WorksPhysics and Astronomy
A New High - Fraction Polycrystalline Co/Ni Superalloy
Abstract
An ingot-processable Co/Ni-based superalloy has been developed for wrought parts in aircraft engines. An 8.5 kg VIM ingot was homogenised and hot rolled to a true strain of 1. A heat treatment was then developed to produce 50% and a grain size of 142 m. High-temperature tensile testing showed yield strengths of 820 MPa at 700 C, 785 MPa at 800 C and 783 MPa at 850 C. Creep tests at 750 C/600 MPa and 800 C/300 MPa demonstrated reduced minimum creep rates and extended rupture lives relative to current wrought Ni-base alloys. Oxidation at 800 C for 100 h formed a 1 m dual chromia/alumina scale with minimal subsurface degradation. Long-term exposure at 800 C for 8000 h showed limited coarsening and no deleterious intermetallic or grain boundary phases. The alloy therefore offers a promising balance of processability, strength and oxidation resistance for high-temperature static and rotating components.or grain boundary phases. The alloy therefore offers a promising balance of processability, strength and oxidation resistance for high-temperature static and rotating components.
High-temperature static aerospace engine components such as turbine casings must sustain load for extended periods and resist oxidation whilst remaining readily manufacturable [1, 2]. Many wrought Ni-base alloys operate near practical temperature limits in these roles, which subsequently motivates the development of alloys that can retain strength and creep resistance at higher temperature whilst maintaining environmental resistance [3, 4]. These parts are commonly large and axisymmetric, and are well suited to ring roll forging. Ring rolling offers efficient production of large-diameter sections with reduced material waste relative to extensive machining from large forgings or billets [5, 6]. This manufacturing route imposes strict constraints on workability, defect tolerance, and process consistency across large sections.
Co/Ni-based – alloys occupy a useful compositional space for such applications because high fractions support yield strength and creep resistance, while a sufficiently low solvus can provide a wide temperature window for hot working in the region, and suitable Cr/Al levels can support the formation of protective oxide scales during long exposures [3, 7, 8]. At the same time, these objectives are coupled. Increasing fraction and solid-solution strengthening generally raises flow stress and can increase susceptibility to cracking during large-scale deformation [4]. Changes made to improve oxidation resistance can also alter phase stability and grain-boundary chemistry, with consequences for processing and long-term performance. Heat-treatment-controlled grain-boundary morphology can also influence workability; cooling-induced serration improved the hot-compression formability of U720Li [9]. Early V208-family compositions demonstrated promising strength and creep performance, motivating further optimisation of creep resistance, microstructural stability and ingot processability [7, 10, 11].
Alloy design for ring-rolled static components is governed by trade-offs between strengthening, oxidation behaviour, and
environmentally assisted intergranular cracking, whilst avoiding segregation-driven cracking, formation of brittle phases, and grain-boundary damage during prolonged exposure [10, 12, 13]. Al supports formation and can contribute to protective scale development, whilst Cr promotes chromia formation and can slow external and internal oxidation at intermediate temperatures [8, 14]. Refractory additions such as Nb, W and Ta can increase creep resistance through solid-solution strengthening and by modifying partitioning and phase stability; excessive additions can promote unwanted intermetallic phases [13, 15, 16]. Ta, Nb and Ti can modify planar fault energies in , with effects on precipitate shearing that depend on composition and fault type [17]. Minor elements are commonly used to control grain-boundary chemistry and carbide/boride populations, which can improve boundary stability and damage tolerance, but can also degrade boundary performance if phase fraction, morphology, or distribution are not well controlled [10, 12, 18].
The alloy reported here is derived from the V208 family and adjusted to suit ingot-based processing and ring-rolling manufacture whilst targeting higher high-temperature capability [7, 10, 19]. The chemistry is selected to maintain a high fraction, limit segregation sensitivity, and retain oxidation resistance through controlled Cr and Al additions. The alloy is processed through an industrially relevant thermomechanical route and evaluated in terms of microstructural stability, yield strength, creep response under relevant conditions, and oxidation resistance with associated environmental sensitivity at elevated temperature.
An ingot was vacuum induction melted (VIM) at the Royce Facility in Sheffield prior to a multi-stage homogenisation treatment in air (1160 °C for 6 h + 1210 °C for 66 h) based on Thermo-Calc predictions, and then hot rolled at 1220 °C to a total true strain = 1, also at the Royce Facility. The resulting 8.5 kg rolled plate was heat treated at Imperial College to achieve an optimal fraction, distribution and morphology using first a 30 min solution treatment at 1160 °C, followed by cooling at 0.3 °C min through the solvus to 1060 °C where it was held for 30 min. The alloy was then cooled at 60 °C min to 850 °C and aged for 3 h. It was subsequently cooled at 0.3 °C min to 800 °C, held for 2 h, and finally furnace cooled to room temperature. DSC was performed using a Mettler Toledo DSC/TGA 2 to obtain an accurate solvus value and workability range of the alloy. Microstructural analysis was performed using a Tescan Clara scanning electron microscope (SEM); meanwhile TEM for STEM-EDX was performed on a Thermo-Fisher Spectra operating at 300 kV. Creep tests were conducted in tension at 750 °C under a 600 MPa load and at 800 °C under a 300 MPa load. Slow strain-rate tensile testing was carried out at 800 °C in vacuum and air at a strain rate of s on a Zwick-Roell testing frame fitted with a 5 kN load cell, and all other tensile tests performed at a strain rate of s from room temperature up to temperatures of 850 °C. Oxidation tests were performed on specimens measuring 10 mm × 10 mm × 2 mm, ground and polished by standard metallographic procedure, and oxidised at 800 °C for 100 h in static air. Long term stability was examined after exposure at 800 °C for 8000 h in air.
Table 1. Nominal alloy compositions in at.%
The fully heat-treated microstructure of the investigated alloy is shown in Figure 1a-Figure 1c in addition to the long term stability shown in Figure 1d. The alloy shows a uniform grain distribution with an average grain size of 142 µm. This is important for an ingot-route alloy of this chemistry: as-cast microsegregation in heavily alloyed systems can produce interdendritic regions susceptible to incipient melting during overly aggressive homogenisation [21, 22]. BSE imaging of the finalised microstructure showing homogeneous grain distribution. In-column backscattered SEM imaging, Figure 1c, reveals a microstructure characterised by grain boundary primary , relatively large ogdoadically diced secondary intragranular precipitates and a finer dispersion of tertiary , defined by its size being under 50 nm. The secondary phase exhibits a faceted, segmented appearance, where individual cubes appear subdivided into smaller units by internal contrast, giving rise to the ogdoadically diced morphology. Split cuboidal morphologies, including eight-cuboid configurations, have previously been documented in Ni-based alloys [23]. The tertiary is more uniform and spherical and occupies the channels between the larger precipitates, contributing to the overall high fraction. The development of distinct secondary and tertiary populations is consistent with the sensitivity of precipitate size distributions to cooling history reported in Ni-based superalloys [24]. A total fraction of 50% is achieved with a tertiary fraction of approximately 10%. The fraction was calculated using the Blavette method from atom probe tomography needles [25, 26].

Figure 1. SEM and EBSD characterisation of the heat-treated Alloy 5 microstructure. (a) Backscattered-electron SEM image showing the recrystallised grain structure, (b) EBSD inverse pole figure map, (c) in-lens SEM image showing the precipitate distribution, (d) In-Lens Backscatter image after 8000 h showing the long term stability of the alloy. (e) and (f) APT needles and 1D concentration profile showing the phase composition and partitioning of analysed ions
DSC results show a solvus of 1110 °C with solidus temperature of 1250 °C. This results in a wide processing window for thermomechanical processing such as ring rolling: the alloy can be homogenised and worked in air at temperatures that are high enough to reduce flow stresses and promote dynamic recovery, and below the measured bulk solidus. Local incipient-melting temperatures in segregated regions must nevertheless be considered when selecting a homogenisation schedule. Local melting of MB borides has also been directly linked to intergranular cracking during hot compression of a Ni-based superalloy with elevated B and C contents [27]. At the same time, the solvus is positioned such that a high retained fraction is present at the service relevant temperatures, rather than collapsing the ordered phase fraction during operation. At the same time, the alloy is stable against intermetallic phase formation after long exposures, such as , shown in Figure 1d.
APT was used to analyse the phase composition and partitioning behaviour, with typical Ni/Co-base partitioning displayed, Figure 1e-Figure 1f. As expected formers such as Al, Ni, Ti and Nb partition strongly, while formers in Ni-base systems such as Cr, Co and Mo partition accordingly. However, there is still a relatively large amount of Co within the phase, in addition to slight partitioning of W to the phase. This highlights a phenomenon seen in Ni/Co-based systems where the (Co,Ni)(Al, W) phase is precipitated [7, 28]. W additions can modify coarsening through changes in phase chemistry and diffusion kinetics; however, W partitioning alone does not establish the rate-controlling species in the present alloy [29]. In addition, no deleterious phases such as are observed at the grain boundaries or within the grain interiors.
Grain boundaries are decorated with intergranular secondary and exhibit pronounced serration, as also reported in slowly cooled V208-derived Co/Ni alloys [10]. In Ni-based superalloys, serrated grain-boundaries have been associated with improved creep rupture lives and improved resistance to time-dependent intergranular crack growth, although these depend on testing conditions [30, 31]. The volume fraction is higher than in most wrought Ni-based superalloys, and comparable to high- wrought alloys, while retaining the hot-rolling capability [1, 4]. Compared with conventional casing alloys, the fraction of ordered phase is significantly higher, moving the design closer to disc-like chemistries. The density of the alloy (8.39 g cm) lies slightly above that of typical Ni-base casing alloys but below many Co-rich alloys, so the penalty in specific strength is limited. Taken together, the microstructural observations and phase stability measurements suggest that the alloy occupies a useful intermediate space between powder Co/Ni superalloys and traditional wrought Ni-base alloys.
Tensile results shown in Figure 2 show that, despite the larger grain size, the presented alloy achieves yield strengths comparable or exceeding commercial wrought Ni-base superalloys across the temperature range investigated [32, 33]. The alloy exhibits a room-temperature 0.2% proof stress of 920 MPa, decreasing to 820 MPa at 700 °C and 783 MPa at 850 °C. At elevated temperature, the 0.2% proof stress remains competitive with Waspaloy in its fine-grained state ASTM 6-8, demonstrating that the high fraction provides effective strengthening without preventing ingot processing and hot rolling. The retained strength is consistent with the high volume fraction, refractory-element partitioning and the serrated grain-boundary microstructure developed during heat treatment.

Figure 2. Alloy 5 stress–strain curves at , including 800 °C air/vacuum tests at , and 0.2% proof stress compared with Waspaloy datasets A and B.
| Element | Partitioning | |||
| Ni | 38.0 | 63.0 | 1.6 | |
| Al | 2.4 | 16.0 | 6.5 | |
| Ti | 0.1 | 1.9 | 18 | |
| Ta | 0.1 | 1.3 | 14 | |
| W | 0.6 | 1.1 | 1.9 | |
| Nb | 0.1 | 0.7 | 9.2 | |
| Co | 33.0 | 12.5 | 0.4 | |
| Cr | 22.0 | 2.2 | 0.1 | |
| Mo | 2.1 | 0.9 | 0.41 |
Table 2. APT-derived phase compositions and partitioning behaviour between the and phases in the heat-treated alloy.
Slow strain rate tensile testing at 800 °C, shown in Figure 2, was used to assess susceptibility to environmentally assisted intergranular cracking, following the approach of Gabb et al. [34]. Comparative tests performed in vacuum and in air assess the effect of oxidation-assisted damage. The reduction in ductility in air indicates some environmental sensitivity at 800 °C. These monotonic tests do not directly measure fatigue crack-growth resistance. Grain-boundary and boundary chemistry can influence oxygen-assisted damage, but a protective mechanism cannot be inferred from the tensile response alone [35].
Creep testing shown in Figure 3 demonstrates that Alloy 5 provides better creep resistance than the comparison Ni-base alloys in its current configuration [11, 20, 32, 36, 37]. The measured minimum creep rates were approximately and , respectively. At all conditions, the alloy exhibits good minimum creep rates and longer rupture lives than RR1000, Udimet 720Li and Waspaloy under comparable testing conditions. This improved creep response is attributed to the combined effect of the high fraction, large grain size, grain-boundary serration and refractory-element additions. The high fraction provides resistance to dislocation motion within the grains, while serrated grain boundaries are expected to reduce grain-boundary sliding and delay intergranular damage. Refractory additions such as Mo may also contribute through matrix solid-solution strengthening [15]. Overall, the mechanical data show that Alloy 5 combines competitive tensile strength with improved creep resistance and acceptable environmental tolerance at 800 °C, supporting its potential use in static aerospace components.

Figure 3. Larson–Miller comparison of Alloy 5 creep rupture behaviour against Ni-base reference alloys and associated creep curves for reported tests.
The oxidation response of Alloy 5 after exposure at 800 °C for 100 h is summarised in Figure 4. Cross-sectional STEM–EDX shows a thin external oxide scale, approximately 1 μm thick, with a Cr-rich outer region and Al enrichment towards the metal/oxide interface. Ti and Ta, which partition to in the unoxidised alloy, are also locally enriched within the scale. Their presence indicates redistribution of these additions during oxidation, although elemental enrichment alone does not establish the formation of separate oxide phases. This layered chemistry is consistent with the chromia/alumina-based oxidation response reported for a related wrought Co/Ni-based alloy, for which the time-dependent scale evolution and elemental redistribution have been examined in detail [38].

Figure 4. Cross-sectional STEM–EDX analysis of Alloy 5 after oxidation at 800 °C for 100 h. (a) HAADF image and (b–d) elemental maps showing the distribution of the principal oxide-forming elements. HAADF image from [38].
The formation of a thin Cr/Al-rich oxide scale is an important result for a Co/Ni-based alloy. Early Co-rich systems were often limited by rapid growth of thick, non-protective cobalt oxides, which restricted their environmental capability despite promising high-temperature strength [39].
In the present alloy, the balanced Co/Ni chemistry, together with controlled Cr and Al additions, suppresses the formation of a thick Co-rich external scale and instead promotes a more protective chromia/alumina-containing oxide, consistent with composition-dependent oxidation trends in Co/Ni alloys [8, 38, 40]. The Cr-rich outer scale is consistent with a barrier to rapid oxidation, while Al enrichment at the metal/oxide interface is consistent with an alumina subscale; the continuity and transport properties of that subscale are not established by elemental maps alone [38, 41].
Beneath the oxide, the microstructure remains largely intact after 100 h at 800 °C. No extensive internal oxidation, deep grain-boundary oxide penetration or large-scale dissolution of the strengthening microstructure is observed over the timescale examined. This is significant because the alloy is designed for static aero-engine components where environmental resistance must be retained alongside creep strength. The limited subsurface degradation observed here indicates that the oxidation response does not rapidly compromise the near-surface microstructure under the present exposure condition [38].
The oxidation data therefore complement the mechanical results by demonstrating that the alloy retains environmental resistance at a temperature relevant to the targeted application. Together with the tensile and creep behaviour, the formation of a thin chromia/alumina-containing scale at 800 °C supports the broader alloy-design objective: an ingot-processable Co/Ni-based superalloy that combines high-temperature mechanical capability with oxidation resistance suitable for static aero-engine components.
In summary, a novel ingot-processable Co/Ni-based – strengthened superalloy has been developed for high-temperature static aero-engine applications. The alloy was produced by VIM, homogenised, hot rolled to a true strain of 1 and heat treated to generate a stable microstructure containing approximately 50% , including approximately 10% tertiary , segmented secondary precipitates and serrated, -decorated grain boundaries.
DSC measurements show a solvus of 1110 °C, with solidus temperature of 1250 °C, providing a wide processing window for ingot processing and ring rolling. The heat-treated alloy exhibits yield strengths comparable to, or higher than, established wrought Ni-base superalloys such as RR1000, Udimet 720Li and Waspaloy, while creep testing at 750 °C/600 MPa and 800 °C/300 MPa demonstrates lower minimum creep rates and longer rupture lives than these reference alloys. Further improvements in yield strength are expected through grain refinement via Hall–Petch strengthening and optimisation of the size distribution, particularly the large intragranular secondary precipitates. Oxidation at 800 °C for 100 h produces a thin Cr/Al-rich protective scale, approximately 1 µm in thickness, with limited subsurface degradation, and long-term exposure at 800 °C for 8000 h shows limited coarsening and no deleterious grain-boundary phases. These results show that Alloy 5 offers a promising balance of processability, microstructural stability, creep strength and oxidation resistance for ingot-processed polycrystalline aero-engine components operating at elevated temperature.
Acknowledgements
The authors would like to acknowledge support from Rolls-Royce plc for their continued support and funding. MC acknowledges funding from Royal Society Tata University Research Fellowship URF/R1/201318, Royal Society Enhancement Award RF/ERE/210200EM1, and ERC CoG DISCO grant 101171966.
References
- [1]R.C. Reed, The Superalloys: Fundamentals and Applications, Cambridge University Press, 2006.
- [2]T.M. Pollock, S. Tin, J. Propuls. Power 22 (2006) 361–374.
- [3]S. Neumeier, L.P. Freund, M. Göken, Scr. Mater. 109 (2015) 104–107.
- [4]S. Neumeier et al., Metall. Mater. Trans. A 55 (2024) 1319–1337.
- [5]J.M. Allwood, A.E. Tekkaya, T.F. Stanisatreit, Steel Res. Int. 76 (2005) 111–120.
- [6]T.F. Stanistreet, J.M. Allwood, A.M. Willoughby, J. Mater. Process. Technol. 177 (2006) 630–633.
- [7]M. Knop et al., JOM 66 (2014) 2495–2501.
- [8]F.B. Ismail et al., Corros. Sci. 116 (2017) 44–52.
- [9]T.-W. Chen et al., J. Alloys Compd. 960 (2023) 170620.
- [10]T.P. McAuliffe et al., Metall. Mater. Trans. A 52 (2021) 1649–1664.
- [11]V.A. Vorontsov et al., Acta Mater. 232 (2022) 117936.
- [12]P. Kontis et al., Acta Mater. 103 (2016) 688–699.
- [13]Z. Fan et al., Metall. Mater. Trans. A 51 (2020) 2495–2508.
- [14]J.W.X. Wo, M.C. Hardy, H.J. Stone, High Temp. Corros. Mater. 100 (2023) 85–108.
- [15]E. Fleischmann et al., Acta Mater. 87 (2015) 350–356.
- [16]M.T. Lapington et al., Metall. Mater. Trans. A 49 (2018) 2302–2310.
- [17]K. Kumar, R. Sankarasubramanian, U.V. Waghmare, Scr. Mater. 142 (2018) 74–78.
- [18]H.-Y. Yan, V.A. Vorontsov, D. Dye, Intermetallics 48 (2014) 44–53.
- [19]M.C. Hardy et al., Alloy, U.S. Patent US11898228B2, granted 13 February 2024, assignee: Rolls-Royce plc (2024).
- [20]K.A. Christofidou et al., Metall. Mater. Trans. A 49 (2018) 3896–3907.
- [21]P.D. Jablonski, C.J. Cowen, Metall. Mater. Trans. B 40 (2009) 182–186.
- [22]H.T. Pang et al., Metall. Mater. Trans. A 47 (2016) 889–906.
- [23]M. Doi, T. Miyazaki, in: Superalloys 1984, The Metallurgical Society of AIME, 1984, pp. 543–552.
- [24]Y.Q. Chen et al., Acta Mater. 85 (2015) 199–206.
- [25]D. Blavette, P. Caron, T. Khan, in: S. Reichman et al. (Eds.), Superalloys 1988, The Metallurgical Society, 1988, pp. 305–314.
- [26]D. Blavette, E. Cadel, B. Deconihout, Mater. Charact. 44 (2000) 133–157.
- [27]B. Schulz, T. Leitner, S. Primig, J. Alloys Compd. 956 (2023) 170324.
- [28]K. Shinagawa et al., Mater. Trans. 49 (2008) 1474–1479.
- [29]N. Baler et al., Materialia 10 (2020) 100632.
- [30]H.U. Hong et al., Mater. Sci. Eng. A 517 (2009) 125–131.
- [31]Y.T. Tang, A.J. Wilkinson, R.C. Reed, Metall. Mater. Trans. A 49 (2018) 4324–4342.
- [32]Special Metals Corporation, Waspaloy, Tech. Rep. SMC-011, Special Metals Corporation (Sep. 2004).
- [33]K.A. Heck et al., in: Superalloys 2020, Springer, Cham, 2020, pp. 142–152.
- [34]T.P. Gabb et al., in: 8th International Symposium on Superalloy 718 and Derivatives, John Wiley & Sons, 2014, pp. 697–712.
- [35]A.A.N. Németh et al., Acta Mater. 126 (2017) 361–371.
- [36]Y.F. Gu et al., Mater. Sci. Eng. A 510–511 (2009) 250–255.
- [37]T.P. Gabb et al., Characterization of the Temperature Capabilities of Advanced Disk Alloy ME3, Tech. Rep. NASA/TM-2002-211796, National Aeronautics and Space Administration (2002).
- [38]C. Crabb et al., Adv. Eng. Mater. 28 (2026) e202503059.
- [39]L. Klein et al., Corros. Sci. 53 (2011) 2027–2034.
- [40]L. Li et al., Mater. Des. 224 (2022) 111291.
- [41]J.W.X. Wo, M.C. Hardy, H.J. Stone, High Temp. Corros. Mater. 101 (2024) 485–509.