Abstract

Skyrmions and antiskyrmions are nanoscale swirling textures of magnetic moments formed by chiral interactions between atomic spins in magnetic non-centrosymmetric materials and multilayer films with broken inversion symmetry. These quasiparticles are of interest for use as information carriers in next-generation, low-energy spintronic applications. To develop skyrmion-based memory and logic, we must understand skyrmion-defect interactions with two main goals – determining how skyrmions navigate intrinsic material defects and determining how to engineer disorder for optimal device operation. Here, we introduce a tunable means of creating a skyrmion-antiskyrmion system by engineering the disorder landscape in FeGe using ion irradiation. Specifically, we irradiate epitaxial B20-phase FeGe films with 2.8 MeV Au4+^{4+} ions at varying fluences, inducing amorphous regions within the crystalline matrix. Using low-temperature electrical transport and magnetization measurements, we observe a strong topological Hall effect with a double-peak feature that serves as a signature of skyrmions and antiskyrmions. These results are a step towards the development of information storage devices that use skyrmions and anitskyrmions as storage bits and our system may serve as a testbed for theoretically predicted phenomena in skyrmion-antiskyrmion crystals.

Introduction

Exchange interactions between neighboring spins within ferro- and antiferromagnetic materials lead to a collinear arrangement of lattice spins that is described by the symmetric Hamiltonian. Strong spin-orbit interactions and broken inversion symmetry can give rise to an antisymmetric exchange interaction called the Dzyaloshinskii-Moriya interaction (DMI), which contributes an additional term to the magnetic Hamiltonian, HDMI=−Dij(Si×Sj)H_{\mathrm{DMI}}=-\mathbf{D}_{ij}(\mathbf{S}_i \times\mathbf{S}_j), for Dij\mathbf{D}_{ij} is the DMI interaction vector, Si\mathbf{S}_i and Sj\mathbf{S}_j represent neighboring spins, and JJ is the exchange constant. Favoring canting of neighboring spins, the DMI begets a panoply of noncollinear magnetic textures. Of particular interest, it can result in the formation of skyrmions — various winding configurations of magnetic moments that can have chiral or achiral forms. Within a material-dependent temperature and magnetic field range, this skyrmion phase is stable, that is, there is an effective energy barrier against the spins within each skyrmion aligning with the ferromagnetic background (topological protection). B20 phase FeGe, for example, has garnered significant interest because its noncentrosymmetric B20 cubic structure enables Dzyaloshinskii-Moriya interactions that result in skyrmion formation. Anisotropic DMIs can engender an antiskyrmion – the antiparticle of a skyrmion – in which the magnetic moments are reversed. Such localized magnetic textures are categorized based on a topological charge (also known as the skyrmion number), Q=14π∫m(r)⋅[∂xm(r)×∂ym(r)] dx dyQ = \frac{1}{4\pi} \int\mathbf{m}(\mathbf{r}) \cdot[\partial_x\mathbf{m}(\mathbf{r}) \times\partial_y\mathbf{m}(\mathbf{r})]\,\mathrm{d}x\,\mathrm{d}y, in which m(r)\mathbf{m}(\mathbf{r}) is the magnetization unit-vector field [1, 2, 3]. Accordingly, antiskyrmions have opposite topological charge from skyrmions, e.g. -1 for skyrmions and +1 for antiskyrmions [1, 3, 4].

Skyrmions and antiskyrmions are of interest for next-generation spintronic devices [5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15]. This is because they are predicted to require less energy to manipulate than charge currents in semiconductor or ferromagnetic domain-based logic [2, 16, 17, 18, 19], and also have considerable stability due to their topological protection. Implementing skyrmion-based spintronics necessitates understanding how to controllably manipulate these magnetic quasiparticles. It also requires understanding how the skyrmion lattice is affected by disorder [20], dictating how skyrmions will either maneuver around or be pinned by energy barriers within the material’s disorder landscape. This goes beyond considering how skyrmions navigate intrinsic material disorder to include the utility of artificially introduced defects. Precisely-engineered disorder landscapes can be used to control the dynamics of skyrmions in disparate ways; for example, the Magnus force can induce effective repulsion from defects and effectuate an increase in net mobility, while strategic choices of defect species may cause a net attraction, possibly pinning skyrmions [21]. Such control could be exploited in device design [22].

Here, we report a systematic investigation of the robustness of the skyrmion phase in FeGe to disorder. To this end, we irradiate epitaxial FeGe films with 2.8 MeV Au4+\mathrm{Au}^{4+} ions, varying the ion fluence to control the densities of induced vacancy clusters. We subsequently capture the disorder-induced evolution of the skyrmion lattice phase in the field-temperature phase diagram using magnetization and Hall effect measurements. We find that the irradiation process induces amorphous regions within a crystalline FeGe matrix and reveal the emergence of a potential skyrmion-antiskyrmion compound system when we pass a certain amorphization threshold.

Results and Discussion

We sputtered 55 nm-thick epitaxial FeGe films with P213P2_{1}3 cubic structure (B20 structure) on Si(111) substrates. The growth process is summarized in the Methods section and further detailed elsewhere [23]. FeGe was ideal for this study because it can be grown epitaxially, therefore with minimal disorder compared to sputtered multilayers, and has been repeatedly shown to host skyrmions associated with a topological Hall effect signature [24, 25, 26, 27, 28] and verified through Lorentz transmission electron microscopy [16, 26, 29, 30, 31] and electron phase microscopy [32]. Moreover, it has a relatively high Curie Temperature TCT_C, measured to be 276.3 K in our pristine (unirradiated) films (see Supplementary Materials Figure S1), consistent with the ordering temperature found in other studies of films [33] and near the bulk value [34, 35, 36]. Using a 6 MV HVEE EN Tandem Van de Graaff Accelerator at the Sandia Ion Beam Lab, we uniformly irradiated multiple 6 mm ×\times 6 mm samples with 2.8 MeV Au4+\mathrm{Au}^{4+} ions, each irradiated with a different fluence of 101110^{11}, 101210^{12}, 101310^{13}, and 101410^{14} ions/cm2^{2} to produce damage levels of 10−310^{-3}, 10−210^{-2}, 10−110^{-1}, 1 displacements per atom (dpa), respectively. Figure 1 shows Stopping and Range of Ions in Matter (SRIM) simulations [37] used to identify the appropriate energies and fluences that would induce our desired range of defect densities. From Figure 1(a), we see that the induced defect density is spread uniformly throughout the depth of the FeGe film and Figure 1(b) highlights a Bragg peak then vanishing dpa within the Si substrate. Consequently, we see that the majority of the 2.8 MeV Au4+\mathrm{Au}^{4+} ions are not implanted within the FeGe, but rather in the substrate. Lastly, the table in Figure 1(c) summarizes the displacement, lattice binding, and surface binding energies used for each species. Refer to the Methods section for more details regarding the irradiation process.

Figure 1. SRIM simulations showing the damage per atom generated by uniform Au4+^{4+} ion irradiation at varying fluences. (a) Displacement profiles for 101110^{11}, 101210^{12}, 101310^{13}, and 101410^{14} ions/cm2^2. (b) Vacancy profile highlighting Bragg peak well within depth of Si substrate. Note that all fluences show a Bragg peak in the same location. (c) Displacement energies (EdisplacementE_{\mathrm{displacement}}), lattice binding energies (ElatticeE_{\mathrm{lattice}}), and surface binding energies (EsurfaceE_{\mathrm{surface}}) for Fe, Ge, and Si used in the simulations, based on parameters from Ref. [38].

Figure S1. Fit of moment vs temperature to the Curie-Weiss Law χ=C(T−TC)−γ\chi= C(T - T_C)^{-\gamma} with a critical exponent γ\gamma of 1.73 for the pristine sample. The extracted Curie temperature was found to be 276.3 K.

To further characterize the effects of irradiation, we perform cross-sectional scanning transmission electron microscopy (STEM) imaging, electron energy loss spectroscopy (EELS), and electron diffraction on FeGe lamellae using a Thermo-Fisher Scientific Spectra 300 STEM Microscope at the Platform for the Accelerated Realization, Analysis, and Discovery of Interface Materials (PARADIM) at Cornell University. The lamellae were prepared with a Thermo Fisher Helios G4 UX focused ion beam (FIB), also at PARADIM. Refer to the Methods section for more details on the FIB and STEM procedures.

First considering the pristine (unirradiated) sample, the STEM image in Figure 2(a) displays an approximately 1 nm-thick FeSi seed layer interlaid between the Si substrate and epitaxial FeGe, as well as clean interfaces. In comparison, Figure 2(b) is a micrograph of the sample that was irradiated with 101310^{13} ions/cm2^2, revealing crystalline and irradiation-induced amorphized regions. We then collected EELS measurements on the same film, which are presented in Figure 2(c) and show an approximately 5 nm-thick surface oxide layer, which we observed in all samples, and a homogeneous concentration of Fe and Ge throughout the film thickness. Scans for Au atoms revealed no Au concentrations above measurement resolution, consistent with simulations showing that Au was not implanted within the FeGe.

Figure 2. Comparison of the microstructure in the irradiated versus the pristine FeGe films. Cross-sectional STEM image of the (a) pristine FeGe film and (b) film irradiated with 101310^{13} ions/cm2^2. Dashed square encloses an irradiation induced amorphous region and the solid square encompasses an example of a crystalline region. Scale bars are 5 nm. (c) EELS measurement of the FeGe film irradiated with 101310^{13} ions/cm2^2. Solid lines show signal intensity for each element; the signal is smoothed using a third-order Savitzky-Golay filter.

The STEM and EELS results show a surface oxide, and that irradiation induces various sizes and densities of amorphized regions. To identify the lattice structures and map grains, we performed x-ray diffraction (XRD) and scanning nanobeam electron diffraction (NBED) shown in Figure 3(a), (Figure 3b), and (Figure 3c,Figure 3d), respectively. The XRD data in Figure 3(a) shows the expected (111) Si and (111) B20 FeGe peaks, and identifies the oxide as (101) GeO2_2 and (121) GeO2_2. The (111) peak appears at 33.1° which corresponds to a measured lattice constant of 4.683 ± 4.121 × 10−410^{-4} nm. This corresponds to a strain of 0.1% compared to the bulk lattice constant of 4.679 nm. The full-width-half-maximum of the (111) peak was measured to be 0.233±0.001∘0.233 \pm0.001^\circ. Additionally, observe that as irradiation fluence is increased, there is a gradual decrease in the height of both the crystalline Si and the (111) B20 FeGe peaks. This is suggestive of increased sample amorphization, and in the film irradiated at 101410^{14} ions/cm2^2, nearly complete amorphization of the B20 FeGe as the peak completely disappears. Amorphorization is also evident from the electron diffraction data. Notably, the NBED data for the sample irradiated at 101310^{13} ions/cm2^2, Figure 3(b), shows Si and FeGe peaks rotated 30∘30^\circ from one another, with a diffuse ring overlapping the FeGe peaks, indicative of partially amorphized FeGe. The colorful mosaics displayed in Figure 3(c,Figure 3d) are false-color grain maps created by Exit Wave Power Cepstrum (EWPC) performed on 4D-STEM NBED data. EWPC cleanly decouples the tilt, thickness, and shape factor information from the lattice structure in thin film diffraction patterns, greatly simplifying the classification of small grain structures at arbitrary orientations. Further details regarding the technique are outlined in Ref. [39]. From the grain maps, areas with similar Bragg peaks rotation and periodicity are assigned the same color, thus the color map reveals the distribution and sizes of grains. Regions without clear boundaries are amorphized areas [e.g. the dull green region in Figure 3(d)].

Figure 3. Lattice structure mapping and grain identification of pristine and irradiated FeGe films. (a) Cu-Kα_{\alpha} XRD patterns of pristine and irradiated films. Void regions are due to removal of peaks produced by sample mounting hardware. (b) Select Area Electron Diffraction data of film irradiated at 101310^{13} ions/cm2^{2} along the (111) plane. Note the diffuse ring indicative of amorphous material overlaid on the crystalline FeGe peaks. Scale bar is 5 nm−1^{-1}. (c) Grain orientation map of film irradiated at 101310^{13} ions/cm2^{2}. Colored granular regions in top half of image correspond to individual crystalline and amorphous grains. (d) Grain orientation map of film irradiated at 101410^{14} ions/cm2^{2}. Void region in top right of image is empty space off of the sample surface. Scale bars in (c-d) are 5 nm.

Topological Hall Effect Measurements

To map the magnetic phase diagram, we perform Hall effect measurements at variable temperatures and magnetic fields. We then use the topological Hall effect (THE) as the hallmark of the emergence of nontrivial spin textures [40] – namely, skyrmions. Noncollinear spin textures engender an effective magnetic field that deflects charge carrier motion, resulting in a THE. Such textures include topological states (different types of skyrmions, antiskyrmions), spin chirality in Kagome and triangular lattices, and right- or left-handed chiral domain walls [40]. In FeGe, the THE is a recognized signature of skyrmions [24, 25, 26, 27, 28].

To this end, we conduct electrical transport measurements on microfabricated six-point Hall bar devices and out-of-plane magnetization MM measurements on approximately 3 mm ×\times 3 mm unpatterned films. We directly measure the total Hall resistivity ρxy\rho_{xy}, which consists of contributions from three different effects: the ordinary Hall effect, the anomalous Hall effect, and the topological Hall effect. It can therefore be expressed as the sum of three terms [28, 33, 40, 41, 42]

ρxy=ρOHE+ρAHE+ρTHE,(1)\rho_{xy} = \rho_{OHE} + \rho_{AHE} + \rho_{THE}, \tag*{(1)}

for ordinary Hall resistivity ρOHE=R0μ0H\rho_{OHE} = R_0\mu_0H, ordinary Hall coefficient R0R_0, externally applied out-of-plane magnetic field μ0H\mu_0H, anomalous Hall resistivity ρAHE=RAHM(T,H)\rho_{AHE} = R_{AH}M(T,H), anomalous Hall coefficient RAHR_{AH}, and topological Hall resistivity ρTHE\rho_{THE}. Through the anomalous Hall effect contribution RAH(ρxx)R_{AH}(\rho_{xx}), ρxy\rho_{xy} also depends on the longitudinal resistivity ρxx\rho_{xx}, which we measure in conjunction with ρxy\rho_{xy}, and the measured sample out-of-plane magnetization M(T,H)M(T,H).

To extract ρTHE\rho_{THE}, we calculate and subtract both ρOHE\rho_{OHE} and ρAHE\rho_{AHE} from ρxy\rho_{xy}. First, recognizing that in saturation, all topological magnetic textures vanish and ρTHE\rho_{THE} is zero, we find that

ρxyμ0H=R0+RAHMμ0H,H>Hsat.(2)\frac{\rho_{xy}}{\mu_0 H} = R_0 + R_{AH}\frac{M}{\mu_0 H}, \quad H > H_{\mathrm{sat}}. \tag*{(2)}

After antisymmetrizing the raw resistivity and magnetization data, we determine R0R_0 and RAHR_{AH} by performing a linear fit to ρxy/H\rho_{xy}/H versus M/μ0HM/\mu_0 H, noting R0R_0 as the intercept and RAHR_{AH} as the slope, as seen in Equation (2). From the extracted coefficients, we can then calculate ρOHE\rho_{OHE}, ρAHE\rho_{AHE}, and subsequently ρTHE\rho_{THE}. This topological Hall resistivity is proportional to the net topological charge, such that larger ∣ρTHE∣\lvert\rho_{THE}\rvert corresponds to a higher density of topological magnetic textures.

Figure 4(a) shows the field-dependent Hall resistivities for the pristine FeGe film at 200 K. The blue curve is the extracted ρTHE\rho_{THE}, which shows one prominent positive-valued peak in the negative-field region as the applied magnetic field is swept from high to low. This is the typical shape expected from FeGe [25, 26, 27, 28], and we attribute this peak to the presence of skyrmions. The evolution of the peak with temperature is shown in Figure 4(c) and Figure S3; the THE peak persists down to the lowest measurement temperature of 10 K. Similar results are seen for the film irradiated at 101110^{11} ions/cm2^2 and 101210^{12} ions/cm2^2, as shown in Figure S3 and Figure S3.

Topological Hall resistivity curves for pristine and irradiated FeGe films

Figure 4. Topological Hall effect in pristine and irradiated FeGe films. (a-b) Subtracting OHE and AHE components to extract ρTHE\rho_{THE}. Blue ρTHE\rho_{THE} are plotted versus the right axes in both plots. (c-d) Isothermal plots of ρTHE\rho_{THE} versus applied magnetic field for a (c) pristine and a FeGe film that was irradiated at 101310^{13} ions/cm2^2. The field is swept from high to low for all curves. Arbitrary offsets added for clarity. Tick marks on y-axis have spacings of 500 nΩ\Omega cm.

Composite topological Hall resistivity measurements for all samples in six panels

Figure S3. Composite ρTHE\rho_{\mathrm{THE}} for all samples. We see the emergence of the double-peak feature in (e) and (f).

As defect density increases, we see the emergence of a second peak – in the positive-field region – as seen in Figure 4(b). Specifically, we see the single-peak behavior in the unirradiated film and samples irradiated with 2.8 MeV Au4+^{4+} fluences below 101310^{13} ions/cm2^2, corresponding to damage levels below 10−110^{-1} dpa, and double-peak features at and above 101310^{13} ions/cm2^2. We label the peaks (1) and (2) in Figure 4(b), and find that the data has a similar shape to that observed in the inverse Heusler system Mn1.4_{1.4}Pt0.9_{0.9}Pd0.1_{0.1}Sn [43] and that peak (1) is consistent with the presence of skyrmions. To identify the origin of peak (2), we consider the relative properties of another magnetic texture that may be present.

The topological Hall resistivity is directly proportional to the topological charge density, which can be written as a product of polarization pp and vorticity WW [44],

ρTHE=RTHE⟨η⟩=pW,(3)\rho_{\mathrm{THE}} = R_{\mathrm{THE}}\langle\eta\rangle= pW, \tag*{(3)}

where RTHER_{THE} is the topological Hall coefficient and ⟨n⟩\langle n\rangle is the total topological charge density of the sample. Note that RTHER_{THE} is proportional to both the carrier density and the carrier polarization. Moreover, the carrier density is invariant under field sweeps, such that any change in the sign of ρTHE\rho_{THE} during a field sweep is due solely to a change in the sign of ⟨n⟩\langle n\rangle.

The magnetic textures associated with each peak must have topological charges ⟨n⟩\langle n\rangle of the same sign, yet polarities p=±1p = \pm1 of opposite sign. This is because, first, the ρTHE\rho_{THE} of the dual peaks have the same sign, hence ⟨n⟩\langle n\rangle has the same sign for each peak. Second, the magnetization MM for each peak has opposite sign, such that the sign of the polarity must be opposite. As we see from Eq. (3), given that the two textures both produce positive ρTHE\rho_{THE}, yet polarities of opposite sign, then they must have vorticities W=±1W = \pm1 of opposite sign. This reasoning [43] therefore suggests that as peak (1) is representative of skyrmions (with vorticity +1+1), peak (2) may be caused by a texture of opposite polarity and vorticity 11 – antiskyrmions. Figure 5(a) is a cartoon depicting the type of topological spin texture responsible for each peak and dip in ρTHE(H)\rho_{THE}(H), showing skyrmions of polarity +1+1 (upper left quadrant), antiskyrmions of polarity −1-1 (upper right quadrant), antiskyrmions of polarity +1+1 (lower right quadrant), and skyrmions of polarity −1-1 (lower left quadrant).

Magnetic phase diagram in pristine and irradiated FeGe films

Figure 5. Magnetic phase diagram in pristine and irradiated FeGe films. (a) Magnetic field-dependent topological Hall resistivity of FeGe film irradiated at 101310^{13} ions/cm2^2 at 100 K. Each quadrant is labelled with the corresponding topological spin texture type and polarization associated with the peak or dip. (b-f) Two-dimensional heat maps of ρTHE\rho_{THE} (color scale) for each sample. The phase boundary in (e) was found by plotting inflection points in ρTHE\rho_{THE}. All diagrams are plotted with field sweeping from high to low.

Antiskyrmions have been observed in ultrathin multilayer films with interfacial DMIs [45, 46], Heusler compounds with D2dD_{2d} symmetry [47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57], and a schreibersite with S4S_{4} symmetry [58]. They have also been predicted to form in dipolar magnets [3], chiral magnets in tilted magnetic fields [59], and ultra-thin magnetic films grown on semiconductors or heavy metals with C2vC_{2v} symmetry [4]. One study predicted that antiskyrmions would be unstable – immediately vanishing — in chiral magnets [3], however they have in fact recently been observed via Lorentz Transmission Electron Microscopy (LTEM) in a 70 nm-thick lamella of B20-type FeGe [1] and in amorphous Fe0.52_{0.52}Ge0.48_{0.48}, with antiskyrmion stabilization occurring as a result of randomized DMI direction from amorphization [30].

From examining ρTHE\rho_{THE} plotted as a function of both temperature and field, we can construct the effective phase diagrams that are shown in Figure 5(b-Figure 5f). Based on the peak positions in the topological Hall resistivity, we label the corresponding magnetic textures – Sk (skyrmion) and ASk (antiskyrmion). Accordingly, we see evidence of skyrmions alone in the pristine sample (crystalline FeGe) and film irradiated at 101110^{11} ions/cm2^{2} in Figure 5(b) and (Figure 5c), respectively. In the film irradiated at 101210^{12} ions/cm2^{2} [results shown in Figure 5(b)], the skyrmion phase broadens out to lower temperatures, suggesting that skyrmions are forming at these lower temperatures in the amorphized regions. Since composition of amorphous material increases with increased fluence, we deduce that the skyrmion phases in both amorphous FeGe and crystalline FeGe are overlapping to produce the appearance of one broad skyrmion phase. If we compare negative-field skyrmion peak heights between the different samples, we observe that the peak height for the pristine sample and that of the sample irradiated at 1×10111 \times10^{11} ions/cm2^{2} are similar, and a 1.8× increase between the peak height for the sample irradiated at 1×10111 \times10^{11} and that irradiated at 1×10121 \times10^{12} ions/cm2^{2}. Note that the peak height is directly proportional to skyrmion density. The marked decrease in skyrmion density in Figure 5(e) is predicted to be from a lack of skyrmion-favoring crystalline FeGe.

As irradiation fluence increases to 101310^{13} ions/cm2^{2} (increasing the density of amorphous grains) we see the emergence of the double-peak feature. Figure 5e displays the corresponding broad antiskyrmion phase down to single Kelvin temperatures, and the skyrmion phase emerges at temperatures below 210 K and persists down to temperatures lower than in the pristine film. We propose that the magnetic ordering temperature of the skyrmion phase is less than in the pristine film, in which it orders at ∼280\sim280 K, due to a decrease in uniaxial anisotropy resulting from 2.8 MeV Au4+^{4+} irradiation. This implies that the crystalline regions host skyrmions whereas the amorphous regions hosts both skyrmions and antiskyrmions. Examining an idealized Hamiltonian [60] of a ferromagnet with DMI vector Dij\mathbf{D}_{ij}, symmetric exchange coefficient JijJ_{ij}, and uniaxial anisotropy constant KK,

Hij=−∑⟨i,j⟩Jij(Si⋅Sj)−∑⟨i,j⟩Dij⋅(Si×Sj)−K∑i(Siz)2−∑iμ0BSiz(4)H_{ij}=-\sum_{\langle i,j\rangle}J_{ij}(\mathbf{S}_i\cdot\mathbf{S}_j)-\sum_{\langle i,j\rangle}\mathbf{D}_{ij}\cdot(\mathbf{S}_i\times\mathbf{S}_j)-K\sum_i(S_i^z)^2-\sum_i\mu_0B S_i^z \tag*{(4)}

we expect the exchange coefficient and the DMI vector magnitude DijD_{ij} to change minimally as a result of amorphization, because they depend on local bond geometries [61, 62]. On the other hand, the uniaxial anisotropy constant KK and the direction of the DMI vector Dij\mathbf{D}_{ij} could change substantially since they depend on long-range order of the lattice, which is broken during amorphization Note that, in equation 4, BB is the z-oriented magnetic field, SizS_i^z is the z component of Si\mathbf{S}_i, and μ\mu is the magnetic moment of the magnetic atom.

Lastly, as fluence is further increased to 101410^{14} ions/cm2^2, we see predominately antiskyrmions with a narrow skyrmion phase existing between approximately 70 K and 125 K in Figure 5(f). This sample is near-fully amorphized, and the large fluence could have displaced the atoms to the point that short-range-order quantities such as JJ and DD have changed, so magnetic phase boundaries have fully shifted with respect to the lower-fluence samples.

Figure 6(a) shows the saturated value of the AHE resistivity, ρAHE,Sat\rho_{AHE,Sat}, for the pristine and irradiated samples as a function of temperature. Note that the shape of the curves for the films irradiated at 101210^{12} ions/cm2^2, 101310^{13} ions/cm2^2, and 101410^{14} ions/cm2^2 are similar to that found in textured FeGe films [33]. If we compare ρAHE,Sat\rho_{AHE,Sat} for each sample, we can attribute differences to changes in KK and in the direction of Dij\mathbf{D}_{ij}, which we will denote D^\hat{D}. We see that at approximately 210 K, saturation magnetization is effectively identical for all samples containing crystalline FeGe. Neglecting the differences above this temperature, we assume that changes in KK and D^\hat{D} are no longer visible in saturation. Because we have evidence that antiskyrmions may persist at temperatures above 210 K in the sample irradiated at 101310^{13} ions/cm2^2, we can not deduce significant changes in Dij\mathbf{D}_{ij} in the amorphous regions, and attribute all changes in ρAHE,Sat\rho_{AHE,Sat} to KK.

Figure 6. Anomalous Hall resistivity in pristine and irradiated FeGe films. (a) Temperature-dependent ρAHE\rho_{AHE} in the positive-field saturation region for all FeGe samples. (b,c) Fit of Eq. 5 to anomalous Hall resistivity divided by magnetic moment vs longitudinal resistivity, for (b) the pristine sample for temperatures less than 130 K and (c) the sample irradiated at 101310^{13} ions/cm2^2 for temperatures less than 95 K. The open red circle was associated with noise and excluded from from the fit.

Note that ρAHE,Sat\rho_{AHE,Sat} for the fully amorphized sample is lower and has a much smaller rate of change with respect to temperature. We attribute the behavior of ρAHE,Sat\rho_{AHE,Sat} at temperatures above 210 K to be primarily due to crystalline FeGe in the lower fluence samples, since the curves have a significant negative slope and larger values. The vanishing skyrmion phase above 210 K in the sample irradiated at 101310^{13} ions/cm2^2 indicates that KK is important in skyrmion stabilization in the crystalline phase. The lowering of KK in crystalline FeGe is likely due to the randomization of grain direction due to irradiation, and provides an explanation to why the helical ordering temperature is lower in irradiated films.

We now consider how different contributions to the anomalous Hall effect are affected by disorder. The anomalous Hall effect results from the co-action of skew scattering, side-jump scattering, and an intrinsic scattering-independent mechanism (related to the Berry curvature). Accordingly, the anomalous Hall coefficient can be expressed as [27, 33, 63]:

RAH=αρxx+(β+b)ρxx2.(5)R_{AH} = \alpha\rho_{xx} + (\beta+ b)\rho_{xx}^{2}. \tag*{(5)}

Here, the side-jump scattering (coefficient β\beta) and intrinsic (coefficient bb) contributions both depend quadratically on the longitudinal resistivity ρxx\rho_{xx}, whereas the skew-scattering mechanism (coefficient α\alpha) depends linearly on ρxx\rho_{xx}. Side-jump scattering occurs when wave packets formed from spin-orbit coupled Bloch states are scattered by a disorder potential [63] whereas skew-scattering is an antisymmetric scattering process caused by the effective spin-orbit coupling of the conduction electron or impurity from which it scatters [63].

Previous studies of FeGe films have found that the scattering-independent (intrinsic) mechanism prevails and that contributions from skew-scattering, typically only significant in crystals [63, 64], can be neglected [27, 28, 65, 66]. This is partially because finite-temperature effects tend to suppress the skew-scattering (linear) contribution [63, 67]. Ref. [33] also found evidence of a suppressed linear contribution in textured FeGe films and that the predominating quadratic dependence of RAHR_{AH} on ρxx2\rho_{xx}^{2} was consistent with both the intrinsic and the side-jump mechanisms.

To investigate how the relative contributions of the anomalous Hall effect may change in our FeGe films owing to systematically tuned disorder, we compare ρAHE,Sat/m\rho_{AHE,Sat}/m versus ρxx\rho_{xx} in all films. Figure 6(b,Figure 6c) displays the results for the pristine film and for the sample irradiated with 101310^{13} ions/cm2^{2}, respectively, whereas the data for the other samples is shown in Supplemental Materials Figure S4. In all samples, we see evidence that the relative magnitude of the various contributions to ρAHE\rho_{AHE} — skew scattering versus the combined effects of side-jump scattering and intrinsic effects — are temperature dependent. We therefore restrict our analysis to low-temperature regions where simple second order polynomial fits can be made with a convergence of chi-squared χ2<1×10−9\chi^{2}<1\times10^{-9}.

Figure S4. Fit of Eq. (5) to anomalous Hall resistivity divided by magnetic moment vs longitudinal resistivity, for the (a) 101110^{11}, (b) 101210^{12}, and (c) 101410^{14} ions/cm2^{2} samples. No fit is performed in (c) because the low-resistivity data does not fit the model described in Eq (5)

In the pristine sample, the skew-scattering component α\alpha appears to be negligible at temperatures less than ∼\sim130 K, as shown in Figure 6(b). A fit to Eq. (5) is performed, omitting the linear term by setting α≡0\alpha\equiv0, and noting that a good fit can still be made in its absence. We find that β+b=2.12 μΩ−1μA−1\beta+b=2.12\ \mu\Omega^{-1}\mu\mathrm{A}^{-1}. Similarly, for the sample irradiated with a low dose of 101110^{11} ions/cm2^{2}, we find negligible α\alpha. However, fits for the samples irradiated with higher dosages yielded non-negligible α\alpha. For example, for the sample irradiated at 101310^{13} ions/cm2^{2}, we find that α=−2.19×10−3MA−1nm\alpha=-2.19\times10^{-3}\mathrm{MA}^{-1}\mathrm{nm} and β+b=1.24 μΩ−1μA−1\beta+b=1.24\ \mu\Omega^{-1}\mu\mathrm{A}^{-1}. We thus conclude that irradiation increases the contribution of skew-scattering in our FeGe films.

Conclusion

In summary, we induce amorphous regions in epitaxially grown FeGe through 2.8 MeV Au4+\mathrm{Au}^{4+} ion irradiation, and perform subsequent topological Hall effect measurements to investigate topological spin texture formation. Our measurements show evidence that composite skyrmion-antiskyrmion systems form in the partially-amorphized films, with skyrmions existing in the crystalline phase, and both skyrmions and antiskyrmions in the amorphous phase. Fundamentally, such systems are of interest as testbeds for theoretically predicted phenomena such as spin wave emission by current induced skyrmion-antiskyrmion pair annihilation [68], a skyrmion-antiskyrmion liquid [69], as well as skyrmion-antiskyrmion crystals, interactions, and dynamics [70, 71, 72].

Systems hosting coexisting skyrmions and antiskyrmions are of interest for architectures in which the two particles are used for binary data encoding, for example in skyrmion-antiskyrmion racetrack memory [8, 14] and magnetic logic gates [15]. Information could be stored based on the topological charge. Given opposite topological charges, skyrmions and antiskyrmions have opposite topological Magnus forces, which cause them to accumulate on opposite sides of the sample (skyrmion Hall effect) and can be exploited for logic operations [6, 7]. Such a system would prove beneficial for spintronic applications requiring the transport of magnetic textures in the absence of transverse Hall motion [73]. The presence of both textures in the amorphous phase also presents an opportunity for simpler fabrication of these devices, since the growth of a pure amorphous phase would not require specific substrates and would be less dependent on the requirement of pristine substrate surface preparation and condition. Amorphous FeGe phases have also been shown to exhibit larger Hall effects thus making them more sensitive to voltage manipulation [30]. One may also find novel uses for creating precisely-formed amorphous shapes within a surrounding crystalline matrix, which would easily be accomplished by performing irradiations through a hard mask so that only particular sections of films are exposed to incident ions.

Methods

Film growth

The FeGe films measured in this study were grown epitaxially on Si (111) substrates using molecular-beam epitaxy (MBE) in a Veeco GEN10 chamber at the Platform for the Accelerated Realization, Analysis, and Discovery of Interface Materials (PARADIM) at Cornell University. First, a FeSi seed layer is established by depositing a monolayer of Fe onto a 7×77 \times7 reconstructed Si (111) surface then flash annealing at 500∘500^\circ C. Subsequently, B20 FeGe is grown atop the seed layer by codeposition of Fe and Ge sources at 200∘200^\circ C, at 0.50.5 Å/s, and in a base pressure of 2×10−92 \times10^{-9} torr. The sources were 40 cc effusion cells that produce relatively uniform films covering an area of 1.5 inches. For more details on a similar process used to grow epitaxial MnxFe1−xGe\mathrm{Mn}_x\mathrm{Fe}_{1-x}\mathrm{Ge} films, see Ref. [23].

Ion Beam Modification

Ion beam modification was carried out using a 6 MV HVEE EN Tandem Van de Graaff Accelerator at the Sandia National Laboratories Ion Beam Lab. FeGe specimens were sliced into 0.50.5 cm ×0.5\times0.5 cm pieces, adhered to a Si backing plate with double sided carbon tape, inserted into the tandem end station, and pumped to a base pressure of at least 1×10−61 \times10^{-6} torr. Ion irradiation was performed using 2.82.8 MeV Au4+\mathrm{Au}^{4+} ions with an ion beam current of 100 nA (ion flux of 1.56×10111.56 \times10^{11} ions/cm2^2 measured at the sample before and after irradiation of the samples. Estimations of the ion beam damage were performed with Stopping Range of Ion in Matter (SRIM) simulations [37]. Based on parameters from Ref. [38], the SRIM simulation used an FeGe density of 8.148.14 g/cm3^3, Si density of 2.3122.312 g/cm3^3, as well as the displacement energies, lattice energies, and surface energies indicated in the table in Figure 1(c) in the main text.

Focused Ion Beam

We used a cross-sectional focused ion beam (FIB) process to prepare the STEM samples studied for crystal structure characterization and chemical composition analysis, for which the results are displayed in Figure 2. The samples used for grain mapping were prepared using a plan-view FIB process. In both cases, first, we deposit a stack of 20–30 nm of carbon and 0.8–1 μm of Pt on the sample surface to form a protective overlayer. Next, we prepare a lamella using a Ga ion beam. We then adhere it to a needle with a sputtered Pt paste in order to transfer it to a TEM grid. The cross-section or plan-view lamellae are then further milled iteratively on both sides, using a 30 keV Ga ion beam, down to a thickness of 200–500 nm, then at 5 keV until the thickness of the protective Pt layer becomes less than 20 nm. During the plan-view FIB thinning process, the film surface and substrate are milled at a 22–3∘3^\circ angle with respect to the ab-plane to create a smooth gradient of different regions, displayed from the bottom (substrate) to top (film), respectively, in Figure 3(c).

Hall Bar Fabrication

We fabricated 55 nm-thick FeGe films into Hall bars using standard photolithography (laser writer) and broad-beam Ar+^+ ion milling techniques at the Center for Integrated Nanotechnologies (CINT) at Sandia National Laboratories. 100 nm-thick Au contacts were deposited using e-beam evaporation with a 5 nm Ti sticking layer, followed by lift-off in acetone.

Magnetometry Measurements

Magnetization studies were performed using a Quantum Design MPMS3 SQUID magnetometer at the Colorado School of Mines and University of Washington. Samples were cut to approximately 3.5 mm ×\times 3.5 mm to friction-fit within a drinking straw for low-background sample mounting. Hence, in calculations requiring a volume VV, we used V≈6.7375×10−4 mm3V \approx6.7375 \times10^{-4}\ \mathrm{mm}^{3}, considering a nominal film thickness of 55 nm. For all measurements, the magnetic field was applied perpendicular to the film plane and swept in a full hysteresis loop between ±\pm 3 T. Within ±\pm 1.5 T we measure using 100 Oe intervals, and 500 Oe intervals beyond this range. Background from the Si substrate was removed by subtracting a linear fit to the saturated regions of the M(H)M(H) curves at each temperature.

Electrical Transport Characterization

Electrical transport measurements were performed using three SR830 lock-in amplifiers and two SR560 voltage preamplifiers per Hall bar. Devices were measured at either 37 or 41 Hz with an applied current of ∼\sim3.6 μ\muA rms. The longitudinal resistivity ρxx\rho_{xx} and transverse resistivity ρxy\rho_{xy} are measured simultaneously using the lock-in amplifier (and preamplifier), and voltage drop across a 100 Ω\Omega series resistor is recorded using another SR830, ultimately to track the applied current. Voltage preamplifiers were set to a constant gain of 100 and a low-pass filter with a cutoff frequency of 10 kHz. A time constant of 1 s was used for lock-in measurements. A full wiring diagram is given in the Supplemental Materials as Fig. S5.

Acknowledgements

This material is based upon work supported by the National Science Foundation under grants DMR-1905909 and DMR-2330562. This work was performed, in part, at the Center for Integrated Nanotechnologies, an Office of Science User Facility operated for the U.S. Department of Energy (DOE) Office of Science. This work also used synthesis and microscopy facilities at the Platform for the Accelerated Realization, Analysis, and Discovery of Interface Materials (PARADIM), which are supported by the National Science Foundation under Cooperative Agreement No. DMR-2039380. M.B.V. thanks David Lidsky (Sandia National Labs) for assistance in using cleanroom instrumentation at the Center for Integrated Nanotechnologies.

Data availability

Data that support the findings of this study are available from the corresponding authors upon reasonable request.

Author contributions statement

S.E. conceived the experiments, conducted measurements, and advised on device fabrication, measurements, and data analysis; M.B.V. conducted magnetization measurements, Hall effect measurements, as well as SRIM simulations, and performed the Hall bar microfabrication; X.Z. and D.M. imaged the films using transmission electron microscopy measurements and performed the accompanying analysis; E.L. and K.H. irradiated the films; E.L. and S. A. J. performed x-ray diffraction and reflectivity measurements; T.M.L. assisted with microfabrication, electrical transport measurements, and data analysis; P.S. assisted with electrical transport measurements; H. P. grew the FeGe films; P. A. assisted in writing Python scripts for electrical transport measurement. S.E. and M.B.V. wrote the manuscript. All authors commented on the manuscript.

Ethics declarations

The authors declare no competing interests.

References

Supplemental Materials: Inducing a Tunable Skyrmion-Antiskyrmion System through Ion Beam Modification of FeGe Films

M. B. Venuti; Xiyue S. Zhang; Eric J Lang; Sadhvikas J. Addamane; Hanjong Paik; Portia Allen; Peter Sharma; David Muller; Khalid Hattar; Tzu-Ming Lu; Serena Eley

Here we present additional materials in support of the full publication. Additional electron energy-loss spectroscopy (EELS) measurements were performed on pristine FeGe cross-sections, shown in Figure S2, showing the depthwise FeGe-FeSi-Si films structure. We also provide a combined topological Hall resistivity summary of all samples in the study in the form of full hysteresis loops at varying temperatures, shown in Figure S3. We also provide a circuit diagram of the full experimental setup in collecting the transport data, shown in Figure S5. Here, two Stanford Research System (SRS) 830 lock-in amplifiers were used to measure the longitudinal and transverse voltage drops across each Hall bar. Both signals were amplified using SRS 560 voltage pre-amplifiers. A third lock-in amplifier was used to measure the voltage drop across 100 Ω100\ \Omega resistor placed in series with the Hall bar to for a precise measurement of the current through the device.

Curie Temperature

Electron Energy Loss Spectroscopy (EELS)

Atomic compositions as a function of depth

Figure S2. Atomic compositions as a function of depth for a pristine FeGe cross-section.

Topological Hall Measurements

Additional Anomalous Hall Resistivity Fits

Figure S5. Full wiring diagram for the experimental setup for topological Hall resistivity measurements.

References

  1. [1]Zheng, F., Kiselev, N. S., Yang, L., Kuchkin, V. M., Rybakov, F. N., Blügel, S. & Dunin-Borkowski, R. E. Zeroboskyrmion–antiskyrmion pair creation and annihilation in a cubic chiral magnet. Nat. Phys. 18, 863–868 (2022).DOI
  2. [2]Nagaosa, N. & Tokura, Y. Topological properties and dynamics of magnetic skyrmions. Nat. Nanotechnol. 8, 899–911 (2013).DOI
  3. [3]Koshibae, W. & Nagaosa, N. Theory of antiskyrmions in magnets. Nat. Commun. 7, 10542 (2016).DOI
  4. [4]Hoffmann, M., Zimmermann, B., Müller, G. P., Schürhoff, D., Kiselev, N. S., Melcher, C. & Blügel, S. Antiskyrmions stabilized at interfaces by anisotropic Dzyaloshinskii-Moriya interactions. Nat. Commun. 8, 308 (2017).DOI
  5. [5]Yokouchi, T., Sugimoto, S., Rana, B., Seki, S., Ogawa, N., Shiomi, Y., Kasai, S. & Otani, Y. Pattern recognition with neuromorphic computing using magnetic field–induced dynamics of skyrmions. Sci. Adv. 8, eabq5652 (2022).DOI
  6. [6]Leonov, A. O. & Mostovoy, M. Edge states and skyrmion dynamics in nanostripes of frustrated magnets. Nat. Commun. 8, 14394 (2017).DOI
  7. [7]Jiang, W., Zhang, X., Yu, G., Zhang, W., Wang, X., Benjamin Jungfleisch, M., Pearson, J. E., Cheng, X., Heinonen, O., Wang, K. L., Zhou, Y., Hoffmann, A. & te Velthuis, S. G. Direct observation of the skyrmion Hall effect. Nat. Phys. 13, 162–169 (2017).DOI
  8. [8]Hoffmann, M., Müller, G. P., Melcher, C. & Blügel, S. Skyrmion-Antiskyrmion Racetrack Memory in Rank-One DMI Materials. Front. Phys. 9, 2021.
  9. [9]Luo, S. & You, L. Skyrmion devices for memory and logic applications. APL Mater. 9, 050901 (2021).DOI
  10. [10]Song, K. M., Jeong, J.-S., Pan, B., Zhang, X., Xia, J., Cha, S., Park, T.-E., Kim, K., Finizio, S., Raabe, J., Chang, J., Zhou, Y., Zhao, W., Kang, W., Ju, H. & Woo, S. Skyrmion-based artificial synapses for neuromorphic computing. Nat. Electron. 3, 148–155 (2020).DOI
  11. [11]Zhang, X., Zhou, Y., Ezawa, M., Zhao, G. P. & Zhao, W. Magnetic skyrmion transistor: skyrmion motion in a voltage-gated nanotrack. Sci. Rep. 5, 11369 (2015).DOI
  12. [12]Tomasello, R., Martinez, E., Zivieri, R., Torres, L., Carpentieri, M. & Finocchio, G. A strategy for the design of skyrmion race track memories. Sci. Rep. 4, 6784 (2014).
  13. [13]Zhang, X., Zhou, Y., Song, K. M., Park, T.-E., Xia, J., Ezawa, M., Liu, X., Zhao, W., Zhao, G. & Woo, S. Skyrmion-electronics: writing, deleting, reading and processing magnetic skyrmions toward spintronic applications. J. Condens. Matter Phys. 32, 143001 (2020).DOI
  14. [14]Silva, R. C., Silva, R. L. & Pereira, A. R. Magnus-force induced skyrmion–antiskyrmion coupling in inhomogeneous racetrack. J. Phys Cond. Matt. 33, 105802 (2020).DOI
  15. [15]Zhang, X., Ezawa, M. & Zhou, Y. Magnetic skyrmion logic gates: conversion, duplication and merging of skyrmions. Sci. Rep. 5, 9400 (2015).DOI
  16. [16]Yu, X. Z., Kanazawa, N., Onose, Y., Kimoto, K., Zhang, W. Z., Ishiwata, S., Matsui, Y. & Tokura, Y. Near room-temperature formation of a skyrmion crystal in thin-films of the helimagnet FeGe. Nat. Mater. 10, 106–109 (2010).DOI
  17. [17]Yu, X. Z., Kanazawa, N., Zhang, W. Z., Nagai, T., Hara, T., Kimoto, K., Matsui, Y., Onose, Y. & Tokura, Y. Skyrmion flow near room temperature in an ultralow current density. Nat. Commun. 3, 988 (2012).DOI
  18. [18]Fert, A., Cros, V. & Sampaio, J. Skyrmions on the track. Nat. Nanotechnol. 8, 152–156 (2013).DOI
  19. [19]Jonietz, F., Mühlbauer, S., Pfleiderer, C., Neubauer, A., Münzer, W., Bauer, A., Adams, T., Georgii, R., Böni, P., Duine, R. A., Everschor, K., Garst, M. & Rosch, A. Spin Transfer Torques in MnSi at Ultralow Current Densities. Science 330, 1648–1651 (2010).DOI
  20. [20]Lima Fernandes, I., Bouaziz, J., Blügel, S. & Lounis, S. Universality of defect-skyrmion interaction profiles. Nat. Commun. 9, 4395 (2018).DOI
  21. [21]Reichhardt, C., Reichhardt, C. J. O. & Milošević, M. Statics and dynamics of skyrmions interacting with disorder and nanostructures. Rev. Mod. Phys. 94, 035005 (2022).DOI
  22. [22]Arjana, I. G., Lima Fernandes, I., Chico, J. & Lounis, S. Sub-nanoscale atom-by-atom crafting of skyrmion-defect interaction profiles. Sci. Rep. 10, 14655 (2020).arxiv.org/abs/2003.05518
  23. [23]Turgut, E., Paik, H., Nguyen, K., Muller, D. A., Schlom, D. G. & Fuchs, G. D. Engineering Dzyaloshinskii-Moriya interaction in B20 thin-film chiral magnets. Phys. Rev. Mater. 2, 074404 (2018).DOI
  24. [24]Leroux, M., Stolt, M. J., Jin, S., Pete, D. V., Reichhardt, C. & Maiorov, B. Skyrmion Lattice Topological Hall Effect near Room Temperature. Sci. Rep. 8, 15510 (2018).DOI
  25. [25]Gallagher, J. C., Meng, K. Y., Brangham, J. T., Wang, H. L., Esser, B. D., McComb, D. W. & Yang, F. Y. Robust Zero-Field Skyrmion Formation in FeGe Epitaxial Thin Films. Phys. Rev. Lett. 118, 027201 (2017).DOI
  26. [26]Ahmed, A. S., Rowland, J., Esser, B. D., Dunsiger, S. R., McComb, D. W., Randeria, M. & Kawakami, R. K. Chiral bobbers and skyrmions in epitaxial FeGe/Si(111) films. Phys. Rev. Mater. 2, 041401 (2018).DOI
  27. [27]Budhathoki, S., Sapkota, A., Law, K. M., Ranjit, S., Nepal, B., Hoskins, B. D., Thind, A. S., Borisevich, A. Y., Jamer, M. E., Anderson, T. J., Koehler, A. D., Hobart, K. D., Stephen, G. M., Heiman, D., Mewes, T., Mishra, R., Gallagher, J. C. & Hauser, A. J. Room-temperature skyrmions in strain-engineered FeGe thin films. Phys. Rev. B 101, 220405 (2020).DOI
  28. [28]Huang, S. X. & Chien, C. L. Extended Skyrmion Phase in Epitaxial FeGe(111) Thin Films. Phys. Rev. Lett. 108, 267201 (2012).pubmed.ncbi.nlm.nih.gov/23005010
  29. [29]Zhao, X., Tang, J., Pei, K., Wang, W., Lin, S.-Z., Du, H., Tian, M. & Che, R. Current-Induced Magnetic Skyrmions with Controllable Polarities in the Helical Phase. Nano Lett. 22, 8793–8800 (2022).DOI
  30. [30]Streubel, R., Bouma, D. S., Bruni, F., Chen, X., Ercius, P., Ciston, J., N’Diaye, A. T., Roy, S., Kevan, S. D., Fischer, P. & Hellman, F. Chiral Spin Textures in Amorphous Iron–Germanium Thick Films. Adv. Mater. 33, 2004830 (2021).DOI
  31. [31]Shibata, K., Yu, X. Z., Hara, T., Morikawa, D., Kanazawa, N., Kimoto, K., Ishiwata, S., Matsui, Y. & Tokura, Y. Towards control of the size and helicity of skyrmions in helimagnetic alloys by spin–orbit coupling. Nat. Nanotechnol. 8, 723–728 (2013).DOI
  32. [32]Kotani, A., Harada, K., Malac, M., Salomons, M., Hayashida, M. & Mori, S. Observation of FeGe skyrmions by electron phase microscopy with hole-free phase plate. AIP Adv. 8, 055216 (2018).DOI
  33. [33]Porter, N. A., Gartside, J. C. & Marrows, C. H. Scattering mechanisms in textured FeGe thin films: Magnetoresistance and the anomalous Hall effect. Phys. Rev. B 90, 024403 (2014).DOI
  34. [34]Wilhelm, H., Baenitz, M., Schmidt, M., Rößler, U. K., Leonov, A. A. & Bogdanov, A. N. Precursor Phenomena at the Magnetic Ordering of the Cubic Helimagnet FeGe. Phys. Rev. Lett. 107, 127203 (2011).DOI
  35. [35]Lebech, B., Bernhard, J. & Freltoft, T. Magnetic structures of cubic FeGe studied by small-angle neutron scattering. J. Condens. Matter Phys. 1, 6105 (1989).DOI
  36. [36]Ericsson, T., Karner, W., Haggstrom, L. & Chandra, K. Magnetic Structure of Cubic FeGe. Phys. Scr. 23, 1118 (1981).DOI
  37. [37]Ziegler, J. F., Ziegler, M. D. & Biersack, J. P. SRIM - The stopping and range of ions in matter (2010). Nuclear Instruments and Methods in Physics Research, Section B: Beam Interactions with Materials and Atoms 268, 1818–1823 (2010).DOI
  38. [38]Jain, A., Ong, S. P., Hautier, G., Chen, W., Richards, W. D., Dacek, S., Cholia, S., Gunter, D., Skinner, D., Ceder, G. & Persson, K. A. Commentary: The Materials Project: A materials genome approach to accelerating materials innovation. APL Materials 1, 011002 (2013).DOI
  39. [39]Zhang, X., Padgett, E., Zhu, L., Buhrman, R. & Muller, D. A Robust Basis for Grain Identification in Polycrystalline Thin Film Devices Using Cepstrum Transforms of 4D-STEM Diffraction Pattern. Microsc. Microanal. 26, 1620–1622 (Aug. 2020).DOI
  40. [40]Wang, H., Dai, Y., Chow, G.-M. & Chen, J. Topological hall transport: Materials, mechanisms and potential applications. Prog. Mater. Sci. 130, 100971 (2022).DOI
  41. [41]Sürgers, C., Fischer, G., Winkel, P. & Löhneysen, H. v. Large topological Hall effect in the non-collinear phase of an antiferromagnet. Nat. Commun. 5, 3400 (2014).DOI
  42. [42]Nagaosa, N. & Tokura, Y. Emergent electromagnetism in solids. Phys. Scr. 2012, 014020 (2012).DOI
  43. [43]Sivakumar, P. K., Göbel, B., Lesne, E., Markou, A., Gidugu, J., Taylor, J. M., Deniz, H., Jena, J., Felser, C. & Mertig, I. Topological Hall signatures of two chiral spin textures hosted in a single tetragonal inverse Heusler thin film. ACS Nano 14, 13463–13469 (2020).DOI
  44. [44]Hrkac, G., Keatley, P. S., Bryan, M. T. & Butler, K. Magnetic Vortex Oscillators. J. Phys. D 48, 453001 (2015).
  45. [45]Zhang, S., Petford-Long, A. K. & Phatak, C. Creation of artificial skyrmions and antiskyrmions by anisotropy engineering. Sci. Rep. 6, 31248 (2016).DOI
  46. [46]Camosi, L., Rohart, S., Fruchart, O., Pizzini, S., Belmeguenai, M., Roussigné, Y., Stashkevich, A., Cherif, S. M., Ranno, L., de Santis, M. & Vogel, J. Anisotropic Dzyaloshinskii-Moriya interaction in ultrathin epitaxial Au/Co/W(110). Phys. Rev. B 95, 214422 (2017).DOI
  47. [47]Nayak, A. K., Kumar, V., Ma, T., Werner, P., Pippel, E., Sahoo, R., Damay, F., Rößler, U. K., Felser, C. & Parkin, S. S. P. Magnetic antiskyrmions above room temperature in tetragonal Heusler materials. Nature 548, 561–566 (2017).DOI
  48. [48]Ma, T., Sharma, A. K., Saha, R., Srivastava, A. K., Werner, P., Vir, P., Kumar, V., Felser, C. & Parkin, S. S. P. Tunable Magnetic Antiskyrmion Size and Helical Period from Nanometers to Micrometers in a D₂d Heusler Compound. Adv. Mater. 32, 2002043 (2020).DOI
  49. [49]Zuniga Cespedes, B. E., Vir, P., Milde, P., Felser, C. & Eng, L. M. Critical sample aspect ratio and magnetic field dependence for antiskyrmion formation in Mn₁.₄PtSn single crystals. Phys. Rev. B 103, 184411 (2021).
  50. [50]Peng, L., Takagi, R., Koshibae, W., Shibata, K., Nakajima, K., Arima, T.-h., Nagaosa, N., Seki, S., Yu, X. & Tokura, Y. Controlled transformation of skyrmions and antiskyrmions in a non-centrosymmetric magnet. Nat. Nanotechnol. 15, 181–186 (2020).DOI
  51. [51]Shimizu, D., Nagase, T., So, Y.-G., Kuwahara, M., Ikarashi, N. & Nagao, M. Nanoscale Characteristics of a Room-Temperature Coexisting Phase of Magnetic Skyrmions and Antiskyrmions for Skyrmion–Antiskyrmion-Based Spintronic Applications. ACS Appl. Nano Mater. 5, 13519–13528 (2022).DOI
  52. [52]Saha, R., Srivastava, A. K., Ma, T., Jena, J., Werner, P., Kumar, V., Felser, C. & Parkin, S. S. P. Intrinsic stability of magnetic anti-skyrmions in the tetragonal inverse Heusler compound Mn₁.₄Pt₀.₉Pd₀.₁Sn. Nat. Commun. 10, 5305 (2019).DOI
  53. [53]Jamaluddin, S., Manna, S. K., Giri, B., Madduri, P. V. P., Parkin, S. S. P. & Nayak, A. K. Robust Antiskyrmion Phase in Bulk Tetragonal Mn–Pt(Pd)–Sn Heusler System Probed by Magnetic Entropy Change and AC-Susceptibility Measurements. Adv. Funct. Mater. 29, 1901776 (2019).DOI
  54. [54]Jena, J., Göbel, B., Ma, T., Kumar, V., Saha, R., Mertig, I., Felser, C. & Parkin, S. S. P. Elliptical Bloch skyrmion chiral twins in an antiskyrmion system. Nat. Commun. 11, 1115 (2020).DOI
  55. [55]Jena, J., Göbel, B., Kumar, V., Mertig, I., Felser, C. & Parkin, S. Evolution and competition between chiral spin textures in nanostripes with D₂d symmetry. Sci. Adv. 6, eabc0723 (2020).DOI
  56. [56]Kumar, V., Kumar, N., Reehuis, M., Gayles, J., Sukhanov, A. S., Hoser, A., Damay, F. C., Shekhar, C., Adler, P. & Felser, C. Detection of antiskyrmions by topological Hall effect in Heusler compounds. Phys. Rev. B 101, 014424 (2020).DOI
  57. [57]Madduri, P. V. P., Sen, S., Giri, B., Chakrabartty, D., Manna, S. K., Parkin, S. S. P. & Nayak, A. K. ac susceptibility study of magnetic relaxation phenomena in the antiskyrmion-hosting tetragonal Mn-Pt(Pd)-Sn system. Phys. Rev. B 102, 174402 (2020).DOI
  58. [58]Karube, K., Peng, L., Masell, J., Yu, X., Kagawa, F., Tokura, Y. & Taguchi, Y. Room-temperature antiskyrmions and sawtooth surface textures in a non-centrosymmetric magnet with S₄ symmetry. Nat. Mater. 20, 335–340 (2021).DOI
  59. [59]Kuchkin, V. M. & Kiselev, N. S. Turning a chiral skyrmion inside out. Phys. Rev. B 101, 064408 (2020).DOI
  60. [60]Feng, D., Guan, Z., Wu, X., Wu, Y. & Song, C. Classification of skyrmionic textures and extraction of Hamiltonian parameters via machine learning. Phys. Rev. Appl. 21, 034009 (3 2024).arxiv.org/abs/2309.15679
  61. [61]Dzyaloshinsky, I. A thermodynamic theory of “weak” ferromagnetism of antiferromagnetics. J. Phys. Chem. Solids 4, 241–255 (1958).DOI
  62. [62]Noodleman, L. Valence bond description of antiferromagnetic coupling in transition metal dimers. J. Chem. Phys. 74, 5737–5743 (May 1981).DOI
  63. [63]Nagaosa, N., Sinova, J., Onoda, S., MacDonald, A. H. & Ong, N. P. Anomalous Hall effect. Rev. Mod. Phys. 82, 1539–1592 (2010).DOI
  64. [64]Onoda, S., Sugimoto, N. & Nagaosa, N. Quantum transport theory of anomalous electric, thermoelectric, and thermal Hall effects in ferromagnets. Phys. Rev. B 77, 165103 (2008).DOI
  65. [65]Tsymbal, E. & Zutic, I. Handbook of Spin Transport and Magnetism (CRC Press, Boca Raton, FL, 2011).
  66. [66]Li, Y., Kanazawa, N., Yu, X. Z., Tsukazaki, A., Kawasaki, M., Ichikawa, M., Jin, X. F., Kagawa, F. & Tokura, Y. Robust Formation of Skyrmions and Topological Hall Effect Anomaly in Epitaxial Thin Films of MnSi. Phys. Rev. Lett. 110, 117202 (2013).pubmed.ncbi.nlm.nih.gov/25166569
  67. [67]Tian, Y., Ye, L. & Jin, X. Proper Scaling of the Anomalous Hall Effect. Phys. Rev. Lett. 103, 087206 (2009).DOI
  68. [68]Zhang, X., Xia, J., Zhou, Y., Liu, X., Zhang, H. & Ezawa, M. Skyrmion dynamics in a frustrated ferromagnetic film and current-induced helicity locking-unlocking transition. Nat. Commun. 8, 1717 (2017).DOI
  69. [69]Lin, S.-Z. & Hayami, S. Ginzburg-Landau theory for skyrmions in inversion-symmetric magnets with competing interactions. Phys. Rev. B 93, 064430 (2016).DOI
  70. [70]Leonov, A. O. & Mostovoy, M. Multiply periodic states and isolated skyrmions in an anisotropic frustrated magnet. Nat. Commun. 6, 8275 (2015).DOI
  71. [71]Hu, Y., Chi, X., Li, X., Liu, Y. & Du, A. Creation and Annihilation of Skyrmions in the Frustrated Magnets with Competing Exchange Interactions. Sci. Rep. 7, 16079 (2017).DOI
  72. [72]Ritzmann, U., von Malottki, S., Kim, J.-V., Heinze, S., Sinova, J. & Dupé, B. Trochoidal motion and pair generation in skyrmion and antiskyrmion dynamics under spin–orbit torques. Nat. Electron. 1, 451–457 (2018).arxiv.org/abs/1803.00534
  73. [73]Huang, S., Zhou, C., Chen, G., Shen, H., Schmid, A. K., Liu, K. & Wu, Y. Stabilization and current-induced motion of antiskyrmion in the presence of anisotropic Dzyaloshinskii-Moriya interaction. Phys. Rev. B 96, 144412 (2017).DOI

Paper details

vlnc:W_che3kc54
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 9

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents