WorksPhysics and Astronomy
Large anomalous Hall effect in single crystals of the kagome Weyl ferromagnet FeSn
Abstract
The material class of kagome metals has rapidly grown and has been established as a field to explore the interplay between electronic topology and magnetism. In this work, we report a combined theoretical and experimental study of the anomalous Hall effect of the ferromagnetic kagome metal FeSn. The compound orders magnetically at 725 K and presents an easy-plane anisotropy. Hall measurements in single crystals below room temperature yield an anomalous Hall conductivity , which is found to depend weakly on temperature. This value is in good agreement with the band-intrinsic contribution obtained by density-functional calculations. Our calculations also yield the correct magnetic anisotropy energy and predict the existence of Weyl nodes near the Fermi energy.
Introduction
In recent years, a number of materials with kagome layers as structural building block has been investigated. Their electronic structures have been found to host unconventional fermions, such as the Weyl fermions in Mn(Ge,Si) [1, 2] and CoSnS [3, 4], quasi-2D Dirac fermions in FeSn [5], and quasi-2D Dirac fermions together with flat bands in FeSn [6].
The variety of kagome metals is being intensively studied including compounds based on different transition metals, e.g, FeSn and CoSn [7, 8, 9], but also different composition variants for a given transition metal, e.g. FeSn and FeSn. The two-dimensional limit has been also addressed, e.g., in thin films of MnSn [10], FeSn [11] or CoSnS [12] and in monolayers of CuGe, FeGe, and FeSn [13]. The latter are iso-structural monolayers combining the honeycomb lattice structure of Cu or Fe with the triangular lattice of Ge or Sn. Interesting electronic properties have been reported, such as massive Weyl points in the FM state of FeGe and massless Weyl points in the FM state of FeSn [13].
Large efforts have been made to correlate the geometrical aspects of the electronic structure with the electronic response to external fields. In particular, large anomalous Hall and Nernst conductivities have been reported in several kagome metals, both in cases in which the ground state is ferromagnetic [4, 14, 15, 16, 17] or antiferromagnetic [1, 2, 10, 18].
In this work, we study the compound FeSn, one natural structural derivative of FeSn and FeSn [6, 19]. This material has recently attracted attention as a possible permanent magnet due to its large ordering temperature (725 K) and the possibility of changing its magnetic ground state from easy plane to easy axis through alloying [20, 21]. Recently, large anomalous Nernst data in polycrystals of FeSn have been reported [22]. Here, we report the growth of single crystals along with magnetic properties and measurements of the anomalous Hall resistivity. In addition, we calculate the electronic structure by means of density-functional theory (DFT) calculations. Our main result is the experimental finding of a large anomalous Hall conductivity (AHC) of about 500 , a value which is found to agree well with the band-intrinsic contribution computed from DFT. The measured AHC is weakly temperature dependent below room temperature. Further, our calculations indicate the existence of Weyl nodes near the Fermi surface and suggest that moderate hole doping could further increase the AHC up to values of .
This work is organized as follows. Section II describes the experimental and computational methods used in our investigation. Section III presents experimental results with focus on the anomalous transport properties. Section IV contains our theoretical results, which include a characterization of the bulk electronic and magnetic properties, as well as a characterization of the Weyl nodes structure in the ferromagnetic phase. Last, Section V contains our concluding remarks.
Methods
Experimental Methods
The bulk crystal structure of FeSn shown in Figure 1(a,b) consists of layers of iron and tin piled in an A-B stacking. The Fe atoms form a kagome lattice with Sn atoms sitting at the center of the hexagon. This structure belongs to space group (SG 194) with the experimental lattice constants Å and Å, respectively [23, 24].

Figure 1. (a) Crystal structure of Fe₃Sn. (b) Kagome lattice in the −plane along the -axis. (c) Photo of Fe₃Sn single crystals where the hexagonal facets are (001) planes. The vertical scale bar stands for 1 mm.
In view of the narrow stability regime of Fe₃Sn in the iron-tin binary phase diagram [25], we grew single crystals of Fe₃Sn via a solid state reaction. Iron powder (Alfa Aesar, 99.998%) and tin powder (Alfa Aesar, 99.995%) were mixed in a ratio of 3.5 ∼ 3 : 1 and loaded into an evacuated quartz tube. After being heated up to 850 °C, kept for 120 hours and slowly cooled to 800 °C over the course of 400 hours, the quartz tube was quenched to cold water and we found crystals of Fe₃Sn up to the lateral size of 500 μm as we show in Figure 1(c). We note that a small number of Fe₅Sn₃ crystals can also be found in the quartz tubes. We confirmed with X-ray diffraction (XRD) that during the growth process Fe₃Sn and Fe₅Sn₃ tend to crystallize in distinct morphologies: Fe₃Sn forms hexagonal prisms (see crystals in Figure 1(c)) and Fe₅Sn₃ tends to form elongated hexagonal bipyramids. Phase purity of the sample under study is confirmed by powder XRD (see supplemental material, Figure S1) [26]. Electrical transport measurements were performed using the standard five-probe methods in a commercial superconducting magnet. The magnetic field is applied along the -axis and the current within the -plane.
Figure S1. Powder XRD pattern of FeSn used in this study (the wavelength of X-ray used is 1.54 Å).
Computational details
DFT calculations were performed using the full potential local orbital (FPLO) code version 18.00-52 [27, 28]. The Generalized Gradient Approximation with the parametrization of Perdew, Burke, and Ernzerhof was used [29]. Relativistic effects were treated in the four component formalism as implemented in FPLO. Brillouin zone (BZ) integrals were performed with the tetrahedron method based on a -mesh formed of subdivisions. The experimental structure was used as detailed above. To ensure an accurate band structure close to the Fermi level, an enhanced basis set as defined in the appendix to Ref. [30] was used.
Ferromagnetic (FM) configurations were considered with different quantization axes. In particular, the magnetic anisotropy energy (MAE) was computed based on calculations with the magnetic moments oriented within the kagome planes ([100] direction) or perpendicular to these layers ([1] direction).
The study of Weyl nodes, of the surface spectral properties and of the anomalous Hall conductivities are based on a tight-binding model obtained by constructing maximally projected Wannier functions. For this aim, we used the PYFPLO [28] module of the FPLO code. The local Wannier basis set is formed of Fe-3, Fe-4, Sn-5 and Sn-5 orbitals. The search for Weyl nodes was done with a bisection method that detects sources of the Berry curvature field. After a set of candidate nodes is found, the corresponding Chern number associated to each point is computed by integrating the Berry curvature flux through a small sphere centered at the node, as done in Ref. [31].
Finally, the band-intrinsic contribution to the anomalous Hall conductivity is calculated using the formula
where is a band index, is the component of the Berry curvature, is the occupation number of the Bloch state and the Levi-Civita tensor [32]. A -mesh was used for this calculation.
Experimental results
Fe₃Sn is known to order ferromagnetically at K [20, 21]. The resistivity of Fe₃Sn as a function of temperature within the kagome lattice plane is shown in Figure 2(a), exhibiting a residual resistivity ratio (RRR) of 2.9. We assume that the diffusive nature of the solid state reaction process facilitates disorder formation throughout the synthesis process, resulting in the high residual resistivity μΩ · cm and low RRR in Fe₃Sn as compared with it’s cousin compounds Fe₃Sn₂ [19] and FeSn [6].
Figure 2. (a) Resistivity of FeSn as a function of with current in the kagome lattice plane. (b) Hall resistivity as a function of at selected . Here the magnetic field is applied along the -axis. (c) Anomalous Hall resistivity and ordinary Hall coefficient (inset) vs. in FeSn extracted from . (d) -evolution of the anomalous Hall conductivity in FeSn.
As expected in prototypical ferromagnetic metals, we observe in the Hall traces of Fe₃Sn a prominent anomalous component as shown in Figure 2(b). Saturation is observed at about 3 T external field, which we relate to the complete re-orientation of the magnetization from its easy-plane ground state to the -axis. The Hall resistivity can be decomposed into the ordinary and anomalous contributions via , where is the ordinary Hall coefficient, the magnetic induction in -direction, the anomalous Hall coefficient, and the magnetization in -direction. gives the anomalous Hall resistivity . We infer and from the high field intercept and slope (above 3 T) of , respectively. This means, the extracted data refers to saturated . The results are shown in Figure 2(c). grows monotonically with while exhibits a sign reversal; at K corresponds to a carrier density of . The observed suggests the coexistence of both large electron and hole pockets in the system. The anomalous Hall conductivity estimated from via is displayed in Figure 2(d). is found to depend weakly on and the maximum is around . We note that the system is characterized by longitudinal conductivity between , and falls rather in the moderately dirty regime, such that the observed is expected to reflect an underlying intrinsic Berry curvature contribution [33, 34].
COMPUTATIONAL RESULTS
In this section, we first analyze the magnetic properties and electronic structure of FeSn, we report the existence of several Weyl nodes near the Fermi surface and we present calculations of the band-structure-intrinsic contribution to the anomalous Hall conductivity.

Figure 3. (a) Band structures in the scalar relativistic and fully-relativistic approximations with the magnetic quantization axis along [100]. (b) Fully relativistic band structures with the quantization axis along [100] and [1].
Table I shows the total energies and magnetic moments obtained for different quantization axes. The FM state with quantization axis along the [100] direction is found to be the ground state with a total magnetic moment of per FeSn.
The magnetic moment is slightly reduced if the magnetization is oriented along the -axis. The MAE calculated from the energy difference between these two states amounts to meV per FeSn. Note that we refrain from an analysis of in-plane magnetic anisotropy, which is very small in hexagonal systems and not expected to affect the transport properties considered here. Under the assumption of negligible higher-order terms, this translates into an anisotropy constant MJ/m and an anisotropy field of 3.1 T. The former value agrees with earlier theoretical results of MJ/m [20] (the authors of this reference use a sign convention opposite to the usual one) and of -1.5 MJ/m [35]. The calculated anisotropy field agrees with the experimentally observed saturation around 3 T, see Figure 2(b), and with the same result of 3 T obtained from earlier magnetization data [20]. We tried the application of so-called orbital polarization corrections (OPC) [36] which, however, yield a two-fold enhanced anisotropy field. Thus, we conclude that FeSn is better described by conventional GGA than by GGA-OPC and use only GGA data for the further investigation.
| State | Energy (meV / f.u.) | Total moment( / f.u.) |
| FM [100] | 0 | 7.22 |
| FM [1] | 0.64 | 7.20 |
Table 1. Total energy referred to the ground state energy and total magnetic moments (including spin and orbital contributions) for the two considered magnetic states. The reported data are calculated considering the extended basis set.
Figure 3(a) presents the energy dispersion obtained in the scalar and in the fully-relativistic calculations with [100] orientation of the magnetization. Several bands, which mainly present Fe-3d character, cross the Fermi energy. Bands with relatively flat energy dispersion as a fingerprint of the kagome lattice are present in the -- plane around -0.5 eV as well as in the -- plane around +0.6 eV and around -0.8 eV. Without SOC, apparent low-energy band crossings along the paths - and -- can be observed, which appear to be robust to the SOC for this direction of the magnetic moments. Fig. 3(b) compares the bands with SOC for the FM [1] and FM [100] configurations and shows that these crossings become gapped when the magnetization points along [1].
A search of Weyl nodes for the FM [100] ground state yields the existence of several Weyl nodes, the closest to Fermi surface are found 8 meV below the Fermi energy. Notice that in SG 194, for this magnetic configuration, there can be up to eight symmetry-related Weyl nodes generated by the inversion symmetry , the two-fold rotations , , and the reflection symmetries , and , where is the time-reversal operator.
When the magnetization is rotated towards the hard axis, a situation experimentally relevant in view of the MAE found above and the observed saturation of , one can expect the Weyl nodes to move in momentum and energy space as theoretically found in other magnetic compounds [37, 38]. A search of Weyl nodes for the FM [1] indeed leads to sizeable changes in the number and energy of the Weyl nodes near the Fermi energy, as illustrated in Figure 4, which shows the found Weyl nodes ordered according to their energy, relative to the Fermi energy, for both magnetic configurations. We also present the distribution of these Weyl nodes in the Brillouin zone in the supplemental material (see Figure S2 and Figure S3) [26].
!Energy of Weyl nodes near the Fermi surface for the magnetization along the [001] and [100] directions bbox=0.52,0.07,0.93,0.16
Figure 4. Energy of Weyl nodes near the Fermi surface for the magnetization along the [1] and [100] directions. Red, blue and orange dots correspond to Weyl nodes in which the lower band has index , and , respectively, with the number of valence electrons.

Figure S2. Weyl nodes distribution in the three-dimensional (3D) and two-dimensional (2D) Brillouin zone. (a) In 3D for Magnetization along [1] direction (b) In 2D for Magnetization along [1] direction (c) In 3D for Magnetization along [100] direction (d) In 2D for Magnetization along [100] direction. Red, blue and orange dots correspond to Weyl nodes in which the lower band has index , and , respectively, with the number of valence electrons.
Figure S3. Distribution of eight Weyl nodes located at 8 meV below the Fermi level for magnetization along [100] direction (a) In 3D (b) In 2D. Red and blue dots correspond to Weyl nodes with positive and negative chirality, respectively.
Fig. 5 presents the band-intrinsic contribution to the anomalous Hall conductivity as a function of the chemical potential. For quantization axis along [1] ([100]) only () is different from zero. At the charge neutrality point (), the related values are ( and (. The former value is in fairly good agreement with the experimental result. In the supplemental material [26], we analyze the contribution to the AHC from states at different parts of the Brillouin zone and show that the most prominent hot spots acquire a loop structure which reflects the importance of structures other than isolated Weyl nodes for the AHC. The AHC obtained for FeSn is significantly larger than FeSn with a value of 200 ( [19], and is comparable to FeSn with a value of 507 ( [39]. Interestingly, according to the calculations a moderate amount of hole doping could increase and up to maximum values of ( and (, respectively. However, this increase is contingent upon maintaining the stability of the ground state property during the doping process [40, 41]. Recent values of AHC at [42] is found to be larger than our reported value obtained from the enhanced basis calculations, but is well supported with our earlier work [43].
Conclusions
We have studied single crystalline kagome metal FeSn by means of transport experiments and on the basis of density-functional calculations. The system is found to be ferromagnetic, with an easy-plane magnetic anisotropy. A moderate magnetic field of about 3 T is sufficient to reorientate the magnetization along the hexagonal axis. From transport measurements we have inferred
Figure 5. Anomalous Hall conductivity as a function of the chemical potential.
the anomalous Hall conductivity to be . Our DFT results reproduce the preference of the easy-plane anisotropy and our calculation of the band-intrinsic contribution to the AHC agrees well with the experimental results. Interestingly, our calculations indicate that moderate hole doping could largely increase the AHC. All-together, our experimental and theoretical results establish as a kagome Weyl metal with large AHC.
Acknowledgments
We thank Manuel Richter for fruitful discussions, suggestions and for reading the manuscript. We also thank Ulrike Nitzsche for technical assistance. M.P.G. thanks the Alexander von Humboldt-Stiftung for the financial support through equipment grants and renewed research program. M.P.G. was also supported by a grant from UNESCO-TWAS and the Swedish International Development Cooperation Agency (SIDA). The views expressed herein do not necessarily represent those of UNESCO-TWAS, SIDA or its Board of Governors. J.I.F. would like to acknowledge the support from the Alexander von Humboldt-Stiftung and ANPCyT grants PICT 2018/01509 and PICT 2019/00371. L.Y. acknowledges support by the Tsinghua Education Foundation and STC Center for Integrated Quantum Materials, NSF grant number DMR-1231319. This work was funded, in part, by the Gordon and Betty Moore Foundation EPiQS Initiative, through Grants GBMF3848 and GBMF9070 to J.G.C. (material synthesis) and NSF grant DMR-2104964 (material analysis). J.-S.Y. is supported by the National Science and Technology Council (Grant No. MOST 110-2112-M-003-008-MY3) and National Center for Theoretical Sciences in Taiwan. J.v.d.B. acknowledges financial support from the German Research Foundation (Deutsche Forschungsgemeinschaft, DFG) via SFB 1143 Project No. A5 and under Germany’s Excellence Strategy through the Würzburg-Dresden Cluster of Excellence on Complexity and Topology in Quantum Matter ct.qmat (EXC 2147, Project No. 390858490).
References
Supporting Information: Large anomalous Hall effect in single crystals of the kagome Weyl ferromagnet FeSn
X-ray diffraction
This data confirms the phase purity of single crystals of FeSn.
Weyl nodes distribution in Brillouin zone
In the main text, we have presented the energy of the Weyl nodes, as illustrated in Figure 4. Additionally, to provide further insight, we depict the distribution of these Weyl nodes in the Brillouin zone in Figure S2. Weyl nodes closest to Fermi level are found 8 meV below the Fermi energy for the magnetization along [100] direction. There are eight such Weyl nodes connected by symmetry which we present in Figure S3.
Anomalous Hall Conductivity (AHC) and Berry curvature
We have analyzed how states at different parts of the Brillouin zone contribute to the AHC and found that the largest contributions evidence a loop-like structure that reflects weakly gapped nodal lines rather than Weyl nodes as the origin.
Figure S4. Left: Contribution to the AHC from the different planes perpendicular to . Right: as a function of and for the plane that contributes the most to the AHC, indicated by a vertical line in the left panel. The loop-like structure of the hot spots indicates a significant contribution from states other than isolated Weyl nodes. The data corresponds to the Fermi energy and magnetization along [1].
References
- [1]A. K. Nayak, J. E. Fischer, Y. Sun, B. Yan, J. Karel, A. C. Komarek, C. Shekhar, N. Kumar, W. Schnelle, J. Kübler, et al., Sci. Adv. 2, e1501870 (2016).
- [2]K. Kuroda, T. Tomita, M.-T. Suzuki, C. Bareille, A. Nugroho, P. Goswami, M. Ochi, M. Ikhlas, M. Nakayama, S. Akebi, et al., Nat. Mater. 16, 1090 (2017).
- [3]D. Liu, A. Liang, E. Liu, Q. Xu, Y. Li, C. Chen, D. Pei, W. Shi, S. Mo, P. Dudin, et al., Science 365, 1282 (2019).
- [4]E. Liu, Y. Sun, N. Kumar, L. Muechler, A. Sun, L. Jiao, S.-Y. Yang, D. Liu, A. Liang, Q. Xu, et al., Nat. Phys. 14, 1125 (2018).
- [5]L. Ye, M. K. Chan, R. D. McDonald, D. Graf, M. Kang, J. Liu, T. Suzuki, R. Comin, L. Fu, and J. G. Checkelsky, Nat. Commun. 10, 1 (2019).
- [6]M. Kang, L. Ye, S. Fang, J.-S. You, A. Levitan, M. Han, J. I. Facio, C. Jozwiak, A. Bostwick, E. Rotenberg, et al., Nat. Mater. 19, 163 (2020).
- [7]M. Kang, S. Fang, L. Ye, H. C. Po, J. Denlinger, C. Jozwiak, A. Bostwick, E. Rotenberg, E. Kaxiras, J. G. Checkelsky, et al., Nat. Commun. 11, 4004 (2020).
- [8]Z. Liu, M. Li, Q. Wang, G. Wang, C. Wen, K. Jiang, X. Liu, S. Yan, Y. H. Huang, D. Shen, et al., Nat. Commun. 11, 4002 (2020).
- [9]J.-X. Yin, N. Shumiya, S. Mardanya, Q. Wang, S. S. Zhang, H.-J. Tien, D. Multer, Y. Jiang, G. Cheng, N. Yao, et al., Nat. Commun. 11, 4003 (2020).
- [10]T. Matsuda, N. Kanda, T. Higo, N. Armitage, S. Nakatsuji, and R. Matsunaga, Nat. Commun. 11, 909 (2020).
- [11]H. Inoue, M. Han, L. Ye, T. Suzuki, and J. G. Checkelsky, Appl. Phys. Lett. 115, 072403 (2019).
- [12]M. Tanaka, Y. Fujishiro, M. Mogi, Y. Kaneko, T. Yokosawa, N. Kanazawa, S. Minami, T. Koretsune, R. Arita, S. Tarucha, et al., Nano Lett. 20, 7476 (2020).
- [13]L. Liu, C. Wang, J. Li, X.-Q. Chen, Y. Jia, and J.-H. Cho, Phys. Rev. B 101, 165403 (2020).
- [14]Q. Wang, Y. Xu, R. Lou, Z. Liu, M. Li, Y. Huang, D. Shen, H. Weng, S. Wang, and H. Lei, Nat. Commun. 9, 1 (2018).
- [15]H. Yang, W. You, J. Wang, J. Huang, C. Xi, X. Xu, C. Cao, M. Tian, Z.-A. Xu, J. Dai, et al., Phys. Rev. Mater. 4, 024202 (2020).
- [16]L. Ding, J. Koo, L. Xu, X. Li, X. Lu, L. Zhao, Q. Wang, Q. Yin, H. Lei, B. Yan, et al., Phys. Rev. X 9, 041061 (2019).
- [17]K. Geishendorf, P. Vir, C. Shekhar, C. Felser, J. I. Facio, J. van den Brink, K. Nielsch, A. Thomas, and S. T. Goennenwein, Nano Lett. 20, 300 (2020).
- [18]S. Nakatsuji, N. Kiyohara, and T. Higo, Nature 527, 212 (2015).
- [19]L. Ye, M. Kang, J. Liu, F. Von Cube, C. R. Wicker, T. Suzuki, C. Jozwiak, A. Bostwick, E. Rotenberg, D. C. Bell, et al., Nature 555, 638 (2018).
- [20]B. C. Sales, B. Saparov, M. A. McGuire, D. J. Singh, and D. S. Parker, Sci. Rep. 4, 1 (2014).
- [21]B. Fayyazi, K. P. Skokov, T. Faskе, I. Opahle, M. Duerrschabel, T. Helbig, I. Soldatov, V. Rohrmann, L. Molina-Luna, K. Güth, et al., Acta Mater. 180, 126 (2019).
- [22]T. Chen, S. Minami, A. Sakai, Y. Wang, Z. Feng, T. Nomoto, M. Hirayama, R. Ishii, T. Koretsune, R. Arita, et al., Sci. Adv. 8, eabk1480 (2022).
- [23]A. Jain, S. P. Ong, G. Hautier, W. Chen, W. D. Richards, S. Dacek, S. Cholia, D. Gunter, D. Skinner, G. Ceder, et al., APL Mater. 1, 011002 (2013).
- [24]K. Buschow, P. van Engen, and R. Jongebreur, J. Magn. Magn. Mater. 38, 1 (1983).
- [25]H. Giefers and M. Nicol, J. Alloy. Compd. 422, 132 (2006).
- [26]See Supplemental Material at [href] for detailed information about the powder X-ray diffraction, Weyl nodes distribution in the Brillouin zone, and Berry curvature.
- [27]K. Koepernik and H. Eschrig, Phys. Rev. B 59, 1743 (1999).
- [28]Fplo, URL https://www.fplo.de/.
- [29]J. P. Perdew, K. Burke, and M. Ernzerhof, Phys. Rev. Lett. 77, 3865 (1996).
- [32]X. Wang, J. R. Yates, I. Souza, and D. Vanderbilt, Phys. Rev. B 74, 195118 (2006).
- [33]S. Onda, N. Sugimoto, and N. Nagaosa, Phys. Rev. B 77, 165103 (2008).
- [34]N. Nagaosa, J. Sinova, S. Onda, A. H. MacDonald, and N. P. Ong, Rev. Mod. Phys. 82, 1539 (2010).
- [35]O. Y. Vekilova, B. Fayyazi, K. P. Skokov, O. Gutfleisch, C. Echevarria-Bonet, J. M. Barandiarán, A. Kovacs, J. Fischbacher, T. Schrefl, O. Eriksson, et al., Phys. Rev. B 99, 024421 (2019).
- [36]L. Nordström, M. Brooks, and B. Johansson, J. Phys.: Condens. Matter 4, 3261 (1992).
- [37]M. P. Ghimire, J. I. Facio, J.-S. You, L. Ye, J. G. Checkelsky, S. Fang, E. Kaxiras, M. Richter, and J. van den Brink, Phys. Rev. Res. 1, 032044 (2019).
- [38]R. Ray, B. Sadhukhan, M. Richter, J. I. Facio, and J. van den Brink, npj Quantum Matter 7, 1 (2022).
- [39]H. Li, B. Zhang, J. Liang, B. Ding, J. Chen, J. Shen, Z. Li, E. Liu, X. Xi, G. Wu, et al., Phys. Rev. B 101, 140409 (2020).
- [40]A. Ozawa and K. Nomura, Physical Review Materials 6, 024202 (2022).
- [41]G. Guguchia, H. Zhou, C. Wang, J.-X. Yin, C. Mielke III, S. Tsirkin, I. BelopolskI, S.-S. Zhang, T. Cochran, T. Neupert, et al., Npj Quantum Materials 6, 50 (2021).
- [42]C. Shen, I. Samathrakis, K. Hu, H. K. Singh, N. Fortunato, H. Liu, O. Gut Fleisch, and H. Zhang, npj Comput. Mater. 8, 248 (2022).
- [43]M. P. Ghimire, B. P. Belbase, B. Karki, L. Ye, J.-S. You, J. Facio, J. Checkelsky, M. Richter, and J. Van den Brink, Bull. Am. Phys. Soc. 66, M51.00007 (2021).