betaFeedback

WorksPhysics and Astronomy

Site-dependent Local Spin Susceptibility and Low-energy Excitation in a Weyl Semimetal WTe2_2

Abstract

Site-dependent local spin susceptibility is investigated with 125^{125}Te nuclear magnetic resonance in a Weyl semimetal WTe2_2. The nuclear spin-lattice relaxation rate 1/T1T1/T_1T shows a dependence of the square of temperature TT at high temperatures, followed by a constant behavior below 50 K. The temperature dependence features Weyl fermions appearing around the linearly crossing bands. The Knight shift KK scales to the square root of 1/T1T1/T_1T, corroborating a predominant spin contribution in low-lying excitation. The observed dependence of KK and 1/T1T1/T_1T on the four Te sites shows the site-dependent electron correlation and density of states. The angular profile of the NMR spectrum gives the anisotropic hyperfine coupling tensor, consistent with 5p5p hole occupations on Te sites.

Introduction

Weyl semimetals with broken inversion symmetry display a singular electromagnetic response such as chiral anomaly and nonlinear Hall effect,1–5) originating from the Berry curvature in the linearly crossing energy bands. The topological phenomena suggest the presence of magnetic monopoles around the Weyl points,6, 7) which appear on the surface of the semimetals. In contrast to the surface electronic state, the low-lying excitation of the underlying bulk state is less understood owing to the lack of comprehensive magnetic measurement. Nuclear magnetic resonance (NMR) spectroscopy can be a local probe of emergent gauge fields from magnetic monopoles in Weyl semimetals.8, 9) It also extracts the local spin/orbital susceptibility and excitation of Weyl fermions in a site-selective manner, as extensively studied in a molecular material α\alpha-(ET\mathrm{ET})2I3_2\mathrm{I}_3 10) and 5d transition metal compounds such as TaAs and ZrTe5_5.11–15) The low-lying excitation measured with the nuclear spin-lattice relaxation rate 1/T11/T_1 sensitively depends on the energy dispersion curvature and the location of the Fermi level around the Weyl points.8, 9, 16)

One of the most studied materials is the quasi-two-dimensional transition-metal dichalcogenide WTe2\mathrm{WTe}_2, which exhibits versatile topological phenomena such as the quantum spin-Hall effect,17–20) chiral anomaly,21) and nonlinear Hall effect.5) The material also displays extremely large magnetoresistance,22) ferroelectricity,23) and superconductivity.24, 25) TdT_d-WTe2\mathrm{WTe}_2 is classified into a type-II Weyl semimetal with tilted Weyl cones owing to lattice distortion.3) The charge compensation of electron and hole Fermi pockets under magnetic field,26, 27) causes the nonsaturating magnetoresistance in a clean sample,22, 27) where spin-orbit coupling28) and Lifshitz transition29, 30) also play a crucial role in the charge compensation.

The crystal structure of WTe2\mathrm{WTe}_2 (orthorhombic space group Pmn21Pmn2_1) is composed of the W2Te4\mathrm{W}_2\mathrm{Te}_4 layers stacked along the cc axis, as shown in Figure 1.31) There are crystallographically inequivalent two tungsten (W1, W2) and four tellurium sites (Te1, Te2, Te3, Te4), and two each are included in the unit cell. Each Te site has the same site symmetry and three coordinations to W atoms. Owing to the large distortion along the aa axis, there is direct W–W bonding along the aa axis, and the W–Te bond length of the Te2/Te3 sites (∼2.7\sim2.7 Å) is shorter than that of the Te1/Te4 sites (∼2.8\sim2.8 Å). The difference is expected to give a different partial density of states and orbital occupation, which are observed as the local spin susceptibility and the anisotropic hyperfine coupling, respectively. In the band structure, the Weyl points are located near the Γ\Gamma point of the Brillouin zone.32) Both W 5d and Te 5p bands significantly contributes to the Fermi level. Therefore, 125Te{}^{125}\mathrm{Te} NMR spectroscopy can be used as a local probe of the electronic state of the Weyl semimetal.

Crystal structures of $T_d$-$\mathrm{WTe}_2$

Figure 1. (Color online) Crystal structure of TdT_d-WTe2\mathrm{WTe}_2 composed of two tungsten (W1, W2) and four tellurium (Te1, Te2, Te3, Te4) sites in the nonsymmetric Pmn21Pmn2_1 lattice. The W2_2Te4_4 layer in the abab plane (a) is stacked along the cc axis. Two equivalent atomic sites in the unit cell are related by the glide symmetry in the bcbc plane (b) but become inequivalent as the magnetic field is tilted from the mirror plane along the abab and caca planes.

In this paper, we conduct site-selective 125Te{}^{125}\mathrm{Te} NMR measurements in WTe2\mathrm{WTe}_2 single crystals. The local susceptibility observed by the Knight shift gives the site-dependent density of states contributing to the Weyl points. The result compen-

sates the kk-space surface information probed by optical[33, 34, 35] and photoemission spectroscopy.[6, 7, 20, 29, 36] On the basis of crystal structure data, the NMR spectra are assigned to four Te sites with the distinct local spin susceptibility. We evaluate the site-dependent Te 5p5p orbital electron/hole occupation from the Knight shift tensor.

Experimental Method

Single crystals of WTe2_2 were prepared by two methods: chemical vapor transport and Te-flux methods. The latter is expected to give higher quality stoichiometric crystals.[30, 37] In the chemical transport method, we start from powdered tungsten and tellurium kept at 700°C in a vacuum quartz tube for two days and then at 750°C for another two days after grinding.[22] Crystals were grown in a three-zone furnace with a transport agent Br2_2 and a temperature gradient of 750–650°C for one week. In the self-flux method, WTe2_2 and tellurium powder were also heated to 700°C for 2 days and 750°C for another 2 days. After maintaining at 900°C for 10 h, the temperature decreased to 460°C for 100 h. The Te flux was separated by centrifugation and then evaporated in a three-zone furnace with a temperature gradient of 465-280-250°C for two days.

The crystals (named #S1 and #S2) obtained by the transport and flux methods have dimensions of 5 mm × 0.3 mm × 0.05 mm and 5 mm × 1 mm × 0.2 mm, respectively. For NMR measurements of #S1, several thin plate crystals were aligned and stacked. Magnetic susceptibility was measured with a magnetometer (MPMS-XS, Quantum Design Ltd.) at 7 T along the crystal axes. We obtained 125^{125}Te NMR spectra by Fourier transformation of spin-echo signals after the rf pulses tπ/2−τ−tπ−τt_{\pi/2}-\tau-t_{\pi}-\tau (duration tπ/2=1 μst_{\pi/2}=1\ \mu\mathrm{s} and the interval time τ=20−30 μs\tau=20-30\ \mu\mathrm{s}) under constant magnetic fields H=7.389H=7.389 and 9.0891 T. 125^{125}Te Knight shift KK was defined by the relative frequency shift K=(ν−ν0)/ν0K=(\nu-\nu_0)/\nu_0 using the bare resonance frequency ν0=γnH\nu_0=\gamma_nH for the nuclear gyromagnetic ratio γn=13.454\gamma_n=13.454 T/MHz.[38]

Experimental Results

The angular dependence of 125^{125}Te NMR spectra at 200 K for a single crystal of the sample #S2 is shown in Figure 2 for a sample rotated along the orthogonal crystal axes. Four resonance lines observed at bb and cc axes consist of two doublets exhibiting distinct anisotropy for the abab- and caca-plane rotations. One doublet shows a large negative shift with a minimum at the aa axis. Another shows a weak dependence on the field direction with a maximum at the aa axis. As the magnetic field is rotated in the bcbc planes, each spectrum splits into two because two Te sites related by glide symmetry in the unit cell become inequivalent against the magnetic field [See Figure 2(c)]. We refer to the crystal structure for the spectrum assignment. Namely, four Te sites are classified into two groups in terms of the W–Te bond length (Te1/Te4 and Te2/Te3) and possess the identical site symmetry (1a) and the same coordination number (three) to W ions. The stronger hybridization to W bands is expected for Te2/Te3 with shorter W–Te bonds than those for Te1/Te4, resulting in a larger spin density proportional to the amplitude of the Knight shift anisotropy. Thus, we assigned the NMR spectrum into four Te sites, as shown in the symbols of Figure 2(d).

Image not extracted

Figure 2. (Color online) 125^{125}Te NMR spectrum and Knight shift KK for a single crystal of WTe2_2 (#S2) at 200 K. The spectrum was measured with 9°-step rotation of the crystal along (a,d) cc, (b,e) bb, and (c,f) aa axes using a two-axis rotator. The absence of data around the aa axis is due to the alignment of the magnetic field parallel to the rf field. The curves are fitting results using Eq. (1).

The angular dependence of the 125^{125}Te Knight shift KK obtained from a relative frequency shift of each NMR spectrum is shown in Figure 2(d)–Figure 2(f). The anisotropy is governed by the dipolar hyperfine interaction with the Te 5p5p spins, while the isotropic part comes from the Fermi contact interaction and the diamagnetic constant terms. The site dependence of KK reflects the local spin susceptibility and the 5p5p orbital occupation at the Te sites with the different densities of states. The angular dependence of KK is analyzed with a sinusoidal function[39]

K=k1cos⁡2θ+k2sin⁡2θ+k3(1)K = k_1\cos2\theta+ k_2\sin2\theta+ k_3 \tag*{(1)}

for each rotation along the crystal axis with the fitting parameters (k1k_1, k2k_2, k3k_3), as shown in Figure 2(d)–Figure 2(f). For the bcbc-plane rotation, for example, fitting gives the components of the Knight shift tensor K\mathbf{K} using the relations, k1=(Kbb+Kcc)/2k_1=(K_{bb}+K_{cc})/2, k2=(Kbb−Kcc)/2k_2=(K_{bb}-K_{cc})/2, and k3=Kbc=Kcbk_3=K_{bc}=K_{cb}.

From the mirror reflection symmetry along the abab and caca planes, the aa axis must be one of the principal axes of K\mathbf{K}, where the off-diagonal components KabK_{ab} and KacK_{ac} vanish. Thus, we can express K\mathbf{K} as

K=(Kaa000KbbKbc0KcbKcc).(2)\mathbf{K} = \begin{pmatrix} K_{aa} & 0 & 0 \\ 0 & K_{bb} & K_{bc} \\ 0 & K_{cb} & K_{cc} \end{pmatrix}. \tag*{(2)}
KaaK_{aa}KbcK_{bc}KbbK_{bb}KccK_{cc}KXXK_{XX}KYYK_{YY}KZZK_{ZZ}
Te1-0.0180.036-0.047-0.042-0.008-0.018-0.081
Te4-0.0180.036-0.064-0.068-0.030-0.018-0.103
Te2-0.2580.0390.0420.0040.0420.004-0.258
Te3-0.2510.0450.0550.0220.086-0.009-0.251

Table 1. Components of 125^{125}Te Knight shift tensors KK (%) for four Te sites in Eq. (1), obtained from the angular dependence measurement at 200 K in Figure 2. The principal axes (X, Y, Z) for the diagonalized Knight shift tensor correspond to the directions where KK shows a maximum (X) and a minimum (Z).

After the diagonalization of the tensor, we obtained the principal components of the Knight tensor (KXXK_{XX}, KYYK_{YY}, KZZK_{ZZ}) for four Te sites, as listed in Table I. The anisotropy reflects the Te 5p5p orbital occupation dominating the local spin/orbital susceptibility, as discussed below.

Figure 3 shows the temperature dependence of KK along the bb and cc axes. Upon cooling, KK linearly decreases to 50–100 K and becomes nearly constant at low temperatures, scaling to the bulk magnetic susceptibility χ\chi above 100 K. The behavior is characteristic of Dirac/Weyl semimetals having a linear band dispersion.[11, 12, 14] The crossover temperature from the linear to constant behavior reflects the energy scale of chemical potential crossing the Weyl corn. At low temperatures, the system becomes a weakly correlated metal with a finite density of states. The temperature dependence of KK or the spin susceptibility χs\chi_s has been calculated theoretically for three-dimensional (3D) Weyl semimetals.8) For the density of states linear to energy, ρ(E)∝E\rho(E) \propto E, in Dirac/Weyl semimetals, χs\chi_s decreases linearly with kBTk_{\mathrm{B}}T, which is distinct from the TT-invariant behavior in normal metals. KK also includes the component of the orbital susceptibility χorb\chi_{\mathrm{orb}}, which is sensitive to the chemical potential. In comparison with the calculation, the downward Knight shift suggests a negative chemical potential for the Te-dominant band,8) consistent with the hole-like carrier expected from the band calculation in WTe2_2.32)

Image not extracted

Figure 3. (Color online) Temperature dependence of 125^{125}Te Knight shift KK for four Te sites under the magnetic field along the bb axis (a) and the cc axis (b) in the single crystal of WTe2_2 (#S2) at 9.083 T. The bulk magnetic susceptibility (a solid curve) in the right-hand axis in (a) was measured at 7.0 T, where the core diamagnetic susceptibility was subtracted.

As for the site dependence, one of the Te sites in the doublet pair (Te2 and Te4) displays a stronger thermal variation. of K. As a result, the doublet splitting increases upon cooling and reaches ∼0.03%\sim0.03\% for H∥bH\parallel b and cc. Here the Te2/Te4 sites are bonded to two W1 among three W–Te bondings, while Te1/Te3 are connected to two W2. The coordination difference can lead to the site-dependent curvature of the Te bands, leading to a thermal change in local spin susceptibility. The result should be confirmed by the band structure calculation taking into account the atomic sites. We obtained the net hyperfine coupling constants HhfH_{\mathrm{hf}} (=22=22–2626 T/μB\mu_{\mathrm{B}}) for Te sites as the linearity coefficient of the KK–χ\chi plot, which are comparable to that of ZrTe5_5 (∼15\sim15 T/μB\mu_{\mathrm{B}}) 40) and highlight the predominant onsite hyperfine interaction.

The temperature dependence of the nuclear spin-lattice relaxation rate divided by TT, 1/T1T1/T_1T, is measured under magnetic field along the bb and cc axes, as shown in Figure 4. Here, the T1T_1 values for two Te sites within the doublet (Te1 or Te4, Te2 or Te3) are not distinguishable because they are almost the same. Interestingly, the sample dependence was observed for the Te2/Te3 site, which is considered to be sensitive to chemical potential. For sample #S2, 1/T1T1/T_1T for Te2/Te3 is about three times larger than that for Te1/Te4, indicating a higher spin density for Te2/Te3, consistent with the result of KK. We find that 1/T1T1/T_1T is strongly suppressed with decreasing temperature, approximately following a parabolic function ∼C1T2+C2\sim C_1T^2+C_2. The constant term indicates the residual density of state, characteristic of the type-II Weyl semimetal. This is consistent with the observation of the small Fermi surface by photoemission spectroscopy.29, 41) Similar 1/T1T1/T_1T behavior has been commonly observed in type-I Weyl11, 14) and 3D Dirac semimetals15, 42) with the residual density of states.

Temperature dependence of ¹²⁵Te nuclear spin-lattice relaxation rate

Figure 4. (Color online) (a) Temperature dependence of ¹²⁵Te nuclear spin-lattice relaxation rate divided by temperature, 1/T1T1/T_1T, for the single crystals (#S1 and #S2) of WTe₂ under magnetic field along the bb axis. The solid curve is the model fitting for Weyl fermions. (b) 1/T1T1/T_1T for #S2 measured along the cc axis.

The theoretical formula of 1/T1T1/T_1T for 3D Dirac fermions is expressed as

1T1T=2π3μ02γn2e2c∗4×∫−∞∞dE[−∂f(E,μ)∂E]ρ2(E)E2ln⁡2(E2−Δ2)ω0∣E∣,(3)\frac{1}{T_1T}=\frac{2\pi}{3}\mu_0^2\gamma_n^2 e^2 c^{*4}\times\int_{-\infty}^{\infty}dE\left[-\frac{\partial f(E,\mu)}{\partial E}\right]\frac{\rho^2(E)}{E^2}\ln\frac{2(E^2-\Delta^2)}{\omega_0\lvert E\rvert}, \tag*{(3)}

where ρ(E)\rho(E) is the density of states, f(E,μ)f(E,\mu) the Fermi distribution function, c∗=(Δ/m∗)1/2c^*=(\Delta/m^*)^{1/2} the velocity with the effective mass m∗m^*, ω0\omega_0 the NMR frequency, and Δ\Delta half the band gap.16, 43) 1/T1T1/T_1T scales to ∼T2\sim T^2 for μ,Δ≪T\mu,\Delta\ll T and then approaches a constant value for a temperature range T≪μT\ll\mu, following Korringa’s law in normal metals. Although the theoretical calculation does not assume the strong tilting of the Weyl corns, our experimental result well fits to the theoretical calculation of 1/T1T1/T_1T, as shown in Figure 4(a). The agreement suggests that the low-lying excitation is governed by the band curvature around the Weyl points and the density of states, which is commonly linear in energy for both the type-I and type-II Weyl semimetals. Under high magnetic fields, the continuous band can be squeezed into the Landau levels. However, we did not observe indication of the quantization and suppression of the spin density by charge compensation in the field range of 5–9 T.

In weakly correlated metals, (1/T1T)(1/T_1T) is proportional to the square of the density of states, ρ(E)2\rho(E)^2, at the Fermi level, while KK directly scales to ρ(E)\rho(E) depending on temperature. Following the extended Korringa’s relation, KK linearly scales to (1/T1T)1/2(1/T_1T)^{1/2}.14) Indeed, we find a good linear relationship between KK and (1/T1T)1/2(1/T_1T)^{1/2} for an extensive temperature range from 300 to 10 K, as shown in Figure 5. Here, the yy-offset extracts the TT-independent term governed by the diamagnetic chemical shift due to inner electrons and the paramagnetic Van-Vleck shift.

¹²⁵Te Knight shift plotted against $(1/T_1T)^{1/2}$

Figure 5. (Color online) ¹²⁵Te Knight shift KK plotted against (1/T1T)1/2(1/T_1T)^{1/2} as an implicit function of temperature in WTe₂ (#S2).

The linearity yields the ratio between 1/T1T1/T_1T and K2K^2, which is called the Korringa ratio defined by K(α)=(T1TK2)−1/S0\mathcal{K}(\alpha)=(T_1T K^2)^{-1}/S_0, where S0=ℏ(γe/γn)2/(4πkB)S_0=\hbar(\gamma_{\mathrm{e}}/\gamma_{\mathrm{n}})^2/(4\pi k_{\mathrm{B}}) = 2.64×10−62.64\times10^{-6} s is the Korringa constant for free electrons with the gyromagnetic ratio γe\gamma_{\mathrm{e}}. From the linearity in Figure 5, we obtained K(α)\mathcal{K}(\alpha) as 2.6–5.5 depending on the Te site. The enhancement factor can be a measure of the site-dependent electron correlation of Weyl fermions44) and orbital fluctuations.8, 9) In the present experiment, we neglect the anisotropy of the hyperfine coupling because of the lack of the aa-component of KK, which may cause the overestimation of K(α)\mathcal{K}(\alpha).

Discussion

We discuss the Te 5p5p orbital occupation in terms of the anisotropic hyperfine coupling obtained from the Knight shift measurement. The band structure of WTe2_2 has been intensively studied on the basis of the density functional theory and the local density approximation.22, 32, 41) There are two Weyl points and Fermi pockets consisting of the electron and hole-like bands. Not only tungsten 5d5d bands but also tellurium 5p5p bands have a significant weight on the Weyl points carrying the low-lying excitation.32) However, the energy bands are not labeled with crystallographically inequivalent atomic sites.

The anisotropic part of the Knight shift comes from the magnetic dipolar hyperfine interaction with 5p5p spins. The different anisotropy of the hyperfine coupling tensor suggests the site-dependent 5p5p orbital occupation (pxp_x, pyp_y, pzp_z) at the Fermi level. The dipolar hyperfine coupling tensors of pxp_x, pyp_y, and pzp_z orbitals have the diagonal components proportional to (2,−1,−1)(2,-1,-1), (−1,2,−1)(-1,2,-1), and (−1,−1,2)(-1,-1,2), respectively.

The observed KK in Figure 2 shows a prominent minimum for Te2/Te3 around the a(x)a(x) axis. The large negative KZZK_{ZZ} indicates the doubly degenerate pyp_y and pzp_z electron or the pxp_x hole occupation near the Fermi level. In contrast, KK for Te1/Te4 has a minimum in the bcbc plane parallel to the Te1–Te4 bond direction, suggesting a predominant pyp_y or pzp_z hole occupation. The amplitude of the Knight shift is suppressed because of the lower density of states. The orbital selective property of the band structure has recently been investigated via photoexcitation,35) and the contribution of Te 5p5p orbitals to the hole-like bands crossing the Fermi level has been shown, consistent with the result of Knight shifts. Our experimental result of site-selective NMR spectroscopy suggests that all the Te sites contribute to the low-energy property in the orbital-dependent manner.

Conclusion

Local spin and orbital susceptibility was investigated via ¹²⁵Te NMR measurements on single crystals of the Weyl semimetal WTe₂. We obtained the local spin susceptibility of the four Te sites that are classified into two groups with different anisotropies depending on the W–Te bond length. The temperature dependence of the nuclear spin-lattice relaxation agrees with the theoretical calculation in Weyl semimetals. We confirmed Korringa’s law in an extensive temperature range, consistent with the weakly correlated metal. The enhancement factor of the Korringa constant suggests orbital fluctuations of Weyl fermions. The predominant hole occupation in pp orbitals was evaluated from the anisotropy of the Knight shift. These results complement the results of optical and photoemission spectroscopy.

Note: Similar 1/T11/T_1 data of WTe₂ for powder samples were found in the literature during the preparation of the manuscript, which qualitatively agree with our data.[46, 47]

Acknowledgements

We thank S. Inoue and T. Jinno for technical support. This work was supported by JSPS KAKENHI (Grants No. JP19H01837, JP16H04012, and JP19H05824).

References

  1. [6]Y. Wu, D. Mou, N. H. Jo, K. Sun, L. Huang, S. L. Bud’ko, P. C. Canfield, and A. Kaminski: Phys. Rev. B 94 (2016) 121113.
  2. [7]B. Feng, Y.-H. Chan, Y. Feng, R.-Y. Liu, M.-Y. Chou, K. Kuroda, K. Yaji, A. Harasawa, P. Moras, A. Barinov, W. Malaeb, C. Bareille, T. Kondo, S. Shin, F. Komori, T.-C. Chiang, Y. Shi, and I. Matsuda: Phys. Rev. B 94 (2016) 195134.
  3. [11]H. Yasuoka, T. Kubо, Y. Kishimoto, D. Kasinathan, M. Schmidt, B. Yan, Y. Zhang, H. Tou, C. Felser, A. Mackenzie, and M. Baenitz: Phys. Rev. Lett. 118 (2017).
  4. [12]Y. Tian, N. Ghassemi, and J. H. Ross: Phys. Rev. B 100 (2019) 165149.
  5. [14]C. G. Wang, Y. Honjo, L. X. Zhao, G. F. Chen, K. Matano, R. Zhou, and G.-q. Zheng: Phys. Rev. B 101 (2020) 241110.
  6. [20]S. Tang, C. Zhang, D. Wong, Z. Pedramrazi, H.-Z. Tsai, C. Jia, B. Moritz, M. Claassen, H. Ryu, S. Kahn, J. Jiang, H. Yan, M. Hashimoto, D. Lu, R. G. Moore, C.-C. Hwang, C. Hwang, Z. Hussain, Y. Chen, M. M. Ugeda, Z. Liu, X. Xie, T. P. Devereaux, M. F. Crommie, S.-K. Mo, and Z.-X. Shen: Nat. Phys. 13 (2017) 683.
  7. [22]M. N. Ali, J. Xiong, S. Flynn, J. Tao, Q. D. Gibson, L. M. Schoop, T. Liang, N. Haldolaarachchige, M. Hirschberger, N. P. Ong, and R. J. Cava: Nature 514 (2014) 205.
  8. [29]Y. Wu, N. H. Jo, M. Ochi, L. Huang, D. Mou, S. L. Bud’ko, P. C. Canfield, N. Trivedi, R. Arita, and A. Kaminski: Phys. Rev. Lett. 115 (2015) 166602.
  9. [30]Z. Zhu, X. Lin, J. Liu, B. Fauqué, Q. Tao, C. Yang, Y. Shi, and K. Behnia: Phys. Rev. Lett. 114 (2015) 176601.
  10. [33]S.-i. Kimura, Y. Nakajima, Z. Mita, R. Jha, R. Higashinaka, T. D. Matsuda, and Y. Aoki: Phys. Rev. B 99 (2019) 195203.
  11. [34]A. J. Frenzel, C. C. Homes, Q. D. Gibson, Y. M. Shao, K. W. Post, A. Channukha, R. J. Cava, and D. N. Basov: Phys. Rev. B 95 (2017) 245140.
  12. [35]M.-X. Guan, E. Wang, P.-W. You, J.-T. Sun, and S. Meng: Nat. Commun. 12 (2021) 1885.
  13. [36]F. Y. Bruno, A. Tamai, Q. S. Wu, I. Cucchi, C. Barreteau, A. de la Torre, S. McKeown Walker, S. Riccò, Z. Wang, T. K. Kim, H. Hoesch, M. Shi, N. C. Plumb, E. Giannini, A. A. Soluyanov, and F. Baumberger: Phys. Rev. B 94 (2016) 121112.
  14. [37]M. N. Ali, L. Schoop, S. Flynn, Q. Gibson, M. Hirschberger, N. P. Ong, and R. J. Cava: EPL (Europhysics Letters) 110 (2015) 67002.
  15. [38]R. K. Harris, E. D. Becker, S. M. C. de Menezes, R. Goodfellow, and P. Granger: Solid State Nucl. Mag. Res. 22 (2002) 458.
  16. [39]C. P. Slichter: Principles of Magnetic Resonance (Springer, London, 1990).
  17. [46]A. O. Antonenko, E. V. Charnaya, M. K. Lee, L. J. Chang, J. Haase, S. V. Naumov, A. N. Domozhirova, and V. V. Marchenkov: Phys. Solid State 61 (2019) 1979.
  18. [47]W. Papawassiliou, J. P. Carvalho, H. J. Kim, C.-Y. Kim, S. J. Yoo, J. B. Lee, S. Alhassan, S. Orfanidis, V. Psych­aris, M. Karagianni, M. Fardis, N. Panopoulos, G. Papavassiliou, and A. J. Pell: arXiv:2110.01300 (2021).arxiv.org/abs/2110.01300

Paper details

vlnc:W_74pbh3xb
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents