betaFeedback

WorksPhysics and Astronomy

Group-III doping of the p-type oxide SnO

Abstract

Al-, Ga-, and In-doped tin monoxide (SnO) films were grown by molecular beam epitaxy. Hall measurements reveal acceptor character of all investigated group-III dopants in SnO, which correspond to theoretical calculations and previous experiments for Ga and In, but contradicts theoretical calculations predicting donor character for Al in SnO. Doping concentrations of 10e18-1e22 cm-3 were tested and maximum hole concentrations of 2e19, 3e19, and 1e19 cm-3 with doping efficiencies of 3 percent, 9 percent, and 1 percent were found for Al, Ga, and In, respectively. The observed doping limit in the mid e19 cm-3 aligns with the limits observed in literature for different dopants, hinting to fundamental aspects of the SnO defect chemistry. Due to the unexpected Al acceptor behavior, we hypothesized Al1+ being present instead of Al3+. To stabilize the higher Al3+ oxidation state, another sample series of Al-doped SnO was grown in an oxidizing atmosphere. Despite the oxidizing atmosphere, these samples showed p-type character. A more complex defect chemistry is thus expected to explain the Al acceptor character.

© 2026 Author(s). All article content, except where otherwise noted, is licensed under a Creative Commons Attribution (CC BY) license (https://creativecommons.org/licenses/by/4.0/). https://doi.org/10.1063/5.0350201

Over the last few years, transparent semiconducting oxides (TSOs) have emerged as one of the fundamental building blocks for new device concepts and serve as a foundation for novel functional physical properties.[1, 2, 3, 4] More recently, TSOs are considered a promising material class for advanced memory architectures, in which they form an additional back-end-of-line (BEOL) compatible logic and memory layer.[5, 6] Until now, the use of TSOs has been restricted to devices using n-type doped oxides, inhibiting further development of transparent oxide-based homo-pn-junctions and CMOS technology. P-type conductivity remains a major bottleneck for TSOs, as the localized O 2p2p-derived valence bands, represented by low in energy and shallow valence-band maxima, lead to self-compensation and low possible hole mobilities. In contrast, the valence band of the α\alpha-phase of tin(II)monoxide (α\alpha-SnO\mathrm{SnO}), first grown by Pan and Fu,[7] mainly consists of Sn 5s5s orbitals, which are more disperse and higher in energy than O 2p2p orbitals. Hole mobilities ranging from 2 to 20 cm2/V s\mathrm{cm}^{2}/\mathrm{V\,s} measured by the Hall method have been reported in the literature,[6, 9, 10, 11, 12] and p-type-transistors have been realized.[6, 10, 13] Its low synthesis temperature makes SnO\mathrm{SnO} a suitable p-type TSO for BEOL application.[5, 9] The low electronic indirect bandgap of 0.6 eV[4, 14] does not inhibit transparency as this transition is optically forbidden, leading to a higher optical bandgap reported between 2.6 and 3.2 eV.[4] SnO\mathrm{SnO} shows thus the unique combination of a small electronic bandgap, opening the possibility for ambipolar doping[15, 16, 17, 18, 19] with a high optical bandgap, useful for transparent electronics. Undoped SnO\mathrm{SnO} naturally shows p-type behavior.[9, 14, 20] While the underlying mechanisms of intrinsic p-type conductivity are still under debate, density functional theory (DFT) calculations suggest the formation of Sn vacancies (VSnV_{\mathrm{Sn}}),[21, 22] including their complex with hydrogen impurities.[16]

Inspired by the possibility of p-doping SnO\mathrm{SnO} using Ga,[23, 24] Na,[24, 25, 26] K, or Y,[27] the realization of an all-SnO\mathrm{SnO}-based pn-junction emerged as a central topic. However, the search of a suitable n-type dopant turned out to be a challenging task with contradicting results. While Hosono et al. report successful n-doping by Sb,[28] Guo et al. report p-dopant behavior for Sb in SnO\mathrm{SnO}.[28] La was found to act as compensating donor dopant in SnO\mathrm{SnO},[23] making the material more insulating but not n-type conductive. As another promising candidate, Al has been theoretically predicted to show donor behavior,[19, 23] but no experimental Al-doping studies have been performed on phase-pure SnO\mathrm{SnO} yet. The Al-doping studies carried out on phase mixtures of SnO\mathrm{SnO} and the n-type conducting SnO2\mathrm{SnO}_{2} show conflicting data. Some groups report higher conductivity or mobility upon Al-doping,[29, 30] and another group reports compensating donor behavior.[31] Table 1 summarizes the above-mentioned experimental SnO\mathrm{SnO} doping studies.

References (First author (year))Doping elementUID hole density (cm−3^{-3})Maximum hole density (cm−3^{-3})Corresponding doping concentrationMobility (cm2^{2}/V s)Growth techniqueCrystallinityPhase composition
Guo et al. (2018)Y1.1×10181.1 \times10^{18}2.7×10182.7 \times10^{18}5 at. %0.6–0.9EBEPoly-crystallineSnO
Hosono et al. (2018)Sb1.1×10181.1 \times10^{18}1.3×10181.3 \times10^{18}5 at. %0.6–0.9EBEPoly-crystallineSnO
Liang et al. (2021)Sb2.5×10172.5 \times10^{17}n-type10 at. %2.3PLDSingle-crystallineSnO
Kwok et al. (2021)Y5.6×10165.6 \times10^{16}4.7×10164.7 \times10^{16}0.84 at. %0.8, 3.9EBEPoly-crystallineSnO
Kwok et al. (2021)Ga4.6×10184.6 \times10^{18}4.7×10184.7 \times10^{18}1.20%3.6SputteringPoly-crystallineSnO
Egbo et al. (2023)Na4.6×10184.6 \times10^{18}5×10195 \times10^{19}2.80%11–3SputteringPoly-crystallineSnO
Chae et al. [25]Ga6×1018−1×10196 \times10^{18} - 1 \times10^{19}1×10191 \times10^{19}5.3×10195.3 \times10^{19} cm−3^{-3}4–6MBESingle-crystallineSnO
Nguyen et al. (2025)La6×1018−1×10196 \times10^{18} - 1 \times10^{19}1.5×10191.5 \times10^{19}—3–7MBESingle-crystallineSnO
Pan et al. (2030)KNot providedNot provided1.1%1.85 (FE)MBEPoly-crystallineSnO + SnO2_2
Peek et al. (2031)AlNot providedNot provided1%1.17 (FE)SputteringPoly-crystallineSnO + SnO2_2
AlNot providedNot providedNot providedNot providedALDPoly-crystallineSnO + SnO2_2

Table 1. TABLE I. Previously published doping studies of SnO. Used doping element, unintentionally doped (UID) hole charge carrier density, maximum hole charge carrier density reached by doping, corresponding doping concentration, hole mobility, growth technique, and crystallinity and phase composition of the samples. While most studies report the Hall mobility, the two Al-doping studies report the field-effect mobility, marked by (FE) in the table.

In this work, we comparatively explore doping of molecular beam epitaxy (MBE)-grown phase-pure SnO\mathrm{SnO} by the group-III elements Al, Ga, and In. Ga and In are both predicted by ab initio

t1

calculations to act as acceptors.[19, 23] The acceptor character of Ga has additionally been shown experimentally,[23] while no experimental data on In-doping has been published yet. As Al is predicted to act as donor,[19] it is of special interest for ambipolar doping of SnO.

Unintentionally doped (UID), Al-, Ga-, and In-doped, 30–55 nm-thick SnO films were grown on 5×5×0.55 \times5 \times0.5 mm3^{3} single-side polished, yttrium-stabilized zirconia (YSZ) (001) substrates, known to enable epitaxy of single-crystalline SnO(001),[20] by suboxide molecular beam epitaxy (S-MBE). To prepare well-defined, epi-ready substrate surfaces, the YSZ substrates were wiped with a cotton swab in an isopropanol bath and subsequently baked out for 1 h at 1050 °C in a tube furnace, supplying 150 sccm O2_2 flux. As a consequence of the annealing procedure, all substrates showed a step-terrace surface, as shown in Fig. S18 of the supplementary material. The step height of around 0.5 nm is in accordance with the lattice constant of the YSZ substrate of 0.51 nm, indicating singly terminated and epi-ready surfaces. All substrates received an SrRuO3_3 backside coating prior to growth for homogeneous heat absorption from the substrate heater.

For the S-MBE growth process, an SnO suboxide source containing an Al2_2O3_3 crucible filled with a mixture of SnO2_2 and Sn was used.[9, 32] The primary flux species for the (SnO2_2 + Sn) cell is SnO and its oligomers, ensuring a perfect stoichiometry of the grown films. The (SnO2_2 + Sn) cell temperature was kept at 850 °C and the hot-lip at 950 °C, leading to beam equivalent pressures (BEPs) of (0.8−1.4)×10−7(0.8 - 1.4) \times10^{-7} mbar, which correspond to growth rates in the range of 0.5–0.8 nm/min. The doping of the SnO layers was achieved by the co-deposition of the respective dopant element evaporated from an elemental source material. The necessary dopant cell temperatures to achieve a nominal dopant concentration in the film between 1×10181 \times10^{18} and 1×10221 \times10^{22} cm−3^{-3} were extrapolated from temperature-dependent BEP measurements at higher cell temperatures, as explained in the supplementary material. The corresponding cell temperatures for the Al, Ga, and In cells were 700–1000, 530–620, and 475–575 °C, respectively. The substrate temperature (TsubT_{\mathrm{sub}}) was measured by a thermocouple located behind the substrate heater and kept at 375 °C for the Al- and the In-doped samples and at 400 °C for the Ga-doped samples. In the earlier Ga-doping study published by our group,[23] the doping series grown by the plasma-assisted MBE was grown at Tsub=350T_{\mathrm{sub}} = 350 °C, while the doping series grown by the suboxide MBE was grown at Tsub=400T_{\mathrm{sub}} = 400 °C. As no substantial difference in the doping behavior of Ga is observed between these two series, we believe the Ga-doping at Tsub=400T_{\mathrm{sub}} = 400 °C in the present study to adequately represent the Ga-doping behavior at Tsub=375T_{\mathrm{sub}} = 375 °C. During SnO deposition, the growth chamber pressure was below 5×10−95 \times10^{-9} mbar, confirming the absence of parasitic oxygen emission from the suboxide source. The growth was in situ monitored by reflection high-energy electron diffraction (RHEED) (see Fig. S1 of the supplementary material).

For electrical characterization, the films were contacted by In-coated Cu-probes and measured in van der Pauw geometry.[33] A magnetic field of ±800\pm800 mT and currents in the range of 50–100 μA were used. For the analysis of the crystal structure, a four-circle x-ray lab-diffractometer (X’Pert Pro MRD, Philips PANalytical) using Cu Kα_{\alpha} radiation was used. Symmetric out-of-plane 2θ−ω2\theta-\omega scans and rocking curves of the SnO 002 reflection were taken using a 1/2∘1/2^\circ entrance slit and a 1 mm detector slit. Additionally, high-resolution scans of the SnO 002 reflection were performed using an analyzer crystal. The The sample thickness tt is determined from the thickness fringes of the high-resolution XRD scans (marked with *), determined from the thickness fringes at the high-resolution XRD scans (marked with *), respectively, of the supplementary material.

Doping elementTcellT_{\mathrm{cell}} (°C)NDN_D (cm−3^{-3})TsubT_{\mathrm{sub}} (°C)SnO BEP (10−710^{-7} mbar)tt (nm)dqd_q (nm)ρ\rho (Ω cm)QHallQ_{\mathrm{Hall}} (Ω/T)μ\mu (cm2^2/V s)ρHall\rho_{\mathrm{Hall}} (Ω cm)Δω\Delta\omega (°)Δ2Θ\Delta2\Theta (°)rr (nm)
UID…04000.9305+68.314.71.91.100.183.1 × 1018^{18}8 × 1017^{17}
…03751.34510+75.217.54.61.030.111.3 × 1018^{18}3 × 1017^{17}
…1.4 × 1018^{18}3751.25510+80.013.04.60.960.171.4 × 1018^{18}3 × 1017^{17}
Al7008.7 × 1018^{18}3751.242*10+30.46.44.80.350.064.9 × 1018^{18}2 × 1018^{18}
7504.7 × 1019^{19}3751.25010+13.91.44.10.170.039.0 × 1018^{18}2 × 1018^{18}
8002.2 × 1020^{20}3751.25110+6.00.24.10.080.042.2 × 1019^{19}4 × 1018^{18}
8508.8 × 1020^{20}3751.3565+4.60.31.90.130.012.4 × 1019^{19}4 × 1018^{18}
9001.7 × 1021^{21}3751.151*10+8.50.71.50.320.061.3 × 1019^{19}3 × 1018^{18}
9253.2 × 1021^{21}3751.157*10+14.03.91.40.570.107.8 × 1018^{18}3 × 1018^{18}
9501.0 × 1022^{22}3751.15510+34.66.33.10.330.066.0 × 1018^{18}1 × 1018^{18}
Ga5303.3 × 1018^{18}4000.9305+10.00.63.90.080.012.1 × 1019^{19}4 × 1018^{18}
5601.1 × 1020^{20}4000.9305+9.70.23.80.060.012.9 × 1019^{19}5 × 1018^{18}
5903.6 × 1021^{21}4000.9305+9.10.94.20.070.011.0 × 1019^{19}5 × 1018^{18}
6201.0 × 1021^{21}4000.9305+7.911.74.30.440.053.3 × 1018^{18}4 × 1018^{18}
In4758.6 × 1018^{18}3751.134*5+41.90.62.60.250.039.7 × 1018^{18}1 × 1018^{18}
5255.2 × 1020^{20}3751.1455+13.71.31.00.500.051.2 × 1019^{19}2 × 1018^{18}
5752.6 × 1021^{21}3751.1475+10.112.74.70.590.054.1 × 1018^{18}2 × 1018^{18}
Al in O2_2…8.7 × 1018^{18}7501.2505+50.34.04.50.340.134.6 × 1018^{18}7 × 1017^{17}
…2.2 × 1020^{20}8501.1375+41.41.03.60.040.011 × 1019^{19}1 × 1019^{19}
…8.8 × 1020^{20}9001.14510+34.61.32.50.160.041.6 × 1019^{19}4 × 1018^{18}

Table 2. Overview of growth parameters and characterization results of all unintentionally doped (UID), Al-, Ga, and In-doped samples discussed in this work. Doping cell temperature TcellT_{\mathrm{cell}}, nominal doping NDN_D, substrate temperature TsubT_{\mathrm{sub}}, beam equivalent pressure of the (SnO2_2 + Sn) source, Hall resistance ρHall\rho_{\mathrm{Hall}}, hole mobility μHall\mu_{\mathrm{Hall}}, resistance ρ\rho, full width at half maximum of the XRD rocking curves Δω\Delta\omega and Δ2Θ\Delta2\Theta, respectively, and the XRD scans (marked with *), determined from the thickness fringes at the high-resolution XRD scans (marked with *), respectively, of the supplementary material.

SnO layer thicknesses were determined from thickness fringes observed in high-resolution x-ray diffraction (HR-XRD) or by x-ray reflectivity (XRR) if no fringes were observed, as shown in Figs. S9 and S13–S17 of the supplementary material, respectively. The surface morphology was determined by atomic force microscopy (AFM) in peak force tapping mode using a Bruker Dimension Edge. Energy-dispersive x-ray spectroscopy (EDX) measurements were performed in a scanning electron microscope using an EDAX Octane Elect Super detector on selected samples with the highest doping concentrations. To account for contributions from both the thin film and substrate material in the depth probed, the dopant concentrations were obtained from measurements at different acceleration voltages and analyzed using a standards-based quantification routine implemented in the software BadgerFilm.[34] Spectra were acquired over 13×16 μm213 \times16\ \mu\mathrm{m}^{2} areas to average out any lateral variations. Further details on this quantification routine and related challenges can be found in section IV of the supplementary material. Table II provides an overview of the grown and investigated samples along with growth parameters and characterization results.

All investigated samples exhibit positive Hall resistances, as shown in Table II, demonstrating the p-type character irrespective of the dopant used in this study. Figure 1(a) summarizes the measured hole density of the Al-, Ga-, and In-doped SnO as function of nominal dopant concentration. The purple horizontal lines mark the measured hole densities of the two unintentionally doped (UID) SnO reference samples, with the purple shaded area describing their error. These UID hole concentrations are higher compared to values of other groups who achieve UID hole concentrations down to 1017 cm−310^{17}\ \mathrm{cm}^{-3}[25, 28] and 1016 cm−310^{16}\ \mathrm{cm}^{-3}[14] After this study, we replaced the source material by a fresh SnO2+Sn\mathrm{SnO}_{2}+\mathrm{Sn} mixture and observed lower unintentional hole concentrations in the mid-1017 cm−310^{17}\ \mathrm{cm}^{-3}. Consequently, we attribute the higher UID hole concentration of the present doping study to a cross contamination of the source material with acceptor dopant species. More importantly, Figure 1(a) shows that the hole concentration of the Al-, Ga-, and In-doped films increases with the nominal dopant concentrations up to a certain maximum value shown in Table III, proving acceptor dopant type behavior for all the tested group-III dopants.

Hole transport properties determined by Hall measurements

Figure 1. Hole transport properties determined by Hall measurements as function of the nominal doping with Al- (blue diamonds), Ga- (green stars), In- (brown pentagons), and unintentionally doped SnO samples (purple shaded area). (a) Hole density. For comparison, the gray line denotes the nominal acceptor density. Error of the nominal doping concentration determined by the EDX shows exemplarily for the highest doped samples (see supplementary material section IV, EDX). (b) Hole mobility. (c) Resistivity.

Doping elementHighest measured hole density (cm−3^{-3})Nominal doping (cm−3^{-3})Doping efficiencyEAE_A (meV)
Al(2.3±0.4)×1019(2.3 \pm0.4) \times10^{19}8.8×10208.8 \times10^{20}3.3%100
Ga(3.0±0.5)×1019(3.0 \pm0.5) \times10^{19}3.5×10203.5 \times10^{20}8.5%60
In(1.2±0.2)×1019(1.2 \pm0.2) \times10^{19}2.6×10212.6 \times10^{21}0.5%160

Table III. Highest measured hole density and respective nominal doping for Al-, Ga-, and In-doped samples. Furthermore, doping efficiency and acceptor activation energy EAE_A calculated from these values using the charge balance equation Eq. (1).

In terms of dopant type, these findings are qualitatively in line with theoretical predictions for Ga and In (i.e., being present in the Ga1+/In1+\mathrm{Ga}^{1+}/\mathrm{In}^{1+} state on the Sn2+\mathrm{Sn}^{2+} site),[23] yet contradict the theoretical prediction of Al to act as a donor (i.e., being present in the Al3+\mathrm{Al}^{3+} state on the Sn2+\mathrm{Sn}^{2+} site).[23] For Ga-doping, our results are quantitatively in line with previous experimental reports: The maximum hole concentration of (2.9±0.5)×1019 cm−3(2.9 \pm0.5) \times10^{19}\ \mathrm{cm}^{-3} shown here aligns well with the value of 5×1019 cm−35 \times10^{19}\ \mathrm{cm}^{-3} found in the literature,[23, 24] proving the reproducibility and validity of this study. Indium, showing the lowest doping efficiency, contrasts theoretical calculations, which predict In to be a more effective dopant than Ga and Al.[23] In addition to the highest measured hole concentration and the respective nominal doping concentrations for each dopant element, Table III summarizes their ratio as corresponding doping efficiency and a dopant activation energy EAE_A derived from the charge balance equation for incomplete ionization of singly ionized acceptors.[35]

p≈NANV2exp⁡(−EA2kBT),(1)p \approx\sqrt{\frac{N_A N_V}{2}}\exp\left(-\frac{E_A}{2k_{\mathrm{B}}T}\right), \tag*{(1)}

where NAN_A denotes the acceptor concentration, NVN_V the effective valence band density of states, kBk_{\mathrm{B}} the Boltzmann constant, and TT the temperature. NVN_V is calculated from

NV=2(2πmh∗kBTh2)3/2,(2)N_V = 2\left(\frac{2\pi m_h^* k_{\mathrm{B}}T}{h^2}\right)^{3/2}, \tag*{(2)}

assuming a density-of-state hole effective mass of mh∗=1.7⋅mem_h^* = 1.7 \cdot m_e. The low doping efficiency and corresponding high acceptor activation energy around 100 meV suggests Al, Ga, and In to be deep acceptors in SnO. This calculation of the acceptor activation energy assumes complete electrical activation of all dopant atoms. The difference between the measured hole concentration and the nominal dopant concentration may, however, also arise from incomplete dopant activation due to incorporation in electrically inactive configurations, such as interstitial sites or dopant clusters.

Beyond a nominal doping concentration of mid–high 1020 cm−310^{20}\ \mathrm{cm}^{-3} the measured hole density decreases for Al and Ga. Egbo et al. attribute the saturation of the measured hole density beyond a specific doping concentration to an incomplete ionization of the dopants due to pinning of the Fermi level at an e(+/0)e(+/0) charge transition level of GaSn\mathrm{Ga}_{\mathrm{Sn}} near the valence band edge. The formation of secondary phases for even higher doping concentrations could explain the decrease in the measured hole density. The drop in measured hole density is accompanied by a drop of the mobility for Al- and In-doping and an increase in the resistivity [Figs. 1(b) and 1(c), respectively]. Notably, the electrical characterization indicates a constant mobility of ≈4.2 cm2/V s\approx4.2\ \mathrm{cm}^2/\mathrm{V\,s} for Al doped samples in the range of 101810^{18}–1020 cm−310^{20}\ \mathrm{cm}^{-3}.

The highest hole concentration reached by Ga-doping as well as K-25 and Na-doping24 of (2(2–5)×1019 cm−35) \times10^{19}\ \mathrm{cm}^{-3} suggest a hole concentration limit of mid 1019 cm−310^{19}\ \mathrm{cm}^{-3} intrinsic to SnO and independent of the dopant element (compare Table I). Practically posing a limit to the conductivity of SnO, this limit could help gaining more insights into fundamental aspects of the controversially discussed defect chemistry of SnO, requiring further investigation.

As described earlier, we experimentally observed the acceptor character of Al in contradiction to its theoretically predicted donor character. Graužiņytė et al. predicted the incorporation of Al3+\mathrm{Al}^{3+} on the Sn2+\mathrm{Sn}^{2+} site.[19, 23] As the “most straightforward” explanation for the observed p-type character, we considered the incorporation of Al1+\mathrm{Al}^{1+} instead of Al3+\mathrm{Al}^{3+}. A more detailed reasoning for this assumption can be found in section III of the supplementary material. In an attempt to facilitate the incorporation of Al3+\mathrm{Al}^{3+}, we grew another sample series of Al-doped SnO in O2_2 environment, aiming at pre-oxidizing the elemental Al0\mathrm{Al}^{0} to Al3+\mathrm{Al}^{3+}. For this purpose, an O2_2 background pressure of 2×10−52 \times10^{-5} mbar was established by flowing 2 sccm of molecular oxygen into the growth chamber. These conditions should be able to oxidize all provided Al at the growth front to Al2_2O3_3, as we have shown in a separate experiment where even a lower O2_2 flow rate of 0.3 sccm was able to oxidize Al at a growth rate of 0.6 nm/min (will be published). Lee et al. showed that an O2_2-background during growth has a low influence on the hole density of undoped SnO.[11]

Figure 2(a) compares the measured hole densities for the Al-doped SnO films grown in vacuum and in oxygen. Also the Al-doped

Comparison of the electronic properties determined by Hall measurements

Figure 2. Comparison of the electronic properties determined by Hall measurements of Al-doped SnO grown in vacuum (blue diamonds) and in 2×10−52 \times10^{-5} mbar O2_2 atmosphere (pink triangles). The blue and pink shaded areas mark the values for the unintentionally doped samples grown in vacuum and the O2_2 atmosphere, respectively. (a) Hole density. (b) Hole mobility. (c) Resistivity.

SnO films grown in oxygen atmosphere show p-type behavior. The measured hole density over the nominal doping concentration follows the same trend as for the series grown in vacuum. Furthermore, the differences in hole mobility and resistivity between the samples grown in vacuum and oxygen atmosphere Figure 2(b) and Figure 2(c) are within the error bars. It is followed that, contrarily to theoretical predictions,[19, 23] Al acts as an acceptor in SnO, even if the Al3+\mathrm{Al}^{3+} oxidation state should be supported by an oxygen growth atmosphere. This behavior calls for further study of the SnO defect chemistry beyond the scope of the present work to clarify its origin. Given the high oxidation potential of Al,[36] incomplete oxidation seems unlikely and a more complex defect reaction is assumed. For example, the complex of an Al3+\mathrm{Al}^{3+}-interstitial defect with two tin vacancies would act as a singly charged acceptor (Ali3++2VSn2−→[Ali−2VSn]−\mathrm{Al}_{i}^{3+} + 2V_{\mathrm{Sn}}^{2-} \rightarrow[\mathrm{Al}_{i} - 2V_{\mathrm{Sn}}]^{-}). A similar defect complex is proposed by Guo et al. for Sb- or Y-doping.[28]

For completeness, the structural properties of the layers are discussed: Figure 3 shows XRD symmetric out-of-plane 2θ2\theta–ω\omega scans of the undoped and doped samples. The x-ray diffractograms of all films show the characteristic SnO 001 and 002 reflections at 18.3∘18.3^{\circ} and 37.1∘37.1^{\circ}, respectively, additionally to the YSZ 002 substrate reflection at 34.9∘34.9^{\circ}. The absence of further reflections confirms the presence of single-phase SnO (001) layers. Only for the highest Al- and In-doping concentrations, an additional reflection at 30.7∘30.7^{\circ} arises, which we attribute to the Sn 200 reflection in accordance with the hypothesis of elemental Sn-clusters being present in the highly doped SnO films, as discussed in section III of the supplementary material. The SnO 002 reflection of the highest Al-doped sample shows a broad shoulder toward higher diffraction angle, indicating the presence of Al–Sn–O-related secondary phases. The full width at half maximum (FWHM) of the ω\omega rocking curves of the SnO 002 reflection, shown in Fig. S10 of the supplementary material, are in the range of 0.1∘0.1^{\circ}–0.4∘0.4^{\circ} for Al-, Ga-, and In-doping up to 1021 cm−310^{21}\ \mathrm{cm}^{-3} and show no correlation with the nominal doping. These FWHM values are on the lower side of the ones reported in the literature,[11, 14, 20] indicating the high crystalline quality of the grown samples. For Al concentrations above 1021 cm−310^{21}\ \mathrm{cm}^{-3}, the FWHM increases up to 0.8∘0.8^{\circ}, indicating structural deterioration. AFM images of the samples are shown and discussed in section VIII of the supplementary material, and their root mean square roughness is shown in Table II.

X-ray diffraction symmetric out-of-plane scans of undoped and doped SnO samples

Figure 3. X-ray diffraction (XRD) symmetric out-of-plane 2θ2\theta–ω\omega scans of an unintentionally doped SnO sample (black), the Al-doped (blue), Ga-doped (green), In-doped (brown), and Al-doped samples grown in the oxygen atmosphere (pink). The nominal doping concentration is noted on the right side of the graph for each sample. Some samples show the Al 200 reflection, marked with *. A remeasured sample not showing the Al 200 reflection can be found in Fig. S8 of the supplementary material.

f3

In summary, the doping of MBE-grown SnO by the group-III elements Al, Ga, and In is compared. SnO was evaporated from an (SnO2+Sn)(\mathrm{SnO}_{2} + \mathrm{Sn})-source, while the doping elements were evaporated from elemental sources. In-line with theoretical predictions, Ga and In are acceptors and their incorporation leads to an increased hole concentration. In contrast to its theoretically predicted donor character, Al also leads to an increased hole concentration and is thus experimentally shown to act as an acceptor. The attempt to facilitate an Al3+\mathrm{Al}^{3+} donor state by deposition in a background of molecular oxygen did not change its acceptor character, pointing toward a more complex defect chemistry of Al-doping. While dopant concentrations up to at least 1021 cm−310^{21}\ \mathrm{cm}^{-3} were incorporated, the corresponding hole concentrations never exceeded 3×1019 cm−33 \times10^{19}\ \mathrm{cm}^{-3}. The highest hole concentration and doping efficiency was found for Ga. The observed hole concentration limit, roughly in-line with further literature reporting maximum hole concentrations below $5 \times 10^{19}\ \mathrm{cm}^{-3},[23, 24, 25] summarized in Table I, could provide valuable information for the controversially discussed defect chemistry of SnO.

See the supplementary material for RHEED images of a substrate and a sample, additional information on the calculation of the nominal doping, further discussion on the assumed Al-doping mechanism, a description of the EDX procedure, the hole mobility plotted vs the hole concentration, further XRD measurements, XRR measurements and their fits for sample thickness determination, and AFM measurements of a substrate and several samples, including their discussion.

The authors thank H.-P. Schönherr and C. Hermann for their MBE support, and A. Gilbert for critically reading the manuscript. Our research was funded by the Federal Ministry of Research, Technology, and Space and the Berlin Senate.

l

c1

c2

c3

c4

c5

c6

c7

c8

c9

c10

c11

c12

c13

c14

c15

c16

c17

c18

c19

c20

c21

c22

AUTHOR DECLARATIONS

Conflict of Interest

The authors have no conflicts to disclose.

Author Contributions

N. Gutmann: Conceptualization (supporting); Data curation (supporting); Formal analysis (lead); Investigation (lead); Methodology (equal); Project administration (equal); Validation (equal); Visualization (lead); Writing – original draft (lead); Writing – review & editing (equal). G. Hoffmann: Data curation (supporting); Investigation (supporting); Project administration (supporting); Supervision (supporting); Validation (lead); Writing – review & editing (equal). A. F. Campbell: Formal analysis (supporting); Investigation (supporting); Methodology (supporting); Software (lead); Validation (supporting); Writing – original draft (supporting); Writing – review & editing (supporting). J. Lähnemann: Formal analysis (supporting); Methodology (supporting); Software (supporting); Validation (supporting); Writing – review & editing (supporting). O. Bierwagen: Conceptualization (lead); Data curation (lead); Formal analysis (supporting); Methodology (equal); Project administration (equal); Supervision (lead); Validation (equal); Writing – review & editing (equal).

DATA AVAILABILITY

The data that support the findings of this study are available within the article and its supplementary material. Hall- and XRD-raw data were generated at the NOMAD large scale facility. Derived data supporting the findings of this study are available from the corresponding author upon reasonable request.

References

  1. [1]M. Rath, M. Mezhoud, M. Upadhyay, X. Portier, S. Duprey, P. Marie, J. Cardin, C. Labbé, F. Gourbilleau, S. Hurand, A. Cheikh, A. David, A. Fouchet, W. Prellier, and U. Lüders, “Impact of strongly correlated conduction electrons on the functional properties of the transparent conducting oxide SrVO₃,” Adv. Mater. Interfaces 13, e01094 (2026).
  2. [2]M. Mohammdi, F. Ji, T. Sachsewerger, K. Meraji, S. Parayil Shaji, and W. Tress, “Integrated memristor for mitigating reverse-bias in perovskite solar cells,” Nature 651, 933–939 (2026).
  3. [3]Z. Fang, L. Ding, Y. Yang, X. Gu, H. Li, H. Chen, Y. Yin, W. Wang, X. Wu, Z. Rao, L. Ning, D. Yang, H. Zhang, Y. Long, W. Li, F. Zhang, S. Xia, L. Jia, C. Liu, B. Li, B. Liu, S. Ju, W. Du, H. Zhang, Y. Qin, X. Ru, Y. Xu, Y. Lu, Y. He, Z. Li, X. Xu, M. Qu, B. He, J. Liu, and X. Zhang, “Flexible perovskite/silicon tandem solar cell with a dual-buffer layer,” Nature 649, 65–72 (2026).DOI
  4. [4]K. H. L. Zhang, K. Xi, M. G. Blamire, and R. G. Egdell, “P-type transparent conducting oxides,” J. Phys.: Condens. Matter 28, 383002 (2016).
  5. [5]Y.-M. Lin, C.-C. Lu, C.-H. Wu, C.-C. Kuo, E. Ambrosi, Y.-C. Shih, H.-K. Peng, S.-C. Lai, K.-I. Goto, H.-Y. Huang, F.-C. Chu, C.-Y. Chang, Y.-C. Ho, M.-Y. Chuang, G. Doornbos, G. Vellianitis, P. Rincon, M. Van Dal, K. H. Chiang, K. Bao, F.-C. Yang, C.-T. Lin, and M. Cao, “Oxide semiconductor: Technology and applications,” in IEEE International Electron Devices Meeting (IEDM) (IEEE, San Francisco, CA, 2025), pp. 1–4.
  6. [6]C. Wang, C. Kuo, C. Wu, A. Lu, H. Lee, C. Hsu, P. Tzeng, T. Lee, F. Hou, M. Chang, S. Lai, K. Goto, S. Yu, C. Wu, C. Lin, Y. Lin, and X. Bao, “P-type SnO semiconductor transistor and application,” in IEEE Symposium on VLSI Technology and Circuits (VLSI Technology and Circuits) (IEEE, Honolulu, HI, 2024), pp. 1–2.
  7. [7]X. Pan and L. Fu, “Tin oxide thin films grown on the (1012) sapphire substrate,” J. Electroceram. 7, 35–46 (2001).DOI
  8. [9]K. Egbo, E. Luna, J. Lähnemann, G. Hoffmann, A. Trampert, J. Grümbel, E. Kluth, M. Feneberg, R. Goldhahn, and O. Bierwagen, “Epitaxial synthesis of unintentionally doped p-type SnO (001) via suboxide molecular beam epitaxy,” J. Appl. Phys. 133, 045701 (2023).DOI
  9. [10]E. Fortunato, R. Barros, P. Barquinha, V. Figueiredo, S.-H. K. Park, C.-S. Hwang, and R. Martins, “Transparent p-type SnOₓ thin film transistors produced by reactive RF magnetron sputtering followed by low temperature annealing,” Appl. Phys. Lett. 97, 052105 (2010).DOI
  10. [11]S. Lee, A. S. Park, E. Kryskо, C. F. C. Chang, C. Du, V.-A. Ha, F. Giustino, X. Pan, D. Jena, H. G. Xing, and D. G. Schlom, “Tuning the electrical properties of unintentionally doped epitaxial p-type α-SnO thin films while maintaining a shallow hole ionization energy,” APL Mater. 14, 071103 (2026).
  11. [12]M. Minohara, A. Samizo, N. Kikuchi, K. K. Bando, Y. Yoshida, and Y. Aiura, “Tailoring the hole mobility in SnO films by modulating the growth thermodynamics and kinetics,” J. Phys. Chem. C 124, 1755–1760 (2020).DOI
  12. [13]H. Yabuta, N. Kaji, R. Hayashi, H. Kumomi, K. Nomura, T. Kamiya, M. Hirano, and H. Hosono, “Supporting formation of p-type SnO thin-film transistors on glass toward oxide complementary circuits,” Appl. Phys. Lett. 97, 072111 (2010).
  13. [14]A. B. Mei, L. Miao, M. J. Wahila, G. Khalsa, Z. Wang, M. Barone, N. J. Schreiber, L. E. Noskin, H. Paik, T. E. Tiwald, Q. Zheng, R. T. Haaasch, D. G. Sangiorgi, L. F. J. Piper, and D. G. Schlom, “Adsorption-controlled growth and properties of epitaxial SnO films,” Phys. Rev. Mater. 3, 105202 (2019).
  14. [15]N. F. Quackenbush, J. P. Allen, D. O. Scanlon, S. J. Sallis, J. A. Hewlett, A. S. Nandur, B. Chen, K. E. Smith, C. Weiland, D. A. Fischer, J. C. Wojcik, B. E. White, G. W. Watson, and L. F. J. Piper, “Origin of the bipolar doping behavior of SnO from X-ray spectroscopy and density functional theory,” Chem. Mater. 25, 3114–3123 (2013).
  15. [16]J. B. Varley, A. Schleife, A. Janotti, and C. G. Van de Walle, “Ambipolar doping in SnO,” Appl. Phys. Lett. 103, 082118 (2013).DOI
  16. [17]L. Yan Liang, H. Tao Cao, X. Bo Chen, Z. Min Liu, F. Zhuge, H. Luo, J. Li, Y. Cheng Lu, and W. Lu, “Ambipolar inverters using SnO thin-film transistors with balanced electron and hole mobilities,” Appl. Phys. Lett. 100, 263502 (2012).
  17. [18]H. Hosono, Y. Ogo, H. Yanagi, and T. Kamiya, “Bipolar conduction in SnO thin films,” Electrochem. Solid State Lett. 14, H13 (2011).
  18. [19]M. Graunitz, S. Goedecker, and J. A. Flores-Livas, “Towards bipolar tin monoxide: Revealing unexplored dopants,” Phys. Rev. Mater. 2, 104604 (2018).DOI
  19. [20]M. Budde, P. Mazzolini, J. Feldl, C. Golz, T. Nagata, S. Ueda, G. Hoffmann, F. Hatami, W. T. Masselink, M. Ramsteiner, and O. Bierwagen, “Plasma-assisted molecular beam epitaxy of SnO(001) films: Metastability, hole transport properties, Seebeck coefficient, and effective hole mass,” Phys. Rev. Mater. 4, 124602 (2020).DOI
  20. [21]A. Togo, F. Oba, I. Tanaka, and K. Tatsumi, “First-principles calculations of native defects in tin monoxide,” Phys. Rev. B 74, 195128 (2006).
  21. [22]J. P. Allen, D. O. Scanlon, L. F. J. Piper, and G. W. Watson, “Understanding the defect chemistry of tin monoxide,” J. Mater. Chem. C 1, 8194 (2013).DOI
  22. [23]K. Egbo, J. Lähnemann, A. Falkenstein, J. Varley, and O. Bierwagen, “Acceptor and compensating donor doping of single crystalline SnO (001) films grown by molecular beam epitaxy and its perspectives for optoelectronics and gas-sensing,” Appl. Phys. Lett. 122, 122101 (2023).DOI
  23. [24]C. K. G. Kwok, Y. Wang, K. Egbo, and K. M. Yu, “Improving the p-type conductivity and transparency of pure phase SnO by Ga and Na doping,” J. Phys. Chem. C 126, 18963–18971 (2022).DOI
  24. [25]S. Chae, S. Lee, A. Park, M. K. I. Senevirathna, Y. Feng, V. Kanneboina, V.-A. Ha, Y. Hu, C. Du, M. Barone, V. Protasenko, Y. E. Li, N. Podraza, K. Johnson, D. Jena, H. G. Xing, X. Pan, K. Cho, F. Giustino, M. D. Williams, and D. G. Schlom, “Controlling the p-type conductivity of α-SnO thin films by potassium doping,” APL Mater. 13, 101114 (2025).
  25. [26]L. Qin, S. Yuan, Z. Chen, X. Bai, J. Xu, L. Zhao, W. Zhou, Q. Wang, J. Chang, and J. Sun, “Solution-processed transparent p-type orthorhombic K doped SnO films and their application in a phototransistor,” Nanoscale 14, 13763–13770 (2022).DOI
  26. [27]L. Y. Liang, Z. M. Liu, H. T. Cao, W. Y. Xu, X. L. Sun, H. Luo, and K. Cang, “The structural, optical and electrical properties of Y-doped SnO thin films and their p-type TFT application,” J. Phys. D 45, 085101 (2012).
  27. [28]W. Guo, L. Fu, Y. Zhang, X. Zhang, L. Y. Liang, Z. M. Liu, H. T. Cao, and X. Q. Pan, “Microstructure, optical, and electrical properties of p-type SnO thin films,” Appl. Phys. Lett. 96, 042113 (2010).
  28. [29]H.-T. Nguyen, M.-C. Nguyen, J. Choi, S. Han, J. Kim, and R. Choi, “Electrical performance enhancement of p-type tin oxide channel thin film transistor using aluminum doping,” Thin Solid Films 641, 24–27 (2017).DOI
  29. [30]Z. Pan, Y. Jeong, M. Chu, Y. Jang, F. Wang, J. Chen, Y.-S. Kim, J.-K. Song, M. Q. Khokhar, and J. Yi, “Enhancing the mobility of p-type SnOx thin-film transistors through doping and plasma treatment,” Solid-State Electron. 229, 101981 (2025).DOI
  30. [31]B. J. Peek, M. Werner, K. Niang, X. Chen, A. J. Flewitt, O. W. S. Clark, J. C. Goodall, A. L. Johnson, S. Das, F. Alkhalil, P. A. Williams, and P. R. Chalker, “Influence of aluminium incorporation on the semiconducting properties of p-type tin monoxide,” Semicond. Sci. Technol. 41, 055016 (2026).DOI
  31. [32]G. Hoffmann, M. Budde, P. Mazzolini, and O. Bierwagen, “Efficient suboxide sources in oxide molecular beam epitaxy using mixed metal + oxide charges: the examples of SnO and Ga₂O₃,” APL Mater. 8, 031110 (2020).
  32. [33]L. J. van der Pauw, “A method of measuring specific resistivity and Hall effect of discs of arbitrary shape,” Philips Res. Rep. 13, 1–9 (1958).
  33. [34]A. Moy and J. Fournelle, “(φz) distributions in bulk and thin-film samples for EPMA. Part 2: BadgerFilm: A new thin-film analysis program,” Microsc. Microanal. 27, 284–296 (2021).
  34. [35]S. Sze and K. K. Ng, Physics of Semiconductor Devices, 1st ed. (Wiley, 2006).
  35. [36]CRC Handbook of Chemistry and Physics, 97th ed., edited by W. M. Haynes, D. R. Lide, and T. J. Bruno (CRC Press, 2026).

Paper details

vlnc:W_ce892tjt
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents