betaFeedback

WorksPhysics and Astronomy

Strain-enhanced superconductivity in RuO2_2 thin films: Joint experimental and theoretical studies

Abstract

We investigate the superconducting properties of RuO2_2 films grown on TiO2_2 substrates by combining film fabrication and transport measurement with ab initio calculation. Experimentally, we grow several RuO2_2 (110) thin films on TiO2_2 (110) substrates and observe superconductivity with critical temperature (TcT_c) of ∼\sim2.0 K in 20-nm and 30-nm RuO2_2 (110) thin films. Theoretically, we study the superconductivity in both RuO2_2 (110) and RuO2_2 (100) epitaxial films within McMillan formalism of isotropic Migdal-Eliashberg theory. Among the salient results, the calculated phonon dispersion relations of all the considered RuO2_2 films show that the epitaxial films are dynamically stable. Importantly, our ab initio calculations reveal that independent of the film orientation, the [001] compressive strain ε[001]ε_{[001]} pushes the flat Ru dz2d_{z^2}-dominant bands towards the Fermi level (EFE_F), and significantly soften the out-of-plane acoustic phonon mode near the R point in the Brillouin zone, which substantially enhances the electron-phonon coupling (EPC) strength λλ and hence the calculated TcT_c in the RuO2_2 films. Remarkably, the amount of the phonon softening and the enhanced TcT_c increase almost linearly with the increasing ε[001]ε_{[001]}. The calculated TcT_c for the films with thickness of ≥\geq 20 nm agree well with the experimental TcT_c. These findings demonstrate that among other things, lattice mismatch strain provides an effective route for tuning phonon-mediated superconductivity in RuO2_2 and other thin films.

Introduction

Superconductivity in transition-metal oxides (TMOs) continues to be an active area of research because of the wide range of pairing mechanisms and electronic behaviors. TMOs such as ruthenates and cuprates reveal how strong electron correlations give rise to unconventional superconductivity [1]. In particular, oxides based on ruthenium have long been a rich source of emergent quantum phenomena. Unconventional superconductivity in Sr2RuO4\mathrm{Sr}_{2}\mathrm{RuO}_{4}, metamagnetic behavior in Sr3Ru2O7\mathrm{Sr}_{3}\mathrm{Ru}_{2}\mathrm{O}_{7}, and antiferromagnetic and ferromagnetic states in ruthenates based on calcium and strontium are notable examples [2-4]. The understanding of correlated electron systems has improved extensively as a result of these materials.

It is commonly known that rutile-structured RuO2\mathrm{RuO}_{2} is a highly conducting binary oxide [5-7] with numerous engineering applications, including catalysts, thin films, electrodes, and thermometers. Thin films, primarily polycrystalline films, have been produced for these applications using a variety of growth techniques [11, 12, 13, 14, 15, 16, 17] [8, 9, 10]. A further and particularly striking development was the observation that superconductivity can be induced in RuO2\mathrm{RuO}_{2} through epitaxial strain [18, 19]. While bulk RuO2\mathrm{RuO}_{2} remains non-superconducting down to 0.3 K [7], superconductivity with TcT_{\mathrm{c}} on the order of ∼1.0\sim1.0 K was realized in RuO2\mathrm{RuO}_{2} (110) thin films grown on TiO2\mathrm{TiO}_{2} (110) substrates. In contrast, films grown on other rutile orientations and on alternative substrates such as MgF2\mathrm{MgF}_{2} and α−Al2O3\alpha-\mathrm{Al}_{2}\mathrm{O}_{3} (0001) and α−Al2O3\alpha-\mathrm{Al}_{2}\mathrm{O}_{3} (110ˉ2)(11\bar{0}2) were reported to remain non-superconducting [20, 21]. These results establish superconductivity in RuO2\mathrm{RuO}_{2} as highly sensitive to epitaxial orientation and strain anisotropy.

The microscopic origin of the superconductivity in the RuO2\mathrm{RuO}_{2} (110) thin films has been linked to symmetry breaking of the rutile lattice and the resulting modification of the electronic structure [22]. Epitaxial strain alters Ru-O hybridization, redistributes Ru dd-orbital occupancies, and enhances the density of states near the Fermi level, all of which can favor superconductivity [18]. Very recently, superconductivity in strained RuO2\mathrm{RuO}_{2} (100) thin films was also reported, indicating that superconductivity in RuO2\mathrm{RuO}_{2} is not limited to the (110) orientation grown on TiO2\mathrm{TiO}_{2} (110) single-crystal substrates [23].

Previous theoretical and experimental studies suggested that superconductivity in RuO2\mathrm{RuO}_{2} thin films can be strongly influenced by epitaxial strain [18, 19, 23]. In particular, previous ab initio studies RuO2\mathrm{RuO}_{2} films demonstrated that strain-induced structural distortion modifies the low-energy electronic states and lattice dynamics in RuO2\mathrm{RuO}_{2} films, and also indicated that strain can significantly alter the Ru-O bonding environment and the associated electron-phonon interactions that govern superconductivity in RuO2\mathrm{RuO}_{2} films [18, 19, 23]. However, these theoretical works on RuO2\mathrm{RuO}_{2} thin films also reported the appearance of imaginary phonon modes [18, 19, 23], implying lattice instabilities of the strained films and thus hindering a proper description of phonon-mediated superconductivity. This raises an important question regarding the stability of strained RuO2\mathrm{RuO}_2 thin films and the microscopic mechanism responsible for the emergence and enhancement of superconductivity in the RuO2\mathrm{RuO}_2 films.

In this work, we combine both transport experiments and ab initio calculations to examine how lattice mismatch induced-strain affect the electronic structure, phonon dispersion, electron-phonon coupling, and superconductivity in RuO2\mathrm{RuO}_2 thin films. Importantly, in contrast to previous theoretical predictions [18, 19, 23], our calculated phonon dispersions in the RuO2\mathrm{RuO}_2 films do not show any imaginary frequencies, indicating that the strained RuO2\mathrm{RuO}_2 films are dynamically stable. This enable us to provide a proper description of lattice dynamics, electron-phonon coupling and superconductivity in the considered RuO2\mathrm{RuO}_2 films. Indeed, our calculated TcT_c of 2.8 K for 20-nm RuO2\mathrm{RuO}_2 (110) film and 0.8 K for 28-nm RuO2\mathrm{RuO}_2 (100) film agree well with the experimental TcT_c of 2.0 K from this work and 1.0 K [23], respectively.

The rest of this paper is organized as follows. In the next section, we report the results of our experiments on epitaxial RuO2\mathrm{RuO}_2 (110) films on TiO2\mathrm{TiO}_2 (110) substrates. In Sec. III, a brief description of the crystal structure of bulk RuO2\mathrm{RuO}_2 and lattice mismatch strains in the considered RuO2\mathrm{RuO}_2 films is provided. In Sec. IV, we summarize the McMillan formalism of the isotropic Migdal-Eliashberg theory of phonon-mediated superconductivity and details of our ab initio calculations. The calculated electronic band structure, phonon dispersion, electron-phonon coupling and superconductivity are presented and compared with available experiments in § 5 and the supplemental material. In § 7, we discuss the thickness dependence of TcT_c in ultrathin RuO2\mathrm{RuO}_2 films and also examine the effect of screened Coulomb pseudopotential μ∗\mu^* on TcT_c. Finally, the conclusions drawn from this work are summarized in § 8.

Film Fabrication and Measurement

Figure 1(a) shows the X-ray (XRD) scans of RuO2(t)/TiO2\mathrm{RuO}_2(t)/\mathrm{TiO}_2 (110) substrates (RuO2(t)/TiO2\mathrm{RuO}_2(t)/\mathrm{TiO}_2 (110)) with nominal thicknesses (tt) of 3-nm, 8-nm, and 20-nm, grown by using ozone-assisted molecular beam epitaxy (MBE). The reflections from the RuO2\mathrm{RuO}_2 (220) and (330) planes are accompanied by notable thickness fringes, justifying the exceptional crystallinity and thickness uniformity in the RuO2\mathrm{RuO}_2 thin films. By fitting to the XRD, the lattice constants of d(11ˉ0)d_{(1\bar{1}0)}, d(001)d_{(001)}, and d(110)d_{(110)} are extracted and listed in Table I, exhibiting tt-dependent anisotropic strain in the RuO2\mathrm{RuO}_2 films as compared to the bulk RuO2\mathrm{RuO}_2 lattice. For t=3t = 3 nm, the RuO2\mathrm{RuO}_2 film is fully strained to the TiO2\mathrm{TiO}_2 (110) substrate, resulting in a compressive strain of −4.7%-4.7\% along [001] and a tensile strain of about +2.3% along [1-10]. As tt increases to 20 nm, the compressive strain partly relaxes to about -3.1% along [001]. We also note that the film thickness extracted from the thickness fringes and low-angle reflectivity is consistent with the nominal thickness.

Systemd(110)d_{(110)} (Å)d(1−10)d_{(1-10)} (Å)d(001)d_{(001)} (Å)
Bulk RuO2_23.1763.1763.106
30-nm film-3.2483.033
20-nm film3.2303.2453.010
8-nm film3.2373.2493.003
3-nm film3.2363.2482.965
Bulk TiO2_23.2483.2482.959

Table I. The extracted lattice constants of d(1−10)d_{(1-10)}, d(001)d_{(001)} and d(110)d_{(110)} in RuO2_2(tt nm)/TiO2_2(110) with t=3t = 3 nm, 8 nm, 20 nm and 30 nm. Bulk RuO2_2 and TiO2_2 lattice constants are included for comparison.

XRD and transport data of RuO2 films

Figure 1. XRD and transport data of RuO2_2 (tt nm)/TiO2_2(110): (a) XRD scans of RuO2_2(tt nm)/TiO2_2(110) with t=3t = 3 nm, 8 nm, and 20 nm. The reflections from TiO2_2 (110) substrate are labeled with * symbols. Pronounced thickness fringes appear around the RuO2_2 Bragg peaks for all tt values, justifying the high crystallinity and uniform thickness in the RuO2_2 films. (b) The normalized resistivity ρ/ρ3K\rho/\rho_{3K} versus temperature for T≤3T \le3 K in RuO2_2 (tt nm)/TiO2_2(110) with tt ranging from 3 nm to 45 nm, highlighting a superconducting transition with a Tc≈1.97T_c \approx1.97 K for t=20t = 20 nm and non-monotonic tt-dependent TcT_c. The inset shows the tt-dependence of ρ3K\rho_{3K} and TcT_c.

The temperature dependence of normalized resistivity ρ/ρ3K\rho/\rho_{3K} of RuO2_2 (tt nm)/TiO2_2 (110) with various thicknesses down to 1.5 K, are shown in Figure 1(b), highlighting the onset of a superconducting transition at around Tc≈2.2T_c \approx2.2 K for t=20t = 20 nm and 30 nm RuO2_2 thin films. For t=20t = 20 nm, the residual resistivity (RR) at T=5T = 5 K and the residual resistivity ratio (RRR ≡ρ300K/ρ5K\equiv\rho_{300K}/\rho_{5K}) are ∼\sim17.2 μΩ\mu\Omega-cm and 4.0, respectively. It gives a superconducting transition temperature Tc≈1.97T_c \approx1.97 K, which was defined as the temperature at which the resistivity drops by half of its normal state value.

The normal state resistivity ρ3K\rho_{3K} monotonically increases with decreasing tt, but the TcT_c attains a maximum at a thickness ranging from 20 to 30 nm as shown in the inset of Figure 2 (b). The further strain relaxation along [001] for t>30t > 30 nm and the increasing disorder for t<20t < 20 nm tend to suppress the superconductivity, resulting in a non-monotonic tt-dependence of TcT_c as a signature for the strain-stabilized superconductivity in RuO2_2 thin films.

Schematic diagrams, crystal structures, and Brillouin zones of strained RuO2 thin-films

Figure 2. (a, b) Schematic diagram of strain applied on RuO2\mathrm{RuO}_2 (a) (110) thin-film and (b) (100) thin-film. (c, d, e) Crystal structure of RuO2\mathrm{RuO}_2 (c) bulk, (d) (110)-oriented thin-film and (e) (100)-oriented thin-film. (f-h) Brillouin zones of (110) thin-film for (f) b′<c′b' < c' (corresponds to 3-nm thin-film), (g) b′=c′b' = c' (corresponds to bulk RuO2\mathrm{RuO}_2), and (h) b′>c′b' > c' (corresponds to 20-nm thin-film). (i) Brillouin zone of (100) thin-film.

Crystal Structure and Lattice Mismatch Strain

Ruthenium dioxide (RuO2\mathrm{RuO}_2) has a tetragonal rutile crystal structure, with point group D4hD_{4h} and space group P42/mnmP4_2/mnm (No. 136). When RuO2\mathrm{RuO}_2 is deposited on TiO2\mathrm{TiO}_2 (110) substrate, lattice mismatch strain is applied on the RuO2\mathrm{RuO}_2 (110) thin-film, which compress it along [001]-direction (a′a') but extends it along [11ˉ01\bar{1}0]-direction (b′b') [see Figure 2(a)]. As a result, the lattice constant of the out-of-plane (110) direction (c′c') would expand (see Table I). The above effect lowers the point group to D2hD_{2h} while the space group becomes CmmmCmmm (No. 65). The strained RuO2\mathrm{RuO}_2 (110) films thus become orthorhombic. The lattice constants of a strained RuO2\mathrm{RuO}_2 (110) film can be expressed in the form

(a′b′c′)=(001+ϵ[001]1+ϵ[11ˉ0]0001+ϵ[110]0)(2abulk2abulkcbulk)(1)\begin{pmatrix} a' \\ b' \\ c' \end{pmatrix} = \begin{pmatrix} 0 & 0 & 1+\epsilon_{[001]} \\ 1+\epsilon_{[1\bar{1}0]} & 0 & 0 \\ 0 & 1+\epsilon_{[110]} & 0 \end{pmatrix} \begin{pmatrix} \sqrt{2}a_{\mathrm{bulk}} \\ \sqrt{2}a_{\mathrm{bulk}} \\ c_{\mathrm{bulk}} \tag*{(1)} \end{pmatrix}

where ϵ[nml]\epsilon_{[nml]} is the strain along [nml][nml]-direction. Here, abulka_{\mathrm{bulk}} and cbulkc_{\mathrm{bulk}} are the primitive cell lattice constants of bulk RuO2\mathrm{RuO}_2. Detailed information is provided in tbl:2.

On the other hand, when RuO2\mathrm{RuO}_2 is deposited on TiO2\mathrm{TiO}_2 (100) substrate, the in-plane lattice constant along [010]-direction (a′a') expands while the one along [001]-direction (b′b') is compressed. Consequently, the lattice constant of the out-of-plane (110) direction (c′c') expands. The strain effect changes the point group to D2hD_{2h} while the space group becomes PnnmPnnm (No. 58). The strained RuO2\mathrm{RuO}_2 film is orthorhombic and their lattice constants are given by

(a′b′c′)=(01+ϵ[010]0001+ϵ[001]1+ϵ[100]00)(abulkabulkcbulk)(2)\begin{pmatrix} a' \\ b' \\ c' \end{pmatrix} = \begin{pmatrix} 0 & 1+\epsilon_{[010]} & 0 \\ 0 & 0 & 1+\epsilon_{[001]} \\ 1+\epsilon_{[100]} & 0 & 0 \end{pmatrix} \begin{pmatrix} a_{\mathrm{bulk}} \\ a_{\mathrm{bulk}} \\ c_{\mathrm{bulk}} \tag*{(2)} \end{pmatrix}

Theory and Computational Details

All ab initio structural optimizations are performed within the density functional theory (DFT) with the generalized gradient approximation (GGA) plus the PBEsol parameterization [24, 25]. The projector-augmented wave method [26], as implemented in the Vienna Ab Initio Simulation Package (VASP) [27, 28], is employed. A plane-wave energy cutoff of 500 eV is adopted. Brillouin-zone integrations are carried out using the tetrahedron method with a Γ\Gamma-centered 12×12×1812 \times12 \times18 kk-point mesh. Structural optimization is considered converged when the forces on all atoms are less than 0.005 eV/Å. For bulk RuO2\mathrm{RuO_2}, both lattice parameters and internal atomic coordinates are fully relaxed. The calculated lattice constants of bulk RuO2\mathrm{RuO_2} are a=4.4942a = 4.4942 Å and c=3.1097c = 3.1097 Å, agreeing very well with the experimental values (within 0.2%) (Table I).

RuO2\mathrm{RuO_2} (110) and (100) thin films are modeled within a strained-bulk approach (i.e., the effect of finite film thickness is neglected). This approach should work quite well for films with thicknesses of ≥20\geq20-nm. For ultrathin films with thicknesses of ≤10\leq10-nm, however, the effects of disorders, coherence length, surface and interface would become pronounced, and consequently, the ab initio calculations using the strained-bulk approach may not properly describe the observed superconducting properties. See § 7. B for further discussion on this topic. For a RuO2\mathrm{RuO_2} film, the in-plane lattice constants a′a' and b′b' are fixed to the corresponding experimental values. However, the out-of-plane lattice constant (c′c') and all internal atomic positions are allowed to relax to minimize the total energy. We note that such structural optimization calculations are needed to avoid the occurrence of the phonon modes with an imaginary frequency in the strained RuO2\mathrm{RuO_2} films [18, 19, 23] and hence to calculate the superconducting properties properly. The theoretically determined lattice constants c′c' for all the RuO2\mathrm{RuO_2} (110) and (100) thin films are listed in Table II and III, respectively. We notice that the differences between the calculated and experimental lattice constant c′c' are less than 0.6% (see Table I and Table II).

Systema′a' (Å)ϵ[001]\epsilon_{[001]}b′b' (Å)ϵ[11ˉ0]\epsilon_{[1\bar{1}0]}c′c' (Å)ϵ[110]\epsilon_{[110]}
Bulk RuO2_23.10976.35586.3558
30-nm Film3.033-2.466%6.4952.198%6.43231.204%
20-nm Film3.010-3.206%6.4902.180%6.51001.591%
8-nm Film3.003-3.431%6.4982.175%6.46501.681%
3-nm Film2.965-4.653%6.4962.171%6.45902.418%

Table II. Theoretical lattice parameters of bulk RuO2_2 and strained RuO2_2 (110) thin-films. Note that in-plane lattice constants a′a' and b′b' of strained RuO2_2 (110) thin-films are taken from Table I and are fixed. a′=d(001)a'=d_{(001)}, b′=2d(1−10)b'=2d_{(1-10)} and c′=2d(110)c'=2d_{(110)}. Lattice mismatch strains ϵ\epsilon [nm] are also listed, which are defined as [(d(nml)(film)−d(nml)(bulk))/d(nml)(bulk)][(d_{(nml)}(\mathrm{film})-d_{(nml)}(\mathrm{bulk}))/d_{(nml)}(\mathrm{bulk})].

The electronic structure calculations are carried out using a plane-wave pseudopotential formalism, as implemented in the Quantum ESPRESSO package [29, 30]. The optimized norm-conserving Vanderbilt (ONCV) scalar-relativistic pseudopotentials generated with the ONCVPSP code and the PBEsol exchange-correlation functional [31] are adopted. For ruthenium (Ru), the pseudopotential includes the 4s24p64d75s14s^2 4p^6 4d^7 5s^1 electrons as (16) valence electrons, and for oxygen (O), it includes the 2s22p42s^2 2p^4 electrons as (6) valence electrons. The other electrons are treated as part of the frozen cores. In all the calculations, we use plane-wave kinetic-energy and charge-density cutoffs of 90 Ry and 720 Ry, respectively. Brillouin zone integrations for the electronic structure and density of states (DOS) calculations are performed using a 16×16×2416 \times16 \times24 Monkhorst-Pack kk-point mesh. Electronic occupations are treated using Gaussian broadening of 0.05 Ry for all the considered systems except that Gaussian broadening of 0.06 Ry is used for the 3-nm RuO2_2 (110) film. Self-consistency is achieved with an energy convergence threshold of 10−910^{-9} Ry.

Phonon dispersions, phonon DOS and electron-phonon coupling (EPC) matrix elements gmn,ν(k,q)g_{mn,\nu}(\mathbf{k},\mathbf{q}) are computed using the density functional perturbation theory (DFPT) [32], as implemented in Quantum ESPRESSO [29, 30]. A phonon momentum grid of 4×4×64 \times4 \times6 is used for both bulk and all RuO2_2 thin film structures. In this work, we consider phonon-mediated superconductivity in all the considered RuO2_2 films and bulk RuO2_2. The superconducting transition temperatures are evaluated with the McMillan-Allen-Dynes formulas [33, 34]

Tc=ωlog⁡1.2exp⁡[−1.04(1+λ)λ−μ∗(1+0.62λ)](3)T_c = \frac{\omega_{\log}}{1.2}\exp\left[\frac{-1.04(1+\lambda)}{\lambda-\mu^{*}(1+0.62\lambda)}\right] \tag*{(3)}

where ωlog⁡\omega_{\log} is the logarithmic average phonon frequency,

ωlog⁡=exp⁡[2λ∫dωωα2F(ω)log⁡ω](4)\omega_{\log} = \exp\left[\frac{2}{\lambda}\int\frac{d\omega}{\omega}\alpha^2F(\omega)\log\omega\right] \tag*{(4)}

λ\lambda is the dimensionless EPC constant

λ=2∫α2F(ω)ωdω,(5)\lambda= 2\int\frac{\alpha^2F(\omega)}{\omega}d\omega, \tag*{(5)}

μ∗\mu^* is the averaged screened electron-electron interaction and α2F(ω)\alpha^2F(\omega) is the isotropic Eliashberg spectral function, which describes frequency-dependent EPC strength. Within the isotropic Migdal-Eliashberg theory [35],

α2F(ω)=12∑qνωqνλqνδ(ω−ωqν),(6)\alpha^2F(\omega)=\frac{1}{2}\sum_{\mathbf{q}\nu}\omega_{\mathbf{q}\nu}\lambda_{\mathbf{q}\nu}\delta(\omega-\omega_{\mathbf{q}\nu}), \tag*{(6)}

where ωqν\omega_{\mathbf{q}\nu} is the phonon frequency of mode ν\nu at wave vector q\mathbf{q}, and λqν\lambda_{\mathbf{q}\nu} is the phonon mode resolved EPC and is given by

λqν=1N(EF)ωqν∑mn,k∣gmn,ν(k,q)∣2δ(εnk−εF)δ(εmk+q−εF).(7)\lambda_{\mathbf{q}\nu}=\frac{1}{N(E_F)\omega_{\mathbf{q}\nu}}\sum_{mn,\mathbf{k}}\left|g_{mn,\nu}(\mathbf{k},\mathbf{q})\right|^2\delta(\varepsilon_{n\mathbf{k}}-\varepsilon_F)\delta(\varepsilon_{m\mathbf{k}+\mathbf{q}}-\varepsilon_F). \tag*{(7)}

Here N(EF)N(E_F) is the electronic DOS at the Fermi level (EFE_F). Therefore, the λ\lambda and ωlog⁡\omega_{\log} can be obtained from the ab initio calculations. Nevertheless, μ∗\mu^* is generally treated as a semiempirical parameter, and it typically varies from 0.05 to 0.30 [36, 37, 38]. Here we set μ∗=0.25\mu^*=0.25 (See § 7. A for the discussion on the choice of μ∗\mu^*).

Systema′a' (Å)ϵ[010]\epsilon_{[010]}b′b' (Å)ϵ[001]\epsilon_{[001]}c′c' (Å)ϵ[100]\epsilon_{[100]}
Bulk RuO2_24.4943.1104.494
28-nm Film4.5801.914 %3.040-2.241 %4.5180.534%
17-nm Film4.5801.914 %3.020-2.885 %4.5431.090%

Table 3. Theoretical lattice parameters of bulk RuO2_2 and strained RuO2_2 (100) thin-films. Note that the experimental in-plane lattice constants a′a' and b′b' of strained RuO2_2 (100) thin-films from [23] are used. Lattice mismatch strains ϵ[nml]\epsilon_{[nml]} are also listed, which are defined as [(d(nml)(film)−d(nml)(bulk))/d(nml)(bulk)][(d_{(nml)}(\mathrm{film})-d_{(nml)}(\mathrm{bulk}))/d_{(nml)}(\mathrm{bulk})].

Results

Electronic band structure

In Figure 3, we present the calculated electronic band structures along high-symmetry paths in the Brillouin zone and also DOS for bulk RuO2_2 as well as strained 20-nm RuO2_2 (110) and 28-nm RuO2_2 (100) films. The corresponding orbital-projected band structures and atom-decomposed DOS spectra are displayed in Figure S1 in the Supplementary Material (SM) [39]. The calculated band structures and DOS spectra for strained 30-nm, 8-nm, and 3-nm RuO2_2 (110), and 17-nm RuO2_2 (100) films are presented in Figure S2 in SM [39]. The crystal field splits Ru dd-orbital dominant bands to Ru ege_g bands and t2gt_{2g} bands. Since we focus on the superconducting properties of the considered RuO2_2 systems in this work, we plot the energy bands and DOS spectra only in the energy range from 2.0 eV below EFE_F to 2.0 eV above EFE_F. All the energy bands in this energy window are Ru t2gt_{2g} bands [40]. Ru ege_g orbitals hybridize strongly with 12 O pp orbitals, and consequently, twelve O pp-dominated bonding bands lie below -2.0 eV and four Ru ege_g-dominated antibonding bands lie above 2.0 eV [40]. Because of the coordinate systems used in the present calculations, Ru t2gt_{2g}-dominated bands include all five dd-orbitals, namely, dxyd_{xy}, dxzd_{xz}, dyzd_{yz}, dx2−y2d_{x^2-y^2} and dz2d_{z^2}.

Electronic band structures and density of states for bulk RuO2 and RuO2 thin films

Figure 3. (a, c) Electronic band structure and (b, d) density of states (DOS) for bulk RuO2_2, 20-nm RuO2_2 (110) (b), and 28-nm RuO2_2 (100) (d) thin films. The double arrowed lines denote the upwards shift Δelup\Delta_{\mathrm{el}}^{\mathrm{up}} of the flat Ru dz2d_{z^2} bands near R due to the compressive strain ϵ[001]\epsilon_{[001]} in the RuO2_2 films.

Orbital-projected band structures and density of states for bulk and strained RuO2 films

Figure S1. (a, c, e) Orbital-projected band structures and (b, d, f) total and orbital-decomposed density of states (DOS) for bulk RuO2_2, 20-nm RuO2_2 (110), and 28-nm RuO2_2 (100) films. The Fermi level is set to zero.

Electronic band structures and total density of states for strained RuO2 films

Figure S2. (a, c) Electronic band structures and (b, d) the total density of states (DOS) for 30-nm, 8-nm, and 3-nm RuO2_2 (110) and 17-nm RuO2_2 (100) films. The Fermi level is set to zero.

Figure 3, Figure S1 and Figure S2 show that in both bulk RuO2_2 and all considered RuO2_2 films, four energy bands cross the Fermi level. This confirms their metallic behavior, as observed in the present and many previous experiments [18, 19] [5, 6, 7]. Figure S1 in SM [39] further indicates that the energy bands that cross EFE_F arise from Ru dxyd_{xy}, dxzd_{xz} orbitals along Γ-Z direction, and dx2−y2d_{x^2-y^2} orbitals along Γ-X and M-Γ paths. One notable feature in the band structures of all the considered RuO2_2 systems is the occurrence of two flat Ru dz2d_{z^2} dominated bands along the in-plane Z-R-A-Z directions (see Figure 3, Figure S1 and Figure S2), mainly due to the weak interactions among Ru dz2d_{z^2} orbitals in the in-plane directions and being consistent with the isotropic nature of the rutile lattice. Interestingly, there are also two flat bands of dxyd_{xy}, dxzd_{xz}, and dxyd_{xy} characters along the M-Γ direction.

Figure 3, Figure S1 and Figure S2 indicate that the calculated energy bands in all the considered RuO2_2 films are similar to that of bulk RuO2_2. Furthermore, these figures also suggest that the DOS spectra of the RuO2_2 films are qualitatively the same as that of bulk RuO2_2. All the considered RuO2_2 systems show a finite DOS at the Fermi level, consistent with their observed metallic behavior. Moreover, all the considered systems exhibit a pronounced peak in the DOS spectrum slightly below EFE_F, due to the prominent flat Ru dz2d_{z^2} dominated bands along the in-plane Z-R-A-Z directions noted above.

However, noticeable modifications caused by the biaxial strains in the considered RuO2_2 films are observed in the vicinity of the Fermi level. In particular, Figure 3 and Figure S2 in the SM [39] show that the flat Ru dz2d_{z^2} bands along the Z-R-A-Z directions move towards EFE_F monotonically with increasing compressive strain ϵ[001]\epsilon_{[001]} due to the decreasing film thickness. Consequently, the prominent peak in the DOS spectrum also shifts toward EFE_F. Nevertheless, they remain about 0.5 eV below EFE_F (see Figure 3, Figure S1 and Figure S2), and thus the shift hardly modifies the DOS at EFE_F (see Table V). The shift of these flat bands is observed in both RuO2_2 (110) and RuO2_2 (100) films, being nearly orientation-independent (see Figure 3). For example, Figure 3 shows that the shift of the flat bands is more pronounced in the 20-nm RuO2_2 (110) film than in the 28-nm RuO2_2 (100) film. Interestingly, this could be correlated with the relative calculated and experimental TcT_c values in these RuO2_2 films (see Table V). Nevertheless, the increase in N(EF)N(E_F) is rather insignificant (see Table V).

Phonon dispersion relations

The calculated phonon dispersion, total and atom-projected phonon DOS spectra of bulk RuO2_2 are depicted in Figure 4. Because the primitive unit cell contains six atoms, there are 18 phonon bands in Figure 4(a), three acoustic modes and 15 optical modes. The frequencies of the optical modes at the BZ center are listed in Table IV, which can be compared with optical experiments. Indeed, the frequencies of Raman active phonon modes have been measured [41]. Table IV indicates that the calculated and measured frequencies of Raman active modes agree quite well with each other, with the differences being within 8%. Figure 4(b) shows that the PhDOS spectrum below 36 meV mainly results from the vibrations of heavy Ru atoms, while the vibrations of light O atoms dominate the DOS above 36 meV.

Phonon dispersion and total and atom-projected phonon density of states of bulk RuO2

Figure 4. (a) Phonon dispersion and (b) total and atom-projected phonon density of states (PhDOS) of bulk RuO2_2. Experimental PhDOS from inelastic neutron scattering [42] is also plotted in (b) for comparison.

ModeFrequency (meV)ActivityFrequencya^{a} (meV)
B1g_{1g}22.2R20.5
B1u_{1u}23.2Silent
Eu_u35.6×\times2IR
Eu_u48.9×\times2IR
A2g_{2g}49.5Silent
Eg_g60.7×\times2R65.2
A2u_{2u}63.3IR
B1u_{1u}67.9Silent
A1g_{1g}75.4R80.0
Eu_u77.0×\times2IR
B2g_{2g}84.2R88.7

Table IV. Calculated frequencies and optical activities [infra-red (IR) active, Raman (R) active or optically inactive (Silent)] of the phonons at the Brillouin zone center of bulk RuO2_2. Measured frequencies from Raman experiments [41] are also listed for comparison. a^{a} Frequencies from Raman experiments [41].

The calculated total PhDOS spectrum agrees quite well with that determined by neutron scattering experiments [42], especially for phonon energies below 50 meV. Together with the good agreement between the calculated and measured lattice constants, we conclude that our ab initio calculations using the GGA [24] with the PBEsol parameterization [25] can describe well the ground state structural properties and lattice vibrations in the RuO2_2 system.

The phonon dispersion and PhDOS in all the considered RuO2_2 films are plotted in Figure 5 and Figure S3 in the SM [39]. It is clear from Figure 5 and Figure S3 that overall, the phonon dispersion and PhDOS in all the RuO2_2 epitaxial films are similar to bulk RuO2_2. For example, both phonon dispersion and PhDOS spectra in all the considered systems span approximately from 0 to slightly above 80 meV, and have a gap of about 7 meV located at 55 meV. Importantly, as for bulk RuO2_2, the calculated phonon dispersions in all the considered RuO2_2 films exhibit no imaginary frequencies, in contrast to all the previous ab initio calculations [18, 19, 23]. This demonstrates that all the considered RuO2_2 (110) and

Phonon dispersions, phonon density of states, and Eliashberg spectral functions for bulk and thin-film RuO2

Figure 5. (a, d) Phonon dispersions (b, e) phonon density of states (PhDOS) and (c, f) Eliashberg spectral function α2F(ω)\alpha^2F(\omega) (solid lines) and frequency-dependent electron-phonon coupling strength λ(ω)\lambda(\omega) (dashed lines) for bulk RuO2_2, 20-nm RuO2_2 (110) and 28-nm RuO2_2 (100) thin films. The double arrowed lines denote the lowering Δphdn\Delta_{\mathrm{ph}}^{\mathrm{dn}} of the lowest phonon mode frequency near R due to the compressive strain ϵ[001]\epsilon_{[001]} in the RuO2_2 films.

Phonon dispersions, phonon density of states, and Eliashberg spectral functions for RuO2 films

Figure S3. (a, d) Phonon dispersions, (b, e) phonon density of states (PhDOS), (c, f) Eliashberg spectral function α2F(ω)\alpha^{2}F(\omega) and cumulative electron-phonon coupling strength λ(ω)\lambda(\omega) (dashed lines) for the RuO2_2 films.

RuO2_2 (100) films are dynamically stable. This allows us to evaluate the superconducting properties such as TcT_c of RuO2_2 films more reliably than before [18, 23].

However, significant changes caused by the lattice mismatch strains do exist. One pronounced change in the phonon dispersion due to the compressive strain in the RuO2_2 films is as follows. In all considered RuO2_2 films, the low-energy (below 40 meV) optical and out-of-plane acoustic branches along the Γ\Gamma-Z-R-A lines show significant softening (see Figure 5 and Figure S3). Moreover, as the compressive strain ϵ[001]\epsilon_{[001]} increases with the decreasing film thickness, this phonon softening becomes monotonically larger. In fact, as Figure 6 shows, this phonon softening is nearly proportional to the compressive strain ϵ[001]\epsilon_{[001]}. Interestingly, this is correlated with the upwards shift of the flat Ru dz2d_{z^2} bands near the R point in the BZ (Figure 3 and Figure S2 in the SM), which is also proportional to ϵ[001]\epsilon_{[001]}. Ru t2gt_{2g}-orbitals also hybridize significantly with O pp-orbitals, and the flat Ru dz2d_{z^2} bands arise from the antibonding bonding of the Ru dz2d_{z^2}-O pzp_z orbitals. Consequently, the energy levels of the flat Ru dz2d_{z^2} bands are sensitive to the compressive strain along the (001) direction.

Figure 6. The lowering Δphdn\Delta_{\mathrm{ph}}^{\mathrm{dn}} of the lowest phonon mode frequency (see Figure 4 and Figure S3) and the upwards shift Δelup\Delta_{\mathrm{el}}^{\mathrm{up}} of the flat Ru dz2d_{z^2} bands (see Figure 3 and Figure S2) at the R point in the Brillouin zone versus the compressive strain ϵ[001]\epsilon_{[001]} in the considered RuO2_2 films.

Importantly, these softening modes give rise to a noticeable peak at ∼15\sim15 meV in the PhDOS, which leads to a prominent peak in the Eliashberg functions α2F(ω)\alpha^2F(\omega) in the low frequency region in the RuO2_2 films [Figure 5c) and 5f) as well as Figure S3 and S3(f)]. Equation (3) indicates that this low frequency peak in the α2F(ω)\alpha^2F(\omega) will result in a significant increase in the EPC constant λ\lambda and hence enhances the superconductivity in the RuO2_2 films, as will be elaborated in the next section.

To further understand the origin of this intriguing phonon softening, we plot the atomic displacement patterns of the first phonon mode at the R point in bulk RuO2_2 as well as in strained 20-nm RuO2_2 (110) and 28-nm RuO2_2 (100) films in Figure 7. We find that, for bulk RuO2_2 and the 20-nm RuO2_2 (110) film, the atomic vibrations consist of two in-plane components: one along the [001] direction and the other primarily along the [110ˉ11\bar{0}] direction, with a slight deviation from the latter [see Figure 7(a) and 7(b)]. Similarly, for the 28-nm RuO2_2 (100) film, the mode vibrations also have two components, one along the [001] direction but the other along the [110] direction. Thus, in both strained RuO2_2 (110) and RuO2_2 (100) films, the Ru and O vibrations of the first phonon mode at the R point contain the [001] component, along which the lattice is compressed by the lattice mismatch strains in the films. This phonon softening can be attributed to the antibonding nature of the Ru dz2d_{z^2}–O pzp_z states. Under compressive strain, the overlap between the Ru dz2d_{z^2} and O pzp_z orbitals is enhanced, shifting the occupied antibonding states to higher energy (see Figure 3) and thereby weakening the Ru–O bonding interaction. Consequently, the corresponding bond stiffness is reduced, leading to the observed phonon softening (see Figure 5 and 6).

Atomic displacement patterns of the first phonon mode at the R point in bulk RuO2, 20-nm RuO2 (110) film and 28-nm RuO2 (100) film

Figure 7. Atomic displacement patterns of the first phonon mode at the R point in (a) bulk RuO2_2, (b) 20-nm RuO2_2 (110) film and (c) 28-nm RuO2_2 (100) film.

Electron-phonon coupling and superconductivity

Figures 5(c) and 5(f) as well as Figs. S3(c) and S3(f) present the calculated Eliashberg spectral function α2F(ω)\alpha^2F(\omega) (solid lines) and cumulative frequency-dependent EPC strength λ(ω)\lambda(\omega) (dashed lines). tbl:V lists the calculated EPC constant λ\lambda, logarithmic average phonon frequency ωlog⁡\omega_{\log}, and the superconducting transition temperature TcT_c for bulk RuO2_2 and all the considered RuO2_2 films. First of all, these figures indicate that in all the considered systems, the α2F(ω)\alpha^{2}F(\omega) spectrum follows closely the PhDOS spectrum. Second, overall, the α2F(ω)\alpha^{2}F(\omega) spectra of the RuO2_2 films are very similar to that of bulk RuO2_2. One notable difference is the occurrence of the prominent peak at around 15 meV in all the considered RuO2_2 films. As for the PhDOS spectra, this peak results from the softening of the lowest phonon band centered at R due to the compressive strain ϵ[001]\epsilon_{[001]} (see Figure 5 and Figure S3 in the SM [39]), and leads to the significantly increased EPC constant λ\lambda for the RuO2_2 films, as listed in Table V. In particular, the calculated EPC constant λ\lambda for bulk RuO2_2 is 0.50, while that for 20-nm RuO2_2 (110) film and 28-nm RuO2_2 (100) film are 0.78 and 0.63, respectively. This gives rise to the significantly enhanced theoretical TcT_c of 2.77 K in

20-nm RuO2_2 (110) film and 0.83 K in 28-nm RuO2_2 (100) film, compared with the theoretical TcT_c of 0.06 K in bulk RuO2_2. We notice that the calculated TcT_c of 2.77 K 20-nm RuO2_2 (110) is in good agreement with the experimental TcT_c of 1.97 K. For 28-nm RuO2_2 (100), the calculated TcT_c of 0.83 K also agree well with the measured TcT_c of 0.97 K [23]. No superconductivity has been observed in bulk RuO2_2 down to 0.3 K [7], while the calculated TcT_c is 0.06 K. Table V shows that the DOS at EFE_F in the strained RuO2_2 films hardly increases, indicating that the enhanced superconductivity in the strained RuO2_2 films originates mainly from the increased EPC constant λ\lambda caused by the softening of the phonon modes near the R point due to the compressive strain ϵ[001]\epsilon_{[001]}.

Systemϵ[001]\epsilon_{[001]} (%)λ\lambdaωlog⁡\omega_{\log} (K)N(EF)N(E_F) (states/eV/f. u)TcThe.T_c^{\mathrm{The.}} (K)TcExp.T_c^{\mathrm{Exp.}} (K)
Bulk RuO2_20.50459.31.000.06< 0.3a^{a}
30-nm (110)2.3500.67363.11.041.281.97b^{b}
20-nm (110)3.0970.78315.71.052.771.97b^{b}
8-nm (110)3.3160.82297.71.053.47< 1.5b^{b}
3-nm (110)4.5400.95253.91.055.33< 1.5b^{b}
28-nm (100)1.9140.63385.91.020.830.97c^{c}
17-nm (100)1.9140.71344.21.031.840.94c^{c}

Table 5. Calculated electron-phonon coupling constant λ\lambda, logarithmic average phonon frequency ωlog⁡\omega_{\log}, density of states at the Fermi level N(EF)N(E_F), and superconducting transition temperature TcT_c of bulk RuO2_2 as well as all considered RuO2_2 (110) and RuO2_2 (100) films. Theoretical TcT_c are calculated with screened Coulomb repulsion μ∗=0.25\mu^{*}=0.25. Experimental TcT_c values are also listed for comparison. a^{a} Experimental value from Lin et al. [7]; b^{b} Experimental values from this work. c^{c} Experimental data from Wadehra et al. [23].

Figure 8 displays the calculated superconducting transition temperatures TcT_c as a function of compressive strain ϵ[001]\epsilon_{[001]} for both RuO2_2 (110) and (100) films together with available experimental data. For the RuO2_2 (110) films, Figure 8(a) indicates that the calculated TcT_c increases almost linearly with the increasing ϵ[001]\epsilon_{[001]} strain, evolving from a low value of 1.28 K in 30-nm RuO2_2 (110) film to a much higher value of 5.33 K in ultrathin 3-nm RuO2_2 (110) film (see Table V). Note that the calculated TcT_c for bulk RuO2_2 is only 0.06 K, indicating that the compressive strain ϵ[001]\epsilon_{[001]} can cause tens folds of the enhancement of TcT_c in the RuO2_2 (110) films. Another notable trend is that as the thickness of the RuO2_2 (110) film is reduced, e.g., from 30-nm to 3-nm, the enhancement of the TcT_c becomes more pronounced. This is caused by the increased ϵ[001]\epsilon_{[001]} due to the reduced film thickness, and hence more strongly enhanced EPC constant.

Superconducting transition temperature versus compressive strain for RuO2 (110) and RuO2 (100) films

Figure 8. Superconducting transition temperature TcT_c versus compressive strain ϵ[001]\epsilon_{[001]} for (a) RuO2_2 (110) films and (b) RuO2_2 (100) films. The theoretical TcT_c values are calculated using Eq. (3) and μ∗=0.25\mu^* = 0.25. The experimental data from this work and from Wadehra et al. [23], are also plotted for comparison.

Similarly, for the RuO2_2 (100) films, Figure 8(b) suggests that the calculated TcT_c increases monotonically with the ϵ[001]\epsilon_{[001]}, although only two RuO2_2 (100) films have been studied. As mentioned in the preceding paragraphs, Figure 8 shows that for thicker RuO2_2 films (t≥20t \ge20 nm), the calculated TcT_c generally agree quite well with the observed TcT_c. However, even in ultrathin RuO2_2 films with thickness t<10t < 10 nm, the calculated TcT_c continuously increases with decreasing film thickness, consistent with the increasing compressive strain, phonon softening, and enhanced electron-phonon coupling. Nevertheless, the superconductivity is not observed experimentally in these ultrathin RuO2_2 films (see Figure 8, and [18, 19, 23]). The suppression of the superconductivity may be attributed to large disorder and strong interface scattering in these ultrathin RuO2_2 films, as will be further discussed in § 7. B below.

Discussion

Effect of Coulomb pseudopotential μ∗\mu^* on TcT_c

To evaluate the superconducting TcT_c using Eq. (3) with the EPC constant λ\lambda and logarithmically averaged phonon frequency ωlog\omega_{log} from the ab initio calculations, an appropriate choice of the semiempirical Coulomb pseudopotential μ∗\mu^* is required. Equation (3) indicates that in general, a nonzero μ∗\mu^* value suppresses phonon-mediated superconductivity and hence reduces TcT_c. One way to proceed is that a value of μ∗\mu^* is selected such that the calculated transition temperature of a well-known material aligns with the experimental TcT_c of the material. Therefore, we compute TcT_c for bulk RuO2_2, 20-nm RuO2_2 (110) and 28-nm (100) thin films using Eq. (3) for several different μ∗\mu^* values, and the results are summarized in Figure 9. Figure 9 shows that TcT_c decreases monotonically with increasing μ∗\mu^*, reflecting the progressive suppression of the phonon-mediated electron pairing interaction by the screened Coulomb repulsion. No superconductivity has been observed down to 0.3 K in bulk RuO2_2 [7], i.e., the upper bound of TcT_c of bulk RuO2_2 is 0.3 K. Since the calculated TcT_c of bulk RuO2_2 is 0.06 K when μ∗=0.25\mu^* = 0.25, and is zero when μ∗=0.30\mu^* = 0.30, we set μ∗=0.25\mu^* = 0.25 in this work. Furthermore, Table V shows that when μ∗=0.25\mu^* = 0.25, the calculated TcT_c for the 28-nm RuO2_2 (100) film is 0.83 K, in good agreement with the measured value of 0.97 K (Table III). Also, the calculated TcT_c for 20-nm RuO2_2 (110) film is 2.77 K, being close to the experimental value of 1.97 K (Table V). This supports that μ∗=0.25\mu^* = 0.25 provides a reasonable description of the superconducting properties of strained RuO2_2 thin films.

Calculated superconducting transition temperature as a function of the Coulomb pseudopotential

Figure 9. Calculated superconducting transition temperature TcT_c as a function of the Coulomb pseudopotential μ∗\mu^* for bulk RuO2_2, 28-nm RuO2_2 (100) film, and 20-nm RuO2_2 (110) film.

Interestingly, Figure 9 shows that 20-nm RuO2_2 (110) film exhibits the highest TcT_c over the entire range of μ∗\mu^*, while bulk RuO2_2 consistently shows the lowest values. The calculated TcT_c of 28-nm (100) film is between 20-nm RuO2_2 (110) film and bulk RuO2_2. This can be correlated with the fact that the compressive strain ϵ[001]\epsilon_{[001]} in 28-nm (100) film is smaller than in 20-nm (110) film, i.e., strain enhanced EPC strength is stronger in 20-nm (110) film than in 28-nm (100) film. All these results thus demonstrate that although the absolute value of TcT_c depends on the choice of μ∗\mu^*, our predicted strain enhancement of superconductivity in RuO2_2 (110) and (100) films remains robust.

On the thickness dependence of TcT_c in ultrathin RuO2_2 films

As presented above, the present ab initio calculations reproduce the overall experimental trend that superconductivity in RuO2_2 (110) and RuO2_2 (100) films is enhanced under epitaxial strain. Furthermore, the calculated TcT_c of 0.83 K for the 28-nm RuO2_2 (100) film is in good agreement with the measured value of 0.97 K [23] (Table V), and the calculated TcT_c for 20-nm RuO2_2 (110) film is 2.77 K, being close to the experimental value of 1.97 K (Table V). However, as mentioned before, the superconductivity is not observed in ultrathin RuO2_2 films (t≤10t \le10 nm) (Table V) (see [18, 19, 23]), in contrast to the monotonical increase of the calculated TcT_c with the decreasing thickness, which results from the larger compressive strain (Figure 8).

Previous experimental studies suggested that this behavior of the superconductivity in ultrathin RuO2_2 films originates from the competition between intrinsic strain-enhanced superconductivity and disorder-induced superconductivity suppression in the materials [23]. While thinner films experience larger epitaxial strains, greater enhanced EPC and hence higher TcT_c, larger disorder scattering and stronger interface-related effects become increasingly important and suppress the superconductivity [23]. The superconducting coherence lengths in RuO2_2 films are around 15 nm [18] and superconductivity here is three-dimensional. Consequently, the superconductivity in the RuO2_2 films with t≤10t \le10 nm tends to be significantly suppressed. Since the present strained-bulk approach deals with only the strained infinite crystals, the extrinsic effects such as disorders, out-of-plane quantum confinement and interface scattering are not included. As a result, the calculated TcT_c would increase monotonically, independent of the film thickness, resulting in the pronounced discrepancy with the experimental findings in the ultrathin films [18, 19, 23].

Conclusion

In summary, we have investigated the effect of epitaxial strain on the superconductivity in RuO2_2 (110) and (100) thin films both experimentally and theoretically. We have grown several RuO2_2 (110) thin films on TiO2_2 (110) substrates and observe superconductivity with TcT_c of ~2.0 K in 20-nm and 30-nm RuO2_2 (110) thin films. Theoretically, we study the superconductivity in both RuO2_2 (110) and RuO2_2 (100) epitaxial films based on ab initio calculations. First of all, we find that the calculated phonon dispersion relations of the RuO2_2 films have no imaginary frequencies, in contrast to all previous theoretical predictions [18, 19, 23]. Importantly, this allows us to properly describe lattice dynamics, electron-phonon coupling and superconductivity in the considered RuO2_2 films. Our ab initio calculations reveal that independent of the film orientation, the [001] compressive strain ϵ[001]\epsilon_{[001]} pushes the flat Ru dz2d_{z^2}-dominant bands towards EFE_F, and soften the out-of-plane acoustic phonon mode near the R point in the Brillouin zone, which significantly enhances the EPC strength λ\lambda and hence the calculated TcT_c in the RuO2_2 films. The amount of the phonon softening and the enhanced TcT_c increase almost linearly with the increasing ϵ[001]\epsilon_{[001]}. The calculated TcT_c for the films with thickness of ≥\geq20-nm agree well with the experimental TcT_c. For example, the theoretical TcT_c of 2.8 K for 20-nm RuO2_2 (110) film and 0.8 K for 28-nm RuO2_2 (100) film are close to the experimental TcT_c of 2.0 K and 1.0 K, respectively. These findings show that lattice mismatch strain provides an effective route for tuning phonon-mediated superconductivity in RuO2\mathrm{RuO}_2 and other thin films.

Acknowledgments

We thank Drs. S. C. Weng, S. Yang, C. K. Cheng, G. R. Chen, and C. H. Hsu for assistance with the X-ray measurements and analyses at NSRRC Hsinchu, Taiwan. We acknowledge the support from the National Science and Technology Council, National Center for Theoretical Sciences, and Academia Sinica, Taiwan.

Strain-enhanced superconductivity in RuO₂ thin films: Joint experimental and theoretical studies

Moeen ud din; Tsun-Sung Kuo; Yun-Chen Liao; Akhilesh Kr. Singh; Uddipta Kar; Wei-Li Lee; Guang-Yu Guo

This supplemental material contains supplemental notes A and B, figures S1, S2, and S3.

Electronic band structures of RuO₂ films.

Figure S1 presents the orbital-projected band structures as well as total and Ru dd and O pp orbital-decomposed density of states (DOS) for bulk RuO₂, 20-nm RuO₂ (110) and 28-nm RuO₂ (100) films. Figure S1 indicates that in bulk RuO₂, four Ru dd-orbital dominated bands cross the Fermi level (EFE_F). Notably, the doubly degenerate bands along Γ-Z crossing EFE_F (green curves) arise mainly from Ru dxzd_{xz}- and dyzd_{yz}-orbitals, while other bands crossing EFE_F (brown curves) are dominated by Ru dx2−y2d_{x^2-y^2}-orbitals. In 20-nm RuO₂ (110) and 28-nm RuO₂ (100) films, the orbital characters of the bands near EFE_F remain more or less the same [Figure S1 and Figure S1]. Figure S2 shows the band structures and total DOS for 30-nm, 8-nm, and 3-nm RuO₂ (110) films as well as 17-nm RuO₂ (100) film. Figure S2 indicates that the band structures of 30-nm, 8-nm, and 3-nm RuO₂ (110) films remain qualitatively similar to that of bulk RuO₂, with four Ru dd-derived bands crossing EFE_F, confirming that the metallic character is preserved over the full thickness range studied here. One pronounced change is as follows. As the compressive strain ϵ[001]\epsilon_{[001]} increases with the decreasing film thickness (see Table II and III in the main text), Ru dz2d_{z^2}-orbital dominated doubly degenerate bands below the Fermi level along the Z-R-A-Z direction (see red curves in Figure S1) shift monotonically towards EFE_F, reflecting the increasing effect of the contracting cc lattice constant. Nevertheless, for the considered RuO₂ (110) and (100) films, the Ru dz2d_{z^2}-orbital dominated bands remain below EFE_F (see Figure S1 and Figure S2) and hence, their upwards shift hardly leads to a significant increase in the DOS at EFE_F [N(EF)N(E_F)] (see Table V), as discussed in the main text.

Phonon dispersions and electron-phonon coupling in strained RuO2_2 films

Figure S3 presents the phonon dispersions, phonon DOS (PhDOS), Eliashberg spectral functions α2F(ω)\alpha^{2}F(\omega), cumulative electron-phonon coupling strength λ(ω)\lambda(\omega) for 30-nm, 8-nm, and 3-nm RuO2_2 (110) films and 17-nm RuO2_2 (100) film. The same results for 20-nm (110) and 28-nm (100) films have already been displayed in Figure 5 in the main text. Overall, the phonon dispersions of all the considered RuO2_2 films exhibit similar trends as bulk RuO2_2 (see Figure 5 and Figure S3), as discussed in the main text. Importantly, all the calculated phonon dispersions exhibit no imaginary frequencies, in contrast to all the previous ab initio calculations [1-3], i.e., all the considered RuO2_2 (110) and RuO2_2 (100) films are dynamically stable. This allows us to evaluate the superconducting properties such as TcT_c of RuO2_2 films more accurately than before. One prominent change in the phonon dispersion caused by the compressive strain in strained RuO2_2 films is the following. In all considered RuO2_2 films, the low-energy (below 40 meV) optical and out-of-plane acoustic branches along the Γ\Gamma-Z-R-A lines exhibit significant softening (see Figure 5 and Figure S3). Furthermore, as the compressive strain ϵ[001]\epsilon_{[001]} increases with the decreasing film thickness, this phonon softening become monotonically greater. Importantly, these softening modes give rise to a large spectral weight in the Eliashberg functions α2F(ω)\alpha^{2}F(\omega) in the low frequency region in the RuO2_2 films [Figs. 5(c) and 5(f) as well as Figs. S3(c) and S3(f)], thereby resulting in a significant increase in the electron-phonon coupling constant λ\lambda [See Eq. (3)]. In particular, Table V in the main text indicates that λ\lambda increases from 0.5 for bulk RuO2_2 to 0.78 for 20-nm RuO2_2 (110) film to 0.95 for 3-nm RuO2_2 (110) film. This leads to the monotonically enhanced TcT_c with the decreasing film thickness due to the increasing lattice mismatch strains.

References

  1. [11]H. Maiwa, N. Ichinose, and K. Okazaki, Preparation and properties of Ru and RuO₂ thin film electrodes for ferroelectric thin films, Jpn. J. Appl. Phys. 33, 5223 (1994).DOI
  2. [12]Q. X. Jia, X. D. Wu, S. R. Foltyn, A. T. Findikoglu, P. Tiwari, J. P. Zheng, and T. R. Jow, Heteroepitaxial growth of highly conductive metal oxide RuO₂ thin films by pulsed laser deposition, Appl. Phys. Lett. 67, 1677 (1995).DOI
  3. [13]X. Fang, M. Tachiki, and T. Kobayashi, Deposition and properties of PLD grown RuO₂ thin film, Thin Film Physics and Applications, In Third International Conference on Thin Film Physics and Applications 3175, 331-335 (1998).DOI
  4. [14]G. X. Miao, A. Gupta, G. Xiao, and A. Angelouch, Epitaxial growth of ruthenium dioxide films by chemical vapor deposition and its comparison with similarly grown chromium dioxide films, Thin Solid Films 478, 159 (2005).DOI
  5. [15]X. Wang, A. F. Pun, Y. Xin, and J. P. Zheng, Investigation of the growth dynamics of pulsed laser-deposited RuO₂ films using in situ resistance measurement and atomic force microscopy, Thin Solid Films 510, 82 (2006).DOI
  6. [16]J. H. Han, S. W. Lee, S. K. Kim, S. Han, C. S. Hwang, C. Dussarrat, and J. Gatineau, Growth of RuO₂ thin films by pulsed-chemical vapor deposition using RuO₄ precursor and 5% H₂ reduction gas, Chem. Mater. 22, 5700 (2010).DOI
  7. [17]D. Y. Kuo, H. Paik, J. N. Nelson, K. M. Shen, D. G. Schlom, and J. Suntivich, Chlorine evolution reaction electrocatalysis on RuO₂ (110) and IrO₂ (110) grown using molecular-beam epitaxy, J. Chem. Phys. 150, 041726 (2019).DOI
  8. [18]J. P. Ruf, H. Paik, N. J. Schreiber, H. P. Nair, L. Miao, J. K. Kawasaki, and K. M. Shen, Strain-stabilized superconductivity, Nat. Commun. 12, 59 (2021).
  9. [19]M. Uchida, T. Nomoto, M. Musashi, R. Arita, and M. Kawasaki, Superconductivity in uniquely strained RuO₂ films, Phys. Rev. Lett. 125, 147001 (2020).
  10. [20]Z. Fatima, D. Oka, and T. Fukumura, Systematic application of extremely large strain to rutile-type RuO₂ (100) epitaxial thin films on substrates with large lattice mismatches, Cryst. Growth Des. 21, 4083 (2021).DOI
  11. [21]W. Nunn, S. Nair, H. Yun, A. Kamath Manjeshwar, A. Rajapitamahuni, D. Lee, and B. Jalan, Solid-source metal–organic molecular beam epitaxy of epitaxial RuO₂, APL Mater. 9, 091113 (2021).DOI
  12. [22]C. A. Occhialini, L. G. Martins, S. Fan, V. Bisogni, T. Yasunami, M. Musashi, and J. Pelliciari, Strain-modulated anisotropic electronic structure in superconducting RuO₂ films, Phys. Rev. Mater. 6, 084802 (2022).arxiv.org/abs/2208.00718
  13. [23]N. Wadehra, B. Z. Gregory, S. Zhang, N. Schnitzer, Y. Iguchi, Y. E. Li, and D. G. Schlom, Strain-induced superconductivity in RuO2 (100) thin films, Commun. Mater. 6, 135 (2025).
  14. [24]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  15. [25]J. P. Perdew et al., Restoring the density-gradient expansion for exchange in solids and surfaces, Phys. Rev. Lett. 100, 136406 (2008).pubmed.ncbi.nlm.nih.gov/18517979
  16. [26]P. E. Blöchl, Projector augmented-wave method, Phys. Rev. B 50, 17953 (1994).pubmed.ncbi.nlm.nih.gov/9976227
  17. [27]G. Kresse and J. Hafner, Ab initio molecular dynamics for liquid metals, Phys. Rev. B 47, 558 (1993).
  18. [28]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  19. [29]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, and I. Dabo, et al., QUANTUM ESPRESSO: A modular and opensource software project for quantum simulations of materials, J. Phys.: Condens. Matter 21, 395502 (2009).DOI
  20. [30]P. Giannozzi, O. Andreussi, T. Brumme, O. Bunau, M. B. Nardelli, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, and M. Cococcioni, et al.Advanced capabilities for materials modelling with Quantum ESPRESSO, J. Phys.: Condens. Matter 29, 465901 (2017).
  21. [31]M. J. van Setten, M. Giantomassi, E. Bousquet, M. J. Verstraete, D. R. Hamann, X. Gonze, and G.-M. Rignanese, The PseudoDojo: Training and grading a 85 element optimized norm-conserving pseudopotential table, Comput. Phys. Commun. 226, 39–54 (2018).DOI
  22. [32]S. Baroni, S. de Gironcoli, A. Dal Corso, and P. Giannozzi, Phonons and related crystal properties from density-functional perturbation theory, Rev. Mod. Phys. 73, 515 (2001).DOI
  23. [33]W. L. McMillan, Transition temperature of strong-coupled superconductors, Phys. Rev. 167, 331 (1968).DOI
  24. [34]P. B. Allen and R. C. Dynes, Superconductivity at very strong coupling, J. Phys. C 8, L158 (1975).DOI
  25. [35]S. Ponce, E. R. Margine, C. Verdi and F. Giustino, EPW: Electron-phonon coupling, transport and superconducting properties using maximally localized Wannier functions, Comp. Phys. Commun. 209, 116 (2016).DOI
  26. [36]C. Pellegrini, R. Heid and A. Sanna, Eliashberg theory with ab-initio Coulomb interactions: A minimal numerical scheme applied to layered superconductors, J. Phys. Mater. 5, 024007 (2022).DOI
  27. [37]K. Ramesh and G.-Y. Guo, Electron-phonon coupling, superconductivity, and nontrivial band topology in NbN polytypes, Phys. Rev. B 99, 104508 (2019).
  28. [38]S. P. Keshri and G.-Y. Guo, Ab initio study of orbital-selective superconductivity in γ-BiPd, Phys. Rev. B 112, 214518 (2025).DOI
  29. [39]See Supplemental Material at https://link.aps.org/supplemental/ for supplemental notes A (electronic band structures of strained RuO₂ thin films), B(electron-phonon coupling and superconductivity in strained RuO₂ films), and Figs. S1-S3, which includes Refs. [18,19, 23].
  30. [40]G. Demazeau, S. F. Matar, and R. Pöttgen, Chemical bonding in metallic rutile-type oxides TO₂ (T = Ru, Rh, Pd, Pt), Z. Naturforsch. B 62, 949 (2007).
  31. [41]Y. M. Chen, A. Korotcov, H. P. Hsu, Y. S. Huang, and D. S. Tsai, Raman scattering characterization of well-aligned RuO₂ nanocrystals grown on sapphire substrates, New J. Phys. 9, 130 (2007).DOI
  32. [42]K. P. Bohnen, R. Heid, O. D. L. P. Seaman, B. Renker, P. Adelmann, and H. Schober, Lattice dynamics of RuO₂: Theory and experiment, Phys. Rev. B 75, 092301 (2007).DOI

Paper details

vlnc:W_9agmfw5f
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 12

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents