Impact of reaction temperatures on the particle size of V2O5 synthesized by facile hydrothermal technique and their auspicious photocatalytic performance in dye degradation

Abstract

In this study, a complete study of the effect of hydrothermal reaction temperatures on the synthesis and physical properties of V2O5 using the green facile mild hydrothermal method has been performed with six different temperatures 100 °C to 200 °C, in the step of 20 °C. . The XRD pattern confirm the stable orthorhombic crystal structure of the synthesized samples at all reaction temperatures. The SEM and TEM images demonstrate the particle-like morphology, and these characterizations affirmed that the particles size became larger with the increase of reaction temperatures. The FTIR analysis is employed to study the functional groups, and the obtained results are consistent with the XRD analysis. The bandgap has been estimated at various reaction temperatures using UV-vis diffuse reflectance spectra (UV-DRS) and was found to be varied 2.09 eV to 2.15 eV that are suitable range to absorb a significant amount of visible light. The photocatalysis of methylene blue (MB) with synthesized samples has been accomplished to investigate photocatalytic efficiency. The pure V2O5 synthesized at lower reaction temperature (100 °C) possess a lower bandgap and, accordingly, higher photocatalytic efficiency.

Introduction

The transition metal oxides (TMOs) is a unique materials family that scientists spent a great effort to find their fascinating applications [1, 2]. The Vanadium Oxides (VOs) have drawn significant interest as a potential candidate in the TMOs family among researchers due to low-cost facile synthesis and attractive surface morphology [3, 4]. Furthermore, various oxidation states (+2, +3, +4, and +5) of VOs expose a vast research field to the scientists[5]. Accordingly, the vanadium compounds form VO\mathrm{VO}, V2O3\mathrm{V}_{2}\mathrm{O}_{3}, VO2\mathrm{VO}_{2}, and V2O5\mathrm{V}_{2}\mathrm{O}_{5}. Among these, vanadium pentoxide (V2O5\mathrm{V}_{2}\mathrm{O}_{5}) has been studied rigorously over the last decade as it has interesting and charming physical and chemical properties [6]. However, V2O5\mathrm{V}_{2}\mathrm{O}_{5} is a promising candidate for photocatalysis [7, 8, 9], electrochemistry [10], chemical sensor [11, 12], battery materials [13, 14], etc. Recently, the pure and doped V2O5\mathrm{V}_{2}\mathrm{O}_{5} was studied extensively for photocatalytic and environmental purification processes due to its lower bandgap and attractive surface morphology [9, 15].

There are several dry and wet processes accessible for the synthesis of V2O5\mathrm{V}_{2}\mathrm{O}_{5}, for instant, sol-gel [15, 16], decomposition [17], sputtering[18], thermal evaporation method [19], and hydrothermal method [20, 21] and so on. The mild hydrothermal method is one of them that is suitable for synthesizing transition metal oxides [22] Where reaction temperatures are maintained from 100 °C to 200 °C. The numerous research articles have been published on the synthesis of vanadium compounds using the hydrothermal method (HTM). The HTM is efficient for the synthesis of V2O5\mathrm{V}_{2}\mathrm{O}_{5} to achieve improved properties of V2O5\mathrm{V}_{2}\mathrm{O}_{5} with different structure and morphology by varying different parameters during the synthesis process. For instant, Juyi Mu et al. and Young Bok Kim et al. have found that acid and solvent combinations significantly impact the morphology of V2O5\mathrm{V}_{2}\mathrm{O}_{5}; their reaction time and temperature were constant. They show that the belt, flowers, balls, wires and rods shaped morphology can be found merely by changing the combination of acid and solvent [3, 23]. Devika P. Nair et al. and M. Zeng et al. studied the effect of surfactants on the properties of V2O5\mathrm{V}_{2}\mathrm{O}_{5} using the HTM [24, 25]. The ammonium metavanadate (NH4VO3\mathrm{NH}_{4}\mathrm{VO}_{3}) is a commonly used precursor material as the source of vanadium in the HTM. Several articles are reported on the synthesis of V2O5\mathrm{V}_{2}\mathrm{O}_{5} using the NH4VO3\mathrm{NH}_{4}\mathrm{VO}_{3} with different reaction temperatures at 180°C [3, 9, 24, 25, 26, 27, 28, 29], 120°C [30], 160°C [31]. Furthermore, W. Yu et al. synthesized V2O5\mathrm{V}_{2}\mathrm{O}_{5} at both 140°C and 180°C reaction temperatures [32]. All researchers have been used the NH4VO3\mathrm{NH}_{4}\mathrm{VO}_{3} as precursor material. To the best of our knowledge, there is no systematic complete study on the surface morphology and physical properties of V2O5\mathrm{V}_{2}\mathrm{O}_{5} using NH4VO3\mathrm{NH}_{4}\mathrm{VO}_{3} by varying hydrothermal low to high reaction temperatures. We have successfully synthesized single-phase V2O5\mathrm{V}_{2}\mathrm{O}_{5} starting from reaction temperature 100°C to 200°C in the step of 20°C. We have studied the structural, morphological, optical properties of the synthesized samples. The photocatalytic properties of the synthesized samples has also been tested under visible light with methylene blue (MB).

EXPERIMENTAL DETAILS

Materials

In this works, ammonium meta-vanadate (NH4VO3\mathrm{NH}_{4}\mathrm{VO}_{3}) with purity ≥99%\ge99\% (Sigma-Aldrich) was used as precursor. Both ethanol and Nitric acid were parched from Mark, Germany. All chemical were used without further purification.

Synthesis of V2O5\mathrm{V}_{2}\mathrm{O}_{5}

In this present study, the synthesis of pure V2O5\mathrm{V}_{2}\mathrm{O}_{5} was carried out using a facile mild hydrothermal method (FMHTM) at different reaction temperatures (100∘C100^\circ\mathrm{C}-200∘C200^\circ\mathrm{C}, in the step of 20∘C20^\circ\mathrm{C}). All steps involved in the synthesis procedure are shown schematically in Figure 1. First, 2.3396 gm (1M) of ammonium metavanadate was dissolved in 1:1 DI water and ethanol solvent. This solution was continuously stirred for 1h at room temperature. Then freshly prepared 10% HNO3\mathrm{HNO}_{3} was added to the light yellow solution to maintain the pH 2.2-2.5. After that, the dark wine colour solution was transferred to a Teflon-lined stainless steel autoclave (250 ml) and heated at the desired reaction temperature in an oven for 24 hrs. We prepared six samples series with reaction temperature 100°C to 200°C in the step of 20°C. After cooling to room temperature, the obtained produced washed several times by DI water and ethanol using filtration and centrifugation. Then the green color gel was dried for 6 hrs at 100°C. Finally, powder V2_2O5_5 was found, followed by 600°C calcination in a high precision furnace for 2 hrs.

Image not extracted

Figure 1. The schematic illustration of facile mild hydrothermal process of sample preparation.

Characterization Techniques

The structural analysis was performed by the X-ray diffraction spectra (XRD) of the synthesized samples with the Rigaku Smart Lab diffractometer (Cu-Kα radiation and λ=1.5406 Å). The scanning electron microscopy (SEM) (JEOL, JSM6010LA), and the transmission electron microscopy (TEM)(TALOS F200 G2, Thermo Fisher Scientific, USA) were employed to study surface morphology and the particle size distribution. A Fourier-transfer infrared spectrophotometer (FT-IR) (Jupiter, STA449 F3) was used to analyze the vibrational modes of the synthesized samples. The bandgap was also estimated using UV-vis diffuse reflectance spectra (UV-DRS) (LAMBDA 1050, PerkinElmer-USA).

Photocatalytic Efficiency Test

The Photocatalytic efficiency test was performed in the methylene blue (MB) dye using the synthesized samples as a catalyst, and the procedure is given below:-

First, the aqueous solution of MB dye (1 x 10−510^{-5} M, 25 mL) was prepared by vigorous stirring for 30 min to get a homogeneous solution and the solvent was deionized water (DI) water. Then, 5 mg of the catalyst was added to the solution and again magnetically stirred in the dark environment for 30 min to reach the adsorption equilibrium of dye by the catalyst. The efficiency analyzing process was commenced by irradiating the solution with visible light. The degradation of MB was continued for 180 minutes, and the absorbance was taken in 20 minutes intervals. In addition, the catalyst material was separated from the testing solution by centrifugation for 10 minutes before putting the solution in the UV-vis spectrometer.

Results and Discussion

Crystal Structure Analysis

The crystalline structure of as-synthesized samples were studied using the XRD measurement. Figure 2 shows the XRD patterns of powder samples synthesized at different hydrothermal reaction temperatures. It is seen that the most substantial peaks are typical in all samples, and these are (200), (001), (101), (110), (301), (011), (310) and (002) that indicates all samples have orthorhombic crystal structure with the space group PmmnPmmn (JCPDS #09-0387)[33]. The most intense peak is (001) at 2θ2\theta value of 20.4° indicating the crystallites are preferably oriented at ⟨0 0 1⟩\langle0\ 0\ 1\rangle direction. However, there are no other additional peaks found in the XRD analysis of all samples (Figure 2). Therefore, it can be summarized from the crystal structure analysis that high purity V2O5\mathrm{V}_2\mathrm{O}_5 powder without impurities have been synthesized using FMHTM at different reaction temperatures.

Image not extracted

Figure 2. The XRD pattern of V2O5V_2O_5 synthesized by facile mild hydrothermal method (FMHTM) at different reaction temperatures (a) 100 °C, (b) 120 °C, (c) 140 °C, (d) 160 °C, (e) 180 °C, and (f) 200 °C

Morphological Analysis

The morphologies of the as-synthesized V2O5\mathrm{V}_2\mathrm{O}_5 have been analyzed at room temperature by varying reaction temperatures using a scanning electron microscope (SEM) as illustrated in Figure 3 (a-Figure 3f).

Image not extracted

Figure 3. SEM images of V2O5\mathrm{V}_2\mathrm{O}_5 measured at room temperature with different reaction temperatures (a) 100 °C, (b) 120 °C, (c) 140 °C, (d) 160 °C, (e) 180 °C, and (f) 200 °C.

It is seen from the images that all samples alike and agglomerated particles exhibited surface morphology in all reaction temperatures. It is obvious from the images that the agglomeration increases with increasing reaction temperature. This finding is consistent with basic mechanism of agglomeration, where the surface free energy reduces due to increasing particles size and decreasing surface area results the agglomeration takes place.

The transmission electron microscope (TEM) was performed for two synthesized samples (reaction temperature 100 °C and 180 °C) for further confirmation of the particle-like morphology. Figure 4 (a, d) shows the low magnification and (b, e) shows the high magnification TEM images of V2O5\mathrm{V_2O_5} samples synthesized at 100 °C and 180 °C. From the illustration, it is seen that our synthesized samples have particle-like morphology that is also found in the SEM images. Figure 4 (c and f) shows the estimated particles size distribution calculated from the TEM images for 100 °C and 180 °C reaction temperatures, respectively. From the particles size distribution, it seems that the particle size became larger with the increase of reaction temperatures and are found to be 340±7340 \pm7 nm and 457±7457 \pm7 nm for the samples synthesized at 100 °C and 180 °C, respectively. The particle size increases with increasing reaction temperature is due to reduction of surface free energy that is consistent with the finding of the SEM images as well.

Image not extracted

Figure 4. (a, d) and (b, e) high and low magnification TEM images of FMHTM mediated V2O5\mathrm{V_2O_5} at 100 °C and 180 °C reaction temperatures, respectively and inset-SAED pattern for the corresponding samples. (c) and (f) estimated particles size distribution calculated from the TEM images for reaction temperatures 100 °C and 180 °C, respectively.

The single-crystal nature of the synthesized samples have also been confirmed by the inset selected area electron diffraction (SEAED) as depicted in Figure 4 (b, Figure 4e).

Functional Group Analysis

The fourier-transform infrared (FTIR) spectroscopy has been performed at room temperature with various reaction temperatures to analyze vibrational bands as illustrated in Figure 5. All three main characteristics peak of V2_2O5_5 are observed between 400 and 1000 cm−1^{-1}. First, the peak around 420 cm−1^{-1} is for νs\nu_s (symmetric stretching) modes of V-O-V vibration. It is seen that this V-O-V vibration is shifted to a lower wavelength and this downshift occurs due to wreaking of V-O-V bond [34, 35]. There is a wide peak appeared around 818 cm−1^{-1} for asymmetric stretching modes of V-O-V (νas\nu_{\mathrm{as}}). The peak observed around 1020 cm−1\mathrm{cm}^{-1} is attributed to the vibrational bond for terminal oxygen (V = O). However, these two FTIR peaks confirmed the formation of V2O5\mathrm{V_2O_5} [36].

Image not extracted

Figure 5. The FTIR spectra of V2_2O5_5 synthesized using facile mild hydrothermal method at different reaction temperatures.

Hence, the FTIR analysis, in conjunction with the XRD analysis, affirmed the purity of V2O5\mathrm{V_2O_5}.

Optical Properties Analysis

Image not extracted

Figure 6. Absorption spectra obtained from the UV-vis diffuse reflectance for pure V2O5\mathrm{V_2O_5} synthesized by FMHTM at different reaction temperatures.

The optical characterization was accomplished for all samples using UV-vis diffuse reflectance spectra (UV-DRS). The figure 6 illustrates the absorption spectra of pure V2O5\mathrm{V_2O_5} synthesized at six different reaction temperatures starting from 100 °C to 200 °C in step of 20°C. It is observed that all samples show a similar absorption pattern that is somewhat proven the stability of FMHTM. The V2_2O5_5 samples offer strong absorption both in the UV and visible regions. This pattern is the responsible for transferring the charge from O-2p to V-3d orbitals. Rajeshwari S. et al. also found the same absorption spectra patterns for the V2_2O5_5 synthesis [9].

The Kubelka-Munk (K-M) [37] method has been used to determine the bandgap of the pristine V2_2O5_5 powder samples. The figure 7 depicts the estimated band gap of the samples from UV-vis DRS data measured at room temperature. The relation between reflectance, R and the K-M function, F(R) according to the K-M equation are represented by the following equation[38]:

F(R)=(1−R)22R………………1(1)F(R) = \frac{(1-R)^2}{2R} \ldots\ldots\ldots\ldots\ldots\ldots1 \tag*{(1)}

However, F(R) is directly proportional to the coefficient of absorption, α\alpha and using this relation EgE_g can be obtained by plotting [F(R)*hν\nu]2^2 vs hν\nu graph. Now the relation among F(R) and α\alpha is given by the equation,

F∝αF \propto\alpha
F(R)∗hν=A(hν−Eg)n…………2(2)F(R) * h\nu= A(h\nu- E_g)^n \ldots\ldots\ldots\ldots2 \tag*{(2)}

Here in the above equation, hνh\nu is the energy of photon, hh for Plank’s constant, AA is the proportionality constant and EgE_g is for the desired bandgap energy. In this equation, n, determines whether the optical band gap is direct or indirect.

Sample NameHydrothermal Reaction Temperature (°C)Calcination temperatureEgE_g (eV)
V2_2O5_5100500°C2.08
V2_2O5_5120500°C2.10
V2_2O5_5140500°C2.09
V2_2O5_5160500°C2.11
V2_2O5_5180500°C2.11
V2_2O5_5200500°C2.15

Table 1. Table I: Calculated values of EgE_g for synthesized samples

The values of nn are used ½ and 2 for direct and indirect optical band gap, respectively. Here, we used n=2n=2 for calculating the direct bandgap of all synthesized samples.

Figure 7. The [F(R)hν]2[\mathrm{F}(\mathrm{R})h\nu]^2 vs hνh\nu plot to estimate the band gap of synthesized V2O5\mathrm{V}_2\mathrm{O}_5 samples.

The estimated bandgap at room temperature of the synthesized samples are summarized in Table I. It is seen that the V2O5\mathrm{V}_2\mathrm{O}_5 synthesized at 100°C exhibits lower bandgap (2.08 eV) then gradually increased to 2.15 eV for the V2O5\mathrm{V}_2\mathrm{O}_5 synthesized at 200°C. This rising trend can be explained using familiar concept of Burstein-Moss (B-M) for the semiconductor materials where particle size rises with the increase of reaction temperature results the Fermi level moves to the conduction band hence bandgap increases [39]. However, all samples can be able to absorb a significant amount of visible light as their bandgap varies from 2.08 eV to 2.15 eV.

Photocatalytic Degradation Activity Analysis

Photocatalytic degradation activity of methylene blue (MB) dye using two V2O5V_2O_5 samples, one synthesized at low reaction temperature (100°C) and another at high reaction temperature (180°C), The photocatalysis have been performed in aquatic medium (using deionized water) irradiated by visible light (LED) for up to 180 min. Figure 8 (a) and (b) illustrate obtained time variable UV-vis absorption spectra of V2O5V_2O_5 synthesized at 100°C and 180°C, respectively. Figure 8 (c) represents the C/C0C/C_0 plot for the MB degradation for both samples where C0C_0 represent the concentration of the MB at adsorption equilibrium, and CC represents the concentration of dye remaining non-degraded after the irradiation done for a specific time. The amount of degradation efficiency is estimated using the following formula,

Degradation  (%)=(1−C/C0)×100%(3)\mathrm{Degradation}\;(\%) = (1 - C/C_0) \times100\% \tag*{(3)}

The ln⁡(C0/C)\ln(C_0/C) versus time (tt) plot for the MB dye is represented in Figure 8 (d). The rate constants are determined using the equation ln⁡(C0/C)=kt\ln(C_0/C) = kt, where kk is the degradation rate constant.

From figure 8 (c) it is seen that the photodegradation efficiencies are 40% and 25% within 180 min of irradiation for the V2O5V_2O_5 synthesized at 100°C and 180°C, respectively. So, V2O5V_2O_5 synthesized at lower reaction temperature shows higher efficiency. The rate constant (kk) calculated from the linear fitting of logarithmic plot MB dye are (2.0±0.1)×10−3 min−1(2.0 \pm0.1) \times10^{-3}\ \mathrm{min}^{-1} and (1.7±0.1)×10−3 min−1(1.7 \pm0.1) \times10^{-3}\ \mathrm{min}^{-1} for the V2O5V_2O_5 synthesized at 100°C and 180°C, respectively. This higher kk value also confirmed that the V2O5V_2O_5 synthesized at 100°C has higher efficiency. We anticipate this fact is that the smaller particle size, and accordingly, the higher surface to volume ratio and also lower bandgap of V2O5V_2O_5 synthesized at 100°C than that of V2O5V_2O_5 synthesized at 180°C are the reason behind the higher efficiency [40]. However, the photocatalytic result is not good enough. To us, this might be due to the presence of various types of defects, which acts as rapid recombination, thus reducing the generation of active species.

Image not extracted

Figure 8. The photocatalytic illustration. (a, b) time-variable absorption spectra, (c) photodegradation efficiency of V2O5V_{2}O_{5}, and (c) the ln⁡(C0/C)\ln(C_{0}/C) vs Irradiation time graph

Photodegradation mechanism of V2O5V_{2}O_{5}

In a typical photodegradation, when the electromagnetic radiation falls on a photocatalyst then the photons are absorbed, and the electrons in the valence band are excited. The excited electrons are then migrate to the conduction band and, accordingly, the electron-hole produces. It should be noted that the radiation energy should be equal to or greater than that of the bandgap of the photocatalyst. The electron-hole is then produce radicals, and these radicals are participated in the photodegradation process of the contaminants.

Image not extracted

Figure 9. Schematic illustration of the photocatalytic mechanism.

However, there are several redox reactions involved in the degradation of MB under the irradiation of light. First, when the photon of suitable energy interacted with the V2_2O5_5 then the electron-hole pair is produced (Equation (4)).

Photocatalyst V2O5+light (hν)⟶hVB++eCB−(4)\mathrm{Photocatalyst}\ \mathrm{V}_2\mathrm{O}_5+\mathrm{light}\ (h\nu)\longrightarrow h_{\mathrm{VB}}^{+}+e_{\mathrm{CB}}^{-} \tag*{(4)}
Reduction:eCB−+O2⟶∘O2− (Superoxide radical)(5)\textit{Reduction:}\quad e_{\mathrm{CB}}^{-}+\mathrm{O}_2\longrightarrow{}^\circ\mathrm{O}_2^{-}\ (\textit{Superoxide radical}) \tag*{(5)}
H2O⟶OH−+H+(6)\mathrm{H}_2\mathrm{O}\longrightarrow\mathrm{OH}^{-}+\mathrm{H}^{+} \tag*{(6)}
Oxidation:hVB++OH+⟶∘OH (Hydroxyl radical)(7)\textit{Oxidation:}\quad h_{\mathrm{VB}}^{+}+\mathrm{OH}^{+}\longrightarrow{}^\circ\mathrm{OH}\ (\textit{Hydroxyl radical}) \tag*{(7)}
Degredation: Dye(MB)+∘OH or ∘O2−⟶CO2+H2O(8)\textit{Degredation: Dye}(MB)+{}^\circ\mathrm{OH}\ \mathrm{or}\ {}^\circ\mathrm{O}_2^{-}\longrightarrow\mathrm{CO}_2+\mathrm{H}_2\mathrm{O} \tag*{(8)}

Then, the electrons, eCB−e_{CB}^{-} from conduction band interacts with the O2_2 to produce superoxide radicals, ∘O2−^{\circ}\mathrm{O}_{2}^{-} (Equation 5, Reduction). The holes, hVB+h_{VB}^{+} from the valence band interacts with OH−OH^{-} of the water to form hydroxyl radicals, OH+OH^{+} (Equation 7, Oxidation,). Finally, both superoxide and hydroxyl radicals (∘O2−^{\circ}\mathrm{O}_{2}^{-} and OH+OH^{+}) participate in the degradation of dye, MB (Equation 8).

Conclusion

We have successfully synthesized V2O5\mathrm{V}_{2}\mathrm{O}_{5} from ammonium metavanadate at six different reaction temperatures (100°C to 200°C, in the step of 20°C) using an environment-friendly facile mild hydrothermal method. The stable orthorhombic structure of V2O5\mathrm{V}_{2}\mathrm{O}_{5} was confirmed by the XRD analysis. The SEM and TEM study shows that all samples hold particle-like morphology, and reveal that the particle size increases with the increase of reaction temperatures. Furthermore, the SEAED images affirmed the single-crystal nature of the synthesized samples. The FTIR study further confirmed the formation of single phase V2O5\mathrm{V}_{2}\mathrm{O}_{5}. The optical bandgap increases with the rise in reaction temperatures and, accordingly, exhibits the lower photocatalytic efficiency. The degradation efficiency is found to be 25% for 180°C reaction temperature whereas 40% for 100°C. However, the degradation efficiency is not judicious though the bandgap is suitable for higher photocatalytic efficiency. The lower photocatalytic efficiency can be explained due to the presence of various defects that acts as center of rapid recombination results diminishes the generation of active species accordingly declines the photocatalytic efficiency. It is noteworthy that tuning the calcination temperature can further reduces particles size and expect to increase the surface to volume ratio and hence efficiency.

Acknowledgements:

The authors are grateful to the Directorate of Research and Extension (DRE), Chittagong University of Engineering and Technology (CUET), Chattogram-4349, Bangladesh and University of Grant Commission (UGC) for arranging financial assistance under grant numbers CUET DRE (CUET/DRE/2018-19/PHY/008) and ------------------ for arranging the financial support for this work. We are also thankful for the laboratory support of the Materials Science Division, Atomic Energy Centre, Dhaka 1000, Bangladesh for the experimental support.

References

  1. [1]1 T. Dietl, A ten-year perspective on dilute magnetic semiconductors and oxides, Nat. Mater., 2010, 9, 965–974.DOI
  2. [2]2 J. Meyer, S. Hamwi, M. Kröger, W. Kowalsky, T. Riedl and A. Kahn, Transition metal oxides for organic electronics: Energetics, device physics and applications, Adv. Mater., 2012, 24, 5408–5427.DOI
  3. [3]3 J. Mu, J. Wang, J. Hao, P. Cao, S. Zhao, W. Zeng, B. Miao and S. Xu, Hydrothermal synthesis and electrochemical properties of V2O5nanomaterials with different dimensions, Ceram. Int., , DOI:10.1016/j.ceramint.2015.06.091.DOI
  4. [4]Chirayil, T., Zavalij, P. Y., & Whittingham, M. S. (1998). Hydrothermal Synthesis of Vanadium Oxides Hydrothermal Synthesis of Vanadium Oxides. Chem. Mater., 10, 2629–2640.
  5. [5]5 G. Silversmit, D. Depla, H. Poelman, G. B. Marin and R. De Gryse, Determination of the V2p XPS binding energies for different vanadium oxidation states (V5+ to V0+), J. Electron Spectros. Relat. Phenomena, 2004, 135, 167–175.DOI
  6. [6]Gu, G., Schmid, M., Chiu, P. W., Minett, A., Fraysse, J., Kim, G. T., Roth, S., Kozlov, M., Muñoz, E., & Baughman, R. H. (2003). $V_{2}O_{5}$ nanofibre sheet actuators. Nat. Mater., 2, 316–319.
  7. [7]7 M. Shanmugam, A. Alsalme, A. Alghamdi and R. Jayavel, Enhanced photocatalytic performance of the graphene- V2O5 nanocomposite in the degradation of methylene blue dye under direct sunlight, ACS Appl. Mater. Interfaces, 2015, 7, 14905–14911.DOI
  8. [8]8 B. Li, Y. Xu, G. Rong, M. Jing and Y. Xie, Vanadium pentoxide nanobelts and nanorolls: From controllable synthesis to investigation of their electrochemical properties and photocatalytic activities, Nanotechnology, 2006, 17, 2560–2566.DOI
  9. [9]Rajeshwari, P. T. S., Kumar, J. S., Rajendrakumar, R. T., & Ponpandian, N. (2010). Influence of Sn ion doping on the photocatalytic performance of $V_{2}O_{5}$ nanorods prepared by hydrothermal method (pp. 1–25).
  10. [10]10 A. Talledo and C. G. Granqvist, Electrochromic vanadium-pentoxide-based films: Structural, electrochemical, and optical properties, J. Appl. Phys., 1995, 77, 4655–4666.DOI
  11. [11]11 O. Schilling and K. Colbow, A mechanism for sensing reducing gases with vanadium pentoxide films, Sensors Actuators B. Chem., 1994, 21, 151–157.DOI
  12. [12]12 A. V. Grigorieva, S. M. Badalyan, E. A. Goodilin, M. N. Rumyantseva, A. M. Gaskov, A. Birkner and Y. D. Tretyakov, Synthesis, structure, and sensor properties of vanadium pentoxide nanorods, Eur. J. Inorg. Chem., 2010, 4, 5247–5253.DOI
  13. [13]13 J. Yao, Y. Li, R. C. Massé, E. Uchaker and G. Cao, Revitalized interest in vanadium pentoxide as cathode material for lithium-ion batteries and beyond, Energy Storage Mater., 2018, 11, 205–259.DOI
  14. [14]Yue, Y., & Liang, H. (2017). Micro- and Nano-Structured Vanadium Pentoxide ($V_2O_5$) for Electrodes of Lithium-Ion Batteries. Adv. Energy Mater., 7, 1–32.
  15. [15]15 M. P. Subramaniam, G. Arunachalam and R. Kandasamy, Studies on the structural, morphological and optical properties of HCl assisted vanadium oxide/tin oxide nanocomposites prepared by sol-gel method, Appl. Surf. Sci., 2018, 449, 610–616.DOI
  16. [16]16 M. Al Zoubi, H. K. Farag and F. Endres, Sol-gel synthesis of vanadium pentoxide nanoparticles in air- and water-stable ionic liquids, J. Mater. Sci., 2009, 44, 1363–1373.DOI
  17. [17]17 D. H. Shin, C. U. Bang, Y. C. Hong and H. S. Uhm, Preparation of vanadium pentoxide powders by microwave plasma-torch at atmospheric pressure, Mater. Chem. Phys., 2006, 99, 269–275.DOI
  18. [18]Wruck, D., Ramamurthi, S., & Rubin, M. (1989). Sputtered electrochromic $V_2O_5$ films. Thin Solid Films, 182, 79–86.
  19. [19]19 K. Y. Pan and D. H. Wei, Optoelectronic and electrochemical properties of vanadium Pentoxide Nanowires synthesized by vapor-solid process, Nanomaterials, , DOI:10.3390/nano6080140.DOI
  20. [20]Demishev, S. V., Chernobrovkin, A. L., Glushkov, V. V., Grigorieva, A. V., Goodilin, E. A., Ohta, H., Okubo, S., Fujisawa, M., Sakurai, T., Sluchanko, N. E., Samarin, N. A., & Semeno, A. V. (2011). Magnetic properties of vanadium oxide nanotubes and nanolayers. Phys. Rev. B, 84, 94426.
  21. [21]Liang, X., Gao, G., Du, Y., Wang, J., Sun, W., Liu, Y., Zhang, K., & Wu, G. (2018). Synthesis and characterization of various $V_2O_5$ microsphere structures and their electrochemical. J. Alloys Compd., 757, 177–187.
  22. [22]Whittingham, M. S. (1996). Hydrothermal synthesis of transition metal oxides under mild conditions. Curr. Opin. Solid State Mater. Sci., 1, 227–232.
  23. [23]23 Y. B. Kim and M. W. Shin, Synthesis of diverse structured vanadium pentoxides particles by the simplified hydrothermal method, Mater. Lett., 2014, 132, 247–250.DOI
  24. [24]24 M. Zeng, H. Yin and K. Yu, Synthesis of V₂O₅ nanostructures with various morphologies and their electrochemical and field-emission properties, Chem. Eng. J., 2012, 188, 64–70.DOI
  25. [25]Nair, D. P., Sakthivel, T., Nivea, R., Eshow, J. S., & Gunasekaran, V. (2015). Effect of surfactants on electrochemical properties of vanadium-pentoxide nanoparticles synthesized via hydrothermal method. J. Nanosci. Nanotechnol., 15, 4392–4397.
  26. [26]Raj, A. T., Ramanujan, K., Thangavel, S., Gopalakrishan, S., Raghavan, N., & Venugopal, G. (2015). Facile Synthesis of Vanadium-Pentoxide Nanoparticles and Study on Their Electrochemical, Photocatalytic Properties. J. Nanosci. Nanotechnol., 15, 3802–3808.
  27. [27]27 J. Chu, Z. Kong, D. Lu, W. Zhang, X. Wang, Y. Yu, S. Li, X. Wang, S. Xiong and J. Ma, Hydrothermal synthesis of vanadium oxide nanorods and their electrochromic performance, Mater. Lett., 2016, 166, 179–182.DOI
  28. [28]28 J. Liu, X. Wang, Q. Peng and Y. Li, Vanadium pentoxide nanobelts: Highly selective and stable ethanol sensor materials, Adv. Mater., 2005, 17, 764–767.DOI
  29. [29]29 A. Dhayal Raj, P. Suresh Kumar, Q. Yang, D. Mangalaraj, N. Ponpandian and A. Albert Irudayaraj, Compositional, microstructural, and vibrational characteristics of synthesized V₂O₅ microspheres with nanorod formation, J. Phys. Chem. Solids, 2013, 74, 897–901.DOI
  30. [30]Kumar, J. S., & Thangadurai, P. (n.d.). Hydrothermal synthesis of vanadium pentoxide nanowires. AIP Conf. Proc.. https://doi.org/10.1063/1.4947794
  31. [31]31 F. Zhou, X. Zhao, C. Yuan, L. Li and H. Xu, Low-temperature Hydrothermal Synthesis of Orthorhombic Vanadium Pentoxide Nanowires, 2007, 36, 310–311.DOI
  32. [32]32 W. Yu, J. Wang, Z. Gou, W. Zeng, W. Guo and L. Lin, Hydrothermal synthesis of vanadium pentoxide nanostructures and their morphology control, Ceram. Int., 2013, 39, 2639–2643.DOI
  33. [33]Schneider, K., Lubecka, M., & Czapla, A. (2016). $V_2O_5$ thin films for gas sensor applications. Sensors Actuators, B Chem., 236, 970–977.
  34. [34]34 S. Mukhtar, M. Liu, J. Han and W. Gao, Removal of rhodamine B from aqueous solutions using vanadium pentoxide/titanium butyl oxide hybrid xerogels, *Chinese Phys. B*, , DOI:10.1088/1674-1056/26/5/058202.DOI
  35. [35]Reddy, C. V. S., Jin, W., & Zhu, Q.-Y. (2006). Polymer intercalated $V_2O_5$ nanostructured cathodes for secondary batteries. Eur. Phys. JournalApplied Phys., 184, 177–184.
  36. [36]Shafeeq, K. M., Athira, V. P., Kishor, C. H. R., & Aneesh, P. M. (2020). Structural and optical properties of $V_2O_5$ nanostructures grown by thermal decomposition technique. Appl. Phys. A Mater. Sci. Process., 126, 3–8.
  37. [37]Kubelka, P., & Munk, F. (n.d.). An Article on Optics of Paint Layers. Z.Tech. Phys.. https://doi.org/10.1097/SLA.0000000000001706
  38. [38]38 P. Makuła, M. Pacia and W. Macyk, How To Correctly Determine the Band Gap Energy of Modified Semiconductor Photocatalysts Based on UV-Vis Spectra, *J. Phys. Chem. Lett.*, 2018, **9**, 6814–6817.DOI
  39. [39]39 Q. Wang, M. Brier, S. Joshi, A. Puntambekar and V. Chakrapani, Defect-induced Burstein-Moss shift in reduced $V_2O_5$ nanostructures, *Phys. Rev. B*, 2016, **94**, 1–12.DOI
  40. [40]Basith, M. A., Ahsan, R., Zarin, I., & Jalil, M. A. (2018). Enhanced photocatalytic dye degradation and hydrogen production ability of Bi$_{25}$FeO$_{40}$-rGO nanocomposite and mechanism insight. Sci. Rep., 8, 33–35.

Paper details

vlnc:W_bg4gdem3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 4

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents