A multi-scale probabilistic methodology to predict high-cycle fatigue lifetime for alloys with process-induced pores

Abstract

A multi-scale methodology is developed in conjunction with a probabilistic fatigue lifetime model for structures with pores whose exact distribution, i.e. geometries and locations, is unknown. The method takes into account uncertainty in fatigue lifetimes in structures due to defects at two scales: micro-scale heterogeneity & meso-scale pores. An element-wise probabilistic strain-life model with its criterion modified for taking into account multiaxial loading is developed for taking into account the effect of micro-scale defects on the lifetime. Meso-scale pores in the structure are taken into account via statistical modelling of the expected pore populations via a finite element method, based on tomographic scans of a small region of porous material used to make the structure. A previously implemented Neuber-type plastic correction algorithm is used for fast full-field approximation of the strain-life criterion around the statistically generated pore fields. The probability of failure of a porous structure is obtained via a weakest link assumption at the level of its constituent finite elements. The fatigue model can be identified via a maximum likelihood estimate on experimental fatigue data of structures containing different types of pore populations. The proposed method is tested on an existing high-cycle fatigue data-set of an aluminium alloy with two levels of porosity. The model requires lesser data for identification than traditional models that consider porous media as a homogeneous material, as the same base material is considered for the two grades of porous material. Numerical studies on synthetically generated data show that the method is capable of taking into account the statistical size effect in fatigue, and demonstrate that fatigue properties of subsurface porous material are lower than that of core porous material, which makes homogenisation of the method non-trivial.

List of Symbols

SymbolDescription
RRRatio of minimum to maximum stress in a load cycle
σy\sigma_yYield stress of the material
Σa\Sigma_aApplied stress amplitude
ΔΣ\Delta\SigmaApplied stress range
Δε∗\Delta\varepsilon^*Total strain range in an element for the stabilized cycle
Δεe∗\Delta\varepsilon^{e*}Elastic strain range in an element for the stabilized cycle
Δεp∗\Delta\varepsilon^{p*}Plastic strain range in an element for the stabilized cycle
NR∗N_R^*Number of cycles to failure of an element
V∗V^*Volume of an element
ε~∗\widetilde{\varepsilon}^*Total strain tensor of an element
ε~p∗\widetilde{\varepsilon}^{p*}Plastic strain tensor of an element
ε~e∗\widetilde{\varepsilon}^{e*}Elastic strain tensor of an element
Tc\mathcal{T}_cStabilized cycle
n∗n^*Eigenvector associated to the highest eigenvalue of the stress tensor of an element coming from a separate elastic computation
σ#∗\sigma^{\#*}Stress tensor of an element coming from a separate elastic computation
A,α,B,β,CA,\alpha,B,\beta,CParameters of the strain-life model
W\mathcal{W}Weibull distribution
m,λm,\lambdaWeibull shape and scale parameters
FNR∗F_{N_R^*}Cumulative distribution function of failure for elements
fNR∗f_{N_R^*}Probability density function of failure for elements
FNRsF_{N_R}^{s}Cumulative distribution function of failure for a specimen
fNRsf_{N_R}^{s}Probability density function of failure for the specimen
L\mathcal{L}Likelihood function
μ\muSet of optimized parameters
μ~\widetilde{\mu}Set of intermediary parameters tested by an optimizer
H\mathcal{H}Set of fatigue experiments for geometrically homogeneous specimens
I\mathcal{I}Set of fatigue experiments for a fixed heterogeneous specimen
J\mathcal{J}Set of fatigue experiments for porous specimens
K\mathcal{K}Set of all possible configurations of synthetically generated porous specimens
K~\widetilde{\mathcal{K}}Set of finite synthetically generated porous specimens

Introduction

Pores in structures are known to reduce their fatigue lifetimes. For the lifetime prediction of such structures, simplified approaches are available. One approach models the porous material as a homogenised substance with equivalent fatigue properties, eliminating the need to describe individual pores directly [1]. However, the applicability of such models relies on fatigue data from structures made of the specific porous material and cannot be transferred to structures with the same base material but different pore characteristics. Other, more recent approaches rely on the availability of the exact pore distribution in order to predict the fatigue lifetime of the structure, usually obtained via computed tomography (CT) scans [2, 3]. However, this may not be suitable for all scenarios, as CT scans of a structure are expensive to obtain and analyse. Moreover, calibration of such a model requires a database of CT scans for a number of specimens tested for failure. Another category of approaches employ statistical methods to consider all possible pore distributions, based on a small representative CT scan of the porous material, when making lifetime predictions of a structure. Some of these approaches do not explicitly model the pore distribution, but use Poisson point processes to generate simplified pore distributions, and make predictions with the help of a Kitagawa Takahashi (KT) diagram that links the fatigue limit to the size of the pores [4, 5]. These approaches assume that a single killer pore is responsible for fatigue failure, and do not take into account pore morphology or interactions between pores. Furthermore, obtaining the KT diagram is a lengthy experimental process. Finally, other proposals exist that quantify uncertainty in fatigue lifetime due to statistical variability in meso-scale pores by employing finite element analysis to represent the pores. These approaches typically simplify the representation of pore geometries to spheres or ellipses [6, 7], either neglecting inter-pore interactions [8] or restricting the model to two-dimensional structures [9, 10].

We present a multi-scale method that takes into account uncertainty in fatigue lifetime of structures due to uncertainty in entities at two scales: meso-scale pores and micro-scale heterogeneity. Our approach allows to model the lifetime of structures with varying levels of porosity using a unified fatigue model, thereby reducing the total amount of fatigue data required for model identification as compared to the simplified approaches considering homogenized porous behavior. This is because statistical information on fatigue lifetime is shared between datasets of different porosity grades, as the same base material behaviour around the pores is considered. For the behavior of the base material, a local strain-life model, as proposed by Manson [11], is selected. The variability in the base material’s lifetime, resulting from micro-scale heterogeneity — including factors like varying grain orientation and the presence of precipitates [2] — is reflected in the strain-life model by making its criterion probabilistic. The physics of this micro-scale heterogeneity are not explicitly modelled. Moreover, the criterion has been carefully selected to address the existence of two fatigue regimes (dependent on the magnitude of loading) that are commonly observed in experiments [12], and to accommodate multiaxial stress-strain states [13, 14, 15] that are likely to be found in the base material around pores. At the meso-scale, the model incorporates the actual three-dimensional geometries of the pores and typical inter-pore spacing by explicitly modelling them using the finite element method. An elasto-plastic material behaviour is adopted to account for the plasticity present in the vicinity of the pores. The probabilistic lifetime of this porous structure is determined by a weakest link hypothesis [16, 17, 18], on the finite elements that comprise the structure. The entire structure is considered as multiple hot spots may form in porous media due to complex stress fields arising from pore-pore and pore-surface interactions [3]. Due to the presence of ligaments, the location of the critical hot spot is uncertain, making it difficult to apply the concept of critical distances [19] in the fatigue criterion. On the other hand, in highly stressed volume (HSV) approaches, the size of the stressed volume is a parameter that requires experimental pre-identification [4, 20, 21, 22].

In the event of uncertainty regarding the meso-scale pore distribution, the overall lifetime of the structure is addressed by introducing statistical variability into the pore distribution within the structure. In other words, a degree of randomness is assumed in the pore distribution due to the unavailability of precise prior information on the pore states in the structure that lead to fatigue failure. The model operates under the assumption that the precise pore distribution responsible for a particular fatigue lifetime data point is unknown. Instead, a computed tomography (CT) scan of a different volume, made from the same porous material as the structure, is obtained to gather statistical information regarding the pores that are likely to be contributing to the observed failure of the structure. This statistical data serves as the input to the proposed lifetime model, which, by considering various potential pore positions and characteristics, computes a lifetime probability for a given structure without the need for precise knowledge of its pore distribution. This approach allows for the uncertainty in lifetime due to all possible pore distributions to be taken into account, including the effect of pore-pore and pore-surface interactions. We also demonstrate the difficulty of bypassing the multi-scale method with a homogenised model; a fatigue model identified for porous material in one type of structure may not always be accurate when applied to other structures.

Probabilistic lifetime models based on the weakest link approach for non-smooth geometries are identified through iterative optimisation in one of two methods. One approach employs an effective criterion within an equivalent volume to address non-homogeneous stress distributions, thereby reducing the optimisation to a 0D space [23]. Other authors employ full-field mechanical information in the optimisation process. For instance, the stress is utilised when the loading remains elastic throughout [24], while the strain energy is employed in the event of plasticity [18]. However, the majority of weakest link approaches are concerned with notched structures [17, 18, 24, 25]. The identification of a lifetime model based on the weakest link approach for a porous structure modelled with the finite element method, where the exact pore distribution is unknown, has yet to be addressed in the literature and will be discussed in this paper.

The criteria of the lifetime model requires access to the full-field elasto-plastic solutions of structures with varying pore distributions subjected to fatigue loading. The presence of local non-linearity in the material model due to localized plasticity around the pores, the need for a high number of degrees of freedom to model the complex geometries of the pores, and the requirement to obtain the stabilised cycle due to a transient hardening phase all make these computations prohibitively costly. Our final innovation consists in accelerating these computations via our previously developed plastic correction algorithm. The algorithm is a Neuber-type plastic correction heuristic coupled with machine learning methods that allows rapid recovery of the tensorial elasto-plastic solution in entire structures for arbitrary (proportional) applied loading [26].

This paper is divided into six sections. Section two presents a data set pertaining to a material with two levels of porosity, which will be used for further developments. Section three presents the lifetime model and the multi-scale methodology for obtaining the lifetime of porous structures. Section four is dedicated to maximum likelihood methods for identifying the parameters of the lifetime model on experimental high-cycle fatigue data sets, including a proposal for dealing with structures with unknown pore distributions. Section five presents the results of calibration for the previously presented high-cycle fatigue data set, while detailing the process of the convergence of the solution and the optimisation behaviour, and also presents an analysis of the fatigue model complexity. Section six is dedicated to numerical investigations of additional natural properties of the model, including its capacity to account for the size effect and pore-surface interaction effects. This section also tests the limits of a naive homogenisation approach with the objective of reducing the cost of utilising the multi-scale approach, which involves explicit pore descriptions. The paper is concluded with an overview of the findings and some elements of discussion.

Experimental data

Although the proposed methodology is relatively general by design, the developments are dedicated to the case of a specific porous material for which the following data is available: (i) the number of cycles to failure in the high cycle fatigue (HCF) regime for a relatively large number of traction specimens, and (ii) tomographic data to characterise the distribution and morphology of the pores. This dataset is described below.

Composition, grades and manufacturing process.

An Al-Si7Mg0.3 alloy is considered (i.e. 7% silicon, 0.3% magnesium and balance aluminium in weight %). Alloy ’B’ is produced using the lost foam casting process, followed by a heat treatment, and contains shrinkage and gas pores. The second alloy, designated ’C’, is produced using the same lost foam casting process as the alloy ’B’, followed by hot isostatic pressing (HIP) at a temperature of 500°C and a pressure of 1000 bars. This results in a virtually porosity-free alloy, which is then subjected to the same heat treatment as the alloy ’B’. The alloy ’C’ is therefore referred to as the non-porous alloy.

The manufacturing process yields slabs of these materials, and specimens for subsequent characterisation (including fatigue tests and CT scans) were obtained from the centre of these slabs, in order to avoid edge effects during casting and thus ensure the accuracy of the microstructure of the materials. Further details on the manufacturing process can be found in the work of other authors [27].

Microstructure and tension-compression fatigue failure mechanisms.

The microstructures and characteristics of pores in these alloys have been previously investigated by other researchers [4, 28, 29]. The base material found in the two grades ’B’ and ’C’, have very similar microstructural characteristics. These include similar values of dendrite and secondary dendrite arm spacing, similar sizes of silicon precipitates, and comparable grain sizes [27].

The porous alloy ’B’ has a volumetric fraction of pores of approximately 0.28%, exhibiting a distribution of varying pore shapes and sizes. The maximum equivalent pore size, defined by the square root of the area observed by optical microscopy scans, reaches up to 300 μm\mu\mathrm{m}. In the case of the non-porous alloy ’C’, the presence of very small pores (with the maximum effective size < 50 μm\mu\mathrm{m}) has been observed.

In conditions of tension-compression fatigue loading, the porous alloy ’B’ is known to fail due to high stress concentration factors in the vicinity of pores. This often occurs as a result of a crack forming from a surface-breaking pore, from the interaction between sub-surface pores and the surface of the specimen, or from the coalescence of cracks originating from several pores [28, 29]. The primary cause of tension-compression fatigue failure in the non-porous alloy ’C’ is micro-plastic activity, namely the formation of persistent slip bands from which critical cracks originate [28].

Tension-compression fatigue experiments without prior tomography.

A limited data set comprising 32 fatigue experiments for the non-porous alloy and 34 fatigue experiments for the porous alloy is available [28]. These experiments were conducted in the HCF regime, under symmetric tension-compression conditions with zero mean stress (R=−1R = -1) at a frequency of 100 Hz. The applied stress range on these specimens (ΔΣ\Delta\Sigma) is always within the elastic regime and is defined as the difference between the maximum and minimum applied load in a cycle. The applied stress amplitude is defined as half the applied stress range, expressed as follows: Σa=ΔΣ2\Sigma_a = \frac{\Delta\Sigma}{2}.

The geometry of the specimens used is shown in Figure 1a and the results are recalled in a applied stress amplitude (Σa\Sigma_a) - lifetime (NRN_R) plot in Figure 1b. The tomographies of the specimens used for fatigue experiments are not available. As the specimens were cut from a bigger slab, the pores in these specimens are volumetric pores created due to the manufacturing process. For all experiments, a maximum limit on the number of loading cycles was set at 2×1062 \times10^6 cycles. The specimens which did not break (termed run-outs) were counted and reported at the NR=2×106N_R = 2 \times10^6 mark with an arrow to the right to indicate potential failure for a larger number of cycles (Figure 1b).

Computed tomography of a volume with pores.

A computed tomography scan of a 12×13×3 mm312 \times13 \times3\ \mathrm{mm}^3 region of a planar specimen, made using the same porous material as the cylindrical specimens used for fatigue experiments, was carried out in order to get information on the pore characteristics likely to have caused fatigue failure. The planar specimen was cut from a larger slab, as was the case with the cylindrical specimens employed in fatigue testing. Thus, the pores in the planar specimen are also volumetric pores resulting from the manufacturing process. The resolution of the tomograph was ∼11 μm\sim11\ \mu\mathrm{m}. The tomographic volume of interest was 424×1211×1000424 \times1211 \times1000 voxels with 16-bit unsigned images. Segmentation of the pores was carried out using a threshold value in grey-level contrast levels, resulting in a binary 3D image of the pores. A surface mesh was generated using Avizo, employing smoothing to remove artefacts. The resulting surface mesh, illustrated in Figure 2 is used in subsequent sections.

Tomography of a porous planar specimen

Figure 2. Tomography of 12×13×3 mm312 \times13 \times3\ \mathrm{mm}^{3} region of a planar specimen made using the same porous material as the cylindrical specimens used for fatigue experiments

Multi-scale probabilistic fatigue lifetime model

Micro and meso scale defects

A probabilistic multi-scale approach is proposed for the fatigue lifetime prediction of specimens containing a distribution of pores and microstructural heterogeneity. The first scale, henceforth termed the micro-scale, accounts for the effect of microstructural heterogeneity on the fatigue lifetime. The microstructural heterogeneity is not explicitly modelled; its effect is considered by making the fatigue lifetime model probabilistic [31, 32, 33, 34, 35]. This approach is adopted as the exact state of the microstructure is not known and would be too costly to model at the scale of the specimens undergoing fatigue loading. The lifetime distribution of an elementary volume subjected to a uniform stress depends

on its volume and on the mechanical load to which it is subjected; further details of the construction of this probabilistic model will be explained in the next subsection. The second scale, defined as the meso-scale, comprises tomography-informed pore distributions that are embedded in the base material containing the microstructural heterogeneity. This is shown schematically in Figure 3. The effects of the pore distribution on the fatigue lifetime are considered by explicitly modelling these pores via a finite element model (see Figure 4). The sizes, shapes, and locations of pores with respect to other pores and the surfaces of the specimen all influence the fatigue lifetime. The meso-scale part of the model accounts for uncertainty due to varying pore distributions by synthetically generating them.

Example of a specimen containing a sub-volume of pores, with micro-plasticity activating in the base material between the pores

Figure 3. Example of a specimen containing a sub-volume of pores, with micro-plasticity activating in the base material between the pores

Example of a specimen containing a sub-volume of pores as a finite element mesh, with a zoom of the mesh around one pore

Figure 4. Example of a specimen containing a sub-volume of pores as a finite element mesh, with a zoom of the mesh around one pore

Due to the presence of explicitly represented pores in the fatigue specimen, the mechanical stress in the synthetic specimens is heterogeneous. At macroscopic stress greater than σy\sigma_y, local plasticity is expected to develop around the pores due to stress concentrations. The micro-scale model may be used element-wise to obtain a probability distribution of failure per element.

The overall life of such a porous specimen is derived from the lifetime probability density of the individual finite elements that constitute it, via the standard weakest link assumption [16]. This modelling brick will be detailed after the explanation of the micro and meso scales of the model.

Probabilistic modelling of the life span at the material point level (micro-scale uncertainty modelling)

In this section, a probabilistic element-wise strain life model (with two regimes) is developed. The element-wise model needs to be based on multiaxial criterion, as the local stress state for regions around the pores in specimens depicted in Figure 3 is multiaxial. The fatigue lifetime of an element ∗∈E\ast\in\mathcal{E} (where E\mathcal{E} is the set of finite elements constituting a specimen) is obtained as a probability distribution, given a damage criterion Δε∗2\frac{\Delta\varepsilon^{\ast}}{2} and the volume V∗V^{\ast} of the element ∗\ast.

Deterministic strain-life approach.

The strain life approach assumes that the fatigue lifetime of an element NR∗N_{\mathrm{R}}^{\ast} is governed by half the total strain range experienced by the element (Δε∗2)\left(\frac{\Delta\varepsilon^{\ast}}{2}\right) by a standard two-line model [12]:

Δε∗2=g(NR∗)=A(NR∗)−α+B(NR∗)−β+C(1)\frac{\Delta\varepsilon^{\ast}}{2}=g\left(N_{\mathrm{R}}^{\ast}\right)=A\left(N_{\mathrm{R}}^{\ast}\right)^{-\alpha}+B\left(N_{\mathrm{R}}^{\ast}\right)^{-\beta}+C \tag*{(1)}

where AA and α\alpha correspond to the parameters of the high-cycle fatigue (HCF) line, BB and β\beta correspond to the parameters of the low-cycle fatigue (LCF) line and CC controls the fatigue limit, as illustrated in Figure 5. As local plasticity may appear depending on the loading in the element, Δε∗\Delta\varepsilon^{\ast} is computed in the stabilized cycle with period TcT_{\mathrm{c}}, in the following manner [15]:

Figure 5. Schematic of the probabilistic strain-life model with two straight lines connected with an elbow in the log⁡(Δε∗2)\log\left(\frac{\Delta\varepsilon^*}{2}\right)-log⁡(NR∗)\log(N_{\mathrm{R}}^*) plane for modelling the two regimes (for low and high-cycle fatigue), and CC giving the fatigue limit

Δε∗=[max⁡t∈Tc(n∗⋅εc∗(t)⋅n∗)−min⁡t∈Tc(n∗⋅εc∗(t)⋅n∗)](2)\Delta\varepsilon^{\ast}=\left[\max_{t\in T_{\mathrm{c}}}\left(n^{\ast}\cdot\varepsilon_{\mathrm{c}}^{\ast}(t)\cdot n^{\ast}\right)-\min_{t\in T_{\mathrm{c}}}\left(n^{\ast}\cdot\varepsilon_{\mathrm{c}}^{\ast}(t)\cdot n^{\ast}\right)\right] \tag*{(2)}
n∗=arg max⁡n⋅n=1(n⋅σ#∗⋅n)(3)n^{\ast}=\underset{n\cdot n=1}{\operatorname{arg\,max}}\left(n\cdot\sigma^{\#\ast}\cdot n\right) \tag*{(3)}

Here, σ#∗\sigma^{\#\ast} is element’s stress tensor coming from a separate elastic computation and n∗n^{\ast} is the eigenvector associated to the highest eigenvalue of σ#∗\sigma^{\#\ast}. The quadratic form (n∗⋅εc∗(t)⋅n∗)\left(n^{\ast}\cdot\varepsilon_{\mathrm{c}}^{\ast}(t)\cdot n^{\ast}\right) of the element’s total strain tensor εc∗\varepsilon_{\mathrm{c}}^{\ast} is obtained along this critical direction for the full loading sequence. The range of this quantity in the period of the stabilized stress-strain cycle TcT_{\mathrm{c}} is computed. This procedure allows to account for the local multiaxiality that may cause a change in the critical direction from element to element. The underlying assumption is that local non-proportionality remains low [36].

As g(NR∗)g\left(N_{\mathrm{R}}^{\ast}\right) is monotonic, there exists a function g−1g^{-1} defined as:

g−1:]C,+∞)→]0,+∞)(4)g^{-1}: ]C,+\infty)\rightarrow]0,+\infty) \tag*{(4)}

Probabilistic strain-life approach.

The fatigue lifetime model will now be made probabilistic. The fatigue lifetime is considered to be stochastic due to randomness in underlying total damage over all cycles that a specimen with volume V∗V^{\ast} may undergo before failing. The total damage G\mathcal{G} is modelled as a random variable, and the form of the associated probability distribution is considered to be a Weibull distribution that respects weakest link scaling [16]:

NR∗g−1(Δε∗2)=G(5)\frac{N_{\mathrm{R}}^{\ast}}{g^{-1}\left(\frac{\Delta\varepsilon^{\ast}}{2}\right)}=\mathcal{G} \tag*{(5)}

with the cumulative distribution function (CDF) of G\mathcal{G} being denoted as FG(g)F_{\mathcal{G}}(g):

FG(g)=1−{exp⁡(−{gg0}m)}V∗V0(6)F_{\mathcal{G}}(g)=1-\left\{\exp\left(-\left\{\frac{g}{g_{0}}\right\}^{m}\right)\right\}^{\frac{V^{\ast}}{V_{0}}} \tag*{(6)}

where g0=1(ln⁡2)1/mg_{0}=\frac{1}{(\ln2)^{1/m}}, which implies that the median of this Weibull distribution is equal to 1 for a volume V∗=V0V^{\ast}=V_{0}. Here, mm is the shape parameter of the Weibull distribution. By a change of variables, this leads to the following expression for the fatigue lifetime NR∗N_{\mathrm{R}}^{\ast} (with its CDF being denoted as FNR∗(N;Δε∗,V∗))F_{N_{\mathrm{R}}^{\ast}}(N;\Delta\varepsilon^{\ast},V^{\ast})):

NR∗∼W(λ=g−1(Δε∗2){1ln⁡2V0V∗}1/m,m)(7)N_{\mathrm{R}}^{\ast}\sim\mathcal{W}\left(\lambda=g^{-1}\left(\frac{\Delta\varepsilon^{\ast}}{2}\right)\left\{\frac{1}{\ln2}\frac{V_{0}}{V^{\ast}}\right\}^{1/m},m\right) \tag*{(7)}
FNR∗(N)=1−exp⁡(−{Nλ}m)(8)F_{N_{\mathrm{R}}^*}(N)=1-\exp\left(-\left\{\frac{N}{\lambda}\right\}^{m}\right) \tag*{(8)}

where λ\lambda is the scale parameter of the Weibull distribution describing the fatigue lifetime of the element. It is noted that a higher V∗V^* or a higher Δε∗2\frac{\Delta\varepsilon^*}{2} (leading to lower g−1g^{-1}) will cause the Weibull scale parameter λ\lambda to decrease, thus causing the lifetime probability distribution to shift to the left.

The set of parameters introduced, including the strain-life parameters and the Weibull shape parameter, is thus:

μ=[m,A,B,α,β,C](9)\mu=[m,A,B,\alpha,\beta,C] \tag*{(9)}

Henceforth, the dependence of FNR∗F_{N_{\mathrm{R}}^*} on μ\mu will be introduced as FNR∗(N;Δε∗,V∗,μ)F_{N_{\mathrm{R}}^*}(N;\Delta\varepsilon^*,V^*,\mu). The probability density function (PDF) of fatigue lifetime of the element * will be denoted as fNR∗(N;Δε∗,V∗,μ)f_{N_{\mathrm{R}}^*}(N;\Delta\varepsilon^*,V^*,\mu).

Statistical modeling of the pore distributions at the meso-scale

The meso-scale part of the model takes into account the uncertainty in fatigue lifetime of porous specimens due to varying pore distributions by synthetically generating them. In the context of our research, the precise positions and morphology of pores within the specimens for which we aim to predict lifespan are unknown and not sought, resulting in inherent uncertainty. If the positions and morphologies of the pores were known, the model could be identified directly from the exact tomographies of the tested specimens rather than from synthetic ones. This approach would then align with fatigue studies on deterministic geometries, such as notches [18, 24]. The distinct feature of our work lies in addressing the randomness of pore positions rather than deterministic pore distribution configurations, highlighting the unique challenge of random pore distribution in predicting material fatigue.

The synthetically generated porous specimens have the same geometry as the specimens used for fatigue testing (Figure 1a), but with the pores inspired by the computed tomography (Figure 2). These synthetically generated porous specimens thus resemble the traction specimens used for fatigue testing. The resulting meshes have linear elements with a piece-wise constant approximation of the stresses.

Synthetic pore field generator from CT scans.

The tomographic scan of the porous specimen used for getting information on pores was shown in Figure 2. A volume threshold is applied on this scan to exclude small pores. A pore is accepted if the radius of a sphere with the same volume as the pore is greater than 50 μm50\,\mu\mathrm{m}. This is justified by other authors, who show that in presence of large sized porosity, smaller pores have a negligible effect in fatigue life and that in the high cycle fatigue regime, cracks systematically originate from large pores [37, 30, 4]. This size filter step is illustrated in Figure 6.

Segmented defects, with accepted defects shown in black and rejected defects shown in red

Figure 6. Segmented defects, with accepted defects (black) and rejected defects (red) based on their size (acceptance for effective radius of a sphere of same volume as the defect ≥50 μm\ge50\,\mu\mathrm{m})

Surface meshes of the remaining pores after the size-filtering step were obtained using smoothing based on a criterion on sharp angles between surfaces of the pores - the original surfaces from the tomography and the remeshed surfaces are shown in Figure 7. This smoothing is done to facilitate finite element meshing.

Curvature based surface re-meshing of the defect surfaces before and after smoothing

Figure 7. Curvature based surface re-meshing of the defect surfaces

A set of synthetically generated porous specimens (with varying pore distributions) was created by using an algorithm based on this set of size-filtered and smoothed pores. The volume of the gauge section of the cylindrical fatigue specimens, being around 593 mm3593\,\mathrm{mm}^{3}, contains a very large number of pores (and therefore elements). A splitting of the computational domain into sub-volumes is therefore carried out to avoid memory limitations. The following steps were done to synthetically generate porous specimens:

  1. A CAD geometry of the cylindrical specimen used for fatigue experiments was created using GMSH

[38].

  1. The gauge section of this CAD geometry was randomly superposed with the representative volume of pores, and the set of pores intersecting with the geometry were retained for meshing.

  1. A meshing operation is carried out in the base material between the surfaces of the specimens and the pores, with adequate refinement of the mesh close to the pores, using GMSH. Thus, only one region or sub-volume of the gauge section contains pores, henceforth referred to as a ’porous sub-volume’.

  1. The previous two steps were carried out 100 times, to get 100 such specimens each with a different region of pores (illustrated in Figure 8 (a)).

Random intersection of the defects with the geometric CAD representation of the fatigue specimens and assembly of randomly selected porous sub-volumes

Figure 8. (a) Random intersection of the defects with the geometric CAD representation of the fatigue specimens, with the defects being meshed into the specimen if it falls within the colored sub-volumes (process repeated 100 times) (b) Assembly of randomly selected porous sub-volumes to obtain a synthetically generated porous specimen with defects in its gauge section

  1. Elements in the ’porous subvolumes’ of these 100 specimens are extracted. A random combination of porous sub-volumes that equal the volume of the gauge section of the cylindrical specimen makes up one synthetically generated porous specimen (illustrated in Figure 8 (b)).

Elasto-plastic computations.

The multi-scale probabilistic fatigue model developed requires the computation of the local criterion (Δε∗)(\Delta\varepsilon^{*}) for all the finite elements comprising the porous specimens due to applied stress amplitude on the specimen (Σa\Sigma_a) for computation of the specimen’s fatigue lifetime probability distribution. As the presence of pores in the specimen causes high stress concentration factors leading to local yielding, we consider a Chaboche-type plastic material behavior, consisting of non-linear isotropic and kinematic hardening. The equations are recalled in table 1.

Elasticityσ=C:(ε−εp)\sigma= C : \left(\varepsilon- \varepsilon^p\right)
Strain partitioningε=εe+εp\varepsilon= \varepsilon^e + \varepsilon^p
Yield functionfy(σ;X,p)=J(σ−X)−σy−R(p)f_y(\sigma; X,p) = J\left(\sigma-X\right)-\sigma_y-R(p)
Evolution of yield functionfyp˙=0f_y\dot{p}=0 and fy≤0f_y\leq0
Isotropic HardeningR(p)=Q(1−exp⁡(−bp))R(p)=Q\left(1-\exp(-bp)\right)
Kinematic HardeningX˙=23Cε˙p−DXp˙\dot{X}=\frac{2}{3}C\dot{\varepsilon}^p-DX\dot{p}
Flow ruleε˙p=p˙(32σd−XJ(σd−X))\dot{\varepsilon}^p=\dot{p}\left(\frac{3}{2}\frac{\sigma_d-X}{J\left(\sigma_d-X\right)}\right)
Cumulative plastic strainp˙=23ε˙dp:ε˙dp\dot{p}=\sqrt{\frac{2}{3}\dot{\varepsilon}^p_d:\dot{\varepsilon}^p_d}

Table 1. Set of equations used for the mechanical behavior - with σ\sigma being the stress tensor, σd\sigma_d being the deviatoric stress tensor, CC the stiffness tensor, ε\varepsilon the total strain, εe\varepsilon^e and εp\varepsilon^p the elastic and plastic strain tensors respectively, JJ the von Mises yield function, pp the cumulative plastic strain, and εdp\varepsilon^p_d the deviatoric plastic strain [39]

However, time integration of non-linear material behavior is time-consuming and resource heavy, especially for large meshes. Therefore, a plastic corrector is used, which allows rapid approximation/post-processing of the full-field elasto-plastic response of specimens for any proportional loading sequence when given elastic FEA results at one timestep [26]. An example of the approximation quality of the criterion with respect to a reference computation is shown in Appendix § 12 on a subvolume of pores.

The following steps highlight the process:

  1. Elasto-static computations are performed on the sub-volumes of the synthetically generated specimens with the FEniCS [40] software.

  1. The approximate elasto-plastic solution is reconstructed in a space-time domain, for several nominal loading levels, by a plastic corrector that approximates elasto-plasticity for any form of proportional applied loading via post-processing of elasto-static finite element results [26]

  1. The local total strain amplitude (Δε∗\Delta\varepsilon^*) is extracted for the stabilized cycle for all the elements comprising the gauge section of the generated specimens and for all the nominal loading levels.

Probabilistic lifetime model at the structure level : weakest link assumption

A structure with a heterogeneous stress distribution, for example, a structure with pores that are explicitly meshed, or a structure with a notch, will have different values of the criterion (Δε∗\Delta\varepsilon^*) in different elements of the structure for a given applied stress amplitude Σa\Sigma_a. We formally define a function Δε∗(Σa):Σa↦Δε∗\Delta\varepsilon^*(\Sigma_a): \Sigma_a \mapsto\Delta\varepsilon^* that maps the load applied to the structure as boundary condition to the fatigue criterion in element ∗*. This function is computed by FEA. The probabilistic strain-life model developed in section 3.2 can subsequently be applied to all the elements of the FE mesh. The CDF of fatigue lifetime of a given element in the geometrically heterogeneous case is thus obtained as FNR∗(N;Δε∗(Σa),V∗,μ)F_{N_{\mathrm{R}}^*}(N;\Delta\varepsilon^*(\Sigma_a),V^*,\mu), as given in equation (8).

A weakest link hypothesis is used to obtain the fatigue lifetime density of the full structure. In this model, the failure of the structure is given by the failure of the first element of the FE mesh. The weakest link hypothesis assumes that the failure of the elements are statistically independent events. The probability of the survival of a structure ss (modelled by the random variable NRsN_{\mathrm{R}}^s) is given by:

Prob⁡(NRs≥N)=∏∗∈EProb⁡(NR∗≥N)(10)\operatorname{Prob}(N_{\mathrm{R}}^s \ge N)=\prod_{*\in\mathcal{E}}\operatorname{Prob}(N_{\mathrm{R}}^* \ge N) \tag*{(10)}

where E\mathcal{E} is the set of elements comprising the structure. The analytical form of the probability distribution of failure of the structure is the same as that of a 2-parameter Weibull distribution with Weibull scale parameter denoted as λs\lambda^s and given by (the proof is given in Appendix C):

NRs∼W(λs=1{∑∗∈E1λ∗m}1/m,m)(11)N_{\mathrm{R}}^s \sim\mathcal{W}\left(\lambda^s=\frac{1}{\left\{\sum_{*\in\mathcal{E}}\frac{1}{\lambda_*^m}\right\}^{1/m}},m\right) \tag*{(11)}

The CDF of fatigue lifetime of the structure is:

FNRs(N)=1−exp⁡(−{Nλs}m)(12)F_{N_{\mathrm{R}}^s}(N)=1-\exp\left(-\left\{\frac{N}{\lambda^s}\right\}^{m}\right) \tag*{(12)}

The computation of λs\lambda^s is dependent on Σa\Sigma_a as the computation of λ\lambda needs the function Δε∗(Σa)\Delta\varepsilon^*(\Sigma_a). It is also dependent on the parameters of the fatigue model. Henceforth, the cumulative distribution function (CDF) and the probability density function (PDF) of the specimen’s fatigue lifetime are denoted as FNRs(N;Σa,μ)F_{N_{\mathrm{R}}^s}(N;\Sigma_a,\mu) and fNRs(N;Σa,μ)f_{N_{\mathrm{R}}^s}(N;\Sigma_a,\mu), respectively.

Identification of the probabilistic lifetime model from experimental data by maximum likelihood estimation

Identification of the probabilistic lifetime model can be done on experimental fatigue lifetime data. In the following we will expose how this can be done in the case of (i) specimens with homogeneous stress distribution in the gauge section (ii) structures with heterogeneous stress distributions and (iii) structures with heterogeneous stress distributions that arise due to pores whose exact geometries and locations are unknown.

Specimens with homogeneous stress distributions

We recall from section 3.4 that fNRsf_{N_{\mathrm{R}}^s} is the PDF of the fatigue lifetime of a structure with a heterogeneous stress distribution. For specimens with a homogeneous stress distribution in their gauge section, i.e. without stress concentrations, the distribution of fatigue lifetime may be obtained without FEA.

The standard log-likelihood function is defined as [41, 42]:

ln⁡L(μ)=∑i∈Hln⁡fNRs(Ni;Σai,μ)(13)\ln\mathcal{L}(\mu)=\sum_{i\in\mathcal{H}}\ln f_{N_{\mathrm{R}}^s}(N^i;\Sigma_a^i,\mu) \tag*{(13)}

where H\mathcal{H} is the index set of all the specimens with uniform stress distribution tested for fatigue failure, NiN^i is the number of cycles to failure for an applied stress amplitude Σai\Sigma_a^i, and μ\mu is the set of parameters of the fatigue model. A Nelder-Mead algorithm is used for optimisation:

μ=arg⁡max⁡μ~(∑i∈Hln⁡fNRs(Ni;Σai,μ~))(14)\mu=\underset{\tilde{\mu}}{\arg\max}\left(\sum_{i\in\mathcal{H}}\ln f_{N_{\mathrm{R}}^s}(N^i;\Sigma_a^i,\tilde{\mu})\right) \tag*{(14)}

Furthermore, experimental high-cycle fatigue data-sets usually include some data points corresponding to specimens that did not break before reaching the maximum number of cycles allowed Nmax⁡N_{\max}. The latter, termed ”run-outs”, have a finite probability of failing for some number of cycles greater than Nmax⁡N_{\max}. This probability is expressed as:

P(N>Nmax⁡)=1−FNRs(Nmax⁡;Σa,μ)(15)P(N>N_{\max})=1-F_{N_{\mathrm{R}}^s}(N_{\max};\Sigma_a,\mu) \tag*{(15)}

Structures with heterogeneous stress distributions

We remind the reader of the PDF of the fatigue lifetime of structures with a heterogeneous stress distribution fNRf_{N_{\mathrm{R}}} from section 3.4. Structures with multiple distinct geometries can be taken into account here, provided that the exact geometries are known. This could, for example, be structures with different notch geometries, or porous specimens whose exact pore distribution is known for each of the specimens tested. In this case, fNRif_{N_{\mathrm{R}}}^{i} for each distinct geometry ii with fatigue lifetime NiN^{i} at load Σai\Sigma_{\mathrm{a}}^{i} is needed for identification of the model. For identification of the parameters of such a model, previous studies have used Bayesian calibration [17] or manual adjustment of parameters [25], especially on notched geometries. We use the maximum likelihood method:

μ=arg⁡max⁡μ~(∑i∈Iln⁡fNRi(Ni;μ~,Σai))(16)\mu= \underset{\tilde{\mu}}{\arg\max}\left(\sum_{i\in\mathcal{I}}\ln f_{N_{\mathrm{R}}}^{i}\left(N^{i};\tilde{\mu},\Sigma_{\mathrm{a}}^{i}\right)\right) \tag*{(16)}

where I\mathcal{I} is the set of all the structures with heterogeneous stress distributions tested for fatigue failure, NiN^{i} is the number of cycles to failure at an applied stress amplitude Σai\Sigma_{\mathrm{a}}^{i} and μ~\tilde{\mu} is the set of parameters of the fatigue model. A Nelder-Mead process is used for optimisation, outputting parameters μ\mu of the lifetime model that are the most probable given the experimental fatigue results, by maximizing the likelihood function.

To illustrate the computational complexity involved, we note that the computing the Weibull scale parameter of the structure, λs\lambda^{\mathrm{s}}, requires summing the Weibull scale parameters, λ\lambda, of all elements in the FE mesh (equation (11)). This result is then used to compute fNRsf_{N_{\mathrm{R}}}^{\mathrm{s}}. The scale parameters of the elements in turn require the computation of the inverse function g−1(Δε∗2)g^{-1}\left(\frac{\Delta\varepsilon^{*}}{2}\right) for each element (equation (7)). The criterion Δε∗\Delta\varepsilon^{*} is obtained for all the elements by one elasto-static finite element computation combined with the Neuber-type element-wise plastic correction algorithm, and does not need to be re-computed during the optimisation process. As the inverse function g−1(Δε∗2)g^{-1}\left(\frac{\Delta\varepsilon^{*}}{2}\right) depends on some of the parameters of the fatigue model (A,B,α and β)(A, B, \alpha\ \text{and}\ \beta), it needs to be re-computed for all the elements at every iteration of the optimisation process.

Structures with pores whose exact distribution is unknown

We now treat the case of structures with a fixed macroscopic geometry, that contains pores whose exact geometries and locations are unknown. In this case, no observations of the pore distribution in these structures were realized before fatigue testing, which makes the methodology presented in section 4.2, with deterministic geometries, inapplicable. The purpose is to identify a lifetime distribution on fatigue data of structures accounting for all possible pore geometries and localization. This is done by taking an expectation over all the possible configurations of pore distributions in the structures. For example, if J\mathcal{J} is the set of all the porous specimens of a given macroscopic geometry tested for fatigue failure, and K\mathcal{K} is the set of all possible synthetically generated configurations of porous specimens, the parameters of the lifetime distribution are obtained using the following optimisation statement:

μ=arg⁡max⁡μ~(∑i∈Jln⁡(Ek∈KfNRk(Ni;Σai,μ~)))(17)\mu= \underset{\tilde{\mu}}{\arg\max}\left(\sum_{i\in\mathcal{J}}\ln\left(\mathbb{E}_{k\in\mathcal{K}}f_{N_{\mathrm{R}}}^{k}\left(N^{i};\Sigma_{\mathrm{a}}^{i},\tilde{\mu}\right)\right)\right) \tag*{(17)}

Where NiN^{i} is the number of cycles to failure at an applied stress amplitude Σai\Sigma_{\mathrm{a}}^{i}. The expectation is taken over all realisations of the specimen with random meso-scale pore distributions. A Monte Carlo method is used to approximate this expectation over a finite number of synthetically generated porous specimens (denoted as the set K~\tilde{\mathcal{K}}):

μ=arg⁡max⁡μ~(∑i∈Jln⁡(1nK∑k∈K~fNRk(Ni;Σai,μ~)))(18)\mu= \underset{\tilde{\mu}}{\arg\max}\left(\sum_{i\in\mathcal{J}}\ln\left(\frac{1}{n_{\mathcal{K}}}\sum_{k\in\tilde{\mathcal{K}}}f_{N_{\mathrm{R}}}^{k}\left(N^{i};\Sigma_{\mathrm{a}}^{i},\tilde{\mu}\right)\right)\right) \tag*{(18)}

The computational cost of this optimisation is broken down here. Elasto-static finite element computations are required to be performed once for nKn_{\mathcal{K}} synthetically generated porous specimens. The approximation of the criterion Δε∗\Delta\varepsilon^{*} in all the elements of all the synthetic specimens, being a post-processing, takes virtually no time. As explained previously (section 4.2), the inverse function g−1(Δε∗2)g^{-1}\left(\frac{\Delta\varepsilon^{*}}{2}\right) needs to be computed for all elements of nkn_k synthetic specimens, at every iteration of the optimisation process, for computation of the approximated expectation of the fatigue lifetime. The algorithm explained in Algorithm 1 explains how the log-likelihood is computed for this case, including taking run-outs into account.

Algorithm 1  Log-Likelihood (LL) Computation
1: Ensure: ▷ $N$, $\lambda$ are separated into $N_{\mathrm{finite}}$, $\lambda_{\mathrm{finite}}$ (where $N < N_{\max}$) and $N_{\mathrm{inf}}$, $\lambda_{\mathrm{inf}}$ (where $N \ge N_{\max}$)
2: LL ← 0
3: $i$ ← 0
4: while $i < |N_{\mathrm{finite}}|$ do
5:   $s$ ← 0
6:   $k$ ← 0
7:   while $k < n_k$ do
8:     $s \leftarrow s + f^{N_s}_{R}(N_{\mathrm{finite}}[i], \lambda_{\mathrm{finite}}[k][i], m)$
9:     $k \leftarrow k + 1$
10:    $s^{\mathrm{avg}} \leftarrow \frac{s}{n_k}$
11:    $\mathrm{LL} \leftarrow \mathrm{LL} + \log(s^{\mathrm{avg}} + 10^{-10})$
12:    $i \leftarrow i + 1$
13:
14: $i$ ← 0
15: while $i < |N_{\mathrm{inf}}|$ do
16:   $m_{\mathrm{inf}}$ ← 0
17:   $k$ ← 0
18:   while $k < n_k$ do
19:     $m_{\mathrm{inf}} \leftarrow m_{\mathrm{inf}} + (1 - F^{N_s}_{R}(N_{\max}, \lambda_{\mathrm{inf}}[k][i], m))$
20:     $k \leftarrow k + 1$
21:   $m^{\mathrm{avg}}_{\mathrm{inf}} \leftarrow \frac{m_{\mathrm{inf}}}{n_k}$
22:   $\mathrm{LL} \leftarrow \mathrm{LL} + \log(m^{\mathrm{avg}}_{\mathrm{inf}} + 10^{-10})$
23:   $i \leftarrow i + 1$

Calibration and validation on experimental data

In this section, the behavior of the optimisation process presented in § 5 will be studied. The complexity of the fatigue model, i.e. number of required model parameters to fit lifetime data, will also be investigated. The data used is the previously presented experimental high-cycle fatigue data on non-porous and porous specimens (Figure 1). Finally, we will try to identify a fatigue model that is transferable between these two types of pore populations.

Geometry of specimens

(a)

Fatigue experiments

(b)

Figure 1. (a) Geometry of specimens (with values in mm) used for fatigue experiments (from the authors in [30]) (b) Fatigue experiments reported using these specimens (from the authors in [30]), with the applied stress amplitude Σa\Sigma_a as a function of the number of cycles to failure NRN_R. The run-outs (at NR=2×106N_R = 2 \times10^{6} cycles) are all counted and reported with a number and arrow to indicate possible failure for a larger number of cycles

The set K~\widetilde{K} is created with a total of 45 synthetically generated porous specimens2 using the method detailed in § 4.3.

Elasto-plastic computations (elasto-static FEA followed by Neuber-type elasto-plastic correction, as explained in § 4.3) were carried out on each of the synthetically generated porous specimens, for 9 nominal loading levels (Σa\Sigma_a ranging from 20 to 100 MPa). We use the material parameters identified by [28] for the considered alloy. The parameters of the elasto-plastic model are recalled in Table 2. The boundary conditions (shown in Figure 9) replicates the experimental conditions under which the high-cycle fatigue data were obtained. Each loading sequence consisted of 20 symmetric tension-compression cycles (R=−1R = -1), to allow for stabilization of the elasto-plastic response. The fatigue criterion Δε∗\Delta\varepsilon^* in the stabilized (20th) cycle is extracted. An example of the criterion computation in two synthetically generated specimens for one of the nominal loading levels (Σa=80\Sigma_a = 80 MPa), is shown in Figure 10. In this figure, the axial stress-strain histories for some integration points having high values of Δε∗\Delta\varepsilon^* are shown, to highlight the stabilization of the stress-strain cycles.

ParameterEE (MPa)σy\sigma_y (MPa)bbQQ (MPa)CC (MPa)DD
Value7550017019201274991334

Table 2. Parameters of the elasto-plastic model [28]

Boundary conditions and cyclic stress loading for a specimen containing tomography-informed pores

Figure 9. Boundary conditions (shown in red) for a specimen containing a sub-volume of tomography-informed pores, showing where cyclic displacement uau_a is applied, to obtain the different levels of loading desired. In the gauge section of the specimen (away from pores), the von Mises stress reaches the desired stress amplitude levels (here, as an example, Σa=80\Sigma_a = 80 MPa). The 20th cycle (shown in red) is chosen for the computation of Δε∗2\frac{\Delta\varepsilon^*}{2}.

Local criterion fields and axial stress–strain components for test specimens 1 and 10

Figure 10. (a) Test specimen 1. Σa=80\Sigma_a = 80 MPa. (b) Test specimen 10. Σa=80\Sigma_a = 80 MPa. Figure 10: Local criterion (Δε/2)(\Delta\varepsilon/2) field, in two different synthetically generated porous specimens, named test specimens 1 & 10. The criterion around the most critical defects and the axial stress-strain components at the highest points are shown. Refer to Appendix § 12 for an analysis of the accuracy of the fields computed using the plastic correction algorithm compared to that obtained with a full elasto-plastic finite element analysis.

Homogeneous stress distributions: non-porous specimens

The multi-scale methodology is not required for identifying the parameters of the fatigue model on non-porous specimens, as the stress field is homogeneous in the gauge section. The maximum likelihood approach developed in section 4.1 is used to identify the parameters μ\mu of the fatigue model. Optimisation is carried out using the experimental fatigue lifetime data of non-porous specimens, as detailed in section 2.

During the identification of the parameters of the fatigue model, we evaluate the impact of using fatigue models of varying complexity. Three cases are presented:

μ={[m,A,B,α,β,C](i)[m,A,α,C,B=0,β=0](ii)[m,A,α,B=0,β=0,C=0](iii)(19)\mu= \begin{cases} [m,A,B,\alpha,\beta,C] & \text{(i)}\\ [m,A,\alpha,C,\quad B=0,\beta=0] & \text{(ii)}\\ [m,A,\alpha,\quad B=0,\beta=0,C=0] & \text{(iii)} \end{cases} \tag*{(19)}

These three cases presented here correspond to (i) the fatigue model with parameters for both the LCF and HCF lines (AA, α\alpha, BB, β\beta), and the fatigue limit (CC) which we term as the ’two-line fatigue model’ (ii) the fatigue model with one line and the fatigue limit which we term as the ’one-line fatigue model’ (iii) the fatigue model with one line and no fatigue limit.

Optimisation cost and convergence of solution.

For all three models, the optimizer (Nelder-Mead) converges towards solutions with very similar likelihood values. The evolution of the parameters and the solution for the two-line fatigue model (equation (19)(i)) is shown in Figure 11. Even for an initialisation that is far away from the solution at convergence, the optimisation process is well behaved, as seen by the intermediate and final solutions in Figure 11b-Figure 11f).

Evolution and stabilization of the model parameters during optimisation for the two-line fatigue model
Image not extracted

(a) Evolution of parameters

Image not extracted

(b) Iteration number 0 (initial guess)

Image not extracted

(c) Iteration number 75

Image not extracted

(d) Iteration number 125

Image not extracted

(e) Iteration number 200

Image not extracted

(f) Iteration number 300

Figure 11. Evolution and stabilization of the model parameters during optimisation for the two-line fatigue model, μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C]. The solid line represents the median, the dashed lines represent the 15% and 85% quantiles, and the dotted lines represent 1% and 99% quantiles.

:::

The time required to evaluate all the functions during one iteration is dependent on the number of lifetime data points used for identification. For the considered data-set of 34 fatigue lifetime points, the cost of an iteration is around 0.15 seconds, therefore, the full optimisation procedure over 400 iterations takes around 60 seconds.

Comparison between lifetime models of varying complexity.

The results of optimisation are presented in Figure 12. For all the models, it is observed that the solutions for the first and second fatigue models (equation (19)(i) and (ii)) are similar, which suggests that the parameters BB and β\beta, i.e. the second line in the fatigue model, are not required. In our view, this conclusion would have been different had we had access to a richer data-set with more experiments across more loading levels. The third fatigue model (equation (19)(iii)) shows a significant decrease in the quality of the fit, indicating the requirement for the parameter CC for getting a meaningful fatigue limit beyond which the lifetime is infinite.

Two-line model

(a) Two-line model, μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C]

One-line model

(b) One-line model, μ=[m,A,α,C]\mu= [m, A, \alpha, C]

(c) One-line model without the fatigue limit, μ=[m,A,α]\mu= [m, A, \alpha]

Figure 12. Results of the probabilistic strain-life model, with three different fatigue models. The solid line represents the median, the dashed lines represent the 15% and 85% quantiles, and the dotted lines represent 1% and 99% quantiles.

Furthermore, the results show that the model is capable of taking into account run-outs. Indeed, all the quantiles of the model continue past the point NR=2×106N_R = 2 \times10^6 cycles, which indicates the capability of the model to assign a finite probability of failure for some number of cycles greater than NR=2×106N_R = 2 \times10^6 cycles.

Structures with pores whose exact distribution is unknown: porous specimens

The fatigue model is now identified on the experimental fatigue lifetime data of porous material presented in § 3. The multi-scale methodology developed in § 4 for structures with heterogeneous stress distributions due to pores whose exact geometries and locations are unknown is used. The maximum likelihood approach developed in § 5.3 was used as the identification procedure. From the previously defined set K~\widetilde{K}, a total of nk=10n_k = 10 synthetic specimens were randomly selected for each (Ni,Σ‾a)(N^i,\overline{\Sigma}_a) pair in order to approximate the expectation operator in the expression (18) of the likelihood function.3

During the identification of the parameters of the strain-life model, we evaluate the impact of using fatigue models of varying complexity. Two cases are presented (as CC has previously been proven necessary for obtaining a fatigue limit):

μ={[m,A,B,α,β,C](i)[m,A,α,C,B=0,β=0](ii)(20)\mu= \begin{cases} [m,A,B,\alpha,\beta,C] & \text{(i)}\\ [m,A,\alpha,C,\quad B=0,\beta=0] & \text{(ii)} \end{cases} \tag*{(20)}

As defined previously (§ 6.1), the cases correspond to (i) the ’two-line fatigue model’ and (ii) the ’one-line fatigue model’.

Optimisation cost and convergence of solution.

The parameters stabilise after a certain number of iterations of optimisation, as shown in the Figure 13(a) for the two-line fatigue model. In Figure 13 we show an optimisation process that converges well due to good initialisation. Indeed, if the initialisation is very far away from the expected solution, the optimisation process does not yield satisfactory results.

Evolution of parameters and model stabilization during optimisation

Figure 13. Evolution and stabilization of the model parameters during optimisation for the two-line fatigue model, μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C] during optimisation on the porous experimental data using the multi-scale method

The cost of evaluating all the functions during one iteration is dependent on the number of synthetically generated specimens nkn_k taken to compute the expectation of the fatigue lifetime distribution and the number of lifetime data points. It also depends on the number of elements in each synthetically generated specimen, which is around 1.5-2.5 million elements each. For the considered data-set of 32 fatigue lifetime points, the cost of one iteration is around 42 seconds if nk=1n_k=1 and 425 seconds for nk=10n_k=10. For the presented case (nk=10n_k=10), the cost of optimisation over 400 iterations is thus 47 hours.

Wöhler curve representing uncertainty due to pore distributions.

Fatigue lifetime distributions for multiple realizations of synthetically generated porous specimens of the same volume but varying pore distributions (examples previously shown in 10) were obtained, at various nominal loading levels. The synthetically generated porous specimens show variations in their fatigue lifetime distributions, as shown in Figure 14 for two different nominal applied stress amplitude levels, or in Figure 15 for the entire Wöhler curve for a couple of specimens.

Failure densities and uncertainty distributions for porous test specimens

Figure 14. For the two-line strain-life model (parameters μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C]) identified on porous data: Failure densities for 10 different synthetically generated porous test specimens at (a) Σa=80\Sigma_a = 80 MPa (b) Σa=40\Sigma_a = 40 MPa. Proportion of uncertainty coming from a specimen with a fixed pore distribution (black) compared to specimens with varying pore distributions (red histogram constructed by combining 1000 samples each from 10 different porous test specimens) at (c) Σa=80\Sigma_a = 80 MPa (d) Σa=40\Sigma_a = 40 MPa

Results of the multi-scale probabilistic strain-life model

Figure 15. Results of the multi-scale probabilistic strain-life model identified on all available porous data, with all parameters active (μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C]). Proportion of uncertainty coming from fixed pore distributions (two test specimens shown in green and grey hatch) to varying pore distributions (red master curve constructed by combining 1000 samples each from 10 different porous test specimens at every applied stress amplitude level). The solid line represents the median, the dashed lines represent the 15% and 85% quantiles, and the dotted lines represent 1% and 99% quantiles.

A fatigue lifetime distribution or Wöhler curve representing uncertainty due to pore distributions can be constructed by combining samples from a certain number of porous specimens. The failure distribution representing this uncertainty in pore distributions is constructed by combining 1000 samples each from 10 different randomly generated porous test specimens (shown by the red histogram in Figure 14(c,Figure 14d)). The quantiles are then computed on 10000 samples for each nominal stress level, which are joined to construct the quantiles of the porous Wöhler curve (shown by the red area in Figure 15). This failure distribution or Wöhler curve represents uncertainty due to defects at two scales - micro-heterogeneity and varying pore distributions. We note that the uncertainty in fatigue lifetime due to varying pore distributions in the specimen is relatively low as compared to the uncertainty due to the micro-heterogeneity. In other words, at the scale of this specimen, the impact of varying pore distributions on the lifetime is not high. This is because of the volume of the specimen, which is large as compared to the pore size, which increases the likelihood of finding critical pore configurations in all the specimens, and makes all the synthetic specimens have similar stress distributions.

Comparison between lifetime models of varying complexity.

The comparison between a two-line strain life model and one line strain life model is shown in Figure 16. The two models (with four and six parameters) yield qualitatively similar probability distributions for the specimen fatigue lifetime (with the 6 parameter model having only a very slightly lower likelihood value than the one obtained using the 4 parameter model). We will further investigate the more general two-line strain-life model with 6 parameters, to allow for the possibility of two distinct regimes.

Comparison of two-line and one-line strain-life models

Figure 16. Results of the probabilistic strain-life model using the multi-scale approach, identified on all available porous data, with two fatigue lifetime models. The solid line represents the median, the dashed lines represent the 15% and 85% quantiles, and the dotted lines represent 1% and 99% quantiles.

Lifetime prediction on a non-porous test specimen.

Ideally we should also be able to predict the fatigue lifetime of porous materials with different pore distributions than the ones that were experimentally tested. Using the two-line fatigue model identified on the porous data, we try to predict the fatigue behavior of a non-porous specimen. The results are shown in Figure 17. We see that the prediction on the non-porous specimens is incorrect. The predicted lifetime is lower than what experiments suggest. This could be due to three reasons:

Prediction of the multi-scale probabilistic strain-life model identified on all available porous data, with all parameters active, on a non-porous specimen

Figure 17. Prediction of the multi-scale probabilistic strain-life model identified on all available porous data, with all parameters active (μ=[m,A,B,α,β,C]\mu= [m, A, B, \alpha, \beta, C]), on a non-porous specimen. The solid line represents the median, the dashed lines represent the 15% and 85% quantiles, and the dotted lines represent 1% and 99% quantiles.

  1. Misrepresentation of pores: Several uncertainties and assumptions have been propagated while meshing the pores (smoothing the surfaces, removing smaller pores, etc.). This could explain the discrepancy; the real state of stress due to the pores may not be correctly modelled. It is also possible that the surface roughness plays a role, at a scale that is smaller than that of the tomographic scan of the pores, and is not taken into account in the mesh.

  1. Lack of data: The current data-set for porous materials lacks fatigue lifetime data for when the material around the pores is loaded at the same stress levels (100-140 MPa) as in the data-set for non-porous specimens. To address this, we require experiments in one of two ways. One possible solution is obtaining further experimental data on porous specimens at very low stress levels, such that the material around the pores reaches the required stress levels (100-140 MPa) that the non-porous specimens were subject to. Another solution is to obtain experimental data on non-porous specimens at the required (100-140 MPa) levels. Using this additional data during the optimisation process, we can identify a model that is transferable between material with these two levels of porosity.

  1. It could also be possible that the two base materials are different, or that the material in the vicinity of pores behaves differently under fatigue loading. Also, the hydro-static pressure may have an effect on fatigue behavior, but is not taken into account in the fatigue model criterion.

Towards a model transferable between different pore populations using lesser experimental data

In this section, we demonstrate that identifying a model that is transferable between different types of pore populations is facilitated by the multi-scale methodology proposed in this paper.

A simplified method to model the fatigue behavior of materials with different pore populations is to treat them as separate materials with different fatigue properties, and each material is thus fit separately with separate fatigue models. To do this, a large number of data-points would be required for identifying the parameters of the fatigue models for each of these materials.

The multi-scale approach, however, considers different pore populations to have the same base material. Fatigue lifetime data associated with different data-sets pertaining to different pore populations therefore share the same underlying statistics. Thus, the multi-scale approach is expected to require less data for identifying a model that is transferable between different types of pore populations.

Only the two-line fatigue model will be considered for the following numerical examples, in order to allow for the presence of two distinct regimes:

μ=[m,A,B,α,β,C](21)\mu= [m, A, B, \alpha, \beta, C] \tag*{(21)}

We now consider the fatigue lifetime data-set associated with non-porous and porous material presented in § 3. A reduction of the non-porous fatigue lifetime data-set I\mathcal{I} is done by randomly picking one experimental point for each applied stress amplitude level. The resulting reduced non-porous dataset Ired\mathcal{I}^{\mathrm{red}} is shown in Figure 18 (a).

Identified fatigue model on reduced non-porous and porous data

Figure 18. Identified fatigue model on the reduced data-set Ired\mathcal{I}^{\mathrm{red}} of 5 random non-porous data points and the data-set J\mathcal{J} of all the available 32 porous data points, using the multi-scale method

Identification of lifetime model on reduced data-set: multi-scale method.

Here, we are identifying the fatigue lifetime model on both structures with homogeneous stress distributions (non-porous specimens) and structures with pores whose exact distribution is unknown (porous specimens) simultaneously. The function to minimize is taken as a sum of the functions defined in § 5:

μ=arg max⁡μ~(∑i∈Iredln⁡fRNs(Ni;μ~,Σai)+∑i∈Jln⁡(1nk∑k∈K~fRks(Ni;μ~,Σai)))(22)\mu= \underset{\widetilde{\mu}}{\operatorname{arg\,max}}\left(\sum_{i\in\mathcal{I}^{\mathrm{red}}}\ln f_{\mathrm{R}}^{\mathrm{Ns}}\left(N^{i};\widetilde{\mu},\Sigma_{a}^{i}\right)+\sum_{i\in\mathcal{J}}\ln\left(\frac{1}{n_k}\sum_{k\in\widetilde{\mathcal{K}}}f_{\mathrm{R}}^{\mathrm{ks}}\left(N^{i};\widetilde{\mu},\Sigma_{a}^{i}\right)\right)\right) \tag*{(22)}

The reduced set of non-porous fatigue experiments Ired\mathcal{I}^{\mathrm{red}} is used in the optimisation process. The same set K~\widetilde{\mathcal{K}} used in the previous section is taken for the synthetically generated porous specimens, and nk=10n_k = 10.

The model parameters are jointly identified on the reduced non-porous data-set Ired\mathcal{I}^{\mathrm{red}} and the porous data-set J\mathcal{J}. The result of the optimisation process is shown in Figure 18. The fit is consistent on both the non-porous as well as porous cases, despite the reduction of non-porous data. This indicates that fewer fatigue experiments are required to identify the parameters when using the multi-scale approach. This is because the multi-scale approach considers porous and non-porous specimens as the same material, and information from the two sets of data are statistically correlated.

Identification of lifetime model on reduced data-set: homogenised method.

Identifying a probabilistic fatigue model on the reduced data-set Ired\mathcal{I}^{\mathrm{red}} is difficult due to an insufficient data-set, which makes several solutions possible. When considering the porous material as a new ’homogenised’ material, porous specimens may be considered to contain homogenised material with equivalent fatigue properties. A homogenised model is identified without using the multi-scale method, using the 0D identification procedure detailed in section 4.1 on the set J\mathcal{J} of porous experimental data. This gives the fit shown by the red curve in Figure 19. While the fit is good on the porous specimens given the data, the model remains non-transferable to other types of pore populations. This is seen when extrapolating the homogenised porous model to the stress levels at which non-porous specimens were tested. The homogenised porous model overlaps with the non-porous experimental data, which is against the generally observed trend of porous material failing sooner than non-porous material.

Identified fatigue model on homogenised porous material

Figure 19. Identified fatigue model on the data-set J\mathcal{J} of all the available 32 porous data points, considering the porous material as a homogenised material, using a 0D identification method

Numerical investigations of multi-scale method properties

In this section, certain properties of the multi-scale method will be investigated. The dependence of the mesh size on the fatigue lifetime curve will be shown. The pore-surface interaction effect under iso-volume conditions will be investigated, as well as the volumetric size effect. Finally, an attempt to replace the multi-scale method by using a naive homogenization technique will be presented.

Mesh convergence

The influence of the mesh size on the median of the lifetime predicted by the model is studied in this subsection. A synthetic specimen with one pore was meshed at different levels of refinement. The two-line fatigue model with parameters taken from section 5.3 is taken. Figure 20 shows four different refinement levels, with the size of the smallest element going from 5 microns to 29 microns. Figure 21 shows the effect of these mesh sizes on the median lifetime, across several load levels. As seen in this figure, the median fatigue lifetime curve exhibits a dependence on mesh size. The lifetime curve for the mesh with the smallest element size of 5 μ\mum is identical to that for the 10 μ\mum mesh. The optimal mesh size, beyond which further refinement does not change the solution, therefore lies between 10 and 19 μ\mum.

Mesh refinement around a pore

Figure 20. Mesh refinement around a pore, with the smallest element having size (a) 5 μ\mum (b) 10 μ\mum (c) 19 μ\mum (d) 29 μ\mum

Effect of mesh size on the median lifetime for a given set of two-line strain life model parameters

Figure 21. Effect of mesh size on the median lifetime for a given set of two-line strain life model parameters

Pore-surface interaction effect (iso-volume condition)

Thin specimens, transformed from a thicker specimen to have more surface area to volume ratio, while keeping the volume of the two specimens equal, have higher pore-surface interaction, and consequently have a lower lifetime - this effect has been reported before by other authors [43, 5]. This effect is an automatic output of the two scale method introduced in this paper. Figure 22(a) shows the geometries of two specimens: one specimen has radius rr and length LL, the other specimen has radius r/4r/4 and length 2L2L in order to keep the volume constant. Both of them are populated with pores using the same method presented in § 4.3. For the thick specimen, the projected image of the pores (see Figure 22b) shows a few pores interacting with the surface. The thin specimen, owing to lower cross-sectional area, has more pores interacting with the surface.

To avoid the effect of randomness in pore distributions, the expected lifetime needs to be computed for both specimens. Similar to § 6.2, a Wöhler curve representing uncertainty due to varying pore distributions is constructed by combining samples from a certain number of realizations of synthetically generated pore fields in the two specimens. For each nominal stress level, the failure distribution representing this uncertainty in pore distributions is constructed by combining 1000 samples each from 10 different randomly generated realizations. The quantiles are then computed on 10000 samples for each nominal stress level, which are joined to construct the quantiles of the porous Wöhler curve.

The predictions of the fatigue lifetime model, shown in Figure 22c, shows a decrease in the fatigue lifetime of a thinner specimen over all applied stress amplitude levels.

Examples of one realization of synthetically generated specimens

(a) Examples of one realization of synthetically generated specimens: one with radius rr and length LL, the other with radius r/4r/4 and length 42L4^{2}L, thus having the same volume but different levels of pore-surface interaction.

Projection of all the pores in the two specimens into the YZ plane

(b) Projection of all the pores in the two specimens into the YZ plane

Wöhler curves for the original and thin specimens

(c) Wöhler curves for the original and thin specimens

Figure 22. Effect of varying pore-surface interaction under iso-volume conditions on fatigue lifetime, as demonstrated on two specimens

Volumetric size effect (iso-stress condition)

As an automatic outcome of the model, specimens with different volumes but loaded under the same stress amplitude show a statistical size effect. Figure 23 shows the Wöhler curves of three synthetically generated porous specimens with volumes V/2V/2, VV and 2V2V. The same pore population in the smallest specimen was ’tiled’ multiple times to get bigger specimens, to isolate only the specimen volume size effect (and not add lifetime variability due to changing pore distributions as demonstrated in § 6.2). Across all load levels, specimens with successively higher volumes show a decreasing fatigue lifetime. This is the well known statistical size effect in fatigue, i.e. bigger specimens have a larger probability of finding a critical flaw [44, 45].

Synthetically generated porous specimens of volume $V/2$, $V$ and $2V$

(a) Synthetically generated porous specimens of volume V/2V/2, VV and 2V2V (owing to different lengths of gauge sections but same cross sectional area), undergoing the same loading (same applied stress amplitudes)

Wöhler curves for the three specimens

(b) Wöhler curves obtained by the model on the three specimens, with solid lines showing the median fatigue lifetimes and hatch filled areas demarcating the area contained between 1% and 99% quantiles of the fatigue lifetime distributions

Figure 23. Demonstration of the statistical size effect due to varying volumes

Naive homogenization to replace multi-scale method

The multi-scale method developed in this paper is expensive to compute for entire structures, as several configurations of pore distributions need to be evaluated. In this section, we will try to replace the multi-scale method, termed A, with a simplified, homogenised fatigue model, termed B. For the identification of the homogenised model, we will generate synthetic data using the multi-scale method, for several realizations of pore distributions in a given geometry. The question is whether the homogenised model will accurately approximate the fatigue lifetime solution when applied to different geometries. The two-line fatigue model will be used for this study, with a fixed set of parameters (similar to those in section 5.3).

Generation of synthetic fatigue lifetime data using the multi-scale method.

We will now generate synthetic data using the multi-scale method A. A total of 10 cylindrical synthetically generated porous specimens were considered for data generation (examples of the geometries have previously been shown in section 10). For each synthetically generated porous specimen, 1000 samples each across 9 nominal loading levels were generated using this model, as shown by the green markers in Figure 24.

Identification of a homogenised porous fatigue model using synthetic data and a pore-free cylindrical specimen

Figure 24. (a) 3D mesh of a pore-free cylindrical specimen (b) Generated synthetic lifetime data from cylindrical porous specimens, identified homogenised model and predictions of the homogenised model on the 3D mesh of the pore-free cylindrical specimen. Identification of the parameters of a 0D homogenised porous fatigue model B on generated synthetic lifetime data from the model A, and validation on a 3D FE pore-free cylindrical specimen of the same shape and volume as the original cylindrical porous specimens

Identification of a homogenised 0D fatigue model.

Using the 0D identification procedure as described in section 4.1, the parameters of a fatigue lifetime model that maximized the likelihood of the synthetic generated data were obtained. This model B is a homogenised porous fatigue lifetime model. To check the quality of this homogenised model, a 3D mesh of a homogeneous pore-free cylindrical specimen of the same size and geometry as the porous cylindrical specimens was created (shown in Figure 24(a)), and the model B was used to obtain predictions on it using the weakest link method developed in section 3.4. The results, shown in Figure 24(b), indicate that the homogenised model B works well to replace the multi-scale method for the given geometry.

Notched geometry.

A geometry with a macroscopic notch was created, as shown in Figure 25. The sub-volume of pores used to create a porous version of this geometry was taken from the same tomography used to create the cylindrical porous specimens. Next, several configurations of the notched specimen were created:

Creation of a notched specimen

Figure 25. Creation of a notched specimen (a) boundary conditions (b) sub-volume of pores used for creation of a porous notched specimen (c) resulting mesh of the porous notched specimen

  1. Porous notched specimen with the normal expected pore density, with pores interacting with the notch

  1. Porous notched specimen with a surface-breaking pore interacting with the notch artificially removed

  1. Notched specimen without pores

The criterion of the lifetime model was obtained on all these geometries via the plastic corrector methodology. The elements in the notched region were extracted for lifetime prediction, with the assumption that fatigue lifetime failure is influenced only by this volume. The extracted volumes of the different versions are shown in Figure 26. In the specimen with the normal expected pore density, there are two pores interacting with the notch that give rise to very high levels of plasticity. Concerning the specimen with removed surface-breaking pore interacting with the notch, there is a lesser amount of plasticity due to reduced pore-notch interaction. The specimen without pores has the least amount of plasticity, developing only due to the notch.

Extracted volume of the notched specimen with normal density of pores

(a)

Extracted volume of the notched specimen with reduced pores interacting with notch

(b)

Extracted volume of the notched specimen with no pores

(c)

Figure 26. Extracted volume (for lifetime prediction) of different versions of the notched specimen (a) normal density of pores (b) reduced pores interacting with notch (c) no pores

Transferability of homogenised model to notched geometry.

We are now in a position to check the transferability of the homogenised model B to the notched geometry. Lifetime predictions (shown in 27) were obtained using the following configurations:

  1. Model A on the notched volume with normal density of pores (red)

  1. Model A on the notched volume with one less surface-breaking pore in the notch region (green)

  1. homogenised model B on the notched volume with no pores (black)

The first case i.e. obtained using the multi-scale method A on the volume with the normal expected pore density, can be considered as the reference solution. The predictions using the same method A on the volume with a surface-breaking pore interacting with the notch artificially removed shows a increase in the fatigue lifetime, due to lesser stresses in the notch region. However, both of these predictions show lesser lifetimes of the porous notch volume as compared to the homogenised porous model B. This indicates that the homogenised model B identified on cylindrical specimens is not transferable to other geometries.

Lifetime predictions using model A on the notched volume with normal density of pores, model A on the notched volume with one less pore interacting with the notch, and homogenised model B on a notched volume with no pores

Figure 27. Lifetime predictions using model A on the notched volume with normal density of pores (red) model A on the notched volume with one less pore interacting with the notch (green) homogenised model B on a notched volume with no pores (black)

Overview of findings and elements of discussion

Need for meshing pores

The multi-scale method can be applied to arbitrary geometries for fatigue lifetime predictions. However, there is a need to explicitly mesh the pores in these geometries. This is because a homogenised model (simulating porous material behavior on the fatigue lifetime) that remains transferable across varying geometries of structures is difficult to obtain. The reasons for this difficulty are that (a) the core and surface materials exhibit different fatigue behaviour, as shown in § 7.2, and (b) the homogenised model identified for one geometry cannot capture the pore-notch interaction in the notched geometries, as discussed in § 7.4. Thus, there is a need to mesh the pores when using the multi-scale method for fatigue lifetime predictions on arbitrary geometries containing porous material.

Choice of fatigue model complexity

When optimisation is performed on only the non-porous data points (results shown in Figure 12), we observe that the strain-life model with two lines (parameters AA, α\alpha, BB, β\beta and CC) and the model with one line (parameters AA, α\alpha and CC) have the same quality of fit, i.e. there is no need for the second line when fitting data in only one regime (HCF regime). However, if more data is present, especially in the LCF regime, it is likely that both lines of the strain life model would be required to obtain a consistent fit. Figure 12c shows a significant decrease in the quality of the fit when the parameter CC is omitted, which highlights its importance for getting a sensible fatigue limit. The probabilistic fatigue curves show a decrease in the uncertainty with increasing applied stress amplitude, which is a widely observed phenomenon in fatigue, and enforced with g−1(Δε2)g^{-1}\left(\frac{\Delta\varepsilon}{2}\right) in the numerator of the Weibull scale parameter, i.e. the scale reduces for higher loads and lower NRN_R for a fixed shape parameter.

When optimisation is performed on only the porous data points (results shown in Figure 16) both the two-line model and one line model seem to give good fits. However, as the porous data points contain information about both LCF and HCF behavior of the alloy, it is better to work with the two-line strain-life model. Material points around pores that are highly loaded should behave in the LCF regime and points in the non-loaded zones should behave in the HCF regime.

Enabling transferability of fatigue models between different types of pore populations

Any fatigue lifetime model that needs to be accurate across different loading regimes (LCF and HCF) first needs to be properly identified with experimental data across the entire load spectra. The multi-scale method’s capability of treating different alloys of porous material as made of the same base material is thus advantageous. The base material is considered to have a unique behavior, thus sparse data on different types of pore populations across various loading spectra can be exploited with ease. This is because the multi-scale method, by design, only requires a small representative tomography of the pore population for each grade of porosity. Additionally, the required FEA computations on statistically representative pore fields are accelerated by the plastic corrector [26].

The numerical results on the aluminium data-set demonstrate this: the model is able to treat the non-porous grade and the porous grade to be made of the same base material, and identification of a transferable model between these two grades is possible with lesser data than the simplified approach of treating the porous material as a different material than the non-porous one.

Diversity of exploitable lifetime data for a model transferable between pore populations

Two types of lifetime data are usable to identify a fatigue lifetime model with the proposed multi-scale approach. For example, to identify the model in the HCF regime, one may either load porous specimens at very low levels of stress such that the base material around the pores is loaded in the HCF regime, or by loading specimens made of the base material itself in the HCF regime. This can be particularly helpful if lifetime data on the base material (without porosity) is expensive or time consuming to obtain, or if a limited amount of lifetime data is present for each category of porosity.

For the example presented in this paper in § 6.2, the two-line fatigue model (identified on the limited set of porous fatigue experiments, across a small range of loading levels) lacks information on distinguishing between the fatigue regimes. However, when the model is given some non-porous fatigue lifetime points at lower stress levels (in § 6.3), it learns to better differentiate between the two regimes of fatigue behaviour of the base material. The base material behavior in the HCF regime is identified using these non-porous points. In porous specimens, the base material near pores, being loaded at a higher level, informs the LCF fatigue behaviour. In other words, the model learns about different regimes of fatigue behavior of the base material from the lifetime data of the two grades of porosity.

Conclusions

In this paper, we propose a probabilistic fatigue lifetime model combined with a multi-scale method to model the lifetime of structures with pores whose exact distribution is unknown. The effect of the pores on the fatigue lifetime is modelled using statistical methods based on a small representative tomography of the porous material. The multi-scale aspect is facilitated by a FEA accelerator for lifetime criterion computations when non-linearity is present in the material model.

The identification procedure involves a maximum likelihood estimate, utilizing pre-computed statistically representative heterogeneous 3D elasto-plastic fields obtained via FEA during optimisation. Run-outs are used as valid experimental data by assigning them a finite probability of future failure.

The multi-scale approach developed in this paper allows materials with varying grades of porosity to be treated as if made of the same base material, thus enabling the use of lifetime data from materials with different pore populations for the identification of a singular fatigue lifetime model. This approach reduces the overall lifetime data required for identifying the fatigue lifetime model as compared to approaches that treat each porous grade as a different material.

Additionally, the model naturally accounts for the fact that, in porous materials, fatigue resistance at the subsurface level is lower than that at the core. The model also considers the statistical size effect, where larger volumes fail earlier under iso-stress conditions.

The model allows for the approximation of Wöhler curves across arbitrary geometries, enabling lifetime estimation even without the need for full tomography of the structure. This is achieved using a small representative volume containing information about the pores, making the model both efficient and effective. The prediction time is comparable to the cost of an elastic-static FEA computation, as the plasticity in the stabilized cycle is computed through the use of a plastic corrector [26]. However, the model does require meshes where pores are explicitly represented, as a simple homogenization of the porous material does not reproduce the multi-scale method’s prediction for all geometries. Additionally, the optimisation process, particularly when solving fatigue lifetime computation via residual minimization, is resource-intensive.

Acknowledgements

The authors would like to thank the French National Research Agency (ANR-20-THIA-0022) for the partial funding of this project. The direct financial support of Mines Paris - PSL is also acknowledged. The authors are particularly grateful to Pierre Osmond (CETIM) for tomographies of the porous specimens.

Conflict of interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Quality of strain-life fatigue lifetime criterion approximation

A plastic corrector is used for computation of the full-field Δε\Delta\varepsilon in the synthetically generated porous specimens [26]. Figs. 28 and 29 show the quality of approximations as compared to a reference computation performed using the Z-Set suite [46]. The plastic corrector approximates an elastoplastic solution pointwise using a plastic correction heuristic. The heuristic is a modified Neuber rule coupled with a local proportional evolution rule, which, along with the constitutive relations, form a closed set of equations which are solved for the approximated elasto-plastic response.

Comparison of the plastic corrector and reference computation in a porous specimen

Figure 28. A comparison between Δε\Delta\varepsilon computed via the plastic corrector [26] and a reference computation via Z-Set [46] in a specimen containing a subvolume of pores. The loading corresponds to Σa=80\Sigma_a = 80 MPa (around 47% of R0), which is the highest level of loading for which experimental high-cycle fatigue data is available.

Scatter plot comparing strain ranges

(a)

Scatter plot comparing accumulated plasticity

(b)

Figure 29. A scatter plot comparing Δε\Delta\varepsilon and Δp\Delta p computed via the plastic corrector [26] and a reference computation via Z-Set [46] in all the integration points of a specimen containing a subvolume of pores. The loading corresponds to Σa=80\Sigma_a = 80 MPa (around 47% of R0), which is the highest level of loading for which experimental high-cycle fatigue data is available.

Analytical form of the failure density of a specimen undergoing heterogeneous stresses

The life of the porous specimen is dependent on the elements that constitute its volumes:

Prob⁡(NRs≥N)=∏∗∈EProb⁡(NR∗≥N)(23)\operatorname{Prob}(N_{\mathrm{R}}^{s} \ge N) = \prod_{*\in\mathcal{E}} \operatorname{Prob}(N_{\mathrm{R}}^{*} \ge N) \tag*{(23)}

Therefore, the cumulative probability distribution (CDF) of the specimen failing is given by:

FNRs(N)=1−∏∗∈E(1−FNR∗(N))(24)F_{N_{\mathrm{R}}^{s}}(N) = 1 - \prod_{*\in\mathcal{E}} \left(1 - F_{N_{\mathrm{R}}^{*}}(N)\right) \tag*{(24)}

The CDF of failure of an element was defined as:

FNR∗(N)=1−exp⁡(−{Nλ}m)(25)F_{N_{\mathrm{R}}^{*}}(N) = 1 - \exp\left(-\left\{\frac{N}{\lambda}\right\}^{m}\right) \tag*{(25)}

Substituting this expression in the expression for the CDF of the specimen, we get:

FNRs(N)=1−∏∗∈E(exp⁡(−{Nλ}m))(26)F_{N_{\mathrm{R}}^{s}}(N) = 1 - \prod_{*\in\mathcal{E}} \left(\exp\left(-\left\{\frac{N}{\lambda}\right\}^{m}\right)\right) \tag*{(26)}
FNRs(N)=1−exp⁡(∑∗∈E(−{Nλ}m))(27)F_{N_{\mathrm{R}}^{s}}(N) = 1 - \exp\left(\sum_{*\in\mathcal{E}} \left(-\left\{\frac{N}{\lambda}\right\}^{m}\right)\right) \tag*{(27)}
FNRs(N)=1−exp⁡(−Nm∑∗∈E{1λ}m)(28)F_{N_{\mathrm{R}}^{s}}(N) = 1 - \exp\left(-N^{m}\sum_{*\in\mathcal{E}}\left\{\frac{1}{\lambda}\right\}^{m}\right) \tag*{(28)}

This is equivalent to a Weibull distribution with Weibull scale parameter denoted as λs\lambda^{s}:

FNRs(N)=1−exp⁡(−{Nλs}m)(29)F_{N_{\mathrm{R}}^{s}}(N) = 1 - \exp\left(-\left\{\frac{N}{\lambda^{s}}\right\}^{m}\right) \tag*{(29)}
λs=1{∑∗∈E1λm}1/m(30)\lambda^{s} = \frac{1}{\left\{\sum_{*\in\mathcal{E}}\frac{1}{\lambda^{m}}\right\}^{1/m}} \tag*{(30)}
NRs∼W(λs,m)(31)N_{\mathrm{R}}^{s} \sim W\left(\lambda^{s},m\right) \tag*{(31)}

The probability density function (PDF) and the cumulative distribution function (CDF) of the specimen’s fatigue lifetime are denoted by fNRs(N;Σa,μ)f_{N_{\mathrm{R}}^{s}}(N;\Sigma_{a},\mu) and FNRs(N;Σa,μ)F_{N_{\mathrm{R}}^{s}}(N;\Sigma_{a},\mu) to show the dependence of these functions on the set of parameters μ\mu and the applied stress amplitude Σa\Sigma_{a}.

References

  1. [1]A. Ezanno, C. Doudard, S. Calloch, T. Millot, J.-L. Heuzé, Fast characterization of high-cycle fatigue properties of a cast copper–aluminum alloy by self-heating measurements under cyclic loadings, Procedia Engineering 2 (2010) 967–976. doi:https://doi.org/10.1016/j.proeng.2010.03.105, fatigue 2010.
  2. [2]V.-D. Le, N. Saintier, F. Morel, D. Bellett, P. Osmond, Investigation of the effect of porosity on the high cycle fatigue behaviour of cast al-si alloy by x-ray micro-tomography, International Journal of Fatigue 106 (2018) 24–37. URL: https://www.sciencedirect.com/science/article/pii/S0142112317303778. doi:https://doi.org/10.1016/j.ijfatigue.2017.09.012.
  3. [3]A. K. Mahapatra Raghavendra, V. Maurel, L. Marcin, H. Proudhon, Fatigue life prediction at mesoscopic scale of samples containing casting defects: A novel energy based non-local model, International Journal of Fatigue 188 (2024) 108485. URL: https://www.sciencedirect.com/science/article/pii/S0142112324003438. doi:https://doi.org/10.1016/j.ijfatigue.2024.108485.
  4. [4]D. El Khoukhi, F. Morel, N. Saintier, D. Bellett, P. Osmond, V.-D. Le, J. Adrien, Experimental investigation of the size effect in high cycle fatigue: Role of the defect population in cast aluminium alloys, International Journal of Fatigue 129 (2019) 105222. doi:https://doi.org/10.1016/j.ijfatigue.2019.105222.
  5. [5]S. Romano, S. Miccoli, S. Beretta, A new fe post-processor for probabilistic fatigue assessment in the presence of defects and its application to am parts, International Journal of Fatigue 125 (2019) 324–341. URL: https://www.sciencedirect.com/science/article/pii/S014211231930132X. doi:https://doi.org/10.1016/j.ijfatigue.2019.04.008.
  6. [6]L. Lacourt, Étude numérique de la nocivité des défauts dans les soudures, Thèse de doctorat, Université Paris Sciences et Lettres, Matériaux, 2019. NNT : 2019PSLEM050, tel-02512870.DOI
  7. [7]M. Shirani, G. Härkegård, Damage tolerant design of cast components based on defects detected by 3d x-ray computed tomography, International Journal of Fatigue 41 (2012) 188–198. URL: https://www.sciencedirect.com/science/article/pii/S0142112311002660. doi:https://doi.org/10.1016/j.ijfatigue.2011.09.011, fatigue Design & Material Defects.
  8. [8]L. Bercelli, S. Moyne, M. Dhondt, C. Doudard, S. Calloch, J. Beaudet, A probabilistic approach for high cycle fatigue of wire and arc additive manufactured parts taking into account process-induced pores, Additive Manufacturing 42 (2021) 101989. URL: https://www.sciencedirect.com/science/article/pii/S2214860421001548. doi:https://doi.org/10.1016/j.addma.2021.101989.
  9. [9]R. Talemi, A numerical study on effects of randomly distributed subsurface hydrogen pores on fretting fatigue behaviour of aluminium alsi10mg, Tribology International 142 (2020) 105997. URL: https://www.sciencedirect.com/science/article/pii/S0301679X19305146. doi:https://doi.org/10.1016/j.triboint.2019.105997.
  10. [10]Y. Hou, Z. Hu, T. Wauters, R. Talemi, Combined effect of random porosity and surface defect on fatigue lifetime of additively manufactured micro-sized ti6al4v components: An investigation based on numerical analysis and machine learning approach, Theoretical and Applied Fracture Mechanics 131 (2024) 104451. URL: https://www.sciencedirect.com/science/article/pii/S0167844224002003. doi:https://doi.org/10.1016/j.tafmec.2024.104451.
  11. [11]S. S. Manson, Behavior of materials under conditions of thermal stress, Technical Note TN 2933, National Advisory Committee for Aeronautics (NACA), 1953.
  12. [12]E. Astm, 739-91. standard practice for statistical analysis of linear or linearized stress-life (sn) and strain-life (ε-n) fatigue data, ASTM International (2015).
  13. [13]M. Brown, K. Miller, A theory for fatigue under multiaxial stress-strain conditions, Proceedings of the Institute of Mechanical Engineers 187 (1973) 745–756.
  14. [14]A. Fatemi, D. Socie, A critical plane approach to multiaxial fatigue damage including out-of-phase loading, Fatigue and Fracture of Engineering Materials and Structures 11 (1988) 149–166.
  15. [15]A. Karolczuk, E. Macha, A review of critical plane orientations in multiaxial fatigue failure criteria of metallic materials, International Journal of Fracture 134 (2005) 267–304. doi:10.1007/s10704–005–1088–2.
  16. [16]F. W. Zok, On weakest link theory and weibull statistics, Journal of the American Ceramic Society 100 (2017) 1265–1268. URL: https://ceramics.onlinelibrary.wiley.com/doi/abs/10.1111/jace.14665. doi:https://doi.org/10.1111/jace.14665. arXiv:https://ceramics.onlinelibrary.wiley.com/doi/pdf/10.1111/jace.14665.
  17. [17]X. Liu, R. Wang, D. Hu, J. Mao, A calibrated weakest-link model for probabilistic assessment of lcf life considering notch size effects, International Journal of Fatigue 137 (2020) 105631. URL: https://www.sciencedirect.com/science/article/pii/S0142112320301626. doi:https://doi.org/10.1016/j.ijfatigue.2020.105631.
  18. [18]X.-K. Li, S.-P. Zhu, D. Liao, J. A. Correia, F. Berto, Q. Wang, Probabilistic fatigue modelling of metallic materials under notch and size effect using the weakest link theory, International Journal of Fatigue 159 (2022) 106788. URL: https://www.sciencedirect.com/science/article/pii/S0142112322000676. doi:https://doi.org/10.1016/j.ijfatigue.2022.106788.
  19. [19]D. Talor, Geometrical effects in fatigue: a unifying theoretical model, International Journal of Fatigue 21 (1999) 413–420. URL: https://www.sciencedirect.com/science/article/pii/S0142112399000079. doi:https://doi.org/10.1016/S0142–1123(99)00007–9.
  20. [20]R. Kuguel, A relation between theoretical stress concentration factor and fatigue notch factor deduced from the concept of highly stressed volume, in: ASTM proc, volume 61, 1961, pp. 732–748.
  21. [21]C. M. Sonsino, H. Kaufmann, V. Grubisic, Transferability of material data for the example of a randomly loaded forged truck stub axle, SAE Technical Paper Series No. 970708 (1997) 1–22.
  22. [22]J.-C. He, S.-P. Zhu, A. T. Taddesse, X. Niu, Evaluation of critical distance, highly stressed volume, and weakest-link methods in notch fatigue analysis, International Journal of Fatigue 162 (2022) 106950. URL: https://www.sciencedirect.com/science/article/pii/S0142112322002195. doi:https://doi.org/10.1016/j.ijfatigue.2022.106950.
  23. [23]M. Muñiz-Calvente, A. Fernández Canteli, V. Shlyannikov, E. Castillo, Probabilistic weibull methodology for fracture prediction of brittle and ductile materials, in: Damage Mechanics: Theory, Computation and Practice, volume 784 of Applied Mechanics and Materials, Trans Tech Publications Ltd, 2015, pp. 443–451. doi:10.4028/www.scientific.net/AMM.784.443.
  24. [24]D. B. Lanning, T. Nicholas, A. Palazotto, Hcf notch predictions based on weakest-link failure models, International Journal of Fatigue 25 (2003) 835–841. URL: https://www.sciencedirect.com/science/article/pii/S0142112303001567. doi:https://doi.org/10.1016/S0142–1123(03)00156–7, international Conference on Fatigue Damage of Structural Materials IV.
  25. [25]A. Karolczuk, T. Palin-Luc, Modelling of stress gradient effect on fatigue life using weibull based distribution function, Journal of Theoretical and Applied Fracture Mechanics 51 (2013) 297–311.
  26. [26]A. Palchoudhary, S. Peter, V. Maurel, C. Ovalle, P. Kerfriden, A plastic correction algorithm for full-field elasto-plastic finite element simulations : critical assessment of predictive capabilities and improvement by machine learning, 2024. arXiv:2402.06313.
  27. [27]V.-D. Le, Etude de l’influence des hétérogénéités microstructurales sur la tenue en fatigue à grand nombre de cycles des alliages d’aluminium de fonderie, Ph.D. thesis, ENSAM, 2016. URL: http://www.theses.fr/2016ENAM0012, thèse de doctorat dirigée par Morel, Franck Saintier, Nicolas et Bellett, Daniel Mécanique-matériaux Paris.
  28. [28]V.-D. Le, F. Morel, D. Bellett, N. Saintier, P. Osmond, Multiaxial high cycle fatigue damage mechanisms associated with the different microstructural heterogeneities of cast aluminum alloys, Materials Science and Engineering: A 649 (2016) 426–440. doi:https://doi.org/10.1016/j.msea.2015.10.026.
  29. [29]D. El Khoukhi, F. Morel, N. Saintier, D. Bellett, P. Osmond, V.-D. Le, J. Adrien, Scatter and size effect in high cycle fatigue of cast aluminium-silicon alloys: A comprehensive experimental investigation, Procedia Structural Integrity 38 (2022) 611–620. URL: https://www.sciencedirect.com/science/article/pii/S2452321622002761. doi:https:// doi.org/10.1016/j.prostr.2022.03.063, fatigue Design 2021, International Conference Proceedings, 9th Edition.
  30. [30]V.-D. LE, F. Morel, D. Bellett, E. Pessard, N. Saintier, P. Osmond, Microstructural-based analysis and modelling of the fatigue behaviour of cast al-si alloys, Procedia Engineering 133 (2015) 562–575. doi:https://doi.org/10.1016/j.proeng.2015.12.630, fatigue Design 2015, International Conference Proceedings, 6th Edition.
  31. [31]C. Doudard, S. Calloch, F. Hild, P. Cugy, A. Galtier, Identification of the scatter in high cycle fatigue from temperature measurements, Comptes Rendus Mécanique 332 (2004) 795–801. doi:https://doi.org/10.1016/j.crme.2004.06.002.
  32. [32]K. Ni, S. Mahadevan, Strain-based probabilistic fatigue life prediction of spot-welded joints, International Journal of Fatigue 26 (2004) 763–772. URL: https://www.sciencedirect.com/science/article/pii/S0142112303002834. doi:https://doi.org/10.1016/j.ijfatigue.2003.10.021.
  33. [33]E. Pessard, F. Morel, A. Morel, D. Bellett, Modelling the role of non-metallic inclusions on the anisotropic fatigue behaviour of forged steel, International Journal of Fatigue 33 (2011) 568–577. URL: https://www.sciencedirect.com/science/article/pii/S0142112310002471. doi:https://doi.org/10.1016/j.ijfatigue.2010.10.012.
  34. [34]I. Koutiri, D. Bellett, F. Morel, E. Pessard, A probabilistic model for the high cycle fatigue behaviour of cast aluminium alloys subject to complex loads, International Journal of Fatigue 47 (2013) 137–147. URL: https://www.sciencedirect.com/science/article/pii/S0142112312002472. doi:https://doi.org/10.1016/j.ijfatigue.2012.08.004.
  35. [35]H. Li, D. Wen, Z. Lu, Y. Wang, F. Deng, Identifying the probability distribution of fatigue life using the maximum entropy principle, Entropy 18 (2016). URL: https://www.mdpi.com/1099-4300/18/4/111. doi:10.3390/e18040111.DOI
  36. [36]R. Desmocrat, Fast estimation of localized plasticity and damage by energetic methods, International Journal of Solids and Structures 39 (2002) 3289–3310. URL: https://www.sciencedirect.com/science/article/pii/S0020768302000021. doi:https://doi.org/10.1016/S0020- 0763(02)00002–1.
  37. [37]H. Kitagawa, Applicability of fracture mechanics to very small cracks or the cracks in the early stage, in: Proceedings of 2nd ICM, Cleveland, 1976, pp. 627–631.
  38. [38]C. Geuzaine, J.-F. Remacle, Gmsh, 2020. URL: http://http://gmsh.info/.
  39. [39]J. Chaboche, Constitutive equations for cyclic plasticity and cyclic viscoplasticity, International Journal of Plasticity 5 (1989) 247–302. doi:https://doi.org/10.1016/0749-6419(89)90015–6.
  40. [40]M. S. Alnaes, J. Blechtа, J. Hake, A. Johansson, B. Kehlet, A. Logg, C. Richardson, J. Ring, M. E. Rognes and G. N. Wells, The fenics project version 1.5, archive of numerical software 3, 2015. URL: doi.org/10.11588/ans.2015.100.20553.
  41. [41]R. D. Pollak, A. N. Palazotto, A comparison of maximum likelihood models for fatigue strength characterization in materials exhibiting a fatigue limit, Probabilistic Engineering Mechanics 24 (2009) 236–241. URL: https://www.sciencedirect.com/science/article/pii/S0266892008000057X. doi:https://doi.org/10.1016/j.probengmech.2008.06.006.
  42. [42]S. Lee, O. Norovrinchen, C. Sumiyadorj, Fatigue strength estimation based on the maximum likelihood method, in: Proceedings of the second International Conference on Resources and Technology (RESAT 2023), Atlantis Press, 2023, pp. 98–106. URL: https://doi.org/10.2991/978-94-6463-318-4_8. doi:10.2991/978-94-6463-318-4_8.
  43. [43]J. Pegues, M. Roach, R. Williamson, N. Shamsaei, Effect of specimen surface area size on fatigue strength of additively manufactured ti-6al-4v parts, 2017.
  44. [44]M. Makkonen, Statistical size effect in the fatigue limit of steel, International Journal of Fatigue 23 (2001) 395–402. URL: https://www.sciencedirect.com/science/article/pii/S0142112301000032. doi:https://doi.org/10.1016/S0142-1123(01)00003–2.
  45. [45]D. El Khoukhi, F. Morel, N. Saintier, D. Bellett, P. Osmond, V.-D. Le, Probabilistic modeling of the size effect and scatter in high cycle fatigue using a monte-carlo approach: Role of the defect population in cast aluminum alloys, International Journal of Fatigue 147 (2021) 106177. URL: https://www.sciencedirect.com/science/article/pii/S0142112321000372. doi:https://doi.org/10.1016/j.ijfatigue.2021.106177.
  46. [46]J. Besson, R. Leriche, R. Foerch, G. Cailletaud, Object-oriented programming applied to the finite element method part ii. application to material behaviors, Revue Européenne des Éléments 7 (2012) 567–588. doi:10.1080/12505659.1998.10511322.

Paper details

vlnc:W_cnpvccwm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 8

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Computer Science

Not recorded for this paper

View statement
Looking for related papers…
Contents