Comprehensive structural and optical analysis of differently oriented Yb-implanted -GaO
Abstract
This study presents investigations of Yb-doped -GaO, an ultrawide bandgap semiconductor with potential use in future power and optoelectronic devices operating in high-radiation environments. The research has focused on the problem of structural damage caused by the implantation of Yb-ions into three differently oriented crystals and the optical response of created systems. The (001), (010), and (-201)-oriented -GaO crystals were implanted with three different fluences of 150 keV Yb ions and examined using a variety of experimental techniques: high-resolution X-ray diffraction (HRXRD), Rutherford backscattering spectrometry in channeling mode (RBS/c), Raman and photoluminescence (PL) spectroscopies, to provide comprehensive information about studied systems. Furthermore, the RBS/c studies were supported by Monte Carlo simulations. The results show distinctions between differently oriented crystals. In particular, (010)-oriented crystals are characterized by the lowest concentration of extended defects and the presence of compressive stress. In contrast, samples with the other two orientations exhibit tensile stress and significantly higher levels of extended defects. Interestingly, the PL spectra of (010)-oriented -GaO show the lowest emission from Yb ions, suggesting that specific types of extended defects, whose formation is more favorable in the other two orientations than in (010), enhance Yb luminescence instead of suppressing it.
Introduction
The development of materials has always played a key role in advancing technology and driving scientific progress. The discovery of new properties can open up new applications or improve the existing ones. One of particularly interesting materials nowadays, fulfilling the modern application market requirements, is a wide bandgap semiconductor - gallium oxide (GaO). It first captured the interest of researchers over 70 years ago, but in recent years it has seen a renewed interest and has been increasingly studied due to its remarkable properties.
There are several polymorphs of gallium oxide: , , , , and [1]. Among them, only the monoclinic phase is thermodynamically stable [2]. Consequently, it is the commonly used polymorph, and it has been investigated in this work. With a bandgap of 4.8 eV -GaO belongs to the group of ultrawide bandgap semiconductors (UWBG). These materials are characterized by high critical breakdown field [1]. These properties allow -GaO to handle high voltages. Moreover, it is chemically inert and can withstand high temperatures and other harsh conditions.
Gallium oxide is optically transparent to visible and UV light, down to 250 nm [3, 4], which can be particularly useful in optoelectronic devices. Furthermore, -GaO can be easily produced in bulk wafers of high quality, and the cost is lower than for common wide bandgap semiconductors such as SiC and GaN [1, 2]. Because of its many advantages, the material has found numerous applications, including solar-blind UV photodetectors, efficient high-power switches [5], Schottky barrier diodes, metal-oxide-semiconductor field-effect transistors (MOSFET), and high electron mobility transistors (HEMT) [1]. Due to its resistance gallium oxide is a promising material for harsh environments, such as space systems or nuclear power plants [6].
The luminescence range for undoped -GaO extends from ultraviolet to visible light [4]. Doping the material with rare earth ions (RE) such as ytterbium (Yb) extends this range into the infrared spectral range, which broadens the scope of applications [7]. -GaO is considered a good host for rare earth ions, as it has been shown that the larger the band gap, the lower the thermal quenching effect [8]. Thus, Yb-doped -GaO, which is investigated in this work, has potential use in future optoelectronic devices such as high-power LEDs and high-end photodetectors operating even in high-irradiation environments.
Doping of -GaO with RE elements during the growth process frequently results in the formation of secondary phases or RE precipitation as a consequence of the low solubility limit of RE in this material and the high melting points of the dopants [9, 10]. Thus, one of the most common doping methods is ion implantation [11], since the dopant concentration and depth profile can be precisely controlled by selecting an appropriate ion fluence and energy. Moreover, implantation is a strongly non-equilibrium process allowing the introduction of any kind of atoms into solids with a concentration well above solid solubility limits. However, apart from many advantages, ion implantation can induce the formation of structural defects or phase transitions, which can alter the properties and the performance of the material. In the case of -GaO the effects of implantation have not been fully explored and are still under investigation.
-GaO belongs to the () space group [13]. The lattice parameters of monoclinic -GaO are reported as Å, Å, Å and [14], and the unit cell is shown in Figure 1. In the structure of -GaO two types of gallium and three types of oxygen atoms are distinguished, making up GaI O tetrahedrons and GaII O octahedrons. Due to such a complicated structure and low symmetry, strong anisotropy is expected, which gave impetus to the studies of differently oriented crystals carried out in this work.

Figure 1. The unit cell of -GaO created by VESTA [12].
In this work, the radiation-induced structure changes in (001), (010), and (-201)-oriented -GaO implanted with different fluences of Yb ions were examined with a wide range of experimental methods: high-resolution X-ray diffraction (HRXRD), Rutherford backscattering spectrometry in channeling mode (RBS/c), Raman spectroscopy and photoluminescence spectroscopy (PL). HRXRD scans illustrate crystal quality and its changes after implantation depending on crystal orientation. RBS/c combined with Monte Carlo simulations shows changes in defect concentrations and depth profiles. On the other hand, Raman spectroscopy provides information about the phonon energy distribution in the material, which reflects any changes in crystalline quality. Finally, the photoluminescence measurements are useful in analyzing the electronic and optical properties of the material and in determining its potential applications. These complementary methods deliver unique insights into the properties of Yb-doped -GaO systems, offering a comprehensive understanding of their structural, electronic, and optical behavior.
Experimental Section
Sample preparation Samples investigated in this work were (001), (010) and (-201)-oriented UID -GaO crystals from Novel Crystal Technology Inc. The crystals were n-type with electron concentration levels lower than . The samples measuring approximately 8x8 mm and 0.68 mm thick were obtained by dicing commercially available wafers. A capping layer was deposited before the dicing, which was then etched using organic cleaning.
Implantation Crystals were implanted at room temperature with 150 keV Yb ions with fluences of , and ions/cm. To avoid channeled implantation the samples were tilted approximately . The implantation processes were carried out at Helmholtz-Zentrum Dresden-Rossendorf (HZDR), Germany. The selected implanted crystals were subsequently annealed in oxygen at 800°C for 10 minutes using Rapid Thermal Annealing (RTA) system Accu Thermo AW-610 from Allwin21 Co. at the Institute of Physics, Polish Academy of Sciences (IP PAS), Warsaw, Poland.
XRD High Resolution X-Ray Diffraction (HRXRD) measurements were performed at UNIPRESS Institute of High Pressure Physics, Polish Academy of Sciences, Warsaw, Poland, with Empyrean X-ray diffractometer operating at Cu K1 wavelength (40 kV, 30 mA), equipped with a hybrid 2-bounce monochromator and a threefold Ge(220) analyzer. For each sample scan of symmetrical reflection were done to measure the implantation effect.
RBS/c The RBS/c measurements were performed at HZDR, Dresden, Germany. For each sample two different modes of measurements were applied: random and aligned, i.e. with the crystal oriented randomly and aligned along the surface orientation. A beam of 1.7 MeV He ions was delivered with a Van de Graaff accelerator. A silicon detector with a scattering angle of , depth resolution of about 5 nm and energy resolution of less than 20 keV was used.
Raman spectroscopy The Raman spectroscopy measurements of -GaO were performed at HZDR, Dresden, Germany. The phonon spectra have been obtained in backscattering geometry in the range of 50 to 1000 cm using a 532 nm Nd:YAG laser with a liquid nitrogen-cooled charge-coupled device camera. Eight selected samples were examined by Raman spectroscopy.
PL spectroscopy Photoluminescence (PL) spectroscopy measurements of Yb implanted and annealed -GaO were carried out at IP PAS at T=300 K under near-band edge excitation at 5.82 eV with an Edinburgh Instrument FLS 1000 fluorescence spectrometer and a CCD3-x camera to collect the spectra at the wide range from 1.17 to 4.97 eV and an InGaAs camera (DU49 X) to collect spectra only in the near-infrared (NIR) spectral range. Yb-related inner shell emissions were detected in single photon counting mode in the range of 1.20-1.28 eV.
Results and discussion
HRXRD
HRXRD scans provide detailed information about the crystalline quality of the material and its changes after ion implantation. The asymmetry of the main peaks and the appearance of additional ones may indicate the development of strain, amorphization, or formation of other crystal phases in the studied material.
The HRXRD results for (-201)-oriented -GaO crystal implanted with three fluences of , and ions/cm of Yb are presented in Figure 2a. The sharp signal coming from the symmetric (-402) reflection of -GaO crystals implanted with the lowest fluence has a full width at half maximum (FWHM) calculated from scans equal to . This is consistent with the results calculated for the virgin - crystal from the rocking curve, presented in our previous work [7], and indicates that the quality of the initial crystals is very high. However, the asymmetry of the reflection towards increased lattice parameters due to tensile strain is also visible, which indicates the beginning of the structural changes for a sample with the lowest implantation fluence. Distinct evolution of the central peak at occurs with increasing implantation fluence and shoulder peaks at and are clearly visible. The first shoulder peak is related to implantation-induced strain [7, 15] while the second one appears due to radiation-induced phase transformation from to phase [7, 16, 17]. In the crystals implanted with the middle fluence, i.e. ions/, the radiation-induced phase transformation from - to - phase is evident. As can be seen in Figure SM1 in the Supplementary Materials, the phase was developed in the entire implanted zone. In addition, the presence of oscillations in the diffraction pattern, coming from the - layer, allows us to determine its average thickness to be approximately nm. In the crystals implanted with the highest fluence, i.e. ions/ two additional shoulder peaks remain visible. However, comparing this diffraction pattern with the one obtained for the middle fluence used ( ions/) reveals that the peak coming from - phase becomes wider and its intensity decreases. The peaks shift their positions toward the lower angles (higher lattice parameters). This indicates a deterioration of the structural quality, including the beginning of the amorphization process as the implantation fluence increases up to ions/. These observations were confirmed by Nano-Beam electron Diffraction (NBD) patterns taken from the selected layers visualized by HRTEM image (see Figure SM2 in Supplementary Materials, with a detailed description in the work of Ratajczak et al. [18]). It is worth noting that after annealing, the radiation-induced phase of gallium oxide disappears and the strain is reduced, as can be seen in Figure 2b and Figure SM3.

Figure 2. HRXRD scans of (-201)-oriented -GaO crystal (a) implanted with Yb ions with different fluences and (b) implanted with Yb with fluence of ions/cm and annealed in oxygen at 800°C for 10 minutes.

Figure SM1. Nano-Beam electron Diffraction (NBD) patterns taken from the selected layers of -GaO implanted with Yb ions/cm, visualized by HRTEM image.

Figure SM2. Nano-Beam electron Diffraction (NBD) patterns taken from the selected layers of -GaO implanted with Yb ions/cm, visualized by HRTEM image.

Figure SM3. Nano-Beam electron Diffraction (NBD) patterns taken from the selected layers of -GaO implanted with Yb ions/cm and annealed in O at 800°C for 10 min, visualized by HRTEM image.
HRXRD scans presented in Figure 3 show how the crystalline structure of differently oriented - changes after implantation with the highest Yb fluence. As can be seen, in the case of both (001) and -oriented crystals the evolution of the peak suggests implantation-induced tensile strain. In contrast, for (010)-oriented crystals compressive strain is observed [15]. In addition, in the diffraction patterns for the (010) and -oriented crystals additional peaks associated with the formation of - can be observed [7, 16]. According to the work of Gottschalk et al. [19], in the angular region of the diffractogram collected for the (001)-oriented crystal there are no peaks originating from -.

Figure 3. HRXRD scans of -oriented - crystal implanted with Yb ions with a fluence of ions/
RBS/c
Rutherford backscattering spectrometry measures the energy and number of analyzing ions scattered back from the atoms of the investigated material. This method allows for depth analysis of the stoichiometry and the impurities near the surface (up to about ). In the case of Yb-implanted -, all three elements present differ greatly in atomic mass. Hence, the signals coming from ions scattered on Ga, O, and Yb atoms can be easily distinguished and analyzed separately.
For RBS measurements performed in the channeling mode (RBS/c), when the beam is aligned perpendicular to the crystal surface, the backscattering yield is much lower than in the random mode. It is due to the channeling effect [20]. For both the undoped and implanted crystals a surface peak appears, which corresponds to ions scattered from surface atoms. Because of the defects induced by the implantation process, the backscattering yield for implanted crystals is higher than for undoped ones. It is worth mentioning that different types of defects affect the spectra in different ways. Simple defects induce the direct backscattering of analyzing ions and cause the growth of the characteristic damage peak, while extended defects result in an increased backscattering yield behind the damage peak, due to the mechanism called dechanneling, which results in delayed scattering [21]. This term is also commonly used to refer to the yield behind the damage peak itself.
The RBS/c spectra, presented in Figure 4, show the number of ions scattered on gallium atoms (a) and ytterbium atoms (b) in differently oriented -GaO. The signal from oxygen that appears at the lowest energy range (below the energy of 616 keV) is barely visible due to the low cross-section for scattering on light elements and was not analyzed. The spectra in the energy range corresponding to Ga provide information about the defect distribution and those obtained for Yb show the dopant lattice site location and its depth profile. As expected, the characteristic damage peak in Figure 4 increases with fluence. The defect accumulation process appears to be very similar for all tested crystals. However, significant differences in the dechanneling levels can be observed. This is partly due to the different sensitivity of the RBS/c method on different surface orientations of the crystals because the crystal channels do not look the same (see Figure 5 and the work of Anam et al. [22]). Therefore, significant differences can be seen even in the aligned spectra obtained for undoped crystals. Nevertheless, the performed simulations described below show that it does not fully explain the differences observed for Yb-implanted differently oriented crystals.

Figure 4. RBS random (open symbols) and aligned (solid symbols) spectra for differently oriented -GaO crystals implanted with different fluences of Yb ions. The spectra on the left (a) show the signal from gallium atoms and the spectra on the right (b) - from ytterbium atoms.

Figure 5. The angular scans obtained by RBS/c analysis of virgin samples of , , and -oriented -GaO crystals.
In order to better understand the RBS/c spectra, McChasy simulations were performed to obtain information about defect types and their distributions. McChasy is a Monte Carlo simulation tool, which reproduces the path of a projectile in the given material [23, 24]. The distributions of two distinct types of defects can be obtained by McChasy: simple and extended ones. In the program, the simple defects, which act as channel-blocking defects and lead to direct backscattering of the analyzed ions, are modeled as randomly displaced atoms (RDA). In turn, extended defects (named DIS) refer to those that cause the bending of crystal channels like edge dislocations, clusters, or grain boundaries, causing the local distortion effect of the crystal lattice. It should be pointed out that the reorganization of atoms due to the changes in phase or orientation compared to the bulk crystal, reported in the work of Azarov et al. [16] is also viewed as a defect according to McChasy. The same contribution to the RBS-aligned spectrum derived by different defects or other structural changes makes the full identification impossible. For this reason, a variety of techniques were used, which have their own limitations but are complementary to each other.
The results of McChasy simulations performed for the differently oriented -GaO crystals implanted with the highest fluence, i.e. ions/cm, are presented in Figure 6. As can be observed, the distribution of RDA-type defects is relatively consistent for all considered crystal orientations of -GaO, whereas the concentration of bending channels defects is notably lower for (010)-oriented crystal compared to (001) and (-201). This difference is the main reason for the lower dechanneling level observed in the aligned spectra behind the damage peak for the implanted crystal. It is also worth mentioning that the distribution of RDA becomes bimodal for fluences exceeding ions/cm due to the formation of two phases in the implanted crystals: amorphization and phases [18] (see Figure SM2).

Figure 6. Concentrations of simple defects (RDA) and extended defects (DIS) obtained by McChasy for the differently oriented -GaO implanted with Yb to the fluence of ions/cm
Additionally, as can be seen in Figure 4b, the Yb behavior is similar for all surface orientations. Its signal in the aligned spectra is at the same level as in the random spectra for the visible fluences. However, due to the phase change occurring in the modified layer after implantation, no conclusions can be drawn regarding the position of the Yb ions sites in the -GaO crystal lattice.
Raman spectroscopy
Raman spectroscopy is a technique based on inelastic scattering of photons. The energy of the incident photon may decrease or increase as a result of excitation or deexcitation of vibrations. Since the energies of incident and scattered photons are close and the difference between them is measured, the incident radiation must be monochromatic. Therefore, a laser is used for measurements, and the Raman shift expressed in cm, i.e. in the unit of the wave vector, is marked on the spectrum axis.
Characteristic Raman spectra contain peaks, which correspond to different vibration modes of microstructures in the studied material - phonon modes. The positions of peaks may differ from ideal under the influence of such factors as temperature, stress, or when the material contains structural defects and impurities. The presence of defects can also affect the Raman lineshape [25].
The primitive unit cell of -GaO has four gallium and six oxygen atoms, resulting in 30 phonon modes in the first Brillouin zone [13, 26]. The irreducible representation in point is
where modes with index are Raman-active and modes with index are IR-active. Therefore, ten and five active phonon modes are expected in the Raman spectroscopy measurements for -GaO crystals. These phonon modes are listed in Table 1. The collected Raman spectra, presented in Figure 7 show signals from almost all of these phonon modes of -GaO.

Figure 7. Raman spectra of undoped and Yb-implanted -GaO. The scale is different for each part of the spectrum, but it is the same for different surface orientations. The experimental data is marked with dots and the solid line indicates the fit to the Lorentz distribution. Phonon modes with values from the work of Dohy et al. [27] are marked with dashed lines.
| Phonon mode | |||||||||||||||
| Raman shift — Literature | 111 | 114 | 147 | 169 | 199 | 318 | 346 | 353 | 415 | 475 | 475 | 628 | 651 | 657 | 763 |
| Raman shift — This work | 108 | 112 | 142 | 167 | 198 | 318 | 344 | - | 414 | 473 | 473 | 628 | 650 | 656 | 764 |
Table 1. Raman shifts in cm of phonon modes from literature [27] and from this work in the undoped (010)-oriented crystal.
The peaks on the Raman spectra were fitted to the Lorentz distribution with a flat background. The calculated positions for undoped (010)-oriented crystal are also listed in Table 1. The Raman peak positions, @page 7/15 starts_mid=1 ends_mid=1 obtained in this work are similar to those reported in the literature [13, 26, 27, 28]. Moreover, no additional peaks were observed, which means that only -GaO structure was noted.
The collected Raman spectra showed variation in the intensity of certain modes depending on the sample rotation in the horizontal plane. The samples were measured at three rotation positions 0, 45, and 90°. In the case of the 45° angle, no regular changes were observed so no further analysis was performed for such spectra. For 0° and 90° angles the spectra differed particularly in the ratio of the intensity of and modes and and , which can be seen in Figure 8. These differences allowed us to assign the angles to measurements in order to compare results for the same polarization. The spectra measured for samples rotated 90° were chosen for further analysis.

Figure 8. Raman spectra of (010) undoped -GaO crystal rotated 90°.
Differently oriented -GaO crystals show the presence of different phonon modes and peak intensities, as shown in Figure 7. In particular, in the case of (001) and (-201)-oriented -GaO the mode is dominant over mode. In contrast, for (010)-oriented crystal the mode is present and the mode has a much higher intensity than (see Figure 9, Table 2). As can be found in the literature [29] corresponds to the bending vibration of the Ga(O) bonds and to the symmetrical stretching vibration of the Ga(OO) bonds of the GaO tetrahedrons. is assigned to the asymmetrical stretching vibration of the Ga(O) bonds of the same tetrahedral unit. Furthermore, the signal from and has a considerably lower intensity for (010)-oriented crystal. is associated with stretching and bending of GaO as well [29]. Even though the collected Raman spectra do not show any characteristic response to strain, such as shifts of the modes to the right or left depending on the type of strain [30], the differences in the intensities of these peaks indicate specific properties of the studied material.

Figure 9. (657 cm) and (651 cm) modes in a function of surface orientations of the crystal fitted as a sum of two Lorentz distributions. Dotted lines correspond to the two components of the sum.
| Surface orientation | Amplitude | FWHM [cm] | Amplitude | FWHM [cm] | Ratio of amplitudes |
| (001) | 0.46 | 4.8 | 3.07 | 4.0 | 0.15 |
| (010) | 12.04 | 6.8 | 0.81 | 3.1 | 15 |
| (-201) | 1.26 | 5.7 | 5.65 | 4.0 | 0.22 |
Table 2. Amplitudes and FWHM of and modes for undoped crystals.
Moreover, one can observe the differences in the intensity of the modes for different fluences. Although the differences are not significant, a decrease in the intensity with the increasing fluence is noticeable, due to the damage [30]. However, for the highest Yb fluence of ions/cm the amplitude of the peaks is higher than for the virgin one, in the case of all tested crystal orientations, and the FWHM is the lowest for most of the phonon modes. It may be hypothesized that this phenomenon is associated with the plastic deformation of the crystal with the clearly observed threshold in the vicinity of this specific fluence [7].
PL spectroscopy
PL spectroscopy is a powerful tool for studying the electronic structure, local symmetry, excitation, and relaxation dynamics of emission centers associated with local defects and impurities in solids [31]. This technique was applied here to study the optical properties of Yb ions implanted in -GaO crystals with different crystallographic orientations.
Typical photoluminescence spectra collected for -GaO with Yb systems, under optical excitation at energy eV above the band gap energy of -GaO, are shown in Figure 10. The spectra on the left represent the spectra collected in the wide spectral range from ultraviolet (UV) to near-infrared (NIR). The spectra on the right correspond to the NIR range, where the characteristic 4f inner shell transitions of the Yb ions in the oxidation state can be observed separately from the other characteristic emissions of -GaO [32].

Figure 10. The PL spectra of (001), (010), and (-201)-oriented -GaO crystals, implanted with Yb ions with fluence of ions/cm and annealed in oxygen at 800°C for 10 min. The inset shows a diagram of radiative transitions between spin-orbital levels of terms of Yb ions.
As has already been reported, Yb ions remain optically inactive directly after implantation and annealing is necessary to get the optical response, and the most efficient luminescence of Yb-implanted -GaO is obtained after annealing in oxygen for 10 minutes at 800° [33]. Annealing under these conditions leads to the definite disappearance of the phase and to the reduction of radiation-induced strain (see Figure 2b). In the case of the highest fluence used i.e. ions/cm such annealing conditions lead to -GaO recrystallization in both the -GaO and the amorphous phases (see Figure SM3). However, due to the defects in the near-surface layer, -GaO recrystallization process is probably different (non-planar) than in the deeper part of the crystal, and the recovered -GaO layer might regrow misoriented with respect to the bulk crystal [16]. It could be the reason for the observed increase in the dechanneling level of the RBS-aligned spectra after annealing (see Figure SM4). However, the other factors such as dislocation migration, grain boundaries, and formation of RE-O and/or defect clusters cannot also be excluded. Consequently, further studies are essential for a comprehensive understanding of this phenomenon.

Figure SM4. RBS random (open symbols) and aligned (solid symbols) spectra for differently oriented β-Ga₂O₃ crystals implanted with Yb ions at a fluence of ions/cm². Solid lines represent spectra for post-implanted annealed samples in oxygen at 800°C for 10 minutes. The spectra on the left (a) correspond to the signal from gallium atoms, while the spectra on the right (b) correspond to the signal from ytterbium atoms.
The PL spectra collected in a broad spectral range from UV to NIR (left part of Figure 10) do not reveal the characteristic near-band edge emission of -GaO around 4.8 eV, mostly due to the efficient interactions of free electrons with self-trapped holes and indirect energy bandgap [34, 35]. Instead, a broad PL band in the 3.8-2 eV range with a maximum of 2.8 eV associated with native local defects (LD band) and a narrow emission line of Yb ions at 1.265 eV (=980 nm) are observed. In this case, the LD band is characterized by a short emission decay time of =7.8 ns. This value does not change over the spectral contour of this broadband. This fact allows us to state that this band is associated with a local defect of the same type and is formed by phonon modes of the emitter center. The origin of this center has not yet been established, but it could be associated with a divacancy or a vacancies complex, as well as a vacancy-impurity complex [35, 36, 37, 38, 39].
As can be seen in the right part of Figure 10, the Yb PL line is formed by the transition between the split-orbit levels of the excited F and ground F states of the Yb ion (see the diagram of the transitions in Figure 10f). A weak PL band in the range of 1.2-1.24 eV is most likely associated with native local defects radiative transitions since this band is also observed in undoped samples of -GaO crystals.
For different orientations, strong differences in the PL intensity of Yb ions are observed. At the same time, the energy and width of the spin-orbit components remain constant with the accuracy of the fit. The highest intensity of the Yb main peak is obtained for (001)-oriented -GaO. Recall that such oriented crystals exhibit the highest level of radiation-induced DIS-type defect, while the lowest level of this type of defect is observed for (010)-oriented crystals. Some reports [40, 41] indicate the important role of dislocations in enhancing luminescence in -GaO. Dislocations could be trapping centers for dopant ions, stabilizing them in the lattice at the dislocation core. Such location makes it easier to transfer energy from the crystal lattice to the ions, which enhances light emission from dopant [42]. Such a situation also may take place in this case, which would explain the high level of bending channel defects in (001) and (-201)-oriented crystals. However, other proof is necessary. Nevertheless, the correlation between LD and Yb emission is simple: the lower the defect excitation, the higher the Yb luminescence.
Conclusion
The Yb-implanted and annealed -GaO crystals with (010), (001), and (-201) surface orientations were investigated with HRXRD, RBS/c, Raman spectroscopy and PL spectroscopy. The analyses of the results obtained by RBS/c were supplemented with MC simulations using McChasy.
The presented results clearly show the structural and optical anisotropy of Yb-implanted -GaO, with the different response of (010)-oriented crystals to the implantation process. The HRXRD scans for Yb implanted -GaO reveal that radiation-induced compressive strain develops for (010)-oriented crystals, while tensile strain for (001) and (-201)-oriented crystals was observed. The Raman measurements showed that the high-frequency phonon modes associated with the stretching and bending of GaO tetrahedrons appear only for (010)-oriented crystals. Finally, the RBS/c studies, supported by McChasy simulations, demonstrated a significantly lower tendency to develop bending channel defects in the (010)-oriented crystals in comparison with the other tested crystal orientations. For (001) and (-201)-oriented Yb-implanted -GaO crystals the concentration of this type of defect is similar. The PL spectra obtained for (010)-oriented implanted crystal reveal the highest point-defect-related luminescence, which results in the low luminance efficiency from Yb. In contrast, the high Yb-related luminescence in (001) and (-201)-oriented crystals was observed. Thus, the results may suggest the important role of dislocations (or another bending channel defect) in the mechanism of Yb luminescence in -GaO, which are probably trapping centers for dopant ions and/or defects leading to enhancing RE emission. The mechanism is the subject of further research. This strong dependence of radiation-induced damage on the crystal orientation and different optical responses to these structural changes mean that (001) and (-201)-oriented -GaO can be recommended for optoelectronic applications that can be operated in harmful conditions e.g. high radiation environment and (010)-oriented -GaO for power electronics devices.
Acknowledgements
The research was carried out within the NCN project UMO-2022/45/B/ST5/02810. The experimental work was supported by the Helmholtz-Zentrum Dresden-Rossendorf (21002661-ST, 21002663-ST).
References
Supplementary materials
Comprehensive structural and optical analysis of differently oriented Yb-implanted -GaO
Joanna Matulewicz, Renata Ratajczak, Mahwish Sarwar, Ewa Grzanka, Vitalii Ivanov, Damian Kalita, Cyprian Mieszczynski, Przemyslaw Jozwik, Slawomir Prucnal, Ulrich Kentsch, Rene Heller, and Elzbieta Guziewicz
References
- [1]Mingfei Xu, Dawei Wang, Kai Fu, Dnusha Herath Mudiyanselage, Houqiang Fu, and Yuji Zhao. A review of ultrawide bandgap materials: properties, synthesis and devices. Oxford Open Materials Science, 2(1):itac004, 2022. doi:10.1093/oxfmat/itac004.DOI
- [2]Masataka Higashiwaki. β-Ga₂O₃ material properties, growth technologies, and devices: a review. AAPPS Bulletin, 32(1):3, 2022. doi:10.1007/s43673-021-00033-0.DOI
- [3]SJ Pearton, Jiancheng Yang, Patrick H Cary, Fan Ren, Jihyun Kim, Marko J Tadjer, and Michael A Mastro. A review of Ga₂O₃ materials, processing, and devices. Applied Physics Reviews, 5(1), 2018. doi:/10.1063/1.5006941.DOI
- [4]Loh Kean Ping, Dilla Duryha Berhanuddin, Abhay Kumar Mondal, P Susthitha Menon, and Mohd Ambri Mohamed. Properties and perspectives of ultrawide bandgap Ga₂O₃ in optoelectronic applications. Chinese Journal of Physics, 73:195–212, 2021. doi:10.1016/j.cjph.2021.06.015.DOI
- [5]Michele Baldini, Zbigniew Galazka, and Günter Wagner. Recent progress in the growth of β-Ga₂O₃ for power electronics applications. Materials Science in Semiconductor Processing, 78:132–146, 2018. doi:10.1016/j.mssp.2017.10.040.DOI
- [6]AI Titov, KV Karabeshkin, AI Struchkov, VI Nikolaev, Alexander Azarov, DS Gogova, and PA Karaseov. Comparative study of radiation tolerance of GaN and Ga₂O₃ polymorphs. Vacuum, 200:111005, 2022. doi:10.1016/j.vacuum.2022.111005.DOI
- [7]Mahwish Sarwar, Renata Ratajczak, Cyprian Mieszczyński, Aleksandra Wierzbicka, Sylwia Gieraltowska, René Heller, Stefan Eisenwinder, Wojciech Wozniak, and Elżbieta Guziewicz. Defect accumulation in β-Ga₂O₃ implanted with Yb. Acta Materialia, 268:119760, 2024. doi:10.1016/j.actamat.2024.119760.DOI
- [8]PN Favennec, H L’haridon, M Salvi, D Moutonnet, and Y Le Guillou. Luminescence of erbium implanted in various semiconductors: IV, III-V and II-VI materials. Electronics Letters, 25(11):718–719, 1989.DOI
- [9]Janusz Sadowski, Piotr Dłużewski, Sławomir Kret, Elżbieta Janik, Elżbieta Łusakowska, Janusz Kanski, Adam Presz, Feriał Terki, Salam Charar, and Dong Tang. GaAs: Mn nanowires grown by molecular beam epitaxy of (Ga, Mn) As at MnAs segregation conditions. Nano Letters, 7(9):2724–2728, 2007. doi:10.1021/nl071190f.DOI
- [10]David R Lide. CRC handbook of chemistry and physics, volume 85. CRC press, 2004.
- [11]Alena Nikolskaya, Evgenia Okulich, Dmitry Korolev, Anton Stepanov, Dmitry Nikolichev, Alexey Mikhaylov, David Tetelbaum, Aleksei Almaev, Charles Airton Bolzan, Antônio Buaczik, et al. Ion implantation in β-Ga₂O₃: Physics and technology. Journal of Vacuum Science & Technology A, 39(3), 2021. doi:10.1116/6.0000928.DOI
- [12]Koichi Momma and Fujio Izumi. VESTA 3 for three-dimensional visualization of crystal, volumetric and morphology data. Journal of applied crystallography, 44(6):1272–1276, 2011. doi:10.1107/S0021889811038970.DOI
- [13]Benjamin M. Janzen, Roland Gillen, Zbigniew Galazka, Janina Maultzsch, and Markus R. Wagner. First- and second-order Raman spectroscopy of monoclinic β-Ga₂O₃. Phys. Rev. Mater., 6:054601, May 2022. doi:10.1103/PhysRevMaterials.6.054601.DOI
- [14]JA Kohn, Gerald Katz, and JD Broder. Characterization of β-Ga₂O₃ and its Alumina Isomorph, θ-Al₂O₃. American Mineralogist: Journal of Earth and Planetary Materials, 42(5-6):398–407, 1957. pdf.
- [15]Snorre Braathen Kjeldby, Alexander Azarov, Phuong Dan Nguyen, Vishnukanthan Venkatachalapathy, R Mikošová, A Macková, Andrej Kuznetsov, Øystein Prytz, and Lasse Vines. Radiation-induced defect accumulation and annealing in Si-implanted gallium oxide. Journal of Applied Physics, 131(12), 2022. doi:10.1063/5.0083858.DOI
- [16]Alexander Azarov, Augustinas Galeckas, Ildikó Cora, Zsolt Fogarassy, Vishnukanthan Venkatachalapathy, Eduard Monakhov, and Andrej Kuznetsov. Optical Activity and Phase Transformations in γ/β-Ga₂O₃ Bilayers Under Annealing. Advanced Optical Materials, page 2401325, 2024. doi:10.1002/adom.202401325.DOI
- [17]Timothy Yoo, Xinyi Xia, Fan Ren, Alan Jacobs, Marko J Tadjer, Stephen Pearton, and Hongyu Kim. Atomic-scale characterization of structural damage and recovery in Sn ion-implanted β-Ga₂O₃. Applied Physics Letters, 121(7), 2022. doi:10.1063/5.0099915.DOI
- [18]Renata Ratajczak, Mahwish Sarwar, Damian Kalita, Przemysław Jozwik, Cyprian Mieszczynski, Joanna Matulewicz, Magdalena Wilczopolska, Wojciech Wozniak, Ulrich Kentsch, René Heller, et al. Anisotropy of radiation-induced defects in yb-implanted β-Ga₂O₃. Scientific Reports, 14(1):24800, 2024. doi:10.1038/s41598-024-75187-6.DOI
- [19]Volker Gottschall, Stefan Merker, Steffen Blaurock, Max Kneib, Ulrike Teschner, Marius Grundmann, and Harald Krautscheid. Heteroepitaxial growth of α-, β-, γ-and κ-Ga₂O₃ phases by metalorganic vapor phase epitaxy. Journal of Crystal Growth, 510:76–84, 2019. doi:10.1016/j.jcrysgro.2019.01.018.
- [20]Wei-Kan Chu, James W Mayer, and Marc A Nicolet. Backscattering spectrometry, 1978.
- [21]A Caçador, P Jóźwik, S Magalhães, JG Marques, E Wendler, and K Lorenz. Extracting defect profiles in ion-implanted GaN from ion channeling. Materials Science in Semiconductor Processing, 166:107702, 2023. doi:10.1016/j.mssp.2023.107702.DOI
- [22]Bushra Anam and Nicola Gaston. Structural, thermal, and electronic properties of two-dimensional gallium oxide (β-Ga₂O₃) from first-principles design. ChemPhysChem, 22(22):2362–2370, 2021. doi:10.1002/cphc.202100267.DOI
- [23]Przemysław Jóźwik, Afonso Caçador, Katharina Lorenz, Renata Ratajczak, and Cyprian Mieszczynski. Monte Carlo simulations of ion channeling in the presence of dislocation loops: New development in the McChasy code. Nuclear Instruments and Methods in Physics Research Section B: Beam Interactions with Materials and Atoms, 538:198–204, 2023. doi:10.1016/j.nimb.2023.03.002.DOI
- [24]Przemyslaw Jozwik, Lech Nowicki, Renata Ratajczak, Cyprian Mieszczynski, Anna Stonert, Andrzej Turos, Katharina Lorenz, and Eduard Alves. Advanced Monte Carlo simulations for ion-channeling studies of complex defects in crystals. Theory and Simulation in Physics for Materials Applications: Cutting-Edge Techniques in Theoretical and Computational Materials Science, pages 133–160, 2020. doi:10.1007/978-3-030-37790-8_8.DOI
- [25]Leah Bergman and Robert J Nemanich. Raman spectroscopy characterization of semiconductors. Annu. Rev. Mater. Sei, 26:551–79, 1996. pdf.
- [26]Christian Kranert, Chris Sturm, Rüdiger Schmidt-Grund, and Marius Grundmann. Raman tensor elements of β-Ga₂O₃. Scientific reports, 6(1):35964, 2016. doi:10.1038/srep35964.DOI
- [27]D Dohy, G Lucazeau, and A Revcolevschi. Raman spectra and valence force field of single-crystalline β-Ga₂O₃. Journal of Solid State Chemistry, 45(2):180–192, 1982. doi:10.1016/0022-4596(82)90274-2.DOI
- [28]T. Onuma, S. Fujioka, T. Yamaguchi, Y. Itoh, M. Higashiwaki, K. Sasaki, T. Masui, and T. Honda. Polarized Raman spectra in β-Ga₂O₃ single crystals. Journal of Crystal Growth, 401:330–333, 2014. Proceedings of 17th International Conference on Crystal Growth and Epitaxy (ICCGE-17), doi:10.1016/j.jcrysgro.2013.12.061.DOI
- [29]Kun Zhang, Zongwei Xu, Shengnan Zhang, Hong Wang, Hongjuan Cheng, Jianmin Hao, Jintong Wu, and Fengzhou Fang. Raman and photoluminescence properties of un-/ion-doped β-Ga₂O₃ single-crystals prepared by edge-defined film-fed growth method. Physica B: Condensed Matter, 600:412624, 2021. doi:10.1016/j.physb.2020.412624.DOI
- [30]DR Myers, PL Gourley, and PS Peercy. The effects of ion-implantation damage on the first-order Raman spectra of GaP. Journal of applied physics, 54(9):5032–5038, 1983. doi:10.1063/1.333773.
- [31]Kartik N Shinde, SJ Dhoble, HC Swart, and Kyeongsoon Park. Phosphate phosphors for solid-state lighting. Springer Science & Business Media, 2012.DOI
- [32]S Prucnal, L Rebohle, and W Skuropa. Blue electroluminescence of ytterbium clusters in SiO₂ býáco-operative up-conversion. Applied Physics B, 98:451–454, 2010. doi:10.1007/s00340-009-3751-1.DOI
- [33]Mahwish Sarwar, Renata Ratajczak, Vitalii Yu Ivanov, Sylwia Gieraltowska, Aleksandra Wierzbicka, Wojciech Wozniak, René Heller, Stefan Eisenwinder, and Elżbieta Guziewicz. Crystal lattice recovery and optical activation of yb implanted into β-Ga₂O₃. Materials, 17(16):3979, 2024. doi:10.3390/ma17163979.DOI
- [34]Kenji Yamaguchi. First principles study on electronic structure of β-Ga₂O₃. Solid state communications, 131(12):739–744, 2004. doi:10.1016/j.ssc.2004.07.030.DOI
- [35]Xi Guo, Mengmeng Chang, Jinbin Wang, Ruxue Bai, Xiangli Zhong, Fabi Zhang, Fengmin Wu, and Daoyou Guo. Gallium vacancy displacement damage induced by 1 MeV neutron irradiation in β-Ga₂O₃ solar-blind photodetector. The European Physical Journal Special Topics, pages 1–9, 2024. doi:10.1140/epjs/s11734-024-01387-w.DOI
- [36]Linpeng Dong, Renxu Jia, Bin Xin, Bo Peng, and Yuming Zhang. Effects of oxygen vacancies on the structural and optical properties of β-Ga₂O₃. Scientific reports, 7(1):40160, 2017. doi:10.1038/srep40160.DOI
- [37]Rujun Sun, Yu Kee Ooi, Praneeth Ranga, Arkka Bhattacharyya, Sriram Krishnamoorthy, and Michael A Scarpulla. Oxygen annealing induced changes in defects within β-Ga₂O₃ epitaxial films measured using photoluminescence. Journal of Physics D: Applied Physics, 54(17):174004, 2021. doi:10.1088/1361-6463/abdefb.DOI
- [38]J. B. Varley, J. R. Weber, A. Janotti, and C. G. Van de Walle. Oxygen vacancies and donor impurities in β-Ga₂O₃. Applied Physics Letters, 97(14):142106, 2010.DOI
- [39]Laurent Binet and Didier Gourier. Origin of the blue luminescence of β-ga2o3. Journal of Physics and Chemistry of Solids, 59(8):1241–1249, 1998.DOI
- [40]Parvaneh Ravadgar, Ray-Hua Horng, Li-Wei Tu, Sin-Liang Ou, Hui-Ping Pan, and Shu-De Yao. Defects study of MOCVD grown β-Ga₂O₃ films. In Oxide-based Materials and Devices IV, volume 8626, pages 239–246. SPIE, 2013. doi:10.1117/12.2002913.DOI
- [41]DM Esteves, AL Rodrigues, LC Alves, E Alves, MI Dias, Z Jia, W Mu, K Lorenz, and M Peres. Probing the Cr³⁺ luminescence sensitization in β-Ga₂O₃ with ion-beam-induced luminescence and thermoluminescence. Scientific Reports, 13(1):4882, 2023. doi:10.1038/s41598-023-31824-0.DOI
- [42]Honghui Zhou, Matthew F Chisholm, Punam Pant, Hye Jung Chang, J Gazquez, Stephen J Pennycook, and Jagdish Narayan. Atomic structure of misfit dislocations in nonpolar ZnO/Al₂O₃ heterostructures. Applied Physics Letters, 97(12), 2010. doi:10.1063/1.3489687.DOI