betaFeedback

WorksPhysics and Astronomy

The effect of iron layer thickness on the interlayer exchange coupling in Fe/MgO (001) superlattices

Abstract

We describe the effect of the Fe layer thickness on the antiferromagnetic interlayer exchange coupling in [Fe/MgO]N_N superlattices. An increase in coupling strength with increasing Fe layer thickness is observed, which highlights the need of including the extension of both the layers when discussing the interlayer exchange coupling in superlattices.

Introduction

Epitaxial Fe/MgO heterostructures have sparked an intense research effort due to their large tunneling magnetoresistance [2] [1]. High crystal quality trilayer Fe/MgO/Fe heterostructures exhibit antiferromagnetic interlayer exchange coupling (IEC) [4, 5, 6] [3] mediated by spin-polarized tunneling through the MgO barrier [7, 8] [3]. The coupling strength is exponentially decaying with increasing MgO layer thickness tMgOt_{\mathrm{MgO}} [9, 10, 11]. In [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N superlattice structures with NN Fe/MgO bilayers, the interlayer exchange coupling has also been observed to exponentially decay with tMgOt_{\mathrm{MgO}} between 16.3 and 22.1 Å MgO [5]. Furthermore, in these epitaxial [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N superlattices, discrete layer-by-layer magnetic switching is observed, resulting from the competition between the interlayer coupling and magnetocrystalline anisotropy [5]. However, understanding and tuning the sequential magnetic switching in these heterostructures and the precise mechanism governing it has been proven challenging [6, 12]. The MgO layer thickness, impurities or defects in the MgO layer, temperature, and growth conditions are important parameters affecting the interlayer coupling [5, 6, 9, 11, 13, 14, 15] [3]. Oxygen vacancies [9, 13], along with magnetic impurities which might be present in the MgO layers [15] have also been shown to be relevant. Finally, a non-trivial dependence of the coupling strength in [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N superlattices on the number of bilayer repetitions, i.e., the extension of the whole stack has been reported [12].

Systematic variations of the MgO layer thickness in previous works [5, 9, 10, 11] relate to the modification of the tunneling barrier. On the other hand, the study of the dependence on NN in superlattices, highlights potential collective effects between quantum well states in the Fe layers making up the [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N superlattices [12]. A detailed investigation of the Fe layer thickness dependence, would thus shed light on the importance of the extension of the quantum wells formed in the Fe layers for the interlayer coupling strength. To this end, we investigate the influence of the Fe layer thickness on the IEC and sequential switching in [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N superlattices. The Fe layer thickness was varied while the MgO layer thickness was kept constant. We present a detailed characterization of the layering and crystal structure of the superlattices, employing x-ray scattering techniques, and report on the increase of the IEC with increasing Fe layer thickness.

Methods

Superlattices of [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_N with N=8N = 8 and 10 bi-layer repetitions were deposited on single crystalline MgO (001) substrates by direct current (dc) and radio frequency (rf) magnetron sputtering. Within one deposition process, identical copies were grown on a 10×10 mm210 \times10\ \mathrm{mm}^2 and a 20×20 mm220 \times20\ \mathrm{mm}^2 sized substrate, eliminating this way all uncertainties concerning differences in growth conditions. The thicknesses of the MgO layers were kept constant at tMgO=17(1)t_{\mathrm{MgO}} = 17(1) Å, while the thickness of the Fe layers was chosen to vary in the range of tFe=11t_{\mathrm{Fe}} = 11 to 23 Å. Prior to the deposition, the substrates were annealed in vacuum at 1273(2) K for 600 s. The base pressure of the growth chamber was below 5×10−75 \times10^{-7} Pa. The target-to-substrate distance in the deposition chamber was approximately 20 cm. The depositions were carried out in an Ar atmosphere (gas purity ≥99.999\geq99.999 %, and a secondary getter based purification) from an elemental Fe (50 W, dc, diameter: 5.08 cm) and an MgO compound target (50 W, rf, diameter: 5.08 cm) at 438(2) K and 0.67 Pa. Target power and deposition temperature were optimized previously with respect to well-defined layering in combination with the highest crystal quality. In order to prevent surface oxidation of the films, the samples were capped at ambient temperature (<313(2)< 313(2) K) and 1.07 Pa with 50 Å Pt (50 W, dc, diameter: 5.08 cm). The targets were cleaned by sputtering against closed shutters for at least 60 s prior to the deposition of each layer. The deposition rates (Fe: 0.1 Å/s, MgO: 0.01 Å/s, Pt: 0.8 Å/s) were calibrated prior to the growth of the samples. In order to ensure thickness uniformity, the substrate holder was rotated at 30 rpm during the deposition.

X-ray reflectometry (XRR) and diffraction (XRD) were carried out using a Bede D1 diffractometer equipped with a Cu Kα1_{\alpha1} x-ray source operated at 35 mA and 50 kV. For monochromatizing the beam by reducing the Cu Kβ_\beta radiation, the setup included a Göbel mirror and a Ni filter on the incidence and detector side, respectively. A circular beam mask (diameter: 0.005 m), incidence and detector slits (both 0.0005 m) were also used. The X-rays were detected with a Bede EDRc x-ray detector. The instrument angles for the coupled 2θ2\theta-θ\theta scans were aligned to the sample surface for XRR and to the [Fe/MgO] crystal planes for XRD measurements. The measured XRR data was fitted using GenX [16, 17] enabling the determination of the scattering length density (SLD) profile, which includes information on layer thickness and roughness. Rocking curve measurements in XRD were fitted with a Pseudo-Voigt function to mimic the effect of mosaic spread.

Figure 1. a) X-ray scattering pattern of a [Fe/MgO]10_{10} superlattice with 20(1) Å Fe layer thickness. In b) x-ray reflectivity is displayed separately including a fit. The scattering length density profile based on the fit is displayed in the inset. c) X-ray diffraction of [Fe/MgO]10_{10} superlattice samples with different Fe layer thicknesses.

Magnetization measurements were performed at ambient temperature using a longitudinal magneto-optical Kerr effect (L-MOKE) setup with ss-polarized light. The magnetic response was measured parallel to an in-plane applied magnetic field along the Fe magnetic easy and hard axes, i.e. Fe [100] and Fe [110], respectively. The data was averaged over 10 full loop recordings. Additional measurements were conducted in an Evico Magnetics KerrLab Kerr microscope in longitudinal and transverse mode. The determined saturation fields are corrected for the coercivity. The values of the saturation field along magnetic easy and hard axes were determined by the intersection of the hysteresis loop with two straight lines at M=MSM = M_S (the hard axis case is illustrated in the SM). Displayed error bars of the saturation fields and the remanence magnetization correspond to the standard deviation of the extracted parameters from the two symmetrical axes (90-degrees sample rotation), two field-scan directions, and two field polarities.

Results and Discussion

Layering and crystal structure

A full x-ray scattering pattern of an [Fe/MgO]10_{10} superlattice with 20(1) Å Fe and 17(1) Å MgO layer thicknesses is displayed in Fig. 1a. Below 10 degrees in 2θ2\theta, pronounced Kiessig fringes [18] are observed, consistent with the presence of flat and distinct layering with low layer roughness (below 5(1) Å), which is confirmed in the scattering length density (SLD) profile based on a fit displayed in Fig. 1b. All nominal Fe and MgO layer thicknesses within this study were determined using XRR. Analysis of the results confirmed that the MgO layer thickness was the same, 17(1) Å, while the thicknesses of the Fe layers were determined to be 11(1) Å, 15(1) A˚15(1)\,\text{\AA}, 20(1) A˚20(1)\,\text{\AA}, and 23(1) A˚23(1)\,\text{\AA}. Henceforth, all presented thicknesses correspond to the experimentally determined thicknesses of the Fe and MgO layers.

Diffraction peaks at around 39 and 43 degrees in 2θ2\theta are observed, arising from the Pt capping and the MgO (001) substrate, respectively. Laue oscillations around the Pt Bragg peak are obtained for all the samples, see Fig. 1c, providing conclusive evidence for well-defined texture and thickness of the Pt layer [19]. Fe/MgO superlattice satellite peaks are visible between 52 and 70 degrees in 2θ2\theta. Their spacing and positions relate to the Fe/MgO bilayer thickness and, hence, vary with Fe layer thickness, which was confirmed with x-ray scattering intensity simulations employing GenL [19]. Their intensity relates to the amount of scattering material, i.e., the total Fe and MgO layer thicknesses. Furthermore, the satellite peak intensity is elevated by the broad Fe (002) Bragg peak, which is observed at around 65 degrees in 2θ2\theta. The Bragg peak intensity relates to the total Fe layer thickness and is, therefore, higher for the samples with thicker Fe layers. No Laue oscillations are visible between the superlattice satellite peaks for [Fe/MgO]8_8 and [Fe/MgO]10_{10}. This is attributed to the mismatch between the layers, giving rise to defects causing incoherent scattering from the Fe atomic planes [20, 21]. The out-of-plane atomic distances in Fe and MgO are 2.866 Å [22] and 4.212 Å [23], respectively. Hence, the atomic step heights in the Fe and MgO lattices are incommensurate, yielding finite terrace widths in the superlattice, which can suppress both, diffraction peaks as well as Laue oscillations [19, 24]. This is in stark contrast to, e.g., the growth of [Fe/V]N_N (001) superlattices, within which the layers have similar lattice parameters [25]. Furthermore, the mismatch results in biaxial elastic in-plane strain in both Fe and MgO, which may cause a tetragonal distortion of the cubic unit cells. Strain in Fe has an impact on its magnetic properties [26]. Moreover, dislocations for relaxation at the critical thickness, which is around 20 Å for Fe (001) on MgO (001) [21], can affect the magnetic properties. Defects may also originate from substrate twinning, which is common in commercially available MgO substrates [27]. More twins and larger mosaic spreads were observed for 20×2020\times20 mm2^2 compared to 10×1010\times10 mm2^2 substrates. In specular scans for samples on 20×2020\times20 mm2^2 substrates, multiple reflections attributed to asymmetric substrate peaks were observed, indicating defects in the single crystalline structure. This difference in crystal quality between the substrates is found to alter the magnetic properties in [Fe/MgO]N_N superlattices (see Supplemental Material (SM)). Therefore, a comparison between samples, in particular for different (substrate) batches, has to be done with care, as observations in magnetic properties need to be related to the crystal structure.

Magnetic characterization

Magnetic hysteresis loops of [Fe/MgO]10_{10} superlattices, measured with an applied magnetic field along the Fe easy axis, are displayed in Figure 2a. Kerr microscopy revealed domain wall nucleation and motion during the magnetization reversal, as expected in sequential switching of the magnetic layers. The magnetic domain size in the Fe layers was determined to lie in the order of several hundreds of micrometers to millimeters [28] and is, thus, comparable to the probing area of L-MOKE measurements. No dependence of the domain size on the Fe layer thickness was found. Hence, sequential switching of the layers in the superlattices is apparent from the presence of discrete steps in the field response, which is assumed to stem from a single or few domains in each Fe layer. The findings are in line with previous reports [5, 6]. Coming from positive saturation, the first switching occurs at a positive applied field, in agreement with an antiferromagnetic IEC of the Fe layers in all samples [5, 6]. The hysteresis loops obtained for the samples having 8 bilayers, are shown in the SM.

Figure 2. Magnetic hysteresis loops of [Fe/MgO]10_{10} superlattices measured with L-MOKE on 10×1010\times10 mm2^2 samples with varying Fe layer thickness with an applied field along the a) Fe magnetic easy axis, i.e., Fe [100] and b) Fe magnetic hard axis, i.e., Fe [110].

Figure 3. Remanent magnetization MRM_R normalized to the saturation magnetization MSM_S displayed over Fe layer thickness tFet_{\mathrm{Fe}} for [Fe/MgO]N_N superlattices with 8 and 10 bilayer repetitions NN on 10 × 10 mm2^2 substrates for an applied magnetic field along the Fe easy axis.

The remanent configuration changes with Fe layer thickness. For the sample with the thinnest Fe layers, 11(1) Å, the remanent state corresponds to 0.48(6) × MSM_S, consistent with every other layer pointing along the sensitivity axis and the others oriented perpendicular to that [6, 12]. The inferred 90 degrees configuration could either be enabled by the presence of an activation barrier for the switching or by the presence of a biquadratic coupling [15]. Biquadratic coupling is commonly associated with coupling in systems with metal spacer layers, which varies between antiferromagnetic and ferromagnetic with varying spacer layer thickness. Biquadratic coupling may be attributed to an extrinsic fluctuation mechanism leading to frustration of the bilinear exchange coupling [29, 30]. However, for insulating spacers, the coupling is reported to be only antiferromagnetic [8]. A 90 degrees remanent configuration has been observed for [Fe/MgO]10_{10} superlattices with thicker MgO barriers of 19.6 Å, which was attributed to the coupling strength being smaller than the nucleation field of the domain reversal in the samples [6]. In contrast, the remanent magnetization in the samples with larger Fe layer thickness is closer to being compensated, i.e., 0.151(3) × MSM_S, 0.039(4) × MSM_S, and 0.031(5) × MSM_S for the samples with 15(1), 20(1), and 23(1) Å Fe layer thickness, respectively. A compensated remanent state corresponds to a fully antiferromagnetic alignment and was reported for [Fe/MgO]10_{10} with thinner MgO barriers of 16.4 Å [6], having larger coupling strength as compared to the thicker layers [5]. In these samples, the coupling between the Fe layers seems however sufficiently strong to drive the order to an antiferromagnetic remanent state. The normalized remanent magnetization MR/MSM_R/M_S is plotted as a function of Fe layer thickness in Fig. 3 for [Fe/MgO]8_8 and [Fe/MgO]10_{10}. Independent of whether a superlattice consists of 8 or 10 bilayer repetitions, the remanent magnetization decreases with increasing Fe layer thickness.

Besides the coupling strength, different strain states can affect the magnetic properties of Fe [26] and defects can act as pinning points for domain wall motion. In Fe layers exceeding the critical thickness of around 20 Å, a higher defect density is expected. However, no signs of domain wall pinning in samples with thicker Fe layers is observed. The metastable 90 degrees configuration is observed for samples with thinner Fe layers and based on the hysteresis loops displayed in Figure 2a, the coercive field is not found to be increasing with increasing Fe layer thickness. Hence, the influence of different strain states on the remanent configuration is neglected in the further analysis.

The same relative change in remanent magnetization MR/MSM_R/M_S with Fe layer thickness is observed in loops measured with an applied field along the Fe magnetic hard axis, which are displayed in Figure 2b for [Fe/MgO]10_{10} superlattices. Here we notice that more than four times larger fields are required to overcome the crystalline anisotropy as compared to the saturation field along the easy axis of the samples. Differences in the switching are also noticed for the two magnetic field directions, where discrete steps are observed up until 2 to 5 mT, when the field is applied along the hard axis of the samples. The magnetization at these fields is approximately 0.63 × MSM_S, indicating a mixture of switching and coherent rotation of layers. Hence, when the applied field is along the easy axis, the individual layers do switch, one or more at the time, which is not observed when the field is applied along the hard axis. Above the threshold, the change in the alignment of magnetization of the Fe layers appears to be dominated by coherent rotation for fields along the hard axis. The saturation fields along the easy and hard axes, HSEAH_S^{EA} and HSHAH_S^{HA}, were extracted from the hysteresis loops. The results are shown in Figure 4. As seen in the figure, the saturation field increases with increasing Fe layer thickness in both cases.

Figure 4. Saturation field HSH_S displayed over Fe layer thickness tFet_{\mathrm{Fe}} for [Fe/MgO]N_N superlattices with 8 and 10 bilayer repetitions NN on 10×1010 \times10 mm2^2 substrates for an applied magnetic field along a) the Fe easy axis, b) the Fe hard axis.

To obtain quantitative determination of JJ and KK, we define the energy density EiE_i of the layer ii as:

Ei=−μ0MSHcos⁡(θi)+K4sin⁡2(2θi)−Jcos⁡(θi−θi+1)−Jcos⁡(θi−θi−1),(1)E_i = -\mu_0 M_S H \cos(\theta_i) + \frac{K}{4}\sin^2(2\theta_i) - J\cos(\theta_i-\theta_{i+1}) - J\cos(\theta_i-\theta_{i-1}), \tag*{(1)}

where MS=1.71M_S = 1.71 kA/m is the saturation magnetization [31], μ0\mu_0 is the vacuum permeability, HH is the applied field, and θi\theta_i is the angle of the magnetization of the layer ii measured from the easy axis. For the outermost layers, with only one neighboring Fe layer present, one of the last two terms vanishes. With this definition, JJ is negative for an antiferromagnetic IEC. From this expression, it is possible to calculate the saturation field along the hard axis HSHAH_S^{\mathrm{HA}} (see SM) as:

HSHA=2K−4Jμ0MS.(2)H_S^{\mathrm{HA}} = \frac{2K - 4J}{\mu_0 M_S}. \tag*{(2)}

The dependence of the saturation field along the easy axis HSEAH_S^{\mathrm{EA}} as a function of KK and JJ is not accessible in an analytical form for a multilayer structure [32] [1] and has therefore to be extracted from simulations of the data. The functional dependence of HSEA(K,J)H_S^{\mathrm{EA}}(K,J) was calculated, and it was found that it decays with KK, converging to HSEA=−2J/MSH_S^{\mathrm{EA}} = -2J/M_S in the limit of large K/∣J∣K/|J| (for details see SM). With both experimental values for HSHAH_S^{\mathrm{HA}}, HSEAH_S^{\mathrm{EA}} and Eq. (2) as well as HSEA(K,J)H_S^{\mathrm{EA}}(K,J) (see SM), it is possible

to calculate the values of the coupling strength JJ and the Fe cubic anisotropy KK, which are shown in Figure 5. The anisotropy is determined to be weakly changing with Fe thickness (60(4) kJ/m3^3) in the range studied here. For 20 Å Fe on MgO, hence in a comparable thickness range, a K=56K = 56 kJ/m3^3 was reported [3]. Moreover, in line with the findings about the remanent state being affected by the Fe layer thickness, the antiferromagnetic coupling strength is found to increase with Fe layer thickness, independent of the number of bilayer repetitions.

Figure 5. a) Fe cubic anisotropy KK and b) volumetric coupling strength JJ displayed over Fe layer thickness tFet_{\mathrm{Fe}} for [Fe/MgO]N_N superlattices with 8 and 10 bilayer repetitions NN on 10×1010 \times10 mm2^2 substrates determined from hysteresis loops measured with an applied magnetic field along the Fe easy and hard axes.

Summary

The antiferromagnetic coupling strength [Fe/MgO]N_N superlattices with 17 Å thick MgO layers is found to linearly increase with Fe layer thickness, in the range between 11 and 23 Å. The Fe cubic anisotropy was determined to be weakly increasing in the same thickness range, being close to the value reported for Fe single layers. These findings indicate that the coupling in [Fe/MgO]N_N superlattices is not solely defined by the thickness of the MgO barriers, but along with the number of bilayer repetitions NN [12], the thickness of the individual Fe layers is also an essential parameter. This calls for a closer look on the coupling mechanism and effects in such superlattices, highlighting the importance of all length scales present in these (tMgOt_{\mathrm{MgO}}, tFet_{\mathrm{Fe}}, and N(tMgO+tFe)N(t_{\mathrm{MgO}}+t_{\mathrm{Fe}})). These observations challenge our current understanding of electronic and spin effects in magnetic quantum well structures comprised of metal-oxide heterostructures, with potential impact on emergent technologies employing their magnetic properties.

Acknowledgments

VK would like to acknowledge financial support from the Swedish Research Council (Project No. 2019-03581). MPG and VK also acknowledge support from the Carl Trygger Foundation (Project No. CTS21:1219).

Data availability

The data that support the findings of this study are available from the authors upon reasonable request.

References

Magnetic hysteresis loops of superlattices with 8 bilayer repetitions

The magnetic hysteresis loops of [Fe/MgO]8[\mathrm{Fe}/\mathrm{MgO}]_{8} superlattices with varying Fe layer thickness, measured with an applied field along the Fe magnetic easy and hard axis, are shown in Supplementary Fig. 1a and b, respectively. Qualitatively, the loops exhibit the same shape as the loops recorded for superlattices with 10 bilayer repetitions. All extracted values for relative remanent magnetization MR/MSM_{\mathrm{R}}/M_{\mathrm{S}} and saturation fields μ0HSEA\mu_{0}H_{\mathrm{S}}^{\mathrm{EA}} and μ0HSHA\mu_{0}H_{\mathrm{S}}^{\mathrm{HA}} are displayed in the main text.

Figure 1 (PDF p. 7). Magnetic hysteresis loops of [Fe/MgO]8[\mathrm{Fe}/\mathrm{MgO}]_{8} superlattices measured with L-MOKE on 10×10 mm210 \times10\ \mathrm{mm}^{2} samples with varying Fe layer thickness with an applied field along the a) Fe magnetic easy axis, i.e., Fe [100] and b) Fe magnetic hard axis, i.e., Fe [110].

Dependence of the magnetic properties on the substrate size

All analysis presented in the main text was conducted on [Fe/MgO]N[\mathrm{Fe}/\mathrm{MgO}]_{N} superlattices grown on 10×10 mm210 \times10\ \mathrm{mm}^{2} MgO (001) substrates. However, copies of the deposited [Fe/MgO]10[\mathrm{Fe}/\mathrm{MgO}]_{10} superlattices on 20×20 mm220 \times20\ \mathrm{mm}^{2} MgO (001) substrates show differences in the magnetization reversals, displayed in Supplementary Figure S2, despite an identical layering and a similar crystal structure. All 20×20 mm220 \times20\ \mathrm{mm}^{2} samples exhibit a remanent state around 0.5(0)×MS0.5(0) \times M_{\mathrm{S}} corresponding to a 90 degrees orientation of the magnetization in the Fe layers at remanence. The sample with 15(1) Å Fe layer thickness shows a slightly lower remanent magnetization but exhibits 0.5(0)×MS0.5(0) \times M_{\mathrm{S}} already at applied fields below 1 mT. A strong dependence of the shape of the magnetic hysteresis loop on the measured position on the sample was found. Furthermore, the saturation field of the [Fe/MgO]10[\mathrm{Fe}/\mathrm{MgO}]_{10} superlattices on 20×20 mm220 \times20\ \mathrm{mm}^{2} MgO (001) substrates is significantly lower and in the order of 10 to 15(1) mT, compared to their copies on 10×1010 \times10 mm2^2 substrates. Based on the previous analysis of remanent state and saturation field, the coupling strength in the samples on 20×2020 \times20 mm2^2 is smaller compared to their 10×1010 \times10 mm2^2 counterparts. Nevertheless, the trends observed for the saturation fields with Fe layer thickness were found to be valid for both, 20×2020 \times20 mm2^2 and 10×1010 \times10 mm2^2 samples in relative comparison.

Figure S2. Magnetic hysteresis loops of [Fe/MgO]10_{10} superlattices measured with a Kerr microscope on 20×2020 \times20 mm2^2 samples with varying Fe layer thickness with an applied field along the Fe magnetic easy axis, i.e., Fe [100].

The change in magnetic properties is attributed to differences in the substrate quality. As the switching mechanism in [Fe/MgO]N_N superlattices is found to rely on domain wall movements, crystallographic defects may inhibit this motion and lower the coupling strength between the layers. More surface area of an MgO (001) substrate increases the probability for the presence of crystallographic twins and an increase in mosaic spread, i.e., crystal misorientation, in line with the analysis of the crystal structure of the superlattices on these substrates, presented above. Therefore, the coupling strength in [Fe/MgO]N_N superlattices is found to be highly dependent on substrate quality and crystal structure/quality.

Dependence of the easy-axis saturation field on KK and JJ

The dependence of HSEAH_S^{EA} as a function of the antiferromagnetic IEC JJ and the cubic anisotropy KK only becomes trivial in the limit of large KK [S1, S2], where:

HSEA=2Jμ0MS.(3)H_S^{EA} = \frac{2J}{\mu_0 M_S}. \tag*{(3)}

In this limit, the switching process is modeled by a first-order transition where the magnetization of one layer is exactly 90 or 180 degrees from the direction defined by the applied field. This process is known as spin-flip. When the cubic anisotropy is weaker, the magnetization of the different layers can explore a broader range of configurations in order to minimize the energy.

In the case where the magnetization of one layer rotates to θ=π/2\theta= \pi/2, the system can further minimize its energy if the magnetization of the two neighboring layers drives away from saturation. This could be understood from the large slope of the term Jcos⁡(θi−θ±1)J \cos(\theta_i-\theta_{\pm1}) in Eq. (1) in the main text, when θi−θ±1=π/2\theta_i-\theta_{\pm1} = \pi/2, and the small slope of μ0HMScos⁡(θ±1)\mu_0 H M_S \cos(\theta_{\pm1}) when θi=0\theta_i = 0. Therefore, it is expected that the value of HSEAH_S^{EA} depends on both KK and JJ as HSEA=F(J,K)H_S^{EA} = F(J,K). This dependence can be written as h=f(k)μ0MSh = \frac{f(k)}{\mu_0 M_S}, where h=HSEA/∣J∣h = H_S^{EA}/|J| and k=K/∣J∣k = K/|J| are adimensional parameters. In order to explore this dependence, Eq. 1 in the main text was used to determine the angle θ±1\theta_{\pm1}, which minimizes the energy, and the field at which the spin-flip becomes energetically favorable. The minimal model to study the deviation from Eq. S1 requires considering 5 layers. To calculate the reduced saturation field hh, a switched state is proposed, and its energy is compared with the saturated state. In the switched configuration, the angles θi\theta_i of the magnetization of the layer ii are:

θ1=θ5=0,θ2=θ4=δ,θ3=π/2.(4)\begin{aligned} \theta_1 &= \theta_5 = 0, \\ \theta_2 &= \theta_4 = \delta, \\ \theta_3 &= \pi/2. \tag*{(4)} \end{aligned}

It must be noted that if θ3\theta_3 is unconstrained, it always minimizes the energy at the exact angle of π/2\pi/2. By taking a step in δ\delta of 0.009 rad, and 0.0011 in hh it was possible to obtain f(k)f(k). A similar procedure was followed to calculate the reduced field related to a spin-flop transition (second-order transition), where the system transitions from saturation to a configuration with θodd=−θeven\theta_{\mathrm{odd}}=-\theta_{\mathrm{even}}. In this case, only two layers have to be considered. However, to take the boundary conditions imposed by the outermost layers into account, the IEC term in Eq. (1) in the main text has to be multiplied by a factor (N−1)/N(N-1)/N, where NN is the amount of layers of the superlattice. The results for both spin-flip and spin-flop are shown in Supplementary Fig. 3. For values under k=1k=1, spin-flop dominates at higher fields.

Figure 3 (PDF p. 9). Calculated values of ff as a function of the reduce parameter k=K/∣J∣k=K/\lvert J\rvert. For each kk, the highest value dominates the transition from saturation.

It can be observed that in the limit of large kk the factor f(k)f(k) for spin-flip converges to 2 in agreement with Eq. (3). From Postava et al. [S3] and Eq. (3) is it possible to estimate that kk should lie close to 3. Therefore, f(k)f(k) can be approximated in the range k∈[2.8;3.9]k\in[2.8; 3.9] by a linear function fl(k)=Ak+Bf_l(k)=Ak+B. With this simplified expression, the saturation field can be calculated as:

HSEA=AK+BJμ0MS,(5)H_{S}^{\mathrm{EA}}=\frac{AK+BJ}{\mu_{0}M_{S}}, \tag*{(5)}

where A=−0.04A=-0.04 and B=−2.26B=-2.26.

Dependence of the hard-axis saturation field on K and J

For extracting values for the coupling strength from hard axis hysteresis loops, a ferromagnetic multilayer with a fourfold magnetocrystalline anisotropy is considered. The interlayer exchange coupling is antiferromagnetic (J<0J<0). When the external magnetic field HH is reduced from saturation, each layer system goes through a second-order transition at the critical field HSHAH_{S}^{HA}, as shown in Supplementary Fig. 1b or in the main text. At lower fields, the angle θi\theta_i between the magnetization of each layer MiM_i and the magnetic field takes a non-zero value. Therefore, the total magnetization along the field direction can be calculated as MSN∑iNcos⁡(θi)\frac{M_S}{N}\sum_{i}^{N}\cos(\theta_i), where NN is the number of layers. However, if N>2N>2, the layers with two neighbors present a higher saturation field HSHAH_{S}^{HA} which can be extracted from the measured hysteresis loops. For each of these "middle" layers, if even and odd layers angles satisfy θ=−θ\theta=-\theta, the energy density per layer is reduced to:

E=−μ0MSHcos⁡(θ)−K4sin⁡2(2θ)−Jcos⁡(2θ).(6)E=-\mu_{0}M_{S}H\cos(\theta)-\frac{K}{4}\sin^{2}(2\theta)-J\cos(2\theta). \tag*{(6)}

From here, the minima can be found from:

∂E∂θ=μ0MSHsin⁡(θ)−Ksin⁡(2θ)cos⁡(2θ)+2Jsin⁡(2θ)=0.(7)\frac{\partial E}{\partial\theta}=\mu_{0}M_{S}H\sin(\theta)-K\sin(2\theta)\cos(2\theta)+2J\sin(2\theta)=0. \tag*{(7)}

Using sin⁡(2θ)=2sin⁡(θ)cos⁡(θ)\sin(2\theta)=2\sin(\theta)\cos(\theta), this equation can be written as:

μ0MSHsin⁡(θ)−4Ksin⁡(θ)cos⁡(θ)cos⁡(2θ)+4Jsin⁡(θ)cos⁡(θ)=0.(8)\mu_{0}M_{S}H\sin(\theta)-4K\sin(\theta)\cos(\theta)\cos(2\theta)+4J\sin(\theta)\cos(\theta)=0. \tag*{(8)}

One trivial solution is θ=0\theta= 0 and it represents the ground state at H>HSHAH > H_{S}^{HA}. We know that below the saturation field, this minimum will no longer be the ground state and the system will transition to a solution with θ≠0\theta\ne0. However, at the critical field, this second solution should present θ=0\theta= 0. Therefore, by discarding the trivial solution and imposing θ=0\theta= 0 we obtain μ0MSH−8K+4J=0\mu_{0}M_{S}H - 8K + 4J = 0, and the critical field is calculated as:

HSHA=2K−4Jμ0MS.(9)H_{S}^{HA} = \frac{2K - 4J}{\mu_{0}M_{S}}. \tag*{(9)}

At this field, all the layers are expected to go through a soft transition. From this expression and Eq. (5), it is possible to calculate the values of JJ and KK from HSHAH_{S}^{HA} and HSEAH_{S}^{EA}.

Experimental determination of HSHA

For each sample, hysteresis loops were measured with L-MOKE along the two hard axis directions, i.e., Fe [110] and [1̄10]. The saturation field was determined from the intersection with a straight line at M/MS=1M/M_{S} = 1. One example of this procedure is given in Figure 4.

Figure Supplementary Fig. 4. Magnetic hysteresis loop of a [Fe/MgO]10_{10} superlattice measured with L-MOKE on a 10×1010 \times10 mm2^{2} sample with an Fe layer thickness 15(1) Å. The external magnetic field is applied along a Fe magnetic hard axis, i.e., Fe [110]. The red lines indicate the error of the estimated saturation field.

For the determination of the saturation field along the easy axis, a similar procedure was followed, but the error was smaller as the switching of the magnetization direction from saturation is more abrupt.

References

References

  1. [2]S. Yuasa, T. Nagahama, A. Fukushima, Y. Suzuki, and K. Ando, Nat. Mater. 3, 868 (2004).
  2. [4]T. Ishigaki, T. Kawahara, R. Takemura, K. Ono, K. Ito, H. Matsuoka, and H. Ohno, in 2010 Symposium on VLSI Technology (2010) pp. 47–48.
  3. [5]R. Moubah, F. Magnus, T. Warnatz, G. K. Palsson, V. Kapaklis, V. Ukleev, A. Devishvili, J. Palisaitis, P. O. A. Persson, and B. Hjörvarsson, Phys. Rev. Appl. 5, 044011 (2016).
  4. [6]F. Magnus, T. Warnatz, G. K. Palsson, A. Devishvili, V. Ukleev, J. Palisaitis, P. O. A. Persson, and B. Hjörvarsson, Phys. Rev. B 97, 174424 (2018).
  5. [7]J. C. Slonczewski, Phys. Rev. B 39, 6995 (1989).
  6. [8]P. Bruno, Phys. Rev. B 52, 411 (1995).
  7. [9]T. Katayama, S. Yuasa, J. Velev, M. Y. Zhuravlev, S. S. Jaswal, and E. Y. Tsymbal, Appl. Phys. Lett. 89, 112503 (2006).
  8. [10]A. Kozioł-Rachwał, W. Skowroński, M. Frankowski, J. Chęciński, S. Ziętek, P. Rzeszut, M. Ślęzak, K. Matlak, T. Ślęzak, T. Stobiecki, and J. Korecki, J. Magn. Magn. Mater. 424, 189 (2017).
  9. [11]C. Bellouard, A. Duluard, E. Snoeck, Y. Lu, B. Negulescu, D. Lacour, C. Senet, S. Robert, N. Maloufi, S. Andrieu, M. Hehn, and C. Tiusan, Phys. Rev. B 96, 134416 (2017).
  10. [12]T. Warnatz, F. Magnus, N. Strandqvist, S. Sanz, H. Ali, K. Leifer, A. Vorobiev, and B. Hjörvarsson, Sci. Rep. 11, 1942 (2021).
  11. [13]M. Y. Zhuravlev, E. Y. Tsymbal, and A. V. Vedyayev, Phys. Rev. Lett. 94, 026806 (2005).
  12. [14]C. Bellouard, J. Faure-Vincent, C. Tiusan, F. Montaigne, M. Hehn, V. Leiner, H. Fritzsche, and M. Gierlings, Phys. Rev. B 78, 134429 (2008).
  13. [15]Y. F. Chang, J. J. Li, J. W. Wong, X. Tan, Y. Li, K. Pi, W. H. Wang, H. W. K. Tom, and R. K. Kawakami, Phys. Rev. B 79, 184410 (2009).
  14. [16]M. Björck and G. Andersson, J. Appl. Crystallogr. 40, 1174 (2007).
  15. [17]A. Glavic and M. Björck, J. Appl. Crystallogr. 55, 1063 (2022).
  16. [18]H. Kiessig, Ann. Phys. 402, 715 (1931).
  17. [19]A. L. Ravensburg, J. Bylin, G. K. Pålsson, and V. Kapaklis, arXiv e-prints, arXiv:2310.13539 (2023), arXiv:2310.13539 [cond-mat.mtrl-sci].
  18. [20]T. Mühge, A. Stierle, N. Metoki, H. Zabel, and U. Pietsch, Appl. Phys. A 59, 659 (1994).
  19. [21]A. L. Ravensburg, G. K. Pålsson, M. Pohlt, B. Hjörvarsson, and V. Kapaklis, Thin Solid Films 761, 139494 (2022).
  20. [22]J. L. Vassent, M. Dyna, A. Marty, B. Gilles, and G. Patrat, J. Appl. Phys. 80, 5727 (1996).
  21. [23]G. Chiarotti, 1.6 Crystal structures and bulk lattice parameters of materials quoted in the volume: Datasheet from Landolt-Börnstein - Group III Condensed Matter · Volume 24B: “Electronic and Vibrational Properties” in SpringerMaterials (1994), Springer-Verlag Berlin Heidelberg.
  22. [24]H. Raanaei, H. Lidbaum, A. Liebig, K. Leifer, and B. Hjörvarsson, J. Phys. Condens. Matter. 20, 055212 (2008).
  23. [25]P. Isberg, B. Hjörvarsson, R. Wäppling, E. Svedberg, and L. Hultman, Vacuum 48, 483 (1997).
  24. [26]M. Friák, M. Šob, and V. Vitek, Phys. Rev. B 63, 052405 (2001).
  25. [27]J. Schroeder, A. Ingason, J. Rosén, and J. Birch, J. Cryst. Growth 420, 22 (2015).
  26. [28]T. Warnatz, Magnetic Properties of Epitaxial Metal/Oxide Heterostructures, Ph.D. thesis, Uppsala University, Materials Physics (2021).
  27. [29]J. C. Slonczewski, Journal of Applied Physics 73, 5957 (1993), https://pubs.aip.org/aip/jap/article-pdf/73/10/5957/18657325/5957_1_online.pdf.
  28. [30]S. O. Demokritov, Journal of Physics D: Applied Physics 31, 925 (1998).
  29. [31]J. Crangle and G. M. Goodman, Proc. R. Soc. A, Mathematical and Physical Sciences 321, 477 (1971).
  30. [32]P. J. H. Bloemen, H. W. van der Kesteren, H. J. M. Swagten, and W. J. M. de Jonge, Phys. Rev. B 50, 13505 (1994).

Paper details

vlnc:W_8hay7mdh
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents