betaFeedback

WorksPhysics and Astronomy

Ablation of black-Si by (Gauss-)Bessel femtosecond laser beams

Abstract

Laser machining and modification of black-Si (b-Si) by femtosecond laser Gaussian (G-) and Gauss-Bessel (GB-) beams are compared at a wavelength of 1030 nm. The GB-beam was generated using a diffractive axicon lens and 10x demagnification optics. It was found that modification of b-Si well below (a factor 50x) the single pulse ablation fluence of 0.2 J/cm2 was possible, corresponding to ablation/melting of nano-needles. The width of modification was almost independent of pulse energy/fluence and had a width of 1/e2-intensity profile at the melting regime. For the GB-beam, the smallest width of laser modification at 0.2 J/cm2 threshold (at the center core) was close to the FWHM of the core of the GB-beam. The aspect ratio of the ablated groove on the surface of b-Si made by GB-beam was twice as large - up to 8 - compared to that achievable with G-beam, and it was at a lower fluence of 4 J/cm2 (50x reduction). Reflectivity of two-side nanotextured b-Si on plasma-thinned 70-micrometers thick Si was strongly reduced in the near-IR range, reaching transmittance >95% at 1.7-2.1 micrometres wavelengths.

Introduction

Black-Silicon (b\mathrm{b}-Si) is a surface-modified form of silicon (Si). It is termed ”black” because it appears visually black due to its ability to absorb in the visible wavelength range with the surface containing a random nano-needle pattern[1, 2, 3]. The typical method for producing it involves plasma etching of silicon wafers. B-Si was produced using a standard gas-based SF6/O2\mathrm{SF}_{6}/\mathrm{O}_{2} etching process, widely available in the context of standard semiconductor industrial processing[4, 5, 6]. The same results can be achieved by using gas breakdown with a femtosecond (fs) laser. However, this method tends to result in an S-doped surface[7]. Other production methods include electrochemical[8, 9], stain etching[10, 11], and metal-assisted chemical etching, which is favored in recent years due to low fabrication costs and versatility in generating high aspect ratio nanostructures[12, 13, 14]. One of the applications of b-Si is Si solar cells for the improvement of energy conversion due to the reflectivity of b-Si can reach values below 1% over the visible spectral range[15, 16, 17, 18, 19], other applications includes photodetectors[20, 21], sensors[22], and even biocidal applications of nanotectured surfaces - mechanical antibiotics[23]. The height of nano-needles is defined by the etching time, ranging from 250 nm (15 min) to 450 nm (30 min)[24].

In order to understand the energy deposition efficiency on such unusual surfaces, it is important to understand how laser machining behaves on such anti-reflective materials and acquire a clearer comprehension of the ablation, amorphization, and melting thresholds[25]. If laser ablation/cutting can utilize smaller pulse energies, then the propensity of self-focusing can be reduced. The increase in efficient energy deposition is of significant interest, especially for Si. For conventional materials, localized melting of the solid may result in volume expansion, which leads to structural failure. However, in very few cases, such as Si, the mass density of molten Si is higher than solid at 2.57 g/cm−3^{-3} and 2.33 g/cm−3^{-3}, respectively. Other such materials include Ge, Ga, Bi, Sb[26], some compounds, such as H2_{2}O, or some alloys, e.g., certain Ce– or Bi– based alloys[27, 28]. Hence, controlled (re-)melting inside the volume of solid Si can be achieved without volume expansion and avoid structural failure. This is promising for hyper-doping of Si by ion implantation and laser annealing[29, 30, 31, 32]. Using beams with a long axial extent of the focal region, such as Bessel-like beams, offers an advantage in efficiently modifying a structured surface, such as b-Si, compared to standard Gaussian beams[33, 34, 35, 36]. With high aspect ratio and precision, Bessel beams are becoming increasingly popular[37, 38] after an early demonstration of 3D capability of fs-laser modifications of transparent materials by Bessel beam[35, 39]. Bessel beams can be generated by several different approaches[36, 40, 41].

Here, we demonstrate the possibility for thinning Si down to tens-of-μ\mum thickness using dry plasma etching technique and further modify the surface by adding b-Si nano-textures on either one or both surfaces. This texturing further reduces the reflectance of b-Si, achieving near 100% transmittance for 70-μ\mum thick double-sided b-Si sample at a wavelength of ∼2 μ\sim2~\mum. We investigated laser structuring by ablation on the anti-reflective b-Si surfaces. It was found that surface modification through melting of the nano-needles occurs below the ablation threshold of Si (0.2 J/cm2^{2}[25, 42]), extended to fluences by an order of magnitude smaller using Gaussian (G-) as well as Gauss-Bessel (GB-)beams. In order to compare the energy deposition of G- and GB-beams, geometrical analysis of the focusing and ablation sites was carried out. It is shown that the Liu method of ablation threshold determination[43] is applicable to the central core of the GB-beam.

Absorbance spectra measured with an integrating sphere

Figure 1. Absorbance A=1−(R+T)A = 1 - (R + T) spectra measured with integrating sphere by detection of reflectance RR and transmittance TT of b-Si (40 and 20 min etched; one side etched of 0.5-mm-thick Si wafer); measured with UV-Vis spectrometer (Lambda 1050 UV/Vis, PerkinElmer). The inset shows schematics of measurements.

Experimental: samples and methods

Black-Si: plasma thinning and reflectance in visible-to-IR spectral range

Black-Si (b-Si) is produced by dry plasma etching using a simple SF6/O2\mathrm{SF}_6/\mathrm{O}_2 gas mixture1.

Silicon thinning of a standard 300, 500 μ\mum wafer down to tens-of-μ\mum has become a fast and simple fabrication step. It starts with lithography performed using AZ 4562 photoresist: spin-coated at 1500 rpm for 30 s and soft-baked at 110 ∘C110\,^\circ\mathrm{C} for 4–5 min. A photomask was generated using the direct-write system (Micropatterning SF100 XPRESS) and aligned with the substrate. UV exposure was conducted using an ABM UV flood light source at 450 mJ/cm2^2. Development was completed in undiluted AZ 726 MIF for 12 min, with visual inspection to confirm full pattern formation. A post-development bake was ramped from 90 ∘C90\,^\circ\mathrm{C} to 140 ∘C140\,^\circ\mathrm{C} at 1 ∘C1\,^\circ\mathrm{C}/min, held at 140 ∘C140\,^\circ\mathrm{C} for 5 min, and cooled gradually. The final resist thickness was approximately 10.9 μ\mum.

Silicon etching was carried out using SF6\mathrm{SF}_6 gas in a Plasmalab100 ICP380 RIE system (Oxford Instruments). Over 30 minutes, approximately 250 μ\mum of silicon and 5 μ\mum of photoresist were etched, corresponding to an estimated etch rate of ∼8.3\sim8.3 μ\mum/min. These values were approximated using a profilometer (Ambios XP-200), and the process remained stable with no observed plasma flickering or reflected power issues.

Figure 1 shows the angular dependence of the absorbance of b-Si with different heights of nano-needles, corresponding to 40 min and 20 min plasma etch. For a broad spectral range of 450–1000 nm, low reflectance R<1%R < 1\% (large absorbance A>99%A > 99\%) was observed even up to angles of incidence θi∼30∘\theta_i \sim30^\circ. Figure 2 shows the infrared (IR) transmittance of one-sided and two-sided b-Si samples with a Si wafer thickness of ∼70\sim70-µm. The texturing further increased the transmission in the IR region from 80% to nearly 100% for the one-sided and two-sided b-Si structures, respectively.

Figure 2. (a) IR transmittance of one and two-sided b-Si (70-μ\mum-thick; see schematic thumbnail images as insets). (b) Plasma thinned Si wafer from 250 μ\mum down to 25 μ\mum at the selected regions. Direct-write mask was used to define the pattern. Silicon etching was carried out using SF6_6 gas in a Plasmalab100 ICP380 reactive ion etching system (Oxford Instruments). Over a 30-minute process, approximately 250 μ\mum of silicon and 5 μ\mum of photoresist were etched, corresponding to an estimated silicon etch rate of ∼\sim8.3 μ\mum/min. These values were approximated using a profilometer (Ambios XP-200).

Geometrical parameters of the focal region produced by an axicon

Axicon is a conical lens that transforms an incoming plane wave of a Gaussian intensity distribution into a Gauss-Bessel beam with a long axial extension. Refractive and diffractive axicons are used. For the refractive axicon, the cone acts as a prism sending the incoming light into a tilted beam, making a half-cone angle γ\gamma (with optical axis). Refractive axicons are defined by the wedge angle required to form the full 180° angle at the tip of the axicon (same angle at the base of the axicon), Then, from Snell’s law sin⁡(α+γ)=naxsin⁡α\sin(\alpha+\gamma)=n_{\mathrm{ax}}\sin\alpha, where the refractive index of axicon nax=1.4n_{\mathrm{ax}}=1.4 (for silica).

The diffractive axicons are defined by the ring angle (peak-to-peak angle), which is equivalent to the full-cone angle 2γ2\gamma of the refractive axicon; we used γ∼1∘\gamma\sim1^\circ axicon (the ring angle 2∘2^\circ).

Length of the central non-diffracting part of the Gauss-Bessel beam is defined by the diameter DD of the beam as Zmax⁡=D2sin⁡γ=π2NZRBZ_{\max}=\frac{D}{2\sin\gamma}=\frac{\pi}{2}NZ_{\mathrm{RB}}, where the number of rings N=Dsin⁡γλN=\frac{D\sin\gamma}{\lambda} and ZRB=π22k⊥2Z_{\mathrm{RB}}=\frac{\pi^2}{2k_{\perp}^2} is the Rayleigh length associated with the asymptotic width of an individual ring (ZRB=2.656Z_{\mathrm{RB}}=2.656 mm for λ=1030\lambda=1030 nm and γ=1∘\gamma=1^\circ). The component of wavevector perpendicular to propagation k⊥=ksin⁡γk_{\perp}=k\sin\gamma, where the wavevector k=2π/λk=2\pi/\lambda. The GB-beam central spot size is typically defined as twice the first zero of the Bessel function J0(k⊥ρ)J_0(k_{\perp}\rho), where ρ\rho is the radius d0=2ρ0=4.816k⊥=4.816ksin⁡γd_0=2\rho_0=\frac{4.816}{k_{\perp}}=\frac{4.816}{k\sin\gamma} (45.2 μ\mum for λ=1030\lambda=1030 nm and γ=1∘\gamma=1^\circ); the full width half maximum (FWHM) central cross section is d0FWHM=0.36λsin⁡γd_0^{\mathrm{FWHM}}=0.36\frac{\lambda}{\sin\gamma} (21.2 μ\mum)[44].

For actual fabrication, these values of d0d_0 and Zmax⁡Z_{\max} are further down-sized using a 4f relay telescope; here we used Md=10×M_d=10\times demagnification which also correspondingly increased cone angle γ′\gamma' (in air for the sample position) sin⁡γ=sin⁡γ′/Md\sin\gamma=\sin\gamma'/M_d as described in the next section, Sec. II C, and shown in Figure 3.

Laser micro-machining setup

Figure 3. Laser micro-machining setup (WOP, Lithuania) based on Carbide-40W fs-laser (Light Conversion, Lithuania). (a) Alignment of GB-beam. (b) Fabrication and observation solution; LPA1,2 are laser power attenuators, BD1,2 - beam dumps, CAM1,2,3 – observation CCD cameras, DM – dichroic mirror, RDM – removable dielectric mirror, AX - diffractive axicon, µPS1,2,3 – micro-positioning stages and OBJ are objective lenses with numerical aperture NANA; the final objective lens has f-number of f#=F/D=1/(2NA)=1.92f\# = F/D = 1/(2NA) = 1.92 with focal length F=20F = 20 mm and diameter of entrance pupil D=10.4D = 10.4 mm (10× Mitutoyo Plan Apo NIR). The solid red line in (b) indicates the fabrication laser beam path, and the dashed line is the sample observation beam path. These schematics do not show a mirror that switches beam paths. The observation beam path in (b) is used for G-beam machining.

The energy flux associated with any ring of the Gauss-Bessel beam is equal to that of any other ring and of the central spot. The optimum central spot illumination efficiency is given by[45]:

ϵop=PringPtotal=2e×λw0sin⁡γ=2e×1N(1)\epsilon_{op} = \frac{P_{ring}}{P_{total}} = \frac{2}{\sqrt{e}} \times\frac{\lambda}{w_0 \sin\gamma} = \frac{2}{\sqrt{e}} \times\frac{1}{N} \tag*{(1)}

where w0w_0 is the 1/e21/e^2-radius of the Gaussian beam intensity, i.e., the diameter of the laser beam on the axicon is D=2w0=3.5D = 2w_0 = 3.5 mm in this study. Then, the length of non-diffractive region Zmax=100Z_{max} = 100 μ\mum, the number of rings N=59N = 59, and the efficiency of central spot illumination ϵop=2%\epsilon_{op} = 2\%; for comparison, the G-beam efficiency of light collection into the focus is 100%.

The axial intensity distribution along the GB-beam propagation (z-axis) is given[44]:

IGB(z)=P08πzsin⁡2γλw02exp⁡[−2(zsin⁡γw0)2](2)I_{GB}(z) = P_0 \frac{8\pi z \sin^2\gamma}{\lambda w_0^2} \exp\left[-2\left(\frac{z\sin\gamma}{w_0}\right)^2\right] \tag*{(2)}

where w0w_0 is the waist of the Gaussian beam incident on the axicon and P0P_0 [W] is the peak power of the Gaussian beam.

The axial intensity (Eqn. (2)) maximum for the diffractive axicon has two axially-shifted positions for two perpendicular polarisations. This results in two distinct peaks when a circularly polarised incident beam is used[46]. It is caused by the form birefringence with two distinct refractive indices. This was the case for our study with circularly polarised beam (λ\lambda/4-plate was inserted into the laser output). Hence, the final 10× down-sized GB-beam had double length of ∼500\sim500 μ\mum; for one polarisation, Zmax/10≈266Z_{max}/10 \approx266 μ\mum is expected for the used setup/geometry (see Sec. II C and Figure 4).

Figure 4. Determination of the central core diameter of the GB-beam from the width (diameter), WW, of ablation hole in 40-nm-thick AlOx mask on Si. (a) Diameter ablated in alumina mask W2(ln⁡(Ep))W^2(\ln(E_p)). The slope of the best fit defines the radius d0/2=slope/2d_0/2 = \sqrt{\mathrm{slope}/2} of the central core. The inset photo shows an image of the GB-beam at the alignment position (see Figure 3(a)). (b) Determination of the effective diameter d0d_0 along the focal region of the GB-beam. A sample of b-Si was placed at the position marked by an arrow, which corresponded to d0=5.2 μmd_0 = 5.2\ \mu\mathrm{m}. The axial extent of the non-diffracting region was ∼500 μm\sim500\ \mu\mathrm{m}. Circularly polarised light was used, which caused doubling of the characteristic axial GB-beam profile (Eqn. (2)) shown in the inset for ordinary and extraordinary refractive indices of the form birefringent structure of diffractive axicon no,en_{o,e}.

Laser micro-machining setup

For the GB-beam we used Workshop of Photonics (WOP) fs-fab station with a Carbide (Light Conversion) laser at 40 W, fundamental harmonic 1030 nm, repetition rate 602.7 kHz, pulse duration 201 fs (Figure 3). A diffractive axicon with a ring angle of 2γ=2∘2\gamma= 2^\circ was used (Holo OR). A combination of f=200f = 200 mm lens (placed close to the axicon) with an objective lens MPlan APO NIR 10×10\times Mitutoyo, NA=0.26NA = 0.26 and f=20f = 20 mm was used to form a 4f system for the imaging and downscaling 10 times the intensity distribution on the sample (Figure 3(b)). Observation and inspection were carried out by MPlanApoNIR 2×2\times NA=0.055NA = 0.055.

In a separate experiment, determination of the ablation threshold at the central core of the GB-beam was carried out using a 40-nm-thick AlOx mask on Si wafer surface and applying the standard Liu method developed for G-beams[43]. Ablation of AlOx mask makes a very distinct hole and is useful to determine the central focal spot of GB-beam at the fabrication position; such masks were used in the fabrication of light trapping surface of Si solar cell[47].

The diameter of the ablated hole in the nano-thin alumina mask vs fs-pulse energy was plotted W2(ln⁡[Ep])W^2(\ln[E_p]) for different positions along the non-diffracting zone using the same objective lenses and setup described above (Figure 4(a)). The sample position for fs-laser machining was decided by axial location, where the steepest dependence of the diameter of the ablated hole on the pulse energy was observed (Figure 4(a)). The corresponding threshold pulse energy was Ep(th)≈900E_p^{(th)} \approx900 nJ (entire pulse) and the effective beam waist for the ablation at the center core was d0/2=2.6 μmd_0/2 = 2.6\ \mu\mathrm{m}. The estimate of average fluence per central core (per pulse) for the used efficiency ϵop=1%\epsilon_{\mathrm{op}} = 1\% of GB-beam (1% is considered instead of 2% due to circularly polarised beam and separation of the intensity maxima into two peaks for two perpendicular polarisations). One finds Fp(th)=ϵopEp(th)π(d0/2)2=0.043 J/cm2F_p^{(th)} = \frac{\epsilon_{\mathrm{op}}E_p^{(th)}}{\pi(d_0/2)^2} = 0.043\ \mathrm{J/cm^2}. The difference of diameters at the first-zero and FWHM of the GB-beam for the used geometry is d0/d0FWHM=2.13d_0/d_0^{\mathrm{FWHM}} = 2.13. Then the energy in the central core per d0FWHMd_0^{\mathrm{FWHM}} for the ablation threshold corresponds to the threshold fluence Fp(th)×2.132=0.2 J/cm2F_p^{(th)} \times2.13^2 = 0.2\ \mathrm{J/cm^2}, which exactly matches that for Si. The d0FWHM=d0/2.13=5.2/2.13=2.44d_0^{\mathrm{FWHM}} = d_0/2.13 = 5.2/2.13 = 2.44 μ\mum.

The analysis of focusing using geometry outlined above for diffractive axicon γ=1∘\gamma= 1^\circ and 10×10\times demagnification, corresponds to the center core energy of 1% of that incident, which is focused onto a spot of d0FWHM=2.44d_0^{\mathrm{FWHM}} = 2.44 μ\mum. These conditions will be used for analysis of fs-laser modification (melting and ablation) of b-Si and determination of the fluence at the center core (defined by d0FWHMd_0^{\mathrm{FWHM}}).

Results

Ablation and energy deposition onto b-Si was investigated using 1030 nm/200 fs pulses at different spacing between pulses in a linear scan. Gaussian and Gauss-Bessel fs-laser beams were used with comparable size of the central focal spot: 2.8 μ\mum (Gaussian) and 2.6 μ\mum (center-core Gauss-Bessel) diameters.

Gaussian beam

The diameter of the Gaussian (G-)beam can be estimated as dG=1.22λ/NAd_G = 1.22\lambda/NA for the objective lens of numerical aperture; NA=0.45NA = 0.45 in this study. It is the diameter of the Airy disk, i.e., between two minima (zero intensity) in cross section for a plane wave focusing limited only by diffraction. In terms of energy under the envelope of the Gaussian beam intensity profile (86.5%) and within the Airy-disk for the plane wave (84%), both are very similar.

Figure 5 shows a typical sample with lines laser ablated at different pulse energies and spacing between adjacent irradiation spots. A sample of b-Si was cleaved across the line pattern for the side view observation of the ablation depth DD and width WW (Figure 5(a)). At very low pulse fluence, well below the ablation threshold of Si 0.2 J/cm2^2[42], surface modification of b-Si had clear imprint of melted nano-needles with discernable rim with diameter of 2.8 μ\mum, which matched the focal spot size for the used NA=0.45NA = 0.45 objective lens 2rG=1.22λ/NA=2.82r_G = 1.22\lambda/NA = 2.8 μ\mum. This diameter was used for the determination of the average pulse fluence Fp=Ep/(πrG)2F_p = E_p/(\pi r_G)^2.

Black-Si ablation by Gaussian fs-laser beam

Figure 5. Black-Si ablation by Gaussian fs-laser beam. (a) Photo of fs-laser machined regions and side view SEM image of ablation crater. (b) SEM image of laser-ablated sites with distinct imprints of 2.8 μ\mum focal spots on the surface of b-Si. The diffraction limit 1.22λ/NA=2.81.22\lambda/NA = 2.8 μ\mum for λ=1030\lambda= 1030 nm wavelength and objective lens of numerical aperture NA=0.45NA = 0.45.

The dependence of ablation/modification width on the pulse fluence is presented as W2(ln⁡[Fp])W^2(\ln[F_p]) in Figure 6(a). Log-log presentation is chosen to better reveal the change of slope, which is linked to the mechanism of the modification. This is similar to the Lin-log presentation of the same dependence known as the Liu method[43]. For the largest separation between pulses close to the focal diameter, the threshold of modification is close to 0.2 J/cm2^2, which is the expected threshold for Si ablation. However, at much lower fluence ∼4\sim4 mJ/cm2^2 by a factor of 50, a clear surface modification was observed. It is linked to the melting of nano-needles of b-Si and was lower as observed on flat Si[25]. There was almost no change in the width of melt-modification. This confirms that direct energy deposition occurred only over the focal spot and the lateral heat diffusional spread was negligible, as shown in Figure 6(b). Interestingly, at the maximal used fluence, the width was increasing at a steeper rate vs FpF_p, departing from the expected linear dependence of the Liu plot. This could be linked to the better energy deposition at the surface of b-Si due to low reflectance. Figure 7 shows the evolution of the depth and aspect ratio of the ablated groove. For the low pulse overlap, close to single pulse ablation conditions, the threshold fluence projects

Width versus single pulse fluence and SEM images of black-Si

Figure 6. (a) The width vs. single pulse fluence W2(Fp)W^2(F_p) for different pulse densities (pulse-to-pulse separation/spacing) ranging from just separated pulses to strongly overlapped. Error bars for single pulse data are 20%. (b) SEM images of the lowest fluence modification made by remelting the b-Si surface.

Figure 7. (a) Depth vs. fluence per pulse. The top inset shows a SEM image of high-fluence, small spacing ablation. (b) The aspect ratio vs. fluence per pulse.

to the expected 0.2 J/cm20.2\ \mathrm{J}/\mathrm{cm}^{2} for Si.

Gauss-Bessel beam

To calculate the energy, fluence and irradiance (intensity) per pulse at the center core of the Gauss-Bessel (GB-)beam is not trivial, as in the case of the Gaussian beam, since the energy of the GB-beam is spread over the number of rings, which carry the same energy and converge onto optical axis at different locations along the propagation. Moreover, for the diffractive axicon, there are two axially shifted intensity distributions (Eqn. (2)) for two perpendicular polarisations[46]. This reduce energy distribution per ring twice. It is noteworthy that the Liu method can be used for different non-Gaussian beam shapes[48].

We adopted the established Liu method[43] for G-beam to measure the effective diameter of the focal spot at different locations along the focal region (non-diffractive zone of GB-beam) as described in Sec. II C. The test sample for measurement of ablated diameter vs the pulse energy was 40-nm-thick AlOx coated mask on Si. It was placed at different positions of ∼1\sim1 mm long focal region of the GB-beam using the same axicon and focusing conditions.

According to the Liu method[43] for the G-beam, the diameters, WW, of the abated pits (or width of the ablated line) on the sample at different pulse energies are determined. The intercept of a linear fit of W2[ln⁡(Ep)]W^{2}[\ln(E_p)] corresponds to a threshold pulse energy EthE_{th} (also threshold fluence Fth=Eth/(πw02)F_{th}=E_{th}/(\pi w_0^{2})) while the slope corresponds to 2w022w_0^{2}.

W2=2w02ln⁡(Ep/Eth).(3)W^{2}=2w_0^{2}\ln(E_p/E_{th}). \tag*{(3)}

The waist (radius) of the Gaussian beam at the focus is w0=slope/2w_0=\sqrt{\mathit{slope}/2} (Eqn. (3)).

We verified this experimental procedure of focal diameter determination using ablation of AlOx mask on Si using GB-beam for the center-core ablation/modification as described in Sec. II C and shown in Figure 4. It was determined that the ablation threshold of Si 0.2 J/cm20.2\ \mathrm{J}/\mathrm{cm}^{2} corresponds to the energy at the center core over its FWHM cross section. Also, as in the case of G-beam, the diameter of the center core (energy deposition) is determined from the low pulse energies.

Typical patterns of GB-beam ablated b-Si are shown in Figure 8. The dark-field optical image in (a) shows a pattern at high energy/fluence at the surface of the sample and 1 μm1~\mu\mathrm{m} depth. SEM images at the same high fluence and down to low energy EpE_p when only the center core is discernible are overlayed in (b). Counterintuitively, the width of the central opening was narrower for the high EpE_p. This is caused by the formation of a high-aspect-ratio central groove and redeposition/oxidation around the center core. For this particular reason, analysis by Eqn. (3) cannot be applied for the b-Si; however, it was verified for the mask hole ablation of alumina-coated Si as described previously (Sec. II C).

Dark-field image and SEM top-view images of black-Si ablation by Gauss-Bessel beam

Figure 8. Black-Si ablation by Gauss-Bessel beam. (a) Dark-field image (with NA=0.9NA = 0.9 objective lens) of ablated line at high pulse energy EpE_p. The top inset shows the lowest pulse energy ablated line and the bottom inset shows the Bessel function where x=k⊥ρx = k_{\perp}\rho. (b) SEM top-view images of ablated lines at different pulse energies (by group number). Ripples at off-center locations of GB-beam show that polarisation was linear (or elliptical) rather than circular, which is aimed at the center core.

At the lowest pulse energies, a clear molten b-Si surface is observed with clearly discernible 2.6 μm2.6~\mu\mathrm{m} diameter (Figure 9). It is very close to the expected FWHM diameter of 2.44 μm2.44~\mu\mathrm{m} as determined from the geometrical conditions and focusing (Sec. II C). This diameter was used to calculate pulse fluence at the center core as previously validated in the adaptation of the Liu method. The sample position for the alumina mask ablation on Si and b-Si was the same as all the beam delivery optics.

SEM image of b-Si ablated by Gauss-Bessel beam at lowest pulse energy

Figure 9. SEM image of b-Si ablated by Gauss-Bessel beam at lowest pulse energy. It was used to determine the diameter of the center core. The right-side inset shows a photo of the b-Si sample cleaved across all the patterns recorded under different conditions for the side-view imaging of the depth and width. The position of the first ring maximum is barely recognisable (marked by a red arrow).

Figure 10 shows the depth and aspect ratio evolution with fluence per center core at different pulse-to-pulse spacings. Close to linear dependence was observed over the span of one order of magnitude in FpF_p (per pulse per center core). Since the large surface area is affected, the determination of width WW had a large uncertainty (obvious also from Figure 8(b)). This is why some data points are excluded from the aspect ratio plot in (b). A formidable high aspect ratio >5> 5 was observed for the center fluence >2.5 J/cm2> 2.5~\mathrm{J/cm^2}. A deep central ablation groove was formed under those conditions, and the imprint of up to 3 rings was present on the surface. Apparently, the energy deposition has a larger aspect ratio as compared with the G-beam case. This can be facilitated by the anti-reflective property of b-Si, deeper optical light penetration due to 1030 nm wavelength being close to the bandgap of Si.

Figure 10. The depth DD (a) and aspect ratio W/DW/D vs effective fluence per center-core d0=2.6 μmd_0 = 2.6\ \mu\mathrm{m} diameter. The fluence was calculated as EpE_p over the area of diameter d0d_0 (experimentally observed at lowest fluences); a factor of 1% was used for energy redistribution into the center core as determined in Sec. II C.

Discussion

It is shown here that the Liu methodology of determination of ablation threshold, originally demonstrated for G-beams, is applicable to the center core GB-beams. When the FWHM of the central core was taken as the diameter of the energy deposition, the efficiency of energy at the center beam was calculated using ideal Bessel beam properties at the employed focusing conditions. This is useful for comparison of G- and GB-beam laser machining, at least at the semi-quantitative level. Exact Bessel-like beam geometry and properties are affected by focusing, filling/clipping at the entrance apertures, and demagnification telescope alignment in addition to the type of optical element, refractive, diffractive, metasurface, and the quality, which sets phase imperfections.

Anti-reflective property of b-Si allowed very precise control of energy deposition with clear accumulation effect revealed in Figure 6: the smaller spacing, i.e., the larger pulse overlap, the slope of W2W^2 vs FpF_p dependence is less steep, especially towards smaller fluencies. Apparently, the cumulative effect of irradiation is enhancing energy deposition and remelting of nano-needles. Larger droplets at stronger overlap signify larger surface temperatures over larger volumes, which was able to minimize surface area by forming spheroidal droplets. Such controlled melting has potential for surface doping of materials when b-Si is coated by other elements which are potential dopants for n- or p-type conductivity as well as formation of intra-band for IR sensors[49] Black-Si produced by plasma etch has a surface with native oxide similar to the flat Si with detectable F presence[50]. This makes doping and remelting of nano-needles with surface deposited dopants a promising avenue for tailoring surface properties and chemistry.

We can put forward a conjecture that light localisation between nano-needles and at the interface Si-air with large E-field components normal-to-the-interface contributes to energy deposition. Inducing defects which enhance absorption of subsequent pulses drived energy deposition onto this antireflective surface. Indeed, it corresponds to the p-polarisation rather than s-polarisation. and has lower reflectance (see simulations in ref.[51]).

Ablation threshold of black-Si

Easily recognisable surface modification is observed at a much lower threshold than expected for Si ablation at 0.2 J/cm2^2 per pulse (for optically flat Si)[42]. Ablation thresholds of metals (m) and dielectrics/semiconductors (d) is related to ionisation and are estimated from the energy deposition which exceeds the cumulative binding energy (enthalpy of vaporisation) ϵb\epsilon_b and electron work function (for metals) wew_e or ϵb\epsilon_b and ionisation potential JiJ_i for dielectrics and semiconductors[52]:

Fth(m)=38(ϵb+we)λne2π,Fth(d)=34(ϵb+Ji)ls∗neA.(4)F_{\mathrm{th}}^{(m)} = \frac{3}{8}(\epsilon_b+w_e)\frac{\lambda n_e}{2\pi}, \qquad F_{\mathrm{th}}^{(d)} = \frac{3}{4}(\epsilon_b+J_i)\frac{l_s^* n_e}{A}. \tag*{(4)}

where ls∗=c/(ωκ)≡λ/(2πκ)l_s^* = c/(\omega\kappa) \equiv\lambda/(2\pi\kappa) is the absorption depth (the skin depth for the EE field) in the plasma with electron density nen_e and refractive index n∗=n+iκn^* = n + i\kappa with cc and ω\omega being the speed and cyclic frequency of light, respectively; AA is the absorption coefficient (for good metals A≈2ωls∗cA \approx\frac{2\omega l_s^*}{c}). At high intensity, the pulse can exceed the ionization threshold and the first ionization is completed (before the end of the pulse), at which the number density of free electrons saturates at the level ne≈nan_e \approx n_a, where nan_a is the number density of atoms in the target material.

For ablation of dielectrics and semiconductors, which are ionized during the fs-pulse, a metal-like reflective plasma has A≈0.5A \approx0.5; i.e., half of the light is absorbed by the strongly excited material. The exact absorbed portion A=1−RA = 1 - R, where RR accounts for the reflected portion of the laser pulse, can be precisely calculated from the refractive index n∗≡n+iκn^* \equiv n + i\kappa as A=4n/[(n+1)2+κ2]A = 4n/[(n + 1)^2 + \kappa^2]. The ablation threshold of metals Eqn. (4) scales with wavelength Fth(m)∝λ5/2F_{\mathrm{th}}^{(m)} \propto\lambda^{5/2}. Equation (4) is based on the required energy budget to evaporate material ϵb\epsilon_b and to ionize it: wew_e for metals and JiJ_i for dielectrics. These thresholds are confirmed by experiments for metals and dielectrics.[52]

For unperturbed Si, ϵb=383\epsilon_b = 383 kJ/mol, the first ionisation potential Ji=786.52J_i = 786.52 kJ/mol (8.152 eV per atom) and typical n∗=3.5+i0.01n^* = 3.5 + i0.01 corresponding to a low doping Si ne=1×1016n_e = 1 \times10^{16} cm−3^{-3} (or resistivity ∼1\sim1 Ω\Omega.cm); the skin depth reciprocal to the absorption coefficient (for intensity E2E^2) ls=1/α=(4πκ/λ)−1=8.2l_s = 1/\alpha= (4\pi\kappa/\lambda)^{-1} = 8.2 μ\mum; α=1.22×103\alpha= 1.22 \times10^3 cm−1^{-1}, A=69.1%A = 69.1\% at λ=1030\lambda= 1030 nm wavelength. Upon fs-laser irradiation, the electron density is approaching the critical plasma density ncr=ω2ϵ0me∗/e2n_{\mathrm{cr}} = \omega^2\epsilon_0m_e^*/e^2 at which the real part of permittivity is decreasing and the imaginary part is increasing ϵ∗=ϵ1+iϵ2\epsilon^* = \epsilon_1 + i\epsilon_2. Under such conditions, the most efficient energy deposition is taking place (energy per volume), and dielectric breakdown follows. For λ=1030\lambda= 1030 nm, ncr=1.05×1021n_{\mathrm{cr}} = 1.05 \times10^{21} cm−3^{-3}, where ϵ0\epsilon_0 is the permittivity of free space, me∗m_e^* is the effective mass of electron. The dielectric breakdown is defined by the real part of permittivity becoming zero: ϵ1=(n2−κ2)≡0\epsilon_1 = (n^2 - \kappa^2) \equiv0 and n=κn = \kappa; ϵ2=2nκ\epsilon_2 = 2n\kappa defines absorption losses of light in the sample. Assuming that photo-excited Si approach n=κ=0.2n = \kappa= 0.2, one finds A=54.1%A = 54.1\% and for the plasma density close to critical ne≈ncrn_e \approx n_{\mathrm{cr}}, at which the ablation threshold of Si becomes FthSi=0.232F_{\mathrm{th}}^{\mathrm{Si}} = 0.232 J/cm2^2 (Eqn. (4)); for these conditions ls≡ls∗/2=410l_s \equiv l_s^*/2 = 410 nm (close to the height of b-Si nano-needles[24]) α=2.44×104\alpha= 2.44 \times10^4 cm−1^{-1}. The threshold is close to the experimentally observed ablation threshold on flat Si by ultra-short laser pulses 0.2 J/cm2^2[42].

When Si is turned into black-Si, the material properties ϵb\epsilon_b and JiJ_i remain the same, however, the absorption coefficient AA is effectively increased due to the reduced reflectivity. Indeed, when there is no transmission T=0T = 0 (an optically thick sample), the energy conservation A+R+T=1A + R + T = 1 demands A=1−RA = 1 - R. This can be interpreted as a reduced ablation threshold expected for the anti-reflective surface and observed experimentally in this study (Figure 6).

Ablation (removal of material) takes place when the pool of energy absorbed by electrons transfers it to the lattice and heats it above the evaporation conditions (the binding energy). The temperature of electrons in the skin depth is Te=(1−R)Fp/(lsϵcna)T_e = (1 - R)F_p/(l_s\epsilon_c n_a)[52], where FpF_p is the fluence per pulse, ce∼3/2c_e \sim3/2 is the electron specific heat, which acquires the value of 3/2 of the ideal gas after full ionization of material, and nan_a is the atomic number density of the material (for Si n0=ρSiNav/MSi=4.99×1022n_0 = \rho_{\mathrm{Si}}N_{\mathrm{av}}/M_{\mathrm{Si}} = 4.99 \times10^{22} cm−3^{-3}, here the mass density ρSi=2.33\rho_{\mathrm{Si}} = 2.33 g/cm3^3, molar mass MSi=28.08M_{\mathrm{Si}} = 28.08 g and NavN_{\mathrm{av}} is the Avogadro number). This energy deposited into electrons acts as an energy reservoir for ablation after its transfer to lattice atoms/ions, with TeT_e reaching ∼2\sim2 keV in typical metal and silicon drilling[53]. The maximum of material removed by a single pulse can be estimated from energy conservation[52]: Vmax⁡=(1−R)Ep/(naEat/NA)V_{\max} = (1 - R)E_p/(n_aE_{\mathrm{at}}/N_A), where EatE_{\mathrm{at}} [J/mol] is the molar enthalpy of atomization and NAN_A the Avogadro constant. Also here, the low reflectivity maximises material removal facilitated by larger absorbance (Eqn. (4)), which is additionally enhanced due to p-pol. at a large angle of incidence at the laser pulse and side-walls of nano-needles θi∼θB≈75∘\theta_i \sim\theta_B \approx75^\circ, where θB\theta_B is the Brewster angle.

Conclusions and Outlook

It is demonstrated that the anti-reflective surface of b-Si facilitates very precise energy deposition at the focal spot with a smooth transition from the ablation (removal of material via ionisation above 0.2 J/cm20.2\ \mathrm{J/cm^2}) to a well-controlled energy deposition and melting of the surface nanotexture at fluencies 4 mJ/cm24\ \mathrm{mJ/cm^2}. The width of the molten - re-solidified region closely follows the focal spot size. The reduction of ablation threshold by 50×50\times is related to the increased absorbance (reduced reflectance) of b-Si. Change of reflectance of Si vs b-Si RRb=1−Rb1−R=AbA≈40%1%∼40\frac{R}{R_b}=\frac{1-R_b}{1-R}=\frac{A_b}{A}\approx\frac{40\%}{1\%}\sim40. This factor of ablation threshold reduction is achievable due to optical properties and energy deposition into the very same Si (same binding energy and ionisation potential), governed by geometrical factors of the surface texture. It is noteworthy that an estimation of such a reduction factor of ablation threshold is only qualitative since the energy deposition is a dynamic fast process governed via free carrier (electron-hole) generation and self-action on the incoming light, which determines the energy deposition via the instantaneous complex permittivity ε∗\varepsilon^* of irradiated surface of b-Si. Further experimental efforts to explore the reduction of ablation thresholds due to the texture of the same material as the host substrate could open new methods for controlling resolution and feature size of the nanoscale energy deposition.

Acknowledgments

This study was carried out via ARC DP240103231 grant. This work was performed on the fs-fab laser station at Swinburne, which is jointly funded with the Melbourne Centre for Nanofabrication (MCN), the Victorian Node of the Australian National Fabrication Facility (ANFF). We thank Workshop-of-Photonics (WOP) Ltd., Lithuania for the patent licence and technology transfer project by which the industrial fs-laser fabrication setup was acquired for Nanolab, Swinburne.

References

  1. [1]Y.-F. Huang, S. Chattopadhyay, Y.-J. Jen, C.-Y. Peng, T.-A. Liu, Y.-K. Hsu, C.-L. Pan, H.-C. Lo, C.-H. Hsu, Y.-H. Chang, C.-S. Lee, K.-H. Chen, and L.-C. Chen, “Improved broadband and quasi-omnidirectional anti-reflection properties with biomimetic silicon nanostructures,” Nature Nanotechnology 2, 770–774 (2007).DOI
  2. [2]Y. Nishijima, R. Komatsu, S. Ota, G. Seniutinas, A. Balčytis, and S. Juodkazis, “Anti-reflective surfaces: Cascading nano/microstructuring,” APL Photonics 1, 076104 (2016).DOI
  3. [3]Z. Fan, D. Cui, Z. Zhang, Z. Zhao, H. Chen, Y. Fan, P. Li, Z. Zhang, C. Xue, and S. Yan, “Recent Progress of Black Silicon: From Fabrications to Applications,” Nanomaterials 11, 41 (2020).DOI
  4. [4]K. M. Eisele, “SF 6, a Preferable Etchant for Plasma Etching Silicon,” Journal of The Electrochemical Society 128, 123–126 (1981).DOI
  5. [5]H. Jansen, M. De Boer, H. Wensink, B. Kloeck, and M. Elwenspoek, “The black silicon method. VIII. A study of the performance of etching silicon using SF6/O2-based chemistry with cryogenic wafer cooling and a high density ICP source,” Microelectronics Journal 32, 769–777 (2001).
  6. [6]V. T. H. Nguyen, F. Jensen, J. Hübner, P. Leussink, and H. Jansen, “On the formation of black silicon in SF6-O2 plasma: The clear, oxidize, remove, and etch (CORE) sequence and black silicon on demand,” Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films 38, 043004 (2020).DOI
  7. [7]M.-J. Sher, Y.-T. Lin, M. T. Winkler, B. Franta, and E. Mazur, “Femtosecond laser doped silicon for photovoltaic applications,” in Nano-Optics for Enhancing Light-Matter Interactions on a Molecular Scale, edited by B. Di Bartolo and J. Collins (Springer Netherlands, Dordrecht, 2013) pp. 449–449.DOI
  8. [8]X. Liu, P. R. Coxon, M. Peters, B. Hoex, J. M. Cole, and D. J. Fray, “Black silicon: Fabrication methods, properties and solar energy applications,” Energy Environ. Sci. 7, 3223–3263 (2014).DOI
  9. [9]R. Bilyalov, R. Lüdemann, W. Wettling, L. Stalmans, J. Poortmans, J. Nijs, L. Schirone, G. Sotgiu, S. Strehlke, and C. Lévy-Clément, “Multicrystalline silicon solar cells with porous silicon emitter,” Solar Energy Materials and Solar Cells 60, 391–420 (2000).DOI
  10. [10]R. J. Martín-Palma, L. Vázquez, J. M. Martínez-Duart, M. Schnell, and S. Schaefer, “Antireflective porous-silicon coatings for multicrystalline solar cells: The effects of chemical etching and rapid thermal processing,” Semiconductor Science and Technology 16, 657–661 (2001).DOI
  11. [11]M. Saadoun, N. Mliki, H. Kaabi, K. Daoudi, B. Bessais, H. Ezzaouia, and R. Bennaceur, “Vapour-etching-based porous silicon: a new approach,” Thin Solid Films 405, 29–34 (2002).DOI
  12. [12]H.-D. Um, N. Kim, K. Lee, I. Hwang, J. Hoon Seo, Y. J. Yu, P. Duane, M. Wober, and K. Seo, “Versatile control of metal-assisted chemical etching for vertical silicon microwire arrays and their photovoltaic applications,” Scientific Reports 5, 11277 (2015).DOI
  13. [13]13 C. Huo, J. Wang, H. Fu, X. Li, Y. Yang, H. Wang, A. Mateen, G. Farid, and K.-Q. Peng, “Metal-Assisted Chemical Etching of Silicon in Oxidizing HF Solutions: Origin, Mechanism, Development, and Black Silicon Solar Cell Application,” Advanced Functional Materials 30, 2005744 (2020).DOI
  14. [14]14 J. Soueiti, R. Sarieddine, H. Kadiri, A. Alhussein, G. Lerondel, and R. Habchi, “A review of cost-effective black silicon fabrication techniques and applications,” Nanoscale 15, 4738–4761 (2023).DOI
  15. [15]15 M. Halbwax, T. Sarnet, Ph. Delaporte, M. Sentis, H. Etienne, F. Torregrosa, V. Vervisch, I. Perichaud, and S. Martinuzzi, “Micro and nano-structuration of silicon by femtosecond laser: Application to silicon photovoltaic cells fabrication,” Thin Solid Films 516, 6791–6795 (2008).DOI
  16. [16]16 K. Nguyen, D. Abi-Saab, P. Basset, E. Richalot, F. Marty, D. Angelescu, Y. Leprince-Wang, and T. Bourouina, “Black silicon with sub-percent reflectivity: Influence of the 3d texturization geometry,” in 2011 16th International Solid-State Sensors, Actuators and Microsystems Conference (IEEE, 2011) pp. 354–357.DOI
  17. [17]17 J. Oh, H.-C. Yuan, and H. M. Branz, “An 18.2%-efficient black-silicon solar cell achieved through control of carrier recombination in nanostructures,” Nature Nanotechnology 7, 743–748 (2012).DOI
  18. [18]18 M. Otto, M. Algasinger, H. Branz, B. Gesemann, T. Gimpel, K. Füchsel, T. Käsebier, S. Kontermann, S. Koynov, X. Li, V. Naumann, J. Oh, A. N. Sprake, J. Ziegler, M. Zilk, and R. B. Wehrspohn, “Black Silicon Photovoltaics,” Advanced Optical Materials 3, 147–164 (2015).
  19. [19]19 J.-H. Chai, B. Wong, and S. Juodkazis, “Black-silicon-assisted photovoltaic cells for better conversion efficiencies: a review on recent research and development efforts,” Materials Today Energy 18, 100539 (2020).DOI
  20. [20]20 J. Lv, T. Zhang, P. Zhang, Y. Zhao, and S. Li, “Review application of nanostructured black silicon,” Nanoscale Research Letters 13, 110 (2018).DOI
  21. [21]21 Z. Zhao, Z. Zhang, J. Jing, R. Gao, Z. Liao, W. Zhang, G. Liu, Y. Wang, K. Wang, and C. Xue, “Black silicon for near-infrared and ultraviolet photodetection: A review,” APL Materials 11, 021107 (2023).DOI
  22. [22]22 Q. Tan, F. Lu, C. Xue, W. Zhang, L. Lin, and J. Xiong, “Nano-fabrication methods and novel applications of black silicon,” Sensors and Actuators A: Physical 295, 560–573 (2019).DOI
  23. [23]23 E. P. Ivanova, J. Hasan, H. K. Webb, G. Gervinskas, J. Juodkazis, V. K. Truong, A. H. Wu, R. N. Lamb, V. A. Baulin, G. S. Watson, J. A. Watson, D. E. Mainwaring, and R. J. Crawford, “Bactericidal activity of black silicon,” Nature Communications 4, 2838 (2013).DOI
  24. [24]24 Y. Nishijima, H. Nishijima, M. Ohashi, T. Katkus, and S. Juodkazis, “Efficient water evaporation using black silicon,” ACS Sustainable Resource Management 2, 316–321 (2025).DOI
  25. [25]25 M. Garcia-Lechuga, N. Casquero, J. Siegel, J. Solis, R. Clady, A. Wang, O. Utéza, and D. Grojo, “Amorphization and ablation of crystalline silicon using ultrafast lasers: Dependencies on the pulse duration and irradiation wavelength,” Laser & Photonics Reviews 18, 2301327 (2024).DOI
  26. [26]26 N. N. Greenwood and A. Earnshaw, Chemistry of the Elements, 2nd ed. (Butterworth-Heinemann, Oxford Boston, 1997).
  27. [27]27 R. Perkins, L. Geoffrion, and J. Biery, Densities of Some Low Melting Plutonium Alloys (IAEA, 1966) pp. p. 473–491.
  28. [28]28 R. A. Khairulin, S. V. Stankus, R. N. Abdullaev, and V. M. Sklyarchuk, “The density and interdiffusion coefficients of bismuth-tin melts of eutectic and near-eutectic composition,” High Temperature 48, 188–191 (2010).DOI
  29. [29]29 W. Yang, J. Mathews, and J. Williams, “Hyperdoping of Si by ion implantation and pulsed laser melting,” Materials Science in Semiconductor Processing 62, 103–114 (2017), advanced doping methods in semiconductor devices and nanostructures.DOI
  30. [30]30 C. Li, J.-H. Zhao, and Z. Chen, “Infrared absorption and sub-bandgap photo-response of hyperdoped silicon by ion implantation and ultrafast laser melting,” Journal of Alloys and Compounds 883, 160765 (2021).DOI
  31. [31]31 Z. Tong, M. Bu, Y. Zhang, D. Yang, and X. Pi, “Hyperdoped silicon: Processing, properties, and devices,” (2022).DOI
  32. [32]32 J. Kaupūzs, P. Onufrijevs, P. Ščajev, H. H. Cheng, G.-E. Chang, and Y. Tsuchiya, “Phase field calculations of Sn redistribution in GeSn/Si structures after pulsed laser irradiation,” Optics Laser Technology 189, 113046 (2025).DOI
  33. [33]33 R. L. Nowack, “A tale of two beams: An elementary overview of Gaussian beams and Bessel beams,” Studia Geophysica et Geodaetica 56, 355–372 (2012).DOI
  34. [34]34 M. Duocastella and C. Arnold, “Bessel and annular beams for materials processing,” Laser & Photonics Reviews 6, 607–621 (2012).DOI
  35. [35]35 R. Stoian, M. K. Bhuyan, G. Zhang, G. Cheng, R. Meyer, and F. Courvoisier, “Ultrafast Bessel beams: Advanced tools for laser materials processing,” Advanced Optical Technologies 7, 165–174 (2018).DOI
  36. [36]36 A. S. Rao, “A conceptual review on Bessel beams,” Physica Scripta 99, 062004 (2024).DOI
  37. [37]37 M. K. Bhuyan, F. Courvoisier, P. A. Lacourt, M. Jacquot, R. Salut, L. Furfaro, and J. M. Dudley, “High aspect ratio nanochannel machining using single shot femtosecond Bessel beams,” Applied Physics Letters 97, 081102 (2010).DOI
  38. [38]38 A. Mathis, F. Courvoisier, L. Froehly, L. Furfaro, M. Jacquot, P. A. Lacourt, and J. M. Dudley, “Micro-machining along a curve: Femtosecond laser micromachining of curved profiles in diamond and silicon using accelerating beams,” Applied Physics Letters 101, 071110 (2012).
  39. [39]39 A. Marcinkevicius, S. Juodkazis, B. Matsuo, V. Mizeikis, and H. Misawa, “Application of bessel beams for microfabrication of dielectrics by femtosecond laser,” Japanese Journal of Applied Physics 40, L1197 (2001).
  40. [40]S. N. Khonina, N. L. Kazanskiy, P. A. Khorin, and M. A. Butt, “Modern types of axicons: New functions and applications,” Sensors 21 (2021), 10.3390/s21196690.DOI
  41. [41]R. Dharmavarapu, S. Bhattacharya, and S. Juodkazis, “Diffractive optics for axial intensity shaping of bessel beams,” Journal of Optics 20, 085606 (2018).DOI
  42. [42]J. Bonse, S. Baudach, J. Krüger, W. Kautek, and M. Lenzner, “Femtosecond laser ablation of silicon–modification thresholds and morphology,” Appl Phys A 74, 19–25 (2002).DOI
  43. [43]J. M. Liu, “Simple technique for measurements of pulsed gaussian-beam spot sizes,” Opt. Lett. 7, 196–198 (1982).pubmed.ncbi.nlm.nih.gov/19710869
  44. [44]V. V. Belloni, L. Froehly, C. Billet, L. Furfaro, and F. Courvoisier, “Generation of extremely high-angle bessel beams,” Appl. Opt. 62, 1765–1768 (2023).DOI
  45. [45]R. Herman and T. Wiggins, “Production and uses of diffractionless beams,” Journal of the Optical Society of America A 8, 932–942 (1991).DOI
  46. [46]V. Anand, J. Maksimovic, T. Katkus, S. H. Ng, O. Ulčinas, M. Mikutis, J. Baltrukonis, A. Urbas, G. Slekys, H. Ogura, D. Sagae, T. Pikuz, T. Somekawa, N. Ozaki, A. Vailionis, G. Seniutinas, V. Meizeikis, K. Glazebrook, J. P. Brodie, P. R. Stoddart, L. Rapp, A. V. Rode, E. G. Gamaly, and S. Juodkazis, “All femtosecond optical pump and x-ray probe: holey-axicon for free electron lasers,” Journal of Physics: Photonics 3, 024002 (2021).
  47. [47]T. Katkus, S. H. Ng, H. Mu, N. H. A. Le, D. Stonytė, Z. Khajehsaeidimahabadi, G. Seniutinas, J. Baltrukonis, O. Ulčinas, M. Mikutis, V. Sabonis, Y. Nishijima, M. Rienäcker, U. Römer, J. Krügener, R. Peibst, S. John, and S. Juodkazis, “Bessel-beam direct write of the etch mask in a nano-film of alumina for high-efficiency si solar cells,” Advanced Engineering Materials 26, 2400711 (2024).arxiv.org/abs/2403.14237
  48. [48]M. Garcia-Lechuga and D. Grojo, “Simple and robust method for determination of laser fluence thresholds for material modifications: an extension of Liu’s approach to imperfect beams,” Open Res Europe 1, 7 (2021).
  49. [49]J. Fu, D. Yang, and X. Yu, “Hyperdoped crystalline silicon for infrared photodetectors by pulsed laser melting: A review,” physica status solidi (a) 219, 2100772 (2022).DOI
  50. [50]P. Ščajev, T. Malinauskas, G. Seniutinas, M. Arnold, A. Gentle, I. Aharonovich, G. Gervinskas, P. Michaux, J. Hartley, E. Mayes, P. Stoddart, and S. Juodkazis, “Light-induced reflectivity transients in black-si nanoneedles,” Solar Energy Materials and Solar Cells 144, 221–227 (2016).DOI
  51. [51]D. P. Linklater, F. Haydous, C. Xi, D. Pergolesi, J. Hu, E. P. Ivanova, S. Juodkazis, T. Lippert, and J. Juodkazytė, “Black-si as a photoelectrode,” Nanomaterials 10 (2020), 10.3390/nano10050873.DOI
  52. [52]E. G. Gamaly, A. V. Rode, and B. Luther-Davies, “Ablation of solids by femtosecond lasers: Ablation mechanism and ablation thresholds for metals and dielectrics,” Physics of Plasmas 18, 949 – 957 (2002).DOI
  53. [53]S. Juodkazis, H. Okuno, N. Kujime, S. Matsuo, and H. Misawa, “Hole drilling in stainless steel and silicon by femtosecond pulses at low pressure,” Appl. Phys. A 79, 1555 – 1559 (2004 (DOI: 10.1007/s00339-004-2846-0)).DOI

Paper details

vlnc:W_62bjpu87
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 8

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents