betaFeedback

WorksPhysics and Astronomy

Interplay between local moment and itinerant magnetism in the layered metallic antiferromagnet TaFe1.14_{1.14}Te3_3

Abstract

Two-dimensional (2D) antiferromagnets have garnered considerable interest for the next generation of functional spintronics. However, many available bulk materials from which 2D antiferromagnets are isolated are limited by their sensitivity to air, low ordering temperatures, and insulating transport properties. TaFe1+y_{1+y}Te3_3 offers unique opportunities to address these challenges with increased air stability, metallic transport properties, and robust antiferromagnetic order. Here, we synthesize TaFe1+y_{1+y}Te3_3 (yy = 0.14), identify its structural, magnetic, and electronic properties, and elucidate the relationships between them. Axial-dependent high-field magnetization measurements on TaFe1.14_{1.14}Te3_3 reveal saturation magnetic fields ranging between 27-30 T with a saturation magnetic moment of 2.05-2.12 μBμ_B. Magnetotransport measurements confirm TaFe1.14_{1.14}Te3_3 is metallic with strong coupling between magnetic order and electronic transport. Angle-resolved photoemission spectroscopy measurements across the magnetic transition uncover a complex interplay between itinerant electrons and local magnetic moments that drives the magnetic transition. We further demonstrate the ability to isolate few-layer sheets of TaFe1.14_{1.14}Te3_3 through mechanical exfoliation, establishing TaFe1.14_{1.14}Te3_3 as a potential platform for 2D spintronics based on metallic layered antiferromagnets.

Introduction

Identifying candidate low-dimensional materials combining metallic transport behavior with robust antiferromagnetic order is crucial to advancing spin-based nanotechnologies. Van der Waals (vdW) magnets, in particular, provide an ideal platform for fabricating atomically-thin spintronics and magneto-optic devices[1, 2, 3, 4, 5], as they possess diverse magnetic phases and electronic properties that persist down to the two-dimensional (2D) limit. Within this family of materials, those exhibiting metallic electronic transport have received intense attention due to their potential functionality as spin injectors[6, 7], magnetic tunnel junction electrodes[8], or spin-orbit torque devices[9, 10]. Among the available 2D magnets, layered antiferromagnets are exceptionally attractive due to the increased resilience to external magnetic fields[11, 12], sensitivity of electrical resistance to field-induced antiferromagnetic-to-ferromagnetic transitions[13, 14], faster spin dynamics[15], utility in high-frequency spin-orbit torque experiments[16], and capability for higher packing density than ferromagnets in memory storage devices due to the absence of stray fields[17]. Despite an obvious need, vdW materials integrating metallic behavior with layered antiferromagnetic order are notably scarce[18]. TaFe1+y_{1+y}Te3_3[19, 20, 21, 22] is one candidate to overcome many existing limitations of vdW magnets, boasting a high Néel temperature ranging between 160 and 200 K[19, 21, 23, 24, 25], metallic charge transport properties[19, 23, 24, 26, 27], and stability under ambient conditions, showcasing its promise for metallic antiferromagnet-based spintronics. However, a comprehensive understanding of the magnetic and electronic properties of TaFe1+y_{1+y}Te3_3 has yet to be achieved.

In this work, we synthesize TaFe1+y_{1+y}Te3_3 (y=0.14y = 0.14) and explore its electronic and magnetic properties, uncovering its potential for atomic-scale spintronic devices based on vdW materials. Temperature- and magnetic-field-dependent magnetization measurements reveal a paramagnetic (paramagnetic)-to-antiferromagnetic transition

Results and Discussion

Single crystals of TaFe1.14_{1.14}Te3_3 are grown using the chemical vapor transport method (see methods for full details). Tantalum, iron, tellurium, and TeCl4_4 powders are pressed into a pellet, and sealed in a fused silica tube under vacuum. After seven days in a temperature gradient of 700°C to 600°C, needle-like crystals are obtained in the sink side of the tube. We performed single crystal X-ray diffraction (SCXRD) to determine the structure (Figure 1A-C). The low-dimensional layered telluride TaFe1.14_{1.14}Te3_3 crystallizes in the P21/mP2_1/m space group. The structure features Ta-Fe1-Fe-Ta ribbons aligned along the bb-axis while sandwiched between Te layers. Along the ribbon, the Ta atoms are octahedrally coordinated by six Te atoms, and the Fe1 atoms, which make a one-dimensional zig-zag chain, are tetrahedrally coordinated by four Te atoms. Unlike the Fe1 site, the Fe2 site is partially occupied, and the Fe2 atom nestles in the center of the square pyramid formed by Te atoms (Figure 1A). Single crystals are stable under ambient conditions and the layered nature of the structure and corresponding interlayer vdW bonds allows for the isolation of air-stable few-layer flakes of TaFe1.14_{1.14}Te3_3 through mechanical exfoliation down to the monolayer limit (Figure 1D). Corresponding tapping-mode atomic force microscopy images of an exfoliated sample can be found in Figure S1. Previously reported neutron diffraction measurements on TaFe1+y_{1+y}Te3_3 determined that the magnetic moments are localized on the Fe atoms and that the magnetic structure is A-type antiferromagnetic with Fe1 spins within each layer coupling ferromagnetically while Fe1 spins between the layers couple antiferromagnetically[23]. The Fe2 spins within each layer align parallel with Fe1 spins (Figure 1B). The atomic ratio of different constituent elements was determined through SCXRD occupancy refinement (Tab. S1) and confirmed by energy dispersive X-ray spectroscopy (EDX) on freshly cleaved samples (Tab. S2). Corresponding scanning electron microscopy (SEM)/EDX elemental maps of a TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} single crystal for Ta, Fe, and Te with each collection normalized to Te demonstrate that there is no evidence of Fe clustering down to the micron scale (Figure 1E-G).

Structure and composition of TaFe1.14Te3

Figure 1. Structure and composition of TaFe1.14_{1.14}Te3_3. A) Crystal structure of TaFe1.14_{1.14}Te3_3 viewed along the crystallographic bb-axis. Morphological long in-plane (LIP) (green), short in-plane (SIP) (red), and out-of-plane (OOP) (blue) directions are shown relative to the crystallographic aa, bb, and cc-axes. B) Crystal structure of TaFe1.14_{1.14}Te3_3 viewed along the crystallographic bb-axis with the orientation of the Fe1 (orange arrows) and Fe2 (purple arrows) magnetic moments in the antiferromagnetic state overlayed. C) Crystal structure of TaFe1.14_{1.14}Te3_3 viewed along a direction that clearly displays the Fe1/Fe2 chain structure. The Te atoms are removed for clarity. D) False-colored optical microscope image of a TaFe1.14_{1.14}Te3_3 flake exfoliated onto polydimethylsiloxane (PDMS). The corresponding layer numbers for different regions were determined by atomic force microscopy and optical contrast (Figure S1). E-G) Ta (E), Fe (F), and Te (G) elemental maps of a single crystal of TaFe1.14_{1.14}Te3_3 as determined by SEM/EDX. The lower right inset of each elemental map gives the corresponding elemental composition normalized to Te. In (E) and (F), the error bars represent the standard deviation of multiple measurements between various crystals and growth batches.

Mechanical exfoliation of TaFe$_{1.14}$Te$_3$ flakes

Figure S1. Mechanical exfoliation of TaFe1.14_{1.14}Te3_3 flakes. A, E) Grey-scale optical images of two sample TaFe1.14_{1.14}Te3_3 flakes exfoliated onto PDMS using the previously-described tape method. White and black colors correspond to the PDMS substrate and thick TaFe1.14_{1.14}Te3_3 flakes, respectively. In (A), the extracted optical contrast for 1, 3, and 4L regions is denoted. B-D) tapping-mode atomic force microscope topography (B), amplitude error (C), and phase (D) for the region in (A) defined by the dashed black box. The inset of (B) shows a height-profile line cut of the step edge. F-H) tapping-mode atomic force microscope topography (F), amplitude error (G), and phase (H) for the region in (E) defined by the dashed black box.

Since the Fe2\mathrm{Fe}_{2} site is only partially occupied, we first characterize the uniformity of the Fe2\mathrm{Fe}_{2} distribution and the impact of Fe2\mathrm{Fe}_{2} on the local electronic properties. We performed scanning tunneling microscopy (STM) and spectroscopy (STS) on cleaved bulk TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3}. In Figure 2A, we present an atomically-resolved STM image of the vdW plane at 7.5 K. The selected distances determined by a fast Fourier transform (FFT) of the real-space STM topography are Te ⋯\cdots Te (nearest neighbor) = 0.35, 0.36 nm, Fe2⋯\mathrm{Fe}_{2} \cdots Te = 0.52 nm, and Te ⋯\cdots Te (next nearest neighbor) = 1.01 nm (Figure 2B), in good agreement with those obtained from SCXRD (Figure 1A). With its atomic precision, STM allows us to view the topographical corrugation of the Fe chains in detail. We observe an inhomogeneity of the intensity in the image, which may indicate random nanometer-scale clustering of Fe2\mathrm{Fe}_{2} in the crystal, as previously hypothesized in a Mössbauer spectroscopy study of TaFe1+yTe3\mathrm{TaFe}_{1+y}\mathrm{Te}_{3}[20]. Corresponding STS measurements show a metallic-like density of states (DOS) at all points across multiple Fe chains, revealing that the occupancy of the Fe2\mathrm{Fe}_{2} site does not significantly impact the local electronic structure (Figure S2).

Atomic-scale characterization of TaFe1.14Te3

Figure 2. Atomic-scale characterization of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3}. A) STM image of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} cleaved along the vdW gap. The image was obtained at T=7.5T = 7.5 K in constant current mode (Vb=400V_b = 400 mV, I=50I = 50 pA). B) Corresponding FFT of the STM image. Select periodicities are denoted by dashed white circles. C) TEM micrograph of an exfoliated TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} flake with a thickness <50< 50 nm viewed along the OOP direction. D) Corresponding electron diffraction image of the same flake in (C). Select dd-spacings are denoted by solid black bars. In all panels, the orientation of the images with respect to the morphological SIP and LIP directions is given in the lower left inset.

Scanning tunneling microscopy and spectroscopy of TaFe$_{1.14}$Te$_3$

Figure S2. Scanning tunneling microscopy and spectroscopy of TaFe1.14_{1.14}Te3_3. A) Scanning tunneling microscopy image of bulk TaFe1.14_{1.14}Te3_3 along the out-of-plane direction at T=7.5T = 7.5 K. The image was obtained in constant current mode (Vb=400V_b = 400 mV, I=50I = 50 pA). B) Local density of states (LDOS) versus energy at 7.5 K and zero magnetic field. The trace is a line-average scan across multiple TaFe1.14_{1.14}Te3_3 chains. The direction and length of the line-scan average are denoted by a black dashed line in (A). C) Zoom-in of the line-averaged LDOS versus energy trace at 7.5 K and zero magnetic field.

To confirm that the quasi-one-dimensional nature of the structure persists in exfoliated flakes, we performed transmission electron microscopy (TEM) and corresponding selected-area electron diffraction (SAED) measurements on an exfoliated flake of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} with a thickness <50< 50 nm (Figure 2C, D; see methods for details). The diffraction pattern shows that the crystallinity is intact in the exfoliated flake of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3}. This is also seen in the real-space image, in which we observe distinct lines of atoms along the direction of the chains as depicted in Figure 1C. Select atomic distances from the SAED image are 0.17 nm for the close-range Fe atoms and 0.94 nm for the interchain Fe atoms (Figure 2D), in good agreement with those obtained from SCXRD (Tab. S1 and Figure 1A, B) and STM (Figure 2A, B).

We measured the magnetic susceptibility (χ\chi) of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} as a function of magnetic field (HH) and temperature (TT). In Figure 3A, we present χ\chi vs. TT curves with HH along the SIP, LIP, and OOP morphological directions (see Figure 1A for reference to crystallographic axes). When cooling the sample from room temperature, the measurements show a paramagnetic-to-antiferromagnetic phase transition, characterized by a peak in χ\chi at the Néel temperature TN=164±2T_{\mathrm{N}} = 164 \pm2 K (Figure S3, Figure S4 for additional data). The Néel temperature is also confirmed through HH-dependent heat capacity measurements (Figure S5). Below the Néel temperature, the zero-field-cooled (ZFC) and field-cooled (FC) branches separate, signaling the emergence of a spin-glassy phase below ≈100\approx100 K (Figure S6-Figure S9 for a more detailed analysis)[25]. This behavior, often associated with competing antiferromagnetic and ferromagnetic interactions, has been observed in other TaFe1+yTe3\mathrm{TaFe}_{1+y}\mathrm{Te}_{3} stoichiometries[25] and certain FexMn1−xTiO3\mathrm{Fe}_{x}\mathrm{Mn}_{1-x}\mathrm{TiO}_{3} systems where long-range antiferromagnetic and re-entrant spin-glass phases can coexist[28, 29, 30, 31]. The extracted Weiss temperatures (ϑW\vartheta_{\mathrm{W}}) in the paramagnetic phase convey strong ferromagnetic coupling, with values of 154 K, 158 K, and 149 K for the OOP, LIP, and SIP directions, respectively (inset of Figure 3A). The Curie-Weiss fit estimates an effective magnetic moment (μeff\mu_{\mathrm{eff}}) ranging between 4.26-4.28 μB\mu_{\mathrm{B}} for all morphological directions, in line with the expected local moment of 4 μB\mu_{\mathrm{B}} for a majority high-spin tetrahedral Fe2+\mathrm{Fe}^{2+} ion (Figure S23)[32].

High-field magnetic properties of TaFe1.14Te3

Figure 3. High-field magnetic properties of TaFe1.14_{1.14}Te3_3. A) χ\chi versus TT for HH oriented along the SIP (solid green lines), LIP (solid blue lines), and OOP (solid red lines) directions. Both zero-field-cooled (ZFC) and field-cooled (FC) traces are shown. All traces were collected with a field of H=0.1H = 0.1 T. The extracted Néel temperature is shown by a black dashed line. Layered antiferromagnetic and paramagnetic phases are denoted by grey and white regions, respectively. The inset shows inverse χ\chi versus TT for HH oriented along the SIP (solid green line), LIP (solid blue line), and OOP (solid red line) directions. Dashed black lines are linear fits to each trace. The extracted θw\theta_\mathrm{w} and μeff\mu_\mathrm{eff} are given in the upper left and lower right insets, respectively. B-D) MM versus HH at different TTs for HH oriented along the OOP (B), LIP (C), and SIP (D) directions. In each plot, the extracted saturation magnetization (MsatM_\mathrm{sat}) and HsatH_\mathrm{sat} are given in the inset. Note that because both the OOP and SIP directions contain a component parallel to the Fe1/Fe2 spin directions, they both exhibit metamagnetic transitions. The LIP direction, however, is completely perpendicular to the Fe1/Fe2 spin directions and only displays a gradual spin-canting process.

Field-dependent magnetic susceptibility on TaFe1.14Te3

Figure S3. Field-dependent magnetic susceptibility on TaFe1.14_{1.14}Te3_3. A-C) Field-cooled magnetic susceptibility versus temperature for magnetic fields oriented along the out-of-plane (A), long in-plane (B), and short-in-plane (C) directions. The magnetic field at which each trace was taken is given in the insets. TNT_{\mathrm{N}} is denoted by a dashed black line in each plot.

Temperature-dependent magnetization data for TaFe1.14Te3

Figure S4. Temperature-dependent magnetization data TaFe1.14_{1.14}Te3_3. A-C) Color maps of magnetization versus magnetic field (x-axis) and temperature (y-axis) for magnetic fields oriented along the out-of-plane (A), long in-plane (B), and short-in-plane (C) directions. The color bar scale is given above each plot. TNT_{\mathrm{N}} is denoted by a dashed black line in each plot.

Specific heat capacity of TaFe$_{1.14}$Te$_3$

Figure S5. Specific heat capacity of TaFe1.14_{1.14}Te3_3. A) Specific heat capacity versus temperature at zero magnetic field. B) Plot of specific heat capacity divided by the temperature versus temperature squared. The dashed black line is a linear fit to the data. The fit equation and extracted fit parameters are given in the inset. C) Specific heat capacity versus temperature across the PM-AFM transition at zero magnetic field (solid black dots) and 9 T9\ \mathrm{T} (solid red dots). The Néel temperature at 0 T0\ \mathrm{T} and 9 T9\ \mathrm{T} is denoted by a black and red dashed line, respectively.

Observation of the spin-glass phase in TaFe$_{1.14}$Te$_3$

Figure S6. Observation of the spin-glass phase in TaFe1.14_{1.14}Te3_3. A-C) Magnetic susceptibility versus temperature for magnetic fields oriented along the out-of-plane (A), long in-plane (B), and short-in-plane (C) directions. Both field-cooled and zero-field-cooled traces are shown. All traces were acquired with a magnetic field of 25 mT25\ \mathrm{mT}. TNT_\mathrm{N} is denoted by a dashed black line in each plot.

Powder X-ray diffraction patterns of TaFe1.14Te3 crystals

Figure S9. Powder X-ray diffraction of bulk TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 crystals before and after grinding. Powder X-ray diffraction (PXRD) intensity versus 2θ2\theta for the empty puck (solid black line), a single crystal of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 (solid red line), a TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 single crystal ground with LN2\mathrm{LN}_2 (solid blue line), and a TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 single crystal ground with LN2\mathrm{LN}_2 after being pressurized up to 1.3 GPa (solid green line). Simulated TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 PXRD peaks are denoted with black tick marks.

X-ray photoelectron spectroscopy on bulk TaFe$_{1.14}$Te$_3$

Figure S23. X-ray photoelectron spectroscopy on bulk TaFe1.14_{1.14}Te3_3. A) Intensity versus binding energy survey of a bulk sample taken at 298 K with a beam diameter of 100 µm and a source power of 25 W. Ta, Fe, and Te spectral regions are noted with blue, orange, and yellow, respectively. B-D) Intensity versus binding energy focused on expected Ta (B), Fe (C), and Te (D) peak regions.

Fig. 3B-D plots the magnetization (MM) vs. applied HH along all morphological directions (see Figure 1A) up to 35 T at various TT. The OOP- and SIP-oriented MM vs. HH curves at 1.5 K reveal a series of steps in MM between 9-15 T after which MM continues to increase until saturating at 29 T and 30 T, respectively (Figure 3B, D, and Fig. S10).

The exact nature of these steps is unclear without further measurements of the high-field magnetic structure, but are likely due to metamagnetic transitions (see Figure S11 and S12 for additional data). The LIP-oriented MM vs. HH curve at 1.5 K is linear up to 27 T after which it saturates, indicating a gradual spin canting process (Figure 3C). This confirms the LIP direction as the hard axis (Figure 3C and Figure S10). At 1.5 K, the sample reaches a saturation magnetic moment for all axial orientations ranging between 2.05-2.12 μB\mu_\mathrm{B}, which is significantly smaller than the μeff\mu_\mathrm{eff} determined for the high-TT paramagnetic phase. As expected, increasing TT decreases the saturation magnetic moment and the HH value at which the moment saturates.

High-field magnetometry of TaFe1.14Te3 at 1.5 K

Figure S10. Analysis of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 high-field magnetometry at 1.5 K. A-C) Magnetization (solid blue lines) and derivative of magnetization (solid yellow lines) versus magnetic field at 1.5 K for magnetic fields oriented along the out-of-plane (A), long in-plane (B), and short in-plane (C) directions. In each plot, the extracted saturation magnetization and saturation magnetic field are given in the inset.

High-field magnetometry on two TaFe1.14Te3 single crystals

Figure S11. High-field magnetometry on two TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} single crystals. A-C) Magnetization versus magnetic field at 1.5 K for magnetic fields oriented along the out-of-plane (A), long in-plane (B), and short in-plane (C) directions for two separate TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} crystals. Each plot’s blue and red traces correspond to the different TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_{3} crystals. In each plot, the extracted saturation magnetization is given in the inset.

Our measured saturation moments of ≈\approx2 μB\mu_\mathrm{B} are consistent with those assigned previously based on neutron diffraction measurements of the antiferromagnetic phase[23]. The discrepancy between μeff\mu_\mathrm{eff} and the measured saturation magnetic moment implies that both local moment and itinerant magnetism coexist in TaFe1.14_{1.14}Te3_3. For further insight, we performed first-principles DFT calculations on TaFe1+y_{1+y}Te3_3 with y=0y = 0, 0.25, and 1 with various magnetic orderings (see methods for details). We find that the antiferromagnetic order shown in Figure 1B, with intraplane ferromagnetic order and interplane antiferromagnetic order, is always electronically stable and typically lower in energy than other magnetic orderings (including non-magnetic), although the energy differences are often times small. Löwdin charge analysis of Fe atoms gives a positive charge of 0.30.3-0.50.5 and a magnetic moment of 2.22.2-2.4 μB2.4\ \mu_\mathrm{B}, for both Fe1 and Fe2 (Table S3), in good agreement with our measured saturation moment. Because DFT with common functionals is not appropriate for strongly correlated electrons, the agreement with experiment supports the picture that electron itinerancy is responsible for the suppression of the magnetic moment. Although the character of the bands near the Fermi energy (EFE_\mathrm{F}) is found to be

TaFeTe3\mathrm{TaFeTe}_3
Non-magneticAntiferromagnetic
ElementChargeElementChargeMag. Moment
Ta0.3Ta0.3±0.2\pm0.2
Fe10.4Fe10.52.2
Fe2—Fe2——
Te-0.1Te0.00.0
TaFe1.25Te3\mathrm{TaFe}_{1.25}\mathrm{Te}_3
Non-magneticAntiferromagnetic
ElementChargeElementChargeMag. Moment
Ta0.2Ta0.3±0.2\pm0.2
Fe10.4Fe10.52.2
Fe20.4Fe20.52.3
Te0.0Te0.00.0
TaFe2Te3\mathrm{TaFe}_2\mathrm{Te}_3
Non-magneticAntiferromagnetic
ElementChargeElementChargeMag. Moment
Ta0.2Ta0.1±0.1\pm0.1
Fe10.1Fe10.42.3
Fe20.1Fe20.32.4
Te0.0Te-0.10.0

Table S3. Calculated Löwdin charge and magnetic moments for TaFe1+yTe3\mathrm{TaFe}_{1+y}\mathrm{Te}_3. Calculated charge and magnetic moment per atom (Ta, Fe1, Fe2, and Te) for TaFeTe3\mathrm{TaFeTe}_3, TaFe1.25Te3\mathrm{TaFe}_{1.25}\mathrm{Te}_3, and TaFe2Te3\mathrm{TaFe}_2\mathrm{Te}_3. Note that due to the arbitrary nature of atomic orbitals used for projection, the Löwdin charges do not necessarily sum to zero.

a complex and nearly equal mixture of Fe 3d3d, Ta 5d5d and Te 5p5p orbitals (Figure S20,Figure S21), all DFT calculations predict a metallic electronic structure, whose properties we study further by magnetotransport measurements.

Calculated band structures for TaFeTe3 and TaFe2Te3

Figure S20. Calculated band structures for TaFeTe3\mathrm{TaFeTe}_{3} and TaFe2Te3\mathrm{TaFe}_{2}\mathrm{Te}_{3}. A, B) Element-resolved band structure calculations for TaFeTe3\mathrm{TaFeTe}_{3} in the antiferromagnetic (A) and non-magnetic (B) configurations. Red squares, blue circles, and green triangles correspond to Fe 3d orbitals, Ta 5d orbitals, and Te 5p orbitals. C, D). Element-resolved band structure calculations for TaFe2Te3\mathrm{TaFe}_{2}\mathrm{Te}_{3} in the antiferromagnetic (C) and non-magnetic (D) state. Red squares, blue circles, and green triangles correspond to Fe 3d orbitals, Ta 5d orbitals, and Te 5p orbitals.

Element-resolved calculated partial density of states for TaFe$_{1+y}$Te$_3$

Figure S21. Element-resolved calculated partial density of states (PDOS) for TaFe1+yTe3\mathrm{TaFe}_{1+y}\mathrm{Te}_3. A, B) Element-resolved partial density of states (PDOS) calculated for TaFeTe3\mathrm{TaFeTe}_3 in the non-magnetic (A) and antiferromagnetic (B) configuration. C, D) Element-resolved partial density of states (PDOS) calculated for TaFe2Te3\mathrm{TaFe}_2\mathrm{Te}_3 in the non-magnetic (C) and antiferromagnetic (D) configuration.

In Figure 4, we report the magnetotransport of TaFe1.14_{1.14}Te3_3 single crystals. Transport devices were fabricated using a micro-soldering technique which consists of drawing micron-scale contacts with Field’s metal using a micromanipulator (see methods for details)[33, 34]. Figure 4A plots the zero-field resistivity (ρ\rho) of TaFe1.14_{1.14}Te3_3 versus TT. Overall metallic behavior is observed with ρ\rho decreasing with decreasing TT. At T=175±3T = 175 \pm3 K, there is a sharp jump in the derivative of ρ\rho versus TT, which is attributed to the onset of antiferromagnetic order. Below this temperature ρ\rho varies approximately as T2T^2, saturating to a constant value at low TT.

Electronic transport properties of TaFe1.14Te3

Figure 4. Electronic transport properties of TaFe1.14_{1.14}Te3_3. A) ρ\rho (left) and dρ/dT\mathrm{d}\rho/\mathrm{d}T (right) versus TT at zero HH. The extracted residual resistivity ratio (RRR=R(300K)/R(2K)RRR = R(300\mathrm{K})/R(2\mathrm{K})) is given in the inset. The extracted TNT_\mathrm{N} is shown by a black dashed line. B) MM versus HH at 1.5 K1.5\ \mathrm{K} for HH parallel to the OOP direction. C) RHallR_\mathrm{Hall} versus HH above (solid yellow line) and below (solid magenta line) TNT_\mathrm{N}. Two distinct linear regions (denoted by dashed black lines) are observed below TNT_\mathrm{N}, whereas a single linear region is observed above TNT_\mathrm{N}. Additional traces at different temperatures can be found in Figure S18. An optical image of the device is given in the inset. D) Magnetoresistance ratio, MRR=[(R(H)−R(H=0))/R(H=0)]×100MRR = [(R(H)-R(H=0))/R(H=0)]\times100, versus HH at various TT for fields parallel to the OOP direction. Both forward and backward traces are shown. The TT at which each trace was taken is given in the inset. The dashed black line denotes the 1.5 K1.5\ \mathrm{K} metamagnetic transition.

Figure 4D presents the HH dependence of the magnetoresistance ratio (MRRMRR). MRRMRR is defined as MRR=[(R(H)−R(H=0))/R(H=0)]×100MRR = [(R(H)-R(H=0))/R(H=0)]\times100, where HH is oriented along the OOP direction. Above TNT_{\mathrm{N}}, the system is in the paramagnetic phase characterized by a broad negative MRRMRR (nMRRnMRR) due to the field-induced suppression of spin-flip scattering between conduction electrons and local magnetic moments. Well below TNT_{\mathrm{N}} at 1.5 K, we observe a negligible MRRMRR up to a critical field of HC=8.5±0.2H_{\mathrm{C}} = 8.5 \pm0.2 T above which, the absolute value of MRRMRR sharply increases and continues to increase linearly for H>HCH>H_{\mathrm{C}}. The response of MRRMRR closely follows the measured MM vs HH traces (Figure 4B and Figure S13-Figure S17), indicating that HCH_{\mathrm{C}} is correlated with the jump in MM vs HH. As TT increases, HCH_{\mathrm{C}} decreases towards zero at TNT_{\mathrm{N}}, consistent with the magnetization measurements. These results demonstrate that TaFe1.14_{1.14}Te3_3 exhibits a relatively strong coupling between electrical properties and magnetic order. The fact that MRRMRR decreases as MM increases suggests the primary mechanism could be a field-induced suppression of interlayer spin-flip scattering. However, elucidating the exact mechanism behind this coupling will require further measurements of the field-induced magnetic structure.

Analysis of the metamagnetic transition far below $T_{\mathrm{N}}$ in TaFe$_{1.14}$Te$_3$

Figure S13. Analysis of the metamagnetic transition far below TNT_{\mathrm{N}} in TaFe1.14_{1.14}Te3_3. A) Magnetization (solid black line) and the derivative of magnetization (solid red line) versus magnetic field at 1.5 K for fields parallel to the out-of-plane direction. B) Magnetoresistance ratio, MRR=[R(H)−R(H=0)]/R(H=0)×100MRR = [R(H)-R(H=0)]/R(H=0)\times100, versus magnetic field at 1.5 K for fields parallel to the out-of-plane direction. The inset is an optical image of the device along with the measurement configuration. C) Hall resistance versus magnetic field at 1.5 K. Two distinct linear regions (denoted by dashed black lines) are observed below TNT_{\mathrm{N}}. The inset is an optical image of the device along with the measurement configuration. In A-C, the vertical gray bars demarcate the magnetic field at which a spin-flop metamagnetic transition occurs (HCH_{\mathrm{C}}). This spin-flop transition (A) results in a sharp decrease in MRRMRR (B) and a sharp increase in the anomalous Hall contribution to RHallR_{\mathrm{Hall}} (C).

Temperature dependence of the 12 T MRR and Hall resistance in TaFe$_{1.14}$Te$_3$

Figure S17. Temperature dependence of the 12 T MRR and Hall resistance in TaFe1.14_{1.14}Te3_3. Left axis: MRR at 12 T versus temperature extracted from longitudinal resistance measurements (solid blue diamonds) and the symmetric component of the Hall resistance measurements (solid blue circles). Right axis: Hall resistance at 12 T versus temperature. The Hall resistance was anti-symmetrized to remove components of the raw data that were symmetric in the magnetic field. The Néel temperature is denoted by a solid gray line. The magnetic field was oriented parallel to the out-of-plane axis for all measurements.

The coupling between electrical and magnetic properties can also be seen in the Hall measurements presented in Figure 4C. In magnetic materials, the Hall resistance (RHallR_{\mathrm{Hall}}) is typically determined by two components arising from the external and internal magnetic fields[35]. In general, RHallR_{\mathrm{Hall}} is proportional to the applied HH (the slope of which is related to the carrier density) plus the sample magnetization. These two contributions can be seen clearly seen in Hall measurements across the magnetic transition (Figure 4C; see also Figure S13-Figure S18). Above TNT_{\mathrm{N}} (at 300 K), since the sample has negligible magnetization (Figure S15), the RHallR_{\mathrm{Hall}} versus HH is linear, from which we extract a corresponding carrier density of 1.30±0.03×1021 cm−31.30 \pm0.03 \times10^{21}\ \mathrm{cm}^{-3}, consistent with previous measurements on similar TaFe1+y_{1+y}Te3_3 stoichiometries[24, 26]. Below TNT_{\mathrm{N}} (130 K), RHallR_{\mathrm{Hall}} versus HH is linear at low HH with the same slope as the 300 K trace, corresponding to the normal Hall contribution from external HH. Once HH reaches HCH_{\mathrm{C}}, RHallR_{\mathrm{Hall}} sharply increases and then continues to increase linearly with HH for H>HCH>H_{\mathrm{C}}. The slope of RHallR_{\mathrm{Hall}} versus HH when H>HCH>H_{\mathrm{C}} is larger than the slope for H<HCH<H_{\mathrm{C}} due to the additional Hall component from the linear sample magnetization (Figure S14). The slope of RHallR_{\mathrm{Hall}} versus HH for both H>HCH>H_{\mathrm{C}} and H<HCH<H_{\mathrm{C}} has a non-monotonic temperature dependence which may arise from temperature-dependent magnetic fluctuations (Figure S18)[24]. It’s worth emphasizing that other factors could contribute to RHallR_{\mathrm{Hall}}, such as temperature- and field-dependent changes in the band structure. However, our results bear similarities to other TaFe1+y_{1+y}Te3_3 stoichiometries[24, 26] and ARPES measurements on TaFe1.14_{1.14}Te3_3 (as will be seen below) show only minor changes in the band structure across the magnetic transition, indicating RHallR_{\mathrm{Hall}} is primarily determined by the sample carrier density and the sample magnetization (see Figure S13-Figure S18 for additional data). This clear effect of the sample magnetization on the measured RHallR_{\mathrm{Hall}} further demonstrates the strong coupling between magnetism and electronic properties in TaFe1.14_{1.14}Te3_3.

Analysis of the metamagnetic transition near $T_{\mathrm{N}}$ in TaFe$_{1.14}$Te$_3$

Figure S14. Analysis of the metamagnetic transition near TNT_{\mathrm{N}} in TaFe1.14_{1.14}Te3_3. A) Magnetization (solid black line) and the derivative of magnetization (solid red line) versus magnetic field at 130 K for fields parallel to the out-of-plane direction. B) Magnetoresistance ratio, MRR=[R(H)−R(H=0)]/R(H=0)×100MRR = [R(H)-R(H=0)]/R(H=0)\times100, versus magnetic field at 130 K for fields parallel to the out-of-plane direction. The inset is an optical image of the device along with the measurement configuration. C) Hall resistance versus magnetic field at 130 K. Two distinct linear regions (denoted by dashed black lines) are observed below TNT_{\mathrm{N}}. The inset is an optical image of the device along with the measurement configuration. In A-C, the vertical gray bars demarcate the magnetic field at which a spin-flop metamagnetic transition occurs (HCH_{\mathrm{C}}). This spin-flop transition (A) results in a sharp decrease in MRRMRR (B) and a sharp increase in the anomalous Hall contribution to RHallR_{\mathrm{Hall}} (C).

Analysis of magnetometry and transport above $T_{\mathrm{N}}$ in TaFe$_{1.14}$Te$_3$

Figure S15. Analysis of magnetometry and transport above TNT_{\mathrm{N}} in TaFe1.14_{1.14}Te3_3. A) Magnetization (solid black line) versus magnetic field at 300 K for fields parallel to the out-of-plane direction. B) Magnetoresistance ratio, MRR=[R(H)−R(H=0)]/R(H=0)×100MRR = [R(H)-R(H=0)]/R(H=0) \times100, versus magnetic field at 300 K for fields parallel to the out-of-plane direction. The inset is an optical image of the device along with the measurement configuration. C) Hall resistance versus magnetic field at 300 K. A single linear region (denoted by a dashed black line) is observed over the entire field range. The inset is an optical image of the device along with the measurement configuration.

Temperature dependence of anti-symmetrized Hall data in TaFe$_{1.14}$Te$_3$

Figure S18. Temperature dependence of anti-symmetrized Hall data in TaFe1.14_{1.14}Te3_3. Anti-symmetrized Hall resistance versus magnetic field at various temperatures for fields parallel to the out-of-plane direction. Both forward and backward traces are shown. The temperature at which each trace was taken is given in the inset. The dashed black lines denote the zero crossings. The inset is an optical image of the device along with the measurement configuration.

To experimentally probe the electronic structure of TaFe1.14_{1.14}Te3_3, we performed ARPES on a freshly cleaved surface (vdW plane) under ultra-high vacuum (UHV) across the magnetic transition (Figure 5). The Fermi surface at 20 and 210 K are shown in Figure 5A, B, respectively. Two sets of periodic wave-like Fermi surfaces (FSs) are identified, indicated by α\alpha and α′\alpha' in Figure 5A. The modulated FSs perpendicular to Fe1-Te1 chain directions (i.e., ΓˉYˉ\bar{\Gamma}\bar{Y}) point to significant inter-chain interactions. The FS features look similar between the paramagnetic and antiferromagnetic phases, except for the thermal broadening, consistent with the previous report[27]. The broadened spectroscopic features are likely a result of the disorder associated with the Fe2 site.

Evolution of the Fermi surface and electronic states of TaFe1.14Te3 across the magnetic transition

Figure 5. Evolution of the Fermi surface and electronic states of TaFe1.14_{1.14}Te3_3 across the magnetic transition. ARPES Fermi surface maps at 20 K (A) and 210 K (B). Dark blue (white) colors correspond to high (low) photoelectron intensity. The Fermi surfaces are symmetrized at ky=0k_y = 0 Å−1^{-1}. In both (A) and (B), the black dashed rectangle represents the surface Brillouin zone. The ΓˉXˉ\bar{\Gamma}\bar{X} and ΓˉYˉ\bar{\Gamma}\bar{Y} directions are along (LIP) and perpendicular (SIP) to the Fe-Te chains, respectively. C) ARPES intensity map along the Yˉ−Γˉ−Yˉ\bar{Y} - \bar{\Gamma} - \bar{Y} direction is shown as cut #1 (purple dashed line in (A)). Calculated non-magnetic band structure is overlayed as semi-transparent white lines. D) Energy distribution curves (EDCs) at Γˉ\bar{\Gamma} and Yˉ\bar{Y} symmetry points (vertical dashed white lines in (C)) at 20 K (solid blue lines) and 210 K (solid black lines). E) ARPES intensity map along the Xˉ−Γˉ−Xˉ\bar{X} - \bar{\Gamma} - \bar{X} direction is shown as cut #2 (orange dashed line in (A)). Calculated non-magnetic band structure is overlayed as semi-transparent white lines. F) EDCs at ky=0.07k_y = 0.07 Å−1^{-1} (α\alpha) and ky=0.65k_y = 0.65 Å−1^{-1} (β\beta) (vertical dashed white lines in (E)) at 20 K (solid blue lines) and 210 K (solid black lines). G) ARPES intensity map along cut #3 (magenta dashed lined in (A)). H) EDCs at kx=0.30k_x = 0.30 Å−1^{-1} (vertical dashed white line in (G)) at 20 K and 210 K. All data were acquired with a photon energy of 21.22 eV. For (C), (E), and (G), purple (yellow) colors correspond to low (high) photoelectron intensity. All calculated band structures were scaled down by 1.4 and shifted down by 0.2 eV.

The ARPES intensity maps along the Yˉ−Γˉ−Yˉ\bar{Y}-\bar{\Gamma}-\bar{Y} and Xˉ−Γˉ−Xˉ\bar{X}-\bar{\Gamma}-\bar{X} paths in the low-TT antiferromagnetic phase are shown in Figure 5C, E (cut #1 and #2 in Figure 5A). ARPES intensity maps are compared to our DFT band structures of non-magnetic TaFeTe3_3, where the EFE_{\mathrm{F}} was empirically shifted to best match the ARPES data (additional orbital-resolved band structures and partial density of states can be found in Figure S20,Figure S21). Along the Xˉ−Γˉ−Xˉ\bar{X}-\bar{\Gamma}-\bar{X} path, we observe two hole-like bands, α\alpha and α′\alpha', crossing EFE_{\mathrm{F}}. Another less dispersive band (β\beta) is also observed near EFE_{\mathrm{F}}. Overall, experimental ARPES intensity maps show reasonable agreement with our DFT calculations, when the bandwidth of the latter is reduced by a factor of 1.4 (Figure 5C, E). The necessity of this rescaling signals relatively strong electron correlations that are not captured by standard DFT. Figure 5D displays the energy distribution curves (EDCs) at Γˉ\bar{\Gamma} and Yˉ\bar{Y} points across the magnetic transition. We observe a distinct change in spectral intensity and a transfer of spectral weight from high-to-low binding energy, along with a slight shift in the energy of the bands. A more detailed TT dependence reveals that the most significant changes occur below ≈\approx100 K (Figure S22). The evolution of EDCs across the magnetic transition for the α\alpha and β\beta bands is shown in Figure 5F. Below the magnetic transition, the β\beta band shows an enhancement in quasiparticle (QP) spectral weight near EFE_{\mathrm{F}}. However, no such change was observed for the α\alpha band. ARPES intensity maps along cut #3 (shown as a dashed line in Figure 5A) and EDCs are shown in Figure 5G, H, respectively. A strong enhancement of the integrated spectral weight of ≈\approx16% is observed within 0 to −1.25-1.25 eV in the antiferromagnetic phase, relative to the paramagnetic phase. These combined results reflect that the magnetic transition is driven by the electronic structure

Temperature dependence of ARPES spectra

Figure S22. Temperature dependence of ARPES spectra. A) ARPES spectrum along Yˉ−Γˉ−Yˉ\bar{Y} - \bar{\Gamma} - \bar{Y} path at 20 K. The purple and yellow colors represent the lowest and highest photoelectron intensities, respectively. B) EDCs at various temperatures at kx=0k_x = 0 Å−1^{-1}, showing a two-peak structure corresponding to two bands. The peak near the Fermi level shows enhancement of spectral intensity at low temperatures, but negligible above ≈125 K. C) Change of the energy position at kx=0k_x = 0 Å−1^{-1} (Γˉ\bar{\Gamma}) with temperature. The top band slightly shifted downward with increasing temperature and no measurable band shift is observed for the bottom band, except for the increase of broadening. D) Change of the energy position at kx=0.31k_x = 0.31 Å−1^{-1} (Yˉ\bar{Y}) with temperature. The band appears to shift slightly downward with increasing temperature across the magnetic transition. For (C) and (D), the purple and yellow colors represent the lowest and highest photoelectron intensities, respectively.

reconstruction rather than Fermi surface nesting. Our results suggest that the electronic states undergo a band-dependent reconstruction across the magnetic transition due to the interplay between orbital and spin degrees of freedom. This behavior is known to occur in other systems containing local moments and itinerant electrons[36, 37, 38, 39], such as heavy fermion compounds[40], Fe-based superconductors[41, 42], and other strongly-correlated transition-metal oxides[43, 44]. The coexistence of itinerant and local-moment magnetism in TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3, combined with the fact that TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 can be exfoliated down to atomically thin flakes, provides new opportunities to study such correlated magnetic systems in the 2D limit.

Conclusions

Through a combination of magnetic, electronic, and transport measurements, supported by first-principles DFT calculations, we resolve the interplay between the magnetic and electronic properties in the layered vdW magnet TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3. We performed high-field magnetometry revealing the full direction-dependent magnetic properties. Calculations and magnetotransport measurements confirm the metallic nature of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 and display strong coupling between electronic transport properties and magnetic order. Temperature-dependent ARPES measurements show minor band shifts and strong spectral weight renormalization across the magnetic transition. This, combined with a low observed saturation moment of 2.05-2.12 μB\mu_{\mathrm{B}} found in both the high-field magnetometry measurements and DFT calculations, indicate a complex interplay between local moment and itinerant magnetism in TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3. Finally, we demonstrate the isolation of air-stable few-layer flakes of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 down to the monolayer limit. Altogether, our results establish TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 as an exciting material for 2D spintronics, manifesting both robust A-type antiferromagnetism, metallic transport properties, and stability under ambient conditions. Furthermore, the intersection of local-moment and itinerant magnetism typically occurs in correlated electronic systems, offering TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 as a promising platform for studying magnetism in 2D correlated electronic materials.

Methods

Synthesis of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3

Single crystals of TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 were grown by chemical vapor transport. Tantalum, iron, tellurium, and TeCl4\mathrm{TeCl}_4 powders were combined in a 1:1.15:3:0.02 mole ratio, pressed into a pellet, and sealed in a fused silica tube (7 mm in diameter and approximately 40 cm in length) under vacuum. The sealed tube was loaded into a three-zone furnace and heated to a temperature gradient of 700°C to 600°C over 24 hours, with the pellet placed in the hot zone. After seven days, needle-like crystals were obtained in the sink end of the tube.

Energy Dispersive X-ray Spectroscopy (EDX) and Scanning Electron Microscopy (SEM)

SEM images were acquired on a Zeiss SIGMA VP scanning electron microscope with a Bruker XFlash 6|30 Detector for EDX measurements. Single TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 crystals were washed with hexanes, placed on carbon tape, and the surface was freshly cleaved with Scotch Magic tape immediately before loading into the chamber. SEM images were acquired with a beam energy of 5 kV. EDX spectra were acquired with a beam energy of 18 kV. The EDX collection time was automatically set by the Bruker ESPRIT 2 software using the “precise” acquisition setting. Elemental compositions and atomic percentages were estimated by integrating under the characteristic spectrum peaks for each element using Bruker ESPRIT 2 software.

Vibrating Sample Magnetometry (VSM) up to 9T

Vibrating sample magnetometry was conducted on a Quantum Design PPMS Dynacool system. TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 single crystals were attached to a quartz paddle using GE varnish (which was cured at room temperature under ambient conditions for 45 minutes) and oriented with long in-plane (LIP), short in-plane (SIP), or out-of-plane (OOP) direction parallel to the applied magnetic field. The same crystal was used for all direction-dependent measurements. Variable temperature magnetic susceptibility and magnetic field-dependent magnetization curves for each orientation were measured during the same measurement cycle. Samples were removed using a 1:1 ethanol/toluene solution, dried in air, and then remounted to the quartz paddle using GE varnish.

Vibrating Sample Magnetometry (VSM) up to 35T

The high-field magnetization data were obtained at the National High Magnetic Field Laboratory (NHMFL) using a conventional Vibrating Sample Magnetometer. The measurement was performed on a few single crystal samples with a total mass of 19.6 mg glued on a Torlon (polyamidimide) sample holder with GE7031 varnish. A water-cooled resistive magnet was used to apply magnetic fields up to 35 T.

Scanning Tunneling Microscopy/Spectroscopy (STM/S)

STM and STS measurements were conducted in a home-built STM under ultra-high vacuum at 7.5 K. The tungsten tunneling tip was electrochemically etched and calibrated against the Au(111) surface state prior to each sample approach. Crystals were cleaved in vacuum prior to measurement. Topography was acquired in constant current mode with a set bias of 400 mV and a set current of 50 pA.

Transmission Electron Microscopy (TEM)

TaFe1.14_{1.14}Te3_3 flakes were isolated through mechanical exfoliation of single crystals and placed on a TEM grid. TEM images were taken with a Thermofisher Scientific Talos F200X. The sample was slightly tilted to the desired orientation and bright-field mode imaging was set by using the Objective Aperture 100 μ\mum.

Electrical Transport Device Fabrication

TaFe1.14_{1.14}Te3_3 crystals were bonded to a 16-pin DIP socket using low-temperature non-conducting epoxy (Loctite EA 1C) and the top surface was freshly cleaved. All contacts to bulk TaFe1.14_{1.14}Te3_3 were made with Field’s metal using a microsoldering technique[33, 34]. A micromanipulator and heated sample holder were placed under an optical microscope. The temperature of the sample holder was raised to 70∘^\circC to melt the Field’s metal. The tip of the micromanipulator was lowered into the Field’s metal and slowly drawn out to produce a contact with a few-micron-wide tip. The contact was then aligned on top of the sample with the micromanipulator and placed on the sample while heating to 100∘^\circC. Direct electrical connections from the Field’s metal contact to the dip socket gold pads were made by hand with silver paint (Dupont 4929N) and 25 μ\mum diameter aluminum wirebonding wire.

Electrical Transport Measurements

Longitudinal and Hall resistances were measured in a 4-terminal configuration using a Keithley 6221 as a high-precision current source and a Keithley 2182A as a DC voltmeter. The two instruments were operated in delta mode to reduce background noise. A source current of 5 mA was used for all measurements unless otherwise stated. Due to the morphology of the TaFe1.14_{1.14}Te3_3 crystals, current and longitudinal resistance were measured parallel to the long in-plane direction (LIP) and the Hall voltage was measured along the short in-plane direction (SIP). Variable temperatures between 1.5 K and 300 K and magnetic fields between -12 T and 12 T were achieved in an Oxford TeslatronPT dry 4^4He cryostat.

Exfoliation

Thin flakes of TaFe1.14_{1.14}Te3_3 were isolated using a two-step exfoliation procedure. First, single TaFe1.14_{1.14}Te3_3 crystals were cleaved multiple times with Nitto REVALPHA thermal release tape[45]. Then, Scotch Magic tape was used to exfoliate the crystals from the thermal release tape and transfer them onto commercially available polydimethylsiloxane (PDMS) stamps. Once on the PDMS stamps, the thickness of exfoliated flakes was inferred from atomic force microscopy and optical contrast.

Atomic Force Microscopy (AFM)

Atomic force microscopy was performed in a Bruker Dimension Icon using OTESPA-R3 tips in tapping mode. Flake thicknesses were extracted using Gwyddion to measure the height difference between the substrate and the desired TaFe1.14_{1.14}Te3_3 flake.

X-ray Photoemission Spectroscopy (XPS)

XPS measurements were performed by a VersaProbe II (Physical Electronics) equipped with Al Kα\alpha X-rays and dual beam neutralization (10 eV Ar+^+ ions and electrons) at 45-degree measuring angle. The pass energies for survey and individual elements are 117.4 eV and 23.5 eV, respectively.

Single crystal X-ray diffraction

Single crystal diffraction measurements were collected on TaFe1.14_{1.14}Te3_3 crystals using an Agilent Supernova single-crystal diffractometer. The crystals were mounted onto a MiTeGen MicroLoops holder with paratone oil. The X-ray source was a Mo Kα\alpha micro-focus tube energized to 50 kV and 0.8 mA. The collection temperature was maintained between 300 K and 100 K using an Oxford instruments nitrogen cryostream. The data collection, integration, and reduction were performed using the Crysalis Pro software suite. The crystal structure was solved and refined using ShelXT and ShelXL respectively.

Powder X-ray diffraction (PXRD)

Powder diffraction patterns were collected on a Panalytical Aeris diffractometer with a Cu Kα\alpha X-ray source energized to 40 kV and 15 mA. The X-ray beam was filtered with a Niβ\beta filter. The powder sample of TaFe1.14_{1.14}Te3_3 (prepared by grinding single crystals in liquid nitrogen) was mounted on a Si-zero background holder which was spun to reduce preferred orientation.

Heat capacity

Heat capacity measurements were performed with a Quantum Design PPMS Dynacool system. The background heat capacity of the sample puck plus grease (Apiezon N grease) was measured over the desired temperature and magnetic field ranges before the sample was loaded onto the platform. The background was then subtracted from the total measured heat capacity (sample plus grease and puck) to obtain the heat capacity of the sample.

Angle-resolved Photoemission Spectroscopy (ARPES)

The sample was attached to a sample holder using Agepoxy and cleaved in-situ using Kapton tape, just before the ARPES measurements. The ARPES experiments were carried out at OASIS-laboratory at Brookhaven National Laboratory using a Scienta SES-R4000 electron spectrometer with monochromatized He-Iα\alpha (21.22 eV) radiation (VUV-5k)[46]. The total instrumental energy resolution was ≈10\approx10 meV. The angular resolution was better than 0.15θ0.15\theta and 0.4θ0.4\theta along and perpendicular to the slit of the analyzer, respectively.

Preparation of TaFe1.14_{1.14}Te3_3 powder samples for magnetometry measurements under pressure

Single crystals of TaFe1.14_{1.14}Te3_3 were placed in a thin porcelain crucible with enough liquid N2_2 to fully submerge the crystals. The crystals were then ground with a thermally equilibrated pestle for 5 mins. The resulting powder was rinsed with acetone to remove residual moisture from condensation.

Determination of applied hydrostatic pressure for magnetometry measurements under pressure

Since the superconducting (SC) critical temperature (TCT_{\mathrm{C}}) of Pb is well-known to linearly depend upon applied hydrostatic pressure (PP) at a rate of dTC/dP=0.379dT_{\mathrm{C}}/dP = 0.379 K·GPa−1^{-1}[47], we use the measured TCT_{\mathrm{C}} of Pb to determine the PP on TaFe1.14_{1.14}Te3_3. First, the Pb plus TaFe1.14_{1.14}Te3_3 sample is zero-field cooled below the SC transition to 6 K. Then, the magnetic susceptibility (χ\chi) versus temperature (TT) is measured with a small measuring field of 5 Oe (much smaller than the zero-temperature upper critical field of Pb[48]). χ\chi versus TT is measured at a rate of 0.05 K·min−1^{-1} to ensure the transition is precisely resolved and traces with increasing and decreasing TT were measured. The Pb TCT_{\mathrm{C}} is extracted by finding the condition where χ=0.5χN\chi= 0.5\chi_{\mathrm{N}} (χN\chi_{\mathrm{N}} is the susceptibility in the normal state).

Vibrating sample magnetometry under hydrostatic pressure

All vibrating sample magnetometry under PP was conducted on a Quantum Design PPMS Dynacool system using the commercially-available HMD high-pressure cell. Before and after the VSM measurements, PXRD was used to confirm there was no significant change in structure upon grinding or after applying maximum pressure (Figure S9). The powder was then combined with Daphne 7373 oil and a ≈1\approx1-2 mm long wire of Pb in a Teflon capsule, which was then inserted into the pressure cell. The variable temperature scans and field-dependent magnetic susceptibility curves for each PP were measured during the same measurement cycle. The measurements performed at different pressures were done sequentially with increasing pressure (from zero applied pressure up to the maximum achievable pressure). After the final maximum pressure measurement, the capsule containing the TaFe1.14_{1.14}Te3_3 powder, Daphne 7373 oil, and the Pb manometer was removed, fixed to a brass paddle with GE varnish, and re-measured as a consistency check of the zero-pressure measurement.

Computational Methods

The computational results were obtained using density functional theory, as implemented in the QUANTUM ESPRESSO package[49, 50]. We used projector-augmented wave pseudopotentials (Ta.pbe-spn-kjpaw_psl.1.0.0.UPF, Fe.pbe-spn-kjpaw_psl.1.0.0.UPF, and Te.pbe-n-kjpaw_psl.1.0.0.UPF from http://www.quantum-espresso.org) with the Perdew-Burke-Ernzerhof exchange-correlation functional[51], with nonlinear core correction and scalar relativistic effects. Gaussian smearing was set to 0.005 Ry. The wave function and density energy cutoffs were 100 Ry and 400 Ry, respectively. The Brillouin zone was sampled with a 7x7x7 kk-space mesh for the paramagnetic, primitive cells and with a 3x7x7 kk-space mesh for the 2x1x1 AFM supercells. The unit cell was taken from MaterialsProject (mp-8848)[52]. Relaxed positions of atoms within the unit cell were used.

Acknowledgements

We would like to thank Daniel Chica and Amy-marie Bartholomew for their help in analyzing SCXRD data and Mike Ziebiel for useful discussions on magnetic data. We would also like to acknowledge the use of Python-based data acquisition software developed by Maëlle Kapfer for all transport measurements. Synthesis and structural/compositional characterization of layered metallic antiferromagnets was supported by the National Science Foundation (NSF) through the Columbia University Materials Research Science and Engineering Center (MRSEC) on Precision-Assembled Quantum Materials DMR-2011738. Magnetotransport measurements were supported as part of Programmable Quantum Materials, an Energy Frontier Research Center funded by the U.S. Department of Energy (DOE), Office of Science, Basic Energy Sciences (BES), under award DESC0019443. Magnetic characterization was supported by the Air Force Office of Scientific Research award FA9550-22-1-0389. Imaging experiments were supported by the NSF CAREER award DMR-1751949. S.J.B. acknowledges support from the NSF Award DGE-2036197. The authors acknowledge the use of facilities and instrumentation supported by the NSF through Columbia University, Columbia Nano Initiative, and the Materials Research Science and Engineering Center DMR-2011738. The National High Magnetic Field Laboratory is supported by the NSF through NSF/DMR-1644779 and the State of Florida. The research at Brookhaven National Laboratory was supported by the US Department of Energy, Office of Basic Energy Sciences, Contract No. DESC0012704.

Author Contributions

S.Y.H. and E.J.T. collected and analyzed the SCXRD data. S.Y.H. and R.W. optimized the synthesis procedure and synthesized the single crystals. S.Y.H. and E.J.T. performed the SEM/EDX and analyzed the data. S.T. performed the STM and STS experiments. A.Z. collected and analyzed the TEM data. S.J.B. performed DFT calculations. S.Y.H. and E.J.T. performed the low-field magnetometry. S.Y.H., E.J.T., and E-S.C. performed the high-magnetometry. S.Y.H. prepared the single-crystal transport devices and E.J.T. performed the transport measurements and analyzed the data. A.K. collected and analyzed the ARPES data. T-D.L. performed the XPS experiments. S.Y.H. and E.J.T. exfoliated few-layer flakes and performed the atomic force microscopy and contrast analysis. S.Y.H. and E.J.T. performed heat capacity measurements and analyzed the data. S.Y.H. performed and analyzed the PXRD data. The manuscript was prepared with input from all coauthors.

Supporting Information

Supporting information is available at the end of this document after the references.

Conflict of Interest

The authors declare no conflict of interest.

Powderization enhancement of the spin-glass phase in TaFe1.14Te3

Figure S7. Powderization enhancement of the spin-glass phase in TaFe1.14_{1.14}Te3_3. A-D) Magnetic susceptibility versus temperature with a measuring field of 0.01 T (A), 0.1 T (B), 1 T (C), and 9 T (D). Both field-cooled and zero-field-cooled traces are shown and denoted. Top panels are collected from a single TaFe1.14_{1.14}Te3_3 crystal with the magnetic field applied parallel to the short in-plane direction. Bottom panels are collected from the same powderized crystal.

Magnetic properties of TaFe1.14Te3 spin-glass phase under hydrostatic pressure

Figure S8. Magnetic properties of TaFe1.14_{1.14}Te3_3 spin-glass phase under hydrostatic pressure. A) Magnetic susceptibility versus temperature across the superconducting transition for the lead manometer for various applied pressures. The corresponding applied pressure is given in the inset. All traces were offset and normalized for clarity. A measuring field of 5 Oe was used. B) Field-cooled (dashed traces) and zero-field-cooled (solid traces) magnetic susceptibility versus temperature for various applied pressures. The corresponding pressure is given in the inset. A measuring field of 1000 Oe was used. C) Magnetization versus magnetic field at 2 K for various applied pressures. Due to the pressure-cell preparation, the magnetic field direction is averaged along all crystal axes. The corresponding pressure is given in the inset. For all panels, measurements were performed in order of increasing pressure. The final measurement (0.000 GPa) is a reference measurement of the sample plus Teflon capsule measured outside of the pressure cell on a brass paddle sample mount.

Background high-field magnetization from the sample paddle

Figure S12. Background high-field magnetization from the sample paddle. Magnetization versus magnetic field at 1.5 K for two sample paddles with GE varnish. The blue and red traces correspond to the different paddles.

Temperature dependence of the first metamagnetic transition field in TaFe$_{1.14}$Te$_3$

Figure S16. Temperature dependence of the first metamagnetic transition field in TaFe1.14_{1.14}Te3_3. The magnetic field at which the first metamagnetic transition occurs as measured by magnetometry (solid black pluses and red crosses), longitudinal magnetoresistance (solid blue circles), and Hall resistance (solid green diamonds). The dashed black line is a guide to the eye. The Nèel temperature is denoted by a solid gray line. The magnetic field was aligned parallel to the out-of-plane axis for all measurements.

Current dependence of magnetotransport in TaFe$_{1.14}$Te$_3$

Figure S19. Current dependence of magnetotransport in TaFe1.14_{1.14}Te3_3. Magnetoresistance ratio, MRR=[R(H)−R(H=0)]/R(H=0)×100MRR = [R(H)-R(H=0)]/R(H=0) \times100, versus magnetic field at various source currents for fields parallel to the out-of-plane direction. Both forward and backward traces are shown. The traces were all taken at 1.5 K. The dashed black lines denote the zero crossings. The inset is an optical image of the device along with the measurement configuration.

300 K200 K100 K
Empirical FormulaTaFe1.14_{1.14}Te3_3TaFe1.12_{1.12}Te3_3TaFe1.12_{1.12}Te3_3
Formula weight627.42626.02626.58
Temperature300.01(10) K200.00(10) K100.00(10) K
Wavelength0.71073 Å0.71073 Å0.71073 Å
Crystal systemMonoclinicMonoclinicMonoclinic
Space groupP21/mP2_{1}/mP21/mP2_{1}/mP21/mP2_{1}/m
aa7.4171(3) Å7.4076(3) Å7.4105(4) Å
α\alpha90°90°90°
bb3.63280(10) Å3.62530(10) Å3.61940(10) Å
β\beta109.129(5)°109.175(4)°109.189(6)°
cc9.9740(4) Å9.9661(4) Å9.9626(5) Å
γ\gamma90°90°90°
Volume253.908(18) Å3^3252.789(17) Å3^3252.37(2) Å3^3
ZZ222
Density (calculated)8.207 g/cm3^38.225 g/cm3^38.246 g/cm3^3
Absorption coefficient41.478 mm−1^{-1}41.593 mm−1^{-1}41.690 mm−1^{-1}
F(000)F(000)517516516
Crystal size0.239 × 0.049 × 0.019 mm3^30.239 × 0.049 × 0.019 mm3^30.239 × 0.049 × 0.019 mm3^3
θ\theta collection range2.161° to 28.400°2.164° to 28.402°2.164° to 28.539°
Index ranges−9≤h≤9-9 \le h \le9, −4≤k≤4-4 \le k \le4, −13≤l≤12-13 \le l \le12−9≤h≤9-9 \le h \le9, −4≤k≤4-4 \le k \le4, −13≤l≤12-13 \le l \le12−9≤h≤9-9 \le h \le9, −4≤k≤4-4 \le k \le4, −13≤l≤12-13 \le l \le12
Reflections collected296629502962
Independent reflection681 [Rint=0.0410R_{\mathrm{int}}=0.0410]674 [Rint=0.0428R_{\mathrm{int}}=0.0428]682 [Rint=0.0498R_{\mathrm{int}}=0.0498]
Completeness to θ=25.242∘\theta=25.242^\circ100%100%100%
Refinement methodFull-matrix least-squares on F2F^2Full-matrix least-squares on F2F^2Full-matrix least-squares on F2F^2
Data/restraints/parameters681/0/35674/0/35682/0/35
Goodness-of-fit1.0821.1211.047
Final RR indices [I>2σ(I)I>2\sigma(I)]Robs=0.0261R_{\mathrm{obs}}=0.0261, wRobs=0.0601wR_{\mathrm{obs}}=0.0601Robs=0.0267R_{\mathrm{obs}}=0.0267, wRobs=0.0578wR_{\mathrm{obs}}=0.0578Robs=0.0284R_{\mathrm{obs}}=0.0284, wRobs=0.0627wR_{\mathrm{obs}}=0.0627
RR indices [all data]Rall=0.0291R_{\mathrm{all}}=0.0291, wRall=0.0624wR_{\mathrm{all}}=0.0624Rall=0.0283R_{\mathrm{all}}=0.0283, wRall=0.0587wR_{\mathrm{all}}=0.0587Rall=0.0299R_{\mathrm{all}}=0.0299, wRall=0.0638wR_{\mathrm{all}}=0.0638
Extinction coefficient0.0015(3)0.0024(3)0.0019(3)
Largest diff. peak and hole1.725 e·Å−3^{-3} and -2.003 e·Å−3^{-3}2.093 e·Å−3^{-3} and -2.263 e·Å−3^{-3}2.136 e·Å−3^{-3} and -2.824 e·Å−3^{-3}

Table S1. Crystallographic parameters determined through SCXRD for TaFe1.14_{1.14}Te3_3 at various temperatures. R=Σ∣∣Fo∣−∣Fc∣∣/Σ∣Fo∣R=\Sigma||F_o|-|F_c||/\Sigma|F_o|, wR={Σ[w(∣Fo∣2−∣Fc∣2)2]/Σ[w(∣Fo∣4)]}1/2wR=\{\Sigma[w(|F_o|^2-|F_c|^2)^2]/\Sigma[w(|F_o|^4)]\}^{1/2} and w=1/[σ2(Fo2)+(0.021P)2+1.7407P]w=1/[\sigma^2(F_o^2)+(0.021P)^2+1.7407P], where P=(Fo2+2Fc2)/3P=(F_o^2+2F_c^2)/3.

EJT-001RJ-1-30SJH-164SJH-171SJH-208Combined
Ta1.00±0.081.00 \pm0.080.88±0.040.88 \pm0.040.89±0.060.89 \pm0.060.85±0.030.85 \pm0.030.87±0.020.87 \pm0.020.90±0.060.90 \pm0.06
Fe1.21±0.051.21 \pm0.051.19±0.051.19 \pm0.051.16±0.061.16 \pm0.061.26±0.251.26 \pm0.251.22±0.031.22 \pm0.031.21±0.041.21 \pm0.04
Te3.003.003.003.003.003.00

Table S2. Extracted chemical compositions for multiple TaFe1.14Te3\mathrm{TaFe}_{1.14}\mathrm{Te}_3 growth batches. Relative concentration of Ta, Fe, and Te normalized to the measured Te concentration for each growth batch. The last column is the average concentration of each element between all growth batches. Error bars represent the standard deviation. All chemical concentrations were extracted from SEM/EDX data.

References

  1. [1]E. C. Ahn, 2d materials for spintronic devices, npj 2D Materials and Applications 4, 17 (2020).DOI
  2. [2]A. Arora, Magneto-optics of layered two-dimensional semiconductors and heterostructures: Progress and prospects, Journal of Applied Physics 129, 190902 (2021).DOI
  3. [3]F. Hendriks and M. H. D. Guimarães, Enhancing magneto-optic effects in two-dimensional magnets by thin-film interference, AIP Advances 11, 035132 (2021).DOI
  4. [4]Y. Zhang, H. Xu, J. Feng, H. Wu, G. Yu, and X. Han, Magnetic two-dimensional van der waals materials for spintronic devices, Chinese Physics B 30, 118504 (2021).DOI
  5. [5]T. Lan, B. Ding, and B. Liu, Magneto-optic effect of two-dimensional materials and related applications, Nano Select 1, 298 (2020).DOI
  6. [6]Z. Chen, B. Wang, D. Y. Xing, and J. Wang, A spin injector, Applied Physics Letters 85, 2553 (2004).DOI
  7. [7]V. P. Ningrum, B. Liu, W. Wang, Y. Yin, Y. Cao, C. Zha, H. Xie, X. Jiang, Y. Sun, S. Qin, X. Chen, T. Qin, C. Zhu, L. Wang, and W. Huang, Recent advances in two-dimensional magnets: Physics and devices towards spintronic applications, Research 2020 (2020).DOI
  8. [8]Q. H. Wang, A. Bedoya-Pinto, M. Blei, A. H. Dis-mukes, A. Hamo, S. Jenkins, M. Koperski, Y. Liu, Q.-C. Sun, E. J. Telford, H. H. Kim, M. Augustin, U. Vool, J.-X. Yin, L. H. Li, A. Falin, C. R. Dean, F. Casanova, R. F. L. Evans, M. Chshiev, A. Mishchenko, C. Petrovic, R. He, L. Zhao, A. W. Tsen, B. D. Gerardot, M. Brotons-Gisbert, Z. Guguchia, X. Roy, S. Tongay, Z. Wang, M. Z. Hasan, J. Wrachtrup, A. Yacoby, A. Fert, S. Parkin, K. S. Novoselov, P. Dai, L. Balicas, and E. J. G. Santos, The magnetic response of two-dimensional van der waals materials, ACS Nano 16, 6960 (2022).DOI
  9. [9]I. Shin, W. J. Cho, E.-S. An, S. Park, H.-W. Jeong, S. Jang, W. J. Baek, S. Y. Park, D.-H. Yang, J. H. Seo, G.-Y. Kim, M. N. Ali, S.-Y. Choi, H.-W. Lee, J. S. Kim, S. D. Kim, and G.-H. Lee, Spin-orbit torque switching in an all-van der waals heterostructure, Advanced Materials 34, 2101730 (2022).arxiv.org/abs/2102.09300
  10. [10]F. Martin, K. Lee, M. Schmitt, A. Liedtke, A. Shahee, H. T. Simensen, T. Scholz, T. G. Saunderson, D. Go, M. Gradhahd, Y. Mokrüsov, T. Denneulin, A. Kovács, B. Lotsch, A. Brataas, and M. Kläui, Strong bulk spin–orbit torques quantified in the van der waals ferromagnet Fe3GeTe2, Materials Research Letters 11, 84 (2023).DOI
  11. [11]T. Jungwirth, X. Marti, P. Wadley, and J. Wunderlich, Antiferromagnetic spintronics, Nature Nanotechnology 11, 2016).DOI
  12. [12]S. M. Rezende, A. Azevedo, and R. L. Rodríguez-Suárez, Introduction to antiferromagnetic magnons, Journal of Applied Physics 126, 151101 (2019).DOI
  13. [13]H. Yan, Z. Feng, P. Qin, X. Zhou, H. Guo, X. Wang, H. Chen, X. Zhang, H. Wu, C. Jiang, and Z. Liu, Electric-field-controlled antiferromagnetic spintronic devices, Advanced Materials 32, 1905603 (2020).DOI
  14. [14]K. Ueda, Electrical resistivity of antiferromagnetic metals, Journal of the Physical Society of Japan 43, 1497 (1977).DOI
  15. [15]X.-X. Zhang, S. Jiang, J. Lee, C. Lee, K. F. Mak, and J. Shan, Spin dynamics slowdown near the antiferromagnetic critical point in atomically thin FePS₃, Nano Letters 21, 5045 (2021).
  16. [16]H. Bai, X. Zhou, Y. Zhou, X. Chen, Y. You, F. Pan, and C. Song, Functional antiferromagnets for potential applications on high-density storage and high frequency, Journal of Applied Physics 128, 210901 (2020).
  17. [17]S. Rahman, J. F. Torres, A. R. Khan, and Y. Lu, Recent developments in van der waals antiferromagnetic 2d materials: Synthesis, characterization, and device implementation, ACS Nano 15, 17175 (2021).
  18. [18]K. F. Mak, J. Shan, and D. C. Ralph, Probing and controlling magnetic states in 2d layered magnetic materials, Nature Reviews Physics 1, 646 (2019).
  19. [19]J. Neuhausen, E. Potthoff, W. Tremel, J. Ensling, P. Gütlich, and R. K. Kremer, TaFe₁.₁₄Te₃, a new low-dimensional ternary tantalum telluride., ChemInform 24 (1993).
  20. [20]C. Pérez Vicente, M. Womes, J. C. Jumas, L. Sánchez, and J. L. Tirado, Distribution of cations and vacancies in TaFe₁.₂₅Te₃ studied by mössbauer spectroscopy, The Journal of Physical Chemistry B 102, 8712 (1998).
  21. [21]M. E. Badding, J. Li, F. J. DiSalvo, W. Zhou, and P. P. Edwards, Characterization of TaFe₁.₂₅Te₃, a new layered telluride with an unusual metal network structure, Journal of Solid State Chemistry 100, 313 (1992).
  22. [22]M. Opačić, N. Lazarević, D. Tanasković, M. M. Radonjić, A. Milosavljević, Y. Ma, C. Petrovic, and Z. V. Popović, Small influence of magnetic ordering on lattice dynamics in TaFe₁.₂₅Te₃, Physical Review B 96, 174303 (2017).
  23. [23]X. Ke, B. Qian, H. Cao, J. Hu, G. C. Wang, and Z. Q. Mao, Magnetic structure of quasi-one-dimensional antiferromagnetic TaFe₁₊yTe₃, Physical Review B 85, 214404 (2012).
  24. [24]R. H. Liu, M. Zhang, P. Cheng, Y. J. Yan, Z. J. Xiang, J. J. Ying, X. F. Wang, A. F. Wang, G. J. Ye, X. G. Luo, and X. H. Chen, Spin-density-wave transition of Fe1 zigzag chains and metamagnetic transition of Fe2 in TaFe₁+yTe₃, Physical Review B 84, 184432 (2011).
  25. [25]Y. Liu, J. J. Bao, C. Q. Xu, W. H. Jiao, H. Zhang, L. C. Xu, Z. Zhu, H. Y. Yang, Y. Zhou, Z. Ren, P. K. Biswas, S. K. Ghosh, Z. Yang, X. Ke, G. H. Cao, and X. Xu, Coupling between antiferromagnetic and spin-glass orders in the quasi-one-dimensional iron telluride TaFe₁+xTe₃ (x=0.25), Physical Review B 104, 104418 (2021).
  26. [26]R. Roy Chowdhury, S. DuttaGupta, C. Patra, A. Kataria, S. Fukami, and R. P. Singh, Anisotropic magnetotransport in the layered antiferromagnet TaFe₁.₂₅Te₃, Physical Review Materials 6, 084408 (2022).
  27. [27]M. Xu, L.-M. Wang, R. Peng, Q.-Q. Ge, F. Chen, Z.-R. Ye, Y. Zhang, S.-D. Chen, M. Xia, R.-H. Liu, M. Shi, X.-H. Chen, W.-G. Yin, W. Ku, B.-P. Xie, D.-L. Feng, M. Arita, K. Shimada, H. Namatame, M. Taniguchi, M. Matsunami, and S. Kimura, Electronic structure reconstruction across the antiferromagnetic transition in TaFe₁.₂₃Te₃ spin ladder, Chinese Physics Letters 32, 027401 (2015).
  28. [28]H. Aruga, A. Ito, H. Wakabayashi, and T. Goto, Field-dependent phenomena in reentrant-spin-glass: Fe(x)mn(1-x)tiO(3) with x=0.60, 0.65, and 0.75, Journal of the Physical Society of Japan 57, 2636 (1988).
  29. [29]A. Ito, S. Morimoto, and H. Aruga, Studies on spin-glass freezing and antiferromagnetic long-range order in an ising spin-glass system fe(x)mn(1-x)tiO(3), Hyperfine Interactions 54, 567 (1990).
  30. [30]H. A. Katori and A. Ito, Magnetic property and phase diagram of a frustrated system with competing exchange interactions, fe(x)mn(1-x)tiO(3), Journal of the Physical Society of Japan 62, 488 (1993).
  31. [31]H. Yoshizawa, S. Mitsuda, H. Aruga, and A. Ito, Reentrant spin-glass transition and a mixed phase in an ising system fe(x)mn(1-x)tiO(3), Journal of the Physical Society of Japan 58, 1416 (1989).
  32. [32]T. Yamashita and P. Hayes, Analysis of xps spectra of Fe2+ and Fe3+ ions in oxide materials, Applied Surface Science 254, 2441 (2008).
  33. [33]Ç. Ö. Girit and A. Zettl, Soldering to a single atomic layer, Applied Physics Letters 91 (2007).
  34. [34]A. Kerelsky, L. J. McGilly, D. M. Kennes, L. Xian, M. Yankowitz, S. Chen, K. Watanabe, T. Taniguchi, J. Hone, C. Dean, A. Rubio, and A. N. Pasupathy, Maximized electron interactions at the magic angle in twisted bilayer graphene, Nature 572, 95 (2019).
  35. [35]E. M. Pugh and N. Rostoker, Hall effect in ferromagnetic metals, Reviews of Modern Physics 25, 151 (1953).
  36. [36]Y. Zhang, F. Chen, C. He, L. X. Yang, B. P. Xie, Y. L. Xie, X. H. Chen, M. Fang, M. Arita, K. Shimada, H. Namatame, M. Taniguchi, J. P. Hu, and D. L. Feng, Strong correlations and spin-density-wave phase induced by a massive spectral weight redistribution in α-Fe₁.₀₆Te, Physical Review B 82, 165113 (2010).
  37. [37]X. Xu, Y. W. Li, S. R. Duan, S. L. Zhang, Y. J. Chen, L. Kang, A. J. Liang, C. Chen, W. Xia, Y. Xu, P. Malinowski, X. D. Xu, J. H. Chu, G. Li, Y. F. Guo, Z. K. Liu, L. X. Yang, and Y. L. Chen, Signature of non-stoner ferromagnetism in the van der waals ferromagnet Fe₃GeTe₂, Physical Review B 101, 201104 (2020).
  38. [38]S. Schmitt, N. Grewe, and T. Jabben, Itinerant and local-moment magnetism in strongly correlated electron systems, Physical Review B 85, 024404 (2012).
  39. [39]Z. K. Liu, R. H. He, D. H. Lu, M. Yi, Y. L. Chen, M. Hashimoto, R. G. Moore, S. K. Mo, E. A. Nowadnick, J. Hu, T. J. Liu, Z. Q. Mao, T. P. Devereaux, Z. Hussain, and Z. X. Shen, Measurement of coherent polarons in the strongly coupled antiferromagnetically ordered iron-chalcogenide Fe₁.₀₂Te using angle-resolved photoemission spectroscopy, Physical Review Letters 110, 037003 (2013).
  40. [40]Q. Y. Chen, X. B. Luo, D. H. Xie, M. L. Li, X. Y. Ji, R. Zhou, Y. B. Huang, W. Zhang, W. Feng, Y. Zhang, L. Huang, Q. Q. Hao, Q. Liu, X. G. Zhu, Y. Liu, P. Zhang, X. C. Lai, Q. Si, and S. Y. Tan, Orbital- selective kondo entanglement, and antiferromagnetic order in USb₂, Phys. Rev. Lett. 123, 106402 (2019).
  41. [41]Y. Zhang, C. He, Z. R. Ye, J. Jiang, F. Chen, M. Xu, Q. Q. Ge, B. P. Xie, J. Wei, M. Aeschlimann, X. Y. Cui, M. Shi, J. P. Hu, and D. L. Feng, Symmetry breaking via orbital-dependent reconstruction of electronic structure in detwinned nafeas, Physical Review B 85, 085121 (2012).DOI
  42. [42]L. X. Yang, Y. Zhang, H. W. Ou, J. F. Zhao, D. W. Shen, B. Zhou, J. Wei, F. Chen, M. Xu, C. He, Y. Chen, Z. D. Wang, X. F. Wang, T. Wu, G. Wu, X. H. Chen, M. Arita, K. Shimada, M. Taniguchi, Z. Y. Lu, T. Xiang, and D. L. Feng, Electronic structure and unusual exchange splitting in the spin-density-wave state of the BaFe₂As₂ parent compound of iron-based superconductors, Physical Review Letters 102, 107002 (2009).pubmed.ncbi.nlm.nih.gov/19392146
  43. [43]A. K. Kundu, S. Barman, and K. S. R. Menon, Role of surface termination in the metal–insulator transition of V₂O₃(0001) ultrathin films, ACS Applied Materials & Interfaces 13, 20779 (2021).DOI
  44. [44]M. B. J. Meinders, H. Eskes, and G. A. Sawatzky, Spectral-weight transfer: Breakdown of low-energy-scale sum rules in correlated systems, Physical Review B 48, 3916 (1993).pubmed.ncbi.nlm.nih.gov/10008840
  45. [45]Y. Deng, Y. Yu, Y. Song, J. Zhang, N. Z. Wang, Z. Sun, Y. Yi, Y. Z. Wu, S. Wu, J. Zhu, J. Wang, X. H. Chen, and Y. Zhang, Gate-tunable room-temperature ferromagnetism in two-dimensional Fe₃GeTe₂, Nature 563, 94 (2018).DOI
  46. [46]C. K. Kim, I. K. Drozdov, K. Fujita, J. C. S. Davis, I. Božović, and T. Valla, In-situ angle-resolved photoemission spectroscopy of copper-oxide thin films synthesized by molecular beam epitaxy, Journal of Electron Spectroscopy and Related Phenomena 257, 146775 (2022).
  47. [47]High pressure cell user manual (2016).
  48. [48]G. Chanin and J. P. Torre, Critical-field curve of superconducting lead, Physical Review B 5, 4357 (1972).DOI
  49. [49]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, I. Dabo, A. D. Corso, S. de Gironcoli, S. Fabris, G. Fratesi, R. Gebauer, U. Gerstmann, C. Gougoussis, A. Kokalj, M. Lazzeri, L. Martin-Samos, N. Marzari, F. Mauri, R. Mazzarello, S. Paolini, A. Pasquarello, L. Paulatto, C. Sbraccia, S. Scandolo, G. Scauzero, A. P. Seitsonen, A. Smogunov, P. Umari, and R. M. Wentzcovitch, Quantum espresso: a modular and open-source software project for quantum simulations of materials, Journal of Physics: Condensed Matter 21, 395502 (2009).DOI
  50. [50]P. Giannozzi, O. Andreussi, T. Brumme, O. Bunau, M. B. Nardelli, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, M. Cococcioni, N. Colonna, I. Carnimeo, A. D. Corso, S. de Gironcoli, P. Delugas, R. A. DiStasio, A. Ferretti, A. Floris, G. Fratesi, G. Fugallo, R. Gebauer, U. Gerstmann, F. Giustino, T. Gorni, J. Jia, M. Kawamura, H.-Y. Ko, A. Kokalj, E. Küçükbenli, M. Lazzeri, M. Marsili, N. Marzari, F. Mauri, N. L. Nguyen, H.-V. Nguyen, A. O. O. de-la Roza, L. Paulatto, S. Poncé, D. Rocca, R. Sabatini, B. Santra, M. Schlipf, A. P. Seitsonen, A. Smogunov, I. Timrov, T. Thonhauser, P. Umari, N. Vast, X. Wu, and S. Baroni, Advanced capabilities for materials modelling with quantum espresso, Journal of Physics: Condensed Matter 29, 465901 (2017).DOI
  51. [51]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  52. [52]A. Jain, S. P. Ong, G. Hautier, W. Chen, W. D. Richards, S. Dacek, S. Cholia, D. Gunter, D. Skinner, G. Ceder, and K. A. Persson, Commentary: The Materials Project: A materials genome approach to accelerating materials innovation, APL Materials 1 (2013).DOI

Paper details

vlnc:W_a6v3jy4v
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents