betaFeedback

WorksPhysics and Astronomy

Capacitance of Undoped Thin-Film Diodes

Abstract

The capacitance of thin-film diodes based on undoped semiconductors are dominated by injected charge carriers rather than doping-induced carriers. However, an analytical framework of the capacitance in these devices has remained elusive. Here, we derive an analytical description of the capacitance, fully accounting for injected charge carrier and electrode charge effects. Based on these findings, a method to extract the built-in voltage in these devices is presented. The theoretical framework is substantiated numerically by drift-diffusion simulations and experimentally on organic solar cells.

Thin-film diode devices based on undoped organic semiconductors have shown great promise for a variety of emerging applications, including light-emitting diodes, solar cells, sensors and photodetectors [1]. A key parameter of any thin-film diode is the built-in potential, providing the driving force for charge extraction in photovoltaic devices and controlling the onset for injection in light-emitting diodes. Capacitance-voltage (CC-VV) measurements have been widely used to probe the built-in voltage in semiconductor diode devices [2, 3]. To this end, the CC-VV characteristics are routinely analysed using Mott-Schottky analysis, where the built-in potential is extracted from the intercept in an inverse-square of the capacitance (1/C21/C^2) vs voltage plot [2]. However, Mott-Schottky analysis is only valid for sufficiently thick active layers with uniform doping. In contrast, Mott-Schottky analysis has been demonstrated to be highly unreliable in devices with thin active layers and/or low doping levels [4–6]. These devices instead behave as metal-insulator-metal (mm-ii-mm) diodes, characterized by fully depleted, effectively undoped active layers [7, 8]. The dark capacitance of a mm-ii-mm diode device, at low voltages, is ideally described by its geometric capacitance [9],

Cgeo=εε0d,(1)C_{\mathrm{geo}} = \frac{\varepsilon\varepsilon_0}{d}, \tag*{(1)}

where ε\varepsilon is the relative permittivity of the active layer, ε0\varepsilon_0 is the vacuum permittivity, and dd is the thickness of the active layer. However, in devices with injecting contacts (e.g., light-emitting diodes and solar cells), the capacitance typically exceeds CgeoC_{\mathrm{geo}}, generally showing a pronounced voltage dependence [10–13]. This has been attributed to injected charge carriers that have diffused into the active layer from the contacts [5, 11], resulting in an additional chemical contribution to the capacitance [14]. While analytical models for incorporating the chemical (or diffusion) capacitance have been proposed in the past [15, 16], these descriptions do not account for space charge effects, influencing both the charge within the active layer and the charge at the electrodes, and thus the associated electrode capacitance.

Injected charge carriers are known to induce space charge effects and energy level bending near the contacts in thin-film devices [17, 18, 19, 20]. On the other hand, any space charge within the active layer will inevitably also influence the charge on the electrodes [21], giving rise to an electrode capacitance that depends non-trivially on the voltage [22]. To the best of our knowledge, a rigorous analytical treatment which accounts for the interdependence between the space charge induced by injected carriers, their influence on the electrode charge, and the built-in potential has not yet been presented.

In this work, we present a theoretical framework incorporating the mutual dependence between injected charge carriers, the electrode charge, and the capacitance of sandwich-type devices based on undoped semiconductors. Based on these considerations, we derive analytical expressions describing the dark CC-VV characteristics of mm-ii-mm diodes at low frequencies, and its relation to the built-in potential. The analytical framework is validated by numerical drift-diffusion simulations. Based on the analytical findings, a method to extract the built-in potential from CC-VV characteristics of thin-film diode devices is proposed and demonstrated experimentally on organic solar cell devices.

We consider a thin-film diode structure constituting an active semiconductor layer sandwiched between two electrodes: a hole-injecting anode and an electron-injecting cathode. The anode contact is situated at x=0x = 0 and the cathode contact at x=dx = d, where xx denotes the position in the device. The active semiconductor layer is assumed to be undoped, corresponding to the case of a thin enough device where space charge effects induced by traps and dopants are negligible. In this case, the electron and hole densities, n(x)n(x) and p(x)p(x), in the active layer are related to the electric field E(x)E(x) through the Poisson equation:

∂E(x)∂x=ρ(x)εε0,(2)\frac{\partial E(x)}{\partial x} = \frac{\rho(x)}{\varepsilon\varepsilon_0}, \tag*{(2)}

where ρ(x)=q[p(x)−n(x)]\rho(x)=q\left[p(x)-n(x)\right] is the space charge density and qq is the elementary charge. Conversely, E(x)E(x) is related to the applied voltage VV via

V−Vbi,0=∫0dE(x) dx,(3)V-V_{\mathrm{bi},0}=\int_0^d E(x)\,\mathrm{d}x, \tag*{(3)}

where Vbi,0=[Φan−Φcat]/qV_{\mathrm{bi},0}=\left[\Phi_{\mathrm{an}}-\Phi_{\mathrm{cat}}\right]/q is the total built-in potential determined by the difference between the work function at the anode (Φan\Phi_{\mathrm{an}}) and cathode (Φcat\Phi_{\mathrm{cat}}) contact. Finally, the electron [hole] density at the cathode [anode] is assumed to be given by ncat=Ncexp⁡(−φcat/kT)n_{\mathrm{cat}}=N_{\mathrm{c}}\exp\left(-\varphi_{\mathrm{cat}}/kT\right) [pan=Nvexp⁡(−φan/kT)p_{\mathrm{an}}=N_{\mathrm{v}}\exp\left(-\varphi_{\mathrm{an}}/kT\right)], where φcat=Φcat−χp\varphi_{\mathrm{cat}}=\Phi_{\mathrm{cat}}-\chi_{\mathrm{p}} [φan=χn−Φan\varphi_{\mathrm{an}}=\chi_{\mathrm{n}}-\Phi_{\mathrm{an}}] is the injection barrier at the cathode [anode], χn\chi_{\mathrm{n}} [χp\chi_{\mathrm{p}}] is the electron affinity [ionization potential], NcN_{\mathrm{c}} [NvN_{\mathrm{v}}] is the effective density of electron [hole] states, kk is the Boltzmann constant, and TT the temperature. Note that qVbi,0=Eg−φan−φcatqV_{\mathrm{bi},0}=E_{\mathrm{g}}-\varphi_{\mathrm{an}}-\varphi_{\mathrm{cat}}, where Eg=χp−χnE_{\mathrm{g}}=\chi_{\mathrm{p}}-\chi_{\mathrm{n}} is the energy level gap.

The simulated CC-VV characteristics of an exemplary organic mm-ii-mm diode device with ohmic contacts and d=100d=100 nm is shown in Figure 1(a). For the simulations, a numerical drift-diffusion model is used [23]; the parameters used are provided in the Supplemental Material [24]. The capacitance is obtained at a sufficiently low frequency, in a regime where the CC-VV plot is not limited by transport and independent of frequency. A pronounced voltage dependence is observed, with the capacitance increasing with increasing forward bias. While the capacitance is slowly saturating towards the geometric capacitance in the reverse-bias. Importantly, as demonstrated in the inset of Figure 1(a), the inverse square of the capacitance (1/C21/C^2) does not follow the linear voltage dependence expected for a device dominated by (uniformly distributed) doping-induced carriers; the obtained 1/C21/C^2 vs VV plot instead suggests a strongly nonuniform charge carrier distribution, characteristic of injected carriers.

Image not extracted

Figure 1. (a) Simulated CC-VV characteristics of a 100 nm thick organic mm-ii-mm diode with two ohmic contacts. The capacitance is normalized to the geometric capacitance CgeoC_{\mathrm{geo}}. In the inset of (a) the corresponding Mott-Schottky plot (i.e., C−2C^{-2} vs VV) is included for comparison. (b) The energy level diagram of an mm-ii-mm diode for a forward biased voltage VV below the built-in potential. The charge −Qdispl-Q_{\mathrm{displ}} at the anode side is balanced by an equal but opposite charge QdisplQ_{\mathrm{displ}} at the cathode side. (c) Normalized CC-VV characteristics of a mm-ii-mm diode with two ohmic contacts simulated at different active layer thicknesses. (d) The same curves from (c) but replotted as (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} vs VV. The simulated curves are depicted by solid lines, while the analytical expressions Eq. (10) and Eq. (12) are indicated by dashed lines.

To obtain analytical insight into this behaviour, we consider steady-state conditions, corresponding to the low-frequency limit. Subsequently, an increase δV\delta V in the applied voltage VV will give rise to a change in the electric field across the device. This will on one hand induce a corresponding change in the surface charge stored at the electrodes; on the other hand, modify the electron and hole density profiles within the active layer. In the process, a charge δQdispl\delta Q_{\mathrm{displ}} will be displaced across the system. The associated device capacitance is given by

C=∂Qdispl∂V,(4)C=\frac{\partial Q_{\mathrm{displ}}}{\partial V}, \tag*{(4)}

where

Qdispl=Qan−Qcat2+qd2(nˉ+pˉ),(5)Q_{\mathrm{displ}}=\frac{Q_{\mathrm{an}}-Q_{\mathrm{cat}}}{2}+\frac{qd}{2}\left(\bar{n}+\bar{p}\right), \tag*{(5)}

in accordance with the law of charge conservation [24]. Here, Qan=εε0E(0)Q_{\mathrm{an}}=\varepsilon\varepsilon_0E(0) and Qcat=−εε0E(d)Q_{\mathrm{cat}}=-\varepsilon\varepsilon_0E(d) are the surface charge densities at the anode and cathode, respectively, while nˉ=(1/d)∫0dn(x) dx\bar{n}=(1/d)\int_0^d n(x)\,\mathrm{d}x and pˉ=(1/d)∫0dp(x) dx\bar{p}=(1/d)\int_0^d p(x)\,\mathrm{d}x.

Eq. (5) represents the displaced charge in a mm-ii-mm diode (with injecting contacts) for the case of an undoped, trap free active layer [see Figure 1(b)]. The first term accounts for the charge stored at the electrodes [21], while the second term accounts for a chemical charge stored within the active layer [25]. Note that in the absence of injected carriers (n=p=0n=p=0), the electric field will be uniform and given by E=[V−Vbi,0]/dE=[V-V_{\mathrm{bi},0}]/d; in this limit, Qdispl=Cgeo[V−Vbi,0]Q_{\mathrm{displ}}=C_{\mathrm{geo}}\left[V-V_{\mathrm{bi},0}\right] and C=CgeoC=C_{\mathrm{geo}}. In the presence of injected carriers, however, additional voltage dependences in both the chemical charge within the active layer and the charge stored at the electrodes are generally obtained, giving rise to an enhanced CC relative to CgeoC_{\mathrm{geo}}.

To account for injected carriers, we note that, for VV below Vbi,0V_{\mathrm{bi},0}, the charge within the active layer is primarily concentrated to regions near the electrodes. Holes dominate the space charge near the hole-injecting anode contact, while electrons dominate the space charge near the electron-injecting cathode contact. Subsequently, we may divide the active layer into a hole-dominated region (0≤x<x∗0\leq x<x^*) and an electron-dominated region (x∗<x≤dx^*<x\leq d), where x∗x^* is the width of the hole-dominated region. Inside the active layer sufficiently far away from both contacts, the space charge is negligible, and E(x)E(x) is constant and given by the bulk field EbulkE_{\mathrm{bulk}}. Then, integrating Eq. (2) in the hole-dominated region yields qpˉd=εε0[Ebulk−E(0)]q\bar{p}d=\varepsilon\varepsilon_0\left[E_{\mathrm{bulk}}-E(0)\right]. A similar integration in the electron-dominated region reveals qnˉd=εε0[Ebulk−E(d)]q\bar{n}d=\varepsilon\varepsilon_0\left[E_{\mathrm{bulk}}-E(d)\right]. Hence, Eq. (5) simplifies to

Qdispl=εε0Ebulk.(6)Q_{\mathrm{displ}}=\varepsilon\varepsilon_0E_{\mathrm{bulk}}. \tag*{(6)}

Note that for the case of a hole-only [electron-only] diode with an injecting anode [cathode] contact and a non-injecting cathode [anode] contact, we get Ebulk=E(d)E_{\mathrm{bulk}}=E(d) [Ebulk=E(0)E_{\mathrm{bulk}}=E(0)].

To obtain a general expression for EbulkE_{\mathrm{bulk}}, we approximate the hole density for x<x∗x<x^* by p(x)=panexp⁡(−qφ(x)/kT)p(x)=p_{\mathrm{an}}\exp\left(-q\varphi(x)/kT\right), where φ(x)=∫0xE(x′) dx′\varphi(x)=\int_0^x E(x')\,\mathrm{d}x'. This approximation is valid as long as the hole quasi-Fermi level remains flat in the accumulation region near the anode. Similarly, the electron density for x>x∗x>x^* is approximated by n(x)=ncatexp⁡[q(φ(x)−φ(d))/kT]n(x)=n_{\mathrm{cat}}\exp\left[q\left(\varphi(x)-\varphi(d)\right)/kT\right]. Then, by assuming that ρ(x)≈qp(x)\rho(x)\approx qp(x) for x<x∗x<x^*, and ρ(x)≈−qn(x)\rho(x)\approx-qn(x) for x>x∗x>x^*, Eq. (2) can be solved separately in these regions [20, 26, 27, 28]. Assuming that E(x)→EbulkE(x) \to E_{\mathrm{bulk}} and ρ(x)→0\rho(x) \to0 sufficiently far away from both contacts, we find

E(x)={Ebulkcoth⁡[q∣Ebulk∣x2kT+sinh⁡−1(q∣Ebulk∣λan2kT)],if x<x∗,Ebulkcoth⁡[q∣Ebulk∣(d−x)2kT+sinh⁡−1(q∣Ebulk∣λcat2kT)],if x>x∗,(7)E(x)= \begin{cases} E_{\mathrm{bulk}}\coth\left[\frac{q\lvert E_{\mathrm{bulk}}\rvert x}{2kT}+\sinh^{-1}\left(\frac{q\lvert E_{\mathrm{bulk}}\rvert\lambda_{\mathrm{an}}}{2kT}\right)\right], & \text{if } x<x^*,\\ E_{\mathrm{bulk}}\coth\left[\frac{q\lvert E_{\mathrm{bulk}}\rvert(d-x)}{2kT}+\sinh^{-1}\left(\frac{q\lvert E_{\mathrm{bulk}}\rvert\lambda_{\mathrm{cat}}}{2kT}\right)\right], & \text{if } x>x^*, \end{cases} \tag*{(7)}

where λan=2εε0kTq2pan\lambda_{\mathrm{an}}=\sqrt{\frac{2\varepsilon\varepsilon_0 kT}{q^2p_{\mathrm{an}}}} and λcat=2εε0kTq2ncat\lambda_{\mathrm{cat}}=\sqrt{\frac{2\varepsilon\varepsilon_0 kT}{q^2n_{\mathrm{cat}}}} are the Debye screening lengths at the anode and cathode, respectively.

Accordingly, the field depends strongly on xx near the injecting contacts but saturates rapidly to the constant value E(x)→EbulkE(x)\to E_{\mathrm{bulk}} inside the active layer for ∣Ebulk∣≫2kTqd\lvert E_{\mathrm{bulk}}\rvert\gg\frac{2kT}{qd}. After applying the boundary condition Eq. (3) to Eq. (7), we obtain

Ebulk=V−Vbi(V)d,(8)E_{\mathrm{bulk}}=\frac{V-V_{\mathrm{bi}}(V)}{d}, \tag*{(8)}

where Vbi(V)V_{\mathrm{bi}}(V) represents the effective built-in potential

Vbi(V)=Vbi,0−2kTqln⁡[12{1+(2kTdq[Vbi(V)−V]λan)2+1}]−2kTqln⁡[12{1+(2kTdq[Vbi(V)−V]λcat)2+1}](9)V_{\mathrm{bi}}(V)=V_{\mathrm{bi},0}-\frac{2kT}{q}\ln\left[\frac{1}{2}\left\{\sqrt{1+\left(\frac{2kTd}{q[V_{\mathrm{bi}}(V)-V]\lambda_{\mathrm{an}}}\right)^2}+1\right\}\right]-\frac{2kT}{q}\ln\left[\frac{1}{2}\left\{\sqrt{1+\left(\frac{2kTd}{q[V_{\mathrm{bi}}(V)-V]\lambda_{\mathrm{cat}}}\right)^2}+1\right\}\right] \tag*{(9)}

and depends on the applied voltage. Note that Vbi(V)V_{\mathrm{bi}}(V) is generally reduced compared to Vbi,0V_{\mathrm{bi},0}, owing to the energy-level bending induced by accumulation of injected charge carriers near the contacts, reflecting the true built-in electric field experienced by carriers inside the active layer. The corresponding magnitude of the energy-level bending at the anode and cathode contact is quantified by the second and third term on the right-hand-side of Eq. (9), respectively. A schematic energy level diagram of the situation is shown in Figure 1(b).

Finally, after inserting Eq. (8) and Eq. (9) into Eq. (6) and making use of implicit differentiation, the capacitance of an mm-ii-mm diode is obtained as

C(V)=Cgeo×[1−2kTq[Vbi(V)−V]×η(V)]−1(10)C(V)=C_{\mathrm{geo}}\times\left[1-\frac{2kT}{q[V_{\mathrm{bi}}(V)-V]}\times\eta(V)\right]^{-1} \tag*{(10)}

where η=ηan+ηcat\eta=\eta_{\mathrm{an}}+\eta_{\mathrm{cat}} with

ηan(cat)(V)=1−11+(2kTdq[Vbi(V)−V]λan(cat))2(11)\eta_{\mathrm{an(cat)}}(V)=1-\frac{1}{\sqrt{1+\left(\frac{2kTd}{q[V_{\mathrm{bi}}(V)-V]\lambda_{\mathrm{an(cat)}}}\right)^2}} \tag*{(11)}

and Vbi(V)V_{\mathrm{bi}}(V) given by Eq. (9). Alternatively, in terms of the inverse of the relative capacitance difference ΔC/Cgeo\Delta C/C_{\mathrm{geo}}, Eq. (10) can be rearranged as

[ΔC(V)Cgeo]−1=q2η(V)kT[Vbi(V)−V−2η(V)kTq](12)\left[\frac{\Delta C(V)}{C_{\mathrm{geo}}}\right]^{-1}=\frac{q}{2\eta(V)kT}\left[V_{\mathrm{bi}}(V)-V-\frac{2\eta(V)kT}{q}\right] \tag*{(12)}

where ΔC(V)=C(V)−Cgeo\Delta C(V)=C(V)-C_{\mathrm{geo}} is the excess capacitance induced by injected charge carriers inside the active layer. The above analysis is valid for voltages that are smaller than few kT/qkT/q below Vbi−2ηkT/qV_{\mathrm{bi}}-2\eta kT/q.

The analytical model [Eq. (10)] accurately reproduces the simulated voltage dependence of the capacitance for voltages below VbiV_{\mathrm{bi}}, as shown in Figure 1(a). Accordingly, ΔC(V)\Delta C(V) depends on both the dielectric properties of the active layer and the injecting contacts. Figure 1(c) shows the simulated CC-VV characteristics of a mm-ii-mm diode with two ohmic contacts at different active layer thicknesses. The corresponding (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} vs VV plot is shown in Figure 1(d). The effect of a varying hole-injection barrier φan\varphi_{\mathrm{an}} at the anode is demonstrated in Figure 2, showing the simulated CC-VV characteristics and (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} vs VV plots for the case of an electron-injecting and a non-injecting cathode contact. Comparison between numerical simulations (solid lines) and the analytical predictions (dashed lines) reveals an excellent agreement between the two, provided that the voltage is a few kT/qkT/q below Vbi−2ηkT/qV_{\mathrm{bi}}-2\eta kT/q.

Image not extracted

Figure 2. Simulated C/CgeoC/C_{\mathrm{geo}} and (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} as a function of voltage of a 100 nm-thick organic mm-ii-mm diode is shown in (a) and (b), respectively, for the case of varying hole injection barrier at the anode contact, assuming the cathode contact remains ohmic for electron injection. (c) and (d) show an otherwise identical situation to (a) and (b), respectively, but for the case of a non-injecting cathode contact having a fixed electron injection barrier of 0.5 eV. Simulated curves (solid lines) are depicted by solid lines, while the analytical expressions Eq. (10) and Eq. (12) are indicated by the dashed lines. For comparison, corresponding (ΔC(V)/Cgeo)−1/3(\Delta C(V)/C_{\mathrm{geo}})^{-1/3} curves of the data in (c) and (d) are plotted in the inset of (d).

In the limit of ohmic contacts, η\eta becomes independent of voltage. If both contacts are ohmic, corresponding to λan,λcat≪d\lambda_{\mathrm{an}},\lambda_{\mathrm{cat}}\ll d, then η=2\eta=2. In this regime, the inverse of ΔC(V)\Delta C(V) is directly proportional to the electric field inside the active layer, (ΔC)−1∝[Vbi(V)−V](\Delta C)^{-1}\propto[V_{\mathrm{bi}}(V)-V]. Note that VbiV_{\mathrm{bi}} decreases with increasing dd as per Eq. (9). Consequently, the CC-VV and (ΔC)−1(\Delta C)^{-1} vs VV curves of the thicker devices in Figure 1(c) and Figure 1(d), respectively, are shifted to smaller voltages. As the injection barrier is gradually increased at one of the contacts, as shown Figure 2(a) and (b), η\eta becomes voltage dependent and takes a value between η=1\eta=1 and η=2\eta=2. Eventually, as the injection barrier is large enough, corresponding to the case of a hole-only or electron-only diode with one ohmic and one non-injecting contact, η\eta again becomes independent of the applied voltage as η→1\eta\to1.

Finally, when both contacts become non-ohmic, a strong deviation from the ohmic contact regime is obtained. This is seen in Figure 2(c) and (d), where a transition from the ohmic contact regime to the weakly-injecting contact regime is obtained as φan\varphi_{\mathrm{an}} is increased. In the limit of two weakly-injecting contacts (λan,λcat≫d)(\lambda_{\mathrm{an}},\lambda_{\mathrm{cat}}\gg d), Eq. (10) reads

C(V)≈Cgeo+2(kT)2dq[Vbi,0−V]3(pan+ncat)(13)C(V)\approx C_{\mathrm{geo}}+\frac{2(kT)^2d}{q[V_{\mathrm{bi},0}-V]^3}(p_{\mathrm{an}}+n_{\mathrm{cat}}) \tag*{(13)}

with ΔC(V)\Delta C(V) instead obeying a (ΔC)−1/3∝[Vbi,0−V](\Delta C)^{-1/3}\propto[V_{\mathrm{bi},0}-V] type dependence; see inset of Figure 2(d). In this limit, ΔC≪Cgeo\Delta C\ll C_{\mathrm{geo}} generally applies, with ΔC\Delta C being directly proportional to the carrier densities at the contacts, approaching C→CgeoC\to C_{\mathrm{geo}} as the injection barrier is increased. Note that the energy-level bending is negligible in this regime, with the carrier profiles being purely exponential.

The origin of the voltage dependence of the capacitance, seen in Figure 1 and 2, can be traced back to the voltage modulation of the energy-level bending induced by the accumulation of injected carriers at the contacts. These carrier-accumulation regions are highly conductive, acting as virtual extensions of the contacts, effectively decreasing the thickness of the active layer. In accordance with Eq. (10), the effective width of the hole (electron) accumulation region at the anode (cathode) contact can be written as Δwan(cat)=2kTdq[Vbi−V]ηan(cat)\Delta w_{\mathrm{an(cat)}}=\frac{2kTd}{q[V_{\mathrm{bi}}-V]}\eta_{\mathrm{an(cat)}}. The accumulation regions become wider with increasing voltage and thickness, resulting in an increased capacitance. Larger VV and dd both translate into smaller magnitudes of the opposing electric field, allowing injected carriers to diffuse further into the active layer. Conversely, at high reverse bias, the strong electric field restricts diffusion of injected carriers, shrinking the accumulation regions and, ultimately, leading to a saturation of the capacitance to CgeoC_{\mathrm{geo}} with increasing reverse-bias voltage.

The above analytical framework can be applied to probe the built-in potential within the device. It should be stressed, however, that both Vbi(V)V_{\mathrm{bi}}(V) and η(V)\eta(V) have a non-negligible dependence on the voltage. To extract the (effective) built-in potential at V=0V=0, we therefore expand Eq. (12) to the first order to obtain a linear approximation for [ΔC(V)/Cgeo]−1[\Delta C(V)/C_{\mathrm{geo}}]^{-1} in this voltage region (see Supplemental Material). Provided that at least one of the contacts is ohmic, Eq. (12) can be approximated for voltages near V=0V=0 by

[ΔC(V)Cgeo]−1≈qC(0)2ηkTCgeo{Vbi−2ηkTq[1+CgeoC(0)]−fSV}(14)\left[\frac{\Delta C(V)}{C_{\mathrm{geo}}}\right]^{-1} \approx\frac{qC(0)}{2\eta kT C_{\mathrm{geo}}} \left\{V_{\mathrm{bi}}-\frac{2\eta kT}{q}\left[1+\frac{C_{\mathrm{geo}}}{C(0)}\right]-f_S V\right\} \tag*{(14)}

with the notation Vbi=Vbi(0)V_{\mathrm{bi}}=V_{\mathrm{bi}}(0) and η=η(0)\eta=\eta(0), and where

fS=η2−6[η+1η]+12(15)f_S=\eta^2-6\left[\eta+\frac{1}{\eta}\right]+12 \tag*{(15)}

Note that Eq. (14) takes the form [ΔC/Cgeo]−1=S×(V∗−V)[\Delta C/C_{\mathrm{geo}}]^{-1}=S\times(V^*-V), where SS is the slope and V∗V^* the VV-intercept. Hence, from a linear fit of [ΔC(V)/Cgeo]−1[\Delta C(V)/C_{\mathrm{geo}}]^{-1} near V=0V=0, η\eta and VbiV_{\mathrm{bi}} can be deduced from the corresponding slope and intercept. Specifically, in the limiting case when one contact is ohmic and the other contact is either ohmic (η=2\eta=2) or completely non-injecting (η=1\eta=1), where fS→1f_S\to1, we obtain S=qC(0)/(2ηkTCgeo)S=qC(0)/(2\eta kTC_{\mathrm{geo}}). In this limit, the value of VbiV_{\mathrm{bi}} can be directly calculated from the estimated SS and V∗V^* using Vbi=V∗+S−1×[1+C(0)/Cgeo]V_{\mathrm{bi}}=V^*+S^{-1}\times[1+C(0)/C_{\mathrm{geo}}].

To substantiate the theoretical framework, we tested the method on organic bulk-heterojunction solar cells with undoped active layers. Figure 3(a) shows dark CC-VV characteristics of an ITO/ZnO/PBDTTTC:PC71_{71}BM(170 nm)/MoO3_3/Ag device, reported by Zonno et al. [29]. The corresponding (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} versus VV plot is shown in Figure 3(b) with an estimated CgeoC_{\mathrm{geo}} of 20 nF/cm2^2. For comparison, the CC-VV characteristics of an 80 nm-thick DCV2_2-5T-Me(3,3):C60_{60} device, measured in this work, is provided in Figure 3(c). To ensure ohmic contacts, highly doped electrode interlayers were used for the DCV2_2-5T-Me(3,3):C60_{60} device. Furthermore, a frequency of 100 Hz was used for the CC-VV measurements to ensure that the capacitance was not limited by charge carrier transport. For details on processing conditions CC-VV measurement setup, see Ref. [30] and Ref. [31], respectively. The (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} versus VV plot for DCV2_2-5T-Me(3,3):C60_{60} is shown in Figure 3(d), with Cgeo=51.2C_{\mathrm{geo}} = 51.2 nF/cm2^2. The experimental (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} versus VV plots for both devices show a linear behaviour near V=0V = 0. The corresponding slopes suggest that η=2\eta= 2 for both cases (assuming T=300T = 300 K), consistent with bipolar mm-ii-mm diodes with two ohmic injecting

Image not extracted

Figure 3. Experimental CC-VV characteristics of organic bulk heterojunction solar cell device based on PBDTTT-C:PC71_{71}BM, reported by Zonno et al. [29], are shown in (a). The respective (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} versus VV plot is shown in (b), assuming Cgeo=20C_{\mathrm{geo}} = 20 nF/cm2^2. In (c), the measured CC-VV characteristics of a DCV2_2-5T-Me(3,3):C60_{60} device are shown. The corresponding (ΔC/Cgeo)−1(\Delta C/C_{\mathrm{geo}})^{-1} versus VV plot is shown in (d), with Cgeo=51.2C_{\mathrm{geo}} = 51.2 nF/cm2^2. The solid lines indicate linear fits based on Eq. (14) allowing for the VbiV_{\mathrm{bi}} at V=0V = 0 V to be extracted from the intercepts.

contacts. Subsequently, from the intercept, built-in potentials of Vbi=1.03V_{\mathrm{bi}} = 1.03 V for the PBDTTT-C:PC71_{71}BM device and Vbi=0.92V_{\mathrm{bi}} = 0.92 V for the DCV2_2-5T-Me(3,3):C60_{60} device were extracted at V=0V = 0. The obtained value for VbiV_{\mathrm{bi}} aligns well with the open-circuit voltage for the latter system [30, 32].

In conclusion, the effect of injected carriers on the capacitance of thin-film mm-ii-mm diode devices, based on undoped semiconductor active layers, has been clarified. After accounting for both the electrode charge and the space charge induced by the injected charge carriers within the active layer, an analytical description of the CC-VV characteristics is derived. Based on the analytical framework, a method to extract the built-in potential from CC-VV measurements in thin-film diode devices with intrinsic or lightly doped active layers (including organic solar cells and diodes) is presented. Additionally, the method can be used to identify and quantify ohmic contacts in these diodes. This method provides a complement to MottSchottky analysis that is only applicable to sufficiently doped active layers.

O.J.S. acknowledges funding from the Research Council of Finland through Project No. 357196. M.N. and J.B. acknowledge partial funding from the European Union’s Horizon 2020 research and innovation programme, grant number 101008701 (EMERGE).

References

  1. [14]J. Bisquert, Chemical capacitance of nanostructured semiconductors: its origin and significance for nanocomposite solar cells, Phys. Chem. Chem. Phys. 5, 5360 (2003).DOI
  2. [15]D. C. Tripathi and Y. N. Mohapatra, Diffusive capacitance in space charge limited organic diodes: analysis of peak in capacitance-voltage characteristics, Appl. Phys. Lett. 102, 253303 (2013).
  3. [16]V. Nandal and P. R. Nair, Anomalous scaling exponents in the capacitance-voltage characteristics of perovskite thin film devices, J. Phys. Chem. C 122, 27935 (2018).DOI
  4. [17]S. L. M. van Mensfoort and R. Coehoorn, Effect of Gaussian disorder on the voltage dependence of the current density in sandwich-type devices based on organic semiconductors, Phys. Rev. B 78, 085207 (2008).DOI
  5. [18]I. Lange, J. C. Blakesley, J. Frisch, A. Vollmer, N. Koch, and D. Neher, Bending in conjugated polymer layers, Phys. Rev. Lett. 106, 216402 (2011).pubmed.ncbi.nlm.nih.gov/21699323
  6. [19]P. de Bruyn, A. H. P. van Rest, G. A. H. Wetzelaer, D. M. de Leeuw, and P. W. M. Blom, Diffusion-limited current in organic metal-insulator-metal diodes, Phys. Rev. Lett. 111, 186801 (2013).pubmed.ncbi.nlm.nih.gov/24237546
  7. [20]O. J. Sandberg and A. Armin, Diode equation for sandwich-type thin-film photovoltaic devices limited by bimolecular recombination, PRX Energy 3, 023008 (2024).DOI
  8. [21]S. A. Hawks, B. Y. Finck, and B. J. Schwartz, Theory of current transients in planar semiconductor devices: insights and applications to organic solar cells, Phys. Rev. Applied 3, 044014 (2015).DOI
  9. [22]I. Zonno, H. Zayani, M. Grzeslo, B. Krogmeier, and T. Kirchartz, Extracting recombination parameters from impedance measurements on organic solar cells, Phys. Rev. Applied 11, 054024 (2019).DOI
  10. [23]O. J. Sandberg, K. Tvingstedt, P. Meredith, and A. Armin, Theoretical perspective on transient photovoltaic and charge extraction techniques, J. Phys. Chem. C 123, 14261 (2019).
  11. [24]See Supplemental Material for additional derivations and approximations.
  12. [25]P. Hartnagel, S. Ravishankar, B. Klingebiel, O. Thimm, and T. Kirchartz, Comparing methods of characterizing energetic disorder in organic solar cells, Adv. Energy Mater. 13, 2300329 (2023).
  13. [26]R. de Levie and H. Moreira, Transport of ions of one kind through thin membranes: I. general and equilibrium considerations, J. Membr. Biol. 9, 241 (1972).DOI
  14. [27]R. de Levie, N. G. Seidah, and H. Moreira, Transport of ions of one kind through thin membranes: II. nonequilibrium steady-state behavior, J. Membr. Biol. 10, 171 (1972).pubmed.ncbi.nlm.nih.gov/4669446
  15. [28]D. Cheyns, J. Poortmans, P. Heremans, C. Deibel, S. Verlaak, B. P. Rand, and J. Genoe, Analytical model for the open-circuit voltage and its associated resistance in organic planar heterojunction solar cells, Phys. Rev. B 77, 165332 (2008).DOI
  16. [29]I. Zonno, A. Martinez-Otero, J.-C. Hebig, and T. Kirchartz, Understanding Mott-Schottky measurements under illumination in organic bulk heterojunction solar cells, Phys. Rev. Applied 7, 034018 (2017).DOI
  17. [30]I. Wolansky, C. Hoffmann, M. Panhas, L. C. Winkler, F. Talnack, S. Hutsch, H. Zhang, A. Kirch, K. M. Yallum, H. Friedrich, J. Kublitski, F. Gao, D. Spoltore, S. C. B. Mannsfeld, F. Ortmann, N. Banerji, K. Leo, and J. Benduhn, Sensitive self-driven single-component organic photodetector based on vapor-deposited small molecules, Adv. Mater. 36, 2402834 (2024).
  18. [31]M. Kumar, C. Ding, J. Yang, O. J. Sandberg, M. Nyman, C.-Q. Ma, and R. Österbacka, Effect of thermal stress on the ion density and mobility distribution in perovskite solar cells, J. Phys. Chem. Lett. 17, 1527 (2026).DOI
  19. [32]M. Kaienburg, A. Jungbluth, I. Habib, S. Vajjala Kesava, M. Nyman, and M. K. Riede, Assessing the photovoltaic quality of vacuum-thermal evaporated organic semiconductor blends, Adv. Mater. 34, 2107584 (2022).DOI

Paper details

vlnc:W_axerbsdb
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents