Cubic-Zn(1-x)Mn(x)Te optical modes across the phonon and phonon-polariton regimes

Abstract

Alloying offers a convenient route to tune the physical properties of semiconductors, at the price, however, of local lattice/bond distortions needed to accommodate the lattice mismatch. Being nearly lattice-matched and moreover highly resistant to lattice and bond distortions thanks to a largely covalent bonding, cubic Zn(1-x)Mn(x)Te sets a benchmark to test the sensitivity of lattice vibrations to minimum lattice and bond distortions induced by alloying. We explore experimentally the two transverse optical regimes of cubic Zn(1-x)Mn(x)Te (x<0.7), with ab initio calculations in support: (1) the phonon-polariton regime at quasi-infinite (photon-like) wavelengths averaging over the alloy disorder, probed by forward-Raman scattering, and (2) the purely-mechanical phonon regime down to minimum wavelengths nearly matching the lattice constant zooming into the alloy disorder, achieved by inelastic neutron scattering. The short Zn-Te bond is found to exhibit a compact optical duo distinguishing homo from hetero local bond environments (1 bond: 2 mode), as explained by the percolation model. This deviates from the historical Zn(1-x)Mn(x)Te MREI (modified-random-element-isodisplacement) scheme inspired from classical Raman and infrared studies, in which the optical modes are blind to the bond environment (1-bond: 1-mode). So, the test is positive, reinforcing the status of the percolation scheme as a robust decryptor of (even small) lattice distortions induced by alloying through the lattice dynamics.

The disordered (high-entropy) magnetic II-VI semiconductors alloys (SCA) involving the magnetic Mn2+^{2+} ion in substitution, such as Zn1−x_{1-x}Mnx_xTe with cubic/zincblende-zb structure (x≤0.7x \le0.7), are attractive for spintronics due to their capacity to combine, through alloying, magnetic and optical properties[1]. A major drawback, however, is that alloying causes local lattice distortions, needed to accommodate the contrasts in atom/bond physical properties (atomic mass, atomic size, bond length-ll, bond force constant-kk). The lattice distortions fragilize the crystal and degrade the physical properties, limiting applications[2].

The lattice dynamics offers a suitable playground to explore the lattice distortions at all length scales since the wavelength (λ\lambda) of lattice vibrations ranges from quasi infinite near the Brillouin zone center Γ\Gamma (BZC, q=2π×λ−1→0q = 2\pi\times\lambda^{-1} \to0), “averaging” over the alloy disorder, all the way down to minimum of twice the lattice constant (aa) near the Brillouin zone boundary (BZB, λ∼2×a\lambda\sim2 \times a), “zooming” into the alloy disorder.

For probing the lattice distortion of SCAs through the lattice dynamics the optical modes seem preferable over the acoustic modes. The latter are the genuine collective lattice vibrations, dragging all bond species of a SCA into the same dynamics, i.e., at the same frequency[3, 4]. As the acoustic modes already fail to distinguish bond species, a fortiori they presumably fail also to distinguish local environments of a given bond, being hence “double-blind”, i.e., bond-insensitive and environment-insensitive. In contrast, the optical modes, inherently originating from effective bond-stretching, offer a local (bond-related) insight into the lattice distortions. One may moreover hope that the optical modes are not only bond-sensitive but also environment-sensitive. The latter virtue is denied by the historical modified-random-element-isodisplacement (MREI) model[5] set at the emergence of zb-SCAs in the 1960s. Accordingly, the like bonds of a given species vibrate at the same frequency at a given composition xx (1-bond→\to1-mode), irrespectively of the local environment. One may say, in a nutshell, that the MREI optical modes are “single-blind”, i.e., bond-sensitive but environment-insensitive. In our percolation model, designed in the 2000s[6], the optical modes “see everything”, distinguishing homo from hetero environments per bond (1-bond→\to2-mode). The cluster model[7] promoted the same view ahead of time, distinguishing like bonds according to their first-neighbor environment, among four possible ones per bond in a zb-SCA (1-bond→\to4-mode). However, to our view the cluster model is biased[8, 9] – hence not further discussed below – by a 1D/3D ambivalence that the equations of motion per atom are scalar (one-dimensional, 1D) while the elementary oscillators behind the individual Raman/IR features, i.e., the first-neighbor clusters, are defined in the real (three-dimensional, 3D) crystal.

To elucidate the MREI vs. percolation nature of the lattice dynamics of a SCA, we focus on the transverse optical (TO) modes (u⃗⊥q⃗\vec{u} \perp\vec{q}), due to atom vibrations (u⃗\vec{u}) perpendicular to the direction of propagation (given by the wavevector q⃗\vec{q}). The TO modes exhibit a phonon-polariton (PP) regime[10, 11] resulting from phonon-photon coupling at quasi infinite (photon-like) wavelengths near Γ\Gamma (λ→104×a\lambda\to10^{4} \times a) plus a mechanical (mTO) phonon regime[10, 11], ruling over the BZwide rest (102×a>λ>a10^{2} \times a > \lambda> a) – methods. The TO variety contrasts with the basic invariance of the electrical/mechanical longitudinal optical (LO, u⃗∥q⃗\vec{u} \parallel\vec{q}) phonon[10, 11] (methods), offering the possibility to explore the alloy disorder from different (PP + mTO) angles. The PP and mTO regimes are probed by forward inelastic visible-light/Raman scattering[11] (forward-RS, schematically operated in “transmission”) using lasers and by inelastic neutron[12] (INS) or X-ray[12] (IXS) scattering using nuclear reactors and synchrotrons, respectively. The maximum qq achieved by RS (λ∼102×a\lambda\sim10^{2} \times a), i.e., in backward scattering (backward-RS, schematically operated in “reflection”)[11], matches the minimum qq achieved by INS/IXS[12]. So, RS and INS/IXS are complementary and not competing.

The percolation model successfully applied to all tested SCA so far, with cubic (zincblende[6], diamond[13]) and hexagonal (wurtzite[14]) structures, suggesting its universality. The emphasis was placed on mismatched SCA with the idea in mind, verified in the case studies, that a large mismatch (Δaa\frac{\Delta a}{a}) would clarify the percolation TO-duo per bond. Here, we proceed the other way around and test the percolation model on zb-Zn1−x_{1-x}Mnx_xTe that features an ultimately positive case of alloying. The Zn and Mn substituents stand close by on the same line of the periodic table and thus have comparable atomic masses (Δmm∼15%\frac{\Delta m}{m}\sim15\%) and covalent radii (ΔRcRc∼12%\frac{\Delta R_c}{R_c}\sim12\%). Remarkably, the light Mn atom is the big one. That matters for the percolation scheme (cf. infra). Besides, the lattice mismatch hits minimum (Δaa∼2.75%\frac{\Delta a}{a}\sim2.75\%, Mn-Te being the long species – cf. infra)[15] while the bond covalency hits maximum, falling between the II-VI and III-V values for Zn-Te[16, 17], and matching the III-V values for Mn-Te[18]. Generally, the bond-stretching and bond-bending force constants (symbolized by kk) increase with the bond covalency[19]. And along with it, the resistance to bond distortions in shear[16], inherent to alloying and so destabilizing for the lattice. In brief, being well-matched and highly covalent, zb-Zn1−x_{1-x}Mnx_xTe is subject to minimum lattice/bond distortions and is moreover highly resistant to lattice/bond distortions. As such, it features a benchmark to trace the onset of the percolation TO-duo per bond in SCAs back to a slight difference in bond relaxation/distortion depending on the local homo/hetero environment[6].

The state of the art about the zb-Zn1−x_{1-x}Mnx_xTe lattice relaxation/dynamics summarizes as follows. Mn incorporation achieves up to ∼70\sim70 at.% in the zb-lattice of ZnTe[1], differing from the NiAs-lattice of MnTe[20]. As apparent in extended X-ray absorption fine structure (EXAFS) data (0.15≤x≤0.650.15 \le x \le0.65)[22], the parent-like Zn-Te and Mn-Te bond lengths (ll) are preserved at any xx (within error bars), as in most zb-SCAs[21], and also the nominal tetrahedron angle (109.8∘109.8^\circ) of the regular zb-structure, even at maximum alloying (x∼0.5x \sim0.5). A bond softens (k↘k \searrow) when it is stretched (l↗l \nearrow), and vice versa. Along this naive one-to-one “lattice relaxation vs. lattice dynamics” 1D-correspondence, the ll-invariant 1-bond→\to1-ll EXAFS picture for zb-Zn1−x_{1-x}Mnx_xTe transposes into a kk-invariant 1-bond→\to1-kk MREI scheme for its mTO modes.

Earlier studies of the zb-Zn1−x_{1-x}Mnx_xTe lattice dynamics (Figure 1), listed below in chronological order, were conducted in-house using optical techniques, i.e., backward-RS and infrared-reflectivity (IR). By force of the quasi vertical dispersion of the visible (RS) and infrared (IR) light sources, both techniques operate near the BZC, specifically addressing the mTO and LO modes at qq values of the order of one percent of the BZsize[11] (λ∼102×a\lambda\sim10^2 \times a). Nothing whatsoever is yet produced about the zb-Zn1−x_{1-x}Mnx_xTe optical modes at lower (PP-like) or higher (BZB-like) qq values.

Overview of zb-Zn$_{1-x}$Mn$_x$Te optical modes at ambient conditions

Figure 1. Overview of zb-Zn1−x_{1-x}Mnx_xTe (x≤0.7x \le0.7) optical (mTO, LO) modes at ambient conditions. Existing mTO (filled symbols) and LO (empty symbols) frequencies, and current Raman data (circles) are indicated. Solid lines: quadratic mTO-frequency vs. xx MREI-like (two-mode) descriptions. Dotted lines: corresponding LO-frequency vs. xx variations derived from the LO-RCS. Thick curves: mTO MREI- (2-mode, right-oriented black curves/notations) and percolation-type (3-mode, left-oriented red curves/notations) RCS at the experimentally studied xx values. Thin curves: Corresponding LO MREI- (right-oriented black curves) and percolation-type (left-oriented red curves) RCS. Outside main panel: mTO (thick curves) and LO (thin curves) RCS of the parent compounds. A small phonon damping (1 cm−1^{-1}) is used throughout to distinguish small and/or neighboring features.

The pioneering IR[23, 24] and RS[24, 25, 26] studies, done at x≤0.15x \le0.15, pointed towards a 2-mode MREI pattern involving a large Zn-Te mTO-LO band beneath a narrow Mn-Te one, the two arranged into a compact mTO-LO-mTO-LO sequence. This is highly intricate due to a strong overlapping of the parent mTO-LO bands, the RS/IR frequencies matching within 4 cm−1^{-1} (Ref. 27). The phonon intricacy is aggravated by the Mn-impurity mode in zb-ZnTe (which marks the closure of the Mn-Te TO-LO band at x∼0x \sim0) being quasi degenerated with the matrix-like Zn-Te LO mode (within 2 cm−1^{-1}). A similar phonon intricacy, complicating the phonon assignment, occurs with zb-In1−x_{1-x}Gax_xAs[28] and zb-Cd1−x_{1-x}Znx_xTe[29]. By increasing xx the Mn-Te band expands while the Zn-Te band shrinks, as clarified by RS thanks to a breakthrough in crystal growth opening the entire zb-domain (x≤0.7x \le0.7)[27]. Notably, the lower LO mode suffers a major softening (∼20\sim20 cm−1^{-1}). All alternative optical modes are hardly xx-sensitive. Only, the m-TO branches slightly bend downward (by ∼10\sim10 cm−1^{-1}) in a ω(x)\omega(x)-plot (Figure 1, ω\omega is the phonon frequency), due to the macroscopic tensile strain suffered by both bond species when the lattice expands by increasing xx. Generally, the reported mTO Raman modes in the literature are obscured by LO modes nearby, rendering it difficult to appreciate any percolation-type mTO fine structure.

In this work we test whether the minimum lattice/bond distortions suffered by zb-Zn1−x_{1-x}Mnx_xTe suffice, or not, to generate any percolation TO-duo per bond beyond the admitted MREI description[27]. The test is done by specifically addressing experimentally the TO modes in their full (PP + mTO) diversity using high-quality zb-Zn1−x_{1-x}Mnx_xTe (x≤0.70x \le0.70)[27] single crystals grown by the Bridgman technique (methods, Figure S1 – the prefix S stands for supplementary material). The mTO regime is studied not only in backward-RS near the BZC (λ∼102×a\lambda\sim10^2 \times a)[11] but also by INS near the BZB (λ∼2×a\lambda\sim2 \times a) in hope that a percolation mTO-duo for Zn1−x_{1-x}Mnx_xTe, if any, will be best resolved at the latter limit, as observed with cubic-Zn0.67_{0.67}Be0.33_{0.33}Se[30] and hexagonal-Zn0.67_{0.67}Mg0.33_{0.33}S[14]. Forward-RS is further used to probe the PP dispersion from the deep photon-like regime ultimately close to the BZC (forward-RS, λ→104×a\lambda\to10^{4} \times a) all the way back to the native mTO-regime of the PPs (backward-RS, λ∼102×a\lambda\sim10^{2} \times a)[11]. The experimental data are discussed using our generic qq-dependent PP-RCS set within the linear dielectric formalism (specifically using Eq. 1 of Ref. 29), covering the PPs together with their asymptotic mTO and LO modes near the BZC (104×a≥λ≥102×a10^{4} \times a \ge\lambda\ge10^{2} \times a), with ab initio (SIESTA[31]) mTO-phonon calculations near the BZC (λ∼102×a\lambda\sim10^{2} \times a) at x∼0x \sim0 in support.

Zn$_{1-x}$Mn$_x$Te crystal structure

Figure S1. Zn1−x_{1-x}Mnx_xTe crystal structure. (a) Powder X-ray diffractograms recorded at nearly ambient pressure on the PSICHÉ beamline of synchrotron SOLEIL with the 0.3738 Å radiation at x=0.12x=0.12 and 0.37. The diffraction lines due to Au used for pressure calibration are indicated. The individual peaks are labeled using the (hkl) Miller indices of the corresponding diffraction planes in the zincblende-zb structure. (b) a(x)a(x) dependence (symbols) derived from the lattice parameter aa and the composition xx independently measured in laboratory by powder X-ray diffraction with the Cu K-alpha radiation at ambient pressure and by applying the inductively coupled plasma-optical emission spectroscopy method to powders, respectively. The linear a(x)a(x) variation found by Liu et al.[15] using epitaxial layers is added for comparison.

Results and discussion

A basic rule is that the percolation TO-duo is best resolved for the small-RcR_{\mathrm{c}} substituent, hence typically the light one that vibrates at high frequency[6]. This is because the small substituent has more room to accommodate locally the lattice mismatch, with concomitant impact on its TO frequencies, being more diversified. Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} is a special case in that the small-RcR_{\mathrm{c}} substituent, i.e., Zn, is the heavy one, vibrating a low frequency. This points towards a three-TO {2×(Zn−Te),1×(Mn−Te)}\{2 \times(\mathrm{Zn}-\mathrm{Te}), 1 \times(\mathrm{Mn}-\mathrm{Te})\} percolation scheme.

Mechanical-TO (m-TO) phonon regime

In principle, the native mTO regime of the PPs is best suited to elucidate the TO mode behavior of a SCA. This is because mechanical modes hardly couple and thus preserve the natural phonon diversity of a complex system like a SCA. The mTO modes of pristine zb-ZnTe[32, 33] and zb-MnTe[34] hardly disperse across the BZ (by few cm−1\mathrm{cm}^{-1} at most), suggesting the same for zb-Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te}. The Anderson’s criterion for phonon localization[35] is thus easily fulfilled. Hence, even minor changes in bond distortion, e.g., those depending on the local homo/hetero bond environment in the spirit of the percolation model, are likely to generate distinct mTO modes per bond.

Pure-mTO Γ\Gamma-like ab initio calculations

A pure-mTO ab initio insight near Γ\Gamma at x∼0x \sim0 suffices to fix ideas. An isolated Mn atom in a large (64-atom) zb-ZnTe supercell (x∼0x \sim0) generates a local compression because Mn-Te is longer than Zn-Te. The Zn-Te bonds near Mn are thus shorter than the matrix-like Zn-Te bonds (Figure 2b) and hence create a minor/local mTOZn−TeMnmTO_{\mathrm{Zn-Te}}^{\mathrm{Mn}} mode due to Zn-Te vibrations (subscript) in the hetero Mn-environment (superscript) at a higher frequency than the dominant/matrix mTOZn−TeZnmTO_{\mathrm{Zn-Te}}^{\mathrm{Zn}} mode due to Zn-Te bonds away from Mn vibrating in homo environment (Figure 2a, inset). Small as it is (∼5 cm−1\sim5\ \mathrm{cm}^{-1}), the mTOZn−TeMnmTO_{\mathrm{Zn-Te}}^{\mathrm{Mn}}-mTOZn−TeZnmTO_{\mathrm{Zn-Te}}^{\mathrm{Zn}} frequency gap is a priori visible by RS (∼0.3 cm−1\sim0.3\ \mathrm{cm}^{-1}) and possibly also by INS away from Γ\Gamma[14, 30] (∼13 cm−1\sim13\ \mathrm{cm}^{-1} at ∼160 cm−1∼20 meV\sim160\ \mathrm{cm}^{-1} \sim20\ \mathrm{meV}), thanks to the high spectral resolutions of both techniques, as specified in brackets.

Zb-Zn1-xMnxTe mTO regime

Figure 2. Zb-Zn1−x_{1-x}Mnx_xTe mTO regime. (a) Ab initio (SIESTA code) Zn-Te (curve) and Mn-Te (shaded curve) mTO Γ\Gamma-projected PhDOS of a large (2×2×22 \times2 \times2) zb-Zn31_{31}Mn1_1Te32_{32} supercell (x∼0x \sim0). Mn creates a local compression, as sketched out (diverging arrows), impacting the phonon frequencies and bond lengths (trans-panel arrows). (b) Corresponding bond lengths (ll) distribution. (c) Crossed-polarized pure-mTO Zn1−x_{1-x}Mnx_xTe backward-RS spectra recorded with the incident laser excitation λi=632.8\lambda_i = 632.8 nm across the zb-domain (x≤0.7x \le0.7). (d) Zn0.63_{0.63}Mn0.37_{0.37}Te mTOZn−Tem\mathrm{TO}^{\mathrm{Zn-Te}} Raman intensity as a function of the azimuth angle α\alpha in crossed (filled symbols, ⊥\perp) and parallel (hollow symbols, ∥\parallel) polarizations of the incident (e⃗i\vec{e}_i) and scattered (e⃗s\vec{e}_s) lights. The theoretical Greekcross- (solid line) and butterfly-like (dotted line) motifs are superimposed, for comparison. (e) Zn0.33_{0.33}Mn0.67_{0.67}Te mTO INS spectra recorded along [001ˉ][00\bar{1}] near the BZC-(331) (at 10% of the BZsize, central curve) and near the BZB-(330) (at 90% of the BZsize, top curve). The neutron data (symbols) are fitted (thick curves) by two (∼\simBZC) and three (BZB) Gaussian functions (thin curves) using oblique baselines. The mTO backward-RS spectrum near the BZC-(000) (at 1% of the BZsize, bottom curve) is added for reference purpose. AA denotes acoustic modes.

Backward Raman scattering

Pure-mTO zb-Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} backward-RS spectra display separate Zn-Te (lower) and Mn-Te (upper) MREI-like signals (Figure 2c). The Zn-Te duo and the Mn-Te mode are genuine mTO modes at any xx, as was verified by symmetry analysis in crossed/parallel polarizations (Figure 2d-Figure S2), further attesting the high vibrational quality of our crystal series. The symmetry analysis is not so positive at maximum alloying (not shown). So, x=0.51x=0.51, while punctually used thereafter, is not emphasized below.

Polarized Zn$_{1-x}$Mn$_x$Te mTO backward-RS spectra

Figure S2. Polarized Zn1−x_{1-x}Mnx_xTe mTO backward-RS spectra taken with the incident laser excitation λi=632.8\lambda_i = 632.8 nm. Cross (top, ⊥\perp) and parallel (down, ∥\parallel) polarized Zn1−x_{1-x}Mnx_xTe mTO backward-RS spectra excited at the same sample spot of (110)-cleaved crystal faces depending on the azimuth angle α\alpha between the incident polarization (e⃗i\vec{e}_i) and the [1ˉ10][\bar{1}10] crystal axis across the zb-phase, as sketched out (right). (a/b) x=0.12x=0.12. (c/d) x=0.37x=0.37. (e/f) x=0.67x=0.67. (g/h). Corresponding experimental (symbols) vs. theoretical (curve) Greekcross- (⊥\perp) and butterfly-like (∥\parallel) α\alpha-variations of the Zn-Te Raman intensity at small (x=0.12x=0.12, g) and large (x=0.67x=0.67, h) alloying. Corresponding data at moderate alloying (x=0.67x=0.67) are shown in Figure 2d. AA denotes acoustic modes.

Looking closely, the Zn-Te signal around maximum zb-alloying (x=0.51,0.67x=0.51, 0.67) seems bimodal. According to the ab initio insight (Figure 2a), the lower and upper modes are assigned as mTOZn−TeZnmTO_{\mathrm{Zn-Te}}^{\mathrm{Zn}} and mTOZn−TeMnmTO_{\mathrm{Zn-Te}}^{\mathrm{Mn}}, respectively. The Raman intensities scale as ∼2\sim2:1 at x=0.51x=0.51 and ∼1\sim1:1 at x=0.67x=0.67, indicating a sensitivity to homo (pure-Zn + Zn/Mn-mixed) and hetero (pure-Mn) environments up to second-neighbors[9, 29], assuming a random Zn/Mn substitution. As xx gets smaller, the related oscillator fractions (f-terms) massively turn to the advantage of the lower-mTOZn−TeZnmTO_{\mathrm{Zn-Te}}^{\mathrm{Zn}} mode. The Zn-Te duo nevertheless persists in the form of a slightly asymmetrical Zn-Te lineshape at x∼0.3x \sim0.3 (the intensity ratio is ∼\sim6:1) but disappears at x∼0.1x \sim0.1 (∼\sim50:1). This is consistent with the only reported pure-mTO Zn1−x_{1-x}Mnx_xTe RS spectrum in the literature, taken by Peterson et al.[27] at x=0.19x=0.19 (Figure 2b therein), showing no trace of the Zn-Te duo.

In brief, there are positive signs of a Zn-Te mTO duo near the BZC (λ∼102×a\lambda\sim10^2\times a) at moderate/large Mn content. However, the duo is so compact that it can hardly emerges in ab initio nor in experiment (backward-RS), unless one attentively concentrates on it.

Inelastic neutron scattering

The situation might improve by INS. Indeed, the percolation Zn-Te mTO-duo being due to a slight difference in local lattice relaxation around Zn-Te depending on its homo/hetero environment, it should be best resolved by INS at minimum λ\lambda (∼2×a\sim2\times a) “zooming” into the local alloy disorder than by RS at large λ\lambda (104×a>λ>102×a10^4\times a>\lambda>10^2\times a) “averaging” over the alloy disorder[14, 30]. The Zn-Te mTO-duo, while compact when probed by RS near the BZC (λ∼102×a\lambda\sim10^2\times a, Figure 2e, bottom curve), broadens in INS data acquired along [001ˉ][00\bar{1}] at ∼10%\sim10\% of the BZsize (λ∼10×a\lambda\sim10\times a, central curve) and eventually divides into a distinct duo near the BZB (λ→a\lambda\to a, top curve), as expected. Small error bars due to large neutron-counting times (six hours per spectrum) ascertain the trends, clarified by two- (∼\simBZC) and three-Gaussian (BZB) fits (solid curves) of the neutron data (symbols). Nevertheless, although the INS data point toward a change in paradigm from the MREI model to a percolation picture for Zn1−x_{1-x}Mnx_xTe, they should be regarded as indicative only, since the relatively large sample (∼75 mm3\sim75\ \mathrm{mm}^3) investigated by INS does not exhibit the same high structural quality as the smaller crystal pieces (a few mm3\mathrm{mm}^3) used for RS (methods).

Phonon-polariton (PP) regime

Additional experimental insight is searched for by departing from the mTO-phonon regime probed by INS/backward-RS and exploring the PP regime by forward-RS. Advantage is taken that the small-RcR_c substituent (Zn) supporting the best-resolved TO-duo in principle (cf. supra) vibrates at low frequency. In this rare case (given that the small-RcR_c substituent is generally the light one vibrating at high frequency), the TO-duo, however compact it may be in the mTO-phonon regime away from Γ\Gamma, breaks away on entering the PP regime towards Γ\Gamma. Basically, the lower submode dramatically softens by converging onto the quasi vertical photon asymptote, whereas the upper submode remains pinned within the native m-TO band. In Figure 3, an overview of the zb-Zn0.63_{0.63}Mn0.37_{0.37}Te qq-dependent PP-RCS involving a percolation mTO-duo reflecting a sensitivity of Zn-Te vibrations to second neighbors, is illustrative with this respect. Both the Raman frequencies (curves) and the Raman intensities (thickness of curves) are indicated.

Zn₀.₆₃Mn₀.₃₇Te phonon-polariton Raman cross section

Figure 3. Zb-Zn₀.₆₃Mn₀.₃₇Te phonon-polariton Raman cross section (PP-RCS). Main panel. Zn₀.₆₃Mn₀.₃₇Te qq-dependent PP-RCS in a generic percolation-type three-mode {2×(Zn−Te),1×(Mn−Te)}\{2 \times(\mathrm{Zn}-\mathrm{Te}), 1 \times(\mathrm{Mn}-\mathrm{Te})\} description including a triple fine structure of the mTOMn−TemTO_{\mathrm{Mn-Te}} oscillator (see text for detail). The PP dispersion (frequency aspect, curves) and Raman efficiency (intensity aspect, thickness of curves) are indicated. Ph±Ph^{\pm} denote the phonon asymptotes (dotted/red lines, methods). Raman scan lines at various scattering angles θ\theta for the incident laser excitation λi=632.8\lambda_i =632.8 nm are indicated (oblique/red curves). Right. Native mTO-RCS of the PPs at large qq in the crude three-mode (thick/red curve) and refined “three-mode + fine structure” (thin/black curve) descriptions. Left. Corresponding asymptotic LO-RCS limits of the PPs at q=0q=0 (using the same code). Top. Zn₀.₆₃Mn₀.₃₇Te θ\theta-dependent PP-RCS throughout the PP regime in the refined “three-mode + fine structure” description (thin curves) calculated for the 632.8 nm incident laser excitation. ωT\omega_T and cc used to define the dimensionless yy parameter from qq are the mTO frequency of pristine ZnTe and the speed of light in vacuum, respectively. A small phonon damping (1 cm⁻¹) is used throughout to distinguish small and/or neighboring features.

To probe the kind of PP-RCS shown in Figure 3 nothing yet can be expected from ab initio calculations due to the difficulty in handling the macroscopic qq-dependent photon-like PP electric field. Prospective ab initio calculations of the PP dispersion (frequency aspect) are underway for pristine cubic-GaP and hexagonal-GaN[36], however, not addressing the Raman efficiency (intensity aspect). INS/IXS fall also short of addressing PPs due to a common selection rule limiting the INS/IXS insight to the sole longitudinal modes within the first BZ, where the photon dispersion develops[12] and hence also the PP coupling. The point is that PPs are transverse modes[11]. Forward-RS is the only option left, yet unused to study the PPs of SCAs, apart in our own recent works (Ref. 29 and refs. therein).

At any xx, cross-polarized zb-Zn1−x_{1-x}Mnx_xTe forward-RS spectra taken with the 632.8 nm laser line manifest three novel features (Figure S3-Figure S4), absent in backward-RS. The three consist of genuine PPs since they disperse and strengthen/collapse by changing θ\theta. The TO character is further attested by the three modes obeying the same forward-RS selection rules (Figure 4-Figure S4) as their native Zn-Te and Mn-Te mTO modes probed in backward-RS (Figure S2). The lower-PPint−PP^{int-} and upper-PPint+PP^{int+} modes refer to the heavy Zn-Te and light Mn-Te bonds, respectively. The intermediary-PPint−PP^{int-} mode disperses near the Zn-Te mTO band, hence ZnTe-like. Altogether, the three PPs support an effective change of paradigm from MREI/2-mode to percolation/3-mode for zb-Zn1−x_{1-x}Mnx_xTe (x≤0.7x\le0.7).

Forward-RS spectra across the phonon-polariton regime

Figure 4. Zb-Zn0.67_{0.67}Mn0.33_{0.33}Te forward-RS spectra across the phonon-polariton regime. (a) Cross-polarized Zn0.67_{0.67}Mn0.33_{0.33}Te forward-RS PP spectra depending on the scattering angle θ\theta inside the crystal, as sketched out, taken with the incident laser excitation λi=632.8\lambda_i=632.8 nm. The corresponding backward-RS spectra taken at the same crystal spot in the mTO regime of the PPs is added (top/thick curve), for reference purpose. Inset. Zn0.63_{0.63}Mn0.37_{0.37}Te PP−PP^- Raman intensity at θmin⁡∼0∘\theta_{\min}\sim0^\circ in its dependence on the azimuth angle α\alpha (Figure 2) in crossed (filled symbols) polarizations (e⃗i⊥e⃗s\vec{e}_i \perp\vec{e}_s). The raw data are shown in Figure S4. The theoretical Greekcross-like (solid line) motif is superimposed, for comparison. (b) Nominal percolation-type 3-mode {2×(Zn−Te),1×(Mn−Te)}\{2 \times(Zn-Te), 1 \times(Mn-Te)\} (red curves) PP-RCS at qmin⁡q_{\min} (θ=0∘\theta=0^\circ) for the 632.8 nm laser line and corresponding asymptotic LO (q=0q=0) and mTO (qmax⁡q_{\max}) RCS. Truncated 2-mode {1×(Zn−Te),1×(Mn−Te)}\{1 \times(Zn-Te), 1 \times(Mn-Te)\} descriptions are used to generate the uncoupled PP−PP^- and PPint+PP^{int+} RCS (black curves) separately due to mTOZn−TeZnmTO^{Zn}_{Zn-Te} and mTOZn−TeMnmTO^{Mn}_{Zn-Te}, respectively, at qmin⁡q_{\min}. Dashed guidelines are used to facilitate the comparison between the experimental (a) and theoretical (b) Raman frequencies. A small phonon damping (1 cm−1^{-1}) is used throughout to distinguish small and/or neighboring features. AA denotes acoustic modes.

Figure S3

Figure S3. Zn0.33Mn0.67Te\mathrm{Zn}_{0.33}\mathrm{Mn}_{0.67}\mathrm{Te} forward-RS spectra across the phonon-polariton regime. (a) Cross-polarized Zn0.33Mn0.67Te\mathrm{Zn}_{0.33}\mathrm{Mn}_{0.67}\mathrm{Te} forward-RS PP spectra depending on the scattering angle θ\theta inside the crystal, taken with the incident laser excitation λi=632.8 nm\lambda_i = 632.8\ \mathrm{nm}. The corresponding backward-RS spectra taken at the same crystal spot in the native mTO regime of the PPs is added (top/thick curve), for reference purpose. Inset. Zn0.63Mn0.67Te\mathrm{Zn}_{0.63}\mathrm{Mn}_{0.67}\mathrm{Te} PPint+PP^{int+} Raman intensity at θmin⁡∼0∘\theta_{\min} \sim0^\circ as a function of the azimuth angle α\alpha (as sketched out in Figure 2) in crossed (filled symbols) polarizations (e⃗i⊥e⃗s\vec{e}_i \perp\vec{e}_s). The raw data are shown in Figure S4. The theoretical Greekcross-like (solid line) motif is superimposed, for comparison. (b) Nominal percolation-type 3-mode {2×(Zn−Te),1×(Mn−Te)}\{2 \times(\mathrm{Zn}-\mathrm{Te}), 1 \times(\mathrm{Mn}-\mathrm{Te})\} (red curves) PP-RCS at qmin⁡q_{\min} (θ∼12∘\theta\sim12^\circ) for the 632.8 nm laser line and corresponding asymptotic LO (q=0q=0) and mTO (qmax⁡q_{\max}) RCS. Truncated 2-mode {1×(Zn−Te),1×(Mn−Te)}\{1 \times(\mathrm{Zn}-\mathrm{Te}), 1 \times(\mathrm{Mn}-\mathrm{Te})\} descriptions are used to generate the uncoupled PP−PP^- and PPint+PP^{int+} RCS (black curves) separately due to mTOZn−TeZnmTO^{\mathrm{Zn}}_{\mathrm{Zn}-\mathrm{Te}} and mTOZn−TeMnmTO^{\mathrm{Mn}}_{\mathrm{Zn}-\mathrm{Te}}, respectively, at qmin⁡q_{\min} (see main text). Dashed guidelines are used to facilitate the comparison between the experimental (a) and theoretical (b) Raman frequencies. A small phonon damping (1 cm−1\mathrm{cm}^{-1}) is used throughout to distinguish small and/or neighboring features. AA denotes acoustic modes.

Polarized zb-Zn$_{1-x}$Mn$_x$Te forward-RS spectra

Figure S4. Polarized zb-Zn1−x_{1-x}Mnx_xTe forward-RS spectra (θ∼0∘\theta\sim0^\circ) taken with the incident laser excitation λi=632.8\lambda_i = 632.8 nm. Cross-polarized (⊥\perp) Zn1−x_{1-x}Mnx_xTe forward-RS spectra excited at the same sample spots of (110)-cleaved crystal faces depending on the azimuth angle α\alpha between the incident polarization (e⃗i\vec{e}_i) and the [1ˉ10][\bar{1}10] crystal axis across the zb-phase, as sketched out in Figure S2. (a) x=0.12x=0.12. (b) x=0.37x=0.37. (c) x=0.67x=0.67. AA denotes acoustic modes.

PP-coupling

However, the observed PPs exhibit odd attributes. First (anomaly 1), the high-frequency (superscript) PPint+PP^{int+} (probed at θmin∼0∘\theta_{min}\sim0^\circ) and LO+LO^+ (θ\theta-independent) modes are sharper than their native Zn-Te and Mn-Te mTO modes (probed at θmax∼180∘\theta_{max}\sim180^\circ). Second (anomaly 2), at θmin\theta_{min} PPint−PP^{int-} and PPint+PP^{int+} emerge at lower frequencies than predicted by theory (PP-RCS) even in perfect forward-RS (θ=0∘\theta=0^\circ, Figure 4 – double-arrows). This happens to such extent that PPint−PP^{int-} even disperses (slightly) outside the ZnTe mTO duo/band, and not inside it (anomaly 3). It is just the opposite for LO+LO^+ (a variant of anomaly 2), showing up at (slightly) higher frequency in experiment than predicted by theory (LO-RCS, Figure S3).

Anomaly 1 (linewidth) cannot be explained by a breaking of the translational symmetry due to the alloy disorder, leading to the contribution of q≠0q\ne0 modes to the Raman signal, in the spirit of the spatial correlation model[37], as done, e.g., for Al1−x_{1-x}Gax_xAs, another well-matched zb-SCA[3]. Indeed, the mTO and LO modes of zb-ZnTe are hardly dispersive and much dispersive, respectively[32, 33]. So, involving q≠0q\ne0 modes besides the nominal Raman active q=0q=0 modes would leave the mTO mode sharp and broaden the LO mode. This is just the opposite for zb-Zn1−x_{1-x}Mnx_xTe. In fact, it was argued that the spatial correlation model may not apply in case of alloying, the Raman signal primarily referring to q=0q=0[38].

The conjunction of anomalies 1 (linewidth) and 2 (frequency) affecting PPint+PP^{int+} and LO+LO^+ cannot be merely fortuitous, suggesting a common origin. Notably, anomaly 1 marks a difference between, on the one hand, PPint+PP^{int+} and LO+LO^+, carrying electric fields (ET,LE_{T,L}, the subscript standing for transverse-PP and longitudinal-LO), and, on the other hand, their native purely-mechanical mTO modes. Hence, anomaly 1 relates to ET,LE_{T,L}. To appreciate how anomaly 1 develops with qq, PP+PP^+ is a better candidate than LO+LO^+ since ETE_T carried by PPint+PP^{int+} is qq-dependent whereas ELE_L accompanying LO+LO^+ is permanent. Basically, ETE_T achieves maximum in the deep PP regime probed by forward-RS near Γ\Gamma at θ→0\theta\to0 and vanishes to zero by deviating a few degrees from the strict normal incidence/detection, which suffices to off-shift the TO modes away from Γ\Gamma towards the native mTO regime of the PPs.

Anomaly 1 affecting the Mn-related PPint+PP^{int+} mode is especially clear at large Mn content (x=0.37x=0.37, 0.67 – Figure 4-Figure S3). A close examination of the θ\theta-dependent forward-RS spectra reveals that PPint+PP^{int+} suffers an abrupt, and not progressive, broad→sharp transition on crossing the photon-like PPint+PP^{int+} extinction near the S-inflexion, at which limit ETE_T suddenly takes on a macroscopic (photon-like) character. Basically, PPint+PP^{int+} is broad ante extinction (away from Γ\Gamma), as its native mTO mode, and sharp post extinction (near Γ\Gamma). Notably, just beyond the S-like extinction, PPint+PP^{int+} is fast (photon-like), well-supported by the lattice (phonon-like, attested by a significant Raman efficiency) and has a long lifetime (sharp). This is interesting for photonics in view to transfer information at high velocity through the lattice in the THz.

To our view, anomaly 1 reflects an intramode transfer of oscillator strength mediated by ETE_T. This presupposes some fine structuring of the native mTO modes of the PPs. The fine structure originates from local xx-fluctuations inherent to alloying, impacting the Raman frequencies. Ante extinction, ETE_T has not yet developed into a macroscopic field and remains local. So, the elementary PPint+PP^{int+} modes due to the individual mTO submodes forming the fine structure hardly ETE_T-couple. In this “uncoupled” case, the overall PPint+PP^{int+} (ET≠0E_T\ne0) and mTO (ET=0E_T=0) modes exhibit similar fine structures “echoing” each other. Hence, the PPint+PP^{int+} and mTO modes are equally broad. Post extinction, the elementary PPint+PP^{int+} submodes couple via ETE_T that has turned macroscopic. The net effect of the ETE_T-coupling is to channel most of the available oscillator strength towards the lower PPint+PP^{int+} oscillator of the series, becoming giant and downshifted beneath the series[39]. It is just the opposite for the ELE_L-coupling, the upper oscillator being favored and upshifted[39, 40]. As PPint−PP^{int-} at θmin\theta_{min} and LO+LO^+ refer to a unique mode of the series, they are both sharp, explaining anomaly 1. Anomaly 2 affecting PPint+PP^{int+} and LO+LO^+ is due to their respective downward and upward shifts.

The reported Zn0.63_{0.63}Mn0.37_{0.37}Te PPint+PP^{int+} simulations for the 632.8 nm laser line in Figure 3 (top curves) illustrate how the ETE_T-coupling develops by reducing θ\theta. A discrete Mn-Te mTO fine structure is involved, arbitrarily comprising three equally-spaced sub-mTO oscillators – sufficient to fix ideas – sharing the available Mn-Te oscillator strength in proportion to 30%-40%-30% (right, black curve). Ante extinction (θ↗\theta\nearrow) PPint+PP^{int+} divides into three distinct submodes with similar intensities in echo to the native three distinct mTOMn−TemTO_{Mn-Te} submodes. Post extinction, the lower PPint+PP^{int+} submode attracts most of the available Mn-Te oscillator strength. At θmin\theta_{min} this PPint+PP^{int+} submode (top, black curve) emerges below (double-arrows) the PPint+PP^{int+} mode generated in absence of mTOMn−TemTO_{Mn-Te} fine structuring (red curve).

At x∼0.37x\sim0.37, any mTOMn−TemTO_{Mn-Te} “manipulation” (absence/presence of fine structure) leaves the LO+LO^{+} frequency unchanged (Figure 3-Figure 4). However, anomaly 2 (upward shift) affecting the sharp LO+LO^{+} mode becomes appreciable at x∼0.67x\sim0.67 corresponding to similar Zn-Te and Mn-Te mTO Raman intensities (Figure S3). This supports an effective fine structuring of the latter two (broad) features from the LO point of view, in line with the PP point of view.

One may well wonder why PP−PP^{-} related to Zn-Te is not as sharp as PPint+PP^{int+} related to Mn-Te, since the native mTO modes of PPint+PP^{int+} and PP−PP^{-}, i.e., mTOMn−TemTO_{Mn-Te} and mTOZn−TeZnmTO^{Zn}_{Zn-Te}, respectively, are equally broad, hence subject to similar multi-mode decompositions. This PP−PP^{-} vs. PPint+PP^{int+} discrepancy is due to an experimental limitation of our forward-RS setup that the laser-focusing (ki⃗\vec{k_i}) and light-collecting (ks⃗\vec{k_s}) cones have finite angles. This generates a continuous distribution of scattering angles θ=(ki⃗,ks⃗)\theta= (\vec{k_i},\vec{k_s}) inside the crystal around the mean θˉ\bar{\theta} defined by the mean ki⃗\vec{k_i} and ks⃗\vec{k_s} along the cone axis. A typical θ\theta-uncertainty of Δθ∼±0.5\Delta\theta\sim\pm0.5 has been estimated for our forward-RS setup with hexagonal-GaN41. In turn Δθ\Delta\theta creates a Δω\Delta\omega uncertainty on the PPPP frequency. Its magnitude depends on the slope of the probed portion of the ω\omega vs. qq PPPP dispersion at θˉ\bar{\theta}. PPint+PP^{int+} probed at θmin\theta_{min} is sharp (Δω→0\Delta\omega\to0) because PPint+PP^{int+} is quasi dispersionless post the photon-like extinction where θmin\theta_{min} operates (Figure 3). In contrast, θmin\theta_{min} probes the bottleneck of the PP−PP^{-} dispersion on entry to the deep photon-like regime where the PP−PP^{-} dispersion is so steep (Figure 3). So, even if unimodal (cf. supra), the PP−PP^{-} mode at θmin∼0∘\theta_{min}\sim0^\circ, integrated over Δθ\Delta\theta, happens to be broad.

PP-decoupling

Anomaly 3 concerned with PPint−PP^{int-} is a separate case. By no way a simulation based on a fine structuring of the native mTO modes, so successful to explain anomalies 1 and 2 affecting PPint+PP^{int+} and LO+LO^{+}, can generate a PPint−PP^{int-} dispersion outside the Zn-Te mTO band (Figure 4b, double-arrows). Various attempts in this line (not shown), playing with the number and spacing of oscillators forming the mTO fine structure, repeatedly turned out to be a sterile exercise.

To our view the slight homo/hetero difference in local lattice distortions around the Zn-Te bonds, at the origin of the mTOZn−TeZn−mTOZn−TeMnmTO^{Zn}_{Zn-Te}-mTO^{Mn}_{Zn-Te} percolation mTO-duo, suffices to prevent an effective ETE_T-coupling between the related PP−PP^{-} and PPint−PP^{int-} modes. Hence, albeit the mTOZn−TeZnmTO^{Zn}_{Zn-Te} and mTOZn−TeMnmTO^{Mn}_{Zn-Te} modes are quasi degenerate (Figure 2), they engage the PP regime on their own as uncoupled modes. Retrospectively, the PP-decoupling is a positive surprise. By preserving their natural oscillator strengths, without ETE_T-mediated pooling, PPint−PP^{int-} and PP−PP^{-} remain visible at any θ\theta. Strictly speaking, due to their uncoupling, PPint−PP^{int-} and PP−PP^{-} should rather be labeled in terms of PPZn−TeMnPP^{Mn}_{Zn-Te} and PPZn−TeZnPP^{Zn}_{Zn-Te} in accordance with their direct mTOZn−TeMnmTO^{Mn}_{Zn-Te} and mTOZn−TeZnmTO^{Zn}_{Zn-Te} ascendants, respectively. However, the original notation is maintained since the latter two ZnTe-like modes, if not coupled to each other, do separately couple with the MnTe-like mode on entering the PP-regime.

At moderate Mn content (xx=0.12, 0.37), mTOZn−TeZnmTO^{Zn}_{Zn-Te} is awarded most of the available Zn-Te oscillator strength, and mTOZn−TeMnmTO^{Mn}_{Zn-Te} gets very few of it (Figure 5a). So, the related PP−PP^{-} and PPint−PP^{int-} modes at θmin\theta_{min} disperse far below the native mTO band and very close to it, respectively (Figure 4a). At large Mn content (xx=0.67), the Zn-Te oscillator strength shares nearly equally between both native mTO submodes. In this case the PP−PP^{-} and PPint−PP^{int-} downshifts at θmin\theta_{min} are comparable (Figure S3).

Three-panel percolation-type 3-oscillator Raman cross-sections

Figure 5. Percolation-type 3-oscillator {2×(Zn−Te),1×(Mn−Te)}\{2 \times(Zn - Te), 1 \times(Mn - Te)\} Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} RCS in their xx-dependence. (a) Mechanical-TO (mTO) RCS (b) Uncoupled-LO RCS. (c) Coupled-LO RCS. A small phonon damping (1 cm−11\ \mathrm{cm}^{-1}) is used throughout to distinguish small and/or neighboring features.

The Zn1−x_{1-x}Mnx_xTe PP-RCS at θmin=0∘\theta_{min}=0^\circ calculated for the 632.8 nm laser line by assuming a Zn-Te sensitivity to homo/hetero environments to second-neighbors (methods) fairly support the PP-uncoupling at x=0.37x=0.37 and x=0.67x=0.67 (Figure 4).

LO phonon regime

We cannot escape a brief discussion of the ELE_L-coupling. This generates massive LO distortions apparent in Figure 5 displaying tilted RCS views (three-dimensional, best suited to appreciate the Raman intensities in their xx-dependence) of the {mTOZn−TeZn,mTOZn−TeMn,mTOMn−Te}\{mTO^{Zn}_{Zn-Te},mTO^{Mn}_{Zn-Te},mTO_{Mn-Te}\} (a), uncoupled-{LOZn−TeMn,LOZn−TeZn,LOMn−Te}\{LO^{Mn}_{Zn-Te},LO^{Zn}_{Zn-Te},LO_{Mn-Te}\} (b) and coupled-{LO−,LOint,LO+}\{LO^-,LO^{int},LO^+\} (c) modes of zb-Zn1−x_{1-x}Mnx_xTe virtually expanded over 0≤x≤10\leq x\leq1. Frontal views (two-dimensional, more appropriate to compare the Raman frequencies in their xx-dependence) are provided in supplementary material (Figure S5, top). The same set of input parameters, notably a small phonon damping (1 cm−1^{-1}) to distinguish neighboring modes, is used throughout. The same notation with a subscript (vibrating bond) and a superscript (homo/hetero environment) is used to label the native naturally-uncoupled mTO modes and their artificially-uncoupled LO-descendants.

Theoretical LO-coupling in zb-Zn$_{1-x}$Mn$_x$Te

Figure S5. Theoretical LO-coupling in zb-Zn1−x_{1-x}Mnx_xTe (0≤x≤10 \le x \le1) – Percolation vs. MREI approaches. Top. Three-mode percolation model / frontal-2D views (the corresponding tilted-3D views are displayed in Figure 5). (a) Mechanical-TO (mTO) RCS. (b) Uncoupled-LO RCS. (c) Coupled-LO RCS. Bottom. Two-mode MREI model. The percolation mTO Zn-Te duo is grasped into a unique MREI oscillator carrying the whole available Zn-Te oscillator strength – dotted/red line in panel (a). (d) Amount of coupling/mixing τ\tau. (e) Uncoupled-LO RCS. (f) Coupled-LO RCS. A small phonon damping (1 cm−11\ \mathrm{cm}^{-1}) is used throughout to distinguish small and/or neighboring features.

Dramatic ELE_L-mediated LOZn−TeZn→LOMn−TeMnLO_{Zn-Te}^{Zn}\rightarrow LO_{Mn-Te}^{Mn} inter-bond (x∼0x\sim0) and intra-bond/duo (Zn-Te) LOZn−TeZn→LOZn−TeMnLO_{Zn-Te}^{Zn}\rightarrow LO_{Zn-Te}^{Mn} (x∼0.5x\sim0.5) transfers of oscillator strength (intensity aspect) manifested by strong repulsions (frequency aspect) occur at the resonances corresponding to frequency matching of the related uncoupled-LO modes, as specified in brackets. The net effect of the ELE_L-coupling is to create a giant LO+LO^+ mode with quasi stable intensity and frequency in the Mn-Te spectral range above a minor LOintLO^{int} mode that collapses downward the Zn-Te spectral range by increasing xx. The remaining LO−LO^- oscillator, quasi deprived of oscillator strength, hence not visible experimentally, repelled close to the lower mTOZn−TeZnmTO_{Zn-Te}^{Zn} mode, plays a minor role.

So, in first approximation a MREI model of two {LOZn−Te,LOMn−Te}\{LO_{Zn-Te},LO_{Mn-Te}\} ELE_L-coupled harmonic oscillators (Figure S5, bottom) suffices to describe the inter-bond LO coupling, as proposed for zb-Cd1−x_{1-x}Znx_xTe and zb-Ga1−x_{1-x}Inx_xAs29{^{29}} [29]. This comes to merge the mTOMn−TemTO_{Mn-Te}–mTOZn−TeZnmTO_{Zn-Te}^{Zn} percolation mTO-duo into a mTOZn−TemTO_{Zn-Te} MREI-singlet with oscillator fraction fZn−Te(x)=1−xf_{Zn-Te}(x)=1-x. Comparative insights into the MREI (2-mode, black/right-oriented) and percolation (3-mode, red/left-oriented) mTO (thick curves) and LO (thin curves) RCS at the experimentally studied xx values are shown in Figure 1. By diagonalizing the dynamical matrix and expressing the unit perpendicular eigenvectors from ∣LO+⟩=(cos⁡δ,sin⁡δ)|LO^+\rangle=(\cos\delta,\sin\delta), cos⁡2δ\cos^2\delta and sin⁡2δ\sin^2\delta estimate how much in percent the Zn-Te and Mn-Te bonds are involved in the upper (LO+LO^+) coupled mode depending on xx, and vice versa for the lower (LO−LO^-) one. τ=tan⁡θ\tau=\tan\theta is a direct marker of bond-mixing. Not surprisingly, the LO modes are (quasi) decoupled (bond-specific, τ→0\tau\rightarrow0) at x→1x\rightarrow1, i.e., away from the resonance, and strongly coupled (bond-mixed, τ→τmax\tau\rightarrow\tau_{max}) at x→0x\rightarrow0, i.e., near the resonance (Figure S5). Remarkably, zb-Zn1−x_{1-x}Mnx_xTe achieves a higher bond-mixing (τmax∼0.5\tau_{max}\sim0.5 at x∼0.10x\sim0.10) than zb-Cd1−x_{1-x}Znx_xTe and zb-Ga1−x_{1-x}Inx_xAs (τmax∼0.4\tau_{max}\sim0.4 at x∼0.05x\sim0.05)[29].

Conclusion and perspectives

Cubic-Zn1−x_{1-x}Mnx_xTe (x≤0.7x\leq0.7) offers a benchmark to test the sensitivity of the TO-percolation model[6] to minimum lattice/bond distortions induced by alloying. A Zn-Te TO-duo marking a difference in lattice relaxation around Zn-Te depending on its local homo/hetero environment, in the spirit of the percolation model, is evidenced in the mTO regime. However, the mTO-duo is so compact and the mTO regime so dispersionless across the BZ that the duo can hardly be resolved ab initio or experimentally, whether probing finite-small qq in backward-RS or maximum qq by INS. The situation clarifies on entry to the highly-dispersive PP regime at q→0q\rightarrow0, probed by forward-RS. The Zn-Te duo splits off, supporting an effective MREI27{^{27}}-{1 ×\times (Zn−Te)(Zn-Te), 1 ×\times (Mn−Te)(Mn-Te)} →\rightarrow percolation6{^{6}}-{2 ×\times (Zn−Te)(Zn-Te), 1 ×\times (Mn−Te)(Mn-Te)} shift of paradigm for the optical modes of zb-Zn1−x_{1-x}Mnx_xTe. Odd attributes (linewidth, frequency, intensity) of the individual PP modes depending on qq are discussed in terms of the microscopic↔macroscopic transition affecting their accompanying transverse (photon-like) electric field on crossing the photon resonance.

Along with disordered (high-entropy) semiconductor alloys (SCAs), the high-entropy (metallic) alloys (HEAs) are exemplary systems to study how the lattice dynamics is impacted by disorder. Their lattice dynamics, governed by the bond force constants, i.e., a local (microscopic) mechanical property, attracts a special interest due to HEAs’ outstanding (macroscopic) mechanical properties[42]. The acoustic modes of HEAs were extensively studied over the past few years[43, 44, 45]. However, the optical modes, despite their unique ability to probe the local alloy disorder (percolation scheme), did not. Either because the optical modes are just absent[43, 44, 45], or, on the contrary, because they present a too complex or confusing pattern[46] (depending on the number of atoms per primitive cell). Anyway, an insight into the capacities of the percolation scheme set from SCAs in relation to HEAs might be intriguing.

Methods

Samples

Zn1−x_{1-x}Mnx_xTe single crystals at well-separated compositions xx (x=0x=0, 0.12, 0.37, 0.51, 0.67) are grown from the melt by mixing high-purity ZnTe (5N quality) with Mn (2N quality) using the Bridgman method. The zb-structure is attested throughout by powder X-ray diffraction either done at ambient pressure in laboratory conditions using the 1.541 Å Cu Kα\alpha line and/or at nearly ambient pressure at the PSICHÉ beamline of synchrotron SOLEIL using the 0.3738 Å radiation (Figure S1). The lattice parameter aa depends linearly on xx (Figure S1) measured (with accuracy better than 1 at.%) by inductively coupled plasma-optical emission spectroscopy[47], as expected in case of a regular Zn↔Mn substitution on the cationic site[48].

Ab initio calculations

An ab initio insight into the capacity of the optical modes due to the Zn-Te bonds of zb-Zn1−x_{1-x}Mnx_xTe to distinguish homo from hetero environments in the spirit of the percolation model, is achieved by applying the SIESTA code[31] to a large 2×2×22 \times2 \times2 (64-atom) ZnTe-like zb-supercell containing an isolated Mn-impurity (x∼0x \sim0, Figure 2). The finite-displacements force constants calculation is done after full relaxation (lattice constant and atom positions). As no disposition was applied to long-range electric fields, the reported ab initio data are thus of the pure-mTO type, more precisely concerned with the mTO phonon density of states projected at Γ (Γ-projected mTO-PhDOS), that assimilates with the pure-mTO Raman signal in first approximation.

Inelastic neutron scattering (INS)

The mTO regime of zb-Zn0.33_{0.33}Mn0.67_{0.67}Te is studied by INS at the thermal-neutron triple-axis IN22 of Institut Laüe Langevin at room temperature along the [001ˉ\bar{1}] direction of the reciprocal space using a large crystal (∼\sim75 mm3^3) with homogeneous composition (the Raman shifts across the sample surface are less than 1 cm−1^{-1}) aligned in the ([001ˉ\bar{1}], [110]) horizontal scattering plane. IN22 was set up in a W configuration and inelastic scans were performed with constant kf=2.662k_f=2.662 Å−1^{-1}, where kfk_f is the wavevector of the scattered neutron beam. A pyrolytic graphite (PG(002)) monochromator and analyzer were used. Higher-order contamination was removed using a PG filter in the scattered neutron beam.

The mTO signal is specifically probed at ∼\sim10% of the BZsize, near the intense Bragg peak (331), i.e., at (330.9), and exactly at the BZB, i.e., (330). The neutron data (Figure 2e, symbols with error bars corresponding to the square root of counts) were fitted with two (330.9) and three (330) Gaussian functions (after subtraction of oblique baselines), to appreciate the relative weights of the individual mTO-phonon modes. The linewidth per Gaussian function at a given transferred energy to the crystal (Ei−EfE_i-E_f) at least matches the spectral resolution δ\delta at the magnitude kik_i of the corresponding wavevector of the incident neutron beam. For IN22, δ\delta changes quasi linearly (with a slight negative bowing) from 1 meV to ∼\sim2 meV for (Ei−EfE_i-E_f) varying from 0 to 30 meV.

A meticulous in-plane (horizontal) scan at the (331) Bragg diffraction operated by (vertical) rotation of the crystal reveals a spurious Bragg diffraction due to a second minor crystal tilted by ∼\sim7° from the main one. Moreover, it is common that large Zn1−x_{1-x}Mnx_xTe crystals grown by the Bridgman method are subject to twinning1, due to stacking faults in the …ABCABC… sequence of hexagonal cation and anion close-packed planes along [111]. Hence, probing the main crystal at a selected (hklhkl) point of the (horizontal) scattering plane alternatively probes simultaneously (h′k′l′h'k'l') points of the secondary and/or twinned crystals, rendering the phonon assignment a difficult task. Even if an obstacle for a reliable study of the acoustic modes, this is not so critical for the currently studied mTO modes that are nearly dispersionless.

Raman scattering (RS)

Backward/forward-RS is done at ambient conditions using the 632.8 nm laser excitation at near-normal incidence/detection onto/through tiny (few mm3^{3}) (110)-oriented crystal faces obtained by cleavage, corresponding to a pure-TO (TO allowed, LO forbidden) symmetry[49]. Generally, crossed polarizations of the incident laser (e⃗i\vec{e}_i) and of the scattered light (e⃗s\vec{e}_s) are used, to reduce the second-order signal obscuring the first-order TO (mTO, PP) one (Figure S2). The TO symmetry is analyzed by rotating in pair the crossed (or parallel) polarizations at a given sample spot until completing a full revolution (360°) of the azimuth polarization angle (α\alpha, step-increased by 20°) between e⃗i\vec{e}_i and the [1ˉ10\bar{1}10] crystal axis taken as an arbitrary reference. The nominal TO (mTO or PP) Raman intensity (area of peak – modeled using a Lorentzian/Gaussian function – normalized to the area of the most intense peak of the series) vs. α\alpha variation describe Greekcross- and butterfly-like motifs for crossed (⊥\perp) and parallel (∥\parallel) polarizations, respectively. The laser stability is checked by repeating the initial measurement at the end of the run.

The backward-RS and forward-RS geometries probe specific variants of the TO modes[11]. Due to the ionicity of the chemical bonding in a zb-SCA, its TO modes are likely to carry a transverse electric field E⃗T\vec{E}_T. However, the latter can propagate only if qq for the TO mode (nearly) matches that for a photon, the pure transverse electric field, corresponding to λ\lambda covering as much as 10410^{4} crystal unit cells. Such small qq is achievable by forward-RS, minimizing the q⃗\vec{q}-transfer to the crystal. The probed TO mode in forward-RS is thus a phonon-photon coupled mode with mixed “electrical + mechanical” character, called a phonon-polariton (PP).

A single-oscillator pristine zb-crystal exhibits two PP−PP^{-} and PP+PP^{+} branches in repulsion with phonon and photon asymptotes. The latter describe the dispersion of light/photon in vacuum weighted by the static and high-frequency dielectric constants of the crystals on both sides on the phonon resonance[11], labelled Ph+Ph^{+} and Ph−Ph^{-} (Figure 3), respectively. Alloying introduces multiple intermediary PPintPP^{int} branches (dividing from PPint−PP^{int-} to PPint+PP^{int+} from low to high frequency in case of multiple oscillators) with a characteristic S-like dispersion governed by two phonon asymptotes, mTO-like away from Γ\Gamma and LO-like near Γ\Gamma. Generally, the PP modes suffer a Raman extinction on crossing (PPintPP^{int}) or converging (PP−PP^{-} and PP+PP^{+}) onto the photon-like asymptotes. This conforms to intuition that only matter-like excitations scatter light efficiently, whereas the photon-like ones do not.

Backward-RS achieves a maximum qq-transfer to the crystal, i.e., q∼2×kiq \sim2 \times k_i, falling far away from the q(ω)q(\omega) dispersion of a photon in the far-IR spectral range of a phonon. At this limit E⃗T\vec{E}_T cannot propagate. Hence, a TO mode probed in backward-RS reduces to a purely-mechanical phonon (mTO), deprived of electric field. It emerges that E⃗T\vec{E}_T is qq-dependent. In contrast, the electric field E⃗L\vec{E}_L of a LO mode, being longitudinal, does not suffer any photon-like restriction. A LO mode thus keeps a uniform/permanent “electrical + mechanical” character at any qq. Strictly at Γ\Gamma, E⃗T=E⃗L\vec{E}_T = \vec{E}_L because at q=0q = 0 there is no means to distinguish vibrations polarized perpendicularly to q⃗\vec{q} (transverse) from vibrations polarized along q⃗\vec{q} (longitudinal).

The same generic multi-oscillator (SCA-like) RCS, given by Eq. (1) of Ref. 29, derived within the linear dielectric formalism of Hon and Faust[50], is used to model the PP in their qq-dependence (q→0,λ∼104×aq \to0,\lambda\sim10^{4} \times a) as well as their native mTO modes (q→∞,λ∼102×aq \to\infty,\lambda\sim10^{2} \times a) away from Γ\Gamma (being clear that RS operates near Γ\Gamma – main text) and their coupled- and uncoupled-LO modes near Γ\Gamma (q→0,λ→∞q \to0,\lambda\to\infty). The individual RCS due to a given uncoupled-LO/PP mode is obtained by removing all alternative oscillators from the LO/PP-RCS of zb-Zn1−x_{1-x}Mnx_xTe. As for the regular multi-mode LO/PP-RCS, it naturally provides the coupled-LO/PP RCS.

Most input parameters of the RCS relate to the parent zb-ZnTe and zb-MnTe compounds. Together with ε∞\varepsilon_{\infty}, the mTO (ωTO\omega_{TO}) and LO (ωLO\omega_{LO}) Raman frequencies define the parent oscillator strengths S=ε∞×ωTO−2×(ωLO2−ωTO2)5S = \varepsilon_{\infty} \times\omega_{TO}^{-2} \times(\omega_{LO}^{2} - \omega_{TO}^{2})^{5}. The used (ε∞\varepsilon_{\infty}, ωTO\omega_{TO}, ωLO\omega_{LO}, CFHC_{FH}) values for zb-ZnTe and zb-MnTe are (7.3 – Ref. 24, 177.5 cm−1^{-1} – Ref. 24, 207.0 cm−1^{-1} – Ref. 24, -0.11 – Ref. 29) and (7.0 – Ref. 24, 188.0 cm−1^{-1}, 214.5 cm−1^{-1}, −6.65×10−3-6.65 \times10^{-3}), respectively, where CFHC_{\mathrm{FH}} denotes the Faust-Henry coefficient. The last three values were adjusted in this work so as to best fit the experimental data. CFHC_{\mathrm{FH}} for MnTe, not available in the literature, was adjusted so as to fairly replicate the experimental intensity ratio between the well-resolved Zn-Te and Mn-Te mTO backward-RS signals showing up with comparable intensities at x=0.67x=0.67 (not shown).

The only alloy-related input parameters are ωT,p(x)\omega_{\mathrm{T},p}(x) (apparent in Figure 5a, the MREI description in the Zn-Te spectral range is linearly interpolated between the parent and impurity values – dotted curve) and γp(x)\gamma_p(x) of the mTOs directly observed in backward-RS experiments. Besides, Sp(x)S_p(x) and Cp(x)C_p(x) scale linearly with the fraction fp(x)f_p(x) of oscillator-pp in the crystal^{51}. In the percolation-type three-oscillator {2×(Zn−Te),1×(Mn−Te)}\{2 \times(\mathrm{Zn}-\mathrm{Te}), 1 \times(\mathrm{Mn}-\mathrm{Te})\} description of zb-Zn1−x_{1-x}Mnx_xTe, the Zn-Te duo distinguishes purely-hetero Mn-Te environments at high-frequency from homo- and homo/hetero-mixed environments regrouped at low-frequency, as defined at the second-neighbor scale. The corresponding fp(x)f_p(x) are (1−x)3+2×x×(1−x)2(1-x)^3 + 2 \times x \times(1-x)^2 and x2×(1−x)x^2 \times(1-x), respectively^{29}. For a MREI-like oscillator, that is blind to the local environment, fp(x)f_p(x) matches the corresponding bond fraction^{29}, i.e., xx (Mn-Te) or 1−x1-x (Zn-Te).

The Zn1−x_{1-x}Mnx_xTe relative dielectric function εr(ω,x)\varepsilon_r(\omega,x), governing the resonance term Δ(ω,q,x)=εr(ω,x)−q2c2ω−2\Delta(\omega,q,x) = \varepsilon_r(\omega,x) - q^2 c^2 \omega^{-2} of the RCS, plays a central role. A classical εr(ω,x)\varepsilon_r(\omega,x) form is used comprising a linearly xx-dependent electronic background ε∞(x)\varepsilon_\infty(x) besides Lorentzian Lp(ω,x)L_p(\omega,x) phonon mode contributions, i.e., pp in total, depending on the used MREI- (p=2p=2) or percolation-type (p=3p=3) descriptions. Each pp mode is characterized by its mTO frequency, noted ωT,p(x)\omega_{\mathrm{T},p}(x), its (sample-dependent) damping γp(x)\gamma_p(x) fixing the full width at half maximum of the Raman signal, and its oscillator strength Sp(x)S_p(x) controlling both the magnitude of the pp-related mTO – LO band and its absolute mTO Raman intensity. The RCS also involves the pp-related Faust-Henry coefficients, noted Cp(x)C_p(x), measuring the relative Raman scattering efficiencies of the non-polar (mTO) and polar (LO, PP) pp-type modes. The Cp(x)C_p(x) terms act as supplementary weighting factors on the individual pp-related Raman intensities.

The Raman spectra are recorded at a quasi-fixed scattering angle θ=(k⃗i,k⃗^s)\theta= (\vec{k}_i,\widehat{\vec{k}}_s) between the adjustable-incident and fixed-scattered wavevectors inside the crystal. The qq-dependence of the RCS is transformed into a proper θ\theta-dependence, more appropriate for comparison with experiment, via the scalar form of the wavevector conservation q⃗=k⃗i−k⃗s\vec{q} = \vec{k}_i - \vec{k}_s, that governs the q⃗\vec{q}-transfer to the crystal. The subscripts refer to the incident and scattered lights. The accurate θ\theta value per forward-RS spectrum was derived from the criteria that the experimentally probed q(ω)q(\omega) dispersion (referred to as the Raman scan line in Figure 3), would cross the zb-Zn1−x_{1-x}Mnx_xTe branches q(ω)q(\omega) PP dispersions exactly at the experimentally observed PP frequencies. In practice, the mTO modes are visible on top of the PP modes in the forward-RS spectra. This is because the incident laser generates a (spurious) backward-RS (mTO-like) signal after reflection at the top crystal face besides the (regular) forward-RS (PP-like) signal generated by the laser beam on its way forth to the top crystal face.

Despite the small transfer of (far-infrared) energy to the crystal by Raman scattering (operated in the visible), i.e., merely of the order of one percent, meaning that ki−ksk_i-k_s, qmin⁡=∣ki−ks∣=c−1×∣n(ωi)ωi−n(ωs)ωs∣q_{\min} = \lvert k_i-k_s \rvert= c^{-1} \times\lvert n(\omega_i)\omega_i - n(\omega_s)\omega_s \rvert achieved in perfect forward-RS for θ=0∘\theta=0^\circ can never be zero in a cubic crystal (at ωi≠ωs\omega_i \ne\omega_s). This is because the refractive index of cubic semiconductors reduces with energy below the optical band gap^{2} where the (“transmission-like”) forward-RS is done. So, the difference in energy between the incident and scattered lights is emphasized by the corresponding difference in refractive indices of the crystal, whether using the Stokes (ωi>ωs\omega_i > \omega_s) or anti-Stokes (ωi<ωs\omega_i < \omega_s) scattering geometries. The current n(ω)n(\omega) dispersions are derived from the reported data in the literature, measured by spectroscopic ellipsometry with zb-Zn1−x_{1-x}Mnx_xTe epitaxial layers^{15}. Direct ellipsometry measurements on our single crystals are prevented by possible crystal inhomogeneity and twins at the surface scale of few mm2^2 probed by ellipsometry, evidenced in the large crystals studied by INS.

Data availability

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Acknowledgements

We acknowledge assistance from the IN22 beamline staff of Institut Laüe Langevin (ILL, Proposal CRG-3343, A.E., N.B., F.B., P.B., M.M. & O.P. (2026). Effect of size versus mass disorder on phonon behavior in disordered Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} and Mg1−xMnxTe\mathrm{Mg}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} semiconductor alloys), from the PSICHÉ beamline staff of synchrotron SOLEIL (Proposal 20210410 – BAG for PSICHÉ beamline led by Y.L.G., sub-project HP-ZnMnTe, A.P., M.M. & O.P.), from the IJL core facility (Université de Lorraine – http://ijl.univ-lorraine.fr/recherche/centres-de-competences/rayons-x-et-spectroscopie-moessbauer-x-gamma) for the X-ray diffraction measurements at ambient pressure, from the Ellipsometry platform of LCP-A2MC – https://lcp-a2mc.univ-lorraine.fr/plateformes/ellipsometrie), and from Mathieu Hebmann for technical assistance in Raman scattering. Calculations have been done using the facilities of the EXPLOR HPC Center of the Université de Lorraine (project 2019CPMXX0918). This work was funded by the French PIA project Lorraine Université d’Excellence (LUE), part of the France 2030 Program, reference ANR-15-IDEX-04-LUE, within the ViSA – IRP «Vibrations of Semiconductor Alloys – International Research Partnership» wall-less associated international laboratory (2024 – 2028), co-funded by the Excellence Initiative – Research University program at Nicolaus Copernicus University in Toruń (Poland). We further acknowledge financial support from the 2FDN – Fédération Française de la Diffusion Neutronique.

Author contributions

High-quality Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} mixed crystals with zincblende structure were grown using the Bridgman method by T.N. & K.S. Powder X-ray diffraction measurements at ambient pressure were done in laboratory conditions by S.D., completed by high-pressure ones at the PSICHÉ beamline of synchrotron SOLEIL by M.M., A.P. & O.P. with the assistance of Y.L.G., N.G. & J.P.I. The high-pressure data were subsequently analyzed by M.M. The alloy composition xx was determined by S.M. applying the inductively coupled plasma-optical emission spectroscopy method to powders. Prospective ellipsometry measurements in the visible on selected crystal pieces were recorded by A.E & L.B. on crystal faces polished to optical quality by P.F. & A.M. Ab initio mTO-phonon calculations at x→0x \to0, useful to guide experiments, were done by A.V.P. using the SIESTA code. Inelastic neutron scattering measurements on large crystal pieces were done at the IN22 beamline of Institut Laue Langevin by A.E., M.M. & O.P. with the assistance of P.B., F.B. & N.B. Backward/forward Raman spectra onto/through tiny single crystals were recorded by M.M., T.N., S.T., T.T. & O.P. with the technical assistance of P.F. Analytical calculations of the (phonon-polariton, mTO, LO) Raman cross section (RCS) within the linear dielectric formalism done by O.P. & M.M. were implemented by M.M. using the MATLAB programming language. M.M. made the figures. O.P. wrote the manuscript, with contributions from all co-authors.

Competing interests

The authors declare no competing interests.

Additional information

Supplementary information The online version contains supplementary material concerning additional experimental and theoretical data further supporting the discussion of the lattice structure (X-ray diffraction) and lattice dynamics (Raman scattering) of zb-Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te}, available at https://...

Correspondence and requests for materials should be addressed to Olivier Pagès.

Affiliations

Université de Lorraine, LCP-A2MC, F-57000 Metz, France

M. Mina, T. Ngulezhu, S. Thiam, A. V. Postnikov, T. Tite, A. En Naciri, L. Broch, P. Franchetti & O. Pagès

Laboratoire Léon Brillouin, CEA-CNRS, Saclay, France

A. Elmahjoubi & P. Bourges

Institute of Physics, Faculty of Physics, Astronomy and Informatics, Nicolaus Copernicus University in Toruń, ul. Grudziądzka 5, 87-100 Toruń, Poland

T. Ngulezhu & K. Strzałkowski

Université Grenoble Alpes, CEA, IRIG, MEM, MDN, F-38000 Grenoble, France

F. Bourdarot & N. Biniskos

Institut de Minéralogie, de Physique des Matériaux et de Cosmochimie, Sorbonne Université — UMR CNRS 7590, F-75005 Paris, France

A. Polian & Y. Le Godec

Synchrotron SOLEIL, L’Orme des Merisiers Saint-Aubin, BP 48 F-91192 Gif-sur-Yvette Cedex, France

Y. Le Godec, N. Guignot & J.-P. Itié

Université de Lorraine, CNRS, IJL, F-57000, Metz, France

S. Diliberto & S. Michel

Université de Lorraine, CentraleSupélec, LMOPS, F-57000 Metz, France

A. Maillard

Funding

ViSA-IRP project referenced ANR-15-IDEX-04-LUE within the French PIA project «Lorraine Université d’Excellence», part of the France 2030 Program.

Synchrotron SOLEIL (Proposal 20210410) within BAG for PSICHÉ beamline (led by Y.L.G.).

2FDN – Fédération Française de la Diffusion Neutronique within Proposal CRG-3343 (led by A.E.) on the IN22 beamline of Institut Laüe Langevin.

Mesocenter of calculation EXPLOR at the University of Lorraine within Project project 2019CPMXX0918 (led by A.V.P.).

Supplementary information (prefixed S) reports on additional experimental and theoretical data further supporting the discussion of the lattice structure (Sec. SI) and dynamics (Sec. SII) of Zn1−x_{1-x}Mnx_xTe taken in the zb-phase, in relation to X-ray diffraction (XRD) and Raman scattering (RS), respectively. In the latter case both experimental and theoretical data are reported, concerned with backward/mTO-like and forward/PP-like Raman signals, and with the intra-bond LO-coupling within the Zn-Te dual optical mode of zb-Zn1−x_{1-x}Mnx_xTe, respectively.

Zn1−x_{1-x}Mnx_xTe lattice structure

Raw Zn1−x_{1-x}Mnx_xTe XRDiffractograms obtained at minor (x=0.12x=0.12) and large (x=0.37x=0.37) alloying at the PSICHÉ beamline of SOLEIL synchrotron using the 0.3738 Å radiation at nearly ambient pressure by inserting finely ground powders inside a diamond anvil cell is displayed in Figure S1. Au and Ne are used for pressure calibration and as the pressure transmitting medium, respectively. An additional powder XRDiffractogram related to large Mn content (x=0.67x=0.67) was separately measured at ambient pressure in laboratory conditions using the 1.541 Å Cu Kα\alpha line (not shown). Sharp diffraction peaks, attesting a high crystal quality, indicate that all studied samples crystallize in the same zincblende (zb) structure as ZnTe. The individual XRDiffractiction peaks in Figure S1 are labelled accordingly via their (hkl) Miller’s indices.

Zn1−x_{1-x}Mnx_xTe lattice dynamics

  1. Backward-RS

Figure S2 displays the full series of cross-polarized backward-RS spectra taken at the same sample spot with the 632.8 nm laser line across the zb-phase of Zn1−x_{1-x}Mnx_xTe (x≤0.7x \leq0.7) depending on the azimuth angle α\alpha between the incident polarization (e⃗i\vec{e}_i) and the [110] crystal axis taken as an arbitrary reference, step-increased by 20° until completing a full revolution (over 360°) at the sample surface. The reported symmetry analysis at x=0.37x=0.37 in the inset of Figure 2 refers to the α\alpha-dependence of the normalized (to the largest signal) Raman intensity (area) of the main ZnTe-like peak (modeled as a Lorentzian/Gaussian function) in crossed (⊥\perp, filled symbols) and parallel (∥\parallel, hollow symbols) polarizations of the incident (e⃗i\vec{e}_i) and scattered (e⃗s\vec{e}_s) lights. The Zn-Te and Mn-Te Raman intensities exhibit the same α\alpha-dependence corresponding to the theoretical quatrefoil Greekcross-like (⊥\perp) and bilobed butterfly-like (∥\parallel) motifs axed [11ˉ0][1\bar{1}0] and [001][001], as ideally expected. Similar motifs are observed at x=0.12x=0.12 (Figure S2) and x=0.67x=0.67 (Figure S2). So, the lower/main Zn-Te and upper/minor Mn-Te Raman peaks consist of genuine mTO modes. The raw cross-top/parallel-bottom polarized Raman spectra collected at all studied xx values (0.12, 0.37, 0.67) are displayed in Figure S2. In each panel, the extreme (top and bottom) curves, referring to the same α\alpha addressed at the start and at the end of the revolution, help to appreciate the stability of the laser source across the full α\alpha-revolution.

Forward-RS

Figure S3 displays a selection of cross-polarized forward-RS spectra obtained at various scattering angles θ\theta with zb-Zn0.33_{0.33}Mn0.67_{0.67}Te using the 632.8 nm laser line at quasi normal incidence/detection across parallel (110)-oriented crystals faces obtained by cleavage. The specified θ\theta per spectrum are estimated so that the corresponding θ\theta-dependent Raman scan line crosses the qq-dependent zb-Zn0.33_{0.33}Mn0.67_{0.67}Te PP-RCS (comparable to that reported for x=0.37x=0.37 in Figure 3) exactly at the experimentally observed PP−PP^- (small θ\theta) or PPint+PP^{int+} (large θ\theta) frequencies. By decreasing θ\theta, the PPs progressively soften from their native Zn-Te and Mg-Te mTO modes. The PP−PP^- mode hardly departs from its native mTOZn−TeZnmTO^{Zn}_{Zn-Te} mode as long as θ≥0.95∘\theta\ge0.95^\circ (Figure S3) and then suddenly emerges as a distinct feature downshifted (frequency aspect) far below (by as much as ∼\sim50 cm−1^{-1}) the mTOZn−TeZnmTO^{Zn}_{Zn-Te} mode at θ≤0.85∘\theta\le0.85^\circ (Figure S3). No intermediate stage is observed. This is consistent with PP−PP^- suffering a massive Raman extinction (intensity aspect) when it gets massively photon-like on crossing the photon asymptotes, which precisely occurs at the critical θ\theta value θc∼0.90∘\theta_c \sim0.90^\circ (Figure 3). Remarkably, θc\theta_c is also critical with respect to the PPint+PP^{int+} mode, subject to a broad↔\leftrightarrowsharp transition (linewidth aspect) at this limit (Figure S3). This cannot be merely fortuitous, proving on an experimental basis that the latter transition can be traced back to the crossing of the photon-like asymptotes. The θc\theta_c-coincidence affecting the PP−PP^- and PPint+PP^{int+} modes is presumably intrinsic to zb-Zn1−x_{1-x}Mnx_xTe alloying since it is independently observed with zb-Zn0.63_{0.63}Mn0.37_{0.37}Te (Figure 4).

Figure S4 shows the raw forward-RS cross-polarized spectra at minimum scattering angle (θ∼0∘\theta\sim0^\circ) behind the reported PP−PP^- symmetry analysis at x=0.37x=0.37 (Figure 4, inset) and x=0.67x=0.67 (Figure S3, inset) using the 632.8 nm laser line. Similar spectra for x=0.12x=0.12 complete the series. At a given xx, the forward-RS PP-symmetry analysis is done at the same sample spot as the backward-RS mTO-symmetry analysis in Figure S2. The specified α\alpha values do correspond. The PP−PP^- Raman intensity α\alpha-dependence exhibits the same Greekcross-like motif (inset of Figure 4, filled symbols) as that of the native mTOZn−TeZnmTO^{Zn}_{Zn-Te} mode (inset of Figure 2, filled symbols) attesting that they both consist of genuine TO modes. More generally, all three PP−PP^-, PPint−PP^{int-} and PPint+PP^{int+} follow the same Raman selection rules depending on α\alpha (as apparent at any xx in Figure S4) attesting their identical (PP) nature.

Inter-bond LO-coupling – simplified two-oscillator MREI-like description

In the main text the inter-bond LO-coupling in Zn1−x_{1-x}Mnx_xTe with zb-phase artificially expanded across the entire composition domain is treated in full by using the nominal three-oscillator percolation-type approach, referring to the native {mTOZn−TeZn,mTOZn−TeMn,mTOMn−Te}\{mTO^{Zn}_{Zn-Te},mTO^{Mn}_{Zn-Te},mTO_{Mn-Te}\} modes behind the LO modes. The corresponding oscillator fractions fp(x)f_p(x) are listed in methods. A simplified MREI-like two-oscillator {mTOZn−Te,mTOMn−Te}\{mTO_{Zn-Te},mTO_{Mn-Te}\} description is achieved by merging the percolation-type mTOMn−TemTO_{Mn-Te}–mTOZn−TeZnmTO^{Zn}_{Zn-Te} duo into a unique MREI-like mTOZn−TemTO_{Zn-Te} oscillator with fraction fZn−Te(x)=1−xf_{Zn-Te}(x)=1-x. The remaining Mn-Te oscillator, already of the MREI-type, is represented in the crystal with fraction fMn−Te(x)=xf_{Mn-Te}(x)=x. The corresponding two-mode uncoupled-{LOZn−Te,LOMn−Te}\{LO_{Zn-Te},LO_{Mn-Te}\} and coupled-{LO−,LO+}\{LO^-,LO^+\} RCS are displayed in Figure S5, using a minimum phonon damping (1 cm−1^{-1}). The ELE_L-coupling is manifested by a strong LO repulsion at the resonance (x∼0x\sim0) due to a massive LOZn−Te→LOMn−TeLO_{Zn-Te}\to LO_{Mn-Te} transfer of oscillator strength, reflected in the LO−LO^- (minor) and LO+LO^+ (dominant) Raman intensities (Fig. S5-top, thickness of curves), in line with observed trends within the three-oscillator scheme (Figure 5). The simplified two-oscillator scheme is, notably useful to compare on equal footing zbzb-Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} with zbzb-Cd1−xZnxTe\mathrm{Cd}_{1-x}\mathrm{Zn}_{x}\mathrm{Te} and zbzb-Ga1−xInxAs\mathrm{Ga}_{1-x}\mathrm{In}_{x}\mathrm{As}, earlier treated in the same (MREI-like) way[29]. The comparison involves the dimensionless parameter τ\tau (Figure S5), introduced in the main text, representing the amount of Zn-Te/Mn-Te mixing per coupled-LO mode depending on xx. The full treatment, outlined in the main text offering the access to τ\tau, is detailed in Ref. 29, referring specifically to Eqs. 3-to-5 therein. Remarkably, near the resonance (x∼0x \sim0), a higher mixing is achieved for zbzb-Zn1−xMnxTe\mathrm{Zn}_{1-x}\mathrm{Mn}_{x}\mathrm{Te} (τmax⁡∼0.5\tau_{\max} \sim0.5 at x∼0.10x \sim0.10) than for Cd1−xZnxTe\mathrm{Cd}_{1-x}\mathrm{Zn}_{x}\mathrm{Te} and zbzb-Ga1−xInxAs\mathrm{Ga}_{1-x}\mathrm{In}_{x}\mathrm{As} (τmax⁡∼0.4\tau_{\max} \sim0.4 at x∼0.05x \sim0.05) – Ref. 29 (Fig. 7d therein).

References

  1. [1]Giebultowicz, T.M. et al. Harmonic magnons in Cd₁₋ₓMnₓTe and Zn₁₋ₓMnₓTe. Phys. Rev. B 39, 6857–6870 (1989).pubmed.ncbi.nlm.nih.gov/9947333
  2. [2]Adachi, S. Properties of Semiconductor Alloys : Group-IV, III-V and II-VI. Ed. John Wiley & Sons (2009).
  3. [3]Jusserand, B. & Sapriel, J. Raman investigation of anharmonicity and disorder-induced effects in Ga₁₋ₓAlₓAs epitaxial layers. Phys. Rev. B 24, 7194–7205 (1981).DOI
  4. [4]Turner, S.R. et al. Phonon behavior in a random solid solution: a lattice dynamics study on the high-entropy alloy FeCoCrMnNi. Nat. Commun. 13, 7509 (2022).
  5. [5]Chang I.F. & Mitra S.S. Long wavelength optical phonons in mixed crystals, Adv. Phys. 20, 359–404 (1971).DOI
  6. [6]Alhaddad, T. et al. Taxonomy of high-pressure vibration spectra of zincblende semiconductor alloys based on the percolation mode, Sci. Rep. 15,1212 (2025).DOI
  7. [7]Verleur, H.W. & Barker, A.S. Infrared lattice vibrations in GaAsᵧP₁₋ᵧ alloys. Phys. Rev. 149, 715–729 (1966).
  8. [8]Pagès, O., Souhabi, J., Postnikov, A.V. & Chafi, A. Percolation versus Cluster models for multimode vibration spectra of mixed crystals: GaAsP as a case study. Phys. Rev. B 80, 035204 (2009).DOI
  9. [9]Elmahjoubi, A., Alhaddad, T., Postnikov, A.V. & Pages, O. Comment on Infrared dielectric function of Ga(As,P) semiconductor alloys near the reststrahlen bands (Applied Physics Letters 123, 172102, 2023). Appl. Phys. Lett. 125, 086101 (2024).arxiv.org/abs/2401.04529
  10. [10]Born, M. & Huang, K. in Dynamical theory of crystal lattices, Oxford University Press (New York, 1954).
  11. [11]Claus, R., Merten, L. & Brandmüller, J. Light scattering by phonon-polaritons, ed. by G. Höhler (Springer-Verlag, Berlin, 1975).
  12. [12]Hippert, F., Geissler, E., Hodeau, J.L., Lelièvre-Berna, E. & Regnard, J.R. in Neutron and X-ray Spectroscopy, Ed. Springer (The Netherlands, Springer, 2006).
  13. [13]Pagès, O., Souhabi, J., Torres, V. J. B., Postnikov, A.V. & Rustagi, K. C. Re-examination of the SiGe Raman spectra – Percolation / one-dimensional-cluster scheme and ab initio calculations. Phys. Rev. B 86, 045201 (2012)
  14. [14]Elmahjoubi, A. et al. Hexagonal Zn₁₋ₓMgₓS sheds light on the Lattice dynamics of atomic alloys, Sci. Rep. 15, 34523 (2025).DOI
  15. [15]X. Liu, Bindley, U., Sasaki, Y. and Furdyna, J.K. Optical properties of epitaxial ZnMnTe and ZnMgTe films for a wide range of alloy compositions. J. Appl. Phys. 91, 2859–2865 (2002).DOI
  16. [16]C. Vérié, Beryllium substitution-mediated covalency engineering of II–VI alloys for lattice elastic rigidity reinforcement, J. Crystal Growth 184/185, 1061–1066 (1998).
  17. [17]N. E. Christensen, S. Satpathy, and Z. Pawlowska, Bonding and ionicity in semiconductors, Phys. Rev. B 36, 1032–1050 (1987).pubmed.ncbi.nlm.nih.gov/9942909
  18. [18]Perkowitz, S., kim, L. S. & Becla, P. Infrared ionicity in ternary II-VI alloys. Solid State Commun. 77, 471–474 (1991).DOI
  19. [19]Martin, R.M. Elastic properties of ZnS structure semiconductors. Phys. Rev. B 1, 4005–4011 (1970).DOI
  20. [20]Mimasaja, M., Sakamoto, I., Murata, K., Fujii, Y. & Onodera, A. Pressure-induced phase transitions of MnTe. J. Phys. C: Solid State Phys. 20, 4689–4694 (1987).
  21. [21]Schnohr, C.S. Compound semiconductor alloys: From atomc-scale structure to band gap bowing. Appl. Phys. Rev. 2, 031304 (2015).
  22. [22]Happ, N. Zn, Mn and Te K-edges EXAFS studies of the diluted magnetic semiconductor Zn₁₋ₓMnₓTe. J. Phys.: Condens. Matter 8, 4315–4323 (1996).
  23. [23]Olszewski, A., Wojdowski, W. & Nazarewicz, W. Infrared spectra of MnₓZn₁₋ₓTe mixed crystals. Phys. Stat. Sol. (b) 104, K155 (1981).DOI
  24. [24]Oles, B. & von Schnering, H. G. Raman and infrared studies of optical phonons in Zn₁₋ₓMnₓTe mixed crystals. J. Phys. C: Solid State Phys. 18, 6289–6296 (1985).DOI
  25. [25]Ya Valakh, M. & Litvinchuk, A.P. Observation of weak dipole vibration in single-mode MnₓZn₁₋ₓTe solid solutions. Sov. Phys. Solid State 25, 1597–1598 (1983).
  26. [26]Talwar, D. N. et al. Optical and structural characteristics of Bridgman grown cubic Zn₁₋ₓMnₓTe alloys. Materials Chemistry and Physics 220, 460–468 (2018).DOI
  27. [27]Peterson, D.L., Petrou, A., Giriat, W., Ramos, A.K. & Rodriguez, S. Raman scattering from the vibrational modes in Zn₁₋ₓMnₓTe. Phys. Rev. B 33, 1160–1165 (1986).pubmed.ncbi.nlm.nih.gov/9938381
  28. [28]Groenen, J. et al. Optical-phonon behavior of Ga₁₋ₓInₓAs: The role of microscopic strains and ionic plasmon coupling, Phys. Rev. B 58, 10452–10462 (1998).DOI
  29. [29]Alhaddad, T. et al. Raman study of Cd₁₋ₓZnₓTe phonons and phonon-polaritons – Experiment and ab initio calculations. J. Appl. Phys. 133, 065701 (2023).
  30. [30]Rao, M.N. et al. Lattice dynamics of the model percolation-type (Zn, Be)Se alloy: inelastic neutron scattering, ab initio study, and shell model calculations. Phys. Rev. B 89, 155201 (2014).DOI
  31. [31]García, A. et al. SIESTA : Recent developments and applications, J. Chem. Phys. 152, 204108 (2020).
  32. [32]Vagelatos, N., Wehe, D. & King, J.S. Phonon dispersion and phonon densities of states for ZnS and ZnTe. J. Chem. Phys. 60, 3613–3618 (1974).DOI
  33. [33]Rajput, B. D. & Browne, D. A. Lattice dynamics of II-VI materials using the adiabatic bond-charge model. Phys. Rev. B 53, 9052–9058 (1996).pubmed.ncbi.nlm.nih.gov/9982405
  34. [34]Talwar, D.N. & Becal, P. Infrared and Raman characteristics of bulk Cd₁₋ₓMnₓTe and (MnTe)ₘ/(CdTe)ₙ short period superlattices. Materials Letters 175, 279–283 (2016).DOI
  35. [35]Cardona, M., Etchegoin, P. Fuchs, H. D. & molinà-Mata, P. Effect of isotopic disorder and mass on the electronic and vibrational properties of three-, two- and one-dimensional solids. J. Phys.: Condens. Matter 5, A61 (1993).DOI
  36. [36]Hellman, O. & Kronik, L. Microscopic theory of phonon polaritons and long wavelength dielectric response. ArXiv:2505.03915v1 [cond-mat.mtrl-sci].
  37. [37]Parayanthal, P. & Pollak, F.H. Raman scattering in alloy semiconductors: “Spatial correlation model”. Phys. Rev. Lett. 52, 1822–1825 (1984).DOI
  38. [38]Brafman, O. & Manor, R. Raman line asymmetry in alloys and in ion-implanted polar crystals. Phys. Rev. B 51, 6940–6946 (1995).pubmed.ncbi.nlm.nih.gov/9977248
  39. [39]Hajj Hussein, R. et al. Percolation-type multi-phonon pattern of Zn(Se,S): Backward/forward Raman scattering and ab initio calculations. J. Alloy. Compd. 644, 704–720 (2015).DOI
  40. [40]Pagès, O. et al. Long wave phonons in ZnSe-BeSe mixed crystals: Raman scattering and percolation model. Phys. Rev. B 70, 155319 (2004).DOI
  41. [42]Fantin, A. et al. Short-range chemical order and local lattice distortion in a compositionally complex alloy. Acta Materialia 193, 329–337 (2020).DOI
  42. [43]Körmann, F., Ikeda, Y., Grabowski, B. & Sluiter, M. H. F. Phonon broadening in high entropy alloys, npj computational materials 3, 36 (2017).DOI
  43. [44]Mu, S. et al. Unfolding the complexity of phonon quasi-particle physics in disordered materials. npj Comput. Mater. 6, 4 (2020).DOI
  44. [45]Turner, S. R. et al. Phonon behavior in a random solid solution: a lattice dynamics study on the high-entropy alloy FeCoCrMnNi, Nat. Commun. 13, 7509 (2022).
  45. [46]Janssen, T., Chapuis, G. & de Boissieu, M. Aperiodic Crystals. From modulated phases to quasicrystals, (Oxford University Press, Oxford, 2018, second edition), Vol. 20, IUCr Monographs on Crystallography.
  46. [47]Douvrīs, C., Vaughan, T., Bussan, D., Bartzas, G. & Thomas R. How ICP-OES changed the face of trace element analysis: Review of the global application landscape. Sci. Total Environ. 905, 167242 (2023).DOI
  47. [48]Wang, S.Z. et al. The role of nitrogen-nitrogen pairs in the deviation of the GaAsN lattice parameter from Vegard’s law. J. Appl. Phys. 96, 2010–2014 (2004).DOI
  48. [49]Yu, P.Y. & Cardona, M. in Fundamentals of Semiconductors – Physics and Materials Properties, Springer (4ᵗʰ edition, Heidelberg, 2010).
  49. [50]Hon, D.T. & Faust, W.L. Dielectric parametrization of Raman lineshapes for GaP with a plasma of charge carriers. Appl. Phys. 1, 241–256 (1973).DOI

Paper details

vlnc:W_8hwr5sky
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 2

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents