betaFeedback

WorksPhysics and Astronomy

NaRe2_2(PO4_4)3_3 phosphate-based ceramic with kosnarite structure as a matrix for technetium immobilization. Production. Properties

Abstract

NaRe2_2(PO4_4)3_3 phosphate-based ceramic with the structure of kosnarite mineral was obtained by spark plasma sintering. Rhenium (Re) served as a chemical and structural analog of technetium. The ceramic relative density was 85%. The mechanism of Re static leaching from NaRe2_2(PO4_4)3_3 ceramic at room temperature was investigated. The leaching rate of rhenium was 1.3×10−51.3\times10^{-5} g/(cm2^2*day).

Introduction

Technetium-99 (99Tc{}^{99}\mathrm{Tc}) is one of the most widespread and long-lived radiotoxic isotopes in spent nuclear fuel (SNF). It is one of the key elements in SNF separation strategies such as UREX + for isolation and encapsulation in solid waste forms [1]. Immobilizing 99Tc{}^{99}\mathrm{Tc} is a complex scientific and practical challenge. Thus far, immobilization of 99Tc{}^{99}\mathrm{Tc} as metal alloys [2, 3, 4], cements [5, 6, 7], and glasses [2, 8, 9] has been researched. During glass transition, which is the most widely used process for high-level radioactive waste (RAW), technetium is partly oxidized or disproportionated and therefore evaporates as heptaoxide, causing environmental pollution. An alternative approach to immobilizing 99Tc{}^{99}\mathrm{Tc} consists in introducing a cation into a mineral-like matrix [10, 11, 12, 13, 14, 15, 16], which has the potential to help avoid formation of highly mobile pertechnetate TcO4−\mathrm{TcO}_{4}^{-} ions during RAW processing. Tc-containing compounds with the structures of pyrochlore (Nd2Tc2O7\mathrm{Nd}_2\mathrm{Tc}_2\mathrm{O}_7), perovskite (SrTcO3\mathrm{SrTcO}_3) and lamellar perovskite (Sr2TcO4\mathrm{Sr}_2\mathrm{TcO}_4) have been studied in [13, 14]. 28 days of hydrolytic tests of Nd2Tc2O7\mathrm{Nd}_2\mathrm{Tc}_2\mathrm{O}_7 pyrochlore-based ceramic helped establish the Tc leaching rate to be 1.48⋅10−71.48 \cdot10^{-7} g/(mm2^2·day), which is approximately four times slower than the rate of leaching from borosilicate glass (∼6.43⋅10−7\sim6.43 \cdot10^{-7} g/(mm2^2·day)). A disadvantage of the compounds studied in [13, 14] is the long (2–10 days) duration of high-temperature annealing during solid-phase synthesis.

Including technetium in compounds in Mg2Ti1−xTcxO4\mathrm{Mg}_2\mathrm{Ti}_{1-x}\mathrm{Tc}_x\mathrm{O}_4 spinels has been studied in [11, 16]. Synthesis of such compounds is demanding and time consuming and their leaching rate was (3–7)⋅10−3(3\text{–}7) \cdot10^{-3} g/(m2^2·day) after testing for 40 days at room temperature.

In [15] describes compounds with NZP structure of ARe2(PO4)3\mathrm{ARe}_2(\mathrm{PO}_4)_3 (where A = AM [alkali metal]). These compounds were produced by fusing concentrated phosphoric acid, ammonium perrhenate, and AM chlorides, further annealed at 400 °C in air and at 550 °C under an inert atmosphere in a vacuum-sealed ampoule. There have been no studies of chemical stability of the synthesized compounds.

This paper researches NaRe2(PO4)3\mathrm{NaRe}_2(\mathrm{PO}_4)_3 phosphate with kosnarite structure as a potential ceramic matrix for immobilizing 99Tc{}^{99}\mathrm{Tc}. Rhenium (Re) served as a chemical and structural analog of technetium. Solution chemistry was used to obtain NaRe2(PO4)3\mathrm{NaRe}_2(\mathrm{PO}_4)_3 while the ceramic was produced through Spark Plasma Sintering (SPS) [17].

Materials and methods

A solution of 1M orthophosphoric acid was gradually added to a mixture of sodium chloride and ammonium perrhenate solutions taken in stoichiometric amounts with constant vigorous stirring in order to obtain NaRe2(PO4)3\mathrm{NaRe}_2(\mathrm{PO}_4)_3 powders with the NZP structure. Their synthesis occurred as per the following formula: NaCl+2NH4ReO4+3H3PO4=NaRe2(PO4)3+HCl+2NH4OH+4H2O\mathrm{NaCl} + 2\mathrm{NH}_4\mathrm{ReO}_4 + 3\mathrm{H}_3\mathrm{PO}_4 = \mathrm{NaRe}_2(\mathrm{PO}_4)_3 + \mathrm{HCl} + 2\mathrm{NH}_4\mathrm{OH} + 4\mathrm{H}_2\mathrm{O}. The resulting clear solution was evaporated at 80 °C with constant stirring, dried at 200 and 300 °C until moisture was completely removed and the intermediate reaction products partially decomposed. The load turned black after annealing. The resulting powder was annealed in a vacuum-sealed quartz ampoule at 600, 700, or 800 °C for 12 hours.

A Shimadzu LabX XRD-6000 X-ray diffractometer (CuKα\alpha filtered radiation) was used to determine the phase composition of the powders and ceramics. A DSC-204 F1 Phoenix thermal analyzer was used to perform a differential thermal analysis within 25-1200 °C range. The heating rate was 10 °C/min. A Shimadzu FTIR-8400S IR Fourier spectrophotometer was used to study the functional composition of the compounds at room temperature within a frequency range of 400–4000 cm−1\mathrm{cm}^{-1}.

A Dr. Sinter model SPS-625 was used to produce the ceramics. The powders were placed in a graphite mold with an inner diameter of 10 mm and heated by millisecond pulses of direct electric current of high power (up to 3 kA). A Chino IR-AH pyrometer focused on the graphite mold surface was used to measure the sintering temperature. Sintering was performed in vacuum (6 Pa). The accuracy of temperature measurements was ±10\pm10 °C, with a pressure maintenance accuracy of 1 MPa. The dilatometer in the Dr. Sinter model SPS-625 was used to monitor the shrinkage and shrinkage rate of the powders.

A Sartorius CPA balance was used to measure the density of the sintered samples by hydrostatic weighing in distilled water. Microstructural parameters of the samples were analyzed using a Jeol JSM-6490 scanning electron microscope (SEM) with an Oxford Instruments INCA 350 X-ray microanalyzer.

The chemical stability of the ceramics was studied by leaching in a static mode during 28 days. The tests were performed at room temperature in distilled water. The Re concentration in water samples was determined using an ELEMENT 2 high-resolution inductively coupled plasma mass spectrometer using external calibration. Calibration was performed using the ICP-MS-68A-A High-Purity Standards solutions and iDplus Performance time-of-flight mass spectrometer.

During the experiment, the normalized weight loss was calculated using the following formula:

NLi=akiM0i×S,(1)NL_i = \frac{a_{ki}}{M_{0i} \times S}, \tag*{(1)}

where NLiNL_i is the normalized weight loss of element ii, g/cm2\mathrm{g/cm^2}; akia_{ki} is the mass of component ii dissolved during leaching, g; M0iM_{0i} is the mass concentration of the element in the sample at the beginning of testing, g/g; SS is the sample surface area, cm2\mathrm{cm^2}.

The leaching rate RiR_i was calculated using the following formula:

Ri=NLitn,(2)R_i = \frac{NL_i}{t_n}, \tag*{(2)}

where tnt_n is the time interval, days.

The DeGroot – van der Sloot model [18] was used to determine the mechanism of cation leaching from the ceramic, which can be represented as the following equation:

lg⁡Bi=Alg⁡t+const,(3)\lg B_i = A\lg t + \mathrm{const}, \tag*{(3)}

where BiB_i is the total yield of Re from the sample during contact with water, mg/m2\mathrm{mg/m^2}; tt is the contact time, days. The BiB_i value was calculated using the following formula:

Bi=Ci(L/S)tn(tn−tn−1).(4)B_i = C_i(L/S)\frac{\sqrt{t_n}}{\left(\sqrt{t_n}-\sqrt{t_{n-1}}\right)}. \tag*{(4)}

where CiC_i is the concentration of Re in the solution by the end of the nthn^{th} period, mg/l; L/SL/S is the ratio of solution volume to sample surface area, l/m2^2; tnt_n and tn−1t_{n-1} is the time of the nn- and n−1n-1 experiment stages, respectively, in days.

The following leaching mechanisms correspond to the values of the coefficient A in equation (3): <0.35 – leaching from the surface of the compound; 0.35–0.65 – diffusion from inner layers; >0.65 – dissolution of the compound surface layer [19, 20].

Results and discussion

According to the XRD data (Figure 1), a monophase product is obtained after annealing at 700 °C. Once annealed at 600 and 800 °C, the powder contains insignificant traces of Re2P2O7\mathrm{Re_2P_2O_7} rhenium pyrophosphate and ReO2\mathrm{ReO_2} rhenium (IV) oxide, respectively. The resulting monophasic compounds crystallized in the expected NZP structure and belonged to the R-3c space group.

Image not extracted

Figure 1.

Further studies were performed with the powder synthesized at 700 °C.

The particle size distribution of the powder was heterogeneous. The electron microscopy data suggested that the synthesized powder contained two types of particles: large faceted particles approx. 10 μ\mum in size, which are likely to be single crystals, and agglomerates consisting of particles up to 1 μ\mum in size (Figure 2a, Figure 2b). Energy dispersive microanalysis confirmed the presence of Re in the structure of the synthesized powder (Figure 2c).

Differential scanning calorimetry (DSC) (Figure 3) revealed an endothermic effect in the temperature range of 970-1030 °C, which corresponded to the decomposition of NaRe2(PO4)3\mathrm{NaRe_2(PO_4)_3} and was confirmed by the thermal gravimetric analysis (TGA).

Image not extracted

Figure 3.

A wide band in the range of 980-1120 cm−1^{-1} and a high-frequency band at 1247 cm−1^{-1} of the IR spectrum under study (Figure 4) can be attributed to asymmetric stretching ν3\nu_3 vibrations of the PO43−\mathrm{PO_4^{3-}} ion. We believe that a low-intensity high-frequency band in the range of 1247 cm−1^{-1}, which is not typical for phosphates, may be associated with the influence of the Re4+\mathrm{Re^{4+}} highly charged ion that polarizes the P–O–Re bond. The band in the range of 883 cm−1^{-1} corresponded to symmetric stretching ν1\nu_1 vibrations. The bands in the 640-438 cm−1^{-1} range belong to bending vibrations: the bands within 650-540 cm−1^{-1} corresponded to asymmetric ν4\nu_4 vibrations while the 445 cm−1^{-1} band corresponded to symmetric ν2\nu_2 vibrations.

Image not extracted

Figure 4.

SPS of NaRe2(PO4)3\mathrm{NaRe_2(PO_4)_3} powder was performed under constant heating rate. There was no isothermal holding at the sintering temperature. Table 1 contains the main sintering parameters of the ceramic samples – heating rate VhV_{\mathrm{h}}, average applied uniaxial pressure PP, sintering temperature TsT_{\mathrm{s}} and isothermal time tst_{\mathrm{s}} at sintering temperature.

SequenceTsT_{\mathrm{s}}, °CVhV_{\mathrm{h}}, °C/mintst_{\mathrm{s}}, minPP, MPaρ\rho, g/cm³ρrel\rho_{\mathrm{rel}}, %NLReNL_{\mathrm{Re}}, g/cm²RReR_{\mathrm{Re}}, g/(cm²·day)
1110050070----
2800500704.15484.94.4⋅10−44.4 \cdot10^{-4}1.3⋅10−51.3 \cdot10^{-5}
38001000704.17485.3--
48002000704.16885.2--

Table 1. Main parameters of sintering NaRe₂(PO₄)₃ powders, density and hydrolytic stability of the resulting samples

Preliminary sintering of NaRe₂(PO₄)₃ powders was performed by heating them to 1100 °C at a rate of 50 °C/min (Seq. # 1) to define the optimal SPS modes. Figure 5a shows the sintering modes as dependences between temperature (TT, °C), applied uniaxial pressure (PP, kN), vacuum levels (Vac, Pa), and SPS time. Figure 5b shows the dependence between shrinkage (LL, mm), shrinkage rate (SS, mm/s), and the heating temperature. Figure 5b demonstrates that the powder shrinkage starts at TT = 600 °C; with the shrinkage rate being small and not exceeding Smax⁡∼4.5⋅10−3S_{\max} \sim4.5 \cdot10^{-3} mm/s (Figure 5b). A shrinkage peak was observed at 1000 °C, which is likely to be associated with a phase transition in NaRe₂(PO₄)₃ powder. It should also be noted that at temperatures above 850 °C powder decomposition was observed, which manifested itself in a decrease in the vacuum level in the sintering chamber of the Dr. Sinter model SPS-625 (Figure 5a). Sample decomposition during SPS upon heating to 1100 °C prevented its density from being reliably determined through the Archimedes' principle.

Image not extracted

Figure 5.

As a way to minimize or exclude decomposition of the powder sample, further sintering of the ceramics was performed at TsT_{\mathrm{s}} = 800 °C with different heating rates (Seq. # 2-4). It is of interest to note that the maximum shrinkage rates Smax⁡S_{\max} increased slightly from ∼0.2⋅10−3\sim0.2 \cdot10^{-3} to ∼1.5⋅10−3\sim1.5 \cdot10^{-3} mm/s with an increase in the heating rate from 50 to 200 °C/min. The sintered samples were a powder compressed to a density ρrel≈85%\rho_{\mathrm{rel}} \approx85\% with a particle size similar to the size of the initial powder particles dd = 1-10 μm (Figure 6). After sintering, many particles retained their faceted shape, indicating a low intensity of diffusion during SPS. The postsintering density was insufficient to produce durable ceramics. The phase composition of the ceramic did not change after sintering (Figure 7).

Image not extracted

(a)

Image not extracted

(b)

Image not extracted

(c)

Image not extracted

(d)

Image not extracted

(e)

Image not extracted

(f)

Figure 6.

Image not extracted

Figure 7.

Table 1 shows the minimal rates of Re leaching from NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} samples. Figure 8 shows graphs of dependence between the normalized weight loss NLiNL_i, leaching rate RiR_i, and testing time tt. The resulting data suggest that the rhenium leaching rate on day 28 was R=1.3⋅10−5 g/(cm2⋅day)R = 1.3 \cdot10^{-5}\ \mathrm{g}/(\mathrm{cm}^{2}\cdot\mathrm{day}). The calculated leaching rate is slightly lower, yet comparable to the rate of technetium leaching from other mineral-like compounds [11, 13, 14, 16]. It should be noted that the real surface area SS of the ceramics under study is greater than the value calculated based on geometric dimensions because of their increased porosity (Figure 6). We therefore believe that these results characterize the terminal value RR for this compound.

Image not extracted

Figure 8.

Using formula (3) to determine the mechanism of rhenium leaching from NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} ceramic, the dependence between coefficient BB and the experiment time tt was plotted in logarithmic coordinates (Figure 9). The data in Figure 9 show that the value of coefficient AA is −0.38−0.3-0.38-0.3. It allows us to conclude that rhenium leaching occurs through washing out of the open surface of NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} ceramic. This result is qualitatively in good agreement with the previous conclusion that open porosity has a significant effect on the high rate of Re leaching from NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} ceramic.

Image not extracted

Figure 9.

Conclusions

NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} monophasic phosphate with the structure of the kosnarite mineral was obtained by synthesis at 700 ∘C700\ ^\circ\mathrm{C}. An increased or decreased synthesis temperature does not allow a monophasic product to be obtained. The synthesized NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} compound manifests a non-uniform particle size distribution, with large single-crystal particles of ∼10 μm\sim10\ \mu\mathrm{m} and agglomerated μm\mu\mathrm{m} particles present in the powder.

In terms of achieving the maximum possible density of the ceramic (ρrel=85.3%\rho_{\mathrm{rel}}=85.3\%) while maintaining the phase composition, the optimal SPS mode consists in heating the sample to Ts=800 ∘CT_{\mathrm{s}}=800\ ^\circ\mathrm{C} at a rate of Vh=100 ∘C/minV_{\mathrm{h}}=100\ ^\circ\mathrm{C}/\mathrm{min} under uniaxial pressure of P=70 MPaP=70\ \mathrm{MPa}.

The terminal rate of rhenium leaching from NaRe2(PO4)3\mathrm{NaRe}_{2}(\mathrm{PO}_{4})_{3} ceramic on Day 28 was 1.3⋅10−5 g/(cm2⋅day)1.3\cdot10^{-5}\ \mathrm{g}/(\mathrm{cm}^{2}\cdot\mathrm{day}), which makes it possible to class the phosphate under study as highly hydrolytically stable. It was established that the dominant mechanism of rhenium leaching in the static mode at room temperature is the leaching of cations from the surface of the ceramic.

Acknowledgements

This work has been performed with the support of Research and Educational Center of Nizhny Novgorod region in the framework of the agreement No 16-11-2021/49 (contract reference number 000000S407521QRR0002) and under contract No. 217/4571-D "Validation of radiation resistance of matrices. Validation of radiation resistance of phosphate ceramic matrices. Technology testing support" between the Lobachevsky State University of Nizhny Novgorod (UNN) and V.G. Khlopin Radium Institute.

Список литературы

Image not extracted

(a)

Image not extracted

(b)

Image not extracted

(c)

Figure 2.

References

  1. [1]Paviet–Hartmann, P., Lineberry, M., & Benedict, R. (2009). Nuclear Fuel Reprocessing in Nuclear Engineering. In Nuclear Engineering (pp. 315–366). https://doi.org/10.1201/9781420053913
  2. [2]Laverov N.P., Yudintsev S.V., Omel’yanenko B.I. Isolation of long-lived technetium-99 in confinement matrices // Geology of Ore Deposits, 2009, v.51, iss. 4. p. 259–274. doi:10.1134/S1075701509040011DOI
  3. [3]Keiser D.D., Abraham D.P., Richardson J.W. Influence of technetium on the microstructure of a stainless steel–zirconium alloy // J. Nucl. Mater. 2000, v.277, iss.2–3, p.333–338. doi:10.1016/S0022-3115(99)00158-0DOI
  4. [4]Hartmann, T. (2008). Synthesis and Properties of Metallic Technetium and Technetium–Zirconium Alloys as Transmutation Target and Radioactive waste storage form in the UREX+1 Process. Proc. «Atalante – 2008», 3–13.
  5. [5]Popova N.N., Tananaev I.G., Rovnyi S.I., Myasoedov B.F. Technetium: behaviour during reprocessing of spent nuclear fuel and in environmental objects // Russian Chemical Reviews, 2003, v.72, iss. 2, p. 101-121. doi:10.1070/RC2003v072n02ABEH000785DOI
  6. [6]Mattigod S.V., Whyatt G.A., Serne J.R., Wood M.I. Diffusion of iodine and technetium-99 through waste encasement concrete and unsaturated soil fill material // Proc. of Sympos. “Sci. Bas. Nucl. Waste Management XXVIII”. Warrendale: MRS, 2004, v.824, p.391–398.DOI
  7. [7]Aloy, A., Kovarskaya, E. N., Harbour, J. R., & al., . et . (2007). Pretreatment of Tc-containing waste and its effect on Tc-99 leaching from grouts. Proc. Of Sympos. “Sci. Bas. Nucl. Waste Management XXX”, 985, CD-version. Paper NN 10-02.
  8. [8]Ebert W.L., Wolf S.F., Bates J.K. The release of technetium from defense waste processing facility glasses // Proc. of sympos. “Sci. Bas. Nucl. Waste Management XIX”. Pittsburgh: MRS, 1996, v.412, p.221–227.DOI
  9. [9]McKeown D.A., Buechele A.C., Lukens W.W. et al. Raman studies of technetium in borosilicate waste glass. // Radiochim. Acta. 2007, v.95, p.275–280. doi:10.1524/ract.2007.95.5.275DOI
  10. [10]Carter M.L., Stewart M.W.A., Vance E.R. et al. HIPed tailored ceramic waste forms for immobilization of Cs, Sr, and Tc // Proc. of sympos. “Global 2007”. Idaho. 2007, p. 1022–1028.
  11. [11]Khalil M.Y., White W.B. Magnesium titanate spinel: a ceramic phase for immobilization of technetium-99 from radioactive waste // Comm. Amer. Ceram. Soc. 1983, v.66, iss.10, p.197–198. doi:10.1111/j.1151-2916.1983.tb10554.xDOI
  12. [12]Yudintsev, S. V., Konovalov, E. E., Kuprin, A. V., Galgovskii, E. M., Nikonov, B. S., & Omel’yanenko, B. I. (2010). Immobilization of technetium and rare earth-actinide fraction in crystalline matrices using self-sustaining high-temperature synthesis. Geology. Engineering Geology, Hydrogeology, Geocryology, (3), 232–242.
  13. [13]Hartmann T., Alaniz–Ortez I.J. Fabrication and Chemical Durability of Ceramic Technetium–based Pyrochlores and Perovskites as Potential Waste Forms // Advances in Science and Technology. 2014, v. 94, p.85–92. doi:10.4028/www.scientific.net/AST.94.85DOI
  14. [14]Hartmann T., Alaniz A.J., Antonio D.J. Fabrication and Properties of Technetium-bearing Pyrochlores and Perovskites as Potential Waste Forms // Procedia Chemistry, 2012, V.7. P.622–628. doi:10.1016/j.proche.2012.10.095DOI
  15. [15]Sukhanov M.V., Pet'kov V.I. Technetium and rhenium orthophosphates with kosnarite–type structure // Proc. 7th International Symposium on Technetium and Rhenium – Science and Utilization / Moscow, Russia, 2011, Publishing House GRANISTA, p.75–78.
  16. [16]Exter, M. J., Neumann, S., & Tomasberger, T. (2006). Immobilization and behavior of technetium in a magnesium titanate matrix for final disposal. Proc. Of Sympos. “Sci. Bas. Nucl. Waste Management XXIX”, 932, 567–574.
  17. [17]Tokita M. Progress of Spark Plasma Sintering (SPS) method, systems, ceramics applications and industrialization // Ceramics, 2021, v.4, iss.2, p.160-198. doi:10.3390/ceramics4020014DOI
  18. [18]De Groot G.J., Van der Sloot H.A. Determination of leaching characteristics of waste minerals leading to environmental product certification, in: T.M. Gilliam, C.C. Wiles (Eds.), Stabilization and Solidification of Hazardous, Radioactive and Mixed Wastes, V. 2, ASTM, Philadelphia, 1992, pp. 149–170.DOI
  19. [19]Torras J., Buj I., Rovira M., de Pablo J. Semi-dynamic leaching tests of nickel containing wastes stabilized/solidified with magnesium potassium phosphate cements // J. Hazard. Mater. 2011, v.186, p.1954–1960. doi:10.1016/j.jhazmat.2010.12.093.DOI
  20. [20]Xue, Q., Wang, P., Li, J.-S., & al., . et . (2017). Investigation of the leaching behavior of lead in stabilized/solidified waste using a two-year semi-dynamic leaching test. Chemosphere, 166, 1–7. https://doi.org/10.1016/j.chemosphere.2016.09.059

Paper details

vlnc:W_6n7xfa8b
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 6

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents