betaFeedback

WorksPhysics and Astronomy

Role of chemical disorder in tuning the Weyl points in vanadium doped Co2_2TiSn

Abstract

The lack of time-reversal symmetry and Weyl fermions give exotic transport properties to Co-based Heusler alloys. In the present study, we have investigated the role of chemical disorder on the variation of Weyl points in Co\textsubscript{2}Ti\textsubscript{1-x}V\textsubscript{x}Sn magnetic Weyl semimetal candidate. We employ the first principle approach to track the evolution of the nodal lines responsible for the appearance of Weyl node in Co2_2TiSn as a function of V substitution in place of Ti. By increasing the V concentration in place of Ti, the nodal line moves toward Fermi level and remains at Fermi level around the middle composition. Further increase of the V content, leads shifting of nodal line away from Fermi level. Density of state calculation shows half-metallic behavior for the entire range of composition. The magnetic moment on each Co atom as a function of V concentration increases linearly up to x=0.4, and after that, it starts decreasing. We also investigated the evolution of the Weyl nodes and Fermi arcs with chemical doping. The first-principles calculations reveal that via replacing almost half of the Ti with V, the intrinsic anomalous Hall conductivity increased twice as compared to the undoped composition. Our results indicate that the composition close to the 50% V doped Co2_2TiSn, will be an ideal composition for the experimental investigation of Weyl physics.

Introduction

Weyl semimetals (WSMs) have created vast interest in recent years due to their novel electronic and transport properties [1, 2], such as very high electron mobilities [3], Fermi arcs on the surface [4, 5], extremely large magnetoresistance [3, 6], anomalous Hall effect [7, 8], and the anomalous Nernst effect [9, 10]. WSMs also exhibit unconventional optical properties, such as large and quantized photo-currents [11, 12, 13, 14], second-harmonic generation [15, 16], and Kerr rotation [17, 18]. These properties can lead to more efficient electronic and photonic applications [1]. WSMs are an especial class of the topological materials, characterized by the crossings of singly degenerate energy bands near the Fermi energy, leading to the formation of pairs of Weyl nodes [19, 20, 21]. WSMs provide a platform for manipulating and understanding the physics of the chiral Weyl fermions [22, 23].

Inversion symmetry (IS) or time-reversal symmetry (TRS) must be broken to obtain Weyl nodes/WSMs [2, 23, 24]. WSMs with broken IS have been investigated extensively [3, 19, 20], while WSMs with broken TRS, known as magnetic WSMs, were recently discovered in experiments [9, 25]. Magnetic WSMs created much interest because, in this class of WSMs, the properties can be manipulated using a magnetic field as an external degree of freedom. Heusler alloys have emerged as an important class of materials to investigate the Weyl physics and its consequences [8, 25, 26, 27, 28, 29, 30, 31]. In Heusler compounds, we either look at half-Heusler or inverse Heusler compounds (IS breaking) [26], at magnetic compounds (TRS breaking) [25, 27, 28, 29], or compounds with both IS and TRS breaking [8, 30, 31]. In most magnetic Heuslers, the magnetization direction can be changed quite easily. Since the location of Weyl nodes in the momentum space depends on the direction of magnetization, Heusler compounds can prove to be useful to understand the physics of Weyl fermions. Combined with their extensive tunability, Heusler WSMs are a promising platform for practical topological applications [1, 2].

Co2MnGaCo_2MnGa has been theoretically predicted and experimentally proven to be a WSM. The Weyl nodes lie close to the Fermi energy [25, 32], and transport measurements have shown large anomalous Hall and Nernst effects [10, 33, 34, 35, 36, 37]. Besides Co2MnGaCo_2MnGa, other Heusler compounds have also been predicted to be WSM [38, 39, 40, 41]. Although, for most of the proposed Heusler WSMs, the Weyl nodes lie away from the Fermi energy, which reduces the topological properties of these materials [27, 28, 38, 39, 40, 41]. By tuning the Fermi energy, it can coincide with the energy of the nodes, which can significantly improve the properties [40, 42, 43].

Co2TiSnCo_2TiSn, a Heusler compound that has a high Curie temperature and shows half-metallic behavior [44, 45, 46, 47, 48], has been proposed as a WSM candidate [28, 39, 40]. Co2TiSnCo_2TiSn has 26 valence electrons and has Weyl nodes with chemical potential a few hundred meV above the Fermi energy [28, 39, 40]. The number of valence electrons must be increased to make the nodes chemical potential coincide with the Fermi energy [28]. To achieve this, Ti, which has 2 electrons in its valence 3d3d orbital, can be substituted with V, which has 3 electrons in the 3d3d orbital. Wang et al. suggested that the doping of 10% V in place of Ti (i.e., Co2_2Ti0.9_{0.9}V0.1_{0.1}Ga) to obtain the WSM phase [40]. However, efforts to synthesize thin films Co2_2Ti0.9_{0.9}V0.1_{0.1}Sn have not been successful, and the most stable composition was found to be Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn (i.e., 40% V doped) [49]. Transport measurements for Co2_2TiSn and Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn thin films show anomalous Hall and Nernst effects [49, 50]. Interestingly, the anomalous Nernst angle and coefficient for the doped compound (i.e., Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn) were significantly higher than the undoped one [50].

In this manuscript, we investigated the effect of V doping on the electronic structure of Co2_2Ti1−x_{1-x}Vx_xSn (xx = 0.0, 0.2, 0.4, 0.6, 0.8 and 1.0). The position of nodal lines, responsible for Weyl node formation in Co2_2TiSn, changes as a function of V substitution in place of Ti. With increasing V in place of Ti, nodal lines and Fermi arcs get shifted towards the Fermi level close to the mid composition (i.e Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn). The intrinsic anomalous Hall conductivity obtained from the theory for the 50% V doped composition (Co2_2Ti0.5_{0.5}V0.5_{0.5}Sn) is nearly twice as compared to the undoped composition, due to the existence of the Fermi arcs very close (≈\approx 7-23 meV) to the Fermi energy.

Methods

The calculations were performed using the full-potential Korringa–Kohn–Rostoker (KKR) Green’s function method, as implemented in the SPRKKR package [53] and pseudo-potential based density functional theory (DFT) as implemented in Quantum ESPRESSO (QE)[58] and Vienna ab-initio simulation package (VASP)[59, 60]. The exchange-correlation potential is approximated through PBE-GGA functional [54]. A k-mesh consisting of (22 ×\times 22 ×\times 22) k-points was used, and the angular momentum cut-off number was chosen to be lmax⁡l_{\max} = 3. The Fermi energies were determined using the Lloyd formula [55]. For the calculations of the Bloch spectral functions spin-orbit coupling (SOC) has been taken into account. The band structures were calculated for both the spin-polarized, non spin-orbit coupling case as well as the case with spin-orbit coupling, taken as the a scalar relativistic correction to the original Hamiltonian. The ground state energies obtained when the magnetization quantization directions are kept in the [1], [110] and [111] directions are found to be the same within the limits of the methodology, indicating that the magnetization directions, and therefore the positions of the Weyl nodes, can be changed easily. This matches with the literature on Co2_2TiSn, Co2_2VSn and similar Heusler compounds [39, 40]. The disorder was taken into account through the coherent potential approximation (CPA) in the SPR-KKR calculations [56, 57]. Optimized pseudopotentials [65] are used in the calculations and the kinetic energy cutoff for the planewave is taken as 80 RyRy. The electronic integration over the Brillouin zone (BZBZ) is approximated by the Gaussian smearing of 0.005 RyRy both for the self-consistent (sc) and non-self-consistent (nsc) calculations. The Monkhorst-Pack k-grid of 8 ×\times 8 ×\times 8 are considered for the Brillouin zone integration for the DFT band structure calculations. The Wannier interpolated bands, the anomalous Hall conductivity (AHC), normalized Berry curvature and the Fermi arcs were calculated using Wannier90 [61, 62, 63] and WannierTool [64] starting from the plane wave based pseudo potential DFT band structures. The transition metal dd-orbitals are used in the energy selective downfolding projections for the wannier90 calculations. The AHC calculation is carried out with a dense k-grid of 75 ×\times 75 ×\times 75. Further, through the adaptive refinement technique a fine mesh of 5 ×\times 5 ×\times 5 is added around the points wherever the mod of the Berry curvature (∣Ω(k)∣|\Omega(\mathbf{k})|) exceeds 100 Bohr2^2. All the calculated structures are optimized with tight convergence threshold both for the energy (10−10Ry10^{-10} Ry) and Feynman Hellman force (10−10Ry/Bohr10^{-10} Ry/Bohr). The self consistent calculations are converged with the energy cut-off of 10−8Ry10^{-8} Ry.

Results and Discussion

Optimisation of lattice parameters

The lattice parameters for all the compositions were obtained by varying the parameters and calculating the respective ground state energies. The equilibrium values were found using the Birch-Murnaghan equation of state [66] fit for the total energy as a function of the unit cell volume. The plots of total energy vs. the unit cell volume are shown in Figure 1. The calculated lattice parameters values, 6.104 Å (for x=0.0), 6.087 Å (for x=0.2), 6.083 Å (for x=0.4), 6.065 Å (for x=0.6), 6.050 Å (for x=0.8) and 6.04 Å (for x=1.0) are in well agreement with the experimentally reported lattice parameters 6.076 Å, 6.051 Å, 6.040 Å, 6.034 Å, 6.014 Å, 5.98 Å for x = 0.0, 0.2, 0.4, 0.6, 0.8, and 1.0 respectively, which follow similar trend with change in the composition[51, 52].

Total energy versus volume plots for Co$_2$Ti$_{1-x}$V$_x$Sn

Figure 1. Total energy vs. volume of the unit cell for Co2_2Ti1−x_{1-x}Vx_xSn (xx = 0.0, 0.2, 0.4, 0.6, 0.8, 1.0). The Birch-Murnaghan equation of state is used to determine the equilibrium values [66].

Band structure calculations for stoichiometric Co2_2TiSn and Co2_2VSn Heusler compounds

The band structures calculated using plane wave based pseudo-potential for the end (stoichiometric) compositions, with spin-orbit coupling (SOC), are shown in Figure 2. The band structures for both the stoichiometric compositions, Co2_2TiSn and Co2_2VSn, have been calculated using the Heusler (L21_1) cubic structure with space group Fm3ˉmFm\bar{3}m. In the conventional unit cell of this structure,

Crystal structure, Brillouin zone, and spin-orbit coupled band structures of Co$_2$TiSn and Co$_2$VSn

Figure 2. (a) Crystal structure of Co2_2TiSn. Co atoms are represented by green spheres, Ti atoms by blue spheres, and Sn atoms by yellow spheres. (b) Brillouin zone showing the high-symmetry points and the k-path followed in the band structures for the primitive unit cell. (c),(e) Calculated band structures of Co2_2TiSn and Co2_2VSn with spin-orbit coupling in the [110] quantization direction. (d),(f) Calculated band structures of Co2_2TiSn and Co2_2VSn with spin-orbit coupling in the [1] quantization direction. The red circles indicate the location of the crossings in the Co-Y (Y = Ti, V) hybridized 3d bands.

Co occupies the 8c (1/4, 1/4, 1/4) Wyckoff position, Ti (or V) occupies 4b (1/2, 1/2, 1/2), and Sn is at 4a (0, 0, 0), as shown in Figure 2(a) for Co2_2TiSn as an example.

Figure 2 shows the spin-orbit coupled band structures along the high symmetry lines in the BZ for Co2_2TiSn and Co2_2VSn with magnetization oriented along the [110] and [1] directions. Red circles mark the nodal lines of interest which may form the Weyl nodes. An analysis of the hybridisation and symmetry of these nodal lines is detailed in the appendix. In Co2_2TiSn, the nodal line remains unaffected when the magnetization is oriented in the [1] direction (Figure 2(d)), but very slight gaps occur when it is oriented in the [110] direction (Figure 2(c)). In the band structure for the [110] magnetization direction (Figure 2(c)), the nodal line crossing along Γ−W\Gamma- W has a very small gap, not visible in the figure, while the crossings along Γ−X\Gamma- X and Γ−K\Gamma- K remain unaffected. The crossings of the nodal line bands with the surrounding band along Γ−W\Gamma- W and Γ−K\Gamma- K also have gaps, according

to the magnetization direction, as can be seen next to the red circles in the figures (Figure 2(c) and Figure 2(d)). In Co2_2VSn, these nodal lines lie entirely below the Fermi energy, as seen in Figure 2(e) and Figure 2(f).

Bloch spectral functions for Co2_2Ti1−x_{1-x}Vx_xSn

For disordered compounds, it is difficult to determine the EE versus kk dispersion relations using methods for periodic ordered systems, such as the plane wave pseudo potential based DFT calculations. One approach is to construct a supercell to add the substituted element in the required ratio and calculate the dispersion relations. However, this results in complex band structures with additional bands due to symmetry. These supercell bands can then be unfolded to get an effective band structure[69, 70]. Using this approach to calculate the dispersion for a range of compositions is cumbersome and is feasible only for specific compositions.

Here, we use Bloch spectral functions to represent the electronic structure. The Bloch spectral function AB(k,E)A_{\mathrm{B}}(\mathbf{k}, E), defined as the Fourier transform of the Green’s function G(r,r′,E)G(\mathbf{r},\mathbf{r}',E), can be written as

AB(k,E)=−1πNIm⁡Tr⁡{∑n,n′eik(Rn−Rn′)×∫Ωd3rG(r+Rn,r+Rn′,E)}(1)A_{\mathrm{B}}(\mathbf{k}, E) = -\frac{1}{\pi N} \operatorname{Im}\operatorname{Tr}\left\{\sum_{n,n'} e^{i\mathbf{k}(\mathbf{R}_{n}-\mathbf{R}_{n'})} \times\int_{\Omega} d^{3}rG(\mathbf{r}+\mathbf{R}_{n},\mathbf{r}+\mathbf{R}_{n'},E)\right\} \tag*{(1)}

This function can be interpreted as the k-resolved density of states [55].

The Bloch spectral function (BSF) plots are shown in Figure 3. The nodal line can be seen shifting downward with respect to the Fermi energy as the concentration of V increases. At x=0.4x = 0.4, the point of highest energy of the nodal line tunes with the Fermi energy, along Γ−K\Gamma-K. This has been also seen in the Fermi surface plots (Figure 4) where for x=0.4x = 0.4, the two bands touch at the extremities, along Γ−K\Gamma-K. For higher V doped composition e.g. x=0.6x = 0.6, the nodal lines lie entirely below the Fermi energy. This means that for all compositions having V concentration in the range of 0.6≤x≤10.6 \leq x \leq1, the nodal lines lie entirely below the Fermi level.

Bloch spectral function plots of Co₂Ti₁₋ₓVₓSn for the primitive unit cell

Figure 3. Bloch spectral function plots of Co₂Ti₁₋ₓVₓSn for the primitive unit cell. The majority and minority spin states are represented by the blue and red lines, respectively. The nodal line can be seen shifting downwards with respect to the Fermi level as the concentration of V increases, tuning with the Fermi level at x=0.2x = 0.2 and x=0.4x = 0.4.

Fermi surface plots and Brillouin zone diagrams

Figure 4. Fermi surface plots of Co2_2Ti1−x_{1-x}Vx_xSn with chemical potential set at the Fermi energy for the spin polarized calculations without SOC. Majority spin states are presented in blue. Since all the compositions are half-metallic, there are no minority spin states at the Fermi level. On the right is a diagram of the Brillouin zone (BZ) in the conventional unit cell setting showing the high-symmetry lines and points, along with the Fermi surface cross-section (cut through the BZ at kz=0k_z = 0). The dotted shaded square region shows the first BZ.

A distinct feature of the BSF plots of the substituted compounds are the broadening of the majority bands. This broadening occurs in the energy range -0.5 eV to 2.0 eV. These are the same Co-X (X = Ti, V) hybridized

3d3d bands which form the nodal lines of interest. In the substituted compounds, the bands in this energy range are primarily formed by the 3d3d states on the 4b Wyckoff position, which contain the Ti and V atoms, and have a negligible contribution from Co atoms. The Co atoms in the substituted compounds have more contribution in the states below the nodal lines. The broadening in the bands occurs due to the randomly substituted additional 3d3d electron of the V atom. Since the band corresponding to the additional electron has a different energy, random fluctuations are induced in the energy window of the 3d3d states. The new electronic state manifests as an intermediate state, which can be seen becoming more well defined as the concentration of V increases.

Fermi surface

The evolution of the Fermi surface with respect to the V concentration can be seen in Figure 4. These calculations were done by using the primitive unit cell, however, the data is represented in the conventional settings (kxk_x, kyk_y, kzk_z axis) of the BZ for better presentation. The Fermi surface plots show the electronic states in the xyxy-plane of the BZ, at kz=0k_z = 0, lying on the Fermi energy. On the right is a schematic diagram showing the high-symmetry points in the Brillouin zone and a cross-section of the Brillouin zone at kz=0k_z = 0. The intermediate state formed by the addition of the 3d3d V electron can be seen becoming more well-defined along the X−ΓX-\Gamma and W−KW-K directions as the concentration of V increases. The bands which form the nodal lines can be seen clearly in the Fermi surface plots; one has a Fermi surface around the Γ\Gamma point and the other around the KK point. At x=0.2x = 0.2, the nodal line tunes with the Fermi energy along Γ−W\Gamma-W, as can be seen in both the BSF and Fermi surface plots. At x=0.4x = 0.4, the Fermi surface plot shows the two bands touching at the extremities, along Γ−K\Gamma-K. For 0.6≤x≤10.6 \le x \le1, the nodal lines lie entirely below the Fermi energy.

Density of states and magnetization

The stoichiometric compounds Co2_2TiSn and Co2_2VSn have been reported as half-metallic ferromagnets [44, 71, 72, 73, 74]. To investigate the half-metallic character as a function of chemical disorder, we performed density of states (DOS) calculations as a function of xx in Co2_2Ti1−x_{1-x}Vx_xSn. The evolution of the density of states (DOS) is given in Figure 5. The Fermi energy always lies in the minority spin band gap for all compositions, indicating half-metallic behavior throughout. The magnitude of the gap increases slightly with the increase in V concentration, and the gap for the stoichiometric compounds is in good agreement with the literature. The band gap (ΔE\Delta E) for compositions x=0.0x=0.0, 0.2, 0.4, 0.6, 0.8 and 1.0 is found to be 0.491 eV, 0.505 eV, 0.518 eV, 0.518 eV, 0.532 eV and 0.546 eV, respectively. This reveals that the ΔE\Delta E is slightly increasing with increasing V substitution in place of Ti.

Density of states of Co$_2$Ti$_{1-x}$V$_x$Sn

Figure 5. Density of states of Co2Ti1−xVxSnCo_{2}Ti_{1-x}V_{x}Sn (xx=0.0, 0.2, 0.4, 0.6, 0.8 and 1.0). For each compound, the positive y-axis represents the density of the majority spin states, and the negative y-axis represents the minority spin states.

Having obtained the evaluation of nodal lines and half-metallic character, we turn our discussion regarding the magnetic behavior of Co2_2Ti1−x_{1-x}Vx_xSn alloys. The magnetic moments calculated for all the compounds are given in Table I. Interestingly the magnetic moment of Co increases initially and after that, it starts decreasing, which is in very well agreement with the experimental findings (Table I) [51, 52]. The magnetic moment of Co is oriented antiparallel with the Ti moment and parallel with the V moment. Ti has a low magnetic moment of around 0.1 μB\mu_B per atom, while V has a higher moment ranging from 0.73 to 0.88 μB\mu_B per atom. The total magnetic moment per formula unit obtained here shows an increasing trend with V substitution and found 3μB\mu_B, which is well agreement with previous reported literature [77]. Thus our all results are in accordance with the observed behavior in the experiments and explain the unusual large anomalous Nernst coefficient for the Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn as compared to the stoichiometric compound Co2_2TiSn [50].

xxExperimental (μB\mu_B) μCo\mu_{Co} [52]Calculated (μB\mu_B) μCo\mu_{Co}μTi\mu_{Ti}μV\mu_{V}μtotal\mu_{total}
0.00.981.078-0.117-2.03
0.20.981.097-0.1160.7192.23
0.41.071.097-0.1260.8302.43
0.60.911.091-0.1320.8732.63
0.80.881.089-0.1450.8782.82
1.00.601.094-0.8513.00

Table 1. Magnetic moments for Co2Ti1−xVxSnCo_{2}Ti_{1-x}V_{x}Sn (xx=0.0, 0.2, 0.4, 0.6, 0.8 and 1.0). The moments for individual atoms are given in units of μB\mu_B per atom, and the total moment is given in μB\mu_B per formula unit.

Weyl nodes, Fermi arcs and Berry curvatures

We combined the Wannier function basis set based technique starting from pseudo potential plane wave DFT band structure using the energy selective down-folding methodology to extract the Fermi arcs and the normalized Berry curvature. We have used the primitive cell, containing one formula unit of the atoms, for this calculations for the sake of simplicity. The calculated pairs of Weyl nodes with opposite chirality are shown in the table II. To understand the texture of the Weyl points and nodal lines in details, we have plotted these in the Figure 6-Figure 8. The Figure 6(a) shows the Fermi-arc of the Co2TiSnCo_{2}TiSn, calculated with chemical potential 278 meV above the Fermi energy. From this figure, it is clearly evident that a pair of Weyl nodes of opposite chirality (+1 and -1) designated by WP+ and WP- respectively, located in the momentum space (-0.274, -0.157, -0.448) and (0.274, 0.157, 0.448) respectively. To clarify the nature of the above mentioned Weyl nodes, we have plotted the normalized Berry curvatures (Figure 6(b)).

Calculated Weyl nodes and Fermi arcs for Co₂TiSn

Figure 6. Calculated Weyl nodes and Fermi arcs for the are shown for Co₂TiSn with chemical potential 278 mev above the Fermi energy. (a) shows the Weyl nodes of two opposite Chern numbers (WP+ and WP-) connected by Fermi arcs in the momentum space in the primitive Brillouin zone (shown in inset). (b) Normalized Berry curvatures show source and sink type of flux and the flow chart of the average position of Wannier charge centers (WCC) obtained by the Wilson-loop method applied on a sphere that encloses the two nodes of opposite chirality.

Calculated Weyl nodes and Fermi arcs for Co₂Ti₀.₅V₀.₅Sn

Figure 8. Calculated Weyl nodes and Fermi arcs are shown for the Co₂Ti₀.₅V₀.₅Sn in the twice supercell in primitive setting. (a) shows the two equivalent pairs of Weyl nodes with two opposite chirality [WP1+ (WP2+) and WP1- (WP2-)] of +1 and -1 respectively. Insets show the WCC for the two paris separately, running in the opposite direction in the K-space. (b) and (c) show the normalized Berry curvatures for opposite chirality (source and sink type of flux) for WP1 and WP2 respectively.

The normalized Berry curvatures indicate that the flux at these two Weyl points (WP) are opposite in chiral nature, WP− is sink type, where the flux is moving inward whereas, the WP+ is more like source type, where the flux comes outward from the point. These analysis confirm the opposite chiral nature of these two Weyl nodes. Moreover, we also calculated the flow chart of the average position of Wannier charge centers (WCC) obtained by the Wilson-loop method applied on a sphere that encloses these two nodes of opposite chirality and we found that the WCC is moving in the two opposite directions, one is from south to north (WP-) and another is from north to south (WP+), confirming the opposite chiral nature. We did the similar exercise for the Co2VSnCo_{2}VSn Weyl nodes are shown for the chemical potential 227 meV below the Fermi energy and we found that the WP of opposite chiralities are located in the (-0.273,-0.150,-0.441) and (0.273,0.150,0.441) with Chern numbers -1 and +1 respectively, as shown in the bottom panel of Figure 7(b). Point to be noted that, the main features of the Fermi arcs and the normalized Berry curvatures of Co2VSnCo_{2}VSn and Co2TiSnCo_{2}TiSn are very similar, which is consistent with the result found from the band structure calculations, which show very similar energy dispersion. The main difference is that the chemical potential for the Fermi arcs, is above and below of the Fermi energy for the Co2TiSnCo_{2}TiSn and Co2VSnCo_{2}VSn, respectively.

Calculated Weyl nodes and Fermi arcs for Co₂VSn

Figure 7. Calculated Weyl nodes and Fermi arcs are shown for Co₂VSn with chemical potential 227 mev below the Fermi energy. (a) shows the Weyl nodes of two opposite Chern numbers (WP+ and WP-) connected by Fermi arcs in the momentum space in the primitive BZ. (b) Normalized Berry curvatures show source and sink type of flux and the flow chart of the average position of Wannier charge centers (WCC) obtained by the Wilson-loop method applied on a sphere that encloses the two nodes of opposite chirality.

In the 50% V doped compound, due to the reduction of some symmetry elements due to V substitution within the same crystal structure, the WP pairs do not appear symmetrically in the momentum space, as highlighted in the table II. It should be noted that, due to the two times supercell of the primitive cell is being used to accommodate 50% doping in the DFT band structure calculations followed by Wannier interpolation, the number of bands and the Weyl points band crossing near the Fermi energy is also twice compared to that of the undoped compounds. However, if we consider any one pair of the Weyl nodes, say WP1±, the main features of the Fermi arcs are very similar to that of the two stoichiometric compositions, which ensures the consistency of the calculations. In the Figure 8(a), we have shown two pairs of Weyl nodes, designated by WP1 and WP2, and the connected nodal lines between the opposite chiral WP1 (and WP2) points having Chern number +1 and -1, designated by WP1+ (WP2+) and WP1- (WP2-) respectively, which are appearing very close to the Fermi energy. The Figure 8(b)-(c) show the normalized Berry curvatures of two opposite chirality Weyl points for the both WP1 and WP2, respectively. Important to note that, for the doped compound the Weyl points are appearing very close to the Fermi energy, however not exactly at the same chemical potentials, resulting the Fermi arcs connected through these Weyl points forming some sort of nodal lines (as

CompoundCoordinates in K-spaceChemical Potential (meV)Chern number
Co₂TiSn-0.270 -0.167 -0.448278-1 (WP-)
0.274 0.157 0.448278+1 (WP+)
Co₂Ti₀.₅V₀.₅Sn-0.083 -0.368 0.2237-1 (WP1-)
0.142 -0.160 0.34518+1 (WP1+)
0.095 0.180 -0.40614-1 (WP2-)
0.035 0.371 -0.217-23+1 (WP2+)
Co₂VSn-0.273 -0.150 -0.441-227-1 (WP-)
0.273 0.150 0.441-227+1 (WP+)

Table II. Representative coordinates in the momentum space in the primitive unit cell setting of the Weyl nodes with their chemical potentials with respect to the Fermi energy together with corresponding Chern number. The Co₂TiSn and Co₂VSn calculations are done with the primitive cell contaning one fourmula unit of atoms, while the Co₂Ti₀.₅V₀.₅Sn calculations are done with the two times supercell of the primitive cell to accommodate 50% doping level.

evident from the Figure 8(a). The chemical potentials of the corresponding Weyl points were mentioned in the table II. The nature of the two pairs of the Weyl nodes are clear from the sink and source type of normalized Berry curvatures and the oppositely running WCC as shown in the inset of Figure 8(a). From these analysis we showed that via chemical doping we can tune the nodal line position in the energy spectrum as well as the nature of the Fermi arcs.

Anomalous Hall conductivity

The anomalous Hall effect/conductivity is direct consequence of the Berry curvature of the electronic band structure near the Fermi level, which act as pseudo-magnetic field in momentum space.The Berry curvature near the Fermi level introduces a transverse momentum in electron motion and derives large anomalous Hall conductivity(AHC). So in our case the middle composition is interest of research due to the fact that Weyl nodes are situated near the Fermi level.To substantiate our compositional dependent theoretical analysis on variation of position of Weyl point in band structure, we theoretically calculated the AHC with the expectation that large AHC should exhibit around the mid composition. To calculate the intrinsic anomalous Hall conductivity (AHC) for the pure and doped systems, the conventional unit cells have been considered (unless otherwise specified). The Bloch wave functions are projected into maximally localized Wannier functions in order to compute the intrinsic AHC. The intrinsic AHC is proportional to the Brillouin zone (BZ) summation of the Berry curvature over all occupied states [63, 75, 78]

σxy=−e2ℏ∑n∫BZdk(2π)3Ωn,z(k)fn(k),(2)\sigma^{xy}=-\frac{e^2}{\hbar}\sum_n\int_{\mathrm{BZ}}\frac{\mathrm{d}\mathbf{k}}{(2\pi)^3}\Omega_{n,z}(\mathbf{k})f_n(\mathbf{k}), \tag*{(2)}

where fn(k)f_n(\mathbf{k}) is the Fermi distribution function for the band nn, Ωn,z(k)\Omega_{n,z}(\mathbf{k}) is the zz component of the Berry curvature at the wave vector k\mathbf{k}. The Berry curvature is related to the Berry connection (An(k)A_n(\mathbf{k})) as

Ωn(k)=∇k×An(k),(3)\Omega_n(\mathbf{k}) = \nabla_{\mathbf{k}} \times\mathbf{A}_n(\mathbf{k}), \tag*{(3)}

where ``n'' is the band index and An(k)\mathbf{A}_n(\mathbf{k}) in terms of cell-periodic Bloch states ∣unk⟩=e−ik⋅r∣ψnk⟩|u_{n\mathbf{k}}\rangle= e^{-i\mathbf{k}\cdot\mathbf{r}}|\psi_{n\mathbf{k}}\rangle is defined as An(k)=⟨unk∣i∇k∣unk⟩\mathbf{A}_n(\mathbf{k}) = \langle u_{n\mathbf{k}}|i\nabla_{\mathbf{k}}|u_{n\mathbf{k}}\rangle [63].

Co2_2TiSn possesses the fcc L21L2_1 (space group # 225) structure which has three mirror planes, mxm_x, mym_y and mzm_z in the absence of any net magnetic moment. These mirror planes protect the gap-less nodal lines in the band structure in kx=0k_x = 0, ky=0k_y = 0, and kz=0k_z = 0 planes[39, 40]. To compute AHC, the spin-orbit coupling is introduced and the direction of the magnetization has been set along (001). Therefore, due to symmetry breaking of mirror planes the nodal lines in the kx=0k_x = 0 and ky=0k_y = 0 planes will exhibit a finite band gap while the gap-less nodal line will survive only along the magnetization direction (in the kz=0k_z = 0 plane) [39, 40]. However, due to helical distribution of Berry curvature around this gap-less nodal line, in the mirror plane, the total flux is zero and thereby it does not contribute to the intrinsic AHC [28]. Concurrently, the Berry curvature around the broken nodal lines is oriented along the direction of magnetization and contributes to the intrinsic AHC [28]. Our calculated intrinsic AHC value (99.38 S/cmS/cm and 92.40 S/cmS/cm for the primitive cell) at EFE_F for the pure system is in excellent agreement with the value (100 S/cmS/cm) reported in literature [28]. In addition to this, as it is shown in Figure 9 the intrinsic anomalous Hall conductivity is almost constant in the vicinity of EFE_F. Earlier, we have seen that the band crossing points of the pure compound (Co2_2TiSn) shift downwards with respect to the Fermi level (EFE_F) as the concentration of V increases (Figure 2), and particularly, two of such crossing points which lie in the unoccupied region (for the stoichiometric composition Co2_2TiSn) come close to EFE_F as composition approaches toward 50% V doped Co2_2TiSn. Hence, it is expected that the intrinsic AHC will be enhanced for the 50% V doped Co2_2TiSn compositions due to strong energy dispersion ∼2.5\sim2.5 times higher than the value that obtained near EFE_F of the pure compound [28]. Considering that the calculation with x= 0.4 doping concentration is computationally very expensive, we have chosen x= 0.5 to calculate intrinsic AHC, which is expected to provide us maximum value. While simulating AHC as a function of energy, around 0.25 eVeV above the EFE_F, we get ∼1.9\sim1.9 times higher AHC than that of the AHC at EFE_F. The same has been further confirmed when the bands are filled along the +ve energy (w.r.t EFE_F), which is achieved in the form of V doping. The calculated AHC along the direction of magnetization at EFE_F in 50 % V doped Co2_2TiSn is found to be 196.84 S/cmS/cm, nearly twice of the AHC in the pure system(Co2_2TiSn). Hence, the higher AHC value (in 50 % doped system as well as at ∼0.25\sim0.25 eVeV above the EFE_F in the pure compound) is attributed to the presence of nodal lines that are very close to EFE_F.

Comparison of Wannier interpolated and full electronic band structures and calculated intrinsic anomalous Hall conductivity

Figure 9. (a) Comparison of Wannier interpolated band structure (red) with the full electronic band structure (blue) of Co2_2TiSn. The Fermi energy is set to 0 eVeV. (b) The calculated intrinsic anomalous Hall conductivity at different energies. The conductivity is found to be constant in the vicinity of EFE_F (EF±0.2E_F \pm0.2 eVeV).

Conclusion

To summarise, we performed abab-initioinitio calculations on the Co-based Heusler compounds Co2_2Ti1−x_{1-x}Vx_xSn with x = 0.0, 0.2, 0.4, 0.6, 0.8 and 1.0. We have calculated the band structures, Bloch spectral functions and DOS using KKR-GF methods. We have also calculated the Fermi arcs, normalized Berry curvatures, WCC and intrinsic AHC for the x = 0.0, 0.5 and 1.0 compositions using Wannier90 interpolation of the plane wave pseudo-potential band structures. We found that nodal lines shift with V substitution and the point of highest energy of the nodal line responsible for Weyl nodes tunes with the Fermi energy for Co2_2Ti0.6_{0.6}V0.4_{0.4}Sn. For composition between x= 0.6 and 1 the nodal line lie entirely below the Fermi energy. We observed a half-metallic character for the entire range of composition. The magnetic moment on each Co atom as a function of V concentration increases linearly up to x=0.4 and thereafter, it starts decreasing. A detailed investigation reveals that the signature of the Weyl nodes and the Fermi arcs are more prominent near the Fermi energy for the 50% V doped compound in comparison to the stoichiometric compounds, which emphasize the importance of the chemical doping in the present series of compounds. The intrinsic AHC was found to increase by nearly twice for the 50% doped system as compared to the undoped composition. Our study suggests that Co2Ti1−xVxSn\mathrm{Co}_{2}\mathrm{Ti}_{1-x}\mathrm{V}_{x}\mathrm{Sn} series of Heusler alloys in general and Co2Ti0.6V0.4Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.6}\mathrm{V}_{0.4}\mathrm{Sn} composition in particular is important to investigate Weyl physics and various exotic transport phenomena.

Acknowledgments

SS thanks Science and Engineering Research Board of India for financial support through the award of Ramanujan Fellowship (grant no: SB/S2/RJN-015/2017), Early Career Research Award (grant no: ECR/2017/003186). SK thanks the Department of Science and Technology (DST), Govt. of India for providing INSPIRE research funding (Grant No. DST/INSPIRE/04/2016/000431; IFA16-MS91). S.W.D and J.M would like to thank CEDAMNF project financed by the Ministry of Education, Youth and Sports of Czech Republic, Project No. CZ.02.1.01/0.0/0.0/15.003/0000358 and also for the support by the GACR via the project 20-18725S. KKD and GKS acknowledge the DST-INSPIRE scheme for support through a fellowship.

Payal Chaudhary and Surasree Sadhukhan contributed equally to this work.

*[email protected]

Electronic structures of stoichiometric compounds

First, we look at the band structure of Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} (Figure 10(a)). When SOC is not considered, the compound possesses three mirror symmetries, MxM_x, MyM_y, and MzM_z (along the planes kx=0k_x = 0, ky=0k_y = 0, and kz=0k_z = 0), and three C4C_4 rotation axes kxk_x, kyk_y, and kzk_z. Due to these symmetries, there exist nodal lines in the momentum space on each of the three planes, formed by the crossings of the spin-up states of the Co-Ti hybridized 3d3d electron bands. These crossings can be seen in the band structures in Figure 10 along the Γ−X\Gamma- X, Γ−K\Gamma- K and Γ−W\Gamma- W high-symmetry lines, circled in blue. The energy of these nodal lines oscillates around the Fermi energy, reaching a maximum energy of 0.45 eV, along the Γ−K\Gamma- K direction, and a minimum of -0.35 eV, along the Γ−X\Gamma- X direction. The high-symmetry points and the directions followed in the band structures are the same as illustrated in Figure 2(b).

Spin-polarized band structures of Co2TiSn and Co2VSn

Figure 10. Spin-polarized band structures of Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn} with (a),(c) calculated lattice parameters and (b),(d) experimental lattice parameters. The black lines represent majority spin states, and the red lines represent minority spin states. The blue circles show the majority band crossings that form nodal lines in the momentum space.

When Ti is replaced by V, from Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} to Co2VSn\mathrm{Co}_{2}\mathrm{VSn}, an additional 3d3d electron is added. As a result, in Co2VSn\mathrm{Co}_{2}\mathrm{VSn}, one of the spin-up Co-V (previously Co-Ti) hybridized 3d3d bands, which had higher energy in Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn}, now lies on the Fermi energy. The Fermi energy itself increases, and the other states below the Fermi level only shift rigidly maintaining the same band shape. There is no change in the shape of the spin-down states across all energy levels, and the half-metallic character is retained.

The minority spin band gap and total magnetic moment per formula unit are 0.491 eV and 2.03 μB2.03\,\mu_B, and 0.546 eV and 3.01 μB3.01\,\mu_B, for Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn} respectively, in good agreement with literature [44, 71, 72, 73, 74]. The difference in the minority spin band gap, which arises from the splitting of the anti-bonding Co 3d3d orbitals [74, 76], is nearly 0.05 eV. This difference may be attributed to the difference in lattice parameters of the two compounds [73].

Figure 10 (a) and (c) show the spin-polarised, non spin-orbit coupled band structures of Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn} obtained using the calculated lattice parameters. Non-SOC band structures provide an insight into the symmetry of the bands, and how the symmetry changes when SOC is considered and Weyl nodes are formed. Through these structures we can also study how the hybridisation of these bands changes on inclusion of spin-orbit coupling. When SOC is considered, the mirror symmetries are broken according to the direction of magnetization. Due to this, the nodal lines gap out results in Weyl points, and there is a large Berry curvature in the vicinity of Fermi level.

Thermodynamic and dynamical stability

In order to examine the stability of the pure and doped compounds we have calculated the enthalpy of formation (Δ\Delta) for two end-compounds, Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn}, as shown in the following plot (Figure 11(a)). The negative values (dotted curves) of Δ\Delta for both the compounds suggest their thermodynamical stability, the same are already synthesized experimentally. Further, we have calculated the defect formation energy (ΔEf\Delta E_f) at the mid composition (Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn}), with respect to Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn}, using the relation

Defect formation energy and phonon dispersion relations

Figure 11. (a) Defect formation energy of Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn} varies with the chemical potential of Ti. The enthalpy of formation for two end-compounds, Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn}, are also shown in the same plot. (b) Phonon dispersion relations of Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn} crystal along the high-symmetry lines of the optimized structure.

ΔEf=E(Co2Ti0.5V0.5Sn)−E(Co2TiSn)−∑iΔniμTi,(4)\Delta E_f = E(\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn}) - E(\mathrm{Co}_{2}\mathrm{TiSn}) - \sum_i \Delta n_i \mu_{\mathrm{Ti}}, \tag*{(4)}

where the first two terms are the total energies of doped and pure systems respectively. Δni\Delta n_i is the change in the number of atoms of species ii, +ve for V (introduced) and -ve for Ti (removed). μTi\mu_{\mathrm{Ti}} is the chemical potential of the element Ti. Since we are calculating the ΔEf\Delta E_f with respect to Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn}, the range of elemental chemical potential of the species Ti is defined as μTi(bulk)+Δ(Co2TiSn)≤μTi≤μTi(bulk)\mu_{\mathrm{Ti}}(\mathit{bulk}) + \Delta(\mathrm{Co}_{2}\mathrm{TiSn}) \le\mu_{\mathrm{Ti}} \le\mu_{\mathrm{Ti}}(\mathit{bulk}). The variation of ΔEf\Delta E_f, versus μTi\mu_{\mathrm{Ti}}, in case of Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn} is shown in the same figure. The figure suggests that ΔEf\Delta E_f is more -ve when we approach towards the Ti poor condition which also suggests the possibility of vacancy formation. The results for Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn} further indicates that the compound will certainly be thermodynamically stable at any doping level. Because, the thermodynamically stable 50% doping composition is the highest doping concentration in Co2Ti1−xVxSn\mathrm{Co}_{2}\mathrm{Ti}_{1-x}\mathrm{V}_x\mathrm{Sn} series of Heusler alloys in which two end-compounds are also stable. The stability of Co2Ti0.5V0.5Sn\mathrm{Co}_{2}\mathrm{Ti}_{0.5}\mathrm{V}_{0.5}\mathrm{Sn} is further examined by calculating its phonon dispersion curve along the appropriate high-symmetry paths of the optimized structure. The absence of imaginary frequency in Figure 11(b) further suggests the dynamical stability of Co2Ti1−xVxSn\mathrm{Co}_{2}\mathrm{Ti}_{1-x}\mathrm{V}_x\mathrm{Sn} series of Heusler compounds.

Surface spectral functions

The calculated surface spectral function of [100] surface using slab model calculations using the Wannier derived Hamiltonian for the stoichiometric compositions Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn} are shown in the Figure 12(a) and (b) respectively. To understand the Fermi arcs in the surface state, we have plotted the surface spectral function along the k-path (kwwk^{ww}) connecting the pair of Weyl points of opposite chirality, say, WP+ and WP-. The figure clearly shows the bands responsible for the Fermi arcs connecting the WP- and WP+ points appearing in the surface state as well.

Calculated surface states for Co2TiSn and Co2VSn

Figure 12. Calculated surface states using slab calculations for the stoichiometric compositions (a) Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and (b) Co2VSn\mathrm{Co}_{2}\mathrm{VSn} for the [100] surface. The surface spectral function crossing one pair of Weyl points of opposite chirality in the BZ for Co2TiSn\mathrm{Co}_{2}\mathrm{TiSn} and Co2VSn\mathrm{Co}_{2}\mathrm{VSn} respectively. The dashed line represents the chemical potentials where the WP’s are appearing. The spectral function responsible for showing Fermi arcs are marked in the figure. Fermi energy set at zero in the energy axis.

References

  1. [1]J. Hu, S.-Y. Xu, N. Ni, and Z. Mao, Transport of topological semimetals, Annu. Rev. Mater. Res. 49, 207 (2019).DOI
  2. [2]N. P. Armitage, E. J. Mele, and A. Vishwanath, Weyl and Dirac semimetals in three-dimensional solids, Rev. Mod. Phys. 90, 015001 (2018).DOI
  3. [3]C. Shekhar, A. K. Nayak, Y. Sun, M. Schmidt, M. Nicklas, I. Leermakers, U. Zeitler, Y. Skourski, J. Wosnitza, Z. Liu, Y. Chen, W. Schnelle, H. Borrmann, Y. Grin, C. Felser, and B. Yan, Extremely large magnetoresistance and ultrahigh mobility in the topological Weyl semimetal candidate NbP, Nat. Phys. 11, 645 (2015).DOI
  4. [4]X. Wan, A. M. Turner, A. Vishwanath, and S. Y. Savrasov, Topological semimetal and Fermi-arc surface states in the electronic structure of pyrochlore iridates, Phys. Rev. B 83, 205101 (2011).DOI
  5. [5]S. Jia, S.-Y. Xu, and M. Zahid Hasan, Weyl semimetals, Fermi arcs and chiral anomalies, Nat. Mater. 15, 1140 (2016).DOI
  6. [6]D. Son and B. Spivak, Chiral anomaly and classical negative magnetoresistance of Weyl metals, Phys. Rev. B 88, 104412 (2013).DOI
  7. [7]A. A. Burkov, Anomalous Hall effect in Weyl metals, Phys. Rev. Lett. 113, 187202 (2014).DOI
  8. [8]C. Shekhar, N. Kumar, V. Grinenko, S. Singh, R. Sarkar, H. Luetkens, S.-C. Wu, Y. Zhang, A. C. Komarek, E. Kampert, Y. Skourski, J. Wosnitza, W. Schnelle, A. McCollam, U. Zeitler, J. Kübler, B. Yan, H.-H. Klauss, S. S. P. Parkin, and C. Felser, Anomalous Hall effect in Weyl semimetal half-Heusler compounds RP̄TiBi (R = Gd and Nd), Proc. Natl. Acad. Sci. USA 115, 9140 (2018).DOI
  9. [9]M. Ikhlas, T. Tomita, T. Koretsune, M.-T. Suzuki, D. Nishio-Hamane, R. Arita, Y. Otani, and S. Nakatsuji, Large anomalous Nernst effect at room temperature in a chiral antiferromagnet, Nat. Phys. 13, 1085 (2017).DOI
  10. [10]A. Sakai, Y. P. Mizuta, A. A. Nugroho, R. Sihombing, T. Koretsune, M.-T. Suzuki, N. Takemori, R. Ishii, D. Nishio-Hamane, R. Arita, P. Goswami, and S. Nakatsuji, Giant anomalous Nernst effect and quantum-critical scaling in a ferromagnetic semimetal, Nat. Phys. 14, 1119 (2018).DOI
  11. [11]K. Taguchi, T. Imaeda, M. Sato, and Y. Tanaka, Photovoltaic chiral magnetic effect in Weyl semimetals, Phys. Rev. B 93, 201202 (2016).DOI
  12. [12]C.-K. Chan, N. H. Lindner, G. Refael, and P. A. Lee, Photocurrents in Weyl semimetals, Phys. Rev. B 95, 041104 (2017).
  13. [13]F. de Juan, A. G. Grushin, T. Morimoto, and J. E. Moore, Quantized circular photogalvanic effect in Weyl semimetals, Nat. Commun. 8, 15995 (2017).DOI
  14. [14]G. B. Osterhoudt, L. K. Diebel, M. J. Gray, X. Yang, J. Stanco, X. Huang, B. Shen, N. Ni, P. Moll, Y. Ran, and K. S. Burch, Colossal mid-infrared bulk photovoltaic effect in a type-I Weyl semimetal, Nat. Mater. 18, 471 (2019).DOI
  15. [15]T. Morimoto and N. Nagaosa, Topological nature of nonlinear optical effects in solids, Sci. Adv. 2, e1501524 (2016).DOI
  16. [16]L. Wu, S. Patankar, T. Morimoto, N. L. Nair, E. Thewalt, A. Little, J. G. Analytis, J. E. Moore, and J. Orenstein, Giant anisotropic nonlinear optical response in transition metal monopnictide Weyl semimetals, Nat. Phys. 13, 350 (2017).
  17. [17]W. Feng, G.-Y. Guo, J. Zhou, Y. Yao, and Q. Niu, Large magneto-optical Kerr effect in noncollinear antiferromagnets Mn₃X (X= Rh, Ir, Pt), Phys. Rev. B 92, 144426 (2015).DOI
  18. [18]T. Higo, H. Man, D. B. Gopman, L. Wu, T. Koretsune, O. M. van’t Erve, Y. P. Kabanov, D. Rees, Y. Li, M.-T. Suzuki, S. Patankar, M. Ikhlas, C.L. Chien, R. Arita, R.D. Shull, J. Orenstein, and S. Nakatsuji, Large magneto-optical Kerr effect and imaging of magnetic octupole domains in an antiferromagnetic metal, Nat. Photonics 12, 73 (2018).DOI
  19. [19]S.-Y. Xu, I. Belopolski, N. Alidoust, M. Neupane, G. Bian, C. Zhang, R. Sankar, G. Chang, Z. Yuan, C.-C. Lee, S.-M. Huang, H. Zheng, J. Ma, D. S. Sanchez, B. Wang, A. Bansil, F. Chou, P. P. Shibayev, H. Lin, S. Jia, and M. Zahid Hasan, Discovery of a Weyl Fermion semimetal and topological Fermi arcs, Science 349, 613 (2015).DOI
  20. [20]S.-Y. Xu, N. Alidoust, I. Belopolski, Z. Yuan, G. Bian, T.-R. Chang, H. Zheng, V. N. Strocov, D. S. Sanchez, G. Chang, C. Zhang, D. Mou, Y. Wu, L. Huang, C.-C. Lee, S.-M. Huang, B. Wang, A. Bansil, H.-T. Jeng, T. Neuppert, A. Kaminski, H. Lin, S. Jia, and M. Zahid Hasan, Discovery of a Weyl Fermion state with Fermi arcs in Niobium Arsenide, Nat. Phys. 11, 748 (2015).
  21. [21]M. Zahid Hasan, S.-Y. Xu, I. Belopolski, and S.-M. Huang, Discovery of Weyl Fermion semimetals and topological Fermi arc states, Annu. Rev. Condens. Matter Phys. 8, 289 (2017).DOI
  22. [22]X. Huang, L. Zhao, Y. Long, P. Wang, D. Chen, Z. Yang, H. Liang, M. Xue, H. Weng, Z. Fang, X. Dai, and G. Chen, Observation of the chiral-anomaly-induced negative magnetoresistance in 3D Weyl semimetal TaAs, Phys. Rev. X 5, 031023 (2015).DOI
  23. [23]B. Yan and C. Felser, Topological materials: Weyl semimetals, Annu. Rev. Condens. Matter Phys. 8, 337 (2017).DOI
  24. [24]S. Kar and A. Jayannavar, A primer on Weyl semimetals: Down the discovery of topological phases, Asian J. Res. Rev. Phys. 4, 34-35 (2021).DOI
  25. [25]I. Belopolksi, K. Manna, D. S. Sanchez, G. Chang, B. Ernst, J. Yin, S. M. Zhang, T. Cochran, N. Shumiya, H. Zheng, B. Singh,G. Bian, D. Multer, M. Litskevich, X. Zhou, S. M. Huang, B. Wang, T.R. Chang, S.-Y. Xu, A. Bansal, C. Felser, H. Lin, and M. Zahid Hasan, Discovery of topological Weyl Fermion lines and drumhead surface states in a room temperature magnet, Science 365, 1278 (2019).
  26. [26]X. Liu, L. Li, Y. Cui, J. Deng, and X. Tao, A nonmagnetic topological Weyl semimetal in quaternary Heusler compound CrAlTiV, Appl. Phys. Lett. 111, 122104 (2017).DOI
  27. [27]K. Manna, L. Muechler, T.-H. Kao, R. Stinshoff, Y. Zhang, J. Gooth, N. Kumar, G. Kreiner, K. Koepernik, R. Car, J. Kübler, G.H. Fecher, C. Shekhar, Y. Sun, and C. Felser, From colossal to zero: controlling the anomalous Hall effect in magnetic Heusler compounds via Berry curvature design, Phys. Rev. X 8, 041045 (2018).
  28. [28]B. Ernst, R. Sahoo, Y. Sun, J. Nayak, L. Muechler, A. K. Nayak, N. Kumar, J. Gayles, A. Markou, G. H. Fecher, and C. Felser, Anomalous Hall effect and the role of Berry curvature in Co₂TiSn Heusler films, Phys. Rev. B 100, 054445 (2019).
  29. [29]R. P. Dulal, B. R. Dahal, A. Forbes, N. Bhattarai, I. L. Pegg, and J. Philip, Weak localization and small anomalous Hall conductivity in ferromagnetic Weyl semimetal Co₂TiGe, Sci. Rep. 9, 3342 (2019).
  30. [30]Y. Nakajima, R. Hu, K. Kirshenbaum, A. Hughes, P. Syers, X. Wang, K. Wang, R. Wang, S. R. Saha, D. Pratt, J.W. Lynn, and J. Paglione, Topological RPdBi half-Heusler semimetals: A new family of noncentrosymmetric magnetic superconductors, Sci. Adv. 1, e1500242 (2015).DOI
  31. [31]H. Kim, K. Wang, Y. Nakajima, R. Hu, S. Ziemak, P. Syers, L. Wang, H. Hodovanets, J. D. Denlinger, P. M. Brydon, D. F. Agterberg, M. A. Tanatar, R. Prozorov, and J. Paglione, Beyond triplet: Unconventional superconductivity in a spin-3/2 topological semimetal, Sci. Adv. 4, eaao4513 (2018).
  32. [32]G. Chang, S.-Y. Xu, X. Zhou, S.-M. Huang, B. Singh, B. Wang, I. Belopolski, J. Yin, S. Zhang, A. Bansil, H. Lin, and M. Zahid Hasan, Topological hopf and chain link semimetal states and their application to Co₂MnGa, Phys. Rev. Lett. 119, 156401 (2017).
  33. [33]H. Reichlova, R. Schlitz, S. Beckert, P. Szwkis, A. Markou, Y.-C. Chen, D. Kriegner, S. Fabretti, G. Hyeon Park, A. Niemann, S. Sudheendra, A. Thomas, K. Nielsch, C. Felser, and S. T. B. Goennenwein, Large anomalous Nernst effect in thin films of the Weyl semimetal Co₂MnGa, Appl. Phys. Lett. 113, 212405 (2018).
  34. [34]S. N. Guin, K. Manna, J. Noky, S. J. Watzman, C. Fu, N. Kumar, W. Schnelle, C. Shekhar, Y. Sun, J. Gooth, and C. Felser, Anomalous Nernst effect beyond the magnetization scaling relation in the ferromagnetic Heusler compound Co₂MnGa, NPG Asia Mater. 11, 16 (2019).
  35. [35]T. Sato, S. Kokado, M. Tsujikawa, T. Ogawa, S. Kosaka, M. Shirai, and M. Tsunoda, Signs of anisotropic magnetoresistance in Co₂MnGa Heusler alloy epitaxial thin films based on current direction, Appl. Phys. Express 12, 103005 (2019).DOI
  36. [36]A. Markou, D. Kriegner, J. Gayles, L. Zhang, Y.-C. Chen, B. Ernst, Y.-H. Lai, W. Schnelle, Y.-H. Chu, Y. Sun, and C. Felser, Thickness dependence of the anomalous Hall effect in thin films of the topological semimetal Co₂MnGa, Phys. Rev. B 100, 054422 (2019).
  37. [37]G.-H. Park, H. Reichlova, R. Schlitz, M. Lammel, A. Markou, P. S̆w̄ekis, P. Ritzinger, D. Kriegner, J. Noky, J. Gayles, Y. Sun, C. Felser, K. Nielsch, S. T. B. Goennenwein, and A. Thomas, Thickness dependence of the anomalous nernst effect and the mott relation of Weyl semimetal Co₂MnGa thin films, Phys. Rev. B 101, 060406 (2020).
  38. [38]J. Kübler and C. Felser, Weyl points in the ferromagnetic Heusler compound Co₂MnAl, Europhys. Lett. 114, 47005 (2016).DOI
  39. [39]G. Chang, S.-Y. Xu, H. Zheng, B. Singh, C.-H. Hsu, G. Bian, N. Alidoust, I. Belopolski, D. S. Sanchez, S. Zhang, H. Lin, and M. Zahid Hasan, Room-temperature magnetic topological Weyl Fermion and nodal line semimetal states in half-metallic Heusler Co₂TiX (X = Si, Ge, or Sn), Sci. Rep. 6, 38839 (2016).
  40. [40]Z. Wang, M. G. Vergniory, S. Kushwaha, M. Hirschberger, E. V. Chulkov, A. Ernst, N. P. Ong, R. J. Cava, and B. A. Bernevig, Time-reversal-breaking Weyl Fermions in magnetic Heusler alloys, Phys. Rev. Lett. 117, 236401 (2016).DOI
  41. [41]S. Chadov, S.-C. Wu, C. Felser, and I. Galanakis, Stability of Weyl points in magnetic half-metallic Heusler compounds, Phys. Rev. B 96, 024435 (2017).DOI
  42. [42]S. K. Kushwaha, Z. Wang, T. Kong, and R. J. Cava, Magnetic and electronic properties of the Cu-substituted Weyl semimetal candidate ZrCo₂Sn, J. Phys.: Condens. Matter 30, 075701 (2018).DOI
  43. [43]M. Yang, G. Gu, C. Yi, D. Yan, Y. Li, and Y. Shi, Magnetic and transport properties of Zr₁₋ₓNbₓCo₂Sn, J. Phys.: Condens. Matter 31, 275702 (2019).DOI
  44. [44]J. Barth, G. H. Fecher, B. Balke, S. Ouardi, T. Graf, C. Felser, A. Shkakbo, A. Weidenkaff, P. Klaer, H. J. Elmers, H. Yoshiakawa, S. Ueda, and K. Kobayashi, Itinerant half-metallic ferromagnets Co₂TiZ (Z = Si, Ge, Sn): Ab initio calculations and measurement of the electronic structure and transport properties, Phys. Rev. B 81, 064404 (2010).
  45. [45]J. Barth, G. H. Fecher, B. Balke, T. Graf, A. Shkakbo, A. Weidenkaff, P. Klaer, M. Kallmayer, H.-J. Elmers, H. Yoshiakawa, S. Ueda, K. Kobayashi, and C. Felser, Anomalous transport properties of the half-metallic ferromagnets Co₂TiSi, Co₂TiGe and Co₂TiSn, Phil. Trans. R. Soc. A 369, 3588 (2011).
  46. [46]R. Ooka, I. Shigeta, Y. Sukino, Y. Fujimoto, R. Y. Ume_ts_u, Y. Miura, A. Nomura, K. Yubuta, T. Ya- mauchi, T. Kanomata, and M. Hiroi, Magnetization and spin polarization of Heusler alloys Co₂TiSn and Co₂TiGa₀.₅Sn₀.₅, IEEE Magn. Lett. 8, 3101604 (2017).
  47. [47]L. Bainsla and K. G. Suresh, Spin polarization studies in half-metallic Co₂TiX (X = Ge and Sn) Heusler alloys, Curr. Appl. Phys. 16, 68 (2016).DOI
  48. [48]I. Shigeta, Y. Fujimoto, R. Ooka, Y. Nishisako, M. Tsujikawa, R. Y. Umetsu, A. Nomura, K. Yubuta, Y. Miura, T. Kanomata, M. Shirai, J. Gouchi, Y. Uwatoko, and T. Hiroi, Pressure effect on the magnetic properties of the half-metallic Heusler alloy Co₂TiSn, Phys. Rev. B 97, 104414 (2018).DOI
  49. [49]J. Hu, J. Niu, B. Ernst, S. Tu, A. Hamzić, C. Liu, Y. Zhang, X. Wu, C. Felser, and H. Yu, Unconventional spin-dependent thermopower in epitaxial Co₂Ti₀.₆V₀.₄Sn₀.₇₅ Heusler film, Solid State Commun. 299, 113661 (2019).DOI
  50. [50]J. Hu, B. Ernst, S. Tu, M. Kuveždić, A. Hamzić, E. Tafra, M. Basletić, Y. Zhang, A. Markou, C. Felser, A. Fert, W. Zhao, J. Ansermet, and H. Hu, Anomalous Hall and Nernst effects in Co₂TiSn and Co₂Ti₀.₆V₀.₄Sn Heusler thin films, Phys. Rev. Appl. 10, 044037 (2018).
  51. [51]R. Dunlap and G. Stroink, Conduction electron contributions to the Sn hyperfine field in the Heusler alloy Co₂Ti₁−xVₓSn, J. Appl. Phys. 53, 8210 (1982).DOI
  52. [52]W. Pendl Jr, R. Saxena, A. W. Carbonari, J. Mestnik Filho, and J. Schaf, Investigation of the magnetic hyperfine field at the Y site in the Heusler alloys (Y = Ti, V, Nb, Cr; Z = Al, Sn), J. Phys.: Condens. Matter 8, 11317 (1996).DOI
  53. [53]H. Ebert, M. Battocletti, D. Beneа, S. Bornemann, J. Braun, S. Chadov, M. Deng, H. Freyer, T. Huhne, D. Kodderitzsch, M. Kosuth, S. Lowitzer, S. Mankovsky, J. Minar, A. Perlov, V. Popescu, O. Sipr, Ch. Zecha, The munich SPRKKR package, version 6.3, URL:https://www.ebert.cup.uni-muenchen.de/index.php/de/. (2012).
  54. [54]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  55. [55]H. Ebert, D. Koedderitzsch, and J. Minar, Calculating condensed matter properties using the KKR-Green’s function method—recent developments and applications, Rep. Prog. Phys. 74, 096501 (2011).DOI
  56. [56]P. Soven, Coherent-potential model of substitutional disordered alloys, Phys. Rev. 156, 809 (1967).DOI
  57. [57]P. Soven, Contribution to the theory of disordered alloys, Phys. Rev. 178, 1136 (1969).DOI
  58. [58]P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, I. Dabo, A. D. Corso, S. de Gironcoli, S. Fabris, G. Fratesi, R. Gebauer, U. Gerstmann, C. Gougoussis, A. Kokalj, M. Lazzeri, L. Martin-Samos, N. Marzari, F. Mauri, R. Mazzarello, S. Paolini, A. Pasquarello, L. Paulatto, C. Sbraccia, S. Scandolo, G. Sciauzero, A. P. Seitsonen, A. Smogunov, P. Umari, and R. W. Wentzcovitch, Quantum Espresso: a modular and open-source software project for quantum simulations of materials, J. Phys. Condens. Matter 21, 395502 (2009).DOI
  59. [59]G. Kresse and J. Hafner, Ab initio molecular dynamics for liquid metals, Phys. Rev. B 47, 558 (1993).
  60. [60]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  61. [61]N. Marzari and D. Vanderbilt, Maximally localized generalized Wannier functions for composite energy bands, Phys. Rev. B 56, 12847 (1997).DOI
  62. [62]I. Souza, N. Marzari, and D. Vanderbilt, Maximally localized generalized Wannier functions for entangled energy bands, Phys. Rev. B 65, 035109 (2001).DOI
  63. [63]G. Pizzi, V. Vitale, R. Arita, S. Blügel, F. Freimuth, G. Géranton, M. Gibertini, D. Grech, C. Johnson, T. Koretsune, J. Ibáñez-Azpiroz, H. Lee, J.-M. Lihm, D. Marchand, A. Marrazzo, Y. Mokrousov, J. I. Mustafa, Y. Nohara, Y. Nomura, L. Paulatto, S. Pončé, T. Ponweiser, J. Qiao, F. Thöle, S. S. Tsirkin, M. Wierzbowska, N. Marzari, D. Vanderbilt, I. Souza, A. A. Mostofi, and J. R. Yates, Wannier90 as a community code: new features and applications, J. Phys. Condens. Matter 32, 165902 (2020).
  64. [64]Q. Wu, S. Zhang, H.-F. Song, M. Troyer, and A. A. Soluyanov, WannierTools: An open-source software package for novel topological materials, Comput. Phys. Commun. 224, 405 (2018).
  65. [65]D. Hamann, Optimized norm-conserving Vanderbilt pseudopotentials, Phys. Rev. B 88, 085117 (2013).DOI
  66. [66]F. Birch, Finite elastic strain of cubic crystals, Phys. Rev. 71, 809 (1947).DOI
  67. [69]V. Popescu and A. Zunger, Effective band structure of random alloys, Phys. Rev. Lett. 104, 236403 (2010).pubmed.ncbi.nlm.nih.gov/20867256
  68. [70]V. Popescu and A. Zunger, Extracting E versus k effective band structure from supercell calculations on alloys and impurities, Phys. Rev. B 85, 085201 (2012).
  69. [71]S. C. Lee, T. D. Lee, P. Blaha, and K. Schwarz, Magnetic and half-metallic properties of the full-Heusler alloys Co₂TiX (X = Al, Ga; Si, Ge, Sn; Sb), J. Appl. Phys. 97, 10C307 (2005).DOI
  70. [72]M. Hickey, A. H. Hussmann, S. Holmes, and G. Jones, Fermi surfaces and electronic structure of the Heusler alloy Co₂TiSn, J. Phys.: Condens. Matter 18, 2897 (2006).DOI
  71. [73]H. C. Kandpal, G. H. Fecher, and C. Felser, Calculated electronic and magnetic properties of the half-metallic, transition metal based Heusler compounds, J. Phys. D: Appl. Phys. 40, 1507 (2007).DOI
  72. [74]A. Aguayo and G. Murrieta, Density functional study of the half-metallic ferromagnetism in Co-based Heusler alloys Co₂MSn (M = Ti, Zr, Hf) using LSDA and GGA, J. Magn. Magn. Mater. 323, 3013 (2011).DOI
  73. [75]J. Kübler and C. Felser, Berry curvature and the anomalous Hall effect in Heusler compounds, Phys. Rev. B 85, 012405 (2012).DOI
  74. [76]I. Galanakis, P. Dederichs, and N. Papanikolaou, Slater-Pauling behavior and origin of the half-metallicity of the full-Heusler alloys, Phys. Rev. B 66, 174429 (2002).DOI
  75. [77]V. Shukla, S. O. Kumar, Destruction of half-metallicity in Co₂VSn Heusler alloy due to X-Y swapping disorder, J. Supercond. Nov. Magn. 33, 3615 (2020).DOI
  76. [78]X. Wang, J. R. Yates, I. Souza, and D. Vanderbilt, Ab initio calculation of the anomalous Hall conductivity by Wannier interpolation, Phys. Rev. B 74, 195118 (2006).

Paper details

vlnc:W_aq2gqe7c
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy