betaFeedback

WorksPhysics and Astronomy

SrMn2_2Ge2_2: A metallic system with anomalous magnetotransport properties

Abstract

The structural, electronic, and physical properties of previously unexplored layered tetragonal compound SrMn2_2Ge2_2 are reported. The compound crystallizes in the ThCr2_2Si2_2-type structure with a crystallographic parameters c/ac/a ratio of 2.535(3)2.535(3), significantly smaller than those of the related BaMn2_2Pn2Pn_2 compounds (Pn=Pn = P, As, Sb, Bi), indicating enhanced interlayer interaction between the moment-bearing Mn-ions. Magnetic susceptibility measurements suggest an antiferromagnetic ground state with a high Neél temperature TN>350T_{\rm N} > 350~K@. A large and positive magnetoresistance (MR) of approximately 50%50\% is observed at low temperatures, which follows a power-law field dependence with exponent n=1.50(8)n = 1.50(8). Low-temperature electrical resistivity data reveal Kondo-like features. Heat capacity measurements show no signs of a phase transition below 300~K and further confirm a metallic ground state. Electronic structure calculations reveal a three-dimensional Fermi surface and suggest the presence of substantial electronic correlation effects.

Introduction

The discovery of high-TcT_{\mathrm{c}} superconductivity[1, 2, 3, 4] and several other exciting ground states, such as highly frustrated magnetic state,[5] prototypical half-metallic behavior,[6, 7, 8] Anderson localization, and large negative magnetoresistance (MR)[9, 10, 11] have sparked intense interest in ThCr₂Si₂-type 122 compounds. Among these compounds, the RRMn₂Ge₂ (RR: rare earth) series has been shown to exhibit a wide variety of complex magnetic structures and behaviours.[12, 13, 14, 15, 16, 17, 18] These include reentrant ferromagnetism, a variety of metamagnetic transitions, as well as a host of noncollinear structures.[19, 20, 21] Furthermore, the subtle and layered nature of the underlying magnetic sublattices in these systems can lead to unusual magnetotransport behaviour.[22, 23] For example, LaMn₂Ge₂ which exhibits a non-trivial spin structure, has been reported to show anomalously large and positive MR of ∼ 80% at 4.2 K in an applied field of μ0H=5\mu_{0}H = 5 T.[22] In addition, this compound has recently been reported to exhibit a large topological Hall effect near room temperature that highlights its technological relevance.[17, 18]

The related AMn₂Ge₂ (AA = Ca, Sr, Ba) series remains largely unexplored, with only a few studies on crystal and magnetic structures having been reported so far. Both CaMn₂Ge₂ and BaMn₂Ge₂ have been shown to be antiferromagnetic (AFM) with high Néel temperatures and collinear G-type magnetic ordering, with TN=670T_{\mathrm{N}} = 670 K reported for the former.[24, 25] On the other hand, only structural properties of SrMn₂Ge₂ have been reported so far.[26] Interestingly, all three members of this series feature small c/ac/a ratios, as well as short interlayer Ge-Ge distances dGe−Ged_{\mathrm{Ge-Ge}}, where the latter is close to the single covalent Ge–Ge bond distance of ∼ 2.45 Å (Table 1). These observations collectively suggest the presence of interlayer Ge–Ge dimerization, leading to a collapsed tetragonal (cT) structure in all three AMn₂Ge₂ compounds, as well as in LaMn₂Ge₂ and EuMn₂Ge₂. Furthermore, the c/ac/a ratios of AMn₂Ge₂ compounds are significantly smaller than those reported for BaMn₂Pn₂ (PnPn = P, As, Sb, Bi), where the magnetism of the Mn-sublattice has been reported to be quasi-two-dimensional in nature.[27] These crystallographic observations therefore suggest that the underlying electronic and magnetic interactions in the discussed Ge-compounds are likely to be more three-dimensional (3D) in nature.

To gain a better understanding of the underlying interactions and properties of Ge-based ThCr₂Si₂-type 122 compounds, we have investigated previously unexplored compound SrMn₂Ge₂. Here we report a comprehensive investigation of the physical properties of polycrystalline SrMn₂Ge₂ using x-ray diffraction, magnetic, thermal, electronic and magneto-transport measurements. Additionally, we also present Density Functional Theory (DFT) based electronic structure calculations and discuss these results in relation to the experimentally obtained data. Our results indicate the presence of an AFM ground state with TN>350T_{\mathrm{N}} > 350 K and show an unusual positive MR of about 50% at low temperatures. The observed unusual MR indicates the presence of correlated multiband electrical transport and/or complex magnetic scatterings which may, in some sense, be similar to those in LaMn₂Ge₂. Hence, our results suggest that SrMn₂Ge₂ could be a promising candidate for investigation of topologically relevant electrical transport behavior.

Experimental and computational details

Single crystal growth of SrMn₂Ge₂ is nontrivial. Several attempts using different fluxes, including Sn, In, Ge, and self flux MnGe, were unsuccessful. Similarly, obtaining a high-purity polycrystalline sample of this compound proved highly challenging. Polycrystalline samples of SrMn₂Ge₂ were synthesized by the arc-melting technique under a partial argon pressure using high-purity constituent elements: Sr (99.9% from Merck), Mn (99.99% from Alfa Aesar), and Ge (99.999% from Alfa Aesar). While Mn and Ge were taken in the stoichiometric ratio, Sr was taken with a varying amount of excess (<7 at.%) to compensate for the anticipated losses due to evaporation, given its relatively low boiling temperature. Numerous synthesis attempts employing different excess Sr concentrations were performed, and the highest purity sample used in the present study with about approximately 5 wt.% of Mn₅Ge₃ was obtained in one of the attempts using 3 at.% excess of Sr. The occurrence of the impurity phase Mn₅Ge₃ was also previously reported in CaMn₂Ge₂ and BaMn₂Ge₂ compounds investigated using neutron diffraction measurements.[24] Room temperature powder x-ray diffraction (XRD) measurements were performed using a Rigaku Miniflex powder diffractometer equipped with a Cu-Kα\alpha radiation source. Rietveld refinements were performed using the FullPROF package [28]. Temperature- and magnetic-field-dependent electrical resistivity and magnetoresistance measurements were performed using the conventional four-probe method in a Physical Properties Measurement System (PPMS) of Quantum Design Inc., USA. Two-component Epo-Tek epoxy was used for connecting the annealed Pt leads to the sample. For field-dependent transport measurements, the magnetic field was applied transverse to the direction of the electrical current. Heat capacity, magnetic susceptibility, and isothermal magnetization measurements were also carried out using the PPMS. For the heat capacity measurements, the sample was thermally anchored to the measurement platform using Apiezon N grease. The magnetic measurements were performed using the quartz sample holder of the Vibrating Sample Magnetometer Option of the same PPMS.

DFT-based calculations were performed using the GPAW software [29, 30, 31, 32]. These calculations were performed with r2SCAN meta-GGA exchange-correlation functional [33, 34] as implemented in libxc [35]. r2SCAN is an all-purpose meta-GGA functional that often provides better consistency than GGAs for correlated materials. Additional results obtained from calculations using the PBEsol exchange-correlation functional [36, 37] are provided as these were found to provide similar agreement with experimental results. Total-energy calculations were performed for the ferromagnetic (FM) configuration, as well as four AFM configurations: A-type, C-type, S-type, and G-type. Among these, the G-type AFM configuration, which is also adopted by CaMn2_2Ge2_2 and BaMn2_2Ge2_2, [24] yielded the lowest total energy. Accordingly, all subsequent calculations were performed assuming the G-type AFM ground state, using the experimentally determined lattice parameters and atomic positions as input. Calculations were performed with a plane-wave energy cutoff of 900 eV, as well as 30 ×\times 30 ×\times 12 Monkhorst-Pack mesh. A denser kk-space sampling of 30 points per Å−1^{-1} was used for the Density of States (DOS) calculation leading to a spacing of 10 meV per bin for the DOS as a function of energy. Tetrahedron integration, as implemented in GPAW, was used.

Results

Crystal structure

Rietveld refinement of the room temperature powder XRD of SrMn2_2Ge2_2 using the ThCr2_2Si2_2-type structure with space group I4/mmmI4/mmm (SG: 139) led to a satisfactory fit to the data [Fig. 1]. However, this refinement revealed a few small impurity peaks in the range 20° < 2θ\theta < 60°. The most intense impurity peak, with intensity < 2% of the highest intensity peak of the pattern, occurs at ∼ 42°. These impurity peaks can be indexed to the hexagonal, FM Mn5_5Ge3_3. The same impurity phase was present in samples of CaMn2_2Ge2_2 and BaMn2_2Ge2_2 that were previously investigated using neutron diffraction. [24] A two-phase refinement, using SrMn2_2Ge2_2 and Mn5_5Ge3_3 as the phases, resulted in an improved fit to the data and resulted in a weight fraction of 5.1(2)% Mn5_5Ge3_3.

The tetragonal lattice parameters aa and cc, as well as the variable cc-axis Ge position parameter zGez_{\mathrm{Ge}} obtained from the two-phase refinement are listed in Table 1 together with the corresponding

ParameterCaMn₂Ge₂ Ref. [24]SrMn₂Ge₂ (This work)BaMn₂Ge₂ Ref. [24]LaMn₂Ge₂ Ref. [39]EuMn₂Ge₂ Ref. [40, 41]
aa (Å)4.153(2)4.3052(2)4.473(5)4.204(2)4.24972(3)
cc (Å)10.864(4)10.9289(4)10.98(3)10.996(6)10.9084(2)
c/ac/a2.616(3)2.535(3)2.455(6)2.615(3)2.5668(2)
zGez_{\mathrm{Ge}}0.379(2)0.3798(1)0.3778(8)0.380(1)0.38
dMn−Mnabd_{\mathrm{Mn-Mn}}^{ab} (Å)2.937(2)3.0442(2)3.163(4)2.973(2)3.0050(3)
dGe−Ged_{\mathrm{Ge-Ge}} (Å)2.63(4)2.627(3)2.68(2)2.64(2)2.618(4)

Table 1. Structural parameters of SrMn₂Ge₂, as well as those reported for AMn2Ge2AMn_2Ge_2 (AA = Ca, Ba) and RMn2Ge2RMn_2Ge_2 (RR = La, Eu). All these compounds crystallize with ThCr₂Si₂-type body centre tetragonal structure [space group: I4/mmmI4/mmm (139)]. The crystallographic parameters provided are the unit cell parameters aa, cc, c/ac/a, zGez_{\mathrm{Ge}}, the intralayer distance between two nearest Mn atoms dMn−Mnab=12ad_{\mathrm{Mn-Mn}}^{ab} = \frac{1}{\sqrt{2}}a, and interlayer distance between two nearest Ge atoms dGe−Ge=c(1−2zGe)d_{\mathrm{Ge-Ge}} = c(1-2z_{\mathrm{Ge}}).

Crystal structure and powder X-ray diffraction refinement of SrMn2Ge2

Figure 1. (a) ThCr2_2Si2_2-type (space group: I4/mmmI4/mmm) crystallographic unit cell of SrMn2_2Ge2_2. The interlayer Ge-Ge distance is shown. (b) The top view of the unitcell. The intralayer Mn-Mn distance is indicated. (c) Room temperature powder x-ray diffraction data IobsI_{\mathrm{obs}} of SrMn2_2Ge2_2, together with two-phase Rietveld refinement fit IcalI_{\mathrm{cal}}, difference profile Iobs−IcalI_{\mathrm{obs}}-I_{\mathrm{cal}} and calculated Bragg peak positions for SrMn2_2Ge2_2 (green bars) and impurity phase Mn5_5Ge3_3 (purple bars).

parameters reported for CaMn2_2Ge2_2, BaMn2_2Ge2_2, and the relevant rare-earth counterparts LaMn2_2Ge2_2 and LuMn2_2Ge2_2. In addition, the intralayer Mn-Mn distance dMn−Mnabd_{\mathrm{Mn-Mn}}^{ab}, as well as the interlayer Ge-Ge distance dGe−Ged_{\mathrm{Ge-Ge}} [Fig. 1] estimated from the refined/reported lattice parameters are also included in Table 1. The relatively small c/ac/a ratio, together with dGe−Ged_{\mathrm{Ge-Ge}} values close to the single covalent Ge-Ge bond distance of ∼ 2.45 Å suggest the presence of interlayer bonding between Ge atoms, leading to a cT structure. It has been observed that interlayer bonding between metalloids has a direct influence on the ionic state of the transition-metal ions and, consequently, on the magnetic properties of the compounds. [38] This will be further discussed in the following sections.

Magnetic properties

The zero-field-cooled (ZFC) magnetic susceptibility χ=M/H\chi= M/H data of SrMn2_2Ge2_2 show a large increase in χ\chi as temperature TT is decreased below 350 K [Fig. 2 (a)]. While the observed response is indicative of an AFM system, its small value at T=2T = 2 K, χ2 K=8.2×10−2\chi_{2\ \mathrm{K}} = 8.2 \times10^{-2} cm3^3/mol, does not support the existence of an FM ground state in this compound. The same conclusion can be drawn from the low-TT ordered moment MoM_o deduced from the isothermal magnetization M(H)M(H) data discussed below. Furthermore, the observed large increase in χ\chi is consistent with the presence of small amounts of an FM impurity (with TC≈300T_C \approx300 K) embedded within an AFM or non magnetic system. In such a case, a substantial magnetic contribution of the FM impurity below its Curie temperature TCT_C can mask the intrinsic low-χ\chi or −M-M of the compound. A similar observation was previously made in the case of a related compound BaMn₂As₂. [42] As discussed in the previous section, the two-phase refinement performed on the XRD data reveals the presence of about 5 wt.% of FM impurity Mn₅Ge₃. Depending upon the sample, the TCT_C of Mn₅Ge₃ is reported to vary between 290 and 305 K. [43, 44] This suggests that the increase in χ\chi with decreasing TT could likely be originating from the contribution of the embedded impurity phase and not an intrinsic property of SrMn₂Ge₂.

In order to determine the intrinsic susceptibility of SrMn₂Ge₂, corrected for the presence of FM impurities, we now examine the isothermal M(H)M(H) data measured at temperatures between 2 and 350 K [Fig. 2(b)]. The M(H)M(H) curves exhibit a negative curvature at low magnetic fields (μ0H≲2\mu_0H \lesssim2 T), which becomes more pronounced with decreasing temperature. As HH increases above ∼2\sim2 T, the M(H)M(H) isotherms tend toward saturation and subsequently display nearly linear or slightly sub-linear behaviour. The tendency to saturation and the resulting ordered moment can be attributed to Mn₅Ge₃ impurity, which has an average magnetic moment of 2.64 μB\mu_B per Mn atom. A 5.1% wt fraction of Mn₅Ge₃ will result in a measured saturation magnetization of ∼0.5 μB\sim0.5\,\mu_B, which is close to the Mo≈0.43 μBM_o \approx0.43\,\mu_B obtained at 2 K. To correct the χ(T)\chi(T) data for the presence of FM impurities, we determined the high-field slopes of the M(H)M(H) isotherms by performing linear fits to the data for fields μ0H>3\mu_0H > 3 T. Since FM contributions typically saturate at high fields (μ0H≳1\mu_0H \gtrsim1 T), the high-field slopes provide the intrinsic susceptibility χint\chi_{\mathrm{int}} of the sample under consideration, corrected for impurity contributions. The χint\chi_{\mathrm{int}} values of SrMn₂Ge₂ obtained in this manner are plotted as orange diamonds in Figure 2(a). We find that χint<χ\chi_{\mathrm{int}} < \chi throughout the measured temperature range and χint≪χ\chi_{\mathrm{int}} \ll\chi for T≤275T \leq275 K where the FM impurity begins to saturate. Furthermore, χint\chi_{\mathrm{int}} exhibits a decrease with decreasing temperature which is consistent with the hypothesis that SrMn₂Ge₂ is an AFM with TN>350T_N > 350 K, as is reported for the neighbouring compounds CaMn₂Ge₂ and BaMn₂Ge₂, as well as related compound EuMn₂Ge₂, which has similar lattice parameters and G-type AFM structure (Table 1). [24] The value of χint=2.1×10−3 cm3/mol\chi_{\mathrm{int}} = 2.1 \times10^{-3}\ \mathrm{cm^3/mol} at T=2 KT = 2\ \mathrm{K} is similar to what is reported for the related compounds BaMn2_2Pn2_2 (Pn=P, As, Sb, BiPn = \mathrm{P},\ \mathrm{As},\ \mathrm{Sb},\ \mathrm{Bi}). [27, 42, 46, 47] While temperature-dependent neutron diffraction measurements are required to confirm the exact nature of the magnetic ground state, this agreement further supports the consistency of the above approach and suggests for a long-range AFM ground state for SrMn2_2Ge2_2.

Zero-field-cooled magnetic susceptibility and magnetization curves

Figure 2. (a) Zero-field-cooled magnetic susceptibility χ=M/H\chi= M/H of SrMn₂Ge₂ as a function of temperature TT, measured in an applied magnetic field μ0H=3\mu_0H = 3 T. The orange diamonds represent the χ\chi values obtained from linear fits to the magnetic isotherms M(H)M(H) shown in panel (b) for μ0H>2\mu_0H > 2 T. The solid orange line connecting the diamonds is a guide to the eye. (b) Magnetization MM versus HH at five different temperatures.

Electrical transport and magnetoresistance

Electrical resistivity ρ\rho of SrMn2_2Ge2_2 exhibits a monotonic increase with increasing TT at high temperatures and has a finite value at the lowest TT of our measurement, highlighting the metallic nature of the compound (Figure 3 (a)). The observed metallic behavior is consistent with heat capacity measurements and electronic structure calculations discussed later in the text. Furthermore, at low temperatures and in the absence of an applied field, the ρ(T)\rho(T) data exhibits Kondo-like features, where a resistivity minimum and maximum appear at T∼17T \sim17 and ∼5.5 K\sim5.5\ \mathrm{K}, respectively. These features are highlighted on a semi-log scale in the inset of Figure 3 (a). The high-field ρ(T)\rho(T) data measured at μ0H=7 T\mu_0H = 7\ \mathrm{T} overlaps with the zero-field data for T≳160 KT \gtrsim160\ \mathrm{K}, below which large and positive MR is observed. Such large and positive MR is unusual but not unique, and has been previously reported in the related compound LaMn2_2Ge2_2, where MR values approaching 100% were observed at 4.2 K under an applied field of 7 T. [22] The Kondo-like features observed at low temperatures in the absence of an applied field are smoothed out and partially suppressed upon application of the high field, resulting in a nearly constant ρ\rho below T∼7 KT \sim7\ \mathrm{K} [Inset, Fig. 3 (a)]. Additionally, the resistivity minimum located near T∼17 KT \sim17\ \mathrm{K} in zero field broadens and shifts to T∼44 KT \sim44\ \mathrm{K} under μ0H=7 T\mu_0H = 7\ \mathrm{T} suggesting a magnetic origin.

Resistivity and magnetoresistance of SrMn2Ge2

Figure 3. (a) Resistivity ρ\rho of SrMn2_2Ge2_2 as a function of temperature TT at two different fields μ0H=0\mu_0H = 0 and 77 T. Inset: Low-TT features of ρ(T)\rho(T) displayed on a semi-log scale. (b) Magnetoresistance (MR) versus HH at five different temperatures. Inset: MR versus HH for T≤50T \le50 K on a log-log scale.

Figure 3(b) shows the MR =ρ(H)−ρ(0)ρ(0)= \frac{\rho(H)-\rho(0)}{\rho(0)} versus HH, measured at five temperatures between 2 and 200 K. The measured MR values are consistently positive and increase monotonically with increase in HH. Additionally, the MR of SrMn2_2Ge2_2 does not follow a quadratic field dependence, which indicates the presence of correlated multiband electrical transport and/or complex magnetic scatterings. When plotted on a log-log scale, the MR data for T≤50 KT \le50\ \mathrm{K} exhibit the same sub-quadratic power-law dependence for all isotherms [Inset, Fig. 3 (b)]. Linear fits to these MR isotherms for fields ≥1 T\ge1\ \mathrm{T} results in a power-law exponent of n=1.50(8)n = 1.50(8).

Heat capacity

The isobaric heat capacity Cp(T)C_p(T) of SrMn2_2Ge2_2 does not show any evidence of a phase transition within the measured range of 1.8 K≤T≤300 K1.8\ \mathrm{K} \le T \le300\ \mathrm{K} (Figure 4). Furthermore, the CpC_p data saturate to the Dulong-Petit limit of CV=3nR=15R=124.7 J/(mol K)C_V = 3nR = 15R = 124.7\ \mathrm{J/(mol\ K)} at room temperature, where n=5n = 5 is the number of atoms per formula unit and RR is the molar gas constant.

Heat capacity of SrMn2Ge2

Figure 4. Heat capacity CpC_{\mathrm{p}} as a function of temperature TT for SrMn2_2Ge2_2. The solid green curve is a Debye model fit to the data as described in the text. Inset: Cp/TC_{\mathrm{p}}/T vs T2T^2 at low temperatures. The solid curve corresponds to a fit to the data using Eq. (1a), while the solid line represents a fit using Eq. (1b).

The Cp/TC_p/T versus T2T^2 data exhibits a linear behavior for T<4 KT < 4\ \mathrm{K}, but over all exhibits a positive curvature at low temperatures [Inset, Figure 4], indicating the possible dominance of a higher-order term proportional to T5T^5 in lattice contribution to the CpC_p. A similar positive curvature is observed in the related Mn-based insulator BaMn2_2P2_2. [27] Thus, the low-TT Cp/TC_p/T data were fitted using two different equations: Eq. (1a), which indicates the dominance of a higher-order term manifested as a positive curvature, and Eq. (1b), which assumes its absence, leading to a linear variation below 4 K.

Cp/T=γ+βT2+δT4,(1)C_p/T = \gamma+ \beta T^2 + \delta T^4, \tag*{(1)}
Cp/T=γ+βT2,(2)C_p/T = \gamma+ \beta T^2, \tag*{(2)}

where β\beta and δ\delta are coefficients describing the lattice vibrational contribution to CpC_p at low temperatures, and γ\gamma is the Sommerfeld coefficient representing the electronic contribution to CpC_p. A good fit to the data was obtained using both methods, resulting in the following fitted parameters: Eq. (1a): γ=6.9(2) mJ/mol K2\gamma= 6.9(2)\ \mathrm{mJ/mol\ K^2}, β=0.11(2) mJ/mol K4\beta= 0.11(2)\ \mathrm{mJ/mol\ K^4}, and δ=0.006(3) mJ/mol K6\delta= 0.006(3)\ \mathrm{mJ/mol\ K^6}; and Eq. (1b): γ=6.3(3) mJ/mol K2\gamma= 6.3(3)\ \mathrm{mJ/mol\ K^2} and β=0.24(2) mJ/mol K4\beta= 0.24(2)\ \mathrm{mJ/mol\ K^4}. The non-zero γ\gamma confirms a metallic ground state of SrMn2_2Ge2_2, in agreement with the ρ(T)\rho(T) data, as well as the electronic structure results described below. Moreover, the γ\gamma can be used to estimate the experimental DOS at the Fermi level EFE_F, Dγ(EF)D^\gamma(E_F) using,

γ=π2kB23Dγ(EF).(3)\gamma= \frac{\pi^2 k_{\mathrm{B}}^2}{3}D^\gamma(E_F). \tag*{(3)}

This yields Dγ(EF)=2.93(8) states/eV f.u.D^\gamma(E_F) = 2.93(8)\ \mathrm{states/eV\ f.u.} [Eq. (1a)] and 2.7(2) states/eV f.u.2.7(2)\ \mathrm{states/eV\ f.u.} [Eq. (1b)]. Furthermore, the Debye temperature ΘD\Theta_{\mathrm{D}} can be calculated from the β\beta obtained above using,

ΘD=(12π4Rn5β)1/3.(4)\Theta_{\mathrm{D}} = \left(\frac{12\pi^4 R n}{5\beta}\right)^{1/3}. \tag*{(4)}

The estimated values are ΘD=445(20) K\Theta_{\mathrm{D}} = 445(20)\ \mathrm{K} [Eq. (1a)] and 346(4) K346(4)\ \mathrm{K} [Eq. (1b)]. The ΘD\Theta_{\mathrm{D}} obtained from Eq. (1a) is significantly larger than those reported for BaMn2_2P2_2 and BaMn2_2As2_2, namely 348(17) and 246(4) K, respectively. [27, 42] In contrast, the ΘD\Theta_{\mathrm{D}} estimated from Eq. (1b) is in better agreement with the reported values. Hence, it remains unclear if the use of a higher-order term that seems to dominant at elevated temperatures is physically realistic or not. Such behaviors may also indicate the presence of some sort of structural or electronic anomaly influencing the low-temperature properties.

The Cp(T)C_p(T) data over the measured temperature range of 1.8 K<T<300 K1.8\ \mathrm{K} < T < 300\ \mathrm{K} were fitted using

Cp(T)=γT+nCVD(T),(5)C_p(T) = \gamma T + nC_{\mathrm{VD}}(T), \tag*{(5)}

where n=5n = 5 and γ=6.9(2) mJ/mol K2\gamma= 6.9(2)\ \mathrm{mJ/mol\ K^2} were held fixed to the value obtained above. Here CVD(T)C_{\mathrm{VD}}(T) is the Debye model heat capacity of acoustic phonons given by the expression

CVD(T)=9R(TΘD)3∫0ΘD/Tx4ex(ex−1)2 dx,(6)C_{\mathrm{VD}}(T) = 9R\left(\frac{T}{\Theta_{\mathrm{D}}}\right)^3 \int_0^{\Theta_{\mathrm{D}}/T}\frac{x^4 e^x}{(e^x-1)^2}\,dx, \tag*{(6)}

A high-accuracy Padé approximant [48] of the integral in Eq. (6) was used, and the obtained fit was satisfactory [Figure 4]. The fitted ΘD=284(3) K\Theta_{\mathrm{D}} = 284(3)\ \mathrm{K}, which is significantly lower than that obtained from the low-temperature Cp(T)C_p(T) data, appears more reasonable, as the Cp(T)C_p(T) data show a clear tendency to saturate toward the Dulong-Petit limit near room temperature. While the exact reason for this discrepancy is not clear, we anticipate that this might arise because of the TT-dependence of ΘD\Theta_{\mathrm{D}}, which is observed in several materials.[49]

Electronic structure

ThCr2_2Si2_2-type compounds with high c/ac/a ratios and ucT tetragonal structure often exhibit quasi-2D features in their electronic and magnetic properties. Additionally, the electronic band structures of these compounds often feature flat bands which, if in close proximity to the Fermi level EFE_{\mathrm{F}}, can result in substantial electronic instabilities.[38] Given the relatively small c/ac/a ratio exhibited by SrMn2_2Ge2_2, it was unclear whether quasi-2D properties and flat bands will occur in this compound. To investigate the potential occurrence of these features in the electronic structure of SrMn2_2Ge2_2, we first computed the total energy for the FM configuration, as well as three different AFM configurations—A-type, C-type, and G-type (see Table 2). The G-type AFM configuration, adopted by CaMn2_2Ge2_2 and BaMn2_2Ge2_2,[24] resulted in the lowest total energy. Using this AFM configuration, we obtain magnetic moments of 3.28 and 3.77 μB\mu_{\mathrm{B}}/Mn atom with PBEsol and r2^2SCAN, respectively.

The electronic band structure of SrMn2_2Ge2_2 features a confluence of bands at the Z-point, with multiple crossings just above the EFE_{\mathrm{F}} (Figure 5). The r2^2SCAN, which typically captures correlation effects to a greater extent, pushes these bands apart reducing the metallicity of the compound. This behavior is further evidenced by Figure 6, where the Dband(EF)D^{\mathrm{band}}(E_{\mathrm{F}}) is found to decrease when computed using the r2^2SCAN functional resulting in 0.8 states/(eV f.u.) compared to the PBEsol value of 2.1 states/(eV f.u.). These values are lower than the Dγ(EF)D^{\gamma}(E_{\mathrm{F}}) we obtained from the Cp(T)C_{\mathrm{p}}(T) data (see § 3.4) indicating the presence of substantial electronic correlation effects and associated quasiparticle mass enhancement in SrMn2_2Ge2_2. Further, the band structure of SrMn2_2Ge2_2 does not exhibit dispersion-less bands near EFE_{\mathrm{F}}, suggesting the absence of electronic instabilities in this compounds. The closest flat band to the EFE_{\mathrm{F}} is located approximately 0.75 eV above EFE_{\mathrm{F}} between the XX and RR points. Hence, we conclude that the electronic structure exhibits 3D characteristics, which is consistent with the crystal structure revealing a relatively low c/ac/a ratio and a short dGe−Ged_{\mathrm{Ge-Ge}}.

Electronic band structure of SrMn₂Ge₂

Figure 5. Electronic band structure of SrMn₂Ge₂ calculated using PBEsol (solid blue lines) and r2SCAN (dotted orange lines). All calculations have been performed using the G-type AFM configuration.

Total, atom-decomposed, and orbital-decomposed density of states

Figure 6. (a) Total and atom-decomposed density of States (DOS) computed with PBEsol (left panel) and r2r^{2}SCAN (right panel), and (b) orbital-decomposed DOS computed with PBEsol (left panel) and r2r^{2}SCAN (right panel) for SrMn2_{2}Ge2_{2} using the G-type AFM configuration.

Ordering typePBEsolr2SCAN
NM1.7423.797
FM0.4030.384
AFM-A0.3820.477
AFM-C0.1420.145
AFM-S0.3660.358
AFM-G00

Table 2. Density functional theory total energies per formula unit in electron volts for the different magnetic configurations, relative to the G-type antiferromagnetic (AFM-G) ground state, calculated using the PBEsol and r2SCAN exchange-correlation functionals. The abbreviations are defined as follows: nonmagnetic (NM); ferromagnetic (FM); and antiferromagnetic (AFM).

Discussion

To gain deeper insight, the structural and physical properties of tetragonal compounds AMn2Ge2\mathrm{A}\mathrm{Mn}_{2}\mathrm{Ge}_{2} (A=Ca,Sr,Ba\mathrm{A} = \mathrm{Ca}, \mathrm{Sr}, \mathrm{Ba}) need to be evaluated in comparison to those of LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2} and BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2} (Pn=P,As,Sb,Bi\mathrm{Pn} = \mathrm{P}, \mathrm{As}, \mathrm{Sb}, \mathrm{Bi}). On one hand, LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2} appears structurally closer to SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, exhibiting a similar c/ac/a ratio and dGe−Ged_{\mathrm{Ge-Ge}}. On the other hand, BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2} shows similarities of magnetic ground states, as infered by the same G-type AFM spin structure and similar values of observed Mn magnetic moment. [24, 50]

It has been established that in ThCr2_{2}Si2_{2}-type 122 pnictides, the interlayer coupling between the Pn\mathrm{Pn}-ions controls dPn−Pnd_{\mathrm{Pn-Pn}}. Consequently, dPn−Pnd_{\mathrm{Pn-Pn}} correlates with the effective ionic state of the transition metal ions, and as a result, with the magnetic ground state of the compounds. [38] The uncollapsed tetragonal (ucT) structure of BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2} infers a weak interlayer coupling between the Pn\mathrm{Pn}-ions, leading to a Pn−3\mathrm{Pn}^{-3} valence state. This further results in a +2+2 valence state of the Mn ions. In contrast, for collapsed tetragonal (cT) SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, the small dGe−Ged_{\mathrm{Ge-Ge}} indicates interlayer Ge-Ge dimerization. Following the analogy of the Pn\mathrm{Pn}-counterparts, this dimerization would result into the Ge valence valency that is likely similar to those of Pn\mathrm{Pn}-ions. This could stabilize a +2+2 valence state of the Mn ions in SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, and hence, result in a magnetic moment similar to those of BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2}. We emphasize that the ionic valence picture often breaks down in metallic systems. Therefore, the above discussion is intended only to provide a qualitative understanding of the similar magnetic features of SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2} and BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2}. Neutron diffraction measurements are essential to explore the underlying magnetic structure of the material. Additionally, detailed spectroscopic and transport properties studies are required to achieve a deeper understanding of the complex mechanisms that govern the magnetism and its manifestations in this unexplored compound.

Furthermore, the magnetic interactions and the resulting properties of ucT semiconducting BaMn2Pn2\mathrm{BaMn}_{2}\mathrm{Pn}_{2} compounds have been successfully described using J1J_{1}-J2J_{2}-JcJ_{c} Heisenberg model of stacked-square lattice of Mn-moments. [50] Here, J1J_{1} and J2J_{2} represent the nearest and next-nearest neighbor intralayer exchange interactions within the Mn square lattice, respectively, while JcJ_{c} denotes the interlayer exchange interaction between adjacent Mn layers along the crystallographic cc-axis. It would be interesting to explore whether the same model remains applicable in the case of cT metallic SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, where metallic nature may lead to a pronounced itinerant character and the three-dimensional character of the underlying magnetic sublattice may require additional exchange parameters.

The observed magnetoresistance (MR) of SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2} is intriguing and indicates that a multiband conduction mechanism, as well as complex magnetic scattering processes are likely present and dominant. Here, of course, we assume that the presence of small amount of Mn5Ge3\mathrm{Mn}_{5}\mathrm{Ge}_{3} impurity does not significantly affect the conduction mechanism within the primary phase. Somewhat similar observations of positive MR have been reported in LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2}. [22] However, in contrast to a power-law dependence of MR on HH in SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, the MR in LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2} exhibits a nearly linear dependence on HH. Additionally, LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2} displays complex competing magnetic states below its Tc=326T_{c} = 326 K, which can be described as an evolving nonlinear conical spin structure with a ferromagnetic component. [17] Therefore, a direct comparison of the magnetotransport properties of SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2} vis-a-vis LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2} may not be prudent. Nevertheless, the intriguing observation of giant room-temperature topological Hall effect in LaMn2Ge2\mathrm{LaMn}_{2}\mathrm{Ge}_{2}, which is relevant to spintronics applications, motivates a careful investigation of the magnetic ground state, as well as of the electronic transport mechanism in SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2}, preferably using single-crystal samples.

Conclusion

A comprehensive investigation of the physical properties of the previously unexplored tetragonal compound SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2} is reported. Powder x-ray diffraction data confirm the ThCr2_{2}Si2_{2}-type structure. Magnetic measurements are consistent with a possible antiferromagnetic ground state with a TN>350T_{N} > 350 K; however, high-temperature measurements and neutron diffraction studies are necessary to confirm the magnetic ground state. The heat capacity data, together with electronic structure calculations, suggest for the presence of sizable electronic correlations in the material. Notably, SrMn2Ge2\mathrm{SrMn}_{2}\mathrm{Ge}_{2} exhibits an unusually large magnetoresistance of approximately 50% at low temperatures, obeying a power-law field dependence with an exponent of n=1.50(8)n = 1.50(8). This intriguing observation indicates the dominance of a multiband conduction mechanism, as well as the presence of complex magnetic scattering processes. Furthermore, the low-TT resistivity data exhibits Kondo-like features. The intriguing properties of SrMn2_{2}Ge2_{2} warrant further investigation, particularly on high-quality single crystals, using microscopic probes such as neutron diffraction and scattering, NMR, ARPES, and XPS. Such studies would provide deeper insight into its magnetic and electronic properties and help understand the mechanisms that govern the observed phenomena.

Conflicts of interest

There are no conflicts to declare.

Data availability

Electronic structure input and output files are available at the open data repository with the following DOI: https://doi.org/10.5281/zenodo.19330078.

All data supporting the findings of this study are available within the article and/or its supplementary information.

Acknowledgements

This work is based on the research supported in part by the National Research Foundation of South Africa (Ref Numbers: SRUG2205098188). A.P. acknowledges the financial support from the Friedel Sellschop fellowship of the University of the Witwatersrand, South Africa. RW acknowledges the Centre for High Performance Computing (CHPC), South Africa, for providing computational resources to this research project.

References

  1. [1]M Rotter, M. Tegel, and D. Johrendt, Phys. Rev. Lett., 2008, 101, 107006.
  2. [2]J. Paglione and R. L. Greene, Nat. Phys., 2010, 6, 645.
  3. [3]D. C. Johnston, Adv. Phys., 2010, 59, 803.
  4. [4]G. Stewart, Rev. Mod. Phys., 2011, 83, 1589.
  5. [5]A. Sapkota, B. G. Ueland, V. K. Anand, N. S. Sangeetha, D. L. Abernathy, M. B. Stone, J. L. Niedziela, D. C. Johnston, A. Kreyssig, A. I. Goldman, and R. J. McQueeney, Phys. Rev. Lett., 2017, 119, 147201.
  6. [6]A. Pandey,B. G. Ueland, S. Yeninas, A. Kreyssig, A. Sapkota, Yang Zhao, J. S. Helton, J. W. Lynn, R. J. McQueeney, Y. Furukawa, A. I. Goldman, and D. C. Johnston, Phys. Rev. Lett., 2013, 111, 047001.
  7. [7]B. G. Ueland, A. Pandey, Y. Lee, A. Sapkota, Y. Choi, D. Haskel, R. A. Rosenberg, J. C. Lang, B. N. Harmon, D. C. Johnston, A. Kreyssig, and A. I. Goldman, Phys. Rev. Lett., 2015, 114, 217001.
  8. [8]A. Pandey and D. C. Johnston, Phys. Rev. B, 2015, 92, 174401.
  9. [9]K. K. Huynh, T. Ogasawara, K. Kitahara, T. Tanabe, S. Y. Matsushita, T. Tahara, T. Kida, M. Hagiwara, D. Arčon, and Tanigaki K, Phys. Rev. B, 2019, 99, 195111.
  10. [10]T. Ogasawara, K. Huynh, T. Tahara, T. Kida, M. Hagiwara, D. Arčon, M. Kimata, S. Y. Matsushita, K. Nagata, and K. Tanigaki, Phys. Rev. B, 2021, 103, 125108.
  11. [11]T. Ogasawara, K. K. Huynh, S. Y. Matsushita, M. Kimata, T. Tahara, T. Kida, M. Hagiwara, D. Arčon, and K. Tanigaki, Phys. Rev. B, 2022, 106, L041114.
  12. [12]N. P. Kolmakova, A. A. Sidorenko, and R. Z. Levitin, Low Temp. Phys., 2002, 28, 653.
  13. [13]M. Duraj, R. Duraj, A. Szytula, and Z. Tomkowicz, J. Magn. Magn. Mater., 1988, 73, 240.
  14. [14]R. B. van Dover, E. M. Gyorgy, R. J. Cava, J. J. Krajewski, R. J. Felder, and W. F. Peck, Phys. Rev. B, 1993, 47, 6134.
  15. [15]15 M. L. McLanahan , D. Lederman , and A. P. Ramirez, Phys. Rev. Mater., 2025, 9, L051402.
  16. [16]16 R. Welter, G. Venturini, E. Ressouche, and B. Malaman, J. Alloys Compd., 1995, 218, 204.
  17. [17]17 G. Gong, L. Xu, Y. Bai, Y. Wang, S. Yuan, Y. Liu, and Z. Tian, Phys. Rev. Mater., 2021, 5, 034405.
  18. [18]18 S. Roychowdhury, P. Yanda, K. Samanta, C. Yi, M. Yao, F. Orlandi, P. Manuel, D. Khalyavin, E. Giuseppe Della Valle, P. Constantinou, V. N. Strocov, M. G. Vergniory, C. Shekhar, and C. Felser, Adv. Mater., 2024, 36, 2305916.
  19. [19]19 H. Fujii, T. Okamoto, T. Shigeoka, T. Shigeoka, N. Iwata, Solid State Commun., 1985, 53, 715.
  20. [20]20 T. Shigeoka, N. Iwata, H. Fujii, and T. Okamoto, J. Magn. Magn. Mater., 1985, 53, 83.
  21. [21]21 X. X. Wang , W. Q. Wang, W. D. Hutchison, C. W. Wang, H. Y. Hao, F. Su, Y. F. Xue, J. C. Debnath, S. J. Campbell, Z. X. Cheng, and J. L. Wang, J. Alloys Compd., 2022, 909, 164784.
  22. [22]22 R. Mallik, E. V. Sampathkumaran, and P. L. Paulose, Appl. Phys. Lett., 1997, 71, 2385.
  23. [23]23 E. V. Sampathkumaran, P. L. Paulose, and R. Mallik, Phys. Rev. B, 1996, 54, R3710.
  24. [24]24 B. Malaman, G. Venturini, R. Welter, and E. Ressouche, J. Alloys Compd., 1994, 210, 209.
  25. [25]25 R. Welter, I. Ijjaali, G. Venturini, E. Ressouche, B. Malaman, J. Magn. Magn. Mater., 1998, 187, 278D292.
  26. [26]26 W. Dorrscheidt, N. Niess, and H. Schafer Z. Naturforsch. B, 1976, 31, 890.
  27. [27]27 B. S. Jacobs and A. Pandey, Phys. Rev. Mater., 2023, 7, 044410.
  28. [28]28 J. Rodríguez-Carvajal, Physica B, 1993, 192, 55; see also www.ill.eu/sites/fullprof/
  29. [29]29 J. J. Mortensen et al., J. Chem. Phys., 2024, 160, 092503.
  30. [30]30 A. H. Larsen et al., J. Phys.: Condens. Matter, 2017, 29, 273002.
  31. [31]31 J. Enkovaara et al., J. Phys.: Condens. Matter, 2010, 22, 253202.
  32. [32]32 J. J. Mortensen, L. B. Hansen, and K. W. Jacobsen, Phys. Rev. B, 2005, 71, 035109.
  33. [33]33 J. W. Furness, A. D. Kaplan, J. Ning, J. P. Perdew, and J. Sun, J. Phys. Chem. Lett., 2020, 11, 8208.
  34. [34]34 J. W. Furness, A. D. Kaplan, J. Ning, J. P. Perdew, and J. Sun, J. Phys. Chem. Lett., 2020, 11, 9248.
  35. [35]35 S. Lehtola, C. Steigemann, M. J. T. Oliveira et al., SoftwareX, 2018, 7, 1.
  36. [36]36 J. P. Perdew, A. Ruzsinszky, G. I. Csonka, O. A. Vydrov, G. E. Scuseria, L. A. Constantin, X. Zhou, and K. Burke, Phys. Rev. Lett., 2008, 100, 136406.
  37. [37]37 L. A. Constantin, J. P. Perdew, and J. M. Pitarke, Phys. Rev. B, 2009, 79, 075126.
  38. [38]38 A. Pandey, D. G. Quirinale, W. Jayasekara, A. Sapkota, M. G. Kim, R. S. Dhaka, Y. Lee, T. W. Heitmann, P. W. Stephens, V. Ogloblichev, A. Kreyssig, R. J. McQueeney, A. I. Goldman, A. Kaminski, B. N. Harmon, Y. Furukawa, and D. C. Johnston, Phys. Rev. B, 2013, 88, 014526.
  39. [39]39 G. Venturini, R. Welter, E. Ressouche, and B. Malaman, J. Alloys Compd., 1994, 210, 213.
  40. [40]40 M. Hofmann, S. J. Campbell, and A. V. J. Edge, Phys. Rev. B, 2004, 69, 174432.
  41. [41]41 I. Felner and I. Nowik, J. Phys. Chem. Solids, 1978, 39, 763.
  42. [42]42 Y. Singh, A. Ellern, and D. C. Johnston, Phys. Rev. B, 2009, 79, 094519.
  43. [43]43 Songlin, Dagula, O. Tegus, E. Brück, F.R de Boer, and K. H. J Buschow, J. Alloys Compd., 2002, 337, 269.
  44. [44]44 K. Synoradzki, K. Urban, P. Skokowski, H. Głowiński, and T. Toliński, Magnetism, 2022, 2, 56.
  45. [46]46 N. S. Sangeetha, V. Smetana, A.-V. Mudring, and D. C. Johnston, Phys. Rev B, 2018, 97, 014402.
  46. [47]47 B. Saparov and A. S. Sefat, J. Solid State Chem., 2013, 204, 32.
  47. [48]48 R. J. Goetsch, V. K. Anand, A. Pandey, and D. C. Johnston, Phys. Rev. B, 2012, 85, 054517.
  48. [49]49 E. S. R. Gopal, Specific heats at low temperatures, Plenum, New York, 1966.
  49. [50]50 D. C. Johnston, R. J. McQueeney, B. Lake, A. Honecker, M. E. Zhitomirsky, R. Nath, Y. Furukawa, V. P. Antropov, and Y. Singh, Phys. Rev. B, 2011, 84, 094445.

Paper details

vlnc:W_8sth4pp9
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents