Sustainable photocatalytic CO2 conversion using microalgae as a carbon-negative scavenger

Abstract

Photocatalytic CO2 conversion driven by solar energy is a highly promising approach in addressing rising atmospheric CO2 levels; however, its practical application remains limited by low conversion efficiency. In this study, a new strategy to enhance CO2 reduction toward CO and CH4 is proposed through the employment of microalgae as a sacrificial agent, and the efficiency is compared with conventional CO2 conversion without and with the use of microplastics as sacrificial agents. To realize this strategy, an AB2O6-type high-entropy oxide (HEO), (Cs1/7Ba4/7Bi2/7)(Nb1/2Ta1/2)2O6, with bi-polymorphy of layered perovskite and pyrochlore, is rationally designed. The HEO incorporates alkali metal cesium and alkaline earth metal barium to increase surface basicity for CO2 chemisorption, bismuth with its stereochemically active lone pairs for localized polarization and charge separation, and tantalum and niobium to form octahedral crystalline frameworks for charge transport. The utilization of microalgae during photocatalytic reactions leads to a remarkable enhancement in CO2 conversion compared to catalysis with or without using microplastics, with CO and CH4 production increasing by 10- and 4-fold, respectively, compared to the system using only HEO. These findings not only demonstrate a new family of polymorphic AB2-type HEOs for photocatalysis but also show the potential of microalgae as a sustainable sacrificial agent, offering an environmentally friendly pathway for efficient CO2 capture (through photosynthesis by microalgae) and CO2 conversion (through photocatalysis by HEOs).

Introduction

As a central component of the carbon cycle, the CO₂ concentration in a stable range is critical to sustaining life and preserving ecological balance on the Earth.[1] However, the excessive exploitation and use of fossil fuels, along with human-induced environmental issues such as deforestation and other industrial activities, have led to the release of large amounts of CO₂ into the atmosphere.[2] In addition to green energy transition policies to replace fossil fuels, methods for converting CO₂ into fuel products such as CO, CH₄, or other chemical compounds have emerged as a strategic approach for carbon mitigation and energy exploitation. Photocatalysis is a promising and sustainable method for CO₂ conversion,[3, 4] relying on suitable catalysts and solar radiation as the energy source. Nevertheless, properties of photocatalysts, including band structure, surface features, active sites, charge recombination under irradiation, stability, and toxicity, significantly affect the efficiency of the process and its practical application in CO₂ reduction.[5] In addition, most photocatalytic CO₂ conversion reactions are conducted in aqueous environments.[5] As a result, photogenerated electrons must compete between CO₂ reduction and H₂O reduction, posing a major challenge in the rational design of effective catalysts. In addition to challenges with the design of the catalyst that should be addressed, the need for a sacrificial agent is another issue in CO₂ conversion because most sacrificial agents, like alcohol, are produced by chemical methods that involve CO₂ emissions.

To address the first issue, recent research has increasingly focused on the photocatalytic activity of Nb- and Ta-based materials.[6, 7, 8, 9] Niobium and tantalum are group V transition metals in the periodic table and possess relatively low electronegativity. In their oxidized states, they typically exhibit a d⁰ electronic configuration.[10] The presence of empty d orbitals can facilitate efficient charge transfer.[11] Moreover, niobium and tantalum can provide octahedral frameworks to accommodate other elements. For example, several alkali and alkaline earth metal oxides, such as KNbO₃,[12, 13] NaNbO₃,[13] and BaNb₂O₆,[14] have been shown to be environmental semiconductors with high potential for photocatalytic applications. These Nb- and Ta-based catalysts show strong oxidative power while maintaining excellent structural stability.[15, 16, 17]

To further enhance photocatalytic efficiency and structural robustness, high-entropy ceramics have emerged as a novel design concept by integrating multiple cations into a single lattice.[18] The use of niobium and tantalum to generate octahedral frameworks of high-entropy oxides (HEO) offers opportunities to synergistically modulate electronic structure and catalytic properties by incorporating various cations. However, most attempts to use niobium and tantalum result in chemical separation of elements.[18, 19, 20, 21] One possible strategy to use the benefits of niobium and tantalum is designing stable crystal structures similar to perovskites (ABO3_3) or layered perovskites (AB2_2O6_6), where the A site is an element with a large atomic radius, such as alkali, alkaline earth, or rare earth elements, while the B site is an element with a smaller radius, such as transition metals. While there are still significant limits in selecting the elements for the ABO3_3-type perovskites, as discussed elsewhere,[20] the AB2_2O6_6-type compositions are expected to incorporate a wider range of elements in A and B sides with a wider possible polymorphism.

Regarding the second issue, designing photocatalytic processes that simultaneously use both electrons and holes is crucial for enhancing CO2_2 reduction efficiency and improving product yields. To consume holes, hole scavengers such as alcohol are commonly introduced into photocatalytic systems. However, the use of alcohol significantly increases the cost of photocatalytic CO2_2 conversion compared with alternative approaches such as biological, thermochemical, or electrochemical conversion.[5] Moreover, production of alcohol involves CO2_2 emissions, which negatively affect the carbon-neutrality of photocatalysis. Therefore, it is necessary to replace alcohol with other sacrificial agents that are inexpensive, abundant, and nature-friendly. Based on these requirements, microalgae can be considered a candidate for a sacrificial agent. Microalgae are well-known as photosynthetic organisms that are widely distributed in most aquatic environments.[22] Under conditions from normal to extremely harsh environments of light intensity, pH, and nutrient availability, microalgae can still sustain growth.[23] Unlike alcohol, whose production emits CO2_2, cultivating microalgae captures CO2_2 from the atmosphere through photosynthesis. The current study hypothesizes that the harvested microalgae can subsequently contribute to CO2_2 conversion by being employed as a sacrificial agent in photocatalysis.

In this study, a photocatalytic process is introduced in which microalgae are employed as a sacrificial agent to enhance CO2_2 conversion. A novel high-entropy material with the AB2_2O6_6 structure is designed and synthesized by high-pressure torsion (HPT)[24] and subsequent calcination for this process. The A site contains alkali metal cesium and alkaline earth metal barium to enhance CO2_2 chemisorption and bismuth to stereochemically activate lone pairs for charge separation via localized polarization.[11] In addition, a higher atomic percentage of barium compared to bismuth and cesium was chosen to (i) ensure proper occupation of the A-site cations within the cuboctahedral cavities, and (ii) limit the volatility of cesium during the high-temperature synthesis. Niobium and tantalum occupy the B site, constructing a robust octahedral framework that promotes charge carrier transport. Analysis using a catalytic system, illustrated in Figure 1, confirms that the integration of microalgae for CO2_2 conversion in the presence of the HEO (Cs1/7_{1/7}Ba4/7_{4/7}Bi2/7_{2/7})(Nb1/2_{1/2}Ta1/2_{1/2})2_2O6_6 leads to higher CO and CH4_4 production, compared to conventional photocatalysis or photocatalysis utilizing polyethylene terephthalate (PET) microplastics as a sacrificial agent. These results offer a new sustainable route to both CO2_2 capture (through photosynthesis) and CO2_2 conversion (through photocatalysis). A main benefit of this route is that its scavenger does not produce CO2_2 during its production (unlike alcohol), but it captures and converts CO2_2, which can be considered a carbon-negative sacrificial agent.

Schematic of the CO2 conversion experiment using microalgae as sacrificial agent

Figure 1. Schematics of the CO2_2 conversion experiment using microalgae as sacrificial agent.

Materials and methods

Reagents

Five metal oxides, including cesium tantalum oxide (CsTaO3_3, 99.9 %), barium peroxide (BaO2_2, 99 %), bismuth trioxide (Bi2_2O3_3, 99.9 %), niobium pentoxide (Nb2_2O5_5, 99 %), and tantalum pentoxide (Ta2_2O5_5, 99.9 %), were obtained from Mitsuwa Pure Chemical, Kojundo, and Fujifilm, Japan. Sodium bicarbonate (NaHCO3_3) and PET plastic powder were purchased from Nacalai Tesque and Fujifilm, Japan, respectively.

Synthesis of photocatalyst

To synthesize the HEO, the initial five metal oxides were calculated and weighed to form the formula (Cs1/7_{1/7}Ba4/7_{4/7}Bi2/7_{2/7})(Nb1/2_{1/2}Ta1/2_{1/2})2_2O6_6. Since some losses of Cs can occur at high temperatures, the amount of the element was calculated over the nominal values to reach the final composition after the synthesis. By considering BaNb2_2O6_6 as a reference, barium in the A site was kept high, while Cs was kept low to avoid chemical separation in the form of CsTaO3_3. These oxides were mixed by grinding in ethanol for 30 min. The resulting powder was then compressed into a small disc with a volume of 0.063 cm3^3 and a diameter of 1 cm. Subsequently, the disc was processed by HPT[24] under a pressure of 6 GPa, with 3 rotations at a speed of 1 rpm at ambient temperature. The HPT process was repeated once more after grinding under similar HPT treatment. The sample was calcined at 1373 K for 24 h, reprocessed by HPT, and recalcined under identical conditions to ensure elemental homogeneity.

Characterization of photocatalyst

The properties of the HEO were investigated by various analytical techniques. The crystal structure and phase composition of the HEO were determined through X-ray diffraction (XRD) using a Cu Kα\alpha radiation source. Raman spectroscopy analysis with a laser light source at a wavelength of 532 nm was used to determine molecular vibrations in the HEO. Scanning electron microscope (SEM) and energy-dispersive X-ray spectroscopy (EDS) were used to confirm the morphology and elemental distribution at the microscale. Furthermore, these results were corroborated by transmission electron microscopy (TEM) and scanning transmission electron microscopy (STEM) analyses at the nanoscale. TEM and STEM micrographs were obtained at 200 keV, including bright-field (BF), dark-field (DF), selected area electron diffraction (SAED), and high-resolution analyses. Using synchrotron radiation (beamline BL11 at the Saga Light Source), X-ray absorption spectroscopy (XAS) was conducted, which provided high-intensity and tunable beams that enabled detailed analysis of the atomic structure of the material. XAS consists of two complementary regions, including X-ray absorption near-edge structure (XANES) and extended X-ray absorption fine structure (EXAFS). XANES is sensitive to the electronic structure and oxidation states, whereas EXAFS characterizes bonding configurations, structural disorder, and neighboring atomic arrangements in the HEO. X-ray photoelectron spectroscopy (XPS) with Al Kα\alpha radiation and ultraviolet photoelectron spectroscopy (UPS) using a He I source were applied to identify elemental oxidation states and to estimate the valence band maximum (VBM) of the catalyst. UV-Vis spectroscopy in the 200-800 nm range was conducted to assess light absorption properties. Based on Kubelka-Munk theory and UV-Vis results, the band gap of the catalyst was determined. Charge carrier recombination involving photogenerated electrons and holes was investigated by the photoluminescence technique using a 325 nm excitation laser. In addition, oxygen vacancies in the samples were investigated by electron spin resonance (ESR) measurements performed at a microwave frequency of 9.4688 GHz to probe unpaired electrons.

Microalgae cultivation

In this study, microalgae were employed as sacrificial agents in the photocatalytic CO2_2 conversion. To collect microalgae, a laboratory-scale cultivation procedure was carried out. Initially, the wild-type Chlamydomonas reinhardtii CC-124 strain was supplied from the Chlamydomonas Resource Center (CRC), USA. The microalgae were cultured in petri dishes containing tris–acetate–phosphate (TAP) and agar medium, as suggested in the recipe on the CRC website. Specifically, 1 L of TAP medium was prepared from 20 mL of 1 M tris base, 1 mL of phosphate buffer II (10.8 g K2_2HPO4_4 and 5.6 g KH2_2PO4_4 per 100 mL), 10 mL of solution made from 20 g NH4_4Cl, 5 g MgSO4_4·7H2_2O, and 2.5 g CaCl2_2·2H2_2O per 500 mL, 1 mL of Hutner’s trace elements, and 1 mL of glacial acetic acid. For a solid medium, 15 g L−1^{-1} of agar was added. A continuous light source with an intensity of 0.048 mmol photons m−2^{-2}s−1^{-1} was maintained throughout the cultivation period (a 24 h/day light cycle) at 293 K. For scaling up the amount, the cultures were transferred from petri dishes into Erlenmeyer flasks containing TAP medium under ambient temperature conditions. The flasks were agitated on a rotary shaker at 150 rpm to facilitate gas exchange for microalgal growth. Once the microalgae reached 110 mL, the culture was transferred to a 15 L large-scale reactor containing TAP medium. The culture was further stirred and aerated under atmospheric conditions, then filtered through a 220 nm membrane filter. After achieving the desired biomass, 2.0 g of microalgae were collected and centrifuged for 10 min. The harvested cells were subsequently dehydrated by lyophilization to obtain the final product. Finally, the samples were refrigerated at 253 K, transported, and preserved for further use. Prior to photocatalytic experiments, the microalgae were characterized using Fourier transform infrared spectroscopy (FTIR) coupled with single-reflection attenuated total reflectance (ATR).

CO2_2 conversion experiments

Figure 1 illustrates the schematic of the CO2_2 conversion experiment. An 856 mL cylindrical-shaped photoreactor was placed on a magnetic stirrer operating at a speed of 420 rpm. For sample preparation, 100 mg of catalyst was added to the reaction vessel, followed by adding 4.2 g of bicarbonate and 500 mL of deionized (DI) water as a neutralized aqueous environment using a magnetic stirrer. Subsequently, 100 mg of the PET plastic powder or microalgae cluster, as sacrificial agents for holes, were introduced, depending on the experiment. For comparison with a conventional sacrificial agent, a similar experiment was conducted using 450 mL of DI water and 50 mL of methanol, corresponding to 10 vol% of the total solution. The lid is then sealed to ensure an anaerobic environment for the experiment. The lid was equipped with two valves connected to a thermostatic cooling system, enabling the experimental temperature to be maintained at 291 K. Next, a mercury lamp (1.4 W cm−2^{-2}) was placed in the void inside the lid as a radiation source for the experiment. A continuous stream of CO2_2 gas at a flow rate of 30 mL/min was then bubbled into the solution through an inlet pipe. Two gas chromatographs (GC), one connected with a methanizer and flame ionization detector (FID) and the other with a thermal conductivity detector (TCD), were connected to the outlet pipe to quantify gaseous products evolution (H2_2, CH4_4, and CO) generated from the photocatalytic CO2_2 conversion. A control test was first conducted under off-light conditions for 30 min to make sure that CO2_2 conversion did not occur in the absence of irradiation. Subsequently, the mercury lamp was switched on to initiate the reaction. Gas sampling was performed automatically at hourly intervals, and the concentration analysis data were displayed using monitoring software.

Following the photocatalysis, the reaction mixture was passed through a polytetrafluoroethylene wheel filter (Code: PTFE013045, pore size: 0.45 μm, radius: 6.5 mm) to separate the liquid phase. An aliquot of 20 mL of the resulting filtrate was placed in a separatory funnel and mixed with 5 mL of hexane, 2 mL of saturated KCl solution, and 2 mL of deionized water, then subjected to liquid–liquid extraction for 30 min. The upper organic layer was collected, and the lower layer was subjected to a second time extraction with an additional 5 mL of hexane to maximize the recovery of organic composition from the liquid phase. The organic extracts were subsequently dried by argon gas to concentrate the sample. For chemical composition identification, 1 μL of the concentrated extract was injected directly into gas chromatography-mass spectrometry (GC-MS). The GC analysis employed a CP-Sil 8CB capillary column with a split ratio of 50:1. The oven temperature was held at 313 K for 2 min, heated to 513 K at 4 K min−1^{-1}, and kept at 513 K for 2 min. Mass spectrometric analysis was carried out with an ion source temperature of 473 K, an interface temperature of 523 K, and an m/zm/z (ratio of mass to charge) scanning range of 50-700.

Results

Crystal structure and composition

Figure 2 describes the crystal structure of the material at different stages of synthesis. The XRD profile shows the transformation of the crystal structure from the initial mixture of oxides to new phases. It can be observed that after the first processing stage, where the sample was treated by HPT twice and subsequently calcinated, the resulting material (HPT + HPT + C) exhibits new diffraction peaks that differ in position and intensity compared to the peaks of the initial oxide mixture. This indicates a rearrangement of the elements in the crystal lattice structure to form a new oxide. This arrangement is further enhanced by repeating the HPT process and calcination. In this second processing stage, the peaks associated with the binary oxides completely vanish, while the new peaks become more separated and their intensity becomes higher. Figure 2 shows a more detailed observation of the HEO material after the synthesis process (HPT + HPT + C + HPT + HPT + C). The Rietveld refinement (Rwp=8.51%R_{\mathrm{wp}} = 8.51\%, Rp=6.07%R_{\mathrm{p}} = 6.07\%, Re=2.40%R_{\mathrm{e}} = 2.40\%, s=3.54s = 3.54) indicates that the material contains two phases: 56 wt% cubic (Fd3ˉmFd\bar{3}m space group, a=b=c=10.5183a = b = c = 10.5183 Å; α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ) and 44 wt% tetragonal (P4bmP4bm space group, a=b=12.519a = b = 12.519 Å, c=3.948c = 3.948 Å; α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ). The Fd3ˉmFd\bar{3}m space group is associated with a pyrochlore-type structure of AB2_2O6_6 oxides.[25] Meanwhile, the Pb4mPb4m space group is related to the AB2_2O6_6-type layered hexagonal perovskite structure, which is also similar to tetragonal tungsten bronze structures in tantalates, such as SrTa2_2O6_6 (unit cell: a=b=12.41a = b = 12.41 Å, c=3.90c = 3.90 Å, α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ) or BaTa2_2O6_6 (unit cell: a=b=12.60a = b = 12.60 Å, c=3.95c = 3.95 Å, α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ).[26] Figure 2 depicts the Raman spectra of the HEO acquired at four randomly selected positions. All Raman spectra show no significant differences, indicating a high level of material homogeneity. In addition, the structure of the HEO is also better understood through the different vibrational modes corresponding to each Raman peak. First, a peak at 152 cm−1^{-1} is related to lattice vibration.[4] Second, the peak at 252 cm−1^{-1} is assigned to Ba–O vibration in the crystal structure, representing a feature similar to the A-site position in perovskites.[20] Third, the peak at 499 cm−1^{-1} is assigned the A1g_{1g} + B1g_{1g} vibration.[27, 28] Meanwhile, the peak at 616 cm−1^{-1} can be attributed to the A1g_{1g} vibration mode.[27, 28] Finally, a low-intensity peak at 872.7 cm−1^{-1} should be related to the vacancy defects.[20]

Thermomechanical synthesis of HEO

Figure 2. Thermomechanical synthesis of HEO. (a) XRD spectra at each synthesis stage implemented by HPT and calcination, (b) XRD spectrum, corresponding Rietveld refinement, and real image (insert) of HEO. (c) Raman spectrum of HEO examined at four different sites.

Figure 3 illustrates the elemental distribution in the HEO using two techniques: SEM-EDS and STEM-EDS. Homogeneous elemental distribution is evident at the micrometer scale in fig:3a and at the nanometer scale in fig:3b. Elemental atomic percentages measured by SEM-EDS and STEM-EDS are listed in Table 1, indicating that, within the precision limits of EDS for quantitative chemical analyses, the final composition reaches the designed one, (Cs1/7Ba4/7Bi2/7)(Nb1/2Ta1/2)2O6(\mathrm{Cs}_{1/7}\mathrm{Ba}_{4/7}\mathrm{Bi}_{2/7})(\mathrm{Nb}_{1/2}\mathrm{Ta}_{1/2})_2\mathrm{O}_6, after evaporation of some cesium [29] and bismuth.[30]

Homogeneous arrangements of elements in HEO, showing SEM and HAADF micrographs with corresponding EDS mappings

Figure 3. Homogeneous arrangements of elements in HEO. (a) SEM micrograph with EDS mappings and (b) HAADF micrograph by STEM with corresponding EDS mappings for HEO.

Composition (at%)
CsBaBiNbTaO
SEM-EDS1.46.12.59.08.772.3
STEM-EDS1.46.43.19.97.671.6

Table 1. Elemental composition of HEO analyzed by SEM-EDS and STEM-EDS.

The cation oxidation states and the oxygen reduction state in the HEO were determined by fitted XPS spectra, as presented in Figure 4. The observed peaks for Cs 3d5/23d_{5/2}, Ba 3d5/23d_{5/2}, Bi 4f7/24f_{7/2}, Nb 3d5/23d_{5/2}, and Ta 4f7/24f_{7/2} appear at 724.1, 780.1, 159.1, 206.8, and 25.5 eV, respectively. Peak deconvolution of XPS spectra confirms the fully oxidized states of the cations in the HEO (Cs1+\mathrm{Cs}^{1+}, Ba2+\mathrm{Ba}^{2+}, Bi3+\mathrm{Bi}^{3+}, Nb5+\mathrm{Nb}^{5+}, and Ta5+\mathrm{Ta}^{5+}). The XPS spectrum and peak deconvolution of oxygen in the HEO reveal the presence of three peaks. Among them, the peak at 529.8 eV is assigned to lattice O 1s,[11] the peak at 531.5 eV is associated with hydroxyl groups and oxygen vacancies,[20] and the peak at 533.3 eV corresponds to adsorbed water on the HEO surface.[31]

XPS spectra showing the chemical state of metals and oxygen in HEO

Figure 4. Chemical state of metals and oxygen in HEO. XPS spectra for (a) cesium, (b) barium, (c) bismuth, (d) niobium, (e) tantalum, and (f) oxygen in HEO.

Nanostructure and atomic structure

Figure 5 illustrates the nanostructural features of the HEO. The TEM (a) BF and (b) DF micrographs show the presence of nanograins in the HEO. These grains appear as a typical feature of the HPT process, which apparently remains even after high-temperature calcination. fig:5c depicts the SAED pattern of HEO and shows concentric rings representing specific crystal planes of the cubic and tetragonal phases in the HEO. In addition, fig:5d and fig:5e also confirm the existence of cubic and tetragonal phases through HR micrographs and fast Fourier transforms, respectively. The observation of the nanostructure shows that, in addition to high-angle grain boundaries, dislocation cells are also present, as described in fig:5f. Several studies have shown that the presence of dislocations and their pair vacancies can contribute to increased charge separation, and thus improve the efficiency of the photocatalysis process. [32, 33]

Formation of nanograins and dislocation cells in HEO

Figure 5. Formation of nanograins and dislocation cells in HEO. (a) BF, (b) DF, (c) SAED, and (d-f) HR analyses of HEO taken by TEM.

The atomic structure characteristics of the four metals (Cs L3_3-edge, Ba L3_3-edge, Bi L3_3-edge, Ta L3_3-edge) in the HEO and their corresponding binary and ternary oxides are described using XANES and EXAFS spectra, as shown in Figure 6. Based on the XANES spectra (fig:6a, fig:6c, fig:6e, fig:6g), a similarity can be observed between the absorption edges of the metals in the HEO and the binary and ternary oxides, reflecting that the oxidation state and local electronic structure of the metals do not significantly differ. In addition, XANES provides further information about the oxidation states of the metals through the white line.[34] The white line is known as the strong, sharp absorption peak that appears right above the absorption edge. A higher white line reflects a higher oxidation state based on a higher 5d unoccupied state.[34] Therefore, it can be seen that barium and bismuth in the HEO have more unoccupied states compared to barium in BaO2\mathrm{BaO}_{2} and bismuth in Bi2O3\mathrm{Bi}_{2}\mathrm{O}_{3}. In contrast, the number of unoccupied states of cesium and tantalum in the HEO is lower than that of cesium in CsTaO3\mathrm{CsTaO}_{3} and tantalum in Ta2O5\mathrm{Ta}_{2}\mathrm{O}_{5}. Additionally, the region adjacent to the white line shows a shift toward lower energy levels for the Cs and Ba peaks, while the Bi peak shifts toward higher energy, and Ta remains unchanged. This indicates that the bond lengths of Cs–O and Ba–O in the HEO are shorter than in their corresponding binary oxides, whereas the Bi–O bond length is longer. It should be noted that the bond lengths achieved by binary oxides in this study are consistent with the literature.[35, 36] Figure 6 b, Figure 6 d, Figure 6 f, and Figure 6 h provide information about the vicinity of the cations through the oscillations of the 50-1000 eV energy absorption spectrum on the absorption edge determined by EXAFS analysis.[37, 38] In these figures, the high-intensity peak at approximately 1-2 Å typically characterizes oxygen bonded to the metal, while the subsequent peaks (second or third) usually describe the bonding of the metal to itself or other metals within a material. It can be observed that there are differences in most peak positions, except for one Ta peak at 1.5 Å. This confirms the preservation of the bonding between Ta5+\mathrm{Ta}^{5+} and six O2−\mathrm{O}^{2-} atoms in a TaO6\mathrm{TaO}_{6} octahedron. Meanwhile, the arrangement of A-site elements such as Ba, Bi, and Cs is completely different between the HEO and their corresponding binary oxides. These atomic structure characteristics also confirm the perovskite structure of HEO. Furthermore, these features can influence photocatalytic processes such as the conversion of CO2\mathrm{CO}_{2} into CH4\mathrm{CH}_{4} or CO products.

Transformation in local electronic structure and neighbourhood of cations in HEO compared with relevant binary and ternary oxides

Figure 6. The transformation in local electronic structure and neighbourhood of cations in HEO compared with relevant binary and ternary oxides. (a, c, e, g) XANES spectra and (b, d, f, h) Fourier-transformed EXAFS spectra in R-space for (a, b) Cs L3L_3-edge, (c, d) Ba L3L_3-edge, (e, f) Bi L3L_3-edge, (g, h) Ta L3L_3-edge of HEO and relevant binary and ternary oxides.

Optical and spin characterizations

fig:7a depicts the UV-Vis absorption spectrum of the HEO. A strong absorption edge is observed at a wavelength of 380 nm, indicating that the HEO absorbs the light mainly in the UV region. Through UV-Vis analysis by the Kubelka-Munk method, fig:7b shows the direct bandgap value of HEO at 3.0 eV. fig:7c depicts the UPS spectrum to estimate the valence band maximum (VBM) value. The measured VBM and secondary energy cut-off (SECO) values are 4.0 and 18.5 eV versus the Fermi level, respectively. The VBM versus

vacuum was obtained based on (1), where ϕ\phi denotes the work function, hh corresponds to Planck's constant, ν\nu denotes the photon frequency, and hνh\nu is 21.2 eV. The band structure of HEO is described in fig:7d, where the VBM value is -6.7 eV versus vacuum or 2.26 eV versus normal hydrogen electrode (NHE). The conduction band minimum (CBM) value is obtained by subtracting the bandgap from the VBM, reaching -0.74 eV versus NHE. Compared with the band structures of Nb2_2O5_5 [39] (bandgap: 3.4 eV, VBM: 2.5 eV versus NHE, CBM: −0.9 eV versus NHE) and Ta2_2O5_5 [40] (bandgap: 3.9 eV, VBM: 3.49 eV versus NHE, CBM: −0.41-0.41 eV versus NHE), the HEO exhibits a narrower bandgap along with a modified band structure. This band structure of HEO satisfies the energy requirements for the CO2\mathrm{CO}_2 conversion process, i.e., the CBM of the HEO is higher than the reduction potential of CO2/CO\mathrm{CO}_2/\mathrm{CO} (−0.11-0.11 eV versus NHE) and CO2/CH4\mathrm{CO}_2/\mathrm{CH}_4 (0.170.17 eV versus NHE).[11]

EVBM vs. vacuum=−(EVBM vs. Fermi level+hν−ESECO)(1)E_{\mathrm{VBM}\ \mathrm{vs.}\ \mathrm{vacuum}} = -\left(E_{\mathrm{VBM}\ \mathrm{vs.}\ \mathrm{Fermi\ level}} + h\nu- E_{\mathrm{SECO}}\right) \tag*{(1)}

Figure 7 provides information on vacancy defects through ESR analysis. The signal with g=1.936g = 1.936 most likely originates from paramagnetic defects based on the Nb antisite.[41] Additionally, a small dual peak with a turning point at g=2.001g = 2.001 is characteristic of oxygen vacancies with an unpaired electron.[4] The gg value at 2.0082.008 with high peak intensity is generally attributed to paramagnetic oxygen vacancies associated with lattice strain.[4] This result also supports the information on the XPS of O 1s as illustrated in Figure 4. The confirmation of the presence of oxygen vacancy defect sites also forms the basis for catalyst selection to enhance the efficiency of photocatalytic reactions. Several studies have shown these sites can be active sites that provide CO2\mathrm{CO}_2 uptake and generate more electrons to activate the CO2∙−\mathrm{CO}_2^{\bullet-} intermediate.[16, 42] In addition, the PL spectrum in Figure 7 also reveals the presence of a low-intensity peak at 600 nm, which shows that this HEO has small charge recombination. The intensity of this peak is about 40 times lower than the PL intensity for anatase TiO2\mathrm{TiO}_2, examined under similar conditions. Improvements in the optical properties of the material are expected to contribute to improved performance of photocatalytic processes, such as the conversion of CO2\mathrm{CO}_2 to form more CH4\mathrm{CH}_4 and CO.

Optical characterization and appropriate band structure of HEO for CO2 conversion

Figure 7. Optical characterization and appropriate band structure of HEO for CO2\mathrm{CO}_{2} conversion. (a) UV-Vis light absorbance analysis, (b) direct bandgap estimation based on Kulbelka-Munk method, (c) UPS analysis (He I, bias −4-4 V, VBM: valence band maximum, SECO: secondary electron cut-off), (d) band structure with valence band and conduction band values versus normal hydrogen electron and versus vacuum, and (e) ESR spectrum and (f) PL spectrum for HEO.

Photocatalytic activity

fig:8a, fig:8b, and fig:8c illustrate the photocatalytic CO2\mathrm{CO}_2 conversion process under four different conditions for the evolution of H2\mathrm{H}_2, CO, and CH4\mathrm{CH}_4, respectively. In Experiment 1, only HEO was used without scavengers. Experiments 2, 3, and 4 were conducted under the same conditions as Experiment 1, with the introduction of PET micro-powder, microalgae, and methanol as sacrificial agents. All experiments were initially carried out for 4 h to reach a steady state, then continuous sampling was conducted every hour for 20 h. It can be observed that during CO2\mathrm{CO}_2 conversion using only the HEO, the average CO production reaches 5.6 μ\mumol/g⋅\cdoth, while CH4\mathrm{CH}_4 evolution is approximately 1.1 μ\mumol/g⋅\cdoth and no H2\mathrm{H}_2 is detected. Based on the methane production rate and the CO formation rate, as well as the number of electrons required to reduce CO2\mathrm{CO}_2 into these products, the methane selectivity of HEO is 44%, while its CO selectivity is 56%.

CH4 Selectivity=100×8rCH42rCO+8rCH4(2)\mathrm{CH}_4\ \mathrm{Selectivity} = 100 \times\frac{8r_{\mathrm{CH}_4}}{2r_{\mathrm{CO}} + 8r_{\mathrm{CH}_4}} \tag*{(2)}

Upon the addition of PET, the conversion efficiency increases, with CO and CH4\mathrm{CH}_4 concentrations reaching 25.9 and 1.6 μ\mumol/g⋅\cdoth, respectively. The introduction of PET as a sacrificial agent reduces the recombination of electrons and holes, allowing electrons sufficient time to get involved in the CO2\mathrm{CO}_2 reduction process, contributing to the formation of more conversion products. When methanol is used as a conventional sacrificial scavenger, the production rate of CO and CH4\mathrm{CH}_4 does not increase and remains at 2.7 and 0.6 μ\mumol/g⋅\cdoth, respectively. However, the H2\mathrm{H}_2 production rate significantly increases with the addition of methanol and reaches 24.8 μ\mumol/g⋅\cdoth. Microalgae also have a similar mechanism of action to PET and methanol as a scavenger for the reaction; however, the use of microalgae is more effective than PET and methanol. Specifically, in the presence of microalgae during CO2\mathrm{CO}_2 conversion by the HEO, the average evolution rates of CO and CH4\mathrm{CH}_4 increase to large values of 63.9 and 4.6 μ\mumol/g⋅\cdoth, respectively. Additionally, H2\mathrm{H}_2 is also produced at a rate of 37.0 μ\mumol/g⋅\cdoth by the addition of microalgae, which is higher than that using methanol. To further evaluate the role of microalgae, two control experiments were conducted in the absence of the HEO, in which the microalgae were irradiated to assess their self-degradation capability. The first experiment was performed with a continuous stream of CO2\mathrm{CO}_2 gas, while the second one was conducted with a stream of argon gas. As shown in fig:8d, the results of two experiments show that after 24 h of irradiation, the production rate of CO and CH4\mathrm{CH}_4 reached approximately 20.0 and 2.0 μ\mumol/g⋅\cdoth, respectively. These values are less than one-third of those obtained in the presence of HEO and microalgae, indicating that microalgae themselves can undergo degradation under strong irradiation to form products. However, in the presence of the photocatalyst, the efficiency is significantly enhanced. The stability of the HEO was evaluated through cycling tests, as shown in fig:8e. Moderate variations in product yields are observed without a clear trend. While the second cycle resulted in a slight increase in product concentration, the third cycle shows a slight decrease. These small changes may stem from differences in the shapes and sizes of the microalgal clusters, as shown in fig:S1. Such structural heterogeneity can influence degradation rates, light absorption, mass transfer, and contact efficiency with the HEO catalyst, thereby leading to fluctuations in product yield during repeated cycles.

fig:8f characterizes the microalgae after photocatalysis through FT-IR analysis. The FT-IR spectra confirm the structure of Chlamydomonas reinhardtii microalgae, with major components including carbohydrates, lipids, and proteins. After photocatalysis, the peaks of the carbohydrate group have almost completely disappeared, while the peaks of the lipids and proteins have very low intensity. Based on the complexity of the structure of the lipids and proteins, their complete decomposition requires more time than the carbohydrate group. A comparison of XRD spectra (fig:8g) of the HEO before and after experiments confirms the long-term stability of the HEO. These results show that the use of HEO helps maintain the structural stability and photocatalytic activity, while microalgae significantly enhance the efficiency of CO2\mathrm{CO}_2 conversion products.

Discussion

Enhancing product yields from CO₂ photocatalytic conversion remains a major challenge in photocatalysis, because the strong C=O bonds make CO₂ highly stable during reduction reactions.[5] Research on high-entropy photocatalysts promoted innovation in this field by incorporating a variety of cations in a single crystal; however, the CO₂ conversion activity still needs further improvement. In this study, microalgae are used as hole scavengers for CO₂ conversion, contributing to improved yields of CO and CH₄. Besides, a novel HEO is designed and synthesized for this photocatalytic CO₂ conversion reaction. This section discusses in more detail two aspects: (i) evaluation of the performance of the HEO in comparison with other materials and reasons behind the outstanding catalytic activity of HEO, and (ii) the mechanism and the advantages of using microalgae as a scavenger in photocatalysis.

Regarding the first issue, as shown in Table 2, the HEO exhibits higher performance compared with conventional photocatalysts. [16, 17, 42, 43, 44, 45, 46, 47, 48, 49] This improvement arises from several distinctive features related to material configuration. First, the HEO possesses an intriguing structural characteristic in which its two polymorphs share nearly identical frameworks: the cubic phase has a pyrochlore structure close to the one reported for (AxA′y)B2O6+z(\mathrm{A}_x\mathrm{A'}_y)\mathrm{B}_2\mathrm{O}_{6+z} (1<x+y<1.31 < x + y < 1.3, z<1z < 1), [25, 43, 50] while the tetragonal phase resembles an AB2O6\mathrm{AB}_2\mathrm{O}_6 layered perovskite or tungsten bronze structure. [26] The B-site atoms niobium and tantalum, with a coordination number of 6, form octahedral frameworks that connect at the corners of the lattice. [25, 43] Several A sites with a coordination number of 8 create an elongated cube for the cubic phase. While other A sites with a coordination number of 12 form a perovskite-like structure, and others with a coordination number of 15 allow some octahedral rings to be inserted into the structure, forming a tetragonal phase. [26] The two phases share the same octahedral structure, reflecting their polymorphism in a single chemical composition. This is supported by SEM-EDS and STEM-EDS results (Figure 3), which demonstrate the homogeneous distribution of all elements throughout the HEO. The significant similarity between the two phases leads to the formation of an electronic junction [3, 51] while maintaining uniform elemental distribution, thereby enhancing charge separation and facilitating more efficient charge transport in the catalyst. Several previous studies have also reported the formation of dual-phase HEOs consisting of fluorite and pyrochlore structures within the same composition, [52] as well as order–disorder transitions between these structures. [53] In addition, phase stability (e.g., cubic versus tetragonal) is strongly influenced by factors such as cation size, disorder, and electronegativity differences, [54] further supporting this transition behavior. Besides, it should also be noted that the current authors observed that this polymorphic transition depends on the synthesis and post-synthesis conditions. The phase fractions used in this study are observed when the HEO is synthesized at 1373 K and rapidly cooled under atmospheric pressure. However, as demonstrated in fig:S2, when the synthesized HEO is annealed at 673 K for 1 h, the fraction of the cubic phase increases, suggesting the occurrence of a tetragonal-to-cubic phase transformation.

CatalystReaction systemScavenger for HolesCo-catalystCO2_2 conversion (μ\mumol/g.h) COCO2_2 conversion (μ\mumol/g.h) CH4_4CO2_2 conversion (μ\mumol/g.h) H2_2Ref.
HEO (0.1 g)- Continuous gas-solid reactor - Light: 400 W mercury- - Methanol (50 mL) - PET plastic (0.1 g) - Microalgae (0.1 g)-5.6 2.7 25.9 63.91.1 0.6 1.6 4.6- 24.8 - 37.0This study
ZnTa2_2O6_6 (0.5 g)- Continuous gas-solid reactor - Light: 400 W mercury-3 wt% Ag43.7--[16]
SrNb2_2O6_6 (0.01 g)- Continuous gas-solid reactor - Light: 100 W xenon--16.63.36.5[17]
In2_2O3_3 with oxygen vacancy (0.01 g)- Continuous gas-solid reactor - Light: 300 W xenonTriethanolamine (2 mL)-63.30.811.6[42]
CsBi2_2Ta5_5O16_{16} (0.1 g)- Batch gas-solid reactor - Light: 300 W xenon-10 wt% NiO1.1 -0.2 7.2- -[43]
NaNbO3_3- Continuous gas-solid reactor - Light: 4 fluorescents, a total irradiance of 71.7 Wm−2^{-2}--6.470.0152.9[44]
NaTaO3_3- Continuous gas-solid reactor - Light: 4 fluorescents, a total irradiance of 71.7 Wm−2^{-2}--0.060.0060.12[44]
NaNb0.5_{0.5}Ta0.5_{0.5}O3_3 (0.1 g)- Continuous gas-solid reactor - Light: 4 fluorescents, a total irradiance of 71.7 Wm−2^{-2}--2.40.032.4[44]
P25 TiO2_2 (0.2 g)- Batch gas-solid reactor - Light: 300 W xenonMethanol (20 mL)-1.3-2.7[45]
Porous Ta2_2O5_5 (0.1 g)- Continuous gas-solid reactor - Light: 300 W xenon--0.3-1.5[46]
SnTa2_2O6_6- Continuous gas-solid reactor - Light: 300 W xenon-1 % Ag1.8-0.2[47]
Sn2_2Ta2_2O7_7 (0.02 g)- Continuous gas-solid reactor - Light: 350 W xenon--28--[47]
Bi4_4O5_5Br2_2 (0.02 g)- Batch gas-solid reactor - Light: 300 W xenon--31.6--[48]
ZnIn2_2S4_4 (0.05 g)- Batch gas-solid reactor - Light: 300 W xenon (λ≥420\lambda\ge420 nm)Triethanolamine (10 mL)Undoped Er-doped1.6 0.60.03 6.74.1 1.6[49]

Table 2. Summary of photocatalytic CO and CH4_4 production using different catalysts

Second, catalyst design is based on the integration of elements niobium and titanium as the octahedral framework, while the three other elements (bismuth, cesium, and barium) provide benefits for the reaction. Earlier studies showed that mixing elements with different cationic configurations can provide both electron-donating and electron-accepting sites [11] and have been shown to improve charge-transfer processes in HEOs. In addition, the incorporation of alkali and alkaline earth metals such as cesium and barium increases surface basicity, enhances CO2\mathrm{CO}_2 chemisorption, and suppresses charge recombination. [11, 41, 42] Moreover, the incorporation of bismuth in the form of Bi3+\mathrm{Bi}^{3+} introduces a stereochemically active 6s26s^2 lone pair. [55] This lone pair exerts a strong polar distortion on the local coordination environment, generating a localized dipole moment (i.e., localized polarization). This internal electric field actively drives the separation of photogenerated electron–hole pairs, suppressing their recombination. [55] Finally, the formation of oxygen vacancies, as evidenced by the O 1s XPS and ESR spectra, is considered to generate active sites for photocatalytic reactions. [3, 32] Taken together, all these features synergistically contribute to the enhanced CO2\mathrm{CO}_2 reduction performance of the HEO.

Regarding the second issue, the results shown in Figure 8 can be used to elucidate a CO2\mathrm{CO}_2 conversion mechanism in which microalgae act as a sacrificial agent. It is clearly observed that, in the presence of microalgae, the CO production efficiency increases by 10-fold and that of CH4\mathrm{CH}_4 by 4-fold compared with the photocatalytic process using only HEO. Microalgae as a sacrificial agent also demonstrates higher performance when compared with PET plastic, a common environmental pollutant with high potential for photoreforming, [35, 36] used in this study as a sacrificial agent. This can be explained by the fact that microalgae are more degradable and can be readily decomposed compared to plastic under light irradiation in a neutral pH environment. As a result, smaller molecular components are generated, which can effectively scavenge photogenerated holes and promote charge separation. In addition, microalgae possess a complex composition leading to multiple different oxidation pathways, which contribute to enhanced overall reaction kinetics. After the photocatalysis, the microalgal clusters were almost completely degraded. FT-IR analyses indicate that easily degradable carbohydrate groups disappear, while only weak intensities corresponding to the characteristic peaks of lipid and protein groups remain. Additionally, GC–MS analysis was conducted, as described in fig:S3 of the supplementary information; however, no specific components were detected in the liquid phase extracted after the reaction. The decomposition of microalgae contributes to enhanced CO2\mathrm{CO}_2 reduction and the formation of a greater quantity of products such as CO and CH4\mathrm{CH}_4. As schematically shown in Figure 9, the use of microalgae as a sacrificial agent not only diminishes the necessity of using alcohols whose production emits CO2\mathrm{CO}_2, but also contributes to CO2\mathrm{CO}_2 capture because microalgae capture CO2\mathrm{CO}_2 during their cultivation through the photosynthesis process. [22, 23]

Enhanced CO₂ conversion process efficiency using HEO as photocatalyst and microalgae as sacrificial agent

Figure 8. Enhanced CO₂ conversion process efficiency using HEO as photocatalyst and microalgae as sacrificial agent. (a) H₂, (b) CO, and (c) CH₄ production from photocatalysis reactions under various conditions. (d) Average product concentration from photocatalysis and microalgae degradation. (e) Photocatalytic production rates for three cycles by using HEO and microalgae. (f) FT-IR spectra of microalgae before and after photocatalysis. (g) XRD analysis of HEO before and after CO₂ conversion.

Figure 9. Schematic illustration of photocatalytic CO2_2 conversion using microalgae as hole sacrificial agent, realized by HEO.

It should be noted that the morphology and size of the microalgae clusters can affect the efficiency of the photocatalytic process. Further studies could evaluate the effects of different microalgal strains and optimize their dosage as well as particle size. Future experiments on ternary or quaternary AB2O6\mathrm{AB}_2\mathrm{O}_6-type oxides by omitting or substituting individual elements can also further clarify the effect of individual elements in the HEO on the photocatalytic CO2\mathrm{CO}_2 conversion mechanism in the presence of microalgae. A detailed life cycle assessment and carbon balance estimation, together with electrochemical analyses, should also be applied to fully evaluate the environmental and charge transfer impact of photocatalysis. Finally, the design of high-entropy photocatalysts that can function under visible light and ultimately sunlight can be an important step towards realizing energy efficiency in the microalgae-based photocatalytic system. This study, together with an earlier study, [56] suggests the high potential of bio-scavengers in photocatalysis, although optimization of the process and catalyst should be studied in the future.

Conclusion

In this study, a novel pathway for CO2\mathrm{CO_2} conversion is suggested by using microalgae as a sacrificial agent in photocatalysis. For this pathway, an AB2O6\mathrm{AB_2O_6}-type high-entropy material, (Cs1/7Ba4/7Bi2/7)(Nb1/2Ta1/2)2O6(\mathrm{Cs}_{1/7}\mathrm{Ba}_{4/7}\mathrm{Bi}_{2/7})(\mathrm{Nb}_{1/2}\mathrm{Ta}_{1/2})_2\mathrm{O}_6, is synthesized, which has bi-polymorphism (layered perovskite and pyrochlore) while maintaining high homogeneity of all elements. The new pathway exhibits an improvement in the production efficiency of CH4\mathrm{CH_4} and CO. These results indicate that the use of microalgae is beneficial not only for CO2\mathrm{CO_2} capture during its cultivation but also for CO2\mathrm{CO_2} conversion during photocatalysis, suggesting a sustainable route for the carbon cycle.

Author contributions

All authors participated in conceptualization, investigation, methodology, validation, and writing - review & editing.

Conflicts of interest

The authors declare no conflict of interest.

Data availability

Data will be made available on request.

Acknowledgements

H.T.N.H. would like to express gratitude to the Yoshida Scholarship Foundation (YSF) for its support in the form of a Ph.D. scholarship. This research was funded in part by Mitsui Chemicals, Inc., Japan; in part by the ASPIRE initiative of the Japan Science and Technology Agency (JST) (JPMJAP2332), and in part by the São Paulo Research Foundation (FAPESP), grant number 2024/01639-0.

Notes and references

References

  1. [1]D. Schimel, B. B. Stephens and J. B. Fisher, Effect of increasing CO₂ on the terrestrial carbon cycle, Proc. Natl. Acad. Sci. U. S. A., 2015, 112, 436–441.
  2. [2]G. Rothenberg, A realistic look at CO₂ emissions, climate change and the role of sustainable chemistry, Sustain. Chem. Clim. Action, 2023, 2, 100012.DOI
  3. [3]H. T. N. Hai, J. Hidalgo-Jiménez and K. Edalati, Boosting hydrogen and methane formation on a high-entropy photocatalyst by integrating atomic d⁰+d¹⁰ electronic junctions and microscopic P/N heterojunctions, Int. J. Hydrogen Energy, 2025, 162, 150762.
  4. [4]J. Hidalgo-Jiménez, T. Akbay, X. Sauvage, T. Ishihara and K. Edalati, Photocatalytic carbon dioxide methanation by high-entropy oxides: Significance of work function, Appl. Catal. B: Environ. Energy, 2025, 371, 125259.
  5. [5]S. Fang, M. Rahaman, J. Bharti, E. Reisner, M. Robert, G. A. Ozin and Y. H. Hu, Photocatalytic CO₂ reduction, Nat. Rev. Methods Primers, 2023, 3, 61.
  6. [6]P. M. Bacirhonde, D. Shrestha, K. Kang, E. M. Hia, N. Komalla, N. Y. Dzade, M. Buldu-Akturk, M. P. Browne, M. B. Poudel, D. J. Yoo, E. Jeong, A. Y. Mohamed, B. G. Han, D. Cho, M. T. Curnan, G. H. Gu, J. W. Han and C. H. Park, Understanding the metal-center mediated adsorption and redox mechanisms in a FeMn(NbTa)₂O₆ columbite material for anion exchange membrane water electrolyzers, Adv. Energy Mater., 2025, 15, 2404479.
  7. [7]S. A. Da Silva and S. M. Zanetti, Processing of Bi₁.₅ZnNb₁.₅O₇ ceramics for LTCC applications: Comparison of synthesis and sintering methods, Ceram. Int., 2009, 35, 2755–2759.DOI
  8. [8]W. Luo, S. Wang, S. Zheng, J. Li, M. Wang, Y. Wen, L. Li and J. Zhou, Dielectric response of ANb₂O₆ (A = Zn, Co, Mn, Ni) columbite niobates: From microwave to terahertz, J. Adv. Ceram., 2024, 13, 1189–1197.
  9. [9]K. Alageshwaramoorthy, P. Mannu, S. Mahalingam, T. T. T. Nga, H.-W. Chang, Y. Masuda and C.-L. Dong, Synthesis and characterization of visible-light-driven novel CuTa₂O₆ as a promising practical photocatalyst, Front. Chem., 2023, 11, 1197961.DOI
  10. [10]E. E. Nikishina, E. N. Lebedeva, D. V. Drobot, Niobium- and tantalum-containing oxide materials: Synthesis, properties, and application, Inorg. Mater., 2012, 48, 1243–1260DOI
  11. [11]J. Hidalgo-Jiménez, T. Akbay, T. Ishihara and K. Edalati, Active high-entropy photocatalyst designed by incorporating alkali metals to achieve d⁰+d¹⁰+s⁰ cationic configurations and wide electronegativity mismatch, Acta Mater., 2026, 302, 121632.
  12. [12]Q.-P. Ding, Y.-P. Yuan, X. Xiong, R.-P. Li, H.-B. Huang, Z.-S. Li, T. Yu, Z.-G. Zou and S.-G. Yang, Enhanced photocatalytic water splitting properties of KNbO₃ nanowires synthesized through hydrothermal method, J. Phys. Chem. C, 2008, 112, 18846–18848.
  13. [13]Y. Huan, H. Shen, Y. Zhu, M. Li, H. Li, Z. Wang, Y. Hao and T. Wei, Enhanced ferro-photocatalytic performance for ANbO₃ (A= Na, K) nanoparticles, Math. Biosci. Eng., 2019, 16, 4122–4134.
  14. [14]J. F. D. L. Nascimento, Y. Leyet Ruiz, O. Da Cunha Mendes, F. M. C. Batista, A. Cabot, J. M. E. D. Matos, R. D. Ferreira, M. V. Botelho Do Nascimento, L. B. Saraiva, J. N. N. Quaresma and F. X. Nobre, BaNb₂O₆ at room temperature by ball milling method: Structural, optical, morphology, and electrochemistry properties, Ind. Eng. Chem. Res., 2024, 63, 20020–20033.
  15. [15]J. Ye, A novel series of water splitting photocatalysts NiM₂O₆ (M= Nb, Ta) active under visible light, Int. J. Hydrogen Energy, 2003, 28, 651–655.
  16. [16]S. Iguchi, K. Teramura, S. Hosokawa and T. Tanaka, A ZnTa₂O₆ photocatalyst synthesized via solid state reaction for conversion of CO₂ into CO in water, Catal. Sci. Technol., 2016, 6, 4978–4985.
  17. [17]S. Xie, Y. Wang, Q. Zhang, W. Deng and Y. Wang, SrNb₂O₆ nanoplates as efficient photocatalysts for the preferential reduction of CO₂ in the presence of H₂O, Chem. Commun., 2015, 51, 3430–3433.DOI
  18. [18]S. Akrami, P. Edalati, M. Fuji and K. Edalati, High-entropy ceramics: Review of principles, production and applications, Mater. Sci. Eng. R, 2021, 146, 100644.DOI
  19. [19]X. Wang, X. Chen, S. Zou, Z. Jia, B. Li, H. Wang and D. Xu, Geochronology, geochemistry, and mineral chemistry of the Lingshan-Huangshan complex, South China: Insights into Nb and Ta enrichment, Ore Geol. Rev., 2023, 157, 105433.DOI
  20. [20]H. T. N. Hai, M. Arita and K. Edalati, High-entropy perovskites as new photocatalysts for photocatalyst-free water splitting, Appl. Catal. B: Environ. Energy, 2026, 383, 126081.DOI
  21. [21]T. T. T. Nguyen and K. Edalati, High-entropy oxide with tailored heterogeneous electronic structure as a low-bandgap catalyst for antibiotic photodegradation under visible light, Appl. Catal. B: Environ. Energy, 2026, 382, 126011.DOI
  22. [22]A. Randhir, D. W. Laird, G. Maker, R. Trengove and N. R. Moheimani, Microalgae: A potential sustainable commercial source of sterols, Algal Res., 2020, 46, 101772.DOI
  23. [23]G. Zuccaro, A. Yousuf, A. Pollio and J.-P. Steyer, Microalgae cultivation systems, in A. Yousuf (ed.), Microalgae Cultivation for Biofuels Production, Elsevier, 2020, pp. 11–29.
  24. [24]K. Edalati and Z. Horita, A review on high-pressure torsion (HPT) from 1935 to 1988, Mater. Sci. Eng., A, 2016, 652, 325–352.DOI
  25. [25]M.H. Khanmiri, R. Bogdanov, E. Puchkova, A. Titov, A. Yadollahi, On the issue of comparing the immobilization characteristics of matrix materials based on Nb–Ta–Ti-oxides of the types AB₂O₆ and A₂B₂O₇, Sci. Rep., 2024, 14, 17992.DOI
  26. [26]F. Galasso, G. Layden and G. Ganung, ANb₂O₆ and ATa₂O₆ phases, Mater. Res. Bull., 1968, 3, 397–407.DOI
  27. [27]G. Davidson (ed.), Spectroscopic Properties of Inorganic and Organometallic Compounds, RCS, Cambridge, 2005, volume 37.
  28. [28]L. Palliyaguru, U. S. Kulathunga, L. I. Jayarathna, C. D. Jayaweera and P. M. Jayaweera, A simple and novel synthetic route to prepare anatase TiO₂ nanopowders from natural ilmenite via the H₃PO₄/NH₃ process, Int. J. Miner. Metall. Mater., 2020, 27, 846–855.DOI
  29. [29]W. M. Haynes and D. R. Lide, eds., CRC Handbook of Chemistry and Physics: A Ready-Reference Book of Chemical and Physical Data, CRC Press, Boca Raton, Fla., 92nd edn, 2011.
  30. [30]S. Nakagawa, I. Fujii, H. Nam, S. Ueno and S. Wada, Fabrication of BaTiO₃–Bi(Mg₀.₅Ti₀.₅)O₃–BiFeO₃ ceramics at lower temperature by using citrate method, J. Ceram. Soc. Jpn., 2024, 132, 358–363.DOI
  31. [31]J. V. Rojas, M. Toro-González, M. C. Molina-Higgins and C. E. Castano, Facile radiolytic synthesis of ruthenium nanoparticles on graphene oxide and carbon nanotubes, Mater. Sci. Eng., B, 2016, 205, 28–35.DOI
  32. [32]H. T. N. Hai, T. T. Nguyen, M. Nishibori, T. Ishihara and K. Edalati, Photoreforming of plastic waste into valuable products and hydrogen using a high-entropy oxynitride with distorted atomic-scale structure, Appl. Catal. B: Environ. Energy, 2025, 365, 124968.DOI
  33. [33]T. T. Nguyen, J. Hidalgo-Jiménez, X. Sauvage, K. Saito, Q. Guo and K. Edalati, Phase and sulfur vacancy engineering in cadmium sulfide for boosting hydrogen production from catalytic plastic waste photoconversion, Chem. Eng. J., 2025, 504, 158730.DOI
  34. [34]A. Bianconi, Surface X-ray absorption spectroscopy: Surface EXAFS and surface XANES, Appl. Surf. Sci., 1980, 6, 392–418.
  35. [35]W. Zhang, S. Zhan, J. Xiao, T. Petit, C. Schlesiger, M. Mellin, J. P. Hofmann, T. Heil, R. Müller, K. Leopold and M. Oschatz, Coordinative stabilization of single bismuth sites in a carbon–nitrogen matrix to generate atom-efficient catalysts for electrochemical nitrate reduction to ammonia, Adv. Sci., 2023, 10, 2302623.DOI
  36. [36]J. Ribeiro, G. Tremiliosi-Filho, P. Olivi and A. R. de Andrade, XAS characterization of the RuO₂–Ta₂O₅ system local (crystal) structure, Mater. Chem. Phys., 2011, 125, 449–460.DOI
  37. [37]F. He, Y. Liu, X. Yang, Y. Chen, C.-C. Yang, C.-L. Dong, Q. He, B. Yang, Z. Li, Y. Kuang, L. Lei, L. Dai and Y. Hou, Accelerating oxygen electrocatalysis kinetics on metal–organic frameworks via bond length optimization, Nano-Micro Lett., 2024, 16, 175.
  38. [38]K. Mori, N. Hashimoto, N. Kamiuchi, H. Yoshida, H. Kobayashi and H. Yamashita, Hydrogen spillover-driven synthesis of high-entropy alloy nanoparticles as a robust catalyst for CO₂ hydrogenation, Nat. Commun., 2021, 12, 3884.DOI
  39. [39]A. G. S. Prado, L. B. Bolzon, C. P. Pedrosso, A. O. Moura and L. L. Costa, Nb₂O₅ as efficient and recyclable photocatalyst for indigo carmine degradation, Appl. Catal. B: Environ. Energy, 2008, 82, 219–224.DOI
  40. [40]X. Yang, A. Roy, M. Alhbradi, M. Alruwaili, H. Chang and A. A. Tahir, Fabrication and Characterization of Tantalum–Iron Composites for Photocatalytic Hydrogen Evolution, Nanomater., 2023, 13, 2464.DOI
  41. [41]H. Qin, X. Chen, J. Zhang, Y. Song, L. Zhang, Q. Liu, F. Wang, D. Wang, Y. Sang and H. Liu, Electronic paramagnetic resonance analysis of point defects in lithium niobate: progress and prospects, Mater. Adv., 2025, 6, 6648–6663.DOI
  42. [42]X. Zhu, J. Yang, X. Zhu, J. Yuan, M. Zhou, X. She, Q. Yu, Y. Song, Y. She, Y. Hua, H. Li and H. Xu, Exploring deep effects of atomic vacancies on activating CO₂ photoreduction via rationally designing indium oxide photocatalysts, Chem. Eng. J., 2021, 422, 129888.DOI
  43. [43]M. Ni, L. Wang, Y. Chai, B. Wang, D. Li, J. Shen, Z. Zhang and X. Wang, Multimetal tantalate catalysts CsBi₂Ta₃O₁₀ for photocatalytic conversion of CO₂ with H₂O into CH₄ and O₂, Appl. Surf. Sci., 2022, 588, 152933.
  44. [44]F. Fresno, S. Galdón, M. Barawi, E. Alfonso-González, C. Escudero, V. Pérez-Díezte, C. Huck-Iriart and V. A. De La Peña O’Shea, Selectivity in UV photocatalytic CO₂ conversion over bare and silver-decorated niobium-tantalum perovskites, Catal. Today, 2021, 361, 85–93.DOI
  45. [45]D.-E. Lee, D. Jin Kim, V. Devthade, W.-K. Jo and S. Tonda, Size-dependent selectivity and activity of highly dispersed sub-nanometer Pt clusters integrated with P25 for CO₂ photoreduction into methane fuel, Appl. Surf. Sci., 2022, 584, 152532.DOI
  46. [46]S. Wei, Q. Heng, Y. Wu, W. Chen, X. Li and W. Shangguan, Improved photocatalytic CO₂ conversion efficiency on Ag loaded porous Ta₂O₅, Appl. Surf. Sci., 2021, 563, 150273.DOI
  47. [47]J. Zhao, Z. Xiong, J. Wang, Y. Qiu, P. Liu, Y. Zhao and J. Zhang, SnTa₂O₆: A novel CO₂ reduction photocatalyst with nearly 100% CO selectivity, Chem. Eng. J., 2022, 446, 134722.
  48. [48]Y. Bai, P. Yang, L. Wang, B. Yang, H. Xie, Y. Zhou and L. Ye, Ultrathin Bi₄O₅Br₂ nanosheets for selective photocatalytic CO₂ conversion into CO, Chem. Eng. J., 2019, 360, 473–482.
  49. [49]F. Zhou, Y. Zhang, J. Wu, W. Yang, X. Fang, T. Jia, Y. Ling, P. He, Q. Liu and J. Lin, Utilizing Er-doped ZnIn₂S₄ for efficient photocatalytic CO₂ conversion, Appl. Catal. B: Environ., 2024, 341, 123347.DOI
  50. [50]A. El Haimouti, D. Zambon, M. El-Ghozzi, D. Avignant, F. Leroux, M. El Aatmani and M. Daoud, Synthesis and structural characterization of new defect pyrochlore type AₓLn₃Sb₂O₆+z antimoniates (0<x, y<1; A = Rb, Cs, Tl; Ln = Eu, Gd and Y) prepared by coprecipitation, Mater. Res. Bull., 2003, 38, 1423–1436.
  51. [51]T. T. Nguyen and K. Edalati, Synergistic interface and oxygen/nitrogen vacancy engineering in g-C₃N₄/Cu₂O under high pressure for efficient CO₂ photoreduction, J. Colloid Interface Sci., 2026, 702, 138951.DOI
  52. [52]W. Ji, J. Hou, Y. Miao and C. Ma, Phase stability and thermal properties of dual-phase high-entropy fluorite-pyrochlore oxides, Ceram. Int., 2025, 51, 12951–12962.DOI
  53. [53]A. J. Wright, Q. Wang, C. C. Hu, Y. T. Yeh, R. Chen and J. Lou, Single-phase duodenary high-entropy fluorite/pyrochlore oxides with an order–disorder transition, Acta Mater., 2021, 211, 116858.
  54. [54]J. Zhang, S. Liu, Z. Tian, Y. Zhang and Z. Shi, The Formation and Phase Stability of A-Site High-Entropy Perovskite Oxides, Mater., 2023, 16, 2214.DOI
  55. [55]R. Seshadri and N. A. Hill, Visualizing the Role of Bi 6s “Lone Pairs” in the Off-Center Distortion in Ferromagnetic BiMnO₃, Chem. Mater., 2002, 13, 2892–2899.
  56. [56]H. T. N. Hai, A. D. Luchessi and K. Edalati, A sustainable photocatalytic pathway for concurrent hydrogen and value-added chemical production utilizing microalgae as bio-scavenger in water, Int. J. Hydrogen Energy, 2026, 228, 154704.DOI

Paper details

vlnc:W_axy3srw6
Version
v1 · latest
Published
Added
License
CC0-1.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents