Direct imaging of the Ni ege_g hole orbitals in the bilayer nickelate La2_2SmNi2_2O7_7

Abstract

Models of unconventional superconductivity in cuprates and nickelates depend sensitively on the distribution of valence electrons among the dd orbitals. But accurately determining the orbital electron or hole occupations in these systems remains a difficult and unresolved task. Here, using ss-core-level non-resonant inelastic x-ray scattering at the Ni M1M_1 edge, we determine the angular distribution of the Ni 3d3d holes in a single crystal of La2_2SmNi2_2O7_7. Our results demonstrate that the hole occupation ratio \hz/\hx = 0.94\pm0.06, thus significantly above the expected value of 2/32/3 for a filled dz2d_{z^2} orbitals models and close to value expected in a Hund's-coupling picture. Our results support superconductivity scenarios in which both ege_g orbitals contribute to the electron-pairing mechanism in La2_2SmNi2_2O7_7.

Superconductivity in transition-metal oxides is intimately linked to the way the valence electrons occupy the dd orbitals [1]. In the cuprates where Cu has a nominal 3d93d^9 configuration, the hole resides in a single dx2−y2d_{x^2-y^2} orbital on each Cu ion, and much of their physics can be understood from this single-band starting point [2, 3, 4]. Whether high-temperature superconductivity requires such a single-orbital configuration, or can also emerge when holes are distributed across multiple orbitals, has long remained an open question. The bilayer Ruddlesden–Popper nickelates now offer an opportunity to address this question. In La3_3Ni2_2O7_7, superconductivity appears under pressure with a critical temperature TcT_c approaching 80 K [5]. Rare-earth substitution raises TcT_c to 82 K in the bulk superconductor La2_2PrNi2_2O7_7 [6] and to 92 K in La2_2SmNi2_2O7_7 and 96 K in the Sm-richer La1.57_{1.57}Sm1.43_{1.43}Ni2_2O7−δ_{7-\delta} [7], and compressive strain stabilizes superconductivity at ambient pressure in thin films [8, 9, 10].

In these compounds, Ni has a nominal 3d7.53d^{7.5} configuration and both ege_g orbitals contribute to the states at the Fermi level. The dz2d_{z^2} orbitals of the two layers couple through the inner apical oxygen and form bonding and antibonding bands, whereas dx2−y2d_{x^2-y^2} forms a wide in-plane band [11, 12]. Theories differ on which orbital drives the pairing: interlayer superexchange of the dz2d_{z^2} electrons in one class of models [13, 14, 15] whereas others emphasize the dominant role of the dx2−y2d_{x^2-y^2} states at the Fermi level [16]. They also start from different orbital fillings. Simple electron counting, with a filled bonding dz2d_{z^2} band, gives 1 dz2d_{z^2} and 0.5 dx2−y2d_{x^2-y^2} electron per Ni, whereas the equal-occupation model of Ref. [11] gives about 0.75 electron in each orbital. Electronic correlations can shift this balance: correlated calculations find a strong Ni–O charge transfer toward a dominant Ni d8d^8 configuration [17, 18], in which Hund’s coupling favors one hole in each ege_g orbital.

The ratio hz2/hx2−y2h_{z^2}/h_{x^2-y^2} of dz2d_{z^2} to dx2−y2d_{x^2-y^2} holes is therefore a direct test of the starting point of these models, ranging from 2/3 for a filled bonding band to about 1 for Hund’s-coupled d8d^8.

Measuring this ratio in a bulk crystal is, however, difficult. Angle-resolved photoelectron spectroscopy (ARPES) finds a renormalized dz2d_{z^2} flat band 30–50 meV below EFE_F [19] or very close to EFE_F [20], a difference attributed to oxygen vacancies. But ARPES is surface sensitive, probes quasiparticles near EFE_F rather than the orbital density integrated over the band, and finds an additional hole-doped dz2d_{z^2} pocket around the MM point in superconducting thin films [21]. Electron-energy-loss spectroscopy (EELS) finds ligand holes on the inner apical and planar oxygens [22], and RIXS identifies Ni ege_g and O 2p2p states at low energy [23]. X-ray linear dichroism at the O KK edge shows holes in both ege_g orbitals in thin films [24], and polarization-dependent x-ray absorption shows a weak orbital polarization in bulk samples [25], but a quantitative sum-rule analysis [26] is complicated by the Ni LL-edge multiplets and by the overlapping La M4M_4 edge.

Non-resonant inelastic x-ray scattering from an ss core level (ss-NIXS) overcomes these limitations [27]. It uses hard x-rays and is therefore bulk sensitive. At large momentum transfer q\mathbf{q}, the dipole-forbidden 3s→3d3s \rightarrow3d (Ni M1M_1) transition dominates. Because the 3s3s core hole is spherically symmetric, the dependence of the energy-integrated intensity on the direction q\mathbf{q} directly images the angular distribution of the 3d3d holes, free from multiplet effects. The method was demonstrated in NiO [27] and recently applied to perovskite, infinite-layer and single-layer nickelates [28]. Here we use ss-NIXS on a bulk La2_2SmNi2_2O7_7 crystal to measure hz2/hx2−y2h_{z^2}/h_{x^2-y^2}. We find a ratio close to 1, well above the value 2/3 of a filled bonding band, which points to Hund’s-coupled Ni d8d^8 with ligand holes.

The single crystal (50×50×110 μm350 \times50 \times110\ \mu\mathrm{m}^{3}) was grown at ambient pressure from a K2CO3\mathrm{K}_{2}\mathrm{CO}_{3} flux, as described in Ref. [7] which also reports its superconductivity under high pressure. At ambient pressure the structure is monoclinic (P21/mP2_{1}/m), with Sm preferentially occupying the rare-earth site between the bilayers [7, 29]. Prior to the ss-NIXS measurements, the crystal was oriented by x-ray diffraction within the average tetragonal space group I4/mmmI4/mmm (139), with a≃3.8a \simeq3.8 Å and c≃20c \simeq20 Å [30]. In the following, x=[100]x = [100] and y=[010]y = [010] run along the Ni–O bonds and z=[001]∥cz = [001] \parallel c. The azimuthal orientation is known to within 0.5∘0.5^\circ, so that a misalignment reduces the dx2−y2d_{x^{2}-y^{2}} contribution according to cos⁡22φ\cos^{2} 2\varphi (with φ\varphi the deviation angle from perfect alignment) to less than 10−310^{-3}.

The measurements were performed at room temperature on the GALAXIES beamline at SOLEIL Synchrotron using the MATRIXS spectrometer equipped with 40 Si(110) spherically bent analyzer crystals (R=1R = 1 m). The spectrometer operates in a fixed Johann geometry with a Bragg angle of 87∘87^\circ. In this geometry, the analyzer energy is fixed at 9.70 keV, while the incident energy is scanned from 9.785 to 9.825 keV across the Ni M1M_{1} edge energy. The overall energy resolution is 1 eV at ∣q∣=9.65|\mathbf{q}| = 9.65 Å−1^{-1} as estimated from the width of the elastic line. Of the 40 analyzers, the ten analyzers closest to the backscattering direction (2ϑ=155∘2\vartheta= 155^\circ) were selected, and their signals summed. The resulting solid angle covers ±10∘\pm10^\circ both within and perpendicular to the scattering plane, corresponding to an angular spread of about ±5∘\pm5^\circ in q^\hat{\mathbf{q}} (where q^\hat{\mathbf{q}} is the mean direction over the selected analyzers) since a rotation δ\delta of the scattered wave vector rotates q^\hat{\mathbf{q}} by δ/(2sin⁡ϑ)\delta/(2 \sin\vartheta). To obtain the orbital symmetry, the crystal was rotated about the yy axis, so that q^\hat{\mathbf{q}} sweeps the (x,z)(x,z) plane at an angle θ\theta from zz [Fig. 1(b)]. Each spectrum contains the La N4,5N_{4,5} and Ni M1M_{1} edges. The Sm N4,5N_{4,5} edge which falls at approximately 129 eV is not included in our energy loss window.

Figure 2(a) shows an example of ss-NIXS spectrum at one angle. The complete data set is provided in the Supplemental Material [30]. The spectrum consists of a strong signal from the La N4,5N_{4,5} edges between 98 and 107 eV, followed by the Ni M1M_{1} edge centered at 110.76±0.08110.76 \pm0.08 eV. As the La contribution is isotropic (see Suppl. Mat.), it can be used to normalize the Ni M1M_{1} signal from possible intensity variations arising from changes in the scattering volume upon rotation, as well as variations in absorption and incident-beam intensity. To extract the ss-NIXS angular dependence, the full spectrum is fitted for each angle using the sum of a quadratic background, a single Gaussian for the Ni peak and the La edge line shape, which was derived from measurements in the Ni-free cuprate La2−xSrxCuO4\mathrm{La}_{2-x}\mathrm{Sr}_{x}\mathrm{CuO}_{4} and is only scaled in amplitude.

We note that the width of the Ni contribution (5.57±0.225.57 \pm0.22 eV) is larger than the spectrometer resolution; the implications for the results are discussed below.

Figure 2(b) shows the Ni spectra after subtraction of the La edge and of the background. The integrated Ni intensity exhibits a pronounced angular dependence, with similar values along zz and along xx and a minimum near 45∘45^\circ.

Sum of the energy-loss spectra and Ni M1 peak after subtraction

Figure 2. (a) Sum of the energy-loss spectra of La2_2SmNi2_2O7_7 (points) with the fit: La N4,5N_{4,5} edge (blue, line shape of La2−x_{2-x}Srx_xCuO4_4), Ni M1M_1 peak (purple), quadratic background (dashed). Residuals are shown below. (b) Ni M1M_1 peak after subtraction of the La edge and background, for three directions of q\mathbf{q} obtained by symmetry averaging (offset for clarity). Lines: Gaussian of fixed position and width with free area.

Considering a hole in an orbital ψ\psi, the 3s→3d3s \rightarrow3d intensity [27, 31] can be expressed as ∣⟨R3d∣j2(qr)∣R3s⟩∣2∣ψ(q^)∣2|\langle R_{3d}|j_{2}(qr)|R_{3s}\rangle|^{2}|\psi(\hat{\mathbf{q}})|^{2}. Here j2j_{2} is a spherical Bessel function, and ∣ψ(q^)∣2|\psi(\hat{\mathbf{q}})|^{2} is the angular part of the orbital density. The radial factor is the same for both the ege_g orbitals and is included into a global scaling factor I0I_{0}. For q^\hat{\mathbf{q}} in the (x,z)(x,z) plane,

I(θ)=I0[hz2516π(3cos⁡2θ−1)2+hx2−y21516πsin⁡4θ],(1)I(\theta)=I_{0}\left[h_{z^{2}}\frac{5}{16\pi}(3\cos^{2}\theta-1)^{2}+h_{x^{2}-y^{2}}\frac{15}{16\pi}\sin^{4}\theta\right], \tag*{(1)}

where hz2h_{z^{2}} and hx2−y2h_{x^{2}-y^{2}} are the numbers of holes in each orbital. Equation (1) assumes that the t2gt_{2g} shell is fully occupied. A t2gt_{2g} (dxzd_{xz}) hole would add a sin⁡22θ\sin^{2}2\theta term, which reaches a maximum at 45∘45^\circ. Adding such a term, with a free amplitude AtA_{t}, to the fit of the data gives At/Az=−0.03±0.06A_{t}/A_{z} = -0.03 \pm0.06 relative to the dz2d_{z^{2}} amplitude: it is compatible with zero, so there is no evidence of t2gt_{2g} holes, and hz2/hx2−y2h_{z^{2}}/h_{x^{2}-y^{2}} is unchanged [30]. Equation (1) also neglects off-diagonal dz2d_{z^{2}}–dx2−y2d_{x^{2}-y^{2}} terms. In the low-symmetry structure these terms are allowed. They give a contribution ∝(3cos⁡2θ−1)sin⁡2θcos⁡2φ\propto(3\cos^{2}\theta-1)\sin^{2}\theta\cos2\varphi, which changes sign between twin domains rotated by 90∘90^\circ. It therefore cancels for equal twin fractions, which is supported by x-ray diffraction on the crystal [30].

Figure 3 shows the measured intensity as a function of the angle θ\theta between q\mathbf{q} and zz [Fig. 3(a)] and folded into one quadrant by the mirror symmetries z→−zz \rightarrow-z and x→−xx \rightarrow-x [Fig. 3(b)]. The main result is already apparent from the data: After symmetry averaging, the intensities near the zz and xx directions are nearly equal. The Ni/La intensity ratios are 0.45±0.030.45 \pm0.03 at θ≃5∘\theta\simeq5^\circ and 0.45±0.020.45 \pm0.02 at θ≃81∘\theta\simeq81^\circ. The fitted intensity contrast, I(z)/I(x)=0.95±0.05I(z)/I(x) = 0.95 \pm0.05, is substantially larger than the value of 0.73 expected for a hole occupancy ratio hz2/hx2−y2=2/3h_{z^{2}}/h_{x^{2}-y^{2}} = 2/3. The intensity reaches a minimum near θ=45∘\theta= 45^\circ.

We fit (1) to the data after averaging over the ±5∘\pm5^\circ acceptance angle using three free parameters: Az=I0hz2A_{z} = I_{0}h_{z^{2}}, Ax=I0hx2−y2A_{x} = I_{0}h_{x^{2}-y^{2}} and an angular offset θc\theta_{c}. We obtain Az=1.19±0.04A_{z} = 1.19 \pm0.04, Ax=1.27±0.06A_{x} = 1.27 \pm0.06 and θc=7.7±1.0∘\theta_{c} = 7.7 \pm1.0^\circ, with a reduced χ2\chi^{2} of 1.09; the uncertainties are scaled by χred2\sqrt{\chi_{\mathrm{red}}^{2}}. The offset is close to the 6.6∘6.6^\circ expected from the orientation of the crystal determined by x-ray diffraction. Including the correlation between AzA_{z} and AxA_{x}, we find

hz2/hx2−y2=0.94±0.06 (stat) −0.01+0.08 (syst).(2)h_{z^{2}}/h_{x^{2}-y^{2}} = 0.94 \pm0.06\ \text{(stat)}\,{}^{+0.08}_{-0.01}\ \text{(syst)}. \tag*{(2)}

This corresponds to a fraction 48.4±1.6%48.4 \pm1.6\% of the ege_g holes in dz2d_{z^{2}}. A fit of the symmetry-averaged data gives 0.93 ±\pm 0.06. The systematic range comes from varying one analysis choice at a time [30]: the selection thresholds, the angular acceptance, the angular offset, the background and the Ni line shape (Fig. S3 of Ref. [30]). The largest change, +0.08, comes from a cubic background. The ratio also depends on the assumed width of the Ni peak, by −0.11 per eV (1.02, 0.91 and 0.83 for imposed widths of 5, 6 and 7 eV). The width is determined by the data, and its statistical uncertainty, ±0.22\pm0.22 eV, changes the ratio by ±0.02\pm0.02 [30].

Average tetragonal structure, scattering geometry, and angular dependence of the Ni $M_1$ intensity

Figure 1. (a) Average tetragonal structure of La2_2SmNi2_2O7_7 (I4/mmmI4/mmm, no. 139), viewed along [10] with the axes [100] and [1] ∥c\parallel c (as in panels b and c); the actual symmetry is monoclinic P21/mP2_1/m [7]. Ni gray, O red, La/Sm green/pink, drawn with the average occupancy (La 2/3, Sm 1/3) on all rare-earth sites. (b) Scattering geometry. The incident beam (ki\mathbf{k}_i, ωi\omega_i) is scattered by the sample; the analyzers select the energy ωf\omega_f of the scattered beam (kf\mathbf{k}_f) and image it on a two-dimensional detector. The momentum transfer q=ki−kf\mathbf{q} = \mathbf{k}_i - \mathbf{k}_f lies in the horizontal plane. The sample rotates about the vertical axis y=[010]y = [010], so that q\mathbf{q} sweeps the (x,z)(x,z) plane; θ\theta denotes the angle between q\mathbf{q} and z∥cz \parallel c. The shapes drawn at the sample are the angular densities ∣Yz2∣2\lvert Y_{z^2}\rvert^2 (green), along zz, and ∣Yx2−y2∣2\lvert Y_{x^2-y^2}\rvert^2 (pink), along xx and yy. Only the ten analyzers closest to backscattering are used here. (c) Angular dependence of the Ni M1M_1 intensity from Eq. (1) for hz2/hx2−y2=2/3h_{z^2}/h_{x^2-y^2}=2/3 (filled bonding dz2d_{z^2} band), 0.87 (DMFT [17]) and 0.94 (this work), normalized at θ=90∘\theta= 90^\circ.

If all ege_g holes were localized on Ni and the bonding dz2d_{z^2} band were fully occupied, each Ni would have one dz2d_{z^2} hole and 1.5 dx2−y2d_{x^2-y^2} holes, yielding hz2/hx2−y2=2/3h_{z^2}/h_{x^2-y^2}=2/3. Our measured value exceeds this by 4.4 statistical standard deviations, and constraining the ratio to 2/3 deteriorates the fit χr2\chi_r^2 value from 1.09 to 2.53. All alternative analyses yield values above 2/3, the lowest being 0.93 ±\pm 0.06. The same conclusion holds when the Ni peak width is fixed to values between 4 and 7 eV; the lowest ratio in this range is 0.83 ±\pm 0.05, obtained for a width of 7 eV. Our result is consistent with the DMFT prediction of hz2/hx2−y2≃0.87h_{z^2}/h_{x^2-y^2} \simeq0.87 [17], which is obtained from Wannier occupations of 0.60 (dz2d_{z^2}) and 0.54 (dx2−y2d_{x^2-y^2}) per spin orbital. Our accuracy does not distinguish this value from 1.

A ratio close to 1 can be understood within an atomic picture. In presence of strong Hund’s coupling, a high-spin (S=1S = 1) Ni d8d^8 ion has one hole in each ege_g orbital, yielding hz2/hx2−y2=1h_{z^2}/h_{x^2-y^2}=1. In contrast, a low-spin d7d^7 ion with its ege_g electron in dz2d_{z^2} yields a ratio of 0.5 while a filled bonding band yields a ratio of 2/3. Our result therefore suggests a Ni configuration close to d8d^8 with the remaining holes residing on the oxygen ligands. This interpretation is consistent with the Ni 3dd count of approximately 8.24 obtained in DMFT calculations [17] indicating a dominant contribution from the d8d^8 configuration [18]. DFT+UU calculations of La3_3Ni2_2O7_7 likewise find a Ni 3dd charge close to d8d^8 on all Ni sites, the d7d^7 character of the low-spin sites appearing only in the spin density [16]. In this picture, Hund’s coupling rather than the bonding–antibonding splitting of dz2d_{z^2} governs the ege_g occupations. This picture is consistent with the holes found in both ege_g orbitals by linear dichroism at the O KK edge in films [24] and with the weak orbital polarization observed in bulk samples, also interpreted in terms of Hund’s-coupled d8d^8 [25]. Our finding adds a quantitative estimate in a bulk crystal without the difficulties associated with multiplet effects and proximity of the La M4M_4 edge.

The DMFT calculation also points to the origin of this deviation. The total Ni 3dd count is approximately 8.24 compared to the nominal value of 7.5 [17]. Compared with the ionic limit, most of the additional electrons go into dx2−y2d_{x^2-y^2} (0.58 per Ni, against 0.2 in dz2d_{z^2}). These extra Ni 3dd electrons are transferred from the neighboring oxygen, leading to ligand holes with mainly in-plane x2−y2x^2-y^2 symmetry, which is reminiscent of Zhang–Rice singlet states in cuprates [3]. This picture is consistent with our measured orbital hole-occupancy ratio. Two caveats should, however, be considered. First, the calculations are performed in the high-pressure phase; to our knowledge, no equivalent calculation has been reported at ambient pressure. Second, electron-energy-loss spectroscopy finds ligand holes with comparable densities on the planar and on the inner apical oxygens [22]; the latter hybridize with dz2d_{z^2} and act in the opposite direction. This is an intrinsic effect, already included in our measurement. Finally, oxygen vacancies, located mainly on the inner apical site [22], donate electrons, which fill the ligand holes on the planar and inner apical oxygens almost equally [22]. A slight oxygen deficiency is therefore not expected to bias the ratio in a definite direction.

The quantity measured here is the hole ratio hz2/hx2−y2h_{z^2}/h_{x^2-y^2}; the orbital electron occupations, ni=2−hin_i = 2 - h_i, also depend on the total number of ege_g holes h=hz2+hx2−y2h = h_{z^2} + h_{x^2-y^2}, which is not measured. Between the ionic value h=2.5h = 2.5 and the DMFT value h≃1.72h \simeq1.72, our hole ratio of 0.94 yields an electron-occupation ratio nx2−y2/nz2≃0.90n_{x^2-y^2}/n_{z^2} \simeq0.90–0.95, and no lower than 0.73 for the lowest hole ratio found when the width of the Ni peak is varied (0.83, for 7 eV). By comparison, a hole ratio of 2/3 (a fully occupied bonding dz2d_{z^2} band) gives nx2−y2/nz2=0.5n_{x^2-y^2}/n_{z^2} = 0.5 for h=2.5h = 2.5, and the equal-occupation picture of Ref. [11] gives nx2−y2/nz2=1n_{x^2-y^2}/n_{z^2} = 1, i.e. hz2/hx2−y2=1h_{z^2}/h_{x^2-y^2} = 1, independently of hh. Our result is close to the latter estimate, lending strong support to scenarios in which both orbitals take part in the pairing [14, 15].

In summary, we have probed the Ni ege_g holes distribution in the bilayer nickelate La2_2SmNi2_2O7_7 using s-NIXS. We obtain a hole occupation ratio hz2/hx2−y2=0.94−0.01+0.08h_{z^2}/h_{x^2-y^2} = 0.94^{+0.08}_{-0.01}, significantly above the value of 2/3 expected for a filled-bonding-band and consistent with charge-transfer DMFT calculations. Our results suggest that theories of superconductivity in these materials should start from nearly equal ege_g occupations at ambient pressure. A cluster or multiplet calculation of the Ni M1M_1 final states and a DFT+DMFT calculation of La2_2SmNi2_2O7_7 at ambient pressure would allow a more direct comparison with our data, since the available DMFT occupations were obtained for the high-pressure phase [17].

ss-NIXS has several limitations still. First, it probes the Ni-projected hole density averaged over the fluctuating dnd^n configurations while providing no information about band dispersion. Second, the method remains relative as determining the absolute number of holes hh would require a reference compound to be measured using the same setup. Finally, our measurements were performed at room temperature, above the density-wave transition near 150 K reported in La3_3Ni2_2O7_7 [32]. Nevertheless, our approach provides a model-free description of the orbital physics in bulk correlated systems which applies well to nickelates. In these systems, the method could be extended to the full rare-earth series where chemical pressure is predicted to alter the ege_g occupations [33, 34, 35], or different sample environments such as low temperature to cross the density-wave transition or under applied pressure in a diamond anvil cell.

Acknowledgments

We acknowledge SOLEIL for provision of beamtimes at GALAXIES beamline (Proposals 20210421, 20221287, 20231963, 20240332, 20250647 and 99260232). This work was supported by the Paris Ile-de-France Region within the DIM MaTerRE (project DAC-VX) and DIM-MAP (project MATRIXS-4H) programs. Junjie Zhang was supported by the Natural Science Foundation of Shandong Province, China (Grant No. ZR2026ZD32) and the National Natural Science Foundation of China (Grants Nos. 12374457 and 12074219).

Data availability. The data that support the findings of this article are available from the authors upon reasonable request.

Supplemental Material for “Direct imaging of the Ni ege_g hole orbitals in the bilayer nickelate La2_2SmNi2_2O7_7”

Ethan Saïman; Feiyu Li; Junjie Zhang; Jean-Pascal Rueff; Victor Balédent

SM_v4.pdf

Supplemental Material for ``Direct imaging of the Ni ege_g hole orbitals in the bilayer nickelate La2_2SmNi2_2O7_7''

Sample

The La2_2SmNi2_2O7_7 single crystal (50 ×\times 50 ×\times 110  μm3\ \mu\mathrm{m}^3) was grown at ambient pressure from a K2_2CO3_3 flux at Shandong University, following [1]. Its structure is monoclinic (P21/mP2_1/m), with Sm preferentially on the rare-earth site between the bilayers [1]. It was oriented by x-ray diffraction at the Laboratoire de Physique des Solides, with an accuracy better than 0.5° on the azimuthal angle; the corresponding reduction of the dx2−y2d_{x^2-y^2} term, cos⁡22φ\cos^2 2\varphi, is below 10−310^{-3}. We use pseudo-tetragonal axes, with x=[100]x = [100] and y=[010]y = [010] along the Ni–O bonds and z=[001]∥cz = [001] \parallel c.

X-ray diffraction

The crystal used for the ss-NIXS measurements was characterized on the high-pressure diffraction setup developed at the Laboratoire de Physique des Solides (Orsay, France). The diffractometer uses a microfocus Mo x-ray tube (Incoatec GmbH) with Montel multilayer focusing optics, which delivers a monochromatic beam (λ=0.711\lambda= 0.711 Å) with a 100 μ\mum spot size and a divergence of 0.5 mrad at the sample. The diffracted intensity is recorded on a large-area MAR345 image-plate detector (MarXperts GmbH). Data were acquired in steps of 1° over a rotation range of 340°, with an exposure of 300 s per frame. The images were indexed with CrysAlisPro [2]: 1017 of the 1252 measured Bragg reflections are indexed with a tetragonal cell of 5.4×5.4×20.165.4 \times5.4 \times20.16 Å3^3. This cell is the 2×2\sqrt{2} \times\sqrt{2} cell of the I4/mmmI4/mmm cell used in the main text (a=5.4/2≃3.8a = 5.4/\sqrt{2} \simeq3.8 Å, c≃20.2c \simeq20.2 Å).

The tetragonal average structure shows that the crystal is not a single monoclinic domain, the monoclinic distortion of the P21/mP2_1/m structure being averaged over domains rotated by 90° relative to each other, with comparable populations. This is the condition for which the off-diagonal dz2−dx2−y2d_{z^2-d_{x^2-y^2}} terms cancel.

Data acquisition and reduction

The measurements were performed at room temperature on the GALAXIES beamline of SOLEIL. The spectrometer has 40 spherically bent Si(110) analyzers (R=1R = 1 m), imaged on a two-dimensional detector, which select a fixed final energy of 9.70 keV. The incident energy is scanned from 9.857 to 9.825 keV with 161 points and 30 s per point (10 s per point for the scans at nominal angles −100∘-100^\circ to −60∘-60^\circ); the energy resolution is 1 eV. For this work we use the ten analyzers closest to backscattering, centered at 2ϑ=155∘2\vartheta= 155^\circ (∣q∣=9.65|q| = 9.65 Å−1^{-1}), which give the best statistics.

For each angle, an elastic scan and an energy-loss scan were recorded. The data set contains 36 energy-loss scans at 26 nominal angles; repeated scans at the same angle are treated as independent points. For each scan, the procedure is as follows:

  1. Hot and dead pixels are replaced by the median of their neighbors.

  1. One region of interest is defined for each analyzer and is re-centered on the elastic image of the same scan.

  1. The energy scale of each analyzer is calibrated on the elastic line of the same scan (or, if absent, on the first elastic scan at that angle).

  1. The ten analyzer spectra are interpolated on a common energy axis and summed.

No normalization by a beam monitor is applied. The normalization is provided by the La N4,5N_{4,5} area (Sec. ). This area is an internal reference measured simultaneously with the Ni signal, on the same detector pixels and from the same scattering volume.

Line-shape model

La N4,5 edge

The 4d→4f4d \to4f excitation of La3+\mathrm{La}^{3+} connects a full 4d4d shell to an empty 4f4f shell. It is not purely dipolar: at large qq the operator eiq⋅re^{i\mathbf{q}\cdot\mathbf{r}} contains all multipoles of rank k=1k=1, 3 and 5 allowed between l=2l=2 and l=3l=3, with qq-dependent weights (radial integrals of jk(qrj_k(qr)). Because the initial state is a closed shell (1S0{}^{1}S_{0}, J=0J=0), a multipole of rank kk can only reach final states with Jf=kJ_f=k, so that different ranks do not interfere, and for each of them the sum over MfM_f of ∣YkMf(q^)∣2\left|Y_{kM_f}(\hat{\mathbf{q}})\right|^2 is independent of q^\hat{\mathbf{q}}. Non-dipolar contributions therefore modify the shape of the edge, and not its isotropy. As the weights depend on ∣q∣\lvert q\rvert, the line shape must be measured at the same ∣q∣\lvert q\rvert as the nickelate, which is the case for La2−xSrxCuO4\mathrm{La}_{2-x}\mathrm{Sr}_x\mathrm{CuO}_4 (Sec. ). The intensity of the whole edge is therefore independent of the direction of q\mathbf{q} at every energy loss, apart from the crystal-field splitting of the 4f4f final states (tens of meV), which is negligible at the 1 eV resolution. The edge (98–107 eV) lies entirely within the fit window (88–126 eV) and is fitted as a whole. Its shape is described by five Gaussians (four peaks and a shoulder at 107 eV) determined on La2−xSrxCuO4\mathrm{La}_{2-x}\mathrm{Sr}_x\mathrm{CuO}_4, a La compound without Ni (Sec. , Table S1). In the fit of each spectrum, this shape is shifted rigidly by 0.06 eV (determined on the sum of the retained spectra; the allowed range is ±0.5\pm0.5 eV), and only a global scale SS is free. The quantity analyzed in the main text is the Ni M1M_1 area divided by the area of the main La Gaussian times SS. The Sm N4,5N_{4,5} edge sets in at about 126 eV, with a maximum at 129 eV, at the upper end of the window.

PeakPosition (eV)FWHM (eV)Relative area
0105.461.561
1101.841.750.550
299.601.520.155
3103.641.730.364
4 (shoulder)107.123.850.122

Table S1. La N4,5N_{4,5} line shape determined on La2−xSrxCuO4\mathrm{La}_{2-x}\mathrm{Sr}_x\mathrm{CuO}_4 (Gaussians; areas relative to the main peak; positions before the 0.06 eV shift).

Check of the La N4,5 line shape on a Ni-free compound

The La edge is the reference for the whole analysis, so its shape must not depend on the sample. We determined it on a compound that contains La but no Ni, the cuprate La2−xSrxCuO4\mathrm{La}_{2-x}\mathrm{Sr}_x\mathrm{CuO}_4 (x=0.08x=0.08), measured at 300 K in the same setup, with the same analyzers and the same scattering angle (2ϑ=155∘2\vartheta=155^\circ). Its spectrum has the same La N4,5N_{4,5} edge and, at higher energy, the Cu M1M_1 peak at 121.6 eV (Figure S1). The spectrum of this compound is the sum of all its measurements, fitted with La N4,5N_{4,5} (five Gaussians, Table S1), a parabolic background and the M1M_1 peak (χr2=1.67\chi_r^2=1.67). In Figure S1 we superimpose the La N4,5N_{4,5} edge of the two compounds, i.e. the data minus the fitted background and M1M_1 peak, each normalized to the maximum of the edge. The two edges coincide in position and in the relative weights of the three structures at 99.6, 102 and 105.5 eV. After the rigid energy shift of 0.06 eV used in the fits, which is within the calibration uncertainty, the rms difference between 97 and 108 eV is 1.3% of the maximum, and the largest deviation is 3% (Figure S1, bottom), i.e. 1.2 times the noise. These deviations are of the order of the noise and of the uncertainty on the subtraction of the M1M_1 tail. The La edge of La2SmNi2O7\mathrm{La}_2\mathrm{SmNi}_2\mathrm{O}_7 therefore has the shape of an isolated La3+ 4d→4f\mathrm{La}^{3+}\ 4d \to4f edge, and the shape of Table S1, which is used for the nickelate with only a shift and an amplitude, does not contain a Ni contribution. We use this comparison only for the La line shape, not for the M1M_1 peaks of the two compounds.

Check of the La N₄,₅ line shape

Figure S1. Check of the La N4,5_{4,5} line shape. (a) La2_2SmNi2_2O7_7: data minus background (points), La N4,5_{4,5} edge (blue) and Ni M1M_1 peak (purple); the La maximum is set to 1. (b) La2−x_{2-x}Srx_xCuO4_4, a La compound without Ni, in the same units: La N4,5_{4,5} edge (blue) and Cu M1M_1 peak (orange). (c) La N4,5_{4,5} edges of the two compounds (data minus background and M1M_1 peak), normalized to their maximum; the energy of the cuprate is shifted by 0.06 eV. Bottom: difference between the two (nickelate minus cuprate); the gray band is the noise (±1σ\pm1\sigma).

Background and Ni M1M_1 peak

The background is a quadratic polynomial over the full window; linear and cubic backgrounds are tested in Table S2. The Ni M1M_1 peak is a single Gaussian of non-negative amplitude. Its position, 110.76 ±\pm 0.08 eV, and width, FWHM = 5.57 ±\pm 0.22 eV, are fixed on the sum of the retained spectra at nominal angles −20∘-20^\circ to 30∘30^\circ, i.e. with q^\hat{q} within ≃25∘\simeq25^\circ of zz, where the peak is strongest. For each spectrum, only the Ni area A≥0A \ge0, the La scale SS and the background are free. The noise of each spectrum is estimated from point-to-point differences. The uncertainty on A/SA/S is obtained from the covariance matrix, including the AA–SS correlation. The width exceeds the 1 eV resolution; its effect on the hole ratio is discussed in Sec. .

VariantNNM1 FWHM (eV)hz2/hx2−y2h_{z^2}/h_{x^2-y^2}χr2\chi_r^2
Reference235.570.939±0.0610.939\pm0.0611.09
Symmetrized reference23 (10 groups)5.570.935±0.0560.935\pm0.0560.56
θc\theta_c fixed to the diffraction value (6.6°)245.570.977±0.0680.977\pm0.0681.35
Acceptance ±0∘\pm0^\circ235.570.938±0.0610.938\pm0.0611.07
Noise cut 1.0×1.0\times median195.630.967±0.0720.967\pm0.0721.15
Noise cut 1.5×1.5\times median245.640.943±0.0610.943\pm0.0611.09
No spectra retained by hand (−50∘-50^\circ to −30∘-30^\circ)205.570.932±0.0620.932\pm0.0621.09
Without 160∘160^\circ and 200∘200^\circ225.600.941±0.0640.941\pm0.0641.13
M1 amplitude of either sign235.570.939±0.0610.939\pm0.0611.09
Lorentzian M1225.300.953±0.0600.953\pm0.0600.79
M1 position in 111–113 eV225.260.963±0.0620.963\pm0.0620.89
Linear background254.930.981±0.1040.981\pm0.1043.59
Cubic background245.601.020±0.0921.020\pm0.0921.69
M1 FWHM imposed to 3 eV223.001.327±0.1141.327\pm0.1140.74
M1 FWHM imposed to 4 eV244.001.131±0.0991.131\pm0.0991.47
M1 FWHM imposed to 5 eV245.001.023±0.0791.023\pm0.0791.44
M1 FWHM imposed to 6 eV236.000.909±0.0580.909\pm0.0581.07
M1 FWHM imposed to 7 eV227.000.825±0.0500.825\pm0.0500.91

Table S2. Hole ratio for single-parameter variations of the analysis. NN: number of spectra used; M1 FWHM: width of the Ni peak. The last rows impose the width of the Ni peak and are not included in the systematic range.

Selection of the spectra

Of the 36 spectra, 13 are discarded. Ten of them belong to the block of nominal angles −100∘-100^\circ to −60∘-60^\circ, where the counting time was 10 s per point instead of 30 s, i.e. three times shorter. Six of these have an uncertainty on Ni/LaN_{\mathrm{i}}/La above 1.2 times the median (0.045, for a median of 0.037). Three scans at −65∘-65^\circ and −60∘-60^\circ, whose uncertainty is below that threshold, are excluded with the rest of the block. The tenth (−70∘-70^\circ#2) is rejected as an outlier (see below). Two spectra at −20∘-20^\circ have an uncertainty of 0.070 and 0.091, above the threshold. After a first robust fit of the orbital model, spectra whose residual exceeds 2.5 robust standard deviations (median absolute deviation) are rejected iteratively; this removes −70∘-70^\circ#2 and one spectrum at 160∘160^\circ. The spectra at −50∘-50^\circ, −40∘-40^\circ and −30∘-30^\circ have an uncertainty of 0.046–0.051, slightly above the threshold; they are retained because they lie near the minimum of the angular dependence (without them, hz2/hx2−y2=0.932±0.062h_{z^2}/h_{x^2-y^2}=0.932\pm0.062, Table S2). The remaining 23 spectra, at 19 angles, are used. The effect of the thresholds on the hole ratio is given in Table S2.

Orbital fit

Individual spectra. Figure S2 shows the Ni M1M_1 peak of each of the 23 retained spectra, after subtraction of the fitted La N4,5N_{4,5} edge and background, in the same way as Fig. 2(b) of the main text. The spectra are ordered by the angle θ\theta between q\mathbf{q} and zz, folded into [0,90∘][0,90^\circ]. Each spectrum is normalized to the La scale of its own fit (area of the main La Gaussian equal to 1), so that the area of the Gaussian is the Ni/La ratio listed in each panel. The Gaussian has the position and width fixed on the sum of the spectra (Sec. ), and only its area is free. The ratio is largest for q\mathbf{q} close to zz (θ≲20∘\theta\lesssim20^\circ) and to the xyxy plane (θ≳70∘\theta\gtrsim70^\circ), and smallest around θ=40\theta=40–50∘50^\circ, as expected from Eq. (1) of the main text. The spectra differ in statistical quality, because the signal depends on the direction of q\mathbf{q}. Some spectra show structures that the Gaussian does not describe, such as a small dip between 115 and 120 eV or a rise above 123 eV. They come from the imperfect subtraction of the tail of the La edge and of the background; they are the origin of the dependence of the ratio on the width of the Ni peak discussed in Sec. .

The Ni/La ratio is fitted with

R(θ)=Az⟨∣Yz2(θ−θc)∣2⟩+Ax⟨∣Yx2−y2(θ−θc)∣2⟩,(3)R(\theta)=A_z\left\langle\left|Y_{z^2}(\theta-\theta_c)\right|^2\right\rangle+A_x\left\langle\left|Y_{x^2-y^2}(\theta-\theta_c)\right|^2\right\rangle, \tag*{(3)}

with ∣Yz2∣2=516π(3cos⁡2θ−1)2\left|Y_{z^2}\right|^2=\frac{5}{16\pi}(3\cos^2\theta-1)^2 and ∣Yx2−y2∣2=1516πsin⁡4θ\left|Y_{x^2-y^2}\right|^2=\frac{15}{16\pi}\sin^4\theta in the (x,z)(x,z) plane. Brackets denote the average over the in-plane acceptance, ±5∘\pm5^\circ (21 points). The offset θc\theta_c is free. Weighted least squares give Az=1.19±0.04A_z=1.19\pm0.04, Ax=1.27±0.06A_x=1.27\pm0.06 and θc=7.7±1.0∘\theta_c=7.7\pm1.0^\circ for 23 points, with χr2=1.09\chi_r^2=1.09. Uncertainties are scaled by χr2\sqrt{\chi_r^2}. Then hz2/hx2−y2=Az/Ax=0.939±0.061h_{z^2}/h_{x^2-y^2}=A_z/A_x=0.939\pm0.061, including the covariance of AzA_z and AxA_x (correlation −0.25-0.25), and the dz2d_{z^2} fraction is Az/(Az+Ax)=48.4±1.6%A_z/(A_z+A_x)=48.4\pm1.6\%. The ratio differs from 2/32/3 by 4.4 standard deviations; accordingly, fixing hz2/hx2−y2=2/3h_{z^2}/h_{x^2-y^2}=2/3, with one free amplitude and θc\theta_c free, raises χ2\chi^2 from 21.7 to 53.0 (χr2\chi_r^2 from 1.09 to 2.53).

Symmetry averaging. The intensity is invariant under z→−zz\rightarrow-z and x→−xx\rightarrow-x. The retained spectra are folded into 0≤θ≤90∘0\leq\theta\leq90^\circ and grouped within 5∘5^\circ. The spectra of each group are summed and refitted. The ten groups give hz2/hx2−y2=0.935±0.056h_{z^2}/h_{x^2-y^2}=0.935\pm0.056 (χr2=0.56\chi_r^2=0.56). Near zz (θ≃5∘\theta\simeq5^\circ, two spectra) and near xx (θ≃81∘\theta\simeq81^\circ, four spectra), the Ni/La ratios are 0.454±\pm0.027 and 0.452±\pm0.021. The contrast I(z)/I(x)=4hz2/(hx2−y2+3hz2)I(z)/I(x)=4h_{z^2}/(h_{x^2-y^2}+3h_{z^2}) of the fit is 0.95±\pm0.05; the value expected for hz2/hx2−y2=2/3h_{z^2}/h_{x^2-y^2}=2/3 is 0.73. Figure S4 shows the data of Fig. 3 of the main text without folding.

Data of Fig. 3 of the main text without folding

Figure S4. Data of Figure 3 of the main text without folding. (a) Ni M1_1/La N4,5_{4,5} as a function of θ\theta (as in Figure 3a). (b) Polar representation over 360∘360^\circ: individual spectra (gray) at their measured angle θ\theta between qq and z=[001]z = [001] (the axes are labeled by their crystallographic directions, x=[100]x = [100]); symmetry-averaged spectra (open circles) in one quadrant. Black line: fit; green and pink: dz2d_{z^2} and dx2−y2d_{x^2-y^2} contributions.

Angular acceptance

A rotation δ\delta of kf\mathbf{k}_{\mathrm{f}} rotates q=ki−kf\mathbf{q}=\mathbf{k}_{\mathrm{i}}-\mathbf{k}_{\mathrm{f}} by δkf/q=δ/(2sin⁡ϑ)≃0.51δ\delta k_{\mathrm{f}}/q=\delta/(2\sin\vartheta)\simeq0.51\delta at 2ϑ=155∘2\vartheta=155^\circ. The ±10∘\pm10^\circ spread of the analyzers thus corresponds to about ±5∘\pm5^\circ on q\mathbf{q}, in and out of the scattering plane. The fit includes the in-plane spread. The out-of-plane spread gives a small yy component and multiplies the dx2−y2d_{x^2-y^2} term by cos⁡22φ≃1−4⟨φ2⟩\cos^2 2\varphi\simeq1-4\langle\varphi^2\rangle. Averaging the model over the two-dimensional acceptance (±5∘\pm5^\circ in and out of the plane) leaves the hole ratio unchanged (0.938±\pm0.061) and gives χr2=1.08\chi_r^2=1.08.

Ni M1 peak spectra and fitted Gaussians

Figure S2. Ni M1M_1 peak of the 23 retained spectra after subtraction of the La N4,5N_{4,5} edge and of the background (points with statistical error bars), with the fitted Gaussian (line; fixed position and width, free area). Each panel is normalized to the La scale of the spectrum (area of the main La Gaussian = 1). The spectra are ordered by the angle θ\theta between q\mathbf{q} and z\mathbf{z} (folded into [0,90∘][0,90^\circ]), indicated with the Ni/La ratio in each panel. Green: θ<30∘\theta< 30^\circ; gray: 30∘<θ<60∘30^\circ< \theta< 60^\circ; pink: θ>60∘\theta> 60^\circ. The dotted line marks the position of the peak, 110.76 eV.

Assumptions of the model

  • Full t2gt_{2g} shell. A t2gt_{2g} hole (dxzd_{xz}) would add a contribution ∝sin⁡22θ\propto\sin^2 2\theta, peaked at 45∘45^\circ. Adding a free term At1516πsin⁡22θA_t \frac{15}{16\pi}\sin^2 2\theta to the fit gives At=−0.03±0.07A_t=-0.03\pm0.07 (At/Az=−0.03±0.06A_t/A_z=-0.03\pm0.06), compatible with zero, and χr2=1.13\chi_r^2=1.13,

with hz2/hx2−y2=0.938±0.062h_{z^2}/h_{x^2-y^2}=0.938\pm0.062, unchanged.

  • No dz2−dx2−y2d_{z^2}-d_{x^2-y^2} coherence. In the monoclinic structure, a hole orbital αdz2+βdx2−y2\alpha d_{z^2}+\beta d_{x^2-y^2} adds a term 2αβ5316π(3cos⁡2θ−1)sin⁡2θcos⁡2φ2\alpha\beta\frac{5\sqrt{3}}{16\pi}(3\cos^2\theta-1)\sin^2\theta\cos2\varphi. It changes sign between twin domains rotated by 90∘90^\circ (φ→φ+90∘\varphi\to\varphi+90^\circ) and cancels for equal twin fractions. The x-ray diffraction of the crystal gives a tetragonal average cell, which indicates domains rotated by 90∘90^\circ in comparable proportions.

  • Equal radial factors. The 3s→3d3s\to3d radial integral ⟨R3d∣j2(qr)∣R3s⟩\langle R_{3d}|j_2(qr)|R_{3s}\rangle is taken to be the same for both ege_g orbitals.

Systematic uncertainties

Table S2 and Figure S3 give hz2/hx2−y2h_{z^2}/h_{x^2-y^2} when one analysis choice is varied at a time, all other choices being those of the reference analysis. The variants concern the angular offset (fixed to the value 6.6∘6.6^\circ expected from the x-ray diffraction orientation), the angular acceptance, the noise threshold (1.0 and 1.5 times the median), the spectra retained by hand, the amplitude of the Ni peak (negative values allowed), its profile (Lorentzian) and position (restricted to 111–113 eV), the degree of the background, and symmetrization. All variants lie between 0.932 and 1.020. Except for the background, they differ from the reference by less than 0.04. The cubic background gives the largest change, +0.08, with a larger uncertainty (±0.09\pm0.09); the linear background gives 0.98±0.100.98\pm0.10 but a poor fit (χr2=3.6\chi_r^2=3.6). We quote the range covered by these variants as the systematic uncertainty: hz2/hx2−y2=0.94±0.06h_{z^2}/h_{x^2-y^2}=0.94\pm0.06 (stat) −0.01+0.08{}^{+0.08}_{-0.01} (syst).

Plot of $h_{z^2}/h_{x^2-y^2}$ for the reference analysis and analysis variants

Figure S3. hz2/hx2−y2h_{z^2}/h_{x^2-y^2} for the reference analysis (black; gray band: statistical uncertainty) and for the analysis variants of Table S2 (purple; error bars: statistical). The rows with an imposed width of the Ni peak are not shown. Dashed and dotted lines: filled bonding band (2/3) and DMFT [3].

The ratio also depends on the width of the Ni M1M_1 peak, which is correlated with the high-energy tail of the La edge: it decreases from 1.33 to 0.83 when the width is imposed between 3 and 7 eV (last rows of Table S2), by about −0.11-0.11 per eV near the fitted value. These rows are not included in the systematic range, because the width is determined by the data, 5.57±0.225.57\pm0.22 eV. Imposing the limits of this statistical interval, 5.35 and 5.80 eV, gives 0.956±0.0640.956\pm0.064 and 0.922±0.0590.922\pm0.059, i.e. a change of ±0.02\pm0.02 of the ratio. All widths between 3 and 7 eV give a ratio above 2/32/3.

Polar representation over 360°

Figure S4 shows the data of Figure 3 of the main text without folding. The Cartesian panel (a) is that of Figure 3(a). In the polar panel (b), the individual spectra (gray) are drawn at their measured angle θ=α−θc\theta=\alpha-\theta_c (modulo 360∘360^\circ), where

Ni M1/La N4,5 intensity as a function of angle

Figure 3. (a) Ni M1M_1/La N4,5N_{4,5} intensity of La2_2SmNi2_2O7_7 as a function of the angle θ\theta between q\mathbf{q} and z=[001]z = [001], over one period of 180∘180^\circ. Gray: individual spectra (spectra at θ\theta outside the window are shifted by 180∘180^\circ; horizontal bars: ±5∘\pm5^\circ acceptance); open circles: symmetry-averaged spectra. Black line: fit with Eq. (1); green and pink: dz2d_{z^2} and dx2−y2d_{x^2-y^2} contributions. (b) The same data in polar coordinates, folded into one quadrant. The fit gives hz2/hx2−y2=0.94±0.06h_{z^2}/h_{x^2-y^2} = 0.94 \pm0.06 with χr2=1.09\chi_r^2 = 1.09.

References

α\alpha is the nominal angle; those outside the window of Figure 3(a) are shifted there by 180°. The symmetry-averaged spectra (open circles) are shown in a single quadrant. The intensity has the symmetry of the orbital densities, I(θ)=I(−θ)=I(θ+180∘)I(\theta) = I(-\theta) = I(\theta+ 180^\circ), which is why the fit is the same in the four quadrants.

References

  1. [1]Y. Tokura and N. Nagaosa, Orbital physics in transition-metal oxides, Science 288, 462 (2000).pubmed.ncbi.nlm.nih.gov/10775098
  2. [2]J. G. Bednorz and K. A. Müller, Possible high Tc superconductivity in the Ba-La-Cu-O system, Z. Phys. B 64, 189 (1986).
  3. [3]F. C. Zhang and T. M. Rice, Effective hamiltonian for the superconducting Cu oxides, Phys. Rev. B 37, 3759 (1988).pubmed.ncbi.nlm.nih.gov/9944993
  4. [4]B. Keimer, S. A. Kivelson, M. R. Norman, S. Uchida, and J. Zaanen, From quantum matter to high-temperature superconductivity in copper oxides, Nature 518, 179 (2015).DOI
  5. [5]H. Sun, M. Huo, X. Hu, J. Li, Z. Liu, Y. Han, L. Tang, Z. Mao, P. Yang, B. Wang, J. Cheng, D.-X. Yao, G.-M. Zhang, and M. Wang, Signatures of superconductivity near 80 K in a nickelate under high pressure, Nature 621, 493 (2023).
  6. [6]N. Wang, G. Wang, X. Shen, J. Hou, J. Luo, X. Ma, H. Yang, L. Shi, J. Dou, J. Feng, J. Yang, Y. Shi, Z. Ren, H. Ma, P. Yang, Z. Liu, Y. Liu, H. Zhang, X. Dong, Y. Wang, K. Jiang, J. Hu, S. Nagasaki, K. Kitagawa, S. Calder, J. Yan, J. Sun, B. Wang, R. Zhou, Y. Uwatoko, and J. Cheng, Bulk high-temperature superconductivity in pressurized tetragonal La2PrNi2O7, Nature 10.1038/s41586-024-07996-8 (2024).DOI
  7. [7]F. Li, Z. Xing, D. Peng, J. Dou, N. Guo, L. Ma, Y. Zhang, L. Wang, J. Luo, J. Yang, J. Zhang, T. Chang, Y. S. Chen, W. Cai, J. Cheng, Y. Wang, Y. Liu, T. Luo, N. Hirao, T. Matsuoka, H. Kadobayashi, Z. Zeng, Q. Zheng, R. Zhou, Q. Zeng, X. Tao, and J. Zhang, Bulk superconductivity up to 96 k in pressurized nickelate single crystals, Nature 10.1038/s41586-025-09954-4 (2026).DOI
  8. [8]E. K. Ko, Y. Yu, Y. Liu, L. Bhatt, J. Li, V. Thampy, C.-T. Kuo, B. Y. Wang, Y. Lee, K. Lee, J.-S. Lee, B. H. Goodge, D. A. Muller, and H. Y. Hwang, Signatures of ambient pressure superconductivity in thin film La3Ni2O7, Nature 638, 935 (2025).DOI
  9. [9]G. Zhou, W. Lv, H. Wang, Z. Nie, Y. Chen, Y. Li, H. Huang, W. Q. Chen, Y. J. Sun, Q. K. Xue, and Z. Chen, Ambient-pressure superconductivity onset above 40 K in (La,Pr)3Ni2O7 films, Nature 640, 641 (2025).DOI
  10. [10]M. Wang, H.-H. Wen, T. Wu, D.-X. Yao, and T. Xiang, Normal and superconducting properties of La3Ni2O7, Chin. Phys. Lett. 41, 077402 (2024).
  11. [11]Z. Luo, X. Hu, M. Wang, W. Wú, and D.-X. Yao, Bilayer two-orbital model of La3Ni2O7 under pressure, Phys. Rev. Lett. 131, 126001 (2023).
  12. [12]Y. Zhang, L.-F. Lin, A. Moreo, and E. Dagotto, Electronic structure, dimer physics, orbital-selective behavior, and magnetic tendencies in the bilayer nickelate superconductor La3Ni2O7 under pressure, Phys. Rev. B 108, L180510 (2023).
  13. [13]Q.-G. Yang, D. Wang, and Q.-H. Wang, Possible s±-wave superconductivity in La3Ni2O7, Phys. Rev. B 108, L140505 (2023).
  14. [14]Y.-f. Yang, G.-M. Zhang, and F.-C. Zhang, Interlayer valence bonds and two-component theory for high-tc superconductivity of La3Ni2O7 under pressure, Phys. Rev. B 108, L201108 (2023).
  15. [15]C. Lu, Z. Pan, F. Yang, and C. Wu, Interlayer-coupling-driven high-temperature superconductivity in La3Ni2O7 under pressure, Phys. Rev. Lett. 132, 146002 (2024).
  16. [16]H. LaBollita, V. Pardo, M. R. Norman, and A. S. Botana, Assessing spin-density wave formation in La3Ni2O7 from electronic structure calculations, Phys. Rev. Mater. 8, L111801 (2024).
  17. [17]D. A. Shilenko and I. V. Leonov, Correlated electronic structure, orbital-selective behavior, and magnetic correlations in double-layer La3Ni2O7 under pressure, Phys. Rev. B 108, 125105 (2023).DOI
  18. [18]J. Zhou, R. Song, and H. Lu, Pressure-driven evolution of electronic and magnetic correlations in bilayer nickelate La3Ni2O7, arXiv:2608.02261 (2026).arxiv.org/abs/2608.02261
  19. [19]J. Yang, H. Sun, X. Hu, Y. Xie, T. Miao, H. Luo, H. Chen, B. Liang, W. Zhu, G. Qu, C. Q. Chen, M. Huo, Y. Huang, S. Zhang, F. Zhang, F. Yang, Z. Wang, Q. Peng, H. Mao, G. Liu, Z. Xu, T. Qian, D. X. Yao, M. Wang, L. Zhao, and X. J. Zhou, Orbital-dependent electron correlation in double-layer nickelate La3Ni2O7, Nat. Commun. 15, 4373 (2024).DOI
  20. [20]Y. Li, X. Du, Y. Cao, C. Pei, M. Zhang, W. Zhao, K. Zhai, R. Xu, Z. Liu, Z. Li, J. Zhao, G. Li, Y. Qi, H. Guo, Y. Chen, and L. Yang, Electronic correlation and pseudogap-like behavior of high-temperature superconductor La3Ni2O7, Chinese Physics Letters 41, 10.1088/0256-307X/41/8/087402 (2024).DOI
  21. [21]P. Li, G. Zhou, W. Lv, Y. Li, C. Yue, H. Huang, L. Xu, J. Shen, Y. Miao, W. Song, Z. Nie, Y. Chen, H. Wang, W. Chen, Y. Huang, Z. H. Chen, T. Qian, J. Lin, J. He, Y. J. Sun, Z. Chen, and Q. K. Xue, Angle-resolved photoemission spectroscopy of superconducting (La,Pr)3Ni2O7/SrLaO4 heterostructures (2025).
  22. [22]Z. Dong, M. Huo, J. Li, J. Li, P. Li, H. Sun, L. Gu, Y. Lu, M. Wang, Y. Wang, and Z. Chen, Visualization of oxygen vacancies and self-doped ligand holes in La3Ni2O7−δ, Nature 630, 847 (2024).DOI
  23. [23]X. Chen, J. Choi, Z. Jiang, J. Mei, K. Jiang, J. Li, S. Agrestini, M. Garcia-Fernandez, H. Sun, X. Huang, D. Shen, M. Wang, J. Hu, Y. Lu, K. J. Zhou, and D. Feng, Electronic and magnetic excitations in La3Ni2O7, Nat. Commun. 15, 9597 (2024).DOI
  24. [24]X. Ren, R. Sutarto, X. Wu, J. Zhang, H. Huang, T. Xiang, J. Hu, R. Comin, X. J. Zhou, and Z. Zhu, Resolving the electronic ground state of La3Ni2O7−δ films, Commun. Phys. 8, 10.1038/s42005-025-01971-z (2025).DOI
  25. [25]W. He, X. Guo, X. Luo, J. Thomas, J. Sears, S. F. R. TenHuisen, Z. Guan, X. Chen, D. A. Dahlbom, B. Zager, J. Pelliciari, Y.-F. Zhao, H. LaBollita, H. Zheng, M. K. Lajer, J. F. Mitchell, V. Bisogni, A. S. Botana, M. Mitrano, S. Johnston, and M. P. M. Dean, Layer architecture shapes electronic, magnetic, and lattice interactions in ruddlesden-popper nickelates (2026).arxiv.org/abs/2609.04532
  26. [26]M. Wu, E. Bencikser, M. W. Haverkort, et al., Strain and composition dependence of orbital polarization in nickel oxide superlattices, Phys. Rev. B 88, 125124 (2013).DOI
  27. [27]H. Yavaş, M. Sundermann, K. Chen, A. Amorese, A. Severing, H. Gretarsson, M. W. Haverkort, and L. H. Tjeng, Direct imaging of orbitals in quantum materials, Nat. Phys. 15, 559 (2019).
  28. [28]E. Abarca Morales, M. Sundermann, B. Leedahl, V. Sundaramurthy, G. Poelchen, U. Burkhardt, R. Cardoso, P. Puphál, A. Komarek, B. Keimer, M. Hepting, L. H. Tjeng, and B. H. Goodge, Unveiling orbital landscapes in strongly correlated bulk nickelates with s-NIXS, arXiv:2606.06144 (2026).
  29. [29]J. Huang, S. Ramakrishnan, P. Rodière, P. Toulemonde, Z. Rahmany, V. Balédent, B. Vignolle, S. Marik, P. Fertey, and P. Foury-Leylekian, Pressure-driven structural transitions without a displacive charge-density wave in La2SmNi2O7, arXiv:2607.03363 (2026).
  30. [30]See supplemental material at [url will be inserted by publisher] for details of the data reduction, the line-shape model of the La N4,5 and Ni M1 edges, the selection of the spectra, the angular-acceptance correction, and the dependence of the hole ratio on the analysis choices.
  31. [31]M. W. Haverkort, A. Tanaka, L. H. Tjeng, and G. A. Sawatzky, Nonresonant inelastic x-ray scattering involving excitonic excitations: the examples of NiO and CoO, Phys. Rev. Lett. 99, 257401 (2007).pubmed.ncbi.nlm.nih.gov/18233556
  32. [32]D. Zhao, Y. Zhou, M. Huo, Y. Wang, L. Nie, Y. Yang, J. Ying, M. Wang, T. Wu, and X. Chen, Pressure-enhanced spin-density-wave transition in double-layer nickelate La3Ni2O7−δ, Sci. Bull. 70, 1239 (2025).
  33. [33]Y. Zhang, L.-F. Lin, A. Moreo, T. A. Maier, and E. Dagotto, Trends in electronic structures and s±-wave pairing for the rare-earth series in bilayer nickelate superconductor R3Ni2O7, Phys. Rev. B 108, 165141 (2023).
  34. [34]Z. Pan, C. Lu, F. Yang, and C. Wu, Effect of rare-earth element substitution in superconducting R3Ni2O7 under pressure, Chin. Phys. Lett. 41, 087401 (2024).
  35. [35]X. Yan, S. Tong, Z. Huo, G. Li, H. Shi, B. Li, J. Shi, and D. Duan, First-principles study of chemical pressure in La2RNi2O7 (R = Pr, Nd, and Sm), Phys. Rev. B 114, 074501 (2026).

Paper details

vlnc:W_bbx4e9cj
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents