betaFeedback

WorksPhysics and Astronomy

Electronic structure and thermoelectric properties of epitaxial Sc1-xVxNy thin films grown on MgO(001)

Abstract

The electronic structure of Sc1-xVxNy epitaxial films with different alloying concentrations of V are investigated with respect to effects on thermoelectric properties. Band structure calculations on Sc0.75V0.25N indicate that V 3d states lie in the band gap of the parent ScN compound in the vicinity of the Fermi level. Thus, theoretically the presence of light (dispersive) bands at the Γ-point with band multiplicity is expected to lead to lower electrical resistivity while flat (heavy) bands at X-W-K symmetry points are associated with higher Seebeck coefficient than that of ScN. With this aim, epitaxial Sc1-xVxNy thin film samples were deposited on MgO(001) substrates. All the samples showed N substoichiometry and pseudocubic crystal structure. The N-vacancy-induced states were visible in the Sc 2p XAS spectra. The reference ScN and Sc1-xVxNy samples up to x = 0.12 were n type, exhibiting carrier concentration of 1021 cm-3, typical for degenerate semiconductors. For the highest V alloying of x = 0.15, holes became the majority charge carrier as indicated by the positive Seebeck coefficient. The underlying electronic structure and bonding mechanism in Sc1-xVxNy influence the electrical resistivity, Seebeck coefficient, and Hall effect. Thus, the work contributes to the fundamental understanding of the correlated defects and thermoelectric properties to the electronic structure in Sc-N system with V alloying.

Introduction

Conventional thermoelectric materials such as tellurides have been used since long to harvest power from waste heat [1, 2, 3, 4]. These materials have limitations because of toxicity and scarcity [5, 6]. There is thus a great deal of development of nontraditional thermoelectric materials, e.g., Heusler alloys, Zintl phases, silicides, oxides, and selenides [4, 7] [8, 9]. Recently, the semiconducting early transition metal nitrides based on ScN and CrN have emerged as alternative thermoelectric materials and are noteworthy compared to the materials listed above because of abundance, cost-effectiveness, and high symmetry rocksalt crystal structure. The simple cubic structure provides pathways for low electrical resistivity (ρ\rho) with high valley degeneracy and low thermal conductivity by phonon anharmonicity [10].

The efficiency of any thermoelectric material is determined by the dimensionless thermoelectric figure-of-merit expressed as, zT=(S2σ/κe+κl)TzT = (S^{2}\sigma/\kappa_{\mathrm{e}}+\kappa_{\mathrm{l}})T. Here, S = Seebeck coefficient, σ\sigma = electrical conductivity, κe\kappa_{\mathrm{e}} and κl\kappa_{\mathrm{l}} = electronic and lattice thermal conductivity, respectively, and T = absolute temperature. Thus, zTzT can be optimized by simultaneous increase of S2σS^{2}\sigma (known as the power factor) and lowering of κ\kappa (=κe+κl= \kappa_{\mathrm{e}}+\kappa_{\mathrm{l}}). However, in practice this is difficult to achieve as S is inversely coupled to both σ\sigma and κe\kappa_{\mathrm{e}} [11]. Typical power factor of ScN is 2.52.5-3.5×10−3 W m−13.5 \times10^{-3}\ \mathrm{W\ m}^{-1} K−2K^{-2}) at 600-840 K [11,12] and CrN of 1.51.5-5×10−35 \times10^{-3} W m−1^{-1} K−2^{-2} at 300 K [13,14], comparable to Bi2_2Te3_3 at 350 K and PbTe at 500 K [15,16]. The thermal conductivity of CrN-based thin films is ∼4\sim4 W m−1^{-1} K−1^{-1} [13], but the thermal conductivity of ScN is typically 10-12 W m−1^{-1} K−1^{-1} [17] at room temperature and requires reduction [11]. Since natural 45^{45}Sc has no isotopes, mass contrast due to isotope reduction has no effect on the thermal conductivity of pure ScN.

Hence, defects induced by doping/alloying (Cr, Nb) [18,19] and domain size reduction [17] in ScN have been used as a mechanism to reduce the thermal conductivity of ScN by increasing the phonon scattering. Furthermore, vacancies (≤3\le3 atomic %) in the Sc (p-type) or N (n-type) site can retain high SS with low metal-like ρ\rho increasing the overall power factor [20]. Alloying and ion-implantation (i.e., doping) with the same element (e.g., Mg) in ScN alters two different properties. The former enhances the power factor while the latter reduces the thermal conductivity in ScN [21,22]. Defects induced by ion implantations (Li+^{+}, Ar+^{+} and He+^{+}) in ScN increases ρ\rho, but results in an increase in SS and reduction in κ\kappa by overall increasing the zTzT [23–25].

The choice of suitable alloying elements for possible enhancement of the power factor is reflected in the electronic density of states (DOS) near the Fermi level (EFE_{\mathrm{F}}) or by modulating the band structure [26]. According to the Mott equation for degenerate semiconductors and metals [27], SS can be expressed as [2],

S=−π2kB2T3q[d{ln⁡σ(E)}dE]E=EFS=-\frac{\pi^{2} k_{\mathrm{B}}^{2} T}{3q}\left[\frac{d\{\ln\sigma(E)\}}{dE}\right]_{E=E_{\mathrm{F}}}

Here, electrical conductivity σ(E)∝DOS\sigma(E) \propto DOS, since the assumption is made that the electronic scattering is independent of energy [28]. Thus, a sharp slope with local increase in the DOS accompanied by asymmetry in the energy distribution function is key to achieve enhanced thermoelectric properties [20,29].

The electronic structure of ScN has been studied based on the contributions of different hybridization states of Sc and N [30] to understand the role of point defects (N vacancy, O and C substitution of the N-site, Mg, Be and Zr substitution of the Sc-site) on the thermoelectric properties of ScN [20]. Substantial amount of theoretical research using band structure calculations have been dedicated to obtain a correct bandgap of ScN, which is ∼0.9\sim0.9 eV [11,31]. Alloying of V in ScN is expected to yield a stable solid solubility with low negative enthalpy of mixing due to small lattice mismatch [32]. The atomic mass of V (50.94 g mol−1^{-1}) is slightly higher than Sc (44.96 g mol−1^{-1}) with two more valence electrons, which is expected to change the carrier concentration (nn) in stoichiometric ScN. Further, nn is related to SS (∝1/n2/3\propto1/n^{2/3}) and ρ\rho (∝1/n\propto1/n) [11], which should alter the thermoelectric properties. This underscores the need to investigate the electronic band structure of Sc1−x_{1-x}Vx_xNy_y near EFE_{\mathrm{F}}, correlating the electronic structure and thermoelectric properties of Sc1−x_{1-x}Vx_xNy_y.

In the present work, we probe the electronic structure and thermoelectric properties with alloying of V in ScN thin films. The structural and electronic properties of the alloyed samples are studied with a combination of experimental and theoretical methods, to elucidate the correlations between the charge carrier concentration, carrier mobility (μ\mu) and thermoelectric properties to the underlying electronic structure and chemical bonding.

Methods

Computational details

Electronic structure calculations were performed within a density-functional-theory framework and the projector augmented wave (PAW) method [33] as implemented in the Vienna ab initio simulation package (VASP) 6.3.0 [34,35] using a self-consistent energy convergence criteria of 1×10−51 \times10^{-5} eV. Convergence during structural relaxation was obtained by minimizing the forces on the ions to <0.001<0.001 eV/Å using a 29×29×2929 \times29 \times29 k-point mesh. GGA [36] with a combination of a Hubbard Coulomb term (GGA+U) [37,38] was used for treating electron exchange-correlation effects. Hubbard terms of U=3.5U=3.5 eV was applied to the Sc 3d3d and V 3d3d orbitals. The energy cutoff for plane waves included in the expansion of wave functions was 700 eV. The ScN unit cell contained 4 Sc atoms and 4 N atoms, while the (Sc,V)N cell contained 3 Sc atoms, 1 V atom and 4 N atoms exhibiting cubic rocksalt NaCl B1 type structure. Sampling of the Brillouin zone was done using a Monkhorst-Pack scheme [39] on a grid of 20×20×2020 \times20 \times20 k-points. For calculating the band structure, a kk-mesh of 80 points per line between the symmetry points was used. In the present study, we avoid the supercell calculations with doping (instead of alloying) of V in ScN due to the undesired band folding across the symmetry points which may lead to misleading results in the theoretical band structure calculations.

Experimental Details

Epitaxial Sc1−x_{1-x}Vx_xNy_y and reference ScN thin film samples were deposited on single-side polished single crystalline MgO(001) substrates by dc magnetron sputtering [40]. Prior to deposition, the MgO(001) substrates were cleaned following the procedures referred by le Febvrier et al. [41] and post in-situ annealed at 800°C for 30 mins. Sc (2-inch, purity 99.9%) and V (2-inch, purity 99.5%) target power was varied from 110-98 W and 0-15 W, respectively depending on the alloying concentration. The base pressure was ≤2.6×10−7\leq2.6 \times10^{-7} Pa (2×10−92 \times10^{-9} Torr) and the substrate temperature during deposition was 800°C. The Ar and N2_2 flow were kept constant at 13 sccm (30%) and 31 sccm (70%) keeping the total flow always constant at 44 sccm. The substrate rotation was fixed at 15 rpm to achieve better uniformity. More details about the deposition chamber can be found elsewhere [40].

The compositions of the samples were investigated by Energy Dispersive X-ray Spectroscopy (EDS) and time-of-flight Elastic Recoil Detection Analysis (ToF-ERDA). EDS measurements were performed at an accelerating voltage of 20 kV in a Zeiss Sigma 300 Scanning Electron Microscope (SEM) equipped with an X-Max 80 mm2^2 EDS detector from Oxford Instruments. The data was sampled and analyzed using AZtec software. ERDA measurements were performed using 36 MeV primary iodine ion (127^{127}I8+^{8+}) beam at the Pelletron Tandem accelerator (5 MV NEC-5SDH-2), Uppsala University, Sweden [42]. The incident beam angle to the sample surface normal was 67.5°, while the ToF-telescope and the gas ionization detector were placed at 45° relative to the incident beam direction. The depth profile of the elemental compositions were acquired from the ToF-ERDA time and energy coincidence spectra using the POTKU 2.0 software [43]. In addition, complementary RBS measurements were also done on the samples and discussed in the supplementary information (section 1 in the SI).

The out-of-plane X-Ray Diffraction (XRD) measurements were performed using a Malvern PANalytical X’Pert PRO MPD diffractometer equipped with a Cu-Kα source in BraggBrentano (θ\theta-2θ2\theta) geometry. The operating voltage and current were set at 45 kV and 40 mA. The incident optics consisted of a 1/2∘1/2^\circ divergence slit and 1/2∘1/2^\circ anti-scatter slit. The diffracted optics were composed of a 5.0 mm anti-scatter slit, a 0.04 rad Soller slit, a Ni-filter, and an X’Celerator detector. Subsequently, the Bragg-Brentano θ\theta-2θ2\theta scans at chi, χ=0∘\chi= 0^\circ and 45∘45^\circ were performed using a Malvern PANalytical X’Pert MRD diffractometer in line mode using a hybrid mirror with a divergence slit of 1/2∘1/2^\circ in the incident beam optics. At the diffracted beam optics, a triple axis monochromator compatible to a hybrid mirror equipped with receiving slits of 1/8∘1/8^\circ (at χ=0∘\chi= 0^\circ) or 1∘1^\circ (for χ=45∘\chi= 45^\circ) were used. The ϕ\phi-scans and X-ray reflectivity (XRR) (discussed in section 2 of the SI) measurements were also performed using a Malvern PANalytical X’Pert MRD diffractometer with a similar optics and 1∘1^\circ receiving slit. The voltage and current were set at 45 kV and 40 mA, respectively.

The soft X-ray absorption near-edge spectroscopy (XANES) and resonant inelastic X-ray scattering (RIXS) data [41,42] were measured at the SPECIES beamline, MAX IV, Lund, Sweden at the Sc 2p2p-edge, V 2p2p-edge, and N 1s1s-edge. The XANES spectra were recorded in both total electron yield (surface-sensitive) and total fluorescence yield (bulk-sensitive) modes. To probe the anisotropic nature (if any) around the electronic structure, the linearly polarized X-rays were incident at a grazing angle of 20∘20^\circ either in-plane (a-b plane) to the substrate (vertical polarization) or nearly 80% along the c-axis (horizontal polarization). The energy resolutions were 0.30 eV and 0.35 eV for Sc, and V 2p2p absorption edges, respectively. For normalization of the absorption edges, a 4 μ\mum thick Au reference foil was measured directly after each scan. For RIXS, the total energy resolution for the Sc LL – N KK emission was 0.58 eV and 0.62 eV for the V LL-emission. The base pressure was ≤6.7×10−7\le6.7 \times10^{-7} Pa during all the measurements. To minimize self-absorption effects [46], the angle of incidence was 20∘20^\circ from the surface plane during the emission measurements. The X-ray photons were detected parallel to the polarization vector of the incoming beam to minimize elastic (Rayleigh) scattering.

Core-level X-ray photoelectron spectroscopy (XPS) (discussed in section 3 of the SI) and the valence band spectroscopy (VBS) were performed on freshly deposited samples. An Axis Ultra DLD instrument, Kratos Analytical (UK) equipped with monochromatized Al-Kα_\alpha radiation (1486.6 eV) was used. The base pressure was ∼1.3×10−7\sim1.3 \times10^{-7} Pa during measurements. Prior to measurements, samples were sputter etched for 10 minutes using 0.5 keV Ar+^+ ions at an incident angle of 70∘70^\circ from the surface normal. Such pretreatment has been shown to minimize the sputter damage effects in transition metal nitrides [47]. The area affected by the Ar+^+ beam was 3×33 \times3 mm2^2, while the analysis area was 0.3×0.70.3 \times0.7 mm2^2 (centered in the middle of the etched crater). The analyzer pass energy was 20 eV, resulting in a full width at half maximum of 0.55 eV for the Ag 3d5/23d_{5/2} peak from the reference Ag sample. The charge referencing for all the samples was done by setting the low energy (density of states) cut-off to 0 eV. Due to the low electrical conductivity of Sc0.93_{0.93}V0.07_{0.07}N0.87_{0.87}, an electron flood gun was used during the data acquisition.

A standard four-point-probe set-up (Jandel Model RM3000) at room temperature was used to measure the sheet resistance of the samples. The electrical resistivity (ρ\rho = sheet resistance multiplied with film thickness) of the samples were calculated. The obtained film thickness was around 130 nm measured using XRR (see Table S1 in the SI). The Seebeck coefficients were measured using a home-built setup [48] which uses a resistive heater placed on one end of the sample providing the desired temperature gradient by controlling the applied voltage via a Keithley 2400 Source measure unit. The charge carrier concentration and mobility were measured by Hall measurements in a home-made setup employing a 0.485 T permanent magnet:VEVENT while measuring the Hall voltage in van der Pauw configuration. All the electrical measurements were performed at room temperature.

Results

Band structure calculations of ScN and (Sc,V)N

Figure 1(a) and (b) show calculated band structures of stoichiometric ScN and Sc0.75_{0.75}V0.25_{0.25}N along the L-Γ\Gamma-X-W-K-Γ\Gamma directions in the Brillouin zone. Figure 1(c) and (d) show the cubic rocksalt B1 type crystal structures of ScN and Sc0.75_{0.75}V0.25_{0.25}N. For ScN with NaCl B1 structure, the self-consistent calculations resulted in an equilibrium lattice constant (minimum in the total energy) of a=4.518a = 4.518 Å consistent with literature values [49]. For Sc0.75_{0.75}V0.25_{0.25}N with B1-NaCl structure, the relaxed equilibrium lattice constant was a=4.410a = 4.410 Å.

For ScN, the conduction band minimum (CBM, above EFE_{\mathrm{F}}) is dominated by Sc 3d3d t2gt_{2g} orbitals while the valence band maximum (VBM) is dominated by electronegative N 2p2p orbitals (below EFE_{\mathrm{F}}) [49]. The VB consists of both heavy (flat) and light (dispersive) hole bands at the Γ\Gamma-point. Two direct bandgaps of 3.04 eV and 1.64 eV are located at the Γ\Gamma and X-symmetry points, respectively, and an indirect bandgap of 0.65 eV is located along the Γ\Gamma-X direction. Initially, the band structure of ScN was debated and assigned to either a semi-metal [50,51] or a semi-conductor [52,53], but it is by now long-established that ScN is an indirect (∼0.9\sim0.9 eV) narrow bandgap semi-conductor material [54]. Flat (heavy) bands ascribed to high effective electron/hole mass lead to enhanced Seebeck coefficients SS [55] that is negative for negatively charged carriers (electrons), and positive for positively charged carriers (holes). In contrast, highly dispersive light bands with low electronic effective mass provide higher charge carrier mobility μ\mu resulting in an increase in electrical conductivity σ\sigma (=neμ)(= ne\mu) [56]. Thus, the prominent thermoelectric power factor of ScN with metal-like resistivity ρ\rho and high SS is reflected in the underlying band structure.

The bands of V 3d3d states occur in the vicinity of EF_\mathrm{F} with strong V 3dxy3d_{xy}, 3dxz3d_{xz}, 3dyz3d_{yz} bands crossing the EF_\mathrm{F} halfway at the Γ\Gamma-point. Thus, the EF_\mathrm{F} is shifted into the CB and an overlap of the CB and VB occurs implying that V alloying drives the system to a metallic-like behavior. This reflects that electrons are the majority charge carriers here indicating nn type charge carrier concentrations. The V 3d3d states are dispersive at the Γ\Gamma-point but are flat around the X-W-K symmetry points. Thus, the light dispersive bands with band multiplicity (here valley degeneracy) indicates to an increase of σ\sigma [55–57]. Moreover, the flat band (high effective electron/hole mass) signifies that the DOSDOS distribution is localized along the X-W-K direction near to EF_\mathrm{F} and should result in high SS. [2] [10]

Compositional analysis

Table I shows the elemental composition of the reference ScN and Sc1−x_{1-x}Vx_xNy_y samples obtained from EDS and ToF-ERDA measurements. Within the error bar, the atomic % of metals (Me) match well with each other as obtained from both measurements. The reference ScN is N substoichiometry with a N/Me ratio of 0.87 with ~5% of unintentional O content. With V alloying (4-15%) in ScN, N substoichiometry results in a varying N/Me ratio from 0.81 to 0.87 within the Sc1−x_{1-x}Vx_xNy_y samples. All the Sc1−x_{1-x}Vx_xNy_y samples contain unintentional O which varies between 5.3 - 8.2 at.%. However, (N+O)/Me ratio is nearly equal to 1, indicating that the O possibly occupies the N-site in the crystal structure.

SamplesFilm compositionEDS (at. % of Me without N) (±1%)ERDA (at. %) (±1%)
ScVScVNO
N/Me ratio(N+O)/Me ratio
ScN0.87_{0.87}--50.4-43.85.00.870.97
Sc0.96_{0.96}V0.04_{0.04}N0.85_{0.85}95548.12.142.85.90.850.97
Sc0.93_{0.93}V0.07_{0.07}N0.87_{0.87}93746.73.443.65.30.870.97
Sc0.91_{0.91}V0.09_{0.09}N0.83_{0.83}891144.94.641.27.50.830.98
Sc0.88_{0.88}V0.12_{0.12}N0.86_{0.86}881243.6642.66.80.860.99
Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81}831742.77.540.68.20.810.97

Table I. Compositional details of ScN and Scx_xV1−x_{1-x}Ny_y samples obtained from EDS and ToF-ERDA. Me = metal, and the nomenclature of the samples was given by normalizing the metal site to 100% occupancy.

Structural analysis

X-ray diffraction

Figure 2(a) shows out-of-plane XRD data of the Sc1−x_{1-x}Vx_xNy_y and the ScN0.87_{0.87} reference thin film samples deposited on MgO(001) substrates, measured in the Bragg-Brentano geometry. The MgO(001) substrate provides a template for the growth of (002) and higher order (004) reflections for all the samples. Substrate 002 and 004 peaks also appear (indicated by stars at the top of Figure 2(a)) near the vicinity of the 002 and the 004 peaks of ScN0.87_{0.87}/Sc1−x_{1-x}Vx_xNy_y. No secondary phase up to the highest V alloying concentration (up to 15%) is observed indicating formation of a stable solid solution [32].

Figure 2. (a) 2θ2\theta-ω\omega X-ray diffraction patterns of reference ScN0.87_{0.87} and Sc1−x_{1-x}Vx_xNy_y thin film samples deposited on MgO(001) substrates. The stars denote the corresponding substrate peaks. (b) Bragg-Brentano short scan at χ=0∘\chi= 0^\circ along [2] and in-plane short scan at χ=45∘\chi= 45^\circ along [220] direction. (c) ϕ\phi-scans performed on (220) plane at χ=45∘\chi= 45^\circ.

Figure 2(b) shows out-of-plane and in-plane XRD data keeping the tilt angle χ=0∘\chi= 0^\circ and 45∘45^\circ, respectively, in the Bragg-Brentano geometry. In both the 002 and the 220 peaks, a shift along higher diffraction angle is observed upon increasing V content in Sc1−x_{1-x}Vx_xNy_y, indicating a decrease of lattice parameters compared to the reference ScN0.87_{0.87} sample. This observation is in accordance with our theoretical calculations along with earlier reported first principles density functional calculations [32]. By fitting the 002 and the 220 peaks by pseudo-Voigt functions, the out-of-plane (a⊥a_\perp) and in-plane (a∥a_{\parallel}) lattice parameters were evaluated and listed in Table II. For the reference ScN0.87_{0.87} sample, the a⊥a_\perp and a∥a_{\parallel} values were 4.530 Å and 4.487 Å. For the Sc1−x_{1-x}Vx_xNy_y samples, a⊥a_\perp values decrease from 4.522 Å at 4% V content to 4.484 Å at 15% V content, while the a∥a_{\parallel} values change from 4.480 - 4.445 Å (x=0.04x = 0.04-0.15). The contraction of the cell parameters (lattice parameter/volume) in Sc1−x_{1-x}Vx_xNy_y is caused by the substitution of Sc by the smaller V ion and corresponding changes in the bond strength and bond distance. All the samples have a⊥/a∥a_\perp/a_{\parallel} ratio in between 1.008 and 1.009 and reveals that the crystal structure of Sc1−x_{1-x}Vx_xNy_y samples is pseudocubic. The slight distortion in the cubic structure deviates from our theoretical crystal structure calculations and previous reports of cubic ScN in the literature [22,54]. We attribute the pseudomorphic distortion of the cubic structure is due to ≤7%\leq7\% of lattice mismatch between the samples and MgO substrate.

Figure 2c shows a φ\varphi-scan (at tilt angle χ=45∘\chi= 45^\circ, ScN0.87/Sc1−xVxNy\mathrm{ScN}_{0.87}/\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} {220}) of the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} and the reference ScN0.87\mathrm{ScN}_{0.87} samples with different alloying concentrations. Four peaks appear at 90∘90^\circ apart indicating a fourfold symmetry and confirms the epitaxial nature of all the samples. Thus, the epitaxial relationship is ScN0.87/Sc1−xVxNy\mathrm{ScN}_{0.87}/\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} (001)[100] ∥\parallel MgO(001)[100]. The average full width at half maximum (FWHM) of the diffraction peaks for ScN0.87\mathrm{ScN}_{0.87} (3.99∘3.99^\circ) is lower than for the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples where the average FWHM varies from 4.82∘4.82^\circ to 5.35∘5.35^\circ (listed in Table II). The increase in the average FWHM for the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples compared to the ScN0.87\mathrm{ScN}_{0.87} sample indicates a slightly degraded crystalline quality due to local distortions induced by V alloying in ScN.

SamplesOut-of-plane lattice parameter a⊥a_{\perp} (±0.004\pm0.004) (Å)In-plane lattice parameter a∥a_{\parallel} (±0.004\pm0.004) (Å)a⊥/a∥a_{\perp}/a_{\parallel}Volume (a∥2a⊥a_{\parallel}^{2}a_{\perp}) (Å3^{3})Average FWHM in the φ\varphi-scans (°)
ScN0.87\mathrm{ScN}_{0.87}4.5304.4871.00991.2033.99 (±0.06\pm0.06)
Sc0.96V0.04N0.85\mathrm{Sc}_{0.96}\mathrm{V}_{0.04}\mathrm{N}_{0.85}4.5224.4801.00990.7584.82 (±0.09\pm0.09)
Sc0.93V0.07N0.87\mathrm{Sc}_{0.93}\mathrm{V}_{0.07}\mathrm{N}_{0.87}4.5124.4721.00890.2344.98 (±0.20\pm0.20)
Sc0.91V0.09N0.83\mathrm{Sc}_{0.91}\mathrm{V}_{0.09}\mathrm{N}_{0.83}4.5024.4611.00989.5925.35 (±0.13\pm0.13)
Sc0.88V0.12N0.86\mathrm{Sc}_{0.88}\mathrm{V}_{0.12}\mathrm{N}_{0.86}4.4994.4541.00989.2514.93 (±0.12\pm0.12)
Sc0.85V0.15N0.81\mathrm{Sc}_{0.85}\mathrm{V}_{0.15}\mathrm{N}_{0.81}4.4844.4451.00888.5945.03 (±0.18\pm0.18)

Table II. Structural details: in-plane and out-of-plane lattice parameters of the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} and the ScN0.87\mathrm{ScN}_{0.87} samples with the corresponding volume. The average FWHM was obtained by fitting the φ\varphi-scans.

Electronic structure of Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y}

Polarization dependent X-ray Absorption Spectroscopy

Figure 3(a) and 3(b) shows polarization dependent normalized XAS data measured at the N 1s1s-edge, Sc 2p3/2,1/22p_{3/2,1/2}-edge and V 2p3/2,1/22p_{3/2,1/2}-edge of Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} and a reference ScN0.87\mathrm{ScN}_{0.87} sample. As observed in Figure 3(a), for all the samples, five prominent peaks appear at 399.8 eV, 400.6 eV (I), 402.3 eV (II), 404.9 eV (III) and 406.7 eV (IV). We assign the peak at 399.8 eV to the N 1s1s-edge due to dipole allowed N 1s→2p1s \rightarrow2p transitions (Δl=±1\Delta l = \pm1) from the core to the valence states. The features I and II are attributed to Sc 2p3/22p_{3/2} - t2gt_{2g} and Sc 2p3/22p_{3/2} - ege_g states, whereas the higher energy features III and IV are attributed to 2p1/22p_{1/2} - t2gt_{2g} and 2p1/22p_{1/2} - ege_g states, respectively. The appearance of lower energy t2gt_{2g} states and higher energy ege_g states are due to the dominating octahedral symmetry with highly directional polar-covalent ege_g (dz2d_{z^2}, dx2−y2d_{x^2-y^2}) orbitals strongly bonded to N pzp_z orbitals forming σ\sigma-type bonds and metallic non-directional t2gt_{2g} (dxyd_{xy}, dxzd_{xz}, dyzd_{yz}) orbitals forming π\pi-type bonds with the N pxp_x and the pyp_y orbitals [59]. Due to the crystal field splitting (10Dq10Dq), both 2p3/22p_{3/2} and 2p1/22p_{1/2} peaks further split into t2gt_{2g} (Sc 2p3/2→2p_{3/2}\rightarrowSc 3d3d +N 2pπ2p\pi) and ege_g (Sc 2p1/2→2p_{1/2}\rightarrowSc 3d3d +N 2pσ2p\sigma) peaks. The observed spin-orbit and crystal-field splitting are ∼\sim4.2 and ∼\sim1.7 eV, respectively [60,61]. The crystal field splitting directly scales with the bond length [62], and a larger crystal field splitting indicates stronger Sc 3d3d - N 2p2p bonding in the material. The extent of the crystal-field splitting depends on the coordination environment of the N ligands around the Sc ions in the crystal structure. The crystal field splitting [∝\propto (bond distance)−5^{-5}] appears to be rather constant within the energy resolution for the V alloying concentrations and does not increase with decrease in the lattice parameters.

Figure 3. Polarization-dependent X-ray absorption measurements at the N 1s1s-edge and the Sc 2p3/2,1/22p_{3/2,1/2}-edge (a) and the V 2p3/2,1/22p_{3/2,1/2}-edge (b) of the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} and the ScN0.87\mathrm{ScN}_{0.87} thin film samples. The data were normalized below and above each absorption edge.

In addition to a previous publication [60], we observe a distinct N 1s1s-edge feature in the XAS spectra (see Figure 3(a)). The appearance of the distinct N 1s1s-edge appears at the lower photon energy due to higher charge transfer to N ion from V and/or Sc ions compared to the absorption edge expected for a neutral N atom. It is noteworthy that in Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples, an additional feature appears at around 399.2 eV. We attribute this feature to N vacancy and unintentional O induced localized Sc 3d3d t2g∗t_{2g}^{*} defect states. The polarization dependent XAS studies at the N 1s1s and the Sc 2p3/2,1/22p_{3/2,1/2} edges indicate distinguishable intensity variations along horizontal and vertical polarizations only at the Sc 2p3/2,1/22p_{3/2,1/2}-edge for Sc0.85V0.15N0.81\mathrm{Sc}_{0.85}\mathrm{V}_{0.15}\mathrm{N}_{0.81}. The anisotropic contribution for the Sc0.85V0.15N0.81\mathrm{Sc}_{0.85}\mathrm{V}_{0.15}\mathrm{N}_{0.81} sample corresponds to antibonding π\pi and σ\sigma-type orbitals due to distortion of the octahedral symmetry with different Sc-N bond distances in different crystallographic directions. The absence of intensity variation across the N 1s1s-edge for the same sample is an indication of an isotropic distribution of N-N bonding.

The line shapes of the V 2p3/2,1/22p_{3/2,1/2}-edge absorption in Figure 3(b) are less prominent than for a 100% occupancy of V at the metal site due to the low alloying concentration (x=0.04x = 0.04-0.15) in the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples. The doublet features around 515-516 eV, and 521-523 eV are attributed to the spin-orbit splitting of the 2p3/22p_{3/2} and 2p1/22p_{1/2}-edges with a t2gt_{2g} - ege_g sub splitting of ∼2\sim2 eV. The polarization dependent XAS at V 2p3/2,1/22p_{3/2,1/2}-edges also exhibits variable intensity distribution between the horizontal and the vertical polarizations. Unlike the Sc 2p3/2,1/22p_{3/2,1/2}-edge, the anisotropic contribution is pronounced from the lowest up to the highest V alloying concentration for all the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples. This suggests that the V-V and V-N bonding is less uniformly ordered and more randomly distributed.

Density of states calculations and Valence Band Spectroscopy

Figure 4(a) and 4(b) shows the total and partial density of states (DOS) of Sc0.75_{0.75}V0.25_{0.25}N in comparison to ScN. For comparison, experimental valence band spectra (VBS) of Sc1−x_{1-x}Vx_xNy_y thin films and of a reference ScN0.87_{0.87} sample are shown in Figure 4(c), while Figure 4(d) shows a magnification of the total DOS for all the samples in the vicinity of the Fermi level (EF_F). Due to the final state lifetime broadening and instrumental energy resolution, the experimental VBS occurs broader compared to the calculated DOS (see Figure 4(a) and 4(b)). For the ScN0.87_{0.87} reference sample in Figure 4(c), there are no states observed at the EF_F even for a sample containing N vacancies or O substitution. According to a previous report estimated from the theoretical calculations that combination of N vacancies and O substitution push the EF_F into the conduction band [20]. Thus, our observation suggests appearance of no additional defect states with the added electrons from O at EF_F around the valence band. An increasing V content in Sc1−x_{1-x}Vx_xNy_y results in a gradual increase of intensity in the vicinity of the EF_F (see Figure 4(c)). This can be understood as due to the contribution from two additional valence electrons from each V atom compared to ScN. The additional electrons from V drive the Sc1−x_{1-x}Vx_xNy_y system towards a metallic-type of bonding. Since our samples contain finite amount of O, the contribution of O 2p states in the VBS spectra is discussed with the theoretical calculations in section 4 of the SI. However, no contribution from O appears at/near the EFE_{\mathrm{F}}. Comparing the VBS data of ScN0.87\mathrm{ScN}_{0.87} with the DOS calculations, feature A and shoulder B are dominated by hybridization of N 2p states with Sc 3d states. Partial contribution from Sc 3p states at feature A and Sc 3s states at feature B can also be identified. The higher binding energy (EbE_{\mathrm{b}}) feature C is mostly dominated by N 2s states with partial contribution from Sc 3d and 3p states.

Figure 4. The total and partial-density of states (DOS) of (a) ScN and (b) Sc0.75_{0.75}V0.25_{0.25}N calculated by DFT. (c) Valence band spectra of the Sc1−x_{1-x}Vx_xNy_y and the reference ScN0.87_{0.87} thin film samples with different alloying concentrations. (d) A magnified view of the states near the Fermi level (EF_F) in the VBS spectra measured by XPS.

For the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples, feature A and B are due to hybridization of Sc 3d and N 2p states with partial contribution from V 3d states. Minor contribution from V states can also be observed for the higher EbE_{\mathrm{b}} energy feature C apart from the main hybridizations which are similar to those of ScN0.87\mathrm{ScN}_{0.87}. The shape of the VBS spectra remains similar while there is an increase in the intensity compared to ScN0.87\mathrm{ScN}_{0.87} that can be attributed to the presence of two additional valence electrons in V compared to Sc. For Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y}, the calculated DOS across EFE_{\mathrm{F}} is dominated by V 3d states with a low contribution from Sc 3d and N 2p states.

Resonant Inelastic X-ray Scattering

Figure 5(a) shows Sc L3,2L_{3,2} and N K-RIXS data of the Sc1−x_{1-x}Vx_xNy_y thin film samples compared to ScN0.87_{0.87}. The spectra were excited at 397.8 eV, 399.9 eV, 400.7 eV, 402.4 eV and 430 eV (non-resonant) photon energies, respectively. XAS data (top right) at the N 1s1s-edge and Sc 2p2p-edges were used to determine the absorption peak maxima used for the RIXS measurements.

Figure 5. (a) Combined Sc LL and N KK-RIXS data for excitation energies 397.8 eV, 399.9 eV, 400.7 eV, 402.4 eV and 430 eV (non-resonant), respectively, and Sc 2p-edge and N 1s-edge XAS data (top right), (b) V LL RIXS for excitation energies of 510.8 eV, 514.5 eV, 517 eV, 521.6 eV and 560 eV (non-resonant), respectively, and V 2p-edge XAS (top right) of Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} thin film samples compared to of ScN0.87\mathrm{ScN}_{0.87}. The excitation energies for the normalized RIXS data are marked by the vertical bars in the XAS data.

Starting with the excitation energy of 397.8 eV, the main emission peak at 391.1 eV appears for all the samples due to N 2p→1s2p\mathbin{\to}1s dipole transitions (Δl=±1\Delta l = \pm1). Thus, the emission spectra are dominated by N 2p2p states, and the intensity variation depends on the difference in N content between the samples. Generally, the peak structures of the ScN0.87_{0.87} reference sample are consistent with a previous publication, where the main peak is accompanied by a shoulder peak at ~389.2 eV [61] and the same trend is observed for the Sc1−x_{1-x}Vx_xNy_y samples. This is attributed to the strong Sc 3d3d – N 2p2p hybridization. A weak emission feature at around 394.3 eV occurs due to the Sc L3L_3 (Sc 3d4s→2p3/23d4s\mathbin{\to}2p_{3/2}) emission line.

As the photon energy is increased to 399.9 eV corresponding to N 1s→2p1s\mathbin{\to}2p absorption in the XAS, a doublet feature appears at around 399-400 eV in addition to the main emission peak at 391.1 eV and Sc L3L_3 emission. In the doublet, the highest energy peak at 399.9 eV corresponds to elastic Rayleigh scattering and the lower energy peak at 399.2 eV is due to resonance with the N 1s1s XAS resulting in the appearance of N 2p2p states hybridized with Sc 3d3d states. As the photon energy is further raised to 400.7 eV, corresponding to the Sc 2p3/22p_{3/2}-t2gt_{2g} peak in XAS, the elastic Rayleigh scattering peak appears at 400.7 eV in addition to the main emission peak at 391.1 eV and Sc L3L_3 emission. As the photon energy is further raised to 402.4 eV, the elastic peak becomes significantly stronger. Strong Rayleigh scattering is a signature of localized electron excitations in narrow band systems that is normally observed in highly correlated rare earth systems [63] and corroborates to the covalent bonding for L3L_3-eg∗e_g^* states. For comparison, the relatively weak elastic peaks corresponding to L3L_3-t2g∗t_{2g}^* signifies delocalization that should affect the electrical conductivity. At non-resonant emission of 430 eV excitation energy, only the N 2p2p and Sc L3L_3 emission lines are observed with no additional features.

Figure 5(b) shows V LL RIXS for excitation energies of 510.8 eV, 514.5 eV, 517.0 eV, 521.6 eV and 560.0 eV (non-resonant), respectively, at the V 2p2p absorption edge (top right). For the pre-peak excitation, the emission is very weak while at 514.5 eV corresponding to the 2p3/22p_{3/2}-t2gt_{2g} excitation energy, three broad features are observed. The highest energy feature at 514.5 eV corresponds to elastic Rayleigh scattering while the strong doublet is due to L3L_3-t2gt_{2g} and L3L_3-ege_g having a crystal field splitting of 3.7 eV. As the energy is raised to 517.0 eV, corresponding to the 2p3/22p_{3/2}-ege_g excitation energy, the double peak is less pronounced. As the excitation energy is raised to 521.6 eV corresponding to the V 2p1/22p_{1/2} shell, four distinct features appear where the lower energy doublet corresponds to L3L_3-t2gt_{2g} and L3L_3-ege_g and the higher energy doublet are L2L_2-t2gt_{2g} and L2L_2-ege_g due to V 3d4s→2p3/2,p1/23d4s\mathbin{\to}2p_{3/2},p_{1/2} dipole allowed transitions. Moreover, due to excitation at the V L2L_2 absorption edge, the V L2L_2 features are more intense compared to the V L3L_3 features. The gradual increase in intensity from Sc0.96_{0.96}V0.04_{0.04}N0.85_{0.85} to Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81} at 514.5 eV, 517 eV, and at 521.6 eV excitation energies is associated with the increasing alloying concentration of V. Finally, at non-resonant excitation at 560.0 eV, the spectra become dominated by the O KK emission at 523 eV. However, weak O KK emission is present in all three 514.5, 517 and 521.6 eV emission energies. This further depicts that our samples have a finite amount of oxygen as was confirmed from the ERDA measurements mentioned in § 3.2.

Electrical properties

SamplesSS (μ\muV K−1^{-1})ρ\rho (μΩ\mu\Omegacm)S2σS^{2}\sigma (μ\muW cm−1^{-1} K−2^{-2})nn (cm−3^{-3})μ\mu (cm2^{2} V−1^{-1} s−1^{-1})
ScN0.87_{0.87}−21±7-21 \pm71403.15−2.7×1021-2.7 \times10^{21}16.51
Sc0.96_{0.96}V0.04_{0.04}N0.85_{0.85}−7±6-7 \pm610400.047−2.85×1021-2.85 \times10^{21}2.11
Sc0.93_{0.93}V0.07_{0.07}N0.87_{0.87}−4±7-4 \pm715200.011−3.86×1021-3.86 \times10^{21}1.1
Sc0.91_{0.91}V0.09_{0.09}N0.83_{0.83}−5±7-5 \pm726700.009−3.67×1021-3.67 \times10^{21}0.63
Sc0.88_{0.88}V0.12_{0.12}N0.86_{0.86}−1±4-1 \pm422700.0004−3.53×1021-3.53 \times10^{21}0.78
Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81}10±410 \pm430100.0338.83×10218.83 \times10^{21}2.35

Table II (PDF p. 14). Seebeck coefficient (SS), electrical resistivity (ρ\rho), power factor (S2σS^{2}\sigma), charge carrier concentration (nn) and charge carrier mobility (μ\mu) of the reference ScN0.87_{0.87} and Sc1−x_{1-x}Vx_xNy_y samples at room temperature.

Electrical properties (Seebeck coefficient, electrical resistivity, power factor, charge carrier concentration and carrier mobility) studied at room temperature are tabulated in Table II. The reference ScN0.87_{0.87} shows electron-dominated charge transport with S∼−21S \sim-21 μ\muV K−1^{-1} which is in close agreement with available reports [64]. With V increase in Sc1−x_{1-x}Vx_xNy_y up to x=0.12x = 0.12, Seebeck coefficient remains negative with their absolute values decreasing towards zero. For the highest V containing Sc1−x_{1-x}Vx_xNy_y with x=0.15x = 0.15, the measured Seebeck coefficient changes to positive with a value around +10+10 μ\muV K−1^{-1}. The electrical resistivity values of Sc1−x_{1-x}Vx_xNy_y samples increases gradually from 1040 to 3010 μΩ\mu\Omegacm with increase in alloying concentration from x=0.04x = 0.04 to 0.12, an order of magnitude higher than 140 μΩ\mu\Omegacm for the reference ScN0.87_{0.87} sample. The absolute values of the charge carrier concentration remain nearly the same at (2.7−2.85)×1021(2.7 - 2.85) \times10^{21} cm−3^{-3} for reference ScN0.87_{0.87} and Sc1−x_{1-x}Vx_xNy_y with x=0.04x = 0.04. A slight increase in the carrier concentration is observed with higher V content and the values nearly remain the same within (3.53−3.86)×1021(3.53 - 3.86) \times10^{21} cm−3^{-3} for Sc1−x_{1-x}Vx_xNy_y with x=0.07−0.12x = 0.07 - 0.12. For Sc1−x_{1-x}Vx_xNy_y up to x=0.12x = 0.12 including the reference ScN0.87_{0.87}, the carrier concentration value is negative. For the highest V content (x=0.15x = 0.15), there is at least two times increase in the carrier concentration with a positive value of 8.83×10218.83 \times10^{21} cm−3^{-3}. Simultaneously, there is an abrupt decrease of the charge carrier mobility (2.35−0.78(2.35 - 0.78 cm2^{2} V−1^{-1} s−1^{-1}) for Sc1−x_{1-x}Vx_xNy_y compared to reference ScN0.87_{0.87} (16.51 cm2^{2} V−1^{-1} s−1^{-1}). The increase in ρ\rho with V content might be due to increased local disorder which is reflected as reduction in carrier mobilities as well. The combined effect of reduced SS and increased ρ\rho, results in an overall decrease in S2σS^{2}\sigma from 3.15 μ\muW cm−1^{-1} K−2^{-2} for reference ScN0.87_{0.87} to a range of 0.047-0.0004 μ\muW cm−1^{-1} K−2^{-2} for Sc1−x_{1-x}Vx_xNy_y samples.

Discussion

The GGA+U (U = 3.5 eV) calculations reveal that ScN exhibits a relaxed lattice parameter of 4.518 Å with cubic B1 NaCl structure (see Figure 1(c)). Substitution of 1 Sc atom by V in the unit cell of ScN (i.e., 3 Sc atoms, 1 V atom and 4 N atoms) still retains the rocksalt B1 structure (see Figure 1(d)) with a reduction in the lattice parameter to 4.410 Å in relaxed state. Due to two additional valence electrons of V compared to Sc, the electron concentration of the Sc0.75_{0.75}V0.25_{0.25}N system is expected to be higher, contributing higher DOS across the EF_F and thus higher electrical conductivity compared to ScN.

Band structures and crystal structures of ScN and Sc₀.₇₅V₀.₂₅N

Figure 1. Band structures and crystal structures of ScN (a and c) and Sc0.75_{0.75}V0.25_{0.25}N (b and d) in the cubic rocksalt structure at equilibrium volume. The symmetry points are located at Γ(0,0,0)\Gamma(0,0,0), X(0.5,0,0.5), W(0.5,0.25,0.5), L(0.5,0.5,0.5) and K(0.375,0.375,0.375).

For the Sc0.75_{0.75}V0.25_{0.25}N system (Figure 1(b)), the EF_F shifts into the CB and an overlap of the CB and VB occurs at Γ\Gamma-point. This is different from the direct (Γ\Gamma-Γ\Gamma and X-X symmetry points) and the indirect (Γ\Gamma-X) bandgaps observed for ScN (see Figure 1(a)). The main contribution in the vicinity of the EF_\mathrm{F} originates from V 3dxy3d_{xy}, 3dxz3d_{xz}, 3dyz3d_{yz} bands crossing the EF_\mathrm{F} halfway at the Γ\Gamma-point. The V 3d3d states are dispersive at the Γ\Gamma-point with band multiplicity indicating towards achieving higher σ\sigma and a simultaneous occurrence of flat bands along the X-W-K direction insights for inducing higher SS compared to ScN. Thus, the Sc1−x_{1-x}Vx_xN system shows promise as an efficient thermoelectric material compared to ScN. However, we limited the alloying concentration of V to up to 15% in experiments (and not 25% as calculated theoretically). The reason is to take into consideration the effects of induced defects during the non-equilibrium sputtering process which could not be neglected. The N vacancies and incorporation of unintentional O are especially thermodynamically favorable in the ScN system [20,65]. Thus, the increase in induced defects with increasing alloying concentration in principle could lead to an adverse effect on the thermoelectric properties.

This is supported by a series of Sc1−x_{1-x}Vx_xNy_y (x=0.04x = 0.04-0.15) thin film samples and reference ScN film with N vacancies deposited on MgO(001) substrates. Compositional analysis showed that all the samples were N deficient (y=0.81y = 0.81-0.87) with presence of unintentional O (5 to 8.2 at. %) across the N-site. The origin of O incorporation could be the adaptation of high substrate temperature leading to higher amount of degassing within the chamber and/or air exposure post deposition. It is to be noted that the waiting time to minimize the degassing effect was around 30 mins with an achieved base pressure of ≤1.3×10−6\leq1.3 \times10^{-6} Pa (9.6×10−99.6 \times10^{-9} Torr) prior to the depositions. From the XRD measurements, no additional phases were observed for Sc1−x_{1-x}Vx_xNy_y samples exhibiting epitaxial nature as observed from the ϕ\phi-scans (see Figure 2(c)). The in-plane and out-of-plane XRD revealed that all the samples exhibited slight distortion in the cubic structure with an elongation along the cc-axis.

The XAS data reveals presence of localized Sc 3d3d t2gt_{2g} states in Sc1−x_{1-x}Vx_xNy_y induced due to N vacancies and presence of unintentional O which is the most stable defect configuration in ScN system [66]. However, the defect states in reference ScN0.87_{0.87} cannot be separated out from the N KK-edge. The presence of N vacancies results in excess valence electrons along the metal site (Sc+V) which remains unbounded. However, presence of more electronegative O (along with N at the non-metal site) than N can accommodate two valence electrons/atom but O itself also has an additional valence electron than N. Therefore, an excess of electrons should result in lifting the Fermi level to the conduction band as indicated by theoretical band structure calculations [20]. In comparison to a previous study [60], we found a distinct N 1s1s-edge for the reference ScN0.87_{0.87} sample in XAS (Figure 3(a)) and similar observations were also found for the Sc1−x_{1-x}Vx_xNy_y samples. The appearance of a distinct N 1s1s-edge is expected at the lower photon energy due to higher charge transfer to the N ions from V and/or Sc ions compared to the absorption edge expected for neutral N atoms.

Note that our XRD results show pseudocubic crystal structures for all the samples but polarization dependent XAS reveals the independent contribution of the bonding anisotropy. The polarization dependent XAS study revealed a small distortion of the octahedral symmetry for the highest alloying Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81} sample at the Sc 2p3/2,1/22p_{3/2,1/2}-edge due to variable intensity distribution in horizontal and vertical polarization (Figure 3(a)). However, at the V 2p3/2,1/22p_{3/2,1/2}-edge, distinguishable intensity distribution in both the polarization states was found for the lowest V alloying concentration (see Figure 3(b)). These observations signify different Sc-N bond lengths for Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81} only, while all the V alloyed samples had variable V-V and V-N bond distances along the xx, yy, and zz directions. On the contrary, the distribution of N-N bonds appeared to be isotropic. The difference between the two polarizations (vertical and horizontal) indicates that there may be not only N 2p2p states but also some contribution of O 2p2p states bonding to the 3d3d states of the Sc and V atoms as ligands. This results in slight local distortion of the octahedral symmetry. Thus, we infer that the distortion in the cubic structure of the Sc1−x_{1-x}Vx_xNy_y samples is primarily due to anisotropic V-N and V-V bonds. However, for the highest V alloying concentration, the anisotropic Sc-N bonds also contribute to the distortion in the octahedral symmetry.

The combined VBS results (Figure 4) and DOS calculations show that all the Sc1−x_{1-x}Vx_xNy_y samples have finite density of states across the EF_\mathrm{F}. This population is dominated by V 3d3d states with a minor contribution from Sc 3d3d and N and O 2p2p states. No states are observed for reference ScN0.87_{0.87} from VBS. This is noteworthy, because one might expect features near EF_\mathrm{F} and indicates that the added electrons from O do not add features of a finite DOS at EF_\mathrm{F}. Nevertheless, it has been indicated in literature that Sc vacancies accompanied with substitutional oxygen is a stable defect [66]. These defects push EF_\mathrm{F} inside the conduction band resulting in finite DOS contribution [20]. The appearance of weak elastic Rayleigh scattering peaks (Figure 5a) corresponding to L3L_3-t2g∗t_{2g}^{*} at resonant photon energies of 399.9 eV and 400.7 eV are noted. This signifies delocalization of the Sc1−x_{1-x}Vx_xNy_y and reference ScN0.87_{0.87} systems, indicating contribution of free mobile charge carriers for the electrical conductivity. Indeed, at 399.9 eV, the intensity of ScN0.87_{0.87} is lower compared to Sc1−x_{1-x}Vx_xNy_y samples signifying higher conductivity of ScN0.87_{0.87} compared to Sc1−x_{1-x}Vx_xNy_y. In contrast, at 402.4 eV resonant energy, the strong Rayleigh scattering is a signature of localized electron excitations corroborating to the covalent bonding for L3L_3-eg∗e_g^{*} states. The covalent bonding weakens with higher V alloying. The increase of intensity of the V 2p2p emission lines at 514.5, 517 and 521.6 eV excitation energies with higher V alloying (Figure 5b) further confirms consistent results with the EDS and the ERDA results. The presence of O is also observed at non-resonant 560 eV photon energy in-line with our compositional analysis.

The transport properties of ScN are highly susceptible to the presence of point defects such as vacancies (Sc and N), interstitials (N) and substitutional defects (O). The electrical resistivity and Seebeck coefficient (hold for metals and degenerate semiconductors) are related to the carrier concentration (here for electrons nn but the relations hold for holes pp as well) as [3] [67],

ρ=1neμ\rho= \frac{1}{ne\mu}

and,

S=8π2kB2T3eh2m∗(π3n)2/3S = \frac{8\pi^{2} k_{\mathrm{B}}^{2}T}{3eh^{2}}m^{*}\left(\frac{\pi}{3n}\right)^{2/3}

where, the contribution from majority (electrons/holes) and minority (holes/electrons) charge carriers are [67],

S=Snσn+Spσpσn+σpS = \frac{S_{n}\sigma_{n} + S_{p}\sigma_{p}}{\sigma_{n} + \sigma_{p}}

and the subscripts represent the type of charge carriers (n: electrons, p: holes). Here, kBk_{\mathrm{B}} = Boltzmann’s constant, ee = electronic charge, hh = Planck’s constant, and m∗m^{*} = effective mass of the charge carrier at an absolute temperature TT. Based on the Mahan-Sofo theory, the DOS is associated with the effective mass as [2] [68],

DOS(E)=(md∗)3/22Eℏ3π2DOS(E) = \frac{(m_d^*)^{3/2}\sqrt{2E}}{\hbar^3\pi^2}

Further, it is to be noted here that although charge carriers exhibiting higher effective mass will have lower mobility but it also depends on several other factors like scattering, electronic structure and anisotropy behavior of the crystal system [3].

For Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_x\mathrm{N}_y samples, up to x=0.12x = 0.12, a reduction is observed in the absolute SS values compared to ScN0.87\mathrm{ScN}_{0.87} by an order of magnitude, the values typical for metals [69]. It is worth noting that the charge carrier concentration remains relatively constant for x=0.04x = 0.04 and reference ScN0.87\mathrm{ScN}_{0.87} to x=0.07x = 0.07 - 0.120.12 to x=0.15x = 0.15 suggests a dominant role of the charge carrier mobility to their contribution in the Seebeck values. Although the SS values for Sc0.91V0.09N0.83\mathrm{Sc}_{0.91}\mathrm{V}_{0.09}\mathrm{N}_{0.83} and Sc0.88V0.12N0.86\mathrm{Sc}_{0.88}\mathrm{V}_{0.12}\mathrm{N}_{0.86} samples are at the borderline between positive and negative considering the error bars, the sign of the carrier concentration confirms that the majority charge carriers are electrons for these samples. Later interestingly the charge transport becomes hole-dominated for the highest V content (Sc0.85V0.15N0.81\mathrm{Sc}_{0.85}\mathrm{V}_{0.15}\mathrm{N}_{0.81}). The observed acceptor nature can be attributed to possible Sc vacancies depending on the defect chemistry of ScN having Sc vacancies of acceptor nature while N vacancies and interstitials are triple and single donors, respectively [65].

The obtained charge carrier concentration of ∼1021 cm−3\sim10^{21}\ \mathrm{cm}^{-3} is typical for metals and heavily doped semiconductors [3]. Since in our VBS results we observed an increase in DOS across EFE_{\mathrm{F}} for Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_x\mathrm{N}_y samples compared to ScN0.87\mathrm{ScN}_{0.87}, it suggests a heavier effective mass of electrons in V alloying samples. This reflects in decrease of carrier mobility from an order to even two orders of magnitude lower compared to ScN0.87\mathrm{ScN}_{0.87}. This could be attributed to the presence of defect concentrations such as Sc and N vacancies, V alloying and unintentional O across the non-metal site. Each of them behaves as scattering centers for the electrons which reflects not only in the lowering of the charge carrier mobility but also to an increase in the overall resistivity of the samples by at least an order of magnitude higher compared to ScN0.87\mathrm{ScN}_{0.87}. Consequently, a reduction in the thermoelectric power factor has been observed.

For the highest alloying sample Sc0.85V0.15N0.81\mathrm{Sc}_{0.85}\mathrm{V}_{0.15}\mathrm{N}_{0.81}, holes instead contribute as the majority charge carriers, as indicated by the positive Seebeck coefficient in this sample. From the Hall measurements, the carrier concentration was found to be at least two times higher, and the mobility increased by an order of magnitude compared to the second highest alloying sample Sc0.88V0.12N0.86\mathrm{Sc}_{0.88}\mathrm{V}_{0.12}\mathrm{N}_{0.86}. It was also reflected in an increase of the electrical resistivity for this sample. Essentially the nn to pp type switching here is driven by lower concentration of less mobile electrons which stems from the highest N and Sc vacancies incorporated by O and V along the non-metal and metal site.

Conclusions

In conclusion, the electronic structure of epitaxial Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_x\mathrm{N}_y films with different alloying concentrations of V were investigated. All samples exhibit N substoichiometry with unintentional presence of O along the non-metal site suggesting N substitution. The lattice parameter gradually reduces compared to reference ScN0.87\mathrm{ScN}_{0.87} obeying Vegard’s law. Up to the highest alloying concentration, the Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_x\mathrm{N}_y samples retain a NaCl structure. However, the N–N bond length is symmetrically distributed in the 3D co-ordinate but an asymmetry in the Sc–N bond length is observed for the highest V content (x=0.15x = 0.15). On the contrary, the V–N and V–N bond lengths vary randomly in all the three-coordinate axis. Moreover, N induced Sc 3d t2g∗3d\ t_{2g}^{*} states were observed for the first time experimentally from the Sc 2p2p XAS, in line with the earlier theoretical reports. Band structure calculations demonstrate that for Sc0.75_{0.75}V0.25_{0.25}N an overlap of the conduction and valence band occurs, and the Fermi level lies in the conduction band. Thus, the system is driven to metal-like behavior from semiconducting ScN. The presence of light (dispersive) bands at Γ\Gamma-point with band multiplicity leads to higher electrical conductivity and flat (heavy) bands at X-W-K symmetry points signify higher Seebeck coefficient than ScN demonstrating the potential as a thermoelectric material. Moreover, finite density of states crossing the Fermi level in Sc1−x_{1-x}Vx_xNy_y is due to contribution from V 3d3d states. However, experimentally we observed an increase in the electrical resistivity accompanied with a decrease in the negative Seebeck coefficient. The Hall measurements confirm the reduced charge carrier mobility due to higher scattering by defects to be the primary reason for such a decrease in the thermoelectric power factor. In addition, the mobility reduces so much that instead of the electrons, holes become the majority charge carriers for the highest V alloying sample.

Acknowledgements

The authors acknowledge funding from the Swedish Government Strategic Research Area in Materials Science on Functional Materials at Linköping University (Faculty Grant SFO-Mat-LiU No. 2009 00971), the Knut and Alice Wallenberg foundation through the Wallenberg Academy Fellows program (KAW-2020.0196), the Swedish Research Council (VR) under Project No. 2021-03826. SC acknowledges Victor Hjort for his help during depositions. M.M. also acknowledges financial support from the Swedish Energy Agency (Grant No. 43606-1) and the Carl Tryggers Foundation (CTS23:2746, CTS20:272, CTS16:303, CTS14:310). GG acknowledges the Swedish Energy Agency project 51201-1, the Åforsk Foundation Grant 22-4, and the Olle Enqvist foundation grant 222-0053.

Research conducted at MAX IV, a Swedish national user facility, is supported by the Swedish Research council under contract 2018-07152, the Swedish Governmental Agency for Innovation Systems under contract 2018-04969, and Formas under contract 2019-02496. Anirudha Ghosh and Conny Såthe from SPECIES beamline, MAX IV, Lund, Sweden is acknowledged for the help during the XAS and RIXS measurements. The FEFF calculations were enabled by resources provided by the National Academic Infrastructure for Supercomputing in Sweden (NAISS) at Linköping University, partially funded by the Swedish Research Council through grant agreement no. 2022-06725. Daniel Primetzhofer from Uppsala University is acknowledged for Accelerator operation supported by Swedish Research Council VR-RFI (Contract No. 2019-00191) and the Swedish Foundation for Strategic Research (Contract No. RIF14-0053).

References

Electronic structure and thermoelectric properties of epitaxial Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} thin films grown on MgO(001)\mathrm{MgO}(001)

Susmita Chowdhury; Niraj Kumar Singh; Sanath Kumar Honnali; Grzegorz Greczynski; Per Eklund; Arnaud le Febvrier; Martin Magnuson

Rutherford Backscattering Spectrometry (RBS)

The ERDA results indicate qualitatively about the presence of a heavier element than Sc and V in Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples and reference ScN0.87\mathrm{ScN}_{0.87}. Therefore, Rutherford backscattering spectrometry (RBS) measurements were performed on all the samples to quantify the trace of heavy element contamination observed in ERDA. The RBS measurements were conducted with 2 MeV He+\mathrm{He}^{+} primary ions incident at 5° to the sample surface normal and the resulting spectra was analyzed using the SIMNRA 7.03 software [1]. From fitting of the experimental data (not shown here), a trace amount of Hf was found to be present in all the samples with ≈0.1 atomic %.

X-ray Reflectivity (XRR)

Figure S1 shows the X-ray reflectivity (XRR) of reference ScN0.87\mathrm{ScN}_{0.87} and Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} thin film samples deposited on MgO(001)\mathrm{MgO}(001) substrates. The measurements were performed using PANalytical X’Pert Pro diffractometer equipped with Cu-Kα\alpha source. The fitting of the XRR spectra were performed using Parratt 32 software based on Parrat’s formalism [2] to obtain the thickness and real part of the scattering length density (real SLD) of the samples. The real SLD (α\alpha) is related to the critical momentum transfer vector qc=4πsin⁡θc/λq_{\mathrm{c}} = 4\pi\sin\theta_{\mathrm{c}}/\lambda where, θc=(λ2α/π)1/2\theta_{\mathrm{c}} = (\lambda^{2}\alpha/\pi)^{1/2}. Here, θc\theta_{\mathrm{c}} = critical angle, λ\lambda = wavelength of X-rays. α\alpha is related to the mass density (dd) as, d=αM/NAreZd = \alpha M/N_{\mathrm{A}}r_{\mathrm{e}}Z where, MM is molar mass, NAN_{\mathrm{A}} is Avogadro’s number (6.023×10236.023\times10^{23} mol−1^{-1}), ZZ is atomic number and rer_{\mathrm{e}} is classical electron radius (2.818 fm) [3]. The fitting parameters are tabulated in Table S1. The sample thickness of reference ScN0.87\mathrm{ScN}_{0.87} is ~129 nm while it varies between ~125 to 130 nm for Sc1−xVxNy\mathrm{Sc}_{1-x}\mathrm{V}_{x}\mathrm{N}_{y} samples. With V alloying, there is a gradual increase in real SLD which is expected as V has higher mass density than Sc.

Figure S1. XRR spectra of reference ScN0.87_{0.87} and Sc1−x_{1-x}Vx_xNy_y thin film samples with different alloying concentrations.

SamplesXRR analysis
Thickness (nm)Real SLD (±0.02×10−5\pm0.02 \times10^{-5}) (Å−2^{-2})
ScN0.87_{0.87}129 ±\pm 23.62×10−53.62 \times10^{-5}
Sc0.96_{0.96}V0.04_{0.04}N0.85_{0.85}130 ±\pm 23.70×10−53.70 \times10^{-5}
Sc0.93_{0.93}V0.07_{0.07}N0.87_{0.87}129 ±\pm 63.70×10−53.70 \times10^{-5}
Sc0.91_{0.91}V0.09_{0.09}N0.83_{0.83}129 ±\pm 23.72×10−53.72 \times10^{-5}
Sc0.88_{0.88}V0.12_{0.12}N0.86_{0.86}125 ±\pm 23.74×10−53.74 \times10^{-5}
Sc0.85_{0.85}V0.15_{0.15}N0.81_{0.81}126 ±\pm 23.78×10−53.78 \times10^{-5}

Table S1. The thickness and real part of the scattering length density (SLD) of the thin film samples obtained from fitting of the XRR spectra.

Core level X-ray Photoelectron Spectroscopy (XPS)

Figure S2 shows the Sc 2p2p, N 1s1s and V 2p2p, O 1s1s XPS core level spectra normalized to the highest intensity. For the reference ScN0.87_{0.87} sample (see Figure S2), the N 1s1s peaks at around 396.4 eV and due to spin split doublet peaks Sc 2p3/22p_{3/2} (~400.8 eV) and Sc 2p1/22p_{1/2} (~405.2 eV) appears for Sc. The Sc 2p1/22p_{1/2} is more broadened compared to Sc 2p3/22p_{3/2} due to the Coster-Kroning effect [4]. The spin orbit splitting of ~4.4 eV is same as obtained in XAS within the instrumental resolution. An asymmetry at lower BE side is observed around both Sc 2p3/22p_{3/2} and Sc 2p1/22p_{1/2}. This can be attributed to the finite presence of Sc-O-Nx_x/Sc-O in addition to Sc-N bonding. For Sc1−x_{1-x}Vx_xNy_y, the contribution of Sc-O-Nx_x/Sc-O bonding is more pronounced around the Sc 2p3/22p_{3/2} and Sc 2p1/22p_{1/2} spectra. An interplay between the intensities around D, E, F and G is noted. Initially for reference ScN0.87_{0.87}, the features D and F were intense. However, with increase in alloying concentration of V, the features E and G become more intense. No visible shift around N 1s1s is observed for Sc1−x_{1-x}Vx_xNy_y samples compared to reference ScN0.87_{0.87} except the sample with x=0.09x = 0.09. An asymmetry noted in all the samples around the lower BE of N 1s1s is assigned to the presence of ScOx_xNy_y bonds [5].

Figure S2. XPS core level spectra of Sc 2p2p and N 1s1s (a) and V 2p2p (b) of reference ScN0.87_{0.87} and Sc1−x_{1-x}Vx_xNy_y thin film samples with different alloying concentrations.

Figure S2 shows doublet V 2p3/22p_{3/2} and V 2p1/22p_{1/2} due to spin split (~7.6 eV) in Sc1−x_{1-x}Vx_xNy_y samples. The broadening and asymmetry in V 2p2p core level spectrum is resultant of the multiplet effect due to unpaired electrons in Vδ+^{\delta+} state [6, 7]. No significant shift in the V 2p2p spectra can be noted for all the Sc1−x_{1-x}Vx_xNy_y samples. The O 1s1s core level spectra shows no visible peak shift within Sc1−x_{1-x}Vx_xNy_y samples and reference ScN0.87_{0.87} suggesting no change in the oxidation state of O.

Theoretical DOS with N vacancy and O

Figure S3 shows the theoretical DOS including N vacancies and O in the unit cell of ScN (see Figure S3) and Sc1−x_{1-x}Vx_xN (see Figure S3). As can be seen, N vacancies induce a finite Sc 3d t2g∗t_{2g}^{*} states across the Fermi level. The observation was noted in the unoccupied Sc 2p XAS spectra mentioned in the main manuscript. We do not observe any significant contribution from O 2p states at or around the Fermi level. The contribution can only be noted at around 6-8 eV in the DOS calculations. Therefore, we attribute a contribution of O 2p states around feature B in Figure 4(c) mentioned in the main manuscript.

Figure S3. Theoretical density of states (DOS) considering N vacancies and O in the unit cell of ScN and Sc1−x_{1-x}Vx_xN.

References

  1. [1]M. Mayer, SIMNRA User's Guide, Book (1997).
  2. [2]L. G. Parratt, Surface Studies of Solids by Total Reflection of X-Rays, Phys. Rev. 95, 359 (1954).DOI
  3. [3]A. Daillant, J; Gibaud, X-Ray and Neuron Reflectivity: Principles and Applications (1999).DOI
  4. [4]P. Zimmermann, S. Peredkov, P. M. Abdala, S. DeBeer, M. Tromp, C. Müller, and J. A. van Bokhoven, Modern X-Ray Spectroscopy: XAS and XES in the Laboratory, Coord. Chem. Rev. 423, 213466 (2020).DOI
  5. [5]A. Le Febvrier, N. Tureson, N. Stilkerich, G. Greczynski, and P. Eklund, Effect of Impurities on Morphology, Growth Mode, and Thermoelectric Properties of (1 1 1) and (0 0 1) Epitaxial-like ScN Films, J. Phys. D. Appl. Phys. 52, 035302 (2019).DOI
  6. [6]F. De Groot, Multiplet Effects in X-Ray Spectroscopy, Coord. Chem. Rev. 249, 31 (2005).DOI
  7. [7]R. P. Gupta and S. K. Sen, Calculation of Multiplet Structure of Core P-Vacancy Levels. II, Phys. Rev. B 12, 15 (1975).DOI

Paper details

vlnc:W_ab2jh5r7
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents