High-Efficiency and Large Supercurrent Rectification with Superconducting Coil

Abstract

Superconducting diodes (SDs) are devices that rectify supercurrent through the difference in the superconducting critical current (Ic) between forward and reverse current directions. For bringing such SDs closer to practical superconducting power electronics applications, a combination of both high rectification efficiency (η) and a large Ic difference (ΔIc) is required. Here, we propose and demonstrate a coil-shaped superconducting wire device concept to induce a large SD effect, arising from the compensation between an external magnetic field (Hext) and the field generated by the coil itself. From transport Ic measurements on coil-shaped SDs based on a Sn10-Pb90 solder wire, we achieved a η of 79% with a ΔIc of 140 A at Hext = 500 Oe (coil #2) and a η of 84% with a ΔIc of 125 A at Hext = 530 Oe (coil #3), confirming high rectification values at large supercurrents. The large-current high-efficiency SDE in the coil-shaped SDs will be highly useful for developing the potential field of supercurrent power electronics.

Funding: TMU research fund for young scientists, JST-ERATO (No.: JPMJER2201), and JSPS-KAKENHI (No. 26K22467)

Introduction

Superconducting diodes (SDs) exhibit nonreciprocity in their superconducting critical current (IcI_{\mathrm{c}}); the IcI_{\mathrm{c}} differs between forward and reverse-direction current (Ic+≠∣Ic−∣I_{\mathrm{c}}^{+} \ne\lvert I_{\mathrm{c}}^{-}\rvert). [1, 2, 3, 4] Here, each direction is typically defined as Ic+>∣Ic−∣I_{\mathrm{c}}^{+} > \lvert I_{\mathrm{c}}^{-}\rvert. The SD effect (SDE) has attracted much attention since its observation in Nb-V-Ta superlattice in 2020, where it originates from the simultaneous breaking of spatial-inversion and time-reversal symmetries. [5] Since then, the SDE has been studied in a wide variety of systems, including unconventional-superconducting materials, [6, 7, 8] Josephson junctions, [9, 10, 11] and thin films and crystal flakes. [12, 13]

The most important parameters of SDs are the rectification efficiency (η\eta), which is defined as η=(Ic+−∣Ic−∣)/(Ic++∣Ic−∣)\eta= (I_{\mathrm{c}}^{+} - \lvert I_{\mathrm{c}}^{-}\rvert) / (I_{\mathrm{c}}^{+} + \lvert I_{\mathrm{c}}^{-}\rvert) and the critical-current difference (ΔIc=Ic+−∣Ic−∣\Delta I_{\mathrm{c}} = I_{\mathrm{c}}^{+} - \lvert I_{\mathrm{c}}^{-}\rvert). [14] To enable practical applications in e.g., large-scale superconducting power electronics, the simultaneous achievement of a high η\eta (ideally perfect rectification of η=100%\eta= 100\%), and a large ΔIc\Delta I_{\mathrm{c}} is essential. In low-current devices (ΔIc<10\Delta I_{\mathrm{c}} < 10 mA), relatively high η\eta have been reported under standard measurement conditions with a DC current: η=65%\eta= 65\% in a Pt/V/EuS trilayer film and η=60%\eta= 60\% in a cuprate Josephson junction. [1, 12, 15] A recent work also demonstrated perfect rectification in cuprate Josephson junctions with ΔIc∼1\Delta I_{\mathrm{c}} \sim1 mA albeit using more complex experimental conditions including microwave irradiation. [16] η>50%\eta> 50\% was observed in a YBCO/PrBCO multilayer film but the observed ΔIc\Delta I_{\mathrm{c}} was lower than 1 A. [17] However, when it comes to large supercurrents, so far only low η\eta have been obtained, with a device composed of a cuprate coated conductor and a pair of permanent magnets with antiparallel magnetizations obtaining η∼15%\eta\sim15\% with ΔIc\Delta I_{\mathrm{c}} of 181 A [18]. Thus, to the best of our knowledge, no SD has yet simultaneously achieved a high η\eta (>60%> 60\%) and a large ΔIc\Delta I_{\mathrm{c}} exceeding 100 A.

One of the potential applications for the above mentioned large-current SDs is high-current DC excitation, essential for superconducting magnets employed in emerging applications such as superconducting rotating machines and magnetic refrigeration, where classical current rectification introduces substantial thermal loads into the cryogenic environment. [19, 20, 21] Contactless flux-pump technologies have therefore been actively investigated to energize superconducting field coils. [18] Furthermore, if high-efficiency large current SDs working at T=77T = 77 K can be developed using cuprates, such devices could become essential for a future superconducting power grid system. [22] In this present work, to achieve both requirements of a high η\eta and a large ΔIc\Delta I_{\mathrm{c}}, we propose a coil-shaped superconducting wire device concept to induce a large SDE. We experimentally demonstrate that the device achieves performances of η=79%\eta= 79\% with a ΔIc\Delta I_{\mathrm{c}} of 140 A and an η=84%\eta= 84\% with a ΔIc\Delta I_{\mathrm{c}} of 125 A at T=4.2T = 4.2 K.

Results

Concept and Base Design

As illustrated in Figure 1a, a supercurrent flowing in a coil-shaped superconducting wire generates a magnetic field Hin(I)\mathbf{H}_{\mathrm{in}}(I) with a magnitude of Hin(I)H_{\mathrm{in}}(I) that is, according to the solenoid equation based on Ampère's circuital law, of Hin(I)∼IN/LH_{\mathrm{in}}(I) \sim IN/L with II being the current, NN the number of turns, and LL the length of the coil or solenoid. Given an external magnetic field Hext\mathbf{H}_{\mathrm{ext}} with a magnitude of HextH_{\mathrm{ext}} applied parallel to Hin\mathbf{H}_{\mathrm{in}}, the magnitude of total self-induced magnetic field inside the coil is expressed by Htotal∼∥Hext±Hin(I)∥H_{\mathrm{total}} \sim\lVert\mathbf{H}_{\mathrm{ext}} \pm\mathbf{H}_{\mathrm{in}}(I) \rVert, with the sign depending on the direction of the current. The critical current IcI_{\mathrm{c}} (at which HtotalH_{\mathrm{total}} is the critical field HcH_{\mathrm{c}}) will then also depend on the direction of the current, inducing the SDE. As such, the present design utilizes the limitation of superconducting coils due to field generated by themselves as shown by Onnes[23] but aims to create the non-reciprocity by adding an external field.

Concept and $I_{\mathrm{c}}$ measurements for coil diode

Figure 1. Concept and IcI_{\mathrm{c}} measurements for coil diode (#1). a) External field (HextH_{\mathrm{ext}}) and inductive field (HinH_{\mathrm{in}}) by the supercurrent with forward and reverse directions (I+I^{+} and I−I^{-}). b) A photograph of the measurement configuration with Sn10-Pb90 coil sample (#1) and current and voltage terminals. Additional voltage terminals are prepared to investigate the problem of quenching the wire outside the coil (see dashed white circle). c) VV-II data taken with I+I^{+} and I−I^{-} at T=4.2T = 4.2 K and Hext=250H_{\mathrm{ext}} = 250 Oe, plotted with red and blue circles, respectively. d) HextH_{\mathrm{ext}} dependence of IcI_{\mathrm{c}} at T=4.2T = 4.2 K. The dashed lines are theoretical values of Ic+I_{\mathrm{c}}^{+} and Ic−I_{\mathrm{c}}^{-} estimated from Ic0I_{\mathrm{c0}} and Hc=570H_{\mathrm{c}} = 570 Oe (see Supporting Information for the formula). HextH_{\mathrm{ext}} dependence of expected ΔIc\Delta I_{\mathrm{c}} and rectification efficiency.

According to the working principle, if HextH_{\mathrm{ext}} is set close to HcH_{\mathrm{c}}, a small current on the direction where the generated Hin\mathbf{H}_{\mathrm{in}} is the same as Hext\mathbf{H}_{\mathrm{ext}} (I−I^{-}) would immediately result in surpassing HcH_{\mathrm{c}}, and thus, going to the normal-conducting phase, while a large current window on the opposite direction (I+I^{+}) would be available at the superconducting phase, theoretically providing very high rectification efficiencies close to η∼100%\eta\sim100\%. As summarized in Supporting Information, the SDE parameters within this concept can ideally be described as the following: ΔIc=2Ic0(Hext/Hc)\Delta I_{\mathrm{c}} = 2I_{\mathrm{c0}}(H_{\mathrm{ext}}/H_{\mathrm{c}}) and η=Hext/Hc\eta= H_{\mathrm{ext}}/H_{\mathrm{c}} where Ic0I_{\mathrm{c0}} is the IcI_{\mathrm{c}} at Hext=0H_{\mathrm{ext}} = 0 Oe. Because of the simple working principle, the design strategy proposed here is highly scalable and versatile, allowing for bulk-scale SDs useful for large-scale superconductor applications.

To demonstrate this concept, we created a coil-shaped wire made of Sn-Pb solder (coil diode #1) and performed a four-terminal voltage (VV)-II measurement under Hext\mathbf{H}_{\mathrm{ext}} (Figure 1b). HcH_{\mathrm{c}} of the Sn10-Pb90 solder is 570 Oe, close to that of pure Pb (See Figure S1 for the magnetic characterization for a sample consisting of a small cylinder cut off from a similar wire) because the Sn-Pb solder is a phase-separated superconductor composed of Sn and Pb. [24, 25, 26] We note that, for a type-I superconductor, the demagnetization effect is crucial for discussing HcH_{\mathrm{c}},[27] and the effect can largely affect the diamagnetic property of coil-shaped samples. Since the precise evaluation of the demagnetization effect of complex or large samples such as the present device is complicated, we use the value of Hc=570H_{\mathrm{c}} = 570 Oe estimated from a cylindrical sample with demagnetization-effect correction.

Magnetization dependence on external magnetic field for Sn10-Pb90 solder

Figure S1. HextH_{\mathrm{ext}} dependence of magnetization for Sn10-Pb90 solder at T=4.2T = 4.2 K. Original data has been published in T. Ichikawa et al., Jpn. J. Appl. Phys. 65 100904 (2026). Magnetization was measured using a superconducting quantum interference device (SQUID) magnetometer MPMS3 (Quantum Design) under various fields in the SQUID-VSM mode.

Figure 1c shows a VV-II measurement result at Hext=250H_{\mathrm{ext}} = 250 Oe. Both curves display superconducting behavior below IcI_{\mathrm{c}}, and the voltage dramatically shoots up due to the phase transition from superconducting to normal-conducting state. As expected from the working principle discussed above, for the reverse direction, a smaller Ic−=47.42 AI_{\mathrm{c}}^{-} = 47.42\ \mathrm{A} is obtained, while on the forward direction it is of Ic+=122.70 AI_{\mathrm{c}}^{+} = 122.70\ \mathrm{A}, resulting in a ΔIc\Delta I_{\mathrm{c}} of ∼75 A\sim75\ \mathrm{A} and η=44%\eta= 44\%, experimentally proving the concept. As shown in Figure S2, at Hext>250 OeH_{\mathrm{ext}} > 250\ \mathrm{Oe}, I+I^{+} data could not be obtained due to the quenching at the wire outside the coil, detected by the additional voltage terminal (Figure 1a); the IcI_{\mathrm{c}} of the lead-wire part is consistent with our previous experiments on the same composition (see Figure S3).[26] Noticeably, the voltage near the coil was still zero with I+I^{+} at Hext>250 OeH_{\mathrm{ext}} > 250\ \mathrm{Oe}, which suggests that the Ic+I_{\mathrm{c}}^{+} of the coil part should have still increased with increasing HextH_{\mathrm{ext}}, but the external quenching prevented it from reaching further. In Figure 1d, the experimentally measured HextH_{\mathrm{ext}} dependence of IcI_{\mathrm{c}} is shown. The results are well consistent and in good qualitative agreement with the predicted trends by the coil-shaped SDE parameter ΔIc=2Ic0(Hext/Hc)\Delta I_{\mathrm{c}} = 2I_{\mathrm{c}0}(H_{\mathrm{ext}}/H_{\mathrm{c}}): for I−I^{-}, we observe a linearly decreasing trend converging to 0 at around Hext=Hc=570 OeH_{\mathrm{ext}} = H_{\mathrm{c}} = 570\ \mathrm{Oe}. As for Ic+I_{\mathrm{c}}^{+}, it displays a linearly increasing trend, with a slope similar but opposite to that in I−I^{-} given the additional current needed to first compensate for the opposing HextH_{\mathrm{ext}} and then, in addition, needed to reach HcH_{\mathrm{c}}. Finally, the experimentally obtained ΔIc\Delta I_{\mathrm{c}} and η\eta are shown in Figure 1e as a function of HextH_{\mathrm{ext}}, with the largest values within the measured range (with I+I^{+} lower than IcI_{\mathrm{c}} of the wire part) being ΔIc=75 A\Delta I_{\mathrm{c}} = 75\ \mathrm{A} and η=44%\eta= 44\% at Hext=250 OeH_{\mathrm{ext}} = 250\ \mathrm{Oe}.

V-I measurements near the coil and lead part and external-field dependence of critical currents

Figure S2. (a–c) VV-II measured near the coil and the lead part (see Figure 1a). The sudden increase in blue-triangle data indicates quench at the wire part. (d) HextH_{\mathrm{ext}} dependence of critical currents, Ic+I_{\mathrm{c}}^{+} and IcI_{\mathrm{c}} (lead), for Sn10-Pb90 solder.

Plot of critical current as a function of external magnetic field for a straight-shaped Sn10-Pb90 wire

Figure S3. Hext dependence of IcI_c for a straight-shaped Sn10-Pb90 wire. The original data has been published in T. Ichikawa et al., Jpn. J. Appl. Phys. 65 100904 (2026).

In order to better understand the relation between the experimentally obtained IcI_{\mathrm{c}} and HcH_{\mathrm{c}}, finite element method (FEM) simulations of electromagnetic fields were performed with the commercial software COMSOL Multiphysics® v. 6.4,[28] using the classical Maxwell equations built in the magnetic fields interface of the AC/DC module. The simulation results, summarized in Figure S4 and Figure S5, show that the coil IcI_{\mathrm{c}} is governed by local maximum field in the inner edge. As shown in Figure S4, the experimental results shown in Figure 1 are nicely explained by total field at the wire inner edge. The simulation results confirm that the relevant parameters in coil-shaped SDs can be understood, on a first approximation, with simple electromagnetism for the Sn10-Pb90 wire. Although Ic+I_{\mathrm{c}}^{+} of coil #1 at Hext>250 OeH_{\mathrm{ext}} > 250\ \mathrm{Oe} was not experimentally reached due to the quenching, a larger ΔIc\Delta I_{\mathrm{c}} and a higher η\eta are expected at Hext>250 OeH_{\mathrm{ext}} > 250\ \mathrm{Oe} as shown in Figure S5. Therefore, we next investigate the intrinsic SDE properties of an improved Sn10-Pb90 coil diode design for measurements at Hext>250 OeH_{\mathrm{ext}} > 250\ \mathrm{Oe} by modifying the lead part to prevent quenching outside the coil.

Finite element simulations for the spatial distribution of the magnetic field magnitude around a coil-shaped wire

Figure S4. Finite element simulations for the spatial distribution of the magnetic field magnitude around a coil-shaped wire. (a) 3D rendering of the model coil used. (b,c,d) Calculated HtotalH_{\mathrm{total}} along (b) the center axis of the coil and (c) across cross-sectional cuts of the model, as displayed in (d) the 2D projection of the model on the xzxz-plane cutting the middle of the coil. (e) Color map depicting the HedgeH_{\mathrm{edge}} as a function of HextH_{\mathrm{ext}} and II, together with the HextH_{\mathrm{ext}} dependence of IcI_{\mathrm{c}} at the inner edge (green solid line) and center of the coil (purple dotted line). The experimental points from Figure 1c (green circles) are shown for comparison.

Plot of critical currents versus external magnetic field

Figure S5. HextH_{\mathrm{ext}} dependence of critical currents, Ic+I_{\mathrm{c}}^{+} and Ic−I_{\mathrm{c}}^{-}, for Sn10-Pb90 solder with Hc=570H_{\mathrm{c}} = 570 Oe at T=4.2T = 4.2 K.

High-Efficiency SDE with Superconducting Coil

In Figure 2a, we summarize the coil sample designed to prevent the lead-part quenching at Hext>250H_{\mathrm{ext}} > 250 Oe. We use pure-Cu lead (1.5 mm in diameter) having electrical resistance low enough for IcI_{\mathrm{c}} measurements at I<200I < 200 A at T=4.2T = 4.2 K. We measured two different coil diodes (#2 and #3) with opposite winding directions as shown in Figure 2b (coil diode #2 is right-handed, and #3 is left-handed). Both coil diodes are composed of the Sn10-Pb90 solder wire part (8.5 turns) and the outer pure-Cu wire parts. To avoid weak coupling between the Sn10-Pb90 and the Cu wires, the first and second turns on the outside of the coil are covered by soldering. As reported in Ref. 29, the normal-state resistivity (ρ\rho) of Sn-Pb solder is ρ∼3\rho\sim3 nΩm at T=4.2T = 4.2 K, significantly higher than the typical value of pure Cu with ρ∼0.01\rho\sim0.01 nΩm at T=4.2T = 4.2 K. Therefore, the heating and/or the increase in resistance at the Cu part can be assumed to be negligible in the IcI_{\mathrm{c}} measurement with the examined current range. The voltage terminals are attached to the Sn10-Pb90 wire at about 7.4 cm apart.

Critical current experiments, including schematic, coil photographs, and current–voltage data

Figure 2. Critical current experiments. a) Schematic image of the concept. b) Sample photographs for coils with opposite winding directions. c,d) Typical data for the current dependence of voltage for the right- and left-handed coil diodes (#2 and #3). Here, the criterion for estimating IcI_{\mathrm{c}} is 1 μ\muV/cm. I+I^{+} and I−I^{-} denote the current directions.

Figure 2c and Figure 2d show the selected current dependence of voltage (VV-II) at T=4.2T = 4.2 K for coil diodes #2 and #3. The other VV-II data are displayed in Figure S6 and Figure S7. We determine IcI_{\mathrm{c}} with the 1 μV/cm criterion. For coil #2, the highest η\eta of 79% is observed with ΔIc=140\Delta I_{\mathrm{c}} = 140 A at Hext=500H_{\mathrm{ext}} = 500 Oe. For coil #3, the highest η\eta of 84% is observed with ΔIc=125\Delta I_{\mathrm{c}} = 125 A at Hext=530H_{\mathrm{ext}} = 530 Oe. Although the obtained SDE properties are slightly different between #2 and #3, the results at all the examined fields are comparable. This suggests that the winding direction, right-handed or left-handed, does not affect the working performance of the coil-shaped SDs.

V-I data taken at various Hext for coil diode #2

Figure S6. VV-II data taken at various HextH_{\mathrm{ext}} for coil diode #2.

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=0\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3, left-handed; $\Delta I_{\mathrm{c}}\sim 0.5\ \mathrm{A}$ ($\eta\sim 0.3\%$), with $I^{+}$ and $I^{-}$ curves

(a)

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=100\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3; $\Delta I_{\mathrm{c}}\sim 23\ \mathrm{A}$ ($\eta\sim 12\%$), with $I^{+}$ and $I^{-}$ curves

(b)

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=300\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3; $\Delta I_{\mathrm{c}}\sim 87\ \mathrm{A}$ ($\eta\sim 44\%$), with $I^{+}$ and $I^{-}$ curves

(c)

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=500\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3; $\Delta I_{\mathrm{c}}\sim 147\ \mathrm{A}$ ($\eta\sim 77\%$), with $I^{+}$ and $I^{-}$ curves

(d)

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=530\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3; $\Delta I_{\mathrm{c}}\sim 125\ \mathrm{A}$ ($\eta\sim 84\%$), with $I^{+}$ and $I^{-}$ curves

(e)

V-I data at $T=4.2\ \mathrm{K}$ and $H_{\mathrm{ext}}=550\ \mathrm{Oe}$ for an Sn10-Pb90 coil, coil diode #3; $\Delta I_{\mathrm{c}}\sim 83\ \mathrm{A}$ ($\eta\sim 82\%$), with $I^{+}$ and $I^{-}$ curves

(f)

Figure S7. VV-II data taken at various HextH_{\mathrm{ext}} for coil diode #3.

In Figure 3, Ic+I_{\mathrm{c}}^{+} and Ic−I_{\mathrm{c}}^{-} for coils #2 (Figure 3a) and #3 (Figure 3b) are plotted as a function of HextH_{\mathrm{ext}}. Owing to the improved device design with the pure-Cu lead parts, which avoids quenching outside the coil, Ic+I_{\mathrm{c}}^{+} at higher HextH_{\mathrm{ext}} are reachable in these coils. For both coils, ∣Ic−∣\lvert I_{\mathrm{c}}^{-} \rvert linearly decreases with increasing HextH_{\mathrm{ext}}. Ic+I_{\mathrm{c}}^{+} shows a monotonous increase with increasing HextH_{\mathrm{ext}} up to 400 Oe, but the increase is moderated at Hext>400H_{\mathrm{ext}} > 400 Oe, showing a deviation from the idealized sample and measurement set-up, shown with the dashed lines, suggesting the presence of additional constraints to reach the ideal rectification. Nonetheless, experimentally, the largest Ic+I_{\mathrm{c}}^{+} is observed at Hext∼500H_{\mathrm{ext}} \sim500 Oe for both coils with η=79%\eta= 79\% and 84%, both cases record-high values among the SDE studies with conventional measurement conditions with a DC current.

External field dependence of $I_c$ for the coil diodes, a) #2 and b) #3

Figure 3. External field dependence of IcI_c for the coil diodes, a) #2 and b) #3. The dashed lines are theoretical values estimated from Ic0I_{c0} and Hc=570H_c = 570 Oe.

Discussion

To compare our data with other SDs’ performance, η\eta (higher than 60% for our coil-shaped SDs) is plotted as a function of ΔIc\Delta I_{\mathrm{c}} and working temperature in Figure 4a and Figure 4b. In Figure 4a, we can clearly see that the present work achieved a significant improvement in η\eta for large ΔIc\Delta I_{\mathrm{c}} devices. As for a broader comparison including lower ΔIc\Delta I_{\mathrm{c}}, we observe that only the microwave-irradiated designs, which require much more complex operating conditions, have reported higher η\eta, with our device showing a significant improvement also with respect to other conventional SDs. Our coil-shaped SDs show a high η\eta with a large ΔIc\Delta I_{\mathrm{c}} exceeding 100 A under low operating magnetic field of ∼500\sim500 Oe that can be readily achieved using an ordinary permanent magnet, which are suitable for practical large-current superconductor applications. According to the working principle, ΔIc\Delta I_{\mathrm{c}} becomes larger with increasing zero-field IcI_{\mathrm{c}}, which can be enhanced by a reduction of turn number and/or an increase in HcH_{\mathrm{c}} (or irreversible field of type-II superconductors) by changing the coil material. However, the current working temperature is T=4.2T = 4.2 K, and there is room for improvement for η>60%\eta> 60\% and T>4.2T > 4.2 K; working temperatures of T=20T = 20 and 77 K are important for practical applications with liquid hydrogen and nitrogen. This suggests a potential direction for further exploration using the same concept of coil-shaped SDs using superconductors different from the Sn10\mathrm{Sn}_{10}-Pb90\mathrm{Pb}_{90} solder such as Nb3Sn\mathrm{Nb}_{3}\mathrm{Sn} or cuprate wires that could result in higher working temperatures.

Comparison of the rectification efficiency as functions of a) $\Delta I_{\mathrm{c}}$ and b) experiment temperature

Figure 4. Comparison of the rectification efficiency as functions of a) ΔIc\Delta I_{\mathrm{c}} and b) experiment temperature. The efficiency data for the conventional SDs are mainly provided from J. Ma et al.[1] We included a record-high data for SD without microwave irradiation reported in arXiv.[32]

At the same time, the suppression of Ic+I_{\mathrm{c}}^{+} and deviation from the theoretical expectations for increased HextH_{\mathrm{ext}} shows that there might still be room for design optimization and improvement. In the present work, we do not have a clear answer to the Ic+I_{\mathrm{c}}^{+} deviation from the theoretical value near HcH_{\mathrm{c}} within the present experiments, but Ic+I_{\mathrm{c}}^{+} might be sensitive to small deviations in the field direction or the coil structure including wire diameter or shape. These are thus parameters that could further be explored in future designs. Further improvement of SDE properties including working temperature will improve the performance of various superconducting devices driven with a large current and be an essential tool for developing future superconducting power electronics.[19, 20, 21, 22, 30, 31]

Figures

Conclusion

In this study, we propose coil-shaped SD as a new design strategy to achieve a giant supercurrent rectification and experimentally demonstrate that the coil-shaped Sn10-Pb90 wire shows SDE. The development of SDs had been so far mainly limited to the nano- and micro-scale given their use of thin films and nano- and micro-fabrication approaches, resulting in a focus on small-scale potential applications such as quantum computing. The bulk-scale SDs presented in this work features a simpler design and higher efficiency, and expands the possibilities of bulk-scale SDs to large-scale applications. We demonstrate that a coil-shaped Sn10-Pb90 SD with pure-Cu lead parts exhibits high η\eta and large ΔIc\Delta I_{\mathrm{c}}. We experimentally observed a large enhancement of Ic+I_{\mathrm{c}}^{+} by the field cancellation principle at higher HextH_{\mathrm{ext}}. The highest η\eta values are 79% with ΔIc=140\Delta I_{\mathrm{c}} = 140 A (coil #2) and 84% with $\Delta I_{\mathrm{c}} = 125 A (coil #3), marking a significant improvement to large supercurrent SDs as well as to overall conventional SDs. High-performance SDs with a large ΔIc\Delta I_{\mathrm{c}} will open new pathway for versatile superconducting power applications.

Materials and Methods

Sample information

The measurements were performed using a Sn10-Pb90 (wt.%) solder cylindrical wire with a diameter of 1.65 mm (Sasaki Solder Industry). For coil #2 and #3, the solder wire was connected with pure-Cu wires (99.9%) with a diameter of 1.5 mm (Nilaco). The diameter of pure-Cu wire is enough for IcI_{\mathrm{c}} measurements with I<200I < 200 A. The solder wire and the Cu wire were connected by soldering, and the overlapping parts were covered by solders to enhance the joint IcI_{\mathrm{c}}.

IcI_{\mathrm{c}} measurement for coil diode #1

The transport IcI_{\mathrm{c}} for coil #1 was measured using the cryostat system in NIMS by a standard four-probe method using a Keithley 2182A nanovoltmeter (see Figure 1b for the measured sample). Continuous DC current was used for the measurement, and the sweep speed from zero to the highest current was 20-30 s. Both ends of the solder wire were mechanically fixed to the current terminals. The voltage taps were bonded using low-melting-point solder (U-Alloy 95) and protected with adhesive tape. The distance between the voltage taps near the coil ends was about 10.6 cm. The applied HextH_{\mathrm{ext}} was parallel to the coil-length direction. Measurements were performed in liquid He, and the IcI_{\mathrm{c}} was evaluated using a criterion of 0.1 μV cm−1\mu\mathrm{V\,cm}^{-1}.

IcI_{\mathrm{c}} measurement for coil diodes #2 and #3

The transport IcI_{\mathrm{c}} for coil diodes #2 and #3 was measured using the cryostat system in IMR, Tohoku University, by a standard four-probe method using a Keithley 2182A nanovoltmeter (see Figure 2b). Both ends of the solder coil were connected with the Cu wires by soldering using a Sn40-Pb60 solder. The sample was fixed to the current terminals by soldering using a low-melting-point solder (In52-Sn48). This In52-Sn48 solder was also used for attaching the voltage terminals to the Sn10-Pb90 coil part. The sweep rate of the DC current from zero to the maximum value was 30 sec. The applied field (HextH_{\mathrm{ext}}) was almost parallel to the coil-length direction, and the actual field was measured by a Hall device. The measurements were performed in liquid He, and the IcI_c was evaluated using a criterion of 1 μV cm−11\ \mu\mathrm{V}\,\mathrm{cm}^{-1}.

Acknowledgements

T. Ichikawa and D. Takegami equally contributed to this work. The authors thank M. Mashiko, Y. Watanabe, and T. Ozaki for supports and discussion on this research. The authors thank J. Ma and X. Lin for providing the source data for the efficiency plots published in their review article. This work was partly supported by TMU research fund for young scientists, JST-ERATO (No.: JPMJER2201), and JSPS-KAKENHI (No. 26K22467).

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Conflict of Interest

The authors declare no conflict of interest.

Supporting Information

Expected SDE performances of coil superconducting diodes

We demonstrate that the ideal critical current difference (ΔIc\Delta I_{\mathrm{c}}) and rectification efficiency (η\eta) are determined by Ic0I_{\mathrm{c0}} (IcI_{\mathrm{c}} at Hext=0H_{\mathrm{ext}} = 0 Oe) and the critical current HcH_{\mathrm{c}}. Ic0I_{\mathrm{c0}} depends on the coil shape and the turn number. Because the generated field (HcoilH_{\mathrm{coil}}) is proportional to current in a coil, Ic−I_{\mathrm{c}}^{-} is described as Ic−=Ic0[1−(Hext/Hc)]I_{\mathrm{c}}^{-} = I_{\mathrm{c0}}[1 - (H_{\mathrm{ext}}/H_{\mathrm{c}})]. Similarly, Ic+I_{\mathrm{c}}^{+} is described as Ic+=Ic0[1+(Hext/Hc)]I_{\mathrm{c}}^{+} = I_{\mathrm{c0}}[1 + (H_{\mathrm{ext}}/H_{\mathrm{c}})]. Therefore, the ideal ΔIc(Hext)\Delta I_{\mathrm{c}}(H_{\mathrm{ext}}) and η(Hext)\eta(H_{\mathrm{ext}}) are described as following.

ΔIc=2Ic0(HextHc)\Delta I_{\mathrm{c}} = 2I_{\mathrm{c0}}\left(\frac{H_{\mathrm{ext}}}{H_{\mathrm{c}}}\right)
η=(HextHc)\eta= \left(\frac{H_{\mathrm{ext}}}{H_{\mathrm{c}}}\right)

Finite element method simulations

Finite element method (FEM) simulations of electromagnetic fields were performed with the commercial software COMSOL Multiphysics® v. 6.4, using the classical Maxwell equations built in the magnetic fields interface of the AC/DC module. The core part of the coil was modelled using a solenoid with an inner diameter of 2 mm, a wire diameter of 1.65 mm and an axial pitch of 2.5 mm, resulting in a total length of around 21 mm. Additional cylindrical and toroidal elements were attached to the ends to simulate the straight and curved sections of the contacts respectively, as shown in Figure S4, although the details on the external elements did not result in significant differences in the area of interest within and surrounding the coil. A constant intensity of II was set entering / exiting through the contacts as boundary conditions, and the current density within the wire was simulated based on Ohm’s law. We note that the present calculations are a first approximation based on the classical, normal conduction equations. An electric permittivity of εr=1010\varepsilon_r = 10^{10}, relative permeability of μr=10−5\mu_r = 10^{-5} and resistivity of ρ=10−15Ωm\rho= 10^{-15}\Omega\mathrm{m} were used for the wire. A box of empty space of 4 cm × 4 cm × 20 cm was defined centered at the coil to allow for enough space for the out magnetic flux lines to propagate. The external field was simulated by setting homogeneous magnetic field along the z direction on the top and bottom surfaces of the box. The remaining faces, and in the case of zero field calculations, all faces, were set as magnetic insulators, i.e. with the perpendicular component of the field to be 0.

Figure S4–Figure S4 display the spatial distribution of the magnetic field using the parameters Hext=250H_{\mathrm{ext}} = 250 Oe and I±=±80I^{\pm} = \pm80 A. For I−I^{-}, the magnetic field generated inside the coil due to the current is on the same direction as the external field, with their magnitudes adding up, and resulting in a field well above the experimentally determined HcH_{\mathrm{c}}, as observed in the magnetic field along the central axis of the coil, represented in Figure 3b. Meanwhile, for I+I^{+}, given the opposite direction of the magnetic field generated by coil and HextH_{\mathrm{ext}}, the field inside is still well below HcH_{\mathrm{c}}, of the order of ∣Hcoil−Hext∣\lvert H_{\mathrm{coil}} - H_{\mathrm{ext}}\rvert where HcoilH_{\mathrm{coil}} denotes HH generated by the coil. This would result in the wire remaining superconducting only for I+I^{+}, as conceptualized and experimentally demonstrated above. We observe that the field, which outside the coil is of HextH_{\mathrm{ext}}, decreases near the boundary of the coil, dropping to 0 and then increasing again in magnitude after HcoilH_{\mathrm{coil}} surpasses HextH_{\mathrm{ext}}. Additional non-trivial asymmetric behavior is present between I±I^{\pm}, due to the distortion of the external field in presence of the coil. Figure S4 displays a colourmap of the magnetic field magnitude distribution generated by the model coil on top of an external field. Outside the coil, we observe uniformly low values due to the magnetic field lines being highly dispersed through all the available space. On the other hand, the values inside the coil are much higher due to the concentration of the field. The field inside is far from homogeneous, with the field in the vicinity of the wires being significantly higher. In the cross-sectional cut, shown in Figure S4, the field at the inner edges of the coil reaches values around 1.5 times higher than that in the center. This behavior is to be expected, given the 1/d1/d (dd being the distance) dependence of the magnetic field generated by a straight wire section. With this behavior in mind, we can now calculate for a range of values in order to obtain the theoretically expected HextH_{\mathrm{ext}} dependence of IcI_{\mathrm{c}} according to our finite element model. In Figure S4, we show a color map of the HtotalH_{\mathrm{total}} at the inner edge of the wires forming the coil, with the dashed region denoting the parameter space where Htotal>Hc=570H_{\mathrm{total}} > H_{\mathrm{c}} = 570 Oe. The cutoff boundary where Htotal=HcH_{\mathrm{total}} = H_{\mathrm{c}} (corresponding to IcI_{\mathrm{c}}), shown by the green line, is in excellent agreement with the experimentally measured values, showing that the magnetic field magnitude at the inner edge provides a much better prediction of the characteristics of coil-shaped SD devices. The agreement of the IcI_{\mathrm{c}} values obtained with a simplified FEM analysis shows that the working parameters of the coil-shaped SD can be estimated with low-cost computational models using classical electromagnetism. Meanwhile, the cutoff values and IcI_{\mathrm{c}} obtained from the center of the coil in our model (dotted purple line in Figure S4) are in full agreement with the results obtained with the solenoid equation, indicating, thus, consistency of our FEM analysis with the theoretical equations.

References

  1. [1]J. Ma, R. Zhan, and X. Lin, Superconducting Diode Effects: Mechanisms, Materials and Applications., Adv. Phys. Res. 4 (2025): 2400180. DOI: https://doi.org/10.1002/apxr.202400180.
  2. [2]M. Nadeem, M. S. Fuhrer, and X. Wang, The superconducting diode effect., Nat. Rev. Phys. 5 (2023): 558. DOI: https://doi.org/10.1038/s42254-023-00632-w.
  3. [3]H. Narita and T. Ono, Superconducting diode effect in artificial superlattices., JSAP Rev. (2024): 240206. DOI: https://doi.org/10.11470/jsaprev.240206.
  4. [4]V. M. Edelstein, Magnetoelectric Effect in Polar Superconductors., Phys. Rev. Lett. 75 (1995): 2004. DOI: https://doi.org/10.1103/PhysRevLett.75.2004.
  5. [5]F. Ando, Y. Miyasaka, T. Li, J. Ishizuka, T. Arakawa, Y. Shiota, T. Moriyama, Y. Yanase, and T. Ono, Observation of superconducting diode effect., Nature 584 (2020): 373. DOI: https://doi.org/10.1038/s41586-020-2590-4.
  6. [6]T. Le, Z. Pan, Z. Xu, J. Liu, J. Wang, Z. Lou, X. Yang, Z. Wang, Y. Yao, C. Wu, and X. Lin, Superconducting diode effect and interference patterns in kagome CsV₃Sb₅., Nature 630(2024): 64. DOI: https://doi.org/10.1038/s41586-024-07431-y.
  7. [7]Z. Wan, G. Qiu, H. Ren, Q. Qian, Y. Li, D. Xu, J. Zhou, J. Zhou, B. Zhou, L. Wang, T.-H. Yang, Z. Sofer, Y. Huang, K. L. Wang, and X. Duan, Unconventional superconductivity in chiral molecule-TaS₂ hybrid superlattices., Nature 632 (2024): 69. DOI: https://doi.org/10.1038/s41586-024-07625-4.
  8. [8]L. Bauriedl, C. Bäuml, L. Fuchs, C. Baumgartner, N. Paulik, J. M. Bauer, K.-Q. Lin, J. M. Lupton, T. Taniguchi, K. Watanabe, C. Strunk, and N. Paradiso, Supercurrent diode effect and magnetochiral anisotropy in few-layer NbSe₂., Nat. Commun. 13 (2022): 4266. DOI: https://doi.org/10.1038/s41467-022-31954-5.
  9. [9]B. Pal, A. Chakraborty, P. K. Sivakumar, M. Davydova, A. K. Gopi, A. K. Pandeya, J. A. Krieger, Y. Zhang, M. Date, S. Ju, N. Yuan, N. B. M. Schröter, L. Fu, and S. S. P. Parkin, Josephson diode effect from Cooper pair momentum in a topological semimetal., Nat. Phys. 18 (2022): 1228. DOI: https://doi.org/10.1038/s41567-022-01699-5.
  10. [10]B. Turini, S. Salimian, M. Carrega, A. Iorio, E. Strambini, F. Giazotto, V. Zannier, L. Sorba, and S. Heun, Josephson Diode Effect in High-Mobility InSb Nanoflags., Nano Lett. 22 (2022): 8502. DOI: https://doi.org/10.1021/acs.nanolett.2c02899.
  11. [11]C. Baumgartner, L. Fuchs, A. Costa, S. Reinhardt, S. Gronin, G. C. Gardner, T. Lindemann, M. J. Manfra, P. E. Faria Junior, D. Kochan, J. Fabian, N. Paradiso, and C. Strunk, Supercurrent rectification and magnetochiral effects in symmetric Josephson junctions., Nat. Nanotechnol. 17 (2022): 39. DOI: https://doi.org/10.1038/s41565-021-01009-9.
  12. [12]Y. Hou, F. Nichele, H. Chi, A. Lodesani, Y. Wu, M. F. Ritter, D. Z. Haxell, M. Davydova, S. Ilić, O. Glezakou-Elbert, A. Varambally, F. S. Bergeret, A. Kamra, L. Fu, P. A. Lee, and J. S. Moodera, Ubiquitous Superconducting Diode Effect in Superconductor Thin Films., Phys. Rev. Lett. 131 (2023): 027001. DOI: https://doi.org/10.1103/PhysRevLett.131.027001.
  13. [13]U. Nagata, M. Aoki, A. Daido, S. Kasahara, Y. Kasahara, R. Ohshima, Y. Ando, Y. Yanase, Y. Matsuda, and M. Shiraishi, Field-Free Superconducting Diode Effect in Layered Superconductor FeSe., Phys. Rev. Lett. 134 (2025): 236703. DOI: https://doi.org/10.1103/PhysRevLett.134.236703.
  14. [14]A. Daido, Y. Ikeda, and Y. Yanase, Intrinsic Superconducting Diode Effect., Phys. Rev. Lett. 128 (2022): 037001. DOI: https://doi.org/10.1103/PhysRevLett.128.037001.
  15. [15]S. Ghosh, V. Patil, A. Basu, Kuldeep, A. Dutta, D. A. Jangade, R. Kulkarni, A. Thamizhave l, J. F. Steiner, F. von Oppen, and M. M. Deshmukh, High-temperature Josephson diode., Nat. Mater. 23 (2024): 612. DOI: https://doi.org/10.1038/s41563-024-01804-4.
  16. [16]H. Wang, Y. Zhu, Z. Bai, Z. Lyu, J. Yang, L. Zhao, X. J. Zhou, Q. K. Xue, D. Zhang, Quantum superconducting diode effect with perfect efficiency above liquid-nitrogen temperature., Nat. Phys. 22 (2026): 47. DOI: https://doi.org/10.1038/s41567-025-03098-y.
  17. [17]A. Mizuno, Y. Tsuchiya, S. Awaji, and Y. Yoshida, Rectification at Various Temperatures in YBa₂Cu₃Oᵧ Coated Conductors With PrBa₂Cu₃Oᵧ Buffer Layers., IEEE Trans. Appl. Supercond. 32 (2022): 6601005. DOI: https://doi.org/10.1063/5.0248777.
  18. [18]J. M. Brooks, R. Mataira, T. Simpson, R. A. Badcock, C. W. Bumby, A high-Tc superconducting diode with large current carrying capacity., Appl. Phys. Lett. 126 (2025): 082601. DOI: 10.1109/TASC.2022.3154325.a.DOI
  19. [19]S. Han, J. H. Kim, Y. S. Chae, S. H. Lee, H. L. Quach, T. K. Ko, Y. S. Yoon, H. M. Kim, Contactless superconducting field exciter with active current control using hybrid magnet for high-temperature superconducting rotating machine, Cryogenics 129 (2023): 103603. DOI: https://doi.org/10.1016/j.cryogenics.2022.103603.
  20. [20]A. Caughley, G. Lumsden, H. Weijers, S. Jeong, R. A. Badcock., Cooling of Superconducting Motors on Aircraft. Aerospace 11 (2024): 317. DOI: https://doi.org/10.3390/aerospace11040317.
  21. [21]N. Hirano, Y. Onodera, T. Mito, Y. Ueno, A. Kawagoe., Development of static magnetic refrigeration system using multiple high-temperature superconducting coils. IEEE Trans. Appl. Supercond. 32 (2022): 0500105. DOI: https://doi.org/10.1109/TASC.2022.3152456.
  22. [22]Brian G. Marchionini, Y. Yamada, L. Martini, H. Ohsaki, High-Temperature Superconductivity: A Roadmap for Electric Power Sector Applications, 2015–2030., IEEE Trans. Appl. Supercond. 27 (2017): 0500907. DOI: https://doi.org/10.1109/TASC.2017.2671680.
  23. [23]D. van Delft and P. Kes, The discovery of superconductivity., Phys. Today 63 (2010): 38. DOI: https://doi.org/10.1063/1.3490499.
  24. [24]J. D. Livingston, Magnetic properties of superconducting lead-base alloys., Phys. Rev. 129 (1963): 1943. DOI: https://doi.org/10.1103/PhysRev.129.1943.
  25. [25]H. Arima, M. R. Kasem, H. Sepehri-Amin, F. Ando, K. Uchida, Y. Kinoshita, M. Tokunaga, and Y. Mizuguchi, Observation of nonvolatile magneto-thermal switching in superconductors, Commun. Mater. 5 (2024): 34. DOI: https://doi.org/10.1038/s43246-024-00465-9.
  26. [26]T. Ichikawa, G. Nishijima, Y. Hattori, and Y. Mizuguchi, Enhancement of a transport critical current by flux trapping in Sn-Pb superconducting solder wire., Jpn. J. Appl. Phys. 65 (2026): 100904. DOI: https://doi.org/10.35848/1347-4065/ae6ea6
  27. [27]M. Tinkham, Introduction to Superconductivity., 2nd ed., McGraw-Hill, New York (1996).
  28. [28]COMSOL Multiphysics® v. 6.4. www.comsol.com. COMSOL AB, Stockholm, Sweden.
  29. [30]P. Mukherjee, and V. V. Rao, Design and development of high temperature superconducting magnetic energy storage for power applications- A review., Phys. C 563 (2019): 67. DOI: https://doi.org/10.1016/j.physc.2019.05.001.
  30. [31]T. A. Coombs, Q. Wang, A. Shah, J. Hu, L. Hao, I. Patel, H. Wei, Y. Wu, T. Coombs, W. Wang, High-temperature superconductors and their large-scale applications., Nat. Rev. Electrical Eng. 1 (2024): 788 (2024). DOI: https://doi.org/10.1038/s44287-024-00112-y.
  31. [32]R. D. H. Hinlopen, C. Putzke, L. Holeschovsky, R. Nicholls, F. Ronning, E. D. Bauer, N. E. Hussey, P. J. W. Moll, Programmable superconducting diode from nematic domain control in FeSe., arXiv: 2604.26631. DOI: https://doi.org/10.48550/arXiv.2604.26631.

Paper details

vlnc:W_8xqfvj23
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents