Finite-width adiabatic shear banding and dislocation patterning in mesoscale polycrystalline aggregates

Abstract

Dynamic shear banding under adiabatic conditions in a mesoscale polycrystalline aggregate is studied using a model of mesoscale dislocation mechanics and experiments. The model involves a length scale related to hardening induced by excess/polar/geometrically necessary dislocation (GND) density, and utilizes a simple classical crystal plasticity model with isotropic Voce law hardening. Simulations of statistically representative volume elements of a polycrystal determined from experimental samples are conducted. Studies in 2-d (section) and 3-d capture the experimentally observed finite-width shear bands and the formation of low-angle subgrain boundaries even in the absence of heat conduction in the model, as well as size-dependent strengthening for grain sizes from 1 to 20 μμm. The 2-d and large-scale 3-d simulations, the latter involving 1 million finite elements, provide access to the progressive evolution of material strength, stress state, and temperature in the course of large deformations. GND distributions accumulate at grain boundaries and form patterned structures within grain interiors, offering insight into the microstructural changes that precede failure in adiabatic shear bands. Mesh-converged, delocalized and localized plastic flow to very large deformations without softening is observed for a significant range of parameters, reflecting a competition between GND hardening and thermal softening in setting the non-softening steady state in the absence of other ductile damage mechanisms in the model.

Introduction

Adiabatic shear bands are a critical damage and failure mechanism in microstructural metals subjected to high-strain-rate loading [35, 36, 37, 97]. In applications involving impact, ballistic penetration, high-speed machining, and crash worthiness, deformation occurs rapidly enough that heat generated by plastic work cannot diffuse away from the deforming region. Under these adiabatic conditions, thermal and recrystallization softening competes with strain and strain-rate hardening, resulting in the localization of deformation into narrow bands that often serve as precursors to fracture. Experiments reveal that these bands have a finite width and are accompanied by significant microstructural changes, including grain refinement and subgrain formation [37, 69, 40, 53, 54, 71, 72, 73]. Understanding the formation and microstructural evolution of these adiabatic shear bands is therefore essential for predicting material performance under conditions of dynamic loading.

The Split Hopkinson Pressure Bar (SHPB) has long served as the standard experimental technique for characterizing material response at strain rates of 10210^{2} to 104 s−110^{4}\ s^{-1} [83]. Stress wave measurements in the input and output bars provide well-characterized loading conditions, and make SHPB experiments particularly suitable for studying shear band formation in a controlled and repeatable setting. When combined with the top-hat specimen geometry, which concentrates shear deformation within a narrow section of the sample by design, the technique enables localization to occur in a predetermined region. It also produces a nominally shear deformation state that isolates shear band behavior from competing deformation and damage modes [52, 70, 101, 100, 20, 21, 24].

However, post-mortem analysis reveals only the final microstructure, not the path that led to it. The progressive evolution of internal fields, from the onset of plastic instability to the formation of a mature shear band, remains inaccessible by experiment. Physical theory and simulation can address this gap by providing access to the full spatiotemporal evolution of these fields, while boundary conditions informed by experimental measurements enable validation against experimental observables.

Early observations and understanding of shear bands under adiabatic dynamic conditions are due to Zener and Holloman [106]. The early theoretical foundations for understanding shear band formation under dynamic loading were established through linear stability and perturbation analyses [16, 17, 25, 29, 96, 9], which identified the competition between strain-rate hardening, thermal softening, and inertia as the governing factors. In [47], Fressengeas and Molinari developed a modified linear stability approach using relative perturbations (absolute perturbations normalized by homogeneous solutions), demonstrating better agreement with nonlinear results. Fully nonlinear numerical simulations extended these insights beyond the linear regime [95, 98, 75, 86, 48]. Shawki and coworkers [87, 88] developed energy-based criteria demonstrating that localization onset is controlled primarily by inertial forces. Early analytical work by Dodd and Bai [35] established that the shear band width is governed by the thermal length scale introduced through heat conduction, demonstrated later in computations by [33]. In a complementary line of work primarily in the quasi-static setting, Aifantis and Zbib [8, 102, 103, 104] introduced strain gradients into the flow stress, with an associated length-scale required on dimensional grounds, and showed, through linear stability and nonlinear analyses, that this modification regularizes the localization problem and sets the shear band width. Comprehensive reviews of these early foundational works can be found in [87], [97], and [36]. More recent work has suggested a potential role of significant structural evolution within the material leading to adiabatic shear band formation and maturation [56, 64, 61, 62, 31, 30, 32]. Substantial questions remain about material structural evolution at high deformation rates related to adiabatic shear banding and experimental observations.

More recent computational efforts have employed crystal plasticity frameworks to capture microstructural influences on shear band formation [99, 55, 19]. These studies have shown that shear bands can initiate near triple junctions and propagate across grain boundaries, and that texture evolution plays a critical role in localization. However, conventional crystal plasticity theories do not incorporate an intrinsic material length scale and thus cannot capture experimentally observed size-dependent strengthening at the micron scale and below. Various gradient plasticity theories [46, 50, 42, 60] have been proposed to address this limitation which is also expected to affect the prediction of experimentally observed finite width of shear bands. However, an assessment of such models reveals that fundamental issues remain [67, 3], even apart from representing a physically direct association of the gradient effect with the mechanics of dislocation distributions. In the context of shear banding, Kuroda and Needleman [58] have studied higher-order gradient crystal plasticity in the context of dynamic tensile loading of planar single crystals, showing that the interaction between an inertia-induced length scale and the intrinsic material length scale can produce non-monotonic transitions in the localization mode with specimen size, and that the gradient theory regularizes shear band development.

Mesoscale Field Dislocation Mechanics (MFDM) [12, 7] offers an alternative that incorporates an intrinsic length scale through the work-hardening response of the material. That physical description requires the (magnitude of the) Burgers vector to enter into a coefficient that mediates the hardening produced due to geometrically necessary dislocations (GNDs), adapting the works of [68, 43, 5] to the setting of MFDM. The theory/model also accounts for the stress fields of GNDs and their spatiotemporal evolution. MFDM has successfully captured size effects in constrained shearing [81, 79, 2, 14], orientation-dependent behavior in micropillars [3], and kink band formation in nanometallic laminates [4]. Finite-width localization, size-dependent strengthening, and dislocation-driven microstructural evolution are desirable attributes for the study of adiabatic shear band formation and structural evolution at the mesoscale.

In this work, we employ a finite deformation version of Reduced MFDM (RMFDM), first introduced for quasi-static, small deformation analysis in [84] and implemented using the Fast Fourier Transform in [38, 27, 28] for large polycrystalline assemblies. Here, we extend RMFDM to the finite deformation, dynamic setting, with a reformulation specifically designed for phenomena with finite propagation speeds. A particular feature is the discretization of the convected derivative of the evolution of elastic distortion in a structure-preserving manner. While this implementation maintains theoretical equivalence to the version used in [14], it is numerically distinct. We calibrate the model against SHPB experiments on a quenched and tempered low-carbon steel and simulate shear band formation in representative volume elements spanning the shear band region. The simulations capture the experimentally observed finite widths of shear bands. They also display size-dependent strengthening for grain sizes from 1 to 20 μm\mu\mathrm{m}, and the formation of low-angle subgrain boundaries, the latter also observed in experiments [51] and the ones performed in this work.

In the absence of direct experimental evidence of time-dependent evolution at the length and time scales involved for comparison (as well as the controlled boundary conditions facilitated in simulation), the simulations provide insight into the progressive evolution of GND density, material strength, stress state, and temperature within the specific model employed. This work is complementary to that of [82], also concerned with the study of dynamic, adiabatic shear banding modeled at the full macroscopic sample level, without explicit consideration of a polycrystalline aggregate and associated crystal mechanics.

The rest of this Section contains some notational details and terminology used in this work. Notation and terminology: Vectors and tensors are represented by boldface lower and upper-case letters. The action of a second order tensor A\mathbf{A} on a vector b\mathbf{b} is denoted by Ab\mathbf{A}\mathbf{b}. The inner product of two vectors is denoted by a⋅b\mathbf{a}\cdot\mathbf{b}, while the inner product of two-second order tensors is denoted by A:B\mathbf{A}:\mathbf{B}. A rectangular Cartesian coordinate system is invoked for ambient space and all (vector) tensor components are expressed with respect to the basis of this coordinate system. (⋅),i(\cdot)_{,i} denotes the partial derivative of the quantity (⋅)(\cdot) w.r.t. the xix_i coordinate of this coordinate system. $\mathbf{e}_i denotes the unit vector in the xix_i direction. The time derivative of a quantity is denoted by (⋅)˙\dot{(\cdot)}. Einstein’s summation convention is always implied unless mentioned otherwise. The symbols grad, div, and curl denote the gradient, divergence, and curl on the current configuration. For a second order tensor A\boldsymbol{A}, vectors v\boldsymbol{v}, a\boldsymbol{a}, and c\boldsymbol{c}, a spatially constant vector field b\boldsymbol{b}, the operations of div, curl, and cross-product of a tensor (×\times) with a vector are defined as follows:

(div⁡A)⋅b=div⁡(ATb),∀ b(\operatorname{div}\boldsymbol{A})\cdot\boldsymbol{b}=\operatorname{div}(\boldsymbol{A}^{T}\boldsymbol{b}), \qquad\forall\ \boldsymbol{b}
b⋅(curl⁡A)c=[curl⁡(ATb)]⋅c,∀ b,c\boldsymbol{b}\cdot(\operatorname{curl}\boldsymbol{A})\boldsymbol{c}=[\operatorname{curl}(\boldsymbol{A}^{T}\boldsymbol{b})]\cdot\boldsymbol{c}, \qquad\forall\ \boldsymbol{b},\boldsymbol{c}
c⋅(A×v)a=[(ATc)×v]⋅a,∀ a,c.\boldsymbol{c}\cdot(\boldsymbol{A}\times\boldsymbol{v})\boldsymbol{a}=[(\boldsymbol{A}^{T}\boldsymbol{c})\times\boldsymbol{v}]\cdot\boldsymbol{a}, \qquad\forall\ \boldsymbol{a},\boldsymbol{c}.

In rectangular Cartesian coordinates, these are denoted by

(div⁡A)i=Aij,j,(curl⁡A)ri=ϵijkArk,j,(A×v)ri=ϵijkArjvk,(\operatorname{div}\boldsymbol{A})_i=A_{ij,j}, \qquad(\operatorname{curl}\boldsymbol{A})_{ri}=\epsilon_{ijk}A_{rk,j}, \qquad(\boldsymbol{A}\times\boldsymbol{v})_{ri}=\epsilon_{ijk}A_{rj}v_k,

where ϵijk\epsilon_{ijk} are the components of the third order alternating tensor X\boldsymbol{X}.

All strain measures used in discussion of results refer to nominal strain.

Localization: In this work we will identify a region as strain-localized when a context-dependent measure of deformation in that region exceeds the average of the same measure over the complement of the region in the domain by a factor of approximately three or more.

Convergence: The term convergence will be used predominantly in the context of convergence of simulation results w.r.t. mesh refinement. The usage will not be in a strict mathematical sense utilizing a norm(s), but in an approximate physical sense allowing for deviations deemed reasonable, given the large magnitudes and high rates of deformation involved.

Theory

We present the governing equations for finite deformation MFDM (3) and Reduced MFDM (RMFDM) (4).

α˙≡(div⁡v)α+α˙−αLT=−curl⁡(α×V+Lp)(1)\dot{\boldsymbol{\alpha}}\equiv(\operatorname{div}\boldsymbol{v})\boldsymbol{\alpha}+\dot{\boldsymbol{\alpha}}-\boldsymbol{\alpha}\boldsymbol{L}^{T}=-\operatorname{curl}(\boldsymbol{\alpha}\times\boldsymbol{V}+\boldsymbol{L}^{p}) \tag*{(1)}
W=χ+grad⁡f,Fe=W−1curl⁡χ=−αdiv⁡χ=0(2)\begin{aligned} \boldsymbol{W}&=\boldsymbol{\chi}+\operatorname{grad}\boldsymbol{f}, \qquad\boldsymbol{F}^{e}=\boldsymbol{W}^{-1}\\ \operatorname{curl}\boldsymbol{\chi}&=-\boldsymbol{\alpha}\\ \operatorname{div}\boldsymbol{\chi}&=0 \tag*{(2)} \end{aligned}
div⁡(grad⁡f˙)=div⁡(α×V+Lp−χ˙−χL)(3)\operatorname{div}\left(\operatorname{grad}\dot{\boldsymbol{f}}\right)=\operatorname{div}\left(\boldsymbol{\alpha}\times\boldsymbol{V}+\boldsymbol{L}^{p}-\dot{\boldsymbol{\chi}}-\boldsymbol{\chi}\boldsymbol{L}\right) \tag*{(3)}
div⁡[T(W)]=ρv˙(4)\operatorname{div}[\boldsymbol{T}(\boldsymbol{W})]=\rho\dot{\boldsymbol{v}} \tag*{(4)}
α˙≡(div⁡v)α+α˙−αLT=−curl⁡(α×V+Lp)(5)\dot{\boldsymbol{\alpha}}\equiv(\operatorname{div}\boldsymbol{v})\boldsymbol{\alpha}+\dot{\boldsymbol{\alpha}}-\boldsymbol{\alpha}\boldsymbol{L}^{T}=-\operatorname{curl}(\boldsymbol{\alpha}\times\boldsymbol{V}+\boldsymbol{L}^{p}) \tag*{(5)}
Fe=W−1(6)\boldsymbol{F}^{e}=\boldsymbol{W}^{-1} \tag*{(6)}
W˙+WL=α×V+Lp(7)\dot{\boldsymbol{W}}+\boldsymbol{W}\boldsymbol{L}=\boldsymbol{\alpha}\times\boldsymbol{V}+\boldsymbol{L}^{p} \tag*{(7)}
div⁡[T(W)]=ρv˙(8)\operatorname{div}[\boldsymbol{T}(\boldsymbol{W})]=\rho\dot{\boldsymbol{v}} \tag*{(8)}

Here, W\boldsymbol{W} denotes the inverse of the elastic distortion tensor Fe\boldsymbol{F}^{e}, decomposed in MFDM into an incompatible part χ\boldsymbol{\chi} and a compatible part grad⁡f\operatorname{grad}\boldsymbol{f}, where f\boldsymbol{f} is the plastic position vector. The tensor α\boldsymbol{\alpha} represents the dislocation density, v\boldsymbol{v} is the material velocity with velocity gradient L=grad⁡v\boldsymbol{L}=\operatorname{grad}\boldsymbol{v}, and T\mathbf{T} is the symmetric Cauchy stress. The mass density is denoted by ρ\rho, and V\mathbf{V} represents the dislocation density field. All fields in the MFDM system are understood as space-time running averages of their counterparts in the underlying FDM theory [1]. The field Lp\mathbf{L}^{p}, the plastic strain rate produced by statistical dislocations (SD), captures the averaged plastic straining rate arising from dislocations not resolved by the GND/Excess dislocation density, as discussed in [1 Sec. 3]. The plastic strain rate of the GND density is given by α×V\boldsymbol{\alpha} \times\mathbf{V}.

The systems (3)-(4), in principle, are two theoretically equivalent forms of MFDM theory as discussed in [7 App. B]. The alternate forms result from how the evolution of the inverse elastic distortion W\mathbf{W} is described. In the context of numerical algorithms, (3) is better suited for situations where quasi-static balance of linear momentum is a good idealization. Here, the elastic stress field of a dislocation density distribution is subject to ‘instantaneous propagation’ throughout the domain. Under dynamic balance of linear momentum without ignoring inertia, this is not true, and (4) is better suited for numerical computation of finite speed of propagation phenomena. On the other hand, unlike MFDM, it does not allow the calculation of the elastic distortion field consistent with a prescribed GND tensor field, see (3b) above. It is the form (4) of the MFDM that we adopt in this work, which entails the use of a slightly different algorithm than the one described in [14]. As noted in the introduction, RMFDM was first employed for quasi-static, small deformation analysis in [84]; here we extend its use to the finite deformation and dynamic settings. Separately, an FFT-based implementation of RMFDM has been applied in [38, 27, 28] to study large polycrystalline assemblies under quasi-static conditions.

MFDM requires constitutive statements for the stress T\mathbf{T}, the plastic distortion rate Lp\mathbf{L}^{p}, and the dislocation velocity V\mathbf{V}. The details of the thermodynamically consistent constitutive formulations are presented in [14]. To complete the systems of equations, boundary conditions are required for α\boldsymbol{\alpha}, v\mathbf{v} and initial conditions for α\boldsymbol{\alpha}, v\mathbf{v}, W\mathbf{W}, and the motion map. The constitutive equations for the theory are given in Table 1-Table 3 below.

Saint-Venant-Kirchhoff Materialϕ(W)=12ρ∗Ee:C:Ee,T=Fe[C:Ee]FeT\phi(\mathbf{W}) = \frac{1}{2\rho^{*}}\mathbf{E}^{e}:\mathbf{C}:\mathbf{E}^{e},\quad\mathbf{T}=\mathbf{F}^{e}[\mathbf{C}:\mathbf{E}^{e}]\mathbf{F}^{eT}
Core energy densityΥ(α)=12ρ∗ϵα:α\Upsilon(\boldsymbol{\alpha})=\frac{1}{2\rho^{*}}\boldsymbol{\epsilon}\boldsymbol{\alpha}:\boldsymbol{\alpha}

Table 1. Constitutive relations for Cauchy stress and core energy density.

g˙=h(α,g)(∣Feα×V∣+∑knsl∣γ^k∣)\dot{g}=h(\boldsymbol{\alpha},g)\left(|\mathbf{F}^{e}\boldsymbol{\alpha}\times\mathbf{V}|+\sum_{k}^{n_{\mathrm{sl}}}|\hat{\gamma}^{k}|\right)h(α,g)={μ2η2b2(g−g0)k0∣α∣+h0(gs−ggs−g0),g0≤g≤gsμ2η2b2(g−g0)k0∣α∣,g>gsh(\boldsymbol{\alpha},g)=\begin{cases}\dfrac{\mu^{2}\eta^{2}b}{2(g-g_{0})}k_{0}|\boldsymbol{\alpha}|+h_{0}\left(\dfrac{g_{s}-g}{g_{s}-g_{0}}\right), & g_{0}\leq g\leq g_{s}\\ \dfrac{\mu^{2}\eta^{2}b}{2(g-g_{0})}k_{0}|\boldsymbol{\alpha}|, & g>g_{s}\end{cases}

Table 3. Constitutive relations for material strength gg.

Boundary conditions

  • The α\boldsymbol{\alpha} evolution equation needs a convective boundary condition of the form (α×V+Lp)×n=Φ(\boldsymbol{\alpha} \times\mathbf{V} + \mathbf{L}^{p}) \times\mathbf{n} = \boldsymbol{\Phi}, where Φ\boldsymbol{\Phi} is a second order tensor valued function. Φ\boldsymbol{\Phi} is a function of time and position on the boundary. It characterizes the flux of dislocations at the surface, defined by outward unit normal field n\mathbf{n}, satisfying the constraint Φn=0\boldsymbol{\Phi}\mathbf{n} = \mathbf{0}.

    The following boundary conditions are valid for the evolution of α\boldsymbol{\alpha}:

    • Constrained: This condition applies, Φ(x,t)=0\boldsymbol{\Phi}(\mathbf{x},t) = \mathbf{0} at a point x\mathbf{x} on the boundary, for all times. This restricts movement of the dislocations at the external boundary to just be tangential, along with making sure that no dislocation is exiting the body. This makes the boundary plastically constrained, and hence referred to as no-slip or rigid boundary condition.

    • Unconstrained: Specification of dislocation flux α(V⋅n)\boldsymbol{\alpha}(\mathbf{V}\cdot\mathbf{n}) on the inflow part of the boundary, along with L^p×n\hat{\mathbf{L}}^{p}\times\mathbf{n} simply evaluated at the boundary, can be used as a less restrictive boundary condition. The quantity (curl⁡α)×n(\operatorname{curl}\boldsymbol{\alpha})\times\mathbf{n} is imposed to be zero for all the calculations in this project.

  • Based on the problem of interest, the material velocity boundary conditions are applied.

Constitutive relations

In the MFDM framework, constitutive relations are required for the stress T\mathbf{T}, the plastic distortion rate Lp\mathbf{L}^{p}, and the dislocation velocity V\mathbf{V}. The thermodynamically consistent formulations of these constitutive relations are detailed in Sec. 3.1 of [2]. The constitutive relation for the Cauchy stress and mesoscopic core energy density is summarized in Table 1. Additionally, Table 2 and 4 outline the constitutive relations for the SD plastic distortion rate, Lp\mathbf{L}^{p}, and GND dislocation velocity, V\mathbf{V}, respectively. The evolution equation for material strength is provided in Table 3, building on the work [5].

J2J_{2} plasticityL^p=γ^WT′∣T′∣;γ^=γ^0(∣T′∣2gθ)1m\hat{\mathbf{L}}^{p}=\hat{\gamma}\mathbf{W}\frac{\mathbf{T}^{\prime}}{|\mathbf{T}^{\prime}|};\quad\hat{\gamma}=\hat{\gamma}_{0}\left(\frac{|\mathbf{T}^{\prime}|}{\sqrt{2}g_{\theta}}\right)^{\frac{1}{m}}<br>Lp=L^p+l2γ^curl⁡α\mathbf{L}^{p}=\hat{\mathbf{L}}^{p}+l^{2}\hat{\gamma}\operatorname{curl}\boldsymbol{\alpha}
Crystal plasticityL^p=W(∑knslγ^kmk⊗nk)sum\hat{\mathbf{L}}^{p}=\mathbf{W}\left(\sum_{k}^{n_{\mathrm{sl}}}\hat{\gamma}^{k}\mathbf{m}^{k}\otimes\mathbf{n}^{k}\right)_{\mathrm{sum}}<br>Lp=L^p+(l2nsl∑knsl∣γ^k∣)curl⁡α\mathbf{L}^{p}=\hat{\mathbf{L}}^{p}+\left(\frac{l^{2}}{n_{\mathrm{sl}}}\sum_{k}^{n_{\mathrm{sl}}}|\hat{\gamma}^{k}|\right)\operatorname{curl}\boldsymbol{\alpha}<br>γ^k=sgn⁡(τk)γ^0(∣τk∣gθ)1m\hat{\gamma}^{k}=\operatorname{sgn}(\tau^{k})\hat{\gamma}_{0}\left(\frac{|\tau^{k}|}{g_{\theta}}\right)^{\frac{1}{m}}<br>τk=mk⋅Tnk;mk=Fem0k;nk=(Fe)−Tn0k\tau^{k}=\mathbf{m}^{k}\cdot\mathbf{T}\mathbf{n}^{k};\quad\mathbf{m}^{k}=\mathbf{F}^{e}\mathbf{m}_{0}^{k};\quad\mathbf{n}^{k}=(\mathbf{F}^{e})^{-T}\mathbf{n}_{0}^{k}

Table 2. Constitutive relations for plastic strain rate of SDs, Lp\mathbf{L}^{p}, for the MFDM variants of J2J_{2} and Crystal plasticity.

The appearance of the thermally-softened strength gθg_{\theta} in the expressions for the scalar rates γ^k\hat{\gamma}^{k}, γ^\hat{\gamma} is of note in relation to the representation of higher plastic straining in regions of higher temperature, for otherwise equal driving (resolved shear/deviatoric) stresses.

Tij′=Tij−Tmm3δij;ai=13TmmεijkFjpeαpk;cl=εijkTjr′Frpeαpkd=c−(c−a∣a∣)a∣a∣;γ^avg=(1nsl∑k=1nslγ^k)V=ζd∣d∣;ζ=(μg)2η2bγ^\begin{aligned} T'_{ij} &= T_{ij}-\frac{T_{mm}}{3}\delta_{ij}; & a_i &= \frac{1}{3}T_{mm}\varepsilon_{ijk}F^e_{jp}\alpha_{pk}; & c_l &= \varepsilon_{ijk}T'_{jr}F^e_{rp}\alpha_{pk}\\ \mathbf{d} &= \mathbf{c}-\left(\mathbf{c}-\frac{\mathbf{a}}{|\mathbf{a}|}\right)\frac{\mathbf{a}}{|\mathbf{a}|}; & \hat{\gamma}_{avg} &= \left(\frac{1}{n_{sl}}\sum_{k=1}^{n_{sl}}\hat{\gamma}^{k}\right)\\ \mathbf{V} &= \zeta\frac{\mathbf{d}}{|\mathbf{d}|}; & \zeta&= \left(\frac{\mu}{g}\right)^2\eta^2 b\hat{\gamma} \end{aligned}

Table 4: Constitutive relations for dislocation velocity V\mathbf{V}. α×V\boldsymbol{\alpha}\times\mathbf{V} gives the plastic strain rate of GNDs.

The various input material parameters and descriptors entering the constitutive equations in Tables 1–3 are as follows: ρ∗\rho^{*} is the mass density of the pure, unstretched elastic lattice, CC is the fourth order elastic tensor, μ\mu is the shear modulus, mm represents the material rate sensitivity, while γ^0\hat{\gamma}_{0} and γ^k\hat{\gamma}_{k} denote the reference strain rate and the magnitude of statistical dislocations (SD) slipping rate on the kthk^{\mathrm{th}} slip system in the crystal plasticity model, respectively. The number of slip systems is given by nsln_{sl}, with mk\mathbf{m}^{k}, nk\mathbf{n}^{k} and m0k\mathbf{m}_{0}^{k}, n0k\mathbf{n}_{0}^{k} representing the slip direction and slip plane normal in the current and unstretched lattice configurations respectively. The material strength parameters include the initial, g0g_{0}, and saturation, gsg_{s}, while h0h_{0} characterizes the Stage 2 hardening rate. The constants k0k_{0} and η\eta govern the GND related hardening contributions [5]. Additionally, bb denotes the Burgers vector magnitude of a full dislocation in the crystalline material. The quantity ll is a material length related to the gross modeling of mesoscale effects of dislocation core energy. The length ll controls the refinement of the GND microstructure and does not influence the length scale effects as shown in [14]. Both k0k_{0} and ll are the only two additional parameters to the well-accepted model of classical crystal plasticity theory [13, 57, 22, 11].

To model thermal softening, we update the material strength law to model the effect of change in the temperature on the material according to (5). The updated material strength, gθg_{\theta}, is defined from the current strength, gg, as shown in (5) through a simple, commonly used power-law softening relationship, where θ\theta and θ0\theta_{0} represent the current temperature and a reference (often room) temperature:

gθ=g(θθ0)−p.(9)g_{\theta}=g\left(\frac{\theta}{\theta_{0}}\right)^{-p}. \tag*{(9)}

The temperature of the body, θ\theta, is updated using idealized balance of energy under adiabatic conditions according to

θ˙=βT:W−1(α×V+Lp),(10)\dot{\theta}=\beta\mathbf{T}:\mathbf{W}^{-1}\left(\boldsymbol{\alpha}\times\mathbf{V}+\mathbf{L}^{p}\right), \tag*{(10)}
β=κρcp,(11)\beta=\frac{\kappa}{\rho c_{p}}, \tag*{(11)}

with κ\kappa the Taylor-Quinney coefficient, ρ\rho the mass density, and cpc_{p} the specific heat capacity of the material.

The isotropic elastic moduli are updated as

μ=μ0(1−D0exp⁡(θ0θ)−1)andλ=2μν1−2ν.(12)\mu=\mu_{0}\left(1-\frac{D_{0}}{\exp\left(\frac{\theta_{0}}{\theta}\right)-1}\right) \qquad\text{and}\qquad \lambda=\frac{2\mu\nu}{1-2\nu}. \tag*{(12)}

where μ0\mu_{0} is the shear modulus at reference temperature θ0\theta_{0}, and D0D_{0} is a parameter accounting for the softening in the elastic moduli.

Classical J2J_{2} and Crystal plasticity formulations from MFDM: To produce results corresponding to the classical plasticity versions of these constitutive models, we simply set l=0l=0, k0=0k_{0}=0, V=0\mathbf{V}=0.

This effectively also implies that the α\alpha evolution equation (5) does not have to be solved in such cases.

Algorithm and verification

The numerical algorithm used to solve the system (4) is briefly mentioned here, with more details to be found in [14].

The weak forms of the governing equations of MFDM at finite deformation used in this paper for dynamic cases are presented. This is followed by the algorithm summarizing the implementation.

The FEM formulation and computational algorithm outlined here remain general and do not depend on specific constitutive choices for Lp\mathbf{L}^{p}, V\mathbf{V}, or T\mathbf{T}. To solve the governing equations, we employ a numerical scheme based on discrete time increments. Considering a typical step from tnt^{n} to tn+1t^{n+1}, any quantity (⋅)(\cdot) evaluated at these time instances is denoted as (⋅)n(\cdot)^{n} and (⋅)n+1(\cdot)^{n+1}, respectively. The time increment Δtn\Delta t^{n} is given by Δtn=tn+1−tn\Delta t^{n}=t^{n+1}-t^{n}.

  • Weak form for v\mathbf{v}

As described in [14], the finite element mesh is moved to update the geometry using the material velocity field v\mathbf{v}. Balance of linear momentum equation (8) is solved on the current configuration. Given the stresses and material velocity in the domain Ωn\Omega^{n}, the velocity at the next time step, vn+1\mathbf{v}^{n+1}, is obtained using the Forward Euler method as follows:

∫Ωnρ(vin+1−vin)δvi dV=Δtn(∫∂Ωntiδvi dA−∫ΩnTijδvi,j dV).\int_{\Omega^{n}}\rho(v_i^{n+1}-v_i^{n})\delta v_i\,dV=\Delta t_n\left(\int_{\partial\Omega^{n}}t_i\delta v_i\,dA-\int_{\Omega^{n}}T_{ij}\delta v_{i,j}\,dV\right).

To improve computational efficiency, the mass matrix is lumped. It is verified that the lumping process does not significantly impact the accuracy of the results.

  • Weak form for α\boldsymbol{\alpha}

As discussed in [14], the α\boldsymbol{\alpha} transport equation (5) exhibits nonlinear wave type solutions. An explicit Galerkin-Least-Squares FEM approach is adopted here to solve (4a) (cf. [93] for an algorithm in the small-deformation setting), with diagonal lumping for the ‘mass’ term explicitly displayed in (9). Using Lp=L^p+βcurl⁡α\mathbf{L}^{p}=\hat{\mathbf{L}}^{p}+\beta\operatorname{curl}\boldsymbol{\alpha}, (4a) becomes

tr⁡(L)α+α˙−αLT=−curl⁡(α×V+L^p+βcurl⁡α).\operatorname{tr}(\mathbf{L})\boldsymbol{\alpha}+\dot{\boldsymbol{\alpha}}-\boldsymbol{\alpha}\mathbf{L}^{T}=-\operatorname{curl}\left(\boldsymbol{\alpha}\times\mathbf{V}+\hat{\mathbf{L}}^{p}+\beta\operatorname{curl}\boldsymbol{\alpha}\right).
∫Ωnδαij(αijn+1−αijn) dV+R=0(13)\int_{\Omega^{n}}\delta\alpha_{ij}\left(\alpha_{ij}^{n+1}-\alpha_{ij}^{n}\right)\,dV+R=0 \tag*{(13)}

where,

β=(l2nsl∑knsl∣γ^k∣)(14)\beta=\left(\frac{l^{2}}{n_{\mathrm{sl}}}\sum_{k}^{n_{\mathrm{sl}}}\left|\hat{\gamma}^{k}\right|\right) \tag*{(14)}
R=∫Ωnδαij(ΔtnLppαijn−ΔtnαipnLjp) dV+Δtn∫ΩnεjqpεjabαiaVbδαip,q dV+Δtn∫ΩnL^ijpεjqpδαip,qn dV+Δtn∫Ωenβεjabαi,bnεjpqδαip,q dV+Δtn∫∂ΩinBijδαij dA+Δtn∫∂ΩinαijnVnpδαij dA−Δtn∫∂ΩinαiqnVjnqδαij dA−Δtn∫∂ΩinεjpqL^ippnqδαij dA−Δtn∫∂Ωinβεjpqεpbaαia,bnnqδαij dA+c[∫ΩenAriδαri dV+Δtn∫ΩenLmpAriδαri dV−Δtn∫ΩenAriδαrpLip dV+Δtn∫ΩenAri(δαri,qVq−δαrq,qVi+δαriVq,q−δαrqVi,q) dV+Δtn∫ΩenAri(β,pδαrp,i+βδαrp,ip−β,pδαri,p−βδαri,pp) dV].(15)\begin{aligned} R={}&\int_{\Omega^{n}}\delta\alpha_{ij}\left(\Delta t^{n}L_{pp}\alpha_{ij}^{n}-\Delta t^{n}\alpha_{ip}^{n}L_{jp}\right)\,dV\\ &+\Delta t^{n}\int_{\Omega^{n}}\varepsilon_{jqp}\varepsilon_{jab}\alpha_{ia}V_b\delta\alpha_{ip,q}\,dV+\Delta t^{n}\int_{\Omega^{n}}\hat{L}^{p}_{ij}\varepsilon_{jqp}\delta\alpha_{ip,q}^{n}\,dV \\ &+ \Delta t^n \int_{\Omega^n_e} \beta\varepsilon_{jab}\alpha^n_{i,b}\varepsilon_{jpq}\delta\alpha_{ip,q}\,dV + \Delta t^n \int_{\partial\Omega^n_i} B_{ij}\delta\alpha_{ij}\,dA \\ + \Delta t^n \int_{\partial\Omega^n_i} \alpha^n_{ij}V_{np}\delta\alpha_{ij}\,dA - \Delta t^n \int_{\partial\Omega^n_i} \alpha^n_{iq}V_{jnq}\delta\alpha_{ij}\,dA - \Delta t^n \int_{\partial\Omega^n_i} \varepsilon_{jpq}\hat{L}^p_{ip}n_q\delta\alpha_{ij}\,dA \\ - \Delta t^n \int_{\partial\Omega^n_i} \beta\varepsilon_{jpq}\varepsilon_{pba}\alpha^n_{ia,b}n_q\delta\alpha_{ij}\,dA \\ + c\left[\int_{\Omega^n_e} A_{ri}\delta\alpha_{ri}\,dV + \Delta t^n \int_{\Omega^n_e} L_{mp}A_{ri}\delta\alpha_{ri}\,dV - \Delta t^n \int_{\Omega^n_e} A_{ri}\delta\alpha_{rp}L_{ip}\,dV \right.\\ \left. + \Delta t^n \int_{\Omega^n_e} A_{ri}\left(\delta\alpha_{ri,q}V_q-\delta\alpha_{rq,q}V_i+\delta\alpha_{ri}V_{q,q}-\delta\alpha_{rq}V_{i,q}\right)\,dV \right.\\ \left. + \Delta t^n \int_{\Omega^n_e} A_{ri}\left(\beta_{,p}\delta\alpha_{rp,i}+\beta\delta\alpha_{rp,ip}-\beta_{,p}\delta\alpha_{ri,p}-\beta\delta\alpha_{ri,pp}\right)\,dV\right]. \tag*{(15)} \end{aligned}

where,

Ari=Δtn[αrinLpp−αrpnLip+αri,qnVq−αrq,qnVi+αrinVq,q−αrqnVi,q+εipqLrq,pp+β,pαrp,in+βαrp,ipn−β,pαri,pn−βαri,ppn].A_{ri}=\Delta t_n\left[\alpha^n_{ri}L_{pp}-\alpha^n_{rp}L_{ip}+\alpha^n_{ri,q}V_q-\alpha^n_{rq,q}V_i+\alpha^n_{ri}V_{q,q}-\alpha^n_{rq}V_{i,q}+\varepsilon_{ipq}L^p_{rq,p}+\beta_{,p}\alpha^n_{rp,i}+\beta\alpha^n_{rp,ip}-\beta_{,p}\alpha^n_{ri,p}-\beta\alpha^n_{ri,pp}\right].

Here, LL, VV and L^p\hat{L}^p are considered known data. The boundaries ∂Ωin\partial\Omega^n_i and ∂Ωon\partial\Omega^n_o denote the inflow and outflow portions of ∂Ωn\partial\Omega^n, respectively. The term BB represents the input dislocation flux, given by α(V⋅n)\boldsymbol{\alpha}\left(V\cdot n\right) on ∂Ωn\partial\Omega^n. Ωen\Omega^n_e indicates the interiors of the elements. The gradient of β\beta is ignored in the Least-Square stabilization due to degrading computational approximation observed practically. We choose c=1c=1 for MFDM calculations, unless stated otherwise. The reasoning is elaborated in [14].

  • Updating inverse elastic deformation

The new contribution in this work is the algorithm for the evolution of the inverse elastic distortion field, (7), discretely evolved as follows: W˙\dot{W} is not directly discretized in time. Noting that

W˙+WL=α×V+Lp⟺W˙FF−1=α×V+Lp(16)\dot{W}+WL=\alpha\times V+L^p \Longleftrightarrow\dot{W}FF^{-1}=\alpha\times V+L^p \tag*{(16)}

with FF representing the deformation gradient (w.r.t an arbitrarily chosen, but fixed, reference configuration), W˙F\dot{W}F is discretized in time so that when the right-hand side of (16) vanishes, W=F−1W=F^{-1} is recovered in discrete time. The exact update scheme is shown in (17), where aa denotes the field aa at time bb:

Wt+ΔtFt+Δt−WtFtΔt=(α×V+Lp)t(Ft).(17)\frac{W^{t+\Delta t}F^{t+\Delta t}-W^tF^t}{\Delta t}=\left(\alpha\times V+L^p\right)^t\left(F^t\right). \tag*{(17)}

Algorithm

Based on the schemes discussed above, we evolve the coupled system (4). A robust and efficient time stepping criterion used for this model is explained in detail in [14]. Briefly, these criteria are based on plastic relaxation, elastic wave speed in the material and a 0.2% yield strain threshold. A cut-back algorithm is used to ensure stable and robust evolution of state variables. This carefully controls the magnitude of plastic strain in each increment. The algorithm used for the simulations in this work is presented in Table 5.

Given:Material properties, initial conditions, boundary conditions, and applied loading conditions.
Evolution of the system:Assume that vn−1v^{n-1} the state at time tnt^n is known: xnx^n, αn\alpha^n, VnV^n, LpL^p, Δtn\Delta t^n, WnW^n. To get the state at time step tn+1t^{n+1} the following is done:
•Material velocity vnv^n is obtained by solving the balance of linear momentum Eq. (4d) Ωn\Omega^n.
•αn+1\alpha^{n+1} on Ωn+1\Omega^{n+1} is obtained by solving weak form of α\alpha evolution equation (15) on Ωn\Omega^n.
•The configuration of the body is discretely updated, i.e., xn+1=xn+vnΔtnx^{n+1}=x^n+v^n\Delta t^n.
•Wn+1W^{n+1} on Ωn+1\Omega^{n+1} is obtained by using Eq. (17).
State acceptance criteria:Let PSR=(max⁡(∣Fαe×V∣n+1)+max⁡(γ^n+1))PSR=\left(\max\left(\lvert F^e_\alpha\times V\rvert^{n+1}\right)+\max\left(\hat{\gamma}^{n+1}\right)\right). If PSR×Δtn≤0.002PSR \times\Delta t^n \leq0.002, the state is accepted. Δtn+1\Delta t^{n+1}, based on the new state, is calculated as discussed in [14]Table 6 and this algorithm is repeated to get state at increment tn+2t^{n+2}. If the condition is not satisfied:
•Go back to the state at time tnt^n.
•Use Δtn,new=min⁡(0.002PSR,0.5Δtn)\Delta t^{n,\mathrm{new}}=\min\left(\frac{0.002}{PSR},0.5\Delta t^n\right) and repeat the algorithm to obtain a new state at tn+1t^{n+1}.

Table 5. Algorithm for dynamic MFDM

Verification

For verification, we have applied a constant velocity in the uniaxial compression test as shown in Figure 1. As expected, this constant loading produces an elastic wave first, followed a the plastic wave - we use the J2J_2-MFDM plasticity model for this exercise. The domain selected for this simulation is 10×15 μm210 \times15\ \mu\mathrm{m}^2. We calculate the speed of the elastic and plastic waves separately, as discussed below:

Schematic showing the boundary condition used for verification

Figure 1. Schematic showing the boundary condition used for verification. A uniform velocity is applied at the top surface, where AA is the applied strain rate. The displacement profile and the stress deviator are discussed along the black line. The origin is at the center of the domain.

  • Elastic wave speed: This speed is calculated based on the displacement profile. Specifically, we plot the displacement along the vertical line x=0x=0, as shown by the black line in Figure 1. The obtained result is presented in Figure 2. It is observed that the ratio of the analytical linear elastic dilatational wave speed and the calculated speed is nearly 1. This verifies that the simulation is producing the expected elastic wave speed.

Displacement along the $x=0$ line, plotted at different times

Figure 2. Displacement along the x=0x=0 line, plotted at different times to calculate the elastic wave speed.

  • Plastic wave speed: We define the plastic wave speed as the rate at which the plastically yielded material front is moving through the domain as explained in the following. The wave-front of σ′=∣σ′∣\sigma' = \lvert\boldsymbol{\sigma}' \rvert, the magnitude of the deviatoric stress tensor, is tracked in the simulation and its speed calculated. This measure serves as an effective indicator of plasticity. The deviatoric stress normalized by the yield stress is plotted along a vertical line (the black line in Figure 1). Figure 3 shows smoothed curves to enable clearer analysis. Smoothing is performed by taking a moving average, over a fixed size, of the original curve.

Norm of deviatoric stress normalized by yield stress

Figure 3. Norm of deviatoric stress (σ′\sigma') normalized by yield stress (g0g_0) along the x=0x=0 line.

The elastic wave speed calculated in this case is approximately 1.8 times the linear elastic dilatation wave speed. This is reasonable because a nonlinear elastic material has a linearized elastic modulus which depends on elastic strain and typical nonlinear elastic materials become stiffer with increasing compression [105]. Moreover, the plastic wave speed, apapproximately half the elastic wave speed, aligns with experimental findings that plastic wave speeds in steels typically range between 0.2 and 0.6 times the elastic wave speed [65].

Motivating experiments and general considerations for the simulation studies

SHPB, also known as the Kolsky bar [59], is a well-established experimental technique for characterizing material behavior at high strain rates, typically in the range of 10210^{2}–104 s−110^{4}\ \mathrm{s}^{-1}. A schematic of the apparatus is shown in Figure 4. The setup consists of three main components: a striker bar (not shown in the figure), an incident bar, and a transmission bar, with the specimen sandwiched between the incident and transmission bars. Upon impact of the striker bar, a compressive stress wave propagates through the incident bar. At the specimen interface, part of this wave is reflected back into the incident bar while the remainder is transmitted through the specimen into the transmission bar. Strain gauges mounted on the incident and transmission bars record the incident (ϵi\epsilon_i), reflected (ϵr\epsilon_r), and transmitted (ϵt\epsilon_t) strain pulses, from which specimen stress, strain, and strain rate can be inferred. Details of the experimental protocol and underlying formalism can be found in [83].

Schematic of the Split Hopkinson Pressure Bar apparatus

Figure 4. Schematic showing the components of the Split Hopkinson Pressure Bar apparatus: striker bar, incident bar, specimen, and transmission bar.

Cylindrical specimens (6 mm diameter ×\times 6 mm height) machined from an 12\frac{1}{2} in. steel plate along three orthogonal directions were characterized by loading at several different initial temperatures and strain rates [82]. Tests were conducted at nominal strain rates exceeding 1000 s−11000\ \mathrm{s}^{-1}, and the measured stress–strain response was used to calibrate our model parameters, as discussed in § 4.2. The cylindrical geometry, in combination with uniaxial compression boundary conditions, produces a nominally homogeneous deformation field throughout the specimen. We perform simulations on a statistically representative volume element (RVE) [23] subjected to boundary conditions derived from the experimental loading, rather than simulating the full macroscale specimen.

To study adiabatic shear band formation, SHPB experiments were performed using a top-hat specimen geometry. The top-hat geometry features a reduced section (shown in Figure 5) which concentrates deformation into a predetermined shear zone, enabling controlled and reproducible shear band initiation [70]. This design allows for targeted post-mortem characterization of the shear band region.

Top-hat specimen configuration in the SHPB setup

Figure 5. Top-hat specimen configuration in the SHPB setup: (a) undeformed assembly with deformation limiters, (b) deformed configuration showing localized shear regions, and (c) Scanning electron micrograph of a recovered specimen cross-section.

Rather than modeling the entire specimen, we focus on a statistically representative RVEs in the size range of 10 μ\mum - 160 μ\mum, which encompasses the range in which adiabatic shear bands are experimentally observed, as shown in Figure 5c and Figure 6.

Scanning electron micrographs and IPF maps of the top-hat specimen

Figure 6. Scanning electron micrographs (left) and IPF maps (IPF parallel to the loading direction yy) via EBSD (right) of the top-hat specimen under continuous dynamic loading at displacement increments of (a,b) ΔL=0.14 mm\Delta L = 0.14\ \mathrm{mm}, (c,d) ΔL=0.25 mm\Delta L = 0.25\ \mathrm{mm}, and (e,f) ΔL=0.34 mm\Delta L = 0.34\ \mathrm{mm}. Progressive deformation localization (left) and grain refinement with subgrain formation (right) are evident.

The polycrystalline microstructure used in the simulations here is described in [23]. Different boundary conditions, initial conditions, and geometries are employed to probe distinct aspects of localization and thermal softening in dynamic shear banding phenomena.

Experimental observations

Experimental observations provide critical insight into the observed phenomenology of shear band formation and evolution, and guide the selection of appropriate test problems studied in our simulations.

Localization behavior was observed under dynamic loading (Figure 6) conditions. The polycrystalline microstructure used for analysis was informed by high-resolution electron backscatter diffraction (EBSD) measurements of the undeformed material. A ZEIS GEMINI microscope equipped with Oxford Symmetry S3 EBSD detector was used. An EBSD step size of 15 nm15\,\mathrm{nm} was used to collect data. Dictionary indexing (DI) was used to index the EBSD patterns.

In this dynamic test configuration, the incident bar strikes the specimen at high impact velocity (Figure 5a), initiating deformation localization in the region highlighted in Figure 5b. The deformation localizes into a narrow adiabatic shear band at the hat–brim interface of the specimen. The band maintains a finite width on the order of 1010–40 μm40\,\mu\mathrm{m} and remains sharply defined throughout deformation.

This finite-width character of the shear band is a key experimental observation that forms one of the primary questions of our modeling studies.

A particularly noteworthy observation from the EBSD analysis (Figure 6) is the development of intragranular substructure within the shear band region, with the grains exhibiting a slender, elongated morphology approximately parallel to the shear band. The inverse pole figure (IPF) maps reveal subgrain formation at large deformation. These microstructural features suggest that dislocation density evolution plays a central role in the process of shear banding.

A scaling argument to speed up mesoscale simulations

Results from a SHPB test [82] on a cylindrical specimen are used to determine the boundary conditions that are applied to an RVE of the steel and the material parameters of the model. A schematic of the applied boundary conditions is shown in Figure 10a, with details given in Table 6.

BoundaryTypeCondition
TopTraction and velocitytx=0t_x = 0, vy=vlv_y = v_l
BottomTraction and velocitytx=0t_x = 0, vy=vrv_y = v_r
Left and RightTraction-freet=0\boldsymbol{t} = 0

Table 6. Boundary conditions for Compression. vyv_y: yy-component of velocity; vlv_l, vrv_r: prescribed velocities at the top and bottom boundaries from SHPB data; txt_x: traction component in the xx-direction; t\boldsymbol{t}: traction vector. Note: the simulations do not include the unloading phase of the SHPB data.

The procedure for determining the velocity boundary conditions on the specimen from experimental data obtained from the test is first outlined. A detailed description of the approach can be found in [83].

Velocity boundary conditions for SHPB simulations

The experimental data available from the SHPB test are the strain gauge readings shown in Fig. 7a. To obtain the velocity boundary conditions for our calibration simulations, one-dimensional wave analysis is employed. The resulting velocity histories applied at the left and right specimen boundaries are shown in Figure 7b. In this figure, time zero corresponds to the instant when the incident wave reaches the left interface. The boundary condition on the right interface is applied with a time delay equal to the wave transit time through the specimen, calculated using the elastic wave speed of the material. The velocities at the left (vlv_l) and right (vrv_r) boundaries are computed from the strain data as:

Experimental strain gauge readings and velocity boundary conditions

Figure 7. (a) Experimental strain gauge readings from the SHPB test, and (b) velocity boundary conditions derived for the simulations.

vl=cb(ϵi−ϵr),vr=cb(ϵt),(18)\begin{aligned} v_l &= c_b(\epsilon_i-\epsilon_r),\\ v_r &= c_b(\epsilon_t), \tag*{(18)} \end{aligned}

where ϵi\epsilon_i, ϵr\epsilon_r, and ϵt\epsilon_t are the incident, reflected, and transmitted strain pulses, respectively, and cbc_b is the elastic wave speed in the pressure bars.

This approach ensures that the simulation boundary conditions faithfully represent the loading history experienced by the specimen during the experiment, capturing the initial stress wave arrival as well as the subsequent wave reflections within the specimen. In the simulation configuration (Figure 10a), the specimen is oriented vertically: the left experimental boundary is mapped to the top boundary and the right experimental boundary to the bottom boundary. The velocity boundary conditions vlv_l and vrv_r are accordingly applied.

Dimensional analysis to reduce wall-clock time for mesoscale simulations

As mentioned, we consider RVEs of linear dimension in the ∼10−100 μm\sim10-100\ \mu\mathrm{m} range. The experimental specimen has a characteristic dimension of Hexp=6 mmH_{\mathrm{exp}}=6\ \mathrm{mm}, and the velocity boundary conditions shown in Figure 7b correspond to this full-scale specimen. For the RVE of size HRVEH_{\mathrm{RVE}}, we make the assumption of calibrating the behavior of the RVE at the same applied nominal strain rate as the macroscopic SHPB cylindrical sample for which homogeneous deformation conditions are expected to set in after a few wave reflections. Hence,

A=vexpHexp=vRVEHRVE,⟹vRVE=vexp⋅HRVEHexp(19)A=\frac{v_{\mathrm{exp}}}{H_{\mathrm{exp}}}=\frac{v_{\mathrm{RVE}}}{H_{\mathrm{RVE}}},\qquad\Longrightarrow\qquad v_{\mathrm{RVE}}=v_{\mathrm{exp}}\cdot\frac{H_{\mathrm{RVE}}}{H_{\mathrm{exp}}} \tag*{(19)}

where AA is the applied strain rate, and vRVEv_{\mathrm{RVE}} and vexpv_{\mathrm{exp}} are the velocity differences between the top and bottom faces of the RVE and the experimental domain, respectively (vexp=vl−vrv_{\mathrm{exp}}=v_l-v_r (18)). Thus the physical problem that is simulated for the HRVEH_{\mathrm{RVE}} sized sample for the purposes of calibration uses the above scaled magnitude for the velocity-time profile shown in Figure 7b.

The main obstacle when simulating smaller domains and/or the finer meshes (on the scale μm\mu\mathrm{m}) is related to wall clock time taken by simulation for an adequate mesh refinement. As the time stepping is directly proportional to the element size (Courant-Friedrichs-Lewy (CFL) condition) and inversely proportional to the elastic wave speed, when the element size is reduced by a factor with elastic wave speed remaining constant, the simulation time increment decreases and the number of time-steps required for reaching a prescribed strain level at a fixed strain rate, increases by the same factor.

We use Dimensional Analysis [18] to overcome the above bottleneck. This approach is fundamentally based on the idea that physics does not depend on the physical units used to describe any chosen natural phenomena. Relevant observables of the modeling and simulation setup can be written as a function of dimensionless ratios as shown in (16) (example shown for the true stress σt\sigma_t):

σtg0=ϕ(Eg0,γ^0fA,VeH(fA),bH,f,κ,k0),(20)\frac{\sigma_t}{g_0}=\phi\left(\frac{E}{g_0},\frac{\hat{\gamma}_0}{fA},\frac{V_e}{H(fA)},\frac{b}{H},f,\kappa,k_0\right), \tag*{(20)}

where σt\sigma_t is the true stress, g0g_0 is the initial yield strength, EE is the elastic modulus, γ^0\hat{\gamma}_0 is the reference plastic strain rate, AA is the applied strain rate, HH is the length of the domain, Ve=E/ρV_e = \sqrt{E/\rho} is the elastic wave speed, ρ\rho is the mass density, bb is the magnitude of the Burgers vector, ff, κ\kappa, k0k_0 are non-dimensional parameters representing the scaling factor by which the applied strain rate is increased, the Taylor-Quinney coefficient (6), and the GND hardening coefficient (Table 3), respectively.

The main idea is to reach the same strain in a smaller number of steps and if we can increase the amount of strain in each step, keeping the same time stepping, we can resolve the issue. This idea translates to increasing the applied strain rate by a factor ff (i.e., A→fAA \rightarrow fA), while ideally maintaining the ratios in (20) in which AA appears fixed. Thus, we increase the reference plastic strain rate, γ^0\hat{\gamma}_0, by the same factor ff. The other ratio, Ve/HfA\frac{V_e/H}{fA} representing the ratio of an elastic strain-rate defined by an elastic wave speed and specimen geometry to the applied strain rate, is assumed to have no significant effect on the results pertaining to plasticity effects, within the strain rate range of interest. This assumption is verified a-posteriori. As shown in Figure 8, the assumption holds within the given strain range. Here, both AA and γ^0\hat{\gamma}_0 have been increased by the same factor. The factor used for our simulations is f=150f = 150 to balance the computational gain with making sure that the differences in stress-strain response between the f=1f = 1 and f=150f = 150 profiles in Figure 8 are minimal.

Stress-strain curves for different values of applied strain rate

Figure 8. Comparison of stress-strain curve for different values of applied strain rate but keeping the non-dimensional ratio, γ^0fA\frac{\hat{\gamma}_0}{fA}, fixed. Different values of ff are shown in legend.

Using this approach, the simulation time for a given problem was reduced to nearly 1/10th1/10^{\mathrm{th}} when AA was increased by a factor of 25. Initially, the simulation for the given domain was estimated to take around 120 hours (based on extrapolation) using 128 cores. After applying the dimensional analysis approach, the same strain was achieved in just 12 hours by scaling AA and γ^0\hat{\gamma}_0 appropriately. Using more cores results in a speedup. For the same problem, if 128 cores take 12 hours, the task can be completed in approximately 8 hours with 256 cores, without any further attention paid to code efficiencies.

Calibration for 2-d simulations: The experimental stress-strain response shown in Figure 9 is used to define the initial yield stress, g0g_0, and the Stage II hardening rate h0h_0 of the material model. Elastic properties are obtained from independent material characterization tests.

Stress-strain response from the SHPB experiment compared with the simulation

Figure 9. Stress-strain response from the SHPB experiment compared with the simulation.

Boundary conditions for compression

(a)

Boundary conditions used for simulating a shear band

(b)

Figure 10. 10≤H≤16010 \le H \le160 (μ\mum). (a) Boundary conditions for compression and (b) boundary conditions used for simulating a shear band. Details of these boundary conditions are listed in Table 6 and Table 7.

vxv_x, vyv_y: components of the velocity vector; AA: applied strain rate; HH: height of the RVE; MPC: multi-point constraint enforcing uniform vertical displacement. The loading is applied as a step in time, with the velocity equal to zero at t=0t = 0 and held constant for all subsequent times.

Results and Discussion

We present and discuss results of various 2-d and 3-d simulations that were performed to understand the behavior of the model. Behavior under boundary and initial conditions that would induce both nominally homogeneous and heterogeneous deformation in quasi-static motions of a homogeneous material are employed in our dynamic simulations. Comparisons with predictions of classical plasticity theory are provided where appropriate. Details of the evolution of the microstructural state of the material are also shown.

We take as an estimate of the initial statistical dislocation density, ρˉs\bar{\rho}_s (see [1 Eqn. 5] for the definition of the statistical density ρs\rho_s at any time), as

ρˉs=(g0ημb)2.(21)\bar{\rho}_s = \left(\frac{g_0}{\eta\mu b}\right)^2 . \tag*{(21)}

Model setup and material parameters: 2-d simulations

The RMFDM model requires initial conditions for four field variables: velocity (v\boldsymbol{v}), GND density (α\boldsymbol{\alpha}), inverse elastic distortion (W\boldsymbol{W}), and the motion map (x\boldsymbol{x}). The velocity field is initialized to zero throughout the domain, except at the boundaries where loading is applied. The GND density is initialized to zero. The initial inverse elastic distortion W\boldsymbol{W} is set to the transpose of the rotation field that characterizes the polycrystalline microstructure, thereby encoding the crystallographic orientation of each grain. In principle, such an (strain-free) inverse elastic distortion field corresponds to a localized GND distribution at the grain boundaries through its curl field. We intentionally do not include this contribution in the initialization of α\boldsymbol{\alpha} - thus, all subsequent GND accumulation at grain boundaries is an (physically realistic) outcome of our framework.

The polycrystal microstructure used is shown in Figure 11. In this 2-d setting, a synthetic microstructure is constructed, with crystallographic orientations arbitrarily assigned to each grain1, and uniform within it. In the 2-d setting, the orientation of each grain is characterized by a single rotation angle. The grain shapes and sizes are obtained from a cross-sectional plane through the center of the full 3-d polycrystal described below.

Rotation angle field in the undeformed configuration

Figure 11. Rotation angle field in the undeformed configuration. Different colorbar scales are used to highlight the grains.

Boundary conditions are imposed on both v\boldsymbol{v} and α\boldsymbol{\alpha}. For the velocity, periodic boundary conditions, as shown in Figure 10b, are applied on the lateral (side) faces in both directions (Table 7). On the top and bottom faces, a prescribed shear velocity is applied in the horizontal direction, while in the vertical direction, multi-point constraints (MPCs) are used to enforce uniform displacement of the boundary nodes. This constraint ensures that the top and bottom surfaces remain planar throughout the deformation. For the GND density, unconstrained boundary condition (as described in Sec. 2.1) is imposed. The simulation settings and material parameters are listed in Table. Table 8.

BoundaryTypeCondition
TopPrescribed velocityvx=v1=AH/2v_x = v_1 = AH/2, uniform vyv_y via MPC
BottomPrescribed velocityvx=v1=−AH/2v_x = v_1 = -AH/2, uniform vyv_y via MPC
Left and RightPeriodic BCVelocity periodicity in xx and yy

Table 7. Boundary conditions applied for shear band studies in 2-d.

ModelParameterValueDescription
Classical Crystal Plasticityγ^0\hat{\gamma}_0 (s−1^{-1})0.001Reference plastic strain rate (Table 2)
Classical Crystal Plasticitymm0.03Rate sensitivity exponent (Table 2)
Classical Crystal Plasticityg0g_0 (GPa)0.450Initial yield strength (Table 3)
Classical Crystal Plasticitygsg_s (GPa)0.450Saturation yield strength (Table 3)
Classical Crystal Plasticityh0h_0 (GPa)0Stage 2 hardening rate (Table 3)
Classical Crystal PlasticityEE (GPa)200Young’s modulus
Classical Crystal Plasticityν\nu0.30Poisson’s ratio
Classical Crystal Plasticityρ\rho (kg/m3^3)7830Mass density (4d)
Classical Crystal Plasticitybb (Å)4.05Burgers vector magnitude (Table 2)
Classical Crystal Plasticityη\eta13\frac{1}{3}Taylor relationship constant for macroscopic strength vs. dislocation density (Table 2)
MFDM (additional)k0k_00.5Constant in coefficient defining GND hardening (Table 3)
MFDM (additional)ll (μ\mum)0.1732Constant in coefficient defining core energy density (Table 2)
Thermal Parameters (Classical plasticity)θ0\theta_0 (KK)293Reference temperature (5)
Thermal Parameters (Classical plasticity)pp0.38Exponent in thermal softening law (5)
Thermal Parameters (Classical plasticity)κ\kappa0.55Taylor–Quinney coefficient (7)
Thermal Parameters (Classical plasticity)CpC_p (J/Kg . K)490Specific heat capacity (7)
Thermal Parameters (Classical plasticity)D0D_016\frac{1}{6}Parameter related to elastic moduli softening (8)

Table 8. Material parameters used for 2-d simulations, unless mentioned otherwise. k0k_0 has been varied for the size-effect investigation.

Planar slip systems are required for 2-d simulations. However, most, if not all, crystal structures (including BCC Iron) lack planes containing multiple slip systems. To approximately accommodate this feature within a 2-d ansatz, we used a least squares projection of the two predominant deformation slip systems onto a single analysis plane (as shown in Figure 12 (a)).

Figure 12. (a) Schematic showing the slip systems considered and the corresponding analysis plane. (b) Crystallographic view of the slip systems and the analysis plane.

The analysis plane is defined by the normal, n\mathbf{n}, determined by solving the following optimization,

F(z)=(n1⋅z)2+(m1⋅z)2+(n2⋅z)2+(m2⋅z)2F(\mathbf{z}) = (\mathbf{n}_1 \cdot\mathbf{z})^2 + (\mathbf{m}_1 \cdot\mathbf{z})^2 + (\mathbf{n}_2 \cdot\mathbf{z})^2 + (\mathbf{m}_2 \cdot\mathbf{z})^2
n=argmin⁡z,∣z∣=1F(z)\mathbf{n} = \underset{\mathbf{z},\lvert\mathbf{z}\rvert=1}{\operatorname{argmin}} F(\mathbf{z})

where mi\mathbf{m}_i, ni\mathbf{n}_i are, respectively, the slip direction and the normal to the slip plane for the ithi^{th} slip system.

The two projected slip systems capture the dominant deformation modes of the crystal within the analysis plane. A third slip system is then introduced along the remaining in-plane direction to ensure a reasonable level of plasticity.

Modeling adiabatic shear bands

We analyze shear band formation using two models – Classical Crystal Plasticity (CCP) and MFDM. A key feature of MFDM is its explicit treatment of GND density evolution via the Nye tensor, which naturally incorporates an intrinsic material length scale and GND-induced hardening – factors of some significance in the shear localization problem. The two models are compared with respect to convergence of results upon mesh refinement and the predicted shear band width against experimental observations, keeping in mind that the deformation of an RVE is studied under boundary conditions suited more for inducing nominally homogeneous deformation (in a homogeneous material under quasi-static conditions).

The stress-strain curve is obtained by computing the engineering shear strain from the relative lateral displacement between the top and bottom boundaries and the shear stress from the xx-21

component of the reaction force on the top boundary.

Γ=ΔuH,\Gamma= \frac{\Delta u}{H},
τ=rxS,\tau= \frac{r_x}{S},

where Γ\Gamma is the engineering shear strain, Δu\Delta u is the relative lateral displacement between the top and bottom boundaries, HH is the height of the domain, τ\tau is the shear stress, rxr_x is the xx-component of the reaction force on the top boundary, and SS is the area of the top boundary.

We first examine the convergence of the stress-strain response in Figure 13 under progressive mesh refinement, with mesh densities of 100, 200, and 500 elements per direction. The oscillations seen in Figure 13a are the result of elastic wave interactions with the boundary when significant portions of the domain have undergone elastic unloading, observed here primarily due to the (small) size of the domain. The size involved also prevents a direct comparison of the stress-strain response with that of an experiment.

Stress-strain curve for Classical crystal plasticity

(a)

Stress-strain curve for MFDM

(b)

Figure 13. Stress-strain curve for (a) Classical crystal plasticity (CCP) and (b) MFDM for mesh refinements of 1002100^2, 2002200^2, 5002500^2 elements.

As shown in Figure 13a, the stress-strain curve for the CCP case diverges with refinement, and the simulation eventually fails due to the localization of shear in a narrow band (Figure 14). In contrast, the stress-strain behavior in Figure 13b obtained using the MFDM approach remains nearly identical for all mesh sizes as shown.

The shear $F_{12}$ component of the deformation gradient for a coarse mesh

(a)

The shear $F_{12}$ component of the deformation gradient for a fine mesh

(b)

Figure 14. The (shear) F12F_{12} component of the deformation gradient using the Classical crystal plasticity formulation for (a) a coarse mesh (2002200^2 elements) at an applied strain of 0.3 and (b) a fine mesh (5002500^2 elements) at an applied strain of 0.08. The simulation on the fine mesh could not progress further.

The non-convergence in the stress-strain response of CCP (Figure 13a) is also observed in the deformation fields in the domain (Figure 14). MFDM produces a significantly more homogeneous deformation field in comparison (Figure 15) with no localization (as defined in § 1), and the field remains approximately consistent across both mesh resolutions. The field produced by CCP localizes into a narrow band across the domain, accompanied by increased strain concentration within the band with refinement (Figure 14): the maximum value of F12F_{12} inside the band increases from approximately 0.88 on the 2002^{2} mesh to approximately 1.20 for the finer mesh, a roughly 32% increase in strain. This difference arises because classical crystal plasticity lacks an intrinsic material length scale2. As shown in [74], the strain within the band will keep increasing with refinement, even though with rate-dependence and inertia, the band width can attain a converged value. MFDM, however, has an intrinsic length scale through the Burgers’ vector involved in defining the GND hardening term (Table. Table 3) resulting in mesh-independent fields.

The (shear) $F_{12}$ component of the deformation gradient for a coarse and fine mesh

Figure 15. The (shear) F12F_{12} component of the deformation gradient at an applied strain of 0.3 using the MFDM formulation for (a) a coarse mesh (2002^{2} elements) and (b) a fine mesh (5002^{2} elements).

Size effect

Next, we briefly present results that demonstrate the size effect captured at this length scale. Experiments have established that metallic materials exhibit a pronounced size-dependent strengthening response: as specimen dimensions decrease, the material becomes harder, providing greater resistance to plastic flow [77, 15]. To explore this effect in the present context, we perform a series of simulations in which the domain size is scaled from 10 to 160 μm\mu\mathrm{m} in a self-similar manner, maintaining a constant ratio of grain size to domain size of approximately 1/10.

Classical crystal plasticity predicts size-independent behavior and thus cannot capture experimentally observed phenomena, as shown in Figure 16. MFDM, by incorporating the Burgers vector as an intrinsic length scale, and accounting for the contributions of GNDs and their effect in hardening, enables the prediction of size-dependent mechanical response. This effect is more pronounced as we increase the material parameter, k0k_0; an example for the same is shown in the Figure 16c. This observation aligns with the understanding that, accounting more for GND hardening results in more pronounced size effects. Size effects have been simulated in different problems using MFDM. Here, we have shown it in the context of shear banding. As alluded to earlier, in all stress-strain traces shown in Figure 16, the small plateaus are the result of elastic waves from the interior impinging on the top surface where the reaction force is calculated.

Stress-strain curves for varying domain sizes

Figure 16. Stress-strain curves for varying domain sizes using (a) classical crystal plasticity (CCP), (b) MFDM, and (c) MFDM with higher k0k_0 value. The average grain size is ∼\sim one-tenth of the domain size mentioned in the plots.

Additionally, Figure 16b shows that as the domain size increases (with grain size maintained at one-tenth of the domain size), the size effect diminishes and eventually saturates. This behavior is consistent with experimental observations, where size effects become negligible in the limit of large grain sizes [77].

Microstructure evolution

We present results characterizing the possible microstructure evolution in the steel microstructure, with the aim of studying the dynamic behavior and failure mechanisms within the shear band. Adiabatic shear bands are often precursors to fracture in high-strain-rate applications such as ballistic impact, machining, crashworthiness. Understanding microstructure evolution spatially can help identify early signatures of localization before catastrophic failure, enabling better predictive models for structural integrity. The state variables used to describe this evolution are GND density (ρg\rho_g), material strength (gθg_\theta), the magnitude of the stress deviator (σ′\sigma'), and temperature (θ\theta). Fields are shown at overall strain levels of 0, 0.15, and 0.30, corresponding to the stress-strain response in Figure 13b. We will discuss these results.

GND evolution

The GND density is calculated using the measure

ρg=∣α∣b,\rho_g = \sqrt{\frac{|\boldsymbol{\alpha}|}{b}},

where bb is the magnitude of the Burgers vector. Figure 17 shows the spatial distribution of the GND density on a logarithmic scale. As shown in Figure 17(a) and mentioned earlier, the simulation begins with zero initial GND density throughout the polycrystal, i.e., no pre-existing GNDs are assumed within the grains or at the grain boundaries. Of course, the initial statistical dislocation density in the material is non-vanishing (17) and is given, for the 2-d simulations, by

Figure 17. Evolution of GND density plotted on a logarithmic scale (log⁡(ρg/ρˉs)\log(\rho_g/\bar{\rho}_s)) at applied strains of a) 0.0 b) 0.15 and c) 0.30.

ρˉs≈1.995×1015 m−2.\bar{\rho}_s \approx1.995 \times10^{15}\,m^{-2}.

As deformation proceeds, GND density accumulates near grain boundaries. This occurs because incompatibility in the SD plastic strain rate, Lp\mathbf{L}^{p}, acts as a source for the evolution equation for GND density (3a). MFDM theory imposes a jump condition on plastic strain rate (α×V+Lp\boldsymbol{\alpha} \times\mathbf{V} + \mathbf{L}^{p}) at interfaces where it may be discontinuous [6, 79]. This jump condition depends on all 5 grain boundary parameters and naturally produces a greater degree of blocking of plastic flow at interfaces with higher misorientation [79]. With continued shearing, this leads to greater GND accumulation within grains near grain boundaries, and patterned structures emerge within grain interiors.

Evolution of material strength

Figure 18 shows the evolution of material strength in the simulation. Initially, the strength field is uniform across the domain and remains so until the onset of plastic deformation as expected. Recall that, based on the macroscopic experimental results, Figure 9 and Figure 23, we do not consider any hardening due to the SDs, i.e., h0=0h_0 = 0, Table 2. MFDM captures hardening arising from GND accumulation, which serves as the sole source of spatial variation in strength. As the simulation proceeds, grain boundaries become progressively harder relative to grain interiors, consistent with the higher GND densities generated at these interfaces Figure 17.

Figure 18. Evolution of material strength (gθ/g0g_{\theta}/g_{0}) plotted at applied strains of a) 0.0 b) 0.15 and c) 0.30, where g0g_{0} is the initial yield strength.

Stress-strain response from the SHPB experiment and 3-d simulation

Figure 23. Stress-strain response from the SHPB experiment and 3-d simulation. The relatively darker portions in the simulation curve arise from the adaptive time-step cutback algorithm. This technique reduces the time-step size when the plastic strain increment exceeds a prescribed threshold, thus resulting in more dense data output.

The physical implication of this grain boundary hardening is that it creates a mechanical heterogeneity where boundaries act as barriers to dislocation motion, impeding plastic flow across grains. Nevertheless, this spatially localized hardening in concert with thermal softening produces no net hardening in the stress-strain response of the RVE (see Figure 13b, and Figure 16b) for domain sizes 40 μ\mum. and above.

Evolution of stress deviator

Subsequently, we present the microstructural evolution in terms of stress deviator, normalized by the material strength, as shown in Figure 19. Since plasticity is driven by resolved shear stress, which is directly related to the stress deviator, studying its evolution reveals which grains are more favorably oriented for slip and may act as potential failure sites. This also helps us understand differences in plastic strain rate within and across grains. Preferential plastic activity in certain grains reduces the local deviatoric stress due to stress relaxation from plastic deformation (when unconstrained by other kinematic constraints arising from grain boundaries or external boundary conditions).

Figure 19. Evolution of stress deviator plotted at applied strains of a) 0.0 b) 0.15 and c) 0.30.

Evolution of temperature

Figure 20 shows the evolution of the temperature field at applied shear strains of 0.0, 0.15, and 0.30. At the onset of deformation (Figure 20a), the temperature is uniformly distributed at the initial value of 290 K across the undeformed domain. At 0.15 applied shear strain (Figure 20b), the domain has undergone some shearing and the temperature field begins to exhibit heterogeneity, with localized regions of elevated temperature emerging in band-like patterns oriented roughly in the direction of shearing. By 0.30 applied strain (Figure 20c), these bands have intensified significantly, with peak temperatures reaching approximately 410 K. The temperature field at this stage displays a clear banded morphology, with zones of elevated temperature separated by regions that remain closer to the initial temperature. This spatially heterogeneous increase of temperature is a hallmark of adiabatic shear band formation: under the high strain rates considered here, conditions are effectively adiabatic, and the heat generated by plastic dissipation remains confined to the regions of intense shearing. The resulting local thermal softening further concentrates deformation into these bands, producing the characteristic feedback loop between plastic work, temperature rise, and strain localization that contributes adiabatic shear band development.

Figure 20. Evolution of normalized temperature (θ/θ0)(\theta/\theta_0) plotted at applied strains of a) 0.0 b) 0.15 and c) 0.30, where θ0=293\theta_0 = 293 K is the reference temperature.

Subgrain dislocation microstructure formation

Finally, we examine the formation of subgrain structures. Figure 17 reveals localized bands of elevated GND density, suggesting the emergence of intragranular dislocation substructures. To investigate

further, we examine a single grain under deformation and find that the spatial distribution of these GND bands closely aligns with the lattice orientation heterogeneity shown in Figure 22b. The lattice orientation, initially uniform within the grain, develops significant spatial variation over the course of the simulation. These emergent low-angle features resemble the Incidental Dislocation Boundaries (IDBs) observed experimentally by Hughes and Hansen [51] in cold-rolled Nickel in a quasistatic setting. To characterize the misorientation associated with these boundaries, we analyze a selected set of grains (labeled 1 - 6 in Figure 21), with the quantitative results summarized in Table 10. Additionally, Figure 22b highlights specific interfaces within a representative grain, defined by their misorientation angle and boundary normal, demonstrating substructure formation throughout the grain interior. The formation of such intragranular substructures is a pervasive feature observed throughout the entire polycrystalline domain.

Rotation angle field in the deformed configuration

Figure 21. Rotation angle field in the deformed configuration at an applied strain of 0.3. Grains analyzed for misorientation within the grain are marked.

Figure 22. Spatial distribution of the lattice orientation angle in degrees for grain 1 (marked in the Figure 21). (a) The initial undeformed configuration showing a uniform orientation. (b) The deformed configuration at an applied strain of 0.3 exhibiting significant lattice rotation and geometric distortion. The overlaid black lines indicate locations of subgrain boundaries, indicating formation of substructure within the grain.

Grain# Subgrain boundariesMisorientation distribution
00–2∘2^\circ22–5∘5^\circ55–11∘11^\circ>11∘>11^\circ
1132362
281331
392520
461320
582321
661320

Table 10. Subgrain boundary statistics for selected grains.

The substructure evolution observed in our simulations is also consistent with the early stages of rotational dynamic recrystallization, a mechanism first identified and extensively characterized by Meyers and coworkers [10] in their seminal studies of high-strain-rate deformation. They observed via TEM that shock-loaded copper deformed at strain rates of ∼104 s−1\sim10^{4}\ \mathrm{s}^{-1} developed elongated dislocation cells (∼0.1 μm\sim0.1\ \mu m width) that progressively broke down into equiaxed sub-grains and ultimately transformed into recrystallized grains with high-angle boundaries. Subsequently they demonstrated that this microstructural pathway, proceeding from dislocation tangles to elongated cells to sub-grains to recrystallized micrograins, operates across a range of materials including tantalum [76] and titanium [66]. The misorientations and GND localization patterns observed in our simulations appear to align with this well-established precursor stage. Experimental observations also reveal that, at early stages of deformation, the shear band microstructure is dominated by elongated blocks containing a well-defined low-angle boundary substructure with characteristic length scales on the order of ∼200\sim200–300 nm.300\ nm., which progressively evolves into an equiaxed nanograin structure with increasing deformation, as shown in Figure 6. Experimental observations also reveal the evolution of elongated grain structures, as shown in Figure 6. The grain structures predicted by our simulations appear to be qualitatively consistent with these experimental observations.

3-d simulations

We demonstrate the capability of the computational framework to simulate 3-d polycrystalline domains under dynamic loading. The computational domain is a cubic representative volume element. The simulation parameters are presented in Table 11. The polycrystalline microstructure is generated using a procedure developed and described in [89, 23], producing a statistically representative grain structure with orientations assigned to capture the crystallographic texture of the material. Figure 26a shows the polycrystalline microstructure used in the 3-d simulations, with grains colored by crystallographic orientation.

3-d
Domain size40×40×40 μm340 \times40 \times40\ \mu m^{3}
Elements1×1061 \times10^{6}
Strain reached0.40
Slip systems48
Nominal strain rate4×103 s−14 \times10^{3}\ \mathrm{s}^{-1}
Cores1024
Wall-clock time15 hrs

Table 11. Computational details for the 3-d MFDM simulations.

Figure 26. a) 3-d polycrystalline microstructure generated as [89, 23], with grains colored by crystallographic orientation. Field plots of the shear component F12F_{12} are shown at an applied strain of 0.3 for b) Classical crystal plasticity and c) MFDM.

In 3-d, 48 slip systems are used to characterize the BCC crystal. The slip systems used are:

  • 24 {123}\{123\} planes with one ⟨111⟩\langle111\rangle direction.

  • 12 {112}\{112\} planes with one ⟨111⟩\langle111\rangle direction.

  • 6 {110}\{110\} planes with two ⟨111⟩\langle111\rangle directions.

Boundary conditions for the velocity, shown in Figure 24b (and mentioned in 13) are specified as follows: periodic boundary conditions are applied on the lateral faces in the xx and yy directions to approximate an infinite medium. The front and back faces (zz-normal) are traction-free in the xx-yy plane, and motion in the zz-direction is constrained on these faces. On the top and bottom faces, prescribed shear velocities are applied in the horizontal direction, while multi-point constraints (MPCs) enforce uniform vertical displacement to maintain planarity. The initial GND density is set to zero throughout the domain, and the applied nominal strain rate is 4000 s−1\mathrm{s}^{-1}.

Figure 24. Boundary conditions for the 3-d simulations. (a) Uniaxial compression used for calibration (b) Shearing with periodic boundary conditions on lateral faces used for simulating a shear band. Details of these boundary conditions on lateral faces are listed in Table. Table 12 and Table. Table 13

BoundaryTypeCondition
TopPrescribed velocityvx=v1=AH/2v_x = v_1 = AH/2, uniform vyv_y via MPC, tz=0t_z = 0
BottomPrescribed velocityvx=v1=−AH/2v_x = v_1 = -AH/2, uniform vyv_y via MPC, tz=0t_z = 0
Left and RightPeriodic BCVelocity periodicity in xx and yy, tz=0t_z = 0
Front and BackPeriodic BCVelocity periodicity in xx and yy, vz=0v_z = 0

Table 13. Boundary conditions applied to simulate a shear band in 3-d.

To make these large-scale 3-d simulations computationally tractable, we employ the dimensional analysis approach described in § 4.2. By simultaneously scaling the applied strain rate and reference plastic strain rate by the same factor while keeping their ratio fixed, we achieve the same mechanical response in fewer time steps without altering the underlying physics. This reduced the wall-clock time by approximately an order of magnitude, enabling simulations that would otherwise require several days to be completed in a few of hours. The exact number of cores used along with the time for the simulation is mentioned in Table 9 and Table 11.

2-d
Domain size80×80 μm280 \times80\ \mu m^2
Elements25×10425 \times10^4
Strain reached1.80
Slip systems3
Nominal strain rate4×103 s−14 \times10^3\ \mathrm{s}^{-1}
Cores512
Wall-clock time8 hrs

Table 9. Computational details for the 2-d MFDM simulations.

Calibration for 3-d simulations: As in the 2-d case, we calibrate the model against the experimental stress-strain curve from a dynamic compression test on a cylindrical specimen performed using the SHPB, with boundary conditions as described in § 4.2. Zero traction is imposed on the boundaries where there is no velocity boundary condition, to approximate homogeneous uniaxial compression conditions (Figure 24a and Table 12). Since the 3-d model includes all 48 BCC slip systems rather than the reduced set used in 2-d, the material parameters required recalibration; the resulting stress-strain curve is shown in Figure 23.

BoundaryTypeCondition
TopVelocity and tractionvy=vlv_y = v_l, tx=0t_x = 0, tz=0t_z = 0
BottomVelocity and tractionvy=vrv_y = v_r, tx=0t_x = 0, tz=0t_z = 0
Front and BackTraction-freet=0\mathbf{t} = 0
Left and RightTraction-freet=0\mathbf{t} = 0

Table 12. Boundary conditions applied for the 3-d calibration.

The classical hardening modulus h0h_0 is again set to 0 and the initial strength is taken as g0=0.40 GPag_0 = 0.40\,\mathrm{GPa}. The estimate of the initial statistical density for the 3-d simulations is then given by

ρˉs=(g0/ημb)2≈1.576×1015 m−2.\bar{\rho}_s = (g_0/\eta\mu b)^2 \approx1.576 \times10^{15}\,m^{-2}.

vyv_y: yy-component of velocity; vlv_l, vrv_r: prescribed velocities at the left and right boundaries from SHPB data; txt_x, tzt_z: traction components in the xx- and zz-directions; t\mathbf{t}: traction vector.

The CCP and MFDM approaches are studied next in 3-d simulations of adiabatic shear banding. The comparison is carried out along two lines: first, we examine the average stress-strain response obtained from both models and its sensitivity to mesh refinement; second, we analyze the spatial field distributions to investigate the nature of strain localization and the ability of each model to predict the experimentally observed finite width of adiabatic shear bands. We then examine microstructure evolution through the GND density, and material strength. Without access to sophisticated tools for inferring localized 2-d field concentrations in 3-d regions of the simulated body, we attempt to provide some rationalization for the potential formation of 2-d subgrain boundaries within the 3-d shear band region in the simulations.

vxv_x, vyv_y, vzv_z: components of the velocity vector; AA: applied strain rate; HH: height of the RVE; tzt_z: traction component in the zz-direction; MPC: multi-point constraint enforcing uniform vertical displacement across the boundary. The loading is applied as a step in time, with the velocity equal to zero at t=0t = 0 and held constant for all subsequent times.

Stress strain response of 3-d sample

Before examining the localization patterns, we first verify mesh convergence of the stress-strain response under progressive mesh refinement, with mesh densities of 25, 50, and 100 elements per direction. As shown in Figure 25b, the MFDM stress-strain curves remain nearly unchanged across these mesh densities, confirming mesh-independent behavior in 3-d. In contrast, the CCP formulation exhibits continued non-convergence with refinement, with the response changing as the mesh is refined, as shown in Figure 25a.

Three plots showing 3-d simulation results: stress-strain responses for CCP and MFDM on meshes of 25^3, 50^3, and 100^3 elements, and size-dependent strengthening for self-similarly scaled domains

Figure 25. 3-d simulation results: stress-strain response for (a) CCP and (b) MFDM on meshes of 25325^3, 50350^3, 1003100^3 elements and (c) size-dependent strengthening predicted by MFDM for self-similarly scaled domains.

Figure 26 presents the shear component F12F_{12} of the deformation gradient for both CCP and MFDM in the 3-d domain. Consistent with the 2-d results, CCP exhibits pronounced strain localization into narrow bands, while MFDM produces a more distributed deformation field throughout the domain. The 3-d simulations confirm that the mesh-independent behavior observed in 2-d extends to three dimensions, further demonstrating the capability of the MFDM framework for capturing finite shear band widths.

The 3-d simulations also reproduce the size-dependent strengthening behavior discussed in the 2-d setting (§ 5.3). Figure 25c shows results from a series of 3-d simulations in which the domain is self-similarly scaled from 10 to 160 μ\mum, maintaining a constant grain-to-domain size ratio of approximately 1/10. As in 2-d, CCP predicts an identical stress-strain response regardless of domain size, while MFDM captures a clear “smaller is stronger” trend arising from the GND density contribution to hardening. The size effect again diminishes with increasing domain size and saturates as the size of the grains increases. This is consistent with both the 2-d predictions and experimental observations [77, 15].

Microstructure evolution

The evolution of GND density in the 3-d simulations, shown in Figure 27, follows trends qualitatively similar to those observed in 2-d. Starting from a dislocation-free initial state, GND density accumulates progressively at grain boundaries due to the intergranular plastic strain rate jump condition imposed across interfaces, while patterned structures emerge within grain interiors (Figure 28). Two notable distinctions arise in the 3-d case: first, the magnitude of the GND density is significantly higher due to the possible activation of all 48 slip systems; second, the subgrain structures that form exhibit a fully three-dimensional character.

Evolution of GND density at applied shear strains 0.0, 0.15, and 0.30

Figure 27. Evolution of GND density plotted on a logarithmic scale (log⁡(ρg/ρˉs)\log(\rho_g/\bar{\rho}_s)) at applied shear strains of a) 0.0 b) 0.15 and c) 0.30.

Figure 28. GND density distribution on interior cross-sectional planes of the 3-d domain at applied shear strain of 0.30: (a) x=0x = 0, (b) y=0y = 0, and (c) z=0z = 0 plane.

The material strength field, shown in Figure 29, is initially uniform and develops spatial heterogeneity as deformation proceeds, with grain boundaries hardening relative to grain interiors.

Evolution of normalized material strength at applied shear strains 0.0, 0.15, and 0.30

Figure 29. Evolution of normalized material strength (gθ/g0g_\theta/g_0) plotted at applied shear strains of a) 0.0 b) 0.15 and c) 0.30, where g0=0.40 GPag_0 = 0.40\,\mathrm{GPa} is the initial yield strength.

Figure 30 shows the corresponding temperature evolution for the 3-d simulation. The overall progression is qualitatively similar to the 2-d case, with a uniform initial temperature field (Figure 30a) giving way to thermal bands at 0.15 (Figure 30b) and 0.30 (Figure 30c) applied shear strain. Peak temperatures again reach approximately 410 K, and hot spots with temperatures exceeding the surrounding band are visible on the surface.

Figure 30. Evolution of normalized temperature (θ/θ0\theta/\theta_0) plotted at applied shear strains of a) 0.0 b) 0.15 and c) 0.30, where θ0=293 K\theta_0 = 293\,K is the reference temperature.

Subgrain dislocation microstructure formation

Analogous to the 2-d case, substructure formation is observed within individual grains in the 3-d polycrystal simulation as well. Unlike the planar substructure seen in 2-d, however, the substructure in 3-d is non-planar in nature, manifesting as 3-d subgrain formation within the grain interior. To illustrate this, we isolate a single grain from the polycrystal, which, as marked in Figure 31a, begins the simulation with a nominally uniform crystallographic orientation. Following deformation, the GND density distribution within this grain is presented in Figure 31b, revealing the emergence of GND in the grain interior. This can be treated as a signature of subgrain formation. A zoomed view is provided in Figure 32 for additional clarity. Importantly, this substructure formation is not isolated to a single grain but is observed throughout the polycrystal domain, with the subgrain

Figure 31. (a) Rotation angle field on three cross-sections of the 3-d polycrystal showing the initial grain structure. The grain selected for discussion in Figure 32 is marked. (b) GND density distribution within the isolated grain at an applied strain of 0.3, pointing to a potential non-planar subgrain substructure within the grain.

Figure 32. Zoomed view of (a) the rotation angle field and (b) the GND density distribution within an isolated grain from the polycrystalline assembly marked in Figure 31, at an applied strain of 0.3.

structure becoming more pronounced with increasing deformation.

Non-localization under boundary and initial conditions corresponding to nominally homogeneous deformation

The experimental observations (Figure 6) corresponding to macroscopic top-hat experiments reveal that localized bands of deformation fall within a size range of 10 μm−40 μm10\,\mu m - 40\,\mu m under dynamic loading conditions. We extend MFDM simulations on the selected RVE (Figure 11) of size 80 μm280\,\mu m^2 to significantly higher strains compared to the discussion in § 5.2 to investigate whether further localization or stress softening emerges beyond the initially observed response. A convergence study is performed using differently meshed domains, and the results remain converged to a fair degree considering the large overall strains involved, as shown in Figure 33a. The local shear strain reaches values as high as 3.00 at an applied/average nominal engineering shear strain of 1.50. Even at these higher strains, no further localization develops, as shown in Figure 33b, nor does any softening appear in the stress-strain response. Contrast in F12F_{12} is visible across the domain and is likely influenced by the presence of a relatively large grain (homogeneous material) in the microstructure. The temperature, GND density, and material strength profiles at 1.50 applied shear strain are shown in Figure 34.

Figure 33. Extended MFDM simulation results. (a) Normalized stress-strain response (τ/g0\tau/g_0 vs. Γ\Gamma) for three mesh resolutions (1002100^2, 2002200^2, and 4002400^2), demonstrating converged behavior up to 1.70 applied strain with no observed softening. (b) F12F_{12} field at 1.50 strain, showing no further localization.

Figure 34. (a) Temperature, (b) GND density field, and (c) material strength (GPa) shown at 1.50 applied strain.

Under the controlled boundary conditions for nominally homogeneous deformation (for a homogeneous material under quasi-static loading) as used in this study, it is not clear whether softening observed in macroscopic experiments should be expected here in the absence of ductile damage mechanism in the model; note the reductions in material strength observed within the band (Figure 34b), which can possibly serve as sites for ductile damage nucleation. For the domain size and material properties considered, our model, which does not incorporate any damage mechanism, predicts no softening.

We have been able to produce cases in which MFDM exhibits softening in the polycrystal stress-strain response by increasing the value of the Taylor–Quinney factor (κ\kappa) or reducing the value of the GND hardening parameter (k0k_0). For certain values of the κ\kappa and/or k0k_0, softening is observed; however, mesh convergence of the solution was not observed for the meshes considered, although the performance was much improved in comparison to the corresponding classical plasticity simulations. This suggests that there may exist a range of the parameters κ\kappa and k0k_0 where softening with mesh convergence may be observed; the discussion at the end of the following paragraph illustrates another facet of this issue, even without any material parameter adjustment. Such matters are left for future study.

We note here that the dynamic nature of the loading induces a higher stress at the center of the domain where the stress waves from the top and bottom boundaries meet, leading to spatially heterogeneous yielding. However, as is observed, this heterogeneity is not sufficient to induce a persistent shear band with progressive loading in MFDM, in contrast to CCP. This trend persists even for the J2J_2-MFDM model of plasticity as shown in Figure 35 where the polycrystalline aggregate is treated as an effectively homogeneous material (with no corresponding initialization of a grain microstructure). In this latter scenario, a distinct sequence of bands emerge in the shear component F12F_{12} of the deformation gradient. At 0.15 applied shear strain (Figure 35a), F12F_{12} concentrates into a narrow band at the center of the domain, which persists as the dominant feature. As loading continues to 0.60 applied strain (Figure 35b), this central band remains intact while slip-band-like structures begin to emerge on either side of it, spreading outward from the center. By 0.90 strain (Figure 35c), these structures homogenize over the domain, with contrast of high strain to average strain remaining approximately uniform with progress of loading. This trend towards greater homogeneity in deformation is accompanied with a gradual, mesh-converged, softening response as shown in Figure 36b, in contrast to the corresponding non-convergence of the classical plasticity response for the same problem shown in Figure 36a. The gradual softening in the J2J_2-MFDM simulation arises due to the spatially-extended thermal softening following from delocalized plastic straining and the lesser degree of hardening due to reduced GND accumulation because of the absence of grain boundaries, as compared to the MFDM response accounting for the grain microstructure. It is worth noting that this relative decrease in GND accumulation in J2J_2-MFDM occurs even though the model equations contain the same GND hardening term and enforce a common jump condition at surfaces of discontinuity in the total plastic strain rate, α×V+Lp\boldsymbol{\alpha} \times\mathbf{V} + \mathbf{L}^{p}, were they to exist.

(a)

Evolution of the shear component $F_{12}$ for the $J_2$ model at 0.60 applied shear strain

(b)

Evolution of the shear component $F_{12}$ for the $J_2$ model at 0.90 applied shear strain

(c)

Figure 35. Evolution of the shear component F12F_{12} of the deformation gradient for J2J_2 model at (a) 0.15, (b) 0.60, and (c) 0.90 applied shear strain, showing the stages in which a central band forms and persists, before spreading outward into slip-band-like structures. The color bars for the sub-figures span different ranges.

Taken together, these results attest to the strong stabilizing and homogenizing effects of the GND hardening in MFDM, and the kinematically fundamental nature of GND accumulation in the theory, rooted in a conservation law for Burgers vector content.

Localization under boundary conditions corresponding to nominally homogeneous deformation with a spatial perturbation in the initial yield stress

For the boundary conditions and initial conditions considered so far, MFDM does not produce further localization or softening. We now probe the response of MFDM under a different set of initial conditions and, in one case, also of geometry.

A common approach in physical experiments and related modeling for studying localization is to utilize a perturbation in the initial conditions or in the geometry of the domain to induce heterogeneity [29, 39] (e.g., shear band studies in a torsional Kolsky bar experiment). Following this approach, we prescribe a reduced initial yield strength in a horizontal layer near the center of the domain, as shown in Figure 37b. All other aspects of the simulation, including the

Figure 37. (a) Normalized stress-strain response (τ/g0\tau/ g_0 vs. Γ\Gamma) for MFDM and classical crystal plasticity (CCP) at two mesh resolutions (1002100^2 and 2002200^2); CCP results exhibit mesh dependence, whereas MFDM remains converged. (b) Initial yield strength (g0g_0) distribution showing the reduced-strength perturbation layer near the center of the domain. (c) Temperature field at an applied strain of 0.3, showing localization of deformation into a well-defined band within the MFDM framework.

Stress-strain curves for classical $J_2$ plasticity

(a)

Stress-strain curves for $J_2$-MFDM

(b)

Figure 36. Stress-strain curves for (a) classical J2J_2 plasticity, and (b) J2J_2-MFDM, for three mesh resolutions of 1002100^2, 2002200^2, 4002400^2 elements.

applied strain rate and the slip system configuration, remain as described in § 5.1. Simulations are performed using both MFDM and classical crystal plasticity (CCP). For a case shown in Figure 38c, the geometry and initial grain microstructure are self-similarly scaled to a domain size of (40μm)2(40\mu\mathrm{m})^2.

Figure 38. F12F_{12} field for different perturbation layer widths and domain sizes. (a) Perturbation layer width of 10 μ\mum in an 80 μ\mum domain, resulting in a shear band width of approximately 7.5 μ\mum. (b) Perturbation layer width of 6 μ\mum in an 80 μ\mum domain, resulting in a shear band width of approximately 5 μ\mum. (c) Perturbation layer width of 10 μ\mum in a 40 μ\mum domain with a shear band width of 6.8 μ\mum. Fields in (a) and (b) are shown at an applied shear strain of ∼0.8\sim0.8, while (c) is shown at an applied shear strain of ∼1.1\sim1.1.

We observe that the CCP results do not converge with mesh refinement, whereas MFDM yields a mesh-converged response, as shown in Figure 37a.

More importantly, for this type of spatial perturbation in the initial yield stress, localization is observed in MFDM as shown in Figure 38 (a,Figure 38b,Figure 38c), in contrast to the considerations of § 5.14.

We explore some features of this localization w.r.t. the length scales present in the problem. Dimensional analysis suggests that the normalized shear band width Wb/bW_b/b can depend on the following ratios related to length-scales (along with other non-dimensional numbers of the model):

Wbb=f(bH,bSg,Wpb,…),\frac{W_b}{b}=f\left(\frac{b}{H},\frac{b}{S_g},\frac{W_p}{b},\ldots\right),

where HH is the domain size, SgS_g is the average grain size, WpW_p is the perturbation layer width, and bb is the Burgers vector.

We first examine the effect of the ratio related to the perturbation width by varying Wp/bW_p/b while holding b/Hb/H and b/Sgb/S_g fixed. In Figure 38 (a) and (Figure 38b), the predicted band is narrower than the imposed perturbation layer: a Wp=10 μmW_p=10\ \mu\mathrm{m} perturbation in an 80 μm80\ \mu\mathrm{m} domain produces a band of approximately 7.5 μm7.5\ \mu\mathrm{m}, while reducing the perturbation to Wp=6 μmW_p=6\ \mu\mathrm{m} in the same domain yields a band of approximately 5 μm5\ \mu\mathrm{m}.

We next vary b/Sgb/S_g (and correspondingly b/Hb/H, by self-similar scaling of grain microstructure) while holding Wp/bW_p/b fixed. The expectation that the increase in this raio with bb fixed should result in stronger and more stable response is borne out in the simulations. Comparing the results of Figure 38a and Figure 38c corresponding to the average grain size being halved with Wp=10 μmW_p=10\ \mu\mathrm{m} kept fixed, the predicted band width in Figure 38a is 7.5 μm7.5\ \mu\mathrm{m} whereas in Figure 38c the band width is 6.8 μm6.8\ \mu\mathrm{m} respectively, i.e., essentially unchanged. However, we note that as b/Sgb/S_g increases for WpW_p fixed, the strain contrast between the band and its surroundings is reduced, as visible in Figure 38c compared to Figure 38(a,Figure 38b).

MFDM does not produce any softening in the stress-strain response in these simulations as well; instead, a stable flow stress is maintained. The temperature in the domain does rise to values as high as approximately 650 K650\ \mathrm{K}, as shown in Figure 37c. However, a competition between GND hardening and thermal softening results in a stable flow response for the material properties and boundary conditions considered here.

Structural softening and localization – J2J_2-MFDM

For the simulations presented in this Section, we employ the J2J_2-MFDM constitutive model (§ 2.2) within the MFDM framework. A polycrystalline microstructure is not initialized in the full domain, as sufficient information to do so is unavailable; however, the computational cost would remain comparable even if such information were available.

Here we demonstrate the ability of MFDM to capture localization into a finite-width band accompanied by softening in the structural response for a geometry and boundary conditions favoring heterogeneous deformation. The simulation is motivated by the idea of the macroscopic top-hat compression test for concentrating deformation. We use a tensile loading to avoid problems with contact, since our main concern here is to explore a point of principle about the model. We also consider a relatively larger domain than the RVEs previously selected (§ 5.1).

The specimen geometry consists of two rectangular blocks connected through a narrow section, as shown in Figure 39. The left block has dimensions 200×200 μm2200\times200\ \mu\mathrm{m}^2 and the upper-right block

Specimen geometry and boundary conditions

Figure 39. Specimen geometry and boundary conditions. Rollers on the bottom boundary constrain vy=0v_y = 0; rollers on the right boundary constrain vx=0v_x = 0. The top boundary of the upper-right block is pulled upward with prescribed velocity vy=v(t)v_y = v(t). All other boundaries are traction-free.

Force-displacement curve for the softening regime

Figure 40a.

Force-displacement curve beyond initial softening

Figure 40b.

200×200 μm2200 \times200\ \mu\mathrm{m}^{2}. The two blocks are offset vertically by 50 μm50\ \mu\mathrm{m} and overlap horizontally over a 20 μm20\ \mu\mathrm{m} wide strip, creating a narrow neck of 20×50 μm220 \times50\ \mu\mathrm{m}^{2} where localization is forced in order to accommodate the loading. The total specimen width is 380 μm380\ \mu\mathrm{m} and the overall height is 350 μm350\ \mu\mathrm{m}.

The boundary conditions (shown in Figure 39) are chosen to promote localization through the connector region. On the bottom boundary of the left block the vertical velocity is constrained to vanish (vy=0v_y = 0) while leaving the horizontal direction free. On the right boundary of the upper-right block, the horizontal velocity is constrained to vanish (vx=0v_x = 0) while leaving the vertical direction free. The top boundary of the right block is subjected to a prescribed velocity in the yy-direction with a rough applied strain rate of 4×103 s−14 \times10^{3}\ \mathrm{s}^{-1}, pulling the right block upward relative to the vertically constrained left block. All remaining boundaries are traction-free. This loading configuration produces a state of combined tension and shear in the narrow connector, promoting strain localization in the predetermined region.

The reaction force, normalized by the product of the cross-sectional area (SS) and the initial yield strength (g0g_0), is plotted against the displacement of the top boundary of the right block in Figure 40a. A clear softening response is observed in the force-displacement curve. Furthermore, this softening behavior is shown to be converged across two levels of mesh refinement, with the coarser mesh containing approximately 50k elements and the finer mesh approximately 200k elements.

Figure 40. Force-displacement curve shown for (a) the softening regime and (b) beyond initial softening. The coarse mesh has approximately 50k elements and the fine mesh approximately 200k elements. Here, FF is the reaction force on the top-right boundary, and SS and g0g_0 are the cross-sectional area and initial yield strength, respectively. The oscillations arise from elastic wave reflections due to the small domain size and the specific boundary conditions employed.

Mesh convergence and band width

To assess whether MFDM produces mesh-convergent localization, we perform a series of simulations with progressively refined meshes while keeping all other parameters fixed. The deformation is characterized in terms of the norm of the logarithmic strain tensor ∣ln⁡V∣\lvert\ln V \rvert, where VV is the left stretch tensor obtained from the left polar decomposition of the deformation gradient F=VR\mathbf{F} = \mathbf{V}\mathbf{R}, defined with respect to the initial configuration at t=0t = 0.

Figure 41 shows the spatial distribution of ∣ln⁡V∣\lvert\ln V \rvert in the deformed configuration for the two mesh refinements. In both cases, deformation localizes into a band within the narrow connector. The key observation is that both the width of the localized band and the magnitude of ∣ln⁡V∣\lvert\ln V \rvert within the band remain approximately unchanged across mesh resolutions. This demonstrates that MFDM provides mesh-convergent predictions of localization, including the a finite width of the deformation band.

Spatial distribution of the norm of the logarithmic strain tensor in the deformed configuration for two successively refined meshes

Figure 41. Spatial distribution of ∣ln⁡V∣\lvert\ln V \rvert in the deformed configuration for two successively refined meshes, with the element size halved between refinements. The width (approx. ∼15 μm\sim15\,\mu\mathrm{m}) and intensity of the localized band remain essentially unchanged, demonstrating mesh convergence of the localized solution.

The converged band width is approximately 15 μm15\,\mu\mathrm{m}, governed by the interplay between the intrinsic length scale of MFDM (through the Burgers vector and the GND hardening coefficient k0k_0), the applied loading, and thermal softening. Thus, MFDM naturally produces a finite-width localized band when the domain is sufficiently large, and predicts softening in the structural response when the geometry and loading conditions permit it.

Conclusion

Adiabatic shear bands involve complex microstructural changes that are difficult to resolve experimentally at the mesoscopic length scale. Informed by Split Hopkinson Pressure Bar experiments for dynamic shear banding, we studied the phenomenon through theory and simulation. A dimensional analysis was employed to make our mesoscale simulations computationally tractable, especially the large-scale 3-d simulations presented in this work.

Finite width of adiabatic shear bands, consistent with experimental observations, were obtained as part of our results. In the absence of heat conduction, the effect of thermal softening was balanced by GND hardening in our simulations, suggesting a mechanism for the finite widths of the bands. Dislocation substructure formation was also observed, with similarity to experimental observations reported in the literature. A comparison between classical crystal plasticity (CCP) and MFDM demonstrated the well-known mesh-dependent strain localization in CCP into increasingly narrow bands upon refinement. MFDM yielded mesh-convergent fields and stress-strain response across all mesh resolutions tested, in both 2-d and 3-d.

Size-dependent strengthening was observed for grain sizes ranging from 1 to 20 μm\mu m, with the effect saturating as the size was increased. Low-angle subgrain boundaries formed within grain interiors, with misorientations consistent with Incidental Dislocation Boundaries observed in deformed metals. These boundaries correlated spatially with GND density patterns, confirming that dislocation accumulation drives microstructural refinement during shear band formation.

The response of the MFDM theory/model was probed under different combinations of boundary conditions, initial conditions, and geometry to assess when localization and softening emerge. Under boundary conditions corresponding to nominally homogeneous deformation (for a homogeneous material deforming quasi-statically), MFDM predicts no further localization or softening even when the simulation was extended to shear strains as high as 300% (locally), as the competition between GND hardening and thermal softening sustained a stable flow response in the absence of a damage mechanism. A boundary condition-induced stress heterogeneity was not found to be sufficient to form a persistent shear band in MFDM.

When a spatial perturbation in the initial yield stress was introduced, MFDM yielded a mesh-converged localized band whereas classical crystal plasticity did not. Within the material parameter range probed, mesh convergent strain localization with softening was not obtained in MFDM with thermal softening (in the absence of other ductile damage mechanisms in the model).

For a top-hat-inspired geometry simulated with J2J_2-MFDM, the model captured finite-width localization of approximately 15 μm\mu m together with a clear, mesh-convergent softening response in the force-displacement curve. These results demonstrate that MFDM produces finite-width bands and structural softening when the geometry and loading conditions permit heterogeneous deformation, while remaining stable under nominally homogeneous loading conditions, without recourse to ad-hoc/physically dubious regularization mechanisms.

These results provide a mechanistic picture of microstructure evolution within adiabatic shear bands, from GND accumulation and strength heterogeneity to subgrain boundary formation, and establish a framework for further investigation of shear localization in polycrystalline metals.

With regard to advancing theory and simulation tools for the study of plasticity, our concern here has mainly been the study of plasticity problems on smaller scales where (R)MFDM has been validated against experiments relating to size effects and patterning. The approach has been quite successful in addressing a broad array of problems in modern plasticity theory, including size-dependent strengthening and the “smaller is stronger” trend observed in micron and sub-micron scale experiments (thin films, micropillar compression), orientation-dependent mechanical response in confined thin films, spontaneous dislocation patterning and microstructure emergence without introducing non-convexity in the energy, kink band formation in Cu-Nb nanometallic laminates enabled by natural jump/interface conditions, slip transmission constraints at grain boundaries, directionality of the sharp yield point and Lüders-type behavior in strain-aged steels, intermittent plasticity associated with dislocation transport, grain size effects on work hardening in polycrystals, and particle size and interlacing effects on the mechanical response of metal-matrix composites [AA20b, AA20a, AZA20, [3, 4, 81, 6, 80, 63, 44, 78, 79, 34, 45, 91, 90, 85, 92, 41, 94, 38, 26, 49]. This study is the first application of the MFDM framework to the modeling of shear banding phenomena.

Together with the above list of validations, this work establishes MFDM as a framework that passes critical experimental tests of theory posed in the research community for modeling mesoscale plasticity and associated length-scale dependent phenomena. At the level of constitutive specification, it does so with a minimalistic adjustment beyond a basic, and well-accepted, model of classical plasticity.

However, it is to be recognized, as we do, that the mechanisms of strengthening and softening reflected in the constitutive statements we have utilized (Table 3, Eqns. (9), (11) and (12)) are at best rudimentary vis-a-vis capturing the averaged mesoscale behavior of dislocation interactions and energy dissipation, and the softening of elastic moduli at high (and low) temperatures. In the absence of serious, ground-up theoretical understanding of such (very challenging) coarse-graining issues as they pertain to strongly nonlinear, time-dependent thermomechanical plastic response, we have let simplicity guide our constitutive choices for engineering purposes and qualitative understanding, with obvious room for improvement from the research community interested in such matters (but hopefully not through the use of more and more complicated ad-hoc kinematic and empirical constitutive assumptions).

Finally, our framework for 3-d, finite deformation, dynamic simulations of statistically representative RVE with a state-of-the-art model for mesoscale response of polycrystalline aggregates sets the stage for computationally efficient, large-scale statistical data collection of the detailed (thermo)mechanical response of metallic materials to inform coarser scale models, e.g. a principled way of including a grain size effect in the macroscopic response of polycrystalline materials valid for a wide range of grain sizes.

Acknowledgment

This work was supported by the Army Research Laboratory funded Center for Extreme Events in Structurally Evolving Materials (contract W911NF2320073). Generous grants of computer time from the NSF ACCESS program through the Pittsburgh Supercomputing Center are acknowledged.

References

  1. [1]R. Arora and A. Acharya. Dislocation pattern formation in finite deformation crystal plasticity. International Journal of Solids and Structures, 184:114–135, 2020. Physics and Mechanics of Random Structures: From Morphology to Material Properties. doi: 10.1016/j.ijsolstr.2019.02.013.DOI
  2. [2]R. Arora and A. Acharya. A unification of finite deformation J₂ von-Mises plasticity and quantitative dislocation mechanics. Journal of the Mechanics and Physics of Solids, 143:104050, 2020. doi:10.1016/j.jmps.2020.104050.DOI
  3. [3]A. Arora, R. Arora, and A. Acharya. Mechanics of micropillar confined thin film plasticity. Acta Materialia, 238:118192, 2022. doi:10.1016/j.actamat.2022.118192.DOI
  4. [4]A. Arora, R. Arora, and A. Acharya. Interface-dominated plasticity and kink bands in metallic nanolaminates. Crystals, 13(5), 2023. doi:10.3390/cryst13050828.DOI
  5. [5]A. Acharya and A. J. Beaudoin. Grain-size effect in viscoplastic polycrystals at moderate strains. Journal of the Mechanics and Physics of Solids, 48(10):2213–2230, 2000.DOI
  6. [6]A. Acharya. Jump condition for GND evolution as a constraint on slip transmission at grain boundaries. Philosophical Magazine, 87(8-9):1349–1359, 2007. doi:10.1080/14786430600951537.DOI
  7. [7]A. Acharya. Microcanonical entropy and mesoscale dislocation mechanics and plasticity. Journal of Elasticity, 104(1-2):23–44, 2011.
  8. [8]E. C. Aifantis. The physics of plastic deformation. International journal of plasticity, 3(3):211–247, 1987.
  9. [9]L. Anand, K. H. Kim, and T. G. Shawki. Onset of shear localization in viscoplastic solids. Journal of the Mechanics and Physics of Solids, 35:407, 1987.
  10. [10]U. Andrade, M. A. Meyers, K. S. Vecchio, and A. H. Chokshi. Dynamic recrystallization in high-strain, high-strain-rate plastic deformation of copper. Acta Metallurgica et Materialia, 42:3183–3195, 1994.DOI
  11. [11]Lallit Anand. Single-crystal elasto-viscoplasticity: application to texture evolution in polycrystalline metals at large strains. Computer Methods in Applied Mechanics and Engineering, 193(48):5359–5383, 2004. Advances in Computational Plasticity.DOI
  12. [12]A. Acharya and A. Roy. Size effects and idealized dislocation microstructure at small scales: predictions of a phenomenological model of mesoscopic field dislocation mechanics: Part I. Journal of the Mechanics and Physics of Solids, 54(8):1687–1710, 2006.DOI
  13. [13]R. J. Asaro. Micromechanics of crystals and polycrystals. Advances in Applied Mechanics, 23:1–115, 1983.DOI
  14. [14]R. Arora, X. Zhang, and A. Acharya. Finite element approximation of finite deformation dislocation mechanics. Computer Methods in Applied Mechanics and Engineering, 367:113076, 2020. doi:10.1016/j.cma.2020.113076.DOI
  15. [15]A. J. Beaudoin, A. Acharya, S. R. Chen, D. A. Korzekwa, and M. G. Stout. Consideration of grain-size effect and kinetics in the plastic deformation of metal polycrystals. Acta Materialia, 48(13):3409–3423, 2000. doi:10.1016/S1359-6454(00)00136-1.DOI
  16. [16]Y. L. Bai. A criterion for thermo-plastic shear instability. In Proc. Int. Conf. on Metallurgical Effects of High-Strain-Rate Deformation and Fabrication, editors, Shock Waves and High-Strain-Rate Phenomenon in Metals, page 277, Albuquerque, NM, 1981. Plenum Press.
  17. [17]Y. L. Bai. Thermo-plastic instability in simple shear. Journal of the Mechanics and Physics of Solids, 30:195, 1982.DOI
  18. [18]G. I. Barenblatt. Scaling, Self-Similarity, and Intermediate Asymptotics. Cambridge University Press, Cambridge, 1996.
  19. [19]C. A. Bronkhorst, E. K. Cerreta, Q. Xue, P. J. Maudlin, T. A. Mason, and G. T. Gray. An experimental and numerical study of the localization behavior of tantalum and stainless steel. International Journal of Plasticity, 22(7):1304–1335, 2006. doi: 10.1016/j.ijplas.2005.10.002.
  20. [20]C. A. Bronkhorst, E. K. Cerreta, Q. Xue, P. J. Maudlin, T. A. Mason, and G. T. Gray III. An experimental and numerical study of the localization behavior of tantalum and stainless steel. International Journal of Plasticity, 22:1304–1335, 2006.DOI
  21. [21]C. A. Bronkhorst, B. L. Hansen, E. K. Cerreta, and J. F. Bingert. Modeling the microstructural evolution of metallic polycrystalline materials under localization conditions. Journal of the Mechanics and Physics of Solids, 55:2351–2383, 2007.DOI
  22. [22]C. A. Bronkhorst, S. R. Kalidindi, and L. Anand. Polycrystalline plasticity and the evolution of crystallographic texture in fcc metals. Philosophical Transactions of the Royal Society of London, Series A: Physical and Engineering Sciences, 341(1662):443–477, 12 1992.DOI
  23. [23]P. Behnoudfar, D. N. Ponnana, N. J. Schmelzer, J. Wanni, G. T. Gray III, D. J. Thoma, C. A. Bronkhorst, N. Chen, and W. Pan. Split-pinn: Separable probability learning technique via physics-informed neural networks for high-dimensional probabilistic modeling. Journal of the Mechanics and Physics of Solids, Under revision, 2026.arxiv.org/abs/2606.04000
  24. [24]C. A. Bronkhorst, A. R. Ross, B. L. Hansen, E. K. Cerreta, and J. F. Bingert. Modeling and characterization of grain scale strain distribution in polycrystalline tantalum. Computers, Materials, & Continua, 17:149–174, 2010.DOI
  25. [25]T. J. Burns and T. G. Trucano. Instability in simple shear deformations of strain-softening materials. Mechanics of Materials, 1:313, 1982.DOI
  26. [26]S. Berbenni, V. Taupin, and R. A. Lebensohn. A Fast Fourier Transform-based mesoscale field dislocation mechanics study of grain size effects and reversible plasticity in polycrystals. Journal of the Mechanics and Physics of Solids, 135:103808, 2020.DOI
  27. [27]S. Berbenni, V. Taupin, and R. A. Lebensohn. Elasto-viscoplastic FFT-based method for mesoscale field dislocation mechanics with defect energy. In Mathematisches Forschungsinstitut Oberwolfach, editor, Mechanics of Materials: Multiscale design of advanced materials and structures, volume 11/2024, pages 26–27, Oberwolfach, France, March 2024. S. Forest and D. McDowell and S. Müller and E. Werner.
  28. [28]S. Berbenni, V. Taupin, and R. A. Lebensohn. A FFT-based mesoscale continuum dislocation mechanics with defect energy: Applications to composites and polycrystals. European Journal of Mechanics - A / Solids, 111:105548, 2025.DOI
  29. [29]R. J. Clifton, J. Duffy, K. A. Hartley, and T. G. Shawki. On critical conditions for shear band formation at high strain rates. Scripta Metallurgica, 18:443, 1984.DOI
  30. [30]J.D. Clayton. Analysis of shear localization in viscoplastic solids with pressure-sensitive structural transformations. Journal of the Mechanics and Physics of Solids, 193:105880, 2024. URL: https://www.sciencedirect.com/science/article/pii/S0022509624003466, doi:10.1016/j.jmps.2024.105880.DOI
  31. [31][Cla25a] J.D. Clayton. Analytical shear-band process zone model incorporating nonlinear viscous effects and initial defects. Journal of Applied Mechanics, 92(9):091009, 05 2025. arXiv:https://asmedigitalcollection.asme.org/appliedmechanics/article-pdf/92/9/091009/7498899/jam-25-1088.pdf, doi:10.1115/1.4068648.DOI
  32. [32][Cla25b] J.D. Clayton. Phase-field theory of adiabatic shear. Acta Mechanica, 237:239–273, 2025.DOI
  33. [33][CS95] H.P. Cherukuri and T.G. Shawki. An Energy-based Localization theory: I. Basic framework. International Journal of Plasticity, 11(1):15–40, 1995.DOI
  34. [34][DAS16] A. Das, A. Acharya, and P. Suquet. Microstructure in plasticity without nonconvexity. Computational Mechanics, 57(3):387–403, 2016.DOI
  35. [35][DB85] B. Dodd and Y. Bai. Width of adiabatic shear bands. Materials Science and Technology, 1(1):38–40, 1985.
  36. [36][DB12] B. Dodd and Y. Bai. Adiabatic Shear Localization: Frontiers and Advances. Elsevier, London, 2nd edition, 2012.
  37. [37][DB15] B. Dodd and Y. Bai. Introduction to Adiabatic Shear Localization. Imperial College Press, London, revised edition, 2015.
  38. [38][DBTL20] K. S. Djaka, S. Berbenni, V. Taupin, and R. A. Lebensohn. A FFT-based numerical implementation of mesoscale field dislocation mechanics: Application to two-phase laminates. International Journal of Solids and Structures, 184:136–152, 2020. Physics and Mechanics of Random Structures: From Morphology to Material Properties.DOI
  39. [39][DC92] J. Duffy and Y.C. Chi. On the measurement of local strain and temperature during the formation of adiabatic shear bands. Materials Science and Engineering: A, 157(2):195–210, 1992.DOI
  40. [40][Der91] B. Derby. The dependence of grain size on stress during dynamic recrystallization. Acta Metallurgica and Materialia, 39:955–962, 1991.
  41. [41][DTBF15] K. S. Djaka, V. Taupin, S. Berbenni, and C. Fressengeas. A numerical spectral approach to solve the dislocation density transport equation. Modelling and Simulation in Materials Science and Engineering, 23(6):065008, 2015.DOI
  42. [42][EBG04] L.P. Evers, W.A.M. Brekelmans, and M.G.D. Geers. Non-local crystal plasticity model with intrinsic SSD and GND effects. Journal of the Mechanics and Physics of Solids, 52(10):2379 – 2401, 2004. doi:10.1016/j.jmps.2004.03.007.DOI
  43. [43][EM84] Y. Estrin and H. Mecking. A unified phenomenological description of work hardening and creep based on one-parameter models. Acta Metallurgica, 32(1):57–70, 1984.DOI
  44. [44][FAB11] C. Fressengeas, A. Acharya, and A. J. Beaudoin. Dislocation mediated continuum plasticity: Case studies on modeling scale dependence, scale-invariance, and directionality of sharp yield-point. In Computational Methods for Microstructure-Property Relationships, pages 277–309. Springer, 2011.DOI
  45. [45][FBE+09] C. Fressengeas, A. J. Beaudoin, Denis Entemeyer, Tatiana Lebedkina, Mikhail Lebyodkin, and Vincent Taupin. Dislocation transport and intermittency in the plasticity of crystalline solids. Physical Review B, 79(1):014108, 2009.DOI
  46. [46]N. A. Fleck and J. W. Hutchinson. A reformulation of strain gradient plasticity. Journal of the Mechanics and Physics of Solids, 49(10):2245–2271, 2001.
  47. [47]C. Fressengeas and A. Molinari. Instability and localization of plastic flow in shear at high strain rates. Journal of the Mechanics and Physics of Solids, 35:185, 1987.DOI
  48. [48]C. Fressengeas. Shear band morphology at very high strain rates. Int. J. Impact. Engr., 8:141, 1989.
  49. [49]J. Genée, S. Berbenni, N. Gey, R. A. Lebensohn, and F. Bonnet. Particle interspacing effects on the mechanical behavior of a Fe-TiB₂ metal matrix composite using FFT-based mesoscopic field dislocation mechanics. Advanced Modeling and Simulation in Engineering Sciences, 7(1):1–23, 2020.DOI
  50. [50]M. E. Gurtin. A gradient theory of single-crystal viscoplasticity that accounts for geometrically necessary dislocations. Journal of the Mechanics and Physics of Solids, 50(1):5 – 32, 2002. doi:10.1016/S0022-5096(01)00104–1.DOI
  51. [51]D.A Hughes and N Hansen. Microstructure and strength of nickel at large strains. Acta Materialia, 48(11):2985–3004, 2000. doi:10.1016/S1359–6454(00)00082–3.DOI
  52. [52]K.-H. Hartmann, H.-D. Kunze, and L. W. Meyer. Metallurgical effects on impact loaded materials. In M. A. Meyers and Lawrence E. Murr, editors, Shock Waves and High-Strain-Rate Phenomena in Metals, pages 325–337. Plenum Press, New York, 1981.
  53. [53]J. A. Hines and K. S. Vecchio. Recrystallization kinetics within adiabatic shear bands. Acta Materialia, 45:635–649, 1997.DOI
  54. [54]J. A. Hines, K. S. Vecchio, and S. Ahzi. A model for microstructure evolution in adiabatic shear bands. Metallurgical and Materials Transactions A, 29A:191–203, 1998.
  55. [55]K. Inal, P.D. Wu, and K.W. Neale. Instability and localized deformation in polycrystalline solids under plane-strain tension. International Journal of Solids and Structures, 39(4):983 – 1002, 2002. doi:10.1016/S0020–7683(01)00246–3.DOI
  56. [56]Tao Jin, Hashem M. Mourad, C. A. Bronkhorst, Veronica Livescu, Xiaoxuan Zhang, Christian Linder, and Richard A. Regueiro. Three-dimensional explicit finite element formulation for shear localization with global tracking of embedded weak discontinuities. Computer Methods in Applied Mechanics and Engineering, 353:416–447, 2019. doi:10.1016/j.cma.2019.05.011.DOI
  57. [57]S.R. Kalidindi, C.A. Bronkhorst, and L. Anand. Crystallographic texture evolution in bulk deformation processing of fcc metals. Journal of the Mechanics and Physics of Solids, 40(3):537–569, 1992.DOI
  58. [58]M. Kuroda and A. Needleman. Nonuniform and localized deformation in single crystals under dynamic tensile loading. Journal of the Mechanics and Physics of Solids, 125:347–359, 2019. doi:10.1016/j.jmps.2018.12.017.DOI
  59. [59]H. Kolsky. Stress waves in solids. Journal of Sound and Vibration, 1:88–110, 1963.
  60. [60]M. Kuroda and V. Tvergaard. Studies of scale dependent crystal viscoplasticity models. Journal of the Mechanics and Physics of Solids, 54(9):1789–1810, 2006. doi:10.1016/j.jmps.2006.04.002.DOI
  61. [61]Charles K. C. Lieou and C. A. Bronkhorst. Dynamic recrystallization in adiabatic shear banding: Effective-temperature model and comparison to experiments in ultrafine-grained titanium. International Journal of Plasticity, 111:107–121, 2018. URL: https://www.sciencedirect.com/science/article/pii/S0749641918302821, doi:10.1016/j.ijplas.2018.07.011.DOI
  62. [62]Charles K. C. Lieou, H. M. Mourad, and C. A. Bronkhorst. Strain localization and dynamic recrystallization in polycrystalline metals: Thermodynamic theory and simulation framework. International Journal of Plasticity, 119:171–187, 2019. URL: https://www.sciencedirect.com/science/article/pii/S0749641918305461, doi:10.1016/j.ijplas.2019.03.005.DOI
  63. [63]J. C. Mach, A. J. Beaudoin, and A. Acharya. Continuity in the plastic strain rate and its influence on texture evolution. Journal of the Mechanics and Physics of Solids, 58(2):105–128, 2010.DOI
  64. [64]H. M. Mourad, C. A. Bronkhorst, V. Livescu, J. N. Plohr, and E. K. Cerreta. Modeling and simulation framework for dynamic strain localization in elasto-viscoplastic metallic materials subject to large deformations. International Journal of Plasticity, 88:1–26, 2017. URL: https://www.sciencedirect.com/science/article/pii/S0749641916301668, doi:10.1016/j.ijplas.2016.09.009.DOI
  65. [65]M. Andre M. and K. K. Chawla. Mechanical Behavior of Materials. Cambridge University Press, 2nd edition, 2008.
  66. [66]M. A. Meyers, Y. J. Chen, F. D. S. Marquis, and D. S. Kim. High-strain, high-strain-rate behavior of tantalum. Metallurgical and Materials Transactions A, 26:2493–2509, 1995.DOI
  67. [67]Y. Mu, J. W. Hutchinson, and W. J. Meng. Micro-pillar measurements of plasticity in confined Cu thin films. Extreme Mechanics Letters, 1:62–69, 2014. doi:10.1016/j.eml.2014.12.001.
  68. [68]H. Mecking and U. F. Kocks. Kinetics of flow and strain-hardening. Acta Metallurgica, 29(11):1865–1875, 1981.DOI
  69. [69]D. J. Magagnosc, J. T. Lloyd, C. S. Meredith, A. L. Pilchak, and B. E. Schuster. Incipient dynamic recrystallization and adiabatic shear bands in Ti–7Al studied via in situ x-ray diffraction. International Journal of Plasticity, 141:102992, 2021. URL: https://www.sciencedirect.com/science/article/pii/S074964192100067X, doi:10.1016/j.ijplas.2021.102992.DOI
  70. [70]L. W. Meyer and S. Manwaring. Critical adiabatic shear strength of low alloyed steel under compressive loading. In L. E. Murr, K. P. Staudhammer, and M. A. Meyers, editors, Metallurgical Applications of Shock-Wave and High-Strain-Rate Phenomena, pages 657–674, New York, 1986. Marcel Dekker.
  71. [71][MNL+00] M. A. Meyers, V. F. Nesterenko, J. C. LaSalvia, Y. B. Xu, and Q. Xue. Observation and modeling of dynamic recrystallization in high-strain, high-strain rate deformation of metals. Journal of Physics IV France, 10:50–56, 2000.DOI
  72. [72][MNLX01] M. A. Meyers, V. F. Nesterenko, J. C. LaSalvia, and Q. Xue. Shear localization in dynamic deformation of materials: Microstructural evolution and self-organization. Materials Science and Engineering A, 317:206–225, 2001.DOI
  73. [73][MXX+03] M. A. Meyers, Y. Xu, Q. Xue, M. T. Perez-Prado, and T. McNelley. Microstructural evolution in adiabatic shear localization in stainless steel. Acta Materialia, 51:1307–1325, 2003.
  74. [74][Nee88] A. Needleman. Material rate dependence and mesh sensitivity in localization problems. Computer Methods in Applied Mechanics and Engineering, 67(1):69–85, 1988. doi: 10.1016/0045-7825(88)90069-2.DOI
  75. [75][Nee89] A. Needleman. Dynamic shear band development in plane strain. Journal of Applied Mechanics, 56(1):1–9, 1989.
  76. [76][NML+97] V. F. Nesterenko, M. A. Meyers, J. C. LaSalvia, M. P. Bondar, Y. J. Chen, and Y. L. Lukyanov. Shear localization and recrystallization in high-strain, high-strain-rate deformation of tantalum. Materials Science and Engineering A, 229:23–41, 1997.
  77. [77][NT91] T. Narutani and J. Takamura. Grain-size strengthening in terms of dislocation density measured by resistivity. Acta Metallurgica et Materialia, 39(8):2037–2049, 1991. doi: 10.1016/0956-7151(91)90173-X.DOI
  78. [78][PAR11] S. Puri, A. Acharya, and A.D. Rollett. Controlling plastic flow across grain boundaries in a continuum model. Metallurgical and Materials Transactions A, 42, 03 2011. doi: 10.1007/s11661-010-0257-8.DOI
  79. [79][PDA11] S. Puri, S. Das, and A. Acharya. Mechanical response of multicrystalline thin films in mesoscale field dislocation mechanics. Journal of the Mechanics and Physics of Solids, 59(11):2400–2417, 2011.DOI
  80. [80][PRAD10] S. Puri, A. Roy, A. Acharya, and D. Dimiduk. Modeling dislocation sources and size effects at initial yield in continuum plasticity. Journal of Mechanics of Materials and Structures, 4(9):1603–1618, 2010.DOI
  81. [81][RA06] A. Roy and A. Acharya. Size effects and idealized dislocation microstructure at small scales: predictions of a phenomenological model of mesoscopic field dislocation mechanics: Part II. Journal of the Mechanics and Physics of Solids, 54(8):1711–1743, 2006.
  82. [82][RAY+26] R. Rasmussen, C. Adkins, S. Yang, Raman L., J. Wanni, J. D. Borg, J. P Borg, R. Thevamaran, D. J. Thoma, C. Spencer-Coker, and C. A. Bronkhorst. Thermomechanical theory of large deformation plasticity: applied to quenched and tempered low carbon steel and tantalum. International Journal of Plasticity, submitted, 2026.
  83. [83][RG00] III (Rusty) Gray, G. T. Classic Split-Hopkinson Pressure Bar testing. In Mechanical Testing and Evaluation. ASM International, 01 2000. doi:10.31399/asm.hb.v08.a0003296.DOI
  84. [84]A. Roy, S. Puri, and A. Acharya. Phenomenological mesoscopic field dislocation mechanics, lower-order gradient plasticity, and transport of mean excess dislocation density. Modelling and Simulation in Materials Science and Engineering, 15:S167, 12 2006. doi:10.1088/0965-0393/15/1/S14.DOI
  85. [85]T. Richeton, G. F. Wang, and C. Fressengeas. Continuity constraints at interfaces and their consequences on the work hardening of metal-matrix composites. Journal of the Mechanics and Physics of Solids, 59(10):2023–2043, 2011.DOI
  86. [86]T. G. Shawki and R. J. Clifton. Shear band formation in thermal viscoplastic materials. Mechanics of Materials, 8(1):13–43, 1989. doi:10.1016/0167-6636(89)90003-3.DOI
  87. [87]T. G. Shawki. An energy criterion for the onset of shear localization in thermal viscoplastic materials, Part I: Necessary and sufficient initiation conditions. Journal of Applied Mechanics, 61(3):530–537, 09 1994.DOI
  88. [88]T.G. Shawki. An energy criterion for the onset of shear localization in thermal viscoplastic materials, Part II: Applications and implications. J. Appl. Mech., 61(3):538, 1994.
  89. [89]Noah J. Schmelzer, Evan J. Lieberman, Nan Chen, Samuel D. Dunham, Veronica Anghel, George T. Gray, and Curt A. Bronkhorst. Statistical evaluation of microscale stress conditions leading to void nucleation in the weak shock regime. International Journal of Plasticity, 188:104318, 2025.DOI
  90. [90]V. Taupin, S. Berbenni, C. Fressengeas, and O. Bouaziz. On particle size effects: An internal length mean field approach using field dislocation mechanics. Acta Materialia, 58(16):5532–5544, 2010.
  91. [91]V. Taupin, S. Varadhan, J. Chevy, C. Fressengeas, A. J. Beaudoin, M. Montagnat, and P. Duval. Effects of size on the dynamics of dislocations in ice single crystals. Physical Review Letters, 99(15):155507, 2007.
  92. [92]V. Taupin, S. Varadhan, C. Fressengeas, and A. J. Beaudoin. Directionality of yield point in strain-aged steels: the role of polar dislocations. Acta Materialia, 56(13):3002–3010, 2008.DOI
  93. [93]S. Varadhan, A. Beaudoin, A. Acharya, and C. Fressengeas. Dislocation transport using an Explicit Galerkin-Least Squares formulation. Modelling and Simulation in Materials Science and Engineering, 14:1245, 09 2006. doi:10.1088/0965-0393/14/7/011.
  94. [94]S. Varadhan, A. J. Beaudoin, and C. Fressengeas. Lattice incompatibility and strain-ageing in single crystals. Journal of the Mechanics and Physics of Solids, 57(10):1733–1748, 2009.DOI
  95. [95]T.W. Wright and R.C. Batra. The initiation and growth of adiabatic shear bands. Int. J. Plasticity, 1:205, 1985.
  96. [96]F. H. Wu and L. B. Freund. Deformation trapping due to thermoplastic instability in one-dimensional wave propagation. Journal of the Mechanics and Physics of Solids, 32(2):119–132, 1984. doi:10.1016/0022-5096(84)90014-0.DOI
  97. [97]T. W. Wright. The Physics and Mathematics of Adiabatic Shear Bands. Cambridge University Press, Cambridge, cambridge monographs on mechanics edition, 2002.
  98. [98]T. W. Wright and J.W. Walter. On stress collapse in adiabatic shear bands. J. Mech. Phys. Solids, 35:701, 1987.DOI
  99. [99]O. Watanabe, H. M. Zbib, and E. Takenouchi. Crystal plasticity: Micro-shear banding in polycrystals using voronoi tessellation. International Journal of Plasticity, 14(8):771 – 788, 1998. doi:10.1016/S0749-6419(98)00022–9.
  100. [100]Q. Xue, J. F. Bingert, B. L. Henrie, and G. T. Gray III. Ebsd characterization of dynamic shear band regions in pre-shocked and as-received 304 stainless steels. Materials Science and Engineering A, 473:279–289, 2008.
  101. [101]Q. Xue, G. T. Gray, B. L. Henrie, S. A. Maloy, and S. R. Chen. Influence of shock prestraining on the formation of shear localization in 304 stainless steel. Metallurgical and Materials Transactions A, 36:1471–1486, 2005.
  102. [102]H. M. Zbib and E. C. Aifantis. On the localization and postlocalization behavior of plastic deformation. I, II, III. Res Mechanica, 23:261–305, 1988.
  103. [103]H. M. Zbib and E. C. Aifantis. A gradient-dependent flow theory of plasticity: application to metal and soil instabilities. Applied Mechanics Reviews, 42(11):295–304, 1989.
  104. [104]H. M. Zbib and E. C. Aifantis. On the gradient-dependent theory of plasticity and shear banding. Acta Mechanica, 92:209–225, 1992.
  105. [105]X. Zhang, A. Acharya, N. J. Walkington, and J. Bielak. A single theory for some quasi-static, supersonic, atomic, and tectonic scale applications of dislocations. Journal of the Mechanics and Physics of Solids, 84:145–195, 2015. doi:10.1016/j.jmps.2015.07.004.DOI
  106. [106]C. Zener and J. H. Hollomon. Effect of strain rate upon plastic flow of steel. Journal of Applied physics, 15(1):22–32, 1944.

Paper details

vlnc:W_85ekqa4x
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents