WorksPhysics and Astronomy
Thermoelectric and Magnetic Properties in Doped FeVAl within a Bipolar Random Anderson Model
Abstract
We investigate the thermoelectric and magnetic properties of Si-substituted -type and Ti-substituted -type Heusler alloy FeVAl using the bipolar random Anderson model, which has been introduced recently to study antisite-defect effects associated with the sign change of the Seebeck coefficient in thermally quenched FeVAl. Based on the electronic states of both -type and -type compounds, with the rigid-band shift of the Fermi energy and a temperature-dependent scattering rate taken into account, we elucidate how antisite defects simultaneously influence thermoelectric transport and local magnetic moments. We find that the magnetic moments are enhanced in -type FeVAl, whereas they are suppressed in -type FeVAl compared with the undoped compound. These contrasting magnetic responses highlight the impact of antisite spin polarization on thermoelectric properties and demonstrate the crucial role of antisite defects in realizing magneto-thermoelectric functionalities in Heusler-type alloys.
Introduction
The Heusler-type intermetallic -based compounds are known as promising candidates for thermoelectric materials.1) Stoichiometric is nonmagnetic semimetal and the valence-band maximum is located at the point, while the conduction-band minimum lies at the X point, with a small band overlap between them,2–5) resulting in a pseudogap around the Fermi level .6, 7) This subtle electronic structure is the origin of the diverse thermoelectric properties induced by element substitution and quenching processes. In , the resistivity increases as the temperature is lowered and the Seebeck coefficient exhibits positive values over a wide temperature range,8) indicating that holes are the majority carriers. Upon Si substitution, in , however, decreases as temperature is lowered and changes dramatically from positive to negative (-type) even for small Si concentrations of and .9, 10) This strong sensitivity primarily originates from the introduction of electron carriers, which shifts to higher energies within the pseudogap. On the other hand in the -type , 11–13) realized by substituting Ti for V resulting in holes in the valence band, the resistivity becomes metallic at low temperatures9, 10) similar to -type .9, 10) The remains positive and its magnitude increases with increasing Ti concentration up to , and then decreases.11) This -type behavior has also been observed in Mn-substituted .14) As for understanding these transport features in doped , a phenomenological two-band model has been shown to qualitatively account for the temperature dependence of in 15) and evaluations of in both -type and -type have also been performed using the linearized Boltzmann transport equation with a constant relaxation time combined with first-principles electronic-structure calculations.16)
Besides the transport properties, magnetic properties have a diversity. In contrast to nonmagnetic , ferromagnetic order has been observed at low temperatures in Si-substituted -type 17–19) which has been regarded as a weak itinerant ferromagnet,19) since the field-induced magnetic moment is small and weakens with increasing temperature. Furthermore, quenching from high temperatures generates a magnetic moment an order of magnitude larger than that of the unquenched sample.20) Quenched undoped also induces a magnetic moment,21) but its magnitude is only about one-third of that observed in quenched -type 20) highlighting the crucial role of electron doping. Since thermal quenching introduces antisite defects, it is reasonable to attribute such large moments to, for example, V antisites on the Fe sublattice () and Fe antisites on the V sublattice (). Hence, magnetic properties are seen to be strongly affected by antisite defects.
The introduction of antisites also causes remarkable changes in : in , the sign of becomes negative,21) whereas in -type , the magnitude of is reduced.20) A reduction in in has also been reported in thin films22) and annealed samples. Regarding -type , no systematic study has clarified the role of the interplay between antisite defects and their spin polarization. It is therefore necessary to provide a theoretical framework that elucidates the microscopic mechanism of roles played by antisite defects. Hence, systematic understanding based on microscopic analyses in terms of model Hamiltonians is needed to clarify how carrier doping affects the thermoelectric and magnetic properties.
In this paper, we theoretically investigate the thermoelectric properties of doped and the spin polarization associated with antisite defects. We first confirm that a simple rigid-band picture, in which shifts upon carrier doping, captures the overall features of thermoelectric behavior of doped . To incorporate antisites into our theory, we employ an extended version of the single-impurity Anderson model,24) the bipolar random Anderson model (BPRAM),25) which has been introduced recently. In this model, and antisites are treated as randomly distributed impurities in the valence and conduction bands, respectively, and induce carrier redistribution between the two bands while conserving the total electron number. This BPRAM framework has successfully explained the sign change of caused by antisite defects in Fe₂VAl.25) In -type Fe₂VAl, we find that both V and Fe antisites are spin-polarized, in contrast to the undoped case where only V exhibits spin polarization.25) This leads to a magnetic moment approximately twice that of the antisites in undoped Fe₂VAl, when the antisite concentration is fixed. The Seebeck coefficient decreases upon antisite introduction, consistent with experimental observations.20) In -type Fe₂VAl, by contrast, antisite defects lose their magnetic moments because their levels shift above , resulting in only a small change in . The interplay between thermoelectric and magnetic properties is seen to be governed by the spectral conductivity, which is strongly influenced by spin-polarized antisite defects. These findings provide a new guideline for controlling spin-polarized antisite defects in doped Fe₂VAl and demonstrate the crucial role of antisite defects in realizing magneto-thermoelectric functionalities in Heusler-type alloys.
This paper is organized as follows. In Sect. 2, we present calculated results for the density of states, spectral conductivity, resistivity, and Seebeck coefficient in doped Fe₂VAl. In Sect. 3, we introduce the BPRAM and show the electronic states and thermoelectric properties in the presence of antisite defects. Finally, Sect. 4 discusses the implications of the proposed spin polarization of antisite defects and provides a summary.
Thermoelectric Properties in doped Fe₂VAl
First-principles electronic structure calculations based on the local density approximation or generalized gradient approximation for Fe₂VAl have shown a negative band gap, , in which the valence-band maximum at lies higher in energy than the conduction-band minimum at X.2–5) A two-band model with eV and the Fermi energy located at the bottom of the conduction band leads to results consistent with the experimentally observed and .25) Figure 1(a) illustrates this model.
Figure 1. Schematic illustration of the electronic states in Fe₂VAl. (a) undoped Fe₂VAl, (b) -type and (c) -type Fe₂VAl. The valence band around the point is predominantly composed of Fe 3 orbitals with a degeneracy of , whereas the conduction band near the X point mainly consists of V 3 orbitals with a degeneracy of . The top of the valence band is set as the energy reference. The Fermi energy is indicated by horizontal dashed lines. The energy gap , defined as the energy difference between the valence-band top and the conduction-band bottom, is negative () in (a), whereas in (b) and (c) (see text).
According to our previous work,25) we assume an energy dispersion approximated in terms of effective masses. The density of states (DOS) per spin for the valence (v) and conduction (c) bands is given by
with or . The local Green’s function is given by
where is the half bandwidth with (2.0) eV and is the band degeneracy with (1).25) Here, and , where the self-energy arises from hybridization with antisite defects, as described below. By introducing an intrinsic scattering rate for a system without antisite defects, the complex energy is defined as with for the valence band and for the conduction band, where the top of the valence band is taken as the origin of energy (see Figure 1).
The spectral conductivity , which governs electrical and heat currents, is given by26)
with
where is the elementary charge and was determined to reproduces thermoelectric properties in Fe₂VAl: eV and eV.25)
Since the valence-band top and conduction-band bottom are located at different momenta, we assume that there is no direct interplay between the two bands. Under this assumption, the total spectral conductivity is given by . In terms of , the electrical conductivity and thermoelectric conductivity , describing the electrical current density within the linear response theory under an electric field and a temperature gradient ,27) are given by the Sommerfeld-Bethe relationship,
and
Here, is the Fermi distribution function, , where is the Boltzmann constant. The chemical potential is a temperature-dependent quantity, , determined so as to give the total electron density with the total DOS per spin . The and are given by and , respectively. In general, contains contributions from both electrons and phonons;[28] however, the phonon-drag contribution is expected to be small in the present system and is neglected in the following.
Si substitution is expected to modify the underlying electronic states. One obvious effect is an increase in electron carriers due to the replacement of Al by Si, which results in a shift of toward higher energies. Another possible effect is a change of . Indeed, an examination of first-principles results for [15] reveals a very small increase in on the order of 10 meV. Such an enhancement of has also been pointed out in a phenomenological two-band analysis of .[15] Based on these observations, we take as shown in Figure 1(b). Ti-substituted FeVAl, on the other hand, introduces hole carriers into the valence band, resulting in a shift of toward lower energies. At the same time, a upward shift of the V-dominated conduction band is expected, since V is replaced by Ti that has a higher energy level. This modification changes , and we take , as shown in Figure 1(c).
Both n-type FeVAlSi and p-type FeVTiAl exhibit metallic behavior in at low temperatures for .[9, 11] This indicates the presence of a temperature-dependent scattering rate arising from electron-phonon interactions. Accordingly, we incorporate a linear temperature dependence into the
scattering rate for the spectral conductivity by replacing in with . The parameters and , together with , are determined so as to reproduce the experimentally observed for .[9, 11] We obtain meV for both n-type and p-type FeVAl. The value of is taken to be eV/K for the conduction (valence) band and eV/K for the valence (conduction) band in n-type (p-type) FeVAl, where the band hosting the carriers is assumed to have a larger . These values of are comparable to those reported for GeYSbAgTe.[29] Finally, the effects of magnetic ordering reported experimentally[12, 17, 18, 19] are not considered in the present study, since they are expected to become significant only at low temperatures. In addition, possible contributions from magnetic fluctuations to the thermoelectric properties are beyond the scope of the present work and are left for future investigation.
Figure 2(a) shows the total DOS in n-type FeVAl. The vertical line indicates the position of . The zero-temperature spectral conductivity is shown in the inset. Figure 2(b) and Figure 2(c) present the calculated and , respectively, together with experimental data for in FeVAlSi.[9] The calculated results (red solid lines) qualitatively coincide with the experimental data. The change from positive in FeVAl (black dash-dotted line) to negative values originates from the shift of into the conduction band. When decreases from 0.08 eV, corresponding to a decrease in , the increases and the peak in shifts to lower temperatures (not shown). This trend is qualitatively consistent with experimental observations.[9, 10]
Figure 2. (Color online) Electronic states and transport properties in n-type FeVAl. (a) Total DOS per spin. The energy zero is set at the top of the valence band. The inset shows the zero-temperature total spectral conductivity per spin. The vertical line denotes the position of the Fermi energy . (b) Temperature dependence of the resistivity . (c) Temperature dependence of the Seebeck coefficient . The red lines represent calculated results. The black dotted lines correspond to experimental data for FeVAlSi with [9]. For comparison, the calculated results for FeVAl$[25] are shown by black dash-dotted lines in (b) and (c).
Figure 3(a) shows the DOS and the zero-temperature spectral conductivity for -type FeVAl. Figures 3(b) and 3(c) present the calculated and , respectively, together with experimental data for FeVTiAl.[11] It is seen that the calculated (red solid lines) is located between the experimental and data, while the calculated is smaller than that in undoped FeVAl at low temperatures below K and increases with increasing toward K. It is of interest to check experimentally the latter trend at high temperatures.
Doped FeVAl with antisite defects
Thermal quenching of FeVAl-based compounds induces antisite defects.[20, 21, 23] Among these defects, we focus on Fe and V antisites, which affect the underlying electronic states in the valence V and conduction Fe band, respectively. An Fe (V) antisite can be regarded as an impurity in the valence (conduction) band, which is described by the Anderson model.[24] However, since such antisites are randomly distributed within the host sublattice, their effects are more appropriately described by an Anderson-type model with randomly distributed impurities. In addition, charge transfer between an antisite defect and a host band may occur. Assuming that Fe and V are present in equal concentrations, charge conservation requires that the number of electrons transferred from Fe antisites to the conduction band equals the number of holes transferred from V antisites to the valence band. This charge redistribution can give rise to bipolar effects and substantially reduce the energy gap making it strongly negative.
To account for this phenomenon, we introduce the BPRAM,[25] whose Hamiltonian is given by
where is the creation operator for a mobile electron with momentum , spin , and dispersion , is the creation operator for a localized electron at an antisite , and with . is the antisite energy level, is on-site Coulomb interaction at the antisites, and represents the hybridization between mobile and antisite electrons.
Electrons in the valence and conduction bands are scattered by randomly distributed antisite defects via the hybridization term in Eq. (7). This scattering induces a -independent but spin-dependent self-energy for the electrons, denoted by . By applying a single-site approximation for the antisite defects and employing a self-consistent -matrix approximation for the self-energy, we obtain the following self-consistent equation,[25]
where denotes the antisite concentration. Here, is the Green’s function for antisite states, which is written as with . The effective antisite energy level is given by , where the spin-dependent antisite occupation number is defined as .
For the antisite concentration, we assume , as in our previous work on FeVAl.[25] To satisfy the bipolar condition arising from charge transfer together with carrier doping introduced by Si and Ti substitutions, we set the energy gap and Fermi energy to eV and eV for -type FeVAl, and eV and eV for -type FeVAl. For the antisite energy levels, we assume that their energy offsets from the top of the valence band (for ) and from the bottom of the conduction band (for ) remain constant and independent of carrier doping. We set this offset to 0.16 eV. This yields eV, while eV for -type FeVAl and eV for -type FeVAl. Since both and lie below in -type FeVAl, we expect spin polarization at both V and Fe antisites, using eV and eV as in our previous study.[25] In contrast, no spin polarization is expected for antisite defects in -type FeVAl because both and lie above . These expectations are indeed confirmed in our calculations, as shown below. We note that these parameters are chosen as representative values, and our conclusions presented below are robust against small variations in these parameters.
We self-consistently determine the self-energies in Eq. (8) and calculate and to examine the effect of antisite defects on the thermoelectric properties of -type and -type FeVAl. The red solid lines in Figure 4(a) and Figure 4(b) show the calculated and , respectively, for -type FeVAl. The resistivity is reduced compared with the value obtained in the absence of antisites and becomes metallic up to K. These changes are consistent with the experimental data for quenched FeVAlSi,[20] shown by the blue dotted line. This reduction in originates from an enhancement of the spectral conductivity due to the increased DOS near .
Figure 4. (Color online) Temperature dependence of (a) the calculated resistivity and (b) the Seebeck coefficient in the BPRAM for -type FeVAl with antisite defects (red solid lines). The blue dashed lines correspond to experimental data for undoped FeVAlSi containing antisites.[20] For comparison, the results without antisite defects, identical to the red solid lines in Figs. 2(b) and 2(c), are shown by black dashed lines.
To clarify this point, we show the spin-resolved electronic states in the BPRAM in Figure 5. Figure 5(a) and Figure 5(b) display the DOS of the band electrons for each spin. Because of charge transfer, both the valence and conduction bands contribute to the DOS near , resulting in an enhancement compared with the case without antisites [see Figure 2(a)]. As a result, the total spectral conductivity near , shown in Figure 5(g) and Figure 5(h), becomes larger than that in the inset of Figure 2(a), although the deformation of occurs due to the scattering rate shown in Figure 5(e) and Figure 5(f). This enhanced spectral conductivity leads to the reduction of .
Figure 5. (Color online) Electronic states of n-type FeVAl with antisite defects obtained by the BPRAM. The left and right columns correspond to down-spin and up-spin quantities, respectively. (a), (b) The DOS per spin for total electrons (black solid line), valence electrons (red dashed line), and conduction electrons (blue dash-dotted line). (c), (d) The DOS per spin for V and Fe antisites. (e), (f) Imaginary part of the spin-dependent self-energy for valence (red solid line) and conduction (blue solid line) electrons. (g), (h) Zero-temperature spectral conductivity per spin for total (black solid line), valence (red dashed line), and conduction (blue dash-dotted line) electrons. The vertical lines indicate the Fermi energy .
The magnitude of in Figure 4(b) is reduced in the presence of antisite defects at low temperatures compared with the case without antisites. This reduction is mainly attributed to the decreased slope of near , as shown in Figure 5(g) and Figure 5(h), which is caused by antisite scattering. In particular, the conduction-band contribution around eV is suppressed owing to the presence of a peak in at the same energy, leading to a gentler slope of near . The valence-band contribution around eV is also suppressed due to a peak in , resulting in a reduced hole contribution to in the vicinity of . These effects contribute to the negative values of at low temperatures.
With increasing temperature above 300 K, the calculated in Figure 4(b) becomes positive, in contrast to the experimentally observed negative values for quenched FeVAlSi,[20] shown by the blue dotted line. The origin of this discrepancy is unclear, but one possible explanation is a slight modification of due to the presence of antisite defects in n-type FeVAl: a reduction of in the conduction band would enhance the n-type carrier contribution at high temperatures.
Figure 5(b) and Figure 5(d) display the DOS of the antisite states, defined as . Both V and Fe have spin polarization, since energies of their down- and up-spin states with in between. Consequently, the total magnetic moment, given by the sum of the contributions from V and Fe, becomes approximately twice as large as that in FeVAl, where only V antisites are spin-polarized,[25] when the antisite concentration is the same. This enhancement may account for the experimental observation that Si-substituted samples exhibit larger antisite-induced magnetic moments.[20]
Figure 6 shows the calculated and for p-type FeVAl with antisite defects. The magnitude of does not change significantly, although its slope is modified and its value at K increases compared with the case without antisites. The magnitude of at K is also enhanced in the presence of antisites. To confirm these predictions, systematic experiments that control the antisite concentration in p-type FeVTiAl are desired in the future.
Figure 6. (Color online) Temperature dependence of (a) the calculated resistivity and (b) the Seebeck coefficient in the BPRAM for p-type FeVAl with antisite defects (red solid lines). For comparison, the results without antisite defects, identical to the red solid lines in Figure 3(b) and Figure 3(c), are shown by black dashed lines.
The corresponding electronic states are shown in Figure 7. The Fermi energy lies inside the valence band, as shown in Figure 7(a). No spin polarization appears, since the DOS of V and Fe is located above [see Figure 7(b)]. In Figure 7(d), we find that near is strongly suppressed due to the large shown in Figure 7(c). This suppression is the origin of the enhancement of and at low temperatures in Figure 6.
Figure 7. (Color online) Electronic states of p-type FeVAl with antisite defects obtained by the BPRAM. No spin polarization is present. (a) DOS per spin for the total electrons (black solid line), valence electrons (red dashed line), and conduction electrons (blue dash-dotted line). (b) DOS per spin for V, which produces a shoulder, and for Fe, which corresponds to a peak. (c) Imaginary part of the self-energy for the valence (red solid line) and conduction (blue solid line) electrons. (d) Zero-temperature spectral conductivity per spin for the total (black solid line), valence (red dashed line), and conduction (blue dash-dotted line) electrons. The vertical line represents the Fermi energy .
Summary and discussions
Spin polarization of antisite defects gives rise to magnetic moments in FeVAl. In our previous work,[25] we found that V is spin-polarized whereas Fe is not in undoped FeVAl. In this paper, we show that both V and Fe are spin-polarized in n-type FeVAl, while neither of them is polarized in p-type FeVAl, as discussed in § 3. This difference originates from the relative positions of the antisite energy levels with respect to , which depend on whether the system is n-type or p-type.
Figure 8 summarizes the schematic electronic states in FeVAl with antisite defects (the right side of the vertical energy axis). From this illustration, we can predict that antisite-induced magnetic moments decrease from n-type to p-type FeVAl, provided that the antisite concentration is the same. The recent experimental observation that Si-substituted samples exhibit larger antisite-induced magnetic moments compared with the undoped case[20] may reflect this behavior. It is also interesting to note that the magnetic moments in p-type FeVMnAl decrease with increasing .[14] If the magnetic moment at originates from antisite defects, a possible source of the reduction may be the shift of deeper into the valence band, as illustrated in Figure 8(c). Further systematic investigations of the effects of antisite defects in doped FeVAl are desired in the future.
Figure 8. (Color online) Schematic illustration of the electronic states and the spectral conductivity in FeVAl with antisite defects. (a) Undoped FeVAl, (b) n-type, and (c) p-type FeVAl. The top of the valence band is set as the energy reference. The Fermi energy is indicated by horizontal dashed lines. The left side of the vertical energy axis represents the spectral conductivity averaged over spins for the valence band, (red solid curve), and for the conduction band, (blue solid curve). The electronic states are shown on the right side of the vertical energy axis. The valence band is composed of Fe 3d orbitals, whereas the conduction band consists of V 3d orbitals. The DOS per spin ( and ) for the valence and conduction bands is shown by black solid lines. The antisite DOS for V and Fe is depicted by red and blue solid lines, respectively. In (a), the energy level of V, denoted by , appears below for the -spin antisite state, while the -spin state is split upward by the on-site Coulomb interaction . Both spin states of Fe appear above at . In (b), the spin states of Fe are also split by , whereas in (c) no splitting occurs for either V or Fe.
In the left side of the vertical energy axis in Figure 8, the spectral conductivity for the valence (conduction) band, , is shown by red (blue) solid curves. These results highlight the interplay between thermoelectric and magnetic properties in FeVAl with antisite defects. In Figure 8(a), near is suppressed and flattened due to the spin- level of the spin-polarized V antisite. These changes reduce the hole contribution to , resulting in a negative Seebeck coefficient, consistent with the behavior reported for undoped FeVAl.[25] In n-type FeVAl, shown in Figure 8(b), the spin- level of spin-polarized Fe suppresses and flattens . Consequently, and take similar values near , leading to a small Seebeck coefficient at low temperatures, as demonstrated in Figure 4(b). In p-type FeVAl, all antisite levels lie above , and their influence on the spectral conductivity near is weak, as shown in Figure 6(b). These close relationships between spectral conductivity and spin-polarized electronic states demonstrate the crucial role of an. antisite defects in controlling both thermoelectric and magnetic properties of Heusler-type alloys. Dynamical effects associated with fluctuations of antisite magnetic moments, which are not taken into account in the present study, may further contribute to the modification of .
Figure 9. (Color online) Calculated power factor (PF) of undoped and doped FeVAl with (solid lines) and without (dashed lines) antisite defects. The black, red, and blue lines represent the results for undoped, -type, and -type FeVAl, respectively.
The power factor (PF), defined as , serves as a guideline for evaluating the energy conversion efficiency of thermoelectric materials. Figure 9 summarizes the calculated PF for undoped and doped FeVAl with and without antisite defects. In the absence of antisites, PF increases with carrier doping. This enhancement is attributed to both the decrease in and the increase in the absolute value of , as shown in Figure 2 and Figure 3. The PF of -type FeVAl is larger than that of -type FeVAl. This trend is opposite to experimental data.[11] This difference arises because the calculated is larger and smaller than the experimental values for -type and -type FeVAl, respectively.
Figure 3. (Color online) Electronic states and transport properties in p-type FeVAl. (a) Total DOS per spin. The energy zero is set at the top of the valence band. The inset shows the zero-temperature total spectral conductivity per spin. The vertical line denotes the position of the Fermi energy . (b) Temperature dependence of the resistivity . (c) Temperature dependence of Seebeck coefficient . The red lines represent calculated results. The black dashed and dotted lines correspond to experimental data for FeVTiAl with and in (b) and and in (c).[11] For comparison, the calculated results for FeVAl$[25] are shown by black dash-dotted lines in (b) and (c).
With antisites, the calculated PF of undoped FeVAl[25] decreases, in contrast to the experimentally observed large enhancement of PF in fully quenched FeVAl with large antisite concentration.[21] This discrepancy primarily arises from the small magnitude of the calculated , which reflects the low antisite concentration assumed in our model.[25] In addition, dynamical contributions from fluctuations of antisite magnetic moments may lead to a further enhancement of . In -type FeVAl, the introduction of antisite defects reduces the PF, which is consistent with experimental behavior.[20] In -type FeVAl, the PF exhibits nearly the same magnitude with and without antisites. This small change is attributed to the absence of spin-polarized antisites, which leads to weaker scattering of hole carriers near .
In summary, we have investigated the thermoelectric properties and spin polarization associated with antisite defects in doped FeVAl. We have demonstrated that, in doped FeVAl, both the rigid-band shift of the Fermi energy and the temperature-dependent scattering rate play crucial roles in understanding the temperature dependence of the Seebeck coefficient and the resistivity based on the Sommerfeld-Bethe relationship. In the presence of V and Fe antisite defects, the BPRAM with a shifted yields spin polarization at both types of antisites in -type FeVAl, giving rise to a magnetic moment that is approximately twice as large as that of antisites in undoped FeVAl, when the antisite concentration is the same. At the same time, the Seebeck coefficient is reduced in the presence of antisites. These results are consistent with existing experimental observations. In contrast, in -type FeVAl, spin polarization of antisites diminishes because the Fermi energy lies deep inside the valence band and the antisite levels are located above . These theoretical results demonstrate the impact of carrier substitution on the spin polarization of antisite defects in FeVAl and indicate the crucial role of antisites in realizing magneto-thermoelectric functionalities in Heusler-type alloys. Constructing a theoretical framework that takes into account the dynamical effects of antisite magnetic moments remains a challenge for future studies aiming to understand magneto-thermoelectric properties.
References
- [9]9) H. Kato, M. Kato, Y. Nishino, U. Mizutani, and S. Asano, J. Japan Inst. Metals 65, 652 (2001).
- [10]10) C. S. Lue, C. F. Chen, J. Y. Lin, Y. T. Yu, and Y. K. Kuo, Phys. Rev. B 75, 064204 (2007).
- [11]11) H. Matsuura, Y. Nishino, U. Mizutani, and S. Asano, J. Japan Inst. Metals, 66, 767 (2002).
- [12]12) A. Ślebarski, J. Goraus, J. Deniszczyk, and Ł. Skoczeń, J. Phys.: Condens. Matter 18, 10319 (2006).
- [14]14) R. Jha, N. Tsujii, F. Garmoudi, S. Khmelevskyi, E. Bauer, and T. Mori, J. Mater. Chem. C, 12, 8861 (2024).
- [15]15) F. Garmroudi, A. Riss, M. Parzer, N. Reumann, H. Müller, E. Bauer, S. Khmelevskyi, R. Podloucky, T. Mori, K. Tobita, Y. Katsura, and K. Kimura, Phys. Rev. B 103, 085202 (2021).
- [17]17) S. Jemima, A. Mani, A. Bharathi, N. Ravindran,and Y. Hariharan, J. Alloys Compd. 268, 183 (2001).
- [18]18) E. P. Amaldass, A. T. Satya, S. Sharma, K. Vinod, V. Srinivas, C. S. Sundar, and A. Bharathi, J. Alloys Compd. 648, 34 (2015).
- [19]19) N. Tsujii, A. Nishide, J. Hayakawa, and T. Mori, Sci. Adv. 5, eaat5935 (2019).
- [20]20) F. Garmroudi, M. Parzer, M. Knopf, A. Riss, H. Michor, A. V. Ruban, T. Mori, and E. Bauer, Phys. Rev. B 107, 014108 (2023).
- [21]21) F. Garmroudi, M. Parzer, A. Riss, A. V. Ruban, S. Khmelevskyi, M. Reticcioli, M. Knopf, H. Michor, A. Pustogow, T. Mori, and E. Bauer, Nat. Commun. 13, 3599 (2022).
- [23]23) F. X. Zhang, C. Feng, Z. Guan, H. Song, S. Nan, Y. Tang, H. Yang, K. Zeng, X. Yuan, M. Xiao, Z. Lu, Y. Zhang, D. Ma, and Y. Zhang, Acta Materi. 292, 121056 (2025).
- [24]24) P. W. Anderson, Phys. Rev. 124, 41 (1961).
- [25]25) T. Tohyama and H. Fukuyama, J. Phys. Soc. Jpn. 94, 094603 (2025).
- [28]28) M. Ogata and H. Fukuyama, J. Phys. Soc. Jpn. 88, 074703 (2019).
- [29]29) M. Matsubara, T. Yamamoto, and H. Fukuyama, J. Phys. Soc. Jpn. 94, 024601 (2025).