NbOI2_2 has recently emerged as a new van der Waals material combining semiconducting behavior with intrinsic in plane ferroelectricity and pronounced transport and optical anisotropy. However, its photocarrier dynamics remain largely unexplored. Here we report transient absorption spectroscopy of NbOI2_2 using femtosecond pump probe reflectance measurements. A pronounced transient absorption feature is observed near the 2.34 eV excitonic resonance, arising from photocarrier induced excitonic energy shifts and saturation. The decay dynamics reveal an exciton lifetime of several tens of picoseconds and show density-dependent behavior consistent with exciton exciton annihilation and defect-assisted Auger recombination, yielding a rate of 0.4 cm2^2 s−1^{-1}, which is comparable to that in monolayer transition metal dichalcogenides. Polarization resolved measurements further reveal a pronounced in-plane anisotropy in the transient response that follows the linear absorption anisotropy. These findings provide fundamental insight into photocarrier dynamics in NbOI2_2 and establish key parameters for understanding and exploiting its optoelectronic behavior.

Layered niobium oxide dihalides NbOX2\mathrm{NbOX}_{2} (X = Cl, Br, I) have recently emerged as an intriguing family of van der Waals materials that combine semiconducting behavior with intrinsic in-plane ferroelectricity. [1, 2, 3, 4, 5] Among them, NbOI2\mathrm{NbOI}_{2} has shown particularly promising properties as a prototype two-dimensional (2D) ferroelectric semiconductor. Its low-symmetry monoclinic structure features Nb atoms displaced from the center of [NbO2X4][\mathrm{NbO}_{2}\mathrm{X}_{4}] octahedra, producing spontaneous polarization confined within the layers at room temperature, [6] which enables switchable rectification in double-Schottky-barrier devices [7] and antiferroelectric ordering. [2, 8, 9]

The Peierls-distorted polar structure of NbOI2\mathrm{NbOI}_{2}, with anisotropic bonding, gives rise to pronounced anisotropy in its structural, electronic, and optical properties. [10, 11, 12] Mechanical measurements showed a large in-plane anisotropy in Young’s modulus [13] and directional ferroelectric domains. [8, 14] Angle-resolved Raman and absorption studies revealed strongly directional phonon modes, [6] while anisotropic in-plane electrical conductance and photoresponsivity enabled polarization-sensitive photodetection and synaptic transistor functionalities. [6, 15]

The polar structure of NbOI2\mathrm{NbOI}_{2} also leads to exceptional nonlinear optical responses. Multiple studies have reported giant, electrically tunable, and strain-dependent second-harmonic generation in NbOI2\mathrm{NbOI}_{2}, with conversion efficiencies far exceeding those of most 2D materials. [9, 16, 17, 18, 19, 20] NbOI2\mathrm{NbOI}_{2} further exhibits remarkable piezoelectric and electro-optic properties, with exceptionally large piezoelectric coefficients and substantial linear electro-optic and elasto-optic responses in both 2D and bulk forms. [12, 21, 22] These unique properties have inspired exploration of NbOI2\mathrm{NbOI}_{2} for various applications such as polarization-sensitive sensors, [22] nonvolatile and neuromorphic devices, [23, 24] optoelectronic and gas-sensing, [25] and THz emission and detection. [26, 27]

Despite these advances, the semiconducting aspects, particularly the photoexcitation dynamics, of NbOI2\mathrm{NbOI}_{2} remain largely unexplored. Understanding the photocarrier dynamics of NbOI2\mathrm{NbOI}_{2} is critical for elucidating the microscopic origins of its extraordinary THz and nonlinear optical responses, and for enabling its use in high-speed ferroelectric optoelectronic and Figure 1(a) shows the crystal structure of NbOI2\mathrm{NbOI_2}. The displacement of Nb atoms along the bb axis induces a spontaneous polarization along that direction, which defines the polar axis. We adopted a device structure as shown in Figure 1(b), where a NbOI2\mathrm{NbOI_2} flake is sandwiched between two hexagonal boron nitride (hBN) layers on a quartz substrate. The device was fabricated by exfoliating thin flakes of hBN and NbOI2\mathrm{NbOI_2} using adhesive tape and sequentially

tially transferring them onto the substrate, followed by thermal annealing (see Supporting Information). Figure 1(c) presents an optical microscope image of the resulting device. The polar and nonpolar edges of the NbOI2_2 flake is identified according to its anisotropic optical absorption (to be discussed later). Atomic force microscopy measurements (see Supporting Information) show that the NbOI2_2 flake has a thickness of 21 nm, corresponding to 25 monolayers. The top and bottom hBN layers are 15 nm and 36 nm thick, respectively. The hBN encapsulation is crucial for preventing sample degradation during the optical experiments (see Supporting Information).

Figure 1. (a) Crystal structure of NbOI2\mathrm{NbOI_2}. (b) Device structure showing a NbOI2\mathrm{NbOI_2} flake sandwiched between two hexagonal boron nitride (hBN) flakes on a quartz substrate. (c) Optical microscope image of the device used for optical measurements. (d) Schematic band structure of NbOI2\mathrm{NbOI_2} showing the relevant excitonic transitions.

Figure 1(d) schematically illustrates the relevant features of the NbOI2_2 band structure established by angle-resolved photoemission spectroscopy and density functional theory.[16] The conduction band c1c_1 is dominated by Nb dxyd_{xy} character, whereas c2c_2 contains mainly Nb dyzd_{yz} contributions. The topmost valence band v1v_1 originates primarily from Nb dx2−y2/dz2d_{x^2-y^2}/d_{z^2} orbitals, while v2v_2 derives predominantly from I pyp_y orbitals. The conduction-band minimum and valence-band maximum are located at the X and Y points, respectively, making NbOI2_2 an indirect semiconductor. However, ellipsometry and optical absorption measurements have revealed several strong excitonic resonances. The dominant ones in the visible range, at 2.34 eV (P1P_1) and 2.64 eV (P2P_2), arise from the v1v_1–c1c_1 and v2v_2–c1c_1 transitions at kk-points along the nonpolar direction. In contrast, the P4P_4 (3.54 eV) excitonic resonance originates from transitions between higher-lying conduction and deeper valence bands at kk-points along the polar direction.[16]

Here we focus on the transient absorption of the P1P_1 resonance. We first performed transient absorption spectroscopy measurements in reflection geometry (see Supporting Information). The NbOI2_2 flake was photoexcited by a 3.02 eV pump pulse with a peak fluence of 13 μ\muJ cm−2^{-2}, which is expected to inject exciton by the P4P_4 transition [Figure 1(d)]. To estimate the injected carrier density, we measured the reflectance (0.48) and transmittance (0.26) of the sample at this photon energy, which allowed us to deduce an absorption coefficient of 1.43 ×\times 105^5 cm−1^{-1} using the sample thickness of 21 nm. By using Beer’s law, we deduced the peak injected areal carrier densities to be 1.7×1011 cm−21.7 \times10^{11}\ \mathrm{cm}^{-2} at the first layer of the sample. The change in the sample’s absorption coefficient induced by these carriers (known as transient absorption) was detected by measuring the differential reflectance of a tunable probe pulse near the P1P_1 resonance, defined as ΔR/R0=(R−R0)/R0\Delta R/R_0 = (R - R_0)/R_0, where RR and R0R_0 are the reflectance of the pump-excited and unexcited NbOI2_2 device, respectively (Supporting Information).[28]

Figure 2(a) shows the differential reflectance signal as a function of probe photon energy and probe delay. In this measurement, the pump and probe pulses are vertically and horizontally polarized, respectively, while the sample polar direction make an arbitrarily selected angle of 75∘75^\circ from horizontal (detailed angular dependence will be discussed later). A pronounced spectroscopic feature near the 2.34 eV2.34\ \mathrm{eV} resonance with a fast temporal evolution is observed. The peak signal, obtained at a delay of 0.8 ps0.8\ \mathrm{ps}, is plotted in Figure 2(b) as triangles, together with the absorption lineshape of this resonance (red curve) re-plotted from Ref. 16.

Differential reflectance measurements and schematic illustration

Figure 2. (a) Differential reflectance of NbOI2_2 as a function of probe delay and probe photon energy. (b) Peak differential reflectance as a function of probe photon energy, corresponding to the dashed horizontal line in (a). The red curve highlights the excitonic resonance, while the dashed curve represents a fit based on a shift and saturation of the exciton resonance. (c) Time-resolved differential reflectance at two probe photon energies corresponding to the positive and negative peaks. (d) Schematic illustration of the origin of the differential reflectance spectrum from a shifted and saturated excitonic absorption peak.

The rapid rise of the signal, as shown in Figure 2(c), provides unambiguous evidence that the transient absorption originates from pump-injected photocarriers. It is well established that photocarriers in semiconductors can induce transient absorption near an excitonic resonance through energy shift, saturation, and broadening of the transition. [29, 30] By using a blue shift of 0.25 meV and a saturation of 0.14%, we can reproduce the observed spectral shape [dashed curve in Figure 2(b)], as schematically illustrated in Figure 2(d).

We next examined how the signals at the two extreme probe photon energies vary with pump fluence. Under linear absorption, the pump fluence is proportional to the injected carrier density. Although NbOI2_2 possesses relatively large second- and third-order nonlinear susceptibilities,[16, 20] our experiment is conducted at low peak irradiance on the order of 10810^{8} W cm−2^{-2}. At this irradiance, carrier injection via two-photon absorption or absorption of the second-harmonic light is negligible (see Supporting Information). Figure 3(a) shows that the peak signal magnitude increases linearly with pump fluence. This linearity establishes that the differential reflectance is proportional to the carrier density and therefore accurately tracks the carrier dynamics.

Peak differential reflectance magnitude, time-resolved differential reflectance traces, carrier-density dynamics, and extracted recombination coefficient

Figure 3. (a) Peak differential reflectance magnitude of NbOI2_2 as a function of pump fluence, measured with probe photon energies of 2.25 and 2.34 eV, respectively. (b) Representative time-resolved differential reflectance traces at various pump fluences, measured with a 2.34 eV probe. (c) n0/n(t)−1n_0/n(t)-1 calculated from the data as a function of probe delay for several high pump fluences. The red lines represent linear fits to the data at early delays. (d) γn0\gamma n_0 extracted from the fits shown in (c) as a function of the injected carrier density n0n_0. The red line indicates a linear fit.

Owing to the indirect bandgap of NbOI2\mathrm{NbOI_2}, the quasi–steady-state photocarrier population is expected to consist mainly of electrons near the X point and holes near the Y point [Figure 1(d)]. We hypothesize that the dominant photoexcited species are excitons formed by these electrons and holes. Giant exciton binding energies on the order of 600–800 meV have been reported in bulk NbOCl2\mathrm{NbOCl_2}, a material with the same lattice structure and similar electronic properties. [31, 32] Although the exciton binding energy of NbOI2\mathrm{NbOI_2} has not yet been determined, it is reasonable to assume that it is well above 26 meV, making the excitons stable at room temperature. The normalized time-resolved differential reflectance at various pump fluences are shown in Figure 3(b), which clearly reveals two features. First, the signal persists for several tens of picoseconds at all fluences, reflecting the exciton lifetime in NbOI2\mathrm{NbOI_2}. Second, the decay becomes faster at higher fluence, indicating density-dependent excitonic dynamics.

Previously, exciton–exciton annihilation (XXA) and defect-assisted (DA) Auger recombination have been established as dominant nonlinear exciton decay channels in layered semiconductors at elevated densities, and both scale quadratically with exciton density. In the former, two excitons interact and one recombines nonradiatively, transferring its energy to the other. [33, 34, 35] In the latter, a defect traps an exciton (or one of its carriers), and the trapped species recombines with a free exciton. The presence of defect states relaxes crystalline momentum conservation constraints, allowing Auger-like decay to occur efficiently even at moderate densities. [36, 37, 38] With such quadratic decay channels included, the rate equa tion for the exciton density (nn) can be written as

dndt=−nτ−12γn2,(1)\frac{dn}{dt}=-\frac{n}{\tau}-\frac{1}{2}\gamma n^2, \tag*{(1)}

where τ\tau denotes the single-particle exciton lifetime. We define γ=γXXA+γDA\gamma=\gamma_{\mathrm{XXA}}+\gamma_{\mathrm{DA}}, where γXXA\gamma_{\mathrm{XXA}} and γDA\gamma_{\mathrm{DA}} are the bimolecular coefficients for XXA and DA Auger recombination, respectively. When these nonlinear decay channels dominate the exciton dynamics, the first term on the right-hand side of Eq. (1) can be neglected, leading to a simple solution:

n0n(t)−1=γn0t,(2)\frac{n_0}{n(t)}-1=\gamma n_0t, \tag*{(2)}

where n0n_0 is the initially injected exciton density at t=0t=0.

To compare our data with this model, we calculated n0/n(t)−1n_0/n(t)-1 from the time-resolved differential reflectance at elevated pump fluences using the linear relation established in Figure 3(a), and plotted the results in Figure 3(c). At early delays, this quantity increases approximately linearly, as expected from the model. By performing linear fits (red lines), we extracted the parameter γn0\gamma n_0 as a function of n0n_0, as shown in Figure 3(d). The resulting linear dependence further confirms the validity of this model for early probe delays and yields a rate of γ=0.4±0.1 cm2s−1\gamma=0.4\pm0.1\ \mathrm{cm}^2\mathrm{s}^{-1}. This value is on the same order of magnitude with previously reported exciton-exciton annihilation rates in 2D transient metal dichalcogenides.[33, 34] However, our analysis cannot conclusively separate the contributions of the two nonlinear decay mechanisms. We further note that such decay channels are insignificant on pulsewidth-limited ultrafast time scales, as evidenced by the linear dependence of the peak signal on pump fluence [Figure 3(a)].

Finally, we explore the in-plane anisotropy of the transient absorption. The wavefunction of the P1P_1 exciton is confined along the nonpolar direction,[16] and therefore primarily interacts with light polarized along this direction through dipole coupling. In contrast, the higher-energy P4P_4 exciton is confined along the polar direction and thus couples most strongly to light polarized along the polar axis. We first measured the polarization-dependent linear absorption of the sample at the P1P_1 and P4P_4 resonances using the probe and pump pulses individually. As shown in Figure S2, the absorptance at P1P_1 reaches a maximum when the light polarization is aligned with the nonpolar direction, whereas the absorptance at P4P_4 peaks when the polarization is aligned with the polar direction of NbOI₂. These behaviors are consistent with previous report. [16]

Figure 4(a) shows the measured time-resolved differential reflectance at various sample orientations. In these measurements, the pump and probe pulses are linearly polarized along the horizontal and vertical directions in the laboratory frame, while the sample is rotated about its surface normal. This rotation varies the angle θ\theta between the polar axis of the sample and the probe polarization, as illustrated in Figure 4(d). The signal at 0.8 ps is plotted in Figure 4(b) as a function of θ\theta, which shows a characteristic sin⁡2(θ)\sin^{2}(\theta) dependence (dashed curve). The time scans at the two extreme angles are shown in Figure 4(c). The strong angular dependence of the transient absorption confirms the orthogonal confinement of the P1P_{1} and P4P_{4} excitons.[16]

Figure 4. (a) Differential reflectance of NbOI₂ as a function of sample orientation and probe delay. (b) Peak differential reflectance as a function of the angle between the crystal’s polar direction and the probe polarization. The dashed line represents a fit. (c) Time-resolved differential reflectance at selected sample orientations. (d) Measurement configuration showing the pump and probe polarizations (vertical and horizontal in the laboratory frame, respectively) and the definition of the angle θ\theta.

In summary, our transient absorption measurements revealed key aspects of the photocarrier dynamics in NbOI2_{2}. The excitonic resonance near 2.34 eV exhibits pronounced transient absorption due to photocarrier-induced energy renormalization and saturation effects. We deduced an exciton lifetime on the order of several 10’s of picosecond. The observed density-dependent exciton recombination is consistent with exciton–exciton annihilation and defect-assisted Auger recombination. The in-plane anisotropy of the transient response reflects the intrinsic polar symmetry of NbOI2_{2} and its strongly directional optical coupling. These findings reveal the microscopic processes governing exciton relaxation and interaction in this emerging ferroelectric semiconductor and provide a foundation for developing ultrafast, polarization-sensitive optoelectronic and quantum devices based on van der Waals ferroelectric semiconductors.

Acknowledgement

This work was supported by the U.S. Department of Energy, Office of Science, Basic Energy Sciences, under Award # DE-SC0020995.

Supporting Information Available

Sample fabrication and characterization, linear absorption spectroscopy data, analysis of nonlinear absorption mechanisms, transient absorption spectroscopy setup.

TOC Graphic

Figure 5 (PDF p. 16).

References

  1. [1]Guo, Q.; Zhang, Q.; Zhang, T.; Zhou, J.; Xiao, S.; Wang, S.; Feng, Y.; Qiu, C. Colossal in-Plane Optical Anisotropy in a Two-Dimensional van der Waals Crystal. Nat. Photonics 2024, 18, 1170–1175.DOI
  2. [2]Jia, Y.; Zhao, M.; Gou, G.; Zeng, X.; Li, J. Niobium Oxide Dihalides NbOX₂: A New Family of Two-Dimensional van der Waals Layered Materials with Intrinsic Ferroelectricity and Antiferroelectricity. Nanoscale Horiz. 2019, 4, 1113–1123.DOI
  3. [3]Kallioniemi, L.; Lyu, X.; He, R.; Rasmita, A.; Duan, R.; Liu, Z.; Gao, W. Van der Waals Engineering for Quantum-Entangled Photon Generation. Nat. Photonics 2025, 19, 142–148.DOI
  4. [4]Lyu, X.; Kallioniemi, L.; Cai, H.; An, L.; Duan, R.; Wu, S.; Tan, Q.; Zhang, C.; He, R.; Miao, Y.; Liu, Z.; Ling, A.; Zuniga-Perez, J.; Gao, W. Boosting Classical and Quantum Nonlinear Processes in Ultrathin van der Waals Materials. Nat. Commun. 2025, 16, 4987.arxiv.org/abs/2503.23075
  5. [5]Li, Z.; Wang, S.; Wang, C.; Zhang, X.; Yu, Z.; Du, S.; Zeng, Z.; Dai, Y.; Zhang, Y.; Liu, X.; Sun, J.; Xue, J.; Wu, Z.; Fan, L.; Dai, J.; Zhai, K.; Nie, A.; Liu, Z.; Cheng, Y. Peierls Distortion Induced Giant Linear Dichroism, Second-Harmonic Generation, and in-Plane Ferroelectricity in NbOBr₂. Small 2025, 21, 2407729.DOI
  6. [6]Fang, Y.; Wang, F.; Wang, R.; Zhai, T.; Huang, F. 2D NbIO₂: A Chiral Semiconductor with Highly in-Plane Anisotropic Electrical and Optical Properties. Adv. Mater. 2021, 33, 2101505.DOI
  7. [7]Chen, Z.; Hu, Y.; Zhang, L.; Jiang, J.; Hawks, R.; Shi, J. Photoactive Electrically Switchable van der Waals Semiconductor NbOCl₂. Appl. Phys. Lett. 2021, 119, 033103.DOI
  8. [8]Liu, C.; Zhang, X.; Wang, X.; Wang, Z.; Abdelwahab, I.; Verzhbitsky, I.; Shao, Y.; Eda, G.; Sun, W.; Shen, L.; Loh, K. Ferroelectricity in Niobium Oxide Dihalides NbOX₂ (X = Cl, I): A Macroscopic- to Microscopic-Scale Study. ACS Nano 2023, 17, 7170–7179.DOI
  9. [9]Ye, L.; Zhou, W.; Huang, D.; Jiang, X.; Guo, Q.; Cao, X.; Yan, S.; Wang, X.; Jia, D.; Jiang, D.; Wang, Y.; Wu, X.; Zhang, X.; Li, Y.; Lei, H.; Gou, H.; Huang, B. Manipulation of Nonlinear Optical Responses in Layered Ferroelectric Niobium Oxide Dihalides. Nat. Commun. 2023, 14, 5911.DOI
  10. [10]Mortazavi, B.; Shahrokhi, M.; Javvaji, B.; Shapeev, A.; Zhuang, X. Highly Anisotropic Mechanical and Optical Properties of 2D NbOX₂ (X = Cl, Br, I) Revealed by First-Principle. Nanotechnology 2022, 33, 275701.DOI
  11. [11]Pan, L.; Wan, Y.; Wang, Z.; Geng, H.; Chen, X. Two-Dimensional Anisotropic Monolayers NbOX₂ (X=Cl, Br, I): Promising Candidates for Photocatalytic Water Splitting with High Solar-to-Hydrogen Efficiency. J. Appl. Phys. 2023, 134, 085105.DOI
  12. [12]Wu, Y.; Abdelwahab, I.; Kwon, K.; Verzhbitsky, I.; Wang, L.; Liew, W.; Yao, K.; Eda, G.; Loh, K.; Shen, L.; Quek, S. Data-Driven Discovery of High Performance Layered van der Waals Piezoelectric NbOI₂. Nat. Commun. 2022, 13, 1884.DOI
  13. [13]Cui, Y.; Li, S.; Zhang, X.; Wang, T.; Cao, X.; Yan, S.; Zhang, X.; Lei, H.; Tang, G.; Hong, J.; Wang, X. In-Plane Anisotropic Mechanical Properties of Two-Dimensional NbOI₂. Appl. Phys. Lett. 2023, 123, 051905.DOI
  14. [14]Cui, Y.; Wang, T.; Hu, D.; Wang, Z.; Hong, J.; Wang, X. Piezoelectricity in NbOI₂ for Piezotronics and Nanogenerators. npj 2D Mater. Appl. 2024, 8, 62.DOI
  15. [15]Wang, M.; Ouyang, D.; Dai, Y.; Huo, D.; He, W.; Song, B.; Hu, W.; Wu, M.; Li, Y.; Zhai, T. 2D Piezo-Ferro-Opto-Electronic Artificial Synapse for Bio-Inspired Multimodal Sensory Integration. Adv. Mater. 2025, 37, 2500049.DOI
  16. [16]Abdelwahab, I.; Tilmann, B.; Wu, Y.; Giovanni, D.; Verzhbitsky, I.; Zhu, M.; Berté, R.; Xuan, F.; Menezes, L.; Eda, G.; Sum, T.; Quek, S.; Maier, S.; Loh, K. Giant Second-Harmonic Generation in Ferroelectric NbOI₂. Nat. Photo. 2022, 16, 644–649.DOI
  17. [17]Fu, J.; Yang, N.; Liu, Y.; Liu, Q.; Du, J.; Fang, Y.; Wang, J.; Gao, B.; Xu, C.; Zhang, D.; Meixner, A.; Gou, G.; Huang, F.; Zhen, L.; Li, Y. Emission Dipole and Pressure-Driven Tunability of Second Harmonic Generation in Vdws Ferroelectric NbOI₂. Adv. Funct. Mater. 2024, 34, 2308207.DOI
  18. [18]Wang, H.; Chen, Q.; Cao, Y.; Sang, W.; Tan, F.; Li, H.; Wang, T.; Gan, Y.; Xiang, D.; Liu, T. Anisotropic Strain-Tailoring Nonlinear Optical Response in van der Waals NbOI₂. Nano Lett. 2024, 24, 3413–3420.DOI
  19. [19]Wu, M.; An, M.; Lou, Z.; Lin, L.; Zeng, Z.; Wang, J.; Zheng, X. Manipulating Anisotropy of Second Harmonic Generation in NbOI₂ via Precise Strain Engineering. Adv. Funct. Mater. 2025, e16389.DOI
  20. [20]Deka, J.; Gao, J.; Yang, X. Anisotropic Second- and Third-Harmonic Hermite-Gaussian Beam Generation with NbOI₂ Holograms. Adv. Photon. Res. 2025, 2500188.DOI
  21. [21]Zhang, Z.; Di, X.; Paillard, C.; Bellaiche, L.; Jiang, Z. Giant Electro-Optic and Elasto-Optic Effects in Ferroelectric NbOI₂. Phys. Rev. B 2024, 110, L100101.DOI
  22. [22]Sun, X.; Wan, Y.; Fang, Y.; Huang, F. Layered Ferroelectric NbOI₂ Flakes toward in-Plane Anisotropic Self-Powered Sensing. Small Sci. 2024, 4, 2300125.DOI
  23. [23]Hao, Z.; Zhao, G.; Liu, J.; Tong, Y.; Li, H.; Zhang, J.; Liu, J.; Kong, F.; Kozadaev, K.; Li, Y.; Han, X.; Li, H.; Huang, H.; Sun, C.; Tolstik, A.; Novitsky, A.; Pan, L.; Li, D. Observation of Intrinsic and Led Light-Enhanced Memristor Performance in in-Plane Ferroelectric NbOI₂. ACS Nano 2025, 19, 27654–27664.arxiv.org/abs/2504.21737
  24. [24]Hossain, M.; Lu, H.; Khurana, R.; Kholil, M.; Bagheri, S.; Abourahma, J.; Sinitskii, A.; Gruverman, A. Conducting Domain Walls in Van Der Waals Ferroelectric NbOI₂. Nano Lett. 2025, 25, 13844–13849.DOI
  25. [25]Guan, Y.; Ding, Y.; Fang, Y.; Li, J.; Liu, Y.; Wang, R.; Hao, J.; Xie, H.; Xu, C.; Zhen, L.; Li, Y.; Yang, L. Far-Field Femtosecond Laser-Driven λ/73 Super-Resolution Fabrication of 2D van der Waals NbOI₂ Nanostructures in Ambient Air. Nat. Commun. 2025, 16, 4149.DOI
  26. [26]Subedi, S.; Liu, W.; Fang, W.; Fox, C.; Zhai, Z.; Fei, F.; Ping, Y.; Lv, B.; Xiao, J. Colossal Terahertz Emission with Ultrafast Tunability Based on van der Waals Ferroelectric NbOI₂. Adv. Opt. Mater. 2025, 13, 2403471.DOI
  27. [27]Handa, T.; Huang, C.; Li, Y.; Olsen, N.; Chica, D.; Xu, D.; Sturm, F.; McIver, J.; Roy, X.; Zhu, X. Terahertz Emission from Giant Optical Rectification in a van der Waals Material. Nat. Mater. 2025, 24, 1203–1208.DOI
  28. [28]Ceballos, F.; Zhao, H. Ultrafast Laser Spectroscopy of Two-Dimensional Materials beyond Graphene. Adv. Funct. Mater. 2017, 27, 1604509.DOI
  29. [29]Schmitt-Rink, S.; Chemla, D. S.; Miller, D. A. B. Theory of Transient Excitonic Optical Nonlinearities in Semiconductor Quantum-Well Structures. Phys. Rev. B 1985, 32, 6601–6609.pubmed.ncbi.nlm.nih.gov/9936766
  30. [30]Chemla, D. S.; Shah, J. Many-Body and Correlation Effects in Semiconductors. Nature 2001, 411, 549–557.pubmed.ncbi.nlm.nih.gov/11385562
  31. [31]Guo, Q.; Qi, X.; Zhang, L.; Gao, M.; Hu, S.; Zhou, W.; Zang, W.; Zhao, X.; Wang, J.; Yan, B.; Xu, M.; Wu, Y.; Eda, G.; Xiao, Z.; Yang, S.; Gou, H.; Feng, Y.; Guo, G.; Zhou, W.; Ren, X. et al. Ultrathin Quantum Light Source with Van Der Waals NbOCl₂ Crystal. Nature 2023, 613, 53–59.DOI
  32. [32]Ding, Y.; Yan, L.; Wu, Y.; Zhou, L. Exciton-Driven and Layer-Independent Linear and Nonlinear Optical Properties in NbOCl₂. J. Phys. Chem. Lett. 2024, 15, 7191–7198.DOI
  33. [33]Kumar, N.; Cui, Q.; Ceballos, F.; He, D.; Wang, Y.; Zhao, H. Exciton-Exciton Annihilation in MoSe₂ Monolayers. Phys. Rev. B 2014, 89, 125427.DOI
  34. [34]Sun, D.; Rao, Y.; Reider, G. A.; Chen, G.; You, Y.; Brezin, L.; Harutyunyan, A. R.; Heinz, T. F. Observation of Rapid Exciton-Exciton Annihilation in Monolayer Molybdenum Disulfide. Nano Lett. 2014, 14, 5625–5629.DOI
  35. [35]Pareek, V.; Madeo, J.; Dani, K. M. Ultrafast Control of the Dimensionality of Exciton-Exciton Annihilation in Atomically Thin Black Phosphorus. Phys. Rev. Lett. 2020, 124, 057403.DOI
  36. [36]Wang, H. N.; Zhang, C. J.; Rana, F. Ultrafast Dynamics of Defect-Assisted Electron Hole Recombination in Mono Layer MoS₂. Nano Lett. 2015, 15, 339–345.DOI
  37. [37]Wang, H.; Strait, J. H.; Zhang, C.; Chan, W.; Manolatou, C.; Tiwari, S.; Rana, F. Fast exciton annihilation by capture of electrons or holes by defects via Auger scattering in monolayer metal dichalcogenides. Phys. Rev. B 2015, 91, 165411.DOI
  38. [38]Yu, Y.; Yu, Y.; Xu, C.; Cai, Y.-Q.; Su, L.; Zhang, Y.; Zhang, Y.-W.; Gundogdu, K.; Cao, L. Engineering Substrate Interactions for High Luminescence Efficiency of Transition-Metal Dichalcogenide Monolayers. Adv. Funct. Mater. 2016, 26, 4733–4739.DOI

Paper details

vlnc:W_ae6vfp7z
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents