betaFeedback

WorksPhysics and Astronomy

Enhancement of piezoelectric response in V doped LiNbO3 films deposited by RF magnetron sputtering

Abstract

LiNbO3 films doped with vanadium (V) were deposited using RF magnetron sputtering technique. To realize doping with a wider range of V concentration, a 30 mm V metal inlaid target asymmetrically embedded in the 150 mm lithium niobate target was used. The V concentration in the deposited films was a decreasing function of the distance from the V target. The V/Nb ratio in the film decreased from 0.155 to 0.024. Surface and inner morphology and structure, phase and element composition, microstructure, and ferroelectric properties of the undoped and V doped LiNbO3 films were studied. The measured maximal d33 constant of the LiNbVO film with V/Nb ratio of 0.07 was about three times higher than that of the undoped LiNbO3 film, 13.5 pC/N and 4.76 pC/N, respectively. The optimal composition in the deposition geometry used was within the V/Nb ratio range of 0.05 to 0.13. Undoped and V doped LiNbO3 thin films were used as bulk acoustic wave ultrasonic transducers deposited on stainless steel plates to generate longitudinal waves and compare their ultrasonic performance.

Introduction

The excellent piezoelectric performance of lithium niobate (LiNbO3\mathrm{LiNbO}_{3}) with high Curie temperature of ∼1483\sim1483 K and coupling coefficient ktk_t of 0.49 [1, 2, 3, 4] determines its widespread use in piezoelectric devices such as micro-mechanical ultrasonic transducers [5, 6, 7, 8, 9], shear wave resonators [10], surface acoustic wave sensors [11, 12], and precision positioning drivers [13].

In order to simplify structure of the ultrasonic transducer, improve its high temperature durability, and avoid problems of adhesive between transducer and sample, deposition of the piezoelectric transducer in form of thin films is preferred. In addition, thin film deposition technologically is simpler than high quality single crystal growth, thin films have stronger adhesion to substrate, and miniaturization of electronic devices is possible. To prepare LiNbO3\mathrm{LiNbO}_{3} thin films, various techniques can be used, such as RF magnetron sputtering [14, 15], pulsed laser deposition [16, 17], sol-gel method [18, 19], thermal assisted spin coating [20], chemical bath deposition [21], polymeric precursor method [22], photolithographic technique [23], and ion beam sputtering [24].

In recent years, doping specific metal elements into AlN piezoelectric materials has been proven to be an effective method for improving piezoelectric properties. Akiyama et al. showed that Sc doping of AlN (Sc0.43Al0.57N\mathrm{Sc}_{0.43}\mathrm{Al}_{0.57}\mathrm{N} alloy) exhibited a large piezoelectric coefficient d33d_{33} of 27.6 pC/N, which was 500% larger than that of undoped AlN [25]. Similarly, there were made multiple attempts to improve the piezoelectric performance of LiNbO3\mathrm{LiNbO}_{3} in bulk form (crystals and powders) by doping with Mg, B, and Zn. Compared with undoped LiNbO3\mathrm{LiNbO}_{3}, LiNbO3\mathrm{LiNbO}_{3} single crystals [26, 27, 28] and powders [29] doped with Mg up to 10 mol.% demonstrated not significant improvement or deterioration in piezoelectric properties. While LiNbO3\mathrm{LiNbO}_{3} single crystals doped with 5.6 mol.% Zn and 0.44 wt.% Gd after a certain heat treatment showed an increase in piezoelectric d33d_{33} constant to the maximum values of 13.2 pC/N and ∼12\sim12 pC/N, respectively, which are close to that of the single domain pure LiNbO3\mathrm{LiNbO}_{3} single crystals [30, 31].

However, in literature, there is little research on study of ultrasonic response of doped LiNbO3\mathrm{LiNbO}_{3} thin films. Nakamura et al. deposited cc-axis oriented pure LiNbO3\mathrm{LiNbO}_{3} and Pr doped LiNbO3\mathrm{LiNbO}_{3} films using RF magnetron sputtering. The electromechanical coupling coefficient kt2k_t^2 demonstrated increase from 0.8% of the pure film up to 2.2% of the Pr doped film [32], which is closer to the theoretical value of 4% in the cc-axis (Z-cut) oriented LiNbO3\mathrm{LiNbO}_{3} crystal. Recently, Kobayashi et. al prepared 100 μm100\,\mu\mathrm{m} thick LiNbO3/TiO2+SrCO3\mathrm{LiNbO}_{3}/\mathrm{TiO}_{2}+\mathrm{SrCO}_{3} composite films using sol-gel technique and observed high temperature ultrasonic response up to 1050 ∘C1050\,^\circ\mathrm{C} [19]. The other composites, LiNbO3/TiO2\mathrm{LiNbO}_{3}/\mathrm{TiO}_{2} and LiNbO3/Al2O3\mathrm{LiNbO}_{3}/\mathrm{Al}_{2}\mathrm{O}_{3}, demonstrated lower temperature durability up to 700 ∘C700\,^\circ\mathrm{C} [18].

Though the LiNbO3\mathrm{LiNbO}_{3} is high temperature ferro- and piezoelectric material, its d33d_{33} strain constant of ~6 pC/N is very low in comparison with those of other piezoelectric materials [1, 2]. In our previous study, we found that the d33d_{33} constant of LiNbO3\mathrm{LiNbO}_{3} in film form depends on the thickness, but cannot exceed 6 pC/N. In this study, we characterize LiNbO3\mathrm{LiNbO}_{3} thin films doped with vanadium (V) deposited using magnetron sputtering technique. The vanadium doping greatly improves the piezoelectric constant of LiNbO3\mathrm{LiNbO}_{3} piezoelectric films. Effects of V concentration on piezoelectric performance are studied. We also apply V doped LiNbO3\mathrm{LiNbO}_{3} thin films for bulk acoustic wave ultrasonic transducers to generate longitudinal waves.

Results and discussion

In order to reach a wider range of V concentration in the LiNbO3\mathrm{LiNbO}_{3} films an asymmetrically embedded V inlaid target was used, as shown in Figure 1a and 1b. To prepare the inlaid target, a 150 mm target containing LiNbO3\mathrm{LiNbO}_{3} and LiNb3O8\mathrm{LiNb}_{3}\mathrm{O}_{8} phases was drilled at a radial distance of 50 mm, with a hole diameter of 30 mm. The 30 mm V inlaid target was installed in this hole. The rectangular Si and SS substrates were placed relative to the V target, as shown in Figure 1a. In this geometry the V concentration in RF plasma is a decreasing function of the distance from the V target, as shown in Figure 1c for V/Nb atomic ratio in the deposited LiNbO3\mathrm{LiNbO}_{3} film transducers measured by energy dispersive spectroscopy (EDS) technique. As reference samples, pure undoped LiNbO3\mathrm{LiNbO}_{3} film transducers were deposited using the same 150 mm target with an 30 mm inlaid target of the same material (mixture of LiNbO3\mathrm{LiNbO}_{3} and LiNb3O8\mathrm{LiNb}_{3}\mathrm{O}_{8} phases).

Image not extracted

Figure 1. Schematic diagrams of deposition geometry, plane view (a) and cross-section (b). The dependence of V/Nb atomic ratio in deposited films on distance from the V inlaid target (c). The distance scale in all figures corresponds to the xx-axis in figure (c).

In Figure 2 surface and cross-section morphology of the undoped LiNbO3\mathrm{LiNbO_3} film (Figure 2a and Figure 2b) and V doped LiNbO3\mathrm{LiNbO_3} film with V/Nb atomic ratio of 0.07, i.e. at a distance from the inlaid target of 60 mm (Figure 2d and Figure 2e) are shown. In the cross-section image of the undoped film a well developed columnar structure is observed. Therefore, each particle in Figure 2a represents the top of the column. The V doped LiNbO3_3 film has finer and less oriented columnar structure with featureless, probably amorphous, bottom layer of ∼5\sim5 μm in thickness. The total thickness of the deposited transducers in the deposition center and at the edge is ∼24\sim24 μm and ∼15\sim15 μm, respectively. In Figure 2c and Figure 2f AFM images of undoped LiNbO3_3 and V doped LiNbO3_3 films deposited on SS substrate, respectively, are shown. The roughness of the undoped and V doped films measured on an area of 10×1010 \times10 μm2^2 is 31±331 \pm3 nm and 99±899 \pm8 nm, respectively.

Image not extracted

Figure 2. SEM images of surface and cross-section of undoped LiNbO3_3 film (a, b) and V doped LiNbO3_3 film with V/Nb atomic ratio of 0.07 (d, e). AFM images of undoped LiNbO3_3 film (c) and V doped LiNbO3_3 film (f)

In Figure 3a XRD patterns of undoped and V doped LiNbO3_3 films are shown. Undoped film contains two phases, the LiNbO3_3 and Li-deficient piezoelectrically inactive LiNb3_3O8_8 phase with (012) and (116) preferred reflections, respectively. V doped films demonstrate more polycrystalline LiNbO3_3 phase with dominant (012) reflection and traces of LiNb3_3O8_8 phase.

Image not extracted

Figure 3. XRD patterns (a) and unpolarized Raman spectra (b) of undoped LiNbO3\mathrm{LiNbO}_3 film and V doped LiNbO3\mathrm{LiNbO}_3 film with V/Nb atomic ratio of 0.07. Cross-sectional Raman spectra of undoped (c) and V doped films (d) measured at different film depth and corresponding cross-section optical image and measurement points (e).

We can use (012) reflection of the LiNbO3_3 phase to calculate the mean grain size DD by the Scherrer equation:

D=Kλβcos⁡θD = \frac{K\lambda}{\beta\cos\theta}

where K∼0.9K \sim0.9 is a shape factor, λ=0.154\lambda= 0.154 nm is the X-ray wavelength, β\beta is the full width in radian of a certain reflection at its half maximum of intensity (FWHM), and θ\theta is the Bragg angle of the (012) reflection equal to 23.3/223.3/2 deg. The estimated mean grain sizes of undoped and V doped LiNbO3\mathrm{LiNbO}_3 films are 54±254 \pm2 nm and 33±333 \pm3 nm, respectively. The smaller grain size of the V doped LiNbO3\mathrm{LiNbO}_3 film is in agreement with the observation of finer columnar structure in the cross-section SEM image.

In Figure 3b unpolarized Raman spectra of undoped LiNbO3\mathrm{LiNbO}_3 film and V doped LiNbO3\mathrm{LiNbO}_3 film with V/Nb atomic ratio of 0.07 are shown. The undoped LiNbO3\mathrm{LiNbO}_3 film exhibits broad peaks, which were identified with LiNbO3\mathrm{LiNbO}_3 and LiNb3O8\mathrm{LiNb}_3\mathrm{O}_8 phases [33] (blue line). The V doped LiNbO3\mathrm{LiNbO}_3 film demonstrates the main peaks of the LiNbO3\mathrm{LiNbO}_3 phase and traces of the LiNb3O8\mathrm{LiNb}_3\mathrm{O}_8 phase as a shoulder at 688 cm−1\mathrm{cm}^{-1} of the main LiNbO3\mathrm{LiNbO}_3 peak at 620 cm−1\mathrm{cm}^{-1} (orange line). All obtained results are in agreement with the XRD data. Figure 3c and Figure 3d show the Raman spectra of undoped and V doped film measured on cross-section at different depths, respectively. Figure 3e shows the corresponding cross-section and positions of the measurement points (V doped film). Both undoped and V doped films demonstrate similar phase composition independent of the depth. Therefore, the deposited V doped film demonstrates phase homogeneity independent of the film depth.

The SEM-EDS mapping analysis of the undoped LiNbO3\mathrm{LiNbO}_{3} film and V doped LiNbO3\mathrm{LiNbO}_{3} film is shown in Figure 4a and Figure 4b, respectively. In both surface and cross-section maps all films demonstrate homogeneous distribution of Nb, O and V elements in agreement with Raman spectroscopy results.

Image not extracted

Figure 4. SEM-EDS Nb, O, and V mapping of surface and cross-section of undoped LiNbO3\mathrm{LiNbO}_{3} film (a) and V doped LiNbO3\mathrm{LiNbO}_{3} film with V/Nb atomic ratio of 0.07 (b).

Figure 5a shows a bright-field cross-sectional TEM image of V doped LiNbO3\mathrm{LiNbO}_{3} film. The film composes of columns with width in the range of 200-400 nm. In Figure 5b and Figure 5c HRTEM images of two columns are shown. The columns are single crystals with arbitrary orientations, which can be seen in Fast Fourier Transform (FFT) images of the selected area in the insets, in agreement with the XRD results. The chemical composition of the film revealed by TEM-EDX micro-analysis is: O of 68.1 at.%, Nb of 23.6 at.%, V of 1.25 at.%. The EDX spectrum is shown in Figure 5c. There is also C of ~6 at.%, probably due to presence of vacuum pump oil vapor in the chamber. The V/Nb atomic ratio is 0.053, which is slightly lower than 0.07 obtained by the SEM-EDS technique. In Figure 5e Nb, O, and V element EDX mapping of a few columns is shown. It can be concluded that the film has homogeneous distribution of Nb, O and V elements, consistent with SEM-EDS results, but now at the sub micron scale.

Image not extracted

Figure 5. TEM cross-section image (a) and TEM-EDX spectrum (b) of V doped LiNbO3\mathrm{LiNbO}_{3} film with V/Nb atomic ratio of 0.07. HRTEM images of two columns and (FFT) images of the selected area in the insets (c) and (d).

In Figure 6a d33d_{33} constants of undoped and V doped LiNbO3\mathrm{LiNbO}_{3} films as functions of distance from the inlaid target are shown. d33d_{33} constant of the undoped LiNbO3\mathrm{LiNbO}_{3} film demonstrates significant dependence, changing from 1.68 pC/N at the deposition edges to 4.76 pC/N at the deposition center (distance from the inlaid target of 60 mm). The increase in the d33d_{33} constant at the deposition center can be related to the higher crystal quality of the thicker films, as it was found in our previous study [35]. The V doped LiNbO3\mathrm{LiNbO}_{3} film demonstrates similar increase in the d33d_{33} constant from 0.4 to 13.5 pC/N, when the distance from the V target increases from 0 to 60 mm. The maximal value of the d33d_{33} constant is about three times higher than that of the undoped LiNbO3\mathrm{LiNbO}_{3} film. When the distance further increases to 120 mm, the d33d_{33} constant decreases and tends towards the undoped LiNbO3\mathrm{LiNbO}_{3} values at the same distance, which can be explained by the fact that the concentration of V element at long distances is too low to produce any effect.

Image not extracted

Figure 6. d33\mathit{d}_{33} constants of undoped and V doped (V/Nb = 0.07) LiNbO3\mathrm{LiNbO_3} films as functions of distance from the V inlaid target (a) and function of V/Nb atomic ratios (b). d33\mathit{d}_{33} constant ratio of undoped and V doped LiNbO3\mathrm{LiNbO_3} films as function of V/Nb atomic ratio (c). The pulse-echo response (longitudinal waves) of undoped and V doped LiNbO3\mathrm{LiNbO_3} film transducers (d). The amplitudes of L2 echo of undoped and V doped LiNbO3\mathrm{LiNbO_3} films as functions of distance from the inlaid target (e). Wave-forms of multiple echoes of V doped LiNbO3\mathrm{LiNbO_3} film transducer at different temperatures within

However, the distance dependence of the d33d_{33} constant depends on the deposition geometry, which is inconvenient for practical use. Using the distance dependence of V/Nb atomic ratio (Figure 1c), we redrew the d33d_{33} constant as a function of V/Nb atomic ratio, as shown in Figure 6b. The highest d33=13.5d_{33} = 13.5 pC/N is observed at V/Nb atomic ratio of 0.07.

The obtained dependence of the d33d_{33} constant includes two effects. First is the V/Nb atomic ratio dependence itself, representing effect of the composition on piezoelectric response. The second can be called the “geometrical” effect, which includes the mentioned thickness dependence and effect of the crystal orientation, as was found in our previous study on undoped LiNbO3_3 film transducers [33]. In other words, although the asymmetric geometry with the inlaid target used expands the range of V concentration in the films, it does not allow to distinguish effects of doping concentration and thickness/orientation of the deposited films on ultrasonic response. Since both undoped and doped films were deposited in similar conditions, we can minimize the “geometrical” effect by calculating the ratio of d33d_{33} constants of V doped and undoped LiNbO3_3 films as function of V/Nb atomic ratio, as shown in Figure 6c. The maximum now is flatter and wider and in the V/Nb atomic ratio range of 0.05 - 0.13 the d33LNO:V/d33LNOd_{33\mathrm{LNO:V}}/d_{33\mathrm{LNO}} ratio is about 3, demonstrating optimal range of the V concentration.

To independently demonstrate the increase in d33d_{33} constant, we measured the ultrasonic pulse-echo response of V doped LiNbO3_3 film transducers. In Figure 6d the ultrasonic responses of undoped and V doped LiNbO3_3 film transducers deposited at a distance of 60 mm from the inlaid target are shown. Compared to the amplitude of the undoped transducer, doping with V at a V/Nb atomic ratio of 0.07 results in an increase of over 9 times in the amplitude of the longitudinal wave echo L2_2. In Figure 6e distance dependence of the L2_2 echo is shown. Similar to d33d_{33} constant, the longitudinal wave amplitudes show their maximum values at the deposition center. In a wide distance range, the amplitude generated by V-doped LiNbO3_3 transducer is ~9 times larger than that of the undoped LiNbO3_3 transducer.

Next, we have measured in-situ high-temperature pulse-echo response of the V doped LiNbO3_3 transducer deposited on the SS substrate in the temperature range of 30-600 °C, as shown in Figure 6f. As the temperature increases, the wave echoes (L2_2-L6_6) shift towards higher time-of-flight. The shift is explained by increase of the thickness of the SS substrate due to the thermal expansion and by decrease of the speed of sound [36]. As the temperature increases, the wave echo amplitudes decreases, this effect can be explained by a decrease in resistivity of the transducer due to its semiconducting properties, as found in our previous study [37] on undoped LiNbO3\mathrm{LiNbO_3} films.

To study ferroelectric properties of the transducers we have measured ferroelectric Curie temperature using DTA technique. The undoped and V doped films demonstrate an endothermic peak at 1169 °C and 1161 °C, respectively, as shown in Figure 6g, which can be related to the ferroelectric-paraelectric transition of the LiNbO3\mathrm{LiNbO_3} lattice. It can be concluded that V doping does not change significantly the ferroelectric properties of the LiNbO3\mathrm{LiNbO_3}.

the range of 30–600∘C^{\circ}\mathrm{C} (f). DTA curves of undoped and V doped LiNbO3\mathrm{LiNbO}_{3} films and ferroelectric-paraelectric transitions near the TcT_c (g).

The increase in d33d_{33} constant of the V doped LiNbO3\mathrm{LiNbO}_{3} films up to 13.5 pC/N is unlikely due to possible unipolarity of the deposited films [30, 31], since the XRD pattern demonstrates their polycrystalline structure (Figure 3a). In addition, the deposited V doped LiNbO3\mathrm{LiNbO}_{3} films are even more polycrystalline than the textured undoped LiNbO3\mathrm{LiNbO}_{3} films with (012) preferred reflection. The increase in d33d_{33} constant of doped films probably related to the difference between V5+\mathrm{V}^{5+} and Nb5+\mathrm{Nb}^{5+} cation displacements. K. Toyoura et al. using first principle theoretical investigation showed that larger Nb5+\mathrm{Nb}^{5+} cation displacement in LiNbO3\mathrm{LiNbO}_{3} in comparison with Ta5+\mathrm{Ta}^{5+} cation displacement in LiTaO3\mathrm{LiTaO}_{3} results in higher Curie temperature and spontaneous polarization of LiNbO3\mathrm{LiNbO}_{3} [38]. Therefore, a possible larger V5+\mathrm{V}^{5+} cation displacement may lead to stronger spontaneous polarization, resulting in increase in the d33d_{33} constant.

Experimental details

Piezoelectric LiNbO3\mathrm{LiNbO}_{3} (LNO) film transducers undoped and doped with V were deposited on Si (100) and 304 stainless steel (SS) substrates using RF magnetron sputtering technique. The optimized deposition parameters of the film transducers were as follows: target-substrate distance of 50 mm, radial distance from the inlaid target in the target plane within the range of 0–120 mm, RF power of 900 W, gas pressure of 1 Pa, Ar to O2_2 flow ratio of 6/1, deposition time of 12 h, substrate temperatures in the deposition center and opposite of the V target 340 ∘^{\circ}C and 290 ∘^{\circ}C, respectively. A bias of -8 V was applied to improve morphology and structure uniformity of the deposited films. Figure S1 shows the data of optimizing deposition parameters (gas pressure, Ar to O2_2 flow ratio, deposition time, and bias voltage) to obtain the strongest piezoelectric response (strain constant d33d_{33} and pulse echo response). The schematic diagrams of the deposition system and deposition geometry are shown in Figure 7 and Figure 1a, respectively.

Image not extracted

Figure 7. Schematic diagram of the film deposition system.

Optimization of deposition parameters for V doped LiNbO3 film transducers

Figure S1. Optimization of deposition parameters for V doped LiNbO3_3 film transducers: bias voltage, Ar to O2_2 gas flow ratio, gas pressure, and deposition time (from top to bottom). The d33d_{33} constants as functions of V/Nb atomic ratio (left column), L2_2 echo amplitudes as functions of V/Nb atomic ratio (middle column), and pulse-echo response in the time domain (right column).

Crystalline phase analysis was done using XRD technique (Tongda TDM-10 X-ray diffractometer with Cu Kα_{\alpha} source). The surface morphology and cross-sections of the deposited films were examined by a scanning electron microscope (SEM) TESCAN MIRA3. The surface morphology and RMS roughness were measured by an atomic force microscope (AFM) Shimadzu SPM-9500 J3, operated in tapping mode with a measuring area of 10×10 μm210 \times10\ \mu\mathrm{m}^{2}. V/Nb atomic ratio was studied by an Aztec Energy X-Max 20 EDS analyzer attached to the SEM. Unpolarized room temperature Raman spectra were collected using TESCAN MIRA SEM with Raman attachment with an excitation wavelength of 532.08 nm. The microstructure of V doped LiNbO3_{3} film transducers was studied using a JEOL JEM-F200(HR) high-resolution transmission electron microscope (HRTEM). The HRTEM samples were prepared using the focused ion beam technique in a TESCAN GAIA3 SEM. The Curie temperatures of undoped and V doped LiNbO3_{3} films were measured by a Termo Gravimetry Differenfial Thermal Analyzer (TG/DTA) HITACHI STA7300 at a rate of 20 °C/min in the temperature range of 30 °C–1300 °C in N2_{2} atmosphere using a 70 μl Al2_{2}O3_{3} crucible. The piezoelectric strain constant d33d_{33} were measured using a SA1303A d33 Meter tester.

The ultrasonic response of the film transducers deposited on the SS substrates was measured by a DPR300 ultrasonic pulser-receiver (JSR Ultrasonics), as shown in Figure 8. Before the measurement, 3 mm electrodes on the film were made using silver paste. The SS substrate was used as the bottom electrode. Negative spikes with an amplitude of -100 V and a length of 30 ns were used to generate ultrasonic waves using converse piezoelectric effect, as shown in Figure 8a and Figure 8b. The ultrasound echos reflected from the bottom of the substrate (Figure 8c) were converted into electrical signals by the transducer direct piezoelectric effect (Figure 8d), and then detected by the pulser-receiver with a gain of 27 dB, a low pass filter of 1 MHz, and a high pass filter of 60 MHz. The data was collected and processed by LabView code (Figure 8e).

Image not extracted

Figure 8. Schematic diagram of ultrasonic response measurement. A negative electric spike is applied to the transducer (a). An ultrasonic wave is generated and propagates in the SS substrate (b). The ultrasonic wave is reflected from the substrate bottom (c). The ultrasonic wave is transformed by the transducer to the electrical signal (response) (d). Data processing by LabView code (e).

Conclusions

In this study, LiNbO3\mathrm{LiNbO}_{3} film ultrasonic transducers doped with vanadium (V) were deposited using RF magnetron sputtering technique. In order to reach a wider range of V concentration in the LiNbO3\mathrm{LiNbO}_{3} films we used 30 mm V inlaid target asymmetrically embedded in the 150 mm lithium niobate target. The V/Nb atomic ratio in the deposited films was a decreasing function of the distance from the V target from 0.155 at 0 mm to 0.024 at 120 mm. The d33d_{33} constant measurement of the doped films revealed a significant increase in its value. The highest d33=13.5d_{33} = 13.5 pC/N is observed at V/Nb atomic ratio of 0.07, which is three times higher than 4.76 pC/N of the undoped LiNbO3_3 film deposited at the same geometry. The optimal composition in the deposition geometry used was within the V/Nb ratio range of 0.05 to 0.13. The V doped films were used as ultrasonic transducers to generate longitudinal ultrasonic waves. The echo amplitude generated by V-doped transducers was ∼\sim9 times larger than that of the undoped LiNbO3_3 transducers, which proved the increase in d33d_{33} constant of V doped films. The observed increase in d33d_{33} constant explained by a stronger spontaneous polarization due to possible larger V5+^{5+} cation displacement as compared to that of the Nb5+^{5+} cation.

Acknowledgments

This study was supported by the Fundamental Research Funds for the Central Universities, grant No. 4207-413100036; the First Batch of Special Young Scientists Open Fund for Academician Mao Ming's Workstation in 2024; Open Fund of Hubei Key Laboratory of Electronic Manufacturing and Packaging Integration (Wuhan University), grant No. EMPI2024017. We thank Miss Yanli Guo from the Core Facility of Wuhan University for her assistance with SEM-Raman analysis.

Supplement materials

In order to obtain the highest values of the d33d_{33} constant and echo amplitude of the ultrasonic response, some deposition parameters (bias voltage, Ar/O2\mathrm{O}_{2} flow ratio, gas pressure, and deposition time) were optimized, as shown in Figure S1. The decrease of the d33d_{33} constant at high bias voltage (top row in Figure S1) is related to the degradation of the columnar structure morphology due to ion bombardment damage, as found in our previous study on LiNbO3_{3} films [33]. The better piezoelectric performance at lower gas pressure and longer deposition time can be explained by a thickness dependence found in our previous study, where, due to better structure quality, thicker transducers exhibited larger d33d_{33} constants [35].

References

  1. [1]B.R. Tittmann, C.F.G. Batista, Y.P. Trivedi, C.J. Lissenden III and B.T. Reinhardt, State-of-the-Art and Practical Guide to Ultrasonic Transducers for Harsh Environments Including Temperatures above 2120 °F (1000 °C) and Neutron Flux above 10¹³ n/cm², Sensors 19 (2019) 4755, https://doi.org/10.3390/s19214755
  2. [2]R. Kazys, V. Vaskeliene, High temperature ultrasonic transducers: a review, Sensors 21 (2021) 3200, https://doi.org/10.3390/s21093200
  3. [3]S. Zhang, F. Yu, Piezoelectric Materials for High Temperature Sensors, J. Am. Ceram. Soc., 94 (2011), 3153, https://doi.org/10.1111/j.1551-2916.2011.04792.x
  4. [4]Shinekumar, K., Dutta, S. High-Temperature Piezoelectrics with Large Piezoelectric Coefficients. J. Electron. Mater. 44, 613-622 (2015). https://doi.org/10.1007/s11664-014-3534-2
  5. [5]K.J. Kirk, R. Hou, N. Schmarje, N.M. Pragada, L. Torbay, D. Hutson, Investigation of high-temperature ultrasonic transducer design using lithium niobate piezocomposite, Insight, 57 (2015), 193. http://dx.doi.org/10.1784/insi.2015.57.4.193
  6. [6]D.A. Parks, S. Zhang, B.R. Tittmann, High-temperature (>500 °C) ultrasonic transducers: An experimental comparison among three candidate piezoelectric materials, IEEE Trans. Ultrason. Ferroelect. Freq. Control., 60 (2013), 1010. http://dx.doi.org/10.1109/TUFFc.2013.2659
  7. [7]A. Baba, C.T. Searfass, B.R. Tittmann, High temperature ultrasonic transducer up to 1000 °C using lithium niobate single crystal, Appl. Phys. Lett., 97 (2010), 232901. http://dx.doi.org/10.1063/1.3524192
  8. [8]R. Lu, M. Breen, A. E. Hassanien, Y. Yang, S. Gong, A Piezoelectric Micromachined Ultrasonic Transducer Using Thin-Film Lithium Niobate, J. Microelectromech. S. 29 (2020) 1412–1414, https://doi.org/10.1109/JMEMS.2020.3026547
  9. [9]W. Peng, B. Wang, J. Chang, Z. Liu, G. Wang, S. Dong, Giant piezoelectricity of PNN-PIN-PT ceramics via domain engineering, J. Eur. Ceram. Soc. 44 (2024) 5668-5676, https://doi.org/10.1016/j.jeurceramsoc.2024.03.009
  10. [10]Z.H. Qin, S.M. Wu, Y. Wang, K.F. Liu, T. Wu, S.Y. Yu, Y.F. Chen, Solidly Mounted Longitudinally Excited Shear Wave Resonator (YBAR) Based on Lithium Niobate Thin-Film. Micromachines 12 (2021) 1039, https://doi.org/10.3390/mi12091039
  11. [11]C. Zhao, W. Geng, X. Qiao, et al. Anti-irradiation SAW temperature sensor based on 128 YX LiNbO₃ single crystal. Sensor. Actuat. A–Phys. 333 (2022) 113230, https://doi.org/10.1016/j.sna.2021.113230
  12. [12]Collignon, S., Manor, O., Friend, J. Improving and Predicting Fluid Atomization via Hysteresis-Free Thickness Vibration of Lithium Niobate. Advanced Functional Materials, 28(8), (2018) 1704359. https://doi.org/10.1002/adfm.201704359
  13. [13]O. Buruy, I.I. Syvorotka, Y. Suhak, et al. Determination of optimal crystallographic orientations for LiNbO₃ and LiTaO₃ bimorph actuators. J. Sens. Sens. Syst. 10 (2021) 121–126, https://doi.org/10.5194/jsss-10-121-2021
  14. [14]R.N. Zhukov, A.S. Bykov, D.A. Kiselev, M.D. Malinkovich, Yu.N. Parkhomenko, Piezoelectric properties and surface potential behavior in LiNbO₃ thin films grown by the radio frequency magnetron sputtering, J. Alloy. Compd. 586 (2014) S336–S338, https://doi.org/10.1016/j.jallcom.2013.01.116
  15. [15]E. Dogheche, D. Remiens, S. Shikata, A. Hachigo, H. Nakahata, High-frequency surface acoustic wave devices based on LiNbO₃ diamond multilayered structure, Appl. Phys. Lett. 87 (2005) 213503, https://doi.org/10.1063/1.2135383
  16. [16]Y. Shibata, K. Kaya, K. Akashi, M. Kanai, T. Kawai, S. Kawai, Epitaxial growth and surface acoustic wave properties of lithium niobate films grown by pulsed laser deposition. J. Appl. Phys. 77 (1995) 1498–1503, https://doi.org/10.1063/1.358900
  17. [17]L.C. Sauze, N. Vaxelaire, R. Templier, F. Pierre, C. Maeder-Pachurka et al., 6.9 GHz Film Bulk Acoustic Resonator based on Pulsed Laser Deposited LiNbO₃ Film, 2023 IEEE International Ultrasonics Symposium (IUS), Montreal, QC, Canada, 2023, pp. 1-4, https://doi.org/10.1109/IUS51837.2023.10306426
  18. [18]N. Kambayashi, N. Zaito, H. Akatsuka, M. Kobayashi, LiNbO₃-based sol-gel composite ultrasonic transducer poled at low temperatures, Jpn. J. Appl. Phys. 61 (2022) 1060, https://doi.org/10.35848/1347-4065/ac5720
  19. [19]M. Kobayashi, N. Zaito, T. Hamada, High temperature ultrasonic transducer development by sol-gel composite technique, 2023 IEEE International Ultrasonics Symposium (IUS) (2023) 1–4, https://doi.org/10.1109/IUS51837.2023.10308131
  20. [20]MA. Fakhri, E.T. Salim, M.H.A. Wahid, A.W. Abdulwahhab, Z.T. Salim, U. Hashim, Heat treatment assisted-spin coating for LiNbO₃ films preparation: Their physical properties, J. Phys. Chem. Solids. 131 (2019) 180–188, https://doi.org/10.1016/j.jpcs.2019.03.033
  21. [22]V. Bouquet, E.R. Leite, E. Longo, J.A. Varela, M. Guilloux Viry, A. Perrin, Multi-layered LiNbO₃ films prepared by a polymeric precursor method. J. Eur. Ceram. Soc. 21 (2001) 1521-1524, https://doi.org/10.1016/S0955-2219(01)00055-3
  22. [24]M. Sumets, A. Kostyuchenko, V. Ievlev, S. Kannykın, V. Dybov, Sputtering condition effect on structure and properties of LiNbO₃ films, J. Mater. Sci-Mater. El. 26 (2015) 4250–4256, https://doi.org/10.1007/s10854-015-2975-6
  23. [25]Akiyama, M., Kamohara, T., Kano, K., Teshigahara, A., Takeuchi, Y., Kawahara, N. Enhancement of Piezoelectric Response in Scandium Aluminum Nitride Alloy Thin Films Prepared by Dual Reactive Cosputtering. Advanced Materials, 21, (2009) 593 - 596. https://doi.org/10.1002/adma.200802611
  24. [26]B.C. Grabmaier, W. Wersing and W. Koestler, Properties of undoped and MgO-doped LiNbO3 correlation to the defect structure, Journal of Crystal Growth 110 (1991) 339-347. https://doi.org/10.1016/0022-0248(91)90269-B
  25. [27]A.S. Andrushchak, B.G. Mytsyk, H.P. Laba, O.V. Yurkevych, I.M. Solskii, A.V. Kityk, B. Sahraoui, Complete sets of elastic constants and photoelastic coefficients of pure and MgO-doped lithium niobate crystals at room temperature, J. Appl. Phys. 106 (2009) 073510. https://doi.org/10.1063/1.3238507
  26. [28]F. Wang, D. Sun, Q. Liu, Y. Song, F. Zhang, W. Zhou, Y. Sang, D. Wang, H. Liu, Growth of large size near-stoichiometric lithium niobate single crystals with low coercive field for manufacturing high quality periodically poled lithium niobate, Optical Materials, 125 (2022) 112058, https://doi.org/10.1016/j.optmat.2022.112058
  27. [29]A.Z Simões, A.H.M González, A.A Cavalheiro, M.A Zaghete, B.D Stojanovic, J.A Varela, Effect of magnesium on structure and properties of LiNbO3 prepared from polymeric precursors, Ceramics International, 28, (2002), 265-270. https://doi.org/10.1016/S0272-8842(01)00089-X
  28. [30]Palatnikov, M.N., Sandler, V.A., Sidorov, N.V. et al. Physicochemical, dielectric, and piezoelectric properties and conductivity of LiNbO3:ZnO crystals (4.02 - 8.91 mol %). Tech. Phys. 62, 82 - 89 (2017). https://doi.org/10.1134/S1063784217010170
  29. [31]Palatnikov, M.N., Sandler, V.A., Sidorov, N.V. et al. Anomalous increase in the unipolarity of doped lithium niobate crystals in the temperature range 300 - 400 K. Phys. Solid State 42, 1499 - 1507 (2000). https://doi.org/10.1134/1.1307061
  30. [32]K. Nakamura, S. Kudo, J. Jia and T. Yanagitani, Improvement of Electromechanical Coupling Coefficient of Piezoelectric LiNbO3 by Doping Praseodymium, 2022 IEEE International Ultrasonics Symposium (IUS), Venice, Italy, 2022, pp. 1-4, https://doi.org/10.1109/IUS54386.2022.9958265
  31. [33]X. Zeng, X. Zhang, C. Xu, Z. Zeng, Y. Yu, A. Tolstoguzov, X. Ma, H. Hu, J. Zhang, B. Yang, S. Liu, V.O. Pelenovich, Effects of bias voltage on the structure and ultrasonic response of LiNbO3 film transducers deposited by magnetron sputtering, Ceramics International, 2024, acceptedDOI
  32. [35]X. Zeng, V. Pelenovich, X. Zhang, C. Xu, Y. Ding, Z. Wang, Z. Chen, J. Zhang, B. Yang, A. Pogrebnjak, S. Liu. Response Optimization of LiNbO3 Ultrasonic Transducers for High Temperature Measurement. IEEE. SENS. J. 24 (2024) 7513–7520, https://doi.org/10.1109/JSEN.2024.3353252
  33. [36]Liu, W.; Shan, L.; Lin, Z.; Wan, B.; Yang, B.; Zeng, X.; Yang, B.; Pelenovich, V. Dual-Wave ZnO Film Ultrasonic Transducers for Temperature and Stress Measurements. Sensors 2024, 24, 5691. https://doi.org/10.3390/s24175691
  34. [37]X. Zeng, X. Zhang, V. Pelenovich, Y. Liu, Y. Jiang, L. Zeng, A. Pogrebnjak, R. Vildanov, A. Ieshkin, J. Zhang, B. Yang, S. Liu, High temperature thin film lithium niobium oxide transducers for smart bolts, Ceram. Int. 49 (2023) 7710-7716.DOI
  35. [38]K. Toyoura, M. Ohta, A. Nakamura, K. Matsunaga, First-principles study on phase transition and ferroelectricity in lithium niobate and tantalate, J. Appl. Phys. 118, 064103 (2015). https://doi.org/10.1063/1.4928461

Paper details

vlnc:W_5u59swg3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents