WorksPhysics and Astronomy
Non-coplanar helimagnetism in the layered van-der-Waals metal DyTe
Abstract
Magnetic materials with highly anisotropic chemical bonding can be exfoliated to realize ultrathin sheets or interfaces with highly controllable optical or spintronics responses, while also promising novel cross-correlation phenomena between electric polarization and the magnetic texture. The vast majority of these van-der-Waals magnets are collinear ferro-, ferri-, or antiferromagnets, with a particular scarcity of lattice-incommensurate helimagnets of defined left- or right-handed rotation sense, or helicity. Here we use polarized neutron scattering to reveal cycloidal, or conical, magnetic structures in DyTe, with coupled commensurate and incommensurate order parameters, where covalently bonded double-slabs of dysprosium square nets are separated by highly metallic tellurium layers. Based on this ground state and its evolution in a magnetic field as probed by small-angle neutron scattering (SANS), we establish a one-dimensional spin model with off-diagonal on-site terms, spatially modulated by the unconventional charge order in DyTe. The CDW-driven term couples to antiferromagnetism, or to the net magnetization in applied magnetic field, and creates a complex magnetic phase diagram indicative of competing interactions in an easily cleavable helimagnet. Our work paves the way for twistronics research, where helimagnetic layers can be combined to form complex spin textures on-demand, using the vast family of rare earth chalcogenides and beyond.
These two authors contributed equally to this work
‡ Present address: Department of Physics, Faculty of Mathematics and Natural Sciences, Universitas Indonesia, Depok 16424, Indonesia.
Magnetism in layered materials, held together by weak van-der-Waals interactions, is an active field of research spurred on by the discovery of magnetic ordering in monolayer sheets of ferromagnets and antiferromagnets [1, 2, 3, 4]. At the frontier of this field, helimagnetic layered systems, where magnetic order has a fixed, left- or right-handed rotation sense, have been predicted to host complex spin textures [5, 6] and to serve as controllable multiferroics platforms, where magnetic order is readily tuned by electric fields or currents [7, 8, 9, 10]. However, most layered van-der-Waals magnets are commensurate ferro-, antiferro-, or ferri-magnets [3, 4]; the rare helimagnets provided to us by nature are often modulated along the stacking direction, with relatively simple spin arrangement in individual layers (Table E1).
Table E1. Magnetic properties of van-der Waals systems with complex magnetic order. Electrical transport properties are categorized into metals (M), insulators (I), and materials with metal-to-insulator transition (MIT), and spin textures are classified into coplanar (CP) and noncoplanar (NCP). DyTe is the only metallic compound that is (a) incommensurate with the underlying lattice, and (b) has a component of the modulation vector perpendicular to the stacking direction. Moreover, it is a rare example of noncoplanar (NCP) magnetism in a bulk vdW compound.
In the quest for helimagnetism in layered structures with weak van-der-Waals bonds, we focus on rare earth tritellurides (: rare earth element). These materials form a highly active arena of research regarding the interplay of correlations and topological electronic states [11, 12, 13, 14, 15]. Their structure, which can be exfoliated down to the thickness of a few monolayers [16, 17], is composed of tellurium double-layers and covalently bonded slabs, with characteristic square net motifs in both (Figure 1a) [18]. Tellurium electrons are highly localized in square net bilayers ( plane), in which they form highly dispersive bands with elevated Fermi velocity [16, 19, 20, 21]. This quasi two-dimensional electronic structure amplifies correlation phenomena, such as the formation of charge-density wave (CDW) order [22] and superconductivity [23, 24], while also hosting protected band degeneracies [16, 25]. In view of intense research efforts on , it is remarkable that their magnetism has never been discussed in detail; in particular, no full refinement of magnetic structures is available [26, 27, 28, 29, 30, 31].
Figure 1. Conical helimagnetism in the layered square-lattice antiferromagnet . a, Crystallographic unit cell with covalently bonded DyTe bilayers and metallic Te bilayers, with natural cleaving plane (dashed). b, Magnetic exchange interactions in a single DyTe double-square net bilayer. c, Zigzag chain illustration of double-square net structure in . The interactions , connect nearest and next-nearest neighbours in the zigzag chain model, respectively; but the inter-atomic distance in the full crystallographic structure is shorter for , and its antiferromagnetic coupling strength is dominant. Conical, noncoplanar helimagnetism is resolved in the zero-field ground state by neutron scattering. The cone direction, parallel to the -axis, alternates both between pairs of magnetic sites in a zigzag chain, and between stacked zigzag chains. This texture causes polarization along the -axis, i.e. perpendicular to square net bilayers (yellow arrow). Note: The full magnetic unit cell extends two times further along the chain direction (Figure E1). d, Weak anisotropy of the magnetic susceptibility in . The softest direction is , consistent with the modulation direction of the magnetic order in panel c. The inset shows Curie-Weiss temperatures and temperatures of maximal , measured in a small magnetic fields along three crystallographic directions.
Here, we report on helimagnetic, cone-type orders of using polarized elastic neutron scattering. We reveal the magnetic texture in real space, probe its evolution with temperature and magnetic field, and reveal its relationship to charge-density wave formation. In , dysprosium moments are arranged in square net bilayers, where each ion has neighbours within its own layer, and within the respective other layer (Figure 1b). As all zero-field magnetic orders of are uniform along the crystallographic -axis, it is reasonable to understand each square net bilayer as an effective zigzag chain of magnetic rare earth ions and to define magnetic interactions and in terms of nearest- and next-#+#+#+#+ nearest neighbours on the zigzag chain, respectively. On such chains, our experiment shows that pairs of ions have cones pointing along the same direction, followed by a flip of the cone axis (Figure 1c, which illustrates half a magnetic unit cell). The coupling between two DyTe bilayers, i.e. between two zigzag chains, is antiferromagnetic. Despite this complex cone arrangement, the magnetic structure defines a fixed sense of rotation, or helicity. Our theoretical spin model shows that charge-density wave order in rare earth tellurides causes local symmetry breaking, allows for off-diagonal on-site coupling terms in the Hamiltonian, and drives lattice-incommensurate magnetism when combined with antiferromagnetic interactions or with a net magnetization. We further discuss magnetocrystalline anisotropy in this layered structure, with an unconventional combination of metallic and covalent bonds. Helimagnetism of Dy rare earth moments with magnetic shell emerges despite the naive expectation of strong preference for easy-axis or easy-plane anisotropy for , with large orbital angular momentum .
Magnetic properties of
Some essential magnetic properties of are apparent already from the magnetic susceptibility in Figure 1d. In the high temperature regime, anisotropy in the Curie-Weiss law indicates easy-plane behaviour of magnetic moments, favouring the plane with uniaxial anisotropy constant (Methods). At low temperatures, the strongest enhancement of occurs when the magnetic field is along the -axis, i.e. parallel to the zigzag direction defined in Figure 1c. We may deduce that the magnetic moments are aligned, predominantly, along the and axes. All susceptibility curves show maxima around , quite far above the onset of three-dimensional, long-range magnetic order, as shown in the following.
We characterize the phase transition in using thermodynamic and transport probes in Figure 2a,Figure 2b. The specific heat shows a two-peak anomaly, describing the transitions from the paramagnetic (PM) regime to phase II at and to phase I at . Below , the resistivities in the basal plane drop abruptly, suggesting a clear correlation between the behaviour of freely moving conduction electrons and the magnetic structure. The presence of a partial charge gap in the electronic structure, related to magnetic ordering, is inferred from an increase of the ratio of resistivities and . Simultaneously, as discussed in the following, strong neutron scattering intensity appears below at two independent positions in reciprocal space, c.f. Figure 2c. The magnetic scattering intensity rises abruptly upon cooling below .
Figure 2. Bulk characterization and magnetic structure of DyTe from elastic neutron scattering. a, Specific heat showing two transitions at and , with reference data from the nonmagnetic analogue LaTe [32]. b, Below , where resistivity in the basal plane drops sharply, significant anisotropy indicates (partial) gapping of electronic states along the -axis. c, Temperature dependence of magnetic scattering intensity for antiferromagnetic and cycloidal reflections, with Miller indices and , respectively. Grey and green background shading mark phases I and II, respectively. d, Experimental geometry for polarized neutron scattering from layered DyTe (grey plane, square net of Dy indicated). The scattering plane (blue) is spanned by wavevectors , of incoming and outgoing neutron beams, respectively. Separating spin-flip (SF, red) and non-spin flip (NSF, blue) scattering intensities at the detector, we identify conical magnetic order (top). e, Linescan in momentum space, with highlights for three types of reflections including a weak higher harmonic corresponding to . f, Simulation of magnetic intensity from magnetic structure model, corresponding to the linescan in panel e (Methods).
To obtain this neutron data, a single-domain crystal of DyTe is mounted on an aluminium holder and is pre-aligned by means of Laue x-ray diffraction. More quantitatively, we determine the crystallographic directions in DyTe using the crystallographic extinction rule (Extended Section, Figure E11). Figure 2d describes the geometry of our neutron scattering experiment. The scattering plane that includes the incoming and outgoing neutron beams and , is spanned by the - and -axes. Hence, reflections of the type with Miller indices can be detected, as in Figure 2e, where a line scan along provides sharp magnetic intensity. Three types of magnetic peaks , with a reciprocal lattice vector, are observed: A commensurate (C) reflection , ; an incommensurate (IC) reflection , , where and are reciprocal lattice constants (Methods). There is also a higher harmonic (3Q) reflection, corresponding to three times the length of , which describes an anharmonic distortion of the texture. As a main result of this work, we ascribe to a cycloidal structure in the magnetic ground state of DyTe, that results from a coupling between the C order and a charge-density wave (CDW) modulation at , in the rare earth tritelluride family.

Figure E11. Confirmation of crystallographic extinction rule in in sample A. Reflections are forbidden in (space group 63), or specifically is required in the scattering plane, which is used for the present experiment. We observe zero intensity at (031) and 800 counts per second (cps) at (021); the latter reflection is not shown in this figure. When instead rotating the sample into the scattering plane, (130) has 1200 cps and (120) exhibits zero intensity. Specifically, the comparison of (130) and (031) allows us to confirm the alignment of the crystal in our neutron experiment.
Ground state magnetic structure model
We reveal the helimagnetic structure in the ground state of DyTe using polarized neutron scattering. As shown in Figure 2d, the incident neutron spins were polarized perpendicular to the scattering plane. We employ a magnetized single-crystal analyzer to select the energy and spin state of the scattered neutrons (Methods). The scattering processes in which the neutron spins are reversed (remain unchanged) is referred to as spin-flip, SF (non-spin-flip, NSF). For SF scattering, it is required that magnetic moments have a component perpendicular to the spin of the incoming neutron. This means that SF and NSF scattering detect components of within and perpendicular to the scattering plane, respectively.
Polarization analysis of the magnetic reflections shows that and relate to different vector components of the ordered magnetic moment (Figure 3a,Figure 3b and Figure 3e,Figure 3f). We find no hint of SF scattering at , demonstrating collinear antiferromagnetism with magnetic moments exclusively along the -direction. The incommensurate part , in contrast, has no NSF intensity and roughly equal SF signals at various positions in reciprocal space (Figure 3e,Figure 3f and insets). As neutron scattering detects the part of that is orthogonal to , comparison of magnetic reflections situated at nearly orthogonal directions in momentum space suggests and components are both finite in the ground state.

Figure 3. Two components of the cone-type order in the ground state of DyTe. In the geometry of Figure 2d, non spin-flip (NSF) and spin-flip (SF) neutron scattering measure the magnetic moment along the crystallographic -axis and in the plane, respectively. a,b, Polarization analysis of antiferromagnetic component : absence of spin flip (SF) intensity indicates absence of and , while non-spin flip (NSF) intensity reveals dominant . c,d, Two views of the antiferromagnetic collinear component derived from this data, confirmed by full refinement of a number of magnetic reflections in Figure E8. e,f, Polarization analysis for the incommensurate cycloidal reflection . g, Derived magnetic structure model for , where (NSF) vanishes while and (SF) both appear at comparable magnitudes in phase I. The index labels four dysprosium atoms in four layers within the chemical unit cell (red box), where the cycloids at are phase-shifted with respect to cycloids at . The numerical value of is determined in § 6.6. As for a,b,e, and f, we have subtracted background signals, and corrected the effect of imperfect beam polarization.
We determine the quantitative relationship between magnetic moments within a DyTe bilayer (within an effective zigzag chain), by comparing the observed and calculated magnetic structure factors under the constraints imposed by polarized neutron scattering, c.f. Figure E8. The analysis for demonstrates up-up-down-down type ordering along the zigzag chain, visualized from two perspectives in Figure 3c,Figure 3d. At , the refinement yields a cycloid with a phase delay between the upper and lower sheets in a zigzag chain, see Figure 3g. In effect, pairs of nearly parallel magnetic moments are followed by a significant rotation of the moment direction. The coupling between zigzag chains is antiferromagnetic, as imposed by the Miller index () component in both and . Superimposing the three components , , and , we realize the noncoplanar, helimagnetic cone texture of Figure 1c that is, to our knowledge, unique in both insulators and metals. In Extended Sections E3 A, E4 A, we discuss the presence of magnetic domains in the sample and how the occurrence of higher harmonic reflections further supports our magnetic structure model.
Figure E8. Magnetic structure refinement for the ground state of DyTe. Antiferromagnetic (commensurate, ) and cycloidal (incommensurate ) components are refined separately from neutron scattering data, without polarization analyzer, at Ksample B. a, Averaging two AFM domains with equal weight, we find good agreement [reliability factor ] between the measured neutron structure factor and model calculations . b, Likewise, good agreement is found when summing two -domains for the incommensurate order . Here, we minimized by adjusting the value of the phase shift between sheets in a bilayer, as defined in Figure 3g, and the elliptic distortion of the cycloid (§ 6.6).
Charge density wave and magnetic order
We now argue that cone-type magnetism in is realized through (i) a spatial modulation of near-neighbour exchange interactions , in presence of charge-density wave (CDW) order and (ii) unconventional single-ion anisotropy. We turn first to (i), that is the role of the CDW in stabilizing noncoplanar helimagnetism in . We use a 1D chain model to reproduce key features of the modulated magnetic order, neglecting the material’s three-dimensionality (Methods).
In , the local environment and bond characteristics of dysprosium ions in a DyTe square net bilayer (in a zigzag chain) are spatially modulated by the CDW in the adjacent sheets, c.f. Figure 4b [11, 12, 13, 14, 18, 22, 23, 24, 31, 32, 33]. The simplest model approach is to decouple the zigzag chain, with two atoms per unit cell, into two one-dimensional chains, with one atom per unit cell. This allows for a two-parameter model, built from Ising-like exchange interactions together with a spatially modulated onsite coupling,

Figure 4. Modeling helimagnetism in DyTe3. a, Magnetic susceptibility for , overlaid with phase boundaries from specific heat (white open circles) and magnetization (black circles): I (conical ground state), II, III, IV, and V. b, Charge density wave (CDW) on tellurium layers [18], where orange (grey) spheres are distorted (undistorted) ionic positions. Coupling of Dy (violet) and CDW drives lattice-incommensurate magnetic order through spatially modulated modification of the local environment of Dy-ions. c, Squared moment amplitudes (blue) and (red) as functions of , where , from model calculations according to Eq. (1); five and ten percent threshold for the incommensurate part indicated by black and grey dashed lines (Methods). d, Local environment of Dy in DyTe3, with covalent (metallic) bonds to Te-B (Te-A) depicted by solid (dashed) lines, respectively. e, Charge density (CD) of Dy shell under the influence of crystal electric fields (CEF) from the surrounding ions, with exaggerated non-spherical part. If metallic and covalent bonds cause CEF of roughly equal strength (if metallic bonds are screened), oblate (prolate ) is the lowest energy CEF doublet. This favours out-of-plane (in-plane) magnetization, respectively. Colour on CD isosurfaces indicates amplitude of the local CEF. f,g Anisotropy constants and calculated for multiplet in DyTe3 (Methods). The abscissa describes the relative weight of CEF charges on Te-A and Te-B sites. Green lines bound an intermediate regime of weak , where spin tilting and conical order are allowed.
where counts magnetic sites, e.g., on the upper half of the zigzag chain. The are spatial positions along the zigzag chain (-axis). All the coupling constants – , , and – are positive. The and terms are allowed by global and local mirror symmetry breaking due to the CDW, respectively. We may also introduce a Zeemann term to explain the behavior in a magnetic field and further inter-chain coupling to connect the two chains (Extended Section E1).
This 1D model naturally creates different modulation period for the and spin components and robustly reproduces two types of magnetic reflections, and . In good consistency with experiment, Figure 4c shows that on the order of 10 % of can be induced within this model. Based on scattering techniques, we find it difficult to reveal the phase-shift between CDW and the spin cycloid, and between the antiferromagnetic and incommensurate components of the magnetic order; hence, alternative (out-of-phase) locking between cycloid and antiferromagnetic component is also possible (Figure E1).
Figure E1. Two possible magnetic structures in the ground state of . Neutron scattering does not constrain the combination of cycloidal (, ) and antiferromagnetic (AFM, ) components, which can be either in-phase (left) or out of phase (right). The AFM and cycloidal components of in-phase (out of phase) combinations are depicted, in panels b,c (in panels f, g), respectively. Only a single zigzag chain is shown, although there is antiferromagnetic coupling between subsequent zigzag chains along the -axis, c.f. Figure 1. d,h Magnetic texture in a single DyTe magnetic square net bilayer, corresponding to the simplified zigzag-chain picture in panels a,e. Colour on each ionic site (arrows) illustrate the -axis (the -plane) component of the magnetic moments. Dashed lines are guides to the eye, describing the square net in the upper sheet of the DyTe bilayer slab. The bright (dark) highlight marks the size of the magnetic unit cell (the size of half a magnetic unit cell, as shown in panels a-c, e-g, and in the figures of the main text). For clarity, the relative phase between the layers is chosen so that pairs of spins are fully collinear (instead of the experimentally determined 79° phase shift, § 6.6).
Weak magneto-crystalline anisotropy
While strongly anisotropic magnetism is naively expected for dysprosium’s shell, we here report a conical state with comparable , , in DyTe. Consider the local environment of a single Dy in Figure 4d: Te-B ions form covalent bonds with the central Dy, while the point charges of Te-A are effectively screened by itinerant electrons in the conducting tellurium slab. We model the sequence of crystal electric field (CEF) states for the shell of dysprosium as a function of the effective crystal field charge situated on Te-A and Te-B ions (Figure E15). Figure 4e illustrates two limiting cases: When Te-A and Te-B contribute equally to the CEF, the charge cloud is compressed along the -direction, with dominating the ground state wavefunction, and with effective out-of-plane magnetic anisotropy for magnetic moments. Likewise, zero contribution of Te-A, i.e. highly efficient metallic screening of CEFs, favours the prolate orbital with easy-axis anisotropy.

Figure E15. Crystal electric field calculations and local environment of Dy in DyTe3. a, Evolution of the energy gap between ground state doublet (GS, ) and the first (1st ES, ) or second (2nd ES, ) excited state Kramers doublets. We consider a (virtual) charge transfer from the metallic square net (Te-A) to the covalent bonded Tellurium (Te-B) ions, as sketched in the inset. The -axis is labeled by the ratio of effective point charges on the two types of Te ions. Within the red (grey) shaded area, the excitation gaps to the the first and second excited states are (to the first excited state is) on the order of the exchange interaction energy (dashed horizontal line). Panels b-d show the composition of in terms of eigenstates of (b-component of) total angular momentum with , as suitable for the shell of dysprosium. The are probabilities, i.e. absolute squares of amplitudes, for each contribution to the total wavefunction.
Adding exchange interactions as an effective magnetic field, the CEF Hamiltonian of a point charge model is diagonalized for the orthorhombic environment of Dy (Methods). The resulting free energy density described by two parameters , where , are spherical coordinates with respect to the and crystal axes, respectively. Figure 4 f, Figure 4g testify to a transition from easy-axis to easy-plane anisotropy through a sign change of at intermediate charge ratio (pink line)two green lines bound the regime where easy-axis (easy-plane) anisotropy is not strong enough to prevent tilting of along directions intermediate between -axis and the plane. Constraining in agreement with and requiring easy-plane anisotropy , we identify the black box in Figure 4 f, Figure 4g to capture a parameter range well consistent with experiment. Here, the model yields , meaning is preferred over .
Magnetic phase diagram and small-angle neutron scattering
We are ready, now, to consider the evolution of magnetic order in DyTe as a function of temperature and magnetic field. Figure 4a shows a contour map of the magnetic susceptibility (Methods), where the external magnetic field is applied along the in-plane direction [101], i.e. . Heating the sample above K in zero field, we observe a peak splitting of , and a concomitant shift in that indicates the sustained coupling of the two ordering vectors, via the CDW, at elevated temperatures (Figure E13). The sharp enhancement of in Figure 1a further suggests that , survive to higher temperature than , consistent with a putative incommensurate, fan-like order in phase II, which warrants further study.

Figure E13. Incommensurate and commensurate antiferromagnetic component in phase II of DyTe3 (sample A). a,b, Line scans of magnetic intensity through the incommensurate (a) and commensurate (b) reflection on the line, with clear temperature dependence. Shaded Gaussian curves at K indicate a double-Gaussian fit in the regime of phase coexistence between phases I and II. High temperature data is multiplied by a scale factor to enhance visibility. The magnetic intensity vanishes in the incommensurate line entirely at K, with no indications of diffuse scattering in the thermally disordered regime. Above , we observe a weak, diffuse neutron signal along the line, with rapid decay of the coherence length. c, Illustration of discommensuration-driven shift of in for phase II, where a defect every unit cells is introduced to release magnetoelastic strain built up between the crystal lattice and the collinear antiferromagnetic structure. c,d, Temperature dependence of and , respectively. The different regimes, phase I, II and the diffuse scattering regime (Diff), are highlighted by different color shadings.
To explore the regime above the critical field, confirm the coupling between and in phase I, and investigate the correlation of CDW and magnetic order, we carried out small angle neutron scattering (SANS) experiments in a magnetic field. Figure 5a describes the geometry of our SANS experiment and Figure 5b shows the obtained zero field map, while Figure 5c reduces the map into principal line cuts. The noncoplanar, helimagnetic cone texture with coupled and is stable up to T for , c.f. Figure 5f. In fact, this data further supports the existence of coupled commensurate and incommensurate order parameters in phase I, and helps to exclude a domain separation scenario (Figure E14). A pair of phase transitions to phases IV and V is visualized in Figure 5f and Figure E14. In phase V, c.f. Figure 5d and Figure 5e, which is realized when the external magnetic field exceeds T, strong magnetic reflections appear at momentum transfer with , demonstrating direct coupling between incommensurate magnetism and the CDW in absence of the antiferromagnetic order parameter. Although we cannot provide a magnetic structure model based on the available data, the comparison of intensities at Miller indices suggests the presence of both and spin components (inset of Figure 5e).
Figure 5. Coupling of magnetic order and charge-density wave in DyTe3, tracked by small-angle neutron scattering (SANS) in a magnetic field along the -axis at K. a, Experimental geometry of SANS. Orange plate, blue rectangle, , , and are the sample, the area detector – shifted from the center axis to catch reflections with larger –, incoming / outgoing neutron beam wavevector, and the momentum transfer of elastic scattering, respectively. A wedge of three-dimensional space is covered by rotating the sample in steps (angle , Methods). b-e, Scattering intensity in cuts of momentum space (upper) and linecuts along (lower), for intensity integrated along the -direction within the orange and red dashed boxes. The magnetic field induces a transition to ferroic stacking, . f, Integrated intensity of various reflections as a function of magnetic field, covering three magnetic phases. Inset of (e): Experimental ratio in Phase V, compared to simulations for fan-like orders (spin plane indicated, green and grey dashed lines) and a helimagnetic (longitudinal-cone, red dashed line) order. The experiments are consistent with a slightly distorted, conical state of the same period as the underlying charge order.
Figure E14. Coupling of commensurate and incommensurate magnetic order in DyTe₃, tracked by small-angle neutron scattering (SANS) in a magnetic field along the c-axis, for sample E. a, Integrated intensity of commensurate () and incommensurate () reflections of type as a function of magnetic field and at a temperature of K. The observed intensity of both drops simultaneously at around T, with a fixed intensity ratio , as indicated by a grey dashed line in panel b. The error bars correspond to Poisson counting errors of the integrated neutron scattering intensity.
Discussion
As compared to transition metal dichalcogenides, where the magnetic ion is buried inside a rather symmetric block layer [34, 35], harbors more complex structural features, with magnetic ions at the boundary between metallic and covalently bonded blocks. This mixed covalent / metallic environment for the magnetic ion is key to realizing the present scenario: it facilitates coupling between magnetic ions and a charge density wave (CDW) on the tellurium square net, and – at the same time – generates unconventional magnetocrystalline anisotropy. In fact, the present charge-transfer phenomenology is partially inspired by work on thin films of magnetic metals on insulating substrates [36], on electric field control of magnetocrystalline anisotropy [37], and on the behaviour of magnetic materials when charge transfer is induced by oxidation at the surface [38].
Symmetry breaking with cycloid / spiral magnetic order of fixed helicity is rather widely observed in zigzag chain magnets (Extended Section E4 A), but the present combination of antiferromagnetic and cycloidal components is unique. For example, has cones arrayed on one-dimensional chains, with uniform cone direction along the chain [39]. In another metallic system, , jumps in the rotation sense of a helimagnetic texture have recently been identified, with a short magnetic period [40]. In contrast, the rotation of moments in proceeds in nearly parallel pairs, without abrupt jumps in the cycloidal component of the texture. We expect helimagnetic orders of the type observed here to be common in layered materials, and especially in rare earth tellurides and selenides. Here, rich magnetic phase diagrams have been generally observed [41, 42] and could be amenable to modeling by CDW-induced terms as in Eq. (1).
This complex magnetic order, its relationship to a strain-controllable CDW [33], and its (likely) rich excitation spectrum certainly warrant further research. For example, the CDW’s gapped collective excitation, termed Higgs mode, shows a magnetic character in as observed via Raman scattering experiments [15], and its evolution below may provide insights on both the origin of magnetic order and the nature of the CDW in .
Furthermore, the lowest-energy, Goldstone mode of a typical helimagnet corresponds to a spatial shift of the magnetic texture, termed phason excitation [43]. In , the magnetic and CDW phasons [44] are expected to be closely intertwined, as evident from the robust in phase I, and its jump – by the same amount as – in phase II (Figure E13). Such locking between low-energy modes may have implications for dynamic responses, further enriching the spectrum of elementary excitations in .
Concluding remarks
An important open question is the stability of helimagnetism in few-layer devices of , where the cleavage plane, as well as the center of structural inversion, are situated between tellurium bilayers. As a fundamental building block of the structure, we consider a DyTe slab sandwiched by Te square nets – that is half a unit cell in Figure 1 a. Being screened from top and bottom by tellurium layers, we expect no qualitative change of the local crystal field environment of Dy in the few-layer limit. However, the absence of an inversion center for odd numbers of layers, and its presence for even numbers of layers, may have a profound effect on magnetic ordering and the presence or absence of (right- or left-handed) helicity domains in the sample, considering the presence or absence of Dzyaloshinskii-Moriya interactions [45].
Most appealingly, is a potential platform for spin-Moiré engineering in solids, where complex magnetic textures can be designed by combining and twisting two or more helimagnetic sheets. Here, a plethora of noncoplanar spin textures can be engineered at will [6, 46], while highly conducting tellurium square net channels may serve as a test bed for of emergent electromagnetism in a tightly controlled setting [47, 48].
References
Methods
Sample preparation and characterization
Single crystals are grown from tellurium self-flux following the recipe in Ref. [42]: We set elemental Dy and Te at a ratio of 1 : 21.65 in an alumina crucible, which in turn is sealed in a quartz tube in high vacuum. The raw materials are heated to 450 °C for 36 hours and then to 780 °C in 96 hours, where the melt remained for 48 hours, followed by cooling to 450 °C at a rate of 1.375 °C/hour. The final product is centrifuged after renewed heating to 500° Celsius, so that plate-shaped single crystals of typical dimensions are obtained. The face of each plate is perpendicular to the -axis of ’s orthorhombic unit cell, and facet edges tend to be parallel to either or . The existence of impurity phases above 1% volume fraction is ruled out by single-crystal x-ray diffraction on cleaved surfaces in a Rigaku SmartLab X-ray powder diffractometer. The experiment yields lattice constants of Å, Å, and Å at room temperature, in good agreement with previous work [18]. We found it challenging to obtain high-quality powder x-ray data from crushed single crystals, which include traces of Te flux on their surface and form thin flakes, even when thoroughly ground in a mortar. We also verified the stoichiometric chemical composition of our crystals by energy-dispersive x-ray spectroscopy (EDX). Cleaved single crystals have a reddish-brown surface; but even in vacuum, the colour of the surface changes to silver-metallic, and then to black, after two weeks or so. A red hue can be recovered by renewed surface cleaving.
Magnetization measurements and crystal alignment
We use a commercial magnetometer with K base temperature and a maximum magnetic field of 7 T (MPMS, Quantum Design, USA). The measurement is carried out using a rectangular-shaped single crystal of mass mg, with carefully aligned edges along the and crystal axes. By means of a single crystal diffractometer (Malvern Panalytical Empyrean, Netherlands), we confirm the extinction rule in space group . It is difficult to distinguish and axes in this orthorhombic, yet nearly tetragonal structure by eye or with the help of the Laue diffractogram. Temperature dependent susceptibility is measured in a DC magnetometer with 1000 Oe applied field; there is no observable difference between field-cooled and zero-field cooled magnetization traces. A demagnetization correction is carried out according to the standard expression , where , , and are the externally applied magnetic field, the bulk magnetization, and the dimensionless demagnetization factor. The latter is calculated by approximating the crystal as an oblate ellipsoid [49]. For the phase diagram in Figure 4, the direction is aligned within and bulk magnetization is measured in discrete field steps, for selected temperatures. Figure 4 shows data for decreasing magnetic field . Note that hysteresis occurs at all phase transitions shown in Figure 4a, indicating their first-order nature. The magnetic anisotropy energy is expressed as , where is the angle between and the -axis. Utilizing the free energy expression and the Curie-Weiss law , where is the Curie-Weiss temperature along the direction and is the Curie constant of DyTe, we obtain , where is the difference between the Curie-Weiss temperatures in the -plane and along the -axis (c.f. Figure 1d, inset). Specific heat was recorded using a relaxation technique in a Quantum Design PPMS cryostat, in zero magnetic field. For specific heat anomalies in applied magnetic field, we employed the AC calorimetry technique in a custom-built setup. Anisotropy of the resistivity, as in Figure 2, was recorded on exfoliated flakes of thickness using the Montgomery technique. Electric contacts are made with Ag paste (Dupont) and deteriorate with time. To maintain excellent contact resistance , it is crucial to immediately cool the contacted crystal in vacuum, after depositing the silver paste. The sample and contact quality is robust at low temperatures for at least two weeks.
Elastic neutron scattering
We performed unpolarized and polarized neutron scattering experiments using the POlarized Neutron Triple-Axis spectrometer (PONTA) installed at the 5G beam hole of the Japan Research Reactor 3 (JRR-3). Two single crystals of DyTe (Sample A and B) are cut into rectangular shapes with dimension and , respectively. For both samples, the widest surface is normal to the -axis, and the sides are parallel to the or -axis. Each sample is set in an aluminum cell, which is sealed with gas for thermal exchange. We employed a closed-cycle refrigerator with base temperature of , and measured intensities on the horizontal scattering plane. Using a PG (002) monochromator, the energy of the incoming neutron beam is set to (30.5 meV) for unpolarized measurements of sample A (sample B). For the unpolarized measurements, the spectrometer is operated in two-axis mode with horizontal beam collimation of open--. In both unpolarized and polarized experiments, sapphire and pyrolytic graphite (PG) filters are installed between the monochromator and the sample, to suppress higher-order reflections from the monochromator to less than 0.5%. The observed integrated intensities are converted to structure factors after applying the Lorentz factor and absorption corrections.
For sample B, we measured nuclear and magnetic Bragg reflections at 2.2 K by scans. For the scattering profiles showing a well-defined Gaussian-shape peak, we estimated the background from both ends of the profile. For the magnetic reflections located near the powder diffraction lines of the Al sample holder, we carried out background scans at 10 K, and subtracted the intensities from those measured at 2.2 K. We also measured the background data at 10 K for relatively weak commensurate magnetic reflections in the -range of , to check for possible contamination from the nuclear reflections. As for the absorption correction, we calculated the scattering path length inside the sample, based on the dimensions of Sample B and on the incident and scattered directions of the neutrons. The neutron transmission is given by , where is the linear absorption coefficient. Taking into account the incident energy and the absorption and incoherent scattering cross-sections of DyTe, is calculated to be .
The diffraction profiles and integrated intensities shown in Figure 2, Figure 3 were measured using Sample A. Contrary to integrated intensities in the case of refinement, the temperature dependences in Figure 2c, Figure E13 are obtained from -scans of magnetic scattering. The calculation of the scattering intensity in Figure 2f, which includes the third harmonic reflection, takes into account instrumental resolution broadening (Figure E10), anharmonicity of the cycloidal magnetic structure component, and the presence of two magnetic domains (Extended Section E4).

Figure E10. Calibration of instrument resolution at 5G-PONTA at the JRR-3 neutron reactor source, for sample A. Each pair of (red, blue) data points corresponds to the full width at half maximum (FWHM) of a nuclear lattice reflection. The shape of the resolution ellipsoid in the – plane is defined by the width of an -scan (, transverse width) and the width of a scan (, longitudinal width), respectively. These parameters depend on the sample shape, crystal quality, the momentum transfer , and the performance of the instrument. Blue and red dashed lines are a linear fit, and a second order polynomial fit to the data, respectively. These fits can be used for estimation of the instrument resolution at arbitrary positions in the scattering plane, e.g. in Figure 4 c. Error bars correspond to statistical uncertainties of Gaussian fits to the nuclear reflections.
Sample A is also used for polarized neutron scattering, in which the spectrometer is operated in the triple-axis mode with horizontal beam collimation of open---open. A polarized neutron beam with is obtained by a Heusler (111) crystal monochromator. The spin direction of incident neutrons is set to be perpendicular to the scattering plane. We thus applied weak vertical magnetic fields of approximately 5 mT throughout the beam path by guide magnets and a Helmholtz coil. We used a Mezei-type spin flipper placed between monochromator and sample, and employed a Heusler (111) crystal analyzer to select the energy and spin states of scattered neutrons, separating spin-flip (SF) and non-spin flip (NSF) intensities. The spin polarization of the incident neutron beam () is 0.823, as measured using the (002) nuclear Bragg reflection of the sample.
Small angle neutron scattering in magnetic field
SANS measurements were performed using the SANS-I instrument at Paul Scherrer Institute (PSI), Switzerland. A bulk single crystal of DyTe (Sample E, mg) was carefully aligned (c.f. crystal alignment methods) and installed into a 1.8 T horizontal-field cryomagnet so that the -axis is vertical, and the incident neutron beam is in the -plane. The magnetic field is applied parallel to the crystal -axis, as shown in Figure 5a. The incident neutron beam with Å wavelength (15% ) is collimated over a distance of 4.5 m before the sample, and the scattered neutrons are detected by a 1 m two-dimensional multidetector (pixel size 7.5 mm x 7.5 mm) placed 1.7 m behind the sample. To cover a broader -space up to along the (01) direction, the detector was also translated 0.45 m in the horizontal plane. For all SANS data, background signals from the sample and the instrument are subtracted using the data of the nonmagnetic state at K and T. The field-dependent SANS measurements are performed during a field-increasing process, after an initial zero-field cool to the base temperature of 2 K. For each measurement, rocking scans were performed, i.e. the cryomagnet is rotated together with the sample around the vertical crystal -axes (rocking angle ) in a range from to and steps of () and (else). Here is carefully aligned and corresponds to the configuration where the beam is parallel to the crystallographic -axis. The SANS maps shown in this paper are obtained by performing a 2D cut of the volume of reciprocal space measured through cumulative detector measurements taken at each angle of the rocking scan. For the SANS maps shown in Figure 5, the integration width along the out-of-plane () direction is reciprocal lattice units. The line cuts along shown in Figure 5c, Figure 5e are extracted by integrating over a region of reciprocal lattice units in the direction. Peak positions and integrated intensities are calculated using those linecuts and a multi-peak fitting.
Crystal electric field calculations
We use the software package PyCrystalField [50] for the calculation of crystal electric field energies via the point charge model in the limit of strong spin-orbit interactions. The calculation is based on published fractional coordinates of Dy and Te ions within the crystallographic unit cell [18, 22], with a tensile strain along the -axis, lifting tetragonal symmetry and yielding finite . In Figure E15, we vary the effective crystal electric field originating from Te-A (on the Te slab) by changing its point charge, while keeping the total charge in the environment of Dy unchanged. An unperturbed, diagonal Hamiltonian matrix is constructed from the energies in Figure E15, and the operator of total angular momentum is also expressed in the basis of these CEF eigenstates. Adding an effective exchange field ( are vector components), the total Hamiltonian is diagonalized and the expectation value of , , is evaluated in the respective ground state. The anisotropy constants are approximated, as
so that for easy-axis anisotropy along the -axis and if -axis orientation is energetically preferred over the -axis. Here, is shorthand for , where is the ground state of the total Hamiltonian when an exchange field of magnitude is applied along the -direction.
The anisotropic part of the charge density is exaggerated in Figure 4 according to the expression , where corresponds to 10 Bohr radii. More details are given in Figure E15, Figure E16.

Figure E16. Mixing of crystal field states in DyTe3 by exchange interactions. a-c, The maximal and minimal eigenvalues of and d-f of calculated for the crystal field doublets . The charge ratio (-coordinate) describes the ratio of effective charges assigned to Te-A and Te-B tellurium ions corresponding to metallic and ionic bonds around Dy, respectively. A matrix representation of the operators and is calculated on each respective subspace spanned by a Kramers pair of states, and subsequently diagonalized. There is a transition from dominant (easy-plane) to (easy-axis) for the ground state , when reducing the effective crystal electric field charge for Te-A on metallic bonds. The first excited state behaves similarly, while the second excited state generally covers a broader range of eigenvalues. Red and grey shaded areas are defined as in Figure E15. In the red region, the character of the ground state (GS, , left column) changes from predominant to mainly character. It is not possible to generate sizable in-plane (-axis) magnetic moment using any linear combination of , at relative weight of CEF charges on Te-A and Te-B sites ().
Spin model calculations
A model Hamiltonian, Eq. (1), is introduced from the viewpoint of symmetry in § 6.1 of Extended Data, to explain the essential experimental results. Here, magnetic frustration is lifted and the separation of spin components by modulation ()-vectors is explained naturally by the off-diagonal and terms. An analytic solution is obtained in Fourier space, and variational calculations are carried out based on the spin ansatz and ignoring higher harmonics, for simplicity,
In these terms, the energy is given by
and easily optimized at satisfying . The optimal antiferromagnetic moment gives the squared intensities and , depicted in Figure 4.
Acknowledgments
We thank M. Nakano for permission to use his single-crystal x-ray diffractometer, and for support during the measurement. Moreover, we thank S. Kitou for initial advice on crystal field calculations, M. Kriener for support with experiments on magnetization and calorimetry, and Y. Kato for critical advice on the theoretical spin model. We thank P.M. Neves for support with the analysis of the wide-rocking angle SANS diffraction data. This work is based partly on experiments performed at the Swiss spallation neutron source SINQ, Paul Scherrer Institute, Villigen, Switzerland. This work was supported by JSPS KAKENHI Grant Nos. JP22H04463, JP22F22742, JP22K13998, JP23H01119, JP23KJ0557 and JP22K20348 as well as JST CREST Grant Number JPMJCR1874 and JPMJCR20T1 (Japan), and JST FOREST JPMJFR2238 (Japan). M.M.H. was funded by the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) – project number 518238332. The authors are grateful for support by the Fujimori Science and Technology Foundation, New Materials and Information Foundation, Murata Science Foundation, Mizuho Foundation for the Promotion of Sciences, Yamada Science Foundation, Hattori Hokokai Foundation, Iketani Science and Technology Foundation, Mazda Foundation, Casio Science Promotion Foundation, Inamori Foundation, Marubun Exchange Grant, and Kenjiro Takayanagi Foundation.
Data availability
The data supporting the findings of this study are available from the authors upon reasonable request.
Author contributions
Sh.A., M.H., and Y.O. synthesized and characterized the single-crystals. S.E., M.H., and Sh.A. carried out calorimetry and magnetic measurements, while T.N., Se.A., Sh.A., Ri.Y., S.E. and M.H. carried out and analyzed elastic neutron scattering measurements, with extensive guidance from T.-h.A. S.E., J.S.W. and M.H. carried out and analyzed small angle neutron scattering measurements. Electric transport measurements were carried out by S.E. and M.H., and theoretical modeling of crystal fields was conducted by S.E. under the guidance of T.-h.A. S.G., S.O., and Ry.Y. modeled the magnetic structure. M.H., M.M.H., and S.E. wrote the manuscript with contributions and comments from all co-authors.
Competing interests
The authors declare no competing interests.
Spin Hamiltonian
Model Hamiltonian. To describe the ground state and the field-induced transition in DyTe for , consider a one-dimensional (1D) chain, where each unit cell contains a single magnetic site, of index , in the paramagnetic state. For this model, the lattice constant is set to , the reciprocal lattice constant is , the wavevector is dimensionless, and the CDW wavenumber (for ) is [18]. As compared to the effective zigzag chain in , the number of magnetic sites is halved, i.e. the lower part of the chain is omitted. Hence, order for the component of the local, quasi-classical spin is equivalent to order on the zigzag chain.
We start with a real-space ansatz comprising antiferromagnetic exchange, a spatially modulated on-site coupling induced by the lattice distortion from the CDW, and a Zeeman term for magnetic field applied along the chain axis (-axis),
where labels magnetic moments on a single layer of a single zigzag chain. Here, , represent nearest neighbours in the crystal lattice of , so that their coupling can be expected to be stronger than the coupling between the sheets (see next section).
The oscillating off-diagonal terms, and are permitted since the global and the local -mirror are broken by the lattice distortion due to the CDW, respectively. Moving to Fourier space according to the conventions and , where is the number of sites on the chain, we have
For a Heisenberg Hamiltonian without off-diagonal terms, the Luttinger-Tisza rule dictates the choice of a single, optimal for the long-range ordered state; yet here, given the off-diagonal coupling of spin components, we naturally select different wavenumbers for different spin components, explaining the clear separation of spin components by -vector observed experimentally in Figure 2 of the main text. Hereafter, we set for simplicity.
If , the minimum of is at and is realized. If further , is directly locked to the dominant and
realizing the coupled wavevectors that are experimentally observed in phase I of DyTe. Application of a magnetic field larger than enforces and the cross-terms induce and the second harmonics demonstrated experimentally in Figure 5. Indeed, the Zeeman energy per magnetic moment of (Bohr magneton) at the critical field in Figure 5 is roughly 3.6 K, very close to the value of the Néel temperature .
If, in contrast, , there is no reason why wavenumbers such as should appear in the ground state. As compared to anisotropic exchange interactions, for example of the type , the present terms cannot induce spontaneous magnetic order by themselves, but rather they create a ’parasitic’ spin modulation – driven by the charge-density wave of , rare earth – on the back of either AFM order below or of the field-polarized moment above .
Additional Heisenberg coupling on zigzag chain. We introduce an additional between neighbouring sites on the zigzag chain as
which can be separated into three independent equations , , – one for each spin component. Note that , are not nearest neighbours in the lattice of DyTe, so that their coupling is expected to be weaker than the dominant antiferromagnetic in Eq. (6). We use the trial functions
with a helicity parameter indicating the propagation direction of the texture, the incommensurate wavevector in reciprocal lattice units (r.l.u.), as well as the phases and . The latter can only vary in steps of , if we assume a fixed length of the
magnetic moment. Based on this,
and the two cases and yield
These terms in Eq. (16), (17) are independent of ; especially for , optimizing yields a favorable energy contribution for any given , .
Expressions for scattering intensities
We review the expressions used to calculate neutron scattering intensities from atomic and magnetic structures of DyTe, which serve to define a variety of parameters (such as the phase shift ) used in the discussion of the main text. Working with the triple-axis diffractometer PONTA-5G at JRR-3 research reactor, we fit or scans of neutron intensities with Gaussian profiles and calculate the total observed intensity for each reflection, taking the -dependence of the peak shape into account (Figure E10). From this, we calculate the observed structure factor as
where is the Lorentz factor, is the wavelength of the monochromatized neutrons, and is the scattering angle.
To reproduce this quantitatively, we start from the expression for the differential cross-sections for nuclear and magnetic scattering, i.e. the beam intensity scattered into a solid angle corresponding to the direction of the momentum transfer of magnitude and direction
Here, we have introduced the neutron flux , the position of each atom on the lattice , the nuclear scattering length , the unit cell coordinates , the magnetic form factor evaluated from an analytic expression [72], and the component of the magnetic moment at site that is perpendicular to the momentum transfer
Note the scattering lengths for (16.9 fm) and Te (5.8 fm), and that only magnetic ions contribute to Eq. (20).
For nuclear scattering, we use [73]
for a reciprocal lattice vector and using , where the former is a coordinate within the crystallographic unit cell, and the latter labels the origin of each unit cell. , , , are the flux of incident neutrons, the number of crystallographic unit cells (c.u.c., of volume ) in the sample, and the nuclear structure factor. We find good agreement of the experimental scattering data and model when using the atomic positions from the high-temperature space group of DyTe [74]. In reality, the formation of charge order below K lowers the symmetry, as discussed by Malliakas et al. in Refs. [18, 75].
Then, a scale factor is defined by equating to the experimentally observed intensity,
as shown in Figure E7.
Figure E7. Nuclear reflections observed in neutron scattering, consistent with orthorhombic crystal structure of DyTe3. The observed structure factor is compared to model calculations, , in space group as detailed in section E2. We use the reliability index for the structure factor, , where the sums are over all data points; for sample B (a) and for sample A (b) indicate good agreement of model and fit. Note that -scans without absorption correction are used to obtain the integrated intensities for sample A.
Next, for magnetic scattering from a structure with lattice-commensurate magnetic order, we use Eq. (23) with a larger unit cell (reduced set of ) and equate
We introduced the calculated magnetic structure factor , which has three complex components , , ; the volume of the magnetic unit cell (m.u.c.) , the magnetic form factor of Dy, , and the number of m.u.c. in the sample. The prefactor () describes the scattering length of the electron, and the sum is now over all magnetic (dysprosium) ions in the m.u.c.
In case of two domains of this commensurate order, as relevant for the analysis in DyTe, we have
where , are the magnetic structure factors for two domains.
Symmetry and structure factor: commensurate component in phase I
Symmetry consideration (commensurate)
Section E1 discusses oscillatory terms that are allowed in the Hamiltonian due to local symmetry breaking from the charge-density wave (CDW). In this section, we focus on global symmetries of DyTe and their lowering by magnetic order. We start from space group , ignoring the incommensurate CDW at first, and briefly consider the effect of the CDW on global symmetries at the end of the section.
In polarized neutron scattering (PNS), orthorhombic symmetry of the crystal structure allows us to set the scattering plane to , with separation of three orthogonal magnetization components , , and . The PNS data strictly constrains the commensurate moment to be along the -axis, and the observation of reflections of the type (0, odd, 0.5) – while (0, even, 0.5) are absent –, establishes a unit cell with eight magnetic dysprosium ions, vanishing net magnetization along the -axis, as well as opposite directions for moments separated by a distance along the -axis (Fig. E3c). Four free parameters remain, namely
Figure E2. Space group and its symmetries in the set, as well as breaking of bond-symmetry by AFM commensurate order. Only dysprosium ions are shown (blue), including two ions outside the crystallographic unit cell (right) to illustrate the structural zigzag chain feature. a, Mirror plane . b, Mirror plane . c, Glide mirror plane with translation along the -axis (black arrow). d, Two-fold rotation through the inversion center . e, Two-fold rotation through a position shifted by from . f, Screw rotation with shift along the -axis. g Base centering operation , i.e., a translation by . h In the presence of commensurate order , the magnetic space group symmetry is lowered to : and are broken (grey), while survives (red). The equivalence of bonds on the effective zigzag chain (main text) is lifted in presence of or order (black double and single bonds).
the lengths of four magnetic moments in a DyTe slab spanning two crystallographic unit cells, i.e. the upper zigzag chain in Figure E3.

Figure E3. Unit cell, magnetic domains for commensurate spin component, and illustration for structure factor calculation in phase I of (antiferromagnetic part, AFM). a, b, Primitive magnetic unit cell (red boundary, monoclinic) in two AFM domains of , with base centering translation vector and translation vector (plus time reversal) . The base centering operation of the parent structure (C), and its inversion center (I), are also indicated by a violet arrow and cross, respectively. Only magnetic sites are shown, and sites with different -positions have been projected onto a single plane. See section E3. c, Conventional unit cell for two AFM domains in phase I. Circles with dot (with cross) signify magnetic moment pointing into (out of) the plane of the figure. The -axis spacing of magnetic sites in a bilayer (grey shading) is approximately . Inversion centers are indicated by violet crosses. d, Two sets of sites (black, white circles) of magnetic ions in the unit cell. In the calculation of the structure factor for the combined scattering of two equally populated domains A, B according to Eq. (28), the only contributions are from terms for sites in the same set.
The full Hermann–Mauguin symbol for orthorhombic space group (SG63) is , and does not break any of these symmetries. Using the k-Subgroupsmag tool of the Bilbao crystallographic server [76], we determined the highest-symmetry magnetic subgroups of that are consistent with . In (black-and-white-type) Belov-Neronova-Smirnova notation: , , and . From the transformation matrices provided by this tool, we also find the lattice vectors , , in terms of the lattice vectors , , of the ’parent’ : , , and , for the three abovementioned symbols. Here, for example, for basis (unit) vector and lattice constant (and so on).
We rule out and for the commensurate order in DyTe. The former has a mirror plane, which is perpendicular to of the cell and located on the Dy-sites. A moment on the Dy-site is inconsistent with this mirror plane. The latter space group has a glide mirror plane , consisting of a mirror operation perpendicular to combined with a lattice translation by . The moment direction at a given site is unchanged under , but translated by half the length of the magnetic unit cell. Given there are merely four sites in the upper DyTe slab of the magnetic unit cell, this operation requires orders of the type udud, and is thus inconsistent with the expansion of the unit cell along that is implied by .
We focus on monoclinic, centrosymmetric , where includes base centering as a translation and , i.e. the translation combined with time reversal. There are two domains A and B with basis vectors and ; i.e., they are characterized by a reversal of the monoclinic tilt (Figure E3). Only the mirror plane perpendicular to remains intact, the number of inversion centers is halfed as compared to , and the broken -mirror relates the two possible domains A and B depicted in Figure E3c.
Note: A previous x-ray scattering study reports the superspace group for the CDW state in DyTe [75]. In average space group (No. 40), the mirror of is already broken. Starting from this lower-symmetry symbol, analogous discussion leads to for the commensurate component of the magnetic order in phase I.
We consider the possibility of further symmetry lowering, as caused by non-uniform mag-
netic moment length . Magnetic space group has , which ensures that moments in the same layer point in opposite directions, but have the same length. Instead of (up-up-down-down), this leaves as a viable configuration, but rotation symmetry interrelates layers and eliminates this possibility. The neutron data are well described by (or , which leads to the same commensurate structure models), so that a further symmetry lowering – relaxing the uniformity constraint on – is deemed unnecessary.
Structure factor calculation (commensurate)
We now derive explicit expressions for the scattered intensity at commensurate (AFM) reflections in momentum space, in phase I of DyTe.
For momentum transfer in the plane, we define a normalized moment for each domain , where . Assuming equal population of domains A and B, Eq. (27) gives
where the magnetic sites are labeled in Figure E3 d (not Figure 2). In the latter edgy brackets, the two terms cancel (sum to ) when the relationship between magnetic moments at site is opposite (the same) in domains A, B. In addition to four pairs of type , examination of Figure E3 d shows that, for the purpose of evaluating Eq. (28), the magnetic sites can be split into two sets 1 and 2: the non-vanishing terms in the sum correspond to pairs of magnetic moments that are just above / below one another, or two sites apart along the -direction.
The relative distances between sites are the same for set 1 and 2, and there are three types of site pairs in each set:
with both appearing in the sum of Eq. (28). The moments are antiparallel for all pairs of sites, , except the pairs in Eq. (31). We specialize to the scattering plane, so that
as in our experiments, and obtain
which takes the values () for (), independent of . Then, when is even, and for ,
without any explicit dependence on and both (but note the magnetic form factor). The above discussion shows that contributions from domains A, B partially cancel each other, meaning that the ratio of domains can be refined from the data.
Symmetry and structure factor: incommensurate component in phase I
Symmetry consideration (incommensurate)
Starting from Eqs. (12), (13), and given antiferromagnetic coupling between structural bilayers in DyTe, as enforced by in , the phase relation between layers and is fixed to and , . The remaining free parameters, besides , , are a single phase and the parameter , which characterizes the relative helicity in two adjacent layers. We set a single (possibly distorted), incommensurate cycloid into the uppermost layer with , and – enforced by – a copy with into the third layer. We then approximate the incommensurate order by an (arbitrarily large) supercell, and discuss the symmetries that leave the magnetic moments unchanged. From this, we deduce constraints on and .
Starting from , the cycloid in removes the mirror operation. Figure E4a shows the point group symmetries of a cycloid, with one of the operations perpendicular to in DyTe; but the (mirror time reversal) operation is not consistent with the commensurate component of phase I. Instead, a -glide appears in the place of (in the frame of ). The translations and of (Figure E3) are broken by the cycloids in . Without further symmetry lowering, the average magnetic space group is , where – somewhere along the -direction – a global inversion center survives. Due to the remaining symmetry, the four layers are stacked as , where ; recall that and (Figure E4b). Importantly, the configuration is not related to by a broken symmetry and does not have the same energy as ; the energy difference between these two is largely determined by the local Dzyaloshinskii-Moriya (local DMI) interaction on the bond of the zigzag chain (Figure 1), i.e. the local DMI between nearest neighbors on a single square net of the DyTe slab. The competition between inter-layer Heisenberg exchange , Eq. (10), and intra-layer local DMI determines the choice of co-propagating or counter-propagating cycloids, and hence the average magnetic space group.
Figure E4. Symmetry considerations regarding incommensurate magnetic order in phase I, for DyTe3. a, Magnetic point group symmetries of a cycloid. b, A magnetic texture with symmetry and ordering vector . Red arrows: Setting a cycloid in the uppermost layer with helicity , the layer’s structure with is imposed by antiferromagnetic coupling (). Violet arrows: Applying symmetry enforces a counter-propagating cycloid in layers , with , where the phase is fixed to . The texture in layer can be inferred from AFM coupling to . c, Switching between helicity domains in the model with uniform helicity ; for simplicity of the illustration, the phase difference is set to . Grey arrows: assuming broken symmetry, uniform helicity and adjustable phase shift are allowed. The operation (violet arrow) maps , while leaving unchanged. (Nearly) collinear blocks, (purple highlight) remain coupled. d, Simultaneous switching of and via glide mirror , and switching of without by mirror . Highlighted ovals mark pairs of spins with nearly collinear alignment in the plane. Again, is used for the purpose of this illustration, although the experimental value is .
Figure E5. Two ’-domains’ (A′ and B′), consistent with the ordering vector, for the incommensurate part of the magnetic order in phase I of DyTe. The value of the phase shift between sheets in a bilayer is adjusted to minimize the reliability index for the structure factor . Grey arrows indicate the original moment direction that is expected without any phase shift . Note that there is a phase shift of between upper and lower Dy-bilayer, and that reversing the sign of the helicity vector , as defined in section E4, does not affect the value of scattering intensities; is the angle between the -component of the magnetic moment and the crystallographic -axis.
For the stack, a degree of freedom remains regarding the phase relation of cycloids in two layers of a DyTe slab. In particular, the phase shift angle determines whether blocks of parallel moments point along and blocks of antiparallel moments point along , or vice versa. Absent further symmetry lowering, the remaining symmetry in fixes , with , where the sign depends on the position of the inversion center in , i.e., on domain A or B of the AFM order. We have derived an analytic expression for the magnetic structure factor of counter-propagating cycloids in DyTe, section E4 D, and consider the alternative models of high-symmetry, counter-propagating cycloids in that section.
For , we can further lower symmetry to (on average, space group number 9) by shifting away from , thus breaking . However, the spontaneous formation of helimagnetism with a unique sense of rotation is common in zigzag chain magnets, and more generally in systems where two or more sublattices are connected by space inversion, a twofold screw axis along the chain, and / or a glide mirror. Examples are NiVO [77], CuO [78], and the zigzag chain magnet MnWO [79], which all host single-sense helices under these conditions. Thus, we consider the cycloid of uniform helicity (average space group ), which allows the spin system to adjust to minimize inter-chain exchange energy (section E1). We are left with two helicity-domains, and for each AFM domain ( or ). These are related by , which reverses the rotation sense of the cycloids, but maintains the same AFM domain and the same phase relation for a given bond (Figure E4c). As the symmetry is reduced to in each domain, there is no constraint on the number value of . The discussion remains qualitatively unchanged if the commensurate part has magnetic space group .
Figure E2h demonstrates the inequivalence of bonds on the zigzag chain, caused by the commensurate magnetic structure component, which is essential for symmetry reduction and for allowing off-diagonal anisotropy terms such as in the Hamiltonian of section E1. In particular, becomes a refinable parameter only when the average symmetry is lowered to .
Structure factor calculation (incommensurate)
We translate the the spin-chain model, Eqs. (12), (13), into expressions suitable for structure factor calculations. Instead of the full, three-dimensional propagation vector , we use , which helps to define the equations and relative phases of magnetic layers in language that is consistent with the main text and with section E4 A. The magnetic sites are labeled by index as in Figure 2, , where and label the origin of the unit cell and the intra-cell coordinate of the site, respectively. As there is only one magnetic (dysprosium) site per layer [defined in Eqs. (12), (13)], we replace the layer index by and write
where , with two orthogonal unit vectors , . As before, the phase degree of freedom is specific to each layer index , and the prefactors indicate the helicity (sense of rotation, or handedness) in a layer. Based on the discussion in section E4 A, we use , , , and , where indicates two magnetic domains of the phase shift angle .
We insert this into Eq. (20), drop the helicity factor , and define with a normal vector . The quantity is defined analogously, and we are careful to consider the structure factor in the incommensurate case as a sum over the full lattice, not over a single magnetic unit cell,
Now, the sums in Eq. (37), (38) are over a single chemical unit cell (c.u.c.). This can be rewritten, due to the periodicity of the lattice, as
where are the reciprocal lattice vectors. Enforced by the -functions, the depend only on the reciprocal lattice vector from which the incommensurate reflection ’originates’, i.e. and , with
and , , integers.
Specializing to the scattering plane, can be calculated explicitly by considering four types of pairs , as well as four types of non-identical partners (we omit the -component of each vector),
with the spacing, close to , between two layers in a covalently bonded bilayer (Figure E3). Due to the above definition of , these phases are identical for the calculation of both . The parameter by itself is either negative and positive, depending on the domain .
Executing Eqs. (37), (38) in terms of this limited set of atom pairs,
The total scattering intensity for two equally populated domains of the angle is hence zero for even and, for odd,
independent of whether we are looking at the left / right reflection; i.e., the sign in is completely cancelled out. It is, finally, possible to simplify the magnetic moment projection as
with , , and we set , .
Example: intensity ratio of two reflections
| (r.l.u.) | (Å) | (deg.) | (deg.) | |||||||
| 0 | 9 | 0.207 | 0 | 2.228 | 0.302 | 2.248 | 51.853 | 1.272 | 0.825 | 82.27 |
| 0 | 1 | 1.207 | 0 | 0.248 | 1.763 | 1.780 | 40.505 | 1.533 | 0.885 | 7.99 |
Table E2. Calculation of expected intensity ratio of scattered neutron intensity at (0, 9, 0.207) and (0, 1, 1.207), based on magnetic structure model. The intensity ratio is calculated from Eq. (50), using these parameters. For convenience, we use (neutron wavelength ) in the calculation of the Lorentz factor.
Specifically for two reflections and in reciprocal space, with Miller indices (0, 9, 0.207) and (0, 1, 1.207), the corresponding Miller indices for the positions are (090) and (011), respectively. According to Eq. (46) with from the refinement in § 6.6, the intensity ratio is
where (scattering angle ) is the Lorentz factor, which corrects for the scattering geometry. Table E2 shows the numerical values for various steps in the calculation. From the observed ratio of peak intensities in Figure 2, and for these two reflections measured on sample A. This is somewhat larger than the result for sample B with full refinement in § 6.6, but sample A is a larger crystal, with anisotropic shape, where absorption correction is not applied. In particular, the observed intensities are expected to be larger along (0, 1, ), close to transmission geometry. Such limitations of the data quality for sample A do not affect polarization analysis and the qualitative evolution of line scan intensities with temperature.

Figure E6. Testing analytic model for the magnetic structure factor of the magnetic ground state of DyTe3. Observed magnetic structure factor, after correction for the Lorentz factor, for incommensurate reflections with . The inset depicts the relevant region of momentum space in the scattering plane. The red curves (black dashed line) are envelopes to the data (is the center of the envelopes), bounding the data which oscillates according to Eq. (54). Blue and green are reflections with , respectively. The oscillation amplitude rules out , as discussed in section E4 D.
Structure factor for counter-propagating cycloids
Previously, a stack of counter-propagating helices was reported in -LiIrO and ascribed to the presence of Kitaev-type anisotropic exchange interactions [80]. Analogously, we consider the structure factor for the helicity stack as defined in section E4 A. In Eq. (35), () can describe counter-propagating cycloids where the textures of two layers meet, at certain points, to create pairs of moments that are parallel to the -axis (parallel to the -axis). Recognizing that
algebra in line with section E4 B, for one domain of the -angle, yields
Special cases can be considered. When is (nearly) parallel to , and the co- and counter-propagating models deliver the same result (now including two -domains, introducing a separate factor):
This is expected from Eq. (51), where additional ’s appear only before . Figure E6 shows the intensities for , as a function of , with an upper and lower envelope function defined by the magnetic form factor. The maximum amplitude of the oscillation with , , suggests that , excluding and corresponding to counter-propagating cycloids with high symmetry (see above).
Analysis of nuclear elastic neutron scattering
For sample B, we collected 20 nuclear reflections, which contain 17 independent reflections. Observed and calculated nuclear structure factors are compared to determine the scale factor, a parameter for the extinction correction, and isotropic atomic displacement factors . These three parameters are later used in the magnetic structure analysis (§ 6.6).
For simplicity, we assumed that all the tellurium sites have the same . We performed a least-squares fit and found that the observed and calculated structure factors agree well; is 3.28 %. The values of for Dy and Te are determined to be 0.1(2) and 0.8(2), respectively. We also performed the same analysis after averaging the structure factors of the equivalent reflections, and obtained the internal value of 3.35 %.
For sample A, we collected 9 independent nuclear reflections. Observed and calculated nuclear structure factors are compared to determine the scale factor, while fractional coordinates of the atoms and are fixed at the values reported in [81]. We performed a least-squares fit and found that the observed and calculated structure factors agree well:
(Figure E8).
Results of magnetic structure analysis
For sample B, we collected 38 (70) Bragg reflections for the commensurate (incommensurate) magnetic reflections, all of which are independent. The polarized neutron scattering experiment in Figure E12 reveals that the magnetic moments corresponding to the commensurate component are parallel to the -axis. Assuming the volume fractions of two domains in Figure E3 to be equal, we performed a least-squares fit to the nonpolarized neutron scattering data from sample B and found that the magnitude of the commensurate component is , with .

Figure E12. Neutron flipping ratio in sample A for two components of the magnetic order in DyTe3’s ground state. Here, the flipping ratio is the normalized ratio of spin flip (SF) and non-spin flip (NSF) intensities for a magnetic reflection. is the flipping ratio at the nuclear reflection (002) (Methods). In our geometry, SF intensity is dominated by the -component (the -component) of the magnetization at (at ), although the structure and magnetic form factors have to be carefully taken into account when comparing intensities of various reflections (§ 6.6). a, The incommensurate magnetization component at gives dominant SF scattering, with independent of the angle. This implies presence of both and for the incommensurate reflection. b, The antiferromagnetic reflection has dominant NSF scattering, which is again independent of and consistent with magnetization component exclusively along the -axis; hence leading to for all reflections measured.
For the incommensurate magnetic component, polarized neutron scattering shows that the magnetic moments are confined in the -plane. Further considering the existence of the third higher-harmonic magnetic reflections, we assume an elliptic (distorted) cycloidal magnetic modulation, with principal axes parallel to the - and -axes, and moment amplitudes and common to all four Dy atoms in a chemical unit cell. We assume equal volume fraction of two domains for the phase shift , described in section E4, and refine , , and by least-squares analysis. This yields , , and deg, respectively. The value is 8.26% (Figure E8) and combined, the total moment length at the Dy site is
at K, which is about , i.e. still rather close to the critical temperature; the ordered moment at absolute zero temperature is expected to be close to the local-ion value of 10 per dysprosium, also due to an underestimation in our calculation by neglecting higher harmonics contributions. The difference in value between and is consistent with the presence of third harmonic magnetic reflections; such distortions and higher harmonics have also been observed in insulating multiferroics [82].
Our model demonstrates that, at least, the incommensurate component involves both and components, of different amplitudes. Further experiments using spherical neutron polarimetry will be suitable to investigate, in more detail, the directions of the minor and major axes for the spin ellipsis in the plane.
The lattice constants Å, Å are determined from neutron scattering at low temperature. These values are close to the literature values for the orthorhombic, yet nearly tetragonal structure of DyTe, Å, Å [81].
Our neutron measurements are not able to pick up minute atomic displacements due to the CDW, which can be seen in careful x-ray studies [75]; we used the fractional atomic positions of the average structure from Ref. [81] in our analysis of the nuclear and magnetic scattering.
Anisotropic electronic transport properties

Figure E9. Anisotropy of electrical transport properties in basal plane of DyTe. a,b, basal plane resistance ratio as a function of temperature for different samples. In Sample D, the assumed rectangular sample shape (c.f. panel c) is slightly – in particular 4% along the direction – adjusted to match at , c.f. Eq. (59). Both samples show a clear kink at the magnetic phase transition , followed by a broad plateau region, indicated by a red dashed line, with nearly constant ratio. c, Sample C mounted in Montgomery geometry. The orange rectangle depicts the assumed sample shape that is used to estimate the length ratio , where the white scale bar on the bottom right corresponds to 1 mm.
Angle-resolved photoemission (ARPES) studies combined with a tight binding (TB) model in Ref. [20] reveals that, in the family of the rear-earth tritellurides , the states at the Fermi level are mainly formed by the in-plane and orbitals of the Te-A ions in the Te square net, c.f. Figure 1a. Indeed, they are well separated by more than 1 eV from other bands, already indicating anisotropic bonding and transport properties. With a standard four-probe method and a modified Montgomery geometry Ru et al. determined both in-plane () and out-of-plane resistance () of various compounds [22]. They differ by at least one order of magnitude (), consistent with a metallic Te square net as well as covalently bonded slabs.
To further extract the in-plane anisotropy ratio of DyTe, we use the Montgomery technique and follow the method described in Ref. [83]. From temperature dependent resistance measurements and , we calculate the shape of a hypothetical isotropic sample with dimensions and same absolute resistance values and
Based on published data from Ref. [22] and our sample geometry, a thin exfoliated flake, we estimated that the calculation of the anisotropy ratio is possible in the thin-layer limit. Following Ref. [83] and using the real sample dimensions this leads to
and finally to
There is some ambiguity in the interpretation of resistance anisotropy changes at , which can be ascribed either to opening of a partial charge gap in the ordered state, or to fluctuations in the paramagnetic regime and their suppression below . In DyTe, the sign of the observed change in implies that, when moving from the paramagnetic into the ordered regime, the resistance along the -axis becomes larger than the resistance along the -axis. This result can be neatly explained by attributing partial gap opening to , , while unidirectional fluctuations should enhance above , and suppress it below .
References
- [1]B. Huang, G. Clark, E. Navarro-Moratalla, D. Klein, R. Cheng, K. Seyler, E. S. D. Zhong, M. McGuire, D. Cobden, W. Yao, D. Xiao, P. Jarillo-Herrero, and X. Xu, Layer-dependent ferromagnetism in a van der Waals crystal down to the monolayer limit, Nature 546, 270 (2017).DOI
- [2]Gong, C., Li, L., Li, Z., Ji, H., Stern, A., Xia, Y., Cao, T., Bao, W., Wang, C., Wang, Y., Qiu, Z., Cava, R., Louie, S., Xia, J., & Zhang, X. (n.d.). Discovery of intrinsic ferromagnetism in.
- [3]K. Burch, D. Mandrus, and J.-G. Park, Magnetism in two-dimensional van der Waals materials, Nature 563, 47 (2018).DOI
- [4]C. Gong and X. Zhang, Two-dimensional magnetic crystals and emergent heterostructure devices, Science 363, aav4450 (2019).DOI
- [5]D. Amoroso, P. Barone, and S. Picozzi, Spontaneous skyrmionic lattice from anisotropic symmetric exchange in a Ni-halide monolayer, Nature Communications 11, 5784 (2020).DOI
- [6]K. Shimizu, S. Okumura, Y. Kato, and Y. Motome, Spin moiré engineering of topological magnetism and emergent electromagnetic fields, Physical Review B 103, 184421 (2021).DOI
- [7]N. Jiang, Y. Nii, H. Arisawa, E. Saitoh, and Y. Onose, Electric current control of spin helicity in an itinerant helimagnet, Nature Communications 11, 1601 (2020).DOI
- [8]J. Ohe and Y. Onose, Chirality control of the spin structure in monoaxial helimagnets by charge current, Applied Physics Letters 118, 042407 (2021).DOI
- [9]H. Masuda, T. Seki, J. Ohe, Y. Nii, K. Takanashi, and Y. Onose, Chirality-dependent spin current generation in a helimagnet: zero-field probe of chirality, arXiv:2212.10980 (2022).arxiv.org/abs/2212.10980
- [10]Y. Wang, X. Xu, X. Zhao, W. Ji, Q. Cao, S. Li, and Y. Li, Switchable half-metallicity in A-type antiferromagnetic NiI₂ bilayer coupled with ferroelectric In₂Se₃, npj Computational Materials 8, 218 (2022).DOI
- [11]F. Schmitt, P. Kirchmann, U. Bovensiepen, R. Moore, J.-H. Chu, D. Lu, L. Rettig, M. Wolf, I. Fisher, and Z.-X. Shen, Ultrafast electron dynamics in the charge density wave material TbTe₃, New Journal of Physics 13, 063022 (2011).DOI
- [12]A. Kogar, A. Z. ad P.E. Dolgirev, X. Shen, J. Straquadine, Y.-Q. Bie, X. Wang, T. Rohwer, I.-C. Tung, Y. Yang, R. Li, J. Yang, S. Weathersby, S. Park, M. Kozina, E. Sie, H. Wen, P. Jarillo-Herrero, I. Fisher, X. Wang, and N. Gedik, Light-induced charge density wave in LaTe₃, Nature Physics 16, 159 (2020).DOI
- [13]P. Dolgirev, A. Rozhkov, A. Zong, A. Kogar, N. Gedik, and B. Fine, Amplitude dynamics of the charge density wave in LaTe₃: Theoretical description of pump-probe experiments, Physical Review B 101, 054203 (2020).DOI
- [14]I. Gonzalez-Vallejo, V. Jacques, D. Boschetto, G. Rizza, A. Hadj-Azzem, J. Faure, and D. L. Bolloc’h, Time-resolved structural dynamics of the out-of-equilibrium charge density wave phase transition in GdTe₃, Structural Dynamics 9, 014502 (2022).DOI
- [15]Y. Wang, I. Petrides, G. McNamara, M. Hosen, S. Lei, Y.-C. Wu, J. Hart, H. Lv, J. Yan, D. Xiao, J. Cha, P. Narang, L. Schoop, and K. Burch, Axial Higgs mode detected by quantum pathway interference in RTe₃, Nature 606, 896 (2022).DOI
- [16]S. Lei, J. Lin, Y. Jia, M. Gray, A. Topp, G. Farahi, S. Klemenz, T. Gao, F. Rodolakis, J. McChesney, C. Ast, A. Yazdani, K. Burch, S. Wu, N. Ong, and L. Schoop, High mobility in a van der Waals layered antiferromagnetic metal, Science Advances 6, eaay6407 (2020).DOI
- [17]Y. Che, P. Wang, M. Wu, J. Ma, S. Wen, X. Wu, G. Li, Y. Zhao, K. Wang, L. Zhang, L. Huang, W. Li, and M. Huang, Raman spectra and dimensional effect on the charge density wave transition in GdTe₃, Applied Physics Letters 115, 151905 (2019).DOI
- [18]C. Malliakas and M. Kanatzidis, Divergence in the Behavior of the Charge Density Wave in RETe₃ (RE= Rare-Earth element) with Temperature and RE Element, Journal of the American Chemical Society 128, 12612 (2006).pubmed.ncbi.nlm.nih.gov/17002331
- [19]J. Laverock, S. B. Dugdale, Z. Major, M. A. Alam, N. Ru, I. R. Fisher, G. Santi, and E. Bruno, Fermi surface nesting and charge-density wave formation in rare-earth tritellurides, Physical Review B 71, 085114 (2005).DOI
- [20]V. Brouet, W. L. Yang, X. J. Zhou, Z. Hussain, R. G. Moore, R. He, D. H. Lu, Z. X. Shen, J. Laverock, S. B. Dugdale, N. Ru, and I. R. Fisher, Angle-resolved photoemission study of the evolution of band structure and charge density wave properties in RTe₃ (R = Y, La, Ce, Sm, Gd, Tb, and Dy), Physical Review B 77, 235104 (2008).DOI
- [21]A. Chikina, H. Lund, M. Bianchia, D. Curcio, K. Dalgaard, M. Bremholm, S. Lei, R. Singh, L. Schoop, and P. Hofmann, Charge density wave-generated Fermi surfaces in NdTe₃, (2022).DOI
- [22]Ru, N., Condron, C., Margulis, G., Shin, K., Laverock, J., Dugdale, S., Toney, M., & Fisher, I. (2008). Effect of chemical pressure on the charge density wave transition in rare-earth tritellurides RTe₃. Physical Review B, 77, 035114.
- [23]D. A. Zocco, Interplay of Superconductivity, Magnetism, and Density Waves in Rare-Earth Tritellurides and Iron-Based Superconducting Materials, Ph.D. thesis, University of California, San Diego (2011).
- [24]D. A. Zocco, J. J. Hamlin, K. Grube, J.-H. Chu, H.-H. Kuo, I. R. Fisher, and M. B. Maple, Pressure dependence of the charge-density-wave and superconducting states in GdTe₃, TbTe₃, and DyTe₃, Physical Review B 91, 205114 (2015).DOI
- [25]S. Sarkar, J. Bhattacharya, P. Sadhukhan, D. Curcio, R. Dutt, V. Singh, M. Bianchi, A. Pari- ari, S. Roy, P. Mandal, T. Das, P. Hofmann, A. Chakrabarti, and S. Barman, Charge density wave induced nodal lines in LaTe3, Nature Communications 14, 3628 (2023).DOI
- [26]Y. Iyeiri, T. Okumura, C. Michioka, and K. Suzuki, Magnetic properties of rare-earth metal tritellurides RTe3 (R = Ce, Pr, Nd, Gd, Dy), Physical Review B 67, 144417 (2003).DOI
- [27]F. Pfuner, S. Gvasaliya, O. Zaharko, L. Keller, J. Mesot, V. Pomjakushin, J.-H. Chu, I. Fisher, and L. Degiorgi, Incommensurate magnetic order in TbTe3, Journal of Physics: Condensed Matter 24, 036001 (2011).DOI
- [28]Z. Yang, A. Drew, S. van Smaalen, N. van Well, F. Pratt, G. Stenning, A. Karim, and K. Rabia, Multiple magnetic-phase transitions and critical behavior of charge-density wave compound TbTe3, Journal of Physics: Condensed Matter 32, 305801 (2020).DOI
- [29]Q. Guo, D. Bao, L. Zhao, and S. Ebisu, Novel magnetic behavior of antiferromagnetic GdTe3 induced by magnetic field, Physica B: Condensed Matter 617, 413153 (2021).DOI
- [30]O. Volkova, A. Hadj-Azzem, G. Remenyi, J. Lorenzo, P. Monceau, A. Sinchenko, and A. Vasiliev, Magnetic Phase Diagram of van der Waals Antiferromagnet TbTe3, Materials 15, 8772 (2022).DOI
- [31]S. Chillal, E. Schierle, E. Weschke, F. Yokaichiya, J.-U. Hoffmann, O. S. Volkova, A. N. Vasiliev, A. Sinchenko, P. Lejay, A. Hadj-Azzem, P. Monceau, and B. Lake, Strongly coupled charge, orbital, and spin order in TbTe3, Physical Review B 102, 241110(R) (2020).DOI
- [32]K. Y. Shin, V. Brouet, N. Ru, Z. X. Shen, and I. R. Fisher, Electronic structure and charge-density wave formation in LaTe1.95 and CeTe2.00, Physical Review B 72, 085132 (2005).DOI
- [33]J. Straquadine, M. S. Ikeda, and I. Fisher, Evidence for Realignment of the Charge Density Wave State in ErTe3 and TmTe3 under Uniaxial Stress via Elastocaloric and Elastoresistivity Measurements, Physical Review X 12, 021046 (2022).DOI
- [34]R. Dickinson and L. Pauling, The crystal structure of molybdenite, Journal of the American Chemical Society 45, 1466 (1923).DOI
- [35]S. Manzeli, D. Ovchinnikov, D. Pasquier, O. Yazyev, and A. Kis, 2D transition metal dichalcogenides, Nature Reviews Materials 2, 17033 (2017).DOI
- [36]B. Stärk, P. Krüger, and J. Pollmann, Magnetic anisotropy of thin Co and Ni films on diamond surfaces, Physical Review B 84, 195316 (2011).DOI
- [37]E. Torun, H. Sahin, C. Bacaksiz, R. T. Senger, and F. M. Peeters, Tuning the magnetic anisotropy in single-layer crystal structures, Physical Review B 92, 104407 (2015).DOI
- [38]P. Gambardella, S. Stepanow, A. Dmitriev, J. Honolka, F. de Groot, M. Lingenfelder, S. Gupta, D. Sarma, P. Bencok, S. Stanescu, S. Clair, S. Pons, N. Lin, A. Seitsonen, H. Brune, J. Barth, and K. Kern, Supramolecular control of the magnetic anisotropy in two-dimensional high-spin Fe arrays at a metal interface, Nature Materials 8, 189 (2009).DOI
- [39]T. Honda, J. S. White, A. B. Harris, L. C. Chapon, A. Fennell, B. Roessli, O. Zaharko, Y. Murakami, M. Kenzelmann, and T. Kimura, Coupled multiferroic domain switching in the canted conical spin spiral system Mn₂GeO₄, Nature Communications 8, 15457 (2017).DOI
- [40]S. Riberolles, T. Trevisan, B. Kuthanazhi, T. Heitmann, F. Ye, D. Johnston, S. Bud’ko, D. Ryan, P. Canfield, A. Kreyssig, A. Vishwanath, R. McQueeney, L.-L. Wang, P. Orth, and B. Ueland, Magnetic crystalline-symmetry-protected axion electrodynamics and field-tunable unpinned Dirac cones in EuIn₂As₂, Nature Communications 12, 999 (2021).DOI
- [41]S. Lei, V. Duppel, J. Lippmann, J. Nuss, B. Lotsch, and L. Schoop, Charge Density Waves and Magnetism in Topological Semimetal Candidates GdSbxTe₂−x−δ, Advanced Quantum Technologies 2, 1900045 (2019).DOI
- [42]S. Lei, A. Saltzman, and L. Schoop, Complex magnetic phases enriched by charge density waves in the topological semimetals GdSbxTe₂−x−δ, Physical Review B 103, 134418 (2021).DOI
- [43]Grüner, G. (1988). The dynamics of charge-density waves. Reviews of Modern Physics, 60, 1129.
- [44]A. A. Sinchenko, P. Lejay, and P. Monceau, Sliding charge-density wave in two-dimensional rare-earth tellurides, Physical Review B 85, 241104 (2012).DOI
- [45]T. Moriya, Anisotropic Superexchange Interaction and Weak Ferromagnetism, Physical Review 120, 91 (1960).DOI
- [46]D. Ghader, B. Jabakhanji, and A. Stroppa, Whirling interlayer fields as a source of stable topological order in Moiré CrI₃, Communications Physics 5, 192 (2022).DOI
- [47]G. Volovik, Linear momentum in ferromagnets, Journal of Physics C: Solid State Physics 20, L83 (1987).DOI
- [48]Y. Tokura and N. Nagaosa, Nonreciprocal responses from non-centrosymmetric quantum materials, Nature Communications 9, 3740 (2018).DOI
- [49]J. A. Osborn, Demagnetizing Factors of the General Ellipsoid, Physical Review 67, 351 (1945).DOI
- [50]A. Scheie, PyCrystalField: Software for Calculation, Analysis and Fitting of Crystal Electric Field Hamiltonians, Journal of Applied Crystallography 54, 356 (2021).DOI
- [51]Y. Gao, Q. Yin, Q. Wang, Z. Li, J. Cai, T. Zhao, H. Lei, S. Wang, Y. Zhang, and B. Shen, Spon- taneous (Anti)meron Chains in the Domain Walls of van der Waals Ferromagnetic Fe₅−ₓGeTe₂, Advanced Materials 32, 2005228 (2020).DOI
- [52]T. T. Ly, J. Park, K. Kim, H.-B. Ahn, N. J. Lee, K. Kim, T.-E. Park, G. Duvjir, N. H. Lam, K. Jang, C.-Y. You, Y. Jo, S. K. Kim, C. Lee, S. Kim, and J. Kim, Direct Observation of Fe-Ge Ordering in Fe₅−ₓGeTe₂ Crystals and Resultant Helimagnetism, Advanced Functional Materials 31, 2009758 (2021).DOI
- [53]A. F. May, C. A. Bridges, and M. A. McGuire, Physical properties and thermal stability of Fe₅−ₓGeTe₂ single crystals, Physical Review Materials 3, 104401 (2019).DOI
- [54]M. Baenitz, M. M. Piva, S. Luther, J. Sichelschmidt, K. M. Ranjith, H. Dawczak-Dębicki, M. O. Ajeesh, S.-J. Kim, G. Siemann, C. Bigi, P. Manuel, D. Khalyavin, D. A. Sokolov, P. Mokhtari, H. Zhang, H. Yasuoka, P. D. C. King, G. Vinai, V. Polewczyk, P. Torelli, J. Wosnitza, U. Burkhardt, B. Schmidt, H. Rosner, S. Wirth, H. Kühne, M. Nicklas, and M. Schmidt, Planar triangular S = 3/2 magnet AgCrSe₂: Magnetic frustration, short range correlations, and field-tuned anisotropic cycloidal magnetic order, Physical Review B 104, 134410 (2021).DOI
- [55]U. K. Gautam, R. Seshadri, S. Vasudevan, and A. Maignan, Magnetic and transport properties, and electronic structure of the layered chalcogenide AgCrSe₂, Solid state communications 122, 607 (2002).DOI
- [56]T. Kurumaji, S. Seki, S. Ishiwata, H. Murakawa, Y. Kaneko, and Y. Tokura, Magnetoelectric responses induced by domain rearrangement and spin structural change in triangular-lattice helimagnets NiI₂ and CoI₂, Physical Review B 87, 014429 (2013).DOI
- [57]Lebedev, D., Gish, J. T., Garvey, E. S., Stanev, T. K., Choi, J., Georgopoulos, L., Song, T. W., Park, H. Y., Watanabe, K., Taniguchi, T., Stern, N. P., Sangwan, V. K., & Hersam, M. C. (2023). Electrical Interrogation of Thickness-Dependent Multiferroic Phase Transitions in the 2D Antiferromagnetic Semiconductor NiI$_2$. Advanced Functional Materials, 33, 2212568.
- [58]A. Adam, D. Billerey, C. Terrier, R. Mainard, L. Regnault, J. Rossat-Mignod, and P. Mériel, Neutron diffraction study of the commensurate and incommensurate magnetic structures of NiBr₂, Solid State Communications 35, 1 (1980).DOI
- [59]Y. Tokunaga, D. Okuyama, T. Kurumaji, T. Arima, H. Nakao, Y. Murakami, Y. Taguchi, and Y. Tokura, Multiferroicity in NiBr₂ with long-wavelength cycloidal spin structure on a triangular lattice, Physical Review B 84, 060406 (2011).DOI
- [60]C. R. Ronda, G. J. Arends, and C. Haas, Photoconductivity of the nickel dihalides and the nature of the energy gap, Physical Review B 35, 4038 (1987).pubmed.ncbi.nlm.nih.gov/9941930
- [61]Kurumaji, T., Seki, S., Ishiwata, S., Murakawa, H., Tokunaga, Y., Kaneko, Y., & Tokura, Y. (2011). Magnetic-Field Induced Competition of Two Multiferroic Orders in a Triangular-Lattice Helimagnet $\mathrm{MnI}_{2}$. Physical Review Letters, 106, 167206.
- [62]N. J. Ghimire, M. A. McGuire, D. S. Parker, B. Sipos, S. Tang, J.-Q. Yan, B. C. Sales, and D. Mandrus, Magnetic phase transition in single crystals of the chiral helimagnet Cr₁/₃NbS₂, Physical Review B 87, 104403 (2013).DOI
- [63]K. Lu, A. Murzabekova, S. Shim, J. Park, S. Kim, L. Kish, Y. Wu, L. DeBeer-Schmitt, A. A. Aczel, A. Schleife, N. Mason, F. Mahmood, and G. J. MacDougall, Understanding the Anomalous Hall effect in Co₁/₃NbS₂ from crystal and magnetic structures (2022), arXiv:2212.14762 [cond-mat.mtrl-sci].arXiv
- [64]G. Tenasini, E. Martino, N. Ubrig, N. J. Ghimire, H. Berger, O. Zaharko, F. Wu, J. F. Mitchell, I. Martin, L. Forró, and A. F. Morpurgo, Giant anomalous Hall effect in quasi-two-dimensional layered antiferromagnet Co₁/₃NbS₂, Physical Review Research 2, 023051 (2020).DOI
- [65]H. Takagi, R. Takagi, S. Minami, T. Nomoto, K. Ohishi, M.-T. Suzuki, Y. Yanagi, M. Hirayama, N. Khanh, K. Karube, H. Saito, D. Hashizume, R. Kiyanagi, Y. Tokura, R. Arita, T. Nakajima, and S. Seki, Spontaneous topological Hall effect induced by non-coplanar antiferromagnetic order in intercalated van der Waals materials, Nature Physics 19, 961 (2023).DOI
- [66]Kousaka, Y., Ogura, T., Zhang, J., Miao, P., Lee, S., Torii, S., Kamiyama, T., Campo, J., Inoue, K., & Akimitsu, J. (2016). Long Periodic Helimagnetic Ordering in $\mathrm{CrM}_{3}\mathrm{S}_{6}$ ($M = \mathrm{Nb}$ and $\mathrm{Ta}$). Journal of Physics: Conference Series, 746, 012061.
- [67]Miyadai, T., Kikuchi, K., Kondo, H., Sakka, S., Arai, M., & Ishikawa, Y. (1983). Magnetic Properties of $\mathrm{Cr}_{1/3}\mathrm{NbS}_{2}$. Journal of the Physical Society of Japan, 52, 1394.
- [68]L. Wang, N. Chepiga, D.-K. Ki, L. Li, F. Li, W. Zhu, Y. Kato, O. S. Ovchinnikova, F. Mila, I. Martin, D. Mandrus, and A. F. Morpurgo, Controlling the Topological Sector of Magnetic Solitons in Exfoliated Cr₁/₃NbS₂ Crystals, Physical Revie Letters 118, 257203 (2017).DOI
- [69]Obeysekera, D., Gamage, K., Gao, Y., Cheong, S.-. w ., & Yang, J. (2021). The Magneto-Transport Properties of $\mathrm{Cr}_{1/3}\mathrm{TaS}_{2}$ with Chiral Magnetic Solitons. Advanced Electronic Materials, 7, 2100424.
- [70]C. Zhang, J. Zhang, C. Liu, S. Zhang, Y. Yuan, P. Li, Y. Wen, Z. Jiang, B. Zhou, Y. Lei, D. Zheng, C. Song, Z. Hou, W. Mi, U. Schwingenschlögl, A. Manchon, Z. Q. Qiu, H. N. Alshareef, Y. Peng, and X.-X. Zhang, Chiral Helimagnetism and One-Dimensional Magnetic Solitons in a Cr-Intercalated Transition Metal Dichalcogenide, Advanced Materials 33, 2101131 (2021).DOI
- [71]C.-H. Zhang, H. Algaidi, P. Li, Y. Yuan, and X.-X. Zhang, Magnetic soliton confinement and discretization effects in Cr₁/₃TaS₂ nanoflakes, Rare Metals 41, 3005 (2022).DOI
- [72]Tables of Form Factors. (2023). Tables of Form Factors. https://www.ill.eu/sites/ccsl/ffacts/ill.eu/sites/ccsl/ffacts
- [73]Squires, G. L. (2012). Introduction to the Theory of Thermal Neutron Scattering.
- [74]Slovyanskikh, V., Kuznetsov, N., & Gracheva, N. (1985). The Dy-U-Te system. Russian Journal of Inorganic Chemistry, 30, 1666.
- [75]C. Malliakas, S. J. L. Billinge, H. J. Kim, and M. G. Kanatzidis, Square Nets of Tellurium: Rare-Earth Dependent Variation in the Charge-Density Wave of RETe₃ (RE = Rare-Earth Element), Journal of the American Chemical Society 127, 6510 (2005).DOI
- [76]M. I. Aroyo, A. Kirov, C. Capillas, J. M. Perez-Mato, and H. Wondratschek, Bilbao Crystallographic Server II: Representations of crystallographic point groups and space groups, Acta Crystallographica A62, 115 (2006).pubmed.ncbi.nlm.nih.gov/16489249
- [77]Kenzelmann, M., Harris, A. B., Aharony, A., Entin-Wohlman, O., Yildirim, T., Huang, Q., Park, S., Lawes, G., Broholm, C., Rogado, N., Cava, R. J., Kim, K. H., Jorge, G., & Ramirez, A. P. (2006). Field dependence of magnetic ordering in Kagomé-staircase compound Ni$_3$V$_2$O$_8$. Phys. Rev. B, 74, 014429.
- [78]Brown, P., Chattopadhyay, T., Forsyth, J., & Nunez, V. (1991). Magnetic phase transitions of MnWO$_4$ studied by the use of neutron diffraction. J. Phys.: Condens. Matter, 48, 4281.
- [79]G. Lautenschläger, H. Weitzel, T. Vogt, R. Hock, A. Böhm, M. Bonnet, and H. Fuess, Magnetic phase transitions of MnWO₄ studied by the use of neutron diffraction, Phys. Rev. B 48, 6087 (1993).pubmed.ncbi.nlm.nih.gov/10009145
- [80]A. Biffin, R. D. Johnson, I. Kimchi, R. Morris, A. Bombardi, J. G. Analytis, A. Vishwanath, and R. Coldea, Noncoplanar and Counterrotating Incommensurate Magnetic Order Stabilized by Kitaev Interactions in γ−Li₂IrO₃, Phys. Rev. Lett. 113, 197201 (2014).pubmed.ncbi.nlm.nih.gov/25415919
- [81]Pardo, M. P., & Flahaut, J. (1967). Les tellurures superieurs des elements des terres rares, de formules L$_2$Te$_5$ et LTe$_3$. Bulletin de la Société Chimique de France, 3658.
- [82]M. Kenzelmann, A. B. Harris, S. Jonas, C. Broholm, J. Schefer, S. B. Kim, C. L. Zhang, S.-W. Cheong, O. P. Vajk, and J. W. Lynn, Magnetic Inversion Symmetry Breaking and Ferroelectricity in TbMnO3, Phys. Rev. Lett. 95, 087206 (2005).DOI
- [83]C. Dos Santos, A. De Campos, M. Da Luz, B. White, J. Neumeier, B. De Lima, and C. Shigue, Procedure for measuring electrical resistivity of anisotropic materials: A revision of the Montgomery method, Journal of Applied Physics 110 (2011).DOI