Abstract

Antiferromagnets are promising candidates for next-generation spintronic devices owing to their negligible stray fields and ultrafast spin dynamics. The noncollinear antiferromagnet Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} exhibits a large anomalous Hall effect (AHE). However, its specific noncollinear spin configuration leads to the forbiddance of the anomalous Hall conductivity from the (0001) basal plane, σ(0001)σ_{(0001)}, limiting practical applications. Here, using first-principles density functional theory, we demonstrate that Mn enrichment in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} drives a magnetic transition from the coplanar 120∘120^\circ spin configuration to a non-coplanar state with moments tilted toward the cc-axis. This transition is primarily mediated by four-spin ring exchange interaction in the local triangular lattice, which breaks the time-reversal symmetry and generates a giant intrinsic anomalous Hall conductivity over the full three-dimensional space in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}. We predict that σ(0001)σ_{(0001)} reaches as high as ∼ ⁣−468 Ω−1⋅cm−1\sim\!-468~Ω^{-1}\cdot\mathrm{cm}^{-1}, and an enhanced σ(011ˉ0)σ_{(01\bar{1}0)} of ∼ ⁣−229 Ω−1⋅cm−1\sim\!-229~Ω^{-1}\cdot\mathrm{cm}^{-1} is expected in light Mn self-doping of Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} (Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}). Unlike previously reported mechanisms relying on external magnetic fields or strain, our approach exploits intrinsic compositional tuning to stabilize a non-coplanar magnetic ground state for realizing a strong full-space AHE in antiferromagnets, providing another viable pathway toward high-performance, low-power spintronic devices.

Introduction

Antiferromagnets (AFMs) have emerged as compelling platforms for next-generation spintronics, owing to their vanishing stray fields, terahertz-scale dynamics, and robustness against external magnetic perturbations [1, 2, 3]. Yet, unlike ferromagnets, AFMs lack a net magnetization, rendering their readout and control inherently challenging [4]. A breakthrough came with the theoretical prediction that certain noncollinear AFMs can host a large anomalous Hall effect (AHE) despite zero net moment, driven not by magnetization but by the Berry curvature of topologically nontrivial bands in momentum space [5, 6]. Subsequent experiments confirm the kagome AFM Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} exhibits a finite anomalous Hall conductivity (AHC, ∼20 Ω−1 cm−1\sim20\ \Omega^{-1}\,\mathrm{cm}^{-1}) at room temperature [7].

As shown in Figure 1a, stoichiometric Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} has a hexagonal D019D0_{19} structure (space group P63/mmcP6_{3}/mmc). In this structure, Mn atoms are arranged in a kagome lattice on the (0001) basal plane along the cc axis and Sn atoms occupy the centers of the kagome lattice. Below TNT_{\mathrm{N}} (∼420\sim420 K), the Mn moments form a noncollinear triangular spin structure, with neighboring magnetic moments aligned at an angle of 120° [8, 9]. The AHE in this system is captured within a framework of multipole moments: whereas bcc Fe derives its Hall response from a dipole moment, the AHE in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} arises from a cluster octupole moment formed by the six Mn spins [10, 11]. Crucially, this octupole moment transforms as an axial vector parallel to the (0001) basal plane. Combined with effective time-reversal symmetry RSTR_{\mathrm{S}}T and the mirror symmetry about the (0001) plane, it is forbidden for anomalous Hall conductivity on the basal plane σ(0001)\sigma_{(0001)} [12, 13]. Consequently, all topological responses, including AHE [7], anomalous Nernst effect [14], and magneto-optical Kerr effect [15], are only detectable on crystallographic planes perpendicular to the basal plane [1, 16, 17]. While non-basal thin films could access the AHE, their epitaxial growth demands more stringent growth conditions, stricter lattice matching, and fewer substrate types to choose, which severely limits scalability and compatibility with conventional semiconductor processes [8, 16]. Generally, a buffer layer is necessary to improve the compatibility between the thin film and the substrate [18, 19]. On the contrary, (0001)-oriented Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} films offer distinct practical advantages in the aforementioned aspects. Thus, the central challenge becomes clear: how to activate a finite anomalous Hall conductivity on the (0001) plane to achieve the full-space topological responses. Existing approaches, including doping, strain engineering [20], and interfacial Dzyaloshinskii-Moriya interaction (DMI) in heterostructures [21, 22], have sought to break the relevant symmetry and realize a non-zero σ(0001)\sigma_{(0001)}. Here, we propose a self-doping strategy via substituting Sn with Mn, as shown in Figure 1b. This approach could locally break the symmetry protection and induce a non-coplanar spin state on the basal plane, thereby generating a non-zero σ(0001)\sigma_{(0001)} [10].

Schematics of crystal and magnetic structure for stoichiometric Mn3Sn and Mn-rich Mn3Sn

Figure 1. Schematics of crystal and magnetic structure for stoichiometric Mn3_3Sn and Mn-rich Mn3_3Sn. a. Coplanar spin structure on the kagome lattice in Mn3_3Sn. Purple spheres represent Mn atoms, gray spheres represent Sn atoms, and the gray shaded area indicates the basal plane. In this coplanar configuration, time-reversal symmetry RsTR_sT remains a symmetry of the system, leading to a vanishing σ(0001)\sigma_{(0001)}. b. Non-coplanar magnetic structure in Mn-rich Mn3_3Sn. Green spheres represent Mn atoms substituting Sn site. The non-coplanarity breaks time-reversal symmetry and can generate a non-zero anomalous Hall conductivity σ(0001)≠0\sigma_{(0001)} \ne0.

Here, based on first-principles calculations we show that a stable non-coplanar spin state can be constructed by Mn substituting Sn in Mn3_3Sn through four-spin ring exchange interaction in local triangular lattice. The effect of this spin state evolution on the anomalous Hall effect was quantified. It was found that a strong full-space AHE is expected by slightly Mn self-doping in Mn3_3Sn (Mn3.125_{3.125}Sn0.875_{0.875}), the component of the anomalous Hall conductivity σ(0001)\sigma_{(0001)} as high as ∼\sim-468 Ω−1\Omega^{-1} cm−1^{-1} can be achieved, and the component of the anomalous Hall conductivity σ(011ˉ0)\sigma_{(01\bar{1}0)} can be enhanced to ∼\sim-229 Ω−1\Omega^{-1} cm−1^{-1} simultaneously.

Methods and computational details

The first-principles calculations were carried out using density functional theory (DFT) [23, 24] utilizing generalized gradient approximation (GGA) [25, 26] for exchange correlation potential. We used Perdew-Burke-Ernzerhof (PBE) functional for the GGA as implemented in Vienna ab initio simulation package (VASP) [27].

Projector-augmented-wave (PAW) potentials were employed to describe electron-ion interactions, setting a planewave-basis cutoff of 550 eV [28]. Starting from the experimentally determined hexagonal unit cell of Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} (P63/mmcP6_{3}/mmc; a=b=5.665a=b=5.665 Å, c=4.531c=4.531 Å), a 2×1×22\times1\times2 supercell containing 32 atoms was constructed (see Figure 2). All atomic sites in the supercell were systematically labeled for clarity in subsequent analysis. To model Mn-rich compositions, three distinct structural models were generated by substituting Sn with Mn, yielding compositions of Mn24Sn8\mathrm{Mn}_{24}\mathrm{Sn}_{8} (nominal Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}), Mn25Sn7\mathrm{Mn}_{25}\mathrm{Sn}_{7} (Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}), and Mn26Sn6\mathrm{Mn}_{26}\mathrm{Sn}_{6} (Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}). For one Mn doped supercell (Mn25Sn7\mathrm{Mn}_{25}\mathrm{Sn}_{7}), since all Sn atoms are equivalent to each other, only one configuration needed to be considered by symmetry constraints. For the case of two Mn dopants (Mn26Sn6\mathrm{Mn}_{26}\mathrm{Sn}_{6}), the most energetically favorable configurations were selected for calculating the AHC. The whole Brillouin-zone was sampled by a 5×10×65\times10\times6 k-mesh for supercells. Lattice constants and atomic coordinates were fully relaxed until the force on each atom was less than 0.001 eV/Å and the total energy minimization was performed with a tolerance of 10−710^{-7} eV.

Supercell structure of Mn3Sn with Mn and Sn atomic sites labeled

Figure 2. Supercell structure of Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} used in the present study. Mn and Sn atoms are depicted as purple and gray spheres, respectively. The aa, bb, cc axes are along the [21ˉ1ˉ0][2\bar{1}\bar{1}0], [1ˉ21ˉ0][\bar{1}2\bar{1}0], and [0001][0001] directions, respectively. Mn atomic sites are labeled with white numbers (1-24), while Sn sites are labeled with black numbers (25-32). The composition Mn25Sn7\mathrm{Mn}_{25}\mathrm{Sn}_{7} (corresponding to Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}) is obtained by substituting the Sn atom at site 27 with Mn; further substitution of the Sn atom at site 32 yields Mn26Sn6\mathrm{Mn}_{26}\mathrm{Sn}_{6} (Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}).

Maximally localized Wannier functions (MLWFs) were utilized to build an accurate tight-binding model via the Wannier interpolation approach [29, 30, 31]. Based on these Wannier representations, the intrinsic AHC was computed within the tight-binding framework. The calculations were performed on the constructed tight-binding models using a 101×101×101101 \times101 \times101 k-mesh for all supercells, as implemented in the WannierTools package [32, 33]. The AHC σαβA\sigma_{\alpha\beta}^{A} is obtained from [12, 34]:

σαβA=−e2ℏ∑n∫BZd3k(2π)3fn(k)Ωn,αβ(k)(1)\sigma_{\alpha\beta}^{A}=-\frac{e^{2}}{\hbar}\sum_{n}\int_{\mathrm{BZ}}\frac{\mathrm{d}^{3}k}{(2\pi)^{3}}f_{n}(\mathbf{k})\Omega_{n,\alpha\beta}(\mathbf{k}) \tag*{(1)}
Ωn,αβ(k)=2iℏ2∑m≠n⟨un(k)∣v^α∣um(k)⟩⟨um(k)∣v^β∣un(k)⟩(En(k)−Em(k))2(2)\Omega_{n,\alpha\beta}(\mathbf{k})=2i\hbar^{2}\sum_{m\ne n}\frac{\langle u_{n}(\mathbf{k})|\hat{v}_{\alpha}|u_{m}(\mathbf{k})\rangle\langle u_{m}(\mathbf{k})|\hat{v}_{\beta}|u_{n}(\mathbf{k})\rangle}{(E_{n}(\mathbf{k})-E_{m}(\mathbf{k}))^{2}} \tag*{(2)}

where Ωn,αβ(k)\Omega_{n,\alpha\beta}(\mathbf{k}) denotes the Berry curvature of band n in momentum space, fn(k)f_{n}(\mathbf{k}) is the Fermi–Dirac distribution function, v^α  (β,γ)\hat{v}_{\alpha\;(\beta,\gamma)} is the velocity operator, and En(k)E_{n}(\mathbf{k}) is the eigenvalue of the nth eigenstate ∣un(k)⟩|u_{n}(\mathbf{k})\rangle at k point.

Results and Discussion

Local non-coplanar spin structure in Mn-rich Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}

As shown in Figure 3a, the canting angle θ\theta is defined as the angle between the Mn moment and the basal plane. This parameter quantifies the degree of non-coplanarity in the spin structure: θ=0∘\theta= 0^\circ corresponds to a fully coplanar configuration, where the Mn moments lie entirely within the basal plane. The left panels of Figure 3b-Figure 3d show the dependence of the canting angles of Mn moments with the Mn sites in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}, Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}, and Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75} with SOC (yellow bars) and without SOC (green bars), respectively. Only the normal Mn sites labeled 1-24 as shown in Figure 2 are presented here. The colored dashed circles on the right side of each figure represent the spin structure of the 12 nearest-neighbor Mn atoms surrounding the doping site 27 or 32 in undoped (b) and Mn-doped (c-d) cases.

Characterization of the canting angles of Mn moments for Mn3Sn, Mn3.125Sn0.875, and Mn3.25Sn0.75

Figure 3. Characterization of the canting angles θ\theta of Mn moments indicative of the non-coplanarity for Mn3_3Sn, Mn3.125_{3.125}Sn0.875_{0.875}, and Mn3.25_{3.25}Sn0.75_{0.75}. a. Schematic illustration of the canting angle θ\theta defined between the Mn moment and the blue basal plane. Canting angles θ\theta at the 24 regular Mn sites (labeled 1–24, see Figure 2) for b. Mn3_3Sn, c. Mn3.125_{3.125}Sn0.875_{0.875}, and d. Mn3.25_{3.25}Sn0.75_{0.75}. Results with and without SOC are shown as yellow and green bars, respectively. Adjacent colored dashed circles on the right side of each panel are the space distribution of spin structures of the 12 nearest-neighbor Mn atoms surrounding the doping site 27 or 32 in b. Mn3_3Sn, c. Mn3.125_{3.125}Sn0.875_{0.875}, and d. Mn3.25_{3.25}Sn0.75_{0.75}. Red arrows illustrate both the direction and magnitude of the Mn moments.

In stoichiometric Mn3_3Sn (Figure 3b), all Mn moments remain strictly within the basal plane (θ=0∘\theta= 0^\circ), exhibiting a fully coplanar spin structure. The resulting net magnetic moment is negligible (~0.002 μB\mu_{\mathrm{B}}/Mn), in excellent agreement with neutron diffraction experiments [35]. In contrast, the left panel of Figure 3c reveals that the canting angles of all Mn moments deviate from 0∘0^\circ, indicating that Mn self-doping in Mn3.125_{3.125}Sn0.875_{0.875} drives a clear departure from the coplanar spin state. Moreover, the out-of-plane canting is markedly stronger in the blue region compared to the gray region. This spatial correlation demonstrates that the magnitude of the canting angle is directly governed by proximity to the dopant. In other words, the substitutional Mn atom acts as a local perturbation center that reorients neighboring spins within the same kagome layer. Such local symmetry breaking lifts the perfect cancellation of magnetic moments in the ideal coplanar structure, thereby inducing a finite net magnetization of approximately 0.076 μB0.076\ \mu_{\mathrm{B}}/Mn.

Figure 3d shows that further increasing the Mn content to Mn3.25_{3.25}Sn0.75_{0.75} enhances and stabilizes this non-coplanar character. Two distinct canting regions now emerge around the two Mn dopant sites labeled 27 and 32. Due to antiferromagnetic coupling, the Mn moments surrounding site 27 tilt downward (negative cc-axis direction), while those near site 32 tilt upward (positive cc-axis direction). This opposing canting results in partial cancellation of the induced moments, yielding a reduced net magnetization of ∼0.030 μB\sim0.030\ \mu_{\mathrm{B}}/Mn. In summary, Mn substitution at Sn sites not only induces a local non-coplanar spin state but also preserves the overall antiferromagnetic character.

The spin related Hamiltonian for Mn3_3Sn can be written as [36]:

HS=J1∑⟨ij⟩xySi⋅Sj+J2∑⟨ij⟩zSi⋅Sj+∑ijDij⋅(Si×Sj)−∑iK(n^i⋅Si)2(3)H_{\mathrm{S}} = J_1 \sum_{\langle ij\rangle_{xy}} \mathbf{S}_i \cdot\mathbf{S}_j + J_2 \sum_{\langle ij\rangle_z} \mathbf{S}_i \cdot\mathbf{S}_j + \sum_{ij} \mathbf{D}_{ij} \cdot\left(\mathbf{S}_i \times\mathbf{S}_j\right) - \sum_i K\left(\hat{\mathbf{n}}_i \cdot\mathbf{S}_i\right)^2 \tag*{(3)}

where the first and second terms are the in-plane and out-of-plane Heisenberg exchange interactions, respectively; the third term is the DMI; and the fourth term describes the magnetocrystalline anisotropy. Both DMI and magnetocrystalline anisotropy arise from SOC. To determine the origin of the local non-coplanar spin structure in Mn-rich Mn3_3Sn, we computed the magnetic ground states of Mn3_3Sn, Mn3.125_{3.125}Sn0.875_{0.875}, and Mn3.25_{3.25}Sn0.75_{0.75} without including SOC. The resulting canting angles θ\theta shown as green bars in Figure 3b-Figure 3d are nearly indistinguishable from those obtained with SOC (yellow bars) for all 24 regular Mn sites (labeled 1-24). This remarkable agreement demonstrates that the non-coplanar spin texture induced by Mn substitution at Sn sites is predominantly governed by Heisenberg exchange interactions, rather than by SOC-driven effects such as DMI or magnetic anisotropy.

In stoichiometric Mn3_3Sn, the Mn atoms on the basal plane form a global kagome lattice, which constitutes a three-sublattice antiferromagnetic system, as illustrated in Figure 4a. The antiferromagnetic coupling among the three sublattices stabilizes a noncollinear inverse triangular spin structure [7]. The dominant exchange interaction in this system is the conventional two-spin Heisenberg exchange, expressed as [37]:

Magnetic exchange interactions on the basal plane in stoichiometric and Mn-rich Mn3Sn

Figure 4. The magnetic exchange interactions on the basal plane in stoichiometric and Mn-rich Mn3SnMn_3Sn. a. Coplanar 120° antiferromagnetic order in stoichiometric Mn3SnMn_3Sn, stabilized by two-spin Heisenberg exchange interaction within the global kagome lattice. b. Local non-coplanar spin structure in Mn-rich Mn3SnMn_3Sn, driven by four-spin ring exchange interaction arising from Mn atoms substituting Sn sites and forming triangular lattice.

H2-spin=−∑ijJijSi⋅Sj(4)H_{2\text{-spin}}=-\sum_{ij}J_{ij}\mathbf{S}_{i}\cdot\mathbf{S}_{j} \tag*{(4)}

where the exchange integral constant Jij<0J_{ij}<0 reflects antiferromagnetic coupling between Mn spins at sites ii and jj. Upon Mn substitution at Sn sites, a local triangular lattice of Mn atoms emerges around the dopant site, superimposed on the original kagome network, as shown in the area enclosed by the black dashed loop in Figure 4b. Within this local environment, the substitutional Mn atom and its in-plane neighbors form a four-sublattice antiferromagnetic system. A rhombus-shaped four-site plaquette (labeled ii-jj-kk-ll) closed loop enables a higher-order, non-Heisenberg magnetic interaction: the four-spin ring exchange, given by [37]:

H4-spin=−∑ijklKijkl[(Si⋅Sj)(Sk⋅Sl)+(Sj⋅Sk)(Sl⋅Si)−(Si⋅Sk)(Sj⋅Sl)](5)H_{4\text{-spin}}=-\sum_{ijkl}K_{ijkl}\left[(\mathbf{S}_{i}\cdot\mathbf{S}_{j})(\mathbf{S}_{k}\cdot\mathbf{S}_{l})+(\mathbf{S}_{j}\cdot\mathbf{S}_{k})(\mathbf{S}_{l}\cdot\mathbf{S}_{i})-(\mathbf{S}_{i}\cdot\mathbf{S}_{k})(\mathbf{S}_{j}\cdot\mathbf{S}_{l})\right] \tag*{(5)}

where KijklK_{ijkl} is the four-spin exchange integral constant.

Unlike the two-spin Heisenberg interaction, the four-spin ring exchange originates from virtual electron hopping around a closed plaquette and can stabilize complex magnetic structures by permitting a finite solid angle among four spins, thereby enabling non-coplanar spin configurations [38, 39]. Notably, in systems where crystal symmetry forbids the DMI, four-spin exchange alone can stabilize topological spin structures without requiring antisymmetric exchange [40, 41, 42]. In Mn-rich Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}, the interplay between the inherent two-spin Heisenberg exchange of the kagome lattice and the emergent four-spin ring exchange induced by Mn doping gives rise to local noncoplanar spin structures. This competition and cooperation between different exchange pathways provide a microscopic origin for the observed canting angles, even in the absence of strong SOC-driven effects.

Prediction of giant full-space anomalous Hall effect

To further evaluate the AHC of Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}, Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}, and Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}, we first performed band structure fitting for each system. As shown in Figure 5a-Figure 5c, the band structures obtained from first-principles calculations and those reconstructed via Wannier interpolation are in excellent agreement along the selected high-symmetry path. This consistency not only validates the accuracy of our Wannier fitting approach but also establishes a reliable foundation for subsequent analysis of the topological transport properties in these systems.

Electronic band structures and anomalous Hall conductivity for Mn$_3$Sn, Mn$_{3.125}$Sn$_{0.875}$, and Mn$_{3.25}$Sn$_{0.75}$

Figure 5. Anomalous Hall conductivity (AHC) near the Fermi level for Mn3_3Sn, Mn3.125_{3.125}Sn0.875_{0.875}, and Mn3.25_{3.25}Sn0.75_{0.75}. The left, middle, and right columns correspond to Mn3_3Sn, Mn3.125_{3.125}Sn0.875_{0.875}, and Mn3.25_{3.25}Sn0.75_{0.75}. a-c. Electronic band structures along the high-symmetry path Γ\Gamma-A-H-K-Γ\Gamma of the primitive cell. The red solid lines and green dashed lines represent results from first-principles calculations and Wannier interpolation, respectively. d-f. AHC σ(0001)\sigma_{(0001)} as a function of energy EE. g-i. AHC σ(011ˉ0)\sigma_{(01\bar{1}0)} as a function of energy EE. All calculations include SOC and are performed within ±0.5\pm0.5 eV of the Fermi level. The arrows in d–i indicate the AHC values at the Fermi level.

We now systematically analyze the AHC of Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}, Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}, and Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}, focusing on both the basal plane component σ(0001)\sigma_{(0001)} and the vertical plane component σ(011ˉ0)\sigma_{(01\bar{1}0)}. Figure 5d-Figure 5f display σ(0001)\sigma_{(0001)} as a function of energy, while Figure 5g-Figure 5i show σ(011ˉ0)\sigma_{(01\bar{1}0)} as a function of energy. For stoichiometric Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}, σ(0001)\sigma_{(0001)} at the Fermi level EFE_{\mathrm{F}} is nearly zero (Figure 5d), consistent with symmetry constraints and experimental observations [7]. In contrast, Mn enrichment induces a non-coplanar spin structure that breaks time-reversal symmetry. Previous studies have demonstrated that even a slight canting of Mn moments can generate a non-zero σ(0001)\sigma_{(0001)}. For instance, Zhu et al. reported that under an external magnetic field, when the Mn moments in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} are canted by approximately 3∘3^\circ out of the basal plane, σ(0001)\sigma_{(0001)} becomes non-zero [43]. In our work, Mn enrichment in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} stabilizes a pronounced non-coplanar configuration, resulting in a giant intrinsic σ(0001)≈−468 Ω−1 cm−1\sigma_{(0001)} \approx-468\ \Omega^{-1}\,\mathrm{cm}^{-1} at EFE_{\mathrm{F}} for Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875} (Figure 5e). A similar mechanism persists in Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}, where σ(0001)≈−311 Ω−1 cm−1\sigma_{(0001)} \approx-311\ \Omega^{-1}\,\mathrm{cm}^{-1} (Figure 5f). The σ(0001)\sigma_{(0001)} values significantly exceed the maximum σ(0001)\sigma_{(0001)} (∼−140 Ω−1 cm−1\sim-140\ \Omega^{-1}\,\mathrm{cm}^{-1}) at low temperatures reported in Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn} single crystals [7]. Moreover, they compare favorably with those of other notable noncollinear AFMs such as −284 Ω−1 cm−1-284\ \Omega^{-1}\,\mathrm{cm}^{-1} −1^{-1} in Mn3Rh\mathrm{Mn}_3\mathrm{Rh}, -312 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} in Mn3Ir\mathrm{Mn}_3\mathrm{Ir}, and 98 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} in Mn3Pt\mathrm{Mn}_3\mathrm{Pt} [12]. Our theoretical calculation may precisely explain the experimental results of Huang et al., where a non-zero AHE was observed in (0001)-oriented Mn-rich Mn3Sn\mathrm{Mn}_3\mathrm{Sn} [44]. Similarly, Chatterjee et al. observed a non-coplanar spin structure in Mn3Sn\mathrm{Mn}_3\mathrm{Sn}/Ta heterostructures with a small canting angle of 0.10.1-0.2∘0.2^\circ, leading to a non-zero σ(0001)\sigma_{(0001)} [18].

Figure 5g-Figure 5i show the energy-dependent σ(011ˉ0)\sigma_{(01\bar{1}0)} for Mn3Sn\mathrm{Mn}_3\mathrm{Sn}, Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}, and Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}. For Mn3Sn\mathrm{Mn}_3\mathrm{Sn}, σ(011ˉ0)\sigma_{(01\bar{1}0)} at EFE_F is approximately -116 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1}, which is consistent with the value reported (∼\sim-133 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1}) and the overall shape of the energy-dependent curve [12]. Upon Mn doping, σ(011ˉ0)\sigma_{(01\bar{1}0)} at EFE_F increases significantly, reaching approximately -229 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} for Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}, and -297 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} for Mn3.25Sn0.75\mathrm{Mn}_{3.25}\mathrm{Sn}_{0.75}, as indicated in Figure 5h and Figure 5i, respectively. Notably, these values in Mn-rich Mn3Sn\mathrm{Mn}_3\mathrm{Sn} are larger than that of Mn3Ga\mathrm{Mn}_3\mathrm{Ga} (∼\sim81 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1}) and even approach the value reported for Mn3Ge\mathrm{Mn}_3\mathrm{Ge} (∼\sim-330 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1}) [12].

The underlying mechanism for the enhanced AHC in both directions originates from a dual effect of Mn enrichment: it causes minor lattice distortions and stabilizes a non-coplanar magnetic structure. This structural and magnetic reconfiguration concurrently breaks spatial inversion and time-reversal symmetries, substantially lowering the overall symmetry of the system. The resulting symmetry breaking affects the electronic band structure and may generate large Berry curvature that does not cancel out. This enables a giant intrinsic AHC within the basal plane, where it was originally vanishing, and simultaneously a giant enhancement of the out-of-plane AHC, thereby achieving a full-space anomalous Hall response. Our results establish self-doping as an effective strategy for engineering a giant, omnidirectional anomalous Hall effect in Mn3Sn\mathrm{Mn}_3\mathrm{Sn}.

Summary

This work demonstrates that Mn enrichment in Mn3_3Sn controllably induces a non-coplanar antiferromagnetic state, transforming the system from a coplanar 120° order. The transition is primarily mediated by four-spin ring exchange interaction in local triangular lattice instead of two-spin Heisenberg exchange interaction in global kagome lattice. With the help of the non-coplanar spin state, the time-reversal symmetry is broken and the finite σ(0001)\sigma_{(0001)} is allowed. Both the anomalous Hall conductivity (AHC) from the (0001) basal plane σ(0001)\sigma_{(0001)} and the (011ˉ0)(01\bar{1}0) plane σ(011ˉ0)\sigma_{(01\bar{1}0)} are calculated in stoichiometric and Mn-rich Mn3Sn\mathrm{Mn}_{3}\mathrm{Sn}. A strong full-space AHE is expected in Mn3.125Sn0.875\mathrm{Mn}_{3.125}\mathrm{Sn}_{0.875}. The σ(0001)\sigma_{(0001)} as high as -468 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} can be achieved, and the σ(011ˉ0)\sigma_{(01\bar{1}0)} can be enhanced to -229 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} simultaneously. The realization of a full-space anomalous Hall response in an antiferromagnet represents a significant step toward three-dimensional topological spintronic functionality.

ACKNOWLEDGMENTS

This work was supported by the National Natural Science Foundation of China (under grants 51901067, 51971087, 52101233, and 52071279), the Natural Science Foundation of Hebei Province (E2019205234), the Science and Technology Research Project of Hebei Higher Education (QN2019154), the Science Foundation of Hebei Normal University (L2019B11 and L2024B08), the Hebei Normal University Teaching Improvement Project (2022XJJG045), and the “333 Talent Project” of Hebei Province (C20231105).

References

  1. [1]L. Šmejkal, A. H. MacDonald, J. Sinova, S. Nakatsuji, and T. Jungwirth, Anomalous Hall antiferromagnets, Nat. Rev. Mater. 7, 482 (2022).arxiv.org/abs/2107.03321
  2. [2]S. Nakatsuji, Topological magnets-their basic science and potential applications, AAPPS Bull. 32, 25 (2022).DOI
  3. [3]V. Baltz, A. Manchon, M. Tsoi, T. Moriyama, T. Ono, and Y. Tserkovnyak, Antiferromagnetic spintronics, Rev. Mod. Phys. 90, 015005 (2018).DOI
  4. [4]P. Stremoukhov, A. Safin, C. F. Schippers, R. Lavrijsen, M. Bal, U. Zeitler, A. Sadovnikov, E. Kozlova, K. S. Il’kch’y, S. Nikitov, and A. Kirilyuk, Strongly nonlinear antiferromagnetic dynamics in high magnetic fields, Results Phys. 57, 107377 (2024).arxiv.org/abs/2211.00353
  5. [5]H. Chen, Q. Niu, and A. H. MacDonald, Anomalous Hall Effect arising from Noncollinear Antiferromagnetism, Phys. Rev. Lett. 112, 017205 (2014).pubmed.ncbi.nlm.nih.gov/24483927
  6. [6]J. Kübler and C. Felser, Non-collinear antiferromagnets and the anomalous Hall effect, Europhys. Lett. 108, 67001 (2014).
  7. [7]S. Nakatsuji, N. Kiyohara, and T. Higo, Large anomalous Hall effect in a non-collinear antiferromagnet at room temperature, Nature 527, 212 (2015).
  8. [8]A. Markou, J. M. Taylor, A. Kalache, P. Werner, S. S. P. Parkin, and C. Felser, Noncollinear antiferromagnetic Mn₃Sn films, Phys. Rev. Mater. 2, 051001(R) (2018).
  9. [9]T. Nagamiya, S. Tomiyoshi, and Y. Yamaguchi, Triangular spin configuration and weak ferromagnetism of Mn₃Sn and Mn₃Ge, Solid State Commun. 42, 385 (1982).
  10. [10]M. T. Suzuki, T. Koretsune, M. Ochi, and R. Arita, Cluster multipole theory for anomalous Hall effect in antiferromagnets, Phys. Rev. B 95, 094406 (2017).DOI
  11. [11]H. Isshiki, N. Budai, A. Kobayashi, R. Uesugi, T. Higo, S. Nakatsuji, and Y. Otani, Observation of cluster magnetic octupole domains in the antiferromagnetic Weyl semimetal Mn₃Sn nanowire, Phys. Rev. Lett. 132, 216702 (2024).DOI
  12. [12]Y. Zhang, Y. Sun, H. Yang, J. Železný, S. S. P. Parkin, C. Felser, and B. Yan, Strong anisotropic anomalous Hall effect and spin Hall effect in the chiral antiferromagnetic compounds Mn₃X (X = Ge, Sn, Ga, Ir, Rh, and Pt), Phys. Rev. B 95, 075128 (2017).DOI
  13. [13]A. K. Nayak, J. E. Fischer, Y. Sun, B. Yan, J. Karel, A. C. Komarek, C. Shekhar, N. Kumar, W. Schnelle, J. K\uuml;bler, C. Felser, and S. S. P. Parkin, Large anomalous Hall effect driven by a nonvanishing Berry curvature in the noncollinear antiferromagnet Mn₃Ge, Sci. Adv. 2, e1501870 (2016).DOI
  14. [14]H. Reichlova, T. Janda, J. Godinho, A. Markou, D. Kriegner, R. Schlitz, J. Zelezny, Z. Soban, M. Bejarano, H. Schultheiss, P. Nemec, T. Jungwirth, C. Felser, J. Wunderlich, and S. T. B. Goennenwein, Imaging and writing magnetic domains in the non-collinear antiferromagnet Mn₃Sn, Nat. Commun. 10, 5459 (2019).DOI
  15. [15]T. Higo, H. Man, D. B. Gopman, L. Wu, T. Koretsune, O. M. J. van't Erve, Y. P. Kabanov, D. Rees, Y. Li, M.-T. Suzuki, S. Patankar, M. Ikhlas, C. L. Chien, R. Arita, R. D. Shull, J. Orenstein, and S. Nakatsuji, Large magneto-optical Kerr effect and imaging of magnetic octupole domains in an antiferromagnetic metal, Nat. Photonics 12, 73 (2018).DOI
  16. [16]S. Upadhyay, T. Erickson, H. Hall, A. Shrestha, D. C. Ingram, K. Sun, J. C. M. Hernandez, G. H. Cocoletzi, N. Takeuchi, and A. R. Smith, Molecular beam epitaxy and crystal structure of majority a-plane-oriented and substrate-strained Mn₃Sn thin films grown directly on sapphire (0001), J. Vac. Sci. Technol. A 41, 042710 (2023).
  17. [17]S. Hu, D.-F. Shao, H. Yang, C. Pan, Z. Fu, M. Tang, Y. Yang, W. Fan, S. Zhou, E. Y. Tsymbal, and X. Qiu, Efficient perpendicular magnetization switching by a magnetic spin Hall effect in a noncollinear antiferromagnet, Nat. Commun. 13, 4447 (2022).
  18. [18]D. Paul, S. Yadav, S. Gupta, B. Patra, N. Kulkarni, D. Mondal, K. Gavankar, S. K. Sahu, B. Satpati, B. Singh, O. Benton, and S. Chatterjee, Imprinting electrically switchable scalar spin chirality by anisotropic strain in a Kagome antiferromagnet, Adv. Sci. 12, e02569 (2025).DOI
  19. [19]D. Gao, Z. Peng, N. Zhang, Y. Xie, Y. Yang, W. Yang, S. Xia, W. Yan, L. Deng, T. Liu, J. Qin, X. Zhong, and L. Bi, Epitaxial growth of high quality Mn3Sn thin films by pulsed laser deposition, Appl. Phys. Lett. 121, 242403 (2022).DOI
  20. [20]J. M. Taylor, A. Markou, E. Lesne, P. K. Sivakumar, C. Luo, F. Radu, P. Werner, C. Felser, and S. S. P. Parkin, Anomalous and topological Hall effects in epitaxial thin films of the noncollinear antiferromagnet Mn3Sn, Phys. Rev. B 101, 094404 (2020).DOI
  21. [21]J.-J. Liu, K.-K. Meng, J.-K. Chen, Y. Wu, J. Miao, X.-G. Xu, and Y. Jiang, Robust interface-induced unusual anomalous Hall effect in Mn3Sn/Pt bilayers, Rare Met. 41, 3012 (2022).DOI
  22. [22]Y. Cheng, S. Yu, M. Zhu, J. Hwang, and F. Yang, Tunable topological Hall effects in noncollinear antiferromagnet Mn3Sn/Pt bilayers, APL Mater. 9, 051121 (2021).DOI
  23. [23]P. Hohenberg and W. Kohn, Inhomogeneous electron gas, Phys. Rev. 136, B864 (1964).
  24. [24]W. Kohn and L. J. Sham, Self-consistent equations including exchange and correlation effects, Phys. Rev. 140, A1133 (1965).DOI
  25. [25]J. P. Perdew, K. Burke, and M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77, 3865 (1996).pubmed.ncbi.nlm.nih.gov/10062328
  26. [26]J. P. Perdew, K. Burke, and M. Ernzerhof, Perdew, Burke, and Ernzerhof reply, Phys. Rev. Lett. 80, 891 (1998).DOI
  27. [27]G. Kresse and J. Furthmüller, Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set, Phys. Rev. B 54, 11169 (1996).pubmed.ncbi.nlm.nih.gov/9984901
  28. [28]G. Kresse and D. Joubert, From ultrasoft pseudopotentials to the projector augmented-wave method, Phys. Rev. B 59, 1758 (1999).DOI
  29. [29]N. Marzari and D. Vanderbilt, Maximally localized generalized Wannier functions for composite energy bands, Phys. Rev. B 56, 12847 (1997).DOI
  30. [30]I. Souza, N. Marzari, and D. Vanderbilt, Maximally localized Wannier functions for entangled energy bands, Phys. Rev. B 65, 035109 (2001).DOI
  31. [31]A. A. Mostofi, J. R. Yates, G. Pizzi, Y.-S. Lee, I. Souza, D. Vanderbilt, and N. Marzari, An updated version of wannier90: A tool for obtaining maximally-localised Wannier functions, Comput. Phys. Commun. 185, 2309 (2014).
  32. [32]Q. S. Wu, S. N. Zhang, H.-F. Song, M. Troyer, and A. A. Soluyanov, WannierTools: An open-source software package for novel topological materials, Comput. Phys. Commun. 224, 405 (2018).
  33. [33]G. Pizzi, V. Vitale, R. Arita, S. Blügel, F. Freimuth, G. Géranton, M. Gibertini, D. Gresch, C. Johnson, T. Koretsune, J. Ibañez-Azpiroz, H. Lee, J.-M. Lihm, D. Marchand, A. Marrazzo, Y. Mokrousov, J. I. Mustafa, Y. Nohara, Y. Nomura, L. Paulatto, S. Ponce, T. Ponweiser, J. Qiao, F. Thöle, S. S. Tsirkin, M. Wierzbowska, N. Marzari, D. Vanderbilt, I. Souza, A. A. Mostofi, and J. R. Yates, Wannier90 as a community code: new features and applications, J. Phys.: Condens. Matter 32, 165902 (2020).
  34. [34]D. Xiao, M.-C. Chang, and Q. Niu, Berry phase effects on electronic properties, Rev. Mod. Phys. 82, 1959 (2010).DOI
  35. [35]S. Tomiyoshi, Polarized neutron diffraction study of the spin structure of Mn₃Sn, J. Phys. Soc. Jpn. 51, 803 (1982).
  36. [36]J. Liu, and L. Balents, Anomalous Hall effect and topological defects in antiferromagnetic Weyl semimetals: Mn₃Sn/Ge, Phys. Rev. Lett. 119, 087202 (2017).DOI
  37. [37]Ph. Kurz, G. Bihlmayer, K. Hirai, and S. Blügel, Three-dimensional spin structure on a two-dimensional lattice: Mn/Cu(111), Phys. Rev. Lett. 86, 1106 (2001).pubmed.ncbi.nlm.nih.gov/11178021
  38. [38]K. Okigami, and S. Hayami, Four-spin interactions as a route to multiple-Q topological magnetic order, Phys. Rev. B 113, 064442 (2026).arxiv.org/abs/2510.15158
  39. [39]C. Singh, S. Jamaluddin, S. Pradhan, A. K. Nandy, M. Tokunaga, M. Avdeev, and A. K. Nayak, Higher order exchange driven noncoplanar magnetic state and large anomalous Hall effects in electron doped kagome magnet Mn₃Sn, npj Quantum Mater. 9, 43 (2024).DOI
  40. [40]I. A. Ado, O. Tchernyshyov, and M. Titov, Noncollinear Ground State from a Four-Spin Chiral Exchange in a Tetrahedral Magnet, Phys. Rev. Lett. 127, 127204 (2021).DOI
  41. [41]S. Hayami, Skyrmion crystal induced by four-spin interactions in itinerant triangular magnets, Magnetism 4, 281 (2024).DOI
  42. [42]T. Okubo, S. Chung, and H. Kawamura, Multiple-q states and the skyrmion lattice of the triangular-lattice Heisenberg antiferromagnet under magnetic fields, Phys. Rev. Lett. 108, 017206 (2012).pubmed.ncbi.nlm.nih.gov/22304286
  43. [43]X. Li, J. Koo, Z. Zhu, K. Behnia, and B. Yan, Field-linear anomalous Hall effect and Berry curvature induced by spin chirality in the kagome antiferromagnet Mn₃Sn, Nat. Commun. 14, 1642 (2023).DOI
  44. [44]D. Khadka, T. R. Thapaliya, S. H. Parra, X. Han, J. Wen, R. F. Need, P. Khanal, W. Wang, J. Zang, J. M. Kikkawa, L. Wu, and S. X. Huang, Kondo physics in antiferromagnetic Weyl semimetal Mn₃₊ₓSn₁₋ₓ films, Sci. Adv. 6, eabc1977 (2020).DOI

Paper details

vlnc:W_d62hagpz
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents