Magnetic Switching in Monolayer 2D Diluted Magnetic Semiconductors via Spin-to- Spin Conversion

Abstract

The integration of two-dimensional (2D) van der Waals (vdW) magnets with topological insulators or heavy metals holds great potential for realizing next-generation spintronic memory devices. However, achieving high-efficiency SOT switching of monolayer vdW magnets at room temperature poses a significant challenge, particularly without an external magnetic field. Here, we show field-free, deterministic, and nonvolatile SOT switching of perpendicular magnetization in the monolayer, diluted magnetic semiconductor (DMS), Fe-doped MoS2(Fe:MoS2) at up to 380 K with a current density of 7×104Acm−27\times10^4 A cm^{-2}. The in situ doping of Fe into monolayer MoS2 via chemical vapor deposition and the geometry-induced strain in the crystal break the rotational switching symmetry in Fe:MoS2, promoting field-free SOT switching by generating out-of-plane spins via spin-to-spin conversion. An apparent anomalous Hall effect (AHE) loop shift at a zero in-plane magnetic field verifies the existence of z spins in Fe:MoS2, inducing an antidamping-like torque that facilitates field-free SOT switching. A strong topological Hall effect (THE) was also observed, attributed to the interfacial Dzyaloshinskii-Moriya interaction (DMI), reducing the energy barrier for SOT switching. This field-free SOT application using a 2D ferromagnetic monolayer provides a new pathway for developing highly power-efficient spintronic memory devices.

Introduction

Two-dimensional (2D) van der Waals (vdW) magnets have emerged as promising contenders in spintronics, primarily owing to their heightened spin transparency and spin injection efficiency, which results from the absence of dangling bonds and decreased atom intermixing near the interface at the heterostructure surface.[1–5] The spintronics of 2D vdW magnets are particularly beneficial because of their strong perpendicular magnetic anisotropy (PMA),[6–11] paving the way toward versatile manipulation of magnetic ordering via current-induced spin-orbit torque (SOT). SOT switching involves applying a current pulse that induces torque on the magnetization of materials through spin–orbit interactions, efficiently altering the magnetic states of magnetic layers.[12] The spin-orbit interaction is facilitated by integrating 2D magnets with materials exhibiting robust spin-orbit coupling (SOC), such as topological insulators (e.g., WTe2_2, Bi2_2Te3_3) or heavy metals (e.g., W, Ta, Pt).[8,13–15] The synergy between these materials and vdW magnets may significantly enhance the SOT efficiency, attributed to the inherently low magnetic damping in vdW magnets.[8,16,17]

To achieve high efficiency in SOT switching, it is crucial to select high spin transparency materials and minimize the thickness of the magnetic layer to reduce magnetic damping and saturation magnetization.[20] [18, 19] Recently, the use of thin BaPb1−x_{1-x}Bix_xO3_3 and Fe3_3GaTe2_2 heterostructures showed 'field-assisted' SOT switching with current densities on the order of 3×1063 \times10^{6} A cm−2^{-2} at 300 K,[21] [13] with the application of in-plane magnetic fields. However, the ability to achieve SOT switching without an external magnetic field is essential for practical applications. To achieve field-free SOT switching, approaches such as lateral asymmetry,[22] in-plane exchange bias fields,[23] interlayer exchange coupling[24] and interfacial Dzyaloshinskii-Moriya interaction (DMI)-induced symmetry breaking[25] have been explored. A major advancement was reported using the low-crystal-symmetric material WTe2_2 combined with room temperature vdW magnets, where an unconventional out-of-plane anti-damping torque facilitates field-free switching.[26] [11] Field-free SOT switching with WTe2_2/PtTe2_2/CoFeB and WTe2_2/Fe3_3GaTe2_2 devices was achieved at a current density of 2.25×1062.25 \times10^{6} A cm−2^{-2} at 300 K[11] and 2.23×1062.23 \times10^{6} A cm−2^{-2} at 320 K,[10] respectively, while the Curie temperature of Fe3_3GaTe2_2 was 330 K. These vdW magnets (e.g., CrTe2_2, Fe3_3GeTe2_2 and Fe3_3GaTe2_2) are synthesized via flux crystal growth[27, 28] [7] or molecular beam epitaxy,[19] often followed by mechanical exfoliation in a glove box.

Furthermore, thinning these 2D magnets may enhance the system's energy efficiency, as entire magnetic layers interact closely with the spin-accumulated interface[29] [17] and contribute to lowering the energy barrier for magnetization switching by reducing the saturation magnetization.[9,19] However, the Curie temperatures of CrTe2_2 and Fe3_3GaTe2_2 drop to 224 K and 200 K, respectively, when reduced to monolayer thicknesses.[27, 30] Furthermore, the surface of these materials is quickly oxidized when exposed to air,[31, 32] [19] which alters the material's electronic structure and introduces defects and structural irregularities, impairing its performance.[27, 31, 32] [19] This thickness limitation presents a significant challenge for low-current-density, field-free SOT switching. Conversely, substitutional doping of monolayer transition metal dichalcogenides (TMDs), including MoS2_2 and WSe2_2, synthesized via chemical vapor deposition (CVD), thus providing ultimate scalability,[33, 34, 35, 36] enables the formation of 2D diluted magnetic semiconductors (DMS).[37, 38, 39] These DMSs exhibit ferromagnetic properties above room temperature, even at monolayer thicknesses,[37, 38, 39] which makes them ideal candidates for SOT materials at the true 2D limit (i.e., atomically thin monolayers).

Here, we show an ultralow current-density, field-free, deterministic SOT switching of perpendicular magnetization in a CVD-grown, monolayer Fe:MoS2_2 transferred onto a Pt Hall bar. We demonstrate the PMA in Fe:MoS2_2 by measuring the anomalous Hall effect (AHE) in Fe:MoS2_2/Pt heterostructure up to 380 K. We also show that field-free, perpendicular magnetization switching by SOT occurs only when the current flows along the zigzag direction of Fe:MoS2_2 due to strain-induced crystal asymmetry. We demonstrate that the rotational symmetry breaking in Fe:MoS2_2, promoting field-free SOT switching by generating out-of-plane spins via spin-to-spin conversion. To further explore the origins of field-free and low-current-density SOT switching, we characterize the current-induced AHE loop shift and the temperature-dependent topological Hall effect (THE).

Results and Discussion

Materials and device characterization

Monolayer Fe:MoS2_2 was grown via chemical vapor deposition (CVD) (Figure S1). The detailed synthesis and magnetic characterization processes, which showed that the material was a room-temperature DMS, are described elsewhere.[37, 39] A schematic of the crystal structure of monolayer Fe:MoS2_2 is shown in Figure 1A (left), illustrating that Fe atoms substitute for Mo sites within the lattice. The field-free SOT switching of perpendicular magnetization can be facilitated by utilizing low-symmetry crystals with, at most, one mirror symmetry.[7,10,11,40,41] While pristine MoS2_2 exhibits threefold rotational symmetry, the uniaxial strain applied along the y- or x-axis disrupts the rotational symmetry in the hexagonal lattice,[42,43] retaining only the y-z mirror plane symmetry, σv\sigma_{\mathrm{v}} (yz) (z represents the out-of-plane axis), as shown in Figure 1A. The step height of the Pt film, as illustrated in Figure S2A, induces uniaxial strain (ε\varepsilon) in the monolayer Fe:MoS2_2 perpendicular to the edge of the Pt Hall bar.[44–47] Optical images of a typical Fe:MoS2_2/Pt heterostructure are shown in Figure S2B,C.

Crystal characterization: optical and Hall resistance measurements

Figure 1. Crystal characterization: optical and Hall resistance measurements. (A) Schematic illustration of the distorted lattice structure of monolayer Fe:MoS2_2 under armchair strain. The vertical dashed line denotes the preserved mirror symmetry in the y-z plane σv\sigma_{\mathrm{v}} (yz) under armchair strain. (B) Schematic and optical images of monolayer Fe:MoS2_2 transferred on a Pt Hall bar. The strain direction is marked as ε\boldsymbol{\varepsilon}. The optical image presents a fabricated device with a current flow direction, JwJ_w, along the zigzag axis (determined through the edge of the crystal triangle), where the white arrow indicates the laser spot. (C) Polarized Raman spectra of the strained Fe:MoS2_2 on a Pt electrode. (D) Polar plots of the E2g1E_{2g}^{1} and A1gA_{1g} modes shown as a function of the angle between the polarizations of the incident and the scattered light. (E) Prototypical AHE response in the Fe:MoSe2_2/Pt heterostructure for field sweep out of the sample plane (H∥z\mathrm{H} \parallel z) at room temperature. (F) Variation in coercivity (HcH_{\mathrm{c}}) obtained from AHE plots as a function of temperature.

Characterization of CVD-grown monolayer Fe:MoS2

Figure S1. Characterization of CVD-grown monolayer Fe:MoS2_2. (A) Optical image of CVD-grown Fe:MoS2_2 monolayers. (B and C) Atomic force microscopy (AFM) image confirming the monolayer thickness of Fe:MoS2_2. (D and E) High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) characterizing the Fe doping. (F) Intensity spectra from the selected area shown in (e) indicating that the Fe atom exhibits a 40% lower intensity than Mo.

Typical Fe:MoS2/Pt heterostructure

Figure S2. Typical Fe:MoS2_2/Pt heterostructure. (A) Cross-sectional schematic of the Fe:MoS2_2/Pt geometry, inducing a uniaxial strain in Fe:MoS2_2 perpendicular to the Pt Hall bar edge. (Not to scale) (B) Optical image of a typical sample, showing a 20 nm-thick hBN atop Fe:MoS2_2/Pt heterostructure. (C) Zoom-in view of the area indicated by the black dashed square in (B).

To determine the lattice orientation of Fe:MoS2_2, thus controlling the strain direction, we utilized the edge morphology of triangular island single crystals,[48] as shown in Figure 1B and Figure S3, with layers of Pt and FeMoS2_2 marked. Figure 1A (right) shows a schematic representation of the strained Fe:MoS2_2 lattice structure along the armchair and zigzag directions, effectively modulating the crystal symmetry. Previous studies have shown that, in monolayer MoS2_2, covalent bonding between Mo and S is very sensitive to in-plane uniaxial strain due to the strain-induced change in the coupling between the Mo atom dd orbital and S atom pp orbital, which can be probed using angle-resolved polarized Raman spectroscopy. For MoS2_2, in the absence of strain, the E2g1E^{1}_{2g} mode intensities show negligible change.[42,43] This trend persists in monolayer Fe:MoS2_2 transferred onto a flat SiO2_2 surface, for which the E2g1E^{1}_{2g} mode intensity difference is less than 5% (Figure S4B). To confirm the alteration in crystal symmetry, we analyzed the angle-resolved polarized Raman spectra of monolayer Fe:MoS2_2 transferred onto a Pt Hall bar. The polar Raman laser spot is indicated with the white arrow in Figure 1B. Figure 1C, Figure S4 and Figure S4 present their contour maps, where two dominant peaks at 384 cm−1^{-1} and 403 cm−1^{-1}, corresponding to the E2g1E^{1}_{2g} and A1gA_{1g} modes, respectively, exhibit representative twofold symmetry.[42,49] The corresponding polar plots of the E2g1E^{1}_{2g} and A1gA_{1g} intensities are depicted in Figure 1D. Our fitting results distinctly demonstrate the polar behavior of the E2g1E^{1}_{2g} mode, with a notable 50% intensity variation between 0 and 90 degrees. The distinct polarity of the E2g1E^{1}_{2g} peak confirms the occurrence of uniaxial strain, which in turn modulates the crystal symmetry of Fe:MoS2_2. This symmetry alteration is known to promote field-free SOT switching by generating out-of-plane spin accumulation when current is injected along the zigzag axis (x-axis) at the Fe:MoS2_2/Pt interface, similar to the field-free SOT switching of Fe3_3GaTe2_2 using WTe2_2.[7,10]

Fe:MoS2 crystals with different angles relative to the Pt Hall bar

Figure S3. Fe:MoS2_2 crystals with different angles relative to the Pt Hall bar. (A and B) Schematic of Fe:MoS2_2 lattices with uniaxial strain directions altering the crystal symmetry. Under both configurations, the mirror symmetry is maintained along the armchair direction of the crystal. (C and D) Optical images of Fe:MoS2_2 crystals transferred on the Pt Hall bar, showing current flows parallel to the zigzag (C) and armchair (D) directions, respectively.

Polarized Raman and photoluminescence spectra of monolayer Fe:MoS2 and MoS2 on SiO2

Figure S4. Polarized Raman and photoluminescence spectra of monolayer Fe:MoS2_2 and MoS2_2 on SiO2_2. (A and B) Polarized Raman spectra revealing that the E2g1E_{2g}^{1} mode, at approximately 383 cm−1383\ \mathrm{cm}^{-1}, exhibits no polarization from both monolayer Fe:MoS2_2 and MoS2_2 on SiO2_2. This suggests that Fe doping does not alter the crystal symmetry. (C) Photoluminescence (PL) spectra of Fe:MoS2_2 and MoS2_2 on SiO2_2, respectively, illustrating a redshift and quenching effect due to Fe doping.

Figure 1E depicts a hysteresis loop measurement of the Hall resistance (RHR_H) using a Fe:MoS2_2/Pt heterostructure at 300 K. In general, the Hall resistance is expressed by

RH=R0H+RSM+RTHE(1)R_H = R_0H + R_SM + R_{THE} \tag*{(1)}

where R0HR_0H, RSMR_SM and RTHER_{THE} denote the ordinary Hall effect (OHE), AHE and THE, respectively. When a magnetic field is applied along the out-of-plane direction (z-axis), the transverse resistance (RHR_H) exhibits sharp antisymmetric humps superimposed on a step function. The linear background with a weak positive slope at large fields arises from the OHE (R0HR_0H). The change in RHR_H near ±0.25\pm0.25 T can be explained by the AHE (RSMR_SM) signal, which can be approximated by a step function,[50,51] signifying excellent PMA even at room temperature.[27, 30] Notably, this robust PMA arises from a monolayer of vdW material with a thickness of 0.8 nm—a highly desirable feature for applications in high-density magnetic memory.[20, 36] [18] The distinct antisymmetric humps close to 0 T in the Hall resistance shown in Figure 1E closely resemble those identified as THE (RTHER_{THE}) in various ferromagnetic systems (discussed in Figure 4). Figure 1F shows a heterostructure with a large coercivity (HCH_C) of 3 kOe at 4 K, which monotonically decreases to 1.8 kOe at 300 K owing to the increasing thermal fluctuations in Fe:MoS2_2.

Topological Hall effect in the Fe:MoS2/Pt heterostructure

Figure 4. Topological Hall effect (THE) in the Fe:MoS2_2/Pt heterostructure. (A) Measured AHE loops from 4 K to 300 K. (B) Hall resistance after subtracting the ordinary Hall effect. The red curve was further decomposed into two channels (RH1R_{\mathrm{H1}} and RH2R_{\mathrm{H2}}), with each channel exhibiting humps near the magnetic domain reversal. The blue arrows indicate “hump a” near ±2\pm2~2.5 kOe, observed before the domain reversal at ±3\pm3 kOe, while the green arrows mark “hump b” near ±0.5\pm0.5 kOe. (C) Plot of the temperature and applied field of the deduced hump responses. The white arrows indicate the direction of the field scanning. (D) Temperature dependence of the signals from RH1R_{\mathrm{H1}}. With Anomalous Hall resistivity from RH1R_{\mathrm{H1}} (red triangle) and topological Hall resistivity (red circle). The positions of “hump a” maximum HTH_T are shown in blue.

Field-free, deterministic SOT switching via spin-to-spin conversion

Figure 2A illustrates the proposed SOT-driven magnetic switching mechanism within the Fe:MoS2_2/Pt heterostructure, where the SOC and low symmetry facilitate a spin-to-spin conversion to enable perpendicular magnetization switching.[11] For the conventional field-free SOT switching of perpendicularly magnetized layers, the generation of the essential z-polarized spins is typically achieved through charge-to-spin conversion when a charge current flows through materials with low symmetry.[7,10,52] However, in our Fe:MoS2_2/Pt heterostructure, the charge current mainly flows within the Pt layer due to the high resistance of Fe:MoS2_2 (Figure S5), thereby allowing for the generation of y-polarized spins only via the spin Hall effect (SHE). Thus, the generation of z-polarized spins needs to be facilitated by additional spin-to-spin conversions (i.e., y-polarized to z-polarized spins; see Supplementary Note 1). The linear response theory[11] predicts the conversion of an external spin current Js,jkJ^{k}_{s,j} into spin accumulation Si\mathbf{S}_{i}, which is encapsulated by the equation Si=ηi,jkJs,jk\mathbf{S}_{i}=\eta^{k}_{i,j}J^{k}_{s,j}. Here, ηi,jk\eta^{k}_{i,j} is the response tensor connecting Si\mathbf{S}_{i} and Js,jkJ^{k}_{s,j}, where (i,j,k)(i,j,k) are the Cartesian coordinates (x,y,z)(x,y,z). Specifically, ii indicates the direction of the generated spin density, jj denotes the direction of the spin current, and kk signifies the spin polarization direction.

Field-free spin-orbit-torque switching

Figure 2. Field-free spin-orbit-torque (SOT) switching. (A) Schematic illustration of the scenario in which a pulsed current is injected along the low-symmetry axis (x-axis) in the Fe:MoS2_2/Pt heterostructure. (B to D) Field-free SOT switching of Fe:MoS2_2/Pt at different temperatures up to 380 K. For clarity, the RHR_H data are normalized and offset along the y-axis. (E) Comparison of the critical current density, JcJ_c, and operation temperature for the reported SOT switching materials (Fe3_3GeTe2_2,[6,7,53–55] Fe3_3GaTe2_2,[8,10,13] CrTe2_2,[30] [56] Cr2_2Ge2_2Te6_6,[57–59] TaIrTe4_4,[26] and non vdWs[21, 23, 24, 63] [11, 60, 61, 62]).

In accordance with the Neumann principle,[41] pristine MoS2_2, which maintains inversion and mirror symmetry across three planes, would exhibit zero values for the response tensor components ηi,jk\eta^{k}_{i,j}. However, the introduction of uniaxial strain along the armchair direction (y-direction) and Fe doping breaks the inversion symmetry, in addition to decreasing the symmetry with respect to the plane σ0\sigma_{0} (xy) at the Fe:MoS2_2/Pt interface, leaving only the mirror symmetry with respect to the plane σv\sigma_{v} (yz) intact. This symmetry breaking allows a nonzero value of ηz,zy\eta^{y}_{z,z}, which results in the conversion of the y-polarized spin current Js,zyJ^{y}_{s,z} generated in the Pt layer into the z-polarized spin density Sz\mathbf{S}_{z} (Figure 2A, green arrow) at the Fe:MoS2_2/Pt interface. Assisted by this interfacial spin-to-spin conversion, an anti-damping torque τADOOP\tau^{OOP}_{AD} is present in our system. This unconventional, symmetry-breaking, anti-damping torque τADOOP\tau^{OOP}_{AD} is analogous to phenomena observed in other low-symmetry vdW materials, such as WTe2_2 and TaIrTe4_4.[26] [7, 40] The torque can be expressed as τADOOP∝m^×z^×m^\tau^{OOP}_{AD} \propto\hat{\mathbf{m}} \times\hat{\mathbf{z}} \times\hat{\mathbf{m}}, where m^\hat{\mathbf{m}} and z^\hat{\mathbf{z}} are unit vectors along the magnetization of Fe:MoS2_2 and perpendicular to the interface, respectively. This torque is antisymmetric with respect to the charge current flow, JwJ_{w}, facilitating highly efficient SOT-driven reversible magnetization switching by altering the JwJ_{w} direction.

To investigate current-induced SOT switching, current pulses were applied in the x-direction of the Fe:MoS2_2/Pt Hall bar (see Methods). As shown in Figure 2B, the magnetic state of Fe:MoS2_2 was toggled between the z+ and z-directions without needing an external magnetic field at a notably low critical current density of Jc=7×104J_{c}=7 \times10^{4} A cm−2^{-2} at 380 K. This current density corresponds to a power dissipation density of Psw=7.5×1012P_{sw}=7.5 \times10^{12} W m−3^{-3} (i.e., Psw=Jc2ρP_{sw}=J_{c}^{2}\rho, where ρ\rho is the resistivity of the device), which is four orders of magnitude lower than reported vdW SOT materials and three orders of magnitude lower than non-vdW SOT materials.[22] [8, 10, 11, 15]

As depicted in Figure 2B-Figure 2D, the current density required for SOT switching decreased as the temperature increased from 200 K to 380 K. This trend correlated with the diminishing coercive field (HcH_c), indicative of a reduction in effective anisotropy and the energy barrier necessary for switching,[7] as evidenced by the HcH_c trends summarized in Figure S6. Figure 2E and Table S1 summarize the comparison chart and table of the critical current density and operation temperatures in the reported SOT switching materials. This inverse relationship between temperature and current density has also been observed in various SOT devices constructed from 2D vdW materials, including Fe3_3GeTe2_2, Fe3_3GaTe2_2 and CrTe2_2.[6,7,19] Additional evidence supporting the reduction in the effective anisotropy and the energy barrier at elevated temperatures is a sharp transition between the -z and +z magnetic states of Fe:MoS2_2, as depicted in Figure 2C, 2D and S7.

Temperature-dependent critical current density for SOT switching

Figure S6. Temperature-dependent critical current density for SOT Switching. The critical current density decreases as temperature increases, owing to the reduced energy barrier for switching at elevated temperatures.

MaterialsMaximum temperature of SOT switching (K)Switching current density (10610^{6} A cm−2^{-2})HXH_{\mathrm{X}} (Oe)
Py/TaIrTe4_4 [26]30076.50 (Field Free)
L10_{10}-Fe45_{45}Cr5_5Pt50_{50} [24]300270 (Field Free)
CuPt/CoPt [23]30024.70 (Field Free)
[Pt0.6_{0.6}/Hf0.2_{0.2}]6_6/CoFeB [62]3003.60 (Field Free)
BPBO/LSMO [21]3000.4100
Ta/CoFeB [61]3000.41000
W/CoFeB [63]3000.31
Pt/CoFeB [60]3000.34
vdW magnets(Bi1−x_{1-x}Sbx_x)2_2/Cr2_2Ge2_2Te6_6 [59]251000
vdW magnetsCr2_2Ge2_2Te6_6/Ta [58]40.21000
vdW magnetsCr2_2Ge2_2Te6_6/Ta [57]100.5200
vdW magnetsCrTe2_2/ZrTe2_2 [30]5018200
vdW magnetsFe3_3GeTe2_2/Pt [54]180253000
vdW magnetsWTe2_2/Fe3_3GeTe2_2 [55]2003.9300
vdW magnetsWTe2_2/Fe3_3GeTe2_2 [7]2002.50 (Field Free)
vdW magnetsFe3_3GaTe2_2/Pt [13]3005.23000
vdW magnetsFe3_3GaTe2_2/Pt [8]3004.70 (Field Free)
vdW magnetsWTe2_2/PtTe2_2/CoFeB [11]3002.250 (Field Free)
vdW magnetsBi2_2Te3_3/Fe3_3GeTe [6]3002.22000
vdW magnetsWTe2_2/Fe3_3GaTe2_2 [10]3202.230 (Field Free)
vdW magnetsFe:MoS2_2/Pt (Our work)3800.0750 (Field Free)

Table S1. Comparison of SOT current density and operating temperature

Crystal symmetry breaking-induced out-of-plane anti-damping torque

We measured the field-free switching of the perpendicular magnetization of Fe:MoS2_2 by applying a writing current, JwJ_\mathrm{w}, along two different axes at 300 K and explored the occurrence of an out-of-plane anti-damping torque τADOOP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{OOP}}. Monolayers of Fe:MoS2_2 were positioned at two different angles against the Pt Hall bar, as depicted in the inset of Figure 3A (Figure 3B), to induce uniaxial strain along the zigzag (armchair) axis while retaining the mirror symmetry along the y-axis. The JwJ_\mathrm{w} direction was set to the y-axis (armchair direction) or the x-axis (zigzag direction). As depicted in Figure 3A, the magnetization state of Fe:MoS2_2 was first initialized to mz=+1m_\mathrm{z}=+1 (with Hz=+0.32H_\mathrm{z}=+0.32 T); then, JwJ_\mathrm{w} was applied parallel to the y-axis (Jw∥yJ_\mathrm{w}\parallel y), under which it switched to a state with near-zero Hall resistance (mzm_\mathrm{z}, RH≈0R_\mathrm{H}\approx0). For both pulse sweeping directions starting from mz=+1m_\mathrm{z}=+1 (represented by the red and blue data points), this mz≈0m_\mathrm{z}\approx0 state cannot be switched back to mz=+1m_\mathrm{z}=+1 by reversing the current direction. This switching behavior is attributed to either demagnetization of Fe:MoS2_2 by Joule heating or switching of the magnetization direction to the in-plane direction (x-direction) by the in-plane torque τADIP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{IP}}. This behavior is analogous to the demagnetized state observed in conventional bilayer heavy metal (HM)/FM SOT[12] and in the WTe2_2/Fe3_3GaTe2_2 systems,[7,10] where the current was applied along the high symmetry axis.

Crystal symmetry breaking in the SOT system

Figure 3. Crystal symmetry breaking in the SOT system. (A) Room-temperature SOT measurements when the applied current is parallel to the y-axis (armchair direction) of the Fe:MoS2_2 lattice. The red (and blue) curves correspond to current pulses swept from Jw=0→120×106J_{\mathrm{w}}=0 \rightarrow120 \times10^{6} A cm−2→−120×106^{-2} \rightarrow-120 \times10^{6} A cm−2→0^{-2} \rightarrow0 (0→−120×1060 \rightarrow-120 \times10^{6} A cm−2→120×106^{-2} \rightarrow120 \times10^{6} A cm−2→0^{-2} \rightarrow0). Switching from mz=+1m_z=+1 to mz=0m_z=0 was observed for both directions, but the change did not reverse back to mz=+1m_z=+1 because the Fe:MoS2_2 magnetization changed to the in-plane direction (xy plane). (B) Room-temperature SOT measurements when the applied current is parallel to the x-axis (zigzag direction) of the Fe:MoS2_2 lattice. (C) Switching of out-of-plane Fe:MoS2_2 magnetization upon current pulses (1 ms pulse duration) at room temperature. (D) Current-induced AHE loop shift owing to out-of-plane switching τADOOP\tau_{\mathrm{AD}}^{\mathrm{OOP}}. The AHE hysteresis loops were measured by applying HZH_Z at pulsed currents of 8 mA (red) and −8-8 mA (black). (E) AHE loop shift field (HSHH_{\mathrm{SH}}) as a function of the charge current amplitude ∣Jp∣\lvert J_p\rvert for both positive and negative charge currents applied along the x-axis. (inset of a, b: Schematics of the Fe:MoS2_2 single crystal (blue), the Hall bar (yellow), and the strained crystal lattices.)

In contrast, when a current was applied along the low-symmetry axis, as shown in Figure 3B, τADOOP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{OOP}} was generated, allowing the magnetization of Fe:MoS2_2 to be toggled between mz≈±0.8m_\mathrm{z}\approx\pm0.8 upon reversing the current direction. This is consistent with magnetic switching by τADOOP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{OOP}}, in which the magnetization direction can be reversed with a change in the writing current direction. The current density in this scenario was approximately one-tenth of the demagnetizing current density needed for Jw∥yJ_\mathrm{w}\parallel y. Figure 3C shows the applied current pulses (1 ms pulse duration), enabling the switching of out-of-plane Fe:MoS2_2 magnetization at room temperature.

The presence of τADOOP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{OOP}} in low-symmetry systems, including WTe2_2/FM and TaIrTe4_4/FM, was previously determined using spin-torque ferromagnetic resonance (STFMR).[26] [40] It has been established that τADOOP\boldsymbol{\tau}_{\mathrm{AD}}^{\mathrm{OOP}} is not necessarily dependent on the direction of magnetization in ferromagnets but rather on the direction of the writing current JwJ_\mathrm{w}.[7,10,40] This characteristic implies that the out-of-plane magnetization (mzm_\mathrm{z}) can be effectively modulated by applying a charge current along the x-axis, resulting in a shift in the AHE hysteresis loop. As demonstrated in Figure 3D, the AHE loop shift (HSHH_\mathrm{SH}) measured under current pulses shows a notable loop shift toward the positive direction when Ix=+8I_\mathrm{x}=+8 mA, in contrast to Ix=−8I_\mathrm{x}=-8 mA (see Methods). When repeating the measurements at different charge current magnitudes for Jw∥xJ_\mathrm{w}\parallel x, no significant HSHH_{\mathrm{SH}} was observed for current magnitudes smaller than 5 mA (Figure 3E and Figure S8). This is anticipated, as HSHH_{\mathrm{SH}} is only noticeable when τADOOP\tau_{\mathrm{AD}}^{\mathrm{OOP}} compensates for the intrinsic damping torques.1 The asymmetry observed in the positive and negative HSHH_{\mathrm{SH}} is likely due to the unevenness of the crystal shape (i.e., triangular shape) against the x-axis.[26] [7]

AHE loop and field-free SOT at 4 K

Figure S8. AHE loop and field-free SOT at 4 K (A to D) Depiction of the AHE loop at 4 K with pulsed currents under the external magnetic field (HH) perpendicular to the sample plane. The pulse duration was 10 ms with the current amplitude ranging from 0.22 mA to 5 mA. The Hall resistance is normalized as MZ=R/RAHEM_Z = R/R_{AHE}. (E) The amplitude of THE signal (MTHE=RTHE/RAHEM_{THE} = R_{THE}/R_{AHE}) decreases monotonically with increasing ∣JP∣\lvert J_P\rvert. (F) Field-free SOT switching at 4 K.

Field- and temperature-dependence of THE

Figure 4A shows the temperature dependence of the Hall resistance obtained by sweeping the magnetic field. The antisymmetric humps observed near zero in the Hall resistance were preserved from 4 K to 300 K without a significant shape change. The humps are similar to those reported for THE in a range of ferromagnetic systems, which possess ferromagnetic order arising from intrinsic origins or doping.[64] [51] A recurring observation in the literature is that the hump location typically coincides with the AHE domain reversal, which can be attributed to either THE[64, 65, 66] [50, 51] or two-channel AHE.[67, 68] Accordingly, we further decomposed the Hall signal (red curve) into two channels with humps near the domain reversal. As shown in Figure 4.B, RH1R_{\mathrm{H1}} (blue dashed line) presents a Hall loop with domain reversal near ‘hump a’ at ±2.5\pm2.5 kOe, while the remaining Hall signal, RH2R_{\mathrm{H2}} (black dashed curve), shows a Hall loop with domain reversal near ‘hump b’ at ±0.5\pm0.5 kOe.

THE signal is known to be closely related to the Dzyaloshinskii-Moriya interaction (DMI)-induced magnetic skyrmions, where moving spin-polarized electrons acquire the skyrmion-induced Berry phase by adjusting their spins to the local spins of the skyrmion texture, giving rise to the observed humps.[69] The presence of an appropriate DMI intensity (DD) within an FM/HM system is known to be crucial in facilitating field-free SOT magnetization switching.[25, 70] This switching process is initiated by domain nucleation at one edge of the FM, followed by domain wall propagation toward the opposite edge, as proposed by other FM/Pt-based examples and micromagnetic simulations.[25] We have also validated that the formation of THE originates from the interfacial DMI by replacing the Pt layer with Bi2SeTe2\mathrm{Bi_2SeTe_2}, a topological insulator film. In the Fe:MoS2/Bi2SeTe2\mathrm{Fe:MoS_2/Bi_2SeTe_2} heterostructure, as illustrated in Figure S9, the AHE is observed in the absence of any characteristic THE hump, providing a clear distinction between the AHE and THE and reinforcing the role of the interfacial DMI manifested by the THE. To further exam if those two humps are from other effect such as spateial inhomogenility,[71] interface modification[68] or strain,[67, 72] we studied the possible interprerations of “hump a” and “hump b” in Figure 4B (see supplymenray text 3). The origin of 'hump a' suggests the presence of THE, but further spatial scanning of the magnetic vector is required to fully understand the origin of 'hump b'. Figure 4C shows the temperature and magnetic field dependence of humps, consolidating the robust THE response from “hump a” across the entire temperature range. Figure 4D shows the extracted peak positions of the “hump a” (HaH_a) that monotonically decrease as the temperature increases above 170 K. Whereas similar humps can be produced by alternative methods, such as competing ferromagnetic phases caused by interface-induced AHE sign reversal[68] or nonhomogeneous samples,[73] magnetic circular dichroism (MCD) analysis revealed no visible magnetic subdomains in the Fe:MoS2_2 samples.[37] Furthermore, the photoluminescence (PL) mapping of Fe:MoS2_2 corroborates the uniformity of the defect luminescence and Fe-related peak (Figure S10) to rule out the above scenarios. Another possibility is that the humps in AHE measurements can manifest as interface-induced sign reversal, typically requires two ferromagnetic layer with composition difference.[68] However, such a phenomenon is not possible in Fe:MoS2_2/Pt heterostructure, as we only use a monolayer Fe:MoS2_2 for Hall measurement.

Anomalous Hall effect in Fe:MoS₂/Bi₂SeTe₂

Figure S9. Anomalous Hall effect in Fe:MoS2/Bi2SeTe2\mathrm{Fe}:\mathrm{MoS}_{2}/\mathrm{Bi}_{2}\mathrm{SeTe}_{2} (A) AHE measurement of a Fe:MoS2/Bi2SeTe2\mathrm{Fe}:\mathrm{MoS}_{2}/\mathrm{Bi}_{2}\mathrm{SeTe}_{2} heterostructure at 4 K with an external magnetic field applied out-of-plane (zz-direction). (B) Optical image of the Fe:MoS2/Bi2SeTe2\mathrm{Fe}:\mathrm{MoS}_{2}/\mathrm{Bi}_{2}\mathrm{SeTe}_{2} heterostructure, with layers marked. The thickness of the Bi2SeTe2\mathrm{Bi}_{2}\mathrm{SeTe}_{2} layer is 23 nm.

PL mapping of a typical monolayer Fe:MoS$_2$ crystal performed at 4 K, showing optical image, background, defect emission, and Fe emission

Figure S10. PL mapping of a typical monolayer Fe:MoS2_2 crystal performed at 4 K. (A) Optical image of a monolayer Fe:MoS2_2 transferred onto a hBN layer. (B) Hyperspectral PL background signal when scanning off-sample. (C) Mapping of defect emission, filtered within the 650 nm to 800 nm range. (D) Fe-related emission, filtered within the 540 nm to 560 nm range.

Conclusion and Outlook

We have demonstrated ultralow-power, field-free, deterministic, and nonvolatile perpendicular magnetization switching by SOT up to 380 K using a DMS, monolayer Fe:MoS2\mathrm{Fe:MoS_2} through interfacial coupling with a Pt Hall bar. The induced strain in the crystal caused a reduction in the crystal symmetry in monolayer Fe:MoS2\mathrm{Fe:MoS_2}. We showed the anisotropy of field-free SOT on the crystallographic axis of Fe:MoS2\mathrm{Fe:MoS_2} by injecting current in the armchair or zigzag direction. The perpendicular magnetic switching of Fe:MoS2\mathrm{Fe:MoS_2} was confirmed by measuring the AHE in the adjacent Pt layer. An apparent AHE loop shift was observed at a zero in-plane magnetic field, verifying the existence of τADOOP\tau_{\mathrm{AD}}^{\mathrm{OOP}} through spin-to-spin conversion in the Fe:MoS2\mathrm{Fe:MoS_2}/Pt heterostructure with reduced crystal symmetry. We demonstrated a switching current density of 7×1047 \times10^{4} A/cm2^{2}, nearly two orders of magnitude lower than reported field-free SOT systems. The power dissipation density of Psw=7.5×1012P_{\mathrm{sw}} = 7.5 \times10^{12} W m−3^{-3} is four orders of magnitude lower than reported vdW SOT materials and three orders of magnitude lower than non-vdW SOT materials.[22] [6, 7, 8, 9, 10, 15] The magnitude of the topological Hall resistance persists up to 300 K, indicating that a robust magnetic skyrmion is maintained over a wide temperature range and that the topological features at the Fe:MoS2\mathrm{Fe:MoS_2}/Pt interface are stable. This strong manifestation of THE was attributed to the interfacial DMI, which contributed to field-free SOT switching in the Fe:MoS2\mathrm{Fe:MoS_2}/Pt heterostructure. This SOT application using a 2D monolayer DMS provides a new pathway for developing highly power-efficient spintronic devices.

Experimental Section

Synthesis of MoS2_2 monolayers and Fe-doped MoS2_2:

MoS2_2 monolayers were synthesized via low-pressure chemical vapor deposition (LPCVD). For growth, a thin layer of MoO3_3 was deposited via Joule heating thermal evaporation onto a Si substrate covered with a 300 nm thick thermal oxide layer. Another SiO2_2/Si substrate was in direct contact with the MoO3_3-deposited substrate during growth.

To substitutionally dope Fe into the MoS2_2 monolayers, Fe3_3O4_4 particles were applied to the SiO2_2/Si substrate before contacting the MoO3_3-deposited substrate. For a uniform distribution of Fe3_3O4_4 particles, the substrate was washed with deionized (DI) water, creating a thin layer of water on the SiO2_2 surface. Subsequently, the Fe3_3O4_4 particles were applied onto the surface of the substrate. The substrate was then annealed at 110 °C for 5 minutes on a hot plate. furnace was heated at a ramp rate of 18 °C/min and held at 850 °C for 15 minutes. Ar gas was initially supplied at a rate of 30 sccm during heating until the temperature reached 300 °C. Then, H2_2 gas was introduced at a rate of 15 sccm as the temperature increased to 760 °C. Sulfur was added to the furnace once the temperature reached 790 °C. The temperature and gas flow were controlled throughout the procedure.

Fabrication of Fe:MoS2_2/Pt heterostructures

The four Hall bar contacts (Pt/Cr - 8/5 nm) with dimensions of 2 mm × 5 mm were patterned on a SiO2_2/Si substrate via e-beam lithography. First, the substrate was spin-coated with PMMA and then baked at 180 °C for 90 seconds. Subsequently, the photoresist was exposed to the e-beam and developed using a 3:1 mixture of 4-methyl-2-pentanone (MIBK) and 2-propanol (IPA). The Pt/Cr layers were deposited onto the patterned photoresist layer via e-beam evaporation. The photoresist was removed through a lift-off process involving rinsing with acetone and IPA to define Pt/Cr electrodes.

Fe:MoS2_2 monolayers grown on SiO2_2 were coated with a thin layer of PMMA (950 A4) using a dropper. The chip was left under ambient conditions to dry for 60 min. The chip was floated in 10% KOH (aq) for 10 min, after which the Si substrate sunk 10% KOH (aq) due to SiO2_2 etching, leaving the PMMA/MoS2_2 floating on the surface of the KOH solution. Next, the PMMA/MoS2_2 was cleaned in DI water, scooped using another substrate (i.e., target substrate), and dried under ambient conditions for 1 hour. A PMMA film with a Fe:MoS2_2 crystal was attached beneath poly(dimethylsiloxane) (PDMS) and stamped with Fe:MoS2_2 aligned atop the Pt electrode. The PMMA was removed using warm acetone, followed by an IPA rinse. The fabricated Fe:MoS2_2/Pt sample was loaded in a furnace (MTI OTF 1200X) with a 2" quartz tube and annealed at 120 °C for 20 min to enhance adhesion, followed by soaking in 2-hour chloroform (CHCl3_3) at room temperature to remove organic residues thoroughly.

Hall resistance measurement

Magnetoresistance measurements were conducted using a variable temperature insert (VTI) within an attoDRY 1100 cryostat, with a temperature range from 4 K to 300 K and a vertical magnetic field of up to 9 T at 4 K. The Hall resistance was measured using a four-probe by applying 0.1-90 mA of d.c. current with a Keithley 2636B source meter and measuring the voltage drop (Vxy_{xy}) with a Keithley 2182A nanovoltmeter. The AHE loop shift was measured with the same setup by applying a 10 ms pulse using an SDG 2122x (Siglent Technologies) waveform generator. The loop shift measurement was conducted only at 4 K to avoid quenching of the superconducting magnet in an attoDRY 1100.

SOT measurements:

The field-free SOT switching measurements were conducted within an Atto-DRY 1100 cryostat capable of applying a magnetic field of up to 0.5 T at 300 K. Pulses were generated using a Keithley 2636B source meter, with each pulse duration of 1 ms. To mitigate noise, the SOT device was allowed to rest for 5 s after each pulse cycle. The RHR_H values were determined by averaging the Hall resistivity values for 5-10 s, measured with a d.c. of 50-90 µA. For SOT data measurements above 300 K, the same setup was employed in a Cryostat ST-500 (Lakeshore Cryotronics) instrument equipped with a custom-built magnet capable of applying 0.35 T in the z-direction. The SOT data from the Atto-DRY 1100 and Cryostat ST-500 for temperatures between 200 K and 300 K were compatible.

Supporting Information

Supporting Information is available from the Wiley Online Library or from the author.

Acknowledgments

E.H.Y. acknowledges financial support from the AFOSR under Grant FA9550-11-10272 and the NSF under Grant ECCS-1104870. S. S. acknowledges financial support from the NSF under Grants NSF-DMR-1809235, NSF-EFRI-1641094, and ECCS-MRI-1531237. D.S. acknowledges financial support from the DoE under award number DE-SC0020992. This research used microscopy resources, partially funded by the NSF under Grant NSF-DMR-0922522, within the Laboratory for Multiscale Imaging (LMSI) at Stevens Institute of Technology. This work was also partially carried out at the Micro Device Laboratory (MDL) at Stevens Institute of Technology, funded with support from W15QKN-05-D-0011. The authors thank Yuxing Liu and Shivani Bhawsar for their assistance in manuscript preparation.

Author contributions

S.C. and E.H.Y. conceived the experiments for synthesizing and characterizing the materials and devices. S.C., M.F., and Y.Z. carried out the synthesis of Fe:MoS2\mathrm{Fe}:\mathrm{MoS}_{2}. S.C., M.F., Z.T. and L.X carried out optical, Raman, PL, SEM, and XPS characterization and analysis. M.F. and A.S.S. performed AFM characterization. R.S. and S.C. designed the SOT device. S.C. and M.F. performed the fabrication, with contributions from X.Z. and Y.Z.. S.C. designed the electromagnetic measurements, and S.C. and A.S.S. built the experimental setup. N.L. made an initial contribution to the measurement setup. S.C. and Z.T. characterized SOT systems. S.C., R.S., S.S., D.S., and E.H.Y. conducted data analysis. All authors discussed the results and contributed to the final manuscript.

References

Supporting Information

Optical microscope image and source-drain IV characteristics of Fe:MoS₂

Figure S5. Fe:MoS₂ conductivity. a. Optical microscope image of a monolayer single crystal Fe:MoS₂ on Au electrodes. Scale bar, 10 μm. b. Source-drain IV characteristics of a monolayer Fe:MoS₂ at 300 K.

Field-free SOT switching in four different devices

Figure S7. Field-free SOT in different devices. (A to D) Demonstration of field-free SOT switching in four distinct devices by applying 2 ms current pulses along the x-axis (Jw∥xJ_{\mathrm{w}} \parallel x) at 300 K. This showcases the reproducibility and reliability of the SOT device.

Line scanning of Raman peak position and optical image of Fe:MoS2/Pt sample

Figure S12. A. Line scanning of E2g_{2g} Raman peak position in Fe:MoS2_2/Pt. Data in the shaded area was obtained when the Raman laser spot was located inside the Pt Hall bar area. The error bars were determined by s.d. of each measurement. B. Optical image of the Fe:MoS2_2/Pt sample. The red arrow shows the Raman scanning direction.

Fitting for the upper half of RH1R_{\mathrm{H}1} with two tanh functions (two AHE channels) as represented by the blue and green curves. All curves scanned from 3 kOe to -3 kOe. D. Fitting for the upper half of RH1R_{\mathrm{H}1} using one tanh function, indicated by a solid blue curve, with ferromagnetic domain reversal near -0.5 kOe. The remaining signal is attributed to THE. The red arrow on the bottom indicates the scan direction.

Supplementary Text

Spin-to-spin conversion

Spin current injection

The accumulation of y-polarized spins gives rise to a spin chemical potential (μs\boldsymbol{\mu}_{s}), resulting in spins being injected into Fe:MoS2_2, which can be expressed by:

jPS,z=−σP2e∂zμs+θPσPExy(2)\boldsymbol{j}_{PS,z}=-\frac{\sigma_{P}}{2e}\partial_{z}\boldsymbol{\mu}_{s}+\theta_{P}\sigma_{P}E_{x}\boldsymbol{y} \tag*{(2)}

where σP\sigma_{P} and θP\theta_{P} are the electrical conductivity and the spin Hall angle of Pt, respectively. ExE_{x} is the applied electric field along the x direction. The spin-to-spin conversion occurs primarily in the z-direction, given the monolayer thickness of Fe:MoS2_2 (approximately 0.8 nm, Figure S1). The resulting spin current in the z-direction is given by:

jFS,z=−σF2e∂zμs+σFExz(3)\boldsymbol{j}_{FS,z}=-\frac{\sigma_{F}}{2e}\partial_{z}\boldsymbol{\mu}_{s}+\sigma_{F}E_{x}\boldsymbol{z} \tag*{(3)}

where σF\sigma_{F} is the Hall conductivity of Fe:MoS2_2. With the spin current jFS,z\boldsymbol{j}_{FS,z} contributing by both the in-plane electric field along the x direction (ExE_{x}), and the spin diffusion pushed by μs\boldsymbol{\mu}_{s}.

This spin-to-spin conversion process can be described using linear response theory, as presented by Wang et al.[11] From the quantum Liouville equation, the nonequilibrium spin density (δS\delta\boldsymbol{S}) can be expressed by modeling the symmetry breaking in the x-z plane as a Rashba-like spin orbit coupling (SOC):

δS=∑k[δSk0+2αRτs(k×y)×δSk0](4)\delta\boldsymbol{S}=\sum_{k}\left[\delta\boldsymbol{S}_{k}^{0}+2\alpha_{R}\tau_{s}(\boldsymbol{k}\times\boldsymbol{y})\times\delta\boldsymbol{S}_{k}^{0}\right] \tag*{(4)}

where δSk0\delta\boldsymbol{S}_{k}^{0} refers to the resolved contribution in the crystal momentum space of electrons, kk is the crystal momentum of electrons, αR\alpha_{R} is the Rashba parameter up to the first order, and τs\tau_{s} is the spin relaxation time. For a qualitative explanation of the expression of spin current and spin flipping time, we employed a continuity equation within spin dynamics. The spin current (Jk\boldsymbol{J}_{k}) and spin density (SkS_{k}) are related as follows[74]:

∂Sk∂t+∇⋅Jk=−Skτs(5)\frac{\partial S_{k}}{\partial t}+\nabla\cdot\boldsymbol{J}_{k}=-\frac{S_{k}}{\tau_{s}} \tag*{(5)}

where kk represents the spin direction (k=x,y,zk=x,y,z). As a result of the spin Hall effect (SHE), the spin current has the form:

Jk=−DS∇Sk+σθEi(6)\boldsymbol{J}_{k}=-D_{S}\nabla S_{k}+\sigma_{\theta}E_{i} \tag*{(6)}

where σθ\sigma_{\theta}, EiE_{i}, and DSD_{S} represent the spin-hall conductivity, electric field along the ii direction and spin diffusion coefficient, respectively. In a system with SOC, the spin density is related to the spin chemical potential (Sk∝μkS_{k}\propto\mu_{k}), leading to the following continuity equation:

∂μk∂t+∑i∂iJs,ik=−μkτs(7)\frac{\partial\mu_{k}}{\partial t}+\sum_{i}\partial_{i}J_{s,i}^{k}=-\frac{\mu_{k}}{\tau_{s}} \tag*{(7)}

where Js,ikJ_{s,i}^{k} represents the external spin current with kk-spin, flowing in ii-direction. When the system reaches a steady state, we have ∂μk∂t=0\frac{\partial\mu_{k}}{\partial t}=0. With the y-spins being converted into z-spins in Fe:MoS2_2 (JFS,izJ_{FS,i}^{z}), we incorporate the spin accumulation: Sz=ηy,zzJs,yzS_{z}=\eta_{y,z}^{z}J_{s,y}^{z} into equation (4) for z-spins which becomes:

−μzτsF∼∂zJFS,zz+ηy,zzJPS,yz(8)-\frac{\mu_{z}}{\tau_{sF}}\sim\partial_{z}J_{FS,z}^{z}+\eta_{y,z}^{z}J_{PS,y}^{z} \tag*{(8)}

where τsf\tau_{sf} and ηy,zz\eta^{z}_{y,z} are the spin-flipping time and response tensor for converting y-spin to z-spin in Fe:MoS2_2, respectively. The JFs,zzJ^{z}_{Fs,z} and JPs,yyJ^{y}_{Ps,y} are z-spins from Fe:MoS2_2 and y-spins from Pt, respectively, both flowing in the z-direction.

Spin chemical potential

Next, to qualitatively show how the y-spins are converted to z-spins in the Fe:MoS2_2 layer, we derive the expression for spin chemical potential distribution of z-polarized spins (μz(z)\mu_z(z)). Based on the macroscopic model,[75] The spin-diffusion equation gives the partial differential equation relation of μk\mu_k in Pt and Fe:MoS2_2. Given a current flowing in the x direction of the Pt Hall bar, the relation of μy\mu_y can be written as follows, based on the spin-diffusion equation:[75]

∂2μy∂z2=μylsp2(9)\frac{\partial^2\mu_y}{\partial z^2}=\frac{\mu_y}{l_{sp}^2} \tag*{(9)}

where lspl_{sp} is the spin diffusion length in the Pt layer, and μy\mu_y is the chemical potential of y-spins. For the chemical potential of spins in the Fe:MoS2_2 layer, the contribution of spin-to-spin conversion due to SOC should be considered by adding terms including the crystal momentum of electrons (kk):

∂2μy∂z2−ky,zz∂μz∂z=μylsf2(10)\frac{\partial^2\mu_y}{\partial z^2}-k^z_{y,z}\frac{\partial\mu_z}{\partial z}=\frac{\mu_y}{l_{sf}^2} \tag*{(10)}
∂2μz∂z2−kz,zy∂μy∂z=μzlsf2(11)\frac{\partial^2\mu_z}{\partial z^2}-k^y_{z,z}\frac{\partial\mu_y}{\partial z}=\frac{\mu_z}{l_{sf}^2} \tag*{(11)}

Here ki,jak^a_{i,j} is the crystal momentum of electrons with a-spin, where ii denotes the direction of generated spin density and jj represents the flow direction of spin current. and lsfFl_{sf}^{F} is the spin diffusion length of Fe:MoS2_2.

To obtain an approximate solution for Equations 8 and 9, we set up a model as shown in the inset of Figure R1. For a thin film of Fe:MoS2_2 on the top of Pt, we assign z=0 at the Fe:MoS2_2/Pt interface and solve the equation for 0<z<lsfF0<z<l_{sf}^{F}. We ignore the interfacial spin scattering by assuming the interface is transparent to spin transmission. The boundary conditions can be expressed as: μz(z=0)=0\mu_z(z=0)=0, μy(z=0)=1\mu_y(z=0)=1 (normalized maximum μy\mu_y); μy(z=0+)=μy(z=0−)\mu_y(z=0+)=\mu_y(z=0-), μz(z=0+)=μz(z=0−)\mu_z(z=0+)=\mu_z(z=0-); JPs,yy(z=0)=1J^{y}_{Ps,y}(z=0)=1, and JFs,zz(z=0)=0J^{z}_{Fs,z}(z=0)=0. Given that the electrical conductivity of Pt is more than three orders of magnitudes larger than that of Fe:MoS2_2 (σP≫σF\sigma_P\gg\sigma_F), the solution of μz(z)\mu_z(z) for 0<z<lsfF0<z<l_{sf}^{F} can be expressed as:

μz(z)≈2eEx[lsf2ky,zzθP(cosh⁡(zlsfF)−1)+lsfFθFsinh⁡(zlsfF)](12)\mu_z(z)\approx2eE_x\left[l_{sf}^2 k^z_{y,z}\theta_P\left(\cosh\left(\frac{z}{l_{sf}^{F}}\right)-1\right)+l_{sf}^{F}\theta_F\sinh\left(\frac{z}{l_{sf}^{F}}\right)\right] \tag*{(12)}

where ee, ExE_x, θP\theta_P and θF\theta_F represent elementary charge, the electronic field along the x-direction, spin Hall angle of Pt and Fe:MoS2_2, respectively. The detailed distribution of z-spin density can be seen by plotting the μz(z)/k\mu_z(z)/k relation. The spin Hall angle of Fe:MoS2_2 (θF\theta_F) can be estimated by critical current density (JcJ_c) of SOT switching for thin magnet, given by:[76]

Jc≈2eℏμ0MstFMθF(13)J_c\approx\frac{2e}{\hbar}\mu_0M_st_{FM}\theta_F \tag*{(13)}

where μ0\mu_0, MsM_s and tFMt_{FM} are the magnetic permeability in vacuum, saturated magnetization, and thickness of Fe:MoS2_2. Based on our previous literature report,[37] the MsM_s at room temperature is about 65 emu cm−3^{-3}, and we take tFM=0.9t_{FM}=0.9 nm, Jc=20×106J_c=20 \times10^{6} A ⋅\cdot cm−2^{-2} (at 300K), the θF\theta_F is approximately 0.17. Considering the θp\theta_p for Pt is 0.068,[77] we plot the μz(z)\mu_z(z) versus (z/lsf∞)(z/l_{sf}^{\infty}) relation as shown in the blue curve of Figure S11. For ky,zk_{y,z} is a positive constant smaller 1 for Fe:MoS2_2, μz(z)\mu_z(z) increases monotonically for 0<z<lsf∞0<z<l_{sf}^{\infty}, implying the importance role of the thickness of Fe:MoS2_2 layer for the spin (y)-to-spin (z) conversion

Normalized z-polarized spin potential plot with inset showing the coordinate system of the Fe:MoS$_2$/Pt device

Figure S11. Normalized z-polarized spin potential (μz(z)\mu_z(z)) as described by Equation (10) for 0<z/lsf<10<z/l_{\mathrm{sf}}<1. The inset shows the coordinate system of the device, where z=0z=0 represents to the Fe:MoS2_2/Pt interface. The charge current (JJ) is injected along the x-axis.

spin conversion in monolayer Fe:MoS2_2

As shown in Figure S11, the dimension of lsf∞l_{sf}^{\infty} is essential to verify whether spin-to-spin conversion is accountable for the SOT switching, as μz(z)\mu_z(z) decreases parabolically with a reduction of zz. Based on Equation (11) and the previous studies on WTe2_2,[11] the spin-to-spin conversion would be not efficient when z<lsf∞z<l_{sf}^{\infty}. Whereas a precise spin-diffusion length measurement was not conducted in this study, we estimated lsf∞l_{sf}^{\infty} using the spin diffusion length of pristine MoS2_2 (lsm∞l_{sm}^{\infty}). It is noteworthy that lsm∞l_{sm}^{\infty} strongly depends on the number of layers of MoS2_2, as a thinner layer will introduce more inversion symmetry breaking along the out-of-plane (zz) direction. This symmetry breaking enables SOC to generate an equivalent kk-dependent magnetic field via Dresselhaus interactions, leading to spin relaxation through the D’yakonov-Perel (DP) mechanism.[78, 79] Consequently, for a 6-layer MoS2_2, lsm∞l_{sm}^{\infty} is ~200 nm below 30 K,[80] whereas lsm∞l_{sm}^{\infty} is ~15 nm for a monolayer below 30 K.[81, 82] At room temperature, the caculated lsm∞l_{sm}^{\infty} for the monolayer is reduced to ~1.2 nm. [82]

Moreover, a stronger spin scattering has also been reported by Hanle-kerr and spin injection experiments on the monolayer MoS2_2. The reported a spin lifetime (τsm∞\tau_{sm}^{\infty}) is shorter than 200 ps above 40 K [ref],[83, 84] which can further reduce the spin diffusion length in monolayer at room temperature.

For Fe:MoS2_2, Fe substitutional doping is expected to further decrease the spin diffusion length (lsf∞<lsm∞∼1.2l_{sf}^{\infty}<l_{sm}^{\infty}\sim1.2 nm) due to impurity scattering.[75, 85] It is also important to note that the solution of μz(z)\mu_z(z) in Equation (10) is approximation that neglects spin scattering between interface of Fe:MoS2_2/Pt. With the assistance of interface spin scattering, the actual value for μz(z)\mu_z(z) would be higher than our initial prediction in Figure S11.[11]

As a result of DP mechanism dominant spin scattering at high temperatures, enhanced interface spin scattering at 2D limit, and extra Fe doping-induced impurity scattering, it is participated that the monolayer Fe:MoS2_2 possesses a spin diffusion length smaller than 1.2 nm. This suggests that the 0.9 nm thickness of monolayer Fe:MoS2_2 (Figure S1C) is sufficient for the y to z spin conversion.

Modulation of RTHER_{THE} by pulsed current

As shown in Figure S6-Figure S6, after applying a pulsed current (JpJ_p), the RHR_H signal was measured, showing a gradual decrease in RTHER_{THE} signal with increased current amplitude (Figure S6). In contrast to AHE under d.c current, where both RAHER_{AHE} and RTHER_{THE} decrease proportionally with the temperature increase, JPJ_P changes RTHER_{THE} significantly while RAHER_{AHE} remains relatively stable.

Influence of DMI on magnetization switching

The influence of DMI on magnetization switching is quantified through the dynamics of magnetic layers, as described by the Landau-Lifshitz-Gilbert (LLG) equation:

∂m∂t=γ01+α2(m×Heff+αm×m×Heff)+τSOT(14)\frac{\partial\mathbf{m}}{\partial t} = \frac{\gamma_0}{1+\alpha^2}\left(\mathbf{m} \times\mathbf{H}_{eff}+\alpha\mathbf{m}\times\mathbf{m}\times\mathbf{H}_{eff}\right)+\boldsymbol{\tau}^{SOT} \tag*{(14)}

where m\mathbf{m} represents the normalized magnetization vector, α\alpha denotes the Gilbert damping coefficient, γ0\gamma_0 is the gyromagnetic ratio and τSOT\boldsymbol{\tau}^{SOT} is the spin-orbit torque, which includes the torque arising from broken crystal symmetry, τADOOP\boldsymbol{\tau}^{OOP}_{AD}. Since the effective magnetic field Heff\mathbf{H}_{eff} is proportional to the combination of magnetic stray field energy, perpendicular anisotropy energy, interfacial DMI energy and Heisenberg exchange energy [25, 86], the Heff\mathbf{H}_{eff} can be expressed by Heff∝Hstray+Hanis+HDMI+Hexch\mathbf{H}_{eff} \propto\mathbf{H}_{stray}+\mathbf{H}_{anis}+\mathbf{H}_{DMI}+\mathbf{H}_{exch}. Among these components, the interfacial DMI field is directly proportional to the strength of interfacial DMI (HDMI∝D\mathbf{H}_{DMI} \propto D). Therefore, the existence of interfacial DMI here can be a critical factor contributing to field-free SOT switching in the Fe:MoS2_2/Pt heterostructure.

Origin of humps in Hall measurement.

Figure S13A presents Hall resistance (RHR_H) data measured at 4K, showing two sets of antisymmetric humps in the RHR_H loop, one at ±2.5\pm2.5 kOe (hump a) and another at ±0.5\pm0.5 kOe (hump b), marked by blue and green arrows. As shown in Figure S13A, after exhibiting the hump at 0.5 kOe, the Hall signal does not return to the blue dashed lines, indicating there could be another ferromagnetic subdomain.

To explore the origin of the humps, we decomposed the Hall resistance (RHR_H) in Figure S13A using RH=R0H+RAHE+RTHER_H=R_0H+R_{AHE}+R_{THE}. We first subtracted the ordinary Hall effect (R0HR_0H) using a linear background, resulting in the red solid curve in Figure S13B. A recurring observation in the literature is that the hump location typically coincides with the AHE domain reversal, which can be attributed to either THE[64, 65, 66] [50, 51] or two-channel AHE[67, 68]. Accordingly, we further decomposed the Hall signal (red curve) into two channels with humps near the domain reversal. As shown in Figure S13B, RH1R_{H1} (blue dashed line) presents a Hall loop with domain reversal near ‘hump a’ at ±2.5\pm2.5 kOe, while the remaining Hall signal, RH2R_{H2} (black dashed curve), shows a Hall loop with domain reversal near ‘hump b’ at ±0.5\pm0.5 kOe.

Hall resistance data and analysis in Fe:MoS2 monolayers

Figure S13. A. Hall resistance data (RHR_{\mathrm{H}}) in Fe:MoS2_2 monolayers at 4K with IxxI_{\mathrm{xx}}=140 μA. The blue arrows indicate “hump a” near ±2~2.5 kOe, observed before the domain reversal at ±3 kOe, while the green arrows mark “hump b” near ±0.5 kOe. The light-blue dashed lines represent the linear background from the ordinary Hall effect. B. Hall resistance after subtracting the ordinary Hall effect. The red curve was further decomposed into two channels (RH1R_{\mathrm{H1}} and RH2R_{\mathrm{H2}}), with each channel exhibiting humps near the magnetic domain reversal. C.

First we studied the RH1R_{H1} signal under two-channel AHE interpretation, by fitting the upper half of RH1R_{H1} with two M0tanh⁡(Ha0−H0)M_0\tanh\left(\frac{H}{a_0}-H_0\right) functions.[50] As shown in Figure S13C, RH1R_{H1} can be fitted by the superposition of two tanh functions, resulting in the solid red curve. However, because the peak location of RH2R_{H2} occurs before zero, this fitting results in one tanh function crossing the y-axis while x is positive (green solid curve), yielding a negative coercivity (Hc=−1H_c=-1). This is clearly not allowed for the AHE response.

Next, we examined RH1R_{H1} signal under AHE + THE interpretation, with one tanh function adding a hump from THE. In Figure S13D, the solid red curve represents the fitted line for RH2R_{H2} data points, with the blue solid curve showing the AHE signal, where RAHER_{AHE} has an inverted sign and a coercivity of approximately 1 kOe. These fitting results suggest that it is unlikely that the hump b in Figure S13A is attributed to the two-channel AHE. Furthermore, as shown in Figure S9, all hump features disappear when Pt is replaced with BST, suggesting that the Fe:MoS2_2 crystal has homogenous magnetic order and doesn’t fit with two-channel AHE model. Thus, we confirm that these “hump a” from RH1R_{H1} are likely to be related to THE.

For the RH2R_{\mathrm{H2}} signal, the smaller ‘hump b’ can be explained by a THE signal at ±2.5\pm2.5 kOe appearing during the ferromagnetic domain reversals.[65] However, the ‘hump b’ might also be fitted with two groups of tanh function, with one function having yy (RHR_{\mathrm{H}}) sign inverted (see Figure R3.C)[87]. At this stage, the origin of 'hump a' suggests the presence of THE, but further spatial scanning of the magnetic vector is required to fully understand the origin of 'hump b'.

References

  1. [20]X. Y. Zheng, S. Channa, L. J. Riddiford, J. J. Wisser, K. Mahalingam, C. T. Bowers, M. E. McConney, A. T. N’Diaye, A. Vailionis, E. Cogulu, H. Ren, Z. Galazka, A. D. Kent, Y. Suzuki, Nature Communications 2023, 14, 4918.
  2. [21]A. L. Edgeton, I. A. Harris, N. G. Campbell, Y. Chai, M. M. Mazur, G. Gurung, X. Huang, S. Susarla, E. Y. Tsymbal, D. C. Ralph, T. Nan, M. S. Rzchowski, R. Ramesh, C.-B. Eom, Nature Electronics 2023, 6, 973.
  3. [22]M. Yang, L. Sun, Y. Zeng, J. Cheng, K. He, X. Yang, Z. Wang, L. Yu, H. Niu, T. Ji, G. Chen, B. Miao, X. Wang, H. Ding, Nature Communications 2024, 15, 3201.
  4. [23]L. Liu, C. Zhou, X. Shu, C. Li, T. Zhao, W. Lin, J. Deng, Q. Xie, S. Chen, J. Zhou, R. Guo, H. Wang, J. Yu, S. Shi, P. Yang, S. Pennycook, A. Manchon, J. Chen, Nature Nanotechnology 2021, 16, 277.
  5. [24]H. Lyu, Y. Zhao, J. Qi, H. Huang, J. Zhang, G. Yang, Y. Guo, S. Shen, W. Qin, Y. Sun, J. Shen, P. Dou, B. Shao, Y. Zhang, K. Jin, Y. Long, H. Wei, B. Shen, S. Wang, Advanced Functional Materials 2022, 32, 2200660.
  6. [25]W. He, C. Wan, C. Zheng, Y. Wang, X. Wang, T. Ma, Y. Wang, C. Guo, X. Luo, M. E. Steblyi, G. Yu, Y. Liu, A. V. Ognev, A. S. Samardak, X. Han, Nano Letters 2022, 22, 6857.
  7. [26]Y. Liu, G. Shi, D. Kumar, T. Kim, S. Shi, D. Yang, J. Zhang, C. Zhang, F. Wang, S. Yang, Y. Pu, P. Yu, K. Cai, H. Yang, Nature Electronics 2023, 6, 732.
  8. [27]M. Wang, B. Lei, K. Zhu, Y. Deng, M. Tian, Z. Xiang, T. Wu, X. Chen, npj 2D Materials and Applications 2024, 8, 22.
  9. [28]S. Jin, Y. Wang, H. Zheng, S. Dong, K. Han, Z. Wang, G. Wang, X. Jiang, X. Wang, J. Hong, H. Huang, Y. Zhang, T.-L. Xia, X. Wang, Nano Letters 2024, 24, 5467.
  10. [29]H. Yang, S. O. Valenzuela, M. Chshiev, S. Couet, B. Dieny, B. Diény, A. Fert, K. Garello, M. Jamet, D.-E. Jeong, K. Lee, T. Lee, M.-B. Martin, G. S. Kar, P. Séneór, H.-J. Shin, S. Roche, Nature 2022, 606, 663.
  11. [30]X. Zhang, Q. Lu, W. Liu, W. Niu, J. Sun, J. Cook, M. Vaninger, P. F. Miceli, D. J. Singh, S.-W. Lian, T.-R. Chang, X. He, J. Du, L. He, R. Zhang, G. Bian, Y. Xu, Nature Communications 2021, 12, 2492.
  12. [31]Y. Li, X. Hu, A. Fereidouni, R. Basnet, K. Pandey, J. Wen, Y. Liu, H. Zheng, H. O. H. Churchill, J. Hu, A. K. Petford-Long, C. Phatak, ACS Applied Nano Materials 2023, 6, 4390.
  13. [32]W. Xie, J. Zhang, Y. Bai, Y. Liu, H. Wang, P. Yu, J. Li, H. Chang, Z. Wang, F. Gao, G. Wei, W. Zhao, T. Nie, APL Materials 2024, 12, 031102.
  14. [33]K. Kang, K. Godin, Y. D. Kim, S. Fu, W. Cha, J. Hone, E. H. Yang, Advanced Materials 2017, 29, 1603898.
  15. [34]Y. Xia, X. Chen, J. Wei, S. Wang, S. Chen, S. Wu, M. Ji, Z. Sun, Z. Xu, W. Bao, P. Zhou, Nature Materials 2023, 22, 1324.
  16. [35]J. Kwon, M. Seol, J. Yoo, H. Ryu, D.-S. Ko, M.-H. Lee, E. K. Lee, M. S. Yoo, G.-H. Lee, H.-J. Shin, J. Kim, K.-E. Byun, Nature Electronics 2024, 7, 356.
  17. [36]K. S. Kim, J. Kwon, H. Ryu, C. Kim, H. Kim, E.-K. Lee, D. Lee, S. Seo, N. M. Han, J. M. Suh, J. Kim, M.-K. Song, S. Lee, M. Seol, J. Kim, Nature Nanotechnology 2024, 19, 895.
  18. [37]S. Fu, K. Kang, K. Shayan, A. Yoshimura, S. Dadras, X. Wang, L. Zhang, S. Chen, N. Liu, A. Jindal, X. Li, A. N. Pasupathy, A. N. Vamivakas, V. Meunier, S. Strauf, E. H. Yang, Nature Communications 2020, 11, 2034.
  19. [38]S. J. Yun, D. L. Duong, D. M. Ha, K. Singh, T. L. Phan, W. Choi, Y. M. Kim, Y. H. Lee, Advanced Science 2020, 7, 1.
  20. [39]K. Kang, S. Fu, K. Shayan, Y. Anthony, S. Dadras, X. Yuzan, F. Kazunori, M. Terrones, W. Zhang, S. Strauf, V. Meunier, A. N. Vamivakas, E. H. Yang, Nanotechnology 2021, 32, 95708.
  21. [63]Y. Shiokawa, E. Komura, Y. Ishitani, A. Tsumita, K. Suda, Y. Kakinuma, T. Sasaki, AIP Advances 2019, 9, 035236.
  22. [64]Q. Shao, Y. Liu, G. Yu, S. K. Kim, X. Che, C. Tang, Q. L. He, Y. Tserkovnyak, J. Shi, K. L. Wang, Nature Electronics 2019, 2, 182.
  23. [65]L. Wang, Q. Feng, Y. Kim, R. Kim, K. H. Lee, S. D. Pollard, Y. J. Shin, H. Zhou, W. Peng, D. Lee, W. Meng, H. Yang, J. H. Han, M. Kim, Q. Lu, T. W. Noh, Nature Materials 2018, 17, 1087.
  24. [66]J. Matsuno, N. Ogawa, K. Yasuda, F. Kagawa, W. Koshibae, N. Nagaosa, Y. Tokura, M. Kawasaki, Science Advances 2016, 2, e1600304.
  25. [67]H. Chi, Y. Ou, T. B. Eldred, W. Gao, S. Kwon, J. Murray, M. Dryer, R. E. Butera, A. C. Foucher, H. Ambaye, J. Keum, A. T. Greenberg, Y. Liu, M. R. Neupane, G. J. de Coster, O. A. Vail, P. J. Taylor, P. A. Folkes, C. Rong, G. Yin, R. K. Lake, F. M. Ross, V. Lauter, D. Heiman, J. S. Moodera, Nature Communications 2023, 14, 3222.
  26. [68]F. Wang, X. Wang, Y.-F. Zhao, D. Xiao, L.-J. Zhou, W. Liu, Z. Zhang, W. Zhao, M. H. W. Chan, N. Samarth, C. Liu, H. Zhang, C.-Z. Chang, Nature Communications 2021, 12, 79.
  27. [69]N. Verma, Z. Addison, M. Randeria, Science Advances n.d., 8, eabq2765.
  28. [70]S. Shi, S. Liang, Z. Zhu, K. Cai, S. D. Pollard, Y. Wang, J. Wang, Q. Wang, P. He, J. Yu, G. Eda, G. Liang, H. Yang, Nature Nanotechnology 2019, 14, 945.
  29. [71]L. Wang, Q. Feng, H. G. Lee, E. K. Ko, Q. Lu, T. W. Noh, Nano Lett. 2020, 20, 2468.
  30. [72]D. Tian, Z. Liu, S. Shen, Z. Li, Y. Zhou, H. Liu, H. Chen, P. Yu, Proceedings of the National Academy of Sciences 2021, 118, e2101946118.
  31. [73]G. Kimbell, C. Kim, W. Wu, M. Cuoco, J. W. A. Robinson, Commun Mater 2022, 3, 19.
  32. [74]J. Shi, P. Zhang, D. Xiao, Q. Niu, Phys. Rev. Lett. 2006, 96, 076604.
  33. [75]T. Valet, A. Fert, Phys. Rev. B 1993, 48, 7099.
  34. [76]L. Liu, C.-F. Pai, Y. Li, H. W. Tseng, D. C. Ralph, R. A. Buhrman, Science 2012, 336, 555.
  35. [77]Y. Wang, P. Deorani, X. Qiu, J. H. Kwon, H. Yang, Applied Physics Letters 2014, 105, 152412.
  36. [78]M. I. Dyakonov, A. Khaetskii, Spin physics in semiconductors 2008, 211.
  37. [79]M. W. Wu, J. H. Jiang, M. Q. Weng, Physics Reports 2010, 493, 61.
  38. [80]S. Liang, H. Yang, P. Renucci, B. Tao, P. Laczowski, S. Mc-Murtry, G. Wang, X. Marie, J.-M. George, S. Petit-Watelot, A. Djefal, S. Mangin, H. Jaffrès, Y. Lu, Nature Communications 2017, 8, 14947.
  39. [81]L. Wang, M. W. Wu, Phys. Rev. B 2014, 89, 115302.
  40. [82]L. Wang, M. W. Wu, Phys. Rev. B 2014, 89, 205401.
  41. [83]L. Yang, N. A. Sinitsyn, W. Chen, J. Yuan, J. Zhang, J. Lou, S. A. Crooker, Nature Physics 2015, 11, 830.
  42. [84]Y. K. Luo, J. Xu, T. Zhu, G. Wu, E. J. McCormick, W. Zhan, M. R. Neupane, R. K. Kawakami, Nano letters 2017, 17, 3877.
  43. [85]I. Sugai, S. Mitani, K. Takanashi, IEEE Transactions on Magnetics 2010, 46, 2559.
  44. [86]M. Dai, J.-M. Hu, npj Computational Materials 2020, 6, 78.
  45. [87]G. Kimbell, C. Kim, W. Wu, M. Cuoco, J. W. A. Robinson, Communications Materials 2022, 3, 19.

Paper details

vlnc:W_bzfwybsf
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents