The spontaneous exchange bias effect in La2-xCaxCoMnO6 series

Abstract

Structural, electronic and magnetic properties of polycrystalline La2-xCaxCoMnO6 (0 ≤\leq x ≤\leq 0.75) compounds are investigated by x-ray diffraction and magnetometry. All the samples have an orthorhombic structure and show a slight decrease in the unit cell with Ca-doping. Temperature-dependent magnetization measurements reveal a complex magnetic behavior with two ferromagnetic transitions. These transitions are ascribed to Co2+–Mn4+ and Co3+–Mn3+ couplings and suggest the presence of additional antiferromagnetic couplings in these disordered compounds. Field-dependent magnetization curves, measured after cooling the samples in a zero external magnetic field, reveal the spontaneous exchange bias (SEB) effect for the Ca-doped samples. The strengthening of the uncompensated magnetic coupling at the interfaces, caused by the increased antiferromagnetic phase, explains the increase of SEB with increasing the Ca-content.

INTRODUCTION

Oxide perovskites are at the frontline of materials research. Its structural flexibility allows the accommodation of several distinct elements on its general formula ABO3\mathrm{ABO}_{3} [A = alkaline-/rare-earth; B = transition metal (TM)]. This flexibility gives rise to thousands of different compounds already synthesized, many of them displaying properties of fundamental and practical interest, such as superconductivity [1], half-metallicity [2] and multiferroicity [3]. The manganites AMnO3\mathrm{AMnO}_{3} are by far the most investigated perovskites due to their metal-insulator transition, accompanied by colossal magnetoresistance [4]. The intense research on La1−xAxMnO3\mathrm{La}_{1-x}\mathrm{A}_{x}\mathrm{MnO}_{3} mixed-valence manganites has led to the formulation of critical physical concepts as double-exchange interactions and Jahn-Teller polarons. [5]. The cobaltites, ACoO3A\mathrm{CoO}_{3}, are also of great significance because the delicate balance between the crystal field splitting and interatomic Coulomb repulsion for Co electrons in octahedral coordination can lead to distinct spin states for this ion in perovskites, say high spin (HS), low spin (LS) or even intermediate spin (IS) configuration [6]. LaCoO3\mathrm{LaCoO}_{3} for instance exhibits temperature-induced spin-state transition [7], while hole-doped La1−xSrxCoO3\mathrm{La}_{1-x}\mathrm{Sr}_{x}\mathrm{CoO}_{3} compounds show exchange bias (EB) effect [8], which is an unidirectional anisotropy (UA) set at the magnetic interfaces of heterogeneous systems, manifested as a shift of the magnetization hysteresis loop along field axis when the system is cooled down in an external magnetic field (HH) [9].

It is thus not surprising that the combined effect of Co and Mn in the A2CoMnO6\mathrm{A}_{2}\mathrm{CoMnO}_{6} double-perovskites (DP) leads to exciting physical properties. For instance, there is a great interest in the ferromagnetic (FM) insulator La2CoMnO6\mathrm{La}_{2}\mathrm{CoMnO}_{6} compound due to its near room-temperature magnetodielectric effect [10, 11]. In contrast, the alkaline earth-doped La1.5Sr0.5CoMnO6\mathrm{La}_{1.5}\mathrm{Sr}_{0.5}\mathrm{CoMnO}_{6} compound shows a robust spontaneous EB (SEB) effect [12], a phenomenon in which UA is observed even after cooling the system in zero HH, being so also called Zero Field Cooled EB effect [13, 14].

The SEB effect seems to be intrinsically related to the presence of a spin glass (SG) phase resulting from the competing magnetic phases in disordered materials [15, 16]. For the case of CoMn-based DPs, we previously showed that replacing Sr by Ba or Ca in La1.5Sr0.5CoMnO6\mathrm{La}_{1.5}\mathrm{Sr}_{0.5}\mathrm{CoMnO}_{6} also leads to SEB. In that case, the Ca-based sample exhibits a small UA while for the Ba-based one, the magnitude of the effect is intermediate between those of Ca- and Sr-based compounds. Such pronounced changes in the SEB effect from one sample to another can be attributed to different proportions of Co2+/Co3+\mathrm{Co}^{2+}/\mathrm{Co}^{3+} and to the spin state of Co3+\mathrm{Co}^{3+}, that affect the uncompensated antiferromagnetic (AFM) Co–Mn coupling [17, 18, 19]. Interestingly, single-crystalline La2−xAxCoMnO6\mathrm{La}_{2-x}\mathrm{A}_{x}\mathrm{CoMnO}_{6} (A=Ca,SrA = \mathrm{Ca}, \mathrm{Sr}) samples are not reentrant SG and showed no trace of SEB effect, giving further evidence that an SG-like phase is necessary for the emergence of SEB [20]

Very recently, a thorough investigation of the La1.5(Sr0.5−xBax)CoMnO6\mathrm{La}_{1.5}(\mathrm{Sr}_{0.5-x}\mathrm{Ba}_{x})\mathrm{CoMnO}_{6} series has evidenced how the crystal structure affects the SEB effect by indirectly altering the systems’ electronic structure [21]. The lattice expansion due to Sr2+\mathrm{Sr}^{2+} to Ba2+\mathrm{Ba}^{2+} partial substitution increases the portion of HS Co3+\mathrm{Co}^{3+}, which by one hand strengthens the Co3+\mathrm{Co}^{3+}–Mn4+\mathrm{Mn}^{4+} interaction, and by the other, it decreases the portion of uncompensated spins at the magnetic interfaces. The combined effects of enhanced AFM phase and decreased uncompensation in the Co–Mn coupling causes the intermediate region of the series (x≃0.25x \simeq0.25) to present the most significant SEB effect reported so far.

Here, we focus our attention on how the immediate changes performed in the electron configurations of Co and Mn by changing its formal valences impact the SEB of CoMn-based DPs. Our system of interest is La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} (x=0,0.25,0.5,0.75x = 0, 0.25, 0.5, 0.75), for which the proximity between Ca2+\mathrm{Ca}^{2+} and La3+\mathrm{La}^{3+} ionic radii at XII coordination [22] makes the structural changes caused by the chemical substitution minimal, allowing us to ascribe the evolution of the SEB in this series primarily to changes in Co/Mn formal valences. We observe a systematic increase of the SEB field with increasing the Ca to La substitution, which is discussed in terms of the concomitant increase in the fraction of Co3+\mathrm{Co}^{3+} present in the system.

EXPERIMENT DETAILS

Polycrystalline samples of La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} series (x=0x = 0, 0.25, 0.5, 0.75) were synthesized by conventional solid-state reaction method. Stoichiometric amounts of La2O3\mathrm{La}_{2}\mathrm{O}_{3}, CaO\mathrm{CaO}, Co3O4\mathrm{Co}_{3}\mathrm{O}_{4} and MnO\mathrm{MnO} were mixed and heated at 800°C for 12 hours in air atmosphere. Later the samples were re-grinded before the second step of 24 hours at 1200°C. Finally, each sample was ground, pressed into a pellet, and heated at 1300°C for 24 hours. After this procedure, dark-black materials were obtained in 10 mm diameter disks. Attempt to produce the x=1.0x = 1.0 concentration using this synthesis route was unsuccessful, resulting in impurity phases.

High-resolution x-ray powder diffraction (XRD) data were collected for each sample at room temperature using a PANalytical Empyrean diffractometer, operating with Cu KαK_{\alpha} radiation. The XRD data was investigated over the angular range 10∘≤2θ≤90∘10^\circ\leq2\theta\leq90^\circ, with a 2θ2\theta step size of 0.013∘0.013^\circ. Rietveld refinement was performed with GSAS software, and its graphical interface program [23].

Magnetization (MM) as a function of temperature [M(T)M(T)] and MM as a function of HH [M(H)M(H)] measurements were carried out in both zero field cooled (ZFC) and field cooled (FC) modes, using a Quantum Design PPMS-VSM magnetometer. For the ZFC experiments, it was given particular care to eliminate any small trapped field in the magnet, with the samples being demagnetized with an oscillating field at room temperature from one measurement to another, in order to exclude the possibility of the shift in the M(H)M(H) curves be related to instrumental artifact.

RESULTS AND DISCUSSION

The XRD patterns of La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} samples here investigated (here-after called by its Ca-concentration, xx) are shown in Figure 1. There is an open debate concerning whether these compounds form in the monoclinic P21/nP2_{1}/n or the orthorhombic PnmaPnma space group. In practice, the main difference between these space groups is that the Co and Mn ions are expected to alternate orderly inside the oxygen octahedra for the monoclinic structure. In contrast, the cations are disordered along the lattice for the orthorhombic one. The controversy occurs because the Co and Mn scattering factors are very similar for XRD performed with Cu-KαK_{\alpha} radiation. Different groups have reported such compounds as belonging to one of these space groups or even a mixture of both [18, 24, 25, 26, 27]. The Co- and Mn-based perovskites are known to be very sensitive to the synthesis route [6, 29, 30], and the La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} seems to be a clear manifestation of this. In our case, the XRD patterns indicate the formation of single-phase perovskite for every investigated sample.

Rietveld refinement and XRD patterns of La₂₋ₓCaₓCoMnO₆ samples

Figure 1. (a)Rietveld refinement fitting of La2_2CoMnO6_6 sample. The solid black circles represent the experimental data, the red solid lines are for the calculated patterns, the blue line shows the difference between the observed and calculated patterns, and the dark green vertical lines represent the Bragg reflections for the PnmaPnma space group. (b) Comparison between the XRD patterns of all La2−x_{2-x}Cax_xCoMnO6_6 samples. Inset shows the unit cell volume as a function of Ca-concentration, xx.

Figure 1(a) shows the Rietveld refinement fitting of the x=0x = 0 compound as representative of the whole series, for which nearly the same overall quality of refinement was achieved. For the adjustment of the calculated patterns, the lattice parameters, the thermal displacements parameters, and the atomic positions were refined, as well as the peak shapes, for which it was used a pseudo-Voigt function, the UU, VV and WW terms of the Cagliotti’s function being refined for the Gaussian part of the function, and the XX, YY terms being refined for the Lorentzian one. In order to avoid divergence in the calculations and/or unreliable results, the isotropic temperature factors of Co and Mn were constrained to have the same value, as well as those of oxygen ions. The main results obtained from the refinements for the orthorhombic PnmaPnma space group are displayed in Table 1.

Sample00.250.50.75
aa (Å)5.4832(3)5.4580(1)5.4335(1)5.4153(1)
bb (Å)7.7685(3)7.7246(2)7.6869(1)7.6587(2)
cc (Å)5.5206(3)5.4950(1)5.4661(1)5.4405(1)
V (Å3^3)235.16(3)231.67(1)228.31(1)225.64(1)
Atomic Positions
La/Ca xx0.5224(2)0.5195(3)0.5191(3)0.5186(5)
La/Ca yy0.250.250.250.25
La/Ca zz0.0038(6)0.0027(6)0.0032(6)0.0013(10)
O1_1 xx-0.0083(22)-0.0101(24)-0.0137(24)-0.0211(34)
O1_1 yy0.250.250.250.25
O1_1 zz-0.0575(24)-0.0590(20)-0.0528(21)-0.0719(28)
O2_2 xx0.2809(30)0.2679(28)0.2541(26)0.2570(30)
O2_2 yy0.0371(19)0.0343(12)0.0331(12)0.0264(16)
O2_2 zz0.2187(13)0.2129(17)0.2038(15)0.2103(21)
Bonds and Angles
Co/Mn–O1_1 (Å)1.968(2)1.959(2)1.945(2)1.956(1)
Co/Mn–O2_2 (Å)1.978(1)1.891(1)1.792(1)1.788(2)
Co/Mn–O2_2 (Å)1.985(1)2.041(1)2.115(1)2.087(1)
⟨Co/Mn–O⟩ (Å)1.977(2)1.964(2)1.951(1)1.944(1)
Co–O1_1–Mn (°)161.3(6)160.7(6)162.4(7)156.3(2)
Co–O2_2–Mn (°)158.1(6)160.0(5)161.0(5)164.3(1)
⟨Co–O–Mn⟩ (°)159.7(6)160.4(6)161.7(6)160.3(2)
RwpR_{wp} (%)4.73.93.84.1
χ2\chi^21.21.31.31.7

Table 1. Results of Rietveld refinement of crystalline structure for La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_x\mathrm{CoMnO}_6 samples in PnmaPnma space group. The unit cell is centered on the Co/Mn ions, so their atomic position is (0,0,0).

As Figure 1(b) shows, the diffraction peaks could be well indexed in the PnmaPnma structure for all compounds. The maintenance of the crystallographic symmetry along the series is not surprising since the La3+\mathrm{La}^{3+} and Ca2+\mathrm{Ca}^{2+} ionic radii are very close in XII coordination (1.36 Åand 1.34 Å, respectively [22]). However, it is important to point out that our laboratory XRD results may have not enough resolution to unambiguously determine the crystallographic structure of this system, the formation in the P21/nP2_{1}/n space group, or even phase segregation, with the presence of some small amount of a secondary phase, can not be excluded.

A careful inspection of the XRD data reveals a systematic shift of the diffraction peaks to the right with increasing the Ca content, related to the lattice shrinkage as can be seen on the inset of Figure 1(b). This shift could be ascribed to the fact the Ca2+\mathrm{Ca}^{2+} ionic radius is slightly smaller than that of La3+\mathrm{La}^{3+}. However, it is also related to the systematic increase in the oxidation states of Co and Mn, for which the ionic radii are expected to decrease as the formal valences increase [22]. Such changes are also manifested in the average Co/Mn–O bond length and directly impact the systems’ magnetic properties, as will be discussed next.

The ZFC-FC M(T)M(T) measurements were performed with H=100H = 100 Oe for every sample. Figure 2(a) shows the curves for x=0x = 0, where the presence of two FM-like transitions is clear, in agreement with previous reports for this compound [18, 32]. The higher temperature magnetic ordering (TC1T_{\mathrm{C1}}) is usually ascribed to Co2+\mathrm{Co}^{2+}–O–Mn4+\mathrm{Mn}^{4+} coupling, which is predicted by the Goodenough-Kanamori-Anderson rules to be of FM type, while the lower temperature one (TC2T_{\mathrm{C2}}) is proposed to come from Co3+\mathrm{Co}^{3+}–O–Mn3+\mathrm{Mn}^{3+} vibronic FM coupling [32, 33]. There are other possible scenarios, as for instance the well known Mn3+\mathrm{Mn}^{3+}–O–Mn4+\mathrm{Mn}^{4+} FM coupling [4, 5] which is possible due to the antisite disorder (ASD) at Co/Mn site, intrinsic of the crystallographic structure here observed for this DP. In any case, the presence of two FM transitions makes evident that mixed-valence states Co2+/Co3+\mathrm{Co}^{2+}/\mathrm{Co}^{3+} and Mn4+/Mn3+\mathrm{Mn}^{4+}/\mathrm{Mn}^{3+} are present already in our x=0x = 0 sample, as commonly observed for La2CoMnO6\mathrm{La}_{2}\mathrm{CoMnO}_{6} samples produced with similar synthesis routes [18, 32, 34].

ZFC and FC $M(T)$ curves of La$_{2-x}$Ca$_x$CoMnO$_6$ samples for $x=0$, $0.25$, $0.5$, and $0.75$

Figure 2. ZFC and FC M(T)M(T) curves of La2−x_{2-x}Cax_xCoMnO6_6 samples, measured at H=100H = 100 Oe.

For the Ca-doped samples [Figs. 2(b)–(d)], besides TC1T_{\mathrm{C1}} and TC2T_{\mathrm{C2}} it can be noticed a subtle anomaly in the ZFC curves at lower temperatures, in particular for x=0.5x = 0.5 and 0.75 samples, which is usually related to the presence of AFM couplings like Co2+\mathrm{Co}^{2+}–Co2+\mathrm{Co}^{2+}, Co3+\mathrm{Co}^{3+}–Co3+\mathrm{Co}^{3+}, Mn3+\mathrm{Mn}^{3+}–Mn3+\mathrm{Mn}^{3+}, Mn4+\mathrm{Mn}^{4+}–Mn4+\mathrm{Mn}^{4+} and Co3+\mathrm{Co}^{3+}-

Mn4+^{4+}. The AFM exchange interaction may be expected for the PnmaPnma space group where the Co/Mn ions are disorderly distributed along the lattice. The TC1T_{\mathrm{C1}} and TC2T_{\mathrm{C2}} values, defined here by the local minima in the first derivative of the ZFC curves (not shown), are displayed in Table 2 and in Figure 3(a). The subtle anomalies associated with the AFM couplings are partially masked in the curves due to the stronger FM interactions, hampering the estimate of TNT_{\mathrm{N}} from our dc measurements, which is thus not displayed here.

Sample00.250.50.75
TC1T_{C1} (K)225182160150
TC2T_{C2} (K)150140156163
θCW\theta_{\mathrm{CW}} (K)188187171118
μeff\mu_{\mathrm{eff}} (μB\mu_{\mathrm{B}}/f.u.)7.67.26.97.3
HEBH_{\mathrm{EB}} (Oe)-70230670
HCH_{\mathrm{C}} (kOe)10.211.36.86.3
MrM_{\mathrm{r}} (μB\mu_{\mathrm{B}}/f.u.)2.32.00.40.2
MsM_{\mathrm{s}} (μB\mu_{\mathrm{B}}/f.u.)4.24.02.71.9

Table 2. Main parameters obtained from the M(T)M(T) and M(H)M(H) measurements.

Plots of $T_{\mathrm{C1}}$, $T_{\mathrm{C2}}$, $\theta_{\mathrm{CW}}$, and $\mu_{\mathrm{eff}}$ as a function of Ca concentration

Figure 3. (a) TC1T_{\mathrm{C1}} and TC2T_{\mathrm{C2}} extracted from the first derivatives of the ZFC M(T)M(T) curves. (b) θCW\theta_{\mathrm{CW}} and μeff\mu_{\mathrm{eff}} obtained from the fitting of the PM regions of the M(T)M(T) curves with the CW law. Straight lines are guides to the eye.

Figure 3(a) shows a systematic decrease of TC1T_{\mathrm{C1}} with increasing the Ca-content while the changes in TC2T_{\mathrm{C2}} are non-monotonic. Although the ion’s electronic configurations primarily influence the magnetic coupling between Co and Mn, other parameters such as the bond lengths and angles may play an important role. The Co–O–Mn coupling in perovskites is generally understood in terms of the ege_g–ege_g orbital hybridization, but the t2gt_{2g}–t2gt_{2g} interaction is also expected to play its part in non-cubic 3d3d perovskites due to the presence of half-filled t2gt_{2g} orbitals in both Co and Mn ions [35, 36]. In this sense, the decrease of TC1T_{\mathrm{C1}} can be ascribed mainly to the reduction of the Co2+^{2+}–O–Mn4+^{4+} phase due to hole doping.

In the case of TC2T_{\mathrm{C2}}, the Ca-doping also strengths the t2gt_{2g}–t2gt_{2g} interaction due to the additional hole in the Co3+^{3+} t2gt_{2g} orbitals. This π\pi bonding is expected to be weakened by decreasing the tilts and rotations of the oxygen octahedra, i.e., with increasing the Co–O–Mn bond angle. Table 2 shows a decrease of TC2T_{\mathrm{C2}} followed by an increase with Ca-doping, while the opposite trend is observed for the Co–O–Mn angle. This may be the primary parameter to account for the non-systematic changes in TC2T_{\mathrm{C2}}. However, other ingredients such as the presence of of Co–Co and Mn–Mn interactions induced by the cationic disorder can not be ruled out. Finally, we must stress that the proximity between TC1T_{C1} and TC2T_{C2} may be preventing a precise determination of the latter transition temperature from the first derivative of our dc M(T)M(T) curves. Other experiments such as ac magnetic susceptibility would be necessary to accurately determine the magnetic transition temperatures.

It is important to reinforce the sample dependence observed for these CoMn-based perovskites. The widely investigated x=0x = 0 compound is a prime example of that, where depending on the synthesis route, the sample can display one, two, or even three FM transitions. In addition, the AFM couplings are usually present due to the disorder and even possibly a glassy magnetic state is found, resulting from the competition between magnetic phases [10, 11, 18, 32, 34]. This sample dependence is also evident for the x=0.5x = 0.5 concentration, where the magnetic properties here described are similar to those found for samples also produced by solid-state reaction [17, 18]. In contrast, the second FM transition is not observed for samples produced by the sol-gel technique, and the sample develops an anomaly at lower temperatures which is ascribed to canted AFM. Additionally, the reentrant glassy behavior can be classified as canonical SG or cluster SG (CG) depending on the synthesis condition [24, 37]. This is usual for Mn- and Co-based perovskites [4, 6], the La2−x_{2-x}Srx_xCoMnO6_6 system being also very sample-dependent [12, 18].

From the fitting of the paramagnetic (PM) region of the M(T)M(T) curves with the Curie-Weiss (CW) law, we get the CW temperature, θCW\theta_{\mathrm{CW}}, and the effective magnetic moment, μeff\mu_{\mathrm{eff}}, for every sample here investigated, as displayed in Table 2 and Figure 3(b). For x=0x = 0, we have θCW=188\theta_{\mathrm{CW}} = 188 K. This largely positive value indicates that FM coupling dominates, but the fact it is somewhat smaller than TC1=225T_{C1} = 225 K suggests the presence of AFM phases already for the parent compound, as expected for this disordered system.

We can infer the Co/Mn electronic configurations for the x=0x = 0 compound by comparing its μeff=7.6\mu_{\mathrm{eff}} = 7.6 μB\mu_{\mathrm{B}}/f.u. experimentally observed with the value obtained from the usual equation for systems with two or more different magnetic ions [38, 39]

μ=μ12+μ22+μ32+⋯(1)\mu= \sqrt{\mu_1^2 + \mu_2^2 + \mu_3^2 + \cdots} \tag*{(1)}

As aforementioned, one may expect mixed valences for the TM ions already for the x=0x = 0 parent compound. Assuming the same proportion of Co2+/Mn4+\mathrm{Co}^{2+}/\mathrm{Mn}^{4+} and Co3+/Mn3+\mathrm{Co}^{3+}/\mathrm{Mn}^{3+}, considering that Co3+\mathrm{Co}^{3+} is in HS configuration and using the spin only (SO) approximation for these 3d ion moments (μCo2+=μMn4+=3.9 μB\mu_{\mathrm{Co}^{2+}} = \mu_{\mathrm{Mn}^{4+}} = 3.9\ \mu_{\mathrm{B}}; μHSCo3+=μMn3+=4.9 μB\mu_{\mathrm{HSCo}^{3+}} = \mu_{\mathrm{Mn}^{3+}} = 4.9\ \mu_{\mathrm{B}} [40]) we get μ=6.2 μB\mu= 6.2\ \mu_{\mathrm{B}}/f.u., far below the experimental value. One of the main reasons for such large discrepancy may be the fact that some orbital contribution for the magnetic moments should be expected, in special for Co ions [6, 18]. Alternatively, considering the same proportion of mixed valence ions but now using the standard magnetic moments usually found for these 3d TM ions (μCo2+=4.8 μB\mu_{\mathrm{Co}^{2+}} = 4.8\ \mu_{\mathrm{B}}; μHSCo3+=5.4 μB\mu_{\mathrm{HSCo}^{3+}} = 5.4\ \mu_{\mathrm{B}}; μMn3+=5 μB\mu_{\mathrm{Mn}^{3+}} = 5\ \mu_{\mathrm{B}}; μMn4+=4 μB\mu_{\mathrm{Mn}^{4+}} = 4\ \mu_{\mathrm{B}} [40]) we get μ=6.8 μB\mu= 6.8\ \mu_{\mathrm{B}}/f.u., still smaller but now much closer to the experiment. This calculation is undoubtedly just a rough estimate because the precise orbital moment of each ion is unknown, and the exact Co2+/Co3+\mathrm{Co}^{2+}/\mathrm{Co}^{3+} and Mn3+/Mn4+\mathrm{Mn}^{3+}/\mathrm{Mn}^{4+} ratios may be somewhat different from that assumed in La2(Co0.52+Co0.53+)(Mn0.53+Mn0.54+)O6\mathrm{La}_{2}(\mathrm{Co}^{2+}_{0.5}\mathrm{Co}^{3+}_{0.5})(\mathrm{Mn}^{3+}_{0.5}\mathrm{Mn}^{4+}_{0.5})\mathrm{O}_{6}. Besides, one may also have some fraction of Co3+\mathrm{Co}^{3+} in LS configuration, as already found for similar DPs [18, 21, 31]. A detailed investigation employing X-ray absorption spectroscopy, X-ray photoelectron spectroscopy, X-ray magnetic circular dichroism and/or neutron diffraction is necessary to precisely determine each ion’s formal valence and magnetic moment.

Figure 3(b) and Table 2 show that for the x=0x = 0 - 0.5 interval the μeff\mu_{\mathrm{eff}} decreases as the Ca-content increases. Since Mn4+\mathrm{Mn}^{4+} moment is smaller than that of Mn3+\mathrm{Mn}^{3+} whereas the one of HS Co3+\mathrm{Co}^{3+} is larger than that of HS Co2+\mathrm{Co}^{2+}, this decrease in μeff\mu_{\mathrm{eff}} strongly suggests that up to x=0.5x = 0.5 the hole doping acts mainly to increase the Mn formal valence. Otherwise, the effective moment would increase. Assuming thus for x=0.25x = 0.25 and 0.5 the respective general formulas La1.75Ca0.25(Co0.52+Co0.53+)(Mn0.253+Mn0.754+)O6\mathrm{La}_{1.75}\mathrm{Ca}_{0.25}(\mathrm{Co}^{2+}_{0.5}\mathrm{Co}^{3+}_{0.5})(\mathrm{Mn}^{3+}_{0.25}\mathrm{Mn}^{4+}_{0.75})\mathrm{O}_{6} and La1.5Ca0.5(Co0.52+Co0.53+)Mn4+O6\mathrm{La}_{1.5}\mathrm{Ca}_{0.5}(\mathrm{Co}^{2+}_{0.5}\mathrm{Co}^{3+}_{0.5})\mathrm{Mn}^{4+}\mathrm{O}_{6} in Eq. (1) we get the theoretical moments μ=6.7 μB\mu= 6.7\ \mu_{\mathrm{B}}/f.u. and μ=6.5 μB\mu= 6.5\ \mu_{\mathrm{B}}/f.u., respectively, thus capturing the decrease of μeff\mu_{\mathrm{eff}} with increasing xx that is observed experimentally.

Interestingly, for x=0.75x = 0.75 it is observed the increase of μeff\mu_{\mathrm{eff}} with respect to the value found for x=0.5x = 0.5. This rise is because, for x=0.5x = 0.5, all the Mn ions are already at the tetravalent state, and Mn5+\mathrm{Mn}^{5+} is very unlikely. Thus the further increment of Ca2+\mathrm{Ca}^{2+} at La3+\mathrm{La}^{3+} site from x=0.5x = 0.5 to 0.750.75 now acts to remove electrons from Co, increasing its average oxidation state. Assuming La1.25Ca0.75(Co0.252+Co0.753+)Mn4+O6\mathrm{La}_{1.25}\mathrm{Ca}_{0.75}(\mathrm{Co}^{2+}_{0.25}\mathrm{Co}^{3+}_{0.75})\mathrm{Mn}^{4+}\mathrm{O}_{6} for this sample in Eq. (1) we get μ=6.6 μB/f.u.\mu= 6.6\,\mu_{\mathrm{B}}/\mathrm{f.u.}, which represents an increase in comparison to the theoretical value obtained for x=0.5x = 0.5 and again being in accordance with the experimental results. Again, the discrepancies between the theoretical and experimental values indicate an oversimplification of the problem. The presence of two magnetic transitions for the x=0.5x = 0.5 and 0.750.75 samples indicate that one may have, in practice, some small fraction of Mn3+\mathrm{Mn}^{3+} even for these compounds. Such simplified calculations do not intend to give the precise estimate of the proportion between the TM ions but only to give us some insight about the trends induced by Ca-doping. Although the calculated values are somewhat smaller than those obtained experimentally, the trend observed with changing the Ca-concentration could be captured precisely.

Figure 4 shows the M(H)M(H) curves measured up to H=90H = 90 kOe after ZFC each sample down to 55 K. As can be noticed, all loops are closed, nearly vertically symmetric, and show some hysteresis. Notably, the loops gradually lose their squareness with increasing the Ca-concentration and develop a linear field-dependence at high fields, suggesting the increase in the proportion of AFM phase with increasing xx. This change in the shape of the hysteresis curves is also manifested in the systematic decrease of the remanent magnetization (MRM_{\mathrm{R}}), as shown in Figure 4(e). In addition, a similar trend is observed for the coercive field HC=(HC+−HC−)/2H_{\mathrm{C}} = (H_{\mathrm{C}+} - H_{\mathrm{C}-})/2, where HC+H_{\mathrm{C}+} and HC−H_{\mathrm{C}-} are respectively the positive and negative coercive fields, which will have a direct impact on the SEB effect.

M(H) loops and magnetic parameters for La2−xCaxCoMnO6

Figure 4. (a)–(d) M(H)M(H) loops for La2−x_{2-x}Cax_xCoMnO6_6 measured at 5 K after ZFC each sample. Insets show magnified views of the regions near M=0M = 0, highlighting the horizontal shifts in the Ca-doped samples. (e) MRM_R and HCH_C as a function of Ca-concentration, xx. (f) HEBH_{EB} as a function of xx. Straight lines are guides to the eye.

The shift in the M(H)M(H) curves, characteristic of the EB effect, are not large enough for the La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} samples in a way to be apparent in the complete hysteresis loops shown in the main Figure 4(a)-(Figure 4d), but are evidenced at the magnified views of the regions close to M=0M = 0 displayed in the insets. As can be seen, there is no shift for the x=0x = 0 parent compound, but for the Ca-doped samples, the asymmetry in the curves is clear, with the EB field, HEB=∣HC++HC−∣/2H_{\mathrm{EB}} = \lvert H_{\mathrm{C}+} + H_{\mathrm{C}-}\rvert/2, systematically increasing with xx, as shown in Figure 4(f) and Table 2.

The increase of HEBH_{\mathrm{EB}} with increasing the A2+\mathrm{A}^{2+} doping at La3+\mathrm{La}^{3+} site observed here for La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_{x}\mathrm{CoMnO}_{6} is different to the trends reported for La2−xSrxCoMnO6\mathrm{La}_{2-x}\mathrm{Sr}_{x}\mathrm{CoMnO}_{6} and La1.5(Sr0.5−xBax)CoMnO6\mathrm{La}_{1.5}(\mathrm{Sr}_{0.5-x}\mathrm{Ba}_{x})\mathrm{CoMnO}_{6} systems, for which the SEB field is larger at intermediate xx values. For the first series, this trend is directly related to the ASD between the TM ions, which destroys the long-range magnetic order and increases the AFM interactions. The canted AFM phase observed at low temperature is larger for x=0.5x = 0.5. Correspondingly, the SEB is also maxima at this concentration [41]. For La1.5(Sr0.5−xBax)CoMnO6\mathrm{La}_{1.5}(\mathrm{Sr}_{0.5-x}\mathrm{Ba}_{x})\mathrm{CoMnO}_{6} the lattice expansion due to Ba to Sr substitution leads to the increase in the concentration of HS Co3+\mathrm{HS}\ \mathrm{Co}^{3+} ions which in turn leads to two competing effects, the increase of the AFM phase and the reduction of the uncompensation in this AFM coupling. This combined effect results in a maximum in the SEB field for the x=0.25x = 0.25 intermediate

concentration of Ba/Sr [21].

A previous investigation of the SEB effect in La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_x\mathrm{CoMnO}_6 polycrystals prepared by the sol-gel method [26] showed HEBH_{EB} values remarkably different from ours, further demonstrating the severe sample-dependence in this system. Moreover, in contrast to our work, increasing HEBH_{EB} for 0≤x≤0.50 \leq x \leq0.5 samples followed by a decrease for x>0.5x > 0.5 was observed, although the x=0.75x = 0.75 concentration was not investigated. The authors interpreted such changes in terms of the Co/Mn ASD estimated from the MsM_s values. In our case, however, in principle we should expect a systematic decrease of ASD in the 0≤x≤0.50 \leq x \leq0.5 region due to the increased portion of Mn4+\mathrm{Mn}^{4+} ions, whose radius and valence are more distant to those of Co2+/Co3+\mathrm{Co}^{2+}/\mathrm{Co}^{3+} than Mn3+\mathrm{Mn}^{3+}. These parameters are known to play an important role in the ASD of DPs [2, 42].

According to the arguments proposed in Ref. [26], the HEBH_{EB} of our series should decrease for 0≤x≤0.50 \leq x \leq0.5, in contrast to the results. Thus, for our La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_x\mathrm{CoMnO}_6 samples, we ascribe the increase of HEBH_{EB} directly to the changes in the AFM/FM interfaces. The systematic decrease of TC1T_{C1} and θCW\theta_{CW} with increasing xx observed in the M(T)M(T) curves, and the decrease of MrM_r and MsM_s observed in the M(H)M(H) loops, suggest the increase in the portion of the AFM phase with increasing the Ca-content. This strengthens the AFM/FM coupling, enhancing the SEB effect. The loss of squareness of the M(H)M(H) loops with increasing xx and the changes in the shape of the curves are also suggestive of the presence of a glassy magnetic phase for the Ca-doped samples [43], as was already observed for the x=0.5x = 0.5 compound [17, 24, 37], and is also expected for the other concentrations of this disordered system where the magnetic phases compete. The SG-like phase is ubiquitous on the SEB effect observed in DP compounds [15, 16].

Although non-negligible, the SEB here described for the Ca-doped samples is much smaller than those reported for La2−xAxCoMnO6\mathrm{La}_{2-x}\mathrm{A}_x\mathrm{CoMnO}_6 compounds with A = Sr and Ba [12, 18, 21], for which the presence of LS Co3+\mathrm{Co}^{3+} is believed to uncompensate the Co–Mn AFM coupling and thus enhance the UA responsible for the EB effect. The M(T)M(T) data for our Ca-based samples suggest that Co3+\mathrm{Co}^{3+} is in HS configuration, which possibly leads to a nearly compensated AFM coupling and consequently decreases the SEB effect.

CONCLUSIONS

In summary, the La2−xCaxCoMnO6\mathrm{La}_{2-x}\mathrm{Ca}_x\mathrm{CoMnO}_6 (0≤x≤0.750 \leq x \leq0.75) samples here investigated form as single-phase perovskites, the XRD patterns could be successfully refined in the orthorhombic PnmaPnma space group. The magnetic measurements indicate a complex magnetic behavior for all samples, where the presence of Co2+/Co3+\mathrm{Co}^{2+}/\mathrm{Co}^{3+} and Mn3+/Mn4+\mathrm{Mn}^{3+}/\mathrm{Mn}^{4+} mixed-valence states lead to competing FM and AFM interactions, which may result in glassy magnetic behavior and EB effect. The increased portion of the AFM phase with increasing xx, as suggested by the M(T)M(T) data, can explain the rise of the SEB effect with increasing the Ca-doping as observed in the M(H)M(H) curves.

ACKNOWLEDGMENTS

This work was supported by Conselho Nacional de Desenvolvimento Científico e Tecnológico (CNPq) [No. 425936/2016-3], Coordenação de Aperfeiçoamento de Pessoal de Nível Superior (CAPES), Fundação de Amparo à Pesquisa do Estado de Goiás (FAPEG), and Fundação Carlos Chagas Filho de Amparo à Pesquisa do Estado do Rio de Janeiro (FAPERJ) [Nos. E-26/202.798/2019, E-26/211.291/2021].

References

  1. [1]J. G. Bednorz and K. A. Müller, Z. Phys. B Cond. Mat. 64 (1986) 189–193.
  2. [2]D. Serrate, J. M. De Teresa and M. R. Ibarra, J. Phys.: Condens. Matter 19 (2007) 023201.
  3. [3]H. Liu and X. Yang, Ferroelectrics 507:1, (2017) 69-85.
  4. [4]M. B. Salamon and M. Jaime, Rev. Mod. Phys. 73 (2001) 583.
  5. [5]J. M. D. Coey, M. Viret and S. von Molnár, Adv. Phys. 48:2 (1999) 167-293.
  6. [6]B. Raveau and Md. Motin Seikh, Cobalt Oxides: From Crystal Chemistry to Physics (Wiley-VCH, Weinheim, 2012).
  7. [7]P. G. Radaelli and S.-W. Cheong, Phys. Rev. B 66 (2002) 094408.
  8. [8]Y. Tang, Y. Sun, and Z. Cheng, Phys. Rev. B 73 (2006) 174419.
  9. [9]J. Nogués and I. K. Schuller, J. Magn. Magn. Mater. 192 (1999) 203.
  10. [10]Y. Q. Lin and X. M. Chen, J. Am. Ceram. Soc., 94 [3] (2011) 782–787.
  11. [11]J. Krishna Murthy, K. Devi Chandrasekhar, S. Murugavel, and A. Veni-madhav, J. Mater. Chem C 3 (2015) 836.
  12. [12]J. Krishna Murthy and A. Venimadhav, Appl. Phys. Lett. 103 (2013) 25410.
  13. [13]B. M. Wang, Y. Liu, P. Ren, B. Xia, K. B. Ruan, J. B. Yi, J. Ding, X. G. Li, and L. Wang, Phys. Rev. Lett. 106 (2011) 007203 .
  14. [14]A. K. Nayak, M. Nicklas, S. Chadov, C. Shekhar, Y. Skourski, J. Winterlik, and C. Felser, Phys. Rev. Lett. 110 (2013) 127204.
  15. [15]L. T. Coutrim, E. M. Bittar, F. Garcia, and L. Bufaïçal, Phys. Rev. B 98 (2018) 064426.
  16. [16]L. Bufaïçal, L. T. Coutrim, E. M. Bittar, and F. Garcia, J. Magn. Magn. Mater. 512 (2020) 167048.
  17. [17]L. Bufaical, R. Finkler, L. T. Coutrim, P. G. Pagliuso, C. Grossi, F. Stavale, E. Baggio-Saitovitch, and E.M. Bittar, J. Magn. Magn. Mater. 433 (2017) 271–277.
  18. [18]L. T. Coutrim, D. Rigitano, C. Macchiutti, T. J. A. Mori, R. Lora-Serrano, E. Granado, E. Sadrollahi, F. J. Litterst, M. B. Fontes, E. Baggio-Saitovitch, E. M. Bittar, and L. Bufaical, Phys. Rev. B 100 (2019) 054428.
  19. [19]M. Boldrin, L. T. Coutrim, and L. Bufaical, Braz. J. Phys. 50 (2020) 711–715.
  20. [20]C. Macchiutti, J. R. Jesus, F. B. Carneiro, L. Bufaical , M. Ciomaga Hatnean, G. Balakrishnan, and E. M. Bittar, Phys. Rev. Mater. 5 (2021) 094402.
  21. [21]M. Boldrin, A. G. Silva, L. T. Coutrim, J. R. Jesus, C. Macchiutti, E. M. Bittar, and L. Bufaical, Appl. Phys. Lett. 117 (2020) 212402.
  22. [22]R. D. Shannon, Acta Crystallographica A32 (1976) 751.
  23. [23]A. C. Larson and R. B. Von Dreele, Los Alamos National Laboratory Report No. LAUR 86-748, 2000; B. H. Toby, J. Appl. Crystallogr. 34, 210 (2001).
  24. [24]R. C. Sahoo, D.Paladhi, and T. K. Nath, J. Magn. Magn. Mater. 436 (2017) 77-84.
  25. [25]Q. Li, L. Xing, and M. Xu, Phys. Status Solidi B 254 (2017) 9, 1600757.
  26. [26]R. C. Sahoo, S. Das, D. Daw, R. Singh, A. Das, and T. K. Nath, J. Phys.: Condens. Matter 33 (2021) 215804.
  27. [27]Q. Li, N. Li, J. Hu, Q. Han, Q. Ma, L. Ge, B. Xiao, and M. Xu, J. Appl. Phys. 116 (2014) 033905.
  28. [29]I. A. Abdel-Latif, J. Phys. 1 (2012) 3.
  29. [30]B. Martínez, Ll. Balcells, J. Fontcuberta, X. Obradors, C. H. Cohenca, and R. F. Jardim, J. Appl. Phys. 83 (1998) 7058.
  30. [31]V. Vashook, D. Franke, J. Zosel, L. Vasylechko, M. Schmidt, and U. Guth, J. Alloys Compd. 487 (2009) 577–584.
  31. [32]R. I. Dass and J. B. Goodenough, Phys. Rev. B 67 (2003) 014401.
  32. [33]J. B. Goodenough, Magnetism and Chemical Bond (Interscience, New York, 1963).DOI
  33. [34]K. D. Truong, J. Laverdière, M. P. Singh, S. Jandl, and P. Fournier, Phys. Rev. B 76, 132413 (2007).
  34. [35]J. B. Goodenough, A. Wold R. J. Arnott, and N. Menyuk, Phys. Rev. 124, 2 (1961).
  35. [36]G. Blasse, J. Phys. Chem. Solids 26, 1969-1971 (1965).
  36. [37]R. C. Sahoo, S. K. Giri, D. Paladhi, A. Das, and T. K. Nath, J. Appl. Phys. 120 (2016) 033906.
  37. [38]T. Shin-ike, T. Sakai, G. Adachi, and J. Shiokawa, Mat. Res. Bull. 12 (1977) 831-836.
  38. [39]L. Bufaïcal, E. Sadrollahi, F. J. Litterst, D. Rigitano, E. Granado, L. T. Coutrim, E. B. Araújo, M. B. Fontes, E. Baggio-Saitovitch, and E. M. Bittar, Phys. Rev. B 102 (2020) 024436.
  39. [40]N. W. Ashcroft and N. D. Mermin, Solid State Physics, Cengage Learning (1976).
  40. [41]J. Krishna Murthy, K. D. Chandrasekhar, H. C. Wu, H. D. Yang, J. Y. Lin, and A. Venimadhav, J. Phys.: Condens. Matter 28 (2016) 086003.
  41. [42]S. Vasala and M. Karppinen, Prog. Solid State Chem. 43 (2015) 1.
  42. [43]J. A. Mydosh, Spin Glasses: An Experimental Introduction (Taylor & Francis, London, 1993).

Paper details

vlnc:W_8pxab63p
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents