Abstract

The disentanglement of single and many particle properties in 2D semiconductors and their dependencies on high carrier concentration is challenging to experimentally study by pure optical means. We establish an electrolyte gated WS2 monolayer field-effect structure capable to shift the Fermi level from the valence into the conduction band suitable to optically trace exciton binding as well as the single particle band gap energies in the weakly doped regime. Combined spectroscopic imaging ellipsometry and photoluminescence spectroscopies spanning large n- and p-type doping with charge carrier densities up to 10^14 cm-2 enable to study screening phenomena and doping dependent evolution of the rich exciton manifold whose origin is controversially discussed in literature. We show that the two most prominent emission bands in photoluminescence experiments are due to the recombination of spin-forbidden and momentum-forbidden charge neutral excitons activated by phonons. The observed interband transitions are redshifted and drastically weakened under electron or hole doping. This field-effect platform is not only suitable for studying exciton manifold but is also suitable for combined optical and transport measurements on degenerately doped atomically thin quantum materials at cryogenic temperatures.

Introduction

Two-dimensional materials beyond graphene have attracted enormous interest because of their potential for application in several areas including (flexible) nano-opto-/electronics, catalysis, solar energy conversion, (bio-)sensing, spin- and valleytronics[1, 2, 3, 4, 5]. A rich variety of atomically thin materials including metals, semimetals, semiconductors, insulators, superconductors and topological insulators exist. Semiconducting transition metal dichalcogenides (TMDCs) are van der Waals (vdW) layered crystals of the form MX2_2 such as MoS2_2, WS2_2, MoSe2_2, WSe2_2. Those semiconducting TMDCs are the most explored two-dimensional materials post graphene thanks to their availability, stability, ease of processing and interesting physical properties[6]. In particular, semiconducting TMDCs feature unique optical and optoelectronic properties such as an exciton dominated optical response even at room temperature[7, 8, 9, 10], doping induced and presumably exotic superconductivity[11, 12, 13, 14], fascinating spin and valley properties up to room temperature[2] and pronounced interaction physics[15, 16, 17].

Interactions are not only relevant to study electron correlation phenomena and emergent quantum phases, but can also have a strong impact on the electronic band structure as well as on exciton physics and hence the optical properties. Reduced dimensionality together with reduced screening result in large exciton binding energies in the order of 0.5 eV in theses semiconducting TMDCs interfaced to insulators[8, 9, 10]. The attractive Coulomb interaction between the bound electron and hole in an exciton and as a consequence the exciton binding energy can be manipulated with external stimuli such as strain[18], its dielectric environment[19, 20], intense photoexcitation[21] or electron doping in field-effect structures[22, 23]. Such external stimuli can cause band renormalization effects counteracting the change in binding energy such that measured energies in optical interband experiments sensitive to the exciton ground states are only slightly changed with doping[24, 25]. Due to the mutual impact of external stimuli on single particle and excitonic properties, it is extremely difficult to disentangle them in all-optical experiments.

In a similar context, there is an ongoing debate in literature on the microscopic origin of the exciton manifold observed in the photoluminescence (PL) spectra of monolayer (ML) WS2_2 with the lowest interband transition spin-forbidden. The corresponding spectral features are assigned in different studies to recombination of direct excitons, momentum-forbidden and phonon activated excitons, trion species (charged exciton), defect related excitons and biexcitons[23, 26]. A better understanding of the effect of doping on exciton formation, on electric field induced renormalization of electronic bands, electron-electron and electron-phonon interaction is of great interest for the interpretation and the control of optical properties of WS2_2 monolayers. In addition, high electron densities in the order of 101410^{14} cm−2^{-2} are reported to result in the emergence of quantum phase transitions such as gate induced superconductivity in semiconducting TMDCs[13, 14] or even a light controllable electronic phase transition[27].

In order to study the electric field and doping induced impact on the band-gap, optical and emergent properties by all-optical means, an experimental platform is required that allows for an in-situ tuning of electric field and charge carrier density over a wide range from high electron to high hole doping compatible with optical absorption and emission experiments. Substitutional doping[28], chemical treatment[29] or surface evaporation of dopants[30] lacks in-situ tuning of the charge carrier density. The most suitable way is to embed WS2_2 ML in field-effect transistor (FET) structures using e.g. SiO2_2 or hBN layers as gate dielectric. However, the electric field strength achievable with those structures are limited and typically not suitable to shift EFE_F across the band gap for capacitance spectroscopy of the electronic bands and to inject high n−n- and p−p- type doping levels due to limitations of the gate dielectric. A successful strategy is the use of solid or liquid electrolyte gates allowing the injection of high charge carrier densities[31, 32].

In this paper, we report on the successful implementation of solid electrolyte gated WS2_2 MLs suitable to tune the Fermi energy EFE_F from the valence (VB) and conduction band (CB) edge and to study the evolution of exciton manifolds in WS2_2 in presence of charge carriers spanning a large electron and hole doping range up to 101410^{14} cm−2^{-2}. This field-effect platform allows direct optical access to the VB and CB edges of WS2_2 MLs. At the same time, spectroscopic imaging ellipsometry (SIE) provides access to the exciton ground and excited (Rydberg) states, enabling the estimation of exciton binding EbindE_{\mathrm{bind}} and the single particle gap energy EgapE_{\mathrm{gap}} and to trace their evolution while shifting the EFE_F from VB to CB. Both show clear maxima for EFE_F located in the middle of band gap. The corresponding values constitute Ebind≈400E_{\mathrm{bind}} \approx400 meV and Egap≈2.5±0.2E_{\mathrm{gap}} \approx2.5 \pm0.2 eV in agreement with reports in literature[8, 19]. Moreover, combined SIE and PL spectroscopies allow studying the rich exciton physics including higher lying exciton transitions in WS2_2 and their dependencies on the charge carrier polarity and density up to 101410^{14} cm−2^{-2}. We show that the two most prominent emission bands are due to the recombination of momentum- and spin-forbidden charge neutral excitons that are activated by phonons. A third red-shifted emission line appears in the presence of excess charge carriers and is assigned to charged excitons[21, 24]. For high nn- and pp- doping, the evolution of exciton manifolds as well as exciton dissociation (Mott transition)[33] is monitored. We discuss the rich PL spectra in the framework of different partially phonon activated charge neutral excitons, charged excitons, excitons dressed by a cloud of electrons or holes up to fully dissociated electron-hole pairs[17, 26, 34, 35, 36, 37].

Materials and Methods

Sample preparation

WS2_2 field-effect structures are prepared by micromechanical exfoliation and viscoelastic dry transfer of WS2_2 flakes (bulk crystals supplied by HQ graphene) on top of pre-patterned glass substrates (single sided polished BOROFLOAT® 33 borosilicate glass). The metal electrodes contacting the flakes and the electrolyte are patterned by evaporation of 5 nm chromium as adhesion layer followed by 80 nm gold through a shadow mask to avoid surface contamination from resist residues. As an electrolyte top gate, we use a solid polymer electrolyte consisting of poly-(ethylene oxide) and LiClO4_4 (ratio 8:1) dissolved in methanol and deposited by spin-coating using 8000 rpm followed by an annealing step on a hot plate. The process is optimized to get a homogeneous thin polymer electrolyte film with large domains important for optical measurements. For improved results, the thickness of a film for spectroscopic imaging ellipsometry (SIE) measurements shall be less than the wavelength of light in the media and the PE thickness was therefore kept in the order of 350 nm. The thickness of the electrolyte top gate was roughly doubled for PL measurements in order to enhance the long-term stability of the samples under illumination with high light intensities at room temperatures. Those thicker films are prepared by keeping the ion concentration constant. Only the amount of solvent with respect to the solid parts together with the spinning parameters are adjusted. In this way, the gate capacitance of the electric double layer transistor (EDLT) formed by the mobile ions on top of the WS2_2 layer is assumed to be independent from the film thickness. Nonetheless, minor variations are expected from sample to sample. The WS2_2-EDLT electrodes behave like a plate capacitor for a finite density of states in the WS2_2 sheet (meaning EFE_F inside CB or VB). We refer to this situation as regimes II for charge carrier densities <1013 cm−2< 10^{13}\,\mathrm{cm}^{-2} and regime III for densities >1013 cm−2> 10^{13}\,\mathrm{cm}^{-2}. The thickness of the double layer capacitor is in the order of very few nm resulting in an enormous gate capacitance per unit area. In regimes II and III, the capacitance of the investigated devices is approximated to Cg≈1.5 μF/cm−2C_g \approx1.5\,\mu\mathrm{F}/\mathrm{cm}^{-2} with a distance within the EDL in the order of 2-3 nm[31]. This correspond to a change in charge carrier density of roughly 1.25⋅1013 cm−21.25 \cdot10^{13}\,\mathrm{cm}^{-2} per applied volt. We would like to note that in order to avoid surface contamination negatively impacting particularly the modelling of the SIE spectra, the gold electrode is not covered by an insulating film, but in direct contact with the electrolyte such that charge accumulation or depletion as well as surface oxidation and reduction of the gold can occur[38]. In turn, the circuitry consists of two capacitive elements with the capacitance of the semiconducting WS2_2-EDLT electrode beeing changed for EFE_F inside EgapE_{gap} (regime I) and inside CB or VB (regimes II,III). It is not possible to use a reference electrode in our experiments since scattered and reflected light from such an electrode, in particular from the edges would render meaningful SIE investigations nearly impossible. For these reasons, the utilized geometry does not allow for quantitative capacitance spectroscopy providing direct access to the band-gap EgapE_{gap}[39], but still allows for a qualitative capacitance spectroscopy indicating the gate voltage required to shift EFE_F to the CB and VB edges. With EFE_F inside the CB or VB (regimes II and III), the WS2_2-EDLT can be well approximated as plate capacitor with the defined capacitance CgC_g. The impact from the Au-electrode interfacing the EDL on the estimated change in charge carrier density becomes negligible within the experimental uncertainty. Overall more than 8 samples have been prepared and studied and some of the samples have been intensely measured with several gate cycles. The displayed spectra and results are typical spectra achieved from those structures.

Electric control and functionality of the electrolyte gate

Electronic control over the gate potential during the optical measurements is realized by a source-measurement unit (Keysight Technologies). In order to minimize hysteresis effects, the top gate voltage is changed with a very slow scan rate of ≤3.3mVs−1\leq3.3\mathrm{mV}\mathrm{s}^{-1} for PL and 2mVs−12\mathrm{mV}\mathrm{s}^{-1} for SIE measurements, respectively. Leakage currents are monitored during the optical measurements to ensure stability of the gate. The gate voltage is swept at most between -13 V and 13 V. Even with this low scanning approach, well-known hysteresis effects due to low-mobile ions and (interfacially) trapped charges cannot be completely suppressed[39]. For this reason, the sweep direction and rate were kept constant in all measurements.

Spectroscopic Imaging Ellipsometry

Spectroscopic imaging ellipsometry (SIE) measurements are done with an imaging ellipsometer (accurion GmbH) using a supercontinuum white-light source with narrow tunable filters (both NKT Photonics GmbH) for illumination. The experiments are carried out at room temperature. In order to improve the stability of the field-effect structures during optical measurements, the samples are placed inside a home-built vacuum cell (vacuum p<10−3 mbarp < 10^{-3}\,\mathrm{mbar}) with windows suitable for SIE experiments in reflectance geometry using 55∘55^\circ as angle of incidence. The incident light is guided through a polarizer for linear polarization and then through a compensator to prepare elliptically polarized light. The reflected light is directed through an ultra-low NA objective (NA ≈0.01∘\approx0.01^\circ) to maintain nearly parallel light and imaged by an array detector after passing an analyzer. In a suitable coordinate system, the complex reflectance matrix is described by ρ=rp/rs=tan⁡Ψ⋅exp⁡iΔ\rho= r_p/r_s = \tan\Psi\cdot\exp i\Delta, where ρ\rho is the complex reflectance ratio, rpr_p and rsr_s are the amplitudes of the parallel (pp) and orthogonal (ss) components of the reflected light normalized to the amplitude of incoming light, Ψ\Psi and Δ\Delta are the ellipsometric angles. To describe the SIE spectra of the field-effect structures and to extract the dielectric functions of WS2_2 ML in dependence of the gate voltage, a comprehensive multilayer model consisting of substrate, interlayer, WS2_2 and electrolyte layer each described by a suitable combination of Cauchy and/or Lorentzian and/or Tauc-Lorentz terms is developed and fit to the experimental data via regression analysis[40, 41]. This regression analysis enables us to extract the dielectric functions of the WS2_2 layers for different gate voltages. To improve the accuracy, several regions on and off the WS2_2 layers have been investigated. By this approach, SIE measurements provide access to the dielectric function even if the imaginary part is largely suppressed by nearly fully screened excitons as it is the case for high doping densities. In this scenario, measurements of the absorption spectra from differential reflectance and extracting the dielectric functions by a Kramers Kroning analysis is no longer possible[42].

Photoluminescence spectroscopy

PL measurements are done with a home-built microscope set-up using free beam optics. The samples are placed on x-y-z piezo actuators for precise positioning and are excited with the green light of a solid-state diode laser emitting at 532nm. The excitation power is kept constant at around 50μW50\mu\mathrm{W}. The light is focused on the sample using a 50x magnification objective (Mitutoyo) resulting in a spot size with a diameter of less than 2μm2\mu\mathrm{m}. The emitted light is focused to the entrance slit of a single stage grating spectrometer (Princeton instruments) and the dispersed light is collected using a CCD. All optical measurements are carried out in vacuum (p<10−3mbarp < 10^{-3}\mathrm{mbar}) at room temperature.

Results

Optically detected band edges

The optical measurements on highly ambipolar doped WS2_2 monolayers are carried out on the optimized field-effect structures sketched in Figure 1a) that are suitable for gate-voltage dependent PL and SIE studies. The electronic double layer (EDL) provides high capacitance such that electric field tunability and charge carrier dependence of the absorption and emission spectrum over a wide range can be studied. The large geometrical gate capacitance allows to shift the chemical potential μ\mu and hence EFE_F through the band gap from the CB to the VB of WS2_2 and vice versa as schematically depicted in Figure 1b). In this way, exciton species can be studied in absence and presence of free charge carriers with varying polarity and density over a wide range [see Figure 1(b)].

Image not extracted

Figure 1. (a) Sketch of the 1L WS2_2 field-effect structure using a solid electrolyte gate electrode. (b) Schematic density of states N(E)N(E) and the single particle band structure close to the fundamental band-gap for a 2D semiconductor. Since the electrochemical potential μ\mu of the gate electrode is aligned with the Fermi level EFE_F of the WS2_2 semiconductor, EFE_F can be tuned by an applied gate voltage. (c) PL spectra in a false color representation for varying gate voltages VgV_g 13 V to -13 V. The emission intensity is color coded. When the chemical potential and hence EFE_F is aligned with the CB and VB edges, an enhanced emission intensity occurs. Intensity and lineshape is interpreted as interplay of screening and doping dependent behavior of the rich exciton manifolds in WS2_2 MLs. Inset: Integrated intensities for gate-up and down sweeps (hysteresis corrected). [T=300T = 300 K, λLaser=532\lambda_{\mathrm{Laser}} = 532 nm; P=50 μP = 50\,\muW]

The relation between exciton binding energy EbindE_{bind}, optical interband transition EoptE_{opt} and single particle band gap is Egap=Eopt+EbindE_{gap}=E_{opt}+E_{bind} as sketched in Figure 1(b). This relation does not directly allow the determination of EgapE_{gap} and EbindE_{bind} from optical interband emission or absorption measurements. The application of an electric field via the gate voltage VgV_g on the WS2_2 field-effect structure causes a shift of the chemical potential Δμ\Delta\mu of the gate with respect to the electronic band structure and a shift of the electrostatic potential ΔΦ=eΔn(p)/Cg\Delta\Phi=e\Delta n(p)/C_g with Δn(p)\Delta n(p) being the electrostatically induced change in electron (hole) densities and CgC_g the gate capacitance[31, 39]. The Fermi level EFE_F of the semiconductor aligns with the electrochemical potential μ\mu. Overall, we distinguish between three regimes regarding the position of EFE_F (equivalently μ\mu) relative to the band edges as indicated in Figure 1(b). In regime I, the Fermi level EFE_F of the semiconducting WS2_2 ML is located inside the single-particle band gap of WS2_2. Regime II and regime III correspond to EFE_F inside the CB or VB causing high and very high charge doping, respectively.

For regime I, the effect of the gate voltage on the change of the charge carrier density Δn(p)\Delta n(p) is negligible since the density of states N(E)N(E) inside the band gap of a pristine, defect free semiconductor is vanishingly small and as a direct consequence CgC_g becomes vanishingly small as well. Therefore, a change of the gate voltage in regime I causes a shift of μ\mu with eΔVg∝Δμe\Delta V_g\propto\Delta\mu allowing for a qualitative spectroscopy of the CB and VB edges of the semiconductor from the distinct change in the integrated intensity in PL due to Fermi-edge singularities when EFE_F is aligned to the CB or VB edges.[43]

Emission spectra in high-doping regime

In regime II, the chemical potential approaches the VB and CB band edges such that there are, in addition to thermally excited charge carriers, initial electrons (holes) electrostatically injected from the contact to the WS2_2 CB (VB). With further increase of the positive or negative gate voltage, the change of the electrostatic potential is no longer negligible since there is a high density of states NEN_E inside the CB and VB of the semiconductor such that the shift of the electrostatic potential ΔΦ=eΔn(p)/CG\Delta\Phi=e\Delta n(p)/C_G is dominating and large charge carrier densities even in the order of 1014 cm−210^{14}\,\mathrm{cm}^{-2} can be accumulated. Such a high density of itinerant charge carriers has a significant impact on the single particle level as well as on exciton species making an unambiguous prediction of the gate dependent evolution of the electronic and optical properties difficult.

Emission spectra in dependence of a wide range of gate voltages swept from 13V≤Vg≤−13V13\mathrm{V}\leq V_g\leq-13\mathrm{V} are plotted in Figure 1(c). The emission intensity is represented in a false color representation with high intensities displayed in yellow and low intensities in light violet, respectively. At Vg=0VV_g=0\mathrm{V} a bright emission line PL1 is centered around EPL1(0V)≈2eVE_{PL}^{1}(0\mathrm{V})\approx2\mathrm{eV} with a pronounced red tail featuring a substructure as will be discussed in more detail below. We note that the PL signature is corrected by a weak fluorescent background from the PE structure as displayed for the individual spectra in Fig. S1. PL1 remains bright and slightly redshifts with increasing gate voltage between 0V<Vg<7.5V0\mathrm{V}<V_g<7.5\mathrm{V}. The whole PL band significantly redshifts for Vg≤0VV_g\leq0\mathrm{V} and VG>7.5VV_G>7.5\mathrm{V} by transitioning from regimes II to regimes III for electron and hole doping, respectively. The redshift is particularly strong for electron doping (Vg<0V_g<0) and weaker for hole doping (Vg>0V_g>0). Moreover, the intensities reduce rapidly and vanish almost for high negative or high positive gate voltages [regime III(p+/n+p^+/n^+)]. The integrated intensities are plotted as a function of the effective gate voltage as inset in Figure 1(c) for the down-sweep from 13V to -13V and up-sweep from -5V to 13V. The observed and expected hysteretic behavior due to trapped charges and slow ions in the PE is corrected[39]. More information on the gate hysteresis and the corresponding spectra are provided in supplementary Fig. S2. We assign the gate voltage dependency of the PL spectra and in particular the local maxima in intensity around 0V and 7.5V to Fermi-edge singularities, when the chemical potential μ\mu is aligned with the CB edge for Vg≈0VV_g\approx0\mathrm{V} and with the VB edge for VG≈7.5VV_G\approx7.5\mathrm{V}. The intensity increase is interpreted as a result of an increased density of states close to the band edges. The absolute voltage required to shift the chemical potential μ\mu from the VB to the CB is within the uncertainty nearly the same for the up- and down-sweep [inset of Figure 1(c)].

Individual PL spectra are plotted in a waterfall representation in Figure 2(a) from the large nn-doped regime III(n+n^+) to an intermediate pp-doped regime II(p+p^+) from another gate sweep (different doping level at Vg=0VV_g=0\mathrm{V} compared to spectra in Figure 1 due to gate hysteresis). This additional measurement series confirms the overall trend that the main emission band is continuously redshifted in regime I and the overall intensities drop drastically for large electron and hole doping. A rich substructure is evident by displaying the individual spectra. A careful lineshape analysis reveals that the spectra can be well reproduced by a sum of 4 Gaussian (PL1-PL4) in the doped and highly doped regimes II and III, respectively, and by a sum of 3 Gaussian in the intrinsic (undoped) regime I. Exemplary spectra together with the individual Gaussians are shown for 12.6V [regime II(p+p^+)], 7.2V [regime I] and 1.2V [regime II(n+n^+)] in Figure 2(b-Figure 2d).

Image not extracted

Figure 2. (a) Water Fall representation of individual spectra for a gate voltage sweep from 0V to 13V clearly displaying changes in intensity and lineshape. (b)-(d) Line-shape analysis using a sum of 3 or 4 Gaussian reproducing the spectra for gate voltages of 12.6V [II(p)] (b), for 7.2V [I] (c) and of 1.2V [III(n+n^{+})] (d). Emission line PL3 is absent in the intrinsic regime. PL4 is assigned to defect related emission. (e) PL spectra for a WS2_2 ML encapsulated in hBN (green trace) and in hBN and few layer graphene (red trace). The graphene layer drains free charge carriers such that only charge neutral excitons contribute to the emission. The spectra reproduced by 2 or 3 Gaussians such that PL3 is asigned to trion and PL4 to defect emission (absent in encapsulated WS2_2). [T=300KT = 300K, λLaser=532nm\lambda_{Laser} = 532nm; P=50μWP = 50\mu W]

Additional vdW structures consisting of WS2_2 MLs encapsulated either on both sides with hBN or by hBN on one side and a few-layer graphene on the other side are prepared and studied in order to disentangle the individual contributions to the PL spectra and to assign them to charged excitons or interfacial disorder. The hBN encapsulation is known to suppress lineshape broadening due to interfacial inhomogeneities^{44}. The conducting graphene layer is reported to suppress trion emission by draining free charge carriers^{45}. By comparing the deconvoluted emission spectra from the PE gated WS2_2 with hBN and graphene interfaced WS2_2 layers it is evident that emission line PL3 is absent for the graphene supported layer [Figure 2(e)] and also absent for the PE gated sample for a gate voltage of 7.2V [regime I] with the EFE_F deep inside the band gap of WS2_2 [Figure 2(c)]. This leads to the conclusion that the emission line PL3 is due to charged excitons while emission lines PL1 and PL2 originate from charge neutral excitons. The fact that PL4 is absent in the hBN and graphene interfaced WS2_2 ML, but observable in the PE gated WS2_2 in the whole gate voltage range and PL4 is nearly independent from the gate-voltage suggests that the emission line PL4 is caused by interfacial inhomogeneities and excitons localized to trap states^{44}.

Doping dependent dielectric properties and Rydberg states

In order to develop an understanding of the origin of the multiplet emission signatures found for gated WS2_2 MLs and to determine values for EbindE_{bind} and EgapE_{gap} by measuring the exciton Rydberg series^{8}, SIE measurements on the WS2_2-FET structures with a thinner PE electrode are done. In Figure 3(a), spectra of the measured ellipsometric angles Ψ\Psi and Δ\Delta (dots) are plotted for the unbiased case. The solid lines are the corresponding fits to the measured data from regression analysis using a multilayer model^{40} and modeling the layer structure in a consecutive manner (Supplementary Fig. S4). Clear signatures for the AA and BB excitonic ground states A1sA_{1s} and B1sB_{1s}, respectively, and weaker but still observable signatures for the first excited A2sA_{2s} excitonic Rydberg state and the higher lying CC-excitonic band caused by band nesting^{8,40} are apparent in the bare spectra, even though the spectral evolution of the ellipsometric angles is a convolution of all contributing layers. Their spectral positions are indicated by the grey shaded regions in Figure 3(a). In our experience, all as prepared (unbiased) WS2_2-PE structures are moderately nn-type doped [corresponding to regime II(nn)] as also present in the data shown in Figure 1,Figure 2.

Image not extracted

Figure 3. (a) Spectra of the ellipsometric angles Δ\Delta and Ψ\Psi for WS2_2 – PE gate field-effect structure for the unbiased case (symbols). Solid line represents the fit to the model from regression analysis. The excitonic signatures are indicated. (b) Extracted A1s_{1s}, A2s_{2s} and B exciton energies in dependence of positive gate voltages 0V≤Vg≤12V0\mathrm{V} \le V_g \le12\mathrm{V} moving EFE_F from the CB into the band gap to the VB edge. [T = 300K] (c) Extinction coefficient κ(E)\kappa(E) extracted from SIE for unbiased, Vg=1VV_g = 1\mathrm{V} and Vg=−4VV_g = -4\mathrm{V} corresponding to weak [II(n)], moderate [III(n+^+)] and high electron doping [III(n++^{++})], respectively. A1s_{1s}, A2s_{2s}, B and C exciton signatures are indicated. (d) VgV_g dependent evolution of exciton binding energies determined from the energy difference between A1s_{1s} and A2s_{2s} (red) and single particle band gap (black) considering nonlocal screening [upper and lower limit as explained in the text].

The approach and the multilayer model used for fitting the ellipsometric data are identical for the unbiased and biased measurements. The multilayer model consists of glass substrate, interlayer, WS2_2 ML, thin film PE electrode and air. As expected, only the dielectric function of WS2_2 is strongly dependent on the gate voltage^{46}. The dielectric functions and equivalently refractive index n(E)n(E) and extinction coefficient κ(E)\kappa(E) - with the latter being directly proportional to the absorption α(E)\alpha(E) - are extracted from the multilayer model for all investigated gate voltages. The extinction coefficient κ(E)\kappa(E) for increasing nn-type doping is plotted in Figure 3(b) for unbiased, Vg=−1VV_g = -1V and Vg=−4VV_g = -4V corresponding to slightly nn-doped [II(nn)], moderately nn-doped [III(n+n^{+})] and highly nn-doped [III(n++n^{++})] regimes, respectively. In regimes II and III, we assume the change in the charge carrier density to be in the order of Δn(1V)≈1.25⋅1013cm−2\Delta n(1\mathrm{V}) \approx1.25 \cdot10^{13}\mathrm{cm}^{-2} per applied volt between gate-electrode and WS2_2 as defined in the method section. We find that with increasing electron density nn, the A1s_{1s} exciton resonance broadens and completely vanishes for Vg=−4VV_g = -4\mathrm{V} (n++^{++}) similar to the excited A2s_{2s} state that is already unresolvable at Vg=−1VV_g = -1\mathrm{V} (n+^+) indicating the dissociation of the A exciton. The width of the B1s_{1s} exciton resonance is less affected for a moderate increase of the electron density[46], but vanishes as well for high electron doping n++^{++}. Only the C-exciton band remains nearly unaffected from doping what is not surprising since it originates from higher-lying interband excitations with contributions from states between Γ\Gamma and MM point that are far away from the occupied CB states[40]. The observed evolution of the absorption spectra with electron doping can be well understood in terms of the interaction of the bound exciton states with the increasing density of mobile electrons that screens the attractive Coulomb interaction[47]. For moderate doping, the formation of Mahan excitons, “dressed” excitons (exciton in a Fermi sea) and polarons is discussed in literature[48, 49, 50, 51]. For high and highest doping [III(n++^{++}/n+^+, p++^{++})], a Mott-transition to a weakly interacting electron and hole plasma is expected[47]. The occurrence of the Mott-transition in the highly doped regime is debated in literature[48]. Here, we assume the absence of A and B excitons resonances in the highly n-doped regime [III(n++^{++})] as clear indication for transition into the Mott-regime[21, 33].

For positive gate-voltages 0V≤Vg≤12V0\mathrm{V} \le V_g \le12\mathrm{V} signatures for the exciton ground states A1s_{1s} and B1s_{1s} as well as for the first excited exciton state A2s_{2s} are clearly visible in the ellipsometry spectra and well quantified in the extracted dispersion function from regression analysis. The extracted energies for the three lowest exciton signatures as a function of gate-voltage (mainly regime I and partially covering regime II) are summarized in Figure 3(c). The separation between A1s_{1s} and B1s_{1s} excitons is independent of the applied gate voltage and constitutes about 370±20370\pm20 meV. It originates from the spin-orbit split valence bands at the KK, K′K' points and agrees well with literature[47]. There is a slight redshift of the A and B exciton energies of about 40meV with increasing gate voltages from 0V to 12V that covers regimes I and II(n/p). A similar redshift has been observed for the main emission line [see Figure 1(c)]. From the energy difference ΔE12\Delta E_{12} between the exciton ground state A1s_{1s} and the first excited state A2s_{2s}, the exciton binding energy can be deduced from the hydrogenic Rydberg series considering a finite degree of nonlocal screening of the attractive Coulomb interaction between electron and hole because of inhomogeneous dielectric environment normal to the 2D layer. Assuming fully non-hydrogenic scaling, the binding energy constitutes Ebind=2⋅ΔE12E_{\mathrm{bind}} = 2 \cdot\Delta E_{12} and for hydrogenic scaling Ebind=9/8⋅ΔE12E_{\mathrm{bind}} = 9/8 \cdot\Delta E_{12} providing an upper and lower bound of EbindE_{\mathrm{bind}}[19, 47]. The actual value for EbindE_{\mathrm{bind}} is expected within these boundaries and depends on the dielectric screening of substrate and capping PE layer as well as on the doping density in the 2D semiconductor[19]. In the present case, the maximum in the binding energy is found for Vg=4 VV_g = 4\,\mathrm{V} to be in the range between Ebin=0.5 VE_{\mathrm{bin}} = 0.5\,\mathrm{V} and 0.25 eV0.25\,\mathrm{eV} for scaling factors 2 and 9/89/8, respectively [c.f. Figure 3(d)]. The values for the single particle band gap EgapE_{\mathrm{gap}} can then be deduced from the relation

Egap=EA1s+Ebind.E_{\mathrm{gap}} = E_{\mathrm{A}_{1s}} + E_{\mathrm{bind}}.

We find that the binding energy first increases from 0 V0\,\mathrm{V} to ≈4 V\approx4\,\mathrm{V} and decreases again for larger gate voltages as depicted in Figure 3(d). These findings allow for the conclusion that for the investigated structure the chemical potential and hence EFE_F is centered in the middle of the band gap of WS2_2 for Vg≈4 VV_g \approx4\,\mathrm{V} in agreement with emission spectroscopy. EFE_F approaches the CB edge for lower gate voltages and the VB edge for larger voltage such that screening is already slightly increased by thermally excited charge carriers as well as by initially injected carriers. The extracted gap energies are 2.27±0.1 eV2.27 \pm0.1\,\mathrm{eV} and 2.47±0.1 eV2.47 \pm0.1\,\mathrm{eV}, respectively. The binding energy is reduced by about 15% for slight nn-doping and reduced up to about 35% for moderate pp-doping in the experimentally accessible range. For higher doping the A2s_{2s} exciton is no longer well resolved in SIE measurements.

Discussion

We start the discussion with a classification of the different PL emission lines. The gate voltage dependent integrated PL intensities, energies of the emission lines PL1, PL2, PL3 from the deconvolution with Gaussian profiles (c.f. Figure 2) as well as the relative peak intensities are summarized in Figure 4(a-Figure 4c). The measurements are done by sweeping the gate voltage from −6 V≤Vg≤+13 V-6\,\mathrm{V} \le V_g \le+13\,\mathrm{V} (c.f. upsweep in inset of Figure 1(c)). The energies of the absorption peak A1s_{1s} from SIE investigation are included in Figure 4(b) even though the voltage induced charge carrier densities are expected to slightly differ since the measurements are done on different samples. The sweep direction of the gate voltage was identical across the measurements to reduce the impact of the hysteretic effect of the PE gate electrode. We would like to note that the position of EFE_F for the unbiased case changes moderately from sample to sample allowing only a qualitative comparison. Nevertheless, the assignment to different regimes is reliable and is nicely confirmed by the gate dependence of the dielectric properties. While showing nearly the same gate voltage dependence, the energies of A1s_{1s} and PL1 differs independent from the applied gate voltage VgV_g by about 30 meV. This energy difference is robust and has been confirmed by PL and SIE measurements on several samples with and without PE gate electrode. By cooling the WS2_2 ML to 77 K, also a weak blue-shifted emission line appears about 30 meV from the main emission line PL1 (see Fig. S3). The peak energies are compared in Table I for specific gate voltage values corresponding to EFE_F centered in the middle of the band gap [I], EFE_F aligned with CB and VB edges [II(n/pn/p)] and for high electron and hole doping n+/p+≈5⋅1013 cm−2n^+/p^+ \approx5 \cdot10^{13}\,\mathrm{cm}^{-2} [III(n+/p+n^+/p^+)]. There are no values for A1s_{1s} in the high n+n^+ and p+p^+ doped regions because of the screening induced weak absorption intensities. The nearly

Image not extracted

Figure 4. (a) Integrated emission intensities as a function of gate voltages from −5 V≤Vg≤13 V-5\,\mathrm{V} \le V_g \le13\,\mathrm{V} from the spectra displayed in 2(a). The maxima indicate voltage values for which EFE_F is aligned to CB and VB edges. The different doping regimes are highlighted. (b) Peak energies of the line-shape analysis using Gaussian profiles as a function of gate voltages for emission lines PL1, PL2 and PL3. The grey circles are the A1s_{1s} energies from SIE measurements. Since the measurements were done on two different samples, the effective electric field transferred by the gate voltage is expected to slightly differ. (c) Intensities of the emission lines shown in (b) normalized to the integrated emission energies shown in (a).

EFE_F/dopingA1s_{1s} (eV)PL1 (eV)PL2 (eV)PL3 (eV)
n+n^+ (≈5⋅1013 cm−2\approx5 \cdot10^{13}\,\mathrm{cm}^{-2})-1.991.951.92
EF≈ECBE_F \approx E_{CB}2.042.011.9751.96
EF≈ECBE_F \approx E_{CB}2.031.991.95-
EF≈EVBE_F \approx E_{VB}2.011.981.941.92
p+p^+ (≈5⋅1013 cm−2\approx5 \cdot10^{13}\,\mathrm{cm}^{-2})-1.981.941.91

Table 1. Energies of exciton species found in PL and SIE measurements for selected doping concentrations and positions of the Fermi-energy EFE_F. The uncertainty in the determination of the energies is in the order of ten meV.

gate voltage independent energy differences between A1s_{1s} and PL1 constitute 30 to 40 meV and between PL1 and PL2 about 40 meV. Emission line PL3 exhibits a significantly different behavior and vanishes if EFE_F is centered in the band gap. The energy difference between PL2 and PL3 increases with increasing pp and nn doping up to 30 meV for doping densities of about (n+/p+≈5⋅1013 cm−2)(n^+/p^+ \approx5 \cdot10^{13}\,\mathrm{cm}^{-2}).

The fact that the emission lines PL1–PL3 observed at room temperature do not appear in the absorption spectra determined from SIE and are redshifted in energy with respect to the A1s_{1s} peak is a strong evidence for their spin or momentum indirect nature. This points to the involvement of phonons in the recombination process of the associated excitons. Moreover, PL3 is absent in the emission spectra for the charge neutral situation either realized by gate-tuning EFE_F inside the band-gap [regime I] (Figure 4) or by using supporting graphene as a trion filtering layer[45] (c. f. Figure 2). The interpretation of PL3 as trion is supported by the fact that its relative intensity is significantly enhanced in regimes II(nn) and II(pp) and becomes the most intense emission line for increasing doping densities in regimes III(n+n^+) and III(p+p^+) [Figure 4(c)].

We now turn to the interpretation of the two remaining charge neutral phonon assisted emission lines PL1 and PL2. At the lowest energy direct interband transition at the KK, K′K' points, the lowest CB and VB states have opposite spins (see sketch in Figure 5). This optical interband transition is therefore spin-forbidden and hence dark excitons are generated by optical excitation that can only recombine by emitting or absorbing a suitable phonon connecting KK and K′K' valleys in order to mediate momentum conservation. The energy difference between the spin-forbidden “dark” state and spin-allowed “bright” transition from the highest VB state to the spin-split CB state at the KK, K′K' valleys is about 30 meV[47]. This nicely coincides with the energy separation between A1s_{1s} and PL1. Following this argumentation, PL1 is a phonon assisted emission from an exciton formed between the spin-split CB and the VB at the K′/KK'/K points. The remaining peak PL2 is interpreted as phonon-activated transition between the Σ\Sigma-valley in the CB and the KK-valley in the VB. The interpretation that all emission bands observed in room temperature PL experiments are phonon activated spin/momentum indirect transitions are corroborated by the spectrum of the extinction coefficient κ(E)\kappa(E) (Figure 3c) and low-temperature PL measurements (Fig. S3) and in agreement with some experimental and theoretical reports in literature[17, 26, 36, 52].

Image not extracted

Figure 5. Schematic representation of the exciton formed by holes (red spheres) residing in the KK valley and electrons (blue spheres) residing in KK, K′K' and Σ\Sigma valleys that are interpreted to originate B1s_{1s}, A1s_{1s}, PL1 and PL2, respectively.

By tuning EFE_F from the CB edge through the band-gap to the VB edge, the peak energies of the prominent charge neutral excitonic features B1s_{1s}, A1s_{1s}, PL1 and PL2 are monotonously redshift by about 35±535 \pm5 meV between ECBE_{CB} and EVBE_{VB} [see Figure 1c, Figure 2a, Figure 3b, Figure 4b]. There are no electron or only weak charge doping in the relevant regime I, so that we do not expect doping induced band renormalization phenomena. The exciton binding energies of the A1s_{1s} state in this regime are first slightly increased until EFE_F is centered in the band-gap and is then again reduced (Figure 3d). We assume that the monotonous reduction of the transition energies with gate voltage is caused by the different action on the electric field to the orbital states for the relevant CB and VB states[52].

The reduction of the peak energies of PL1, PL2 and PL3 emission lines transitioning from the weakly doped II(nn) regime into the highly electron-doped III(n+n^+) regime can be explained by a combination of doping induced band renormalization and screening effects[52]. Band renormalization effects are highly sensitive to the orbital contributions of the Bloch states at the different high-symmetry points in the 1st Brillouin Zone (BZ)[52].

Assuming kk-dependent renormalization, we can explain that the PL2 emission energies redshift already at a gate voltage of Vg≈1.4V_g \approx1.4 V, while for PL1 the redshift is less pronounced and starts at Vg=1V_g = 1 V in the data set analyzed in Figure 4 because for PL2 the electrons are hosted in the Σ\Sigma-valley, while for PL1 in the KK-valley. Since those emission lines are phonon activated, doping induced phonon renormalization and altered electron-phonon interaction might serve as an additional factor for the gate-dependent evolution of the emission spectra[53, 54].

The evolution of the emission energies for larger electron-doping with increasing negative gate voltages can be understood in terms of compensation of doping induced band renormalization and Coulomb screening lowering EgapE_{gap} and EbindE_{bind} such that the optical transition energies Eopt=Egap−EbindE_{opt} = E_{gap} - E_{bind} remains nearly constant within the experimental resolution[24]. For larger doping densities [III(n++n^{++})], the doping induced screening results in a Mott transition to an electron and hole plasma. This is in agreement with the experimental observation that the PL emission intensity is drastically reduced.

Conclusions

In conclusion, we successfully demonstrated optically detected capacitance spectroscopy of CB and VB edges of WS2_2 MLs realized by a solid-electrolyte gate field-effect structure. The exciton binding EbindE_{bind} and the single particle gap EgapE_{gap} energies determined by analyzing the excitonic Rydberg series from SIE investigations are maximized for EFE_F roughly centered inside the band gap (undoped situation) and constitute Ebind≈0.5E_{bind} \approx0.5 eV and Egap≈2.5E_{gap} \approx2.5 eV, respectively. The method is applicable to other optically active 2D materials. Moreover, we demonstrated ambipolar tunability of the charge carrier density in WS2_2 ML from high nn-type to a pp-type doping exceeding doping level required to induce exciton Mott transition. The gate voltage dependent study of both PL and SIE measurements allowes to assign the dominant emission features to spin- and momentum- forbidden transitions and provide further evidence for this interpretation in comparison with PL spectra from graphene/WS2_2/hBN and hBN/WS2_2/hBN structures. At low charge carrier densities and for the undoped situation, these spin and momentum indirect transitions dominate the optical response. We find that for EFE_F close to the CB and VB edges [regime II(n/pn/p)], charged excitons also contribute to the emission spectrum, while in highly doped regimes the emission signatures are interpreted to originate from an unbound electron hole plasma. In this context, SIE measurements demonstrated that strong exciton resonances occur for regimes [I] and [II(n/pn/p)], while large charge carrier densities result in screening induced reduction and disappearance of exciton resonances in the absorption expressed by the extinction coefficient κ(E)\kappa(E). Our work thus highlights rich physics and tunability of the optical properties of WS2_2 ML embedded in electrolyte gated field-effect structures. This platform is of high relevance for both fundamental understanding and its potential for implementation in quantum devices.

Supplementary Material

The following supporting information can be downloaded: Photoluminescence measurement including fig:S1: Raw gate voltage dependent PL spectra; fig:S2:H fig:S3: Hysteresis in gate voltage dependent measurements; fig:S3: Temperature dependence of a WS2_2 ML; tbl:S1: Fit values of semi-empirical Varshni fits of temperature dependent optical bandgaps extracted from PL peak positions. Spectroscopic imaging ellipsometry; fig:S4: Ellipsometry spectra of different layer structures.

Acknowledgments

We gratefully acknowledge fruitful discussion with Tim O. Wehling. This research was funded by the Deutsche Forschungsgemeinschaft (DFG) through SPP2244 and WU 637/7-1.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

References

References

  1. [1]D. Akinwande, N. Petrone, and J. Hone, Nature communications 5, 1 (2014).
  2. [2]K. F. Mak and J. Shan, Nature Photonics 10, 216 (2016).
  3. [3]N. Briggs, S. Subramanian, Z. Lin, X. Li, X. Zhang, K. Zhang, K. Xiao, D. Geohegan, R. Wallace, L.-Q. Chen, et al., 2D Materials 6, 022001 (2019).
  4. [4]A. Bolotsky, D. Butler, C. Dong, K. Gerace, N. R. Glavin, C. Muratore, J. A. Robinson, and A. Ebrahimi, Acs Nano 13, 9781 (2019).
  5. [5]S. Michaelis de Vasconcellos, D. Wigger, U. Wurstbauer, A. W. Holleitner, R. Bratschitsch, and T. Kuhn, physica status solidi (b) 259, 2100566 (2022), https://onlinelibrary.wiley.com/doi/pdf/10.1002/pssb.202100566.
  6. [6]S. Manzeli, D. Ovchinnikov, D. Pasquier, O. V. Yazyev, and A. Kis, Nature Reviews Materials 2, 1 (2017).
  7. [7]C. Zhang, A. Johnson, C.-L. Hsu, L.-J. Li, and C.-K. Shih, Nano letters 14, 2443 (2014).
  8. [8]A. Chernikov, T. C. Berkelbach, H. M. Hill, A. R. Rigosi, Y. Li, O. B. Aslan, D. R. Reichman, M. S. Hybertsen, and T. F. Heinz, Physical review letters 113, 076802 (2014).
  9. [9]Z. Ye, T. Cao, K. O’Brien, H. Zhu, X. Yin, Y. Wang, S. G. Louie, and X. Zhang, Nature 513, 214 (2014).
  10. [10]M. M. Ugeda, A. J. Bradley, S.-F. Shi, F. H. da Jornada, Y. Zhang, D. Y. Qiu, W. Ruan, S.-K. Mo, Z. Hussain, Z.-X. Shen, et al., Nature materials 13, 1091 (2014).
  11. [11]J. Ye, Y. J. Zhang, R. Akashi, M. S. Bahramy, R. Arita, and Y. Iwasa, Science 338, 1193 (2012).
  12. [12]D. Costanzo, H. Zhang, B. A. Reddy, H. Berger, and A. F. Morpurgo, Nature nanotechnology 13, 483 (2018).
  13. [13]E. Piatti, D. De Fazio, D. Dagher, S. R. Tamalampudi, D. Yoon, A. C. Ferrari, and R. S. Gonnelli, Nano letters 18, 4821 (2018).
  14. [14]J. Lu, O. Zheliuk, O. Chen, I. Leermakers, N. E. Hussey, U. Zeitler, and J. Ye, Proceedings of the National Academy of Sciences 115, 3551 (2018).
  15. [15]B. Miller, J. Lindlau, M. Bommert, A. Neumann, H. Yamaguchi, A. Holleitner, A. Högele, and U. Wurstbauer, Nature communications 10, 1 (2019).
  16. [16]A. Raja, M. Selig, G. Berghäuser, J. Yu, H. M. Hill, A. F. Rigosi, L. E. Brus, A. Knorr, T. F. Heinz, E. Malic, et al., Nano letters 18, 6135 (2018).
  17. [17]E. Malic, M. Selig, M. Feierabend, S. Brem, D. Christiansen, F. Wendler, A. Knorr, and G. Berghäuser, Physical Review Materials 2, 014002 (2018).
  18. [18]I. Niehues, R. Schmidt, M. Druppel, P. Marauhn, D. Christiansen, M. Selig, G. Berghäuser, D. Wigger, R. Schneider, L. Braasch, et al., Nano letters 18, 1751 (2018).
  19. [19]A. Raja, A. Chaves, J. Yu, G. Arefe, H. M. Hill, A. F. Rigosi, T. C. Berkelbach, P. Nagler, C. Schüller, T. Korn, et al., Nature communications 8, 1 (2017).
  20. [20]Y. Kajino, K. Oto, and Y. Yamada, The Journal of Physical Chemistry C 123, 14097 (2019).
  21. [21]A. Chernikov, C. Ruppert, H. M. Hill, A. F. Rigosi, and T. F. Heinz, Nature Photonics 9, 466 (2015).
  22. [22]A. Chernikov, A. M. Van Der Zande, H. M. Hill, A. F. Rigosi, A. Veluthapillai, J. Hone, and T. F. Heinz, Physical review letters 115, 126802 (2015).
  23. [23]X. He, Z. Zhang, C. Zhang, Y. Yang, M. Hu, W. Ge, and X. Zhang, Applied Physics Letters 113, 013104 (2018).
  24. [24]Z. Qiu, M. Trushin, H. Fang, I. Verzhbitskyi, S. Gao, E. Laksono, M. Yang, P. Lyu, J. Li, J. Su, et al., Science advances 5, eaaw2347 (2019).
  25. [25]S. Ulstrup, A. G. Cabo, J. A. Miwa, J. M. Riley, S. S. Grønborg, J. C. Johannsen, C. Cacho, O. Alexander, R. T. Chapman, E. Springate, et al., ACS nano 10, 6315 (2016).
  26. [26]26 D. Bao, A. G. Del Águila, T. T. H. Do, S. Liu, J. Pei, and Q. Xiong, 2D Materials 7, 031002 (2020).
  27. [27]27 M. Qin, X. Han, D. Ding, R. Niu, Z. Qu, Z. Wang, Z.-M. Liao, Z. Gan, Y. Huang, C. Han, et al., Nano letters 21, 6800 (2021).
  28. [28]28 J. Suh, T.-E. Park, D.-Y. Lin, D. Fu, J. Park, H. J. Jung, Y. Chen, C. Ko, C. Jang, Y. Sun, et al., Nano letters 14, 6976 (2014).
  29. [29]29 S. Mouri, Y. Miyauchi, and K. Matsuda, Nano letters 13, 5944 (2013).
  30. [30]30 H. Fang, M. Tosun, G. Seol, T. C. Chang, K. Takei, J. Guo, and A. Javey, Nano letters 13, 1991 (2013).
  31. [31]31 I. Gutiérrez-Lezama, N. Ubrig, E. Ponomarev, and A. F. Morpurgo, Nature Reviews Physics 3, 508 (2021).
  32. [32]32 S. K. Fullerton-Shirey and J. K. Maranas, Macromolecules 42, 2142 (2009).
  33. [33]33 A. Steinhoff, M. Florian, M. Rösner, G. Schönhoff, T. O. Wehling, and F. Jahnke, Nature communications 8, 1 (2017).
  34. [34]34 M. Zinkiewicz, T. Wozniak, T. Kazimierczuk, P. Kapucinski, K. Oreszczuk, M. Grzeszczyk, M. Bartos, K. Nogajewski, K. Watanabe, T. Taniguchi, et al., Nano letters 21, 2519 (2021).
  35. [35]35 J. Madeo, M. K. Man, C. Sahoo, M. Campbell, V. Pareek, E. L. Wong, A. Al-Mahboob, N. S. Chan, A. Karmakar, B. M. K. Marisella, et al., Science 370, 1199 (2020).
  36. [36]36 R. Wallauer, R. Perea-Causin, L. Münster, S. Zajusch, S. Brem, J. Güdde, K. Tanimura, K.-Q. Lin, R. Huber, E. Malic, et al., Nano Letters 21, 5867 (2021).
  37. [37]37 A. Arora, N. K. Wessling, T. Deilmann, T. Reichenauer, P. Steeger, P. Kossacki, M. Potemski, S. M. de Vasconcellos, M. Rohlfing, and R. Bratschitsch, Physical Review B 101, 241413 (2020).
  38. [38]38 T. A. Petach, M. Lee, R. C. Davis, A. Mehta, and D. Goldhaber-Gordon, Phys. Rev. B 90, 081108 (2014).
  39. [39]39 D. Braga, I. Gutierrez Lezama, H. Berger, and A. F. Morpurgo, Nano letters 12, 5218 (2012).
  40. [40]40 S. Funke, B. Miller, E. Parzinger, P. Thiesen, A. Holleitner, and U. Wurstbauer, Journal of Physics: Condensed Matter 28, 385301 (2016).
  41. [41]41 U. Wurstbauer, B. Miller, E. Parzinger, and A. W. Holleitner, Journal of Physics D: Applied Physics 50, 173001 (2017).
  42. [42]42 Y. Li, A. Chernikov, X. Zhang, A. Rigosi, H. M. Hill, A. M. Van Der Zande, D. A. Chenet, E.-M. Shih, J. Hone, and T. F. Heinz, Physical Review B 90, 205422 (2014).
  43. [43]43 H. M. Hill, A. F. Rigoski, K. T. Rim, G. W. Flynn, and T. F. Heinz, Nano letters 16, 4831 (2016).
  44. [45]45 E. Lorchat, L. E. P. López, C. Robert, D. Lagarde, G. Froehlicher, T. Taniguchi, K. Watanabe, X. Marie, and S. Berciaud, Nature Nanotechnology 15, 283 (2020).
  45. [46]46 V. G. Kravets, F. Wu, G. H. Auton, T. Yu, S. Imaizumi, and A. N. Grigorenko, npj 2D Materials and Applications 3, 1 (2019).
  46. [47]47 G. Wang, A. Chernikov, M. M. Glazov, T. F. Heinz, X. Marie, T. Amand, and B. Urbaszek, Reviews of Modern Physics 90, 021001 (2018).
  47. [48]48 A. Schleife, C. Rödl, F. Fuchs, K. Hannewald, and F. Bechstedt, Physical review letters 107, 236405 (2011).
  48. [49]49 T. Palmieri, E. Baldini, A. Steinhoff, A. Akrap, M. Kollár, E. Horváth, L. Forró, F. Jahnke, and M. Chergui, Nature communications 11, 1 (2020).
  49. [50]50 M. Sidler, P. Back, O. Cotlet, A. Srivastava, T. Fink, M. Kroner, E. Demler, and A. Imamoglu, Nature Physics 13, 255 (2017).
  50. [51]51 F. Caruso, P. Amsalem, J. Ma, A. Aljarb, T. Schultz, M. Zacharias, V. Tung, N. Koch, and C. Draxl, Phys. Rev. B 103, 205152 (2021).
  51. [52]52 D. Erben, A. Steinhoff, C. Gies, G. Schönhoff, T. Wehling, and F. Jahnke, Physical Review B 98, 035434 (2018).
  52. [53]53 Y. Ge and A. Y. Liu, Physical Review B 87, 241408 (2013).
  53. [54]54 B. Miller, E. Parzinger, A. Vernickel, A. W. Holleitner, and U. Wurstbauer, Applied Physics Letters 106, 122103 (2015).

Paper details

vlnc:W_8puvdz5x
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents