Strain-transfer at the Cu nanoparticle-Si(111) interface: static atomistic modelling and simulated Bragg CDI

Abstract

Substrate strain offers a route to control deformation in supported metallic nanoparticles, provided that interfacial coupling transmits the imposed loading into the particle. We assess this feasibility using five static Cu/Si(111) configurations spanning 0-2% biaxial tensile substrate strain. A 211,288-atom Cu particle is supported by a nominally 50 x 50 x 20 nm Si slab with its bottom 1 nm fixed, using the Jelinek modified embeddedatom potential. Relative to the relaxed supported 0% state, Cu-only local fits reveal heterogeneous, anisotropic deformation: particle-wide mean hydrostatic strain is negative at every nonzero loading, from -3.12 x 10-6 to -8.84 x 10-6, while the upper-particle mean varies nonmonotonically. Simulated Bragg CDI of Cu(111), obtained by inversion of known complex atomic scattering amplitudes, maps loading-dependent projected displacement and strain. The combined atomistic and Bragg CDI representations provide strong preliminary support for the feasibility of substrate-mediated strain transfer in this idealized system and identify spatial signatures for experimental investigation. Experiments remain indispensable to confirm transfer in real Cu/Si(111) nanoparticles and determine its magnitude.

Introduction

Straining a support offers a route to control deformation in an attached metallic nanoparticle. Interfacial coupling competes with free-surface relaxation, so a biaxially stretched substrate can generate different lateral and normal responses within the particle. Atomistic simulations of Co particles on expanded Cu substrates demonstrated spatially heterogeneous transfer, sensitive to temperature and interface structure [1]. For Cu on Si, studies of cluster deposition and film growth established the importance of epitaxy, intermixing, and preparation conditions [2, 3]. How prescribed substrate strain changes the deformation of an individual supported Cu particle remains the question addressed here.

The interface and surface termination are central to this response. Surface stress depends on the strain derivative of surface free energy [4], while Si(111) reconstruction [5] and its strain dependence [6] affect the atomic contact. We isolate substrate loading in a model with an initially ideal, oxide-free, unpassivated Si(111) surface, consistent particle preparation, and a fixed anchoring depth.

Bragg coherent diffraction imaging (BCDI) links nanocrystal deformation to a complex-object phase encoding the displacement projected along a reciprocal-lattice vector [7]. Its directional derivative gives the corresponding normal strain [8]. Atlan et al. combined electrochemical BCDI of Pt with atomistic and density-functional modelling to resolve heterogeneous strain and propagation from surface to interior [9]. Chatelier et al. combined multireflection BCDI with atomistic modelling to study strained Ni3_3Fe/Ni-rich core–shell formation [10]. These studies provide a precedent for calculating Bragg scattering from atomic positions and analysing the resulting displacement and strain fields in a diffraction representation.

The present study connects three stages of this proposed control route: prescribed biaxial deformation of Si(111), the resulting static response of a supported Cu particle, and its representation by simulated Bragg CDI. The supports span 0%, 0.5%, 1%, 1.5%, and 2% tensile strain. Hydrostatic distributions and directional tensor components characterize the Cu response relative to the relaxed supported 0% state, while simulated Bragg CDI of the same coordinates identifies projected-displacement signatures.

The objective is a preliminary assessment of strain-transfer feasibility under a defined atomistic preparation protocol. Experimental confirmation is indispensable for establishing transfer in real Cu/Si(111) systems. The calculations provide a microscopic basis for that investigation by linking substrate loading to heterogeneous particle deformation and to candidate signatures in Bragg CDI. The analysis distinguishes hydrostatic and projected strain and states the numerical and model limits of this interpretation.

Computational methodology

Geometry, initial state, and loading

The model contains 211,288 Cu atoms and 2,496,000 Si atoms (Figure 1). The Cu particle has initial coordinate spans of 19.914 × 19.914 × 11.278 nm and a construction lattice parameter of 3.615 Å. Its atom count, crystalline geometry, orientation, and initial internal displacements are preserved across substrate strains. The diamond-cubic Si slab uses a reference lattice parameter of 5.431 Å, with x∥[11ˉ0]x \parallel[1\bar{1}0], y∥[112ˉ]y \parallel[11\bar{2}], and z∥[111]z \parallel[111]. Its 64 (111) bilayers span 19.833 nm between outermost planes, corresponding to a 20.068 nm bulk-repeat thickness.

Figure 1. Initial Cu nanoparticle on Si(111) at 0% substrate strain. (a) Side view: Si is shown in a central 0.3 nm-thick slice and Cu in projection. The bottom 1 nm is fixed and the outermost Si-plane separation is 19.83 nm. (b) Top view in the 49.924 × 49.887 nm periodic lateral cell. Cu is orange, mobile Si light blue, and fixed Si dark blue. Dashed lines mark the simulation cell.

The reference lateral cell is 49.92386 × 49.88692 nm and its height is 38.80707 nm. Boundaries are periodic in xx, yy, and nonperiodic in zz. Si coordinates and lateral cell lengths are initially scaled by

FSiinit=diag⁡(1+ϵ,1+ϵ,1),ϵ∈{0,0.005,0.01,0.015,0.02}.(1)\mathbf{F}_{\mathrm{Si}}^{\mathrm{init}} = \operatorname{diag}(1+\epsilon,1+\epsilon,1), \qquad \epsilon\in\{0,0.005,0.01,0.015,0.02\}. \tag*{(1)}

Cu is rigidly recentered, without rescaling, above Si with a 2.5 Å initial gap. Cell dimensions remain fixed during relaxation. The bottom 1 nm of Si comprises 136,500 atoms in seven planes. Their coordinates remain fixed while their interactions with mobile atoms remain active. All other atoms are mobile. The supports are therefore prestrained before attachment, with normal Si relaxation allowed. Cell dimensions and construction details are listed in Supplementary Section S1 and Table S1.

Interatomic potential and static relaxation

LAMMPS [11] calculations use the modified embedded-atom method [12] with the Al–Si–Mg–Cu–Fe parameterization [13] distributed by NIST [14]. Conjugate-gradient relaxation holds the cell fixed, disables the energy-change criterion, and uses min_modify dmax 0.1 norm max. All five states request 10−610^{-6} eV/Å maximum per-atom force norm, with limits of 10,000 iterations and 100,000 force evaluations.

All calculations terminate with linesearch alpha is zero. Attained maximum mobile-atom force norms range from 1.07×10−41.07 \times10^{-4} to 2.29×10−42.29 \times10^{-4} eV/Å (Supplementary Table S2), above the requested tolerance. The dataset comprises approximately relaxed, constrained athermal configurations. The implications for strain-transfer feasibility are discussed in § 4.3.

Cu is initially identical across loadings, whereas each Si support is prestrained before the combined configuration is relaxed. This preparation compares separately relaxed contacts and does not trace a quasistatic loading path of an already attached particle. The study addresses the static response of this preparation protocol.

Reference-relative hydrostatic deformation

Full-precision minimized coordinates at 0% define the reference. Atom IDs establish material correspondence, with no affine cell remapping. For reference and current neighbor vectors Rij\mathbf{R}_{ij} and rij\mathbf{r}_{ij}, the local least-squares deformation gradient [15] and Green–Lagrange tensor are

Fi=argmin⁡F ∑j∈Ni0∥rij−FRij∥2,\mathbf{F}_i = \underset{\mathbf{F}}{\operatorname{argmin}}\ \sum_{j\in\mathcal{N}_i^0}\left\lVert\mathbf{r}_{ij}-\mathbf{F}\mathbf{R}_{ij}\right\rVert^2,
Ei=12(FiTFi−I).(2)\mathbf{E}_i = \frac{1}{2}\left(\mathbf{F}_i^{\mathsf{T}}\mathbf{F}_i-\mathbf{I}\right). \tag*{(2)}

The primary reference neighborhood contains Cu atoms within 5 Å. It therefore measures deformation within the metal rather than fitting a common affine transformation to metal and substrate atoms.

The hydrostatic and deviatoric parts are separated by

hi=13tr⁡(Ei),h_i = \frac{1}{3}\operatorname{tr}(\mathbf{E}_i),
Ei=hiI+Eidev,tr⁡(Eidev)=0.(3)\mathbf{E}_i = h_i\mathbf{I}+\mathbf{E}_i^{\mathrm{dev}},\qquad\operatorname{tr}\left(\mathbf{E}_i^{\mathrm{dev}}\right)=0. \tag*{(3)}

Here hih_i is the three-dimensional scalar named Volumetric Strain in OVITO [16]. Its sign characterizes the isotropic part of the fitted tensor, without specifying the signs of individual components. For the lateral average E∥,i=(Exx,i+Eyy,i)/2E_{\parallel,i}=(E_{xx,i}+E_{yy,i})/2, the exact identity

hi=13(2E∥,i+Ezz,i)(4)h_i = \frac{1}{3}\left(2E_{\parallel,i}+E_{zz,i}\right) \tag*{(4)}

links the hydrostatic response to lateral and normal deformation. The identity also holds for means taken over the same material cohort with the same weights.

The local affine volume ratio is Ji=det⁡FiJ_i=\det\mathbf{F}_i, and Ji−1≈3hiJ_i-1\approx3h_i only in the infinitesimal limit. Neither hih_i nor an average of JiJ_i is a tessellated measurement of total particle volume. These kinematic quantities do not determine mechanical stress [17] or separate elastic and plastic deformation. The reference is a relaxed supported particle, so negative hih_i denotes a change relative to that state, rather than a negative absolute stress relative to free Cu.

Statistics are evaluated for all Cu and for the 166,908 Cu atoms whose relaxed reference height is at least 2 nm above the lowest Cu atom. Fixed material cohorts preserve the same IDs across states. Reported quantities are the mean, median, positive fraction f+=NR−1∑i∈R1(hi>0)f_+ = N_R^{-1}\sum_{i\in R}\mathbf{1}(h_i>0), distributions, and 1 nm height profiles. A global affine fit to centered Cu coordinates provides a particle-wide comparison. Mixed Cu/Si-neighbor fits and non-affine residuals probe interfacial sensitivity. Their definitions and numerical checks appear in Supplementary Section S2.

Simulated Bragg CDI

Only Cu atoms contribute to the coherent sum, evaluated with pynx.scattering (PyNX 2023) [18, 19]. For angular reciprocal coordinates Q\mathbf{Q},

Aϵ(Q)=∑j=1NCuwj(Q)e−iQ⋅rj(ϵ),Iϵ(Q)=∣Aϵ(Q)∣2.(5)A_{\epsilon}(\mathbf{Q})=\sum_{j=1}^{N_{\mathrm{Cu}}}w_j(\mathbf{Q})e^{-i\mathbf{Q}\cdot\mathbf{r}_j(\epsilon)},\qquad I_{\epsilon}(\mathbf{Q})=\left|A_{\epsilon}(\mathbf{Q})\right|^2. \tag*{(5)}

Here wjw_j is an atomic scattering weight. PyNX coordinates in cycles per unit length satisfy Q=2πs\mathbf{Q}=2\pi\mathbf{s}. Phase conversion uses the angular convention. Each Cu point cloud is centered at its coordinate mean.

A 1283128^3 Bragg volume is sampled using the nominal Cu lattice parameter 3.615 Å. A centered forward Fourier transform of the conjugated complex amplitude recovers a real-space object. Reciprocal-space phase is therefore known in this simulation. The normalized-amplitude support threshold is 0.3, and the final crop retains 1283128^3 voxels. Amplitude and phase receive the same center-of-mass shift, followed by nonperiodic phase unwrapping, linear-ramp removal on a 0.64 support, support-mean phase subtraction, and Fourier-domain Blackman filtering. Fourier signs, supports, and filtering affect quantitative interpretation [20] and are therefore paramount to the analysis. Complete processing and reciprocal-centroid records are given in Supplementary Section S4.

For the processed object phase ϕB\phi_B and analysis vector QBragg\mathbf{Q}_{Bragg},

u111=ϕB∣QBragg∣,ϵ111=Q^Bragg⋅∇u111.(6)u_{111}=\frac{\phi_B}{\left|\mathbf{Q}_{Bragg}\right|},\qquad \epsilon_{111}=\widehat{\mathbf{Q}}_{Bragg}\cdot\nabla u_{111}. \tag*{(6)}

The conjugate-amplitude convention determines the displacement sign. In the small-deformation limit, the normal strain is Q^BraggTϵQ^Bragg\widehat{\mathbf{Q}}_{Bragg}^{T}\boldsymbol{\epsilon}\widehat{\mathbf{Q}}_{Bragg}, with ϵ\boldsymbol{\epsilon} the infinitesimal tensor. A single reflection resolves a projection, whereas hh is a tensor trace.

Differential displacement uses the 0% wavevector norm for every loading,

Δϵϵ,0=Q^d,ϵ⋅∇[ϕB(ϵ)−ϕB(0)∣QBragg,0∣].(7)\Delta\epsilon_{\epsilon,0}=\widehat{\mathbf{Q}}_{d,\epsilon}\cdot\nabla\left[\frac{\phi_B^{(\epsilon)}-\phi_B^{(0)}}{\left|\mathbf{Q}_{Bragg,0}\right|}\right]. \tag*{(7)}

The differentiation vectors, final-state voxel-size variables, and reused 2% plotting support are detailed in Supplementary Section S4.

Removing a ramp β⋅r\boldsymbol{\beta}\cdot\mathbf{r} changes projected strain by the constant −Q^Bragg⋅β/∣QBragg∣-\widehat{\mathbf{Q}}_{Bragg}\cdot\boldsymbol{\beta}/\left|\mathbf{Q}_{Bragg}\right|. Subtracting a constant phase only changes the displacement origin. Processed maps describe spatial variations with a fitted uniform offset removed.

Results

Imposed loading and relaxed substrate response

All five systems retain their atom counts and fixed cell dimensions. At prescribed strains of 0.5%, 1%, 1.5%, and 2%, sampled interior Si gives mean E∥=0.50%E_{\parallel}=0.50\%, 1.01%, 1.51%, and 2.02%, respectively. These values follow the Green–Lagrange conversion [(1+ϵ)2−1]/2[(1+\epsilon)^2-1]/2. Normal means are −0.235%, −0.473%, −0.714%, and −0.959%. The slab retains lateral extension while contracting normally. Sampling and minimization records appear in Supplementary Section S1.

Spatial redistribution of deformation in Cu

Both hydrostatic signs coexist in every loaded configuration (Figure 2). Cu-only particle-wide means are negative and become successively more negative across the sampled loadings: −3.12, −5.36, −6.04, and −8.84, in units of 10−610^{-6} dimensionless hh (Table 1). Medians remain negative, whereas positive fractions vary nonmonotonically between 37.89% and 44.51%. These increments characterize changes in the supported Cu particle relative to its relaxed 0% configuration.

Table 1: Cu-only hydrostatic statistics at 5 Å cutoff. hh is dimensionless. The upper cohort contains the same 166,908 reference atoms at height ≥2\ge2 nm.

Regionϵ\epsilon (%)106⟨h⟩10^{6}\langle h\rangle106med⁡(h)10^{6}\operatorname{med}(h)f+f_{+} (%)
All Cu0.5−3.123−1.48041.30
All Cu1−5.365−0.51744.51
All Cu1.5−6.040−2.11137.89
All Cu2−8.841−1.57341.19
Above 2 nm0.5−0.379−1.46839.28
Above 2 nm1−0.588−0.46843.87
Above 2 nm1.5−1.192−2.23133.82
Above 2 nm2−0.701−1.59138.87

Table 1.

Figure 2. Reference-relative Cu hydrostatic strain at 0.5%, 1%, 1.5%, and 2% substrate strain, from left to right. A central 1 nm-thick reference slice is shown in reference coordinates, relative to the relaxed 0% state. Cu-only neighbors within 5 Å define the tensor. The common scale saturates outside ±0.005%. The dashed line marks the 2 nm upper-cohort boundary. The complete 20 nm Si slab is omitted.

The upper-Cu mean is smaller and nonmonotonic, with its most negative sampled value at 1.5%: −1.192×10−6-1.192 \times10^{-6}. Height profiles contain regions of both signs and distinguish the four loadings (Figure 3). The different loading dependence of particle-wide and upper-Cu means shows that deformation is redistributed spatially. The response cannot be represented by a uniform particle-wide contraction.

Figure 3. Five-state static response. (a) Loaded-state mean and median hh. (b) Positive fractions for Cu-only and mixed-species neighborhoods. (c) Cu-only mean hh in 1 nm reference-height bins above 2 nm. (d) Upper-Cu directional means. Lines connect separately relaxed configurations and do not define a quasistatic loading path or a critical strain. Spatial atom counts are not independent replicas.

Global affine fits also give negative hydrostatic increments, but a different loading dependence: −3.26, −4.12, −0.851, and −4.02, in units of 10−610^{-6}. A global fit weights spatial displacements differently from an average of local tensors. Its behavior confirms that a single particle-wide scalar does not characterize the full heterogeneous field.

Anisotropic tensor balance and distributions

All four upper-Cu cohorts have negative mean ExxE_{xx} and positive mean EyyE_{yy} and EzzE_{zz} (Table 2). The hydrostatic mean is negative because contraction along xx outweighs expansion along yy and zz. At 1.5%, all three mean component magnitudes are largest among the sampled loadings: Exx=−14.55×10−6E_{xx} = -14.55 \times10^{-6}, Eyy=+8.71×10−6E_{yy} = +8.71 \times10^{-6}, and Ezz=+2.27×10−6E_{zz} = +2.27 \times10^{-6}. The smaller component magnitudes at 2% yield a less negative upper-Cu mean. The nonmonotonic hydrostatic response follows this balance of directional components.

Table 2: Upper-Cu mean components in units of 10−610^{-6} dimensionless strain. Identical cohort weights satisfy 3⟨h⟩=⟨Exx+Eyy+Ezz⟩3\langle h\rangle= \langle E_{xx} + E_{yy} + E_{zz}\rangle.

ϵ\epsilon (%)⟨Exx⟩\langle E_{xx}\rangle⟨Eyy⟩\langle E_{yy}\rangle⟨Ezz⟩\langle E_{zz}\rangle⟨h⟩\langle h\rangle
0.5−4.160+2.644+0.380−0.379
1−5.167+2.535+0.868−0.588
1.5−14.553+8.708+2.271−1.192
2−5.716+2.265+1.346−0.701

Table 2.

The hydrostatic distributions overlap substantially (Figure 4). Upper-Cu spatial standard deviations range from 0.0011% to 0.0014%, much larger than the corresponding mean offsets. The 5th–95th percentile intervals are [−0.0016, +0.0017]% at 0.5% and [−0.0018, +0.0019]% at 1.5%, the endpoint 2% interval is [−0.002, +0.002]%. Mean, median, positive fraction, and width therefore describe different aspects of the response. Percentiles characterize spatial heterogeneity, not uncertainty in a replicated mean.

Figure 4. Upper-Cu hydrostatic distributions for all four nonzero loadings. (a) Histogram bin counts divided by the full cohort. (b) Cumulative fractions. One horizontal unit is 10−310^{-3}%, or 10−510^{-5} dimensionless hh. The common display window is ±0.007\pm0.007%, out-of-window fractions are 0.19%, 0.29%, 0.26%, 0.57% at 0.5%, 1%, 1.5%, and 2%, respectively. Full-cohort statistics are used in Table 1.

Interfacial contribution and neighborhood dependence

The contact region contributes disproportionately to particle-wide statistics. Mixed Cu/Si-neighbor fits give positive particle-wide means, while Cu-only means remain negative (Supplementary Table S3). For the 4,051-atom reference contact cohort, mixed-neighbor mean hh increases from 0.0498% at 0.5% loading to 0.55% at 2%. The corresponding Cu-only means are −0.005% and −0.016%. Mixed fits combine deformation within Cu with relative Cu–Si motion, and their non-affine residuals increase with loading. Above 2 nm, both neighborhood definitions yield identical tensors because Si lies outside the fitting radius. This separates deformation within the upper metal from affine-fit sensitivity at the junction. Full neighborhood and residual statistics are given in Supplementary Section S2.

Signatures in simulated Bragg CDI

The five Cu(111) Bragg volumes share a compact maximum and anisotropic fringes. Full phase fields and particle outlines are similar. Projected-strain sections retain a strong positive base-region band even at 0% (Figure 5). Differential fields are therefore needed to isolate loading-dependent changes. Supplementary Figures S1–S3 document the complete five-state baseline comparison.

Simulated Bragg CDI of Cu(111) for the supported 0% reference

Figure 5. Simulated Bragg CDI of Cu(111) for the supported 0% reference: a reciprocal-space intensity section, complex-object phase section, and projected-strain section. Units are logarithmic arbitrary intensity, radians, and percent. This baseline is used to form differential fields. Full orthogonal sections for all five states appear in Supplementary Figures S1–S3.

Differential phases vary spatially rather than following a uniform sign sequence (Figure 6). At 0.5%, a negative central region is pronounced near the lower part of the xzxz section. The 1% field is more laterally asymmetric, with mixed interior signs. At 1.5% and 2%, extended negative central regions coexist with positive lateral contrast and alternating features near the base. Full orthogonal sections show the corresponding three-dimensional heterogeneity (Supplementary Figure S4).

Differential phase maps for four simulated Bragg CDI states

Figure 6. Differential phase from simulated Bragg CDI of Cu(111), in radians: (a) 0.5%–0%, (b) 1%–0%, (c) 1.5%–0%, and (d) 2%–0%. Zoomed xzxz sections retain the original coordinates and common color scale. Full xyxy, xzxz, and yzyz sections are in Supplementary Figure S4.

Differential projected strain contains both signs at every loading (Figure 7). Alternating base-region contrasts accompany weaker interior patches, whose locations and amplitudes change between states. Phase sign does not fix derivative sign, and neither field directly gives the hydrostatic scalar. The common differential display ranges are ±0.02 rad and ±0.041% for phase and projected strain. These common ranges allow visual comparison of the loading-dependent spatial contrast.

Differential projected strain maps for four simulated Bragg CDI states

Figure 7. Differential projected strain from simulated Bragg CDI, in percent, with the same state order and xzxz sections. A fitted uniform phase-ramp contribution has been removed. This directional field differs from the atomistic hydrostatic scalar. Full orthogonal sections are in Supplementary Figure S5.

The differential maps connect substrate loading to changes in the spatial distribution of projected Cu displacement and strain. Their relationship to the atomistic tensor, and the conditions for experimental confirmation, are discussed below.

Discussion

Feasibility of substrate-mediated strain transfer

The model links prescribed Si loading to a deformation response in Cu. The substrate retains lateral extension and contracts normally, while the Cu particle develops loading-dependent tensor components and spatially heterogeneous hydrostatic fields. Cu is initially identical across loadings and is not directly rescaled. Its response arises through interactions with differently strained supports and their relaxed contacts. Deformation extends into the upper particle, beyond the immediate junction.

The central outcome is an anisotropic response to substrate loading. Contraction along one lateral direction coexists with expansion along the other lateral and normal directions. Particle-wide hydrostatic means become more negative across the sampled loadings, whereas upper-Cu means are nonmonotonic. The 1.5% configuration has the most negative sampled upper-Cu mean, but does not define a critical strain or a uniform transition. These findings support a picture in which the interface and free surfaces redistribute the imposed deformation.

Combined with the loading-dependent simulated Bragg CDI fields, this model response provides strong preliminary support for the feasibility of substrate-mediated strain transfer in supported Cu nanoparticles. It gives a concrete microscopic basis for experimental investigation. Registry changes, slip, surface relaxation, and defects are possible contributors to the anisotropy. Structural analysis such as polyhedral template matching [21] would help distinguish them.

Connecting hydrostatic deformation to simulated Bragg CDI

Hydrostatic strain and a single-reflection strain describe complementary aspects of the same deformation. In the infinitesimal limit, write ε=hlinI+εdev\boldsymbol{\varepsilon}=h_{\mathrm{lin}}\mathbf{I}+\boldsymbol{\varepsilon}^{\mathrm{dev}}. The normal strain projected along the Bragg vector is

ε111=hlin+Q^BTεdevQ^B.(8)\varepsilon_{111}=h_{\mathrm{lin}}+\widehat{\mathbf{Q}}_{\mathrm{B}}^{\mathrm{T}}\boldsymbol{\varepsilon}^{\mathrm{dev}}\widehat{\mathbf{Q}}_{\mathrm{B}}. \tag*{(8)}

The deviatoric contribution can outweigh the hydrostatic term. Consequently, a negative hydrostatic mean can coexist with positive projected strain, and heterogeneous displacement can remain appreciable when the scalar mean is small. Using the finite-strain scalar in this relation is an approximation appropriate to weak interior deformations, with additional care required at rearranged contact sites.

Simulated Bragg CDI translates the atomistic response into projected-displacement and strain contrast. Differential maps isolate loading-dependent spatial changes from the supported 0% baseline and identify candidate regions for experimental comparison. Both analyses derive from the same coordinates and provide complementary representations within the model. A quantitative comparison requires matched physical grids, spatial resolution, supports, and phase references. Linear-ramp removal changes a uniform projected-strain offset. The processed maps therefore emphasize spatial variations. Supplementary Section S4 records these conventions.

Experimental confirmation and scope

Experiments are indispensable to confirm strain transfer in real Cu/Si(111) nanoparticles and determine its magnitude. A direct test would impose and independently measure the substrate strain while tracking the response of the same supported particle by Bragg CDI, referenced to an unloaded state. Multiflection measurements could resolve directional responses, building on combined atomistic and BCDI approaches [9, 10]. Experimental confirmation would establish whether the predicted response persists with the actual surface termination, contact structure, and achievable measurement sensitivity.

The present assessment remains preliminary. All minimizations stop by line-search termination above their common force target, so stability of the weak hydrostatic means and the nonmonotonic upper-Cu response can be challenged. The ideal oxide-free interface, anchoring depth, finite periodic cell, empirical potential, and separately prepared contacts define the model scope. The known-amplitude inversion does not establish recovery from experimental intensity alone, and the present images do not determine a transfer efficiency or experimental detection threshold. These limits constrain quantitative extrapolation. Within this scope, the model defines an experimentally testable link between substrate strain and particle deformation.

Conclusions

Five static Cu/Si(111) configurations spanning 0–2% biaxial substrate strain show loading-dependent, anisotropic deformation in a supported Cu particle. Cu-only hydrostatic means are negative at all nonzero loadings, with coexisting positive and negative regions and a nonmonotonic upper-particle response. Simulated Bragg CDI of Cu(111) maps the associated redistribution of projected displacement and strain, connecting the atomistic response to candidate experimental signatures.

Together, these preliminary results provide strong support for the feasibility of substrate-mediated strain transfer in the idealized Cu/Si(111) system and motivate its experimental investigation. Experiments are indispensable to confirm transfer in real nanoparticles and establish its magnitude and reproducibility. Numerical convergence, realistic interface conditions, and quantitative treatment of projected fields will determine how far the present predictions extend to such measurements.

Supplementary materials

Supplementary fig:S1–S5 show complete orthogonal fields. Supplementary Sections S1–S4 document geometry, static records, the potential, and processing conventions.

Acknowledgments

The author acknowledges the CEA for providing access to high-performance computing (HPC) resources. The author thanks Dr. C. Atlan, Dr. E. Polack and Dr. E. Bellec for the fruitful discussions.

References

  1. [1]J. Zhou, S. Saranu, and U. Herr, “Determination of lattice distortion in nanoparticles on strained substrates using molecular dynamics,” Journal of Physics: Conference Series 144, 012010 (2009). doi:10.1088/1742-6596/144/1/012010.DOI
  2. [2]H. F. Gong, G. P. Li, S. X. Zhang, W. Lu, and L. M. Wang, “Atomistic Study of the Copper Cluster Deposition on Si(001) and Si(111) Surface,” Materials Science Forum 850, 287–298 (2016). doi:10.4028/www.scientific.net/MSF.850.287.DOI
  3. [3]G. Zhu, M. Han, B. Xiao, and Z. Gan, “On the Microcrystal Structure of Sputtered Cu Films Deposited on Si(100) Surfaces: Experiment and Integrated Multiscale Simulation,” Molecules 28, 4786 (2023). doi:10.3390/molecules28124786.DOI
  4. [4]R. Shuttleworth, “The Surface Tension of Solids,” Proceedings of the Physical Society. Section A 63, 444–457 (1950). doi:10.1088/0370-1298/63/5/302.DOI
  5. [5]K. Takayanagi, Y. Tanishiro, M. Takahashi, and S. Takahashi, “Structural analysis of Si(111)-7 × 7 by UHV-transmission electron diffraction and microscopy,” Journal of Vacuum Science & Technology A 3, 1502–1506 (1985). doi:10.1116/1.573160.DOI
  6. [6]R. Zhachuk, S. Teys, and J. Coutinho, “Strain-induced structure transformations on Si(111) and Ge(111) surfaces: A combined density-functional and scanning tunneling microscopy study,” The Journal of Chemical Physics 138, 224702 (2013). doi:10.1063/1.4808356.DOI
  7. [7]M. A. Pfeifer, G. J. Williams, I. A. Vartanyants, R. Harder, and I. K. Robinson, “Three-dimensional mapping of a deformation field inside a nanocrystal,” Nature 442, 63–66 (2006). doi:10.1038/nature04867.DOI
  8. [8]O. Gorobtsov and A. Singer, “Shear displacement gradient in X-ray Bragg coherent diffractive imaging,” Journal of Synchrotron Radiation 29, 866–870 (2022). doi:10.1107/S1600577522002363.DOI
  9. [9]C. Atlan, C. Chatelier, I. Martens, M. Dupraz, A. Viola, N. Li, L. Gao, S. J. Leake, T. U. Schülli, J. Eymery, F. Maillard, and M.-I. Richard, “Imaging the strain evolution of a platinum nanoparticle under electrochemical control,” Nature Materials 22, 754–761 (2023). doi:10.1038/s41563-023-01528-x.DOI
  10. [10]C. Chatelier, C. Atlan, M. Dupraz, S. Leake, N. Li, T. U. Schülli, M. Levi, E. Rabkin, L. Favre, S. Labat, J. Eymery, and M.-I. Richard, “Unveiling Core–Shell Structure Formation in a Ni3Fe Nanoparticle with In Situ Multi-Bragg Coherent Diffraction Imaging,” ACS Nano 18(21), 13517–13527 (2024). doi:10.1021/acsnano.3c11534.DOI
  11. [11]A. P. Thompson, H. M. Aktulga, R. Berger, D. S. Bolintineanu, W. M. Brown, P. S. Crozier, P. J. in ’t Veld, A. Kohlmeyer, S. G. Moore, T. D. Nguyen, R. Shan, M. J. Stevens, J. Tranchida, C. Trott, and S. J. Plimpton, “LAMMPS—a flexible simulation tool for particle-based materials modeling at the atomic, meso, and continuum scales,” Computer Physics Communications 271, 108171 (2022). doi:10.1016/j.cpc.2021.108171.DOI
  12. [12]M. I. Baskes, “Modified embedded-atom potentials for cubic materials and impurities,” Physical Review B 46, 2727–2742 (1992). doi:10.1103/PhysRevB.46.2727.DOI
  13. [13]B. Jelinek, S. Groh, M. F. Horstemeyer, J. Houze, S. G. Kim, G. J. Wagner, A. Moitra, and M. I. Baskes, “Modified embedded atom method potential for Al, Si, Mg, Cu, and Fe alloys,” Physical Review B 85, 245102 (2012). doi:10.1103/PhysRevB.85.245102.DOI
  14. [14]National Institute of Standards and Technology, Interatomic Potentials Repository, entry for Jelinek et al. (2012), Al–Si–Mg–Cu–Fe, LAMMPS implementation. Repository record and parameter files (accessed 12 October 2026).
  15. [15]F. Shimizu, S. Ogata, and J. Li, “Theory of Shear Banding in Metallic Glasses and Molecular Dynamics Calculations,” Materials Transactions 48, 2923–2927 (2007). doi:10.2320/matertrans.MJ200769.DOI
  16. [16]OVITO documentation, Atomic strain: local deformation, hydrostatic indicator, and reference-cell mapping (accessed 12 October 2026).
  17. [17]LAMMPS documentation, compute stress/atom: kinetic and virial contributions and normalization (accessed 12 October 2026).
  18. [18]V. Favre-Nicolin, G. Girard, S. Leake, J. Carnis, Y. Chushkin, J. Kieffer, P. Paleo, and M.-I. Richard, “PyNX: high-performance computing toolkit for coherent X-ray imaging based on operators,” Journal of Applied Crystallography 53, 1404–1413 (2020). doi:10.1107/S1600576720010985.
  19. [19]PyNX documentation, pynx.scattering: atomic structure-factor and reciprocal-coordinate conventions (accessed 13 October 2026).
  20. [20]J. Carnis, L. Gao, S. Labat, Y. Y. Kim, J. P. Hofmann, S. J. Leake, T. U. Schülli, E. J. M. Hensen, O. Thomas, and M.-I. Richard, “Towards a quantitative determination of strain in Bragg Coherent X-ray Diffraction Imaging: artefacts and sign convention in reconstructions,” Scientific Reports 9, 17357 (2019). doi:10.1038/s41598-019-53774-2.DOI
  21. [21]P. M. Larsen, S. Schmidt, and J. Schiøtz, “Robust structural identification via polyhedral template matching,” Modelling and Simulation in Materials Science and Engineering 24, 055007 (2016). doi:10.1088/0965-0393/24/5/055007.DOI

Paper details

vlnc:W_9s4g9t6s
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents