Spontaneous Formation of Lateral Defect-Density Gradient in CVD-Grown MoS2 Monolayers

Abstract

Defect engineering in two-dimensional materials is a powerful strategy for tuning electronic, optical, and catalytic properties. While pristine molybdenum disulfide (MoS2) has been thoroughly studied, defective MoS2 remains poorly understood due to the complexity and inconsistency of controlled defect creation. Here, we report a defect-density gradient that forms spontaneously in MoS2 flakes during chemical vapor deposition (CVD) growth. Photoluminescence and Raman spectroscopy mapping reveal the lateral arrangement of this gradient across a single flake. Deconvolution of the excitonic photoluminescence emission identifies electron doping as the key factor governing the spatial variation in optical response. This doping likely originates from sulfur vacancies formed during CVD growth, as further supported by the observed Raman mode shifts. We propose that this gradient arises from precursor depletion near the nucleation center during growth, resulting in a gradual variation in defect density. This lateral defect structure provides a convenient platform for systematically characterizing defective MoS2 across a continuous range of defect densities within a single sample. The sulfur-vacancy-driven surface activation identified here can also be important for future catalytic applications.

Introduction

Molybdenum disulfide (MoS2MoS_2) is recognised as a promising two-dimensional semiconductor with remarkable optical and electronic properties. In its monolayer form, MoS2MoS_2 exhibits a direct bandgap and strong photoluminescence (PL), in contrast to the indirect bandgap of bulk and multilayer MoS2MoS_2. Reduced dielectric screening and strong Coulomb interactions in the two-dimensional limit [2] result in large exciton binding energies, allowing excitonic states to remain stable at room temperature. Its two-dimensional nature enables its electronic and optical properties to be tuned through strain [3, 4, 5, 6, 7], doping [8, 9, 10] or defect engineering [11, 12]. Although pristine MoS2\mathrm{MoS}_{2} is generally preferred for studies of fundamental light-matter interactions, defect engineering offers an alternative strategy for tailoring the material towards applications such as broadband photodetectors [13, 14], gas sensors [15, 16], and hydrogen production [17, 18].

Common preparation methods for MoS2\mathrm{MoS}_{2} include mechanical exfoliation (ME) and chemical vapour deposition (CVD). While ME produces high-quality crystals, it offers limited efficiency, scalability and reproducibility. In contrast, CVD enables large-area growth of MoS2\mathrm{MoS}_{2} but typically introduces defects that reduce the crystal quality. Sulfur vacancies (VSV_{\mathrm{S}}) are the dominant defect type in CVD-grown MoS2\mathrm{MoS}_{2}, whereas other defects, including molybdenum vacancies (VMoV_{\mathrm{Mo}}) and antisites (SMoS_{\mathrm{Mo}} and MoS\mathrm{Mo}_{\mathrm{S}}), are less prevalent [11]. Importantly, VSV_{\mathrm{S}} can substantially alter the local electronic structure and chemical reactivity of MoS2\mathrm{MoS}_{2}. Vacancy-induced electronic states can modify charge-carrier [19] and optical [20] behaviour, while the altered local bonding around sulfur vacancies can promote molecular adsorption and increase chemical reactivity [21, 22, 23]. Consequently, engineering the concentration and distribution of VSV_{\mathrm{S}} provides a route towards tailoring MoS2\mathrm{MoS}_{2} for sensing and catalytic applications, including the hydrogen evolution reaction. Numerous approaches have therefore been developed to introduce defects in MoS2\mathrm{MoS}_{2}. Most rely on external stimuli to control defect formation, including plasma exposure [24], ion bombardment [25, 26] and gas annealing [23, 27]. While these methods allow the defect density to be modified after growth, they require additional processing and may introduce unwanted structural modifications. An alternative strategy is to engineer defects directly during material synthesis. Spontaneous defect formation during growth eliminates the need for additional chemical or physical treatment [28]. Moreover, CVD offers a scalable route towards the production of defective MoS2\mathrm{MoS}_{2}. Direct control of defect formation during CVD could therefore combine material synthesis and defect engineering within a single scalable process.

Most studies, however, focus on layers with spatially uniform defect distributions. Such samples provide information only at a limited range of defect densities, making systematic defect-dependent studies reliant on comparisons between separate samples. Variations between samples can then complicate the direct correlation between defect density and the resulting material properties. This limitation can be addressed by introducing a non-uniform defect distribution across the MoS2\mathrm{MoS}_{2} surface. A continuous defect-density gradient provides a range of defect concentration within a single monolayer, enabling defect-dependent changes in material properties to be investigated while reducing sample-to-sample variability. This concept is particularly compatible with spatially resolved spectroscopic techniques, such as PL and Raman mapping, which can probe the optical and vibrational response continuously across the same flake. Beyond its use as an experimental platform, spatial control over VSV_{\mathrm{S}} may provide a route towards laterally varying optical, electronic, or chemical functionality within a chemically homogeneous MoS2\mathrm{MoS_2} monolayer. Such defect-defined structures could potentially enable spatially patterned sensing or catalytic activity without introducing a second material or chemical composition. Previous studies of lateral heterostructures have primarily relied on variations in chemical composition [17, 29, 30, 31], whereas the direct formation of a lateral defect-density gradient in a single growth step has not yet been demonstrated experimentally.

In this work, we present a spontaneously formed gradient of defect density within single-layer MoS2\mathrm{MoS_2} flakes. The continuous transition from pristine to defective monolayer MoS2\mathrm{MoS_2} originates directly from the CVD growth process. Using spatially resolved PL and Raman spectroscopy, we map the optical and vibrational response associated with increasing defect density across individual flakes. Our results demonstrate that spatially varying defect densities can be generated directly during MoS2\mathrm{MoS_2} growth and investigated within a single continuous monolayer, providing a scalable platform for studying defect-dependent properties and a potential route towards spatially engineered functionality in two-dimensional materials.

Results

The MoS2\mathrm{MoS_2} flake was first characterized using microscopic techniques. Figure 1a shows an optical microscope image of the MoS2\mathrm{MoS_2} flake, with no visible inhomogeneity on the surface. The SEM image in Figure 1b, obtained using secondary electron signal, also shows no contrast on the flake. Figure 1c shows the morphology of the MoS2\mathrm{MoS_2} flake in AFM, with focus on the flake edge emphasized in Figure 1b by white square. The height profile in the inset plot (along the black line in Figure 1c) reveals the difference of height Δh=0.8 nm\Delta h = 0.8\ \mathrm{nm}, which confirms a single-layer nature of MoS2\mathrm{MoS_2}. Therefore, the flake is homogeneous, and any observed differences must be intrinsic, rather than being caused by thickness variance.

Triangular MoS2 flake grown by CVD: optical microscope image, SEM image, and AFM topography image

Figure 1. Triangular MoS2\mathrm{MoS}_{2} flake grown by CVD. a) Optical microscope image, b) SEM image showing the contrast in secondary electrons, c) AFM topography image with height profile across the flake edge, indicating the flake is a single layer MoS2\mathrm{MoS}_{2}.

Photoluminescence (PL) mapping of the MoS2\mathrm{MoS}_{2} flake first revealed an inhomogeneity in the MoS2\mathrm{MoS}_{2} quality. To analyse the PL data correctly, the PL peak of MoS2\mathrm{MoS}_{2} was deconvolved into three most prominent components: A exciton, A−A^{-} trion and B exciton (as illustrated in Figure 2d), e)). The exciton energies are defined by the energy levels within the valence band, which are split due to strong spin-orbit coupling. This gives the exciton quasiparticles a large binding energy of Eb≈140E_{\mathrm{b}} \approx140 meV, making them stable at room temperature. The A−A^{-} trion is a negatively charged quasi-particle that arises from an additional electron binding to the neutral A exciton. The A−A^{-} trion binding energy is estimated from the energy separation between the A−A^{-} trion and the A exciton as Eb,A−≈40E_{\mathrm{b},A^{-}} \approx40 meV. The main component of the PL emission is the A exciton. Figure 2a) shows the intensity of the A exciton mapped over the flake. There is a gradual decrease in intensity in the bottom region, with a continuous gradient over a relatively short distance of 15 μ\mum. Such spatial variation is uncommon, as most MoS2\mathrm{MoS}_{2} flakes are homogeneous or exhibit edge-to-centre variation. The channel of PL emission can be studied by comparing the intensity of A−A^{-} trion and A exciton. Figure 2b) shows the trion/exciton intensity ratio, emphasizing that the PL is dominated by A exciton in the pristine region, while A−A^{-} trions are dominant in the defective region. The energy of the A exciton is mapped in Figure 2c). This demonstrates a red shift in the bottom region, indicating bandgap narrowing. Figure 2d) and 2e) show characteristic PL spectra from opposite sides of the gradient (for pristine and defective region in Figure 2d) and 2e), respectively), accompanied by an illustrative spectrum deconvolution into A exciton, B exciton and A−A^{-} trion.

PL mapping of a CVD-grown MoS₂ flake on a SiO₂ substrate

Figure 2. PL mapping of CVD-grown MoS2\mathrm{MoS}_{2} flake on a SiO2\mathrm{SiO}_{2} substrate. After deconvolution of the PL peak into A exciton, A−^{-} trion and B exciton, mapping of the A exciton shows a gradient of a) intensity and c) energy, illustrating the energy shift induced by electron doping. b) Trion/exciton intensity ratio indicating the main PL channel across the flake. d) PL spectrum taken from the pristine region with peak deconvolution. e) PL spectrum from the defective region to show the difference in PL peak composition. The rise of A−^{-} trion, in contrary to the decrease of A exciton, indicates a shift in the PL channel over the flake.

This observation can be explained using two phenomena: growth-induced strain or chemical inhomogeneity. The strain effect is commonly observed in CVD-grown MoS2\mathrm{MoS}_{2} flakes, primarily due to the contraction mismatch of MoS2\mathrm{MoS}_{2} and substrate during the cooling stage of the growth process. Adhesion to the substrate might induce tensile strain in the single layer, resulting in significant changes to the electronic properties and optical response of MoS2\mathrm{MoS}_{2}. Such tensile strain would lead to bandgap narrowing or PL red shifting, similar to the presented data. In the literature, growth-induced strain is usually formed in the centre-to-edge geometry due to the contraction mismatch [32]. In our case, the strain would need to be induced in the bottom part of the flake, possibly due to stronger adhesion to the substrate. Thus, the growth-induced strain is not a key consideration in determining the origin of the gradient in this work.

A common distortion of the chemical homogeneity of MoS2_2 is the formation of sulfur vacancies, which occurs particularly during growth. The growth mechanism is sensitive to the directionality and composition of the precursor flow, so any inhomogeneity in precursor flow (due to chamber geometry, sample attachment, etc.) results in a defective MoS2_2 layer. As sulfur atoms are supplied insufficiently, the S:Mo ratio decreases and sulfur vacancies are created. They translate into electronic properties of MoS2_2, because sulfur vacancies act as donors, thus inducing electron doping (n-doping) into the layer. The additional electrons bind to the neutral A excitons, which increases the population of charged A−^{-} trions. The A exciton population is reduced, decreasing its scattering rate and, subsequently, leading to PL quenching in the bottom region. The A exciton red shift is then due to one of three factors: i) local strain relaxation around sulfur vacancies, ii) doping-induced bandgap renormalisation, or iii) defect-bound exciton emission. Finally, A−^{-} trions decay non-radiatively due to the presence of sulfur vacancies. Proposed mechanisms for the channel of A−^{-} trion non-radiative decay are i) recombination centres on sulfur vacancies (via phonon generation) or ii) Auger recombination.

The variation of PL signal can be correlated with Raman spectroscopy mapping of the MoS2\mathrm{MoS}_2 flake, since lattice properties are sensitive to electronic changes and strain. Figure 3a and 3b show maps of the E2g1\mathrm{E}^{1}_{2g} and A1g\mathrm{A}_{1g} Raman mode intensities, picturing the gradient in the same direction, but with opposite slope compared to the PL mapping. The A1g\mathrm{A}_{1g} optical phonon, which corresponds to the out-of-plane lattice vibration, exhibits a greater (more than twofold) increase in Raman scattering intensity in contrary to in-plane E2g1\mathrm{E}^{1}_{2g} mode. Figure 3c plots the distance between the Raman peaks of the E2g1\mathrm{E}^{1}_{2g} and A1g\mathrm{A}_{1g} modes (Δω=ω(A1g)−ω(E2g1)\Delta\omega= \omega(\mathrm{A}_{1g}) - \omega(\mathrm{E}^{1}_{2g})). The gradient in this map indicates that the Raman mode shifts are affected differently, relative to the MoS2\mathrm{MoS}_2 quality. Figure 3d shows two Raman spectra selected from the pristine and defective region, along with the fitted modes for illustration. The defective region shows stronger intensity than the pristine region. To describe the Raman shift gradient, Figure 3e and 3f plot the extracted Raman shifts along the white line in Figure 3a across the MoS2\mathrm{MoS}_2 flake gradient. Both modes are fitted with a linear function, giving slopes of (0.041±0.003)(0.041 \pm0.003) cm−1^{-1}/μm and (0.075±0.004)(0.075 \pm0.004) cm−1^{-1}/μm for the E2g1\mathrm{E}^{1}_{2g} and A1g\mathrm{A}_{1g} modes, respectively.

MoS$_2$ Raman spectroscopy mapping and spectra

Figure 3. MoS2_2 Raman spectroscopy mapping of the mode intensity, showing decrease in both a) in-plane E2g1^{1}_{2g} Raman mode and b) out-of-plane A1g_{1g} mode. c) Raman spectroscopy mapping of the E2g1^{1}_{2g}-A1g_{1g} distance, reflecting the different trend between the two Raman modes. d) Single Raman spectra of two distinct regions of the flake. The Raman shift is extracted along the white line from a) to show the gradient of the Raman shifts of e) E2g1^{1}_{2g} mode and f) A1g_{1g} mode. Their comparison shows that the A1g_{1g} mode is more sensitive to the changes.

The A1g\mathrm{A}_{1g} Raman mode, with larger gradient across the flake, is sensitive to doping density in MoS2\mathrm{MoS}_2, in contrary to the E2g1\mathrm{E}^{1}_{2g} mode which is not very affected by doping [5, 33]. Therefore, the analysis of the Raman modes mapped across the flake indicates that electron doping is the primary cause of the gradient, particularly in the bottom region. Tensile strain would not affect the out-of-plane A1g\mathrm{A}_{1g} mode to the extent [5] observed in Figure 3b. Further evidence of electron doping can be found in the increased Raman intensity of both modes in the bottom region. As the electron density (and A−^{-}-trion population) increases in the defective region, more phonons are generated in the scattering process, and a stronger Raman signal is observed in Figure 3a and 3b. Such Raman scattering enhancement contrasts with the PL quenching, but the increased electron density, originating from sulfur vacancies, suffices as an explanation for all the observed changes.

The observed Raman shifts of the A1g\mathrm{A}_{1g} vibrational mode can be utilized for quantitative estimate of the doping density variation in MoS2\mathrm{MoS}_2. Assuming a linear relationship Δω=α⋅Δn\Delta\omega= \alpha\cdot\Delta n with a proportionality coefficient of α=2.22\alpha= 2.22 cm−1^{-1}/1013^{13} cm−2^{-2} (based on literature reports [33, 34]), the net change in doping density across the studied MoS2\mathrm{MoS}_2 flake is estimated to 1.13×1013cm−21.13 \times10^{13} cm^{-2}. This value agrees with the reported range of values for CVD-grown MoS2\mathrm{MoS}_2 [11].

To confirm the origin of the observed gradient in the PL and Raman spectra of the MoS2\mathrm{MoS}_2 flake, power-dependent PL and Raman spectroscopy (single spectra) measurements were performed in both the defective and pristine region. Figure 4 shows the extracted peak intensities and energies (or Raman shifts), plotted against the excitation laser power in the range from 300 µW to 20 mW. The intensity and energy of the A exciton are plotted in Figure 4a) and 4b), respectively, with intensity and laser power plotted on a logarithmic scale. The PL intensity should follow the power law I∼PxI\sim P^x, where xx indicates the channel of energy dissipation [35]. The linear dependence in Figure 4a) corresponds to xx close to unity, indicating radiative exciton recombination. The defective region (blue curve) shows a loss of linearity at higher powers (see inset in Figure 4a)), indicating exciton recombination saturation. This suggests a change in exciton behaviour with respect to defect density. In Figure 4b), the A exciton energy shows a gradual red shift, as described elsewhere [36, 37]. This is caused by an increase in the exciton population, which results in bandgap renormalisation. There is also a thermal effect due to lattice heating caused by the increased laser power. However, this trend changes in the defective region for optical powers above 1 mW (emphasized in green), where the red shift rate increases compared to pristine MoS2\mathrm{MoS}_2. This might indicate a change in the energy dissipation channel. A suggested explanation is that the defect sites act as traps for photogenerated excitons. At low power, most of the excitons recombine radiatively without getting trapped. Above 1 mW of optical power, the defect traps become dominant and defect-mediated emission takes place, resulting in lattice heating. Such a change in local environment causes a bandgap renormalization, observed as an increase in red shift of the defective region.

Power dependence of the optical properties of MoS₂ flakes

Figure 4. Power dependence of the optical properties of MoS₂ flakes, comparing the pristine (red) and defective (blue) region. Intensity and optical power are plotted on a logarithmic scale. The green background indicates the high-power regime. a) The intensity of A exciton shows a linear trend with a slope of unity, indicating the excitonic emission. b) The energy red shift of A exciton is caused by the bandgap renormalization arising from the increased exciton density. This trend

is, however, more pronounced in the defective region due to defect traps dominating energy dissipation, leading to lattice heating. c) and e) The intensity of E2g1E^{1}_{2g} and A1gA_{1g} Raman modes in MoS2_2 increases proportionally to the incident laser power. d) and f) The Raman shift of the E2g1E^{1}_{2g} and A1gA_{1g} modes reflects the symmetry of the modes. The in-plane E2g1E^{1}_{2g} mode is not greatly affected by defects, whereas the out-of-plane A1gA_{1g} mode changes significantly with heat dissipation saturation in defect sites at high powers (green background). This is evident as a change in slope in the doped region, in contrast to the more stable pristine region.

Figure 4c) – Figure 4f) show the E2g1E^{1}_{2g} and A1gA_{1g} Raman modes, along with their intensity and Raman shift dependencies on laser power. The intensities (Figure 4c), 4e)) increase proportionally to the incident laser power, reflecting the increased phonon density. Defective region shows a subtle intensity increase compared to the pristine region, corresponding with the Raman intensity gradient in Figure 3. Remarkably, Figure 4d) and 4f) reflect a different nature of the E2g1E^{1}_{2g} and A1gA_{1g} modes. The E2g1E^{1}_{2g} peak is an in-plane vibrational mode and is not very sensitive to doping. Figure 4d) shows a fluctuation in Raman shift with laser power; however, the difference in defect density only introduces a small constant offset in the Raman shift. In Figure 4f), however, the power dependence of the A1gA_{1g} Raman shift exhibits two regimes (distinguished by green background). The first is a low-power regime in which the defective region remains unchanged from the pristine one. The second is a high-power regime (above 1 mW) in which the defective region exhibits a significant red shift in the Raman shift, notably deviating from the pristine region. This is consistent with the conclusion drawn from Figure 4b) that energy is dissipated into the lattice. Such local lattice heating softens the bonds and thus decreases the Raman shift. Pristine MoS2_2 shows a negligible shift in the A1gA_{1g} Raman shift with power, confirming that exciton recombination is sufficient. These observations confirm that sulfur vacancies (and corresponding electron density increase) are responsible for the change in optical properties of the MoS2_2 flakes.

Regarding the origin of the sulfur vacancy-density gradient in MoS2_2 flakes, this phenomenon can be attributed to (i) precursor depletion, (ii) local variations in the Mo:S ratio, or (iii) a temperature gradient. Although temperature can vary across the SiO2_2 substrate, ohmic heating from the outer chamber walls is not expected to produce such spatially localized gradients within a single flake. Furthermore, if a temperature gradient were responsible, neighbouring flakes would be expected to show an even larger shift in PL energy relative to the flake under study – this was not observed. Local variation in the Mo:S ratio offers another possible explanation; however, a molybdenum excess would be expected to change flake morphology. While such morphological changes are indeed observed at the wafer scale (a transition from triangular to hexagonal flakes with dendritic structures), no comparable variation is seen at the microscopic scale within a single MoS2\mathrm{MoS}_2 flake. This leaves precursor depletion as the most plausible explanation. As the gaseous sulfur precursor flows through the CVD chamber, it reaches the nucleation site via surface diffusion or direct adsorption, where it is progressively consumed during growth. This consumption leads to local sulfur depletion and, consequently, to the formation of sulfur vacancies in the direction of precursor flow. Supporting this interpretation, optical microscopy shows that upstream flakes are consistently larger than downstream ones (Supplementary Information, Figure S1), consistent with a higher local precursor concentration upstream relative to downstream. Altogether, these observations demonstrate that localized precursor depletion during CVD growth is the primary cause of the sulfur vacancy-density gradient in MoS2\mathrm{MoS}_2 flakes.

Large area optical image of the sample with MoS$_2$ flakes

Figure S1. Large area optical image of the sample with MoS2_2 flakes

Conclusion

In summary, we have demonstrated the spontaneous formation of a defect-density gradient in CVD-grown MoS2\mathrm{MoS}_2 monolayer flakes. Spatially resolved photoluminescence and Raman spectroscopy mapping reveal how the optical properties vary with defect density across a single flake. Detailed analysis of the spectroscopic data shows that these variations are driven by increasing electron density, which we attribute to a gradient in sulfur vacancy concentration. We propose that this gradient originates from directional precursor depletion near the nucleation site during growth. Together, these results establish a straightforward approach for producing MoS2\mathrm{MoS}_2 layers with tunable, spatially controlled defect density, offering potential opportunities for optoelectronic and catalytic applications such as hydrogen evolution.

Experimental details

Single-layer MoS2\mathrm{MoS}_2 was synthesized in a CVD chamber using a standard down-flow configuration, with sulfur powder placed in the upper heating zone and MoO3\mathrm{MoO}_3 powder in the lower zone, alongside the substrate positioned horizontally in a boat. Precursor amounts were set to m(S)=240m(\mathrm{S}) = 240 mg, m(MoO3)=4m(\mathrm{MoO}_3) = 4 mg, yielding large-area single-layer MoS2\mathrm{MoS}_2 flakes. Optical microscopy was performed using a 100×100 \times objective. Additional morphological characterization was carried out by scanning electron microscopy (Verios 360L, Thermo Fisher Scientific) in ultra-high resolution (UHR) mode using secondary electron contrast, and by atomic force microscopy (AFM, Bruker Dimension Icon) in ScanAsyst mode, with subsequent data analysis performed in Gwyddion software. Spectroscopic mapping was performed using a 532 nm continuous-wave laser with 10 mW optical power, focused to a 0.5 μm0.5\,\mu\mathrm{m} spot size through a 100×100 \times objective. Photoluminescence and Raman spectra were acquired using 150 and 600 lines/mm gratings, respectively. Maps were recorded at 64×6464 \times64 pixel resolution, with integration times of 0.1 s for photoluminescence and 2 s for Raman spectroscopy. Concerning power-dependent measurements, the laser power was adjusted using a rotatable gradual neutral density filter.

Acknowledgement

The authors gratefully acknowledge Prof. Yan-Wen Lan of the Department of Physics, National Taiwan Normal University, for providing laboratory facilities that made this study possible. Financial support from the National Science and Technology Council of Taiwan under Grant Nos. NSTC 114-2112-M-003-014 and NSTC 115-2112-M-003-007 is gratefully acknowledged. This work was also supported by the project "NEXT GENERATION BUT: Enhancing the Quality and Relevance of Education at BUT", funded as project No. CZ.02.02.XX/00/23_022/0009052 by Programme Johannes Amos Comenius. Additionally, CzechNanoLab Research Infrastructure (ID 90251), funded by MEYS CR, is gratefully acknowledged for the financial support of the measurements/sample fabrication. This work was also supported by the project CZ.02.01.01/00/22_008/0004594 TERAFIT. We acknowledge the support by the Czech Science Foundation (Grant No. 23-07617S).

Supplementary Information

In Supplementary Information, the gas flow direction is illustrated with optical microscope image across a large area of the sample surface.

Conflict of Interest

The authors have no conflict to disclose.

Author Contributions

M.K. performed the fabrication and sample analysis and wrote the manuscript, H.-S.C. and C.-Y.H. supported the experiments, Y.-R.C. contributed to the experiments, J.M. and M.B. contributed to the methodology and revised the manuscript, J.Š. assisted with experiments, T.Š. supervised the research project and W.-C.L. directed the entire study and revised the manuscript.

Data Availability

The datasets generated and analyzed during the current study are available in the Zenodo repository at https://doi.org/10.5281/zenodo.23949233.

Literature

Supplementary Information

Gas flow direction - OM image showing how the flakes change in the flow direction (white arrow). Up-stream flakes are bigger than down-stream. Gradient is oriented the same way as the gas flow. Defects are on the down-stream side.

References

  1. [2]Lin, Y. et al. Dielectric screening of excitons and trions in single-layer MoS2. Nano Lett. 14, 5569–5576 (2014).DOI
  2. [3]Castellanos-Gomez, A. et al. Local strain engineering in atomically thin MoS2. Nano Lett. 13, 5361–5366 (2013).
  3. [4]Moon, H. et al. Dynamic Exciton Funneling by Local Strain Control in a Monolayer Semiconductor. Nano Lett. 20, 6791–6797 (2020).DOI
  4. [5]Michail, A., Delikoukos, N., Parthenios, J., Galiotis, C. & Papagelis, K. Optical detection of strain and doping inhomogeneities in single layer MoS2. Appl. Phys. Lett. 108, (2016).DOI
  5. [6]Conley, H. J. et al. Bandgap engineering of strained monolayer and bilayer MoS2. Nano Lett. 13, 3626–3630 (2013).DOI
  6. [7]Okada, M., Okigawa, Y., Kubo, T., Nakajima, H. & Yamada, T. Strain Engineering of MoS2 by Tuning the Transfer Process. ACS Appl. Electron. Mater. 7, 3590–3598 (2025).DOI
  7. [8]Mouri, S., Miyauchi, Y. & Matsuda, K. Tunable photoluminescence of monolayer MoS2 via chemical doping. Nano Lett. 13, 5944–5948 (2013).DOI
  8. [9]Shu, K., Nguyen Do, L., Gao, W., Biscaras, J. & Shukla, A. Photoluminescence in single-layer MoS2: The role of impurities and doping. J. Appl. Phys. 138, (2025).DOI
  9. [10]Mak, K. F. et al. Tightly bound trions in monolayer MoS 2. Nat. Mater. 12, 207–211 (2013).
  10. [11]Hong, J. et al. Exploring atomic defects in molybdenum disulphide monolayers. Nat. Commun. 6, (2015).DOI
  11. [12]Abraham, J., Shepherd, N. D., Littler, C., Syllaios, A. J. & Philipose, U. Engineering the Morphology and Properties of MoS2 Films Through Gaseous Precursor-Induced Vacancy Defect Control. Nanomaterials 15, (2025).DOI
  12. [13]Abidi, I. H. et al. Oxygen Driven Defect Engineering of Monolayer MoS2 for Tunable Electronic, Optoelectronic, and Electrochemical Devices. Adv. Funct. Mater. 34, (2024).DOI
  13. [14]Jiang, W., Liu, L. & Xu, J. Improved detectivity and response speed of MoS2 phototransistors based on the negative-capacitance effect and defect engineering. Opt. Express 30, 46070 (2022).DOI
  14. [15]Ramanathan, A. A. Defect Functionalization of MoS2 nanostructures as toxic gas sensors: A review. in IOP Conference Series: Materials Science and Engineering vol. 305 (Institute of Physics Publishing, 2018).DOI
  15. [16]Nhiem, L. T., Khanh Linh, D. T., Nguyen, H. & Hieu, N. H. Defect-Driven MoS2 Nanosheets toward Enhanced Sensing Sensitivity. ACS Omega 9, 27065–27070 (2024).
  16. [17]Liu, X. et al. Lateral Heterostructures of Defect-Patterned MoS2 for Efficient Hydrogen Production. Small 21, (2025).DOI
  17. [18]Liu, L., Liu, N., Chen, B., Dai, C. & Wang, N. Recent Modification Strategies of MoS2 towards Electrocatalytic Hydrogen Evolution. Catalysts 14, (2024).DOI
  18. [19]Song, S. H., Joo, M. K., Neumann, M., Kim, H. & Lee, Y. H. Probing defect dynamics in monolayer MoS2 via noise nanospectroscopy. Nature Communications 8, (2017).DOI
  19. [20]Saha, A. K. & Yoshiya, M. Native point defects in MoS2 and their influences on optical properties by first principles calculations. Physica B Condens. Matter 532, 184–194 (2018).DOI
  20. [21]Li, H., Huang, M. & Cao, G. Markedly different adsorption behaviors of gas molecules on defective monolayer MoS2: A first-principles study. Physical Chemistry Chemical Physics 18, 15110–15117 (2016).DOI
  21. [22]Ye, G. et al. Defects Engineered Monolayer MoS2 for Improved Hydrogen Evolution Reaction. Nano Lett. 16, 1097–1103 (2016).DOI
  22. [23]Wang, X. et al. Single-Atom Vacancy Defect to Trigger High-Efficiency Hydrogen Evolution of MoS2. J. Am. Chem. Soc. 142, 4298–4308 (2020).DOI
  23. [24]Li, H. et al. Activating and optimizing MoS2 basal planes for hydrogen evolution through the formation of strained sulphur vacancies. Nat. Mater. 15, 48–53 (2016).DOI
  24. [25]Chen, Y. et al. Tuning Electronic Structure of Single Layer MoS2 through Defect and Interface Engineering. ACS Nano 12, 2569–2579 (2018).DOI
  25. [26]Yang, J. et al. Single Atomic Vacancy Catalysis. ACS Nano 13, 9958–9964 (2019).DOI
  26. [27]Nan, H. et al. Strong photoluminescence enhancement of MoS2 through defect engineering and oxygen bonding. ACS Nano 8, 5738–5745 (2014).DOI
  27. [28]Man, P. et al. Salt-Induced High-Density Vacancy-Rich 2D MoS2 for Efficient Hydrogen Evolution. Advanced Materials 36, (2024).DOI
  28. [29]Yang, R. et al. Progress and Challenges in the Synthesis of Two-Dimensional Lateral Heterostructures. Precision Chemistry 3, 492–515 (2025).DOI
  29. [30]Nawaz, M. Z. et al. Modern 2D Heterostructures: From Fabrication Challenges to Emerging Applications. Small Methods 10, 02365 (2026).DOI
  30. [31]Kundu, B. et al. Synthesis of lateral heterostructure of 2D materials for optoelectronic devices: challenges and opportunities. Emergent Mater. 4, 923–949 (2021).DOI
  31. [32]Liu, Z. et al. Strain and structure heterogeneity in MoS 2 atomic layers grown by chemical vapour deposition. Nat. Commun. 5, (2014).DOI
  32. [33]Chakraborty, B. et al. Symmetry-dependent phonon renormalization in monolayer MoS 2 transistor. Phys. Rev. B Condens. Matter Mater. Phys. 85, (2012).DOI
  33. [34]Kukuckska, G. & Koltai, J. Theoretical Investigation of Strain and Doping on the Raman Spectra of Monolayer MoS2. Phys. Status Solidi B Basic Res. 254, (2017).
  34. [35]Schmidt, T., Lischka, K. & Zulehner, W. Excitation-power dependence of the near-band-edge photoluminescence of semiconductors. Phys. Rev. B 45, 8989 (1992).pubmed.ncbi.nlm.nih.gov/10000759
  35. [36]Bhuyan, C. A., Madapu, K. K. & Dhara, S. Excitation-dependent photoluminescence intensity of monolayer MoS2: Role of heat-dissipating area and phonon-assisted exciton scattering. J. Appl. Phys. 132, (2022).DOI
  36. [37]Ko, P. J. et al. Laser power dependent optical properties of mono- and few-layer MoS2. J. Nanosci. Nanotechnol. 15, 6843–6846 (2015).pubmed.ncbi.nlm.nih.gov/26716254

Paper details

vlnc:W_c8s66j2u
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy