermann, D. Klimm, T. Straubinger, T. Schroeder, and M. Bickermann, Appl. Phys. Lett. 120, 152101 (2022).
  60. [60]Z. Galazka, J. Appl. Phys. 131, 031103 (2022).
  61. [61]C. Kristokat, peak-o-mat2, https://github.com/kurisutsukato/peak-o-mat.git (2026), analysis was performed in part with a non-public alpha-version.
  62. [62]C. Kristokat, peak-o-mat (2026), https://qceha.net/.
  63. [63]K. Momma and F. Izumi, J. Appl. Crystallogr. 44, 1272 (2011).
  64. [64]E. Kroumova, M. Aroyo, J. Perez-Mato, A. Kirov, C. Capillas, S. Ivantchev, and H. Wondratschek, Ph. Transit. 76, 155 (2003).
  65. [65]C. Sturm (Universität Leipzig), Private communication.
  66. [66]See Supplemental Material at [provided by Publisher] for a detailed description of the coordinate systems and their respective transformations as well as the comprehensive set of contour plots, plots of the fitted model function and respective fit residual.
  67. [67]W. Hayes and R. Loudon, Scattering of light by crystals, A Wiley-Interscience publication (Wiley, New York, 1978) p. 31.

Paper details

vlnc:W_5mjdbmbc
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 9

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents