Abstract

Silicon photonics faces a persistent challenge in extending photodetection capabilities beyond the 1.6 um wavelength range, primarily due to the lack of appropriate epitaxial materials. Colloidal quantum dots (QDs) present a promising solution here, offering distinct advantages such as infrared wavelength tunability, cost-effectiveness, and facile deposition. Their unique properties position them as a potential candidate for enabling photodetection in silicon photonics beyond the conventional telecom wavelength, thereby expanding the potential applications and capabilities within this domain. In this study, we have successfully integrated lead sulfide (PbS) colloidal quantum dot photodiodes (QDPDs) onto silicon waveguides using standard process techniques. The integrated photodiodes exhibit a remarkable responsivity of 1.3 A/W (with an external quantum efficiency of 74.8%) at a wavelength of 2.1 um, a low dark current of only 106 nA and a bandwidth of 1.1 MHz under a -3 V bias. To demonstrate the scalability of our integration approach, we have developed a compact 8-channel spectrometer incorporating an array of QDPDs. This achievement marks a significant step toward realizing a cost-effective photodetector solution for silicon photonics, particularly tailored for a wide range of sensing applications around the 2 um wavelength range.

Introduction

Silicon photonics is renowned for its capability to miniaturize complex bulk systems into cost-effective and robust chips, which find applications in fields ranging from data/tele communications to sensing[1, 2, 3]. Despite the widespread use of silicon photonics, current applications predominantly use light with wavelengths shorter than 1.6 μm\mu\mathrm{m}. This limitation is not a choice. Numerous applications, including environmental monitoring, medical diagnostics, and industrial sensing, would profit from photonic chips operating at longer wavelengths [4, 5]. Such applications are, however, hampered by the lack of a scalable and cost-effective integrated technology for photodetection beyond 1.6 μm1.6\,\mu\mathrm{m}.

Different strategies are being explored to extend the photodetection wavelength range of silicon photonics. A commonly used technique involves wafer or die bonding of III-V materials onto silicon, utilizing GaSb based compounds[6, 7, 8, 9]. However, this method requires large-area planarized surfaces and relies on costly III-V epitaxy and bonding technology. Also two-dimensional (2D) materials like graphene and black phosphorus are extensively investigated for on-chip photodetection beyond 1.6 μm1.6\,\mu\mathrm{m}[10]. The promise of these materials lies in the favorable substrate compatibility and broad absorption range, yet scalability poses a substantial hurdle for the practical integration of 2D photodetectors. Moreover, the performance of these photodetectors needs further improvement, for example to enhance dark current performance and responsivity[11, 12]. Alternatively, the direct deposition on Si of GeSn alloys[13, 14, 15, 16], III-V quantum dots[17], or poly-crystalline tellurium thin films[18] can result in cost-effective photodetectors with straightforward fabrication processes. However, the current implementations of these methods result in photodetectors with high dark current and low responsivity, necessitating further development.

To address the challenge of cost-effective photodetection beyond the telecom range in silicon photonics, colloidal quantum dots (QDs) offer a promising solution. First of all, QDs have economical advantage in both material synthesis and deposition processes. Synthesized through wet-chemical methods, they exhibit significantly lower material cost ($10 to $60 per gram)[19], and can be deposited as thin films on 200 mm silicon wafers through, for example, spin-coating or spray coating. The excellent compatibility of QDs with various substrates make QDs particularly well-suited for heterogeneous material integration, in stark contrast with more traditional III-V epitaxial semiconductors. Moreover, the absorption spectrum of QDs can be readily tuned across the infrared by adjusting the QD size and utilizing different materials. Photodetectors made from PbS\mathrm{PbS}[20, 21, 22, 23], HgTe\mathrm{HgTe}[24, 25], Ag2Se\mathrm{Ag_2Se}[26, 27] or InAs\mathrm{InAs}[28] QDs have all shown sensitivity for short-wave and mid-wave infrared light.

Given the appealing features of QDs, interest is growing in integrating QD-based emitters and detectors on photonic chips. In particular for visible light, electrically pumped light emitting devices and optically pumped lasers have been demonstrated by combining CdSe-based QDs with silicon nitride (SiN) photonic chips[29, 30, 31, 32, 33]. More recently, waveguide-coupled QD-based photodiodes operating at around 1.3 μm1.3\,\mu\mathrm{m} were demonstrated on the same SiN platform. This achievement underscored the potential of QDs as scalable photodetectors within photonic integrated circuits (PICs)[34]. For wavelengths beyond 1.6 μm1.6\,\mu\mathrm{m}, recent developments include the demonstration of plasmonic HgTe-based photoconductors on silicon waveguides[35] operating at 2.3 μm2.3\,\mu\mathrm{m} with a responsivity of 23 mA/W23\,\mathrm{mA/W}. On the other hand, PbS QD-based photodiodes (QDPDs) sensitive up to 2.1 μm2.1\,\mu\mathrm{m} with a responsivity of 0.385 A/W were achieved by sandwiching the QD film between a NiO p-type and a ZnO n-type contact[36]. Such reports point towards to promise of using integrated QDPDs for photodetection beyond 1.6 μ\mum, provided that low dark currents and high responsivity can be realized in integration-ready QDPD stacks.

In this work, we report on a silicon photonics, waveguide-coupled QD photodiode (WG-QDPD) that features a spectral response extending beyond 1.6 μ\mum. Leveraging an optimized QDPD design and a proven process flow[34], we demonstrate WG-QDPDs exhibiting a responsivity of 1.3 A/W at 2.1 μ\mum, a low dark current of 106 nA, and a bandwidth of 1.1 MHz. Moreover, we show that our WG-QDPD exhibits a low noise equivalent power (NEP) of 0.15 pW/Hz\sqrt{\mathrm{Hz}}, due to its high responsivity and low dark current, which is attractive for low-noise, weak signal detection. We demonstrate the reliability of the integration approach by realizing a compact on-chip spectrometer that features an array of 8 WG-QDPDs and operates in the spectral window between 2.063 and 2.135 μ\mum.

Results and Discussion

QDPDs with wavelength response up to 2.1 μ\mum

Before integrating QDPDs on waveguides, we optimized the material stack using dummy surface-illuminated QDPDs fabricated on glass-ITO substrates. Our approach involved adapting the p-i-n structure developed to form 1.3 μ\mum WG-QDPDs for PbS QDs with a band gap transition at 2.1 μ\mum[34]. All PbS QDs were synthesized by reacting lead oleate with a substituted thiourea, where different QD sizes were obtained by using differently substituted thioureas in agreement with literature[37]. The resulting PbS QDs have a surface terminated by lead oleate. More details on the synthesis and the materials characteristics can be found in APPENDIX A.

As shown in Figure 1a, we made QDPD stacks consisting of a 100 nm thick ITO transparent bottom electrode, a 30 nm thick sol-gel ZnO film functioning as an electron transport and hole blocking layer, a multilayer QD stack and an Au top electrode. Within the QD film, the photosensitive layer consisted of QDs with a band-gap transition at 2.1 μ\mum (APPENDIX A Figure 7). In a first design (Structure A in Figure 1a), this film – formed by spin coating – was exposed to a methanol solution containing 10 mg/mL tetra-n-butylammonium iodide (TBAI) for 30 s. This process removes as-synthesized surface ligands, thereby turning the QD film n-type and enhancing the electron mobility. As the hole transport and electron blocking layer, we employed a film of PbS QDs featuring a 0.94 μ\mum band-gap transition. This film was similarly exposed to a 0.01 vol% ethanedithiol (EDT) in methanol solution, which leads to p-type doping[38, 39], and a gold contact was evaporated on top.

Structure and characterization of QDPD

Figure 1. Structure and characterization of QDPD. (a) Vertical QDPD structures with surface illumination. (b) Influence of the interface layer on dark current density. (c) Dark current and photocurrent of Structure B QDPD, with an area of 1.77 mm21.77\ \mathrm{mm}^2. The photocurrent was measured with 2.1 μm2.1\ \mu\mathrm{m} laser gaussian beam illuminated from the bottom glass side, with a peak power density of 220 mW/cm2220\ \mathrm{mW}/\mathrm{cm}^2. Inset: responsivity of QDPD vs. bias voltage.

Absorption spectra for three types of QD inks

Figure 7. Absorption spectra for three types of QD inks (dispersed in n-octane) used in QPDDs.

However, as shown in Figure 1b (red line), this stack showed little rectification, and a dark current density of nearly 10 mA/cm210\,\mathrm{mA}/\mathrm{cm}^{2} at −2 V-2\,\mathrm{V} reverse bias, which is more than two orders higher than QDPDs using PbS QDs with 1.3 μm1.3\,\mu\mathrm{m} bandgap transition as photosensitive layers (APPENDIX § 8 Figure 8). In an attempt to reduce the dark current, we explored two additional QDPD stacks; a first in which the film of 2.1 μm2.1\,\mu\mathrm{m} PbS QDs was sandwiched between layers of 1.3 μm1.3\,\mu\mathrm{m} PbS QDs, which we also treated using TBAI and a second where the 1.3 μm1.3\,\mu\mathrm{m} PbS QDs were only included between the 2.12.1 and 0.94 μm0.94\,\mu\mathrm{m} PbS QD films, see Structure B and C in Figure 1a. Interestingly, structure B showed a strongly enhanced rectification and a 10-fold reduction of the dark current as compared to the initial stack, while structure C only featured a minor reduction of the dark current. This difference indicates that the primary source of dark current is the leakage of charge carriers between the 2.1 μm2.1\,\mu\mathrm{m} PbS QDs and the ZnO contact, possibly assisted through trap states at the ZnO surface [20], for which the 1.3 μm1.3\,\mu\mathrm{m} PbS QD film provides an additional barrier.

The optimized QDPD with Structure B was characterized with a 2.1 μm2.1\,\mu\mathrm{m} laser that had a power of 870 μW870\,\mu\mathrm{W} and a peak power density of 220 mW/cm2220\,\mathrm{mW}/\mathrm{cm}^{2}. Under a −3 V-3\,\mathrm{V} bias, the QDPD shows a dark current of 50.3 μA50.3\,\mu\mathrm{A} (dark current density of 2.8 mA/cm22.8\,\mathrm{mA}/\mathrm{cm}^{2} for a device area of 1.77 mm21.77\,\mathrm{mm}^{2}) and a responsivity of 0.19 A/W0.19\,\mathrm{A}/\mathrm{W} (external quantum efficiency, EQE, of 11.2%), as illustrated in Figure 1c. This relatively low EQE probably reflects the limited absorption of the vertically incident light in the thin layer of 2.1 μm2.1\,\mu\mathrm{m} PbS QDs, and the relatively low transmittance of ITO at 2.1 μm2.1\,\mu\mathrm{m} [36]. The 1.3 μm1.3\,\mu\mathrm{m} PbS-TBAI layer between the 2.1 μm2.1\,\mu\mathrm{m} PbS-TBAI and PbS-EDT layers should be n-doped [38], posing challenges for hole transport and potentially leading to an increase in the series resistance of the QDPD. However, the I-V characteristics at forward bias did not show degradation compared to Structure A (Figure 1b). Possibly, this layer is turned p-type during the subsequent EDT ligand exchange process for the 0.94 μm0.94\,\mu\mathrm{m} PbS QD layer on top. EDT, known for its high reactivity compared to TBAI [40], can soak the 1.3 μm1.3\,\mu\mathrm{m} PbS-TBAI layer underneath, resulting in a change of doping to p-type. To validate this hypothesis, QDPDs with Structure B were fabricated, but the ligand exchange of the top 1.3 μm1.3\,\mu\mathrm{m} PbS QDs was altered to EDT instead of TBAI. QDPDs with either TBAI or EDT ligand exchange on the 1.3 μm1.3\,\mu\mathrm{m} QDs exhibited nearly identical dark and light I-V characteristics (APPENDIX § 8 Figure 9), thus confirming our above assumption. The spectral response of the QDPD with structure B was measured by sweeping the laser wavelength, showing photo response extending up to 2.2 μm2.2\,\mu\mathrm{m} (APPENDIX § 8 Figure 10), consistent with the absorption spectrum of the QDs. More details regarding the fabrication of the QDPD can be found in APPENDIX § 9.

Integration of QDPDs on waveguides

Figure 2a-Figure 2e depicts the process flow used to integrate the QDPD on waveguides. In a first step, waveguides were defined on silicon-on-insulator (SOI) substrates with a 2 μm2\ \mu\mathrm{m} buried oxide and a 220 nm220\ \mathrm{nm} silicon layer, employing a 70 nm70\ \mathrm{nm} shallow etch. To alleviate the power saturation problem of WG-QDPDs, as observed in previous demonstration at shorter wavelength on the SiN platform[34], we defined 30 μm30\ \mu\mathrm{m} wide waveguides. This adjustment serves to lower the optical power density in the QD film. Next, the waveguide was planarized by flowable oxide (hydrogen silsesquioxane, HSQ), followed by annealing at 400 ∘C400\ ^\circ\mathrm{C} in N2N_2 to increase the physical and chemical stability of HSQ. This step resulted in a 45 nm45\ \mathrm{nm} top cladding on the waveguides, shown in light blue in Figure 2a. As outlined in Figure 2b-Figure 2e, the QDPD stack was then integrated on top, starting with sputtering of an 18 nm18\ \mathrm{nm} thick ITO layer as the bottom electrode. The ITO had a sheet resistance of 173 Ω/□173\ \Omega/\square, and the layer thickness was reduced as compared to the dummy surface-illuminated QDPD structure in order to minimize optical losses in the ITO and maximize light absorption in the PbS QD film. To further reduce optical loss, the ITO layer was restricted to the designated area for photodetection using HCl-based wet etching. Next, we deposited the ZnO layer using sol-gel chemistry and patterned it using a dilute HCl solution. Complete coverage of ITO with ZnO is crucial to prevent direct contact between ITO and the subsequently deposited QD film, as this could lead to a significant leakage current. Ti/Au (2020 nm / 100100 nm) was placed on the side of the waveguides as the n-contact pad using a lift-off technique. The same QD stacks with structure B, as we used in the surface-illuminated QDPD, were deposited layer by layer and lifted off simultaneously to achieve the desired pattern. PMMA resist was used for its excellent chemical compatibility with the methanol solvent involved during QDs deposition. Finally, 8080 nm Au was deposited on top as p-contact pads through thermal evaporation and lift-off. The cross-section of the fabricated WG-QDPD is shown in Figure 2f. More details on the integration process can be found in APPENDIX § 10.

Integration steps to fabricate WG-QDPD

Figure 2. Integration steps to fabricate WG-QDPD. (a) Si rib waveguide patterning and planarization. (b) ITO sputtering and patterning with wet etching, followed by ZnO deposition with sol-gel method and patterning with wet etching. (c) N-contact metal patterning with liftoff. (d) QD film patterning with PMMA resist and liftoff. (e) P-contact metal patterning with PMMA resist and liftoff. (f) Cross-section of fabricated WG-QDPD.

Characterization of WG-QDPD

We characterized the WG-QDPDs using a 2.12.1 μ\mum laser, employing grating couplers for convenient light coupling into and out of the waveguide. The optical power in the waveguide was calibrated by measuring the coupling efficiency of the grating coupler for a reference waveguide without QDPDs. The WG-QDPD showed a dark current of 106106 nA at −3-3 V, as illustrated in Figure 3a. Considering a WG-QDPD width of 3030 μ\mum and a length of 200200 μ\mum, the dark current density (1.81.8 mA/cm2^2) is in line with the measurements obtained on the surface-illuminated QDPDs (2.82.8 mA/cm2^2), indicating that the integration process does not introduce spurious leakage paths. The responsivity reaches 1.31.3 A/W (EQE of 74.874.8%) at an optical power of 116116 nW, as shown in Figure 3b. The significantly higher EQE compared to surface-illuminated QDPDs is attributed to increased absorption. during propagation within the waveguides. For WG-QDPDs, the Si and QD stack constitute the hybrid waveguide designed for the propagation of the fundamental TE mode. Light is absorbed via the evanescent tail of the optical mode during its propagation, as depicted in Appendix § 10, Figure 11. In contrast to surface-illuminated QDPDs, which require a thick QD absorption layer for efficient light absorption, the extended absorption path of guided light in WG-QDPDs ensures efficient absorption even with a thin layer of QD. The combination of low dark current and high responsivity leads to a low estimated noise equivalent power (NEP=2Idarkq/R\mathrm{NEP}=\sqrt{2I_{\mathrm{dark}}q}/R, where qq is the elementary charge, and RR is the responsivity) of 0.15 pW/Hz\sqrt{\mathrm{Hz}}, indicating that WG-QDPDs are well-suited for weak signal detection. The photo-current exhibits nonlinear growth with optical power, a phenomenon attributed to QDPD saturation due to high series resistance, as observed in prior studies[34].

Response of WG-QDPDs

Figure 3. Response of WG-QDPDs. (a) I-V curves of WG-QDPDs under dark condition and illumination at 2.1 μm2.1\,\mu\mathrm{m}. (b) Responsivity vs. optical power at -3 V bias voltage. Inset: photo-current vs. optical power. (c) Bandwidth of the integrated WG-QDPD.

The speed of the fabricated WG-QDPD was measured at 1.55 μ\mum, exhibiting a bandwidth of 1.1 MHz, as shown in Figure 3c. Under large reverse bias of -3V, the thin QD absorption layer can be considered completely depleted41. Therefore, the response time (τres\tau_{res}) of the photodetector is determined by the drift progress (τdrift\tau_{drift}) and the resistance-capacitance constant (τRC\tau_{RC}) of the electrical circuit τres=τdrift2+(2.2τRC)2\tau_{res}=\sqrt{\tau_{drift}^{2}+(2.2\tau_{RC})^{2}}42. The drift time τdrift\tau_{drift} is governed by the carrier mobility (μ\mu) and the voltage drop (VV) across the depleted film thickness (dd), with τdrift=d2μV\tau_{drift}=\frac{d^{2}}{\mu V}. The other term, τRC=RC\tau_{RC}=RC, where RR represents the series resistance and CC denotes the capacitance. For a fully depleted QDPD, we estimate the series resistance RR using the access resistance (ITO sheet resistance and contact resistance between n-contact and ZnO), measured to be approximately 100 Ω\Omega for our WG-QDPDs. The capacitance CC is estimated to be around 4.1 pF (C=ε0εrAdC=\frac{\varepsilon_{0}\varepsilon_{r}A}{d}, where ε0\varepsilon_{0} represents the vacuum permittivity, εr=15.5\varepsilon_{r}=15.5 denotes the dielectric constant of the PbS-QD film41, A=6000 μm2A=6000\ \mu\mathrm{m}^{2} is the area of QDPD and d=195d=195 nm is the thickness of the PbS QD film). The estimated τRC\tau_{RC} is 0.41 ns, corresponding to a BW of 388 MHz using the relationship: BW = 0.35/τres\tau_{res}42. Considering a measured BW of 1.1 MHz, the speed of our WG-QDPD is likely drift-limited. Furthermore, we measured the BW of WG-QDPDs with areas of 6000 μm2\mu\mathrm{m}^{2} and 600 μm2\mu\mathrm{m}^{2}, both exhibiting similar bandwidths (see APPENDIX § 11 Figure 13). This area-insensitive BW is contrary to the scenario where τRC\tau_{RC} dominates the speed of QDPDs[23] [41], considering a consistent series resistance and area-related capacitance. This drift-limit speed can be further supported by examining τdrift\tau_{drift}.

The carrier mobility of the 2.1 μ\mum PbS-TBAI absorption layer, extracted via field effect transistor (FET) measurements41, is (0.94 ±\pm 0.6) ×10−4\times10^{-4} cm2^{2}V−1^{-1}s−1^{-1} for electrons and (1.41 ±\pm 0.35) ×10−4\times10^{-4} cm2^{2}V−1^{-1}s−1^{-1} for holes. Considering a thickness of 75 nm for the absorption layer and a voltage drop of 3V, the estimated τdrift\tau_{drift} is around 0.2 μ\mus, corresponding to a bandwidth of 1.75 MHz. The carrier transition time in the 1.3 μ\mum PbS-TBAI and 0.94 μ\mum PbS-EDT layers is disregarded due to the significantly faster carrier mobilities exceeding 1×10−3 cm−2V−1s−11 \times10^{-3}\,\mathrm{cm}^{-2}\mathrm{V}^{-1}\mathrm{s}^{-1} in both layers41. Although the bandwidth of our demonstrated WG-QDPDs may not be as high as that of III-V photodiodes, it meets the requirements of many sensing applications. Further improvement on the speed of the WG-QDPD relies on improved ligand exchange strategies to boost the mobility of the 2.1 μm2.1\,\mu\mathrm{m} PbS QD layer. Reducing the thickness of the QD film can also decrease τdrift\tau_{drift}. This strategy was recently adopted to achieve QDPDs with a response time of 4 ns41. More details on the characterization of WG-QDPDs can be found in APPENDIX § 11.

On the same chip, we incorporated WG-QDPDs with varying lengths, as shown in Figure 4a. We conducted transmission measurements on the waveguides after patterning each material. These measurements allowed us to ascertain the optical loss induced by each material, as shown in Figure 4b. The ITO layer introduced an optical loss of around 0.02 dB/μm0.02\,\mathrm{dB}/\mu\mathrm{m}, resulting from strong free carrier absorption in the infrared43. The addition of the ZnO layer did not introduce measurable extra absorption. The entire QDPD stack raised the optical loss to 0.08 dB/μm0.08\,\mathrm{dB}/\mu\mathrm{m}, indicating the absorption is dominated by the QD film. This strong absorption competes with the absorption from the ITO bottom electrode, ensuring high responsivity of our WG-QDPDs. The dark current of these WG-QDPDs is proportional to the area, with a slope of 1.8 mA/cm21.8\,\mathrm{mA}/\mathrm{cm}^{2}, as shown in Figure 4c. The responsivity of WG-QDPDs, measured at -3 V bias and 400 nW optical power, shows a saturation behavior with respect to PD length, as shown in Figure 4d. The saturation behavior aligns with the prediction from optical loss measurements, as indicated by the blue dashed line in Figure 4d.

Performance of WG-QDPDs with different lengths

Figure 4. Performance of WG-QDPDs with different lengths. (a) Top view of WG-QDPDs. (b) Optical absorption resulting from materials integrated onto waveguides. Measurements were obtained through optical transmission, with varying lengths for each material. (c) Dark current of devices with different area. (d) Responsivity of WG-QDPDs with different lengths. The predicted relationship between responsivity and length is presented by a dashed blue line, derived from optical loss measurements shown in Figure 4b.

We also investigated WG-QDPDs with different shapes as shown in Figure 5a. As we mentioned before, the waveguide width is extended to 30 μ\mum to alleviate the optical power saturation, ensuring an efficient responsivity. However, this strategy also increases dark current due to the larger WG-QDPD area. Consequently, the NEP exhibits a trade-off between responsivity and dark current. Notably, heavy optical power saturation predominantly occurs in the initial section of the WG-QDPD. As light propagates within the waveguides, the optical power decreases exponentially. This insight allows us to narrow down the waveguide width at the far end without introducing significant power saturation. In our design, we implemented waveguide narrowing from 30 μ\mum to 0.9 μ\mum using both linear and exponential tapers, while keeping a consistent length of 200 μ\mum. For the exponential taper, the width decreases at a rate of 0.023 μ\mum−1^{-1} (0.1 dB/μ\mum), similar to the optical absorption measurement in Figure 4b. The QDPD follows the same shape as these tapered waveguides. The linear taper reduces the WG-QDPD area to approximately 1/2, and the exponential taper further decreases the area to around 1/3. Consequently, the decrease in area reduces the dark current to 1/2 and 1/3, respectively, as shown in Figure 5b. As expected, the responsivity of the tapered devices does not degrade significantly, as shown in Figure 5c. This results in a champion NEP of 0.13 pW/Hz\sqrt{\mathrm{Hz}} for the exponentially tapered WG-QDPD, representing a 30% improvement compared to the NEP of the uniform WG-QDPD (0.18 pW/Hz\sqrt{\mathrm{Hz}}).

Performance of WG-QDPDs with different shapes

Figure 5. Performance of WG-QDPDs with different shapes. (a) Top view of WG-QDPDs. Light is coupled into waveguides from the left side. (b) Dark current of different WG-QDPDs. (c) Responsivity of different WG-QDPDs.

Notably, there is an underestimation of the NEP here. The measurements were conducted at a relatively high optical power of 400 nW, which, combined with the nonlinear response to optical power, results in an underestimated responsivity.

We also fabricated a grating-assisted QDPD, where light injected from the left side was scattered vertically and absorbed by the QDPD, as shown in Figure 5a. This configuration yielded the lowest dark current due to the smallest QDPD size of 30 μ\mum by 30 μ\mum. However, the responsivity was significantly lower compared to the evanescent coupling scheme. The degradation in responsivity is attributed to a combined effect of upwards coupling efficiency, incomplete optical absorption in the thin QDs layer, and possibly stronger power saturation.

Demonstration of a 2.1 μ\mum integrated spectrometer

To demonstrate what complex tasks our proposed WG-QDPD integration approach can complete, we combined a WG-QDPD array with an eight-channel planar concave grating (PCG), forming a compact spectrometer, as shown in Fig. 6a. The PCG, designed with IPKISS44, has a central wavelength of 2.1 µm and a wavelength range of around 70 nm. The fabrication was carried out on the same 220 nm SOI chip alongside the aforementioned components. To simplify the fabrication process, we used 70 nm shallow-etched distributed bragg reflectors (DBR) as retroreflectors45. FDTD simulations revealed that these DBR mirrors, with a period of 437 nm, exhibit reflection centered at 2.1 µm (>90%) and a 3 dB bandwidth of 200 nm, meeting the PCG requirements.

The transmission spectrum of the PCG was measured prior to QDPD integration, with a tunable laser around 2.1 µm (IPG Cr:ZnS/Se). The fabricated PCG covers a wavelength range from 2063 nm to 2135 nm, with a cross-talk better than -20 dB and insertion loss less than 3 dB, as shown in Fig. 6b, consistent with design metrics.

For the WG-QDPDs, we used a width of 30 µm and a length of 200 µm, to obtain an efficient photo response. After integrating the WG-QDPD array, the photo-response of each channel was measured at -1 V bias by sweeping the wavelength of the input laser. The response of the QDPD array aligns with the spectrum of the grating coupler (gray line in Fig. 6c), as measured from a reference WG-QDPD without the PCG. This consistent spectral shape indicates uniform responses of the WG-QDPDs, thereby suggesting its potential for scalable integration. The array of WG-QDPDs was measured directly without requiring further calibration. This type of spectrometer is interesting for sensing applications, such as glucose concentration monitoring.

Compact spectrometer based on a WG-QDPD array and planar concave grating

Figure 6.

Image not extracted

Figure 6 (PDF p. 12). Compact spectrometer based on a WG-QDPD array and a planar concave grating. (a) Top view of the spectrometer. Light is injected from the grating coupler on the right side. (b) Transmission spectrum of the planar concave grating. (c) Response of WG-QDPDs from eight channels and a reference waveguide (gray line).

Discussion

Compared with previously reported plasmonic HgTe QD photoconductors integrated on silicon waveguides[35], our integration approach achieves a similar level of dark current (106 nA), demonstrating more than one-order improvement in responsivity (1.3 A/W) and two-order improvement in bandwidth (1.1 MHz). When compared to alternative approaches for extending photodetection capabilities on the SOI platform, our proposed WG-QDPDs remain competitive in terms of dark current and responsivity. Notably, these results are on par with the best-performing bonded III-V photodetectors reported in the literature (responsivity 0.4-1.4 A/W around 2.3 μm, dark current 10 nA-2.5 μA)[6, 8, 9] [46], outperforming monolithically grown GeSn (responsivity <0.52 A/W, dark current >1 mA)[13, 14, 15, 16]. Another class of heterogeneous materials, 2D materials like graphene47 or black phosphorus48,49, also possess the potential to operate beyond the telecommunication wavelength. However, they face challenges in achieving high responsivity (0.07-0.3 A/W at wavelength of 2-3 μm)[11, 12] [50] and scalable integration. It is acknowledged that, despite advancements, the bandwidth of our WG-QDPD still lags behind compared to the GHz bandwidth demonstrated by other approaches51–53. Furthermore, additional efforts are necessary to mitigate the nonlinear response of our WG-QDPD.

The performance of the WG-QDPD could be further improved by optimizing the device structure. Previous reports on QDPDs at 2.1 μm have demonstrated an impressively low dark current density of 10−510^{-5} A/cm² and high responsivity[36]. Implementing such advancements could reduce the dark current of integrated photodetectors to sub-nanoampere levels, which is particularly advantageous for the detection of weak signals in sensing applications.

Also exploring alternative materials for long wavelength WG-QDPDs, such as HgTe[25] [54, 55] and Ag₂Se[26, 27], is compelling to extend the photodetection capabilities within silicon photonics into the mid-infrared range, aligning with heightened interest in sensing applications. Ag₂Se QDs, which rely on intra-band absorption, is thereby the more attractive material because of the greatly reduced toxicity. However, efforts are still needed to improve the responsivity and reduce the dark current for these materials.

CONCLUSION

In this work, we have demonstrated the integration of PbS QDPDs onto silicon waveguides, extending the photodetection capabilities beyond the traditional telecommunication range in silicon photonics. The achieved results at room temperature, including a low dark current of 106 nA106\,\mathrm{nA}, a high responsivity of 1.3 A/W1.3\,\mathrm{A/W} at 2.1 μm2.1\,\mu\mathrm{m}, and a bandwidth of 1.1 MHz1.1\,\mathrm{MHz}, highlight the effectiveness of our approach. The scalability of our integration method is exemplified through the presentation of an 8-channel compact spectrometer integrated with a WG-QDPD array. This integrated system offers a promising solution for on-chip spectroscopy around 2.1 μm2.1\,\mu\mathrm{m}. We believe that QDPD technology holds significant promise for cost-effective photodetection in the near and mid-infrared ranges in silicon photonics, especially for diverse sensing applications. Future work should focus on improving the QDPD characteristics, including detectivity, bandwidth and linearity, and extending sensing wavelength range.

ACKNOWLEDGMENTS

This work was supported by: European Research Council (ERC) under the innovation program grant agreement No. 884963 (ERC AdG NARIOS), FWO-Vlaanderen for research funding (FWO projects G0B2921N and G0C5723N), and China Scholarship Council (CSC Grant 201906120023).

DATA AVAILABILITY

Data available on request from the authors.

APPENDIX

SYNTHESIS OF MATERIALS

Synthesis of 2.1 μm2.1\,\mu\mathrm{m} PbS QDs. Lead oleate and N-n-hexyl-N’-dodecyl thiourea were prepared according to the procedure described by Hendricks et al.37. In a three-neck flask, 1.2 mmol1.2\,\mathrm{mmol} lead oleate (0.9241 g0.9241\,\mathrm{g}) was dissolved in 20 mL20\,\mathrm{mL} n-dodecane at 150 ∘C150\,^\circ\mathrm{C} under nitrogen atmosphere. Separately, N-n-hexyl-N’-dodecylthiourea (1 mmol1\,\mathrm{mmol}, 0.3286 g0.3286\,\mathrm{g}) was mixed with 1 mL1\,\mathrm{mL} of diglyme (Diethylene Glycol Dimethyl Ether) in a vial and heated to 150 ∘C150\,^\circ\mathrm{C}. The pre-heated thiourea solution was then injected swiftly into the lead oleate solution via a syringe and the reaction was allowed to run for 20 minutes at 150 ∘C150\,^\circ\mathrm{C}. Subsequently, the flask was cooled down to ambient temperature by immersion into a water bath. The final dispersion underwent four purification cycles inside a nitrogen-filled glovebox, using a solvent mixture of 4:1 toluene to hexane, with methyl acetate as the non-solvent. The purified PbS QDs were dispersed in anhydrous n-octane to achieve the desired concentration.

Synthesis of 0.94 μm\mu\mathrm{m} PbS QDs. Lead oleate and N-(3,5-bis(trifluoromethylphenyl))-N′-phenylthiourea were synthesized according to [37]. In a three-neck flask, 7.00 mmol lead oleate (5.38 g) was dissolved in 25 mL anhydrous n-octane at 90 °C under a nitrogen atmosphere. In a vial, 4.67 mmol of N-(3,5-bis(trifluoromethylphenyl))-N′-phenylthiourea (1,70 g, 1 eq.) and 2 mL of 1-methoxy-2-(2-methoxyethoxy)ethaan were mixed and heated to 90 °C as well. The thiourea solution was then quickly injected into the lead oleate solution via a syringe and the flask was cooled down to room temperature by immersion into a water batch after one minute. The resulting dispersion was purified four times by aid of n-octane and acetone and stored in anhydrous n-octane for further use.

Synthesis of 1.3 μm\mu\mathrm{m} PbS QDs. In a three-neck flask, 2 mmol lead oleate (1.54 g) was dissolved in 20 mL n-dodecane at 120 °C under a nitrogen atmosphere, and flushed for 30 min. Next, 1.5 mmol of N-(p-(trifluoro-methyl)phenyl)-N′-dodecylthiourea (0.5828 g) was mixed with 1 mL of 1-methoxy-2-(2-methoxyethoxy)ethaan or diglyme under nitrogen atmosphere, preheated at 120 °C and quickly injected in the lead oleate solution at 120 °C. The reaction mixture was cooled down to room temperature by immersing the flask in a water bath after 80 sec. The resulting dispersion was then purified at least four times by aid of n-octane and acetone and stored in anhydrous n-octane for further use.

Dark Current Suppression

Structure and characterization of QDPD with 1.3 µm and 2.1 µm PbS active layers, showing QDPD structures and dark current density

Figure 8. Structure and characterization of QDPD with 1.3 µm and 2.1 µm PbS active layers. (a) QDPD structures. (b) Dark current density.

Dark current and photocurrent of QDPD with an area of 1.77 mm²

Figure 9. Dark current and photocurrent of QDPD with an area of 1.77 mm². The photocurrent was measured with 2.1 µm laser with a gaussian beam illuminating the sample from the bottom glass side, with a peak power density of 220 mW/cm². Red: ZnO / 1.3 µm-PbS-

TBAI / 2.1 µm-PbS-TBAI / 1.3 µm-PbS-TBAI / 0.94 µm-PbS-EDT. Blue: ZnO / 1.3 µm-PbS-TBAI / 2.1 µm-PbS-TBAI / 1.3 µm-PbS-EDT / 0.94 µm-PbS-EDT.

Spectral response of the QDPD with structure B

Figure 10. Spectral response of the QDPD with structure B, measured at a bias of -1 V and a peak power density of 220 mW/cm².

QDPD Fabrication

Substrates with 100 nm ITO on glass (2 cm × 1.5 cm, Ossila) were cleaned in acetone and isopropanol with sonication, followed by exposure to O₂ plasma (PVA TePla 600) for 10 min. A 30 nm layer of ZnO was then formed on top of the ITO layer via spin-coating a precursor solution and annealing at 325 °C for 30 minutes in ambient air. Following this, PbS QDs were spin-coated onto the ZnO layer, with subsequent treatment involving either 10 mg/mL tetra-n-butylammonium iodide (TBAI) in methanol or 0.01 vol% ethanedithiol (EDT) in methanol. The ligand exchange process for each cycle lasted 30 seconds, followed by two washes with methanol. Each cycle resulted in a film with a thickness of 25 nm for 2.1 µm PbS-TBAI, 30 nm for 1.3 µm PbS-TBAI, and 30 nm for 0.94 µm PbS-EDT. The QDs and ligand exchange steps were repeated multiple times to achieve the desired thickness. Finally, an 80 nm layer of gold was evaporated on top using a shadow mask, forming QDPD pixels with a diameter of 1.5 mm.

WG-QDPD Fabrication

Waveguides fabrication. Waveguides were patterned with E-beam lithography (EBL) and dry etching. We used standard SOI substrates with 220 nm Si on top of 2 µm buried oxide in this work. 400 nm ARP6200.13 e-beam resist was used as a mask, exposed by EBL (Voyager Raith 50 kV) with a dose of 160 µC/cm² and developed in n-amyl acetate for 60 s. The resist pattern was transferred to Si by reactive ion etching (ICP-RIE, Oxford Instruments) using SF₆ and CHF₃ chemistry. A 70 nm shallow etch in Si was used to define the optical structures. We then spin-coated the flowable oxide hydrogen silsesquioxane (HSQ, Dow FOX-15) on top of the sample as a top cladding layer. Diluted HSQ (HSQ : MIBK = 1:4) was spun with a speed of 4000 rpm and an acceleration of 1000 rpm/s. The sample was then cured at 400 °C for 2 hours in a nitrogen atmosphere, achieving a cladding thickness of approximately 45 nm.

ITO deposition and patterning. 18 nm thick ITO was deposited on the sample by magnetron sputtering. Then the ITO film was patterned with photolithography (AZ5214 E) and wet etching (37% HCl:H2O=1:5, 15s).

**ZnO deposition and patterning.**30 nm thick ZnO was deposited on the sample using the same solgel method outlined in APPENDIX C. Subsequently, the ZnO film underwent patterning through photolithography (AZ5214 E) followed by wet etching (37% HCl:H2O = 1:1000, 5s).

N-contact deposition and patterning. The N-contact was patterned using photolithography and the liftoff method. The desired pattern was generated using AZ5214 E photoresist, followed by metal evaporation with a composition of 20 nm Ti and 100 nm Au. The sacrificial photoresist and the metal layer on top were removed by immersing the sample in acetone for 1 hour.

QDs deposition and patterning. The QD film was patterned using EBL and the liftoff method. The desired pattern was generated using 400 nm thick ARP672.08 e-beam resist and EBL. Then QD stacks were spin-coated on top with the same procedure in APPENDIX C. The sacrificial e-beam resist and QDs on top were removed by immersing the sample in acetone for 10 min. PMMA has good chemical compatibility with the solvent involved (n-octane and methanol) in QDs deposition.

P-contact deposition and patterning. The P-contact was patterned using EBL and the liftoff method. The desired pattern was generated using 1 µm thick ARP672.08 e-beam resist and EBL. In this process, the e-beam resist baking was adjusted to 60 °C for 5 min on the hotplate, deviating from the standard 150 °C baking temperature. This modification aimed at protecting QDs and avoiding dark current degradation. A short sonication step was incorporated at the end of e-beam resist development to ensure a clean interface between QDs and the P-contact metal. Subsequently, an 80 nm thick layer of Au was evaporated as the P-contact metal. The sacrificial e-beam resist and the layer of QDs on top were removed by immersing the sample in acetone for 30 minutes.

Intensity profile of the fundamental TE mode in the WG-QDPD

Figure 11. Intensity profile of the fundamental TE mode in the WG-QDPD. The cross-section at position x=0x=0 is shown in the right figure.

Light is absorbed through the evanescent tail of the optical mode extended into the 2.1 μm2.1\,\mu\mathrm{m} QD film.

WG-QDPD Characterization

For DC measurements, a 2.1 μm2.1\,\mu\mathrm{m} laser (Cr2+^{2+}:ZnS laser, IPG Photonics) was coupled to a ZrF4_4 fiber and then further coupled to the WG-QDPD through a grating coupler. I-V curves were characterized with a source measure unit (Keithley 2400).

For AC measurements, the setup, as illustrated in Figure 12, involved a 1.55 μm1.55\,\mu\mathrm{m} laser (Santec 510) that was modulated by a Mach-Zehnder electro-optical modulator (EOM). The EOM was adjusted to its linear operation point, where applied radio frequency signals (SMT03, Rohde & Schwarz) were converted to optical intensity modulation. The modulated optical signals were amplified by Erbium-doped fiber amplifier (EDFA) and then coupled to the WG-QDPD through edge coupling. Polarization controllers (PC) were employed before the EOM and our chip to achieve the desired polarization. A DC bias was applied to the WG-QDPD using a source measure unit (Keithley 2400). The photodetector signal was collected by an electrical spectrum analyzer (ESA, FSP, Rohde & Schwarz). Both the DC bias and ESA were connected to the WG-QDPD with a bias tee.

Setup schematics used for bandwidth measurement

Figure 12. Setup schematics used for bandwidth measurement. PC: polarization controller, EOM: electro-optical modulator, EDFA: Erbium-doped fiber amplifier, RF: radio-frequency source, ESA: electrical spectrum analyzer.

Bandwidth of WG-QDPDs with different areas

Figure 13. Bandwidth of WG-QDPDs with different areas. WG-QDPDs, with a dimension of 30 μm×200 μm30\,\mu\mathrm{m} \times200\,\mu\mathrm{m} and 3 μm×200 μm3\,\mu\mathrm{m} \times200\,\mu\mathrm{m}, were measured under a reverse bias of -5 V.

References

  1. [1]M. Traverso, M. Mazzini, K. Lakshmikumar, S. Sunder, A. Kurylak, C. Appel, C. Muzio, R. Tummidi, A. Cervasio, M. Nadeau, W. Li, J. Neiman, and M. Webster, “Integrated silicon photonics transceiver module for 100Gbit/s 20km transmission,” in Optics InfoBase Conference Papers, (Optica Publishing Group (formerly OSA), 2021).DOI
  2. [2]² N. Margalit, C. Xiang, S.M. Bowers, A. Bjorlin, R. Blum, and J.E. Bowers, “Perspective on the future of silicon photonics and electronics,” Appl Phys Lett 118(22), (2021).DOI
  3. [3]³ A.Z. Subramanian, E. Ryckeboer, A. Dhakal, F. Peyskens, A. Malik, B. Kuyken, H. Zhao, S. Pathak, A. Ruocco, A. De Groote, P. Wuytens, D. Martens, F. Leo, W. Xie, U.D. Dave, M. Muneeb, P. Van Dorpe, J. Van Campenhout, W. Bogaerts, P. Bienstman, N. Le Thomas, D. Van Thourhout, Z. Hens, G. Roelkens, and R. Baets, “Silicon and silicon nitride photonic circuits for spectroscopic sensing on-a-chip [Invited],” Photonics Res 3(5), B47 (2015).
  4. [4]⁴ R. Wang, A. Vasiliev, M. Muneeb, A. Malik, S. Sprengel, G. Boehm, M.-C. Amann, I. Šimonytė, A. Vizbaras, K. Vizbaras, R. Baets, and G. Roelkens, “III–V-on-Silicon Photonic Integrated Circuits for Spectroscopic Sensing in the 2–4 μm Wavelength Range,” Sensors 17(8), (2017).DOI
  5. [5]⁵ T. Hu, B. Dong, X. Luo, T.-Y. Liow, J. Song, C. Lee, and G.-Q. Lo, “Silicon photonic platforms for mid-infrared applications [Invited],” Photonics Res 5(5), 417 (2017).DOI
  6. [6]⁶ E. Ryckeboer, A. Gassenq, M. Muneeb, N. Hattasan, S. Pathak, L. Cerutti, J.B. Rodriguez, E. Tournié, W. Bogaerts, R. Baets, and G. Roelkens, “Silicon-on-insulator spectrometers with integrated GaInAsSb photodiodes for wide-band spectroscopy from 1510 to 2300 nm,” Opt Express 21(5), 6101–6108 (2013).DOI
  7. [7]⁷ N. Hattasan, A. Gassenq, L. Cerutti, J.B. Rodriguez, E. Tournié, and G. Roelkens, “Heterogeneous integration of GaInAsSb p-i-n photodiodes on a silicon-on-insulator waveguide circuit,” IEEE Photonics Technology Letters 23(23), 1760–1762 (2011).DOI
  8. [8]⁸ A. Gassenq, N. Hattasan, L. Cerutti, J.B. Rodriguez, E. Tournié, and G. Roelkens, “Study of evanescently-coupled and grating-assisted GaInAsSb photodiodes integrated on a silicon photonic chip,” Opt Express 20(11), 11665 (2012).DOI
  9. [9]R. Wang, S. Sprengel, M. Muneeb, G. Boehm, R. Baets, M.-C. Amann, and G. Roelkens, “2 μm wavelength range InP-based type-II quantum well photodiodes heterogeneously integrated on silicon photonic integrated circuits,” Opt Express 23(20), 26834 (2015).DOI
  10. [10]M. Long, P. Wang, H. Fang, and W. Hu, “Progress, Challenges, and Opportunities for 2D Material Based Photodetectors,” Adv Funct Mater 29(19), (2019).DOI
  11. [11]X. Wang, Z. Cheng, K. Xu, H.K. Tsang, and J. Bin Xu, “High-sensitivity graphene/silicon-heterostructure waveguide photodetectors,” Nat Photonics 7(11), 888–891 (2013).DOI
  12. [12]J. Guo, J. Li, C. Liu, Y. Yin, W. Wang, Z. Ni, Z. Fu, H. Yu, Y. Xu, Y. Shi, Y. Ma, S. Gao, L. Tong, and D. Dai, “High-performance silicon–graphene hybrid plasmonic waveguide photodetectors beyond 1.55 μm,” Light Sci Appl 9(1), (2020).DOI
  13. [13]Y.H. Peng, H.H. Cheng, V.I. Mashanov, and G.E. Chang, “GeSn p-i-n waveguide photodetectors on silicon substrates,” Appl Phys Lett 105(23), (2014).DOI
  14. [14]C.-H. Tsai, K.-C. Lin, C.-Y. Cheng, K.-C. Lee, H.H. Cheng, and G.-E. Chang, “GeSn lateral p-i-n waveguide photodetectors for mid-infrared integrated photonics,” Opt Lett 46(4), 864 (2021).DOI
  15. [15]S. Ghosh, R. Bansal, G. Sun, R.A. Soref, H.H. Cheng, and G.E. Chang, “Design and Optimization of GeSn Waveguide Photodetectors for 2-μm Band Silicon Photonics,” Sensors 22(11), (2022).DOI
  16. [16]C.-H. Liu, R. Bansal, C.-W. Wu, Y.-T. Jheng, and G.-E. Chang, “GeSn Waveguide Photodetectors with Vertical p–i–n Heterostructure for Integrated Photonics in the 2 μm Wavelength Band,” Adv Photonics Res 3(7), 2100330 (2022).
  17. [17]J. Wu, Q. Jiang, S. Chen, M. Tang, Y.I. Mazur, Y. Maidaniuk, M. Benamara, M.P. Semtsiv, W.T. Masselink, K.A. Sablon, G.J. Salamo, and H. Liu, “Monolithically Integrated InAs/GaAs Quantum Dot Mid-Infrared Photodetectors on Silicon Substrates,” ACS Photonics 3(5), 749–753 (2016).DOI
  18. [18]G.H. Ahn, A.D. White, H. Kim, N. Higashitarumizu, F.M. Mayor, J.F. Herrmann, W. Jiang, K.K.S. Multani, A.H. Safavi-Naeini, A. Javey, and J. Vučković, “Platform-agnostic waveguide integration of high-speed photodetectors with evaporated tellurium thin films,” Optica 10(3), 349 (2023).
  19. [19]J. Jean, J. Xiao, R. Nick, N. Moody, M. Nasilowski, M. Bawendi, and V. Bulović, “Synthesis cost dictates the commercial viability of lead sulfide and perovskite quantum dot photovoltaics,” Energy Environ Sci 11(9), 2295–2305 (2018).DOI
  20. [20]S. Lu, P. Liu, J. Yang, S. Liu, Y. Yang, L. Chen, J. Liu, Y. Liu, B. Wang, X. Lan, J. Zhang, L. Gao, and J. Tang, “High-Performance Colloidal Quantum Dot Photodiodes via Suppressing Interface Defects,” ACS Appl Mater Interfaces 15(9), 12061–12069 (2023).DOI
  21. [21]Y. Wang, H. Hu, M. Yuan, H. Xia, X. Zhang, J. Liu, J. Yang, S. Xu, Z. Shi, J. He, J. Zhang, L. Gao, J. Tang, and X. Lan, “Colloidal PbS Quantum Dot Photodiode Imager with Suppressed Dark Current,” ACS Appl Mater Interfaces, (2023).DOI
  22. [22]D.H. Parmar, J. M. Pina, T. Zhu, M. Vafaie, O. Atan, M. Biondi, A.M. Najjariyan, S. Hoogland, and E.H. Sargent, “Controlled Crystal Plane Orientations in the ZnO Transport Layer Enable High-Responsivity, Low-Dark-Current Infrared Photodetectors,” Advanced Materials 34(17), 1–6 (2022).DOI
  23. [23]M. Vafaie, J.Z. Fan, A. Morteza Najarian, O. Ouellette, L.K. Sagar, K. Bertens, B. Sun, F.P. García de Arquer, and E.H. Sargent, “Colloidal quantum dot photodetectors with 10-ns response time and 80% quantum efficiency at 1,550 nm,” Matter 4(3), 1042–1053 (2021).DOI
  24. [24]J. Yang, H. Hu, Y. Lv, M. Yuan, B. Wang, Z. He, S. Chen, Y. Wang, Z. Hu, M. Yu, X. Zhang, J. He, J. Zhang, H. Liu, H.Y. Hsu, J. Tang, H. Song, and X. Lan, “Ligand-Engineered HgTe Colloidal Quantum Dot Solids for Infrared Photodetectors,” Nano Lett 22(8), 3465–3472 (2022).DOI
  25. [25]S. Keuleyan, E. Lhuillier, V. Brajuskovic, and P. Guyot-Sionnest, “Mid-infrared HgTe colloidal quantum dot photodetectors,” Nat Photonics 5(8), 489–493 (2011).DOI
  26. [26]S.B. Hafiz, M.R. Scimeca, P. Zhao, I.J. Paredes, A. Sahu, and D.K. Ko, “Silver Selenide Colloidal Quantum Dots for Mid-Wavelength Infrared Photodetection,” ACS Appl Nano Mater 2(3), 1631–1636 (2019).
  27. [27]S. Bin Hafiz, M.M. Al Mahfuz, S. Lee, and D.K. Ko, “Midwavelength Infrared p-n Heterojunction Diodes Based on Intraband Colloidal Quantum Dots,” ACS Appl Mater Interfaces 13(41), 49043–49049 (2021).DOI
  28. [28]J. Leemans, V. Pejović, E. Georgitzikis, M. Minjauw, A.B. Siddik, Y.H. Deng, Y. Kuang, G. Roelkens, C. Detavernier, I. Lieberman, P.E. Malinowski, D. Cheyns, and Z. Hens, “Colloidal III–V Quantum Dot Photodiodes for Short-Wave Infrared Photodetection,” Advanced Science 9(17), (2022).
  29. [29]L. Elsinger, R. Petit, F. Van Acker, N.K. Zawacka, I. Tanghe, K. Neyts, C. Detavernier, P. Geiregat, Z. Hens, and D. Van Thourhout, “Waveguide-Coupled Colloidal Quantum Dot Light Emitting Diodes and Detectors on a Silicon Nitride Platform,” Laser Photon Rev 15(7), (2021).DOI
  30. [30]W. Xie, Y. Zhu, S. Bisschop, T. Aubert, Z. Hens, D. Van Thourhout, and P. Geiregat, “Colloidal Quantum Dots Enabling Coherent Light Sources for Integrated Silicon-Nitride Photonics,” IEEE Journal of Selected Topics in Quantum Electronics 23(5), (2017).DOI
  31. [31]Y. Zhu, W. Xie, S. Bisschop, T. Aubert, E. Brainis, P. Geiregat, Z. Hens, and D. Van Thourhout, “On-Chip Single-Mode Distributed Feedback Colloidal Quantum Dot Laser under Nanosecond Pumping,” ACS Photonics 4(10), 2446–2452 (2017).DOI
  32. [32]W. Xie, T. Stöferle, G. Rainò, T. Aubert, S. Bisschop, Y. Zhu, R.F. Mahrt, P. Geiregat, E. Brainis, Z. Hens, and D. Van Thourhout, “On-Chip Integrated Quantum-Dot–Silicon-Nitride Microdisk Lasers,” Advanced Materials 29(16), (2017).DOI
  33. [33]H. Jung, M. Lee, C. Han, Y. Park, K.-S. Cho, and H. Jeon, “Efficient on-chip integration of a colloidal quantum dot photonic crystal band-edge laser with a coplanar waveguide,” Opt Express 25(26), 32919 (2017).DOI
  34. [34]C. Pang, Y.-H. Deng, E. Kheradmand, N. Poonk ottil, R. Petit, L. Elsinger, C. Detavernier, P. Geiregat, Z. Hens, and D. Van Thourhout, “Integrated PbS Colloidal Quantum Dot Photodiodes on Silicon Nitride Waveguides,” ACS Photonics 10(12), 4215–4224 (2023).DOI
  35. [35]B. Zhu, M. Chen, Q. Zhu, G. Zhou, N.M. Abdelazim, W. Zhou, S. V. Kershaw, A.L. Rogach, N. Zhao, and H.K. Tsang, “Integrated Plasmonic Infrared Photodetector Based on Colloidal HgTe Quantum Dots,” Adv Mater Technol 4(10), 1–8 (2019).DOI
  36. [36]C. Dong, S. Liu, N. Barange, J. Lee, T. Pardue, X. Yi, S. Yin, and F. So, “Long-Wavelength Lead Sulfide Quantum Dots Sensing up to 2600 nm for Short-Wavelength Infrared Photodetectors,” ACS Appl Mater Interfaces 11(47), 44451–44457 (2019).DOI
  37. [37]M.P. Hendricks, M.P. Campos, G.T. Cleveland, I. Jen-La Plante, and J.S. Owen, “A tunable library of substituted thiourea precursors to metal sulfide nanocrystals,” Science (1979) 348(6240), 1226–1230 (2015).DOI
  38. [38]C.H.M. Chuang, P.R. Brown, V. Bulović, and M.G. Bawendi, “Improved performance and stability in quantum dot solar cells through band alignment engineering,” Nat Mater 13(8), 796–801 (2014).
  39. [39]S. Braun, W.R. Salaneck, and M. Fahlman, “Energy-level alignment at organic/metal and organic/organic interfaces,” Advanced Materials 21(14–15), 1450–1472 (2009).DOI
  40. [40]M. Biondi, M.J. Choi, O. Ouellette, S.W. Baek, P. Todorović, B. Sun, S. Lee, M. Wei, P. Li, A.R. Kirmani, L.K. Sagar, L.J. Richter, S. Hoogland, Z.H. Lu, F.P. García de Arquer, and E.H. Sargent, “A Chemically Orthogonal Hole Transport Layer for Efficient Colloidal Quantum Dot Solar Cells,” Advanced Materials 32(17), (2020).DOI

Paper details

vlnc:W_cukpp4b5
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents