Plasma engineered Hydroxyl Defects in NiO a DFTSupported-Spectroscopic Analysis of Oxygen Hole States and Implications for Water Oxidation

Abstract

Controlling lattice oxygen reactivity in earth abundant OER catalysts requires precise tuning of defect chemistry in the oxide lattice. Here, we combine DFT+U calculations with plasma assisted synthesis to show how O2 and H2O in the discharge govern vacancy formation, electronic structure, and catalytic predisposition in NiO thin films. Oxygen rich plasmas generate isolated and clustered Ni vacancies that stabilize oxygen ligand hole states and produce shallow O 2p Ni 3d hybrid levels, enhancing Ni O covalency. In contrast, introducing H2O during growth drives local hydroxylation that compensates vacancy induced Ni3+ centers, restoring Ni2+ like coordination, suppressing deep divacancy derived in gap states, and introducing shallow Ni O H derived valence-band tails. EXAFS confirms that hydroxylation perturbs only the local environment while preserving the medium-range NiO lattice, and Ni L-edge spectroscopy shows a persistent but redistributed ligand-hole population. These complementary vacancy and hydroxylation driven pathways provide a plasma controlled route to pre define electronic defect landscapes in NiO and to tune its activation toward OER relevant NiOOH formation.

Harol Moreno Fernández – [email protected]

Mohammad Amirabbasi – [email protected]

Jan P. Hofmann – [email protected]

Introduction

Hydrogen and oxygen production via water electrolysis (i.e., water splitting) requires catalysts that are both active and stable, as well as electrically conductive under operating conditions. Precious metal-based catalysts, such as platinum and iridium dioxide, are effective for catalyzing water splitting in acidic media; however, they are expensive and scarce[1]. In contrast, the oxygen evolution reaction (OER) in alkaline environments is typically performed using non-noble transition-metal oxide (TMO) catalysts[2]. However, these generally exhibit lower activity compared to their noble-metal counterparts in acidic media. As a result, significant efforts have been directed toward developing inexpensive, efficient, earth-abundant, and environmentally benign electrocatalysts for these reactions[3]. Nickel oxide (NiO\mathrm{NiO}) is a promising electrode material for the alkaline OER due to its low cost, natural abundance, and favorable redox properties[4]. As a p-type semiconductor with a wide energy gap (>3.0 eV>3.0\ \mathrm{eV})[5], NiO\mathrm{NiO} features partially filled Ni 3d3d states that hybridize with O 2p2p orbitals, providing a basis for redox activity. When immersed in an alkaline electrolyte, its surface readily converts to nickel hydroxide (Ni(OH)2\mathrm{Ni(OH)_2}), an n-type semiconductor with a wide energy gap (>3 eV>3\ \mathrm{eV})[6] [7], which, under anodic potentials, further transforms into the OER-active nickel oxyhydroxide (NiOOH\mathrm{NiOOH}, p-type semiconductor with a reduced energy gap)[6] [8].

Ni hydroxide/oxyhydroxide films are generally accessible via a redox reaction that involves electrochemical activation of NiO\mathrm{NiO} films9,10—which are typically prepared by dry, vacuum-based processes such as sputtering and pulsed laser deposition (PLD)—in an aqueous electrolyte solution. Nevertheless, only a few reports describe the direct preparation of NiOOH\mathrm{NiOOH} and Ni(OH)2\mathrm{Ni(OH)_2} films using dry methods11,12. Separately, several wet-chemical routes—such as sol-gel, dip-coating, and cathodic deposition—can also yield Ni hydroxides and oxyhydroxides13–15. Nonetheless, these reports often lack correlative spectroscopic evidence or systematic comparisons to confirm phase formation as-deposited. This absence of data leaves uncertainty as to whether hydroxide or oxyhydroxide phases, and the associated oxygen-hole states, can be stabilized before electrochemical treatments. Besides, even if dry or wet processes successfully form the NiOOH\mathrm{NiOOH} phase, its instability in air presents a significant challenge for its characterization; even brief exposure to the atmosphere during transfer can degrade NiOOH\mathrm{NiOOH}; thus, by the time the sample is returned to vacuum to be analyzed spectroscopically, the surface may no longer reflect its initial state, as we have shown in recent studies16,17. Therefore, unambiguous identification of the active phase requires vacuum-integrated approaches such as X-ray photoelectron spectroscopy (XPS), ensuring that the deposited phase can be analyzed without ambient degradation.

A further challenge lies in the electrochemical conditioning typically required to activate NiO\mathrm{NiO}. Converting NiO\mathrm{NiO} into Ni(OH)2\mathrm{Ni(OH)_2} often demands tens to hundreds of cyclic voltammetry (CV) cycles before stable properties are achieved16,18. This activation period is critical, as larger amounts of Ni(OH)2\mathrm{Ni(OH)_2} facilitate stabilization of the catalytically active NiOOH\mathrm{NiOOH} phase10,17. Therefore, introducing hydroxyl groups during deposition–for example, by incorporating H2O\mathrm{H_2O} vapor during growth–not only accelerates this transformation but also promotes the formation of mixed Ni−O−H\mathrm{Ni-O-H} coordination environments, as we will show in later sections.

Ni3+−O−\mathrm{Ni^{3+}-O^-} configurations reflect the broader role of lattice oxygen redox, in which oxygen-hole states (O−\mathrm{O^-} species) emerge from strong Ni−O\mathrm{Ni-O} covalency and directly participate in O−O\mathrm{O-O} bond formation19,20. Nevertheless, stabilizing such oxygen holes remains a central challenge: they typically form only under electrochemical bias, are dynamically coupled to structural changes, and are difficult to embed during synthesis without compromising stability21,22. Under oxygen-rich growth conditions, Ni vacancies act as the dominant charge-compensation mechanism and can stabilize Ni3+−O−\mathrm{Ni^{3+}-O^-} configurations by introducing mixed O 2p−Ni 3d\mathrm{O\ 2p-Ni\ 3d} states near the Fermi level. In contrast, when hydroxyl species are incorporated (e.g., under H2O\mathrm{H_2O}-containing plasma conditions), OH−\mathrm{OH^-} ligands tend to compensate vacancy-induced Ni3+\mathrm{Ni^{3+}} centers and restore local Ni2+\mathrm{Ni^{2+}} coordination, thereby suppressing the formation of additional lattice oxygen hole (O−\mathrm{O^-}) states. To rationalize these trends at the electronic-structure level, density-functional theory (DFT) reveals how cation vacancies and incorporated hydroxyl species tune the mixed O 2p−Ni 3d\mathrm{O\ 2p-Ni\ 3d} states near the Fermi level in NiO\mathrm{NiO}. These calculations predict that introducing Ni vacancies generates in-gap states, narrowing the electronic gap23, whereas hydroxylation modifies Ni−O\mathrm{Ni-O} covalency by creating shallow Ni−O−H\mathrm{Ni-O-H} hybrid states rather than stabilizing new ligand-hole configurations. These defect-induced states exhibit a mixed O 2p−Ni 3d\mathrm{O\ 2p-Ni\ 3d} character near the Fermi level, enhancing Ni−O\mathrm{Ni-O} covalency, and in oxygen-rich films can stabilize oxygen-hole configurations that lower the barrier for lattice oxygen participation during OER. However, experimental realization and spectroscopic validation of these predicted states remain scarce. Thus, strategies that directly tune Ni−O\mathrm{Ni-O} hybridization–whether through vacancy formation or controlled hydroxylation–provide a promising pathway to engineer lattice-oxygen-mediated OER in TMOs19,24.

In this study, we integrate plasma-assisted synthesis of NiO\mathrm{NiO} with density functional theory (DFT) and experimental spectroscopy to establish how O2\mathrm{O_2} and H2O\mathrm{H_2O} in the discharge control the formation of Ni vacancies, ligand-hole states, and hydroxylated coordination environments. Controlled plasma deposition allows systematic tuning of vacancy density and hydroxyl content, which in turn modulate Ni−O\mathrm{Ni-O} covalency and the defect-derived electronic states near the valence band edge. Under oxygen-rich conditions, DFT predicts that vacancy clustering can stabilize Ni3+−O−\mathrm{Ni^{3+}-O^-} configurations—although in the experimentally grown 88% O2\mathrm{O_2} films these Ni-centered holes are largely below the detection threshold and the ligand-hole character appears predominantly O-centered—whereas H2O\mathrm{H_2O} incorporation compensates vacancy-induced Ni3+\mathrm{Ni^{3+}} and restores local Ni2+\mathrm{Ni^{2+}} coordination without generating additional ligand holes. This behavior modifies the surface electronic structure, facilitating the NiO→Ni(OH)2→NiOOH\mathrm{NiO \rightarrow Ni(OH)_2 \rightarrow NiOOH} transformation during electrochemical conditioning. Consequently, the combined plasma–DFT approach provides a controlled means to pre-define defect configurations during synthesis and to tailor the activation behavior of NiO.

The manuscript is organized as follows. § 2.1 presents the DFT framework used to evaluate how Ni vacancies and hydroxyl species modify the electronic structure of NiO. § 2.2 describes the plasma-assisted synthesis of NiO and h-NiO thin films and their structural characterization. § 2.3 provides the XPS and valence band analysis that resolves the evolution of Ni–O, Ni–O–H. § 2.4 discusses the Ni K-edge XANES/EXAFS results, highlighting local and medium-range structural changes associated with vacancy formation and hydroxylation. § 2.5 correlates these defects and electronic signatures with the electrochemical OER performance, including Tafel analysis, and turnover frequency (TOF). The final section summarizes the implications of plasma-driven defect engineering for preconditioning NiO-based OER catalysts.

Results and Discussion

Magnetic Structure and Defect-Induced Electronic States of NiO and h-NiO

First-principles calculations are performed within density functional theory (DFT) using the projector augmented-wave (PAW) basis set25 as implemented in the Vienna Ab initio Simulation Package (VASP)26. We first examine the magnetic moments and spin-resolved density of states (DOS) of stoichiometric NiO. In the pristine supercell, all Ni sites carry essentially identical local environments. However, because PBEsol alone cannot adequately capture strong electron-electron correlations, particularly in Mott insulators such as NiO, we treat the Ni 3d3d states with the DFT+UU27,28 method, applying an on-site Coulomb interaction U=4U=4 eV; full parameters are given in the methodology section. With this approach, all Ni sites carry essentially identical local moments of about ±1.61μB\pm1.61\mu_{\mathrm{B}}, arising almost entirely from the 3d3d channel, whereas all O sites are essentially non-magnetic with moments numerically indistinguishable from zero, in good agreement with previous calculations29. The Ni moments are arranged in the conventional antiferromagnetic (AFM) pattern: one sublattice is spin-up and the other spin-down, so the contributions from the two sets of Ni ions cancel and the total magnetization of the cell is zero. The corresponding spin-resolved total and projected DOS (Figure 1a) is nearly perfectly symmetric with respect to spin and exhibits a clear insulating gap at the Fermi energy. The valence band (VB) is dominated by Ni-3d3d states with substantial hybridization to O-2p2p, while the conduction band has mainly Ni-3d3d character.

Density of states plots for pure NiO bulk, one Ni vacancy, two vacancies, and H-terminated two-vacancy NiO

Figure 1. Density of states (DOS) for (a) pure NiO bulk, (b) with one Ni vacancy, (c) with two vacancies, and (d) sample (c) with H-terminations. For two Ni vacancies, one Ni spin up, and one Ni spin down have been removed so that they are in far-field distance. The two nearest neighbors close to Ni-vacancies are oxidized from Ni2+\mathrm{Ni}^{2+} to Ni3+\mathrm{Ni}^{3+}. The local spin moments of reduced Ni ions are +0.81μB+0.81\mu_{\mathrm{B}} and −0.81μB-0.81\mu_{\mathrm{B}}. Hence, the system is still AFM, and the DOS for spin-up and spin-down channels are symmetric, and the total spin moment is zero. In the next step, we terminate O ions close to reduced Ni by H. We find that Ni3+\mathrm{Ni}^{3+} ions go back to Ni2+\mathrm{Ni}^{2+} in AFM order. It should be noted that only for the NiO pure case, the system is an insulator, i.e., the Fermi energy does not penetrate to the CB or VB.

To link our DFT models to experiment, we assume that NiO films grown at 1.0–20% O2_2 content in the plasma discharge develop Ni deficiencies, consistent with the XPS evidence discussed later. We therefore introduce a single Ni vacancy (VNi′′V_{\mathrm{Ni}}^{\prime\prime}) on the spin-up sublattice. When this single vacancy is introduced, the overall AFM order remains intact. Most of the remaining Ni ions retain moments close to ±1.61μB\pm1.61\mu_{\mathrm{B}}, and only a few Ni atoms in the spin-down layer show a modest reduction of the moment to −1.50μB-1.50\mu_{\mathrm{B}}. In contrast to the pristine case, a subset of O ions in the supercell develops small but finite spin polarizations of order 0.040.04-0.06μB0.06\mu_{\mathrm{B}}. The combination of slightly modified Ni moments and these induced O moments compensates for the missing spin of the removed Ni ion, so that the total magnetization of the defective supercell remains practically zero. The DOS for this single-vacancy configuration (Figure 1b) closely resembles that of pristine NiO. It shows that a finite band gap at the spin-up channel and the total DOS at the Fermi energy are essentially zero. The main effect of the vacancy is a subtle redistribution of DOS in the spin-down channel near the top of the VB, where the O-2p contribution becomes somewhat enhanced. The Fermi energy is pinned at the valence band maximum (VBM), reflecting the presence of holes introduced by the VNi′′V_{\mathrm{Ni}}^{''}. However, the absence of appreciable DOS at EFE_{\mathrm{F}} shows that the system remains in an antiferromagnetic insulator, possibly with weak p-type character, rather than becoming metallic. Our findings for a single VNi′′V_{\mathrm{Ni}}^{''} are consistent with previous theoretical and experimental studies on Ni-deficient NiO, which identify VNi′′V_{\mathrm{Ni}}^{''} as the dominant native acceptor and link it to hole states with mixed Ni-3d/O-2p character near the VBM, while the system remains an antiferromagnetic insulator at realistic vacancy concentrations.

Previous DFT+UU and hybrid-functional studies of Ni vacancies, including calculations on NiO (100) surfaces, show that removal of a Ni2+\mathrm{Ni}^{2+} cation introduces two holes with predominant O-2p (ligand-hole) character23,30. Hybrid functionals tend to localize these holes more strongly on oxygen atoms adjacent to the vacancy, whereas DFT+UU descriptions often yield more delocalized hole distributions extending over the Ni–O network. In our bulk PBEsol+UU calculations at the vacancy concentration considered here (U=4U = 4 eV), attempts to enforce fully localized O−\mathrm{O}^{-} or Ni3+\mathrm{Ni}^{3+} configurations via occupation-matrix control relax back to a delocalized hole state, indicating that the holes introduced by a VNi′′V_{\mathrm{Ni}}^{''} remain distributed over the surrounding Ni–O framework rather than being stabilized as discrete O−\mathrm{O}^{-} or Ni3+\mathrm{Ni}^{3+} centers.

We next consider a supercell containing two spatially separated Ni vacancies—reflecting the high-vacancy conditions produced when NiO is processed with 88% O2_2 in the plasma discharge—one on each antiferromagnetic sublattice, as far as possible from each other in a 3×3×33\times3\times3 supercell (7.15 Å). The site-resolved spin moments show that most Ni ions still carry moments close to ±1.61μB\pm1.61\mu_{\mathrm{B}}, as in the pristine system, but two Ni sites exhibit strongly reduced moments of about ±0.85μB\pm0.85\mu_{\mathrm{B}}. These reduced moments are consistent with a change of the local configuration from high-spin Ni2+\mathrm{Ni}^{2+} (S = 1) to low-spin Ni3+\mathrm{Ni}^{3+}. As in the single-vacancy case, some O ions acquire finite moments up to 0.07μB0.07\mu_{\mathrm{B}}, whereas others stay only weakly polarized. The spin-resolved DOS for the double-vacancy configuration (Figure 1c) denotes additional Ni-3d appearing near the valence band edge, which we associate with Ni3+\mathrm{Ni}^{3+} related states created to compensate for the removal of two Ni2+\mathrm{Ni}^{2+} cations. The Fermi energy is again pinned at the top of the VB. Because the two low-spin Ni3+\mathrm{Ni}^{3+} centers reside on opposite spin sublattices, their moments cancel each other, and the total magnetization of the supercell stays essentially zero, so that the global antiferromagnetic character of NiO is preserved even in the presence of two Ni vacancies. For multiple Ni vacancies, our results are consistent with previous work on Ni-deficient NiO, which shows that increasing the Ni-vacancy concentration mainly enhances Ni3+\mathrm{Ni}^{3+}/hole character and adds Ni-3d/O-2p spectral weight near the VBM. At the same time, the material remains antiferromagnetic and insulating over a broad range of nonstoichiometries23,31–33. These studies also find only moderate modifications of the local Ni moments and no robust metallic phase, in agreement with our double-vacancy configuration, where the global AFM order is preserved.

We next passivate the double–Ni-vacancy configuration with two H atoms, each adsorbed on top of an O ligand that is coordinated to one of the Ni3+\mathrm{Ni}^{3+} centers. This operation aims to emulate the hydroxylated NiO (h-NiO) produced experimentally when H2O\mathrm{H}_{2}\mathrm{O} was introduced in the plasma discharge during deposition. Moreover, as confirmed later by TEM analysis, the hydroxylated films preserve the underlying rock-salt NiO structure. The resulting magnetic moments show that most Ni ions still carry ±1.61μB\pm1.61\mu_{\mathrm{B}}, as in pristine NiO, but the strongly reduced Ni sites associated with the vacancies are no longer present. The moments on these Ni ions increase from ±0.85 μB\pm0.85\,\mu_{\mathrm{B}} in the bare double-vacancy case to values close to the bulk (±1.58 μB\pm1.58\,\mu_{\mathrm{B}}). Instead, a few Ni ions exhibit only moderately reduced moments of about 1.471.47–1.55 μB1.55\,\mu_{\mathrm{B}}, indicating that the holes are now more delocalized over the Ni–O–H network rather than being localized on specific Ni3+\mathrm{Ni}^{3+} sites. Some O ions again acquire finite spin polarizations up to 0.06 μB0.06\,\mu_{\mathrm{B}}.

In contrast, the H atoms carry only very small moments of opposite sign (±0.003 μB\pm0.003\,\mu_{\mathrm{B}}), so that the total magnetization of the supercell remains essentially zero. The spin-resolved DOS (Figure 1d) shows that the Fermi energy is pinned at the VBM, and a sharp, almost spin-degenerate H-1s peak appears as a deep, localized state well below the valence band, together with a weak H contribution near the top of the VB, reflecting hybridization with O-2p states. Thus, in this local defect configuration, H incorporation passivates the Ni3+\mathrm{Ni}^{3+} centers created by the Ni vacancies, effectively driving them back toward a Ni2+\mathrm{Ni}^{2+}-like configuration at the hydroxylated sites.

To rationalize these electronic reconstructions within a chemical framework, the DFT-predicted charge redistributions can be expressed through a corresponding defect-compensation reaction that preserves electroneutrality after plasma growth. These mechanisms determine how Ni vacancies, oxygen acceptor states, and hydroxyl species distribute charge within the lattice under different plasma conditions and are summarized in Equations (1)–4.

Under O2\mathrm{O}_{2}-rich sputtering conditions (no H2O\mathrm{H}_{2}\mathrm{O}), NiO deviates from stoichiometry through the formation of Ni vacancies (VNi′′V_{\mathrm{Ni}}^{\prime\prime}). The DFT calculations show that isolated vacancies are primarily compensated by the formation of oxygen-ligand holes (O−\mathrm{O}^{-}), which appear as shallow unoccupied states just above the valence band maximum. At higher vacancy concentrations, neighboring vacancies interact cooperatively, oxidizing adjacent Ni2+\mathrm{Ni}^{2+} to Ni3+\mathrm{Ni}^{3+} and forming localized Ni3+\mathrm{Ni}^{3+}–O−\mathrm{O}^{-} pairs. At sufficiently high oxygen chemical potential, incorporation of oxygen interstitials is also possible, although not seen in our experiments and calculations. Together, these vacancy-driven mechanisms generate the acceptor states and ligand-hole configurations identified in the DOS analysis, accounting for the p-type character of Ni-deficient NiO\mathrm{NiO}34–37.

When H2O\mathrm{H}_{2}\mathrm{O} vapor is introduced during plasma deposition, hydroxyl species bind preferentially to O sites adjacent to Ni vacancies. The DFT results show that OH−\mathrm{OH}^{-} incorporation compensates for the negative charge of VNi′′V_{\mathrm{Ni}}^{\prime\prime} and restores nearby Ni3+\mathrm{Ni}^{3+} centers to Ni2+\mathrm{Ni}^{2+}, removing the di-vacancy in-gap states seen in Figure 1c. The resulting electronic structure contains only shallow OH-derived states (Figure 1d), arising from mixed H 1s–O 2p–Ni 3d character, and does not stabilize Ni3+\mathrm{Ni}^{3+}–O−\mathrm{O}^{-} ligand-hole configurations. This hydroxylation removes the vacancy-associated deep defect states rather than generating Ni3+\mathrm{Ni}^{3+}/O−^{-} ligand-hole configurations, and thus produces the shallow unoccupied state seen in Figure 1d.

Together, these mechanisms highlight that controlling the O2/H2O\mathrm{O}_{2}/\mathrm{H}_{2}\mathrm{O} ratio during plasma growth directly tunes Ni-vacancy formation and Ni–O–H covalency, which in turn influence hole delocalization. To validate these DFT-based predictions experimentally, we synthesized NiO and hydroxylated NiO (h-NiO) thin films under systematically varied plasma compositions, as described in the following section.

Synthesis and physical characterization of NiO and h-NiO thin films

NiO and h-NiO thin films were deposited via reactive magnetron sputtering onto polished nickel foils. For the preparation of NiO thin films, oxygen content in the plasma discharge was used at 1.0%, 20%, 66%, and 88%. For the preparation of h-NiO thin films, water vapor was introduced in the 1.0×10−61.0 \times10^{-6} to 1.0×10−41.0 \times10^{-4} mbar partial pressure range. The deposition parameters used for NiO and h-NiO films are summarized in Table S1, Table S2, and Table S3. For h-NiO thin films and high O2O_2 content in the plasma discharge, the maximum thickness was limited to approximately 15 nm due to a significant reduction in deposition rate. This reduction originates from the reaction of water vapor with the target erosion zone, which forms a less conductive nickel-oxide layer on the target surface and substantially reduces the sputtering yield. This layer causes a substantial decrease in target voltage, thereby reducing the deposition rate38. However, two reference samples were prepared with 1.0% and 20% O2O_2 content, having a thickness of 100 nm, to obtain an acceptable sample for Grazing Incidence X-Ray Diffraction (GXRD) measurements.

Parameters1.0 % O₂1.0 % O₂20 % O₂20 % O₂
15 nm100 nm15 nm100 nm
Base pressure (mbar)1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}
Working pressure (mbar)3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}
Ar flow (sccm)19.819.81616
O₂ flow (sccm)0.20.244
Deposition time (min)43025167
Deposition rate (min)3.53.50.60.6
Power (W)15151515

Table S1. working parameters used to prepare NiO thin films of 15 nm and 100nm.

Parameters1.0 % O₂20 % O₂88 % O₂88 % O₂ + 0.3% H₂O
Base pressure (mbar)1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}1.0×10−81.0 \times10^{-8}
Working pressure (mbar)3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}3.0×10−23.0 \times10^{-2}
Ar flow (sccm)19.8161.31.3
O₂ flow (sccm)0.241010
H₂O pressure (mbar)---1.0×10−41.0 \times10^{-4}
Deposition time (min)4254040
Deposition rate (min)3.50.60.40.4
Power (W)15151515

Table S2. working parameters used for NiO thin films prepared with 1.0%, 20%, 88% O₂, and 88% + 0.3% H₂O.

Parameters0.003 % H2O\mathrm{H_2O}0.03 % H2O\mathrm{H_2O}0.3 % H2O\mathrm{H_2O}11.6 % H2O\mathrm{H_2O}
Base pressure (mbar)1.0×10−81.0 \times10^{-8}
Working pressure (mbar)3.0×10−23.0 \times10^{-2}
Ar flow (sccm)19.821.32
O2\mathrm{O_2} flow (sccm)0.24104
H2O\mathrm{H_2O} pressure (mbar)1.0×10−61.0 \times10^{-6}1.0×10−51.0 \times10^{-5}1.0×10−41.0 \times10^{-4}1.0×10−31.0 \times10^{-3}
Deposition time (min)4604070
Deposition rate (min)3.50.250.40.2
Power (W)15

Table S3. working parameters used for NiO thin films prepared with 88% O2\mathrm{O_2} + different H2O\mathrm{H_2O} concentrations.

The morphology of the 15 nm and 100 nm films prepared with 1.0%, 20%, 66%, and 88% O2+H2OO_2 + H_2O mixtures in the plasma discharge is presented in the 3D AFM micrographs in Figure S1. Two scan sizes (10 × 10 μm2\mu\mathrm{m}^2 and 0.5 × 0.5 μm2\mu\mathrm{m}^2) were used to capture distinct morphological features, with the larger scan highlighting the macroscopically flat regions of the samples, for NiO prepared with 1.0% O2O_2 content (Figure S1) the surface roughness increases with film thickness, characterized by a surface covered with particles exhibiting a pyramidal-shaped structure and a dendritic microstructure (Figure S1). In contrast, higher oxygen concentrations progressively reduce surface roughness, as observed in the 15 nm films (Figure S1-Figure S1) and in the 100 nm thickness film (Figure S1). The variation in surface morphology and roughness can be attributed to increased defect formation during growth. At higher oxygen partial pressure, the amount of metallic Ni0^0 decreases, likely due to enhanced oxidation of sputtered Ni atoms and changes in grain-growth kinetics.38,39

3D AFM micrographs of NiO thin films

Figure S1. 3D AFM micrographs of NiO thin films of 15 and 100 nm and h-NiO thin films for different oxygen concentrations before any electrochemical conditioning (BC). The image was acquired using scan sizes of 10×10 μm210 \times10\ \mu\mathrm{m}^{2} and 0.5×0.5 μm20.5 \times0.5\ \mu\mathrm{m}^{2}.

The GXRD diffractogram of the 100 nm thickness NiO sample prepared with 1.0% O2O_2 (Figure S2) displays four NiO Bragg reflections at (111), (200), (220), and (311) in line with reported values40,41, together with three reflections from the Ni substrate at (111), (200), and (220). Among these, the NiO (200) peak at 2θ=43.9∘2\theta= 43.9^\circ is particularly intense, indicating preferential growth along this crystallographic direction. This preferential (200) orientation reflects the low surface energy of the nonpolar (100)/(200) planes in NiO, which are more stable than the polar (111) surfaces11. The additional reflection at 2θ=44.6∘2\theta= 44.6^\circ corresponds to the Ni (111) lattice, originating from the underlying substrate.

Figure S2. G-XRD diffractograms of NiO thin films of 100 nm prepared with 1.0% and 20% O2_2 content before electrochemical conditioning (BC) and after 200 CV conditioning (AC).

As the O2\mathrm{O}_2 concentration in the plasma process increases, the intensity of the NiO (200) reflection decreases significantly, indicating a shift in the preferential orientation from (200) to (111). This trend is attributed primarily to the reduced adatom mobility under oxygen-rich sputtering conditions39,42. Higher O2\mathrm{O}_2 flow increases scattering and promotes partial oxidation of sputtered species, both of which reduce surface diffusion and favor growth along the (111) direction39.

Electrochemical conditioning further modifies the structural orientation. After 200 CV cycles, the 100 nm NiO film deposited at 1.0% O2\mathrm{O}_2, transforms at the surface into hydrous Ni(OH)2\mathrm{Ni(OH)}_2 (α\alpha-Ni(OH)2\mathrm{Ni(OH)}_2) consistent with previous reports10,17, this transformation coincides with the disappearance of the intense (200) reflection, suggesting that electrochemical conditioning leads to partial loss of the (200) texture, consistent with surface reconstruction during NiO →\to Ni(OH)2\mathrm{Ni(OH)}_2 transformation. The absence of distinct Ni(OH)2\mathrm{Ni(OH)}_2 reflections in the XRD pattern is likely due to the poor crystallinity or low volume fraction.

The structural response to conditioning depends strongly on the initial defect density and preferred orientation established during deposition. For the 20% O2\mathrm{O}_2 film, which initially exhibits a stronger (111) texture and higher Ni deficiency, electrochemical conditioning drives the opposite evolution: the intensity of the (111) reflection decreases significantly. In contrast, a pronounced (200) reflection emerges, suggesting that the initially exposed (111) surface reacts with OH−\mathrm{OH}^{-} ions during conditioning and undergoes structural reconstruction toward a (200)-like texture, consistent with the preference for nonpolar surfaces during hydroxylation. A higher concentration of Ni deficiencies in the film likely facilitates this rearrangement43.

Repeated redox cycling during conditioning enhances ionic mobility and promotes structural reorganization within the film, potentially modifying an initially textured structure into a more polycrystalline or less oriented arrangement44. As a result, the observed decrease in the (111) reflection and increase in the (200) reflection capture the dynamic structural evolution of NiO under electrochemical stress.

While both Ni and NiO crystallize in a face-centered cubic (fcc) structure, their different lattice parameters result in Bragg reflections of the same family of planes appearing at different 2θ2\theta angles. For instance, the (111) reflection occurs at 37.11∘37.11^\circ for NiO and 44.64∘44.64^\circ for Ni, reflecting the intrinsic lattice mismatch between NiO and the Ni substrate, which results in residual strain within the film45. Increasing the O2\mathrm{O}_2 concentration shifts the 2θ2\theta position and broadens the full width at half maximum (FWHM), consistent with reduced coherent domain size as inferred from the Scherrer equation46.

The broadening arises because, when the crystallite size approaches the X-ray wavelength (λ\lambda), fewer coherent scattering planes contribute to the diffraction, resulting in weaker and broader peaks47. However, given the low signal-to-noise ratio in the NiO diffraction patterns and the high defect density of the films, the observed FWHM broadening likely reflects a combination of structural disorder and limited crystallite size48. In such cases, applying the Scherrer equation would yield inaccurate estimates of crystallite size.

In contrast to the clearly separated peaks of Ni and NiO arising from their distinct lattice parameters, although Gong et al.²² attributed the reflections at 2θ=43.1∘2\theta= 43.1^\circ, 62.6∘62.6^\circ, and 75.2∘75.2^\circ to the Ni2O3\mathrm{Ni_2O_3} phase, such assignments are controversial because these peaks overlap with Ni and NiO reflections. Therefore, we cannot give clear evidence to support the presence of Ni2O3\mathrm{Ni_2O_3} in our samples. Consequently, complementary spectroscopic analysis would be required to unambiguously resolve the chemical composition and oxidation states of the films.

The evolution of preferred orientation from (200) to (111) with increasing O2\mathrm{O_2} content, together with peak broadening and subtle 2θ2\theta shifts, points to lattice contraction and enhanced disorder typical of Ni-deficient NiOx\mathrm{NiO_x}38,39. These structural fingerprints indicate that oxygen-rich plasma conditions promote Ni-vacancy formation and alter the local bonding environment. To examine how plasma composition modifies Ni/O stoichiometry, oxidation-state distribution, and spectroscopic signatures associated with ligand-hole formation, we performed in-vacuum XPS analysis, as detailed in the following section.

Chemical Composition Analysis

In-system XPS measurements were conducted on the as-prepared thin films to determine their elemental composition and nickel oxidation states. The quantitative Ni/O atomic ratios derived from the survey spectra are shown in Figure S3. NiO and h-NiO samples deposited at higher O2\mathrm{O_2}% concentrations exhibit a clear Ni deficiency, except for the film grown at 1.0% O2\mathrm{O_2}. Although the reduced Ni/O ratio does not imply the presence of well-defined, isolated Ni vacancies, it reflects a net loss of Ni from the lattice, which can be formally represented as cation-site vacancies (VNi′′V_{\mathrm{Ni}}^{''}) in Kröger–Vink notation. Interestingly, the overall oxygen content does not scale linearly with the O2\mathrm{O_2} fraction in the plasma, suggesting nonlinear incorporation dynamics during growth.

Atomic percentage composition of Ni and O for 15 nm NiO/Ni and 15 nm h-NiO/Ni samples under varying O₂ and H₂O conditions

Figure S3. Atomic percentage composition derived from the XPS analysis of Ni 2p and O 1s core levels.

Under the highly oxidizing plasma conditions used here, the formation of oxygen vacancies is thermodynamically disfavored, and any such sites would rapidly re-oxidize upon exposure to residual oxygen or moisture49,50, since reactive oxygen species are abundant in both the plasma phase and at the film surface. Additionally, XPS is not capable of directly probing oxygen vacancies because such sites heal spontaneously upon exposure to oxygen or moisture. Therefore, the O 1s component at ∼531\sim531 eV—frequently incorrectly ascribed to oxygen vacancies in the literature—arises instead from hydroxyl groups, adsorbed oxygen, or other surface species, as emphasized by Idriss⁴⁹ and reinforced by Easton and Morgan⁵⁰. Therefore, the observed nonstoichiometry is attributed primarily to Ni-site vacancies rather than oxygen deficiency, consistent with defect-chemistry models of NiO under O-rich conditions51.

Ni deficiency is not merely a structural feature but directly affects the electronic properties of the films. Vacancy defects are known to introduce electronic states, modify the band structure, and shift the work function, thereby influencing catalytic activity52,53. For instance, Mark et al.^54 modified the work function of NiO by introducing oxygen vacancies, which, as a result, moved the Fermi level away from the VBM. Similarly, Egbo et al.^55 demonstrated through spectroscopic ellipsometry and first-principles calculations that Ni vacancies alter both the electronic and optical responses, highlighting their role in adjusting conductivity and reactivity. By analogy, the Ni deficiency observed in our sputtered films is expected to contribute not only to the chemical composition, as evident in the XPS features, but also to the catalytic performance discussed in § 2.5.

The compositional trend at high O2\mathrm{O}_2 partial pressures (Figure S3) can be attributed to "target poisoning", where the formation of NiO on the target surface reduces the sputtering yield of Ni, thereby lowering the Ni flux to the substrate56,57. Meanwhile, reactive oxygen species remain abundant, yielding a Ni-deficient film composition. Such changes in the O2\mathrm{O}_2 partial pressures in the plasma discharge not only impact elemental fluxes but also reflect broader shifts in growth dynamics under increasingly oxidizing conditions, as already evidenced in § 2.2.

XPS analysis of the Ni 2p3/22p_{3/2} and O 1s core levels for films prepared at different oxygen partial pressures is presented in Figure 2a-Figure 2c, together with the spectrum of a film deposited in the presence of 0.3% H2O\mathrm{H}_2\mathrm{O} for comparison. The O 1s spectra (Figure 2a and Figure 2c) consistently show a main peak at ∼529.0\sim529.0 eV, corresponding to lattice oxygen (O2−\mathrm{O}^{2-}), and a higher binding energy shoulder at ∼530.6\sim530.6-531.0 eV, which becomes more intense with increasing O2\mathrm{O}_2 concentration. This feature is often attributed to non-lattice oxygen species such as adsorbed oxygen or oxidized lattice oxygen (O−\mathrm{O}^{-}). It may also reflect the presence of defect-related species as Ni vacancies or oxygen bonded to Ni3+\mathrm{Ni}^{3+} centers, which contribute to defect states in the oxide network34,58–60, and hydroxyl groups for films prepared with H2O\mathrm{H}_2\mathrm{O}.

XPS spectra and deconvolution plots of NiO thin films

Figure 2. XPS analysis of NiO thin films prepared with different oxygen concentrations and with varying H2_2O concentrations in the plasma discharge. (a, b) O 1s and Ni 2p3/22p_{3/2} spectra of thin films of 15 nm deposited with 1.0, 20, 66, and 88% O2_2, and with 88% O2_2 + 0.3% H2_2O in the plasma discharge. (c) Deconvolution of the O 1s spectra from (a), showing contributions from lattice oxygen (O2−^{2-}), hydroxyl groups, adsorbed water, and defect-related species. (d, e) O 1s and Ni 2p3/22p_{3/2} spectra for films deposited with 0.03, 0.3, and 11.6% H2_2O in the plasma discharge. (f) Deconvolution of the O 1s spectra from (d), showing contributions from lattice O2−^{2-}, hydroxyl species, adsorbed water, and gas-phase H2_2O. All spectra were collected before air exposure and prior to electrochemical treatment.

Interestingly, as the oxygen concentration in the plasma increases beyond 20%, the entire O 1s envelope shifts toward higher binding energies. In many oxide systems, such as TiO2\mathrm{TiO}_2 or CeO2\mathrm{CeO}_2, increasing O2\mathrm{O}_2 during deposition typically shifts the O 1s peak to lower binding energies due to vacancy passivation61,62. In NiO, however, the opposite trend occurs; the O 1s peak shifts to higher binding energy. This shift has been attributed to enhanced Ni-vacancy formation and reduced final-state screening under highly oxidizing conditions63. When H2O\mathrm{H}_2\mathrm{O} is added to the plasma deposition environment, the peak at ∼530.6\sim530.6 eV broadens and increases, consistent with the formation of surface hydroxyls49, indicating that reactive sputtering in the presence of water vapor promotes hydroxylation rather than further oxidation towards higher nickel valence states. The feature at ∼532.1\sim532.1-532.4 eV corresponds to molecularly adsorbed H2O\mathrm{H}_2\mathrm{O}, whereas the peak at ∼535.5\sim535.5 eV originates from gas-phase H2O\mathrm{H}_2\mathrm{O}64,65.

Figure 2b shows the Ni 2p3/22p_{3/2} core level of the films. The dominant peak at ~854 eV is assigned to the well-screened Ni 2p53d9Z2p^{5}3d^{9}Z state, while the shoulder at ~855 eV corresponds to the Ni 2p53d9L2p^{5}3d^{9}L state associated with O 2p2p ligand holes66. The distinction between these two features has been a subject of debate. Stevie et al.,67 attributed the doublet at 853–856 eV to the multiplet splitting of the Ni 2p3/22p_{3/2} core level. Regardless of the interpretation, the increase in O2_2 concentration enhances the Ni 2p53d9L2p^{5}3d^{9}L state (~855 eV), indicating a higher density of oxygen ligand-holes (O−^{-}) states, in agreement with the O 1s analysis. The shake-up line at ~861 eV arises from de-excitation processes, in which the outgoing photoelectrons excite Ni 3d3d electrons, thereby reducing their kinetic energy and shifting the peak to higher binding energy68.

When H2_2O is introduced during deposition, the evolution of the Ni 2p2p line shape must be interpreted differently. In hydroxylated NiO, changes in the 3d9L/3d9Z3d^{9}L/3d^{9}Z intensity ratio cannot be directly or solely attributed to the formation of additional Ni3+^{3+}–O−^{-} ligand-hole pairs. Instead, they arise from modified final-state screening and stronger Ni–O–H hybridization, which alters the multiplet balance without generating the deep divacancy-derived ligand-hole states characteristic of vacancy-rich NiO. This behavior is fully consistent with DFT predictions that hydroxyl groups compensate vacancy-induced Ni3+^{3+} centers and suppress deep in-gap states.

Figure 2d and e compare the O 1s and Ni 2p3/22p_{3/2} spectra of films grown at 88% O2_2 with increasing H2_2O partial pressure. The main O 1s peak at ~529.1 eV corresponds to lattice O2−^{2-}, while the shoulder near ~530.9 eV is dominated by hydroxyl (OH−\mathrm{OH}^{-}) species introduced during H2O\mathrm{H}_{2}\mathrm{O}-assisted sputtering. This region may still contain contributions from oxidized oxygen and other defect-related environments; the higher-energy feature at ~532.1 eV comes from adsorbed water, as we already mentioned. With increasing H2O\mathrm{H}_{2}\mathrm{O} content, the hydroxyl component grows at the expense of the NiO lattice contribution, indicating progressive hydroxylation of surface and near-surface regions. In the corresponding Ni 2p2p spectra, the increase of the 3d9L3d^{9}L relative to the 3d9Z3d^{9}Z final state indicates globally altered screening and changes in the local Ni–O–H coordination environment. Such an increase is also consistent with a higher degree of ligand-hole character, in line with the Ni L-edge results presented later, which show persistent ligand-hole signatures in hydroxylated films. Thus, the evolution of the Ni 2p2p multiplet structure reflects a combination of modified screening, increased Ni–O–H coordination, and a redistribution of unoccupied 3d3d–O 2p2p hybrid states that accompanies hydroxyl incorporation.

This interpretation is further supported by Ni K-edge XANES (Figure 3l). Both NiO and h-NiO display an absorption edge (E0E_{0}=8346 eV), indicating that the average Ni oxidation state remains unchanged. The pre-edge feature at ~8333.5 eV, arising from 1s→3d1s \rightarrow3d transitions, that gains intensity through Ni 3d3d–O 2p2p hybridization69–71, is shown for both samples. Such pre-edge is well-established as a signature of increased metal-ligand covalency and oxygen-hole character in transition-metal oxides72. The pre-edge intensity observed in both NiO and h-NiO films, therefore, provides complementary evidence of ligand-hole formation (Ni3+^{3+}–O−^{-} or O-centered) and covalency in these materials.

Figure 3. XPS comparison of NiO, Ni(OH)2_2, and h-NiO thin films. (a) O 1s core-level spectra showing lattice oxygen in NiO, hydroxyl-related species in Ni(OH)2_2, and mixed contributions in h-NiO. (b) Ni 2p3/22p_{3/2} spectra highlighting the intermediate binding energy of h-NiO, consistent with mixed O2−^{2-}/OH−^- coordination. (c) Valence band spectra illustrating the intermediate electronic character of h-NiO between NiO and Ni(OH)2_2. (d) Comparison of VBM for NiO and h-NiO, showing that h-NiO exhibits a reduced VBM and defect-related tail states extending above the Fermi level. (e–h) Magnitude of the Fourier transform of the k2k^2-weighted χ(k)\chi(k) spectra in R-space for NiO (e) and h-NiO (f), showing the first peak from the Ni–O scattering path (~1–2 Å, phase-uncorrected) and the second peak from the Ni–Ni scattering path (~2–3 Å). (g, h) Corresponding k2k^2-weighted χ(k)\chi(k) spectra in k-space for NiO (g) and h-NiO (h), with experimental data and best-fit curves. (i–k) High-resolution TEM and Selected-area electron diffraction (SAED) images of NiO prepared with 1.0% O2_2 (i), 88% O2_2 (j), and h-NiO (k). The SAED patterns show cubic NiO diffraction rings for both NiO and h-NiO, confirming preservation of the rock-salt structure. (l) Ni-K edge of ex-situ spectra of NiO and h-NiO, highlighting the pre-edge intensity at ~8333.5 eV, which reflects enhanced Ni 3d–O 2p hybridization, and in operando conditions in 1M KOH at three different potentials of 1.3 V, 1.6 V, and 1.8 V vs RHE, indicating the formation of NiOOH OER active phase. (m,n) Ni-L, and O-K edges for the samples with 1.0 and 88% O2_2, 88% O2_2 + 0.3% H2_2O. The samples are compared to a NiO reference from Sigma Aldrich and a α/β\alpha/\beta-Ni(OH)2_2 sample.

To benchmark the chemical and electronic changes induced by H2O\mathrm{H}_{2}\mathrm{O} incorporation, we compared the O 1s1s, Ni 2p3/22p_{3/2}, and valence band XPS spectra of three samples (Figure 3a-Figure 3c): NiO prepared with 1.0% O2\mathrm{O}_{2}, Ni(OH)2_{2}, and h-NiO (with 11.6% H2O\mathrm{H}_{2}\mathrm{O}). The O 1s1s peak of the reference samples, NiO and Ni(OH)2_{2}, appear at ~529.1 eV and ~531.6 eV, respectively, consistent with previously reported values for these Ni oxide phases16,73. The corresponding Ni 2p3/22p_{3/2} core level for these two samples is located at 853.6 eV and 856.1 eV, respectively, with their VBM located 0.3 eV below the Fermi level, for NiO–reflecting its p-type semiconducting character74–and 1.2 eV for Ni(OH)2_{2}, consistent with its n-type behavior[6] [10].

In contrast, the h-NiO sample shows clear signatures of partial hydroxylation. The O 1s1s spectrum exhibits contributions from both NiO and Ni(OH)2_{2}, with a distinct component at ~530.5 eV assigned to OH−\mathrm{OH}^{-} species, and a reduced oxygen lattice signal near 528.8 eV, consistent with partial hydroxylation (Figure 3a, red). Similarly, the Ni 2p3/22p_{3/2} core level appears between the positions of the two reference phases, consistent with mixed O2−^{2-}/OH−^{-} coordination (Figure 3b, red). The valence band spectrum of h-NiO (Figure 3c, red) shows a slightly deeper VBM than pure NiO, with the VBM located ~0.4 eV below the Fermi level. Additionally, the linear extrapolation of the spectral tail approaches the Fermi level (within ~0.07 eV), consistent with defect-related states arising from Ni vacancies and impurity bands[5] [55, 75].

Although the h-NiO VBM lies slightly deeper than in NiO, the near-edge spectral tail does not necessarily indicate the formation of additional ligand-hole states. Instead, these shallow states could also originate from Ni–O–H hybridization and from the increased local electronic and symmetry disorder introduced by hydroxylation, which broadens the upper valence band. In our DFT model, hydroxylation compensates the Ni-vacancy–induced Ni3+^{3+} centers and suppresses the deep in-gap states associated with clustered vacancies, restoring a predominantly Ni2+^{2+} like configuration around the hydroxylated sites. This DFT description reflects the local electronic reconstruction that occurs specifically at hydroxylated vacancies and should not be interpreted as a change in the global Ni oxidation-state distribution of the film. The Ni3+^{3+} species discussed here correspond to vacancy-induced ligand-hole states in the as-prepared films and are distinct from the NiOOH-type Ni3+^{3+} generated electrochemically during OER.

The experimental evolution of the VBM is consistent with the sequence of defect configurations predicted by DFT (§ 2.1). At low oxygen concentration (1.0 % O2_2), the XPS VBM lies further below the Fermi level, corresponding to the stoichiometric or single-vacancy regime– as predicted by DFT– in which only isolated acceptor-like states appear slightly above the VBM. Increasing the O2_2 fraction (20-66 %) drives the VBM progressively closer to the Fermi level and introduces discernible valence band tailing, in agreement with the DFT description of two-vacancy configurations that generate partially filled O 2p2p–Ni 3d3d hybrid states near the Fermi level. At the highest O2_2 content (88 %) and under H2_2O conditions, the VBM slightly shifts away from the Fermi level. This apparent VBM upshift reflects defect-induced broadening rather than a rigid movement of a true band edge. In the hydroxylated film, the valence-band onset becomes even less well defined. Enhanced Ni–O–H hybridization broadens the upper valence band through enhanced Ni–O–H hybridization and strengthens band tailing, causing the extrapolated VBM to appear deeper.

Local Structural Environment from Ni K-edge EXAFS

To further probe the short-range structure and defect chemistry of NiO and h-NiO, Ni K-edge (~8333.5 eV), an EXAFS analysis was performed on the as-deposited films before electrochemical conditioning (Figure 3e-Figure 3h). The Fourier-transformed spectra and corresponding fits provide direct insight into local coordination, bond distances, and structural disorder.

In both cases, the structural model that best describes the local environment is the cubic rock-salt structure. This structural model is well established for stoichiometric NiO, which exhibits a well-defined NiO6_6 octahedral environment with highly reproducible Ni–O (~2.08 Å) and Ni–Ni (~2.95–3.00 Å) distances reported in neutron diffraction and X-ray absorption studies 71,76,77, providing a physically justified reference for EXAFS modeling. To better track the evolution of the system following the treatment, the same parameters were refined for both samples: the edge energy shift, the scattering amplitude, the interatomic distances, and the Debye–Waller factors for the Ni–O and Ni–Ni shells

For NiO thin film (Figure 3e and Figure 3g), the fitted Ni–O bond length of 2.056 ± 0.006 Å agrees well with these literature values, while the Debye–Waller factor (σ2\sigma^{2} = 0.0060 ± 0.0009 Å2^{2})71 lies near the upper end of reported bulk values (~0.004 Å2^{2}). This increased disorder may arise from the higher surface-induced strain in thin films compared to the bulk material, broadening the first-shell distance distribution.

The Ni–Ni shell appears at 3.05 ± 0.01 Å, a value slightly larger than reported. Moreover, the pronounced local disorder (σ2\sigma^{2} = 0.024 ± 0.002 Å2^{2}) is substantially higher than bulk references (~0.010–0.015 Å2^{2})71; this behavior mirrors the trend observed in the first shell, supporting the idea of structural distortion driven by significant surface strain contributions76–78. These parameters reproduce both the amplitude and phase of the experimental first two shells, indicating that while the local NiO6_{6} octahedron is maintained, the cation-cation environment is more significantly distorted.

In addition, the weak but discernible pre-edge feature in the XANES region at ~8333.5 eV (Figure 3l) reflects enhanced Ni 3d–O 2p hybridization and deviations from centrosymmetric octahedral coordination. Increased pre-edge intensity can arise from several mechanisms—including vacancy-induced distortions, local symmetry breaking, and ligand-hole character—and thus cannot be attributed exclusively to Ni vacancies. Although our EXAFS cannot quantify vacancy concentration directly, the combination of higher σ2\sigma^{2} values and the enhanced pre-edge feature in NiO points to increased local disorder and stronger Ni 3d–O 2p hybridization relative to bulk NiO.

Regarding the h-NiO sample (Figure 3f and Figure 3h), the first-shell Ni–O distance is 2.056 ± 0.007 Å with σ2\sigma^{2} = 0.007 ± 0.001 Å2^{2}. This Ni–O distance is essentially identical to that of NiO within the error bars, indicating that the H2_{2}O treatment does not induce any measurable structural modification in the first coordination shell. The Ni–Ni shell appears at 3.02 ± 0.01 Å, with σ2\sigma^{2} = 0.020 ± 0.001 Å2^{2}: after the treatment, this second shell becomes slightly shorter and shows reduced second-shell structural disorder (i.e., it shows smaller interatomic distances and lower σ2\sigma^{2}). Although the Ni–Ni distance and σ2\sigma^{2} values remain higher than bulk NiO, the reduction in both parameters compared to the oxygen-rich NiO film indicates a partial relaxation of the medium-range structure upon hydroxylation, suggesting that h-NiO retains thin-film–induced strain but exhibits reduced vacancy-induced distortion relative to the 88% O2_{2} sample.

A comparison of the edge energy position and scattering amplitude between the two samples provides insight into the evolution of the absorber oxidation state and the possible formation of defects. After refinement, the edge energy is 8344.4 ± 0.6 eV (8344.38034 ± 0.55777) for both samples (8344.38034 ± 0.55777 in NiO and 8344.43815 ± 0.61934 in h-NiO), clearly indicating that the bulk average oxidation state remains unchanged. The S02_{0}^{2} value also remains constant: it refines to 0.86 ± 0.04 (0.8633 ± 0.0447) for NiO and 0.86 ± 0.05 (0.86228 ± 0.05034) for h-NiO, indicating that the overall amplitude reduction and the fraction of coherently scattering atoms remain comparable between the two samples. Because S02_{0}^{2} is primarily a global scaling factor79, its similarity does not rule out local structural modifications. When combined with the changes in Ni\mathrm{Ni}–Ni\mathrm{Ni} distance and σ2\sigma^{2}, the EXAFS results instead indicate that hydroxylation induces a partial relaxation of vacancy-induced distortions without generating a fundamentally different short-range coordination environment.

Complementary TEM analysis (Figure 3i-Figure 3k) supports these structural trends. Selected-area electron diffraction (SAED) patterns show that films grown at low and high O2\mathrm{O}_{2} content, as well as with H2O\mathrm{H}_{2}\mathrm{O} content, retain the cubic rock-salt NiO\mathrm{NiO} phase without additional reflections.

The Ni\mathrm{Ni}–Ni\mathrm{Ni} distances and coordination numbers differ from those of layered Ni(OH)2\mathrm{Ni(OH)}_{2}, confirming that hydroxylation modifies only the first coordination shell while leaving the medium-range NiO\mathrm{NiO} lattice intact. This interpretation is consistent with the DFT results, which show that H incorporation locally perturbs the vacancy environment, reduces the Ni3+\mathrm{Ni}^{3+} character around hydroxylated vacancies, and removes the deep divacancy-related in-gap states without reconstructing the octahedral framework. Importantly, this local passivation mechanism does not imply the full elimination of Ni3+\mathrm{Ni}^{3+} species in the real film, as experimentally observed by Ni L-edge(Figure 3m); instead, it reflects the electronic restructuring that occurs specifically at hydroxylated sites. Thus, the structural response to hydroxylation is best described as localized Ni\mathrm{Ni}–O\mathrm{O}–H disorder embedded within a largely preserved NiO\mathrm{NiO} lattice, rather than a phase transition toward bulk Ni(OH)2\mathrm{Ni(OH)}_{2}.

Operando Ni K-edge XANES of the h-NiO film (Figure 3l) demonstrates that the material undergoes a clear, potential-driven oxidation even without prior conditioning. Holding the electrode for 30 min at 1.3 V produces a spectrum characteristic of predominantly Ni2+\mathrm{Ni}^{2+} in a hydroxide-like environment. Increasing the potential to 1.6 V for another 30 min produces a distinct positive edge shift, marking the onset of Ni3+\mathrm{Ni}^{3+} formation. At 1.8 V for 30 min, the edge shift grows to ~1.9 eV relative to the as-prepared h-NiO sample, consistent with the establishment of the γ\gamma-NiOOH electronic structure. Notably, this potential-dependent evolution is significantly sharper than in our previous operando study10, indicating that predefined Ni\mathrm{Ni}–O\mathrm{O}–H environments facilitate a more efficient structural and electronic reorganization under anodic polarization.

Beyond the Ni K-edge analysis, complementary O K-edge and Ni L-edge X-ray absorption measurements provide further insight into how oxygen-rich and hydroxylation modulate the electronic structure of NiO and h-NiO. Together, these absorption edges govern transitions into the unoccupied 3d3d electronic states that are essential for understanding OER catalysis.

The O K-edge spectra of the three representative samples (Figure 3n) show how vacancies and hydroxylation modify the unoccupied O 2p2p–Ni 3d3d manifold. The stoichiometric-like 1% O2\mathrm{O}_{2} film closely resembles the NiO reference, with a weak pre-edge at ~529 eV, consistent with a predominantly Ni2+\mathrm{Ni}^{2+}–O2−\mathrm{O}^{2-} octahedral environment and limited hole density. This NiO-like configuration is further supported by its Ni L-edge spectrum, which also matches the reference.

In the 88% O2O_2 film, the pre-edge intensity increases and broadens toward ∼529\sim529–530 eV. Similar enhancements in Ni oxides have been associated with ligand-hole formation driven by Ni vacancies (Ni3+Ni^{3+}–O−O^- configurations) and enhanced Ni 3d3d–O 2p2p covalency80,81. However, in our case, the Ni L-edge does not show sharply resolved Ni3+Ni^{3+} multiplet features, indicating that any Ni3+Ni^{3+} population remains below the sensitivity of this measurement or is partially delocalized, consistent with our DFT results, which show that isolated vacancies introduce delocalized holes rather than fully localized Ni3+Ni^{3+} centers. In contrast, higher vacancy densities enhance hybridization and redistribute 3d/2p3d/2p spectral weight near the valence band edge. Thus, the increased pre-edge intensity in the 88% O2O_2 film reflects a combination of vacancy-induced Ni 3d3d–O 2p2p hybridization, partially delocalized ligand-hole character, and local symmetry distortions around vacancies, with none of these contributions dominating exclusively.

The hydroxylated h-NiO film (h-NiO, 88% O2O_2 + 0.3% H2OH_2O) also displays an enhanced pre-edge, but with subtle differences in line shape. DFT predicts that OH groups bind preferentially at vacancy-adjacent O sites, partially compensating Ni3+Ni^{3+}-like environments and suppressing the deep in-gap states present in the divacancy configuration, restoring more Ni2+Ni^{2+}-like character locally while introducing additional Ni–O–H hybridization in the unoccupied states. Experimentally, this is reflected in the O K-edge by a preserved pre-edge intensity (indicating that vacancy-induced hybridization is not eliminated) and by the Ni L-edge, which shows an increased shoulder near ∼855.5\sim855.5 eV and increased L2L_2-edge intensity. These features indicate that ligand-hole character persists at non-hydroxylated regions even as hydroxylation locally alters the vacancy environment.

Together, the O K-edge, Ni L-edge, and DFT results indicate a heterogeneous defect landscape: oxygen-rich growth enhances Ni 3d3d–O 2p2p hybridization and generates partially delocalized ligand-hole states; hydroxylation locally compensates some vacancy-induced Ni3+Ni^{3+}-like configurations while preserving significant hybridization in the unoccupied manifold. The observed pre-edge evolution across the series, therefore, reflects variations in covalency, symmetry distortion, and vacancy compensation mechanisms, rather than mutually exclusive spectral origins.

Plasma diagnostics (Figure S4) by optical emission spectroscopy (OES) provide context for these structural trends. The Ar/O2O_2 discharge used for NiO deposition exhibits Ar+Ar^+ and oxygen-ion emission features82,83, consistent with an oxidizing environment that favors Ni-vacancy formation. In contrast, the Ar/O2O_2/H2_2O plasma contains additional H emission signatures associated with partial water dissociation84, aligning with the incorporation of Ni–O–H coordination environments detected by XPS. Although OES does not resolve all reactive fragments formed in the discharge, the distinction between oxygen-rich and H-containing plasmas corresponds directly to the defect chemistries extracted from DFT and spectroscopy–vacancy-rich growth under Ar/O2O_2 and hydroxylated surfaces under Ar/O2O_2/H2OH_2O. Full plasma diagnostic analysis is provided in the Supplementary Information.

Figure S4. Optical emission spectra of the Ar, Ar+O₂, and Ar+O₂+H₂O plasmas

It is important to note that the apparent differences between XRD, EXAFS, and TEM reflect the distinct length scales probed by each technique. XRD reveals substantial modifications in crystallite size, texture, and long-range ordering as a function of plasma composition, whereas EXAFS shows that the local NiO6NiO_6 octahedral environment remains largely preserved. TEM/SAED confirms this picture: the rock-salt phase persists, although medium-range disorder and strain–clearly visible in XRD peak broadening–are not resolved in SAED. Thus, the films undergo significant long-range structural evolution without altering their fundamental local NiO coordination.

Electrochemical Analysis

The oxygen evolution activity of NiO and hydroxylated NiO (h-NiO) thin films was systematically compared as a function of O2O_2 and H2OH_2O content during deposition (Figure 4). In previous studies[5] [17, 10, 16] we have used extensive electrochemical cycling (>1000>1000 CV cycles) to convert the surface into Ni(OH)2Ni(OH)_2, facilitating the formation of the subsequently NiOOH. In contrast, the intentional incorporation of H2OH_2O during plasma deposition introduces hydroxyl groups into the films, reducing the need for such long conditioning. Here, only 200 CV cycles between 1.0-1.5 V (vs RHE) were sufficient to precondition the surface for the samples studied, followed by 60 min chronoamperometry (CA) at 1.5 V (vs RHE) to stabilize NiOOH as the active phase in OER. The overpotential at 10 mA cm−2^{-2}, Tafel slopes, and turnover frequency (TOF) were used as descriptors of intrinsic activity and correlated with the defect chemistry and electronic structure modifications described in § 2.2–§ 2.4.

Figure 4. OER activity of NiO thin films as a function of O2O_2 and H2OH_2O content during deposition, highlighting that moderate hydroxylation facilitates the NiOOHNiOOH formation and optimizes reaction kinetics, while excessive hydroxylation reverses performance. (a) Polarization curves for films deposited under different O2O_2 concentrations (1.0%, 20%, 66%, 88%) and with 0.3% H2OH_2O. (b) Polarization curves of the same films after extended conditioning (200 CV cycles between 1.0-1.5 V vs RHE + 60 min chronoamperometry at 1.5 V), where NiOOHNiOOH is stabilized on the surface. (c) Tafel plots derived from (b), showing optimal activity at intermediate O2O_2 levels and further enhancement by hydroxylation (slope ~19.1 mV dec−1^{-1}). (d–f) Effect of H2OH_2O incorporation (0.03%, 0.3%, 11.6%), where moderate hydroxylation improves OER activity, while excessive hydroxylation decreases performance. (g) TOF and TOF × (Q/A) values extracted at 1.5 V vs RHE for representative samples (1.0 % O2O_2, 88 % O2O_2, 88 % O2O_2 +0.3% H2OH_2O). The 88% O2O_2 sample exhibits the highest nominal TOF. The hydroxylated film shows a slightly higher redox charge (Q/A) but a marginally lower TOF×(Q/A), indicating that hydroxylation increases the number of electrochemically addressable Ni sites without improving their intrinsic turnover. Nevertheless, the hydroxylated sample achieves the fastest per-site kinetics, reflected by its lowest Tafel slope. (h) Isolated Ni2+/Ni3+Ni^{2+}/Ni^{3+} oxidation wave used for charge integration (Q) to determine the electrochemically active Ni population.

Effect of the Oxygen and H2OH_2O Concentration in the plasma discharge on the OER.

NiO films grown under low O2O_2 content (1.0%) exhibit higher overpotentials and a larger Tafel slope (34.5 mV dec−1^{-1}) (Figure 4a-Figure 4c), which we attribute to the absence of pre-stabilized Ni3+/O−Ni^{3+}/O^{-} ligand-hole states, following our rationale established by our previous observations and calculations. Increasing the O2O_2 fraction to 20% significantly reduces the slope to 31.4 mV dec−1^{-1}, reflecting slightly accelerated kinetics, which we correlate to higher Ni vacancy densities and shallow acceptor states that enhance Ni–O covalency and shift the valence band closer to the Fermi level (Sections 2.3-2.4). At 66% O2O_2, the slope is further decreased (16.8 mV dec−1^{-1}), indicating faster kinetics, whereas further increasing the O2O_2 content to 88% reverses the performance to 19.8 mV dec−1^{-1}. Since lower Tafel slopes correspond to faster intrinsic reaction kinetics85–87, these results highlight that an intermediate O2O_2 regime (20-66%) was optimal for stabilizing vacancy-derived ligand-hole character and enhanced Ni–O covalency, which facilitates improved OER kinetics. Similar behavior has been reported in NiO thin films, where excessive oxygen incorporation introduces a high defect density, enhancing carrier scattering and reducing hole mobility, ultimately increasing resistivity and degrading the performance of NiO films88.

The introduction of H2OH_2O vapor during deposition provided an additional pathway to tailor the OER activity. For the samples studied, films grown with 0.3% H2OH_2O exhibited the highest OER activity, with a Tafel slope of 19.1 mV dec−1^{-1} and reduced overpotentials compared to oxygen-only samples (Figure 4c). Since the electrochemical surface area decreases with H2OH_2O addition (Figure S5)—compared to its counterpart sample prepared only with 88% O2O_2—this improvement cannot be ascribed to geometric effects but rather to changes in the electronic structure. Moderate hydroxylation introduces mixed Ni–O–H coordination environments and increases first-shell disorder without significantly altering the average Ni–O bond distance (§ 2.4). These local structural perturbations generate shallow Ni–O–H–derived tail states near the valence band edge (§ 2.3), which facilitate charge transfer and accelerate the NiO→Ni(OH)2→NiOOH\mathrm{NiO} \to\mathrm{Ni(OH)}_2 \to\mathrm{NiOOH} transition during electrochemical conditioning. At higher H2OH_2O content (11.6%), the Tafel slope increased again to 24.9 mV dec−1^{-1}, consistent with excessive hydroxylation increasing disorder and reducing hole mobility.

Electrochemical Active Surface Area plot for thin films prepared with different oxygen concentrations and with 0.3% H₂O

Figure S5. Electrochemical Active Surface Area (ECSA) obtained for thin films prepared with different oxygen concentrations and with 0.3% H₂O

Overall, the Tafel slopes of NiO and h-NiO (16–35 mV dec−1^{-1}) fall within the low-slope regime predicted by microkinetic analyses 86 and frequently reported for fast alkaline OER kinetics 87, corresponding to ~RT/3F–~RT/2F. Such low slopes have been associated with lattice-oxygen participation in Ni-based oxides 89, although they are not, by themselves, definitive mechanistic proof. In oxygen-rich films, increased Ni-vacancy concentration promotes stronger Ni–O covalency and O-centered ligand-hole character, consistent with DFT-predicted Ni3+\mathrm{Ni}^{3+}–O−^{-} configurations. In contrast, hydroxylated films achieve rapid kinetics not through an increase in the vacancy-induced Ni3+\mathrm{Ni}^{3+}–O−^{-} ligand-hole density, which is suppressed by hydroxyl incorporation, but through accelerated NiO→Ni(OH)2→NiOOH\mathrm{NiO} \to\mathrm{Ni(OH)}_2 \to\mathrm{NiOOH} transformation during conditioning. Thus, nickel vacancies modulate the intrinsic electronic structure, whereas hydroxylation modulates the chemical activation pathway, yielding surfaces that behave as pre-activated catalysts with enhanced OER activity 10,17. The improved OER performance reflects the interplay between vacancy-induced covalency and hydroxylation-mediated NiOOH formation.

To quantitatively evaluate the intrinsic catalytic activity of NiO and h-NiO, the TOF was calculated following the convention established for Ni-based OER catalysts in alkaline media—in which the number of active sites is derived from the Ni2+/Ni3+\mathrm{Ni}^{2+}/\mathrm{Ni}^{3+} oxidation charge, obtained by integrating the anodic Ni2+→Ni3+\mathrm{Ni}^{2+} \to\mathrm{Ni}^{3+} peak, and converting this charge (Q) into moles of electrochemically accessible Ni sites via Nsite=Q/FN_{\mathrm{site}} = Q/F, assuming a one-electron Ni2+→Ni3+\mathrm{Ni}^{2+} \to\mathrm{Ni}^{3+} transition—and each evolved O2O_2 molecule corresponds to a four-electron process 90,91. The relationship between the measured current density and the number of electrochemically active Ni sites involved in the OER is expressed by equation 1.

TOF=jA4FNsite(1)\mathrm{TOF} = \frac{jA}{4FN_{\mathrm{site}}} \tag*{(1)}

where jj is the steady-state current density (A cm−2^{-2}) at 1.5 V vs RHE, A is the geometric area (cm2^2), F is Faraday's constant, and NsiteN_{\mathrm{site}} is the number of electrochemically active Ni sites estimated from the anodic charge associated with the Ni2+/Ni3+\mathrm{Ni}^{2+}/\mathrm{Ni}^{3+} redox transition in the cyclic voltammogram. Because O2\mathrm{O}_2 evolution involves the transfer of four electrons, the denominator (4F4F) converts total charge into mol O2\mathrm{O}_2 s−1^{-1} cm−2^{-2}. To facilitate comparison between samples and to account for variations in the electrochemically accessible Ni population, the TOF was also scaled by the redox charge per geometric area (Q/A). This charge-normalized quantity (TOF ×\times Q/A) reflects the effective turnover rate per unit area by combining the intrinsic per-site activity with the experimentally accessible Ni-site population extracted from the Ni2+/Ni3+\mathrm{Ni}^{2+}/\mathrm{Ni}^{3+} redox transition.

The resulting TOF values of 0.011 s−1^{-1} (1.0 % O2\mathrm{O}_2), 0.032 s−1^{-1} (88 % O2\mathrm{O}_2), and 0.012 s−1^{-1} (88 % O2\mathrm{O}_2 + 0.3% H2O\mathrm{H}_2\mathrm{O}) are presented in Figure 4g. As the oxygen concentration increased from 1.0% to 88%, the TOF increased by nearly a factor of four, consistent with the formation of vacancy-derived Ni3+/O−\mathrm{Ni}^{3+}/\mathrm{O}^{-} ligand-hole states under oxygen-rich deposition. As expected, the 1.0% O2\mathrm{O}_2 sample shows the lowest intrinsic turnover, whereas the 88 % O2\mathrm{O}_2 film exhibits the highest TOF due to its stronger ligand-hole character.

Upon controlled hydroxylation (88% O2\mathrm{O}_2 + 0.3% H2O\mathrm{H}_2\mathrm{O}), the nominal TOF decreases slightly relative to the oxygen-rich film; even when the redox charge Ni2+/Ni3+\mathrm{Ni}^{2+}/\mathrm{Ni}^{3+} redox charge (Q/A = 1.33 ×10−4\times10^{-4} C cm−2^{-2}) is somewhat larger compared to the 88 % O2\mathrm{O}_2 sample (1.26 ×10−4\times10^{-4} C cm−2^{-2}). Despite this, its charge-normalized activity (TOF ×\times Q/A = 0.00588) remains essentially the same as—and slightly lower than—that of the 88 % O2\mathrm{O}_2 film (0.00598), indicating that hydroxylation increases the number of electrochemically addressable Ni sites but does not enhance their intrinsic catalytic utilization. Because both samples display comparable Ni/O ratios (Figure S3), the differences in catalytic behavior do not reflect changes in the overall degree of Ni deficiency, but rather differences in how Ni vacancies are charge-compensated and coordinated locally. In the 88 % O2\mathrm{O}_2 film, a larger fraction of vacancies is compensated electronically via Ni3+\mathrm{Ni}^{3+} formation and O-centered ligand holes, stabilizing highly active Ni3+/O−\mathrm{Ni}^{3+}/\mathrm{O}^{-} configurations and yielding a higher intrinsic TOF. In contrast, H2O\mathrm{H}_2\mathrm{O} incorporation partially compensates vacancy-induced Ni3+\mathrm{Ni}^{3+} centers through local hydroxylation, forming Ni–O–H environments that facilitate faster electrochemical activation but reduce the intrinsic turnover per active site.

The TOF–Tafel behavior of the 88 % O2\mathrm{O}_2 film aligns with reports that Ni3+/O−\mathrm{Ni}^{3+}/\mathrm{O}^{-} ligand-hole configurations enhance lattice-oxygen-mediated OER pathways in Ni (oxy)hydroxides90. In contrast, hydroxylation reduces ligand-hole density and instead improves charge-transfer kinetics through Ni–O–H coordination, resulting in a lower Tafel slope despite a modestly reduced TOF and TOF×\times(Q/A).

Conclusion

This work demonstrates that plasma-assisted deposition provides deterministic control over the defect landscape and electronic structure of NiO, enabling rational preconditioning of its transformation into the NiOOH OER-active phase. Oxygen-rich growth generates isolated and clustered Ni vacancies that strengthen Ni–O covalency and stabilize Ni3+\mathrm{Ni}^{3+}–O−\mathrm{O}^{-} ligand-hole states, thereby enhancing lattice-oxygen participation and accelerating OER-relevant electronic configurations. In contrast, controlled H2OH_2O incorporation selectively compensates vacancy-induced Ni3+\mathrm{Ni}^{3+} centers, forming Ni–O–H environments that suppress deep divacancy-derived in-gap states while introducing shallow valence-band tails. These hydroxyl-driven modifications preserve the medium-range NiO lattice and promote rapid NiO →\to Ni(OH)2_2 →\to NiOOH activation, improving charge-transfer kinetics.

Although DFT is used here to interpret experimentally accessible plasma conditions rather than to prescribe growth parameters a priori, the resulting electronic-structure framework defines the defect and electronic descriptors required for extension toward predictive plasma-guided design. Specifically, we identify two complementary defect-engineering pathways in NiO: vacancy-driven tuning of intrinsic electronic structure and hydroxylation-driven tuning of activation chemistry. By decoupling these effects during synthesis, plasma processing enables access to catalytic states that are difficult to achieve through post-synthetic approaches. More broadly, the integrated plasma–DFT–spectroscopy framework established here provides generalizable design principles for programming defect chemistry in transition-metal oxides, extendable to CoO, LaNiO3_3, and layered or perovskite-type systems for developing robust, earth-abundant OER catalysts.

Methodology

Computational Details

First-principles calculations were performed within density functional theory (DFT) using the projector augmented-wave (PAW) basis set 25 as implemented in the Vienna Ab initio Simulation Package (VASP) 26. Exchange correlation effects are described by the Perdew–Burke–Ernzerhof functional revised for solids (PBEsol) 92. The PAW basis set treats Ni 3p63d84s23p^{6}3d^{8}4s^{2}, O 2s22p42s^{2}2p^{4}, and H 1s11s^{1} as valence electrons. Because PBEsol alone cannot adequately capture strong electron-electron correlations—particularly in Mott insulators such as NiO—we treat the Ni 3d3d states with the DFT+UU 27,28 method, applying an on-site Coulomb interaction U=4U=4 eV.

All calculations are spin-polarized, and type-II antiferromagnetic (AFM) order is imposed for all systems. A plane-wave kinetic-energy cutoff of 520 eV is used, and Brillouin-zone sampling employs Monkhorst-Pack meshes of 8×8×88 \times8 \times8 for the 1×1×11 \times1 \times1 cell and 3×3×33 \times3 \times3 for the 3×3×33 \times3 \times3 supercell containing vacancies.

Ionic relaxations proceed until the maximum residual force on any atom falls below 0.01 eV Å−1^{-1}.

Sample Preparation

Ni foils were used as the substrates. They were polished using 15 μm and 8 μm silicon carbide (Starcke, Struers) and 0.5 μm alumina paste (MicroPolish Alumina, Buehler). The substrates were cleaned sequentially in an ultrasonic bath with acetone (Carl Roth), isopropanol (Carl Roth), and Millipore water for seven minutes each, dried using nitrogen, and loaded into the deposition chamber, which is a UHV chamber containing a magnetron sputtering source from MeiVac (MAK 2") connected in vacuum to an X-ray Photoelectron Spectroscopy System. The chamber is part of the DAISY-FUN cluster tool (Darmstadt's Integrated System for Fundamental Research).

Before each deposition, the chamber was evacuated to a base pressure of 2⋅10−82 \cdot10^{-8} mbar. Ar and O2\mathrm{O}_2 gas flows were introduced and varied in the plasma discharge, having a working pressure of 3⋅10−23 \cdot10^{-2} mbar for the NiO thin film preparation. For h-NiO deposition, the water was enclosed in a Y-tube Pyrex glass, with a leak valve and needle valve to dose the water insertion into the deposition chamber. Water vapor was introduced in the 1.0 to 1.0⋅10−41.0 \cdot10^{-4} mbar range, measured by a capacitive gauge sensor that measures independently of gas type and concentration. The partial pressures of O2\mathrm{O}_2 and H2O\mathrm{H}_2\mathrm{O} can be estimated using equations 2 and 3, respectively. The working parameters used for NiO and h-NiO deposition for different thicknesses, O2\mathrm{O}_2 concentrations, and H2O\mathrm{H}_2\mathrm{O} concentrations are summarized in Tables S1, S2, and S3.

O2%=fO2fO2+fAr∗100(2)\mathrm{O}_2\% = \frac{f_{\mathrm{O}_2}}{f_{\mathrm{O}_2}+f_{\mathrm{Ar}}} \ast100 \tag*{(2)}
H2O%=PH2O−PbasePworking∗100(3)\mathrm{H}_2\mathrm{O}\% = \frac{P_{\mathrm{H}_2\mathrm{O}}-P_{\mathrm{base}}}{P_{\mathrm{working}}} \ast100 \tag*{(3)}

Where fO2f_{\mathrm{O}_2} and fArf_{\mathrm{Ar}} are oxygen and argon gas flow rates, respectively, PH2OP_{\mathrm{H}_2\mathrm{O}} is water vapour pressure, PbaseP_{\mathrm{base}} is the base pressure, and PworkingP_{\mathrm{working}} is the working pressure.

For h-NiO thin films, the thickness is limited to 15 nm because the deposition rate is reduced considerably due to the reaction of H2O\mathrm{H}_2\mathrm{O} with the target erosion zone, leading to the formation of a less conductive oxide layer at the surface of the metallic nickel and a strong decrease of the target voltage associated with a reduction of the deposition rate. The same phenomenon is expected with higher oxygen concentrations, but in a reduced manner38. Too much water vapor (≫5⋅10−3\gg5 \cdot10^{-3}) also saturates the turbomolecular pump, leading to pumping failure.

Atomic Force Microscopy

The morphology and surface roughness of the NiO and h-NiO films were evaluated using a Bruker Dimension ICON AFM. The cantilever (type PPP-FMAuD-10, Nanosensors) was made of silicon and coated with gold on the detector side. It has a resonance frequency of 45-115 kHz, a force constant of 0.5-9.5 N/m2^2, and a 10-15 μ\mum tip height. During the analysis, the cantilever tip was brought near the center of the sample's surface. Using the Nanoscope Analysis 1.8 software, the tip was positioned in a region where the film was relatively flat and free from abrasions. The scan was done in a tapping mode using the optimum oscillation frequency while recording the image. The images were processed using NanoScope 9.3 software. The plane fit command was initially used to remove image distortions. It computes a single-order polynomial in the image and subtracts it from the image.93 This was followed by the Flatten command, which removes tilt and low-frequency noise from the image.94.

Grazing-Incidence Wide-Angle X-ray Scattering (GIWAXS)

Grazing-Incidence Wide-Angle X-ray Scattering (GIWAXS) was carried out on a Rigaku Smartlab (Cu KαK_{\alpha} radiation) diffractometer in a grazing incidence setup with θsource=0.3∘\theta_{\mathrm{source}} = 0.3^\circ. Data were recorded between 5∘5^\circ and 90∘90^\circ (in units of 2θ2\theta) using a step size of 0.01∘0.01^\circ. This Analysis is limited to a 100 nm NiO thin film since a minimum film thickness is required to generate an observable diffraction signal. Hence, no data is available for the 15 nm h-NiO sample.

Electrochemical Measurements

Electrochemical measurements were conducted in a three-electrode setup in a PECC-2 cell (Zahner-Elektrik GmbH & Co. KG) filled with 1 M KOH (Carl Roth). The NiO sample served as the working electrode, which was in contact with a gold-coated plate connected to the back of the cell. The sample was sealed using a rubber gasket with an internal diameter of 8 mm, corresponding to the film's geometric area exposed to the electrolyte. A Hg/HgO (1 M KOH) and a Pt wire were used as the reference and counter electrodes, respectively. Before any electrochemical measurements, the Hg/HgO reference electrode was calibrated versus a reversible hydrogen electrode (RHE, HydroFlex-Gaskatel).

The samples were exposed to 200 cyclic voltammograms (CV), cycles from 1.0 to 1.5 V (vs. RHE) with a scan rate of 100 mV/s to transform the NiO surface to Ni(OH)2\mathrm{Ni(OH)_2}. After this activation treatment, 5 CVs were recorded from 1.0 to 1.9 V (vs. RHE) at a scan rate of 50 mV/s to verify the OER current density. After that, chronoamperometry (CA) measurement was done at 1.5 V (vs. RHE) for one hour to oxidize the Ni(OH)2\mathrm{Ni(OH)_2} into NiOOH\mathrm{NiOOH}. When the CA was finished, an additional 5 CVs from 1.0 to 1.9 V (vs. RHE) were recorded. The charge (Q) to calculate the n active sites was extracted from the oxidation wave of these scans.

X-Ray Photoelectron Spectroscopy (XPS)

X-ray photoelectron spectroscopy (XPS) spectra were acquired using a SPECS PHOIBOS 150 spectrometer implemented at the DAISY-FUN cluster tool. It is equipped with an Al KαK_{\alpha} X-ray source (monochromatic Focus 500 with XR50 M (SPECS), hν=1486.74h\nu= 1486.74 eV). Survey and detail spectra were measured in fixed analyzer transmission mode while choosing a pass energy of 20 eV (step size of 0.5 eV) for the survey and 10 eV (step size of 0.05 eV) for the core levels. The system was calibrated to 0.00 eV binding energy of the Fermi level of sputter-cleaned Au and Cu, as well as to the emission lines of metallic Au 4f7/24f_{7/2} at 83.98 eV, Ag 3d5/23d_{5/2} at 368.26 eV, and Cu 2p3/22p_{3/2} at 932.67 eV binding energy with deviations ≤0.1\le0.1 eV. The data analysis was performed with CasaXPS, version 2.3.22.95 The core level spectra were fitted with a Shirley background and peaks of a GL(30) line shape. Intensity calculations were done based on relative sensitivity factors published by Scofield.96

Optical Emission Spectroscopy

The plasma was analyzed by optical emission spectroscopy using an OceanOptics spectrometer USB4000 in the UV-Vis range (200-1100nm). Once the desired gas flow (Ar, O2_2, Ar/O2_2, Ar/O2_2/H2_2O) was introduced into the plasma discharge, the emission spectra were recorded using OceanView 2.0 software and then processed and analyzed using OriginLab.

Hard X-ray Absorption Spectroscopy–EXAFS Analysis and Fitting Procedure

EXAFS measurements were performed in transmission mode for the ex-situ sample characterization and in fluorescence mode for the operando characterization at the B18 beamline of the Diamond Light Source (Didcot, UK) during experiment SP38607–1, data set Ni_NiO, Ni_h-NiO, and Ni_NiO_insitu. Samples were analyzed at the Ni K-edge (8333.5 eV) (For technical specifications, verify the official B18 End station at the Diamond website97). A Si crystal cut along the (111) plane was used as the monochromator. Energy calibration was carried out using a metallic Ni foil as the reference standard. Pt-coated mirrors were used to suppress harmonic contributions98.

EXAFS data were reduced using the Demeter package 0.9.2699, and fits of the k2k^2-weighted data were performed in R-space using theoretical functions generated with the FEFF6 code79. To calculate the phases and amplitudes of the Feynman paths, a cubic rock-salt NiO CIF was employed100. For each sample, the first Ni-O and the second Ni-Ni shells were included. For each path, the initial fitting parameters were the mean-square disorder in the neighbor distances σ2\sigma^2 and the interatomic distances r. A common value of energy shift E0E_0 relative to the theoretical value was included, and to account for occupancy effects, the amplitude reduction of S02S_0^2 was also refined. The data were Fourier transformed over k = 2.5 – 13 Å−1^{-1} and back-transformed over R = 1 – 3.3 Å. A Hanning window was used in both transformations (default values: dk = 1.0 and dR = 0.0). Fitting was performed in both k- and R-space using the ranges specified in the Artemis reports, and employing k-weights of 1, 2, and 3 simultaneously. For both samples, the number of fitted parameters was kept below the number of independent points reported by Artemis for the selected k- and R-ranges, according to the Stern rule101.

Soft X-ray Absorption Spectroscopy

Ni L-edge and O K-edge spectra were measured in a high vacuum setup at the ISISS beamline of the German synchrotron facility BESSY II. All spectra were recorded in total electron yield (TEY) mode, which was collected from the analyzer nozzle of an XPS detector. The analyzer nozzle was closely aligned to the sample and biased to 90 V against it to increase the signal-to-noise ratio. The storage ring was operated in low alpha and decay mode with a maximum ring current of 8 mA. Measurements were performed on three different spots per sample, and for each sample position, two consecutive spectra per element were measured. The spectra were normalized to the mirror current. It has to be noted that the energy resolution at the Ni L2,3_{2,3}edge was low for the presented measurements due to the special operation mode of the storage ring. Therefore, the spectral shape differs from NiO spectra typically found in modern literature. Nevertheless, when comparing the spectra taken on the samples to a reference spectrum of NiO taken at identical settings, qualitative changes can still be interpreted. As a reference sample, we have used NiO powder (Sigma Aldrich). Spectra of α/β-Ni(OH)2_2 synthesized with a hydrothermal approach were taken from a previous beamtime.

Transmission Electron Microscopy (TEM)

For the TEM measurements, the thin films were deposited on Cu grids. The TEM analysis was done using a JEOL JEM F2100 TEM equipped with an EDS detector (X-Max 80 SDD-Detektor, Oxford).

Associated Content

Research data supporting Figures and Tables in the main text and supplementary information is made available via ZENODO.org under DOI: XXX.XXX.XXX (made available after acceptance).

Author Contributions

H.M.F.: Writing – original draft, Coordination, Methodology, Conceptualization, Sample preparation, XPS collection, hard XAS collection, soft XAS analysis, Electrochemical Investigation and Analysis. M.A.: DFT simulations and Analysis, Writing. C.Jr.M.: XPS collection, AFM collection, XRD collection, investigation and Analysis, Writing. A.T.: hard-XAS data validation and Analysis, Writing. G.W. and M.T.: Soft-XAS collection, investigation, and Analysis, Writing. E.A.: HRTEM collection and Analysis. T.A.K.: hard-XAS collection. C.C.: XAS data validation and Analysis. L.M.L.: Funding acquisition. J.P.H.: Funding acquisition. All authors participate in the proofreading.

Conflicts of interest

There are no conflicts to declare.

Acknowledgments

H.M.F. G.W., M.F.T., and J.P.H. acknowledge the German Ministry of Research, Technology, and Space (BMFTR) for providing financial support within the H2Giga cluster project PrometH2eus (Fkz: 03HY105H and 03HY105E). M. A. acknowledges financial support from the Collaborative Research Center FLAIR (Fermi level engineering applied to oxide electroceramics), funded by the German Research Foundation (DFG) under Project-ID No. 46318420 −SFB 1548 (subproject A02). E.A., and L.M.L. acknowledge the financial support of DFG in the framework of the Collaborative Research Center Transregio 270 (CRCTRR 270) project No. 405553726 (subproject Z01). H.M.F. thanks Diamond Light Source for allocating beamtime SP38607–1 at the beamline B18. H.M.F. G.W., and M.F.T. acknowledge the allocation of synchrotron radiation beamtime at the ISISS beamline at the BESSY II electron storage ring. G.W. and

M.F.T. thank Axel Knop-Gericke and Detre Teschner for support during the beamtime. M.A. and H.A. thank Marcus Ekholm from the Theoretical Physics Division at Linköping University for his discussions on the calculations. M.A. thanks the Paderborn Supercomputing Center for allocating time for the calculations.

Graphical abstract

Graphical abstract showing DOS plots for almost stoichiometric NiO, NiO with 2 Ni vacancies, and NiO with 2 Ni vacancies and H2O; the transformation from NiO to h-NiO in the presence of O₂+H₂O; and TOF and TOF*Q/A values

Figure 5.

Corresponding authors

Harol Moreno Fernández – [email protected]

Mohammad Amirabbasi – [email protected]

Jan P. Hofmann – [email protected]

Plasma Diagnostics

The optical emission spectra (OES) for the Ar/O2\mathrm{O_2} and Ar/O2\mathrm{O_2}/H2O\mathrm{H_2O} gas mixtures are shown in Figure S5, with peak assignments based on the NIST Atomic Spectra Database[1]. The discharge used for NiO deposition (Ar/O2\mathrm{O_2}) is dominated by Ar+\mathrm{Ar^+} emission and oxygen-derived species assignable to O+\mathrm{O^+}, O2+\mathrm{O_2^+}, and O3+\mathrm{O_3^+}, indicating an oxidizing plasma environment with a relatively high oxygen chemical potential. In contrast, the plasma used to grow h-NiO exhibits additional H+\mathrm{H^+} emission features, consistent with partial dissociation of water in the discharge. Although OES does not detect all fragments produced from H2O\mathrm{H_2O} dissociation, the formation of ionic and radical species such as OH−\mathrm{OH^-}, OH˙\dot{\mathrm{OH}} and H˙\dot{\mathrm{H}} in similar plasmas is well documented[2, 3, 4, 5, 6].

These reactive fragments interact with the surface during growth and are consistent with the incorporation of Ni–O–H coordination environments detected by XPS. The films remain polycrystalline under all plasma conditions, as confirmed by XRD/TEM. While EXAFS confirms that the medium-range NiO-like structure is preserved, it cannot resolve grain size or long-range ordering, and, owing to the fixed coordination numbers used during fitting, EXAFS is not sensitive to the exact concentration of Ni vacancies. XPS identifies mixed surface environments containing Ni2+\mathrm{Ni^{2+}}–O, Ni3+\mathrm{Ni^{3+}}–O−\mathrm{O^-}, and Ni–O–H species, consistent with the defect-rich surface chemistry expected from plasma-grown NiO and h-NiO films.

The differences in plasma composition correlate with the defect chemistry extracted from DFT and spectroscopy. The more oxidizing Ar/O2\mathrm{O_2} discharge supports the formation of isolated and clustered Ni vacancies, producing oxygen-ligand-hole states and, at higher vacancy density, localized Ni3+\mathrm{Ni^{3+}}–O−\mathrm{O^-} configurations. Conversely, hydrogen-containing species in the Ar/O2\mathrm{O_2}/H2O\mathrm{H_2O} discharge contribute to surface hydroxylation, compensate vacancy-induced Ni3+\mathrm{Ni}^{3+}, and suppress the divacancy-related in-gap states predicted by DFT. These effects lead to a defect landscape consistent with XPS, VB, and EXAFS observations. They may contribute to the enhanced OER activity observed in h-NiO films, alongside improved electrochemical activation kinetics.

References

  1. [1]NIST: Atomic Spectra Database Lines Form. https://physics.nist.gov/PhysRefData/ASD/lines_form.html.
  2. [2]Ueta, H. et al. Ni Oxyhydroxide Thin Films Prepared by Reactive Sputtering Using O₂ + H₂O Mixed Gas. Jpn. J. Appl. Phys. 48, 015501 (2009).DOI
  3. [3]Abe, Y., Yamauchi, S., Kawamura, M., Kim, K. H. & Kiba, T. High-rate sputter deposition of electrochromic nickel oxide thin films using substrate cooling and water vapor injection. Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films 36, 02C102 (2018).DOI
  4. [4]Yokoiwa, Y., Abe, Y., Kawamura, M., Kim, K. H. & Kiba, T. Metallic-mode reactive sputtering of nickel oxide thin films and characterization of their electrochromic properties. Jpn. J. Appl. Phys. 58, 055504 (2019).DOI
  5. [5]Teolis, B. D., Vidal, R. A., Shi, J. & Baragiola, R. A. Mechanisms of O₂ sputtering from water ice by keV ions. Phys. Rev. B 72, 245422 (2005).DOI
  6. [6]Green, S. V. et al. Electrochromic properties of nickel oxide based thin films sputter deposited in the presence of water vapor. Thin Solid Films 520, 3839–3842 (2012).DOI

Paper details

vlnc:W_cteyedud
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents