Abstract

We use hybrid density functional calculations to assess n-type doping in monoclinic (Alx_xGa1−x_{1-x})2_2O3_3 alloys. We focus on Si, the most promising donor dopant, and study the structural properties, formation energies and charge-state transition levels of its various configurations. We also explore the impact of C and H, which are common impurities in metal-organic chemical vapor deposition (MOCVD). In Ga2_2O3_3, SiGa_{Ga} is an effective shallow donor, but in Al2O3_2O_3 SiAl_{Al} acts as a DX center with a (+/-) transition level in the band gap. Interstitial H acts as a shallow donor in Ga2_2O3_3, but behaves as a compensating acceptor in n-type Al2O3_2O_3. Interpolation indicates that Si is an effective donor in (Alx_xGa1−x_{1-x})2_2O3_3 up to 70% Al, but it can be compensated by H already at 1% Al. We also assess the diffusivity of H and study complex formation. Sication_{cation}-H complexes have relatively low binding energies. Substitutional C on a cation site acts as a shallow donor in Ga2_2O3_3, but can be stable in a negative charge state in (Alx_xGa1−x_{1-x})2_2O3_3 when x>5%. Substitutional C on an O site (CO_O) always acts as an acceptor in n-type (Alx_xGa1−x_{1-x})2_2O3_3, but will incorporate only under relatively O-poor conditions. CO_O-H complexes can actually incorporate more easily, explaining observations of C-related compensation in Ga2_2O3_3 grown by MOCVD. We also investigate Ccation_{cation}-H complexes, finding they have high binding energies and act as compensating acceptors when x>56%; otherwise the H just passivates the unintentional C donors. C-H complex formation explains why MOCVD grown Ga2_2O3_3 can exhibit record-low free-carrier concentrations, in spite of the unavoidable incorporation of C. Our study highlights that, while Si is a suitable shallow donor in ALGO alloys, control of unintentional impurities is essential to avoid compensation.

Introduction

Monoclinic Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} (β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}) is a wide-band-gap material (4.76–5.1 eV [1, 2, 3, 4]) with a high breakdown field (6-8 MV/cm) [5]. Despite its wide band gap, Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} can be controllably nn-type doped; together with the availability of high-quality yet low-cost substrates these properties render β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} highly promising for applications in high-power electronics and UV optoelectronics [6, 7, 8].

Effective control of the carrier concentration by doping with shallow donors is essential for device applications. This typically requires that the donor impurity has a low ionization energy and that compensation can be avoided. Si, Ge and Sn have been demonstrated to be effective shallow donors in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} with modest ionization energies (≤80\leq80 meV) [9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21]. In addition to these dopants, first-principles calculations have identified interstitial hydrogen (Hi\mathrm{H}_{i}) and carbon on a Ga site (CGa\mathrm{C}_{\mathrm{Ga}}) as shallow donors [20, 22]. Compensation of the shallow donors can occur due to native defects [23, 24] or impurities that act as acceptors, or due to self-compensation if the dopant can occur in different configurations. One form of self-compensation involves the formation of substitutional species on either cation or anion sites. For example, carbon in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} can occur either on the Ga site (CGa\mathrm{C}_{\mathrm{Ga}}), acting as a donor, or on the O site (CO\mathrm{C}_{\mathrm{O}}), acting as an acceptor [22]. Self-compensation can also occur by formation of so-called DXDX centers, in which an impurity expected to act as a shallow donor exhibits a large lattice relaxation and becomes negatively charged by trapping electrons, thus effectively acting as a deep acceptor. In Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}, Si, Ge, and Sn do not form DXDX centers [16, 20, 25]. However, the likelihood of formation of a DXDX center increases as the band gap increases, as is well known for AlGaAs [26] and AlGaN alloys [27].

Alloying with Al raises the band gap of Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} [28, 29]. Heterojunctions of (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} and Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} exhibit a high-density two-dimensional electron gas, which is at the core of field-effect transistors [30]. Modulation doping is required for high mobility, raising the issue of whether nn-type doping of (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} can be achieved. Addressing this issue requires investigating whether dopants that are effective for Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} remain shallow donors in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3}, and whether compensation will occur. In addition, recent experiments on (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} films grown by metal-organic chemical vapor deposition (MOCVD) indicated that control of doping might be challenging; it was found [31] that doping with Si failed to result in nn-type doping below a threshold Si concentration. Above the threshold, an abrupt enhancement of the carrier concentration was observed. Identifying the origin of the compensation in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} alloys is therefore important for further improvements in electronic devices.

Varley et al. [21] recently reported a first-principles study of DXDX-center formation for a large number of candidate donor impurities in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3}. They found that Si emerged as the best candidate, since it continues to act as a shallow donor up to high Al concentrations in the alloy. In the present work we therefore focus on Si as the donor; we perform a more detailed study of its behavior as a DXDX center, and investigate other sources of compensation and potential complex formation.

Our study, based on hybrid density functional theory (DFT), addresses Si impurities in monoclinic Al2_2O3_3 (hereafter denoted as θ\theta-Al2_2O3_3), and reveals a new configuration of the DXDX state. Compensation by native point defects has been previously addressed [23, 24]. Here, we perform an in-depth study of compensation due to other impurities, particularly carbon and hydrogen. Both of these impurities are readily incorporated during MOCVD growth. Carbon on a cation site [22] and hydrogen [20] are both shallow donors in Ga2_2O3_3, but possess (0/−) or (+/−) charge-state transition levels in the band gap in Al2_2O3_3. By interpolating between the end compounds, Ga2_2O3_3 and Al2_2O3_3, we can estimate the position of these defect levels in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, and determine the Al composition at which the onset of compensation occurs. [Note that we use the term “defect” to denote both native point defects and impurities.] Our results show that Si is an effective donor in (Alx_xGa1−x_{1-x})2_2O3_3 up to 70% Al, but it can be compensated by hydrogen already at 1% Al, or by carbon on cation sites at 5% Al.

Given that hydrogen is expected to be quite mobile, we also perform a study of its migration properties. We further assess the possibility of forming hydrogen-related defect complex with Si and C. Sication_\mathrm{cation}–H complex formation is not a major concern, since the complexes have low binding energies. Binding energies are much higher for C–H complexes; in fact, C–H behaves almost as a fixed entity, with properties very similar to a nitrogen impurity. Ccation_\mathrm{cation}–H complexes can act as compensating acceptors in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, but only when the Al content exceeds 56%; otherwise the complexes are mainly neutral and hydrogen passivates the unintentionally carbon donors. This may explain why MOCVD-grown Ga2_2O3_3 can exhibit record-low free-carrier concentrations [32], in spite of the probably unavoidable incorporation of carbon.

Substitutional carbon on an oxygen site (CO_\mathrm{O}), finally, always acts as an acceptor in nn-type (Alx_xGa1−x_{1-x})2_2O3_3, irrespective of Al concentration. CO_\mathrm{O} will incorporate only under relatively cation-rich (oxygen-poor) conditions; we find that CO_\mathrm{O}–H complexes can actually incorporate more easily, explaining experimental observations of carbon-related compensation in Ga2_2O3_3 grown by MOCVD [33, 34].

The paper is organized as follows. In Sec. II, the calculation details, the definition of defect formation energies, and the physics of DXDX centers are introduced. The main results for Si, C, and H and consequences for carrier compensation are presented in Secs. III A, III B, and III C, respectively; complexes are discussed in Sec. III D. Section IV concludes the paper.

Methodology

Computational details

We perform DFT calculations using the projector augmented wave method (PAW) [35] implemented in the Vienna AbAb-initio Simulation Package (VASP) [36, 37]. We focus on the monoclinic phase of Ga2_2O3_3 (denoted β\beta-Ga2_2O3_3) and Al2_2O3_3 (θ\theta-Al2_2O3_3). The structure, illustrated in Figure 1(a), contains two types of cation sites: the tetrahedral site (denoted as I) and the octahedral site (denoted as II). In addition, there are three types of O atoms: three-fold coordinated O(I) (on a shared corner of two edge-sharing AlO6_6 octahedra and one AlO4_4 tetrahedron), three-fold coordinated O(II) (on the shared corner of one AlO6_6 octahedron and two AlO4_4 tetrahedra), and four-fold coordinated O(III).

Crystal structures of monoclinic Al2O3 and a Si-containing supercell

Figure 1. (a) Conventional cell of monoclinic Al2_2O3_3. Two inequivalent Al sites are labeled: tetrahedrally coordinated Al(I) in aqua and octahedrally coordinated Al(II) in purple. For the O sites, threefold-coordinated O(I) are in red, threefold coordinated O(II) in purple, and fourfold-coordinated O(III) in gray. (b) Supercell constructed by creating a 1×3×21 \times3 \times2 multiple of the conventional monoclinic cell of θ\theta-Al2_2O3_3, with one tetrahedrally-coordinated Al replaced by Si. Light blue, red and dark blue spheres denote Al, O and Si atoms, respectively. Structural visualization was performed using VESTA [38].

A plane-wave energy cutoff of 400 eV was employed and Brillouin-zone integration was carried out using the Γ\Gamma-centered 4×4×44 \times4 \times4 k-point mesh for the primitive cell and 2×2×22 \times2 \times2 for the supercell. The PAW potentials correspond to the valence-electron configurations 4s24p14s^{2}4p^{1} for Ga, 3s23p13s^{2}3p^{1} for Al, and 2s22p42s^{2}2p^{4} for O. To correctly describe the electronic structure as well as charge localization we use a hybrid functional, specifically the functional of Heyd, Scuseria, and Ernzerhof (HSE) [39], with a mixing parameter of α=0.32\alpha=0.32. This produces a band gap of 4.83 eV for β\beta-Ga2_2O3_3 and 7.41 eV for θ\theta-Al2_2O3_3, in good agreement with the experimental band gaps of 4.80 for β\beta-Ga2_2O3_3 and 7.40 eV [40] for θ\theta-Al2_2O3_3. An ordered AlGaO3_3 alloy is also investigated, with all Al atoms on octahedral sites and all Ga atoms on tetrahedral sites [28]. The use of an ordered structure serves as an approximation; the

aRef. 41; bRef. 42; cRef. 2; dRef. 3; eRef. 43; fRef. 40.

computation of structures representative of disordered alloys would be computationally prohibitive. We note that for the 50% Al content, ordered AlGaO3_3 was found to be a line compound due to the preference for Al to occupy octahedral sites [28]. Spin polarization is included and full structural optimizations were performed. The optimized computed structural parameters of β\beta-Ga2_2O3_3, AlGaO3_3 and θ\theta-Al2_2O3_3 are summarized in Table I; they compare favorably with experiment.

Ga2_2O3_3AlGaO3_3Al2_2O3_3
CalcExptCalcExptCalcExpt
aa12.1412.21a11.8612.00a11.6611.85e
bb3.023.04a2.942.98a2.882.90e
cc5.785.81a5.695.73a5.575.62e
β\beta103.77103.87a104.25104.03a104.04103.83e
ΔHf\Delta H_f−10.22−11.29b−13.87−16.11
EgapindirE_{\mathrm{gap}}^{\mathrm{indir}}4.835.817.417.40f
EgapdirE_{\mathrm{gap}}^{\mathrm{dir}}4.874.76c, 4.88d5.897.74

Table I. Structural parameters (lattice parameters, Å; angle β\beta, degrees), formation enthalpy per formula unit (ΔHf\Delta H_f, eV/f.u.), and band gaps (EgapE_{\mathrm{gap}}, eV) for monoclinic Ga2_2O3_3, AlGaO3_3 and Al2_2O3_3. Experimental results are also listed for comparison.

A 120-atom supercell was constructed for the point-defect calculations, as shown in Figure 1(b). Selected tests were performed using 160-atom supercells. Tests for larger supercells are too expensive to perform with the hybrid functional, but supercell size convergence was further checked using the generalized gradient approximation of Perdew, Burke, and Ernzerhof (PBE) [44] for Si and C impurities in supercells containing up to 1280 atoms. Transition levels were found to change by less than 0.1 eV. For each point defect, we perform multiple calculations with different symmetry-breaking initial local distortions around the defect in the initial state, and optimize the atomic positions until the Hellmann-Feynman forces are lower than 5 meV/Å. All the supercell calculations are consistently performed at the lattice parameters obtained with the same plane-wave energy cutoff, as listed in Table I.

Migration barriers are calculated using the climbing-image nudged elastic band (cNEB) method [45]. To mitigate computational cost we perform one-shot HSE calculations for the migration barriers (EbE_b): we use PBE [44] in the cNEB calculations, followed by static HSE total energy calculations based on the initial and barrier geometries. We tested the accuracy of this approach for the migration of H+^+ in Al2_2O3_3 and Ga2_2O3_3 along the [10] direction; full HSE calculations yield migration barriers that are within 0.1 eV of the results obtained using one-shot HSE calculations.

After determining the migration barrier of a defect, we can estimate the temperature at which the defect becomes mobile with transition state theory [46]. This temperature is denoted as an “annealing temperature”, above which the defect is in thermodynamical equilibrium. In transition state theory [46], the rate Γ\Gamma at which the defect hops to a neighboring site can be expressed as

Γ=Γ0exp⁡(−EbkBT),(1)\Gamma= \Gamma_0 \exp\left(-\frac{E_b}{k_{\mathrm{B}}T}\right), \tag*{(1)}

where kBk_{\mathrm{B}} is the Boltzmann constant and EbE_b the migration barrier. The prefactor Γ0\Gamma_0 is an effective frequency associated with the vibration of the defect; for the H interstitial in both Ga2_2O3_3 and Al2_2O3_3, we choose Γ0=1014 s−1\Gamma_0 = 10^{14}\ \mathrm{s}^{-1}, which is approximately the dominant O-H vibrational frequency Ga2_2O3_3 [23, 47]. We estimate the annealing temperature as the temperature at which the rate Γ=1 s−1\Gamma= 1\ \mathrm{s}^{-1} [48]. We note that the annealing temperature is not very sensitive to the choice of Γ0\Gamma_0.

Formation energy

The formation energy of a defect is used to assess the likelihood of the presence of the defect and its concentration. For Si substituting on an Al site (SiAl_{\mathrm{Al}}), the formation energy is calculated as

Ef(SiAlq)=Etot(SiAlq)−Etot(Al2O3)−(μSi+μSi0)+(μAl+μAl0)+q(EF+EVBM)+Δq,(2)E^f(\mathrm{Si}_{\mathrm{Al}}^q) = E_{\mathrm{tot}}(\mathrm{Si}_{\mathrm{Al}}^q) - E_{\mathrm{tot}}(\mathrm{Al}_2\mathrm{O}_3) - (\mu_{\mathrm{Si}} + \mu_{\mathrm{Si}}^0) + (\mu_{\mathrm{Al}} + \mu_{\mathrm{Al}}^0) + q(E_{\mathrm{F}} + E_{\mathrm{VBM}}) + \Delta^q, \tag*{(2)}

where Etot(SiAlq)E_{\mathrm{tot}}(\mathrm{Si}_{\mathrm{Al}}^q) is the total energy of one SiAl_{\mathrm{Al}} in charge state qq in the supercell, Etot(Al2O3)E_{\mathrm{tot}}(\mathrm{Al}_2\mathrm{O}_3) is the total energy of the bulk supercell, and EFE_{\mathrm{F}} is the Fermi energy, referenced to the valence-band maximum (VBM). Δq\Delta^q is a finite-size correction term for charged defects [49, 50]. We adopt the previously reported values for the dielectric constants of Ga2_2O3_3, AlGaO3_3, and Al2_2O3_3 [21]. The chemical potentials are referenced to the elemental phases, e.g., μSi=Etot(Si)\mu_{\mathrm{Si}} = E_{\mathrm{tot}}(\mathrm{Si}) and μAl0=Etot(Al)\mu_{\mathrm{Al}}^0 = E_{\mathrm{tot}}(\mathrm{Al}).

The Al and O chemical potentials have to fulfill the stability condition for bulk Al2_2O3_3:

2μAl+3μO=ΔHf(Al2O3),(3)2\mu_{\mathrm{Al}} + 3\mu_{\mathrm{O}} = \Delta H_f(\mathrm{Al}_2\mathrm{O}_3), \tag*{(3)}

where ΔHf(Al2O3)\Delta H_f(\mathrm{Al}_2\mathrm{O}_3) is the formation enthalpy of bulk θ\theta-Al2_2O3_3, as shown in Table I. The calculated formation enthalpies of β\beta-Ga2_2O3_3 and AlGaO3_3 are listed in Table I as well. μAl=0\mu_{\mathrm{Al}} = 0 corresponds to Al-rich conditions, and μO=0\mu_{\mathrm{O}} = 0 to O-rich (Al-poor) conditions. For purposes of presenting results for the impurities, we choose the chemical potentials to correspond to the solubility limit, i.e., the highest value of the chemical potential that is compatible with formation of other phases that can result from interactions of the impurity with the host elements. For μSi\mu_{\mathrm{Si}}, this correspond to equilibrium with SiO2_2:

μSi+2μO=ΔHf(SiO2),(4)\mu_{\mathrm{Si}} + 2\mu_{\mathrm{O}} = \Delta H_f(\mathrm{SiO}_2), \tag*{(4)}

where ΔHf(SiO2)\Delta H_f(\mathrm{SiO}_2) is the calculated formation enthalpy of SiO2_2. For C and H, the upper limits depend on the host chemical potentials: the limits for μC\mu_{\mathrm{C}} correspond to Al4CO4\mathrm{Al}_4\mathrm{CO}_4 for Al-rich and CO2\mathrm{CO}_2 for Al-poor conditions; the limits for μH\mu_{\mathrm{H}} correspond to H2\mathrm{H}_2 for Al-rich and H2O\mathrm{H}_2\mathrm{O} for Al-poor.

To be able to comment on the behavior in (AlxGa1−x)2O3(\mathrm{Al}_x\mathrm{Ga}_{1-x})_2\mathrm{O}_3 alloys, we also calculate formation energies in Ga2O3\mathrm{Ga}_2\mathrm{O}_3. The limiting phases for Si and H are the same as those in the Al2O3\mathrm{Al}_2\mathrm{O}_3 case. The limits for μC\mu_{\mathrm{C}} in Ga2O3\mathrm{Ga}_2\mathrm{O}_3 correspond to graphite for Ga-rich and CO2\mathrm{CO}_2 for Ga-poor conditions. We note that this is different from Ref. 22, where diamond was assumed as the limiting phase under Ga-poor conditions.

The charge-state transition level between charge states qq and q′q', denoted as (q/q′)(q/q'), is calculated based on the formation energies:

(q/q′)=Ef(SiAlq;EF=0)−Ef(SiAlq′;EF=0)q′−q.(5)(q/q') = \frac{E^{f}(\mathrm{Si}_{\mathrm{Al}}^{q};E_{\mathrm{F}}=0)-E^{f}(\mathrm{Si}_{\mathrm{Al}}^{q'};E_{\mathrm{F}}=0)}{q'-q}. \tag*{(5)}

Stability of DX centers

Following Chadi and Chang [26], we label the neutral and positively charged donors on the substitutional site d0d^0 and d+d^+, respectively. DX−DX^- is used to denote the configuration in the negative charge state. The formation of a DXDX center leads to self-compensation, as described by the process

2d0⟶d++DX−.(6)2d^0 \longrightarrow d^+ + DX^-. \tag*{(6)}

The DXDX center can be characterized by the effective correlation parameter UU, defined by

U=Ef(d+)+Ef(DX−)−2Ef(d0).(7)U=E^{f}(d^+)+E^{f}(DX^-)-2E^{f}(d^0). \tag*{(7)}

Stability of the DXDX center is typically characterized by a negative value of UU. However, using UU as the descriptor of the DXDX center can be problematic because of the challenges involved in accurately calculating the energy of the neutral charge state when the (+/0)(+/0) level (and hence the Kohn-Sham state for d0d^0) is near or above the conduction-band minimum (CBM). Instead, we will use the (+/−)(+/-) charge-state transition level as a descriptor: our criterion will be that the DXDX center is stable if the (+/−)(+/-) level lies below the CBM.

Results and discussion

Silicon

The formation energies of Si on the tetrahedral (SiAl(I)\mathrm{Si}_{\mathrm{Al(I)}}) and octahedral (SiAl(II)\mathrm{Si}_{\mathrm{Al(II)}}) sites in θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3 are shown in Figure 2(c,Figure 2d) for cation-rich and cation-poor conditions. For completeness and consistency, we also show the formation energies of Si in Ga2O3\mathrm{Ga}_2\mathrm{O}_3 in Figure 2(a,Figure 2b); these have been calculated previously [20] and our results are consistent with the previous results. Note that in Figure 2 (and all subsequent formation-energy figures) we keep

Figure 2. Formation energy versus Fermi level for Si and C impurities in (a)-(b) β\beta-Ga2_2O3_3 and (c)-(d) θ\theta-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. The grey area indicates the conduction band of β\beta-Ga2_2O3_3.

the horizontal-axis scale the same for β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3, which facilitates comparisons of formation energies. In principle, we could also take the valence-band alignment between β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3 into account to more accurately compare charge-state transition levels [51, 52]; however, since the valence-band offset is relatively small [28], we do not include this alignment.

Similar to β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3, Si prefers to be incorporated on the tetrahedral site in θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3: Ef(SiAl(I)+)E^{f}(\mathrm{Si}_{\mathrm{Al(I)}}^+) is lower than Ef(SiAl(II)+)E^{f}(\mathrm{Si}_{\mathrm{Al(II)}}^+) by 0.80 eV. In β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 Si behaves as a shallow donor on either site, i.e., only the positive charge state is stable for all Fermi-level positions within the band gap. In θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3 a (+/−)(+/-) charge-state transition level occurs in the band gap, at 0.62 eV below the CBM for SiAl(I)\mathrm{Si}_{\mathrm{Al(I)}} and at 0.43 eV below the CBM for SiAl(II)\mathrm{Si}_{\mathrm{Al(II)}} (see Table II). Table II also lists values for the other transition levels. For SiAl(I)\mathrm{Si}_{\mathrm{Al(I)}}, there is a small region of stability for the neutral charge state; we found (+/0)(+/0) and (0/−)(0/-) transition levels at 6.77 eV and 6.81 eV, respectively, corresponding to U=0.04U=0.04 eV. For SiAl(II)\mathrm{Si}_{\mathrm{Al(II)}}, the (+/0)(+/0) level lies above the (0/−)(0/-) level and we have a negative-UU center (i.e., the neutral charge state is never thermodynamically stable), with U=−0.44U=-0.44 eV.

For Fermi levels in the upper part of the gap, SiAl−\mathrm{Si}_{\mathrm{Al}}^{-} is in a negative charge state, associated with the formation of a DXDX center. For SiAl(I)_{\mathrm{Al(I)}} we found that two locally stable DXDX configurations exist. The local geometry and the charge density of the localized electrons are illustrated in Figure 3. Figure 3(a) corresponds to the ground state

Local structure and localized charge density for negatively charged DX configurations

Figure 3. Local structure and localized charge density for negatively charged DXDX configurations of (a) ground-state SiAl(I)−_{\mathrm{Al(I)}}^{-}, (b) metastable-state SiAl(I)−_{\mathrm{Al(I)}}^{-}, and (c) SiAl(II)−_{\mathrm{Al(II)}}^{-} in θ\theta-Al2_2O3_3. Dark blue spheres denote Si, light blue Al, and red O. Percentage changes of bond lengths, referenced to bonds in bulk Al2_2O3_3, are indicated. Isosurfaces of the charge density (0.02 e/A˚30.02\ e/\mathring{\mathrm{A}}^3) of the localized state in the DXDX centers are shown in green.

β\beta-Ga2_2O3_3(+/0)(+/−)(0/−)UUxonsetx^{\mathrm{onset}}
CGa(I)_{\mathrm{Ga(I)}}5.204.924.65−0.54
CGa(II)_{\mathrm{Ga(II)}}4.325.055.771.46
Hi_i5.474.844.21−1.25
HO(I)_{\mathrm{O(I)}}5.475.204.91−0.55
HO(II)_{\mathrm{O(II)}}4.985.015.040.07
HO(III)_{\mathrm{O(III)}}5.715.565.42−0.29
AlGaO3_3(+/0)(+/−)(0/−)UU
SiGa(I)_{\mathrm{Ga(I)}}6.396.196.00−0.39
SiAl(II)_{\mathrm{Al(II)}}6.0656.466.850.79
CGa(I)_{\mathrm{Ga(I)}}4.934.814.69−0.24
CAl(II)_{\mathrm{Al(II)}}4.054.975.901.86
Hi_i5.704.673.65−2.05
HO(I)_{\mathrm{O(I)}}5.925.695.45−0.47
HO(II)_{\mathrm{O(II)}}5.605.214.83−0.77
HO(III)_{\mathrm{O(III)}}5.695.705.710.02
θ\theta-Al2_2O3_3(+/0)(+/−)(0/−)UU
SiAl(I)_{\mathrm{Al(I)}}6.776.796.810.0470%
SiAl(II)_{\mathrm{Al(II)}}7.206.986.76−0.4481%
CAl(I)_{\mathrm{Al(I)}}4.964.954.95−0.015%
CAl(II)_{\mathrm{Al(II)}}4.235.075.901.9551%
Hi_i5.834.833.84−1.991%
HO(I)_{\mathrm{O(I)}}6.516.366.41−0.1037%
HO(II)_{\mathrm{O(II)}}5.785.705.61−0.1613%
HO(III)_{\mathrm{O(III)}}6.116.126.130.0341%

Table 2. Charge-state transition levels (eV) Eq. (5) and effective correlation parameter UU (eV) Eq. (7) for various impurities in β\beta-Ga2_2O3_3, ordered AlGaO3_3, and θ\theta-Al2_2O3_3. The neutral and negative charge states that are used to compute charge-state transition levels and UU all correspond to localized states. Values for Si in Ga2_2O3_3 are missing since the localized neutral and negative charge states cannot be stabilized. We also list xonsetx^{\mathrm{onset}} (%), the Al concentration in (Alx_xGa1−x_{1-x})2_2O3_3 corresponding to the onset of DXDX behavior.

of SiAl(I)−_{\mathrm{Al(I)}}^{-}, while Figure 3(b) represents a metastable state that is 0.40 eV higher in energy. The metastable state [Figure 3(b)] features the type of broken bond that is often considered characteristic of a DXDX center, resulting in a dangling bond on the Si atom that is filled with two electrons. The ground state of SiAl(I)−_{\mathrm{Al(I)}}^{-} [Figure 3(a)] also displays significant bond distortions, both in the SiO4_4 tetrahedron and its nearest AlO4_4; however, no clear bond breaking occurs. Instead, the main effect of the distortion is to reduce the Si-Al distance from 2.88 Å (the distance in bulk θ\theta-Al2_2O3_3) to 2.32 Å, creating a two-electron bond between Si and Al, as clearly seen in Figure 3(a). Octahedrally coordinated SiAl(II)−_{\mathrm{Al(II)}}^{-} also forms a DXDX center, shown in Figure 3(c). Three Si-O bonds are broken in the SiO6_6 octahedron, and two electrons are localized on the Si dangling bond. Tests for the Si DXDX center in a 160-atom supercell yielded very similar local geometries, with bond lengths differing by less than 0.01 Å. The 160-atom supercell calculations yield a (+/−) charge-state transition level that is within 0.05 eV of the result using a 120-atom supercell.

The formation of the silicon DXDX center indicates that Si cannot be a shallow donor in θ\theta-Al2_2O3_3. To gain insight into its effectiveness in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, we evaluate the position of the (+/−) transition level and compare it with the CBM in (Alx_xGa1−x_{1-x})2_2O3_3 alloys. The negative charge state employed to compute the (+/−) transition level has to correspond to a localized state. Such a localized state can be stabilized in Al2_2O3_3 and ordered AlGaO3_3 alloy but not in Ga2_2O3_3. Therefore, the (+/−) transition levels in alloys are interpolated (or extrapolated towards Ga2_2O3_3) based on the values in Al2_2O3_3 and ordered AlGaO3_3 alloy (see values in Table II). The values of the CBM are interpolated based on those in Ga2_2O3_3 and Al2_2O3_3, with the addition of bowing using a bowing parameter of 0.93 eV and assuming all of the band-gap bowing occurs in the CBM [28].

The resulting values of xonsetx^{\mathrm{onset}}, the Al concentration at which the (+/−) level moves below the CBM (i.e., the DXDX center becomes stable) are listed in Table II. We found Si incorporating on the tetrahedral site will be an effective donor over a wide range of Al alloying, up to 70% Al (see Figure 4). This value is somewhat lower than the xonset=86%x_{\mathrm{onset}}=86\% reported in Ref. 21. The difference can be attributed to the fact that our calculated (+/−)(+/-) level in Al2_2O3_3 (AlGaO3_3) is 0.12 eV (0.37 eV) lower than that in Ref. 21, due to the fact that we identified a lower-energy structure for the DXDX center. In addition, we find that Si on the octahedral site is also an effective donor in (Alx_xGa1−x_{1-x})2_2O3_3, up to 81% Al (see Figure 4).

Energy levels as a function of Al concentration

Figure 4. The (+/−)(+/-) levels of SiI_{\mathrm{I}}, SiII_{\mathrm{II}}, CI_{\mathrm{I}}, Hi_{\mathrm{i}}, HO(I)_{\mathrm{O(I)}}, HO(II)_{\mathrm{O(II)}}, HO(III)_{\mathrm{O(III)}}, and the (0/−)(0/-) level of CII_{\mathrm{II}} obtained from calculations in Al2_2O3_3, Ga2_2O3_3 and ordered AlGaO3_3 alloys. The notation SiI_{\mathrm{I}}, resp. SiII_{\mathrm{II}}, denotes substitutional Si on the tetrahedral (I), resp. octahedral (II) cation site, and similarly for CI_{\mathrm{I}} and CII_{\mathrm{II}}. The charge-state transition levels for SiI_{\mathrm{I}} and SiII_{\mathrm{II}} in Ga2_2O3_3 are missing since the localized neutral and negative charge states cannot be stabilized. The dashed lines connecting the calculated values are just a guide to the eye. The CBM/VBM band offsets as a function of the Al concentration for alloys were obtained from Ref. 28.

Our treatment of defect behavior in the alloy by performing linear interpolation (Figure 4) is obviously an approximation. In the case of (Alx_xGa1−x_{1-x})2_2O3_3 alloys, it is likely to be quite reliable, due to the similarity in the properties of Al and Ga cations; indeed, we have found that the geometries of defect configurations are very similar in β\beta-Ga2_2O3_3 and θ\theta-Al2_2O3_3. Some degree of validation is also obtained from the results for transition levels explicitly calculated for AlGaO3_3 alloys. As shown in Figure 4, the results for the alloy generally fall on the line that linearly interpolates between β\beta-Ga2_2O3_3 and θ\theta-Al2_2O3_3; the small deviations that occur for CI_{\mathrm{I}} and Hi_{\mathrm{i}} impurities amount to less than 0.15 eV, which is gratifying agreement. We also note that this interpolation procedure has been demonstrated to be effective for obtaining transition levels in AlGaN alloys [27, 53]. Indeed, experiment [54] indicated that the ON_{\mathrm{N}} transition level in AlGaN alloys varies linearly with alloy concentration, supporting the validity of linear interpolation.

Carbon

Incorporation

Carbon is a commonly observed background impurity in semiconductors, particularly in MOCVD-grown films. In Ga2_2O3_3, carbon on the tetrahedral site is a shallow donor [22, 55]. Here we investigate whether the increase in band gap in (Alx_xGa1−x_{1-x})2_2O3_3 will cause the carbon (+/−)(+/-) level to drop below the CBM, turning carbon into a compensating acceptor. We also study whether carbon on the oxygen site could cause compensation.

Lyons et al. [22] investigated carbon impurities on the anion, cation, and interstitial sites in Ga2_2O3_3 and showed that under most conditions, the carbon impurity prefers the substitutional tetrahedral cation site. For a consistent comparison, we reproduced the formation energies of carbon impurities on the cation sites in Ga2_2O3_3 [see Figure 2(a,Figure 2b)] and our results agree with Lyons et al. [22] under the same condition. Similar to the case of Ga2_2O3_3, C prefers to occupy the tetrahedral site (CAl(I)+^+_{\mathrm{Al(I)}}) in monoclinic Al2_2O3_3, with a formation energy 2.10 eV lower than that of CAl(II)+^+_{\mathrm{Al(II)}} at the VBM (see Figure 2). At the CBM, the formation energy of CAl(I)−^-_{\mathrm{Al(I)}} is 2.03 eV lower than that of CAl(II)−^-_{\mathrm{Al(II)}}. The behavior of CAl_{\mathrm{Al}} as a compensating center

is broadly consistent with previous results for carbon in α\alpha-Al2_2O3_3, the corundum phase [56]. Figure 2 also shows that under Al-rich conditions the formation energy of CAl(I)−^-_{\mathrm{Al(I)}} is high, significantly decreasing when we move to Al-poor conditions. However, carbon incorporation in MOCVD-grown samples is likely not governed by thermodynamic equilibrium, but rather determined by unintentional incorporation due to incomplete dissociation of metal-organic precursors. In the following we therefore examine both CAl(I)_{\mathrm{Al(I)}} and CAl(II)_{\mathrm{Al(II)}}.

Carbon on the tetrahedral site

The small atomic size of carbon leads to bond-breaking and a variety of possible geometries, as depicted in Figure 5. Focusing first on CAl(I)_{\mathrm{Al(I)}}, already in the positive charge state we find two competing configurations of CAl(I)+^+_{\mathrm{Al(I)}}. In the most stable state (not depicted), C forms four C-O bonds, and the oxygen cage shrinks, yielding four C-O bonds with bond lengths ranging from 1.40 to 1.44 Å. In the metastable configuration [see Figure 5(a)], which is only 87 meV higher than the ground state, the C-O(III) bond is broken, and the remaining three C-O bonds have similar lengths (1.28, 1.30, 1.30 Å) and almost lie in the same plane, with nearly 120° angles between the bonds. Carbon effectively forms an sp2sp^2-bonded configuration with its three O neighbors. This 3-fold coordination was also found for CGa(I)_{\mathrm{Ga(I)}} in Ga2_2O3_3 [22], with very similar C-O bond lengths (1.27–1.30 Å). The 3-fold-coordinated configuration is the lowest-energy configuration in Ga2_2O3_3 and AlGaO3_3.

Local structure and localized charge density for six configurations in θ-Al2O3

Figure 5. Local structure and localized charge density for (a) metastable 3-fold-coordinated configuration of CAl(I)+\mathrm{C}_{\mathrm{Al(I)}}^{+}, (b) CAl(I)0\mathrm{C}_{\mathrm{Al(I)}}^{0}, (c) CAl(I)−\mathrm{C}_{\mathrm{Al(I)}}^{-}, (d) CAl(II)+\mathrm{C}_{\mathrm{Al(II)}}^{+}, (e) CAl(II)0\mathrm{C}_{\mathrm{Al(II)}}^{0} and (f) CAl(II)−\mathrm{C}_{\mathrm{Al(II)}}^{-} in θ\theta-Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}. Brown spheres denote C, light blue Al, and red O. Isosurfaces of the charge density (0.01 e/A˚3e/\mathring{\mathrm{A}}^{3}) of the localized electrons in CAl(I)0\mathrm{C}_{\mathrm{Al(I)}}^{0}, CAl(I)−\mathrm{C}_{\mathrm{Al(I)}}^{-}, CAl(II)0\mathrm{C}_{\mathrm{Al(II)}}^{0} and CAl(II)−\mathrm{C}_{\mathrm{Al(II)}}^{-} are shown in green.

For the neutral charge state of CAl(I)_{\mathrm{Al(I)}}, we found that we can stabilize as many as five distinct atomic configurations, starting from initial structures in which different C-O bonds are broken in a CO4_4 tetrahedron. The most stable configuration corresponds to breaking of the C-O(III) bond, forming a nonplanar CO3_3 cluster, as shown in Figure 5(b). The C-O bond lengths are 1.35, 1.39, 1.39 Å, while the distance between C and O(III) is 2.82 Å. This configuration is similar to the 3-fold coordination for the positive charge state, but the carbon has moved beyond the plane of its oxygen neighbors. As seen in Figure 5(b), the C has moved towards a next-nearest Al(I) neighbor in the same (010) plane, reducing the C-Al distance from 3.5 Å (for C on the nominal Al site) to 2.6 Å. In the process, the charge of the localized state becomes confined between C and that next-nearest-neighbor Al atom. The fact that this state is localized clearly indicates that CAl(I)_{\mathrm{Al(I)}} is not a shallow donor in θ-Al2_2O3_3. Indeed, the corresponding Kohn-Sham state lies 4.42 eV below the CBM.

Another configuration in which the same C-O(III) bond is broken can be stabilized with a distance of 2.38 Å between C and O(III); this configuration is only 0.05 eV higher in energy. Other configurations involve breaking a C-O(I) bond (0.80 eV higher than the ground state) or breaking a C-O(II) bond (0.91 eV higher than the ground state). The geometry in which all four C-O bonds in the CO4_4 tetrahedron are maintained is also a local minimum, 0.89 eV higher in energy than the ground-state C-O(III) bond-breaking configuration.

In the negative charge state, the most stable state is similar to the ground state of CAl(I)0^0_{\mathrm{Al(I)}}, with a broken C-O(III) bond [see Figure 5(c)]. Other configurations can be stabilized, but with energies that are at least 1.3 eV higher than the ground state. Figure 5(c) depicts the charge density of the localized state. Comparison with Figure 5(b) indicates that with the addition of an extra electron a C-Al bond has formed with the next-nearest-neighbor Al(I). The C-Al distance is reduced to 2.0 Å after relaxation. This is another example of a DX configuration in which a cation-cation bond forms, but we note the distinction with the DX configuration of SiAl(I)+^+_{\mathrm{Al(I)}} shown in Figure 3(a): SiAl(I)+^+_{\mathrm{Al(I)}} bonds with a nearest-neighbor tetrahedral host cation, while CAl(I)−^-_{\mathrm{Al(I)}} bonds with a next-nearest-neighbor tetrahedral host cation. A similar bonding configuration for the negative charge state of carbon on the tetrahedral site is also observed in Ga2_2O3_3 and AlGaO3_3.

Carbon on the octahedral site

Turning now to CAl(II)_{\mathrm{Al(II)}}, a variety of competing local geometries with different broken bonds are also present in the positive, neutral and negative charge states due to the small atomic size of carbon. In the positive charge state, the ground state corresponds to bond breaking of two C-O(III) bonds and one C-O(I) bond in the nominal octahedron, leaving the remaining three C-O bonds (1.28, 1.28, 1.30 Å) to form a 3-fold coordinated configuration that is similar to the metastable configuration of CAl(I)+^+_{\mathrm{Al(I)}} [see Figure 5(d)]. We also observe a competing metastable state of CAl(II)+^+_{\mathrm{Al(II)}} with a different 3-fold coordinated configuration that exhibits bond breaking of all three C-O(III) within the octahedron. This metastable state is 0.20 eV higher than the ground state. This 3-fold coordinated configuration with three broken C-O(III) bonds becomes the ground state in the neutral charge state [see Figure 5(e)]. The remaining three C-O bonds form a nonplanar CO3_3 cluster, with C-O bond lengths of 1.37, 1.37, 1.41 Å. The charge of the localized state, dominated by a pp-orbital character, is confined between C and the center of the octahedron. Another (metastable) 3-fold coordinated configuration with bond breaking of two C-O(III) and one C-O(II) is 0.28 eV higher.

In the negative charge state of CAl(II)_{\mathrm{Al(II)}}, the most stable configuration is 2-fold coordinated, with two equivalent C-O(I) bonds (1.40, 1.40 Å) [see Figure 5(f)]. The localized states exhibit roughly equal pp- and ss-orbital character and the associated charges are confined near C, with an appreciable weight at the center of the octahedron. We also find another competing 2-fold coordinated metastable configuration, with one C-O(I) bond (1.26 Å) and one C-O(II) bond (1.91 Å) remaining, and with an energy 0.18 eV higher.

Carbon on cation sites as a compensating center

When discussing substitutional C in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, C could be replacing either a Ga or an Al atom; in this section (as in Figure 4) we use the generic notation C(I)_{\mathrm{(I)}} to denote either CGa(I)_{\mathrm{Ga(I)}} or CAl(I)_{\mathrm{Al(I)}}, and C(II)_{\mathrm{(II)}} to denote either CGa(II)_{\mathrm{Ga(II)}} or CAl(II)_{\mathrm{Al(II)}}. C(I)_{\mathrm{(I)}} is a negative-UU center across Ga2_2O3_3, Al2_2O3_3 and the ordered (Alx_xGa1−x_{1-x})2_2O3_3 alloy (see Table II). We can evaluate its (+/−) transition level in the relevant range of (Alx_xGa1−x_{1-x})2_2O3_3 alloy compositions by interpolating between Ga2_2O3_3 and the AlGaO3_3 alloy, with consideration of the band bowing [28] (see Figure 4). For C(I)_{\mathrm{(I)}}, we find that the impurity starts acting as an acceptor in (Alx_xGa1−x_{1-x})2_2O3_3 alloys already at 5% Al. C(II)_{\mathrm{(II)}} is not a negative-UU center, but it can still act as compensating acceptor in nn-type Al2_2O3_3 (see Figure 2). To estimate the onset of C(II)_{\mathrm{(II)}} as a compensator in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, we interpolate the (0/−) transition levels between Al2_2O3_3 and the AlGaO3_3 alloy (see Figure 4), finding that C(II)_{\mathrm{(II)}} starts acting as an acceptor at 51% Al.

Our results indicate that unintentional C incorporation is a potential explanation for the lack of doping efficiency observed at low concentrations of Si in MOCVD-grown (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} alloys. Since unintentionally incorporated C(I) acts as a compensating acceptor in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} with x≥5%x \ge5\%, the Si concentration needs to exceed the concentration of C(I) in order for Si to actually provide nn-type doping.

Carbon on oxygen sites, CO\mathrm{C}_{\mathrm{O}}

In Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}, it was found that CO\mathrm{C}_{\mathrm{O}} acts as a compensating acceptor when the Fermi level is high in the gap [22]. Reference [22] reported results for a single O site and only for O-rich conditions; in Figure 6(a,Figure 6b) we report a full set of results for CO\mathrm{C}_{\mathrm{O}} in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}. Under conditions relevant for nn-type doping, the formation energy of CO\mathrm{C}_{\mathrm{O}} is lowest when the Fermi level is at the CBM under Ga-rich conditions; however, even under these extreme conditions, this formation energy is still 2.69 eV.

Figure 6. Formation energy versus Fermi level for CO_\mathrm{O} in (a)-(b) β-Ga2_2O3_3 and (c)-(d) θ-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. Carbon incorporation on three possible O sites is considered: O(I), O(II), and O(III). The grey area indicates the conduction band of β-Ga2_2O3_3.

The formation energy of CO\mathrm{C}_{\mathrm{O}} can be significantly lower in Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, as shown in Figure 6(c,Figure 6d). For Fermi levels low in the gap (which may be difficult to attain in Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}), CO\mathrm{C}_{\mathrm{O}} prefers the 4+ charge state. At higher Fermi-level positions, the neutral, 1−, and 2− charge states become more favorable. For Fermi levels close to the CBM, CO(I)2−\mathrm{C}_{\mathrm{O(I)}}^{2-} is the energetically most favorable state.

We can therefore conclude that for nn-type doping conditions in both Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, CO\mathrm{C}_{\mathrm{O}} acts as a compensating acceptor. The high formation energy indicates it will not be a concern in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}, but it could more easily incorporate in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} alloys. However, as evident from Figure 6, this sensitively depends on chemical potentials, with cation-rich (oxygen-poor) conditions posing more of a problem. We will return to this issue in Sec. III D 4.

Hydrogen

Hydrogen is another impurity that is commonly unintentionally incorporated, particularly in MOCVD-grown samples. We investigate H substituting on the O site (HO(I)\mathrm{H}_{\mathrm{O(I)}}, HO(II)\mathrm{H}_{\mathrm{O(II)}}, and HO(III)\mathrm{H}_{\mathrm{O(III)}}) and H on the interstitial site (Hi\mathrm{H}_{i}) in θ\theta-Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}; their formation energies are shown in Figure 7(c,Figure 7d). For comparison, we also show our calculated formation energies in β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} [see Figure 7(a,Figure 7b)], which compare well with previous reports [20]. In β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}, all these configurations were found to be shallow donors [20], but in θ\theta-Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} they are stabilized in the negative charge state and thus act as acceptors when the Fermi level is high in the gap.

Figure 7. Formation energy versus Fermi level for substitutional and interstitial hydrogen in (a)-(b) β-Ga2_2O3_3 and (c)-(d) θ-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. The grey area indicates the conduction band of β-Ga2_2O3_3.

Substitutional hydrogen, HO\mathrm{H}_{\mathrm{O}}

In Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, substitutional HO+\mathrm{H}_{\mathrm{O}}^{+} favors incorporation on the O(I) site. Incorporation of a proton on the O(II) [O(III)] site is 0.29 [0.80 eV] higher in energy (see Figure 7). The same site preference is also observed in the ordered AlGaO3_3 alloy: total energies of HO(II)+^+_\mathrm{O(II)} and HO(III)+^+_\mathrm{O(III)} are 0.08 eV and 0.33 eV higher than that of HO(I)+^+_\mathrm{O(I)}, respectively. In Ga2_2O3_3, HO(I)+^+_\mathrm{O(I)} is also most favorable, and HO(II)+^+_\mathrm{O(II)} and HO(III)+^+_\mathrm{O(III)} are slightly higher in energy [20].

Under Al-rich conditions, HO_\mathrm{O} has a low formation energy (<2<2 eV) in Al2_2O3_3, meaning it is easy to incorporate. HO(I)_\mathrm{O(I)} and HO(II)_\mathrm{O(II)} behave as negative-UU centers with U=−0.10U=-0.10 eV and −0.16-0.16 eV, and a (+/−)(+/-) charge-state transition level at 1.05 eV and 1.71 eV below the CBM (see Table II and Figure 7). HO(III)_\mathrm{O(III)} is almost a negative-UU center, with U=+0.03U=+0.03, and (+/0)(+/0) and (0/−)(0/-) charge-state transition levels at 6.11 eV and 6.13 eV, indicating a tiny (0.02 eV) range of stability of the neutral charge state. The formation of negative-UU centers is due to the pronounced energy lowering in their negative charge state, induced by major local structural distortions. The local structures are illustrated in Figure 8(a–Figure 8c); two electrons are localized around H and nearby Al sites. In the case of HO(I)−^-_\mathrm{O(I)} [Figure 8(a)], the H atom is still relatively close to the O(I) site, but the configurations of HO(II)−^-_\mathrm{O(II)} [Figure 8(b)]

Local structure of hydrogen defects in $\theta$-$\mathrm{Al}_2\mathrm{O}_3$

Figure 8. Local structure of (a) HO(I)−\mathrm{H}_{\mathrm{O(I)}}^{-} (b) HO(II)−\mathrm{H}_{\mathrm{O(II)}}^{-}, (c) HO(III)−\mathrm{H}_{\mathrm{O(III)}}^{-} and (d) Hi−\mathrm{H}_{\mathrm{i}}^{-} in θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3. Light blue, red and gray spheres denote Al, O and H atoms. The position of the O atom that was removed in HO−\mathrm{H}_{\mathrm{O}}^{-} was labeled using a black dashed circle. Isosurfaces of the charge density (0.01 e/A˚30.01\ e/\mathring{\mathrm{A}}^{3}) of the localized electrons are shown in green.

and HO(III)−^-_\mathrm{O(III)} [Figure 8(c)] are more like complexes of an oxygen vacancy plus a nearby interstitial H.

HO(I)_\mathrm{O(I)}, HO(II)_\mathrm{O(II)}, HO(III)_\mathrm{O(III)} will act as acceptors in nn-type (Alx_xGa1−x_{1-x})2_2O3_3 alloys due to the emergence of the (+/−)(+/-) transition level in the band gap starting as a critical Al composition xonsetx_\mathrm{onset}. Interpolating (+/−)(+/-) charge-state transition levels between Ga2_2O3_3 and the ordered AlGaO3_3 alloy, the onset Al concentrations for HO(I)_\mathrm{O(I)}, HO(II)_\mathrm{O(II)}, HO(III)_\mathrm{O(III)} acting as compensating centers are 37%, 13% and 41%, respectively (see Figure 4 and Table II).

Interstitial hydrogen, Hi_\mathrm{i}

Turning now to interstitial H in Al2_2O3_3, we find that the lowest-energy configuration in the neutral and positive charge state has H bonded to the three-fold coordinated O(I). In the negative charge state, Hi_\mathrm{i} prefers to sit near two Al(I) atoms; the local geometry is illustrated in Figure 8(d). The local configurations of the −-, 0, and ++ state of Hi_\mathrm{i} are similar to those in Ga2_2O3_3 [20]. In the neutral charge state, the Kohn-Sham state of Hi_\mathrm{i} lies about ∼3\sim3 eV below the CBM. In the negative charge state, the Kohn-Sham state is about 1.3 eV above the VBM, as a result of the formation of two H–Al bonds.

As seen in Figure 7 and Table II, the (+/−)(+/-) level of Hi\mathrm{H}_{\mathrm{i}} in Al2O3\mathrm{Al}_2\mathrm{O}_3 lies at 4.83 eV above the VBM. Hi\mathrm{H}_{\mathrm{i}} is a negative-UU center, with a large magnitude of U=−1.99U=-1.99 eV. Knowledge about the position of the (+/−)(+/-) levels in β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3 allows us to estimate the band lineup between these materials, according to Ref. 57; this leads to an alignment where the VBM of β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 lies 0.01 eV below the VBM of θ\theta-Al2O3\mathrm{Al}_2\mathrm{O}_3. We can compare this result with values obtained by alignment with the vacuum level derived from surface calculations; depending on the surface orientation, this procedure produces values ranging from +0.40+0.40 to −0.08-0.08 eV [58]. The overall agreement with the hydrogen alignment is gratifying.

Figure 7 shows that the formation energies of Hi\mathrm{H}_{\mathrm{i}} in Al2O3\mathrm{Al}_2\mathrm{O}_3 are quite low, suggesting that Hi\mathrm{H}_{\mathrm{i}} will readily incorporate, and in nn-type material it will act as a compensating acceptor. Following our interpolation procedure based on the case of Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and ordered AlGaO3\mathrm{AlGaO}_3 alloy, the (+/−)(+/-) transition level of Hi\mathrm{H}_{\mathrm{i}} will already appear in the band gap of (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_2\mathrm{O}_3 alloys at an Al concentration of 1% (see Figure 4).

Migration of interstitial hydrogen

Since hydrogen is expected to be quite mobile, in order to assess whether hydrogen can play a role in compensation it is important to also assess migration barriers. We investigated the migration barrier (EbE_{\mathrm{b}}) of Hi\mathrm{H}_{\mathrm{i}} using the PBE functional and a one-shot HSE method, as described in Sec. II A. The results are listed in Table III. The annealing temperatures at which H becomes mobile for ++ and −- charge states and for various crystallographic directions, calculated using Eq. (1), are also included in Table III. As expected, the migration of Hi\mathrm{H}_{\mathrm{i}} in the monoclinic structure is anisotropic. In Ga2O3\mathrm{Ga}_2\mathrm{O}_3, we find the migration barrier of Hi+\mathrm{H}_{\mathrm{i}}^{+} along the [10] direction to be 0.28 eV, in good agreement with the 0.34 eV value reported in Ref. 20. The migration path is illustrated in Figure 9(a). Migration along other directions has higher barriers. Along [100] [Figure 9(b)] the barrier is as high as 2.95 eV, and along [1] Figure 9(c), the barrier is 1.73

Potential energy surfaces for H$^{+}_{i}$ migration in $\beta$-Ga$_2$O$_3$

Figure 9. Potential energy for Hi+^{+}_{i} migration along the (a) [10], (b) [100], (c) [100] directions in β\beta-Ga2_2O3_3. Various configurations along the migration path are shown as insets. Green and red spheres denote Ga and O atoms, respectively. Note the very different scales for the potential energy surfaces between (a) and (b) or (c).

H+\mathrm{H}^{+}H−\mathrm{H}^{-}
[10][100][1][10][100][1]
Ga2O3\mathrm{Ga}_2\mathrm{O}_3
EbE_{\mathrm{b}}0.282.951.732.491.831.57
TannealT_{\mathrm{anneal}}1011062623896659565
Al2O3\mathrm{Al}_2\mathrm{O}_3
EbE_{\mathrm{b}}0.232.291.781.332.671.83
TannealT_{\mathrm{anneal}}83824641479961659

Table 3. Calculated migration barriers (EbE_{\mathrm{b}}, eV) of H+\mathrm{H}^{+} and H−\mathrm{H}^{-} in Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and Al2O3\mathrm{Al}_2\mathrm{O}_3 along three crystallographic directions. The calculated annealing temperature (TannealT_{\mathrm{anneal}}, K) is listed, assuming a hopping rate of 1 s−1^{-1}.

eV. The annealing temperature for Hi+\mathrm{H}_{\mathrm{i}}^{+} migration along [10], [100] and [1] directions are 101, 1062, and 623 K, respectively.

Our calculated results for migration paths and barriers for Hi+\mathrm{H}_{\mathrm{i}}^{+} in Al2O3\mathrm{Al}_2\mathrm{O}_3 are quite similar to the results in Ga2O3\mathrm{Ga}_2\mathrm{O}_3; migration is also strongly anisotropic (see Table III). The low migration barrier suggests that Hi+\mathrm{H}_{\mathrm{i}}^{+} can move along the [10] direction (which is the most commonly used growth orientation) even at temperatures well below room temperature.

For Hi−\mathrm{H}_{\mathrm{i}}^{-}, the migration barriers are generally higher. Particularly striking is that migration in Ga2O3\mathrm{Ga}_2\mathrm{O}_3 now has the highest barrier along [10] (see Table III). We attribute this to the fact that in the barrier geometry for Hi−\mathrm{H}_{\mathrm{i}}^{-}, the distance between H and the nearest Ga atoms is quite large (2.1 Å). Since it is Coulombic attraction between Hi−\mathrm{H}_{\mathrm{i}}^{-} and the cations that stabilizes the structure, the lack of strong bonding at the saddle point raises the energy. In contrast, in Al2O3\mathrm{Al}_2\mathrm{O}_3 the corresponding distance is only 1.8 Å, providing for a stronger interaction with the Al atoms and lowering the barrier height. While the migration barriers for Hi−\mathrm{H}_{\mathrm{i}}^{-} are higher than for Hi+\mathrm{H}_{\mathrm{i}}^{+}, the annealing temperatures in Table III indicate that Hi−\mathrm{H}_{\mathrm{i}}^{-} may be mobile at temperatures at which growth or processing of Ga2O3\mathrm{Ga}_2\mathrm{O}_3 and (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_2\mathrm{O}_3 alloys is typically performed.

Figuring out precise migration barriers for Hi\mathrm{H}_{\mathrm{i}} in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_2\mathrm{O}_3 alloys may not be as simple as interpolating the values in Ga2_2O3_3 and Al2_2O3_3. The barriers to be overcome will be determined by the local environment. If, at a particular Al composition, a “percolation path” exists that allows hydrogen to follow favorable atomic arrangements, the lower of the two migration barriers will likely apply. In the absence of such a path, the higher of the two barriers will need to be overcome.

We note that the mobility of Hi−^{-}_{i} will be reduced by binding to positively charged impurities, in particular donor dopants. Formation of a Si–H complex will increase the stability of Hi−^{-}_{i} in the lattice and add to the overall activation energy for hydrogen motion. Therefore interstitial Hi−^{-}_{i}, in addition to substitutional HO−^{-}_{\mathrm{O}}, may play a role in compensation of shallow donors in (Alx_{x}Ga1−x_{1-x})2_2O3_3.

Complexes

Since hydrogen can easily incorporate and has relatively low migration barriers, we need to assess the possibility of complex formation between hydrogen and other impurities, either with the intentionally incorporated Si donor, or with unintentional impurities such as C.

Sication–H complexes

We first discuss complexes with Si on the cation site; as discussed in Sec. III A, we found that Sication_{\mathrm{cation}} is an effective donor in (Alx_{x}Ga1−x_{1-x})2_2O3_3 alloys up to 70% Al incorporation for Si(I) and 81% Al incorporation for Si(II). The formation energy of Si–H complexes in Ga2_2O3_3 is shown in Figure 10(a) for Ga-rich and Figure 10(b) for Ga-poor conditions. We find that similar to the SiGa_{\mathrm{Ga}} impurity, the SiGa_{\mathrm{Ga}}–H complex also has lower energy when Si occupies the tetrahedral cation (I) site.

Formation energy versus Fermi level for isolated Si impurities, H interstitials, and Si–H defect complexes

Figure 10. Formation energy versus Fermi level for isolated Si impurities, H interstitials, and Si–H defect complexes in (a)-(b) β\beta-Ga2_2O3_3 and (c)-(d) θ\theta-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. Dashed lines denote thermodynamic instability of the defect complex, as explained in the text. The grey area indicates the conduction band of β\beta-Ga2_2O3_3.

The formation energy of Si–H complexes under Ga-poor conditions is simply a rigid shift to higher energies of the formation energy under Ga-rich conditions [Figure 10(a,Figure 10b)]; our discussion about the properties of complexes applies to both. We find that when the Fermi level is high in the gap, SiGa_{\mathrm{Ga}}(I)–H complexes are stable in the neutral charge state, indicating that the Si donor has been passivated. We also find that SiGa_{\mathrm{Ga}}(I)–H has a (2+/0) charge-state transition level at 0.41 eV below the CBM. The formation of a Si–H complex might seem unexpected, given that the constituents, SiGa_{\mathrm{Ga}} and Hi_{i}, both prefer to occur in the positive charge state throughout the band gap of Ga2_2O3_3, as evident from Figure 10(a). Our calculated formation energy of point defect SiGa_{\mathrm{Ga}} and Hi_{i} in Ga2_2O3_3 agree well with the previous study [20]. However, as seen in Table II, the (+/−) level of Hi_{i} in Ga2_2O3_3 lies at 4.84 eV above the VBM, i.e., just 0.01 eV above the CBM. It is therefore to be expected that for Fermi levels near the CBM, Hi−_{i}^{-} could be stable enough to lead to formation of a complex with SiGa+_{\mathrm{Ga}}^{+}, particularly when Coulomb attraction is taken into account.

This is confirmed by evaluation of the binding energy of the complex, defined as

Ebind[(SiGa(I)−H)0]=Ef(SiGa(I)+)+Ef(Hi−)−Ef[(SiGa(I)−H)0](8)E_{\mathrm{bind}}[(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0] = E^f(\mathrm{Si}_{\mathrm{Ga(I)}}^+) + E^f(\mathrm{H}_i^-) - E^f[(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0] \tag*{(8)}

where a positive value of the binding energy signifies a stable, bound complex. This yields a binding energy of 0.59 eV. This value (which is smaller than the formation energy of each of the constituents) indicates the complex will not be stable during growth at high temperatures, since entropy favors the isolated entities (see Ref. 59). In addition, formation after growth is not very likely since Hi\mathrm{H}_i will predominantly occur in the positive charge state, which is repelled by SiGa+\mathrm{Si}_{\mathrm{Ga}}^+.

One may then wonder about the stability of (SiGa(I)−H)2+(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^{2+}. Indeed, a binding-energy calculation in this case yields a negative value for EbindE_{\mathrm{bind}} (−0.24-0.24 eV), i.e., the sum of the formation energy of the constituents, SiGa(I)+\mathrm{Si}_{\mathrm{Ga(I)}}^+ and Hi−\mathrm{H}_i^-, is smaller than the formation energy of the (SiGa(I)−H)2+(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^{2+} complex. We show the 2+ charge state of this complex with dashed lines in Figure 10, to indicate that this is a locally stable configuration that is, however, thermodynamically unstable.

The notion that (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0 results from bonding between SiGa(I)+\mathrm{Si}_{\mathrm{Ga(I)}}^+ and Hi−\mathrm{H}_i^- is consistent with the local geometry of the complex: we found in Sec. III C 2 that Hi−\mathrm{H}_i^- prefers to bind to two cation atoms on tetrahedral sites, and the configuration of (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0 is such that the hydrogen atom is located close to a Ga(I) and to the Si(I) atom as seen from Figure 11(a). This is very similar to the geometry shown in Figure 8(d). For (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0, the bond length of Si(I)-H and Ga(I)-H are 1.53 Å and 1.77 Å, respectively.

Local structure of (a) $(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^{0}$, (b) $(\mathrm{Si}_{\mathrm{Ga(II)}}-\mathrm{H})^{0}$, (c) $(\mathrm{C}_{\mathrm{Ga(I)}}-\mathrm{H})^{0}$ and (d) $(\mathrm{C}_{\mathrm{Ga(II)}}-\mathrm{H})^{0}$ in $\mathrm{Ga}_{2}\mathrm{O}_{3}$

Figure 11. Local structure of (a) (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^{0}, (b) (SiGa(II)−H)0(\mathrm{Si}_{\mathrm{Ga(II)}}-\mathrm{H})^{0}, (c) (CGa(I)−H)0(\mathrm{C}_{\mathrm{Ga(I)}}-\mathrm{H})^{0} and (d) (CGa(II)−H)0(\mathrm{C}_{\mathrm{Ga(II)}}-\mathrm{H})^{0} in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}. Green, red, gray, blue and brown spheres denote Al, O, H, Si and C atoms, respectively.

If the (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0 complex does form during cooldown, one may wonder about its stability at room temperature. The activation energy for dissociation can be estimated by adding the migration barrier for the mobile hydrogen species to the binding energy of the complex. All of the Hi−\mathrm{H}_i^- migration barriers are large enough (Table III) to make this activation energy sufficiently high and keep the complex stable at room temperature. Using the lowest migration barrier for Hi−\mathrm{H}_i^- in Ga2_2O3_3 in Table III, we would estimate an activation energy of 0.59+1.57=2.16 eV, which would correspond to an annealing temperature of 778 K. However, since the (2+/0) transition level is so close to the CBM, an alternative dissociation mechanism could occur in which electron excitation to the CBM converts the complex to a 2+ charge state, after which the dissociation will proceed more easily both because of the lower migration barrier of Hi+\mathrm{H}_i^+ (Table III) and because of the Coulomb repulsion between Hi+\mathrm{H}_i^+ and SiGa+\mathrm{Si}_{\mathrm{Ga}}^+.

Venzie et al. [60] recently reported that exposure of Si-doped Ga2_2O3_3 to a hydrogen plasma led to passivation of the Si donor, as evidenced by a reduction in conductivity and an increase in mobility. The mobility increase indicates that the concentration of ionized-impurity centers is reduced, consistent with the formation of a complex (as opposed to mere compensation, where the compensating centers are spatially separated from the ionized donors). Venzie et al. [60] also proposed a geometry for the complex, which suggests that H binds to an O(I) neighbor of the Si donor; our calculations show that this configuration is 3.23 eV higher in energy than the stable geometry where H is bonded to two cations [see Figure 11(a)]. The configuration with cation-H bonds leads to vibrational frequencies significantly lower than the 3477.6 cm−1^{-1} attributed to the Si-H complexes[60], suggesting that these observed modes may be due to other types of complexes that form upon hydrogenation.

The formation energy of the SiGa(II)_{\mathrm{Ga(II)}}–H complex is higher, but otherwise its characteristics are very similar to those of the SiGa(I)_{\mathrm{Ga(I)}}–H complex. The (2+/0) level of SiGa(II)_{\mathrm{Ga(II)}}–H in Ga2_2O3_3 occurs at 0.35 eV below the CBM (compared to 0.41 eV for SiGa(I)_{\mathrm{Ga(I)}}–H), and the binding energy is 0.47 eV. The local geometry of (SiGa(II)−H)0(\mathrm{Si}_{\mathrm{Ga(II)}}-\mathrm{H})^0 is similar to that of (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^0, with a hydrogen binding to two nearby tetrahedral cation sites [see Figure 11(b)]. The H-Ga bond lengths are both 1.67 Å. This reinforces the argument that a (SiGa−H)0(\mathrm{Si}_{\mathrm{Ga}}-\mathrm{H})^{0} complex in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} is related to the Hi−\mathrm{H}_{i}^{-} point defect.

Similar complexes form in Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, as seen in Figure 10(c). The (2+/0)(2+/0) level of the (SiAl(I)−H)(\mathrm{Si}_{\mathrm{Al(I)}}-\mathrm{H}) complex occurs at EF=4.02E_{\mathrm{F}} = 4.02 eV (3.39 eV below the CBM), and the binding energy of the complex is Ebind[(SiAl(I)−H)0]=1.27E_{\mathrm{bind}}[(\mathrm{Si}_{\mathrm{Al(I)}}-\mathrm{H})^{0}]=1.27 eV. For SiAl(II)−H\mathrm{Si}_{\mathrm{Al(II)}}-\mathrm{H}, we find the (2+/0)(2+/0) transition level at 4.31 eV above the VBM (3.10 eV below the CBM), with a binding energy Ebind[(SiAl(I)−H)0]=0.71E_{\mathrm{bind}}[(\mathrm{Si}_{\mathrm{Al(I)}}-\mathrm{H})^{0}]=0.71 eV.

Based on our calculated numbers, we can assess whether complex formation with hydrogen has an impact on conductivity in Si-doped (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} alloys. We have found the neutral complex to be stable in both Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} for Fermi levels close to the CBM, and hence we expect the complex to also be stable in the alloys, with a binding energy that increases with increasing Al content. Indeed, the experiments of Venzie et al. [60] indicated that intentional hydrogenation can produce the complex in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}. However, as discussed above, the relatively modest binding energy indicates the complex will not be formed at the growth temperature. Complex formation would therefore need to occur during cool down. Since this requires bringing Hi\mathrm{H}_{i} close to a Si impurity in the positive charge state, the increasing stability of Hi−\mathrm{H}_{i}^{-} as the Al concentration increases makes complex formation more likely. If complex formation would indeed occur, annealing the sample would serve to dissociate the complex and activate the Si donor, as is well known for hydrogen-related complexes in other semiconductors [61].

SiO\mathrm{Si}_{\mathrm{O}} and SiO\mathrm{Si}_{\mathrm{O}}–H complexes

For completeness, we also investigated SiO\mathrm{Si}_{\mathrm{O}} and SiO\mathrm{Si}_{\mathrm{O}}–H complexes in both Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}. Formation energies are shown in the Supplemental Material (SM) [62]. SiO\mathrm{Si}_{\mathrm{O}} itself is stable in positive charge states when the Fermi level is low, but for Fermi levels close to the CBM SiO(I)\mathrm{Si}_{\mathrm{O(I)}} and SiO(III)\mathrm{Si}_{\mathrm{O(III)}} behave as compensating acceptors, while SiO(II)\mathrm{Si}_{\mathrm{O(II)}} is neutral. However, the formation energies are so large in nn-type material (even under the most favorable O-poor conditions) that they are unlikely to form or play a role in carrier compensation. SiO\mathrm{Si}_{\mathrm{O}}–H complexes also act as acceptors when EFE_{\mathrm{F}} is high in the gap, but again their formation energies are so large that they are unlikely to form.

Ccation\mathrm{C}_{\mathrm{cation}}–H complexes

Figures 12(a,b) show the formation energies of C–H complexes in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}. Similar to the SiGa(I)\mathrm{Si}_{\mathrm{Ga(I)}}–H in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3}, a (2+/0)(2+/0) charge-state transition level of CGa(I)\mathrm{C}_{\mathrm{Ga(I)}}–H occurs in the band gap, at 1.18 eV below the CBM, despite the fact that the individual impurities CGa(I)\mathrm{C}_{\mathrm{Ga(I)}} and Hi\mathrm{H}_{i} are single donors and occur in the positive charge state throughout the band gap. Following a similar definition as in Eq. (8), we can define a binding energy relative to CGa(I)+\mathrm{C}_{\mathrm{Ga(I)}}^{+} and Hi−\mathrm{H}_{i}^{-}, finding Ebind[(CGa(I)−H)0]=2.62E_{\mathrm{bind}}[(\mathrm{C}_{\mathrm{Ga(I)}}-\mathrm{H})^{0}]=2.62 eV. This much greater value of the binding energy and lower position of the (2+/0)(2+/0) transition level for the CGa(I)\mathrm{C}_{\mathrm{Ga(I)}}–H complex as compared to the SiGa(I)\mathrm{Si}_{\mathrm{Ga(I)}}–H complex indicates that a different type of bonding occurs. As pointed out in Sec. III D 1, (SiGa(I)−H)0(\mathrm{Si}_{\mathrm{Ga(I)}}-\mathrm{H})^{0} can be viewed as a combination of Si+\mathrm{Si}^{+} and H−\mathrm{H}^{-}, with the H atom bonding to two tetrahedral cation sites [Figure 11(a)]. In (CGa(I)−H)0(\mathrm{C}_{\mathrm{Ga(I)}}-\mathrm{H})^{0}, on the other hand, the H atom binds to C within the tetrahedral oxygen cage, forming a strong C–H bond with a bond length of 1.06 Å [Figure 11(c)]. The strength of this bond, which is related to the small atomic size of C, makes the C–H combination behave as a unit, similar to a nitrogen atom, and lowers the overall formation energy. For the CGa(I)\mathrm{C}_{\mathrm{Ga(I)}}–H complex, the 2+2+ charge state is actually thermodynamically stable, i.e., it is 0.24 eV lower in energy than the sum of the formation energies of CGa(I)+\mathrm{C}_{\mathrm{Ga(I)}}^{+} and Hi+\mathrm{H}_{i}^{+}. In the donor configuration of the CGa(I)\mathrm{C}_{\mathrm{Ga(I)}}–H complex, H is bonded to a neighboring oxygen atom within the tetrahedral oxygen cage instead of to C. This is also true for other donor (i.e., positively charged) configurations of the Ccation\mathrm{C}_{\mathrm{cation}}–H complex in both Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} and Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}.

Similar behavior is observed for CGa(II)\mathrm{C}_{\mathrm{Ga(II)}}–H: a (2+/0)(2+/0) transition level occurs at 2.25 eV below the CBM, and the binding energy of the neutral complex is 4.00 eV. In this case, the 2+2+ charge state is also thermodynamically stable, i.e., it is 1.13 eV lower in energy than the sum of the formation energies of CGa(II)+\mathrm{C}_{\mathrm{Ga(II)}}^{+} and Hi+\mathrm{H}_{i}^{+} [see Figure 12(a,Figure 12b)]. Again, a C–H bond with a bond length of 1.06 Å forms within the octahedral oxygen cage for (CGa(II)–H)0(\mathrm{C}_{\mathrm{Ga(II)}}\text{–}\mathrm{H})^{0} [see Figure 11(d)]. This C–H bond formation thus indicates a unique structural feature of the C–H complex regardless of which cation site C substitutes on.

Figure 12. Formation energy versus Fermi level for isolated Ccation impurities, H interstitials, and Ccation–H defect complexes in (a)-(b) β\beta-Ga2_2O3_3 and (c)-(d) θ\theta-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. The grey area indicates the conduction band of β\beta-Ga2_2O3_3.

Figure 12(a) shows that CGa\mathrm{C}_{\mathrm{Ga}}–H complexes are lower in energy than isolated CGa\mathrm{C}_{\mathrm{Ga}} impurities under nn-type doping conditions, and this is true over most of the range of Ga chemical potentials. In addition, because of their high binding energy, such complexes may well be present during growth. Measurements of carbon concentrations in MOCVD-grown samples, in which both carbon and hydrogen are likely to be unintentionally incorporated, may thus reflect the presence of such complexes rather than isolated CGa\mathrm{C}_{\mathrm{Ga}} donors. Since the complexes are neutral, they would not impact the conductivity of the sample. This implicit passivation of carbon impurities, which would otherwise act as shallow donors, may well explain why MOCVD-grown Ga2_2O3_3 samples can exhibit free-carrier concentrations as low as 101410^{14} cm−3^{-3} [32].

We now turn to CAl\mathrm{C}_{\mathrm{Al}}–H complexes in Al2_2O3_3. Figure 12(c,Figure 12d) show the formation energy of the complexes

in Al2_2O3_3 in Al-rich conditions. The type of bonding described for Ga2_2O3_3 is also present in Al2_2O3_3, but now we see that for EFE_{\mathrm{F}} high in the gap also a negative charge state can be stabilized, which indicates that the complex could potentially act as an acceptor and cause compensation. However, we note that the (0/−)(0/-) transition level of the complex occurs at a higher position in the band gap than the (+/−)(+/-) transition of the isolated CAl\mathrm{C}_{\mathrm{Al}}. The (0/−)(0/-) level of CAl(I)\mathrm{C}_{\mathrm{Al(I)}}–H occurs at 0.90 eV below the CBM, and a (−/2−)(-/2-) level is also present, at 0.13 eV below the CBM. Similarly, (0/−)(0/-) and (−/2−)(-/2-) levels of CAl(II)\mathrm{C}_{\mathrm{Al(II)}}–H are also observed close to the CBM, at 1.20 and 0.33 eV below the CBM. We note that the formation energy for CAl(II)\mathrm{C}_{\mathrm{Al(II)}}–H in monoclinic Al2_2O3_3 is similar to that in corundum Al2_2O3_3, except that the 1−1- charge state of CAl(II)\mathrm{C}_{\mathrm{Al(II)}}–H is absent in corundum [63]. The CAl(II)\mathrm{C}_{\mathrm{Al(II)}}–H bonding in monoclinic Al2_2O3_3 is also very similar to that in the corundum phase [63], implying that the C–H bonding within an octahedral O cage [as in Figure 11(d)] is a host-independent structural feature.

We verified that the CAl\mathrm{C}_{\mathrm{Al}}–H complexes are thermodynamically stable (i.e., have positive binding energies) in both the neutral and negative charge states. The only exception is (CAl(I)–H)2−(\mathrm{C}_{\mathrm{Al(I)}}\text{–}\mathrm{H})^{2-}, which has a negative binding energy. Formation of this complex is highly unlikely, anyway, since it would require the Fermi level to be within 0.13 eV of the CBM.

The stability of the Ccation–H complexes in the neutral and negative charge states in both Ga2_2O3_3 and Al2_2O3_3 implies they will also be stable in (Alx_xGa1−x_{1-x})2_2O3_3 alloys. The question is whether the behavior as a compensating acceptor that we find in Al2_2O3_3 can occur in (Alx_xGa1−x_{1-x})2_2O3_3 alloys. To assess this, we calculated the position of the (0/−)(0/-) transition level in Ga2_2O3_3 and combined this information with the results for the (0/−)(0/-) level in Al2_2O3_3. This allows us to conclude that the Ccation–H complexes can only occur in a negative charge state (i.e., act as acceptors) when the Al concentration exceeds 56% for C(I)\mathrm{C}_{\mathrm{(I)}}–H or 64% for C(II)\mathrm{C}_{\mathrm{(II)}}–H.

Co–H complexes

We discussed carbon on the oxygen site, CO\mathrm{C}_{\mathrm{O}}, in Sec. III B 5; now we turn to its complexes with hydrogen. As shown in Figure 13(a), Co–H has very low formation energy in Ga2_2O3_3, particularly when the Fermi level is high in the gap and under Ga-rich conditions. Regardless of the O site [O(I), O(II), O(III)] on which carbon is substituting, (+/0)(+/0) and (0/−)(0/-) charge-state transition levels are present in the band gap. We verified that higher negative charge states (such as 2−2-) are not stable for Fermi levels in the band gap. In all these complexes, hydrogen is always bonded to the C atom, with a bond length between 1.07 Å and 1.09 Å. Again, we note that the C–H unit behaves very similarly to an N impurity: Co–H and substitutional NO_{\mathrm{O}} have similar (+/0)(+/0) and (0/−)(0/-) transition levels in the gap, and both behave as acceptors in nn-type material [64].

Formation energy versus Fermi level for Co impurities, H interstitials, and Co–H defect complexes

Figure 13. Formation energy versus Fermi level for Co impurities, H interstitials, and Co–H defect complexes in (a)-(b) β\beta-Ga2_2O3_3 and (c)-(d) θ\theta-Al2_2O3_3. (a) and (c) are for cation-rich, and (b)-(d) for cation-poor conditions. Dashed lines denote thermodynamic instability of the defect complex, as explained in the text. The grey area indicates the conduction band of β\beta-Ga2_2O3_3.

The behavior of Co–H in Al2_2O3_3 is very similar: it also only exhibits (+/0) and (0/−) levels in the gap, and the complex has low formation energies under Al-rich conditions and when the Fermi level is high in the gap. The binding energies of the (Co–H)− complexes are all large in both Ga2_2O3_3 and Al2_2O3_3: all binding energies exceed 3 eV, with the exception of the (Co(III)–H)− complex, where the binding energy is 1.76 eV.

We propose that the Co–H complexes may have a distinct impact on MOCVD-grown Ga2_2O3_3. Seryogin et al. [33] grew Ga2_2O3_3 using a trimethylgallium (TMGa) precursor, which is known to potentially lead to increased C incorporation. They found that films grown with a lower O2_2/TMGa ratio were significantly more resistive and also contained significantly more carbon. These results indicate that carbon is behaving as a compensating acceptor. The authors of Ref. [33] pointed to a computational study [65] that had found CGa_\mathrm{Ga} to be a DXDX center in Ga2_2O3_3, with a (+/−) level 0.81 eV below the CBM. That result is very different from ours, probably due to the particulars of the band-gap correction used in Ref. [65]. In any case, if CGa_\mathrm{Ga} is the culprit, moving from O-rich to

O-poor conditions should reduce the CGa_\mathrm{Ga} incorporation, which is not consistent with the observed increase in C concentration. We think it is much more likely that CO_\mathrm{O} is involved, which indeed acts as a compensating acceptor with a concentration that should increase under O-poor conditions, as seen in Figure 6. However, that figure also shows that the formation energy of CO_\mathrm{O} in the negative charge state is still relatively high, even under the most favorable (extreme O-poor and C-rich) conditions. Figure 13 indicates that this energy can be lowered by complexing with hydrogen, which should of course also be abundantly available during MOCVD growth.

The involvement of Co–H complexes is also consistent with the experiments of Alema et al. [34], who found that adding H2_2O vapor to the oxygen source decreased the carrier concentration, both in unintentionally doped (UID) and lightly Si-doped samples. Hydrogen could either passivate donors or form compensating acceptors. Donor passivation may occur by forming complexes with the Si donor (though in Sec. III D 1 we noted this was not very likely) or with unintentional CGa_\mathrm{Ga} donors; for compensating acceptors, Co–H complexes are most likely, and indeed, Ref. [34] reported an increase in compensating acceptors rather than a decrease in donor concentration upon adding H2_2O.

Conclusions

We have reported a comprehensive investigation of silicon donors in (Alx_xGa1−x_{1-x})2_2O3_3 and the various ways in which they may be compensated. For Si in θ\theta-Al2_2O3_3 we performed a detailed study of DXDX center formation. Two stable DXDX SiAl(I)_\mathrm{Al(I)} configurations were identified, with the configuration involving bonding to two cations and no broken bonds being most energetically favorable. Interpolating the (+/−) charge-state transition levels between β\beta-Ga2_2O3_3 and θ\theta-Al2_2O3_3, we find that Si is an efficient donor over a wide range of Al concentrations in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, up to 70% Al.

We also investigated the behavior of carbon and hydrogen impurities, which are commonly unintentionally present, particularly in MOCVD. Even though these act as shallow donors in β\beta-Ga2_2O3_3, they become deep centers in (Alx_xGa1−x_{1-x})2_2O3_3 alloys. Based on interpolation of the (+/−) transition levels, we find that C(I) acts as a compensating acceptor already at 5% Al, and Hi_i already at 1% Al.

Additionally, complex formation between hydrogen and either Si or C may occur. We found that Sication_\mathrm{cation}–H complexes have relatively low binding energy; if they form, they can probably quite easily be removed by annealing. CGa_\mathrm{Ga}–H complexes are very stable and electrically neutral in nn-type Ga2_2O3_3, and may explain why unintentionally incorporated carbon does not affect the carrier concentration.[32] Ccation_\mathrm{cation}–H complexes do act as acceptors in (Alx_xGa1−x_{1-x})2_2O3_3 alloys, but only if the Al concentration exceeds 56%. Co–H, finally, was found to act as an acceptor over the entire range of alloy compositions, behaving very similarly to a NON_{\mathrm{O}} substitutional impurity and explaining experimental observations of carbon-related compensation in Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} grown by MOCVD [33, 34].

Our findings indicate that the presence of hydrogen or carbon may interfere with controlled low-level Si doping in (AlxGa1−x)2O3(\mathrm{Al}_{x}\mathrm{Ga}_{1-x})_{2}\mathrm{O}_{3} alloys, and our detailed results can be used to devise growth or processing conditions to avoid this.

Acknowledgments

The authors acknowledge Hongping Zhao for fruitful discussions and preliminary experimental results. S. M. is much indebted to Andrew J. E. Rowberg for stimulating discussions and valuable comments on the manuscript. The work was supported by the GAME MURI of the Air Force Office of Scientific Research (FA9550-18-1-0479). This work was partially performed under the auspices of the U.S. DOE by Lawrence Livermore National Laboratory (LLNL) under contract DE-AC52-07NA27344 and partially supported by LLNL Laboratory Directed Research and Development funding under project number 22-SI-003 and by the Critical Materials Institute, an Energy Innovation Hub funded by the U.S. DOE, Office of Energy Efficiency and Renewable Energy, Advanced Manufacturing Office. Work at NRL was supported by the Office of Naval Research through the Naval Research Laboratory’s Basic Research Program, and made use of DoD HPCMP resources. Use was made of computational facilities purchased with funds from the National Science Foundation (NSF) (CNS-1725797) and administered by the Center for Scientific Computing (CSC). The CSC is supported by the California NanoSystems Institute and the Materials Research Science and Engineering Center (MRSEC; NSF DMR 1720256) at UC Santa Barbara. This work also used the Extreme Science and Engineering Discovery Environment (XSEDE), which is supported by the National Science Foundation under Grant No. ACI-1548562, and the Frontera resources at the Texas Advanced Computing Center (TACC) at The University of Texas at Austin (NSF OAC-1818253).

References

  1. [1]H. Tippins, Phys. Rev. 140, A316 (1965).
  2. [2]T. Matsumoto, M. Aoki, A. Kinoshita, and T. Aono, Jpn. J. Appl. Phys 13, 1578 (1974).
  3. [3]C. Sturm, R. Schmidt-Grund, C. Kranert, J. Furthmüller, F. Bechstedt, and M. Grundmann, Phys. Rev. B 94, 035148 (2016).
  4. [4]A. Mock, R. Korlacki, C. Briley, V. Darakchieva, B. Monemar, Y. Kumagai, K. Goto, M. Higashiwaki, and M. Schubert, Phys. Rev. B 96, 245205 (2017).
  5. [5]M. Higashiwaki, K. Sasaki, A. Kuramata, T. Masui, and S. Yamakoshi, Appl. Phys. Lett. 100, 013504 (2012).
  6. [6]R. Suzuki, S. Nakagomi, Y. Kokubun, N. Arai, and S. Ohira, Appl. Phys. Lett. 94, 222102 (2009).
  7. [7]T. Oshima, T. Okuno, N. Arai, N. Suzuki, S. Ohira, and S. Fujita, Appl. Phys. Express 1, 011202 (2008).
  8. [8]F. Alema, B. Hertog, P. Mukhopadhyay, Y. Zhang, A. Mauze, A. Osinsky, W. Schoenfeld, J. S. Speck, and T. Vogt, APL Materials 7, 022527 (2019).
  9. [9]Z. Feng, A. F. M. Anhar Uddin Bhuiyan, M. R. Karim, and H. Zhao, Appl. Phys. Lett. 114, 250601 (2019).
  10. [10]Y. Zhang, F. Alema, A. Mauze, O. S. Koksaldi, R. Miller, A. Osinsky, and J. S. Speck, APL Materials 7, 22506 (2019).
  11. [11]N. Son, K. Goto, K. Nomura, Q. Thieu, R. Togashi, H. Murakami, Y. Kumagai, A. Kuramata, M. Higashiwaki, A. Koikitu, S. Yamakoshi, B. Monemar, and E. Janzen, J. Appl. Phys. 120, 235703 (2016).
  12. [12]A. Parisini and R. Fornari, Semicond. Sci. Technol. 31, 035023 (2016).
  13. [13]N. Ma, N. Tanen, A. Verma, Z. Guo, T. Luo, H. Xing, and D. Jena, Appl. Phys. Lett. 109, 212101 (2016).
  14. [14]M. Higashiwaki, A. Kuramata, H. Murakami, and Y. Kumagai, J. Phys. D 50, 333002 (2017).
  15. [15]N. Moser, J. McCandless, A. Crespo, K. Leedy, A. Green, A. Neal, S. Mou, E. Ahmadi, J. Speck, K. Chabak, N. Peixoto, and G. Jesse, IEEE Electron Device Lett. 38, 775 (2017).
  16. [16]T. A. Neal, S. Mou, S. Rafique, H. Zhao, E. Ahmadi, J. S. Speck, K. T. Stevens, J. D. Blevins, D. B. Thomson, N. Moser, and Others, Appl. Phys. Lett. 113, 62101 (2018).
  17. [17]M. Orita, H. Ohta, M. Hirano, and H. Hosono, Appl. Phys. Lett. 77, 4166 (2000).
  18. [18]T. Oishi, K. Harada, Y. Koga, and M. Kasu, Jpn. J. Appl. Phys. 55, 30305 (2016).
  19. [19]M. Higashiwaki, K. Sasaki, T. Kamimura, M. Hoi Wong, D. Krishnamurthy, A. Kuramata, T. Masui, and S. Yamakoshi, Appl. Phys. Lett. 103, 123511 (2013).
  20. [20]J. B. Varley, J. R. Weber, A. Janotti, and C. G. Van de Walle, Appl. Phys. Lett. 97, 142106 (2010).
  21. [21]J. B. Varley, A. Perron, V. Lordi, D. Wickramaratne, and J. L. Lyons, Appl. Phys. Lett. 116, 172104 (2020).
  22. [22]J. L. Lyons, D. Steiauf, A. Janotti, and C. G. Van de Walle, Phys. Rev. Appl. 2, 064005 (2014).
  23. [23]J. B. Varley, H. Peelaers, A. Janotti, and C. G. Van de Walle, J. Phys. Conden. Matter 23, 334212 (2011).
  24. [24]M. E. Engbertsen, A. Y. Kuznetsov, B. G. Svensson, G. Alfieri, A. Mihaila, U. Badstübner, A. Perron, L. Vines, and J. B. Varley, APL Mater. 7, 022510 (2019).
  25. [25]H. von Bardeleben and J. Cantin, J. Appl. Phys. 128, 125702 (2020).
  26. [26]D. Chadi and K.-J. Chang, Phys. Rev. Lett. 61, 873 (1988).
  27. [27]L. Gordon, J. L. Lyons, A. Janotti, and C. G. Van de Walle, Phys. Rev. B 89, 085204 (2014).
  28. [28]H. Peelaers, J. B. Varley, J. S. Speck, and C. G. Van de Walle, Appl. Phys. Lett. 112, 242101 (2018); Appl. Phys. Lett. 115, 159901 (2019). (erratum)
  29. [29]J. B. Varley, J. Mater. Res. 1 (2021).
  30. [30]Y. Zhang, C. Joishi, Z. Xia, M. Brenner, S. Lodha, and S. Rajan, Appl. Phys. Lett. 112, 233503 (2018).
  31. [31]H. P. Zhao, private communication.
  32. [32]F. Alema, Y. Zhang, A. Osinsky, N. Orischin, N. Valente, A. Mauze, and J. S. Speck, APL Materials 8, 021110 (2020).
  33. [33]G. Seryogin, F. Alema, N. Valente, H. Fu, E. Steinbrunner, A. T. Neal, S. Mou, A. Fine, and A. Osinsky, Appl. Phys. Lett. 117, 262101 (2020).
  34. [34]F. Alema, Y. Zhang, A. Mauze, T. Itoh, J. S. Speck, B. Hertog, and A. Osinsky, AIP Advances 10, 085002 (2020).
  35. [35]P. E. Blöchl, Phys. Rev. B 50, 17953 (1994).
  36. [36]G. Kresse and J. Hafner, Phys. Rev. B 48, 13115 (1993).
  37. [37]G. Kresse and J. Furthmüller, Phys. Rev. B 54, 11169 (1996).
  38. [38]K. Momma and F. Izumi, J. Appl. Crystallogr. 44, 1272 (2011).
  39. [39]J. Heyd, G. E. Scuseria, and M. Ernzerhof, J. Chem. Phys. 118, 8207 (2003); J. Heyd and G. E. Scuseria, J. Chem. Phys. 124, 219906 (2006).
  40. [40]R. Franchy, G. Schmitz, P. Gassmann, and F. Bartolucci, Appl. Phys. A 65, 551 (1997).
  41. [44]J. P. Perdew, K. Burke, and M. Ernzerhof, Phys. Rev. Lett. 77, 3865 (1996).
  42. [45]G. Henkelman, B. P. Uberuaga, and H. Jónsson, J. Chem. Phys. 113, 9901 (2000).
  43. [46]G. H. Vineyard, J. Phys. Chem. Solids 3, 121 (1957).
  44. [47]P. Weiser, M. Stavola, W. B. Fowler, Y. Qin, and S. Pearton, Appl. Phys. Lett. 112, 232104 (2018).
  45. [48]A. Janotti and C. G. Van de Walle, Phys. Rev. B 76, 165202 (2007).
  46. [49]C. Freysoldt, J. Neugebauer, and C. G. Van de Walle, Phys. Rev. Lett. 102, 016402 (2009).
  47. [50]C. Freysoldt, J. Neugebauer, and C. G. Van de Walle, Phys. Status Solidi B 248, 1067 (2011).
  48. [51]J. L. Lyons, A. Janotti, and C. G. Van de Walle, Phys. Rev. B 89, 035204 (2014).
  49. [52]J. L. Lyons and C. G. Van de Walle, npj Comput. Mater. 3, 1 (2017).
  50. [53]M. McCluskey, N. Johnson, C. G. Van de Walle, D. Bour, M. Kneissl, and W. Walukiewicz, Phys. Rev. Lett. 80, 4008 (1998).
  51. [54]C. Skierbiszewski, T. Suski, M. Leszczynski, M. Shin, M. Skowronski, M. Bremser, and R. Davis, Appl. Phys. lett. 74, 3833 (1999).
  52. [55]A. Bouzid and A. Pasquarello, Phys. Status Solidi RRL 13, 1800633 (2019).
  53. [56]M. Choi, J. L. Lyons, A. Janotti, and C. G. Van de Walle, Appl. Phys. Lett. 102, 142902 (2013).
  54. [58]S. Mu, H. Peelaers, Y. Zhang, M. Wang, and C. G. Van de Walle, Appl. Phys. Lett. 117, 252104 (2020).
  55. [60]A. Venzie, A. Portoff, C. Fares, M. Stavola, W. B. Fowler, F. Ren, and S. J. Pearton, Appl. Phys. Lett. 119, 062109 (2021).
  56. [61]C. G. Van de Walle and J. Neugebauer, Annu. Rev. Mater. Res. 36, 179 (2006).
  57. [62]See Supplemental Material at [URL will be inserted by publisher] for the formation energy of SiO and Si–H complexes in Ga₂O₃ and Al₂O₃.
  58. [63]M. Choi, A. Janotti, and C. G. Van de Walle, ACS Appl. Mater. Interfaces 6, 4149 (2014).
  59. [64]H. Peelaers, J. L. Lyons, J. B. Varley, and C. G. Van de Walle, APL Mater. 7, 022519 (2019).
  60. [65]S. Lany, APL Mater. 6, 046103 (2018).

Paper details

vlnc:W_bqde5u5v
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents