betaFeedback

WorksPhysics and Astronomy

Superior Photo-carrier Diffusion Dynamics in Organic-inorganic Hybrid Perovskites Revealed by Spatiotemporal Conductivity Imaging

Abstract

The outstanding performance of organic-inorganic metal trihalide solar cells benefits from the exceptional photo-physical properties of both electrons and holes in the material. Here, we directly probe the free-carrier dynamics in Cs-doped FAPbI3 thin films by spatiotemporal photoconductivity imaging. Using charge transport layers to selectively quench one type of carriers, we show that the two relaxation times on the order of 1 microsecond and 10 microseconds correspond to the lifetimes of electrons and holes in FACsPbI3, respectively. Strikingly, the diffusion mapping indicates that the difference in electron/hole lifetimes is largely compensated by their disparate mobility. Consequently, the long diffusion lengths (3 ~ 5 micrometers) of both carriers are comparable to each other, a feature closely related to the unique charge trapping and de-trapping processes in hybrid trihalide perovskites. Our results unveil the origin of superior diffusion dynamics in this material, crucially important for solar-cell applications.

Introduction

Organic-inorganic lead trihalide perovskite solar cells (PSCs) have been in the limelight of photovoltaic research[1, 2, 3], as exemplified by the outstanding certified power conversion efficiency (PCE) that exceeds 25% to date[4]. Even in the polycrystalline form, the PSC thin films exhibit many remarkable photo-physical properties, such as high absorption coefficient[5], long carrier lifetimes[6], and low impurity scattering rate[7, 8]. For photovoltaic applications, a particularly attractive feature of hybrid perovskites is that both electrons and holes are active in the photoconduction process[6, 7, 8, 9, 10]. From the theoretical point of view, the two types of carriers are expected to exhibit comparable effective mass, intrinsic mobility, recombination lifetime, and diffusion length[11, 12, 13]. In real materials, however, the balance between electrons and holes is usually broken by thin-film deposition conditions, defect structures, ionic disorders, and other sample-dependent parameters[14, 15, 16, 17], which may affect the photo-carrier extraction in functional devices. A thorough understanding of the dynamics of individual charge carriers is thus imperative for continuous improvements of PSC performance towards commercial applications.

The spatiotemporal dynamics of electrons and holes in optoelectronic materials are widely studied by optical measurements such as time-resolved photoluminescence (TRPL) and transient absorption spectroscopy (TAS)[8, 9, 10, 18, 19]. The diffusion length can then be deduced by fitting the results to a diffusion model[8, 9, 10]. It should be noted that TRPL and TAS probe optical excited states and are often dominated by transitions with large oscillator strength. In contrast, the transport of photo-excited carriers is electrical and quasi-static in nature. In order to directly evaluate photoconduction, it is common to measure the photocurrent across electrical contacts, such as scanning photocurrent microscopy (SPCM)[16, 20, 21]. The spatial resolution of SPCM is diffraction-limited and the temporal response is dominated by the carrier transit time and extrinsic metal-semiconductor Schottky effect. In recent years, noncontact methods such as time-resolved microwave conductivity (TRMC)[6, 7, 16, 22, 23, 24, 25] and time-resolved THz spectroscopy (TRTS)[17, 26] are developed to probe the photo-carrier dynamics. These far-field techniques, however, do not offer spatially resolved information such as diffusion patterns.

In this article, we directly probe free-carrier diffusion dynamics in Cs-doped formamidinium lead trihalide (FACsPbI3\mathrm{FACsPbI}_{3}) thin films by laser-illuminated microwave impedance microscopy (iMIM), a unique optical-pump-electrical-probe technique with 20-nm spatial resolution and 10-ns temporal resolution for the electrical detection[27]. The steady-state iMIM experiment addresses the most important photophysical process in solar cells, i.e., the transport of photo-generated mobile carriers under the continuous illumination of ~ 1 Sun. The time-resolved iMIM (tr-iMIM) experiment detects the free-carrier lifetime that is also highly relevant for photoconduction. By depositing a hole or electron transport layer (HTL/ETL) underneath FACsPbI3\mathrm{FACsPbI_3}, we show that the two decay constants in tr-iMIM measurements are associated with the lifetimes of electrons and holes. The spatiotemporal imaging allows us to determine the diffusion coefficients, steady-state carrier density, and mobility of individual carriers. Interestingly, while the lifetime and mobility of electrons and holes differ substantially, their products and thus the diffusion lengths are comparable to each other, which is likely due to the unique defect structures and charge trapping events in PSC thin films. Our results highlight the origin of nearly balanced diffusion dynamics of electrons and holes in hybrid trihalide perovskites, which is highly desirable for photovoltaic applications.

Results

The PSC thin film in this study, hereafter labeled as Sample A, is 5% Cs-doped formamidinium (FA) lead triiodide deposited on cover glasses (see Methods). Compared with methylammonium (MA) based perovskites, FAPbI3\mathrm{FAPbI_3} exhibits superior stability at elevated temperatures and an ideal band gap for sunlight absorption[28]. The Cs-doping further stabilizes the room-temperature photo-active α\alpha-phase by reducing the Goldschmidt tolerance factor[29, 30, 31, 32]. Perovskite films were deposited using the typical anti-solvent-assisted spin-coating procedure. The samples were then capped by spin-coating 15 mg⋅ml−1\mathrm{mg \cdot ml^{-1}} PMMA (Mw ~ 120,000) film in chlorobenzene solution. For iMIM measurements, we chose a film thickness of d=250d = 250 nm that is greater than the absorption length, such that light is fully absorbed, but much less than the carrier diffusion length, such that the photoconductivity is uniformly distributed in the vertical direction within the relevant time scale in our experiment. External quantum efficiency (EQE) spectra were also measured (Supplementary Figure 1), showing good photoresponse across the solar spectrum. PSC devices made from the same material but with thicker film (550 nm) demonstrated a PCE above 20% under the standard Air Mass (AM) 1.5 illumination (Supplementary Figure 1).

Standard AM1.5 solar cell device performance: (a) I–V characteristics and (c) external quantum efficiency spectra

Supplementary Figure 1. Standard AM1.5 solar cell device performance. (a) I-V characteristics of the solar cell device made from the 550-nm-thick FA0.95Cs0.05PbI3\mathrm{FA}_{0.95}\mathrm{Cs}_{0.05}\mathrm{PbI}_{3} thin films. (b) Table of the device parameters, listing the short-circuit current density JscJ_{\mathrm{sc}}, open-circuit voltage VocV_{\mathrm{oc}}, fill factor (FF), and PCE of both films. (c) External quantum efficiency (EQE) spectra of the 250-nm-thick FA0.95Cs0.05PbI3\mathrm{FA}_{0.95}\mathrm{Cs}_{0.05}\mathrm{PbI}_{3} thin film.

The spatiotemporal iMIM setup with a focused laser beam illuminating from below the sample stage is illustrated in Figure 1a. In the tip-scan mode, the laser is focused by one set of piezostage and the second piezo-scanner carries the tip to scan over the sample[27]. In the sample-scan mode, the first set of piezo-stage aligns the center of the laser spot to the tip, whereas the sample is set in motion by the piezo-scanner[33, 34]. In both configurations, one can fix the relative position between tip and sample and perform time-resolved (tr-iMIM) measurements[27]. Here the laser output is modulated by an electro-optic modulator (EOM), which is driven by a 7-kHz square wave from a function generator such that steady-state photoconductivity is reached in the laser-ON state and zero photoconductivity in the laser-OFF state. The same waveform also triggers a high-speed oscilloscope for iMIM measurement. The temporal resolution of our setup is ~ 10 ns (see Methods). The microwave electronics detect the tip-sample impedance, from which the local conductivity can be deduced[35]. The optical excitation in our setup is diffraction limited, whereas the electrical imaging has a spatial resolution 20 ~ 50 nm comparable to the tip diameter. Quantification of the iMIM signals by finite-element analysis (FEA)[36] is detailed in Supplementary Figure 2.

Photoconductivity mapping on FACsPbI3 and diffusion analysis

Figure 1. Photoconductivity mapping on FACsPbI3 and diffusion analysis. (a) Schematic of the iMIM setup with either the tip-scan or sample-scan mode. The tr-iMIM configuration is shown inside the dash-dotted box. The FACsPbI3 thin film deposited on glass substrate and encapsulated by a PMMA layer (Sample A) is also illustrated. (b) Tip-scan iMIM images when the sample is illuminated by a 446-nm diode laser at PC=100 mW/cm2P_\mathrm{C} = 100\ \mathrm{mW}/\mathrm{cm}^{2}. (c) Photoconductivity map based on the iMIM data and FEA simulation. The dashed lines are various linecuts for the calculation of average signals. (d) Image of the laser spot taken by a CCD camera. (e) Line profiles of averaged photoconductivity and laser intensity, from which the diffusion length can be extracted. The solid black and dashed gray lines represent the best curve fitting and upper/lower bounds, respectively. All scale bars are 10 μ\mum.

Comparison between experimental data and simulation results

Supplementary Figure 2. Comparison between experimental data and simulation results. (a) Simulated iMIM response as a function of the conductivity of the perovskite layer. (b) Distribution of quasi-static potential near the tip apex at σ=10−3\sigma= 10^{-3} S/m (left) and 10310^{3} S/m (right). (c) Measured (open circles and triangles) iMIM signals as a function of laser power and simulated (solid and dashed lines) results as a function of the FACsPbI3_3 conductivity. Note that the photoconductivity does not scale with the illumination intensity.

Figure 1b shows the iMIM images when Sample A was illuminated by a 446-nm (hν=2.78h\nu= 2.78 eV) diode laser with the intensity at the center of the laser spot PC=100P_\mathrm{C} = 100 mW/cm2^2, i.e., on the order of 1 Sun. The granular features are due to topographic crosstalk with the polycrystalline sample surface[33]. It is nevertheless evident that the photoresponse is continuous across many grain boundaries (GBs). Based on the iMIM response (Supplementary Figure 2), we can replot the data to a conductivity map (Figure 1c) with high conversion fidelity. For comparison, the optical image of the laser spot acquired from a charge-coupled device (CCD) camera shows much smaller spatial spread in Figure 1d. To improve the signal-to-noise ratio and minimize the topographic artifact, we averaged 8 line profiles shown in Figure 1c. The resultant curve, plotted in Figure 1e, is clearly broader than the Gaussian beam profile (e−r2/w2e^{-r^2/w^2}, w∼2w \sim2 μm). Assuming that the carrier mobility μ\mu is independent of charge density nn within the range of our experiment, the measured photoconductivity profile σ(r)\sigma(r) is proportional to the steady-state density profile n(r)n(r) as

σ(r)=n(r)qμ(1)\sigma(r) = n(r)q\mu \tag*{(1)}

, where qq is the elemental charge. Here n(r)n(r) can be described by the diffusion equation[27, 37, 38]

n(r)−L2∇2n(r)=ηPCτdhνe−r2/w2(2)n(r) - L^2\nabla^2 n(r) = \frac{\eta P_\mathrm{C}\tau}{d h\nu}e^{-r^2/w^2} \tag*{(2)}

, where L=DτL = \sqrt{D\tau} is the diffusion length, DD the diffusion coefficient, τ\tau the lifetime, and η∼1\eta\sim1 the incident photon-to-current conversion efficiency (IPCE). The analytical solution to Eq. (2) is

n(r)∝∫−∞∞K0(r′/L)e−(r−r′)2/w2 dr′(3)n(r) \propto\int_{-\infty}^{\infty} K_0(r'/L)e^{-(r-r')^2/w^2}\,dr' \tag*{(3)}

, where K0K_0 is the modified Bessel function of the second kind. By fitting the iMIM data to Eq. (3), we obtain a diffusion length L=5.1±0.6L = 5.1 \pm0.6 µm, consistent with values reported in the literature for thin-film PSCs[9, 10, 16, 46]. As the laser power increases, LL decreases to ∼4\sim4 µm at PC∼103P_\mathrm{C} \sim10^3 mW/cm2^2 and saturates at 3.5 µm for PC∼104P_\mathrm{C} \sim10^4 mW/cm2^2 (Supplementary Figure 3).

Power-dependent diffusion mapping for Sample A

Supplementary Figure 3. Power-dependent diffusion mapping for Sample A. (a) Power-dependent iMIM-Im/Re and photoconductivity images of Sample A. (b) Line profiles of averaged photoconductivity and laser intensity and curve fittings, from which the diffusion lengths can be extracted. (c) (Upper panel) Spatial distribution of charge carriers with various diffusion lengths. (Lower panel) Carrier density at the center of the illumination spot as a function of diffusion length.

Figure 2a shows a typical tr-iMIM decay curve (averaged over 242,880 cycles) on Sample A illuminated by the 446-nm laser at PC=100P_\mathrm{C} = 100 mW/cm2^2 before t=0t = 0. As the iMIM-Im signal scales with photoconductivity in our measurement range (Supplementary Figure 4), we will just present the raw data in the following analysis. From Eq. (1), the decay of tr-iMIM-Im signal provides a direct measure of the lifetime of mobile carriers in the conduction or valence band. The relaxation fits nicely to a biexponential function y=A1e−t/τ1+A2e−t/τ2y = A_1e^{-t/\tau_1} + A_2e^{-t/\tau_2}, with τ1∼0.7\tau_1 \sim0.7 µs and τ2∼10\tau_2 \sim10 µs. As shown in the inset of Figure 2a, we observed the same τ1\tau_1 and τ2\tau_2 when using 517-nm and 638-nm lasers (Supplementary Figure 5), suggesting that the time constants are intrinsic to the sample and independent on the laser wavelength. In contrast, the TRPL data on Sample A (Figure 2b) exhibit two different times τf∼150\tau_\mathrm{f} \sim150 ns and τs∼0.7\tau_\mathrm{s} \sim0.7 µs, which will be discussed in the next section. By parking the tip at various locations of the film and measuring the decay curves, we also show that the tr-iMIM response is spatially uniform on the sample surface within statistical errors (Supplementary Figure 6 and Supplementary Figure 7).

Time-resolved iMIM and carrier lifetime

Figure 2. Time-resolved iMIM and carrier lifetime. (a) Typical tr-iMIM relaxation curve of Sample A. The sample was illuminated by the 446-nm laser at PC=100P_\mathrm{C} = 100 mW/cm2^{2} before t=0t = 0 μ\mus. The inset shows the two lifetimes under excitation lasers with wavelengths of 446 nm, 517 nm, and 638 nm. (b) TRPL data of Sample A. The blue curve is a biexponential fit to the TRPL data. The inset is a close-up view, showing the two decay time constants from the fitting.

Simulated iMIM response for the ultra-sharp tip as a function of the conductivity

Supplementary Figure 4. Simulated iMIM response for the ultra-sharp tip as a function of the conductivity. Distributions of quasi-static potential are shown at σ=0\sigma= 0 S/m (left) and 10 S/m (right).

Wavelength-dependent tr-iMIM-Im signals for 446 nm, 517 nm, and 638 nm diode lasers

Supplementary Figure 5. Wavelength-dependent tr-iMIM-Im signals with laser intensity ~ 100 mW/cm2^{2}.

Raw AFM and iMIM-Im/Re images of sample A: (a) AFM, (b) iMIM-Im, (c) iMIM-Re

Supplementary Figure 6. Raw AFM and iMIM-Im/Re images of sample A. (a) AFM, (b) iMIM-Im, (c) iMIM-Re images. All scale bars are 4 μm\mu\mathrm{m}.

Supplementary Figure 7. Complete set of tr-iMIM-Im data for 20 points. G1-G10 are points on grains, while B1-B10 are points on grain boundaries.

In order to shed some light on the tr-iMIM data, we studied the carrier dynamics in perovskite thin films with electron or hole transport layers[6, 7, 9, 10, 22, 23]. For the HTL sample, hereafter referred to as Sample B, a 20-nm PTAA (poly-triaryl amine) was spin-coated on the substrate before the same 250-nm FACsPbI3_3 / 30-nm PMMA film was deposited. The PTAA layer rapidly extracts photo-generated holes from FACsPbI3_3 within a sub-10-ns time scale[22, 23, 39]. Similarly, a 40-nm ETL TiO2_2 layer for the extraction of electrons was coated on the substrate before the FACsPbI3_3/PMMA deposition for Sample C. Control experiments have been conducted to ensure that the PL is quenched in both Samples B and C due to the extraction of holes and electrons, respectively (Supplementary Figure 8). Note that the charge dynamics in the transport layers (∼300\sim300 nm below the surface) would not affect the iMIM results due to the shallow probing depth of 50 ∼\sim 100 nm. The tr-iMIM data in Samples B and C under the 446-nm laser illumination with PC=100P_\mathrm{C} = 100 mW/cm2\mathrm{mW}/\mathrm{cm}^2 are shown in Figure 3a. It is evident that only the fast process with τ1∼0.7 μs\tau_1 \sim0.7\ \mu\mathrm{s} survives in Sample B and the slow process with τ2∼10 μs\tau_2 \sim10\ \mu\mathrm{s} in Sample C. The observation strongly suggests that the two time-constants in Sample A are associated with the lifetime of electrons and holes in FACsPbI3\mathrm{FACsPbI}_3.

Results and analysis on HTL/ETL samples

Figure 3. Results and analysis on HTL/ETL samples. (a) tr-iMIM signals on the HTL Sample B (upper panel) and ETL Sample C (lower panel). The layer structures of each sample are illustrated in the insets. (b) Diffusion maps of Sample B and (c) Sample C under the illumination of 446-nm laser at PC=100 mW/cm2P_{\mathrm{C}} = 100\ \mathrm{mW/cm^2}. Scale bars are 10 μm\mu\mathrm{m}. (d) Tabulated parameters for the calculation of electron/hole mobility values by two methods, i.e., μdiff\mu_{\mathrm{diff}} from the Einstein relation and μpc\mu_{\mathrm{pc}} from photoconductivity analysis.

PL data on Samples A, B, and C

Supplementary Figure 8. PL data on Samples A, B, and C at an excitation laser power of 9.6×103 mW/cm29.6 \times10^{3}\ \mathrm{mW}/\mathrm{cm}^{2}

The HTL/ETL samples also allow us to separately address the diffusion dynamics of electrons and holes. Figure 3b and Figure 3c show the tip-scan photoconductivity maps of Samples B and C under PC=100 mW/cm2P_\mathrm{C} = 100\ \mathrm{mW}/\mathrm{cm}^2, from which Le∼5.2 μmL_\mathrm{e} \sim5.2\ \mu\mathrm{m} and Lh∼2.7 μmL_\mathrm{h} \sim2.7\ \mu\mathrm{m} can be extracted, respectively. As tabulated in Figure 3d, we can derive the diffusion coefficient from the diffusion equation L=DτL = \sqrt{D\tau} and carrier mobility (μe,diff=15 cm2/V⋅s\mu_{\mathrm{e,diff}} = 15\ \mathrm{cm}^2/\mathrm{V}\cdot\mathrm{s} and μh,diff=0.3 cm2/V⋅s\mu_{\mathrm{h,diff}} = 0.3\ \mathrm{cm}^2/\mathrm{V}\cdot\mathrm{s}) from the Einstein relation μ=(q/kBT)∗D\mu= (q/k_\mathrm{B}T)*D. A different method to analyze the transport properties is through the photoconductivity (Eq. (1)) and density profile (Eq. (2)). The calculated mobility values are μe,pc=24 cm2/V⋅s\mu_{\mathrm{e,pc}} = 24\ \mathrm{cm}^2/\mathrm{V}\cdot\mathrm{s} and μh,pc=0.3 cm2/V⋅s\mu_{\mathrm{h,pc}} = 0.3\ \mathrm{cm}^2/\mathrm{V}\cdot\mathrm{s}. The small difference between the two methods is within error bars of the measurements. We note that in MAPbI3\mathrm{MAPbI}_3 and FAPbI3\mathrm{FAPbI}_3 thin films, mobility values measured by different techniques vary in a considerable range from 0.2 to 30 cm2/V⋅s\mathrm{cm}^2/\mathrm{V}\cdot\mathrm{s} [6, 7, 8, 9, 10, 14, 17, 23, 24, 25, 28, 40, 41]. As tabulated in Supplementary Fig. 9, either μe>μh\mu_\mathrm{e} > \mu_\mathrm{h} or μe<μh\mu_\mathrm{e} < \mu_\mathrm{h} has been reported in the literature. In our experiment, mobility values are directly calculated from the measured LL and τ\tau under an illumination intensity ∼1\sim1 Sun, with no other assumptions or modeling involved. The pronounced difference between μe\mu_\mathrm{e} and μh\mu_\mathrm{h} is thus genuine. Figure 3d also indicates that the equilibrium carrier density in our experiment is on the order of 101510^{15}–1016 cm−310^{16}\ \mathrm{cm}^{-3}. Within this range, the electron/hole mobility is largely independent of the carrier concentration[42]. It is thus well justified to approximate the density profile by the measured photoconductivity profile in our diffusion analysis (Figure 1e).

Finally, we briefly discuss the iMIM results at higher illumination intensities. As shown in Figure 4a and Figure 4b, the temporal evolution of HTL/ETL samples again displays the biexponential decay when PCP_\mathrm{C} increases beyond 100 mW/cm2\mathrm{mW}/\mathrm{cm}^2 (complete data in Supplementary Fig. 10), with one of the processes substantially suppressed. For instance, while A1/A2∼2A_1/A_2 \sim2 is expected in plain FACsPbI3\mathrm{FACsPbI}_3, the electron dynamics clearly dominate in Sample B such that A1/A2>2A_1/A_2 > 2 in Figure 3c. Conversely, with electrons efficiently removed by the ETL, the hole dynamics prevail and A1/A2<2A_1/A_2 < 2 in Sample C. We have also performed photoconductivity mapping on Samples B and C under various PCP_\mathrm{C} (Supplementary Figs. 11 and 12) and the results are plotted in Figure 4d. As PCP_\mathrm{C} increases towards 103∼10410^{3} \sim10^{4} mW/cm2^{2}, the contribution from the other type of carriers is no longer negligible.

Power-dependent iMIM results

Figure 4. Power-dependent iMIM results. (a) tr-iMIM signals on Sample B and (b) Sample C under various laser powers. Signals below the noise level are truncated for clarity. (c) Power-dependent A1A_{1} and A2A_{2} in Sample B (upper panel) and Sample C (lower panel). The dash-dotted lines are A1/2A_{1}/2 (Sample B) and 2A22A_{2} (Sample C) for comparison with the plain perovskite Sample A, which shows A1/A2∼2A_{1}/A_{2} \sim2. (d) Power-dependent diffusion lengths and (e) photoconductivity at the center of the illumination spot in both samples.

Consequently, in addition to the general trend of decreasing diffusion length at increasing excitation, LL in Sample B decreases further at high PCP_{\mathrm{C}}, whereas LL in Sample C increases slightly at high PCP_{\mathrm{C}}. Similarly, while only one type of carriers is responsible for the low-power photoconductivity, σC\sigma_{\mathrm{C}} does not scale with PCP_{\mathrm{C}} in either sample towards 10410^{4} mW/cm2^{2} Figure 4e.

Discussion

The spatiotemporally resolved iMIM experiments reveal rich information on organometal trihalide perovskite thin films. To begin with, we take a close look at the impact of GBs on charge transport in PSC materials, which has been under intense debate[19, 43, 44, 45, 46]. As summarized in a recent review[47], while GBs strongly affect the current-voltage hysteresis and long-term stability of PSCs, their effect on carrier recombination and thus the open-circuit voltage is rather mild under the illumination of ~ 1 Sun. In a previous report[33], we showed that the photoconductivity is spatially homogeneous over grains and GBs, consistent with conductive AFM and SPCM studies[20, 46]. In this work, we further demonstrate that the carrier diffusion is not impeded by the presence of numerous GBs in all three samples. It is possible that the GBs in the current study are not strong nonradiative recombination (i.e., highly defective) centers, and there is no significant band bending at the GBs to block electron/hole movement across multiple grains[48]. As a result, under the normal solar-cell operation, GBs in our samples do not lead to appreciable spatial variation of transport properties such as the density and mobility of photo-excited carriers, consistent with the early theoretical prediction[49]. We caution that sample-to-sample variation is widely observed in the PSC research. It is still possible that GBs in other hybrid perovskite thin films exhibit strong impacts on the carrier lifetime and transport properties.

Given the extensive use of PL in studying carrier dynamics, it is instructive to compare the TRPL and tr-iMIM results in our samples. In short, TRPL measured excited states such as exciton recombination via emitted photons, whereas tr-iMIM measures the decay of steady-state conductivity following optical injection of free carriers. In TRPL experiments, the signal strength depends on the radiative recombination process that emits photons, whereas the temporal evolution measures the total lifetime of certain carriers or excitons[8, 9, 10, 18, 19]. For the TRPL data of Sample A in Figure 2b, the fast (τf∼150\tau_{\mathrm{f}} \sim150 ns) and slow (τs∼0.7\tau_{\mathrm{s}} \sim0.7 μs) processes are associated with the surface recombination and the relaxation of the shorter-lived electrons in FACsPbI3_{3}, respectively. Note that τs\tau_{\mathrm{s}} matches τ1\tau_{1} in the tr-iMIM data. After the elapse of τs\tau_{\mathrm{s}}, however, no more mobile electrons are available for radiative recombination with mobile holes. As a result, TRPL cannot measure the lifetime of the longer-lived carriers[16]. We emphasize that the extraction of one type of carriers by HTL or ETL quenches the PL process and the TRPL decay constants in these samples no longer represent lifetimes of electrons or holes in plain PSCs[50]. In tr-iMIM, however, both the signal strength and temporal evolution depend on the photoconductivity, which is proportional to the product of carrier density and mobility. For the three time scales above, the decay on the order of 100 ns is not seen in tr-iMIM, presumably due to the small steady-state density and low mobility of surface-bound carriers. On the other hand, because of the low efficiency of radiative recombination in PSCs[16], the removal of free electrons does not lead to appreciable changes in the dynamics of free holes. Consequently, the relaxation process of electrons and holes can be treated independently, as revealed by the tr-iMIM data. It should be noted that PL microscopy has also been utilized to map out the diffusion dynamics in PSC materials[51, 52]. For the same reasons discussed above, it is not straightforward to compare photoluminescence and photoconductivity imaging results across multiple grains, which will be subjected to future experiments.

The difference between photo-physical properties of electrons and holes, as evidenced in Figure 3d, deserves further discussions. In hybrid perovskites, deep-level defects dominate the trapping/de-trapping process and nonradiative recombination of free carriers. In general, the deeper the trap level, the longer time it takes for carriers to be de-trapped, and consequently the longer lifetime and lower mobility. Theoretical studies[53, 54] suggest that cation and anion vacancies create shallow energy levels, while iodine interstitials introduce deep levels in the bandgap. Interestingly, iodine interstitials can be both positively (Ii+\mathrm{I}_{\mathrm{i}}^{+}) and negatively (Ii−\mathrm{I}_{\mathrm{i}}^{-}) charged, which leads to spatially separated trapped electrons and holes with very low recombination efficiency. The transition energy for Ii+\mathrm{I}_{\mathrm{i}}^{+} (0/+) (de-trapping for electron) is calculated to be 0.48 eV below the conduction band minimum (CBM), whereas the transition energy for Ii−\mathrm{I}_{\mathrm{i}}^{-} (0/−) (de-trapping for hole) is 0.78 eV above the valence band maximum (VBM)[54]. The larger de-trapping barrier for hole results in its longer lifetime and lower mobility. When photoexcited electrons are quenched, the remaining holes will be trapped and then de-trapped via Ii−\mathrm{I}_{\mathrm{i}}^{-}, and vice versa. The trapping/de-trapping process induces delayed recombination, as manifested in the tr-iMIM decay curves. This qualitatively explains that the holes have longer carrier lifetime but lower mobility than electrons. Further theoretical work is needed to elucidate this physical picture in a quantitative manner.

As a final remark, we emphasize that in solar cells, diffusion lengths of both electrons and holes much larger than the film thickness is desirable for the effective separation of photo-carriers. Because of the unique defect properties in hybrid perovskite thin films, as well as the competition between the recombination and trapping/detrapping process, the imbalance in mobility (μe≫μh\mu_e \gg\mu_h) is largely compensated by the imbalance in lifetime (τe≪τh\tau_e \ll\tau_h). As a result, the difference between Le∼5L_e \sim5 μm and Lh∼3L_h \sim3 μm is insignificant in our samples, which is of fundamental importance for the superior performance of PSC devices.

In summary, we systematically study the optoelectronic properties of 5%-Cs-doped FAPbI3FAPbI_3 thin films (PCE > 20%) by imaging the carrier diffusion in real space and detecting the photoconductivity evolution in real time. For plain perovskite films, two relaxation processes are observed on the sample. By selectively removing one type of carriers, we demonstrate that the fast and slow decay constants are associated with the lifetimes of photo-generated electrons and holes, respectively. The diffusion mapping on HTL/ETL samples allows us to extract parameters such as diffusion coefficient, equilibrium carrier density, and mobility of both carriers. The imbalance in carrier lifetime is offset by the difference in mobility such that diffusion lengths of electrons and holes are comparable to each other. We emphasize that, prior to our work, separate experiments are needed to measure relaxation time (TRPL or TRTS) and mobility (transport or SPCM on doped samples) of free carriers. To our knowledge, it is the first time that diffusion length, carrier lifetime, and charge mobility can be individually addressed for mobile electrons and holes on the same batch (as-grown, HTL-coated, ETL-coated) of samples. The spatiotemporal microwave imaging provides the most direct measurement of photo-physical properties of organometal trihalides, which is crucial for research and development of these fascinating materials towards commercial products.

Methods

Materials. All solvents were purchased from Sigma-Aldrich and used as-received without any other refinement. Formamidinium iodine (FAI) was purchased from Greatcell Solar. Lead iodide (PbI2PbI_2) was from TCI Corporation. Spiro-OMeTAD was received from Merck Corporation. Cesium iodine (CsI) and PTAA were purchased from Sigma-Aldrich. Patterned fluorine-doped tin-oxidecoated (FTO) glass (<15 Ω<15\ \Omega/square) and indium tin oxide-coated (ITO) glass were obtained from Advanced Election Technology Co., Ltd.

Sample preparation. The perovskite films in this work were deposited on top of cover glasses or ITO glass. The substrate glasses were cleaned extensively by deionized water, acetone, and isopropanol. For the HTL deposition, the PTAA (Sigma-Aldrich) was dissolved in toluene with a concentration of 5 mg⋅mL−15\ \mathrm{mg}\cdot\mathrm{mL}^{-1} and spin-coated on the substrates at 5,000 rpm for 30 s. The spun PTAA films were annealed at 100∘C100^\circ\mathrm{C} for 10 min. For the ETL deposition, a compact titanium dioxide (TiO2\mathrm{TiO_2}) layer of about 40 nm was deposited by spray pyrolysis of 7 mL 2-propanol solution containing 0.6 mL titanium diisopropoxide bis(acetylacetonate) solution (75% in 2-propanol, Sigma-Aldrich) and 0.4 mL acetylacetone at 450∘C450^\circ\mathrm{C} in air. The FA0.95Cs0.05PbI3\mathrm{FA_{0.95}Cs_{0.05}PbI_3} precursor solution was prepared by dissolving 0.4 M Pb2+0.4\ \mathrm{M}\ \mathrm{Pb}^{2+} in dimethyl sulfoxide (DMSO) and dimethylformamide (v/v = 3/7) mixed solvent. Perovskite films were deposited using a three-step spin-coating procedure with the first step of 100 rpm for 3 s, a second step of 3,500 rpm for 10 s, and the last step of 5,000 rpm for 30 s. Toluene (1 mL) was applied on the spinning substrates at 20 s of the third step. After spin coating, the substrates were annealed at 170∘C170^\circ\mathrm{C} for 27 min. The encapsulated perovskite films were capped with PMMA (MwM_\mathrm{w} about 120,000) film by spin-coating 15 mg ml−1^{-1} PMMA in chlorobenzene solution at 4000 rpm for 35 s.

iMIM and tr-iMIM setup. The sample-scan iMIM was performed on a modified ParkAFM XE-100 platform with bottom illumination. The tip-scan iMIM was performed in a customized chamber (ST-500, Janis Research Co.) with positioners and scanners (AttoCube Systems AG). During the measurements, we kept the samples in vacuum by pumping the chamber below 10−410^{-4} mbar. The PtIr tips were purchased from Rocky Mountain Nanotechnology LLC, model 12PtIr400A for diffusion mapping and 12PtIr400A-10 (ultra-sharp tips) for the point measurements in Figure 2. For tr-iMIM, the diode laser was modulated by an electro-optic modulator (M350-160–01 EOM, Conoptics Inc.) with a power supply of 8-ns rise/fall time. The EOM was driven by a 7-kHz square wave from a function generator (DG5071, RIGOL Technologies USA Inc.) with <4<4-ns rise/fall time. The tr-iMIM signals were measured by a 600-MHz oscilloscope (DS6062, RIGOL Technologies USA Inc.) with 5-GSa/s sampling rate.

Finite-element analysis. Finite-element analysis was performed using the AC/DC module of commercial software COMSOL4.4. The tip for diffusion mapping is relatively blunt due to the extensive contact-mode scans on the sample surface. We modeled it as a truncated cone with a half-angle of 15° and a diameter of 200 nm at the apex. The ultra-sharp tip was mostly used for point measurements in Figure 2 and the apex was well preserved. It was thus modeled as a truncated cone with a half-angle of 38° and a diameter of 20 nm at the apex. In the simulation, the dielectric constants of PMMA and FACsPbI3_3 are 3 and 62, respectively, consistent with that reported in the literature[33, 55]. The FEA software computes the real and imaginary parts of the tip–sample admittance (proportional to iMIM-Re/Im signals) as a function of the conductivity of the perovskite layer, using the values at σ=0\sigma= 0 as the reference.

Data Availability. All data supporting the findings of this study are available within the article and/or the SI Appendix. The raw data is available from the corresponding author upon reasonable request.

Acknowledgements

The research at UT-Austin was primarily supported by the NSF through the Center for Dynamics and Control of Materials, an NSF Materials Research Science and Engineering Center (MRSEC) under Cooperative Agreement DMR-1720595. The authors also acknowledge the use of facilities and instrumentation supported by the NSF MRSEC. K.L. and X.M. acknowledge the support from Welch Foundation Grant F-1814. X. Li acknowledges the support from Welch Foundation Grant F-1662. The tip-scan iMIM setup was supported by the US Army Research Laboratory and the US Army Research Office under Grants W911NF-16-1-0276 and W911NF-17-1-0190. The work at NREL was supported by the U.S. DOE under Contract No. DE-AC36-08GO28308 with Alliance for Sustainable Energy, Limited Liability Company (LLC), the Manager and Operator of the National Renewable Energy Laboratory. K.Z., J.H., X.C., X.W. and Y.Y. acknowledge the support on charge carrier dynamics study from the Center for Hybrid Organic-Inorganic Semiconductors for Energy (CHOISE), an Energy Frontier Research Center funded by the Office of Basic Energy Sciences, Office of Science within the U.S. DOE. F.Z. acknowledges the support on devices fabrication and characterizations from the De-Risking Halide Perovskite Solar Cells program of the National Center for Photovoltaics, funded by the U.S. DOE, Office of Energy Efficiency and Renewable Energy, Solar Energy Technologies Office. The views expressed in the article do not necessarily represent the views of the DOE or the U.S. Government. The U.S. Government retains and the publisher, by accepting the article for publication, acknowledges that the U.S. Government retains a nonexclusive, paid-up, irrevocable, worldwide license to publish or reproduce the published form of this work or allow others to do so, for U.S. Government purposes.

Author contributions

K.Z. and K.L. conceived the project. F.Z. and J.H. prepared samples and characterized devices. X.C. and Z.H. performed the TRPL and PL characterization. X.M. and Z.C. performed the iMIM experiments and data analysis. J.Q. and X.L. contributed to the sample-scan experiments. X.W. and Y.Y. contributed to the theoretical explanations. X.M. and K.L. drafted the manuscript with contributions from all authors. All authors have given approval to the final version of the manuscript.

Competing interests

The authors declare no competing interests.

Supplementary Information

† These authors contributed equally to this work

Solar cell device characterization

DirectionJscJ_{\mathrm{sc}} (mA·cm−2^{-2})VocV_{\mathrm{oc}} (V)FFFFPCEPCE (%)
Forward23.811.100.7720.2
Backward23.791.100.7820.4

Table 1.

Solar cell devices using the 5% Cs-doped FA0.95Cs0.05PbI3\mathrm{FA}_{0.95}\mathrm{Cs}_{0.05}\mathrm{PbI}_{3} thin film were prepared on conductive fluorine-doped tin oxide (FTO)-coated glass substrates. The substrates were cleaned extensively by deionized water, acetone, and isopropanol. A compact titanium dioxide (TiO2\mathrm{TiO}_{2}) layer of about 40 nm was deposited by spray pyrolysis of 7-mL 2-propanol solution containing 0.6-mL titanium diisopropoxide bis(acetylacetonate) solution (75% in 2-propanol, Sigma-Aldrich) and 0.4-mL acetylacetone at 450°C in air. The FA0.95Cs0.05PbI3\mathrm{FA}_{0.95}\mathrm{Cs}_{0.05}\mathrm{PbI}_{3} precursor solution was prepared by dissolving 1.2M Pb2+\mathrm{Pb}^{2+} in dimethyl sulfoxide (DMSO) and dimethylformamide (v/v = 3/7) mixed solvent. Perovskite films were deposited using a three-step spin-coating procedure with the first step of 100 rpm for 3 s, a second step of 3,500 rpm for 10 s, and the last step of 5,000 rpm for 30 s. Toluene (1 mL) was applied on the spinning substrates at 20 s of the third step. After spin coating, the substrates were annealed at 170°C for 27 min. The spiro-OMeTAD is prepared by the details in the HTL preparation section and deposited according to the previous report. The devices were finalized by thermal evaporation of 100-nm gold. Solar cell performance measurements were taken under a simulated AM 1.5G illumination (100 mW/cm2^{2}, Oriel Sol3A Class AAA Solar Simulator). The photocurrent density–voltage (JJ–VV) characteristics were measured using a Keithley 2400 source meter. The JJ–VV curves of all devices were measured by masking the active area with a metal mask of area 0.12 cm2^{2}. Both backward-scan and forward-scan curves were measured with a bias step of 10 mV and delay time of 0.05 s. Typical JJ–VV curves are shown in Supplementary Figure 1 and the results are summarized in Supplementary Figure 1, for 550-nm-thick perovskite based solar cells. Supplementary Figure 1 shows the external quantum efficiency (EQE) spectra of our 250-nm-thick FA0.95Cs0.05PbI3\mathrm{FA}_{0.95}\mathrm{Cs}_{0.05}\mathrm{PbI}_{3} thin films measured by a solar cell quantum-efficiency measurement system (QEX10, PV Measurements).

Finite-element analysis of the iMIM signals

The iMIM electronics detect the tip-sample impedance change, from which the local conductivity can be deduced. Supplementary Figure 2 shows the finite-element analysis (FEA) results of the iMIM signals[1]. As the conductivity σ\sigma of FACsPbI3_3 increases, the microwave electrical fields are gradually screened by the free carriers. Consequently, the imaginary part of the signal, iMIM-Im (proportional to tip-sample capacitance), increases monotonically with respect to σ\sigma, whereas the real-part signal iMIM-Re (proportional to tip-sample conductance) peaks at σ∼10\sigma\sim10 S/m. As depicted in the insets of Supplementary Figure 2, the spread of the quasistatic potential indicates that the spatial resolution of iMIM is comparable to the tip diameter. The conversion from iMIM images to conductivity images is achieved by directly comparing the experimental data and simulated results. To this end, we performed a point measurement on Sample A and measured the iMIM signals as a function of the laser intensity. As plotted in Supplementary Figure 2, the response curve computed by FEA (iMIM signals versus conductivity) and the experimental data (iMIM signals versus laser power) are in excellent agreement over a wide range of parameter space[1]. We can therefore replot the raw iMIM images to photoconductivity maps with high conversion fidelity.

Power-dependent diffusion data for Sample A

The power-dependent iMIM-Im/Re images of Sample A are shown in Supplementary Figure 3. As depicted in Supplementary Figure 3, the curve fitting to Eq. (3) in the main text allows us to obtain the diffusion lengths at different laser power. Using Eqs. (2) and (3) in the main text, we can quantitatively analyze the diffusion pattern. Supplementary Figure 3 shows the spatial distribution of charge carriers with various diffusion lengths under an excitation profile e−r2/w2e^{-r^{2}/w^{2}} with w∼2w \sim2 µm. For instance, assuming nc0=η(Pcτ/hν)n_{\mathrm{c0}} = \eta(P_{\mathrm{c}}\tau/h\nu) is the density at the center of laser spot for L=0L = 0 µm, the numerical solution indicates that nc∼0.07nc0n_{\mathrm{c}} \sim0.07 n_{\mathrm{c0}} for L=5L = 5 µm [2]. The analysis is important for the calculation of carrier density and mobility, which are tabulated in Figure 3d.

Finite element analysis for the ultra-sharp tip {#sec:Supplementary Note 4}

For the point experiment shown in Figure 2 of the main text, we used an ultra-sharp tip from Rocky Mountain Nanotechnology LLC, model 12PtIr400A-10 with a nominal radius of 10 nm at the apex, for accurate positioning on grains and grain boundaries. For the FEA modeling, we have used the half-angle of 38° and a diameter of 20 nm at the apex that are consistent with the SEM image. As shown in Supplementary Figure 4, the simulated iMIM-Im signals roughly scales with the conductivity of FACsPbI3_3 up to σ∼10\sigma\sim10 S/m, which is within the photoconductivity range in our experiment. As a result, we directly analyze the tr-iMIM-Im signals rather than converting them to photoconductivity in the time-resolved response.

Wavelength-dependence of the tr-iMIM data

The majority of data presented in the main text were acquired under the illumination of a 446-nm diode laser. We also performed tr-iMIM experiments with two additional diode lasers with wavelengths of 517 nm (green) and 638 nm (red). As shown in Supplementary Figure 5, the two relaxation time constants in Sample A were observed in all three measurements. It is possible that the thermalization to the band edge through phonon emitting is very effective at low laser intensities (~ 1 Sun), after which the trapping/detrapping processes take place. As a result, the carrier temperature is essentially independent of the excitation wavelength. We therefore conclude that the two lifetimes are intrinsic for the FACsPbI3\mathrm{FACsPbI}_{3} thin films.

Complete AFM/iMIM data in the sample-scan mode

The raw AFM and iMIM-Im/Re images are shown in Supplementary Fig. 6. Note that the contrast in the iMIM images is mostly due to topographic crosstalk[3].

Complete tr-iMIM data for grains and grain boundaries

The complete set of tr-iMIM data and biexponential fitting are included in Supplementary Figure 7. It is evident from the raw data that the temporal dynamics of photo-carriers are spatially uniform across microstructures on the FACsPbI3\mathrm{FACsPbI_3} sample surface.

PL measurements on Samples B and C

We have conducted photoluminescence (PL) measurements on Samples A, B, and C to confirm the charge transfer in HTL/ETL samples. As shown in Supplementary Figure 8, the PL signal is quenched by 94% in the PTAA/FACsPbI3\mathrm{FACsPbI}_{3} Sample B and 80% in the TiO2\mathrm{TiO}_{2}/ FACsPbI3\mathrm{FACsPbI}_{3} Sample C.

It should be noted that, for good signal-to-noise ratio, the excitation power (9.6×103 mW/cm29.6 \times10^{3}\ \mathrm{mW}/\mathrm{cm}^{2}, on the order of 100 Sun) is kept high in the PL experiments. The incomplete PL quenching in Samples B and C is consistent with the high-power tr-iMIM data in Figure 4.

Supplementary Note 9. Tabulated mobility values for MAPI/FAPI thin films

CompositionMeasurementsμe\mu_e (cm2^2/V·s)μh\mu_h (cm2^2/V·s)Suppl. Ref.
MAPbI3\mathrm{MAPbI}_{3}TRMC12.57.55
MAPbI3\mathrm{MAPbI}_{3}TRMC3176
MAPbI3\mathrm{MAPbI}_{3}TRPL1.40.97
MAPbI3\mathrm{MAPbI}_{3}TRPL0.70.48
MAPbI3\mathrm{MAPbI}_{3}TRTS2.32269
(FA,MA)Pb(I,Br)3(\mathrm{FA},\mathrm{MA})\mathrm{Pb}(\mathrm{I},\mathrm{Br})_{3}TRTS0.23417.59
(FA,MA,Cs)Pb(I,Br)3(\mathrm{FA},\mathrm{MA},\mathrm{Cs})\mathrm{Pb}(\mathrm{I},\mathrm{Br})_{3}TRTS1.1229.19
MAPbI3\mathrm{MAPbI}_{3}TRMC30.56.510
MAPbI3\mathrm{MAPbI}_{3}TRMC182.511
FAPbI3\mathrm{FAPbI}_{3}TRPL0.23.512
MAPbI3\mathrm{MAPbI}_{3}Transport∼1\sim1∼0.2\sim0.213

Table 9. Tabulated mobility values for MAPI/FAPI thin films. Reference numbers are taken from the list in the main text. Abbreviations: TRMC – Time-resolved microwave conductivity, TRPL – time-resolved photoluminescence, TRTS – time-resolved THz spectroscopy.

Reported mobility values for MAPI/FAPI thin films are shown in Supplementary Fig. 9.

There is no consensus on whether electrons or holes have the higher mobility in the organometal trihalide family. Mobility values measured by the same methods from different groups may also show opposite results, suggesting a strong sample dependence of scattering mechanisms. It is worth noting that, as acknowledged by the authors, the two measured mobilities from Ref. 17 (highlighted in blue) are not unambiguously associated with electrons or holes based on the TRTS method. Instead, the higher one was assigned to holes and lower one to electrons purely based on assumptions from previous reports[4].

Complete tr-iMIM data of Sample B and Sample C

The complete tr-iMIM data (without truncating data below the noise floor in Figure 4a and Figure 4b of the main text) of Sample B and Sample C are shown in Supplementary Figure S10. For the two samples, the power-dependent time constants extracted from biexponential fitting are plotted in Figure S10 and Figure S10, respectively. The two lifetimes τ1∼0.7 μs\tau_{1} \sim0.7\,\mathrm{\mu s} and τ2∼10 μs\tau_{2} \sim10\,\mathrm{\mu s} are consistently observed in both samples.

Complete tr-iMIM data of Sample B and C, with power-dependent lifetimes for Samples B and C

Figure S10. Complete tr-iMIM data of sample B and C. (a) Complete tr-iMIM data in linear scale without truncation. The thick lines shaded in red and blue cover the segments of data with fast and slow decays, respectively. (b) Power-dependent lifetimes for Sample B. (c) Power-dependent lifetimes for Sample C.

Complete diffusion mapping data for Sample B

Supplementary Figure 11 shows the raw iMIM-Im/Re and conductivity images for diffusion mapping in Samples B. Curve fittings to Eq. (3) in the main text are also plotted in the figure.

Analysis of diffusion images for Sample B, showing raw iMIM-Im, iMIM-Re, and conductivity images, and averaged converted conductivity linecuts

Supplementary Figure 11. Supplementary Figure 11. Analysis of diffusion images for Sample B. (Top) The raw iMIM-Im, iMIM-Re, and conductivity images. (Bottom) Averaged converted conductivity linecuts for Sample B.

Complete diffusion mapping data for Sample C

Supplementary Figure 12 shows the raw iMIM-Im/Re and conductivity images for diffusion mapping in Samples C. Curve fittings to Eq. (3) in the main text are also plotted in the figure.

Diffusion mapping images and converted conductivity linecuts for Sample C

Supplementary Figure 12. Analysis of diffusion images for Sample C. (Top) The raw iMIM-Im, iMIM-Re, and conductivity images. (Bottom) Averaged converted conductivity linecuts for Sample C.

Supplementary References

  1. Lai, K., Kundhikanjana, W., Kelly, M., and Shen, Z. X. “Modeling and characterization of a cantilever-based near-field scanning microwave impedance microscope”, Rev. Sci. Instrum. 79, 063703 (2008).

  1. Chu, Z. et al. “Unveiling defect-mediated carrier dynamics in monolayer semiconductors by spatiotemporal microwave imaging”, Proc. Natl. Acad. Sci. 117, 13908–13913 (2020).

  1. Chu, Z. et al. “Impact of grain boundaries on efficiency and stability of organic-inorganic trihalide perovskites”, Nat. Commun. 8, 2230 (2017).

  1. Zhai, Y. et al. “Individual Electron and Hole Mobilities in Lead-Halide Perovskites Revealed by Noncontact Methods”, ACS Energy Lett. 5, 47–55 (2020).

  1. Ponseca, C. S. et al. “Organometal halide perovskite solar cell materials rationalized: ultrafast charge generation, high and microsecond-long balanced mobilities, and slow recombination”, J. Am. Chem. Soc. 136, 5189–5190 (2014).

  1. Oga, H., Saeki, A., Ogomi, Y., Hayase, S., and Seki, S. “Improved understanding of the electronic and energetic landscapes of perovskite solar cells: high local charge carrier mobility, reduced recombination, and extremely shallow traps”, J. Am. Chem. Soc. 136, 13818–13825 (2014).

  1. Stranks, S. D. et al. “Electron-hole diffusion lengths exceeding 1 micrometer in an organometal trihalide perovskite absorber”, Science 342, 341–344 (2013).

  1. Xing, G. et al. “Long-Range Balanced Electron-and Hole-Transport Lengths in Organic-Inorganic CH3NH3PbI3\mathrm{CH_3NH_3PbI_3}”, Science 342, 341–347 (2013).

  1. Zhai, Y. et al. “Individual Electron and Hole Mobilities in Lead-Halide Perovskites Revealed by Noncontact Methods”, ACS Energy Lett. 5, 47–55 (2020).

  1. Hutter, E.M. et al. “Charge Transfer from Methylammonium Lead Iodide Perovskite to Organic Transport Materials: Efficiencies, Transfer Rates, and Interfacial Recombination”, Adv. Energy Mater. 7, 1602349 (2017).

  1. Levine, I. et al. “Can we use time-resolved measurements to get steady-state transport data for halide perovskites?”, J. Appl. Phys. 124, 103103 (2018).

  1. Eperon, G.E. et al. “Formamidinium lead trihalide: a broadly tunable perovskite for efficient planar heterojunction solar cells”, Energy Environ. Sci. 7, 982 (2014).

References

  1. [1]Green, M. A., Ho-Baillie, A. and Snaith, H. J. “The emergence of perovskite solar cells”, Nat. Photonics 8, 506–514 (2014).DOI
  2. [2]Park, N.G. “Perovskite solar cells: an emerging photovoltaic technology”, Mater. Today 18, 65–72 (2015).DOI
  3. [3]Li, Z. et al. “Scalable fabrication of perovskite solar cells”, Nat. Rev. Mater. 3, 18017 (2018).DOI
  4. [4]NREL. Best Research-Cell Efficiency Chart. https://www.nrel.gov/pv/assets/pdfs/best-research-cell-efficiencies.20200803.pdf. Dated Aug 2020.
  5. [5]De Wolf, S. et al. “Organometallic halide perovskites: sharp optical absorption edge and its relation to photovoltaic performance”, J. Phys. Chem. Lett. 5, 1035–1039 (2014).DOI
  6. [6]Ponseca, C. S. et al. “Organometal halide perovskite solar cell materials rationalized: ultrafast charge generation, high and microsecond-long balanced mobilities, and slow recombination”, J. Am. Chem. Soc. 136, 5189–5190 (2014).DOI
  7. [7]Oga, H., Saeki, A., Ogomi, Y., Hayase, S., and Seki, S. “Improved understanding of the electronic and energetic landscapes of perovskite solar cells: high local charge carrier mobility, reduced recombination, and extremely shallow traps”, J. Am. Chem. Soc. 136, 13818–13825 (2014).DOI
  8. [8]Shi, D. et al. “Low trap-state density and long carrier diffusion in organolead trihalide perovskite single crystals”, Science 347, 519–522 (2015).DOI
  9. [9]Stranks, S. D. et al. “Electron-hole diffusion lengths exceeding 1 micrometer in an organometal trihalide perovskite absorber”, Science 342, 341–344 (2013).
  10. [10]Xing, G. et al. “Long-Range Balanced Electron-and Hole-Transport Lengths in Organic-Inorganic CH₃NH₃PbI₃”, Science 342, 341–347 (2013).DOI
  11. [11]Qian, J., Xu, B., and Tian, W., “A comprehensive theoretical study of halide perovskites ABX₃”, Organic Electron. 37, 61–73 (2016).DOI
  12. [12]Ponce, S., Schlipf, M., and Giustino, F., “Origin of Low Carrier Mobilities in Halide Perovskites”, ACS Energy Lett. 4, 456–463 (2019).DOI
  13. [13]Kumavat, S.R., Sonvane, Y., Singh, D., and Gupta, S.K., “Two-Dimensional CH₃NH₃PbI₃ with High Efficiency and Superior Carrier Mobility: A Theoretical Study”, J. Phys. Chem. C 123, 5231–5239 (2019).DOI
  14. [14]Herz, L. M., “Charge-Carrier Mobilities in Metal Halide Perovskites: Fundamental Mechanisms and Limits”, ACS Energy Lett. 2, 1539–1548 (2017).DOI
  15. [15]Edri, E. et al. “Why Lead Methylammonium Tri-Iodide Perovskite-Based Solar Cells Require a Mesoporous Electron Transporting Scaffold (but Not Necessarily a Hole Conductor)”, Nano Lett. 14, 1000–1004 (2014).DOI
  16. [16]Elbaz, G.A. et al., “Unbalanced Hole and Electron Diffusion in Lead Bromide Perovskites”, Nano Lett. 17, 1727–1732 (2017).DOI
  17. [17]Zhai, Y. et al. “Individual Electron and Hole Mobilities in Lead-Halide Perovskites Revealed by Noncontact Methods”, ACS Energy Lett. 5, 47–55 (2020).DOI
  18. [18]Yamada, Y., Nakamura, T., Endo, M., Wakamiya, A., and Kanemitsu, Y., “Photocarrier Recombination Dynamics in Perovskite CH₃NH₃PbI₃ for Solar Cell Applications”, J. Am. Chem. Soc. 136, 11610–11613 (2014).DOI
  19. [19]DeQuilettes, D.W. et al. “Impact of microstructure on local carrier lifetime in perovskite solar cells”, Science 348, 683 (2015).
  20. [20]Liu, S. et al. “Imaging the Long Transport Lengths of Photo-generated Carriers in Oriented Perovskite Films”, Nano Lett. 16, 7925–7929 (2016).DOI
  21. [21]Zhao, Z., Chen, X., Wu, H., Wu, X., and Cao, G., “Probing the Photovoltage and Photocurrent in Perovskite Solar Cells with Nanoscale Resolution”, Adv. Func. Mater. 26, 3048–3058 (2016).DOI
  22. [22]Marchioro, A. et al. “Unravelling the mechanism of photoinduced charge transfer processes in lead iodide perovskite solar cells”, Nat. Photonics 8, 250–255 (2014).DOI
  23. [23]Hutter, E.M. et al. “Charge Transfer from Methylammonium Lead Iodide Perovskite to Organic Transport Materials: Efficiencies, Transfer Rates, and Interfacial Recombination”, Adv. Energy Mater. 7, 1602349 (2017).DOI
  24. [24]Levine, I. et al. “Can we use time-resolved measurements to get steady-state transport data for halide perovskites?”, J. Appl. Phys. 124, 103103 (2018).DOI
  25. [25]Savenije, T.J., Guo, D., Caselli, V.M., and Hutter, E.M., “Quantifying Charge-Carrier Mobilities and Recombination Rates in Metal Halide Perovskites from Time-Resolved Microwave Photoconductivity Measurements”, Adv. Energy Mater. 10, 1903788 (2020).DOI
  26. [26]Rehman, W. et al. “Charge-Carrier Dynamics and Mobilities in Formamidinium Lead Mixed-Halide Perovskites”, Adv. Mater. 27, 7938–7944 (2015).DOI
  27. [27]Chu, Z. et al. “Unveiling defect-mediated carrier dynamics in monolayer semiconductors by spatiotemporal microwave imaging”, Proc. Natl. Acad. Sci. 117, 13908–13913 (2020).DOI
  28. [28]Eperon, G.E. et al. “Formamidinium lead trihalide: a broadly tunable perovskite for efficient planar heterojunction solar cells”, Energy Environ. Sci. 7, 982 (2014).DOI
  29. [29]Lee, J.-W. et al. “Formamidinium and Cesium Hybridization for Photo- and Moisture-Stable Perovskite Solar Cell”, Adv. Energy Mater. 5, 1501310 (2015).DOI
  30. [30]Yi, C. et al. “Entropic stabilization of mixed A-cation ABX₃ metal halide perovskites for high performance perovskite solar cells”, Energy Environ. Sci. 9, 656–662 (2016).DOI
  31. [31]Saliba, M. et al. “Cesium-containing triple cation perovskite solar cells: improved stability, reproducibility and high efficiency”, Energy Environ. Sci. 9, 1989–1997 (2016).pubmed.ncbi.nlm.nih.gov/27478500
  32. [32]Li, Z. et al. “Stabilizing Perovskite Structures by Tuning Tolerance Factor Formation of Formamidinium and Cesium Lead Iodide Solid-StateAlloys”, Chem. Mater. 28, 284–292 (2016).DOI
  33. [33]Chu, Z. et al. “Impact of grain boundaries on efficiency and stability of organic-inorganic trihalide perovskites”, Nat. Commun. 8, 2230 (2017).DOI
  34. [34]Chu, Z. et al. “Energy-Resolved Photoconductivity Mapping in a Monolayer–Bilayer WSe₂ Lateral Heterostructure”, Nano Lett. 18, 7200–7206 (2018).DOI
  35. [35]Chu, Z., Zheng, L., Lai, K. “Microwave Microscopy and Its Applications”, Annu. Rev. Mater. Res. 50, 105–130 (2020).DOI
  36. [36]Lai, K., Kundhikanjana, W., Kelly, M., and Shen, Z. X. “Modeling and characterization of a cantilever-based near-field scanning microwave impedance microscope”, Rev. Sci. Instrum. 79, 063703 (2008).DOI
  37. [37]Kato, T., Kaneko, T., “Transport dynamics of neutral excitons and trions in monolayer WS₂”, ACS Nano 10, 9687–9694 (2016).DOI
  38. [38]Cadiz, F. et al. “Exciton diffusion in WSe₂ monolayers embedded in a van der Waals heterostructure”, Appl. Phys. Lett. 112, 152106 (2018).DOI
  39. [39]Ugur, E. et al. “Carrier Extraction from Perovskite to Polymeric Charge Transport Layers Probed by Ultrafast Transient Absorption Spectroscopy”, J. Phys. Chem. Lett. 10, 6921–6928 (2019).DOI
  40. [40]Li, D. et al. “The Effect of Thermal Annealing on Charge Transport in Organolead Halide Perovskite Microplate Field-Effect Transistors”, Adv. Mater. 29, 1601959 (2017).DOI
  41. [41]Senanayak, S.P. et al. “Understanding charge transport in lead iodide perovskite thin-film field-effect transistors”, Sci. Adv. 3, e1601935 (2017).
  42. [42]Motta, C., El-Mellouhi, F., and Sanvito, S. “Charge carrier mobility in hybrid halide perovskites”, Sci. Rep. 5, 12746 (2015).DOI
  43. [43]Yun, J.S. et al. “Benefit of Grain Boundaries in Organic–Inorganic Halide Planar Perovskite Solar Cells”, J. Phys. Chem. Lett. 6, 875–880 (2015).DOI
  44. [44]Lee, D.S. et al. “Passivation of Grain Boundaries by Phenethylammonium in Formamidinium-Methylammonium Lead Halide Perovskite Solar Cells”, ACS Energy Lett. 3, 647–654 (2018).DOI
  45. [45]Sherkar, T.S. et al. “Recombination in Perovskite Solar Cells: Significance of Grain Boundaries, Interface Traps, and Defect Ions”, ACS Energy Lett. 2, 1214–1222 (2017).
  46. [46]Song, J., Zhou, Y., Padture, N.P., and Huey, B.D. “Anomalous 3D nanoscale photoconduction in hybrid perovskite semiconductors revealed by tomographic atomic force microscopy”, Nat. Commun. 11, 3308 (2020).DOI
  47. [47]Castro-Méndez, A.F., Hidalgo, J., and Correa-Baena, J.P. “The Role of Grain Boundaries in Perovskite Solar Cells”, Adv. Energy Mater. 9, 1901489 (2019).
  48. [48]Lin, Y. et al. “Perovskite solar cells with embedded homojunction via nonuniform metal ion doping”, Cell Rep. Phys. Sci. 2, 100415 (2021).DOI
  49. [49]Yin, W., Shi, T., and Yan Y. “Unique Properties of Halide Perovskites as Possible Origins of the Superior Solar Cell Performance”, Adv. Mater. 26, 4653 (2014).DOI
  50. [50]Li, Y. et al. “Direct Observation of Long Electron-Hole Diffusion Distance in CH₃NH₃PbI₃ Perovskite Thin Film”, Sci. Rep. 5, 14485 (2015).DOI
  51. [51]Tian, W., Zhao, C., Leng, J., Cui, R., and Jin, S. “Visualizing Carrier Diffusion in Individual Single-Crystal Organolead Halide Perovskite Nanowires and Nanoplates”, J. Am. Chem. Soc. 137, 12458 (2015).DOI
  52. [52]Saidaminov, M.I. et al. “Multi-cation perovskites prevent carrier reflection from grain surfaces”, Nat. Mater. 19, 412 (2020).DOI
  53. [53]Yin, W., Shi, T., and Yan Y. “Unusual defect physics in CH₃NH₃PbI₃ perovskite solar cell absorber”, Appl. Phys. Lett. 104, 063903 (2014).DOI
  54. [54]Zhang, X., Turiansky, M.E., Shen, J.-X., Van de Walle, C.G. “Iodine interstitials as a cause of nonradiative recombination in hybrid perovskites”, Phys. Rev. B 101, 140101(R) (2020).DOI
  55. [55]Yang, D. et al. “High efficiency planar-type perovskite solar cells with negligible hysteresis using EDTA-complexed SnO₂”, Nat. Commun. 9, 3239 (2018).DOI

Paper details

vlnc:W_ctk72zm4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents