Formation of yttrium oxalate phase filled by carbon clusters on the surface of yttrium oxide films

Abstract

In the current paper, we report the results of surface modification of cubic Y2O3 films employing carbon-ion implantation. The characterization results demonstrate the formation of a stable yttrium oxalate-based structure with cavities filled with carbon clusters. Theoretical simulations demonstrate that the incorporation of eighteen-atom carbon clusters into the cavities of Y2(C2O4)3 does not lead to valuable changes in the crystal structure of yttrium oxalate. X-ray diffraction and optical measurements demonstrate that the subsurface bulk area of cubic yttrium oxide remains unperturbed. The oxalate "skin" thickness with embedded carbon clusters is estimated to be approximately 10 nm. The prospective employing the method to manage optical properties and increase the biocompatibility of yttria and lanthanide oxides are discussed.

Introduction

Composites of carbon nanodots (from now on referred to as CNDs) and metal oxides have been intensively studied in recent years due to their promising applications in storage materials [1], sensing [2, 3], solar cells [4], and especially catalysis [5, 6, 7, 8, 9, 10]. The combination of wide bandgap in oxides and narrower bandgaps in CNDs having different chemically active centers in both parts of such composites predicts that these materials will be equally important both for photovoltaic and photocatalytic applications [4, 7, 8, 9, 10]. At the same time, one of the limitations hindering this important area's onward development is the composites' stability due to the weak adhesion of CNDs to metal substrates [1, 2, 9, 11]. Another approach to improve the future application of these composites is to reduce the degradation of functional properties of oxides in the presence of carbon nanosystems [12]. The biological activity of some CNDs-metal-oxide composites has recently been reported (see, e.g., Ref. [13]), which may also be a potential source of cytotoxicity. As one of the possible solutions to this problem, the incorporation of nano-carbons into the surface of the metal oxide host is proposed. The results reported in Refs. [14, 15, 16] indicate a simple dissolution of carbon in oxide host matrices without any formation of CNDs. At the same time, unfortunately, only a limited number of both oxides (usually ZnO [17, 18] and TiO2_2 [19]) and a limited number of fabrication methods have been considered, which is not sufficient to clarify the actual situation. Thus, employing other incorporation methods of carbon atoms into the other oxide hosts seems to be a reasonable solution at this stage.

Yttrium oxide Y2O3Y_2O_3 is a rare earth sesquioxide with several promising physical properties that allow us to consider this material as a suitable technological host-oxide for antireflection protective coatings, doped laser applications, barrier coating of high-temperature composites, electric gate interfaces, etc. (see, e.g., Refs. [20, 21, 22, 23, 24]). The above properties usually include a relatively wide bandgap, high melting point, low thermal expansion, and good phase stability. At the same time, the latter feature belongs only to the cubic bixbyite polymorph of yttrium oxide (CC-type Y2O3Y_2O_3 or CC-Y2O3Y_2O_3). In contrast to bixbyite, hexagonal and monoclinic phases can be fabricated only at temperatures above 2325 °C [25] and relatively high pressures [25, 26]. One of the other potential applications of yttrium oxide nanoparticles is bioimaging [23, 27, 29] [28]. Many studies of the potential toxicity of yttrium oxide and the use of yttrium oxide nanoparticles as biomarkers have revealed essential suppression of oxidative stress in various living creatures due to the performed injection of yttrium oxide nanoparticles [30, 31, 32, 33]. The release of yttrium ions (considered free-radical harvesters) from the surface of Y2O3Y_2O_3 nanoparticles was discussed as a leading source of this effect [34, 35]. Additionally, large-scale application of yttria-based nanoparticles for bioimaging requires an increase in the biocompatibility of these materials [36, 37]. Therefore, modifying the yttrium oxide surface through carbon incorporation may have a substantial practical impact beyond what was discussed in the previous paragraph regarding catalytic and sensing properties.

The CC-type atomic structure has an Ia3Ia3 space group with 16 formula units in the elementary cell [25, 38]. Such structural feature is well-suitable for substitution doping with rare-earth ions of lattice-sites yttrium atoms. However, it is not compatible with other ions that are not rare-earth [22, 39]. Since the CC-type Y2O3Y_2O_3 unit cell contains 48 oxygen and 32 yttrium ions located in the center of an approximate cube, interstitial doping is preferred for other ions, and carbon atoms are not an exception. Therefore, cubic Y2O3Y_2O_3 can be considered as a natural candidate for testing the possibility of CNDs formation in a metal-oxide host-matrix.

Ion implantation is a powerful technique for surface modification [40, 41]. Typically, this method can be employed to fabricate point defects (single impurities and clusters) in metals [42] and semiconductors [43, 44]. Among the oxide host-materials ZnO\mathrm{ZnO}, TiO2\mathrm{TiO}_{2} and SiO2\mathrm{SiO}_{2} were usually chosen as the ordinary substrates for implantation. Surface implantation of heavier metals oxides such as Gd2O3\mathrm{Gd}_{2}\mathrm{O}_{3} has been the subject of a small number of studies in which low concentrations of impurities are embedded into the hosts [45, 46]. Some scientific papers also report the formation of a secondary phase in semiconductor host-substrate [47].

In this paper, we report the results of synthesis of cubic yttrium oxide films employing magnetron sputtering and onward incorporation of significant amount of carbon impurities into the surface by means of pulsed ion implantation. The modified films were systematically studied by Scanning Electron Microscopy (SEM), X-Ray Diffraction (XRD), X-Ray Photoelectron and Raman spectroscopy, followed by measurements of optical properties. Experimental results were used for theoretical simulation of carbon nano-clusters embedded into yttrium oxalate phase, formed on the surface of yttrium oxide after implantation of relatively significant amount of carbon ions there.

Experimental details and theoretical method

An yttrium oxide film was deposited on a quartz glass substrate employing constant pulse mode (50 kHz, 10 μ\mus) with the help of reactive magnetron sputtering technology. Immediately before the deposition process, the quartz glass substrate was cleaned in acetone solvent using an ultrasonic bath for 20 min. Then, air drying of the blank substrate was performed. An yttrium source was obtained by cold pressing of yttrium metal powder of 99.99 % purity at 30 MPa pressure, yielding the source geometry 40 mm in diameter and 2 mm thick. The magnetron, the sputtered source, and the blank substrate were loaded into a vacuum chamber, which then was pumped out to 6.6×10−36.6 \times10^{-3} Pa pressure using a turbomolecular pump. The deposition of yttrium was carried out at 30 W of magnetron power for 8 h in a combined argon-oxygen atmosphere with at least 30% volume concentration of oxygen. The substrate temperature during the deposition process was limited to 400±25400 \pm25°C. Then, the final sample was cooled down to room temperature in a vacuum chamber. The final thickness of magnetron sputtered Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} blank (non-implanted) film was ~700 nm, which was determined by the ball abrasion method employing the Calotest system (CSM Instruments SA, Peseux, Switzerland).

Carbon pulsed implantation of synthesized and stored in ambient conditions Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} thick film had been carried out as follows. A beam of C-ions with the energy of 30 keV was generated in the repetitively pulsed mode with a pulse duration of 0.4 µs and 6.25 Hz repetition rate. The vacuum in the implanter chamber was not worse than 0.01 Pa and was kept employing a turbomolecular pump. The ion fluence was 1017 cm−210^{17}\ \mathrm{cm}^{-2}, which is an order larger than typically used for surface modification [45, 48] [47]. The exposure of the sample under a pulsed ion beam was at least 370 seconds. After carbon implantation, the sample was kept in a vacuum chamber for 12 minutes before being placed in a humidity-protected transfer vessel to transfer it to other experimental techniques.

The implanted films deposited on the substrates were visualized using a Carl Zeiss Evo LS10 scanning electron microscope. Structural-phase analysis of the Y2O3\mathrm{Y}_2\mathrm{O}_3 sample under study was performed using an XPertPro MPD diffractometer employing Cu Kα\alpha = 1.54 Å radiation (see XRD pattern shown in Figure 1).

Image not extracted

Figure 1. SEM images of the surface (a,b), XRD patterns (c) and Raman spectra (800–1850 cm−1^{-1}) of Y2_2O3_3:C (black) and Y2_2(C2_2O4_4)3_3·nH2_2O (red) together with their

Since yttrium oxide films are widely used in different optical applications (see Introduction section), it is logical to apply surface-sensitive methods to inspect the chemical composition and grade of the surface of our samples. For this reason, we employed X-ray Photoelectron Spectroscopy (XPS) using survey and core-level analysis with the help of a ThermoScientific K-alpha Plus XPS spectrometer. This spectrometer has a monochromatic microfocused Al Kα\alpha X-ray source and has 0.05 at% element sensitivity. Operating pressure in an analytic chamber during measurements was not worse than 1.3×10−61.3 \times10^{-6} Pa. Dual-channel automatic charge compensator (GB Patent 2411763) was applied to exclude the charging of our sample under XPS analysis because of the loss of photoelectrons. Pre-run-up procedures performed included standard degassing of the sample and analyzer binding energy scale inspection and re-calibration (if needed) employing sputter-cleaned Au (4f7/24f_{7/2} band), Ag (3d5/23d_{5/2} band), and Cu (2p3/22p_{3/2} band) inbuilt XPS Reference Standards according to ISO 16.243 XPS International Standard and XPS ASTM E2108-00 Standard. We used a ThermoScientific XPS spectrometer inbuilt electronic database and a well-known approved NIST XPS Standard Reference Database (USA).

Raman spectra were obtained in a backscattering geometry with the help of Horiba LabRam HR800 Evolution spectrometer equipped with an Olympus BX-FM confocal microscope with 100×/NA=0.9100\times/\mathrm{NA}=0.9 lens and 514.5 nm line of argon-ion laser (“Geoanalyst” Shared Equipment Center, Institute of Geology and Geochemistry, Ural Branch of Russian Academy of Sciences). The registration was carried out via Czerny-Turner monochromator with 600 grooves/mm diffraction grating employing a multichannel electrically cooled CCD detector. The measurements were carried out with a confocal aperture of 50 µm. Spatial axial resolution was ~1.7 μ\mum. To analyze the structure of the submicron layers of the film, the 3D arrays of Raman spectra were collected by the z-depth profiling with 0.3 μ\mum step [49].

Optical transmission and absorption spectra were recorded with the help of Perkin Elmer Lambda 35 spectrophotometer using an integrating sphere in the 190–1100 nm spectral range. The luminescence and excitation spectra of photoluminescence were recorded on a pulsed luminescence spectrometer Perkin Elmer LS 55 in the phosphorescence mode. The size of the registration time window was 12 ms, and the delay was 0.04 ms. Luminescence spectra were recorded in the 300–900 nm spectral range with an optical filter of 290 nm. Photoluminescence excitation spectra were recorded in the 200–350 nm spectral range with filters of 350 and 390 nm.

Theoretical modeling was performed using the QUANTUM-ESPRESSO pseudopotential code [50], employing the generalized gradient approximation [51] for exchange-correlation potential in a spin-polarized mode. A full optimization of atomic positions and lattice parameters was carried out. During optimization, the electronic ground state was consistently found using ultra-soft pseudopotentials [52].

deconvolution using Voigt functions (d). Red numbers on panels (c,d) indicate features linked with Y2(C2O4)3\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3} phase.

Results and discussion

Samples characterization

The first stage of our study is to inspect the surface homogeneity employing Scanning Tunneling Microscopy (SEM). The SEM images shown in Figure 1(a-Figure 1b) persuasively demonstrate the homogeneity of the surface under study. One can conclude from the XRD patterns presented in Figure 1c that the cubic Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} structure is dominating in the inspected sample. The (222) XRD reflex is characterized by the highest intensity with interplanar peak spacing, corresponding to cubic lattice parameter a=10.70 A˚a = 10.70\,\text{\AA} [53]. We have to note that all XRD peaks are characterized by relatively significant width (FWHM = 0.75 – 1.1 deg). Apparently, this can be explained by the noticeable disordering of the initial Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} cubic lattice after carbon implantation. Also, two weak peaks located in the 14.6 and 26.4 degrees region are not associated with the Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} cubic lattice and will be interpreted onward.

Raman spectrum of Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}:C sample in the first-order of carbon vibrations area demonstrates a complex superposition of highly broadened bands 836, 925, 1032, 1142, 1256, 1355, 1429, 1477, 1570, 1640, ∼\sim1800 cm−1\mathrm{cm}^{-1} (Figure 3d). This spectrum can be attributed to typical carbon vibration bands of G, D1_1, D2_2, D3_3, D′′ and D** (Tab.1). The nature of the bands mentioned was described in numerous publications (see, e.g. Refs. [54, 55, 56, 57]). The G-band corresponds to Raman-allowed phonon mode at the center of the Brillouin zone with E2g_{2g} symmetry and is governed by a single resonance process. It arises from the stretching vibration of sp2^{2}-bonded pairs and indicates a graphitization of material. The D1_1 and D2_2 bands are associated with sp3^{3} defects (disorder), activating the double resonance scattering of single phonons outside the center of the Brillouin zone due to the possibility of electron-hole relaxations. The D3_3 band and the wide bands near 1200 cm−1\mathrm{cm}^{-1} are specific and belong to defective carbons, so they were assigned to the presence of amorphous carbon [58, 59].

Image not extracted

Figure 3. Optimized atomic structure of Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} before (a) and after (b) fabrication of carbon clusters (C18C_{18}) in cavities. Yttrium atoms are shown as large grey-blue spheres, and oxygen and carbon as small red and brown spheres. The calculated charge transfers between carbon clusters and Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} matrix (c). The yellow "clouds" correspond to the increased densities of charge and cyan to the decreased one. Total densities of states of yttrium oxide and oxalate (d). Partial densities of states carbon atom with sp2sp^{2} hybridization from C18C_{18} cluster incorporated into Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} matrix (e). The total densities of states of carbon clusters and Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} matrix after incorporation are shown in panel (f). Fermi energy is set as zero and does not coincide with zero energy in XPS measurements shown in Figs. 2 and Figure 3.

However, it should be noted that the spectra of the Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}:C sample are different from those for mechanically activated and nano-graphites [60, 61]. In particular, this difference consists in the high relative intensity of 1429 and 1477 cm−1\mathrm{cm}^{-1} bands and the presence of weak bands in the region of less than 1000 cm−1\mathrm{cm}^{-1}. The C–O, C–OH, C=O, and H2_2O bonds inherent vibrations of Y2(C2O4)3⋅nH2O\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}\cdot n\mathrm{H}_{2}\mathrm{O} structure and may appear in these areas [62, 63] (see Figure 3d and Tab.1). Accordingly, the presence of Y2(C2O4)3⋅nH2O\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}\cdot n\mathrm{H}_{2}\mathrm{O} phase in the surface layers of Y2O3:C\mathrm{Y}_{2}\mathrm{O}_{3}\mathrm{:C} sample can be hypothesized.

Peak position, cm−1\mathrm{cm}^{-1}
Y2O3:C\mathrm{Y}_{2}\mathrm{O}_{3}\mathrm{:C} a)Y2(C2O4)3\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3} b)[Gd3+]/[oxalate][\mathrm{Gd}^{3+}]/[\mathrm{oxalate}]b)Mechanically activated graphitec)
836860855 (δ(C−C)+ν(C−O)\delta(\mathrm{C-C})+\nu(\mathrm{C-O}))-
925920--
925934--
1032--
1142--1110-1140 (D″)
1256--1260 (D**)
1355--1353 (D₁)
14291423--
14771482-1480 (D₃)
147714961490 (δ(C−OH)+ν(C−O)\delta(\mathrm{C-OH})+\nu(\mathrm{C-O}))1480 (D₃)
1570--1580 (G)
164016421628 (ν(H2O)\nu(\mathrm{H}_{2}\mathrm{O}))1620 (D₂)
∼\sim180017251738 (ν(C=O)\nu(\mathrm{C=O}))-

Table 1. Peak positions and type of vibrations in Raman spectra (800-1850 cm−1^{-1}) of Y2O3:C\mathrm{Y}_{2}\mathrm{O}_{3}\mathrm{:C}, Y2(C2O4)3⋅nH2O\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}\cdot n\mathrm{H}_{2}\mathrm{O} and mechanically activated graphite. Note: a) this work, b) Ref. [63], c) Ref. [60].

Image not extracted

Figure 2. XPS survey (a), Y 3d (b), O 1s (b), and C 1s (d) core-level spectra of Y2O3Y_{2}O_{3}:C in comparance with appropriate XPS external standards.

XPS survey and core-level spectra are shown in Fig. 2. The survey spectra in Fig. 2a demonstrate the absence of contaminations in the range of XPS spectrometer sensitivity (recall that it has 0.05 at. % element sensitivity limits). The spectrum of yttrium 3d3d orbitals of the sample under study (Fig. 2b) differs significantly from the usual spectra of cubic yttria. Based on the comparison mentioned, we can propose significant changes in the atomic structure of Y2O3Y_{2}O_{3}:C in the surface and surface-adjacent areas. The simultaneous increase in the binding energies corresponding to Y 3d3d orbitals can be attributed to the formation of yttrium oxalate Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} phase (see Figure 3a), where Y 3d3/23d_{3/2} and Y 3d5/23d_{5/2} peak positions are 161.6 eV and 159.5 eV, respectively [64]. The helicoidal channels of yttrium oxalate (see Figure 3) and other lanthanides oxalates can be filled with water molecules to form oxalate nonahydrates (Y2(C2O4)3⋅9H2OY_{2}(C_{2}O_{4})_{3}\cdot9H_{2}O). [65] Incorporation of water into the cavities of yttrium oxalate is stable up to 45°C [66]. Such kind of hydration leads to the peaks-shift to 160.5 eV and 158.1 eV [67]. These binding energy values for the sub-bands mentioned are in good agreement with the actually measured Y 3d3d spectrum. The nature of Y 3d3d peaks-shift after filling the pores will be discussed in the next section of the current paper. To prove the conclusion about oxalate phase formation, we inspected XRD data shown in Figure 1c. We found that peak patterns at 14.6 and 26.4 degrees and several other less distinct features are very similar to that for Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} [68]. This conclusion is consistent with the above assumption about the participation of the Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} phase in shaping the Raman spectrum in the region of first-order carbon vibrations. Thus, we can claim with a high degree of probability that at least some part of implanted carbon atoms incorporates into the surface of yttrium oxide as Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3} surface phase. Note that YY 3d3d spectra demonstrate the total absence of Y2O3Y_{2}O_{3} signatures. Since the depth resolution in the XPS method is 7 nm, we can claim that the thickness of oxalate-like skin is more than 7 nm.

XPS O 1s spectrum of Y2O3Y_{2}O_{3}:C shown in Fig. 2c also demonstrates a significant deviation from that for initial (unimplanted) cubic yttrium oxide toward spectra of Y2(C2O4)3⋅9H2OY_{2}(C_{2}O_{4})_{3}\cdot9H_{2}O where the corresponding peak is usually located at 531.4 eV [67]. Note that in non-hydrated yttrium oxalate, the O 1s peak is located at 533.5 eV [64], which is in less agreement with measured spectra. Thus, YY 3d3d and O 1s spectra conform to the proposed model of the formation of an oxalate-like phase with moisture-filed pores in the Y2O3Y_{2}O_{3}:C sample.

A permeation of moisture into the cavities of yttrium oxalate leads to the shift of C 1s core-level from 290.1 eV to 288.5 eV with significant smearing of this peak, which makes it almost undistinguished from the background [64, 67]. Thus, the long tail in the XPS C 1s spectrum shown in Fig. 2d can be linked to the spectral contribution of carbon atoms from Y2(C2O4)3⋅9H2OY_{2}(C_{2}O_{4})_{3}\cdot9H_{2}O-like structure. The band with a distinct maximum at about 284.3 eV is related to some carbon-based structures. The band mentioned is mainly associated with carbon atoms with sp2sp^{2} hybridization. Visible contributions from carbon atoms with sp3sp^{3} and sp1sp^{1} hybridizations were also detected and established. Alternatively, several interpretations of this peak can be proposed. The first is the association of this peak with organic contaminants.

Image not extracted

Figure 2 (PDF p. 9).

We can rule out this interpretation since such characteristic features in the measured CC 1s core-level spectrum are absent over 289 eV due to low-energy soft-sputtering performed directly before XPS measurements according to XPS ASTM E2108-00 Standard. Another possible interpretation is the formation of graphite-like structures (for example, nano-graphenes). These graphite-like clusters have distinct Raman signatures, even for small and distorted structures [55]. At the same time, Raman spectra shown in Figure 1d demonstrate the absence of distinct DD and GG peaks. Thus, the formation of some carbon structures with graphene-like layers can be ruled out. The following interpretation, which can be well-supported by Raman spectra, is the formation of some amorphous carbon-based structures. The typical feature of amorphous carbon is the visible extension of the valence band edge upon the Fermi level [69]. XPS valence band spectra shown in Figure 4 demonstrate an insignificant shift of the valence band edge toward the Fermi level. Thus, the formation of amorphous carbon can also be ruled out. In addition, the sample was washed in acid before XPS measurement. This treatment provides the removal of all discussed above surface contaminants. Since experimentally obtained spectra are close to that for yttrium oxalate with pores filled by the water, it is reasonable to propose the formation of some carbon clusters inside the pores of Y2(C2O4)3Y_{2}(C_{2}O_{4})_{3}, as shown in Figure 3b. Note that incorporation of carbon pairs into the voids of Y-based porous systems was already observed earlier for Y10I13C2Y_{10}I_{13}C_{2} [70].

Image not extracted

Figure 4. XPS spectra of the valence band and valence band edges of Y2O3\mathrm{Y}_2\mathrm{O}_3 and Y2O3:C\mathrm{Y}_2\mathrm{O}_3:\mathrm{C}.

Theoretical modeling

The set of first-principles calculations was carried out to support the model of Y2O3:C\mathrm{Y}_2\mathrm{O}_3:\mathrm{C} phase fabrication based on XRD, XPS, and Raman data combined analysis. In the first stage, we simulated how the formation of surface oxalate skin can affect the valence band structure. Calculations performed, and their data shown in Figure 4d demonstrate the coincidence of valence bands edge of yttrium oxide and oxalate. At the next stage, we simulated carbon nanoclusters with some carbon atoms having mostly sp2sp^2 hybridization. Since helicoidal pores of oxalate nonahydrates can incorporate an additional twelve water molecules [65], we started our simulation with clusters consisting of ten atoms. We proposed several models with small fullerene-like carbon clusters of size smaller than cavities in Y2(C2O4)3\mathrm{Y}_2(\mathrm{C}_2\mathrm{O}_4)_3 and containing several carbon atoms. After that, a full optimization of lattice parameters and atomic positions of yttrium oxalate with incorporated carbon clusters was carried out. Several model clusters collapsed or formed covalent bonds with the surrounding host matrix. One of the clusters shown in Figure 3b survived during the optimization of atomic structure. Note that incorporating C18\mathrm{C}_{18} clusters into the cavities does not provide visible changes in the overall crystal structure of the oxalate matrix. The changes in lattice parameters are also less than 10%, which is of the same order of magnitudes as in commercial Y2(C2O4)3⋅9H2O\mathrm{Y}_2(\mathrm{C}_2\mathrm{O}_4)_3\mathbin{\cdot}9\mathrm{H}_2\mathrm{O} [71]. Thus, the results of simulations are in qualitative agreement with XRD data.

To inspect carbon atom hybridization, partial densities of states have been calculated. Results of the calculations shown in Figure 3e demonstrate the sp2sp^2 hybridization pattern with a significant number of states near the edge of the valence band, which is typical for carbon atoms. Thus, the simulated structure can be used as a model of yttrium oxalate with an embedded carbon system with a visible number of sp2sp^2 hybridized carbon atoms. Calculated total densities of states of C18\mathrm{C}_{18} clusters and Y2(C2O4)3\mathrm{Y}_2(\mathrm{C}_2\mathrm{O}_4)_3 matrix after implantation are shown in Figure 3f. The calculations demonstrate insignificant changes in the overall electronic structure of yttrium oxalate. In the electronic structure of C18\mathrm{C}_{18} clusters, one can see distinct peaks on the edges of the energy gap. Note that this distinct peak in the valence band is located precisely on the edge of the valence band of the oxalate matrix. Thus, the tiny shift of the valence band edge shown in Figure 4 can be interpreted as a contribution from carbon clusters incorporated as a contribution from carbon nanoclusters embedded into the oxalate matrix. To explain the deviation of XRD patterns of Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}:C from Y2(C2O4)3\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}-like to Y2(C2O4)3⋅9H2O\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}\cdot9\mathrm{H}_{2}\mathrm{O}-like, we calculated the transformations of the charge density distribution after incorporating the C18\mathrm{C}_{18} cluster.

Calculations data shown in Figure 3c demonstrate visible charge densities redistribution in both carbon cluster and oxalate matrix. This charge redistribution explains the origin of transformations in the electronic structure of the oxalate matrix after incorporation of carbon cluster (see Figure 3d,Figure 3f) and deviation of XPS spectra from measured for pristine Y2(C2O4)3\mathrm{Y}_{2}(\mathrm{C}_{2}\mathrm{O}_{4})_{3}. In summary of this theoretical section, we want to note that the proposed structure is the only one from a number of stable sp2sp^{2}-carbon clusters that can be fitted into the cavities of yttrium oxalate. However, we propose that the main physical properties of other sp2sp^{2}-carbon clusters will be similar due to the similarity of size and hybridization.

Optical measurements

The last stage of our study is the inspection of the optical properties of the Y2O3:C\mathrm{Y_2O_3:C} sample.

Absorption spectra of initial (unimplanted) and carbon-doped yttrium oxides demonstrate a tiny decrease of the bandgap from 5.76 eV (this is very close to 5.78 eV reported for cubic Y2O3\mathrm{Y_2O_3} films prepared by a different method [72]) in undoped samples to 5.74 eV after carbon incorporation. The spectral shift mentioned can be associated with the shift of the valence band edge shown in Figure 4. Since the calculation results presented in the previous section demonstrate a significant decrease of the bandgap in yttrium oxalate with embedded carbon clusters, we can claim that formation of this structure occurs only in the thin surface part of Y2O3\mathrm{Y_2O_3} sample. Therefore, the contribution of this structure to overall absorption properties is minuscule.

The size of the transparency gap usually depends on the length of the tailing zone in materials of the same composition, and it is determined by the degree of structural disorder [73] [47]. Both doped and non-doped samples demonstrate the presence of long tails in absorption spectra. In the case of Y2O3\mathrm{Y_2O_3} films, this tail is associated with unavoidable defects of surface and subsurface areas. To inspect the influence of carbon doping on surface-related optical properties, we calculated the difference between measured absorption spectra of carbon-doped and non-doped yttrium oxides. The calculation results shown in Figure 5a demonstrate the visible difference in absorption spectra on the whole length of the tailing zone. This difference is linked to the appearance of the surface oxalate phase with embedded carbon clusters discussed in previous sections (see discussions above).

Image not extracted

Figure 5. Optical absorption spectra of Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} and Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}:C and the difference between measured absorption coefficients (a). Spectra of photoluminescence (hνexc=5.06h\nu_{\mathrm{exc}} = 5.06 eV) and photoluminescence excitation (hνemis=3.27h\nu_{\mathrm{emis}} = 3.27 eV and 2.96 eV) of Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}:C sample (b).

Using interference extremes, it is possible to estimate the thickness of the Y2O3\mathrm{Y_2O_3} film using the expression:

d=λ1λ22(λ2n1−λ1n2)d = \frac{\lambda_1\lambda_2}{2(\lambda_2 n_1 - \lambda_1 n_2)}

where n1n_1 and n2n_2 are the refractive indices at wavelengths λ1\lambda_1 and λ2\lambda_2, which correspond to the maxima (minima) of neighboring interference phases. The average value of the film thickness, determined by extremes in the range of 1 eV – 3.5 eV, was 712 ±\pm 28 nm. The analytically obtained value of the film thickness with an error accuracy coincides with the declared at the synthesis stage (see § 2). Based on the magnitudes of absorption coefficients in bulk and surface-related parts of the spectra in Figure 5a, we can estimate the thickness of the carbon-rich surface skin as about a few dozen nanometers.

Figure 5b shows measured photoluminescence and excitation spectra of Y2O3\mathrm{Y}_2\mathrm{O}_3:C films. An asymmetrical photoluminescence band with a maximum of 3.26 eV was recorded using an excitation energy of 5.06 eV. This band can be fitted by Gaussian components (see dashed lines in Figure 5b) in such a way that two components can be distinguished. The first is 3.0 eV (full width at half maximum, further FWHM = 0.306 eV), and the second is 3.3 eV (FWHM = 0.338 eV). The excitation spectra of the PL were recorded at registration energies close to the maxima of the corresponding Gaussian components: 2.96 eV (red maximum) and 3.26 eV (blue maximum). The resulting excitation band in both cases is described by a Gaussian function with a maximum of 5.03 eV. At the same time, the half-width of the band in the first case is FWHM = 0.449 eV, and in the second, FWHM = 0.421 eV, respectively, which may indicate the different nature of detected photoluminescence centers.

For different morphologies of cubic Y2O3\mathrm{Y}_2\mathrm{O}_3 (bulk crystal, transparent ceramics), luminescence at 3.4–3.5 eV is associated with the luminescence of self-trapped excitons (STE) [74, 75]. We propose that the dominant emission band located at 3.3 eV is also associated with the radiative recombination of STE in the Y2O3\mathrm{Y}_2\mathrm{O}_3 film, and the spectral position of this band is shifted to the region of low energies compared to bulk cases. At the same time, as the literature data show, photons with energy in the region of 5 eV in Y2O3\mathrm{Y}_2\mathrm{O}_3 crystals with a cubic lattice can also excite photoluminescence caused by radiative recombination of a bound exciton (BE) localized in the center of F-type anionic vacancies [72, 76]. Thus, we can conclude that the emission bands located at 3.0 eV and 3.3 eV can be attributed to BE and STE, respectively.

Conclusions

In the current paper, we reported the results of carbon-ion implantation into the surface of cubic yttrium oxide using 101710^{17} cm−2^{-2} ion fluence and onward characterization of the synthesized material. XRD, absorption and photoluminescence measurements demonstrate the stability of cubic yttrium oxide structure with some traces of yttrium oxalate-like phase. XPS measurements demonstrate the formation of Y2(C2O4)3⋅9H2O\mathrm{Y}_2(\mathrm{C}_2\mathrm{O}_4)_3\cdot9\mathrm{H}_2\mathrm{O}-like surface “skin” with cavities filled by some carbon structures with prevailing sp2sp^2 hybridization. No spectral signatures of cubic Y2O3\mathrm{Y}_2\mathrm{O}_3 have been detected in the XPS spectra of the sample under study. Measured Raman spectra confirm the possibility of oxalate-like phase formation in near-surface layers and indicate a substantially disordered structure of near-surface carbon. Theoretical simulations demonstrate the possibility of incorporating C18\mathrm{C}_{18} clusters into the cavities of yttrium oxalate without visible distortions of crystal structure. The calculated electronic structure of C18\mathrm{C}_{18} clusters demonstrates carbon atoms with sp2sp^2 hybridization. Since the outer layers survived after washing the sample in acid, we can propose chemical stability of the fabricated carbon-rich surface “skin.” Note that besides yttrium, all lanthanides also form oxalates with the same pattern of crystal structures. Thus proposed method can be used for suppression of the lanthanides ion leakage from oxide surface, which is essential for increasing the safety of lanthanides-oxides-based devises. Overall, the formation of secondary phase on the surface by means of high-fluence ion implantation is the novel method for the fabrication of few nanometer surface phases on various substrates.

Thus, ion implantation can be used to fabricate carbon-rich skin on the surface of these optically active materials, which should increase the biocompatibility of the materials fabricated from discussed oxides, which is crucial for the material used in bioimaging. Note that yttrium oxalate nonahydrate is a precursor for the synthesis of superconductive YBa2Cu3O7−x\mathrm{YBa_2Cu_3O_{7-x}} (YBCO) [77, 78, 79, 80]. Thus, Y2(C2O4)3⋅9H2O\mathrm{Y_2(C_2O_4)_3\cdot9H_2O}-like surface “skin” can also be discussed as a possible precursor for growing some YBCO-based nanosized layers on Y2O3\mathrm{Y_2O_3} substrates.

Measured absorption spectra also demonstrate some changes in optical properties in the surface area. Since the estimated thickness of oxalate-like surface “skin” is only ten nanometers and the thickness of the film is about 700 nm, the contribution of the carbon-modified part of the system is negligible. Decreasing the oxide film's thickness or the nanoparticles' size will increase the contribution from the carbon-rich surface “skin.” Since the bandgap of pure and carbon-filled yttrium oxalate is narrower than the bandgap of yttrium oxide, the absorption and emission of visible light can be realized. In general, the obtained data on optical and electronic properties indicate new possibilities for the fabrication general-purpose functional materials for photonic and combined optoelectronic devices, elements of information systems, as well as biomarkers and biosensors.

Acknowledgments

The study was supported by the Ministry of Science and Higher Education of the Russian Federation (Ural Federal University Program of Development within the Priority-2030 Program, project 4.38).

References

  1. [1]Y. Ye, H. Wang, H. Liu, Y. Xiang, L. Liu, W. Deng, G. Zou, Y. Liu, H. Hou, X. Ji. Carbon Dots-Regulated Pomegranate-Like Metal Oxide Composites: From Growth Mechanism to Lithium Storage. Small Meth. 6 (2022) 2200245. https://doi.org/10.1002/smtd.202200245
  2. [2]A.G. El-Shamy. New nano-composite based on carbon dots (CDots) decorated magnesium oxide (MgO) nanoparticles (CDots@MgO) sensor for high H2S gas sensitivity performance. Sens. Actuators B: Chem. 329 (2021) 129154. https://doi.org/10.1016/j.snb.2020.129154
  3. [3]Y. Sahu, A. Hashmi, R. Patel, A.K. Singh, Md.A.B.H. Susan, S.A.C. Carabineiro. Potential Development of N-Doped Carbon Dots and Metal-Oxide Carbon Dot Composites for Chemical and Biosensing, Nanomaterials 12 (2022) 3434. https://doi.org/10.3390/nano12193434
  4. [4]H.F. Etefa, T. Imae, M. Yanagida. Enhanced Photosensitization by Carbon Dots Co-adsorbing with Dye on p-Type Semiconductor (Nickel Oxide) Solar Cells. ACS Appl. Mater. Interfaces 12 (2020) 18596–18608. https://doi.org/10.1021/acsami.0c02413
  5. [5]A. Kundu, A.I. Robby A. Shit, H.J. Jo, S.Y. Park. Construction of FeCo2O4@N-Doped Carbon Dots Nanoflowers as Binder Free Electrode for Reduction and Oxidation of Water. Materials 13 (2020) 3119. https://doi.org/10.3390/ma13143119
  6. [6]D. Wu, H. Huang, Y. Zhou, Y. Liu, Z. Kang. N-doped carbon dots modified needle-like NiCo2O4 supported on graphene as efficient dual-functional electrocatalyst for oxygen reduction and evolution reactions. J. Electroanalyt. Chem. 855 (2019) 113617. https://doi.org/10.1016/j.jelechem.2019.113617
  7. [7]Z.W. Heng, W.C. Chong, Y.L. Pang, C.H. Koo. An overview of the recent advances of carbon quantum dots/metal oxides in the application of heterogeneous photocatalysis in photodegradation of pollutants towards visible-light and solar energy exploitation. J. Envir. Chem. Eng. 9 (2021) 105199. https://doi.org/10.1016/j.jece.2021.105199
  8. [8]Z. Hu, H. Huang, F. Yuan, Y. Cai, H. Shu, F. Yu, J. Fang. One-step cladding metal oxide nanowires with a carbon-dots-embedded ZnO amorphous layer toward boosted photoelectrochemical water oxidation, J. Coll. Interf. Sci. 644 (2023) 466-477. https://doi.org/10.1016/j.jcis.2023.04.101
  9. [9]T. Cai, Q. Chang, C. Xue, N. Li, J. Yang, S. Hu. Carbon dots-embedded amorphous nickel oxide for highly enhanced photocatalytic redox performance. J. Coll. Interf. Sci. 630A (2023) 182-190. https://doi.org/10.1016/j.jcis.2022.09.117
  10. [10]R. Atchudan, T.N.J.I. Edison, S. Perumal, N. Karthik, D. Karthikeyan, M. Shanmugam, Y.R. Lee. Concurrent synthesis of nitrogen-doped carbon dots for cell imaging and ZnO@nitrogen-doped carbon sheets for photocatalytic degradation of methylene blue. J. Photochem. Photobiol. A: Chem. 350 (2018) 75-85. https://doi.org/10.1016/j.jphotochem.2017.09.038
  11. [11]M.T. Efa, T. Imae. Hybridization of carbon-dots with ZnO nanoparticles of different sizes. J. Taiwan Inst. Chem. Eng. 92 (2018)112-117. https://doi.org/10.1016/j.jtice.2018.02.007
  12. [12]A.B. Sengul, E. Asmatulu. Toxicity of metal and metal oxide nanoparticles: a review. Environ. Chem. Lett. 18 (2020) 1659–1683. https://doi.org/10.1007/s10311-020-01033-6
  13. [13]D.J. Nemera, H.F. Etefa, V. Kumar, F.B. Dejene. Hybridization of nickel oxide nanoparticles with carbon dots and its application for antibacterial activities. Luminescence 37 (2022) 965-970. https://doi.org/10.1002/bio.4241
  14. [14]C. Wongchoosuk, A. Wisitsoraat, D. Phokharatkul, M. Horprathum, A. Tuantranont, T. Kerdcharoen. Carbon doped tungsten oxide nanorods NO₂ sensor prepared by glancing angle RF sputtering. Sens. Actuators B: Chem. 181 (2013) 388-394. https://doi.org/10.1016/j.snb.2013.01.066
  15. [15]R. Marschall, L. Wang. Non-metal doping of transition metal oxides for visible-light photocatalysis. Catal. Today 225 (2014) 111-135. https://doi.org/10.1016/j.cattod.2013.10.088
  16. [16]Y. Liu, W. Wang, X. Xu, J.-P.M. Veder, Z. Shao. Recent advances in anion-doped metal oxides for catalytic applications. J. Mater. Chem. A 7 (2019) 7280-7300. https://doi.org/10.1039/C8TA09913H
  17. [17]S. Cho, J.-W. Jang, J.S. Lee, K.-H. Lee. Carbon-doped ZnO nanostructures synthesized using vitamin C for visible light photocatalysis. CrystEngComm 12 (2010) 3929-3935. https://doi.org/10.1039/C0CE00063A
  18. [18]J. Zhai, L. Wang, D. Wang, Y. Lin, D. He, T. Xie. UV-illumination room-temperature gas sensing activity of carbon-doped ZnO microspheres. Sens. Actuators B: Chem. 161, (2012) 292-297. https://doi.org/10.1016/j.snb.2011.10.034
  19. [19]J.H. Park, S. Kim, A.J. Bard. Novel Carbon-Doped TiO₂ Nanotube Arrays with High Aspect Ratios for Efficient Solar Water Splitting. Nano Lett. 6 (2006) 24–28. https://doi.org/10.1021/nl051807y
  20. [20]P.S. Das, G.K. Dalapati, D.Z. Chi. Characterization of Y₂O₃ gate dielectric on n-GaAs substrates, Appl. Surf. Sci. 256 (2010) 2245. https://doi.org/10.1016/j.apsusc.2009.10.046
  21. [21]P. Lei, B. Dai, J. Zhu, X. Chen, G. Liu, Y. Zhu, J. Han. Controllable phase formation and physical properties of yttrium oxide films governed by substrate heating and bias voltage, Ceramics International 41 (2015) 8921. https://doi.org/10.1016/j.ceramint.2015.03.165
  22. [22]F. Vetrone, J.-C. Boyer, J.A. Capobianco, A. Speghini, M. Bettinelli. Concentration-Dependent Near-Infrared to Visible Upconversion in Nanocrystalline and Bulk Y₂O₃:Er³⁺, Chem. Mater. 15 (2003) 2737. https://doi.org/10.1021/cm0301930
  23. [23]F. Lu, H. Guo, S. Guo, Q. He, C. Li, W. Tang, G. Chen. Magnetron sputtered oxidation resistant and antireflection protective coatings for freestanding diamond film IR windows, Diamond and Rel. Materials, 18 (2009) 244. https://doi.org/10.1016/j.diamond.2008.09.008
  24. [24]D. Chávez-García, P. Sengar, K. Juárez-Moreno, D.L. Flores, I. Calderón, J. Barrera, G.A. Hirata. Luminescence properties and cell uptake analysis of Y₂O₃:Eu,Bi nanophosphors for bio-imaging applications, J. Mater. Res. Technol. 10 (2021) 797. https://doi.org/10.1016/j.jmrt.2020.11.071
  25. [25]O.N. Carlsson. Bull. Alloy Phase Diagrams, 11 (1990) 61. https://doi.org/10.1007/BF02841584
  26. [26]I. Halevy, R. Carmon, M.L. Winterrose, O. Yeheskel, E. Tiferet, S. Ghose. Pressure-Induced Structural Phase Transitions in Y₂O₃ Sesquioxide, Journal of Physics: Conf. Series 215 (2010) 012003. https://doi.org/10.1088/1742-6596/215/1/012003
  27. [27]G. Kumar Das, T.T.Y. Tan. Rare-Earth-Doped and Codoped Y₂O₃ Nanomaterials as Potential Bioimaging Probes. J. Phys. Chem. C 112 (2008) 11211–11217. https://doi.org/10.1021/jp802076n
  28. [29]S.G. Nath, E.I. Anila. Photoluminescence studies of non-toxic monoclinic yttrium oxide quantum dots synthesized at low temperature for live cell imaging applications. Ceramics Intern. 49 (2023) 13200-13207. https://doi.org/10.1016/j.ceramint.2022.12.199
  29. [30]D. Schubert, R. Dargusch, J. Raitano, S.-W. Chan. Cerium and yttrium oxide nanoparticles are neuroprotective. Biochem. Biophys. Res. Commun. 342 (2006) 86-91. https://doi.org/10.1016/j.bbrc.2006.01.129
  30. [31]M.R. Khaksar, M. Rahimifard, M. Baeeri, F. Maqbool, M. Navaei-Nigjeh, S. Hassani, S. Moeini-Nodeh, A. Kebriaeezadeh, M. Abdollahi. Protective effects of cerium oxide and yttrium oxide nanoparticles on reduction of oxidative stress induced by sub-acute exposure to diazinon in the rat pancreas. J. Trace Elem. Med. Bio. 41 (2017) 79-90. https://doi.org/10.1016/j.jtemb.2017.02.013
  31. [32]S. Kassem, M. Mohamed, H. Sayour, F. Canfarotta, S. Piletsky, M.A.M. Soliman. Functionalized Core-Shell Yttrium Oxide Nanoparticles as Antioxidants Agents in Heat Stressed Rats. Biol. Trace Elem. Res. 198 (2020) 189–197. https://doi.org/10.1007/s12011-020-02036-8
  32. [33]S. Kassem, M.M. Arafa, M.M. Yehya, M.A.M. Soliman. In vivo study of dose-dependent antioxidant efficacy of functionalized core–shell yttrium oxide nanoparticles. Naunyn-Schmiedeberg's Arch. Pharmacol. 395 (2022) 593–606. https://doi.org/10.1007/s00210-022-02219-1
  33. [34]A. Moriyama, U. Takahashi, Y. Mizuno, J. Takahashi, M. Horie, H. Iwahashi, J. Hitoshi. J. Nanosci. Nanotech. 19 (2019) 5418-5425. https://doi.org/10.1166/jnn.2019.16544
  34. [35]F. Zhang, Z. Wang, S. Wang, H. Fang, M. Chen, D. Xu, L. Tang, D. Wang. Physicochemical properties and ecotoxicological effects of yttrium oxide nanoparticles in aquatic media: Role of low molecular weight natural organic acids. Envir. Pollution 212, (2016) 113-120. https://doi.org/10.1016/j.envpol.2016.01.054
  35. [36]E. Kelpsiene, T. Chang, A. Khort, K. Bernfur, I. Odnevall, T.Cedervall, J. Hua. The effect of natural biomolecules on yttrium oxide nanoparticles from a Daphnia magna survival rate perspective. Nanotox.17 (2023) 385-399. https://doi.org/10.1080/17435390.2023.2226712
  36. [37]H. Sayour, S. Kassem, F. Canfarotta, J. Czulak, M.Mohamed, S. Piletsky. Biocompatibility and biodistribution of surface-modified yttrium oxide nanoparticles for potential theranostic applications. Environ. Sci. Pollut. Res. 27 (2020) 19095–19107. https://doi.org/10.1007/s11356-019-04309-9
  37. [38]Y.N. Xu, Z. Gu, W.Y. Ching. Electronic, Structural and Optical Properties of Crystalline Yttria. Phys. Rev. B: Condens. Matter 56 (1997) 14993. https://doi.org/10.1103/PhysRevB.56.14993
  38. [39]L. Laversenne, Y. Guyot, C. Goutaudier, M.Th. Cohen-Adad, G.Boulon. Optimization of Spectroscopic Properties of Yb3+-doped Refractory Sesquioxides: Cubic Y2O3, Lu2O3 and monoclinic Gd2O3. Opt. Mater. 16 (2001) 475. https://doi.org/10.1016/S0925-3467(00)00095-1
  39. [40]N. Teranishi, G. Fuse, M. Sugitani, A Review of Ion Implantation Technology for Image Sensors. Sensors 18 (2018) 2358. https://doi.org/10.3390/s18072358
  40. [41]C.W. White, L.A. Boatner, P.S. Sklad, C.J. McHargue, J. Rankin, G.C. Farlow, M.J. Aziz, Ion implantation and annealing of crystalline oxides and ceramic materials. Nucl. Instr. Meth. Phys. Res. Sect. B: Beam Interact. Mater. Atoms 32 (1988) 11-22. https://doi.org/10.1016/0168-583X(88)90172-3
  41. [42]F. Wang, C. Zhou, L. Zheng, H. Zhang, Corrosion resistance of carbon ion-implanted M50NiL aerospace bearing steel. Prog. Nat. Sci.: Mater. Inter. 27 (2017) 615-621. https://doi.org/10.1016/j.pnsc.2017.07.003
  42. [43]M.A. Capano, A modified oxidation procedure for ion-implanted silicon carbide devices annealed at low temperatures. Appl. Surf. Sci. 184 (2001) 317-322. https://doi.org/10.1016/S0169-4332(01)00511-6
  43. [44]I. Ban, M.C. Öztürk, K. Christensen, D.M. Maher, Effects of carbon implantation on generation lifetime in silicon. Appl. Phys. Lett. 68 (1996) 499-501. https://doi.org/10.1063/1.116379
  44. [45]A.F. Zatsepin, Y.A. Kuznetsova, D.A. Zatsepin, C.-H. Wong, W.-C. Law, C.-Y. Tang, N.V. Gavrilov, D.V. Boukhvalov, Bismuth-doped gadolinium oxide films for UV-Vis multicolor conversion: Combined XPS, DFT and photoluminescence study. J. All. Comp. 949 (2023) 169815. https://doi.org/10.1016/j.jallcom.2023.169815
  45. [46]A. Joseph, G. Lilienkamp, T.F. Wietler, H.J. Osten, Ion-Implanted Epitaxially Grown Gd2O3 on Silicon with Improved Electrical Properties. J. Electron. Mater. 49 (2020) 6270-6275. https://doi.org/10.1007/s11664-020-08392-4
  46. [48]D.A. Zatsepin, A.F. Zatsepin, D.W. Boukhvalov, N.V. Gavrilov Bi-doped silica glass: a combined XPS - DFT study of electronic structure and pleomorphic imperfections. Journal of Alloys and Compounds 829 (2020) 154459. https://doi.org/10.1016/j.jallcom.2020.154459
  47. [49]V. A. Bulatov, Yu. V. Shchapova, D. A. Zamyatin, L. Ya. Sushanek, A. S. Kamenetsky, S. L. Votyakov, Analysis of the chemical composition and structure of films of complex oxides of micron thickness by electron probe microanalysis and confocal Raman spectroscopy (on the example of MgAl2O4 film on SiO2, J. Analytical Chem. 78 (2023) 1-13. https://doi.org/10.31857/S0044050223120034
  48. [50]P. Giannozzi, et al., Advanced capabilities for materials modelling with Quantum ESPRESSO. J. Phys.: Condens. Matter 29 (2017) 465901. https://doi.org/10.1088/1361-648X/aa8f79
  49. [51]J.P. Perdew, K. Burke, M. Ernzerhof. Generalized Gradient Approximation Made Simple, Phys. Rev. Lett. 77 (1996) 3865. https://doi.org/10.1103/PhysRevLett.77.3865
  50. [52]D. Vanderbilt. Soft Self-Consistent Pseudopotentials in a Generalized Eigenvalue Formalism, Phys. Rev. B 41 7892 (1990). https://doi.org/10.1103/PhysRevLett.91.126402
  51. [53]A.F. Zatsepin, Yu.A. Kuznetsova, D.A. Zatsepin, C.H. Wong, W.C. Law, C.Y. Tang, N.V. Gavrilov. Exciton luminescence and optical properties of nanocrystalline cubic Y2O3 films obtained by reactive magnetron sputtering, Nanomaterials 12 (2022) 2726. https://doi.org/10.3390/nano12152726
  52. [54]A.C. Ferrari, J. Robertson, Interpretation of Raman spectra of disordered and amorphous carbon, Phys. Rev. B 61 (2000) 14095–14107. https://doi.org/10.1103/physrevb.61.14095
  53. [55]L. Bokobza, J.-L. Bruneel, M. Couzi, Raman spectra of carbon-based materials (from graphite to carbon black) and of some silicone composites, C 1 (2015) 77–94. https://doi.org/10.3390/c1010077
  54. [56]Z. Li, L. Deng, I.A. Kinloch, R.J. Young, Raman spectroscopy of carbon materials and their composites: Graphene, nanotubes and fibres. Progress in Materials Science 135 (2023) 101089. https://doi.org/10.1016/j.pmatsci.2023.101089
  55. [57]K. Tynyshtykbayev, A. Ainabayev, O. Kononenko, M. Chichkov, Z. Ramazanova, R. Zulkhar­nai, D. Roshchupkin, J. Sorokupudova, V. Starkov, Z. Insepov, Low temperature synthesis of graphene nanocomposites using surface passivation of porous silicon nanocrystallites with carbon atoms. Diam. Rel. Mater. Vol.92 (2019) 53-60. https://doi.org/10.1016/j.diamond.2018.12.012
  56. [58]A. Sadezky, H. Mucken­huber, H. Grothe, R. Niesser, U. Pöschl, Raman microspectroscopy of soot and related carbonaceous materials: spectral analysis and structural information, Carbon 43 (2005) 1731–1742. https://doi.org/10.1016/j.carbon.2005.02.018
  57. [59]M. Pawlita, J.N. Rouzaud, S. Duber, Raman microspectroscopy of carbon blacks: spectral analysis and structural information, Carbon 73 (2015) 479–490. https://doi.org/10.1016/j.carbon.2014.12.030
  58. [60]N.V. Pechishcheva, S.Kh. Estemirova, A.V. Kim, P.V. Zaitceva, E.V. Sterkhov, Yu.V. Shchapova, I.S. Zhidkov, M.Yu. Skrylnik, Adsorption of hexavalent chromium on mechanically activated graphite, Diamond & Related Materials 127 (2022) 109152. https://doi.org/10.1016/j.diamond.2022.109152
  59. [61]J. H. Kwak, S. S. Lee, H. J. Lee, G. Anoop, H. J.Lee, W.S.Kim, S.-W. Ryu, H. S. Kim, and J. Y. Jo, Direct growth of nano-crystalline graphite films using pulsed laser deposition with in-situ monitoring based on reflection high-energy electron diffraction technique. Appl. Phys. Lett. 108 (2016) 123107. https://doi.org/10.1063/1.4944845
  60. [62]G.J. Millar, R.J. Bell, A.Bhargava, I.D.R. Mackinnon, P.M. Frederick­s, FT Raman spectroscopic characterization of oxalate precursors to YBCO superconductors, Materials Lett. 25 (1995) 75-80. https://doi.org/10.1016/0167-577X(96)00025-0
  61. [63]M. Riri, A. Benajjir, T. Eljad­d­i, N. Sefiani, K. Touaj, A. Cherif, M. Hlaïbi. Characterization of two dinuclear complexes of the gadolinium ion by IR and Raman J. Mater. Environ. Sci. 4 (2013) 961-966.
  62. [64]Y. Uwamino, T. Ishizuka, H. Yamatera. X-ray photoelectron spectroscopy of rare-earth compounds. J. Elec. Spect. Rel. Phen. 34 (1984) 67-78. https://doi.org/10.1016/0368-2048(84)80060-2
  63. [65]D. Kustaryono, N. Kerbellec, G. Calvez, S. Freslon, S. Daiguebonne, O. Guillou,New Family of Porous Lanthanide-Containing Coordination Polymers: [Ln2(C2O4)3(H2O)6]nOwith Ln = La–Yb or Y. Cryst. Grow. Design, 10 (2010), 775–781. https://doi.org/10.1021/cg9011668
  64. [66]W.W. Wendlandt, Thermal Decomposition of Scandium, Yttrium, and Rare Earth Metal Oxalates. Anal. Chem. 30 (1958) 58–61. https://doi.org/10.1021/ac60133a015
  65. [67]R.P. Vasquez, XPS Core level spectra of some Y compounds. J. Elec. Spect. Rel. Phen. 50 (1990) 167-170. https://doi.org/10.1016/0368-2048(90)87060-2
  66. [68]M. Ye, L. Zhou, F. Hong, L. Li, Q. Xia, K. Yang, X. Xiong. Synthesis and photoluminescent properties of cuboid-like Y2(C2O4)3:Tb3+ green-emitting phosphors. Optic. Mater. 47 (2015) 161-168. https://doi.org/10.1016/j.optmat.2015.05.012
  67. [69]P. Reinke, P. Oelhafen. Electronic properties of diamond/nondiamond carbon heterostructures. Phys. Rev. B 60 (1999) 15772. https://doi.org/10.1103/PhysRevB.60.15772
  68. [70]M. Kauzlarich, M.W. Payne, J.D. Corbett, Y10I13C2: a novel compound with chains of both carbon-centered and empty clusters. Inorg. Chem. 29 (1990) 3777–3781. https://doi.org/10.1021/ic00344a025
  69. [71]https://www.smolecule.com/products/s1509842 (accessed 3 November 2023)
  70. [72]C. Hua, C. Li, J. Guo, X. Yan, J. Liu, L. Chen, J. Wei, L. Hei, Optical properties of cubic and monoclinic Y2O3 films prepared through radio frequency magnetron sputtering. Surf. Coat. Technol. 320 (2017) 279–283. http://doi.org/10.1016/j.surfcoat.2017.01.004
  71. [73]F. Urbach. The long-wavelength edge of photographic sensitivity and of the electronic Absorption of Solids. Phys. Rev. 92 (1953) 1324. http://doi.org/10.1103/PhysRev.92.1324
  72. [74]A. Lushchik, M. Kirm, C. Lushchik, I. Martinson, G. Zimmerer, Luminescence of free and self-trapped excitons in wide-gap oxides. J. Lumin. 2000, 87–89 (2000) 232–234. http://doi.org/10.1016/S0022-2313(99)00271-9
  73. [75]A. Fukabori, T. Yanagida, J. Pejchal, S. Maeo, Y. Yokota, A. Yoshikawa, T. Ikegami, F. Moretti, K. Kamada, Optical and scintillation characteristics of Y₂O₃ transparent ceramic. J. Appl. Phys. 107 (2010) 073501. http://doi.org/10.1063/1.3330407
  74. [76]V.H. Mudavakkat, V.V. Atuchin, V.N. Kruchinin, A. Kayani, C.V. Ramana, Structure, morphology and optical properties of nanocrystalline yttrium oxide (Y₂O₃) thin films. Opt. Mater. 34 (2012) 893–900. http://doi.org/10.1016/j.optmat.2011.11.027
  75. [77]R.P Vasquez, M.C. Foote, B.D. Hunt, Wet chemical techniques for passivation of YBa₂Cu₃O₇−x. Appl. Phys. Lett. 55 (1989)1801–1803. https://doi.org/10.1063/1.102323
  76. [78]R. P. Vasquez, B. D. Hunt and M. C. Foote, Wet Chemical Passivation of YBa₂Cu₃O₇−x. J. Electrochem. Soc. 137 (1990) 2344. https://doi.org/10.1149/1.2086940
  77. [79]G.S. Grader, D.R. Machado, R. Semiat, Spray pyrolysis of YBCO precursors. J. Mater. Res. 9 (1994) 2490 - 2500. https://doi.org/10.1557/JMR.1994.2490
  78. [80]A.Q. Wang, H.H. Han, M. Li, J.P. Xie, Q.J. Wu, D.Q. Ma, Synthesis and Dispersity of YBCO Powder Produced by Oxalic Acid Precipitation Method. Key Eng. Mater. 645-646 (2015) 145–150. https://doi.org/10.4028/www.scientific.net/KEM.645-646.145

Paper details

vlnc:W_7dt253p6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents