WorksPhysics and Astronomy
Nature of field-induced transitions and hysteretic magnetoresistance in non-collinear antiferromagnet EuIn2As2
Abstract
We examine the magnetic and electrical transport properties of the hexagonal EuIn2As2 compound, combining experimental and theoretical results. This compound is predicted to be an axion-insulator from an electronic point of view and an altermagnet while in the collinear magnetic phase. However, experiments indicate that the Fermi level lies within the valence band rather than in the topological gap, potentially leading to the dominance of magnetic properties. Our detailed studies on magnetization and electrical transport support the presence of a broken-helix antiferromagnetic state, which was previously identified by X-ray and neutron diffraction experiments. Notably, we observed within that state a field-induced metamagnetic transition marked by a large hysteresis in magnetoresistance, which turns into a sharp upturn for the magnetic field tilted by 15 degree from the c-axis of the crystal. Combined with theoretical calculations, it is explained that the application of a magnetic field changes the low-resistivity antiferromagnetic domain walls to the high-resistivity domain walls due to the reduction in the Fermi surface sheets interaction area in the domain walls, originating from p-orbitals of As. EuIn2As2, therefore, presents a new case study that broadens the understanding of complex magnetic structures and their influence on electrical transport.
Introduction
In recent years, considerable attention has been drawn to the ternary europium-based antiferromagnet EuInAs due to exotic physics originating from the interplay of topological and magnetic properties [1, 2, 3, 4]. The compound exhibits two subsequent antiferromagnetic (AFM) transitions at K and K [2, 3, 4]. According to the neutron diffraction results [2], in both magnetic phases the Eu magnetic moments are confined to the hexagonal -plane. Below , they form an amplitude modulated magnetic phase (AMMP) with the propagation vector [2, 3, 5].
In this state, the magnitude of magnetic moments varies sinusoidally along the -axis. In turn, below , the structure transforms into a broken-helical (B-helix) one, defined by the propagation vector . In the B-helix phase, the directions of Eu spins in the adjacent -planes differ by an angle within the range [2, 3]. In strong magnetic fields applied perpendicular to the helical axis (-axis of the crystal), the compound adopts a fan-type magnetic structure [3, 6]. Basically, the magnetic structure is always co-planar with spins lying in the -plane if there is no component of the magnetic field along the -axis. The trigonal crystal structure of EuInAs implies the formation of three types of antiferromagnetic domains related by symmetry. Below , each domain has the B-helix structure in weak magnetic fields and the fan-type structure in strong fields. The structure of the domain wall (DW) is not yet known, but it is understood that it may also exhibit a similarly complex spin arrangement, which could strongly affect the transport properties determined mainly by the bulk magnetic structure, as discussed, e.g., for TbB [7] and EuCuSb [8]. The recent resonant elastic X-ray scattering (REXS) studies corroborated the B-helix AFM transition that occurs at , but no incommensurate propagation vector was found in the lower- phase [3]. The electrical transport measurements indicated the metallic-like nature of EuInAs with a small concentration of hole-type carriers [9]. This implies that the chemical potential in EuInAs crosses the valence band, which contribute to the electrical transport. In such a case, the axion insulating phase may not manifest itself through a quantized Hall resistivity, in line with the experimental findings for EuInAs [10].
In addition, recent theoretical studies demonstrated that the A-type AFM structure of EuInAs is altermagnetic [11], and the A-type AFM structure is part of the magnetic order observed in this compound. Including the complex magnetism will modify some band structure features, but the g-wave altermagnetic spin-splitting will persist [12]. In the non-stoichiometric compound (hole-doped), the main electronic bands from the altermagnetic state are likely to play an important role in the electrical transport of EuInAs [11].
In this paper, we report the results of our comprehensive magnetization and magnetotransport measurements performed on high-quality single crystals of EuInAs. The primary aim of this study is to understand its complex magnetic behavior, combined with the theoretical calculations. The obtained data support the B-helix AFM ground state scenario, yet also revealed a previously unnoticed magnetic field-induced transition below . The novel feature manifests itself as a distinct hysteresis in the transverse magnetoresistance isotherms and can be attributed to the transformation from low-resistive to high-resistive DW states that occurs due to the reduction of the Fermi surface sheets’ intersection area in the DWs, as indicated by our electronic band calculation in EuInAs.
Materials and methods
Crystal growth: Single crystals of EuInAs were grown by self-flux method. The elements were put in a 1:12:4 ratio in an alumina crucible and sealed inside an evacuated quartz ampule. The ampule was heated very slowly to 1100°C and kept for 24 hours, then cooled down to 800°C at 2°C/h kept at this temperature for 20 hours, followed by slow cooling down to 700°C at a rate of 0.5°C/h. Excess flux was removed with a centrifuge. Platelet-shaped EuInAs single crystals with dimensions mm were obtained. The back-scattering Laue diffraction (Laue-COS, Proto Manufacturing) was used to examine the crystal orientation and quality (see Supplementary Fig. S1 [13]).
Magnetic and transport measurements: Magnetization measurements were performed on an oriented single crystal using a SQUID magnetometer (MPMS-XL, Quantum Design). Electrical transport measurements were performed, using PPMS, on a rectangular-shaped sample cut from an oriented single crystal using a wire saw, with 50-m silver wires attached to the sample using silver epoxy paste. An electric current of 3 mA was applied along the basal -plane. The longitudinal resistivity and Hall resistivity were recorded in a complete loop of the magnetic field. To correct for misalignment of the contacts, the and data were symmetrized and antisymmetrized, respectively, as follows:
Where () and () are the swept-up transverse (longitudinal) and swept-down transverse (longitudinal) resistivities, respectively.
Density functional theory: We performed density functional theory-based first-principles calculations as implemented in Quantum ESPRESSO [14]. The antiferromagnetic ground state was obtained using ultra-soft pseudopotentials under generalized gradient approximation with Perdew–Burke–Ernzerhof type of exchange-correlation functional [15, 16]. For the system EuInAs, we used the experimental lattice constants reported in the literature [11]. The kinetic energy cut-off of 65 Ry and charge density cut-off of 780 Ry was used with a uniform Monkhorst-Pack grid (-mesh) of [17]. High electronic self-consistency convergence criteria of at least were followed in all the calculations. Following these calculations, we performed wannierization for all the systems using the Wannier90 code [18]. We performed postprocessing steps in Wannier90 to calculate the anomalous Hall conductivity (AHC) as an integral of the total Berry curvature over the entire Brillouin zone using a dense -mesh of with adaptive mesh refinement scheme [19]. In the case of altermagnets, the contribution to the AHE does not come from the entire -space since the Berry curvature could be zero along high-symmetry points or at the border of the Brillouin zone; therefore, a denser grid is necessary. To avoid numerical inaccuracy with the wannierization without SOC and magnetization, we performed the wannierization of the -In and -As in the nonmagnetic phase without SOC and later, we added SOC and magnetism on the -As states, combining first principles and model Hamiltonian as described in the Supplement materials.
Field-induced transitions and magnetic anisotropy
Figure 1a presents the temperature-dependent magnetic susceptibility () measured under various magnetic fields for the configuration . At low field (0.01 T), a broad magnetic transition is observed. With increasing field (e.g., to 0.05 T), this broad feature splits into two distinct anomalies: K, identified by a change in slope (highlighted by a dotted line), and K, corresponding to a maximum in (see Figure 1b). The derivative of (), shown in Figure 1c, exhibits a clear kink at and a maximum at , with the kink becoming more pronounced at intermediate fields (e.g., 0.13 T). Both transitions shift systematically toward lower temperatures with increasing magnetic field. Additionally, a new anomaly emerges above 0.05 T as a broad maximum, separated from the (see dotted line in Figure 1c), which also shifts to lower temperatures with increasing field. Below , a bifurcation between the zero-field-cooled (ZFC) and field-cooled (FC) curves becomes apparent, at 0.15 T. This bifurcation indicates the presence of a first-order metamagnetic (MM) transition.

Figure 1. (a) Temperature-dependent susceptibility () for , measured in the zero-field cooled under various magnetic fields. Blue dotted line represents the measured under field cooling for 0.01 and 0.15 T. (b) Zoom portion of (a) for the 0.01 and 0.05 T encompassing two transition temperatures ( and ). (c) depicts the three transition temperatures: , , and . Curves are offset for clarity. (d) The real part of the AC susceptibility measured in different DC magnetic fields, , with a driving field of 10 Oe and frequency of 299 Hz. (e) Zoom portion of (a) for the 0.05 and 0.08 T encompassing two transition temperatures ( and ). (f) The imaginary part of the ac susceptibility measured in the same DC and AC fields. The arrows represent the transition temperatures , , and . Data in (d) and (f) are offset by 0.02 and 0.0025 emu/g, respectively.
To further investigate the magnetic transitions, temperature-dependent AC susceptibility measurements were performed. The real part of the AC magnetization (), shown in Figure 1d, confirms the presence of transitions at , , and , all of which shift to lower temperatures with increasing magnetic field. A magnified view of the transition region is presented in Figure 1e, where is associated with a change in slope and appears as a subtle kink, both of which sharpen with increasing field. The transition begins to emerge as a maximum in at 0.12 T, consistent with the DC susceptibility results. The imaginary component of the AC susceptibility (), shown in Figure 1f, further corroborates the presence of the transition. This feature arises above 0.08 T, reaches a maximum, and is fully suppressed above 0.21 T. The presence of at strongly supports the first-order nature of the MM transition, likely associated with a spin-flop mechanism, in agreement with the DC magnetization data. Furthermore, field-dependent AC magnetization measurements reveal the presence of an MM state between and (see Supplementary Figure S2 [13]), consistent with the DC magnetization results. A significant imaginary component in the AC magnetization is also detected within the MM region at 2 K (see Figure S2), coinciding with the field range in which is observed in the temperature-dependent measurements.

Figure S2. (a) The Curie-Weiss law fit (blue line) for the , measured at 0.1 T, above . (b) Magnetization as a function of magnetic field recorded at 2 K in a complete loop for . The dotted line marks the saturation field (). (c) and (d) The real- and imaginary-ac susceptibility as a function of the magnetic field, measured at 2 K. MM is the metamagnetic region.
To get a deeper insight into the nature of the magnetic states, the magnetization () isotherms were measured in increasing (solid lines) and decreasing (dashed lines) magnetic field applied perpendicular to the -axis, (Figure 2a). At 2 K, is nonlinear even in weak magnetic fields and nearly saturates near T (see Figure 2a and Figure 2b). As can be inferred from Figure 2c, the derivative of the data taken in the swept-up-field regime, exhibits two peaks at T and T, while that of data collected in the swept-down-field regime shows corresponding peaks at T and T (see Figure 2d). In addition, we also observed an additional peak at T for the swept-up-field. With increasing temperature, the peak of at shifts to lower fields, while the peaks at (or ) come closer to these at (or ), and above 8 K their positions overlap. In addition, their magnitude rapidly diminishes. Also the values of and come gradually closer to each other and position near T at K. The evolution of the peaks in illustrates the behavior of the hysteresis in that at K develops near 0.1 T and vanishes above 0.3 T, but shrinks with rising temperature and disappears near 16 K (cf. the Figure 2b).

Figure 2. (a) Isothermal magnetization measured at several different temperatures in swept-up field (solid line) and swept-down-field (dotted line) regimes. (b) Similar isothermal magnetization in field range 0 - 0.35 T. Data at different temperatures in this plot are offset by 0.5 for clarity. Derivative of magnetization (taken from Figure 2a) plotted at different temperatures in swept-up-field (c) and swept-down-field (d). The black, red and blue dashed lines represent the (or ), (or ) and transitions, respectively. (e) The color map of the , where ’dn’ and ’up’ mark the data collected in the swept-down- and swept-up-field regime, respectively. , and are the transition temperatures extracted from the DC and AC magnetization data, shown in Figure 1(b-Figure 1f). , , and , are transition fields for swept-up and swept-down fields, respectively, extracted from Figure 2(c-Figure 2d).
The magnetization data collected for with are summarized in Figure 2e in the form of a – phase diagram. Besides the phase boundaries corresponding to the transitions from the paramagnetic state to the AMMP and then into the B-helix state, there are additional lines in this diagram which were defined by the values of , , , , and . These new phase boundaries trace an intermediate metamagnetic (MM) phases (termed , ) and if observed in the swept-up-field and the swept-down-field regime, respectively). Furthermore, there is the fan-type structure state, which emerges in magnetic fields stronger than those which delineate the phase (see Figure 2e). The presence of B-helix and metamagnetic transitions is consistent with previous reports [5, 20], which employed resonant elastic X-ray scattering (REXS) and optical polarimetry, respectively. However, in our measurements, we identify an additional metamagnetic transition () in close proximity to the previously reported one.
To understand the evolution of magnetic structures in with increasing magnetic field strength, it is important to realize that in the B-helix structure state, observed at low temperatures in weak magnetic fields, there are three types of AFM domains. Following Ref. [3], it can be assumed that in the field the Eu spins rotate perpendicular to the magnetic field in two domains, but remain unchanged in the third one. Then, in the field , the Eu-spins in the latter domain flip parallel to the magnetic field, while those in the other two domains gradually turn toward the magnetic field direction. However, in the swept-up-field, an additional transition at suggests that the previously proposed picture of magnetic domain wall evolution under an in-plane magnetic field may need to be amended. Full polarization of the moments in all three domains is achieved above the field . The transition from the helical AFM to the MM state can be first- or second-order, depending on the turn angle between Eu-moments in adjacent layers [21]. The hysteretic behavior of this transition in , accompanied by a large imaginary component in the temperature- and magnetic-field-dependent AC magnetic susceptibility of the compound in the MM state (see Figure 1f and Supplementary Figure S2 [13]), hints at the first-order MM transition.
Hysteretic Magnetoresistance
We determined the magnetoresistance () for , at various temperatures. Results are shown in Figure 3a. Measurements conducted in swept-up and swept-down fields lead to slightly different results, showing the hysteresis of MR in the field range where the compound undergoes magnetic field-induced phase transitions. Notably, at temperatures below 10 K MR measured for the swept-up-field is clearly larger compared to the swept-down-field MR in two ranges of field: around 0.15 T and around 0.35 T. Figure 3b depicts the phase diagram superimposed on a color map of (=), indicating the presence of hysteretic MR in both MM and fan-type structure states. Nevertheless, a key observation is that at low temperatures and for (i.e. in the fan-type state) the MR exhibits significant hysteresis, even though this is not reflected in the magnetization (see Figure 2e and Figure 3b for comparison. The hysteretic MR (Hys-MR) could arise from the complex magnetic structures in the DWs [7] or from the competitive nature of the ground state at the boundary of the collinear phase and helical phase within the domains, like in EuCuSb and EuZnGe [8, 22]. The latter conjecture is ruled out for EuInAs, as its ground state is the homogeneous B-helical phase, without phase boundaries. Thus, we argue that Hys-MR in EuInAs emerges due to DWs’ contribution to the scattering of charge carriers. Furthermore, DWs can be tuned between high and low resistivity, depending on the carrier concentration, and the strength of interaction of conduction electrons with the local magnetic moments [23] or the spin configuration in the magnetic structure [24, 25].

Figure 3. (a) Magnetoresistance (MR) measured at different temperatures in swept-up- (solid line) and swept-down-field (dotted line). Data in this plot are offset for clarity. , , and , are the same characteristic fields, defined in Figure 2(c-Figure 2d). (b) The color map of the (). (c) MR measured at different angles in swept-up and swept-down. Data are offset by 0.05 for clarity. and are transition fields for swept-up and swept-down fields, respectively. are saturation fields interpolated between values determined for and for . The inset shows the diagram of MR measurement. (d) The color map of the , showing the hysteresis in the MM and fan-type structure states.
Next, we investigated the MR at 2 K, for different angles between c-axis and magnetic field, rotating it from B c to B c, as shown in Figure 3c (the current was always perpendicular to the magnetic field). By rotating the magnetic field towards c-axis, the slope of low-field positive MR decreases and reaches zero at around . For negative MR arises and becomes strongest at . The negative MR is due to the gradual alignment of the Eu moments with increasing magnetic field, reducing the spin-disorder electron scattering. However, above a specific field, , MR upturns and reaches a maximum, marking the occurrence of an additional scattering mechanism. In even higher fields, this additional contribution to the scattering gradually fades out and becomes negligible in fields close to .
The color map of the in Figure 3d, shows that in the MM state, hysteresis is suppressed for , but the Hys-MR regime persists even below the , indicating that both have a different source of electron scattering. The hysteresis within the MM state arises due to the first-order nature of the MM transition, which is consistent with the isothermal magnetization. Indeed, above the , the Hys-MR, along with increasing MR, can have numerous mechanisms, for example, proposed in literature, such as Fermi-surface reconstruction [26] or electronic wave localization [27]. In our bulk magnetization measurements, transition is not observed for (see Supplementary Figure S2 [13]), but it manifests in the MR as a minimum (see Figure 3c). It implies that the transition at is not caused by the bulk magnetic structure. In addition, our electronic band structure calculations, combined with the electrical transport measurements, show that the material is a low-carrier-concentration metal with an easily tunable electronic structure near the Fermi level (discussed in detail below). Thus, the Hys-MR, along with increasing MR, can be associated with the electron scattering on DWs, which is tunable between the low resistivity and high resistivity depending on the geometry of the electronic or magnetic structure [23, 24, 25]. For example, in pyrochlores, the antiferromagnetic DWs were reported to be metallic for all-in-all-out spin configurations and insulating for two-in-two-out spin configurations [24, 25]. But this form of spin-configuration does not exist in the EuInAs.
Anomalous Hall Effect
To further understand the origin of the observed hysteresis in MR and its interplay with the electronic structure, we examined the Hall resistivity () shown in the Figure 4a and Figure 4b. These measurements were recorded at different angles of applied magnetic field, rotated from to , at K and K, respectively, both in swept-up and swept-down field regimes, showing no hysteresis. For and fields above , we fitted with the following equation to estimate the carrier concentrations:

Figure 4. Hall resistivity as a function of magnetic field recorded at various angles for (a) K and (b) K. Insets to (b) display the angle-dependent carrier concentration at K, respectively. The carrier concentration was estimated using equation (1).
where , is the angle between B and -axis. Inset of Figure 4b shows the angle-dependent carrier concentrations, which are hole-type.
It is noted that carrier concentration is nearly the same at K and K (see to inset Figure 4b and Supplementary Figure S8 [13]), therefore we obtained by subtracting the ordinary Hall resistivity from the total Hall resistivity, using the relation: , where and are the Hall resistivities measured at temperatures K and K, respectively (see Figure 4a and the 4b), and is shown in the Figure 5a. As reported in [9], the maxima in within the B-helix state are attributed to the non-collinear magnetic structure in this compound.

Figure 5. (a) The residual Hall resistivity, , at 2 K, plotted for different field angles. Data are offset for clarity. (b) Angular dependence of in a field of 3 T, i.e., above the saturation field. (c) Anomalous Hall conductivity plotted against the longitudinal conductivity in a field of 3 T for various angles. The straight violet line is a guide for the eyes, indicating that follows the linear relationship with . Inset: schematic representation of asymmetric scattering of conduction electrons on the local moments of Eu. (d) The anomalous Hall angle, , vs. field orientation angle, , in a field of 3 T. Inset shows the diagram of the Hall measurement.

Figure S8. (a) Hall resistivity as a function of magnetic field recorded at various temperatures for . The arrows represent the up and down directions of the field sweep. Data are offset for clarity. (b) Temperature dependence of carrier concentration. The dotted lines show the AFM transitions. (c) Anomalous Hall resistivity (obtained as described in the main text) as a function of the magnetic field at different temperatures. is the saturation field.
Above , the system enters a fully polarized state and corresponds to the anomalous Hall resistivity (). Figure 5b shows the angle dependence of . At and K, is small. As the angle increases, grows, reaching at .
In polarized ferromagnetic systems, can be described as [28]:
where represents the anomalous Hall coefficient coupled to , which can be intrinsic or extrinsic. For intrinsic and extrinsic transverse scattering, is proportional to the and , respectively [28].
Next, we convert it to anomalous Hall conductivity (AHC) by following the relation: , since .
Above , the local moments are aligned with the field, and remain the same for all angles between and , but it should be noted that does not remain constant (see Figure 5c). It is because the coefficient depends on , causing the to vary with the . For , is equal to the 1.83 Scm. With increasing the angle, increases, and reaches -63 Scm for 90°. The follows the in linear manner (cf. Figure 5c. This underpins the argument of itinerant electrons’ asymmetric scattering induced by the polarized local moments (sketched in the inset of Figure 5c) [28]. Finally, we calculate the Hall angle () defined as:
Figure 5d shows the Hall angle for different , reaching the value of -1.6% at 90°, which is small, as expected for topologically trivial electronic structure with low spin-orbit coupling [28].
Electronic Structure Calculations
To shed more light on the electronic structure, we performed density functional theory (DFT) calculations starting from the collinear antiferromagnetic state with propagation vector and rotating the spin under the effect of the external magnetic field. Therefore, we computed the evolution of the Fermi surface under the in-plane magnetic field by tuning the azimuthal angle of the spins , while to simulate the out-of-plane magnetic field, we tuned the out-of-plane magnetic field (more details are reported in Supplement Materials [13]). In our notation, corresponds to the A-type AFM with in-plane spins, while corresponds to the FM phase with in-plane spins.
We study the Fermi surface for at the energy meV to simulate the p-type Fermi level, which is reported in Figure 6. We obtain 4 Fermi sheets at zero magnetic field corresponding to , we have two degenerate Fermi surfaces since we are in the nodal plane of the altermagnet. A value of different from zero breaks Kramer's degeneracy, pushing the system to a nodeless band structure [29] and we observe 4 Fermi surfaces for and . Increasing to , there is a Lifshitz transition for which 1 FS gaps out at the point and we are left with 3 FS sheets. Increasing the in-plane magnetic field corresponds to increasing , until the system goes towards a fully ferromagnetic phase at . We repeat the same calculation at the same energy meV for an out-of-plane magnetic field and we do not observe any Lifshitz transition (see Figure S13 [13]). Therefore, we have a Lifshitz transition that depends on the magnetic field orientation. For the same orientation for which we theoretically observe the Lifshitz transition, we observe the metamagnetic transition in the experimental results.

Figure 6. Evolution of the Fermi Surface around the point as spin alignment changes from A-type AFM () to FM with spin in the plane () for the energy meV below the Fermi level expected for a stoichiometric compound.

Figure S13. Evolution of the Fermi Surface around the point as spin alignment changes from FM with spins out of plane () to A-type AFM () for the energy meV below the Fermi level expected for a stoichiometric compound.
We examined the magnetic contribution from the As--orbital (at Wyckoff position) and found that the moment of -orbital is antiparallel to the neighboring Eu moments (see Supplementary Figs. S9a and S9b [13]). The Fermi level (approximated from the experimental ordinary Hall resistivity) is located in the valence band. A-type antiferromagnetic coupled moments of Eu exhibit the altermagnetic spin-splitting feature in momentum-space [11].
For (the angle between the As-spin moment and the -axis), the structure of the As-spins is an A-type AFM. The electronic band structure shows non-relativistic spin-splitting, while the electronic bands don’t cross the Fermi level at the point. When the spin’s rotation angle decreases, there is a spin-splitting at the point and grows. In addition, the results of our calculations show that in an applied magnetic field, the spin-splitting from the magnetic field also occurs at the -point (see Figure S11 [13]) and could contribute to magnetotransport. In the presence of As-spin-canting that could be due to the magnetic field via the interaction with the local moments or relativistic weak ferromagnetism, the size of the spin-splitting increases and the bands cross the Fermi level (see Figure S11 [13]). Following the theoretically calculated electronic structure, the longitudinal resistivity could be reduced. Nevertheless, we have observed an upturn of the MR in , which suggests that growing of As-spin via interaction with the local moments could reduce the intersection area of Fermi surface sheets () on the DWs and increase the electron scattering.

Figure S11. Comparison between the dispersion (top) and the resulting intrinsic anomalous Hall conductivity (bottom right) for various angles between spin in As layers, depicted in Figure S9 (a). In the bottom left of the panels, we observe the low-energy part of the dispersion. Panels (a)-(f) show the evolution from the ferromagnetic arrangement () to the A-type antiferromagnet (), in linear increments. The positive and negative peak in the valence and conduction bands derives from the properties of the Berry curvature for topological systems. Different colors are used for different energy bands as a guide for the eyes.
Next, the AHC is calculated for the respective rotation angles (see Figure S11-Figure S11 [13], lower, right-side panel). Due to the topological band structure in the ferromagnetic phase, we have opposite values of the AHE in the valence and conduction band due to the opposite values of the Berry phase in topological materials [30]. For , a finite AHC of the order of 3 S cm is obtained at the Fermi-level, which is quite close to the experimental value of 1.8 S cm for (see Figure 5c). Thus, it shows that As-spin contributes to the AHC with a small positive value, and supports that it plays the main role in DWs scattering. We interpreted the AHC in the polarized FM state of the local moment, where the theoretical scenario applies for . Due to the relatively simple structure of the AHE, which is positive in the conduction band and negative in the valence band and to the impossibility of having strong band structure reconstruction, we can assume that the intrinsic AHC stays small and positive for the different orientations of the magnetic field.
Discussion
EuInAs shows two antiferromagnetic transitions at and , which correspond to the AMMP and B-helix states. With the magnetic field applied in the -plane, the magnetic state changes first to a metamagnetic state, then to a fan-like structure, and finally to a fully polarized ferromagnetic state. Notably, the metamagnetic transition occurs at a lower field when the field is swept-down compared to when it is swept-up, pointing to a dynamic nature of the magnetic structure. MR data are consistent with the magnetization results, but they also exhibit additional features. In particular, the fan state shows a strong hysteresis in MR that is not occurred in the isothermal magnetization measurement. Angle-dependent MR further shows that the metamagnetic transition weakens as the field direction is tilted toward the -axis, while the hysteresis in the fan-state persists. Moreover, an upturn in MR is observed for field angles below about 30°. The combination of strong hysteresis and enhanced scattering in the MR cannot be fully explained by the bulk magnetic structure. Instead, these features likely arise from domain-wall dynamics.
Domain walls can significantly influence charge transport in materials with complex magnetic and electronic structures. According to the theory given in the literature [23], the contribution of scattering on DWs to the resistivity is inversely proportional to , where is the intersection area shared by the Fermi surface sheets on the DWs. The Landau-Büttiker approach indicates that electrons can only transmit over the DWs if their transverse momentum is preserved at the Fermi level, which requires that the sheets of the Fermi surface from two neighboring domains have the intersection of finite area () [31, 32]. That intersection can be controlled by carrier concentration, via changing the size of the Fermi surface sheets on either side of DWs. The lower carrier concentration indicates the presence of a smaller sheet of the Fermi surface, which results in a decrease of in the DWs and in increased electron scattering. So far, domain wall scattering phenomena have only been explored for Weyl or nodal semimetals because they have the nodes at the Fermi level associated with the low carrier concentrations of the order of [23, 32]. Here, we expanded this phenomenon to the non-collinear magnet EuInAs, with a carrier concentration of the order of , about 10-fold lower than in magnetic Weyl semimetal CeAlGe [23]. In EuInAs, the local -level is distant from the Fermi level. Theoretical calculations show that the -orbital of the As atom contributes to states at the Fermi level and that electronic bands are spin-split due to altermagnetism and the induced moment on -orbital by Eu--moments (see Figure S11 [13]). As a result, this spin-splitting modifies the size and geometry of the sheets of the Fermi surface (see Supplementary Fig. S13 [13]). Thus, it could also reduce the intersection area () in the DWs around (or ), and consequently, increase the carrier scattering.
Theoretical calculated AHC for the electronic band structure of the As -orbital yields a small finite value, which agree with the experimental AHC for . This supports the interpretation that the underlying electronic band structure is trivial, due to the position of the Fermi level in the valence band where the relevant spin-orbit coupling originates from As-atoms [11]. These AHC results shed light on the contribution of the -orbitals to the electrical transport, and reveal that the hysteresis observed in magnetoresistance arises from domain walls coupled to the -orbitals of As.
Conclusions
Combining theoretical and experimental results and taking into account magnetic and topological properties, we considered the impact of complex magnetism of EuInAs on its magnetoresistance. We described the metamagnetic transition associated with a large hysteresis in magnetoresistance, which turns into a sharp upturn for the magnetic field tilted by from the -axis of the crystal. Our findings explain the origin of strong MR scattering associated with the hysteresis that arises from DWs. The application of a magnetic field changes the low-resistivity antiferromagnetic domain walls to the high-resistivity domain walls due to the reduction in the Fermi surface sheets interaction area in the domain walls, originating from -orbitals of As.
Acknowledgments
The authors acknowledge Tomasz Dietl for useful discussions. This work was supported by the National Science Centre (NCN, Poland) under Project no. 2021/41/B/ST3/01141 (K.S., O.P., T.R., T.T., P.W. and D.K.). J. S. and C. A. were supported by the “MagTop” project (FENG.02.01-IP.05-0028/23) carried out within the “International Research Agendas” programme of the Foundation for Polish Science co-financed by the European Union under the European Funds for Smart Economy 2021-2027 (FENG). J. S. is supported by the Narodowe Centrum Nauki (NCN, National Science Centre, Poland) Project No. 2019/34/E/ST3/00404. We acknowledge the access to the computing facilities of the Interdisciplinary Center of Modeling at the University of Warsaw, Grant g91-1418, g91-1419, g96-1808 and g96-1809 for the availability of high-performance computing resources and support. We acknowledge the CINECA award under the ISCRA initiative IsC99-”SILENTS”, IsC105-”SILENTSG”, IsB26-”SHINY” and IsCb7-”CHARPHEN” grants for the availability of high-performance computing resources and support. We acknowledge the access to the computing facilities of the Poznań Supercomputing and Networking Center Grant No. pl0223-01 and pl0267-01.
Supplemental Material for Nature of field-induced transitions and hysteretic magnetoresistance in the noncollinear antiferromagnet EuIn₂As₂
Karan Singh; Jan Skolimowski; Giuseppe Cuono; Raghottam M. Sattigeri; A. Ptok; O. Pavlosiuk; Tetiana Romanova; Tomasz Toliński; P. Wiśniewski; Carmine Autieri; D. Kaczorowski

Figure S1. Back-scattered Laue pattern of the EuIn₂As₂ crystal oriented along the (001) direction.
Magnetization
For EuIn₂As₂, inverse follows the Curie-Weiss law in the paramagnetic region, which was measured for at 0.1 T:
Where is the Curie constant, and is the paramagnetic Curie temperature. These parameters are derived from the fitting of the equation S1 (shown as a blue line in Figure S2). The effective magnetic moment () calculated from the parameter is 7.7 , which closely matches with the theoretical value of 7.94 for Eu ions. The obtained Curie temperature () is 19.2 K, indicating the presence of a predominance of ferromagnetic exchange interactions in the antiferromagnetic compound. Magnetization () as a function of the magnetic field in a complete loop was measured at 2 K for and indicates that hysteresis is absent, as illustrated in Figure S2. As the magnetic field increases, the magnetization increases and reaches a saturation value of 7 at field = 2 T. This value is consistent with the theoretical moments for Eu, which correspond to spin magnetic moments since the orbital angular momentum is negligible. The saturation field is larger compared to the one obtained with the field perpendicular to the -axis.
Magnetoresistance
Figure S3 shows the temperature-dependent resistivity () for , recorded at 2K and 0T. The derivative of shows the two antiferromagnetically transitions and (see inset to Figure S3), which corroborate the magnetization results. In this section, we analyze the low-field magnetoresistance, MR () data. Figure S4 shows the average MR () at various temperatures for . At 16 K, the increases with increasing magnetic field and reaches a maximum at 0.5 T. Above 0.5 T, it decreases. This maximum position shifts to higher magnetic fields with decreasing temperature. The decrease in above the maximum is attributed to the polarization of the Eu moments aligning with the applied field, resulting in reduced electron scattering. Below the maximum at 2K, the exhibits a minimum at 0.6 T, which shifts towards the lower field and is suppressed above 8K. In the main text, we have explained that the minimum occurs owing to domain and domain wall scattering, which is balanced at the minima field. With the rising temperature, domain wall scattering increases and becomes dominant above 8 K, suppressing the minima field.

Figure S3. Temperature-dependent resistivity, measured at 0T for . Inset: magnified area of resistivity near the transition temperature, as represented by the left axis. The right axis represents the derivative of the same resistivity. and indicate the two transition temperatures compatible with the magnetization.

Figure S4. (a) Field-dependent magnetoresistance () recorded at various temperatures for (). (b) measured at various angles and at 2K. (c) recorded at different temperature and for ().
Next, we examined magnetoresistance at various angles at 2 K (Figure S4). Interestingly, the exhibits a positive linear dependence on the magnetic field for angles exceeding 10°. For 90°, we measured the at different temperatures (Figure S4), and linear persists up to 14 K and the slope remains positive. The linear magnetoresistance at high fields (where , here, represents the cyclotron frequency, and symbolizes the relaxation time) has established explanations related to electronic properties (like lowest spin-split landau level [33], low carrier mass Dirac surface state [34], magnetic breakdown [35] etc.) or geometrical factors (strong mobility fluctuation [36], disorder [37] etc.). However, its occurrence at low fields () is unexpected. The authors of reference [38] discuss potential origins such as a change of Fermi-surface topology or scattering of charge density wave fluctuations at specific Fermi surface points. This suggests that itinerant electrons experience more abrupt scattering events on the Fermi surface before each collision arising from the change in the Fermi-surface area in sharp edges, which depends on the local magnetic moment configurations. In this scenario, a large is expected [38]. As shown in Figure S4, the reaches 2% at a relatively low applied magnetic field of 0.1 T. This large value at low field supports a changeover of Fermi surface topology turning to a strong scattering. Furthermore, we measured the MR in high magnetic fields up to 9 T for (Figure S5) and (Figure S5), where it reaches a larger value of 63 and 65%, respectively, showing presence of colossal negative magnetoresistance in the system. The MR at 9 T for the is significantly larger than for the , indicating that the Fermi surface topology is anisotropic. Figure S13 shows the calculated evolution of the Fermi surface at the point of the -As from antiferromagnetic () to ferromagnetic () spin alignment induced by the Eu-4f moment at the Fermi level.

Figure S5. Magnetoresistance recorded at different temperatures for (a) (b) .
Hall effect
We have measured the collected at various temperatures for (see Figure S8). The temperature dependence of carrier concentration is plotted in Figure S8. The plot in Figure S8 illustrates the residual Hall effect (), for , displayed across the temperature range of 2-20 K. The extraction of is performed using equation (1) in the high-field region and then extrapolated to the low-field region, as illustrated in Figure S7. Below the , a non-collinear magnetic structure arises with a maximum in the , which declines as temperatures increase. The maximum corresponds to the acquisition of finite spin chirality in the non-collinear magnetic structure [9]. Furthermore, the changes from positive to negative, as detailed in the main text, due to the competition of intrinsic and extrinsic transverse scattering or energy () modification.

Figure S7. Magnetic field dependent Hall resistivity at 2K. The red line represents the fit of the ordinary Hall effect (described in equation (1)) to extract carrier concentrations. A similar procedure was used to extract the carrier concentration (shown in the inset of Figure 4b and Figure S8) for other temperatures and angles.

Figure S6. (a) Magnetoresistance (MR) measured at different temperatures for in swept-up and swept-down. This Figure is plotted in a shifted scale for clarity. (b) represents the color map of MR () calculated from data shown in (a). () represents the field strength for the transition in MR.
Electronic and magnetic properties of the collinear magnetic phases
Using the computational setup from the literature [11] which combines the HSE approach and the Coulomb repulsion , we compare the band inversion of the ferromagnetic phase with spins along the -axis (FMc) and altermagnetic phase with propagation vector and spins along the -axis (AMa, see Figure S9). The system has band inversion at the point between -Cd and -As. The strength of the band inversion for both magnetic phases is shown in Figure S10 as a function of the Coulomb repulsion . Within this approach, the experimental position of the -orbitals is reproduced for values of between 1 and 2 eV [11]. For these values of , the system transits from an antiferromagnetic trivial insulator to a high-order topological ferromagnet known as ferromagnetic axion-insulator [39]. Therefore, we can understand why we can expect a strong evolution of the electronic properties as a function of the magnetic field.

Figure S9. (a) Crystal and magnetic structure of . Regarding the crystal, the Eu atoms are purple, the As atoms are green and the In atoms are grey. Regarding the magnetism, we show the so-called A-type antiferromagnetic structure with the relevant spins on the Eu-- and As--orbitals and with orientation along the -axis. The -orbitals of the As atoms present at the Fermi level have an induced magnetization antiparallel to that in the closest Eu layer; this induced magnetization is relevant for the AHE. The In atoms have no magnetization. (b) Flipping of the As- spins from the A-type antiferromagnetic structure with spin along the -axis to the ferromagnetic structure with spins along the -axis. We introduce the polar angle to simulate the rotation of the spins under an external magnetic field applied along the -axis. For we have the AFM configuration with spins along the -axis (AFM), while for we have the FM phase with spin along the -axis (FM). As and As have the spins of the first sublattice, while As and As have the spins of the second sublattice.

Figure S10. Energy gap for EuInAs as a function of the Coulomb repulsion energy in AFMa phase and in FMc phase. For the negative values of we are in the topological phase, while for positive values, we are in the trivial phase. These results were obtained using the previous computational setup reported in the literature [11].
This phase is altermagnetic with bulk g-wave order as for MnTe [40]. The altermagnetic properties in the valence band are driven by the -orbitals of As since the Eu-4-states are not at the Fermi level and the Cd--orbitals are nonmagnetic. EuInAs and MnTe have the same space group no. 194, however, in EuInAs, the Eu, In, and As atoms occupy Wyckoff 2a, 4f, and 4f positions, respectively. In MnTe, Mn and Te occupy 2a and 2c Wyckoff positions, respectively. Since we examined the magnetism coming from the As (with 4f Wyckoff position), the two compounds could have different properties for the Hall vector. Depending on the symmetry, the anomalous Hall effect in altermagnets can also be present at zero field due to the breaking of the time-reversal symmetry. The direction of the Hall vector depends on the symmetries; additionally, a relativistic weak ferromagnetism appears along the Hall vector [41]. With the spins in the plane but orthogonal to the lattice vectors, the Hall vector points along the -axis of MnTe [42, 43] due to a spin-orbit driven magnetic interaction which shares similarities with the Dzyaloshinskii–Moriya interaction. Among the first-neighbors magnetic atoms in 2a Wyckoff position with space group no. 194 as the Eu atoms in EuInAs, we have the same spin-orbit driven magnetic interaction that could produce weak ferromagnetism. However, this mechanism does not produce the non-collinearity experimentally observed; therefore, the origin of the non-collinearity in EuInAs likely arises from the competition between different magnetic exchanges within the Eu-layers.
Evolution of the Fermi surface and band structure in applied magnetic fields combining first-principles and model Hamiltonian
In the case of a perfectly stoichiometric compound, the system would be a trivial insulator or axion-insulator as discussed in the previous section. Experimentally, EuInAs has Eu-deficiencies and this produces hole carriers with the Fermi level in the valence band, analogously to EuCdAs [44]. Due to the position of the Fermi level,
the topological effects should not influence the experimentally observed electronic and magnetic properties. For the evolution of the Fermi surface and AHE, we study the electronic properties without including the electronic correlations; therefore, the band structure developed in this section would be in the topological phase. We study the evolution of the band structure as a function of the polar angle of the spin [see configuration in Figure S9] as it was analyzed in doped antiferromagnetic insulators [45].
For a realistic simulation of this compound, we need to have As and As belonging to one sublattice while As and As belong to the other sublattice, as shown in Figure S9. We start from the non-magnetic (NM) Hamiltonian obtained with the Wannier functions basis:
The non-magnetic Hamiltonian already contains the crystal symmetries of the NiAs space group. Once the local spin-splitting is added, the altermagnetic spin-splitting will appear. We add the on-site terms as the on-site spin-splitting dependent on the angles and the As spin-orbit coupling meV [46].
while for the s-orbitals there is no SOC. The s-orbitals have neither spin-splitting, while the module of the on-site spin-splitting of As is fixed at meV. The crucial information regarding the spin evolution is included in the real space magnetic configuration and their angular dependence of the As spin described in Figure S9. In the general case, the intrinsic anomalous Hall effect in an altermagnet with flipping spins could be seen as a combination of the anomalous Hall effect from the altermagnet (which depends on the component) and the anomalous Hall effect from the ferromagnetism along the c-axis (which depends on the component). For , the AHE comes only from the altermagnetic properties, while for the AHE depends only on the properties of the ferromagnet. For intermediate values of , the interplay is not straightforward since we cannot decompose the AHE calculated in the k-space in terms of the real space quantities as the polar angle , a similar aspect was proven for a decomposition of the AHE on different layers (see supp. material of the reference [47]).
We study the AHE with spin along the c-axis in the topological regime since we are interested in matching the experimental results in the limit of B where the system becomes a ferromagnetic axion insulator [39]. We calculate the AHE as a function of , where in the experimental realization, the polar angle is controlled by the magnetic field. The results of the AHC are reported in Figure S11. Additionally, we calculate the as a function of for different energies and the results are shown in Figure S12 where we also observe a positive sign of AHC for the three lowest values of , while it is negative for the four highest values with a sign change of the AHC. For negative values of the Fermi level lies in the valence band and the anomalous Hall conductivity gets reduced in an applied magnetic field in qualitative agreement with the experimental results.

Figure S12. Evolution of the intrinsic anomalous Hall resistivity as a function of the polar angle for different energies . The value of corresponds to zero magnetic field, while the value corresponds to the saturation magnetic field.
We also calculated the evolution of the Fermi surface topology at the energy meV below the Fermi level for a stoichiometric compound. We obtain a strong evolution of the Fermi surfaces from the AMa to the FMc phase. The Fermi is calculated at , which is a nodal plane for the altermagnetic phase. In the collinear AMa phases, we can see 2 couples of Fermi surfaces since the altermagnetic spin-splitting is absent at . When we include an component, we have transitioned to a nodeless band structure [29] with 4 distinct Fermi sheets as shown in Figure S13, which are 2 for spin-up and 2 for spin-down. Finally, for the FM phase and close to it (), we are approaching a Lifshitz transition but still have 4 Fermi surfaces. Therefore, the system is prone to have Lifshitz phase transitions induced by the external magnetic field along the z-axis; the Lifshitz phase transition depends on tiny details such as small variations in the filling or the orientation of the magnetic field. However, the in-plane magnetic field produced the Lifshitz phase transition. The magnetic-field induced Lifshitz phase transitions are usually concomitant to metamagnetic transitions [48], especially for compounds hosting f-electrons [49, 50, 51, 52]. Therefore, the metamagnetism experimentally observed can be generated by the Lifshitz phase transition with the in-plane magnetic field.
References
- [1]Y. Xu, Z. Song, Z. Wang, H. Weng, and X. Dai, Higher-Order Topology of the Axion Insulator EuIn₂As₂, Phys. Rev. Lett. 122, 256402 (2019).
- [2]S. X. M. Riberolles, T. V. Trevisan, B. Kuthanazhi, T. W. Heitmann, F. Ye, D. C. Johnston, S. L. Bud’ko, D. H. Ryan, P. C. Canfield, A. Kryssig, A. Vishwanath, R. J. McQueeney, L. L. Wang, P. P. Orth, and B. G. Ueland, Magnetic crystalline-symmetry-protected axion electrodynamics and field-tunable unpinned Dirac cones in EuIn₂As₂, Nat. Commun. 12, 999 (2021).
- [3]J. R. Soh, A. Bombardi, F. Mila, M. C. Rahn, D. Prabhakaran, S. Francoual, H. M. Rønnow, and A. T. Boothroyd, Understanding unconventional magnetic order in a candidate axion insulator by resonant elastic x-ray scattering, Nat. Commun. 14, 3387 (2023).
- [4]E. Donoway, T. Trevisan, A. Liebman-Peláez, R. Day, K. Yamakawa, Y. Sun, J. Soh, D. Prabhakaran, A. Boothroyd, R. Fernandes, J. Analytis, J. Moore, J. Orenstein, and V. Sunko, Multimodal Approach Reveals the Symmetry-Breaking Pathway to the Broken Helix in EuIn₂As₂, Phys. Rev. X 14, 031013 (2024).
- [5]M. Gen, Y. Fujishiro1, K. Okigami, S. Hayami, M. T. Birch1, K. Adachi, D. Hashizume, T. Kurumaji, H. Sagayama, H. Nakao, Y. Tokura1, and T. Hisa Arima, Incommensurate broken helix induced by nonstoichiometry in the axion insulator candidate EuIn₂As₂, Phys. Rev. B 111, L081109 (2025).
- [6]H. Takeda, J. Yan, Z. Jiang, X. Luo, Y. Sun, and M. Yamashita, Incommensurate magnetic order in an axion insulator candidate EuIn₂As₂ investigated by NMR measurement, npj Quantum Mater. 9, 67 (2024).
- [7]S. S. Sunku, T. Kong, T. Ito, P. C. Canfield, B. S. Shastry, P. Sengupta, and C. Panagopoulos, Hysteretic magnetoresistance and unconventional anomalous Hall effect in the frustrated magnet TbMn₆Sn₆, Phys. Rev. B 93, 174408 (2016).
- [8]H. Takahashi, K. Aono, Y. Nambu, R. Kiyanagi, T. Nomoto, M. Sakano, K. Ishizaka, R. Arita, and S. Ishiwata, Competing spin modulations in the magnetically frustrated semimetal EuCuSb, Phys. Rev. B 102, 174425 (2020).
- [9]J. Yan, Z. Z. Jiang, R. C. Xiao, W. J. Lu, W. H. Song, X. B. Zhu, X. Luo, Y. P. Sun, and M. Yamashita, Field-induced topological Hall effect in antiferromagnetic axion insulator candidate EuIn₂As₂, Phys. Rev. Res. 4, 013163 (2022).
- [10]C. Z. Chang, C. X. Liu, and A. H. MacDonald, Colloquium: Quantum anomalous Hall effect, Phys. Mod. Phys. 95, 011002 (2023).
- [11]G. Cuono, R. M. Sattigeri, C. Autieri, and T. Dietl, Ab initio overestimation of the topological region in Eu-based compounds, Phys. Rev. B 108, 075150 (2023).
- [12]N. A. A. Pari, R. Jaeschke-Ubiergo, A. Chakraborty, L. Šmejkal, and J. Sinova, Nonrelativistic linear Edelstein effect in helical EuIn₂As₂, Phys. Rev. B 112, 024404 (2025).
- [13]See Supplemental Material at [URL will be inserted by publisher] for results presenting the sample characterization (including Laue diffractogram, data on magnetization and electrical resistivity), magnetoresistance at the different magnetic field orientation, temperature variation of the Hall effect and carrier concentration, theoretical calculated electronic structure, anomalous Hall conductivity, intrinsic Hall resistivity, and evolution of the Fermi surface, and references [9, 11, 29, and 33-52] therein.
- [14]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, I. Dabo, et al., QUANTUM ESPRESSO: a modular and open-source software project for quantum simulations of materials, J. Phys.: Condens. Matter 21, 395502 (2009).
- [15]P. Grandini, A. Marrazzo, E. Castelli, N. Mounet, and N. Marzari, Precision and efficiency in solid-state pseudopotential calculations, npj Comput. Mater. 4, 72 (2018).
- [16]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett 77, 3865 (1996).
- [17]H. J. Monkhorst and J. D. Pack, Special points for Brillouin-zone integrations, Phys. Rev. B 13, 5188 (1976).
- [18]A. A. Mostofi, J. R. Yates, G. Pizzi, Y.-S. Lee, I. Souza, D. Vanderbilt, and N. Marzari, An updated version of wannier90: A tool for obtaining maximally-localised Wannier functions, Comput. Phys. Comm. 185, 2309 (2014).
- [19]X. Wang, J. R. Yates, I. Souza, and D. Vanderbilt, Ab initio calculation of the anomalous Hall conductivity by Wannier interpolation, Phys. Rev. B 74, 195118 (2006).
- [20]A. Liebman-Pelaez, V. S. Samuel J. Garratt, Y. Sun, J. R. Soh, D. Prabhakaran, A. T. Boothroyd, and J. Orenstein, Goldstone mode of the broken helix in U(1) magnet EuIn₂As₂ (2025), arXiv:2501.09084 [cond-mat.mtrl-sci].
- [21]D. C. Johnston, Magnetic structure and magnetization of helical antiferromagnets in high magnetic fields perpendicular to the helix axis at zero temperature, Phys. Rev. B 96, 104405 (2017).
- [22]T. Kurumaji, M. Gen, S. Kitou, H. Sagayama, A. Ikeda, and T. H. Arima, Anisotropic magnetotransport properties coupled with spiral spin modulation in a magnetic semimetal EuZnGe, Phys. Rev. Mater. 6, 094410 (2022).
- [23]T. Suzuki, L. Savary, J.-P. Liu, J. W. Lynn, L. Balents, and J. G. Checkelsky, Singular angular magnetoresistance in a magnetic nodal semimetal, Science 365, 377 (2019).
- [24]K. Ueda, J. Fujioka, B. J. Yang, J. Shigoi, A. Tsukazaki, S. Nakamura, S. Awaji, N. Nagaosa, and Y. Tokura, Magnetic Field-Induced Insulator-Semimetal Transition in a Pyrochlore Nd₂Ir₂O₇, Phys. Rev. Lett. 115, 056402 (2015).
- [25]K. Ueda, J. Fujioka, Y. Takahashi, T. Suzuki, S. Ishiwata, Y. Taguchi, M. Kawasaki, and Y. Tokura, Anomalous domain-wall conductance in pyrochlore-type Nd₂Ir₂O₇ on the verge of the metal-insulator transition, Phys. Rev. B 89, 075127 (2014).
- [26]G. G. Marcus, D. J. Kim, J. A. Tumalher, J. A. Rodriguez-Rivera, J. O. Birk, C. Niedermeyer, H. Lee, Z. Fisk, and C. L. Broholm, Multi- q Mesoscale Magnetism in CeAuSb₂, Phys. Rev. Lett 120, 097201 (2018).
- [27]Soonbeom Seo and Satoru Hayami and Ying Su and Sean M. Thomas and Filip Ronning and Eric D. Bauer and Joe D. Thompson and Shi Zeng Lin and Priscila F.S. Rosa, Spin-texture-driven electrical transport in multi-Q antiferromagnets, Commun. Phys. 4, 58 (2021).
- [28]N. Nagaosa, J. Sinova, S. Onoda, A. H. MacDonald, and N. P. Ong, Anomalous Hall effect, Rev. Mod. Phys. 82, 1539 (2010).
- [29]R. M. Fernandes, V. S. de Carvalho, T. Birol, and R. G. Pereira, Topological transition from nodal to nodeless Zeeman splitting in altermagnets, Phys. Rev. B 109, 024404 (2024).
- [30]T. M. R. Wolf, O. Zilberberg, I. Levkivskyi, and G. Blatter, Substrate-induced topological minibands in graphene, Phys. Rev. B 98, 125408 (2018).
- [31]A. K. Nguyen, R. V. Shchelushkin, and A. Brataas, Intrinsic domain-wall resistance in ferromagnetic semiconductors, Phys. Rev. Lett. 97, 136603 (2006).
- [32]K. Kobayashi, Y. Ominato, and K. Nomura, Helicity-Protected Domain-Wall Magnetoresistance in Ferromagnetic Weyl Semimetal, J. Phys. Soc. Jpn. 87, 073707 (2018).
- [33]A. A. Abrikosov, Quantum magnetoresistance, Phys. Rev. B 58, 2788 (1998).
- [34]A. A. Abrikosov, Quantum linear magnetoresistance, Europhys. Lett. 49, 789 (2000).
- [35]S. T. Michio Naito, Galvanomagnetic Effects in the Charge-Density-Wave State of 2H-NbSe₂ and 2H-TaSe₂, J. Phys. Soc. Jpn. 51, 228 (1982).
- [36]J. C. Song, G. Refael, and P. A. Lee, Linear magnetoresistance in metals: Guiding center diffusion in a smooth random potential, Phys. Rev. B 92, 180204(R) (2015).
- [37]R. Xu, A. Husmann, M.-L. S. T. F. Rosenbaum, J. E. Enderby, and P. B. Littlewood, Large magnetoresistance in non-magnetic silver chalcogenides, Nature 390, 57–60 (1997).
- [38]Y. Feng, Y. Wang, D. M. Silevitch, J.-Q. Yan, R. Kobayashi, M. Hedo, T. Nakama, Y. Onuki, A. V. Suslov, B. Mihaila, P. B. Littlewood, and T. F. Rosenbaum, Linear magnetoresistance in the low-field limit in density-wave materials, Proc. Natl. Acad. Sci. U.S.A. 166, 11201 (2019).
- [39]A. A. B. Barks, M. Dardanya, S.-M. Huang, B. Ghosh, C.-Y. Huang, H. Lin, A. Bansil, T.-R. Chang, A. Agarwal, and B. Singh, Magnetically tunable Dirac and Weyl fermions in the Zintl materials family, Phys. Rev. Mater. 6, 044204 (2022).
- [40]L. Šmejkal, J. Sinova, and T. Jungwirth, Beyond Conventional Ferromagnetism and Antiferromagnetism: A Phase with Non-relativistic Spin and Crystal Rotation Symmetry, Phys. Rev. X 12, 031042 (2022).
- [41]S. Hayami and H. Kusunose, Essential role of the anisotropic magnetic dipole in the anomalous Hall effect, Phys. Rev. B 103, L180407 (2021).
- [42]P. A. McClarty and J. G. Rau, Landau Theory of Altermagnetism, Phys. Rev. Lett. 132, 176702 (2024).
- [43]C. Autieri, R. M. Sattigeri, G. Guono, and A. Fakhredine, Staggered dyzalozinski-moriya interaction inducing weak ferro- magnetism in centrosymmetric altermagnets and weak ferrimagnetism in noncentrosymmetric altermagnets, Phys. Rev. B 111, 054442 (2025).
- [44]D. Santos-Cottin, I. Mohelský, J. Wyzula, F. Le Mardelé, I. Kapon, S. Nasrallah, N. Barišić, I. Živković, J. R. Soh, F. Guo, K. Rigaux, M. Puppin, J. H. Dil, B. Gudac, Z. Rukelj, M. Novak, A. B. Kuzmenko, C. C. Homes, T. Dietl, M. Orlita, and A. Akrap, EuCd₂As₂: A Magnetic Semiconductor, Phys. Rev. Lett. 131, 186704 (2023).
- [45]S. Chowdhury, K. F. Garrity, and F. Tavazza, Topological Phases of MnA₂X₄ (A=Bi, Sb; X = Se, Te) under Magnetic Field (2022), arXiv:2202.07061 [cond-mat.mtrl-sci].arxiv.org/abs/2202.07061
- [46]A. S. Wadge, G. Grabecki, A. Autieri, B. J. Kowalski, P. Iwanowski, G. Cuono, M. F. Islam, C. M. Canalì, K. Dybko, A. Hruban, A. Łukasowski, T. Wojciechowski, R. Diduszko, A. Lynnyk, N. Olszowska, M. Rosmus, J. Kołodziej, and A. Wiśniewski, Electronic properties of TaAs₂ topological semimetal investigated by transport and ARPES, J. Phys.: Condens. Matter 34, 125601 (2022).
- [47]T. C. van Thiel, W. Brzezicki, C. Autieri, J. R. Hortensius, D. Afanasiev, N. Gauquelin, D. Jannis, N. Janssen, D. J. Groenendijk, J. Fatermans, S. Van Aert, J. Verbeeck, M. Cuoco, and A. D. Caviglia, Coupling Charge and Topological Reconstructions at Polar Oxide Interfaces, Phys. Rev. Lett. 127, 127202 (2021).
- [48]C. A. Marques, L. C. Rhodes, I. Benedičíč, M. Naritsuka, A. B. Naden, Z. Li, A. C. Komarek, A. P. Mackenzie, and P. Wahl, Atomic-scale imaging of emergent order at a magnetic field–induced Lifshitz transition, Sci. Adv. 8, eabq7757 (2022).
- [49]M. Boukahil, A. Pourret, G. Knebel, D. Aoki, Y. Ōnuki, and J. Flouquet, Lifshitz transition and metamagnetism: Thermoelectric studies of CeRu₂Si₂, Phys. Rev. B 90, 075127 (2014).
- [50]M. Bercx and F. F. Assaad, Metamagnetism and Lifshitz transitions in models for heavy fermions, Phys. Rev. B 86, 075108 (2012).
- [51]B. S. Shivaram, L. Holleis, V. W. Ulrich, J. Singleton, and M. Jaime, Field Angle Tuned Metamagnetism and Lifshitz Transitions in UPt₃, Sci. Rep. 9, 8162 (2019).
- [52]A. McCollam, M. Fu, and S. R. Julian, Lifshitz transition underlying the metamagnetic transition of UPt₃, J. Phys.: Condens. Matter 33, 075804 (2020).